Methods for forming different types of memory devices
The single-IC MRAM integration scheme addresses the challenge of integrating diverse MRAM devices by using uniform free layers and varying MTJ critical dimensions, facilitating cost-effective and efficient fabrication on a single chip.
Patent Information
- Application Number
- JP2023078901
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-08-03
- Filing Date
- 2023-05-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-05-11
AI Technical Summary
Conventional MRAM integration schemes struggle to integrate different types of MRAM devices on a single chip without compromising performance, as they require additional photolithography steps and incur extra costs due to varying free layer thicknesses.
A single-IC MRAM integration scheme that allows simultaneous fabrication of different MRAM devices by using uniform thickness free layers and varying magnetic tunnel junction (MTJ) critical dimensions to meet thermal stability and response time requirements, without substantial performance compromises.
Enables the fabrication of multiple MRAM devices on a single IC with reasonable cost and yield, achieving desired performance characteristics for each type without additional photolithography steps.
Smart Images

Figure 0007569884000001 
Figure 0007569884000002 
Figure 0007569884000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a semiconductor device, and more particularly to a method for manufacturing a semiconductor device. [Background technology]
[0002] The semiconductor integrated circuit (IC) industry has experienced exponential growth. Technological advances in IC materials and designs have already produced several generations of ICs with smaller and more complex circuits than the previous generation. During the evolution of ICs, the functional density (i.e., the number of internal interconnect devices per chip area) has generally increased while the geometric dimensions (i.e., the smallest elements (or wires) that can be formed using a manufacturing process) have decreased. Such a process of scaling down generally provides benefits by increasing production efficiency and reducing associated costs. Such scaling down also increases the complexity of processing and IC manufacturing. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] US Patent Application Publication No. 2020 / 0020375 [Patent Document 2] US Patent Application Publication No. 2020 / 0136027 [Patent Document 3] US Patent Application Publication No. 2021 / 0202574 [Patent Document 4] US Patent Application Publication No. 2022 / 0069199 Summary of the Invention [Problem to be solved by the invention]
[0004] Modern electronic devices include volatile or non-volatile electronic memories for storing data. Volatile memory devices store data when powered, whereas non-volatile memory devices can retain the data they store in the absence of power. Magneto-resistive random-access memory (MRAM) is a promising candidate for the next generation of non-volatile memory technology. MRAM devices may come in a variety of forms to meet various design requirements. The integration and fabrication of different MRAM devices on a single chip can present challenges in different configurations. Thus, while conventional MRAM integration schemes are generally sufficient to achieve the desired objectives, they are not entirely satisfactory in all respects. [Means for solving the problem]
[0005] In some embodiments, the present disclosure provides a semiconductor device comprising: a first conductive feature and a second conductive feature disposed on a first dielectric layer; a buffer layer disposed over the first dielectric layer; a second dielectric layer disposed over the buffer layer; a first bottom through-hole extending through the buffer layer and the second dielectric layer to couple to the first conductive feature along a first direction; a second bottom through-hole extending through the buffer layer and the second dielectric layer to couple to the second conductive feature along the first direction; a first bottom electrode disposed in the first bottom through-hole; a second bottom electrode disposed in the second bottom through-hole; and a first magnetic tunnel junction located above the first bottom electrode. The present invention relates to a semiconductor device comprising a first MTJ stack and a second MTJ stack located above a second bottom electrode, the first MTJ stack and the second MTJ stack having the same thickness along a first direction, the first MTJ stack having a first width along a second direction perpendicular to the first direction, and the second MTJ stack having a second width along the second direction, the second width being greater than the first width. In some embodiments, the present disclosure relates to a semiconductor device comprising a first memory structure and a second memory structure, the first memory structure including a first bottom electrode, a first top electrode located above the first bottom electrode, and a first magnetic tunnel junction (MTJ) stack interposed between the first bottom electrode and the first top electrode along a first direction, the second memory structure including a second bottom electrode, a second top electrode located above the second bottom electrode, and a second MTJ stack interposed between the first bottom electrode and the first top electrode along the first direction, the first MTJ stack having a first width along a second direction perpendicular to the first direction, and the second MTJ stack having a second width along the second direction, the second width being greater than the first width.
[0006] In some embodiments, the present disclosure provides a method comprising receiving a workpiece including a first conductive feature and a second conductive feature disposed in a first dielectric layer, a second dielectric layer located above the first dielectric layer, a first bottom through hole extending through the second dielectric layer to couple to the first conductive feature along a first direction, and a second bottom through hole extending through the second dielectric layer to couple to the second conductive feature along the first direction; depositing a bottom electrode layer over the first bottom through hole, the second bottom through hole, and the second dielectric layer; and forming a magnetic tunnel junction. depositing a memory junction (MTJ) stack above the bottom electrode layer; depositing a top electrode layer above the MTJ stack; depositing a hard mask layer above the top electrode layer; patterning the hard mask layer to form a first hard mask pattern directly above the first bottom through-hole and a second hard mask pattern directly above the second bottom through-hole; and etching the top electrode layer, the MTJ stack, and the bottom electrode layer using the first hard mask pattern and the second hard mask pattern as an etching mask to form a first memory structure directly above the first bottom through-hole and a second memory structure directly above the second bottom through-hole, wherein the first hard mask pattern has a first width along a second direction perpendicular to the first direction, and the second hard mask pattern has a second width along the second direction, the second width being greater than the first width. Effect of the Invention
[0007] The present disclosure provides a single-IC MRAM integration scheme that allows different types of MRAM devices to be fabricated simultaneously on the same IC without substantial performance compromise. [Brief description of the drawings]
[0008] The present disclosure is best understood when considered in conjunction with the following detailed description and the accompanying drawings, in which: It should be noted that, as is standard practice in the industry, various features are not drawn to scale and are for illustrative purposes only, and in fact the dimensions of various features may be arbitrarily increased or decreased for clarity. [Figure 1] 1 is a flowchart illustrating a method for forming a semiconductor structure having different memory structures in accordance with one or more aspects of the present disclosure. [Diagram 2] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Diagram 3] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 4] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Diagram 5] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 6] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 7] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 8] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 9] 1 illustrates a schematic diagram of different memory structures embodied in different regions of a single integrated circuit (IC) device, in accordance with one or more aspects of the present disclosure. [Figure 10] 1 is a flowchart illustrating a method for forming a semiconductor structure having different memory structures in accordance with one or more aspects of the present disclosure. [Figure 11] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 12] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 13] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 14] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 15] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 16] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 17] 2 illustrates a partial cross-sectional view of a workpiece in a manufacturing process according to the method of FIG. 1, in accordance with one or more aspects of the present disclosure. [Figure 18] 1 illustrates a schematic diagram of different memory structures embodied in different regions of a single integrated circuit (IC) device, in accordance with one or more aspects of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The following disclosure provides many different embodiments or examples for implementing different features of the provided objects. In the following, in order to simplify the disclosure, specific examples of elements and arrangements are described. Of course, these are merely examples and are not limiting. For example, in the following description, forming a first feature above or on a second feature may include an embodiment in which the first feature and the second feature are formed to be in direct contact with each other, and may also include an embodiment in which an additional feature may be formed between the first feature and the second feature such that the first feature and the second feature are not in direct contact with each other. It should be noted that the present disclosure may repeat symbols and / or letters in various examples. This repetition is for simplicity and clarity, and does not itself dictate a relationship between the various embodiments and / or arrangements described.
[0010] Also, for ease of description, spatially relative terms such as "below," "below...," "down," "above...," "above" may be used herein to describe the relationship of one element or feature to another element or feature as shown. The spatially relative terms are intended to encompass different orientations other than those depicted in the drawings when the device is in use or operation. Devices may be otherwise oriented (rotated 90 degrees or at other orientations) and similarly the spatially relative descriptors used herein may be interpreted accordingly. It should be noted that when a number or range of numbers is expressed as "about," "approximately," and the like, the term is intended to encompass a reasonable range of numbers, as would be understood by one of ordinary skill in the art, given the inherent variations during manufacturing. For example, a number or range of numbers encompasses a reasonable range, such as within + / - 10% of the number, based on known manufacturing tolerances associated with the manufacture of a feature having a characteristic associated with the number. For example, a material layer having a thickness of "about 5 nm" may encompass a dimensional range of 4.25 nm to 5.75 nm, and one of ordinary skill in the art would know that the manufacturing tolerances associated with a deposited material layer are + / - 15%. It should be noted that the present disclosure may repeat symbols and / or letters in various examples. This repetition is for simplicity and clarity, and does not dictate a relationship between the various embodiments and / or configurations being described.
