Suction assistant film and semiconductor wafer suction method
The suction auxiliary film with a base and auxiliary layer addresses suction failures in semiconductor wafers by providing consistent adhesion and preventing defects during backside processing.
Patent Information
- Application Number
- JP2021575688
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-05
- Filing Date
- 2021-01-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-01-14
AI Technical Summary
Semiconductor wafers with steps on the outer periphery cause suction failures due to variations in size and shape, leading to vacuum leaks during processing.
A suction auxiliary film with a base material layer and an auxiliary layer is interposed between the fixture and the semiconductor wafer, where the auxiliary layer has a tensile modulus of 5 MPa to 150 MPa and is made of materials like ethylene-vinyl acetate copolymer or polyolefin elastomer, assisting in adsorption by elastically deforming to match the surface shapes.
The suction auxiliary film effectively suppresses suction failures and defects like wafer cracking during backside processing, ensuring reliable adhesion and uniform suction area regardless of the step variations.
Smart Images

Figure 0007569812000001 
Figure 0007569812000002 
Figure 0007569812000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an auxiliary suction film that assists suction when the surface of a semiconductor wafer on which a circuit is formed is suctioned to a fixture, and to a method of suctioning a semiconductor wafer using the auxiliary suction film. [Background technology]
[0002] During the manufacture of semiconductor components, a semiconductor wafer is thinned by grinding its backside after circuits and the like are formed on its front side. During the grinding process, a protective film 130 is attached to front side 111 of semiconductor wafer 110, and the circuits and the like are covered and protected with this protective film 130, and then front side 111 is adsorbed to fixture 141 via protective film 130 (see FIG. 9). Patent Document 1 discloses a technique for grinding the protective film and the back surface side described above. The processing method of Patent Document 1 includes a cutting step (trimming process) for a semiconductor wafer having a film layer formed on the surface and a chamfered portion formed on the outer peripheral side surface, in which a cutting blade is inserted from the surface of the semiconductor wafer to the outer peripheral edge while rotating the semiconductor wafer, thereby cutting and removing at least the film layer on the chamfered portion in a circular shape. The trimmed semiconductor wafer 110 has a step 113 on the outer periphery of the surface 111. For this reason, the fixture 141 that adsorbs the semiconductor wafer 110 is designed taking the step 113 into consideration. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-43825 A Summary of the Invention [Problem to be solved by the invention]
[0004] It has been found that some semiconductor wafers 110 having the above-mentioned step 113 cause suction failures such as vacuum leaks in the fixture 141. This suction failure is considered to occur due to, for example, in the case of trimming processing, variations in the dimensions and shape of the step 113 caused by limitations in processing accuracy, etc.
[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide a suction assistant film and a semiconductor wafer suction method that can suppress the occurrence of suction failures. [Means for solving the problem]
[0006] As a means for solving the above problems, the present invention is as follows. [1] The invention described in claim 1 is an adsorption assistant film that is interposed between a fixture and a semiconductor wafer when a surface of the semiconductor wafer on which a circuit is formed is adsorbed to the fixture, the film comprising: a base layer attached to the side on which the circuit is formed; and an auxiliary layer that is supported by the base layer and comes into contact with the fixing tool to assist adhesion. [2] The invention described in claim 2 is characterized in that, in the invention described in claim 1, the auxiliary layer is a layer having a tensile modulus of elasticity of 5 MPa or more and 150 MPa or less at a temperature of 25°C or more and 35°C or less. [3] The invention described in claim 3 is the invention described in claim 1 or 2, wherein the semiconductor wafer has a step on the outer peripheral edge of the surface on which the circuit is formed, thereby reducing the suction area of the surface relative to the fixing device. [4] The invention described in claim 4 is characterized in that, in the invention described in any one of claims 1 to 3, the auxiliary layer contains one or more types selected from the group consisting of ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, and polyamide-based elastomers. [5] The invention described in claim 5 is characterized in that, in the invention described in any one of claims 1 to 4, the thickness of the auxiliary layer is 100 μm or more and 500 μm or less. [6] The invention described in claim 6 is characterized in that, in the invention described in any one of claims 1 to 5, the base material layer is a layer having a tensile modulus of elasticity of 5000 MPa or less at a temperature of 25°C or higher and 35°C or lower. [7] The invention described in claim 7 is characterized in that, in the invention described in any one of claims 1 to 6, the base material layer contains one or more types selected from the group consisting of polyester and polyamide. [8] The invention described in claim 8 is characterized in that, in the invention described in any one of claims 1 to 7, the thickness of the base material layer is 10 μm or more and 200 μm or less.
[0007] [9] The invention described in claim 9 includes a suction step of interposing an auxiliary suction film between a surface of a semiconductor wafer on which a circuit is formed and a fixture that suctions the semiconductor wafer, and suctioning the semiconductor wafer to the fixture via the auxiliary suction film, the semiconductor wafer has a step on an outer periphery of a surface on which the circuit is formed, thereby reducing an adsorption area of the surface with respect to the fixture, The adsorption auxiliary film is a base layer attached to the surface on which the circuit is formed; and an auxiliary layer that is supported by the base layer and comes into contact with the fixing tool to assist adhesion.
