Boron nitride particles and manufacturing method thereof
The method of introducing boric acid ester and ammonia gases at specific angles into a reactor produces boron nitride particles for heat dissipation members with improved dielectric properties, addressing the need for low dielectric constant and loss tangent in electronic components.
Patent Information
- Application Number
- JP2021562574
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-06
- Filing Date
- 2020-11-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-11-20
AI Technical Summary
Existing heat dissipation members for electronic components require improved characteristics to support increasing signal transmission speeds and capacities, specifically needing a low dielectric constant and low dielectric loss tangent.
A manufacturing method for boron nitride particles involves introducing boric acid ester and ammonia gases separately through multiple introduction ports into a reactor, with specific angles to enhance mixing and reduce particle size variation, followed by heating steps to produce boron nitride particles with controlled size and shape.
The method yields boron nitride particles that can be used to create heat dissipation members with a low dielectric constant and low dielectric loss tangent, enhancing thermal conductivity and insulation properties.
Smart Images

Figure 0007571046000002 
Figure 0007571046000003 
Figure 0007571046000004
Abstract
Description
[Technical field]
[0001] The present invention relates to boron nitride particles and a method for producing the same. [Background technology]
[0002] In electronic components such as transistors, thyristors, and CPUs, efficient dissipation of heat generated during use is an important issue. For this reason, heat dissipation materials with high thermal conductivity are used together with such electronic components. Meanwhile, boron nitride particles have high thermal conductivity and high insulation properties, so they are widely used as a filler in heat dissipation materials.
[0003] For example, Patent Document 1 describes a boron nitride agglomerated particle composition that exhibits high thermal conductivity and is very useful for heat dissipation sheets required for power semiconductor devices, etc., and has an average particle diameter (D 50 ) is a composition of boron nitride agglomerated particles having a particle size of 1 μm to 200 μm, and is characterized in that the composition satisfies certain conditions. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-036190 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, devices equipped with electronic components have become faster in signal transmission and have larger capacity, so heat dissipation materials are also required to have properties that contribute to this. Specifically, heat dissipation materials with low dielectric constant and low dielectric loss tangent are desirable.
[0006] Therefore, an object of the present invention is to obtain boron nitride particles that can realize a heat dissipation member having a low dielectric constant and a low dielectric loss tangent. [Means for solving the problem]
[0007] As a result of investigations conducted by the present inventors, it was found that in a manufacturing method for obtaining boron nitride particles from a borate ester and ammonia, in order to obtain boron nitride particles that can realize a heat dissipation component with a low dielectric constant and a low dielectric tangent, the method of introducing a gas containing a borate ester and ammonia containing gas into a reactor is important.
[0008] One aspect of the present invention is a method for producing boron nitride particles, comprising: a reaction step in which a first gas containing a borate ester and a second gas containing ammonia are separately introduced into a cylindrical reactor from one end face of the reactor, and the borate ester and ammonia are reacted in the reactor at 750°C or higher to obtain a precursor of boron nitride particles; and a heating step in which the precursor of the boron nitride particles is heated at 1000°C or higher to obtain boron nitride particles, wherein in the reaction step, the first gas is introduced into the reactor from two or more inlets, and the second gas is introduced into the reactor from two or more inlets.
[0009] Of the first gases introduced from two or more inlets, the first gas introduced from at least one inlet may be introduced so that the side of the reactor is located on an extension line of the introduction direction of the first gas.
[0010] Of the second gases introduced from two or more inlets, the second gas introduced from at least one inlet may be introduced so that the side surface of the reactor is located on an extension line of the introduction direction of the second gas.
[0011] Another aspect of the present invention is boron nitride particles having an average particle size of 1 μm or less and a difference between the 10% cumulative particle size and the 100% cumulative particle size of 10 μm or less in a volume-based particle size distribution.
[0012] The average circularity of the boron nitride particles may be greater than or equal to 0.8.
[0013] Another aspect of the present invention is a resin composition containing a resin and the above-mentioned boron nitride particles. Effect of the Invention
[0014] According to the present invention, boron nitride particles can be obtained that can realize a heat dissipation member having a low dielectric constant and a low dielectric loss tangent. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a perspective view showing an example of a reactor used in the method for producing boron nitride particles according to an embodiment. [Diagram 2] 2(a) is a side view of the reactor in FIG. 1 as viewed from the first inlet pipe side, and FIG. 2(b) is a side view of the reactor in FIG. 1 as viewed from the second inlet pipe side. [Diagram 3] 1(a) is a side view of a reactor in another embodiment as viewed from a first inlet pipe side, and FIG. 1(b) is a side view of a reactor in another embodiment as viewed from a second inlet pipe side. [Figure 4] FIG. 1(a) is a side view of the reactor in Comparative Example 1 as viewed from the first inlet pipe side, and FIG. 1(b) is a side view of the reactor in Comparative Example 2 as viewed from the first inlet pipe side. [Diagram 5] FIG. 1(a) is a side view of the reactor in Comparative Example 3 as viewed from the second inlet pipe side, and FIG. 1(b) is a side view of the reactor in Comparative Example 4 as viewed from the second inlet pipe side. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] One embodiment of the present invention is a method for producing boron nitride particles, comprising a reaction step of reacting a boric acid ester with ammonia at 750°C or higher to obtain a precursor of boron nitride particles, and a heating step of heating the precursor of the boron nitride particles at 1000°C or higher to obtain boron nitride particles.
