Thermosetting adhesive composition, thermosetting adhesive sheet and printed wiring board

The thermosetting adhesive composition addresses the issues of high dielectric loss and bending resistance in printed wiring boards by combining specific components, achieving low dielectric properties and temperature stability for high-frequency applications.

JP7569954B1Active Publication Date: 2024-10-18DEXERIALS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024055214
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-10-18
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

Existing adhesive compositions for printed wiring boards fail to maintain low dielectric constant and loss tangent, especially at high frequencies, and do not account for temperature changes that affect signal transmission, while also lacking sufficient bending resistance.

Method used

A thermosetting adhesive composition comprising 65 to 90 parts by mass of a styrene elastomer, 5 to 20 parts by mass of a modified polyphenylene ether resin with a radically polymerizable group, and 4 to 10 parts by mass of polybutadiene or polyisoprene, with a total content of radical polymerization initiator, epoxy resin, and curing agent not exceeding 10 parts by mass, ensuring a styrene ratio of less than 67%, to achieve low dielectric properties and bending resistance.

Benefits of technology

The adhesive composition maintains a dielectric constant and loss tangent below 0.0030 at 23°C and 80°C with a temperature change rate of less than 50%, exhibiting excellent bending resistance and heat resistance, suitable for high-frequency applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569954000001_ABST
    Figure 0007569954000001_ABST
Patent Text Reader

Abstract

Provided is a thermosetting adhesive composition which has a low dielectric constant and dielectric loss tangent even after heat curing, a low temperature change rate of the dielectric loss tangent, and good flex resistance. [Solution] The present technology provides a thermosetting adhesive composition for bonding substrates, which contains, relative to a total of 100 parts by mass of the thermosetting adhesive composition, 65 to 90 parts by mass of a styrene-based elastomer, and as crosslinking components, (A) 5 to 20 parts by mass of a modified polyphenylene ether resin having a radically polymerizable group at a molecular end, and (B) 4 to 10 parts by mass of polybutadiene and / or polyisoprene having a weight average molecular weight of 10,000 to 50,000, a radical polymerization initiator, and an epoxy resin, wherein the total content of the radical polymerization initiator, epoxy resin, and epoxy resin curing agent is 10 parts by mass or less, and the styrene-based elastomer contains a styrene ratio of less than 67%, and the total content of the (A) component and the (B) component is 25 parts by mass or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present technology relates to a thermosetting adhesive composition, a thermosetting adhesive sheet, and a printed wiring board. [Background technology]

[0002] The trend toward higher frequencies for signals on printed wiring boards is accelerating due to the increasing speed and capacity of information communication. To accommodate this trend, materials (e.g., adhesive compositions) used in rigid substrates and flexible printed wiring boards (FPCs) are required to have low dielectric constants and low dielectric loss tangents.

[0003] In particular, the dielectric loss tangent is preferably less than 0.0030, and more preferably less than 0.0020, for example, using liquid crystal polymer (LCP), which is a resin material for high frequencies, as a guideline.

[0004] The signal transmission loss in a high-frequency circuit depends on its dielectric tangent (tan δ), which is an index of the loss, but the dielectric tangent generally deteriorates depending on temperature. Therefore, there is a demand for materials that do not deteriorate the signal transmission loss, i.e., that do not significantly increase the dielectric tangent, even in environments where the surrounding area of ​​the circuit becomes hot due to the signal processing load of the high-frequency circuit.

[0005] For example, Patent Document 1 discloses an adhesive composition for flexible printed wiring boards, and Patent Document 2 discloses an elastomer composition having good adhesive strength to polyimide and good high-frequency characteristics. However, the techniques described in Patent Documents 1 and 2 do not take into consideration, and do not mention or suggest, reducing the rate of change of dielectric tangent with temperature.

[0006] In addition, regarding the flexibility required for flexible printed wiring boards, polyphenylene ether has many advantages as a substrate material with low dielectric properties, but it has the drawback of having poor flexibility because it has a very high melting point (softening point) and is hard at room temperature.

[0007] Thus, it is desirable for the adhesive composition to have a low dielectric constant and dielectric loss tangent even after heat curing, a low rate of change of the dielectric loss tangent with temperature, and good flex resistance. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 7351912 [Patent Document 2] JP 2015-131866 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present technology has been proposed in view of the above conventional circumstances, and provides an adhesive composition that has a low dielectric constant and dielectric tangent even after heat curing, a low rate of change of the dielectric tangent with temperature, and good flex resistance. [Means for solving the problem]

[0010] The present technology is a thermosetting adhesive composition for bonding substrates, containing, relative to a total of 100 parts by mass of the thermosetting adhesive composition, 65 to 90 parts by mass of a styrene-based elastomer, and as crosslinking components, (A) 5 to 20 parts by mass of a modified polyphenylene ether resin having a radical polymerizable group at a molecular end, and (B) 4 to 10 parts by mass of polybutadiene and / or polyisoprene having a weight average molecular weight of 10,000 to 50,000, a radical polymerization initiator, and an epoxy resin, wherein the total content of the radical polymerization initiator, epoxy resin, and epoxy resin curing agent is 10 parts by mass or less, and the styrene-based elastomer contains a styrene ratio of less than 67%, and the total content of the component (A) and the component (B) is 25 parts by mass or less. Effect of the Invention

[0011] According to the present technology, it is possible to provide an adhesive composition that has a low dielectric constant and dielectric tangent even after heat curing, a low rate of change of the dielectric tangent with respect to temperature, and good flex resistance. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the configuration of a printed wiring board. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of the configuration of a multilayer printed wiring board. [Diagram 3] FIG. 3 is a plan view showing an example of the configuration of a TEG used in a bending resistance test. [Figure 4] FIG. 4 is a perspective view showing a measuring device used in the bending resistance test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS In the present specification, normal temperature refers to the range of 20° C.±15° C. (5° C. to 35° C.) as defined by the Japanese Industrial Standards (JIS Z 8703).

[0014] In this specification, the weight average molecular weight (Mn) and number average molecular weight (Mn) are values ​​calculated from the molecular weight in terms of standard polystyrene measured by gel permeation chromatography (GPC). The specific measurement conditions for the GPC method are as follows. Solvent: Tetrahydrofuran Columns: KF-806M, KF-806M, KF-803, KF-801, KF-800D (manufactured by Resonac) Column temperature: 40℃ Sample concentration: 0.25% by mass Detector: RI detector Flow rate (flow rate): 1.0ml / min Injection volume: 200μL Calibration curve: A calibration curve using 10 standard polystyrene samples with Mw = 605 to 5,680,000

[0015] <Thermosetting adhesive composition> The thermosetting adhesive composition according to the present technology contains, relative to a total of 100 parts by mass of the thermosetting adhesive composition, 65 to 90 parts by mass of a styrene-based elastomer, 5 to 20 parts by mass of a modified polyphenylene ether resin having a radical polymerizable group at a molecular end (hereinafter also referred to as component (A)) as a crosslinking component, 4 to 10 parts by mass of polybutadiene and / or polyisoprene having a weight average molecular weight of 10,000 to 50,000 (hereinafter also referred to as component (B)), a radical polymerization initiator, and an epoxy resin. In addition, the thermosetting adhesive composition according to the present technology contains a total of 10 parts by mass or less of the radical polymerization initiator, the epoxy resin, and the epoxy resin curing agent. The thermosetting adhesive composition according to the present technology contains, as the styrene-based elastomer, a styrene-based elastomer having a styrene ratio of less than 67%. The thermosetting adhesive composition according to the present technology contains a total of 25 parts by mass or less of the content of the component (A) and the content of the component (B).