[0011] A bit unit of a magneto-resistive random-access memory (MRAM) device includes a magnetic tunnel junction (MTJ) stack vertically disposed between two electrodes (typically a bottom electrode and a top electrode). The MTJ stack includes a pinning layer separated from a free layer by a tunnel barrier layer. The magnetic orientation of the pinning layer is static (i.e., constant), and the magnetic orientation of the free layer can be switched between a parallel configuration and an anti-parallel configuration with respect to the magnetic orientation of the pinning layer. The parallel configuration provides a low resistance state for digitally storing data as a first bit value (e.g., logic "0"). The anti-parallel configuration provides a high resistance state for digitally storing data as a second bit value (e.g., logic "1"). Switching between the two configurations provides two magnetic states of the MTJ stack. The magnetic states of the MTJ stack are set by applying a write current of appropriate amplitude and polarity, or read by applying a read current and applying a voltage to a read circuit. Depending on the resistance state of the bitcell, the voltage may be high or low.
[0012] In some embodiments, the bit units of the MRAM are controlled by drive transistors located at the substrate process (front-end-of-line; FEOL) level. The drive transistors include a source feature, a drain feature, an active area between the source feature and the drain feature, and a gate structure located above the active area. When the bit units are located in the front-side interconnect structure above the drive transistors, the top electrode is coupled to a bit line (BL) and the bottom electrode is coupled to one of the drain features of the drive transistors through a series of island metal features and contact vias. A source line (SL) is electrically coupled to the source feature of the drive transistor. The gate structure of the drive transistor is coupled to a word line (WL). When the word line (WL) is selected by applying an enable voltage, the drive transistor is turned on. The bit units are coupled between the bit line (BL) and the source line (SL).
[0013] MRAM devices have various characteristics according to various design requirements. For example, flash-type (refluxed) MRAM has good thermal stability and data stored therein is unlikely to be lost through a reflux (heating) process. Refluxed MRAM may have a response time of less than 100 nano-seconds (ns). RAM-based MRAM has short-term non-volatility and can be read or written quickly with a relatively small current. RAM-based MRAM has a short response time, such as less than 20 ns. Non-volatile MRAM (NvMRAM) devices have characteristics intermediate between refluxed MRAM and RAM-based MRAM. Non-volatile MRAM devices have good memory retention but do not need to operate at relatively high temperatures. NvMRAM may have a response time of less than 50 ns. One-time-programmable (OTP) MRAM devices are designed to be written only once by a write voltage. The write voltage is high enough to irreversibly destroy the dielectric layers in the MTJ stack of the OTP MRAM. Thus, the data stored in the OTP MRAM cannot be changed. Different MRAM devices have different configurations. For example, in some embodiments, a flow-through MRAM may have a thicker free layer to improve thermal stability. A RAM-based MRAM may have a thinner free layer to achieve a faster response. However, forming free layers of different thicknesses on the same substrate may require additional photolithography steps and incur additional costs. There is a need to form different MRAM devices on a single IC with reasonable cost and yield.
[0014] The present disclosure provides a single-IC MRAM integration scheme that allows different types of MRAM devices to be fabricated simultaneously on the same IC without substantial performance compromise. The free layer in each MRAM device of the single-IC MRAM integration scheme is of uniform thickness to allow for reasonable cost of fabrication simultaneously. Different MTJ critical dimensions (CDs) are implemented to meet different thermal stability and response time requirements. Since switching of MRAM devices is current density dependent, implementing MTJ stacks with different critical dimensions can change the current density and thereby change the response time. In some embodiments, the MTJ CD of the flow-through MRAM is larger than the MTJ CD of the NvMRAM, and the MTJ CD of the OTP MRAM is larger than the MTJ CD of the RAM-based MRAM or the NvMRAM. In one single-IC MRAM integration scheme, the flow-through MRAM, the NvMRAM, and the OTP MRAM are integrated in one IC. In another single-IC MRAM integration scheme, the RAM-based MRAM, the OTP MRAM, and the NvMRAM are integrated in one IC.
[0015] Hereinafter, each aspect of the present disclosure will be described in detail with reference to the accompanying drawings. Hereinafter, FIG. 1 is a flow chart showing a method 100 for forming an IC device structure according to an embodiment of the present disclosure. Hereinafter, the method 100 will be described in conjunction with FIG. 2-FIG. 8, which show partial cross-sectional views of a workpiece 200 at different manufacturing stages according to each embodiment of the method 100. FIG. 10 is a flow chart showing a method 500 for forming an IC device structure according to an embodiment of the present disclosure. Hereinafter, the method 500 will be described in conjunction with FIG. 11-FIG. 17, which show partial cross-sectional views of a workpiece 200 at different manufacturing stages according to each embodiment of the method 500. The methods 100 and 500 are merely examples and are not intended to limit the present disclosure to the content clearly shown in the method 100 or 500. Additional steps can be provided before, during, and after the method 100 or the method 500, and some of the above-mentioned steps can be replaced, removed, or shifted for additional embodiments of the method. For simplicity, not all steps are described herein. Because the workpiece 200 is fabricated as a semiconductor structure 200 or a semiconductor device 200 upon completion of the fabrication process, the workpiece 200 may be referred to as a semiconductor structure 200 or a semiconductor device 200, depending on the needs of the context.
[0016] 1 and 2, the method 100 includes a block 102 that receives a workpiece 200. The workpiece 200 includes a substrate 201 and an interconnect structure 203 located above the substrate 201. The method 100 can be performed to form a memory device or storage structure in any of about 5 to 19 metal layers (or metallization layers) of the interconnect structure 203. The interconnect structure 203 can be a backside interconnect structure or a frontside interconnect structure. As described further below, the substrate 201 is formed of a semiconductor material and has undergone front-end-of-line (FEOL) processing. Such FEOL processing can form various transistors to correspond to various functions. For example, these various transistors can form a central processing unit (CPU), a graphics process unit (GPU), and access transistors for a memory device. The transistors can be planar transistors or multi-gate transistors. A multi-gate device generally refers to a device or portion thereof having a gate structure disposed over multiple sides of a channel region. Fin-like field effect transistors (FinFETs) and multi-bridge-channel (MBC) transistors are examples of multi-gate devices, which have become popular and promising candidates for high efficiency and low leakage applications. FinFETs have a raised channel surrounded by gates on multiple sides (e.g., the gate surrounds the top and sidewalls of a "fin" of semiconductor material extending from a substrate). MBC transistors have a gate structure that extends to surround some or all of the channel region, providing access to the channel region on both sides or more. Because the gate structure surrounds the channel region, MBC transistors may also be referred to as surrounding gate transistors (SGTs) or gate-all-around (GAA) transistors.Because the channel region of an MBC transistor can be formed of a nanowire, nanosheet, or other nanostructure, the MBC transistor may also be referred to as a nanowire transistor or a nanosheet transistor.
[0017] In some embodiments, substrate 201 comprises silicon (Si). Alternatively or additionally, substrate 201 comprises another elemental semiconductor such as germanium (Ge), a compound semiconductor such as silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide and / or indium antimonide, an alloy semiconductor such as silicon germanium (SiGe), GaAsP, AlInAs, AlGaAs, GaInAs, GaInP and / or GaInAsP, or a combination thereof. In some embodiments, substrate 201 comprises one or more group III-V materials, one or more group II-IV materials, or a combination thereof. In some embodiments, the substrate 201 is a semiconductor-on-insulator substrate, such as a silicon-on-insulator (SOI) substrate, a silicon germanium-on-insulator (SGOI) substrate, or a germanium-on-insulator (GeOI) substrate. The semiconductor-on-insulator substrate may be fabricated by separation by implantation of oxygen (SIMOX), wafer bonding, and / or other suitable methods. Because the method 100 is performed on a workpiece 200 that has undergone FEOL processing on the substrate 201, the substrate 201 is shown in FIG. 2 with only dashed lines and is omitted in FIGS. 3-8.