[0017] In the reaction step, a first gas containing a borate ester and a second gas containing ammonia are separately introduced into a reactor.
[0018] Fig. 1 is a perspective view showing an example of a reactor. As shown in Fig. 1, the reactor 1 is, for example, cylindrical with both ends open (both end faces are opening faces), and has an internal space S located between one end face 1a and the other end face 1b. The length of the reactor 1 may be, for example, 1000 mm or more and 1600 mm or less. The inner diameter of the reactor 1 may be, for example, 30 mm or more and 100 mm or less.
[0019] Both ends of the reactor 1 are held by the holding member 2 so that the outside of the reactor 1 and the internal space S can be isolated (so that the internal space S can be a closed system as necessary). The reactor 1 is installed so that the heating part H is located in a resistance heating furnace (not shown) in order to heat only a part (hereinafter referred to as the "heating part") H between both end faces 1a and 1b. The length of the heating part H (the length in the longitudinal direction of the reactor 1) may be, for example, 500 mm or more and 900 mm or less. By heating the heating part H of the reactor 1, the boric acid ester and ammonia react in the heating part H. The temperature of the heating part H may be, for example, 750°C or more and 1500°C or less.
[0020] A first inlet pipe 3 and a second inlet pipe 4 are separately attached to one end surface 1a of the reactor 1 so that gas can be introduced from the outside of the reactor 1 into the internal space S. Fig. 2(a) is a side view of the reactor 1 seen from the first inlet pipe 3 side. Fig. 2(b) is a side view of the reactor 1 seen from the second inlet pipe 4 side.
[0021] As shown in FIG. 1 and FIG. 2(a), the first introduction pipe 3 has, for example, a cylindrical tip branched and bent in two directions (Y-shaped). The first introduction pipe 3 is introduced from the outside of the reactor 1 into the internal space S so as to extend substantially parallel to the extension direction D extending from one end face 1a of the reactor 1 to the other end face 1b (extension direction extending from one end face 1a as a starting point toward the other end face 1b), and in the internal space S, it bends and extends in two bending directions d11, d12 at a position, for example, 10 to 40 mm away from the one end face 1a. The tip faces of the first introduction pipe 3 in the bending directions d11, d12 are open, and serve as introduction ports 3a, 3b for introducing the first gas. That is, the first introduction pipe 3 has two introduction ports 3a, 3b.
[0022] The angle between one bending direction d11 of the first inlet pipe 3 and the extending direction D of the reactor 1 is θ 11 The angle between the other bending direction d12 of the first inlet pipe 3 and the extending direction D of the reactor 1 is θ 12 The bending directions d11 and d12 of the first introduction tube 3 are defined as directions perpendicular to the introduction ports 3a and 3b (tip end surface) of the first introduction tube 3, respectively.
[0023] As shown in FIG. 1 and FIG. 2(b), the second introduction pipe 4 has, for example, a shape (Y-shape) in which a cylindrical tip is branched and bent in two directions. The second introduction pipe 4 is introduced from the outside of the reactor 1 into the internal space S so as to extend substantially parallel to the extension direction D (extension direction starting from the one end face 1a toward the other end face 1b) of the reactor 1, and in the internal space S, it bends and extends in two bending directions d21, d22 at a position, for example, 10 to 40 mm away from the one end face 1a. The tip faces of the bending directions d21, d22 of the second introduction pipe 4 are open, and serve as introduction ports 4a, 4b for introducing the first gas. That is, the second introduction pipe 4 has two introduction ports 4a, 4b.
[0024] The angle between one bending direction d21 of the second inlet pipe 4 and the extending direction D of the reactor 1 is θ21 The angle between the other bending direction d22 and the extension direction D of the reactor 1 is θ 22 The bending directions d21 and d22 of the second introduction pipe 4 are defined as directions perpendicular to the introduction ports 4a and 4b (tip end surface) of the second introduction pipe 4, respectively.