[0016] The thermosetting adhesive composition according to the present technology has such a constitution, and therefore can have a low dielectric constant and dielectric loss tangent even after thermal curing, and can also have a low temperature change rate of the dielectric loss tangent. Thus, the thermosetting adhesive composition according to the present technology has good dielectric properties after curing.

[0017] The thermosetting adhesive composition according to the present technology has a dielectric tangent after curing of less than 0.0030 at both 23°C and 80°C, and can exhibit a rate of change represented by the following formula 1 of less than 50%. Equation 1: Rate of change (%)=((dielectric loss tangent of the cured thermosetting adhesive composition at 80° C.) / (dielectric loss tangent of the cured thermosetting adhesive composition at 23° C.)-1)×100

[0018] The dielectric constant of the cured thermosetting adhesive composition is preferably less than 2.40, and more preferably less than 2.30. The dielectric constant of the cured thermosetting adhesive composition can be measured by the method described in the Examples below.

[0019] The thermosetting adhesive composition after curing preferably has a dielectric loss tangent of less than 0.0030, more preferably less than 0.0020, at 23° C. The thermosetting adhesive composition after curing preferably has a dielectric loss tangent of less than 0.0030, more preferably less than 0.0020, at 80° C. The dielectric loss tangent of the thermosetting adhesive composition after curing can be measured by the method described in the examples below.

[0020] The smaller the rate of change represented by Formula 1 of the cured thermosetting adhesive composition is, the more preferable, i.e., the smaller the temperature dependency of the dielectric tangent is, the more preferable. For example, the rate of change represented by Formula 1 of the cured thermosetting adhesive composition is preferably less than 50%, more preferably less than 40%, and even more preferably less than 30%.

[0021] In addition, the thermosetting adhesive composition according to the present technology can adjust the glass transition temperature after curing to, for example, a range of 60 to 150°C, and can provide good bending resistance and heat resistance (for example, solder heat resistance) even after heat curing. For example, since the heat resistance of the thermosetting adhesive composition after heat curing is good, even in a high-frequency printed wiring board, component mounting and connection with another printed wiring board can be performed by a solder reflow process or a hot bar solder process, as in the case of a conventional printed wiring board. Therefore, the thermosetting adhesive composition according to the present technology can be suitably used for applications in which substrates are bonded together, for example, as an adhesive (interlayer adhesive) for flexible printed wiring boards.

[0022] An example of the composition of the thermosetting adhesive composition according to the present technology is described below. The thermosetting adhesive composition according to the present technology contains a styrene-based elastomer, component (A), component (B), a radical polymerization initiator, and an epoxy resin, and may further contain an epoxy resin curing agent as necessary.

[0023] [Styrene-based elastomer] The styrene-based elastomer is a copolymer of styrene and an olefin (e.g., a conjugated diene such as butadiene or isoprene) and / or a hydrogenated product thereof. The styrene-based elastomer is a block copolymer having styrene as a hard segment and a conjugated diene as a soft segment. Examples of the styrene-based elastomer include styrene / butadiene / styrene block copolymer, styrene / isoprene / styrene block copolymer, styrene / ethylene / butylene / styrene block copolymer, styrene / ethylene / propylene / styrene block copolymer, and styrene / butadiene block copolymer. In addition, styrene / ethylene / butylene / styrene block copolymer, styrene / ethylene / propylene / styrene block copolymer, styrene / butadiene block copolymer (also called hydrogenated styrene-based elastomer), etc., in which the double bonds of the conjugated diene component are eliminated by hydrogenation, may be used.

[0024] The styrene-based elastomer may have a functional group that accelerates the curing reaction of the epoxy resin. When the styrene-based elastomer has a functional group that accelerates the curing reaction of the epoxy resin, it also has the function of an epoxy resin curing agent, so there is no need to use an epoxy resin curing agent, but a separate epoxy resin curing agent may be used in combination as long as it does not impair the effects of the present technology.

[0025] Examples of functional groups that promote the curing reaction of epoxy resins include functional groups such as amines and acid anhydrides. When using a styrene-based elastomer having a functional group that promotes the curing reaction of epoxy resins, the movement of the polymer chain containing the functional group that promotes the curing reaction of epoxy resins is restricted by forming the thermosetting adhesive composition according to the present technology into a film, so that latency can be imparted to the polymer side (e.g., styrene-based elastomer). Examples of such styrene-based elastomers include amine-modified styrene-based elastomers and acid-modified styrene-based elastomers.

[0026] The thermosetting adhesive composition according to the present technology contains a styrene-based elastomer having a styrene ratio of less than 67% (e.g., 67% by mass). This allows the thermosetting adhesive composition to have good peel strength and flex resistance after curing. In addition, the lower the styrene ratio in the styrene-based elastomer, the better the dielectric constant and dielectric loss tangent of the thermosetting adhesive composition after curing, and the better the peel strength and flex resistance.

[0027] The styrene ratio in the styrene-based elastomer may be, for example, 60% or less, 50% or less, 42% or less, less than 42%, 30% or less, 20% or less, 15% or less, 12% or more and less than 67%, 12 to 42%, or 12 to 30%.

[0028] Specific examples of styrene-based elastomers include Tuftec H1221 (styrene ratio 12%, manufactured by Asahi Kasei Corporation), Tuftec MP1911 (styrene ratio 30%, acid-modified styrene-based elastomer, manufactured by Asahi Kasei Corporation), and Tuftec H1051 (styrene ratio 42%, manufactured by Asahi Kasei Corporation).

[0029] The content of the styrene-based elastomer is 65 to 90 parts by mass relative to 100 parts by mass of the total of the thermosetting adhesive composition. By making the content of the styrene-based elastomer 65 parts by mass or more, the content of other components (e.g., radical polymerization initiator, epoxy resin, and epoxy resin curing agent) is not too high relatively, and the dielectric constant and dielectric loss tangent of the thermosetting adhesive composition after curing, and the temperature change rate of the dielectric loss tangent of the thermosetting adhesive composition after curing can be reduced. In addition, by making the content of the styrene-based elastomer 90 parts by mass or less, the content of other components (e.g., component (A) and component (B)) is not too low relatively, and the temperature change rate of the dielectric loss tangent of the thermosetting adhesive composition after curing can be reduced, and the heat resistance of the thermosetting adhesive composition after curing can be improved.

[0030] The lower limit of the styrene-based elastomer content may be 68 parts by mass or more, 70 parts by mass or more, 71 parts by mass or more, 75 parts by mass or more, or 76 parts by mass or more, relative to a total of 100 parts by mass of the thermosetting adhesive composition.

[0031] The upper limit of the styrene-based elastomer content may be 85 parts by mass or less, 81 parts by mass or less, or 80 parts by mass or less, per 100 parts by mass in total of the thermosetting adhesive composition.

[0032] The styrene-based elastomer may be used alone or in combination of two or more. When two or more styrene-based elastomers are used in combination, it is preferable that the total amount thereof satisfies the above-mentioned range of the content.

