Polymer composite thin film and method for producing the same

The polymer composite thin film combines a self-supporting polymer thin film with cellulose nanofibers to enhance mechanical strength and functionality, addressing the trade-off in existing technologies and enabling efficient gas and air separation.

JP7570634B2Active Publication Date: 2024-10-22NANOMEMBRANE TECHNOLOGIES INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021055885
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-31
Filing Date
2021-03-29
Publication Date
2024-10-22
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Existing polymer composite thin films face a trade-off between mechanical strength and functionality, particularly in gas separation membranes, where thin layers compromise mechanical strength and thick layers reduce permeability, and the manufacturing process is complex due to rapid ligand exchange reactions.

Method used

A polymer composite thin film is developed by combining a self-supporting polymer thin film with a fibrous structure, specifically cellulose nanofibers, to achieve high mechanical strength and functionality while maintaining a thickness of 100 nm or less, using polysiloxane and crosslinkable polymers like epoxy resin.

Benefits of technology

The resulting film exhibits high mechanical strength, gas separation properties, and cost-effectiveness, with improved gas permeability and selectivity, suitable for applications like gas separation and air separation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570634000004
    Figure 0007570634000004
  • Figure 0007570634000005
    Figure 0007570634000005
  • Figure 0007570634000006
    Figure 0007570634000006
Patent Text Reader

Abstract

To provide a polymer composite thin film 1 comprising a high gas separation function by being formed extremely thin, by a more simplified structure in which, a nano film having flexible functionality and a nano support medium excellent in mechanical strength are combined (conjugated), and comprising practical structure stability (self standing properties).SOLUTION: There is provided a polymer composite thin film 1 in which, a polymer thin film 2 whose thickness is equal to or smaller than 100 nm is conjugated to a fibrous structure (cellulose nanofiber 3) having a diameter smaller than the thickness of the polymer thin film 2, therefore the polymer composite thin film having self standing properties, can be acquired.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymer composite thin film that mainly contains a polymer material, and in particular to a polymer composite thin film that has high functionality and significantly improved film strength. [Background technology]

[0002] Recently, interest in organic and inorganic nanofilms has been growing. In the inorganic field, the unique physical properties of graphene, an inorganic carbon compound, have attracted worldwide attention, and the international competition to develop them has suddenly intensified. This trend is further fueled by the development of MoS 2 This has now expanded to other inorganic materials with nanometer thickness, giving rise to a new field of research into two-dimensional materials.

[0003] On the other hand, in the case of organic systems, there has been a huge amount of research on biomembranes with nano-order thickness from the standpoint of biochemistry and biophysics. In addition, organic nanomembranes as industrial materials are expected to have unique properties as two-dimensional materials, but in order to promote practical use, it is necessary to realize large areas, no defects, self-supporting properties, structural stability, etc.

[0004] As an example of organic nanomembranes as industrial materials, there are high hopes for the development of excellent separation membranes that take advantage of nano-order thicknesses. In order to maximize the separation function of a separation membrane, it is desirable to make the membrane as thin as possible in order to ensure high permeability. However, in that case, there is a high possibility that the mechanical strength will decrease and the membrane will become fragile and not withstand practical use. In other words, there is a trade-off between making the separation membrane thin from a functional perspective and its mechanical strength. To solve this problem, it is thought to be effective to combine a functional membrane that is as thin as possible with a strong support and skeletal structure that does not interfere with its function.

[0005] As a technology relating to such a polymer composite thin film, there is a gas separation membrane having a gas separation layer containing a crosslinked cellulose resin and cellulose nanofibers, in which the crosslinked cellulose resin has, in the crosslinked structure, * -OMO-* , * -SMS- * , * -NR a C(=O)- * , * -NR b C(=O)NR b - * , * -O-CH 2 -O- * , * -S-(CH 2 ) 2 -S- * , * -OC(=O)O- * , * -SO 3 - N + (R c ) 3 - * and * -P(=O)(OH)O - N + (R d ) 3 - * A gas separation membrane having at least one linking structure selected from the group consisting of: a , R b , R c and R d each independently represents a hydrogen atom or an alkyl group. * indicates a linking site.) is known. (Patent Document 1)