[10] The invention described in claim 10 is characterized in that, in the invention described in claim 9, the auxiliary layer is a layer having a tensile modulus of elasticity of 5 MPa or more and 150 MPa or less at a temperature of 25°C or more and 35°C or less.
[11] The invention described in claim 11 is characterized in that, in the invention described in claim 9 or 10, the auxiliary layer contains one or more types selected from the group consisting of ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, and polyamide-based elastomers.
[12] The invention described in claim 12 is characterized in that, in the invention described in any one of claims 9 to 11, the thickness of the auxiliary layer is 100 μm or more and 500 μm or less.
[13] The invention described in claim 13 is characterized in that, in the invention described in any of claims 9 to 12, the base material layer is a layer having a tensile modulus of elasticity of 5000 MPa or less at a temperature of 25°C or higher and 35°C or lower.
[14] The invention described in claim 14 is characterized in that, in the invention described in any of claims 9 to 13, the base material layer contains one or more types selected from the group consisting of polyester and polyamide.
[15] The invention described in claim 15 is characterized in that, in the invention described in any one of claims 9 to 14, the thickness of the base material layer is 10 μm or more and 200 μm or less. Effect of the Invention
[0008] According to the suction assistant film and the semiconductor wafer suction method of the present invention, the occurrence of suction failures can be suppressed. [Brief description of the drawings]
[0009] [Figure 1] 1 is a front sectional view illustrating a semiconductor wafer according to the present invention. [Diagram 2] FIG. 2 is an enlarged front sectional view illustrating the adsorption auxiliary film of the present invention. [Diagram 3] 1 is a front sectional view illustrating a trimming process for a semiconductor wafer according to the present invention. [Figure 4] FIG. 2 is a front cross-sectional view illustrating a bonding step of the suction assisting film of the present invention. [Diagram 5] 3 is a front sectional view illustrating a suction step according to the semiconductor wafer suction method of the present invention. FIG. [Figure 6] 1A to 1C are front sectional views illustrating a processing step of a semiconductor wafer according to the present invention. [Figure 7] 10A to 10C are front sectional views illustrating a processing step of a semiconductor wafer according to another embodiment of the present invention. [Figure 8]FIG. 11 is a front sectional view illustrating a semiconductor wafer according to another embodiment of the present invention. [Figure 9] FIG. 11 is a front sectional view illustrating a conventional method for suctioning a semiconductor wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described below with reference to the drawings. The matters shown here are illustrative and are for illustrative purposes of the embodiments of the present invention, and are described for the purpose of providing what is believed to be the most effective and easy-to-understand explanation of the principles and conceptual features of the present invention. In this respect, it is not intended to show structural details of the present invention beyond a certain extent that are necessary for a fundamental understanding of the present invention, and the description in conjunction with the drawings will make it clear to those skilled in the art how some forms of the present invention are actually embodied.
[0011] [1] Semiconductor wafers The semiconductor wafer used in the present invention is used for manufacturing semiconductor parts, and is not particularly limited in terms of material or shape, as long as it has a circuit formed on one side (surface). Usually, a semiconductor wafer is formed into a disk shape using silicon as the material (see FIG. 1). The semiconductor wafer is thinned by grinding the back surface, which is the opposite side to the front surface on which the circuits are formed. The adsorption assistant film of the present invention is used in the back surface processing involved in this thinning. Hereinafter, in the semiconductor wafer, the surface on which the circuits are formed is also referred to as the "non-ground surface," and the surface ground in the thinning involved in the back surface processing is also referred to as the "ground surface." The suction auxiliary film of the present invention is also useful when suction-fixing, to a fixture, the semiconductor wafer having a step on its outer periphery, thereby reducing the suction area of the non-ground surface relative to the fixture.
[0012] Specifically, the semiconductor wafer 10 is formed in a plate shape as shown in Fig. 1. Circuits are formed on the non-ground surface 11 of the semiconductor wafer 10. The semiconductor wafer 10 is thinned to a desired thickness by grinding the ground surface 12 (see Fig. 6). Furthermore, as shown in FIG. 7, the present invention can also be used for grinding the grinding surface 12 in DBG (dicing before gridding) or SDBG (stealth dicing before gridding). The semiconductor wafer 10 has arcuate surfaces 14 at the portions extending from the non-ground surface 11 or the ground surface 12 to the outer surface as a result of the chamfering process. In the trimming process, the arcuate surfaces 14 on the non-ground surface 11 side are cut and removed (see FIG. 3). The trimmed semiconductor wafer 10 has a concave step 13 on the outer periphery of the non-ground surface 11 (see FIG. 1).