[0033] As an example of the use of the styrene-based elastomer, a styrene-based elastomer having a styrene ratio of less than 67% and a styrene-based elastomer having a styrene ratio of 67% or more may be used in combination. In this case, the content of the styrene-based elastomer having a styrene ratio of less than 67% in the thermosetting adhesive composition is preferably 50% by mass or more relative to the total amount of the styrene-based elastomer, and may be 55% by mass or more, 60% by mass or more, 65% by mass or more, 70% by mass or more, 75% by mass or more, 80% by mass or more, 85% by mass or more, 90% by mass or more, 95% by mass or more, or 99% by mass or more. For example, a styrene-based elastomer having a styrene ratio of 42% or less and a styrene-based elastomer having a styrene ratio of 67% or more may be used in combination, and in this case, the content of the styrene-based elastomer having a styrene ratio of 42% or less is preferably 50% by mass or more relative to the total amount of the styrene-based elastomer.

[0034] [Component (A)] The component (A), i.e., a modified polyphenylene ether resin having a radical polymerizable group at the molecular end, is a crosslinking component, has a polyphenylene ether chain in the molecule, and has a radical polymerizable group at the molecular end. As described above, the radical polymerizable group at the molecular end of the component (A) is crosslinked by the radical polymerization initiator in the thermosetting adhesive composition, so that the glass transition temperature of the thermosetting adhesive composition after curing can be adjusted to, for example, a range of 60 to 150°C, and the bending resistance and heat resistance can be improved even after thermal curing. For example, the component (A) preferably has two or more ethylenically unsaturated bonds as radical polymerizable groups in one molecule. In particular, from the viewpoint of compatibility with the above-mentioned styrene-based elastomer and the dielectric properties of the thermosetting adhesive composition after curing, the component (A) preferably has at least one ethylenically unsaturated bond (for example, a (meth)acryloyl group, a vinylbenzyl group) at both molecular ends. Here, the (meth)acryloyl group includes both an acryloyl group and a methacryloyl group.

[0035] Modified polyphenylene ether resins other than component (A), for example, modified polyphenylene ether resins having hydroxyl groups at the molecular terminals, are undesirable because they have too strong a polarity and therefore have poor compatibility with the above-mentioned styrene-based elastomer, which may prevent the thermosetting adhesive composition from being formed into a film.

[0036] An example of component (A) is a modified polyphenylene ether resin having vinylbenzyl groups at both molecular terminals, which can be obtained, for example, by subjecting a difunctional phenol compound and a monofunctional phenol compound to oxidative coupling to convert the terminal phenolic hydroxyl groups of a difunctional phenylene ether oligomer to vinylbenzyl etherification.

[0037] The weight average molecular weight (or number average molecular weight) of component (A) is preferably 1,000 to 3,000 from the viewpoints of compatibility with the above-mentioned styrene-based elastomer and conformability to unevenness when the wiring pattern side of a wired resin substrate comprising a substrate and a wiring pattern and a coverlay are thermally cured (pressed) via the cured product of the thermosetting adhesive composition.

[0038] Specific examples of the component (A) that can be used include OPE-2St (modified polyphenylene ether resin having vinylbenzyl groups at both molecular terminals, manufactured by Mitsubishi Gas Chemical Company, Inc.), OPE-2EA (modified polyphenylene ether resin having acryloyl groups at both molecular terminals, manufactured by Mitsubishi Gas Chemical Company, Inc.), and Noryl SA9000 (modified polyphenylene ether resin having methacryloyl groups at both molecular terminals, manufactured by SABIC Corporation).

[0039] The content of component (A) is 5 to 20 parts by mass relative to a total of 100 parts by mass of the thermosetting adhesive composition. By making the content of component (A) 20 parts by mass or less, it is possible to improve the flex resistance. Furthermore, by making the content of component (A) 5 parts by mass or more, it is possible to reduce the dielectric tangent of the thermosetting adhesive composition after curing.

[0040] The content of component (A) may be 18 parts by mass or less, 15 parts by mass or less, 13 parts by mass or less, 10 parts by mass or less, or 9 parts by mass or less, relative to a total of 100 parts by mass of the thermosetting adhesive composition.

[0041] The content of component (A) may be 6 parts by mass or more, 8 parts by mass or more, 9 parts by mass or more, or 10 parts by mass or more, based on a total of 100 parts by mass of the thermosetting adhesive composition.

[0042] The component (A) may be used alone or in combination of two or more. When two or more types of the component (A) are used in combination, it is preferable that the total amount thereof satisfies the above-mentioned content range.

[0043] [(B) Component] The (B) component is a crosslinking component, and is polybutadiene and / or polyisoprene having a weight average molecular weight of 10,000 to 50,000. The (B) component is at least one of a polybutadiene resin (resin having only a polybutadiene structure) having a weight average molecular weight of 10,000 to 50,000, a polyisoprene resin (resin having only a polyisoprene structure) having a weight average molecular weight of 10,000 to 50,000, and a resin having a polybutadiene structure and a polyisoprene structure and a weight average molecular weight of 10,000 to 50,000, or a combination of these. In addition, the (B) component may contain other structures than the butadiene structure and the polyisoprene structure as long as it contains a butadiene structure or a polyisoprene structure as a main component, as long as it does not impair the effects of the present technology, but from the viewpoint of improving the effects of the present technology, compatibility with other components, dispersibility, etc., it is preferable that the (B) component does not substantially contain other structures (for example, a styrene structure). From the viewpoint of ease of handling, the component (B) is preferably in a liquid state at room temperature.

[0044] The polybutadiene may be any resin having a polybutadiene structure, and the polybutadiene structure may be included in the main chain or in the side chain. The butadiene structure may be partially hydrogenated or may not be hydrogenated.

[0045] The polyisoprene may be any resin having a polyisoprene structure, and the polyisoprene structure may be included in the main chain or in the side chain. The polyisoprene structure may be partially hydrogenated or may not be hydrogenated.

[0046] The (B) component may have a functional group that accelerates the curing reaction of the epoxy resin. When the (B) component has a functional group that accelerates the curing reaction of the epoxy resin, it also has the function of an epoxy resin curing agent, so there is no need to use an epoxy resin curing agent, but an epoxy resin curing agent may be used separately as long as it does not impair the effects of the present technology. Examples of functional groups that accelerate the curing reaction of the epoxy resin include functional groups such as acid anhydrides. Examples of such (B) components include acid-modified polybutadiene and acid-modified polyisoprene.

[0047] Regarding the weight average molecular weight of component (B), by having the weight average molecular weight of component (B) of 10,000 or more, it is possible to prevent the crosslinking density from becoming too high, and to improve the peel strength and flex resistance of the thermosetting adhesive composition after curing. The weight average molecular weight of component (B) may be 15,000 or more, 20,000 or more, 25,000 or more, 30,000 or more, or 35,000 or more.

[0048] Furthermore, by making the weight average molecular weight of component (B) 50,000 or less, it is possible to prevent the crosslink density from becoming too small, to reduce the temperature change rate of the dielectric tangent of the cured thermosetting adhesive composition, and to improve compatibility with component (A). The weight average molecular weight of component (B) may be 45,000 or less, 40,000 or less, 35,000 or less, or 30,000 or less.

[0049] The content of component (B) is 4 to 10 parts by mass relative to a total of 100 parts by mass of the thermosetting adhesive composition. By making the content of component (B) 10 parts by mass or less, the peel strength and flex resistance of the cured thermosetting adhesive composition can be improved. In addition, by making the content of component (B) 4 parts by mass or more, the temperature change rate of the dielectric tangent of the cured thermosetting adhesive composition can be reduced.

