Boron nitride particles, and resin composition and container containing the boron nitride particles
By controlling crystallization to create boron nitride particles with a low-crystallinity center and high-crystallinity periphery, the process is simplified without sacrificing thermal conductivity.
Patent Information
- Application Number
- JP2022510628
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-26
- Filing Date
- 2021-03-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-03-24
AI Technical Summary
Existing methods for manufacturing boron nitride particles require multiple heating stages, which complicates the process and may impair the thermal conductivity of the particles.
Manufacture boron nitride particles with a center portion of low crystallinity and a peripheral portion of high crystallinity by controlling the crystallization process, allowing for simpler production without compromising thermal conductivity.
The simplified process results in boron nitride particles with equivalent thermal conductivity to conventional methods, while reducing manufacturing complexity.
Smart Images

Figure 0007571122000002 
Figure 0007571122000003 
Figure 0007571122000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to boron nitride particles, and a resin composition and a container containing the boron nitride particles. [Background technology]
[0002] In electronic components such as power devices, transistors, thyristors, and CPUs, heat dissipation members are used to efficiently dissipate heat generated during use. The heat dissipation members contain, for example, ceramic particles with high thermal conductivity. As ceramic particles, boron nitride particles have attracted attention because of their properties such as high thermal conductivity, high insulation, and low dielectric constant.
[0003] Various methods are known for producing boron nitride particles. One of the methods involves reacting boric acid alkoxide with ammonia in an ammonia / boric acid alkoxide molar ratio of 1 to 10 with ammonia in an inert gas stream at 750°C or higher for 30 seconds or less, heat treating the mixture in an atmosphere of ammonia gas or a mixed gas of ammonia gas and an inert gas at 1,000 to 1,600°C for 1 hour or more, and then firing the mixture in an inert gas atmosphere at 1,800 to 2,200°C for 0.5 hours or more (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2015 / 122379 Summary of the Invention [Problem to be solved by the invention]
[0005] In the above-mentioned production method, it is necessary to perform heating in at least three stages while changing the conditions, and in order to produce boron nitride particles more efficiently, it is desirable to simplify the process. On the other hand, it is necessary to avoid compromising the properties required for boron nitride particles, such as thermal conductivity, by simplifying the process.
[0006] Therefore, an object of one aspect of the present invention is to provide boron nitride particles that can be produced more simply than conventional particles while having the same thermal conductivity as conventional particles. [Means for solving the problem]
[0007] It was previously believed that in order to obtain high thermal conductivity, it was necessary to crystallize boron nitride as much as possible throughout the entire particle, but the inventors of the present invention have conducted extensive research and have surprisingly found that, as long as the peripheral portion of the particle is sufficiently crystallized, even if the boron nitride in the center of the particle is insufficiently crystallized, this does not adversely affect the thermal conductivity of the boron nitride particle. In other words, it has been found that a thermal conductivity equivalent to that of conventional methods can be obtained even if the process of crystallizing boron nitride is simplified.
[0008] One aspect of the present invention is a boron nitride particle comprising a core portion containing low-crystalline boron nitride and a peripheral portion surrounding the core portion and containing highly-crystalline boron nitride.
[0009] The average circularity of the boron nitride particles may be 0.8 or more.
[0010] Another aspect of the present invention is a resin composition containing a resin and the above-mentioned boron nitride particles.