[0025] In the reaction step, a first gas containing a borate ester is introduced into the internal space S of the reactor 1 through the first introduction pipe 3 from each of the two introduction ports 3a, 3b of the first introduction pipe 3. In addition, separately from the first gas, a second gas containing ammonia is introduced into the internal space S of the reactor 1 through the second introduction pipe 4 from each of the two introduction ports 4a, 4b of the second introduction pipe 4.
[0026] The first gas is obtained, for example, by passing an inert gas through a liquid borate ester. In this case, the first gas is a gas consisting of a borate ester and an inert gas. The borate ester may be, for example, an alkyl borate ester, preferably trimethyl borate. Examples of the inert gas include rare gases such as helium, neon, and argon, and nitrogen gas. The second gas is, for example, a gas consisting of ammonia.
[0027] The molar ratio of the amount of ammonia introduced to the amount of borate ester introduced (ammonia / borate ester) may be, for example, 1 or more and 10 or less.
[0028] The boric acid ester and ammonia introduced into the reactor 1 react in the heated reactor 1 to generate a precursor (white powder) of boron nitride particles. Some of the generated precursor of boron nitride particles adheres to the inside of the reactor 1, but most of the precursor of boron nitride particles is sent to a recovery container (not shown) attached to the other end surface 1b side of the reactor 1 by an inert gas or unreacted ammonia gas and collected. The reaction time for reacting the boric acid ester and ammonia is preferably within 30 seconds from the viewpoint of easily reducing the particle size of the obtained boron nitride particles. The reaction time is the time that the boric acid ester and ammonia remain in the heating section H of the reactor 1, and can be adjusted by the gas flow rate when the first gas and the second gas are introduced and the length of the heating section H.
[0029] In the reaction process described above, since the first inlet pipe 3 and the second inlet pipe 4 each have two inlets, the first gas and the second gas are each introduced into the reactor 1 from two inlets. In this case, it is presumed that the first gas and the second gas are more easily mixed uniformly with each other than when the first gas and the second gas are each introduced into the reactor from one inlet, and the variation in particle size of the obtained boron nitride particles is reduced. Furthermore, by using boron nitride particles with reduced variation in particle size, the dielectric constant and dielectric tangent of the heat dissipation member can be reduced.
[0030] In the above embodiment, the angle θ 11 and θ 12 is an angle such that the side surface (side surface along the extending direction D; the same applies below) 1c of the reactor 1 is located on the extension line of the bending directions d11, d12 of the first inlet pipe 3 (the extension line of the bending directions d11, d12 of the first inlet pipe 3 intersects with the side surface 1c of the reactor 1). Similarly, the above angle θ 21 and θ 22 is at an angle such that the side 1c of the reactor 1 is located on the extension line of the bending directions d21, d22 of the second inlet pipe 4 (the extension line of the bending directions d21, d22 of the second inlet pipe 4 intersects with the side 1c of the reactor 1).
[0031] In this case, the first gas also has an angle θ 11 and θ 12 Similarly, the second gas is introduced in the introduction directions d11 and d12 such that the angle between the second gas and the extension direction D of the reactor 1 is the angle θ 21 and θ 22 The gas is introduced in the introduction directions d21 and d22 such that the gas flows in the first gas introduction direction d11 and the gas flows in the second gas introduction direction d21 and the gas flows in the second gas introduction direction d22. That is, in this embodiment, the side surface 1c of the reactor 1 is located on the extension line of the introduction direction d11 and the gas flows in the second gas introduction direction d21 and the gas flows in the second gas introduction direction d22. The introduction directions d11 and d12 of the first gas are defined as directions perpendicular to the introduction ports 3a and 3b of the first introduction tube 3, similar to the bending directions d11 and d12 of the first introduction tube 3. The introduction directions d21 and d22 of the second gas are defined as directions perpendicular to the introduction ports 4a and 4b of the second introduction tube 4, similar to the bending directions d21 and d22 of the second introduction tube 4.
[0032] In such an embodiment, the variation in particle size of the obtained boron nitride particles can be further reduced. Although the reason is unclear, it is presumed that the first gas and the second gas are more easily mixed with each other uniformly than when the first gas and the second gas are introduced parallel to the extension direction D of the reactor 1, for example, because the first gas and the second gas advance inside the reactor 1 at an angle to the extension direction D of the reactor 1 while colliding with the side surface 1c of the reactor 1. Furthermore, by using boron nitride particles with further reduced variation in particle size, the dielectric constant and dielectric loss tangent of the heat dissipation member can be further reduced.