[0050] The content of component (B) may be 9 parts by mass or less, 8 parts by mass or less, 7 parts by mass or less, 6 parts by mass or less, or 5 parts by mass or less, relative to a total of 100 parts by mass of the thermosetting adhesive composition.

[0051] The content of component (B) may be 5 parts by mass or more, 6 parts by mass or more, 7 parts by mass or more, or 8 parts by mass or more, relative to a total of 100 parts by mass of the thermosetting adhesive composition.

[0052] In addition, the total content of the (A) component and the (B) component is 25 parts by mass or less, optionally 24 parts by mass or less, optionally 23 parts by mass or less, optionally 22 parts by mass or less, optionally 21 parts by mass or less, optionally 20 parts by mass or less, optionally 19 parts by mass or less, optionally 18 parts by mass or less, optionally 17 parts by mass or less, or optionally 16 parts by mass or less.

[0053] The lower limit of the total content of the (A) component and the (B) component is not particularly limited, as long as it is within a range that satisfies the above-mentioned contents of the (A) component and the (B) component, and can be, for example, 15 parts by mass or more, optionally 16 parts by mass or more, optionally 17 parts by mass or more, optionally 18 parts by mass or more, optionally 19 parts by mass or more, or optionally 20 parts by mass or more.

[0054] Furthermore, it is preferable that the content of the component (A) and the content of the component (B) satisfy the following formula 2. Equation 2: (Content of component (A) in thermosetting adhesive composition)>(Content of component (B) in thermosetting adhesive composition)

[0055] When the content of component (A) and the content of component (B) in the thermosetting adhesive composition satisfy formula 2, the dielectric constant and dielectric tangent of the cured thermosetting adhesive composition can be more effectively reduced, the rate of change of the dielectric tangent with temperature can also be more effectively reduced, and the flex resistance and heat resistance of the cured thermosetting adhesive composition can be more effectively improved.

[0056] The (B) component may be used alone or in combination of two or more. When two or more (B) components are used in combination, it is preferable that the total amount thereof satisfies the above-mentioned content range.

[0057] [Radical polymerization initiator] The radical polymerization initiator is a catalyst that promotes the radical curing reaction of unsaturated bonds. The radical polymerization initiator crosslinks the radical polymerizable group at the molecular end of the (A) component or the radical polymerizable group in the (B) component, for example, by thermal curing. The heat resistance of the cured thermosetting adhesive composition can be improved by including a radical polymerization initiator in the thermosetting adhesive composition. From the viewpoint of the storage stability (life) of the thermosetting adhesive composition at room temperature, the radical polymerization initiator is preferably a peroxide having a high reaction initiation temperature, for example, an organic peroxide having a decomposition temperature of 170°C or higher for a half-life of 1 minute. Examples of such organic peroxides include dicumyl peroxide (decomposition temperature for a half-life of 1 minute is 175°C), t-butylcumyl peroxide (decomposition temperature for a half-life of 1 minute is 173°C), and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (decomposition temperature for a half-life of 1 minute is 194°C).

[0058] The content of the radical polymerization initiator is not particularly limited as long as the total content of the radical polymerization initiator, epoxy resin, and epoxy resin curing agent is 10 parts by mass or less relative to a total of 100 parts by mass of the thermosetting adhesive composition, and can be, for example, 0.5 parts by mass or more, optionally 1 part by mass or more, optionally 1 to 5 parts by mass, optionally 1 to 4 parts by mass, or optionally 1 to 3 parts by mass.

[0059] The radical polymerization initiator may be used alone or in combination of two or more. When two or more radical polymerization initiators are used in combination, it is preferable that the total amount thereof satisfies the above-mentioned range of the content.

[0060] [Epoxy resin] Examples of the epoxy resin include epoxy resins having a naphthalene skeleton, bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins, siloxane type epoxy resins, biphenyl type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, hydantoin type epoxy resins, etc. In particular, from the viewpoint of film formability, the epoxy resin is preferably an epoxy resin having a naphthalene skeleton, a bisphenol A type epoxy resin, or a bisphenol F type epoxy resin that is liquid at room temperature.

[0061] The content of the epoxy resin is not particularly limited as long as the total content of the radical polymerization initiator, epoxy resin, and epoxy resin curing agent is within a range of 10 parts by mass or less relative to a total of 100 parts by mass of the thermosetting adhesive composition, and may be, for example, less than 5 parts by mass, 0.5 parts by mass or more, 1 part by mass or more, 1 to 7 parts by mass, 1 to 6 parts by mass, 1 to 5 parts by mass, 1 to 4 parts by mass, or 1 to 3 parts by mass.

[0062] The epoxy resin may be used alone or in combination of two or more. When two or more epoxy resins are used in combination, it is preferable that the total amount thereof satisfies the above-mentioned range of the content.

[0063] [Epoxy resin hardener] The epoxy resin curing agent is a catalyst that promotes the curing reaction of the above-mentioned epoxy resin. For example, imidazole-based, phenol-based, amine-based, acid anhydride-based, organic peroxide-based, etc. can be used as the epoxy resin curing agent. In particular, from the viewpoint of the storage stability (life) of the thermosetting adhesive composition at room temperature, the epoxy resin curing agent is preferably a latent curing agent, and more preferably an encapsulated imidazole-based curing agent that has latent properties. By improving the storage stability at room temperature, it is possible to more easily manage the supply and use of the thermosetting adhesive composition. Specifically, as the epoxy resin curing agent, a microencapsulated latent curing agent that has a latent imidazole modified body as a core and its surface coated with polyurethane can be used. As a commercially available product, for example, Novacure 3941 (manufactured by Asahi Kasei E-Materials Corporation) can be used.

[0064] When the thermosetting adhesive composition contains an epoxy resin curing agent, the content of the epoxy resin curing agent is not particularly limited as long as the total content of the radical polymerization initiator, epoxy resin, and epoxy resin curing agent is within a range of 10 parts by mass or less relative to a total of 100 parts by mass of the thermosetting adhesive composition, and can be, for example, 0.1 parts by mass or more, alternatively 0.5 parts by mass or more, alternatively 0.8 parts by mass or more, alternatively 1 part by mass or more, alternatively 0.1 to 3 parts by mass, or alternatively 0.5 to 3 parts by mass.

[0065] In addition, when the thermosetting adhesive composition contains a styrene-based elastomer having a functional group that accelerates the curing reaction of the epoxy resin as the styrene-based elastomer, the styrene-based elastomer having a functional group that accelerates the curing reaction of the epoxy resin is included in the content of the above-mentioned styrene-based elastomer, but is not included in the content of the epoxy resin curing agent. Similarly, when the thermosetting adhesive composition contains a (B) component having a functional group that accelerates the curing reaction of the epoxy resin as the (B) component, the (B) component having a functional group that accelerates the curing reaction of the epoxy resin is included in the content of the above-mentioned (B) component, but is not included in the content of the epoxy resin curing agent. In addition, when the thermosetting adhesive composition contains a styrene-based elastomer having a functional group that accelerates the curing reaction of the epoxy resin as the (B) component, or when the thermosetting adhesive composition contains a (B) component having a functional group that accelerates the curing reaction of the epoxy resin as the (B) component, the thermosetting adhesive composition may or may not contain a separate epoxy resin curing agent.

[0066] The epoxy resin curing agent may be used alone or in combination of two or more. When two or more epoxy resin curing agents are used in combination, it is preferable that the total amount thereof satisfies the above-mentioned content range.