[0018] The interconnect structure 203 includes several metal layers, but the memory device / storage structure can be formed in any of the metal layers, such as the fourth metal layer (M4), the fifth metal layer (M5), or the sixth metal layer (M6). The interconnect structure 203 can be a front-side interconnect structure or a back-side interconnect structure, so that the memory device / storage structure of the present disclosure can be formed in the fourth front metal layer, the fifth front metal layer, the sixth front metal layer, the fourth back metal layer, the fifth back metal layer, or the sixth back metal layer. With reference to FIG. 2, the conductive features 204 in the first dielectric layer 202 represent the metal layers below the memory device. The first dielectric layer 202 may include, for example, tetraethyl orthosilicate (TEOS) oxide material, undoped or doped silicon silicate glass (BPSG), borophosphosilicate glass (FSG), fused silica glass (FSG), phosphosilicate glass (PSG), boron doped silicon glass (BSG), and / or other suitable dielectric materials. The conductive feature 204 may be a metal line and may include ruthenium (Ru), copper (Cu), nickel (Ni), cobalt (Co), or tungsten (W). In one embodiment, the conductive feature 204 includes copper (Cu). The conductive feature 204 may include a metal line or a contact via.
[0019] Still referring to FIG. 2, the workpiece 200 includes a first region 10, a second region 20, a third region 30, and a fourth region 40. These regions may be adjacent to each other or spaced apart from each other. These different regions may have different configurations for memory devices. In some embodiments, the first region 10 may be a region for forming RAM-based MRAM, the second region 20 may be a region for forming NvMRAM, the third region 30 may be a region for forming OTP MRAM, and the fourth region 40 may be a region that does not include any MRAM structure.
[0020] 1 and 2, the method 100 includes a block 104 of depositing a buffer layer 206 and a second dielectric layer 208 above the workpiece 200. The buffer layer 206 may include silicon carbide (SiC) or silicon oxycarbide (SiOC) to inhibit electromigration of the conductive features 204. The second dielectric layer 208 may include silicon oxide. In one embodiment, the second dielectric layer 208 may include silicon-rich oxide (SRO) and is different from the first dielectric layer 202. As used herein, the silicon content in silicon-rich oxide is less than the stoichiometric ratio of silicon in silicon dioxide. In an embodiment of the present disclosure, the silicon content in the first dielectric layer 202 is greater than the silicon content in the second dielectric layer 208. The buffer layer 206 may be deposited using chemical vapor deposition (CVD). The second dielectric layer 208 may be deposited using a low-pressure CVD (LPCVD) or CVD method.
[0021] 1 and 2, the method 100 includes a block 106 of forming a first bottom through-hole 210-1, a second bottom through-hole 210-2, and a third bottom through-hole 210-3 above the first region 10, the second region 20, and the third region 30, respectively. Although not explicitly shown in FIG. 2, the operation of block 106 may include forming a through-hole opening to expose the conductive feature 204, and forming the first bottom through-hole 210-1, the second bottom through-hole 210-2, and the third bottom through-hole 210-3 in the through-hole opening. Forming the through-hole opening includes a combination of a photolithography process and an etching process. In the illustrative process, a hard mask layer is deposited above the second dielectric layer 208. A photoresist layer is deposited above the hard mask layer. The photoresist layer is then exposed to patterned radiation transmitted through or reflected from a photomask, baked in a post-exposure bake process, developed in a developer solution, and then washed to form a patterned photoresist layer. The hardmask layer is then etched using the patterned photoresist layer as an etch mask to form a patterned hardmask layer. The second dielectric layer 208 and the buffer layer 206 are then etched using the patterned hardmask layer as an etch mask. Etching the second dielectric layer 208 and the buffer layer 206 may include a dry etching process using argon (Ar), a fluorine-containing etchant (e.g., SF6, NF3, CH2F2, CHF3, C4F8 and / or C2F6), an oxygen-containing etchant, a chlorine-containing etchant (e.g., Cl2, CHCl3, CCl4 and / or BCl3), a bromine-containing etchant (e.g., HBr and / or CHBr3), an iodine-containing etchant, or a combination thereof.
[0022] After forming the through-hole openings, a metal fill layer is deposited over the workpiece 200 to fill the through-hole openings. The metal fill layer may include titanium nitride (TiN), ruthenium (Ru), copper (Cu), nickel (Ni), cobalt (Co), or tungsten (W). In one embodiment, the metal fill layer may include titanium nitride (TiN). The metal fill layer may be deposited using physical vapor deposition (PVD), CVD, electroless plating, electrolytic plating, or any other suitable method. After depositing the metal fill layer, the workpiece 200 is planarized to remove excess metal fill layer in a chemical mechanical polishing (CMP) process to expose the second dielectric layer 208. At this time, a first bottom through-hole 210-1 is formed in the first region 10 to electrically and physically couple to the conductive feature 204 in the first region 10, a second bottom through-hole 210-2 is formed in the second region 20 to electrically and physically couple to the conductive feature 204 in the second region 20, and a third bottom through-hole 210-3 is formed in the third region 30 to electrically and physically couple to the conductive feature 204 in the third region 30. It should be noted that no bottom through-hole is formed above the fourth region 40.
[0023] 1 and 2, the method 100 includes a block 108 that deposits a bottom electrode layer 212 above the workpiece 200 and above the second dielectric layer 208, the first bottom through hole 210-1, the second bottom through hole 210-2, and the third bottom through hole 210-3. The bottom electrode layer 212 may be a single layer or a multilayer. If the bottom electrode layer 212 is a single layer, it may include titanium nitride (TiN) or tantalum nitride (TaN). If the bottom electrode layer 212 is a multilayer, it may include a tantalum nitride (TaN) layer and a titanium nitride (TiN) layer. The bottom electrode layer 212 may be deposited using a PVD method or a CVD method. Depositing the entire bottom electrode layer 212 above the workpiece 200 includes depositing it above the first bottom through hole 210-1, the second bottom through hole 210-2, the third bottom through hole 210-3, and the top surface of the second dielectric layer 208.
[0024] 1 and 2, the method 100 includes a block 110 of depositing a magnetic tunnel junction (MTJ) stack 1000 above a bottom electrode layer 212. The first MTJ stack 1000 includes a pinning layer 214 located above the bottom electrode layer 212, a tunnel barrier layer 216 located above the pinning layer 214, a free layer 218 located above the tunnel barrier layer 216, a maintenance layer 220 located above the free layer 218, and a cover layer 222 disposed above the maintenance layer 220. The pinning layer 214 may include a ferromagnetic material such as cobalt iron (CoFe), cobalt iron boron (CoFeB), or a cobalt platinum (Co-Pt) alloy. In some alternative embodiments, the pinning layer 214 may include CoFeTa, NiFe, Co, CoFe, CoPt, an alloy of Ni, Co, and Fe, platinum manganese (PtMn), iridium manganese (IrMn), rhodium manganese (RhMn), iron manganese (FeMn), or OsMn. The tunnel barrier layer 216 may be formed of a metal oxide selected from the group consisting of magnesium oxide (MgO), titanium oxide (TiO), aluminum titanium oxide (AlTiO), magnesium zinc oxide (MgZnO), aluminum oxide (AlO), zinc oxide (ZnO), zirconium oxide (ZrO), hafnium oxide (HfO), or magnesium tantalum oxide (MgTaO). In one embodiment, the tunnel barrier layer 216 is formed of manganese oxide. The free layer 218 is formed of a ferromagnetic material and may include cobalt iron boron (CoFeB). The maintenance layer 220 may be formed of a metal oxide selected from the group consisting of magnesium oxide (MgO), titanium oxide (TiO), aluminum titanium oxide (AlTiO), magnesium zinc oxide (MgZnO), aluminum oxide (AlO), zinc oxide (ZnO), zirconium oxide (ZrO), hafnium oxide (HfO), or magnesium tantalum oxide (MgTaO). In one embodiment, the maintenance layer 220 may include manganese oxide. The cover layer 222 is optional and may include molybdenum (Mo) or ruthenium (Ru).The pinning layer 214, the tunnel barrier layer 216, the free layer 218, the maintenance layer 220, and the cover layer 222 may each be deposited by a PVD method, a CVD method, a plating method, an electroless plating method, or other suitable method. In some embodiments not explicitly shown in the figures, the cover layer 222 may be omitted, and the first MTJ stack 1000 may include only the pinning layer 214, the tunnel barrier layer 216, the maintenance layer 220, and the free layer 218. The second MTJ stack 2000 is described below in conjunction with the alternative method 500. The second MTJ stack 2000 has a stacking order that is reversed from that of the first MTJ stack 1000. It should be understood that the method 100 can also be used to implement the second MTJ stack 2000 instead of the first MTJ stack 1000.