[0013] Here, the above-mentioned trimming process will be described. An example of a trimming device 20 used in the trimming process includes a chuck table 21 that adheres to the semiconductor wafer 10 by vacuum suction, and a trimming blade 22, as shown in FIG. During trimming, the semiconductor wafer 10 is fixed to the chuck table 21 with the grinding surface 12 being attracted to the chuck table 21 . The trimming process is performed by pressing a trimming blade 22 against the outer periphery of the non-ground surface 11 of the semiconductor wafer 10 while rotating a chuck table 21 to which the semiconductor wafer 10 is fixed by suction. In the trimmed semiconductor wafer 10, the arcuate surface 14 on the non-ground surface 11 side is cut and removed by the trimming blade 22, so that a concave step 13 is formed on the outer periphery of the non-ground surface 11.
[0014] The step 13 resulting from the above-mentioned trimming process has a width W in the radial direction of the semiconductor wafer 10 of preferably 1 to 10 mm, more preferably 2 to 8 mm, and particularly preferably 3 to 7 mm (see FIG. 1). Moreover, the height H of this step 13 in the thickness direction of the semiconductor wafer 10 is preferably 10 to 100 μm, more preferably 20 to 80 μm, and particularly preferably 30 to 70 μm (see FIG. 1).
[0015] The step 13 is not limited to that caused by the trimming process. Examples of the semiconductor wafer 10 having the step 13 on the outer periphery of the non-ground surface 11 other than that caused by the trimming process include the semiconductor wafer 10 having the following configuration. In the semiconductor wafer 10 shown in FIG. 8, a plurality of bumps 15 are formed on the non-ground surface 11, resulting in a step 13 being generated on the outer periphery of the non-ground surface 11 side. Although not specifically shown, examples of the semiconductor wafer having the above-mentioned step include a wafer having a multilayer film formed on the non-ground surface.
[0016] Regarding the above-mentioned step 13, the width W and height H are the average values of the measured widths and heights of four step portions selected to be spaced at central angle intervals of 10 to 90 degrees. In the present invention, the step 13 on the semiconductor wafer 10 includes a step caused by trimming processing, and further a step caused by the formation of a bump or a multilayer film. Specifically, the step 13 has a height difference (height H in the thickness direction of the semiconductor wafer 10) of 10 to 300 μm within a width W in the radial direction of the semiconductor wafer 10 from the outer periphery of the step 13 that is within a range of 1 to 30 mm.
[0017] The suction-assisting film of the present invention can be used for any type of semiconductor wafer 10. In particular, a wafer having a reduced suction area for a fixture such as a chuck table is useful as the semiconductor wafer 10. A trimmed wafer is particularly an example of the semiconductor wafer 10 with a reduced suction area. In this trimmed semiconductor wafer 10, the outer peripheral edge of the non-ground surface 11 is trimmed (notched) to provide a step 13, thereby reducing the suction area for a fixture 41 (such as a chuck table) (see FIG. 5). Here, the above-mentioned "adsorption area" refers to the area of the non-ground surface 11 of the semiconductor wafer 10 on which the adsorption force of the fixture 41 can act.
[0018] More specifically, the trimmed semiconductor wafer 10 has a step 13 formed by cutting the outer periphery of the non-ground surface 11 into a concave shape. On the non-ground surface 11 of the semiconductor wafer 10, the step 13 and a portion other than the step 13 do not come into contact with the fixture 41 on the same plane. For this reason, the suction force of the fixture 41 does not act easily or does not act at the step 13. Here, the actual suction area ar1 on the non-ground surface 11 of the semiconductor wafer 10 is a value obtained by subtracting the planar area of the portion corresponding to the step 13 from the planar area ar2 of the semiconductor wafer 10 (see FIG. 1). In other words, in the semiconductor wafer 10 having the step 13 on the outer periphery of the non-ground surface 11, the suction force of the fixture 41 acts only on the suction area ar1 which is smaller than the planar area ar2. In other words, the semiconductor wafer 10 has a step 13 on the outer peripheral edge of the non-ground surface 11, and therefore the adsorption area ar1 of the non-ground surface 11 with respect to the fixing device 41 is subtracted from the planar area ar2 of the semiconductor wafer 10 (non-ground surface 11).
[0019] [2] Adsorption support film The suction-assisting film of the present invention is disposed between a fixture and a semiconductor wafer when the surface (non-ground surface) of the semiconductor wafer on which circuits are formed is suction-attached to the fixture. The adsorption auxiliary film has a base layer and an auxiliary layer (see FIG. 2). The base layer is attached to the surface of the semiconductor wafer on which circuits are formed, that is, the non-ground surface.