[0006] According to Patent Document 1, by forming a gas separation membrane in which a gas separation layer is formed using a crosslinked cellulose resin having a specific linking structure in the crosslinked structure, it is possible to provide a gas separation membrane that has excellent gas permeability as well as excellent gas separation selectivity, is resistant to plasticization even when used under high temperature, high pressure and high humidity conditions, exhibits excellent gas separation performance, is less susceptible to the effects of toluene and the like, which is an impurity component present in natural gas, has excellent folding resistance, can be processed into various module shapes, can be manufactured with a high yield, and further exhibits stable gas separation performance from the beginning of use. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6349026 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0008] However, according to the technology described in Patent Document 1, cellulose nanofibers may be added to the gas separation layer constituting the gas separation membrane, and the thickness of the gas separation layer is preferably 50 nm to 1 μm, but it is assumed that the gas separation layer containing the crosslinked cellulose resin is formed on the upper side of a gas permeable support layer (porous layer). More specifically, a composite membrane having both a gas separation layer and a porous layer is formed by applying a coating liquid (dope) containing the components constituting the gas separation layer (cellulose resin and crosslinking agent) to at least the surface of a porous support. With this configuration, the thickness of the gas separation membrane is ultimately 10 μm to 200 μm.

[0009] In other words, the gas separation layer described in Patent Document 1 functions as a gas separation membrane by being formed on a porous layer, and there is no suggestion that the gas separation layer having a nano-order thickness can stand on its own to form a gas separation membrane, or that this gas separation membrane can exhibit a gas separation function.

[0010] In addition, the porous layer is composed of, for example, a porous membrane of an organic polymer, but no mention is made of the gas permeability of the parts of the porous layer other than the pores, and the presence of the porous layer may reduce the overall gas permeability of the gas separation membrane.

[0011] Furthermore, in the gas separation membrane described in Patent Document 1, in order to construct the gas separation layer from a crosslinked cellulose resin having a specific linking structure in the crosslinked structure, a specific metal complex is used as a crosslinking agent, and a metal bridge is formed by a ligand exchange reaction with the cellulose resin. In this case, the concentration of the cellulose resin and the metal complex as a crosslinking agent in the coating solution is set to a certain level or less to suppress the ligand exchange reaction in the coating solution, and further, by coating this coating solution on a porous support layer as a thin film, the ligand exchange reaction is quickly promoted with the rapid evaporation of the solvent, forming a metal bridge structure in the cellulose resin. This makes the microstructure of the gas separation layer complex, and as a result, the manufacturing process is also complex.

[0012] The present invention has been devised to solve such problems with the conventional technology, and aims to provide a polymer composite thin film that is highly functional and has practical structural stability (self-supporting ability) by being constructed extremely thin, through a simpler configuration that combines (combines) a nanomembrane with flexible functionality with a nanosupport with excellent mechanical strength. [Means for solving the problem]

[0013] The present invention, made to solve the above problems, is a polymer composite thin film characterized in that a polymer thin film having a thickness of 100 nm or less is composited with a fibrous structure having a diameter smaller than the thickness of the polymer thin film, and thus has self-supporting properties.

[0014] This makes it possible to obtain a polymer composite thin film that combines high functionality with high mechanical strength, even if the polymer thin film is not self-supporting.

[0015] The present invention also relates to a polymer composite thin film in which a self-supporting polymer thin film with a thickness of 100 nm or less is composited with a fibrous structure having a diameter smaller than the thickness of the polymer thin film.

[0016] This makes it possible to obtain a polymer composite thin film having both high functionality and high mechanical strength, when the polymer thin film itself is self-supporting.

[0017] In the present invention, the fibrous structure is composed of an organic polymer.

[0018] This makes it possible to produce the polymer composite thin film at lower cost.

[0019] Furthermore, the present invention relates to a fibrous structure in the form of a cellulose nanofiber.

[0020] This makes it possible to produce polymer composite thin films at lower cost, since the material cost of cellulose nanofibers is extremely low.

[0021] In the present invention, the polymer thin film is mainly composed of polysiloxane.

[0022] This makes it possible to obtain a polymer composite thin film having superior mechanical strength, since a thin film made of polysiloxane generally has self-supporting properties.

[0023] In the present invention, the polymer thin film is mainly composed of a crosslinkable polymer.

[0024] This makes it possible to obtain a polymer composite thin film having high functionality and high mechanical strength even by using a crosslinkable polymer such as an epoxy resin, which is a more common polymer material.

[0025] In the present invention, the polymer thin film has gas separating properties.

[0026] This allows the polymer composite membrane to remove selected gases from the atmosphere.

[0027] In the present invention, the polymer thin film is selectively permeable to carbon dioxide.

[0028] This makes it possible to remove (separate) carbon dioxide from a gas using a thin polymer composite membrane.

[0029] In the present invention, the thin polymer film separates oxygen and nitrogen in the air.