[0033] Angle θ 11 , θ 12 , θ 21 and θ 22 From the viewpoint of further reducing the variation in particle size of the obtained boron nitride particles, the angle θ is preferably 50° or more, more preferably 60° or more, further preferably 65° or more, and particularly preferably 70° or more. 11 , θ 12 , θ 21 and θ 22Each of the angles θ is less than 90°, and may be, for example, less than or equal to 80°. 11 , θ 12 , θ 21 and θ 22 About tanθ 11 , tan θ 12 , tan θ 21 and tan θ 22 From the viewpoint of further reducing the variation in particle size of the obtained boron nitride particles, tan θ is preferably 1.2 or more, more preferably 1.7 or more, even more preferably 2.1 or more, and particularly preferably 2.7 or more. 11 , tan θ 12 , tan θ 21 and tan θ 22 may each be, for example, 11.4 or less.
[0034] The method of introducing the first gas and the second gas may take other embodiments than those described above. Figure 3(a) is a side view of the reactor in another embodiment as seen from the first inlet pipe side, and Figure 3(b) is a side view of the reactor in another embodiment as seen from the second inlet pipe side.
[0035] As shown in FIG. 3(a), in another embodiment, the first gas is introduced from the two inlets 13a and 13b of the first introduction pipe 13, and only the first gas introduced from one inlet 13a is arranged such that the side surface 1c of the reactor 1 is located on the extension line of the introduction direction d11 of the first gas introduced from the inlet 13a. 11 The fuel is introduced into the reactor 1 at an angle θ 11 The preferred range of the angle θ 11 The introduction direction d14 of the first gas introduced from the other inlet 13b of the first introduction pipe 13 may be, for example, a direction substantially parallel to the extension direction D of the reactor 1 (i.e., a direction in which the angle between the introduction direction d14 of the first gas and the extension direction D of the reactor 1 is substantially 0°).
[0036] As shown in FIG. 3(b), in another embodiment, the second gas introduced from the two inlets 14a and 14b of the second introduction pipe 14 is introduced from only one inlet 14a such that the side surface 1c of the reactor 1 is located on the extension line of the introduction direction d21 of the second gas introduced from the inlet 14a. 21 The angle θ 21 The preferred range of the angle θ 21 The introduction direction d24 of the second gas introduced from the other inlet 14b of the second introduction pipe 14 may be, for example, a direction substantially parallel to the extension direction D of the reactor 1 (i.e., a direction in which the angle between the introduction direction d24 of the second gas and the extension direction D of the reactor 1 is substantially 0°).
[0037] In this embodiment, the variation in particle size of the obtained boron nitride particles can be further reduced. However, from the viewpoint of further reducing the variation in particle size of the obtained boron nitride particles, as in the embodiment shown in Fig. 2(a), the angle θ between the extension direction D of the reactor 1 and the first gas introduced from the two inlets 3a and 3b of the first introduction pipe 3 is set so that the side surface 1c of the reactor 1 is located on the extension line of the introduction directions d11 and d12 of the first gas introduced from the two inlets 3a and 3b of the first introduction pipe 3. 11 ,θ 12 2(b), the second gas introduced from the two inlets 4a and 4b of the second inlet pipe 4 is preferably introduced into the reactor 1 at an angle θ with the extension direction D of the reactor 1 so that the side surface 1c of the reactor 1 is located on the extension line of the introduction directions d21 and d22. 21 ,θ 22 It is more preferable that the fuel is introduced into the reactor 1 in the above manner.
[0038] In each of the above embodiments, the ends of the first introduction pipe 3 (13) are branched to provide two introduction ports 3a, 3b (13a, 13b), but in another embodiment, two introduction pipes may be inserted into the reactor 1 separately as the first introduction pipe, and each of the two introduction pipes may be provided with one introduction port, so that the first gas can be introduced into the reactor 1 from the two introduction ports as a whole. Similarly, in each of the above embodiments, the ends of the second introduction pipe 4 (14) are branched to provide two introduction ports 4a, 4b (14a, 14b), but in another embodiment, two introduction pipes may be inserted into the reactor 1 separately as the second introduction pipe, and each of the two introduction pipes may be provided with one introduction port, so that the second gas can be introduced into the reactor 1 from the two introduction ports as a whole.
[0039] In addition, in each of the above embodiments, two inlets 3a, 3b (13a, 13b) for introducing the first gas are provided, but the number of inlets for introducing the first gas may be two or more, for example, three or more. Similarly, in each of the above embodiments, two inlets 4a, 4b (14a, 14b) for introducing the second gas are provided, but the number of inlets for introducing the second gas may be two or more, for example, three or more. In these cases, it is preferable that the first gas introduced from at least one of the three or more inlets is introduced so that the side surface 1c of the reactor 1 is located on the extension line of the introduction direction, and it is preferable that the second gas introduced from at least one of the three or more inlets is introduced so that the side surface 1c of the reactor 1 is located on the extension line of the introduction direction.