[0020] Specifically, as shown in FIG. 2, the adsorption auxiliary film 30 has a base layer 31 and an auxiliary layer 32 . In the adhering step for back surface processing, this adsorption auxiliary film 30 is used with the base material layer 31 side facing the non-ground surface 11 of the semiconductor wafer 10. This base material layer 31 is adhered to the non-ground surface 11 of the semiconductor wafer 10 (see FIG. 4). In addition, the adsorption auxiliary film 30 is used with the auxiliary layer 32 side facing the fixture 41 in the adsorption step for back surface processing. The auxiliary layer 32 is brought into contact with the fixture 41 while being supported by the base layer 31, and is adsorbed to the fixture 41 (see FIG. 5). The auxiliary layer 32 corresponds to the surface shape of the non-ground surface 11 of the semiconductor wafer 10 and the surface shape of the fixture 41, and elastically deforms following these shapes. Due to the elastic deformation of the auxiliary layer 32, the suction auxiliary film 30 assists in suction of the semiconductor wafer 10 to the fixture 41 (see FIG. 6). In addition, the suction auxiliary film 30 covers and protects the circuit on the non-ground surface 11 side of the semiconductor wafer 10 during back surface processing.
[0021] There is no particular limitation on the shape of the suction assistant film 30. For example, the suction assistant film 30 may be circular, square, or the like in a plan view. There is no particular limitation on the average thickness of the adsorption auxiliary film 30. Specifically, the average thickness of the adsorption auxiliary film 30 is preferably 150 to 1000 μm, more preferably 175 to 950 μm or more, and further preferably 200 to 750 μm. The average thickness is defined as the average value of the thicknesses actually measured on the film at 10 locations selected at least 2 cm apart.
[0022] The suction assisting film 30 is not limited to being attached directly to the semiconductor wafer, so long as it is interposed between the fixture and the semiconductor wafer and assists suction when the non-ground surface of the semiconductor wafer is suctioned to the fixture. For example, a protective film for protecting the circuits may be applied to the non-ground surface of the semiconductor wafer, and the suction assisting film 30 may be applied over this protective film. Each layer of the adsorption assisting film 30 will now be described.
[0023] (1) Base material layer The base layer 31 is a layer provided for the purposes of protecting the circuits formed on the semiconductor wafer 10 and improving the handling properties and mechanical properties of the suction assist film 30 . There are no particular limitations on the material used for the base layer 31 as long as it has the mechanical strength sufficient to withstand the external force applied during back surface processing. Typically, the material used for the base layer 31 is a synthetic resin film.
[0024] Examples of the synthetic resins mentioned above include one or more thermoplastic resins selected from polyolefins such as polyethylene, polypropylene, poly(4-methyl-1-pentene), poly(1-butene), etc.; ethylene-vinyl acetate copolymers; polyesters such as polyethylene terephthalate, polybutylene terephthalate, etc.; polyamides such as nylon-6, nylon-66, polymetaxylene adipamide, etc.; polyacrylates; polymethacrylates; polyvinyl chloride; polyetherimides; polyacrylonitrile; polycarbonates; polystyrenes; ionomers; polysulfones; polyethersulfones; polyphenylene ethers, etc.
[0025] The base layer 31 preferably contains one or more types selected from the group consisting of polyester and polyamide among the above-mentioned synthetic resins. When the base layer 31 contains them, the handleability of the adsorption assistant film 30 can be improved. Additives can be added to the synthetic resins described above. Examples of additives include plasticizers, softeners (mineral oil, etc.), fillers (carbonates, sulfates, titanates, silicates, oxides (titanium oxide, magnesium oxide), silica, talc, mica, clay, fiber fillers, etc.), antioxidants, light stabilizers, antistatic agents, lubricants, colorants, etc. These additives may be used alone or in combination of two or more.
[0026] The film used as the material of the base layer 31 may be stretched or not. Any of non-stretched films and stretched films such as uniaxially stretched films and biaxially stretched films can be used. Stretched films are particularly useful from the viewpoint of improving mechanical strength. The above-mentioned film may be either a single-layer film or a multi-layer film having a plurality of layers. It is preferable to use a surface-treated film for the base layer 31. In this case, it is possible to improve adhesion to the auxiliary layer 32, etc. Specific examples of the surface treatment include corona treatment, plasma treatment, undercoat treatment, primer coat treatment, etc. The thickness T1 of the base layer 31 is not particularly limited (see FIG. 2). The thickness T1 is preferably 10 to 200 μm, more preferably 20 to 150 μm, and further preferably 30 to 100 μm. The range of the thickness T1 is determined from the viewpoint that the base layer 31 can obtain good characteristics.
[0027] Here, the tensile modulus of elasticity of the base layer 31 and the auxiliary layer 32 is obtained by reading data for each temperature from data obtained by measuring with a dynamic viscoelasticity measuring device (DMA) from 25° C. to 35° C. The measurement conditions are a sample size of 10 mm in width, a chuck length of 20 mm, a frequency of 1 Hz, and a heating rate of 5° C. / min. In the following, the tensile modulus of elasticity of the base layer 31 at 25° C. is defined as E′ 31 (25), the value at 35°C is E' 31 (35), and the value of each temperature between 25℃ and 35℃ is E' 31 Let (t). The tensile modulus of the auxiliary layer 32 at 25° C. is E′ 32 (25), the value at 35°C is E' 32 (35), and the value of each temperature between 25℃ and 35℃ is E' 32 Let (t).