[0011] Another aspect of the present invention is a container comprising the above-mentioned boron nitride particles and a container for containing the boron nitride particles. Effect of the Invention
[0012] According to one aspect of the present invention, it is possible to provide boron nitride particles that can be produced more simply than before and have the same thermal conductivity as before. [Brief description of the drawings]
[0013] [Figure 1] 1 is a TEM image of an entire boron nitride particle of an example. [Diagram 2] 2 is a TEM image of the peripheral region S of the boron nitride particle in FIG. 1. [Diagram 3] 3 is a diagram and graph showing the results of FFT analysis of region S1 of the boron nitride particle in FIG. 2. [Figure 4] 2 is a diagram showing the results of an FFT analysis of regions S2 to S5 in the peripheral portion S of the boron nitride particle in FIG. [Diagram 5] 2 is a graph showing the results of an FFT analysis of regions S2 to S5 of the peripheral portion S of the boron nitride particle in FIG. [Figure 6] 2 is a diagram showing the results of an FFT analysis of regions C1 to C4 in the central portion C of the boron nitride particle in FIG. [Figure 7] 2 is a graph showing the results of an FFT analysis of regions C1 to C4 in the central portion C of the boron nitride particle in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present invention will be described in detail.
[0015] One embodiment of the present invention is a boron nitride particle comprising a core portion including low-crystalline boron nitride and a peripheral portion including high-crystalline boron nitride disposed so as to surround the core portion.
[0016] In this specification, the term "high crystallinity" refers to a crystallinity of 1 to 4 nm in the reciprocal lattice space in an FFT image of boron nitride particles obtained by the following method. -1"Low crystallinity" means a state in which bright spots (peaks) due to periodicity derived from the h-BN (0002) plane are present within the range of 1 to 4 nm on the reciprocal lattice space, and "low crystallinity" means a state in which such bright spots (peaks) are not present. -1 This means that there exists a point in the range where the intensity S after subtracting the background by the B-spline method is 15 times or more the noise intensity N. Here, the noise intensity N is the intensity within 4 nm in the reciprocal lattice space after background processing is performed by the B-spline method. -1 Exceeding 6nm -1 It is defined as the standard deviation value in the range below. In addition, the bright spots (peaks) also include those with fluctuations in the wave number direction or circumferential direction. In the peripheral area containing highly crystalline boron nitride, -1 Within this range, there may be a point where the intensity S is preferably 20 times or more, more preferably 23 times or more, and further preferably 25 times or more, the noise intensity N.
[0017] (How to obtain FFT images) First, a TEM image of boron nitride particles at 400,000 times magnification is obtained using a transmission electron microscope (for example, "JEM-2100" manufactured by JEOL Ltd.) under the following conditions. Objective lens aperture: φ120μm Focusing lens aperture: φ150μm Recording medium: AMETEK "OrisusSC1000A1" Bining:2 Exposure time: 0.5 seconds In addition, image analysis software (for example, "GMS3" manufactured by AMETEC) is used for TEM observation and FFT analysis described later. Next, FFT analysis is performed on an 8.556 nm square region in the obtained TEM image to obtain an FFT image of 256 × 256 pixels.
[0018] The diameter of the core in the boron nitride particle may be, for example, 0.1d or more, 0.15d or more, or 0.2d or more, and 0.6d or less, 0.5 or less, 0.4d or less, 0.35d or less, or 0.3d or less, where d is the particle diameter of the boron nitride particle. The diameter of the core in the boron nitride particle may be, for example, 1 nm or more, 5 nm or more, 10 nm or more, 20 nm or more, or 30 nm or more, and 400 nm or less, 300 nm or less, 200 nm or less, or 100 nm or less. The diameter of the core in the boron nitride particle is within the "highly crystalline" portion defined as above, i.e., 1 to 4 nm on the reciprocal lattice space. -1 This refers to the diameter of the area where bright spots (peaks) exist due to the periodicity derived from the h-BN(0002) surface.
[0019] The thickness of the peripheral part in the boron nitride particle may be, for example, 0.3d or more, 0.33d or more, or 0.35d or more, and 0.45d or less, 0.43d or less, or 0.4d or less, when the particle diameter of the boron nitride particle is d. The diameter of the center part in the boron nitride particle may be, for example, 5 nm or more, 10 nm or more, 20 nm or more, 40 nm or more, or 60 nm or more, and 450 nm or less, 300 nm or less, 200 nm or less, or 100 nm or less. The thickness of the peripheral part in the boron nitride particle is the "low crystallinity" part defined as above, that is, 1 to 4 nm on the reciprocal lattice space. -1 This refers to the thickness of the portion where there are no bright spots (peaks) due to the periodicity derived from the h-BN(0002) surface.