[0030] This enables the polymer composite thin film to function as an air separation membrane, increasing or decreasing the oxygen or nitrogen concentration in the air. Effect of the Invention

[0031] As described above, according to the present invention, it is possible to obtain a polymer composite thin film having high functionality and high mechanical strength. [Brief description of the drawings]

[0032] [Figure 1] 1(a) to 1(d) are explanatory diagrams showing the structure of a polymer composite thin film 1 according to the present invention. [Diagram 2] Photographs (a) to (d) show the deflection of the films obtained in Comparative Example 1 and Example 1 when the same load was applied. [Diagram 3] Graph showing the relationship between stress (σ) and deflection (ε) in the films obtained in Comparative Example 1 and Example 1 [Figure 4] Photograph showing the appearance of a CNF / PDMS film with circular damage DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] 1(a) to (d) are explanatory diagrams showing the configuration of a polymer composite thin film 1 according to the present invention. Hereinafter, an embodiment of the present invention will be described with reference to Fig. 1. The polymer composite thin film 1 is composed of a polymer thin film 2 and cellulose nanofibers 3 as fibrous structures.

[0034] 1(a) to (d), the polymer composite thin film 1 has a configuration in which cellulose nanofibers 3 are contained within the polymer thin film 2. Specifically, as shown in FIGS. 1(a) and 1(b), the cellulose nanofibers 3 may be all contained within the polymer thin film 2 and be unevenly distributed on one side of the surface of the polymer thin film 2, as shown in FIG. 1(c), the cellulose nanofibers 3 may be partly exposed to the outside of the polymer thin film 2, or as shown in FIG. 1(d), the cellulose nanofibers 3 may be all contained within the polymer thin film 2 and be uniformly dispersed within the polymer thin film 2.

[0035] Thus, the polymer composite thin film 1 of this embodiment has a configuration in which the polymer thin film 2 and the cellulose nanofibers 3 are composited. The cellulose nanofibers 3, which are organic polymers, form fibrils as small fibers (fibrous structures). Fibrils as a material have high mechanical strength, and by being composited with the polymer thin film 2, the polymer composite thin film 1 exhibits extremely high mechanical strength. Furthermore, the cellulose nanofibers 3 are produced at low cost by mechanical defibration from abundant resources such as wood, and furthermore, being a plant fiber, they are an environmentally friendly material.

[0036] Suitable materials for forming the polymer thin film 2 include, for example, vinyl polymers, polysiloxanes, and cross-linked polymers. It is believed that vinyl polymers and polysiloxanes alone are unable to ensure the mechanical strength (self-supporting ability) at a film thickness (for example, 100 nm or less) at which functionality such as gas separation can be effectively exhibited. In this case, by combining the polymer thin film 2 mainly composed of vinyl polymers or polysiloxanes with cellulose nanofibers 3, it is possible to achieve both functionality and self-supporting ability of the polymer composite thin film 1 composed of these components.

[0037] On the other hand, crosslinked polymers are considered to be able to stand on their own as materials even at a film thickness where their functionality can be effectively exerted (for example, 100 nm or less, similar to vinyl polymers and polysiloxanes). Here, a crosslinked polymer (crosslinked polymer) refers to a polymer that has a three-dimensional network structure (crosslinked structure) formed by bonding multiple linear polymer chains through a chemical reaction, and includes, for example, epoxy resins in which epoxy groups and amino groups as functional groups are crosslinked through a chemical reaction.

[0038] As for epoxy resin, an example of a self-supporting polymer thin film with a thickness of 20 nm is given in "A Large, Freestanding, 20nm Thick Nanomembrane Based on an Epoxy Resin, H. Watanabe T. Kunitake, Volume19, Issue7, Pages 909-912, 2007." (https: / / onlinelibrary.wiley.com / doi / abs / 10.1002 / adma.200601630) It is published in.

[0039] By combining a polymer thin film 2 mainly composed of a crosslinkable polymer with cellulose nanofibers 3, it becomes possible to obtain a polymer composite thin film 1 composed of these components that has functionality as well as greater mechanical strength.

[0040] In this embodiment, the thickness D2 of the polymer thin film 2 is set to 100 nm or less. By setting the thickness D2 of the polymer thin film 2 to 100 nm or less, it is possible to significantly improve the functionality (here, gas separation performance) of the polymer composite thin film 1. Furthermore, in this embodiment, the thickness D1 of the polymer composite thin film 1 is also set to 100 nm or less.