[0028] The tensile modulus of the base layer 31 is usually E' 31 (t)≦5000 MPa. That is, in the temperature range of 25° C.≦t≦35° C., the tensile modulus of the base layer 31 is always 5000 MPa or less. Therefore, E′ 31 (25)≦5000MPa, E' 31 (35)≦5000 MPa. Also, usually, E' 31 (t)>E' 32That is, in the temperature range of 25° C.≦t≦35° C., the tensile modulus of the base layer 31 is always higher than the tensile modulus of the auxiliary layer 32. There is no limitation on the degree of the difference, but E′ 31 (t) is E' 32 It is preferably 20 to 4850 MPa higher than (t), and more preferably 700 to 4850 MPa higher. Therefore, at t=25° C., the difference (E′ 31 (25)-E' 32 (25)) is 20MPa ≦ E' 31 (25)-E' 32 (25) ≦4850MPa is preferable, and 700MPa ≦ E' 31 (25)-E' 32 (25)≦4850 MPa is more preferable. Similarly, at t=35° C., the difference (E′ 31 (35)-E' 32 (35)) is 20MPa ≦ E' 31 (35)-E' 32 (35) ≦4850MPa is preferable, and 700MPa ≦ E' 31 (35)-E' 32 (35)≦4850 MPa is more preferable.
[0029] (2) Auxiliary layer The auxiliary layer 32 is a layer provided for the purpose of assisting the adhesion of the semiconductor wafer 10 to the fixture 41 during back surface processing. Specifically, auxiliary layer 32 is a layer that can elastically deform in response to both the surface shape of semiconductor wafer 10 having steps 13 and the surface shape of fixture 41. Then, the elastically deformed auxiliary layer 32 assists in adhering semiconductor wafer 10 to fixture 41 (see FIG. 5). The flexibility of the auxiliary layer 32 is increased when the tensile modulus is reduced. In this case, the ability of the auxiliary layer 32 to conform to the surface shapes of the non-ground surface 11 of the semiconductor wafer 10 and the fixture 41 (such as a chuck table) can be improved. Furthermore, when the tensile modulus of elasticity of the auxiliary layer 32 is increased, the hardness of the auxiliary layer 32 is increased. In this case, the auxiliary layer 32 is prevented from sticking to the fixture 41 (such as a chuck table), and the ease of attachment and detachment between the auxiliary layer 32 and the fixture 41 can be improved.
[0030] The tensile modulus of the auxiliary layer 32 is preferably 5 MPa≦E′ 32 (t)≦150 MPa. That is, the tensile modulus of the auxiliary layer 32 is 5 MPa or more and 150 MPa or less in the temperature range of 25° C.≦t≦35° C. In this case, the auxiliary layer 32 can exhibit sufficient elasticity (mechanical stretchability) at the environmental temperature where the back surface processing is performed. More preferably, the tensile modulus E' is 6 MPa or less. 32 (t)≦120 MPa. More preferably, 7 MPa≦E′ 32 (t)≦80 MPa. Particularly preferably, 8 MPa≦E' 32 (t)≦60 MPa. Particularly preferably, 9 MPa≦E′ 32 (t)≦45 MPa.
[0031] There is no particular limitation on the material used for the auxiliary layer 32. The material for the auxiliary layer 32 is preferably a resin, and among resins, a resin having sufficient elasticity (mechanical stretchability) is more preferable, and a resin containing a thermoplastic material having elastomeric properties is particularly preferable. The thermoplastic material having elastomeric properties may be made of a block copolymer having a hard segment and a soft segment, may be made of a polymer alloy of a hard polymer and a soft polymer, or may have properties of both of these. Examples of the thermoplastic material include ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, polyamide-based elastomers, etc. These may be used alone or in combination of two or more.
[0032] When the material of the auxiliary layer 32 is a resin containing the above-mentioned thermoplastic material, the ratio of the thermoplastic material can be preferably 40 to 100 mass %, more preferably 60 to 100 mass %, and further preferably 80 to 100 mass %, based on the entire resin constituting the auxiliary layer 32. In other words, the resin constituting the auxiliary layer 32 may consist only of the above-mentioned thermoplastic material. Among the above-mentioned thermoplastic materials, ethylene-vinyl acetate copolymer is particularly preferred because its elasticity can be adjusted according to the vinyl acetate content. The vinyl acetate content in the ethylene-vinyl acetate copolymer is preferably 4 to 30% by mass, more preferably 5 to 25% by mass, and even more preferably 8 to 20% by mass, based on 100% by mass of the entire polymer. The thickness T2 of the auxiliary layer 32 is not particularly limited (see FIG. 2). The thickness T2 is preferably 100 to 500 μm, more preferably 100 to 400 μm, and further preferably 100 to 250 μm. The range of the thickness T2 is determined from the viewpoint of maintaining a sufficient margin for elastic deformation.