[0067] In the thermosetting adhesive composition according to the present technology, the total content of the radical polymerization initiator, the epoxy resin, and the epoxy resin curing agent is 10 parts by mass or less, or may be 9 parts by mass or less, or may be 5 parts by mass or less, relative to a total of 100 parts by mass of the thermosetting adhesive composition (the styrene-based elastomer, the component (A), the component (B), the radical polymerization initiator, the epoxy resin, and the epoxy resin curing agent). By making the total content of the radical polymerization initiator, the epoxy resin, and the epoxy resin curing agent 10 parts by mass or less, the dielectric properties of the thermosetting adhesive composition after curing can be improved.

[0068] Furthermore, the lower limit of the total content of the radical polymerization initiator, epoxy resin, and epoxy resin curing agent in the thermosetting adhesive composition is not particularly limited, and may be, for example, 0.1 part by mass or more, 0.5 part by mass or more, or 1 part by mass or more, relative to a total of 100 parts by mass of the thermosetting adhesive composition.

[0069] As described above, the thermosetting adhesive composition according to the present technology, in a first embodiment, contains an epoxy resin curing agent when the styrene-based elastomer does not have a functional group that promotes the curing reaction of the epoxy resin. That is, the thermosetting adhesive composition of the first embodiment contains 65 to 90 parts by mass of a styrene-based elastomer, 5 to 20 parts by mass of (A) a modified polyphenylene ether resin having a radical polymerizable group at the molecular end as a crosslinking component, 4 to 10 parts by mass of (B) a polybutadiene and / or polyisoprene having a weight average molecular weight of 10,000 to 50,000, a radical polymerization initiator, an epoxy resin, and an epoxy resin curing agent, the total content of the radical polymerization initiator, the epoxy resin, and the epoxy resin curing agent is 10 parts by mass or less, the styrene-based elastomer contains a styrene-based elastomer having a styrene ratio of less than 67%, and the total content of the (A) component and the (B) component is 25 parts by mass or less.

[0070] In addition, as a second aspect of the thermosetting adhesive composition according to the present technology, when the styrene-based elastomer has a functional group that promotes the curing reaction of the epoxy resin, the thermosetting adhesive composition may or may not contain an epoxy resin curing agent. That is, the thermosetting adhesive composition of the second aspect contains at least 65 to 90 parts by mass of a styrene-based elastomer, 5 to 20 parts by mass of (A) a modified polyphenylene ether resin having a radical polymerizable group at the molecular end as a crosslinking component, 4 to 10 parts by mass of (B) a polybutadiene and / or polyisoprene having a weight average molecular weight of 10,000 to 50,000, a radical polymerization initiator, and an epoxy resin, the total content of the radical polymerization initiator and the epoxy resin being 10 parts by mass or less, the styrene-based elastomer containing a styrene ratio of less than 67%, and the total content of the (A) component and the (B) component being 25 parts by mass or less.

[0071] [Other ingredients] The thermosetting adhesive composition may further contain other components other than the above-mentioned components within a range that does not impair the effects of the present technology. Examples of other components include organic solvents, adhesion-imparting agents such as silane coupling agents, and fillers for adjusting fluidity and imparting flame retardancy. The organic solvent is not particularly limited, and examples thereof include alcohol-based solvents, ketone-based solvents, ether-based solvents, aromatic solvents, and ester-based solvents. Among these, aromatic solvents and ester-based solvents are preferred from the viewpoint of solubility. The organic solvent may be used alone or in combination of two or more types.

[0072] <Thermosetting adhesive sheet> The thermosetting adhesive sheet according to the present technology has a thermosetting adhesive layer made of the above-mentioned thermosetting adhesive composition formed on a substrate, and is in the form of a film. The thermosetting adhesive sheet can be obtained, for example, by diluting the above-mentioned thermosetting adhesive composition with a solvent, applying it to at least one side of the substrate using a bar coater, roll coater, or the like so that the thickness after drying is 10 to 60 μm, and drying it at a temperature of about 50 to 130° C. The substrate can be, for example, a release substrate that is a substrate such as a polyethylene terephthalate film or a polyimide film and, if necessary, is subjected to a release treatment using silicone or the like.

[0073] The thickness of the thermosetting adhesive layer constituting the thermosetting adhesive sheet can be appropriately set depending on the purpose, and can be, for example, 1 to 100 μm, or can also be 1 to 30 μm.

[0074] The thermosetting adhesive layer constituting the thermosetting adhesive sheet is made of a thermosetting adhesive composition that has a low dielectric constant and dielectric loss tangent even after heat curing, a low temperature change rate of the dielectric loss tangent, and good flex resistance and heat resistance even after heat curing, and can be used, for example, as an interlayer adhesive for flexible printed wiring boards, or for bonding and fixing terminal parts of flexible printed wiring boards to connecting substrates for backing them. In addition, the thermosetting adhesive sheet has good peel strength and heat resistance after curing, and good storage properties at room temperature.

[0075] <Printed wiring board> The printed wiring board according to the present technology is, for example, a laminate of the wiring pattern side of a wiring substrate having a substrate and a wiring pattern and a coverlay via a cured product (thermosetting adhesive layer) of the above-mentioned thermosetting adhesive composition. The printed wiring board is obtained, for example, by arranging a thermosetting adhesive layer of a thermosetting adhesive sheet between the wiring pattern side of the wiring substrate and the coverlay, and by thermocompression bonding, integrating the wiring substrate and the coverlay. The coverlay is an insulating layer for protecting the wiring pattern of the wiring substrate.

[0076] The substrate with wiring, like the adhesive composition described above, has excellent electrical properties in the high frequency range, for example, preferably has low dielectric constant and dielectric loss tangent in the frequency range of 1 to 10 GHz. Specific examples of the substrate include substrates mainly composed of liquid crystal polymer (LCP), polytetrafluoroethylene, polyimide, and polyethylene naphthalate. Among these substrates, substrates mainly composed of liquid crystal polymer (liquid crystal polymer film) are preferred. Liquid crystal polymer has a very low moisture absorption rate compared to polyimide, and is less affected by the usage environment.

[0077] An example of the configuration of a printed wiring board using the thermosetting adhesive composition according to the present technology will be described. The printed wiring board 1 shown in Fig. 1 is formed by laminating a copper foil 3 side of a wiring substrate (copper-clad laminate: CCL) including a liquid crystal polymer film 2 and a copper foil (rolled copper foil) 3, and a liquid crystal polymer film 4, via a cured layer 5 made of the above-mentioned thermosetting adhesive composition (thermosetting adhesive layer).

[0078] The printed wiring board may have a multilayer structure as shown in Fig. 2. The printed wiring board 6 shown in Fig. 2 is formed by laminating, for example, the copper plating layer 9 side of a wiring substrate including a polyimide layer 7 (thickness 25 µm), a copper foil 8 (thickness 18 µm), and a copper plating layer 9 (thickness 10 µm) and a coverlay 10 (thickness 25 µm) via a cured layer 5 (thickness 35 µm) made of the above-mentioned thermosetting adhesive composition (thermosetting adhesive layer) (total thickness 201 µm). EXAMPLES

[0079] Hereinafter, examples of the present technology will be described. Note that the present technology is not limited to these examples.