[0041] In other words, in the configurations of Figures 1(a), (b), and (d), the polymer thin film 2 that completely encapsulates the cellulose nanofibers 3 within the membrane is the polymer composite thin film 1 itself, so the thickness D1 of the polymer composite thin film 1 = the thickness D2 of the polymer thin film 2.In the configuration in which part of the cellulose nanofibers 3 are exposed from the polymer thin film 2 as in Figure 1(c), the thickness D1 of the polymer composite thin film 1 > the thickness D2 of the polymer thin film 2.

[0042] The cellulose nanofibers 3 have a diameter (for example, 4 nm to 90 nm) smaller than the thickness of the polymer thin film 2. By making the diameter of the cellulose nanofibers 3 smaller than the thickness of the polymer thin film 2, the functionality of the polymer thin film 2 is fully exhibited. Conversely, if the diameter of the cellulose nanofibers 3 is made larger than the thickness of the polymer thin film 2, the substantial surface area of ​​the film is reduced, making it difficult to exhibit the functionality.

[0043] In Figure 1, the cellulose nanofibers 3 of the same fiber length are depicted as if aligned in a specific direction, but this is merely a schematic depiction. In reality, the fiber lengths of the cellulose nanofibers 3 vary (5 μm or more), and the cellulose nanofibers 3 are oriented in all directions and are contained in the polymer thin film 2 in a complex entangled state.

[0044] In this embodiment, cellulose nanofibers, which are organic polymers, such as oxidized cellulose nanofibers (oxidized CNF) and a mixture of cellulose nanofibers 3 and oxidized cellulose nanofibers can be preferably used as the fibrous structure, but other organic polymers may also be used as the fibrous structure. Examples of other organic polymers that can be used include polymers produced by manufacturing methods such as electrospinning, fibrin, which is a protein formed by bundling fine fibers and is involved in blood clotting, peptides, collagen, etc., and further, deoxyribonucleic acid (DNA) and ribonucleic acid (RNA) may also be used.

[0045] Here, for example, when DNA is used as the fibrous structure, since DNA is a fiber with a diameter of 2 nm, if the thickness of the polymer composite thin film 1 is greater than 2 nm, it is possible to achieve both functionality and mechanical strength. That is, the thickness of the polymer composite thin film 1 according to the present invention can be in the range of 2 nm to 100 nm by selecting the fibrous structure. Even when the fibrous structure is limited to cellulose nanofibers 3, the thickness can be in the range of 4 nm to 100 nm. EXAMPLES

[0046] Hereinafter, Example 1 of the present invention will be described. First, a CNF dispersion containing 0.11 weight percent cellulose nanofibers 3 (hereinafter sometimes referred to as "CNF") (manufactured by Chuetsu Pulp Industries, Nanoforest-S (Nanoforest is a registered trademark)) was prepared, and ion-exchanged water was added to this to prepare an aqueous CNF solution with a specified CNF concentration, which was used in the subsequent operations.

[0047] Separately, a base resin of polydimethylsilicone (PDMS) resin (a type of polysiloxane, SYLGARD184 (SYLGARD is a registered trademark) manufactured by Dow Corning Toray) and a curing agent were mixed in a ratio of 10:1, and hexane was added to this to prepare a 10 weight percent PDMS / hexane solution. A predetermined amount of hexane was added to this to prepare PDMS / hexane solutions of different concentrations, which were used in the subsequent operations.

[0048] Prior to the preparation of polymer composite thin film 1, a polyhydroxystyrene (PHS) / ethanol solution (15 weight percent) was first spin-coated (3,000 rpm / 1 min) onto a glass substrate to form a PHS layer, which was then dried. The substrate was then treated with oxygen plasma to make the surface hydrophilic.

[0049] The CNF aqueous solution prepared by the above procedure was spin-coated onto this substrate, and then the PDMS / hexane solution was spin-coated, and the substrate was then heated at 100° C. for 30 minutes.

[0050] After cooling to room temperature, the substrate was immersed in ethanol (a stripping solution), and the film was peeled off from the substrate in the stripping solution. The film thus obtained (polymer composite thin film 1) is hereafter referred to as a CNF / PDMS film. This CNF / PDMS film was fixed to a concentric circular frame made of Kapton film, and the film was removed from the stripping solution. It was visually confirmed that the CNF / PDMS film fixed to the concentric circular frame had no defects and was self-supporting.

[0051] In addition, for use in the bulge test described below, several samples were obtained by varying the number of times the spin coating operation of the CNF aqueous solution (hereinafter sometimes referred to as "CNF spin coating operation") was performed in the above-mentioned process.