[0033] (3) Other layers The suction assist film 30 is not limited to the above-mentioned layers, and may have other layers. Examples of other layers include a support layer for attaching the adsorption auxiliary film 30 to the non-ground surface 11 side of the semiconductor wafer 10, an unevenness absorbing layer for absorbing the uneven shape caused by the bumps 15 in the case of the semiconductor wafer 10 having the above-mentioned bumps 15, an interface strength improving layer for improving the interface strength with the support layer, a migration prevention layer for suppressing migration of low molecular weight components to the surface of the support layer, an antistatic layer for preventing static electricity buildup on the adsorption auxiliary film 30, etc. These may be used alone or in combination of two or more kinds.
[0034] The retaining layer can be formed by applying or laminating a pressure-sensitive adhesive or adhesive to one surface of the base layer 31 that is the non-grinding surface 11. For example, examples of the pressure-sensitive adhesive include (meth)acrylic pressure-sensitive adhesives, silicone pressure-sensitive adhesives, urethane pressure-sensitive adhesives, rubber pressure-sensitive adhesives, and energy ray curable pressure-sensitive adhesives, while examples of the adhesive include acrylic, epoxy, and silicone pressure-sensitive adhesives. When the retaining layer is an adhesive, the adhesive strength is not particularly limited. The adhesive strength is preferably 0.1 to 10 N / 25 mm. The adhesive strength is more preferably 0.2 to 9 N / 25 mm, and further preferably 0.3 to 8 N / 25 mm. The range of adhesive strength is based on the viewpoint of being able to suppress adhesive residue on the semiconductor wafer during peeling while ensuring good adhesion to the semiconductor wafer. The adhesive strength is the adhesive strength to a silicon mirror wafer. Specifically, it is the measured value when the tape is attached to the surface of a silicon mirror wafer in an environment of 23°C temperature and 50% relative humidity, left for 60 minutes, and then peeled off at 180 degrees from the surface of the silicon mirror wafer. The measurement conditions other than those mentioned above are in accordance with JIS Z0237:2009. When the support layer is an adhesive, its thickness is not particularly limited. The thickness is preferably 1 to 50 μm, more preferably 2 to 45 μm, and even more preferably 3 to 40 μm. The thickness range is based on the viewpoint of exhibiting suitable adhesive strength while being peelable without leaving any adhesive residue.
[0035] The irregularity absorbing layer can be formed by laminating one surface of the base layer 31 on the non-ground surface 11 side, particularly between the base layer 31 and the retaining layer. The material of this irregularity absorbing layer is not particularly limited as long as it has irregularity absorbing properties due to the expression of fluidity or plasticity. Examples of such materials include acrylic resins, olefin resins, and ethylene-polar monomer copolymers. The thickness of the irregularity absorbing layer is not particularly limited as long as it is thick enough to absorb the irregularities caused by the bumps 15. The thickness is preferably 20 μm or more, more preferably 80 μm or more, and even more preferably 170 μm or more.
[0036] [3] Back surface processing As described above, the semiconductor wafer 10 is thinned by performing back surface processing. This back surface processing includes an attachment step of attaching the suction assistant film 30 to the semiconductor wafer 10, an adsorption step of adsorbing the semiconductor wafer 10 with the suction assistant film 30 attached to a fixture 41, and a processing step of processing the back surface of the semiconductor wafer 10. This back surface processing is performed using a processing device 40 equipped with a fixture 41 that adsorbs and fixes the semiconductor wafer 10, and a grinding tool 42 that grinds the grinding surface 12 of the semiconductor wafer 10, as shown in Figures 5 and 6. The bonding step, the adhering step, and the processing step will be described below.
[0037] (1) Pasting process The adhering step is a step for adhering the above-mentioned suction-assisting film 30 to the semiconductor wafer 10. As shown in FIG. 4, in the adhering step, the suction assisting film 30 is adhered to the non-ground surface 11 of the semiconductor wafer 10. In the adhering step, the suction auxiliary film 30 is adhered to the non-ground surface 11 of the semiconductor wafer 10 so as to cover the uneven shape of the non-ground surface 11 of the semiconductor wafer 10, particularly the steps 13 on the outer periphery. In the adhering step, there is no particular limitation on the method and device for adhering the suction assisting film 30 to the semiconductor wafer 10. Existing methods and devices can be used.
[0038] (2) Adsorption process The suction step is a step for the purpose of suctioning the semiconductor wafer 10 to which the suction auxiliary film 30 is attached, onto the fixture 41. By this suction process, an adsorption auxiliary film 30 is interposed between the non-ground surface 11 of the semiconductor wafer 10 and a fixture 41 that adsorbs the semiconductor wafer 10, and the semiconductor wafer 10 is adsorbed to the fixture 41 via the adsorption auxiliary film 30. That is, this adsorption step is included in the adsorption method of the present invention.