[0025] 1 and 2, the method 100 includes block 112 of depositing a top electrode layer 224 above the first MTJ stack 1000. The top electrode layer 224 may be a single layer or a multilayer. If the top electrode layer 224 is a single layer, it may include titanium nitride (TiN) or tantalum nitride (TaN). If the top electrode layer 224 is a multilayer, it may include a tantalum nitride layer and a titanium nitride layer. The top electrode layer 224 may be deposited using a PVD method or a CVD method. Depositing the entire top electrode layer 224 above the workpiece 200 includes depositing it above the first MTJ stack 1000.
[0026] 1, 2 and 3, the method 100 includes a block 114 of patterning the top electrode layer 224, the first MTJ stack 1000 and the bottom electrode layer 212 to form a first storage portion 250 above the first region 10, a second storage portion 255 above the second region 20, and a third storage portion 260 above the third region 30. In the block 114, a photolithography process and an etching process are performed to form the first storage portion 250, the second storage portion 255, and the third storage portion 260. In an example process, depositing the hard mask layer 226 above the workpiece 200 includes depositing the hard mask layer 226 above the top electrode layer 224. In some embodiments, the hard mask layer 226 may include silicon oxide, silicon nitride, or a combination thereof. In one embodiment, the hard mask layer 226 is formed of silicon oxide (e.g., tetraethylorthosilicate (TEOS) oxide) and may be deposited using spin-coating or flowable CVD (FCVD). Then, a photoresist layer is deposited above the hard mask layer 226. Then, the photoresist layer is exposed to patterned radiation transmitted through or reflected from a photomask, baked in a post-exposure bake process, developed in a developer solution, and then washed to form a patterned photoresist layer. Then, as shown in FIG. 2, the hard mask layer 226 is etched using the patterned photoresist layer as an etching mask to form a first hard mask pattern 226-1 above the first region 10, a second hard mask pattern 226-2 above the second region 20, and a third hard mask pattern 226-3 above the third region 30. These patterned hard mask patterns are then used as an etching mask to etch the top electrode layer 224, the first MTJ stack 1000, the bottom electrode layer 212, and the second dielectric layer 208. The etching in block 114 may include ion beam etching (IBE) 300.For patterning the MTJ stack, IBE is preferred over reactive ion etching (RIE) because it is less likely to introduce chemical impurities into the MTJ stack, which would degrade the performance of the storage section. IBE 300 can use one or more inert gas ions, such as Ar, Kr, Xe, and Ne, generated with RF or DC power. It should be understood that IBE typically involves rotation of the workpiece 200.
[0027] In order to form memory devices with different device characteristics, the storage portions have different dimensions. It has been observed that, given the same MTJ stack, a storage portion with a large free layer exhibits better thermal stability than a storage portion with a small free layer. Also, a storage portion with a small free layer provides a shorter response time than a storage portion with a large free layer. In some embodiments where the storage portion has a circular shape when viewed along the vertical direction, the critical dimension (CD) of the storage portion can refer to the diameter of the free layer. In some embodiments shown in FIG. 2, hard mask patterns with different dimensions are implemented to achieve different storage portion diameters (or dimensions). As shown in FIG. 2, the first hard mask pattern 226-1 has a first dimension d1, the second hard mask pattern 226-2 has a second dimension d2, and the third hard mask pattern 226-3 has a third dimension d3. The first dimension d1 may be similar to the second dimension d2. The third dimension d3 is larger than either the first dimension d1 or the second dimension d2.
[0028] 3, the IBE 300 can form pyramidal sidewalls such that each of the first storage portion 250, the second storage portion 255, and the third storage portion 260 has a small top electrode dimension and a large bottom member dimension. The first storage portion 250 includes a first top electrode 224-1 formed from the top electrode layer 224. The second storage portion 255 includes a second top electrode 224-2 formed from the top electrode layer 224. The third storage portion 260 includes a third top electrode 224-3 formed from the top electrode layer 224. In some embodiments, the first storage portion 250 can be characterized by a first MTJ dimension D1, which can be substantially similar to a dimension (or diameter) of the free layer 218 in the first storage portion 250. The second storage portion 255 can be characterized by a second MTJ dimension D2, which can be substantially similar to the dimension (or diameter) of the free layer 218 in the second storage portion 255. The third storage portion 260 can be characterized by a third MTJ dimension D3, which can be substantially similar to the dimension (or diameter) of the free layer 218 in the third storage portion 260. In some embodiments, the first MTJ dimension D1 can be similar to the second MTJ dimension D2. The third MTJ dimension D3 can be larger than either the first MTJ dimension D1 or the second MTJ dimension D2. In some cases, the first MTJ dimension D1 may be between about 20 nm and about 50 nm, the second MTJ dimension D2 may be between about 20 nm and about 55 nm, and the third MTJ dimension D3 may be between about 60 nm and about 85 nm.
[0029] 1, 4, 5 and 6, the method 100 includes a block 116 of forming a passivation structure above the first storage portion 250, the second storage portion 255, and the third storage portion 260. The passivation structure may include a spacer layer 228 disposed along a sidewall of the storage portion, an etch stop layer (ESL) 230 located above the spacer layer 228, and a third dielectric layer 232 located above the ESL 230. Although not explicitly shown in the figures, the operations in block 116 may include blanket depositing the spacer layer 228, etching back the spacer layer 228 to remove the spacer layer 228 (shown in FIG. 4) located on a top-facing surface, depositing the ESL 230 above the spacer layer 228, and depositing the third dielectric layer 232. In some embodiments, the spacer layer 228 may include silicon nitride, silicon oxide, or a suitable material and may be deposited using a CVD or ALD process. In one embodiment, the spacer layer 228 may include silicon nitride. The ESL 230 may include aluminum oxide or a metal oxide that is more etch resistant than the spacer layer 228. The ESL 230 may be deposited using a CVD or ALD process. The third dielectric layer 232 may include a doped silicon silicate, such as tetraethylorthosilicate (TEOS) oxide material, undoped or borophosphosilicate glass (BPSG), fused silica glass (FSG), phosphosilicate glass (PSG), boron doped silicon glass (BSG), and / or other suitable dielectric materials. In some cases, the third dielectric layer 232 may be deposited using a spin-coating or FCVD process. As shown in FIG. 6, the spacer layer 228 is in physical contact with the second dielectric layer 208 located above the first region 10, the second region 20, and the third region 30, the sidewalls of the bottom electrode 212, the pinning layer 214, the tunnel barrier layer 216, the free layer 218, the maintenance layer 220, and the cover layer 222 of the storage section.5, the ESL 230 is not formed above the fourth region 40 because the presence of the ESL 230 above the fourth region 40 would prevent a good electrical connection with the conductive feature 204 in the fourth region 40.
[0030] 1, 7 and 8, the method 100 includes a block 118 for performing other processes. Such other processes may include forming a first contact opening 235-1, a second contact opening 235-2, a third contact opening 235-3, a fourth contact opening 235-4, and a fifth contact opening 235-5 (shown in FIG. 7) and depositing a metal fill layer in the contact openings to form other contact features (shown in FIG. 8). Photolithography and etching processes can be used to form the contact openings. In an example process, the fifth contact opening 235-5 is formed above the fourth region 40, and the first region 10, the second region 20, and the third region 30 are protected by a patterned film, such as a photoresist layer, a bottom antireflective coating (BARC) layer, etc. After removing the patterned film, photolithography and etching processes are used to form a first contact opening 235-1, a second contact opening 235-2, a third contact opening 235-3, and a fifth contact opening 235-5 through the third dielectric layer 232, the ESL 230, the second dielectric layer 208, and the buffer layer 206, as shown in FIG. 7. The conductive feature 204 in the fourth region 40 is exposed to the fourth contact opening 235-4. The first contact opening 235-1 is exposed to the first top electrode 224-1. The second contact opening 235-2 is exposed to the second top electrode 224-2. The third contact opening 235-3 is exposed to the third top electrode 224-3. Because there is no storage portion in the fourth region 40, the fourth contact opening 235-4 and the fifth contact opening 235-5 together form a through opening in the fourth region 40.The etching in block 118 may include a dry etching process using argon (Ar), a fluorine-containing etchant (e.g., SF6, NF3, CH2F2, CHF3, C4F8, and / or C2F6), an oxygen-containing etchant, a chlorine-containing etchant (e.g., Cl2, CHCl3, CCl4, and / or BCl3), a bromine-containing etchant (e.g., HBr and / or CHBr3), an iodine-containing etchant, or a combination thereof.