[0052] As Comparative Example 1, a film was prepared in which a PDMS layer was formed directly on a glass substrate coated with PHS without performing the CNF spin coating operation. This film is hereinafter referred to as the PDMS film.

[0053] The mechanical strength of the film prepared as Example 1 and Comparative Example 1 was evaluated by a bulge test. The films used in the test were four types: (i) a PDMS film as Comparative Example 1, and (ii) a film obtained by performing a CNF spin coating operation once and then spin coating PDMS thereon (CNF / PDMS film) as samples prepared in Example 1, (iii) a film obtained by performing a CNF spin coating operation five times and then spin coating PDMS thereon (CNF-5 / PDMS film), and (iv) a film obtained by performing a CNF spin coating operation ten times (CNF-10 / PDMS film).

[0054] The thicknesses of the polymer composite thin films 1 (ii) to (iv) prepared in Example 1 were all 100 nm or less, specifically in the range of 50 nm to 75 nm. The PDMS film (i) as Comparative Example 1 was exceptionally formed to a thickness of 150 nm. This is because if the thickness of the PDMS film (i) was set to 50 nm to 75 nm, similar to the other samples obtained in Example 1, it would break immediately when taken out into air (it would not be self-supporting), and therefore comparison with Example 1 would not be possible.

[0055] The samples prepared in Comparative Example 1 and Example 1 were attached to the bottom surface of a cylindrical glass tube, and ion-exchanged water was dropped from the top of the glass tube to load the weight on the film. The stress (σ) and strain (ε) were calculated from the shape of the film expanded (warped) due to the weight load.

[0056] 2(a) to (d) are photographs showing the deflection of the films obtained in Comparative Example 1 and Example 1 when the same load was applied to them. Specifically, the film deflection was observed when the same load (water: 3.5 mL introduced, liquid pressure: about 437 Pa) was applied to Comparative Example 1 and Example 1. Here, FIG. 2(a) shows the state of the PDMS film, FIG. 2(b) shows the state of the CNF / PDMS film, FIG. 2(c) shows the state of the CNF-5 / PDMS film, and FIG. 2(d) shows the state of the CNF-10 / PDMS film.

[0057] Fig. 3 is a graph showing the relationship between stress (σ) and deflection (ε) in the films obtained in Comparative Example 1 and Example 1. Specifically, Fig. 3 shows the relationship between stress (σ) and deflection (ε) calculated from the load pressure, film radius, film thickness, deflection length, and film arc length when deflected for each film.

[0058] 2 and 3, the film obtained in Example 1 in which CNF and PDMS are layered (having the configuration shown in any one of Figs. 1(a) to (c) depending on the manufacturing conditions) clearly shows a difference in the film deflection when subjected to a water pressure load, with the amount of deflection decreasing as the amount of CNF introduced increases. Furthermore, as the number of CNF layers increases, the stress also increases (and conversely, the deflection decreases), confirming that the introduction of CNF improves the mechanical strength of the entire film.

[0059] Figure 4 is a photograph showing the appearance of a CNF / PDMS film on which circular damage had occurred. The circular damage was created by piercing the CNF / PDMS film with a needle with a sharp tip. As shown in Figure 4, even when some kind of external damage was inflicted on this CNF / PDMS film, the damage was limited to a part of the film and did not spread over the entire film. Furthermore, the same was true when circular damage was induced on the CNF-5 / PDMS film and the CNF-10 / PDMS film.

[0060] On the other hand, when such damage is formed in a PDMS film, the entire film instantly shrinks and breaks, and the film structure cannot be maintained. Considering this together with the other evaluation results of Example 1, it can be determined that CNF is present in the obtained polymer composite thin film 1. 2 and N 2 The selectivity for both was about 10. 2 / N 2 Considering that the selectivity is about 10 to 11 (Reference: Shigenori Fujikawa, Miho Ariyoshi, Roman Selyanchyn, Toyoki Kunitake, Chemistry Letters, 2019, Vol. 48, No. 11, 1351-1354), it can be said that none of the films produced have defects that would cause gas leaks. EXAMPLES

[0061] Example 2 of the present invention will be described below. Ion-exchanged water was further added to the CNF dispersion liquid with 0.11 weight percent CNF prepared in Example 1 to prepare diluted solutions with different CNF concentrations. CNF / PDMS films were produced using the prepared diluted solutions. The thickness of the CNF / PDMS films as the polymer composite thin film 1 obtained in Example 2 was about 50 nm to 75 nm in each case.