[0039] Specifically, as shown in FIG. 5, the semiconductor wafer 10 to which the suction-assisting film 30 has been attached in the above-mentioned attachment step is adsorbed to a fixture 41 with the non-ground surface 11 facing the fixture 41 side. In this suction step, the surface layer portion of the auxiliary layer 32 of the suction auxiliary film 30 on the side of the fixing tool 41 is elastically deformed to conform to the surface shape of the fixing tool 41 . In other words, the auxiliary layer 32 of the suction auxiliary film 30 elastically deforms so as to maintain the suction area ar3 for the fixture 41 at approximately the same size as the area ar4 of the surface of the fixture 41, without being affected by the surface shape of the non-ground surface 11, and in particular, regardless of the suction area ar1 which becomes uncertain due to variations in the step 13, etc. In other words, by having the elastically deformable auxiliary layer 32, the suction auxiliary film 30 can maintain an suction area ar3 that ensures adhesion to the fixing device 41 without being affected by the surface shape of the semiconductor wafer 10, such as steps 13. Therefore, by interposing the suction assistant film 30 between the semiconductor wafer 10 and the fixture 41, the occurrence of suction failures caused by the step 13 is suppressed. Therefore, the suction auxiliary film 30 of the present invention is particularly useful in a method for suctioning a semiconductor wafer 10 having a step 13 caused by a trimming process.
[0040] (3) Processing process The processing step is a step for the purpose of thinning the semiconductor wafer 10 by grinding the ground surface 12 of the semiconductor wafer 10. As shown in FIG. 6, in the processing step, a grinding tool 42 is brought into contact with the grinding surface 12 of the semiconductor wafer 10 while the semiconductor wafer 10 is kept in a state of being sucked by the fixture 41 in the above-mentioned suction step. In the processing device 40, the grinding tool 42 is configured to be rotatable about an axis extending in the thickness direction of the semiconductor wafer 10 as the center of rotation, and is also configured to be movable in the thickness direction of the semiconductor wafer 10. In addition, in the processing device 40, the fixing tool 41 is configured to be rotatable about its center as the axis. Then, while the grinding tool 42 and the fixing tool 41 are each rotated, the grinding tool 42 moves to keep the grinding tool 42 in contact with the grinding surface 12, thereby grinding the grinding surface 12 and thinning the semiconductor wafer 10. The present invention can also be used in back grinding of DBG or SDBG. That is, as shown in Fig. 7, in DBG or SDBG, the semiconductor wafer 10 has a plurality of half-cut portions 17 in the case of DBG, or a plurality of modified layers 17 in the case of SDBG, on the non-ground surface 11. In the processing step, the ground surface 12 of the semiconductor wafer 10 is ground to thin it, and the semiconductor wafer 10 is separated into a plurality of chips 10A at each half-cut portion 17 or each modified layer 17 and singulated. EXAMPLES
[0041] The present invention will now be described in detail with reference to examples. [Adsorption support film] The adsorption auxiliary film 30 used was for 12 inches. The adsorption auxiliary film 30 has a structure in which the base layer 31 and the auxiliary layer 32 are as follows.
[0042] (1) Base material layer 31 Material: Polyethylene terephthalate film, E' 31 (25): 4726MPa, E' 31 (35): 4581 MPa. Thickness: 50μm.
[0043] (2) Auxiliary layer 32 Example 1 Material: Ethylene vinyl acetate copolymer (vinyl acetate content: 19%), E' 32 (25): 21MPa, E' 32 (35): 17 MPa. Thickness: 120μm. Example 2 Material: Ethylene vinyl acetate copolymer (vinyl acetate content: 9%), E' 32 (25): 40MPa, E' 32 (35): 34 MPa. Thickness: 120μm. Example 3 Material: Ethylene vinyl acetate copolymer (vinyl acetate content: 9%), E' 32 (25): 40MPa, E' 32 (35): 34 MPa. Thickness: 160μm. Comparative Example 1 The auxiliary layer 32 was not provided.
[0044] [Semiconductor wafers] The following was used as the semiconductor wafer 10 provided with circuits. (1) Specifications Diameter: 300mm. Thickness: 810μm. Material: Silicon. (2) Step 13 The width W was set to 5 mm and the height H to 50 μm, and a trimming process was performed to form a step 13.
[0045] [Back surface processing] (1) Pasting process A tape application machine (manufactured by Nitto Seiki, product number "DR-3000II") was prepared, and an adhesion assist film 30 was applied to the non-ground surface 11 of a semiconductor wafer 10, and the excess portion was cut off to obtain samples of Examples 1 to 3 and Comparative Example 1.
[0046] (2) Adsorption process A processing device (Disco Corp., product number "DGP8760") was prepared, and each of the samples of Examples 1 to 3 and Comparative Example 1 was attached to fixture 41 of the processing device, and the presence or absence of suction failure was observed. In this observation, each sample was adsorbed to the fixture 41 three times, and the number of occurrences of adsorption failure was counted. As a result of the observation, in Examples 1 to 3, no adsorption failure occurred at all. On the other hand, in Comparative Example 1, adsorption failure occurred in all three adsorption attempts. The above results show that the adsorption auxiliary film 30 having the auxiliary layer 32 can prevent poor adsorption.