[0031] 8, a metal fill layer is then deposited above the contact opening using a PVD method, a CVD method, an electroplating method, or an electroless plating method. The metal fill layer may include ruthenium (Ru), copper (Cu), nickel (Ni), cobalt (Co), or tungsten (W). In one embodiment, the metal fill layer may include copper (Cu). After depositing the metal fill layer, a planarization process, such as a CMP process, is performed to remove excess metal fill layer located above the third dielectric layer 232. After the CMP process, a first top contact via 236-1 is formed above the first storage portion 250 for electrical coupling to the first top electrode 224-1, a second top contact via 236-2 is formed above the second storage portion 255 for electrical coupling to the second top electrode 224-2, a third top contact via 236-3 is formed above the third storage portion 260 for electrical coupling to the third top electrode 224-3, and a fourth top contact via 236-4 is formed extending through the third dielectric layer 232, the second dielectric layer 208, and the buffer layer 206 for coupling to the conductive feature 204 in the fourth region 40. Although not explicitly shown, a barrier layer may be deposited above the contact opening before depositing the metal fill layer. The barrier layer may include titanium nitride (TiN) or tantalum nitride (TaN). 8. The method 100 may also continue to form other metal layers above the workpiece 200 shown in FIG.
[0032] 9 is a schematic plan view of a first integrated circuit (IC) chip 400 including a processor region 402, a RAM-based MRAM region 404, an NvMRAM region 406, and an OTP MRAM region 408. The processor region 402 may include core transistors at a FEOL level to form a central processing unit (CPU). The RAM-based MRAM region 404 may correspond to the first region 10 and may include a first storage portion 250 at a BEOL level. The NvMRAM region 406 may correspond to the second region and may include a second storage portion 255 at a BEOL level. The OTP MRAM region 408 may correspond to the third region 30 and may include a third storage portion 260 at a BEOL level. As described above, the storage portions in the RAM-based MRAM region 404, the NvMRAM region 406, and the OTP MRAM region 408 may include the same first MTJ stack 1000 and may be formed simultaneously. The first IC chip 400 has a short response time and is therefore applicable to artificial intelligence (AI). Thermal stability of MRAM is of less interest for AI applications. Due to the short response time required in the first IC chip 400, the free layer 218 in the first MTJ stack 1000 may be located on the thin side of the spectrum. In some cases, the free layer 218 in the first MTJ stack 1000 may be between about 1.5 nm and about 3.0 nm.
[0033] As described above, the method 100 can be performed to form the first storage portion 250, the second storage portion 255, and the third storage portion 260 above the first region 10, the second region 20, and the third region 30 of the workpiece 200. Each of the first storage portion 250, the second storage portion 255, and the third storage portion 260 is formed from the same first MTJ stack 1000. The present disclosure further provides a method 500 for forming the fourth storage portion 265, the second storage portion 255, and the third storage portion 260 above the fifth region 50, the second region 20, and the third region 30 of the workpiece 200. Each of the fourth storage portion 265, the second storage portion 255, and the third storage portion 260 is formed from the same second MTJ stack 2000, which is different from the first MTJ stack 1000. Method 500 will now be described with reference to the partial cross-sectional views of workpiece 200 in Figures 11 to 17. Methods 500 and 100 may share similar operations, and descriptions of overlapping features may be intentionally omitted or reduced for the sake of brevity.
[0034] 10 and 11, a method 500 includes a block 502 of receiving a workpiece 200. The operations in block 502 are similar to those in block 102. Therefore, a detailed description of the operations in block 502 is omitted.
[0035] 10 and 11, the method 500 includes a block 504 of depositing a buffer layer 206 and a second dielectric layer 208 above the workpiece 200. The operation in block 504 is similar to the operation in block 104. Therefore, a detailed description of the operation in block 504 is omitted.
[0036] 10 and 11, the method 500 includes a block 506 in which a fourth bottom through-hole 210-4, a second bottom through-hole 210-2, and a third bottom through-hole 210-3 are formed above the fifth region 50, the second region 20, and the third region 30, respectively. The operation in block 506 is similar to the operation in block 106. Therefore, a detailed description of the operation in block 506 is omitted. It should be noted that the workpiece 200 related to the method 500 includes a fifth region 50, not the first region 10. This nomenclature is adopted to indicate that a different storage portion, a fourth storage portion 265, is formed above the fifth region 50. Similarly, the fourth bottom through hole 210-4 is used to indicate an association with the fourth storage portion 265, whether the fourth bottom through hole 210-4 shares the same dimensions as the first bottom through hole 210-1, the second bottom through hole 210-2, or the third bottom through hole 210-3.
[0037] 10 and 11, the method 500 includes a block 508 of depositing a bottom electrode layer 212 above the workpiece 200, so as to deposit the bottom electrode layer 212 above the second dielectric layer 208, the fourth bottom through-hole 210-4, the second bottom through-hole 210-2, and the third bottom through-hole 210-3. The operation in block 508 is similar to the operation in block 108. Therefore, a detailed description of the operation in block 508 is omitted.
[0038] 10 and 11, the method 500 includes a block 510 of depositing a second magnetic tunnel junction (MTJ) stack 2000 above the bottom electrode layer 212. The second MTJ stack 2000 has a stacking order that is reverse to that of the first MTJ stack 1000. As shown in FIG. 11, the second MTJ stack 2000 includes a cover layer 222 located above the bottom electrode layer 212, a maintenance layer 220 located above the cover layer 222, a free layer 218 located above the maintenance layer 220, a tunnel barrier layer 216 located above the free layer 218, and a pinning layer 214 located above the tunnel barrier layer 216. The pinning layer 214 may include a ferromagnetic material such as cobalt iron (CoFe), cobalt iron boron (CoFeB), or a cobalt platinum (Co-Pt) alloy. In some alternative embodiments, the pinning layer 214 may include CoFeTa, NiFe, Co, CoFe, CoPt, an alloy of Ni, Co, and Fe, platinum manganese (PtMn), iridium manganese (IrMn), rhodium manganese (RhMn), iron manganese (FeMn), or OsMn. The tunnel barrier layer 216 may be formed of a metal oxide selected from the group consisting of magnesium oxide (MgO), titanium oxide (TiO), aluminum titanium oxide (AlTiO), magnesium zinc oxide (MgZnO), aluminum oxide (AlO), zinc oxide (ZnO), zirconium oxide (ZrO), hafnium oxide (HfO), or magnesium tantalum oxide (MgTaO). In one embodiment, the tunnel barrier layer 216 is formed of manganese oxide. The free layer 218 is formed of a ferromagnetic material and may include cobalt iron boron (CoFeB). The maintenance layer 220 may be formed of a metal oxide selected from the group consisting of magnesium oxide (MgO), titanium oxide (TiO), aluminum titanium oxide (AlTiO), magnesium zinc oxide (MgZnO), aluminum oxide (AlO), zinc oxide (ZnO), zirconium oxide (ZrO), hafnium oxide (HfO), or magnesium tantalum oxide (MgTaO). In one embodiment, the maintenance layer 220 may include manganese oxide.The cover layer 222 may be optional and may include molybdenum (Mo) or ruthenium (Ru). Each of the pinning layer 214, the tunnel barrier layer 216, the free layer 218, the maintenance layer 220, and the cover layer 222 may be deposited by PVD, CVD, plating, electroless plating, or other suitable methods. In some embodiments not explicitly shown in the figures, the cover layer 222 may be omitted, and the second MTJ stack 2000 may include only the pinning layer 214, the tunnel barrier layer 216, the maintenance layer 220, and the free layer 218.