[0062] The CNF / PDMS film and the PDMS film were placed on a porous polyacrylonitrile film and a gas permeation test was performed. 2 ) and nitrogen (N 2 ) and CO 2 / N 2 The selectivity and the PDMS selectivity are shown in Table 1. The results of the gas permeability test of the PDMS film are shown in the leftmost column of Table 2, which will be described later. [Table 1]

[0063] The same selectivity was observed in all the CNF / PDMS films prepared in Example 2, which indicates that all the films obtained were free of defects that would cause gas leakage. 2 And N 2 The permeability is lower than that of a PDMS film of similar thickness (approximately 50 nm, as described below). Considering that films made of CNF generally have low gas permeability, it is supported that CNF is also introduced into this film. EXAMPLES

[0064] Example 3 of the present invention will be described below. A CNF / ethanol dispersion was prepared so that the content of cellulose nanofiber 3 (CNF) (manufactured by Chuetsu Pulp Industry Co., Ltd., Nanoforest-S) was 0.072 weight percent.

[0065] Separately, the base resin and curing agent of commercially available polydimethylsilicone (PDMS) resin (Toray Dow Corning, SYLGARD 184) were mixed in a volume ratio of 10:1, and the previously prepared CNF / ethanol dispersion and hexane were added to this to prepare a 0.5 volume percent CNF / PDMS / hexane solution, which was used in the subsequent operations.

[0066] Next, a polyhydroxystyrene (PHS) / ethanol solution (15 weight percent) was spin-coated (3000 rpm / 1 min) onto a glass substrate, and after forming a PHS layer, the substrate was treated with oxygen plasma to make the surface hydrophilic. The CNF / PDMS / hexane solution prepared above was dropped onto the substrate, and the substrate was rotated at 4000 rpm for 1 min, and then heated at 100°C for 30 min.

[0067] After cooling to room temperature, the substrate was immersed in ethanol and the film was peeled off from the substrate. The film thus obtained is hereafter referred to as a CNF-PDMS film. This CNF-PDMS film is composed of polydimethylsilicone resin in which CNF is evenly dispersed, and has a different structure from the CNF / PDMS film (in which CNF and PDMS form a layer) described in Example 1 and the like. That is, the CNF-PDMS film obtained in Example 2 has the structure shown in FIG. 1(d).

[0068] This CNF-PDMS film was placed on a porous polyacrylonitrile film and a gas permeation test was performed. As Comparative Example 2, a film (PDMS film) was also produced using only SYLGARD184 as the raw material without mixing cellulose nanofibers 3.

[0069] CO of films made with different film solution concentrations 2 and N 2 permeability and CO 2 / N 2 The permeation selectivity is shown in Table 2. That is, Table 2 shows the relationship between the amount of CNF dispersion mixed and the properties of the obtained CNF-PDMS films (No. 1 to No. 5). [Table 2]

[0070] Here, the presence or absence of self-supporting ability is judged based on whether or not the thin film (film) can maintain its flat membrane shape without breaking when it is peeled off from the substrate in the stripping solution and then pulled up into the air while floating in the solution. In other words, if the membrane structure is maintained without breaking even in the air, it is judged as "self-supporting," and if the membrane structure is maintained while floating in the stripping solution after the substrate is peeled off, but it easily breaks when taken out into the air, it is judged as "not self-supporting" (listed as "easily breaks in air" in [Table 2]).

[0071] It should be noted that the limit for a PDMS film to be self-supporting is a film thickness of about 150 nm, and any thinner film will result in an extremely high rate of film rupture. Therefore, for the PDMS films in [Table 2], the thin film was not lifted up into the air, but instead was scooped up onto a porous polyacrylonitrile film in a release solution and used for gas permeation testing.

[0072] The films produced in Example 3, including the PDMS film, all had a thickness of about 50 nm. As described above, the PDMS film without CNF mixed in could not maintain a flat membrane shape by itself and was broken by shrinkage, so that no flat membrane having the self-supporting property that can be used for gas permeation testing was obtained, but all of the films mixed with CNF were self-supporting. EXAMPLES

[0073] Example 4 of the present invention will be described below. In Example 4, a crosslinkable polymer is used as the polymer material constituting the polymer thin film 2. First, an aqueous dispersion of cellulose nanofiber 3 (CNF) (Nanoforest-S, Chuetsu Pulp Industry Co., Ltd.) was prepared to have a concentration of 0.11 weight percent, and this was used in the subsequent operations.