[0047] (3) Processing process For Examples 1 to 3 in which no suction failure occurred in the suction step (2) above, the back surface was processed using the processing device described above. For this back surface processing, three pieces of each sample were processed on the back surface, and the number of defects such as wafer cracks was measured. As a result, in Examples 1 to 3, no defects such as wafer cracking occurred. The above results show that the auxiliary adhesive film 30 having the auxiliary layer 32 can prevent defects such as wafer cracking during back surface processing. [Industrial Applicability]
[0048] The suction-assisting film of the present invention is widely used in the application of semiconductor component manufacturing. In particular, since it has a property of suitably suppressing suction failure to a fixture in a semiconductor wafer having a step on the outer periphery, it is suitably used for component manufacturing with excellent productivity. [Explanation of symbols]
[0049] 10;semiconductor wafer, 10A;chip, 11: Non-ground surface (surface on which a circuit is formed), 12; grinding surface, 13;Steps, 14; Arc surface, 15;Bump, 17; Half-cut portion or modified layer, 20;Trimming device, 21; Chuck table, 22; trimming blade, 30; Adsorption auxiliary film, 31; base material layer, 32; auxiliary layer, 40; processing equipment; 41; Fixtures; 42;Grinding tools.
Claims
1. An adsorption assistant film that is interposed between a fixture and a semiconductor wafer when a surface of the semiconductor wafer on which a circuit is formed is adsorbed to the fixture, An auxiliary film for use in a case where the semiconductor wafer is a semiconductor wafer having a step on an outer periphery of the surface on which the circuit is formed, thereby reducing an adsorption area of the surface to the fixing tool, a base layer attached to the side on which the circuit is formed; an auxiliary layer that is supported by the base layer and comes into contact with the fixing tool to assist adsorption; The base layer contains one or more materials selected from the group consisting of polyester and polyamide, the auxiliary layer contains one or more elastomers selected from the group consisting of ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, and polyamide-based elastomers; the base layer has a tensile modulus of elasticity that is 20 MPa to 4,850 MPa higher than that of the auxiliary layer at a temperature of 25° C. or higher and 35° C. or lower; The thickness of the auxiliary layer is from 100 μm to 500 μm (excluding 100 μm).
2. The adsorption auxiliary film according to claim 1 , wherein the auxiliary layer has a tensile modulus of elasticity of 5 MPa or more and 150 MPa or less at a temperature of 25° C. or more and 35° C. or less.
3. 3. The adsorption auxiliary film according to claim 1, further comprising an adhesive layer for adhering the base layer to the surface of the semiconductor wafer on which the circuits are formed.
4. 4. The adsorption auxiliary film according to claim 1, wherein the base layer has a tensile modulus of 5000 MPa or less at a temperature of 25° C. or more and 35° C. or less.
5. 5. The adsorption auxiliary film according to claim 1, wherein the thickness of the base layer is from 10 [mu]m to 200 [mu]m.
6. a suction step of interposing an auxiliary suction film between a surface of the semiconductor wafer on which a circuit is formed and a fixture that suctions the semiconductor wafer, and suctioning the semiconductor wafer to the fixture via the auxiliary suction film; the semiconductor wafer has a step on an outer periphery of a surface on which the circuit is formed, thereby reducing an adsorption area of the surface with respect to the fixture, The adsorption auxiliary film is a base layer attached to the surface on which the circuit is formed; an auxiliary layer that is supported by the base layer and comes into contact with the fixing tool to assist adsorption; The base layer contains one or more materials selected from the group consisting of polyester and polyamide, the auxiliary layer contains one or more elastomers selected from the group consisting of ethylene-vinyl acetate copolymers, polyolefin-based elastomers, styrene-based elastomers, polyester-based elastomers, and polyamide-based elastomers; the base layer has a tensile modulus of elasticity that is 20 MPa to 4,850 MPa higher than that of the auxiliary layer at a temperature of 25° C. or higher and 35° C. or lower; A method for adsorbing a semiconductor wafer, wherein the thickness of the auxiliary layer is 100 μm or more and 500 μm or less (excluding 100 μm).
7. 7. The method for adsorbing a semiconductor wafer according to claim 6, wherein the auxiliary layer has a tensile modulus of elasticity of 5 MPa or more and 150 MPa or less at a temperature of 25° C. or more and 35° C. or less.
8. 8. The method for adsorbing a semiconductor wafer according to claim 6, wherein the base layer is a layer having a tensile modulus of elasticity of 5000 MPa or less at a temperature of 25° C. to 35° C.
9. 9. The method for suction mounting a semiconductor wafer according to claim 6, wherein the thickness of the base layer is 10 [mu]m or more and 200 [mu]m or less.
Citation Information
Patent Citations
Semiconductor wafer surface protective tape and resin-made base material film
JP2011151163A
Wafer processing method
JP2012043825A
Substrate processing method
JP2019050357A
Adhesive tape for backgrinding
JP2019161031A
Adhesive tape for semiconductor processing, and semiconductor device manufacturing method