[0080] <Styrene-based elastomer> Tuftec H1221: Hydrogenated styrene-based thermoplastic elastomer (styrene ratio 12%), manufactured by Asahi Kasei Corporation Tuftec M1911: Hydrogenated styrene-based thermoplastic elastomer (styrene ratio 30%), manufactured by Asahi Kasei Corporation Tuftec H1051: Hydrogenated styrene-based thermoplastic elastomer (styrene ratio 42%), manufactured by Asahi Kasei Corporation Tuftec H1043: Hydrogenated styrene-based thermoplastic elastomer (styrene ratio 67%), manufactured by Asahi Kasei Corporation

[0081] <(A) Modified polyphenylene ether resin having radically polymerizable groups at the molecular terminals> OPE-2St2200: Modified polyphenylene ether resin (Mn=2,200) with vinylbenzyl groups at both ends of the molecule, manufactured by Mitsubishi Gas Chemical Company, Inc. SA9000: Modified polyphenylene ether resin (Mw=1,700) with methacryloyl groups at both ends of the molecule, manufactured by SABIC

[0082] <(A') Modified polyphenylene ether resin having no radically polymerizable group at the molecular end> S201A: Polyphenylene ether resin with hydroxyl groups at both ends of the molecule, manufactured by Asahi Kasei Corporation

[0083] <(B) Polybutadiene and / or polyisoprene having a weight average molecular weight of 10,000 to 50,000> Ricon 154: Liquid polybutadiene (Mw=15,000, Mn=5,200), manufactured by Cray Valley LIR-30: Liquid polyisoprene (Mw=28,000), manufactured by Kuraray

[0084] <(B') Polybutadiene and / or polyisoprene having a weight average molecular weight of less than 10,000 or more than 50,000> LIR-50: Liquid polyisoprene (Mw=54,000), manufactured by Kuraray B-3000: Liquid polybutadiene (Mw=8,000, Mn=3,000), manufactured by Nippon Soda Co., Ltd.

[0085] <Radical polymerization initiator> Dicumyl peroxide: (Decomposition temperature for half-life of 1 minute is 175°C) Dilauryl peroxide: (Decomposition temperature for half-life of 1 minute is 116°C)

[0086] <Epoxy resin> JER828: Epoxy resin, manufactured by Mitsubishi Chemical Corporation 4032D: Naphthalene type epoxy resin, manufactured by DIC

[0087] <Epoxy resin hardener> Novacure 3941: A microcapsule-type latent curing agent consisting of a denatured imidazole core and a polyurethane coating on the surface. Manufactured by Asahi Kasei E-Materials Corporation 2E4MZ: 2-Ethyl-4-methylimidazole (non-latent imidazole)

[0088] <Preparation of Thermosetting Adhesive Composition> Each component shown in Tables 1 and 2 was weighed out to the mass shown in Tables 1 and 2, and mixed uniformly in an organic solvent containing toluene and ethyl acetate to prepare a thermosetting adhesive composition (coating for forming a thermosetting adhesive layer). Regarding the "relationship between (A) and (B)" in Tables 1 and 2, for example, in Example 1 in Table 1, the column "(A) + (B) ≦ 25" states "Satisfies 24", which means that the total content of the (A) component and the (B) component is 24 parts by mass, and the above-mentioned formula 1 is satisfied. In addition, in Comparative Example 9 in Table 2, the column "(A) + (B) ≦ 25" states "Does not satisfy 30", which means that the total content of the (A) component and the (B) component is 30 parts by mass, and the above-mentioned formula 1 is not satisfied.

[0089] <Preparation of thermosetting sheet> The obtained thermosetting adhesive composition was applied to a polyethylene terephthalate film that had been subjected to a release treatment, and then dried in a drying oven at 40 to 130°C to produce a thermosetting adhesive sheet having a polyethylene terephthalate film and a 25 μm-thick thermosetting adhesive layer.

[0090] <Evaluation> <Evaluation of the coating properties (film state) of paints for forming thermosetting adhesive layers> When preparing the above-mentioned thermosetting adhesive sheet, the coatability of the thermosetting adhesive composition was evaluated according to the following criteria. The results are shown in Tables 1 and 2. From a practical standpoint, a rating of A is preferable.

[0091] A: The compatibility with the thermosetting adhesive composition is good, and the evaluation described below can be performed in the film state. B: The compatibility of the thermosetting adhesive composition is poor, and it is impossible to perform the evaluation described below in the film state.

[0092] <Dielectric constant (Dk)> The thermosetting adhesive sheets prepared in the examples and comparative examples were laminated together to prepare a test piece having a thickness of 1 mm, which was then thermally cured for 1 hour under conditions of 180°C and 1.0 MPa to prepare a test piece for evaluation. The dielectric constant of this test piece for evaluation was determined by a cavity resonance perturbation method using a dielectric constant measuring device (manufactured by AET) at measurement temperatures of 23°C and 80°C and a measurement frequency of 10 GHz. The dielectric constant was evaluated according to the following criteria. The results are shown in Tables 1 and 2.

[0093] A: Dielectric constant is less than 2.30 B: Dielectric constant is 2.30 or more and less than 2.40 C: Dielectric constant is 2.40 or more and less than 2.60 D: Dielectric constant is 2.60 or more

[0094] In practical terms, the dielectric constant is preferably rated as A or B, and more preferably A.

[0095] <Dielectric loss tangent (Df)> The dielectric loss tangent of the evaluation test piece was determined in the same manner as in the measurement of the dielectric constant described above. The dielectric loss tangent was evaluated according to the following criteria. The results are shown in Tables 1 and 2.

[0096] A: Dielectric tangent less than 0.0020 B: Dielectric tangent is 0.0020 or more and less than 0.0030 C: Dielectric tangent is 0.0030 or more and less than 0.0050 D: Dielectric tangent is 0.0050 or more

[0097] For practical purposes, the dielectric loss tangent is preferably rated as A or B, and more preferably A. That is, the thermosetting adhesive composition has a dielectric loss tangent after curing at both 23° C. and 80° C. that is preferably less than 0.0030, and more preferably less than 0.0020 at both.

[0098] <Rate of change in dielectric tangent> The rate of change (%) of the measured value at 80° C. relative to the measured value at 23° C. was determined and evaluated according to the following criteria. The results are shown in Tables 1 and 2. A: The change rate between 23℃ and 80℃ is less than 30%. B: The rate of change between 23℃ and 80℃ is 30% or more and less than 50% C: Change rate between 23℃ and 80℃ is 50% or more

[0099] For practical purposes, the rate of change in dielectric tangent is preferably evaluated as A or B, and more preferably as A. That is, the thermosetting adhesive composition preferably exhibits a rate of change in dielectric tangent after curing, represented by the above-mentioned formula 1, of less than 50%, and more preferably less than 30%.

[0100] <Peel strength> The obtained thermosetting adhesive sheet was cut into a strip of a predetermined size (2 cm x 5 cm), and the cut thermosetting adhesive layer was temporarily attached to a liquid crystal polymer film of 2 cm x 7 cm x 50 μm thickness with a laminator set at 100 ° C., and then the base material (polyethylene terephthalate film) was removed to expose the thermosetting adhesive layer. The exposed thermosetting adhesive layer was overlaid on the rolled copper foil surface (surface that was not roughened) of a copper-clad laminate (CCL consisting of a rolled copper foil of 12 μm thickness and a liquid crystal polymer film of 50 μm thickness) of the same size, and thermally cured at 180 ° C. and 1.0 MPa for 1 hour. In this way, a sample was produced.