[0040] In the heating step following the reaction step described above, the precursor of the boron nitride particles obtained in the reaction step is heated at 1000°C or higher to obtain boron nitride particles. The heating step may include, for example, a first heating step in which the precursor of the boron nitride particles is heated at 1000 to 1600°C to obtain a first precursor, a second heating step in which the first precursor is heated at 1000 to 1600°C to obtain a second precursor, and a third heating step in which the second precursor is heated at 1800 to 2200°C to obtain boron nitride particles. In this case, after the first heating step is completed, the environmental temperature in which the first precursor is placed is temporarily lowered to room temperature (10 to 30°C) before the second heating step is started. In another embodiment, in the heating step, the first heating step may be omitted, and the second heating step and the third heating step may be performed.
[0041] In the first heating step, the precursor of boron nitride particles obtained in the reaction step is placed in another reaction tube (e.g., an alumina tube) installed in a resistance heating furnace, and nitrogen gas and ammonia gas are introduced separately into the reaction tube. The gas introduced at this time may be only ammonia gas. The flow rates of nitrogen gas and ammonia gas may be appropriately adjusted so that the reaction time is a desired value. For example, the higher the flow rates of nitrogen gas and ammonia gas, the shorter the reaction time.
[0042] Next, the reaction tube is heated to 1000 to 1600° C. The heating time may be, for example, 1 hour or more and 10 hours or less, thereby obtaining the first precursor.
[0043] After the first heating step is completed, the power supply to the resistance heating furnace is turned off, the introduction of nitrogen gas and ammonia gas is stopped, and the temperature inside the reaction tube is lowered to room temperature (10 to 30° C.), and the first precursor is allowed to stand still. The time for standing still may be, for example, 0.5 hours or more and may be 96 hours or less.
[0044] In the second heating step, nitrogen gas and ammonia gas are introduced into the reaction tube again, and the reaction tube is heated again to 1000 to 1600°C. Examples of the flow rates of nitrogen gas and ammonia gas and the heating time may be the same as those described in the first heating step. The conditions of the first heating step and the second heating step may be the same or different from each other. This results in the second precursor.
[0045] In the third heating step, the second precursor obtained in the second heating step is placed in a boron nitride crucible and heated to 1800 to 2200°C in a nitrogen atmosphere in an induction heating furnace. The heating time may be, for example, 0.5 hours or more and 10 hours or less. This produces boron nitride particles.
[0046] The above-described manufacturing method provides boron nitride particles having an average particle size of 1 μm or less and a difference between the 10% cumulative particle size and the 100% cumulative particle size of 10 μm or less in a volumetric particle size distribution. That is, another embodiment of the present invention provides boron nitride particles having an average particle size of 1 μm or less and a difference (D100-D10) between the 10% cumulative particle size (D10) and the 100% cumulative particle size (D100) of 10 μm or less in a volumetric particle size distribution.
[0047] The average particle size of the boron nitride particles may be preferably 0.9 μm or less, 0.8 μm or less, or 0.7 μm or less from the viewpoint of reducing the dielectric constant of a heat dissipation member containing the boron nitride particles (hereinafter also simply referred to as "heat dissipation member"). The average particle size of the boron nitride particles may be preferably 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.2 μm or more, 0.3 μm or more, or 0.4 μm or more from the viewpoint of suppressing an increase in viscosity when the boron nitride particles are mixed with a resin.
[0048] From the viewpoint of reducing the dielectric constant of the heat dissipation member, the D100-D10 of the boron nitride particles may be preferably 8 μm or less, 6 μm or less, 5 μm or less, 4 μm or less, or 3 μm or less. The D100-D10 of the boron nitride particles may be, for example, 0.5 μm or more, 0.8 μm or more, or 1 μm or more.
[0049] The average particle size and D100-D10 of the boron nitride particles are measured by the following procedure. Using distilled water as a dispersion medium for dispersing boron nitride particles and sodium hexametaphosphate as a dispersant, a 0.125% by mass aqueous solution of sodium hexametaphosphate is prepared. Boron nitride particles are added to this aqueous solution at a ratio of 0.1 g / 80 mL, and ultrasonic dispersion is performed once for 1 minute and 30 seconds at AMPLITUDE (amplitude) 80% using an ultrasonic homogenizer (e.g., manufactured by Nippon Seiki Seisakusho, product name: US-300E) to prepare a dispersion of boron nitride particles. The dispersion is taken while stirring at 60 rpm, and the volume-based particle size distribution is measured using a laser diffraction scattering particle size distribution measuring device (e.g., manufactured by Beckman Coulter, product name: LS-13 320). At this time, the refractive index of water is 1.33, and the refractive index of boron nitride particles is 1.7. From the measurement results, the average particle size is calculated as the particle size (median size, d50) at 50% of the cumulative value of the cumulative particle size distribution, and D100-D10 is calculated as the particle size D10 at 10% of the cumulative value of the cumulative particle size distribution minus the particle size D10 at 10% of the cumulative value.