[0074] In addition, a PCGF-PEI / chloroform solution was prepared containing 4 weight percent of poly[(o-cresyl glycidyl eter)-co-formaldehyde] (hereinafter sometimes referred to as "PCGF") (ALDRICH, Mn 870) and polyethylenimine, branched (hereinafter sometimes referred to as "PEI") (ALDRICH, Mn ~ 10,000) as crosslinkable polymers (epoxy resins). After stirring this solution for 4 hours at 40°C, further chloroform was added to prepare a 1 weight percent PCGF-PEI / chloroform solution, which was used in the subsequent operations.

[0075] A polyhydroxystyrene (PHS) / ethanol solution (15 weight percent) was spin-coated (3000 rpm / 1 min) onto a glass substrate, and after forming a PHS layer, the substrate was treated with oxygen plasma to hydrophilize the surface. The CNF aqueous dispersion prepared above was spin-coated (1500 rpm, 2 min) onto the substrate, and the substrate was heated at 100°C for 1 min.

[0076] Next, the substrate was spin-coated (3000 rpm, 1 min) with the 1 weight percent PCGF-PEI / chloroform solution prepared above. The substrate was then heated at 100°C for 5 min. After cooling to room temperature, the substrate was immersed in ethanol, and the film (polymer composite thin film 1) was peeled off from the substrate. The thickness of the film obtained in Example 4 was 75 nm.

[0077] It was visually confirmed that the polymer composite thin film 1 obtained in Example 4 had no defects and was self-supporting. In addition, a test was performed to apply a water pressure load in the same manner as described in Example 1. As a result, the amount of deflection decreased with an increase in the amount of CNF introduced. EXAMPLES

[0078] Example 5 of the present invention will be described below. In Example 5, instead of the above-mentioned CNF aqueous solution, a 0.05 wt% CNF+oxidized CNF aqueous solution in which equal amounts of CNF and oxidized CNF (oxidized cellulose nanofiber) were mixed was used, and the PDMS concentration of the PDMS / hexane solution was set to 0.5 v / v%. Furthermore, the spin coating operation of the CNF+oxidized CNF aqueous solution was performed only once, and a film (CNF+oxidized CNF / PDMS film) was produced using the same process as in Example 1. When the cross section of the produced film was observed with a scanning electron microscope, the film thickness of the CNF+oxidized CNF / PDMS film was 30 nm.

[0079] This CNF + oxidized CNF / PDMS film was placed on a porous polyacrylonitrile film and a gas permeation test was performed. 2 ), nitrogen (N 2 ) and oxygen (O 2 ) and CO 2 / N 2 , CO 2 / O 2 and O 2 / N 2 The selectivity ratio is shown in Table 3. [Table 3]

[0080] As shown in Table 3, the CNF+oxidized CNF / PDMS film of Example 5 also showed no significant difference in the amount of CO 2 The transmittance of O is very large. 2 and N 2 The transmittance of O is also high. 2 and N 2 Focusing on O 2 / N 2 The selectivity ratio was 2.3, clearly indicating that the CNF+oxidized CNF / PDMS film has the air separation function of separating oxygen and nitrogen in the air. That is, the polymer composite thin film 1 according to the present invention functions as an air separation membrane and can increase or decrease the oxygen concentration or nitrogen concentration in the air.

[0081] The air separation function of the CNF + oxidized CNF / PDMS film is exerted by a layer composed of PDMS (polymer thin film, hereafter sometimes referred to as the "PDMS layer"), but as the thickness of the PDMS layer increases, the permeability decreases, which becomes a practical barrier. However, by combining the PDMS layer with a layer composed of CNF (or CNF + oxidized CNF), the mechanical strength is improved, making it possible to make the PDMS layer in the polymer composite thin film 1 as thin as possible.

[0082] In Example 5, as described above, the thickness of the CNF+oxidized CNF / PDMS film was 30 nm, and the thickness of the PDMS layer excluding the thickness of the layer composed of CNF+oxidized CNF is thought to be about 10 nm to 20 nm. By making the PDMS layer extremely thin in this way, a high O of over 1000 GPU (3000 GPU) was achieved. 2 and N 2 It is possible to achieve a high degree of transparency.