[0039] 10 and 11, the method 500 includes a block 512 of depositing a top electrode layer 224 above the second MTJ stack 2000. The operation in block 512 is similar to the operation in block 112. Therefore, a detailed description of the operation in block 512 is omitted.
[0040] 10, 11 and 12, the method 500 includes a block 514 of patterning the top electrode layer 224, the second MTJ stack 2000, and the bottom electrode layer 212 to form a fourth storage portion 265 above the fifth region 50, a second storage portion 255 above the second region 20, and a third storage portion 260 above the third region 30. In the block 514, a photolithography process and an etching process are performed to form the fourth storage portion 265, the second storage portion 255, and the third storage portion 260. In an example process, depositing the hard mask layer 226 above the workpiece 200 includes depositing the hard mask layer 226 above the top electrode layer 224. In some embodiments, the hard mask layer 226 may include silicon oxide, silicon nitride, or a combination thereof. In one embodiment, the hard mask layer 226 is formed of silicon oxide (e.g., tetraethylorthosilicate (TEOS) oxide) and may be deposited using spin-coating or flowable CVD (FCVD). Then, a photoresist layer is deposited on the hard mask layer 226. Then, the photoresist layer is exposed to patterned radiation transmitted through or reflected from a photomask, baked in a post-exposure bake process, developed in a developer solution, and then washed to form a patterned photoresist layer. Then, as shown in FIG. 11, the hard mask layer 226 is etched using the patterned photoresist layer as an etching mask to form a fourth hard mask pattern 226-4 above the first region 10, a second hard mask pattern 226-2 above the second region 20, and a third hard mask pattern 226-3 above the third region 30. These patterned hard mask patterns are then used as an etching mask to etch the top electrode layer 224, the second MTJ stack 2000, the bottom electrode layer 212, and the second dielectric layer 208.The etching in block 514 may include ion beam etching (IBE) 300. For patterning the MTJ stack, IBE is preferred over reactive ion etching (RIE) because it is less likely to introduce chemical impurities into the MTJ stack, which would degrade the performance of the storage portion. IBE 300 may use one or more inert gas ions, such as Ar, Kr, Xe, and Ne, generated by RF or DC power. It should be understood that IBE typically involves rotation of the workpiece 200.
[0041] In order to form memory devices with different device properties, the storage portions have different dimensions. It has been observed that, given the same MTJ stack, a storage portion with a large free layer exhibits better thermal stability than a storage portion with a small free layer. Also, a storage portion with a small free layer provides a shorter response time than a storage portion with a large free layer. In some embodiments where the storage portion has a circular shape when viewed along the vertical direction, the critical dimension (CD) of the storage portion can refer to the diameter of the free layer. In some embodiments shown in FIG. 11, hard mask patterns with different dimensions are implemented to achieve different storage portion diameters (or dimensions). As shown in FIG. 11, the fourth hard mask pattern 226-4 has a fourth dimension d4, the second hard mask pattern 226-2 has a second dimension d2, and the third hard mask pattern 226-3 has a third dimension d3. The fourth dimension d4 is greater than the second dimension d2 or the third dimension d3. The third dimension d3 is greater than the second dimension d2.
[0042] 12, the IBE 300 can form pyramidal sidewalls such that the fourth storage portion 265, the second storage portion 255, and the third storage portion 260 each have a small top electrode dimension and a large bottom member dimension. The fourth storage portion 265 includes a fourth top electrode 224-4 formed from the top electrode layer 224. The second storage portion 255 includes a second top electrode 224-2 formed from the top electrode layer 224. The third storage portion 260 includes a third top electrode 224-3 formed from the top electrode layer 224. In some embodiments, the fourth storage portion 265 can be characterized by a fourth MTJ dimension D4, which can be substantially similar to a dimension (or diameter) of the free layer 218 in the fourth storage portion 265. The second storage portion 255 can be characterized by a second MTJ dimension D2, which can be substantially similar to the dimension (or diameter) of the free layer 218 in the second storage portion 255. The third storage portion 260 can be characterized by a third MTJ dimension D3, which can be substantially similar to the dimension (or diameter) of the free layer 218 in the third storage portion 260. In some embodiments, the fourth MTJ dimension D4 is larger than the second MTJ dimension D2 or the third MTJ dimension D3. The third MTJ dimension D3 can be larger than the second MTJ dimension D2. In some cases, the fourth MTJ dimension D4 may be between about 75 nm and about 100 nm, the second MTJ dimension D2 may be between about 20 nm and about 55 nm, and the third MTJ dimension D3 may be between about 60 nm and about 85 nm.
[0043] 10, 13, 14, and 15, the method 500 includes a block 516 of forming a passivation structure above the fourth storage portion 265, the second storage portion 255, and the third storage portion 260. The passivation structure may include a spacer layer 228 disposed along a sidewall of the storage portion, an etch stop layer (ESL) 230 located above the spacer layer 228, and a third dielectric layer 232 located above the ESL 230. Although not explicitly shown in the figures, the operations in block 516 may include blanket depositing the spacer layer 228, etching back the spacer layer 228 to remove the spacer layer 228 located on the top-facing surface (shown in FIG. 13), depositing the ESL 230 above the spacer layer 228 (shown in FIG. 14), and depositing the third dielectric layer 232 (shown in FIG. 15). In some embodiments, the spacer layer 228 may include silicon nitride, silicon oxide, or a suitable material and may be deposited using a CVD or ALD process. In one embodiment, the spacer layer 228 may include titanium nitride. The ESL 230 may include aluminum oxide or a metal oxide that is more etch resistant than the spacer layer 228. The ESL 230 may be deposited using a CVD or ALD process. The third dielectric layer 232 may include, for example, a tetraethylorthosilicate (TEOS) oxide material, undoped silicate glass or borophosphosilicate glass (BPSG), fused silica glass (FSG), phosphosilicate glass (PSG), boron doped silicon glass (BSG), and / or doped silicon silicate of other suitable dielectric materials. In some cases, the third dielectric layer 232 may be deposited using a spin-coating or FCVD process.15, the spacer layer 228 is in physical contact with the second dielectric layer 208, the sidewall of the bottom electrode 212, the pinning layer 214, the tunnel barrier layer 216, the free layer 218, the maintenance layer 220, and the cover layer 222 of the storage section, which are located above the fourth region 40, the second region 20, and the third region 30. The ESL 230 is in physical contact with the second dielectric layer 208, the spacer layer 228, and the top electrode. In some embodiments shown in FIG. 14, the ESL 230 is not formed above the fourth region 40 because the presence of the ESL 230 above the fourth region 40 would prevent a good electrical connection with the conductive feature 204 in the fourth region 40.
[0044] 10, 16, and 17, the method 500 includes a block 518 for performing other processes. Such other processes may include forming the sixth contact opening 235-6, the second contact opening 235-2, the third contact opening 235-3, the fourth contact opening 235-4, and the fifth contact opening 235-5 (shown in FIG. 16) and depositing a metal fill layer in the contact openings to form other contact features (shown in FIG. 17). Photolithography and etching processes can be used to form the contact openings. In an example process, the fifth contact opening 235-5 is formed above the fourth region 40, and the fifth region 50, the second region 20, and the third region 30 are protected by a patterned film, such as a photoresist layer, a bottom antireflective coating (BARC) layer, or the like. After removing the patterned film, photolithography and etching processes are used to penetrate the third dielectric layer 232, the ESL 230, the second dielectric layer 208, and the buffer layer 206 to form a sixth contact opening 235-6, a second contact opening 235-2, a third contact opening 235-3, and a fifth contact opening 235-5, as shown in FIG. 16. The conductive feature 204 in the fourth region 40 is exposed to the fourth contact opening 235-4. The sixth contact opening 235-6 is exposed to the fourth top electrode 224-4. The second contact opening 235-2 is exposed to the second top electrode 224-2. The third contact opening 235-3 is exposed to the third top electrode 224-3. Because there is no storage portion in the fourth region 40, the fourth contact opening 235-4 and the fifth contact opening 235-5 together form a through opening in the fourth region 40.The etching in block 518 may include a dry etching process using argon (Ar), a fluorine-containing etchant (e.g., SF6, NF3, CH2F2, CHF3, C4F8, and / or C2F6), an oxygen-containing etchant, a chlorine-containing etchant (e.g., Cl2, CHCl3, CCl4, and / or BCl3), a bromine-containing etchant (e.g., HBr and / or CHBr3), an iodine-containing etchant, or a combination thereof.