[0050] The boron nitride particles preferably have a spherical or nearly spherical shape in order to improve the filling property when producing a heat dissipation member and to make the properties of the heat dissipation member isotropic (thermal conductivity, dielectric constant, etc.) From the same viewpoint, the average circularity of the boron nitride particles may preferably be 0.8 or more, 0.82 or more, 0.84 or more, 0.86 or more, or 0.88 or more.
[0051] The average circularity of the boron nitride particles is measured by the following procedure. The image of the boron nitride particle taken with a scanning electron microscope (SEM) (magnification: 10,000 times, image resolution: 1280 x 1024 pixels) is analyzed using image analysis software (e.g., MacView, manufactured by Mountec Co., Ltd.) to calculate the projected area (S) and perimeter (L) of the boron nitride particle. The projected area (S) and perimeter (L) are used to calculate the following formula: Circularity = 4πS / L 2 The circularity is calculated according to the following formula: The average circularity is defined as the average circularity obtained for 100 randomly selected boron nitride particles.
[0052] The boron nitride particles described above are suitable for use in, for example, heat dissipation members. By using the above-mentioned boron nitride particles, a heat dissipation member with a low dielectric constant and a low dielectric loss tangent can be obtained. When the boron nitride particles are used in a heat dissipation member, they are used as a resin composition mixed with, for example, a resin. That is, another embodiment of the present invention is a resin composition containing a resin and the above-mentioned boron nitride particles.
[0053] The content of the above-mentioned boron nitride particles, based on the total volume of the resin composition, is preferably 30 vol. % or more, more preferably 40 vol. % or more, and even more preferably 50 vol. % or more, from the viewpoint of improving the thermal conductivity of the resin composition and making it easier to obtain excellent heat dissipation performance, and is preferably 85 vol. % or less, more preferably 80 vol. % or less, and even more preferably 70 vol. % or less, from the viewpoint of suppressing the generation of voids during molding and the deterioration of insulation and mechanical strength.
[0054] Examples of resins include epoxy resins, silicone resins, silicone rubber, acrylic resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyolefins (polyethylene, etc.), polyimides, polyamideimides, polyetherimides, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS (acrylonitrile-butadiene-styrene) resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins.
[0055] The resin content may be 15 vol.% or more, 20 vol.% or more, or 30 vol.% or more, and may be 70 vol.% or less, 60 vol.% or less, or 50 vol.% or less, based on the total volume of the resin composition.
[0056] The resin composition may further contain a curing agent that cures the resin. The curing agent is appropriately selected depending on the type of resin. For example, when the resin is an epoxy resin, the curing agent may be a phenol novolac compound, an acid anhydride, an amino compound, or an imidazole compound. The content of the curing agent may be, for example, 0.5 parts by mass or more or 1.0 parts by mass or more, and 15 parts by mass or less or 10 parts by mass or less, relative to 100 parts by mass of the resin.
[0057] The resin composition may further contain boron nitride particles other than the above-mentioned boron nitride particles (for example, known boron nitride particles such as chunky boron nitride particles formed by agglomeration of scaly primary particles). EXAMPLES
[0058] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.
[0059] [Example 1] Boron nitride particles were prepared by the following procedure. First, in the reaction process, a cylindrical reactor (quartz tube, reactor length: 1300 mm, inner diameter of reactor: 75 mm, length of part located in resistance heating furnace: 800 mm) as shown in Figures 1 and 2 was heated and raised to 1150°C. On the other hand, a first gas obtained by passing nitrogen gas through trimethyl borate was introduced into the reactor from a first introduction tube. On the other hand, ammonia gas was directly introduced into the reactor.
[0060] The first inlet pipe is located in the inner space of the reactor at a distance of 25 mm from one end face of the reactor, and the angle with the extending direction of the reactor is θ 11 and θ 12 In other words, the angle between the introduction direction of the first introduction gas and the extension direction of the reactor is θ 11 and θ 12 The first gas was introduced from each of the two inlets so that the angle between the first gas and the extension direction of the reactor was θ 1 / 2. 21 and θ 22 In other words, the angle between the introduction direction of the second introduction gas and the extension direction of the reactor is θ 21 and θ 22 The second gas was introduced from each of the two inlets so that θ 11 , θ 12 , θ 21 and θ 22 are tanθ 11 , tan θ 12 , tan θ 21 and tan θ 22 The angle was set so that the value shown in Table 1 was obtained.