[0083] Incidentally, since the polymer composite thin film 1 shown in Examples 1 to 3 also contains a thinned PDMS layer, it is clear that these polymer composite thin films 1 have an air separation function. [Industrial Applicability]

[0084] The polymer composite thin film 1 according to the present invention has high functionality and high mechanical strength, and therefore can be used to reduce greenhouse gases such as CO 2 The polymer composite thin film 1 according to the present invention can be suitably applied to gas separation membranes and the like used in CCS (Carbon dioxide Capture and Storage) for separating and recovering carbon dioxide from sources such as power plants and factories. The polymer composite thin film 1 according to the present invention can be suitably applied to oxygen enrichment devices that utilize air with high oxygen concentration (air with low nitrogen concentration), high-concentration oxygen masks, plant factories, oxygen combustion power plants, oxygen combustion boilers, and the like, as well as inert gas fire extinguishing systems that utilize air with high nitrogen concentration (air with low oxygen concentration). [Explanation of symbols]

[0085] 1 Polymer composite thin film 2 Polymer thin film 3. Cellulose nanofiber 10 Circular injury

Claims

1. A non-self-supporting polymer thin film composed of polysiloxane and having a thickness of 100 nm or less; A fibrous structure having a diameter smaller than the thickness of the polymer thin film and contained in the polymer thin film; Equipped with The polymer composite thin film is characterized in that the fibrous structure and the polymer thin film are combined to have self-supporting properties, and the film thickness is 2 nm to 100 nm.

2. The polymer composite thin film according to claim 1 , wherein the fibrous structures are composed of an organic polymer.

3. 3. The polymer composite thin film according to claim 2, wherein the fibrous structure is a cellulose nanofiber or a mixture of a cellulose nanofiber and an oxidized cellulose nanofiber.

4. The polymer composite thin film according to any one of claims 1 to 3, characterized in that the polymer thin film has a gas separating property.

5. 5. The polymer composite thin film according to claim 1, wherein the polymer thin film is highly selectively permeable to carbon dioxide.

6. 6. The polymer composite thin film according to claim 1, wherein the total thickness of the polymer thin film and the fibrous structures is 30 nm to 75 nm.

7. The polymer composite thin film according to claim 3 , comprising: a layer composed of the polysiloxane; and a layer composed of the polysiloxane and the cellulose nanofibers.

8. The polymer composite thin film described in Claim 7, characterized in that the layer composed of the polysiloxane and the cellulose nanofiber is composed of multiple layers of the cellulose nanofiber superimposed on top of each other.

9. A method for producing a polymer composite thin film according to any one of claims 3 to 8, comprising the steps of: The fibrous structure is a cellulose nanofiber, A first step of preparing a cellulose nanofiber solution containing the cellulose nanofibers and a polymer material-containing solution containing the polysiloxane; A second step of forming a first layer by applying the cellulose nanofiber solution onto a substrate on which a polymer layer that dissolves in a stripping solution has been formed, so as to cover the polymer layer; a third step of applying and heating the polymeric material-containing solution so as to cover the first layer to form a second layer; a fourth step of immersing the substrate in the stripping solution to strip a polymer composite thin film composed of the first layer and the second layer from the substrate; A method for producing a polymer composite thin film, comprising:

10. The method for producing a polymer composite thin film according to claim 9, characterized in that the solvent of the cellulose nanofiber solution is water, and the solvent of the polymer material-containing solution is hexane.

11. The method for producing a polymer composite thin film according to claim 9 or 10, wherein the first layer is formed by repeating the step of applying the cellulose nanofiber solution a plurality of times.

12. A method for producing a polymer composite thin film according to any one of claims 3 to 8, comprising the steps of: The fibrous structure is a cellulose nanofiber, A first step of preparing a cellulose nanofiber dispersion by dispersing the cellulose nanofibers in a first solvent; A second step of mixing the cellulose nanofiber dispersion and a second solvent with the polysiloxane to obtain a mixed solution; a third step of applying the mixed solution to a substrate on which a polymer layer that dissolves in a stripping solution has been formed, and heating the mixed solution so as to cover the polymer layer, thereby forming a polymer composite thin film; a fourth step of immersing the substrate in the stripping solution to strip the polymer composite thin film from the substrate; A method for producing a polymer composite thin film, comprising:

13. 13. The method for producing a polymer composite thin film according to claim 12, wherein the first solvent is ethanol and the second solvent is hexane.

14. The polymer layer is formed by applying an ethanol solution containing polyhydroxystyrene, The method for producing a polymer composite thin film according to any one of claims 9 to 13, characterized in that the stripping solution is ethanol.

15. The method for producing a polymer composite thin film according to any one of claims 9 to 14, characterized in that a surface of the polymer layer is subjected to a hydrophilization treatment.

Citation Information

Patent Citations

  • Culture of malt

    JP1988049026A

  • Nanofiber-reinforced protein porous film

    JP2012075995A

  • Gas separation membrane, and gas separation membrane module

    JP2015160201A

  • Small molecule-based free-standing films and hybrid materials