[0101] The obtained samples were subjected to a 90-degree peel test at a peel speed of 50 mm / min, and the force required for peeling (initial peel strength and peel strength after reliability test) was measured. The results are shown in Tables 1 and 2.

[0102] [Initial (measured directly after heat curing under the above conditions of 180°C and 1.0 MPa)] A: Peel strength is 8N / cm or more B: Peel strength is 6N / cm or more and less than 8N / cm C: Peel strength is 4N / cm or more and less than 6N / cm D: Peel strength is less than 4N / cm

[0103] [After reliability test (85°C, 85% relative humidity, 240 hours (i.e., after heat curing under the above-mentioned conditions of 180°C and 1.0 MPa, place in an environment of 85°C and 85% relative humidity for 240 hours, remove and measure 3 hours later))] A: Peel strength is 7N / cm or more B: Peel strength is 5N / cm or more and less than 7N / cm C: Peel strength is 3N / cm or more and less than 5N / cm D: Peel strength is less than 3N / cm

[0104] In practical terms, the evaluation of the initial peel strength and the peel strength after the reliability test is preferably A or B, and more preferably A.

[0105] <Heat resistance (solder heat resistance)> The above samples were subjected to a solder float test at 288℃ for 10 seconds three times, after which the appearance of the samples was visually inspected and evaluated according to the following criteria to see whether peeling or blistering occurred. The results are shown in Tables 1 and 2.

[0106] A: No abnormalities after three passes B: No abnormalities after two passes, but abnormalities such as peeling or blisters with a diameter of 0.2 mm or more after the third pass C: No abnormalities after one pass, but abnormalities such as peeling or blisters with a diameter of 0.2 mm or more occurred after the second pass. D: Abnormalities such as peeling or blisters with a diameter of 0.2 mm or more occurred on the first try.

[0107] In practical terms, the heat resistance is preferably rated as A or B, and more preferably A.

[0108] <Bending resistance> The obtained thermosetting adhesive sheet was cut into a strip of a predetermined size (1.5 cm x 12 cm), and the cut thermosetting adhesive layer was temporarily attached to a liquid crystal polymer film of 1.5 cm x 12 cm x 50 μm thickness using a laminator set at 100 ° C., and then the substrate (polyethylene terephthalate film) was removed to expose the thermosetting adhesive layer. The exposed thermosetting adhesive layer was overlaid with an FPC-TEG (Test Elementary Group) for MIT flex resistance test, and thermally cured at 180 ° C. and 1.0 MPa for 1 hour to obtain a test piece. The configuration of the TEG for MIT flex resistance test is shown in FIG. 3. TEG11 is a copper wiring formed from a CCL consisting of a liquid crystal polymer film (thickness 50 μm) as a substrate and rolled copper foil (thickness 12 μm). A coverlay (not shown) is laminated on the copper wiring of TEG11. In FIG. 3, "130 mm" is the length of the entire TEG 11, "120 mm" is the length of the coverlay (a laminate of a thermosetting adhesive layer and a liquid crystal polymer film), "15 mm" is the width of the entire TEG 11 and the width of the coverlay, "11 mm" is the distance between the copper wirings (outside), "10 mm" is the distance between the copper wirings (inside), and the copper wiring width is 1 mm. The MIT bending test was performed by setting the prepared test piece 12 in an MIT bending fatigue tester 13 equipped with a plunger 14, an upper chuck 15, a rotating chuck 16, and a bending top 17 as shown in FIG. 4. The bending test was performed under the conditions of a bending angle of 135°, a bending clamp angle R=0.38, and a test speed of 175 cpm. The number of bending times until the copper wiring broke was confirmed. The results are shown in Tables 1 and 2.

[0109] A: More than 1200 bends before breaking B: The number of times of bending until breakage is 600 or more and less than 1200 C: The number of times of bending until breakage is 300 or more and less than 600 D: Less than 300 folds until breakage

[0110] In practical terms, the bending resistance is preferably evaluated as A or B, and more preferably as A.

[0111] <Measurement of glass transition temperature> The thermosetting adhesive sheets thus prepared were laminated together to prepare a test piece having a thickness of 600 μm, which was then thermally cured for 1 hour under conditions of 180°C and 1.0 MPa to prepare a test piece for evaluation. The glass transition temperature of this test piece was determined when it was heated from -60°C to 250°C at a rate of 10°C / min using a dynamic viscoelasticity measuring device (manufactured by TA Instruments). In the case of copolymerized polymers or mixtures of multiple components, multiple tan δ peaks may be detected. In such cases, the temperature of the tan δ peak showing a higher value (the one with a larger change in elastic modulus) was taken as the glass transition temperature. The results are shown in Tables 1 and 2.

[0112] [Table 1]

[0113] [Table 2]

[0114] As in Examples 1 to 10, a thermosetting adhesive composition for bonding substrates containing 65 to 90 parts by mass of a styrene-based elastomer, 5 to 20 parts by mass of component (A) and 4 to 10 parts by mass of component (B) as crosslinking components, a radical polymerization initiator and an epoxy resin, the total content of the radical polymerization initiator, epoxy resin and epoxy resin curing agent being 10 parts by mass or less, containing a styrene-based elastomer having a styrene ratio of less than 67% as the styrene-based elastomer, and the total content of the component (A) and the content of the component (B) being 25 parts by mass or less, had low dielectric constant and dielectric tangent even after heat curing, and also had a low rate of change of dielectric tangent with temperature (rate of change of dielectric tangent with temperature at 23 to 80°C), and was found to have good bending resistance and heat resistance.

[0115] Regarding the dielectric constant and dielectric tangent after curing, the thermosetting adhesive compositions of Examples 1 to 10 were found to have a dielectric tangent after curing of less than 0.003 at both 23° C. and 80° C. Furthermore, regarding the rate of change of the dielectric tangent with temperature, the thermosetting adhesive compositions of Examples 1 to 10 were found to exhibit a rate of change represented by Equation 1 of less than 50%.

[0116] Furthermore, from the results of Example 2 and the other Examples, it was found that a thermosetting adhesive composition in which the contents of components (A) and (B) satisfy formula 2, i.e., the content of component (A) is greater than the content of component (B), tends to have a lower dielectric tangent after curing and a lower rate of change of the dielectric tangent with temperature. Specifically, it was found that the thermosetting adhesive compositions of Examples 1, 3, 5, 6, 7, 9, and 10 had a dielectric tangent after curing of less than 0.0020 at both 23°C and 80°C, and the rate of change represented by formula 1 was less than 30%.

[0117] Furthermore, for example, the results of Example 4 and the other Examples show that a thermosetting adhesive composition that does not use polybutadiene and / or polyisoprene having a weight average molecular weight of more than 50,000 in combination with component (B), in other words, a thermosetting adhesive composition that does not contain polybutadiene and / or polyisoprene having a weight average molecular weight of more than 50,000, tends to have a lower dielectric tangent and a lower rate of change of the dielectric tangent with temperature after curing.

[0118] Furthermore, for example, the results of Example 5 and the other Examples show that thermosetting adhesive compositions that do not use polybutadiene and / or polyisoprene having a weight average molecular weight of less than 10,000 in combination with component (B), in other words, thermosetting adhesive compositions that do not contain polybutadiene and / or polyisoprene having a weight average molecular weight of more than 10,000, tend to have better peel strength and flex resistance.

[0119] Furthermore, for example, the results of Example 7 and the other Examples show that thermosetting adhesive compositions containing a styrene-based elastomer with a styrene ratio of less than 42% (e.g., 12 to 30%) as the styrene-based elastomer tend to have better peel strength and flex resistance in addition to having good dielectric properties.