[0061] The molar ratio of the amount of ammonia introduced to the amount of trimethyl borate introduced (ammonia / trimethyl borate) was set to 4.5. This caused trimethyl borate and ammonia to react with each other to obtain a precursor of boron nitride particles (white powder). The reaction time was set to 10 seconds.
[0062] In the heating step, the precursor of boron nitride particles obtained in the reaction step was placed in another reaction tube (alumina tube) installed in a resistance heating furnace, and nitrogen gas and ammonia gas were introduced into the reaction tube at flow rates of 10 L / min and 15 L / min, respectively. The reaction tube was then heated at 1500°C for 2.5 hours. This resulted in the production of a first precursor (first heating step).
[0063] Next, the power to the resistance heating furnace was turned off, the introduction of the nitrogen gas and the ammonia gas was stopped, and the temperature inside the reaction tube was lowered to 25° C., and the first precursor was left to stand for 2 hours.
[0064] Next, nitrogen gas and ammonia gas were introduced and the inside of the reaction tube was heated under the same conditions as in the first heating step, thereby obtaining a second precursor (second heating step).
[0065] Next, the second precursor obtained in the second heating step was placed in a boron nitride crucible and heated in an induction heating furnace under a nitrogen atmosphere at 2000° C. for 5 hours (third heating step), thereby obtaining boron nitride particles.
[0066] [Example 2] Boron nitride particles were produced in the same manner as in Example 1, except that the configurations of the first and second inlet pipes were changed to those shown in Figures 3(a) and (b), respectively. That is, only the first gas introduced from one of the two inlets was introduced so that the side of the reactor was located on the extension line of the introduction direction, and the first gas introduced from the other inlet was introduced in a direction parallel to the extension direction of the reactor (a direction in which the angle between the introduction direction of the first gas and the extension direction of the reactor is 0°) (the same applies to the second gas).
[0067] [Example 3] The introduction direction of the first gas and the introduction direction of the second gas are defined as tanθ 11 , tan θ 12 , tan θ 21 and tan θ 22 The angle θ such that the value shown in Table 1 is obtained. 11 , θ 12 , θ 21 and θ 22 Boron nitride particles were produced in the same manner as in Example 1, except that the above-mentioned conditions were changed to the above.
[0068] [Comparative Example 1] Boron nitride particles were produced in the same manner as in Example 1, except that the configuration of the first inlet pipe was changed to that shown in Fig. 4(a) (a side view of the reactor viewed from the first inlet pipe side). That is, a first inlet pipe 103 having only one inlet port 103a was used as the first inlet pipe, and a first gas was introduced from the inlet port 103a in a direction d101 parallel to the extension direction D of the reactor 1 (a direction in which the angle between the introduction direction of the first gas and the extension direction of the reactor is 0°) so as to proceed through approximately the center of the reactor 1.
[0069] [Comparative Example 2] Boron nitride particles were produced in the same manner as in Example 1, except that the configuration of the first inlet pipe was changed to that shown in Fig. 4(b) (a side view of the reactor viewed from the first inlet pipe side). That is, a first inlet pipe 113 having only one inlet port 113a was used as the first inlet pipe, and the first gas was introduced from the inlet port 113a in a direction d111 parallel to the extension direction D of the reactor 1 (a direction in which the angle between the introduction direction of the first gas and the extension direction of the reactor is 0°) so as to proceed along a position shifted from the center of the reactor 1 along the side surface.
[0070] [Comparative Example 3] Boron nitride particles were produced in the same manner as in Example 1, except that the configuration of the second inlet pipe was changed to that shown in Fig. 5(a) (a side view of the reactor viewed from the second inlet pipe side). That is, a second inlet pipe 104 having only one inlet port 104a was used as the second inlet pipe, and a second gas was introduced from the inlet port 104a in a direction d102 parallel to the extension direction D of the reactor 1 (a direction in which the angle between the introduction direction of the second gas and the extension direction of the reactor is 0°) so as to proceed through approximately the center of the reactor 1.
[0071] [Comparative Example 4] Boron nitride particles were produced in the same manner as in Example 1, except that the configuration of the second inlet pipe was changed to that shown in Fig. 5(b) (a side view of the reactor viewed from the second inlet pipe side). That is, a second inlet pipe 114 having only one inlet 114a was used as the second inlet pipe, and a second gas was introduced from the inlet 114a in a direction d112 parallel to the extension direction D of the reactor 1 (a direction in which the angle between the introduction direction of the second gas and the extension direction of the reactor is 0°) so as to proceed along a position shifted from the center of the reactor 1 along the side surface.