[0045] 17, a metal fill layer is then deposited above the contact opening using a PVD method, a CVD method, an electroplating method, or an electroless plating method. The metal fill layer may include ruthenium (Ru), copper (Cu), nickel (Ni), cobalt (Co), or tungsten (W). In one embodiment, the metal fill layer includes copper (Cu). After depositing the metal fill layer, a planarization process, such as a CMP process, is performed to remove excess metal fill layer located above the third dielectric layer 232. After the CMP process, a fifth top contact via 236-5 is formed above the fourth storage portion 265 for electrical coupling to the fourth top electrode 224-4, a second top contact via 236-2 is formed above the second storage portion 255 for electrical coupling to the second top electrode 224-2, a third top contact via 236-3 is formed above the third storage portion 260 for electrical coupling to the third top electrode 224-3, and a fourth top contact via 236-4 is formed extending through the third dielectric layer 232, the second dielectric layer 208, and the buffer layer 206 for coupling to the conductive feature 204 in the fourth region 40. Although not explicitly shown, a barrier layer may be deposited above the contact opening before depositing the metal fill layer. The barrier layer may include titanium nitride (TiN) or tantalum nitride (TaN). 17. Additionally, the method 500 may continue to form other metal layers above the workpiece 200 as shown in FIG.
[0046] FIG. 18 is a schematic plan view of a second integrated circuit (IC) chip 600 including a processor region 602, a free-flow MRAM region 610, an NvMRAM region 606, and an OTP MRAM region 608. The processor region 602 may include core transistors at the FEOL level to form a central processing unit (CPU). The free-flow MRAM region 610 may correspond to the fifth region 50 and may include a fourth storage portion 265 at the BEOL level. The NvMRAM region 606 may correspond to the second region 20 and may include a second storage portion 255 at the BEOL level. The OTP MRAM region 608 may correspond to the third region 30 and may include a third storage portion 260 at the BEOL level. As mentioned above, the storage parts in the reflux MRAM region 610, the NvMRAM region 606, and the OTP MRAM region 608 may include the same second MTJ stack 2000 and may be formed at the same time. The second IC chip 600 is used for excellent thermal stability and long-term memory retention, and is therefore applied to a micro-controller unit (MCU). A short response time is not of great concern for MCU applications. Because of the thermal stability required in the second IC chip 600, the free layer 218 in the second MTJ stack 2000 may be located on the thick side of the spectrum. In some cases, the free layer 218 in the second MTJ stack 2000 may be between about 2.0 nm and about 3.5 nm.
[0047] In one exemplary aspect, the present disclosure provides a semiconductor device comprising a first conductive feature and a second conductive feature disposed on a first dielectric layer, a buffer layer disposed over the first dielectric layer, a second dielectric layer disposed over the buffer layer, a first bottom through-hole extending through the buffer layer and the second dielectric layer to couple to the first conductive feature along a first direction, a second bottom through-hole extending through the buffer layer and the second dielectric layer to couple to the second conductive feature along the first direction, a first bottom electrode disposed in the first bottom through-hole, a second bottom electrode disposed in the second bottom through-hole, and a first magnetic tunnel junction located over the first bottom electrode. The present invention relates to a semiconductor device comprising a first MTJ stack and a second MTJ stack located above a second bottom electrode, the first MTJ stack and the second MTJ stack having the same thickness along a first direction, the first MTJ stack having a first width along a second direction perpendicular to the first direction, and the second MTJ stack having a second width along the second direction, the second width being greater than the first width.
[0048] In some embodiments, the first MTJ stack includes a pinning layer located above the first bottom electrode, a tunnel barrier layer located above the pinning layer, and a free layer located above the tunnel barrier layer. In some embodiments, the pinning layer includes cobalt, iron, boron, or platinum, the tunnel barrier layer includes magnesium oxide, and the free layer includes cobalt, iron, or boron. In some cases, the first MTJ stack further includes a maintenance layer located above the free layer and a cover layer located above the maintenance layer. In some embodiments, the maintenance layer includes magnesium oxide, and the cover layer includes molybdenum or ruthenium. In some embodiments, the first width is between about 20 nm and about 55 nm, and the second width is between about 75 nm and about 100 nm. In some embodiments, the buffer layer includes silicon carbide. In some embodiments, the first dielectric layer includes silicon-rich silicon oxide.
[0049] In another exemplary aspect, the present disclosure relates to a semiconductor device including a first memory structure and a second memory structure, the first memory structure including a first bottom electrode, a first top electrode located above the first bottom electrode, and a first magnetic tunnel junction (MTJ) stack interposed between the first bottom electrode and the first top electrode along a first direction, the second memory structure including a second bottom electrode, a second top electrode located above the second bottom electrode, and a second MTJ stack interposed between the second bottom electrode and the second top electrode along the first direction, the first MTJ stack having a first width along a second direction perpendicular to the first direction, and the second MTJ stack having a second width along the second direction, the second width being greater than the first width.
[0050] In some embodiments, the first MTJ stack and the second MTJ stack have the same thickness along the first direction. In some embodiments, the first bottom electrode, the first top electrode, the second bottom electrode, and the second top electrode comprise titanium nitride, tantalum nitride, or a combination thereof. In some embodiments, the first MTJ stack comprises a cover layer located above the first bottom electrode, a maintenance layer located above the cover layer, a free layer located above the maintenance layer, a tunnel barrier layer located above the free layer, and a pinning layer located above the tunnel barrier layer. In some embodiments, the cover layer comprises molybdenum or ruthenium, the maintenance layer comprises magnesium oxide, the free layer comprises cobalt, iron, or boron, the tunnel barrier layer comprises magnesium oxide, and the pinning layer comprises cobalt, iron, boron, or platinum. In some cases, the semiconductor device further comprises a third memory structure comprising a third bottom electrode and a third top electrode located above the third bottom electrode. The semiconductor device includes a third MTJ stack interposed between a third bottom electrode and a third top electrode along a first direction. The third MTJ stack includes a third width along a second direction. The third width is greater than the first width. In some embodiments, the first width is between about 20 nm and about 55 nm, the second width is between about 80 nm and about 100 nm, and the third width is between about 75 nm and about 100 nm.
[0051] In yet another exemplary aspect, the present disclosure provides a method for fabricating a semiconductor device comprising receiving a workpiece including a first conductive feature and a second conductive feature disposed in a first dielectric layer, a second dielectric layer located above the first dielectric layer, a first bottom through hole extending through the second dielectric layer to couple to the first conductive feature along a first direction, and a second bottom through hole extending through the second dielectric layer to couple to the second conductive feature along the first direction; depositing a bottom electrode layer over the first bottom through hole, the second bottom through hole, and the second dielectric layer; and forming a magnetic tunnel junction. depositing a memory junction (MTJ) stack above the bottom electrode layer; depositing a top electrode layer above the MTJ stack; depositing a hard mask layer above the top electrode layer; patterning the hard mask layer to form a first hard mask pattern directly above the first bottom through-hole and a second hard mask pattern directly above the second bottom through-hole; and etching the top electrode layer, the MTJ stack, and the bottom electrode layer using the first hard mask pattern and the second hard mask pattern as an etching mask to form a first memory structure directly above the first bottom through-hole and a second memory structure directly above the second bottom through-hole, wherein the first hard mask pattern has a first width along a second direction perpendicular to the first direction, and the second hard mask pattern has a second width along the second direction, the second width being greater than the first width.
[0052] In some embodiments, the etching includes using ion beam etching (IBE). In some cases, the first memory structure includes a first bottom electrode formed of the bottom electrode layer, the second memory structure includes a second bottom electrode formed of the bottom electrode layer, the first bottom electrode includes a third width along the second direction, and the second bottom electrode includes a fourth width along the second direction. The fourth width is greater than the third width. In some embodiments, the method may further include, after the etching, depositing a spacer layer over the first memory structure and the second memory structure, etching back the spacer layer, depositing an etch stop layer over the spacer layer, the first memory structure, and the second memory structure after the etch back, and depositing a third dielectric layer over the etch stop layer. In some embodiments, the etch stop layer includes aluminum oxide.