[0120] Furthermore, for example, the results of Example 8 and the other Examples show that when the epoxy resin content is less than 5 parts by mass per 100 parts by mass of the total of the thermosetting adhesive composition, the dielectric tangent after curing and the temperature change rate of the dielectric tangent tend to be lower.

[0121] It was found that since the thermosetting adhesive composition of Comparative Example 1 did not contain component (B), it was difficult to suppress the rate of change of the dielectric tangent with temperature.

[0122] It was found that the thermosetting adhesive composition of Comparative Example 2 did not contain the (B) component and contained more than 20 parts by mass of the (A) component, making it difficult to suppress the temperature change rate of the dielectric tangent.

[0123] The thermosetting adhesive composition of Comparative Example 3 does not contain component (B), in other words, does not contain component (B) and contains only (B') polybutadiene and / or polyisoprene having a weight average molecular weight of more than 50,000, and therefore it was found that it was difficult to suppress the rate of change of the dielectric tangent with temperature.

[0124] The thermosetting adhesive composition of Comparative Example 4 did not contain component (B), in other words, it did not contain component (B) and contained only (B') polybutadiene and / or polyisoprene having a weight average molecular weight of less than 10,000, and therefore it was found that the peel strength and flex resistance were not good.

[0125] It was found that it was difficult to reduce the dielectric tangent of the thermosetting adhesive composition of Comparative Example 5 because it did not contain component (A).

[0126] It was found that the thermosetting adhesive composition of Comparative Example 6 had a high content of component (B) of more than 10 parts by mass, and therefore had poor peel strength and flex resistance.

[0127] It was found that the thermosetting adhesive composition of Comparative Example 7 did not contain a styrene-based elastomer with a styrene ratio of less than 67%, and therefore did not have good peel strength and flex resistance.

[0128] Since the thermosetting adhesive composition of Comparative Example 8 did not contain a radical polymerization initiator, it was difficult to reduce the dielectric tangent at 80°C, it was also difficult to suppress the rate of change of the dielectric tangent with temperature, and it was found that the heat resistance was not good.

[0129] It was found that the thermosetting adhesive composition of Comparative Example 9 had poor peel strength and flex resistance because the total content of the (A) component and the (B) component exceeded 25 parts by mass.

[0130] The thermosetting adhesive composition of Comparative Example 10 had a high styrene-based elastomer content of more than 90 parts by mass, and therefore had relatively low contents of components (A) and (B). As a result, it was found that it was difficult to reduce the dielectric tangent at 80°C, it was also difficult to suppress the rate of change of the dielectric tangent with temperature, and the heat resistance was also poor.

[0131] In the thermosetting adhesive composition of Comparative Example 11, the content of the styrene-based elastomer was low, less than 65 parts by mass, and in addition, the total content of the radical polymerization initiator, epoxy resin, and epoxy resin curing agent was high, exceeding 10 parts by mass. Therefore, it was found that it was difficult to reduce the dielectric constant and dielectric tangent, and also difficult to suppress the rate of change of the dielectric tangent with temperature.

[0132] In the thermosetting adhesive composition of Comparative Example 12, the total content of the radical polymerization initiator, epoxy resin, and epoxy resin curing agent was high, exceeding 10 parts by mass, and it was therefore difficult to reduce the dielectric constant and dielectric tangent, and it was also difficult to suppress the rate of change of the dielectric tangent with temperature.

[0133] The thermosetting adhesive composition of Comparative Example 13 did not contain component (A), in other words, it used a polyphenylene ether resin having a hydroxyl group rather than a radically polymerizable group at the molecular end. As a result, the condition of the film was poor and it was found that evaluations (dielectric constant, dielectric tangent, peel strength, rate of change of dielectric tangent with temperature, heat resistance, and flex resistance) could not be performed. [Explanation of symbols]

[0134] 1 printed wiring board, 2 Liquid crystal polymer film, 3 copper foil, 4 Liquid crystal polymer film, 5. A cured layer made of an adhesive composition; 6 printed wiring board, 7 polyimide layer, 8 copper foil, 9 Copper plating layer, 10 Coverlay, 11 TEG, 12 test pieces, 13 MIT folding fatigue test machine, 14 plunger, 15 Upper chuck, 16 Rotating chuck, 17 Folding frame

Claims

1. A thermosetting adhesive composition for bonding substrates, comprising: Relative to a total of 100 parts by mass of the thermosetting adhesive composition, 65 to 90 parts by mass of a styrene-based elastomer having a styrene ratio of 42% or less; As a cross-linking component, (A) 5 to 20 parts by mass of a modified polyphenylene ether resin having a radical polymerizable group at a molecular end, (B) 4 to 10 parts by mass of polybutadiene and / or polyisoprene having a weight average molecular weight of 10,000 to 50,000; A radical polymerization initiator; An epoxy resin is included, the total content of the radical polymerization initiator, the epoxy resin, and the epoxy resin curing agent is 10 parts by mass or less; A thermosetting adhesive composition, wherein the total content of the component (A) and the component (B) is 25 parts by mass or less.

2. The dielectric tangent after curing is less than 0.0030 at both 23°C and 80°C, The thermosetting adhesive composition according to claim 1 , wherein the rate of change represented by the following formula 1 is less than 50%. Equation 1: Rate of change (%)=((dielectric loss tangent of the cured thermosetting adhesive composition at 80° C.) / (dielectric loss tangent of the cured thermosetting adhesive composition at 23° C.)−1)×100

3. 3. The thermosetting adhesive composition according to claim 1, wherein the content of the component (A) and the content of the component (B) satisfy the following formula 2. Equation 2: (Content of component (A) in the thermosetting adhesive composition)>(Content of component (B) in the thermosetting adhesive composition)

4. 3. The thermosetting adhesive composition according to claim 1, wherein the content of the epoxy resin is less than 5 parts by mass.

5. The thermosetting adhesive composition according to claim 2 , wherein the rate of change represented by the above formula 1 is less than 30%.

6. The thermosetting adhesive composition according to claim 1 or 2, further comprising an epoxy resin curing agent.

7. 3. The thermosetting adhesive composition according to claim 1, wherein the radical polymerization initiator is an organic peroxide having a decomposition temperature of 170°C or higher that results in a half-life of 1 minute.

8. 3. The thermosetting adhesive composition according to claim 1, wherein the styrene-based elastomer contains a styrene-based elastomer having a functional group that accelerates the curing reaction of the epoxy resin.

9. A thermosetting adhesive sheet comprising a substrate and an adhesive layer formed on the substrate, the adhesive layer comprising the thermosetting adhesive composition according to claim 1 or 2.

10. A printed wiring board, comprising a resin substrate with wiring, the resin substrate comprising a substrate and a wiring pattern, and a coverlay laminated on the wiring pattern side of the resin substrate via a cured product of the thermosetting adhesive composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Elastomer composition, film and semiconductor device

    JP2015131866A

  • Adhesive composition, thermosetting adhesive sheet and printed wiring board

    JP7351912B2

  • Adhesive composition, thermosetting adhesive sheet, and printed wiring board

    WO2019151014A1

  • Adhesive composition, thermally curable adhesive sheet, and printed wiring board

    WO2021024364A1

  • Resin composition, production method therefor, adhesive film, and bonding sheet for interlaminar bonding

    WO2022255078A1