[0072] For each of the obtained boron nitride particles, the average particle size, the difference between the 10% cumulative particle size and the 100% cumulative particle size (D100-D10), and the average circularity were measured by the following methods. The results are shown in Table 1.
[0073] (Average particle size and D100-D10) Distilled water was used as a dispersion medium for dispersing boron nitride particles, and sodium hexametaphosphate was used as a dispersant to prepare a 0.125% by mass aqueous solution of sodium hexametaphosphate. Boron nitride particles were added to this aqueous solution at a ratio of 0.1 g / 80 mL, and ultrasonic dispersion was performed once for 1 minute and 30 seconds at AMPLITUDE (amplitude) 80% using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho, product name: US-300E) to prepare a dispersion of boron nitride particles. The dispersion was taken while stirring at 60 rpm, and the volume-based particle size distribution was measured using a laser diffraction scattering particle size distribution measuring device (manufactured by Beckman Coulter, product name: LS-13 320). At this time, 1.33 was used as the refractive index of water, and 1.7 was used as the refractive index of boron nitride particles. From the measurement results, the average particle size was calculated as the particle size (median size, d50) at 50% of the cumulative value of the cumulative particle size distribution, and D100-D10 was calculated as the particle size D10 at 10% of the cumulative value of the cumulative particle size distribution minus the particle size D10 at 10% of the cumulative value.
[0074] (Average circularity) First, the projected area (S) and perimeter (L) of the boron nitride particle were calculated by image analysis using image analysis software (e.g., MacView, manufactured by Mountec Co., Ltd.) for an image of the boron nitride particle (magnification: 10,000 times, image resolution: 1280 x 1024 pixels) taken using a scanning electron microscope (SEM). Next, the projected area (S) and perimeter (L) were calculated using the following formula: Circularity = 4πS / L 2 The circularity was determined according to the following formula: The average value of the circularities determined for 100 randomly selected boron nitride particles was calculated as the average circularity.
[0075] The dielectric constant and dielectric loss tangent of each of the obtained boron nitride particles were measured by the following method. The results are shown in Table 1. The boron nitride particles were mixed with polyethylene (product name "Novatec HY540" manufactured by Japan Polyethylene Co., Ltd.) in an amount such that the boron nitride particles constituted 20 volume % and then formed into a sheet having a thickness of 0.2 mm. The mixing and sheet forming were carried out using a twin-screw extruder at a temperature of 180°C. The sheet obtained was measured using a cavity resonator method measuring device at a frequency of 36 GHz and a temperature of 25°C to determine the dielectric constant and dielectric loss tangent of the sheet.
[0076] [Table 1] [Explanation of symbols]
[0077] 1...reactor, 1a...one end face of reactor, 1b...other end face of reactor, 1c...side face of reactor, 2...holding member, 3, 13...first introduction tube, 3a, 3b, 13a, 13b...inlet of first introduction tube, 4, 14...second introduction tube, 4a, 4b, 14a, 14b...inlet of second introduction tube, D...extension direction of reactor, S...internal space of reactor, d11, d12, d13, d14...introduction direction of first gas, d21, d22, d23, d24...introduction direction of second gas.
Claims
1. a reaction step of separately introducing a first gas containing a borate ester and a second gas containing ammonia into a cylindrical reactor from one end surface of the reactor, and reacting the borate ester and the ammonia at 750° C. or higher in the reactor to obtain a precursor of boron nitride particles; a heating step of heating the precursor of the boron nitride particles at 1000° C. or higher to obtain boron nitride particles; A method for producing boron nitride particles comprising: In the reaction step, the first gas is introduced into the reactor through two or more inlets, and the second gas is introduced into the reactor through two or more inlets.
2. 2. The production method according to claim 1, wherein the first gas is introduced from at least one of the two or more inlets such that a side surface of the reactor is located on an extension line of the introduction direction of the first gas.
3. 3. The production method according to claim 1, wherein the second gas introduced from at least one of the two or more inlets is introduced such that a side surface of the reactor is located on an extension line of the introduction direction of the second gas.
Citation Information
Patent Citations
Method and an apparatus for high pressure gas phase preparation of boron nitride spherical powder
CN107161960A
NANO spherical particle having composite structure, powder and method for producing the same
JP2008038163A
Boron nitride spherical nanoparticle and method of producing the same
JP2010180066A
Electrically insulating composite material, method of making this material and method of using said material as an electrical insulator
JP2016531972A
Boron nitride aggregated particle composition, BN aggregated particle-containing resin composition and their compact, as well as production method of boron nitride aggregated particle
JP2017036190A