[0053] The foregoing has outlined features of some embodiments to enable those skilled in the art to better understand the various aspects of the present disclosure. It should be appreciated that those skilled in the art can readily use this disclosure as a basis for designing or modifying other processes and structures for achieving the same purposes and / or advantages for implementing the embodiments introduced herein. Those skilled in the art should also recognize that such equivalent structures do not depart from the spirit and scope of the present disclosure, and that various changes, substitutions, and alterations can be made herein without departing from the spirit and scope of the present disclosure. [Explanation of symbols]
[0054] 10. The First Area 20 The second area 30 The Third Region 40 The Fourth Region 50 The Fifth Region 100, 500 ways 102, 104, 106, 108, 110, 112, 114, 116, 118, 502, 504, 506, 508, 510, 512, 514, 516, 518 blocks 200 Work 201 Substrate 202 First dielectric layer 203 Internal connection structure 204 Conductive Features 206 Buffer Layer 208 Second Dielectric Layer 210-1 First bottom through hole 210-2 Second bottom through hole 210-3 3rd bottom through hole 210-4 4th bottom through hole 212 Bottom electrode layer 214 Pinning Layer 216 Tunnel Barrier Layer 218 Free Tier 220 Maintenance Layer 222 Cover Layer 224 Top electrode layer 224-1 First top electrode 224-2 Second top electrode 224-3 Third top electrode 224-4 4th top electrode 226 Hard Mask Layer 226-1 First hard mask pattern 226-2 Second hard mask pattern 226-3 Third hard mask pattern 226-4 4th hard mask pattern 228 Spacer Layer 230 Etch stop layer 232 Third Dielectric Layer 235-1 First contact opening 235-2 Second contact opening 235-3 3rd Contact Opening 235-4 4th contact opening 235-5 5th contact opening 235-6 6th Contact Opening 236-1 First Top Contact Via 236-2 Second Top Contact Via 236-3 3rd Top Contact Via 236-4 4th top contact via 236-5 5th top contact via 250 First Storage Section 255 Second Storage Section 260 Third Storage Section 265 4th Storage Section 300 Ion Beam Etching 400 First Integrated Circuit Chip 402, 602 processor area 404 RAM system MRAM area 406, 606 NvMRAM area 408, 608 OTP MRAM area 600 Second Integrated Circuit Chip 610 Free flow MRAM area 1000 first magnetic tunnel junction stack 2000 Second MTJ stack d1 First dimension d2 Second dimension d3 third dimension d4 The fourth dimension D1 First MTJ dimension D2 Second MTJ dimension D3 Third MTJ dimension D4 Fourth MTJ dimension
Claims
1. a first conductive feature and a second conductive feature disposed on the first dielectric layer; a buffer layer disposed over the first dielectric layer; a second dielectric layer disposed above the buffer layer; a first bottom through-hole extending through the buffer layer and the second dielectric layer to couple to the first conductive feature along a first direction; a second bottom through-hole extending through the buffer layer and the second dielectric layer to couple to the second conductive feature along a first direction; a first bottom electrode disposed in the first bottom through-hole; a second bottom electrode disposed in the second bottom through-hole; a first magnetic tunnel junction stack located above the first bottom electrode; a second magnetic tunnel junction stack located above the second bottom electrode; a first top electrode located above the first magnetic tunnel junction stack; a second top electrode located above the second magnetic tunnel junction stack; a first top contact via located above the first top electrode; a second top contact via located above the second top electrode; Including, the first magnetic tunnel junction stack and the second magnetic tunnel junction stack have the same thickness along the first direction; the first magnetic tunnel junction stack has a first width along a second direction perpendicular to the first direction, the second magnetic tunnel junction stack has a second width along the second direction, the first top contact via has a third width along the second direction, and the second top contact via has a fourth width along the second direction; The second width is greater than the first width, and the fourth width is greater than the third width.
2. The first magnetic tunnel junction stack comprises: a pinning layer located above the first bottom electrode; a tunnel barrier layer located above the pinning layer; a free layer located above the tunnel barrier layer; The semiconductor device according to claim 1 .
3. the pinning layer comprises cobalt, iron, boron or platinum; the tunnel barrier layer includes magnesium oxide; The semiconductor device according to claim 2 , wherein the free layer contains cobalt, iron, or boron.
4. The first magnetic tunnel junction stack comprises: a maintenance layer located above the free layer; The semiconductor device according to claim 2 or 3, further comprising: a cover layer located above the maintenance layer.
5. The maintenance layer contains magnesium oxide, The semiconductor device according to claim 4 , wherein the cover layer contains molybdenum or ruthenium.
6. a first memory structure including a first bottom electrode, a first top electrode located above the first bottom electrode, and a first magnetic tunnel junction stack interposed between the first bottom electrode and the first top electrode along a first direction; a second memory structure including a second bottom electrode, a second top electrode located above the second bottom electrode, and a second magnetic tunnel junction stack interposed between the second bottom electrode and the second top electrode along the first direction; a first top contact via located above the first top electrode; a second top contact via located above the second top electrode; Equipped with the first magnetic tunnel junction stack has a first width along a second direction perpendicular to the first direction, the second magnetic tunnel junction stack has a second width along the second direction, the first top contact via has a third width along the second direction, and the second top contact via has a fourth width along the second direction; The second width is greater than the first width, and the fourth width is greater than the third width.
7. 7. The semiconductor device of claim 6, wherein the first bottom electrode, the first top electrode, the second bottom electrode, and the second top electrode comprise titanium nitride, tantalum nitride, or a combination thereof.
8. a third memory structure including a third bottom electrode, a third top electrode located above the third bottom electrode, and a third magnetic tunnel junction stack interposed between the third bottom electrode and the third top electrode along the first direction; the third magnetic tunnel junction stack has a third width along the second direction; The semiconductor device according to claim 6 , wherein the third width is greater than the first width.
9. receiving a workpiece including a first conductive feature and a second conductive feature disposed on a first dielectric layer, a second dielectric layer overlying the first dielectric layer, a first bottom through hole extending through the second dielectric layer to couple to the first conductive feature along a first direction, and a second bottom through hole extending through the second dielectric layer to couple to the second conductive feature along the first direction; depositing a bottom electrode layer over the first bottom through-hole, the second bottom through-hole, and the second dielectric layer; depositing a magnetic tunnel junction stack above the bottom electrode layer; depositing a top electrode layer over the magnetic tunnel junction stack; depositing a hard mask layer over the top electrode layer; patterning the hard mask layer to form a first hard mask pattern directly above the first bottom through-hole and to form a second hard mask pattern directly above the second bottom through-hole; Etching the top electrode layer, the magnetic tunnel junction stack, and the bottom electrode layer using the first hard mask pattern and the second hard mask pattern as an etching mask, so as to directly form a first memory structure above the first bottom through-hole and directly form a second memory structure above the second bottom through-hole; forming a first top contact via over the first memory structure and forming a second top contact via over the second memory structure; Equipped with the first hard mask pattern has a first width along a second direction perpendicular to the first direction, the second hard mask pattern has a second width along the second direction, the first top contact via has a third width along the second direction, and the second top contact via has a fourth width along the second direction; A method for manufacturing a semiconductor device, wherein the second width is greater than the first width, and the fourth width is greater than the third width.
10. after the etching, depositing a spacer layer over the first memory structure and the second memory structure; etching back the spacer layer; after the etch back, depositing an etch stop layer over the spacer layer, the first memory structure, and the second memory structure; depositing a third dielectric layer over the etch stop layer; The method for manufacturing a semiconductor device according to claim 9 , further comprising:
Citation Information
Patent Citations
Semiconductor device and manufacturing method thereof
JP2021150364A
Semiconductor structure integrated with magnetic tunneling junction and manufacturing method thereof
US20170092692A1
Method for writing to magnetic random access memory
US20200020375A1
Methods to improve magnetic tunnel junction memory cells
US20200136027A1
Semiconductor structure and method for manufacturing the same
US20200194665A1