[0020] The average particle size of the boron nitride particles is preferably 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, or 0.15 μm or more, from the viewpoint of suppressing an increase in viscosity when the boron nitride particles are mixed with a resin, and may be 1 μm or less, 0.8 μm or less, 0.6 μm or less, or 0.4 μm or less, from the viewpoint of improving the dielectric breakdown characteristics of a heat dissipation component containing the boron nitride particles (hereinafter also simply referred to as a "heat dissipation component").
[0021] The average particle size of the boron nitride particles is measured by the following procedure. Using distilled water as a dispersion medium for dispersing boron nitride particles and sodium hexametaphosphate as a dispersant, a 0.125% by mass aqueous solution of sodium hexametaphosphate is prepared. Boron nitride particles are added to this aqueous solution at a ratio of 0.1 g / 80 mL, and ultrasonic dispersion is performed once for 1 minute and 30 seconds at AMPLITUDE (amplitude) 80% using an ultrasonic homogenizer (e.g., "US-300E" manufactured by Nippon Seiki Seisakusho) to prepare a dispersion liquid of boron nitride particles. This dispersion liquid is taken while stirring at 60 rpm, and the volume-based particle size distribution is measured using a laser diffraction scattering particle size distribution measuring device (e.g., "LS-13 320" manufactured by Beckman Coulter, Inc.). At this time, 1.33 is used as the refractive index of water, and 1.7 is used as the refractive index of boron nitride particles. From the measurement results, the average particle size is calculated as the particle size (median diameter, d50) at the cumulative value of 50% of the cumulative particle size distribution. The average particle size measured in this manner is considered to be the average particle size of boron nitride particles including not only primary particles of boron nitride particles but also particles (secondary particles) formed by agglomerations of the primary particles.
[0022] The boron nitride particles preferably have a spherical or nearly spherical shape in order to improve the filling property when producing a heat dissipation member and to make the properties of the heat dissipation member isotropic (thermal conductivity, dielectric constant, etc.). From the same viewpoint, the average circularity of the boron nitride particles may preferably be 0.8 or more, 0.82 or more, 0.84 or more, 0.86 or more, 0.88 or more, 0.90 or more, 0.91 or more, 0.92 or more, 0.93 or more, or 0.94 or more.
[0023] The average circularity of the boron nitride particles is measured by the following procedure. The image of the boron nitride particle taken with a scanning electron microscope (SEM) (magnification: 10,000 times, image resolution: 1280 x 1024 pixels) is analyzed using image analysis software (e.g., "MacView" manufactured by Mountec Co., Ltd.) to calculate the projected area (S) and perimeter (L) of the boron nitride particle. The projected area (S) and perimeter (L) are used to obtain the following formula: Circularity = 4πS / L 2 The circularity is calculated according to the following formula: The average circularity is defined as the average circularity obtained for 100 randomly selected boron nitride particles.
[0024] The boron nitride particles described above are obtained by intentionally stopping the crystal growth of boron nitride in an incomplete state. In the production of boron nitride particles, crystal growth progresses gradually from the periphery to the center of the particle, but by stopping the crystal growth of boron nitride in an incomplete state, the boron nitride particles obtained have high crystallinity in the periphery and low crystallinity in the center.
[0025] The manufacturing method of the above-mentioned boron nitride particles will be specifically described below. The above-mentioned boron nitride particles can be obtained by a manufacturing method including a first step of reacting a boric acid ester with ammonia at 750 to 1400°C to obtain a precursor of the boron nitride particles, and a second step of heating the precursor at 1000 to 1600°C to obtain the boron nitride particles.
[0026] In the first step, for example, a reaction tube (for example, a quartz tube) installed in a resistance heating furnace is heated to 750 to 1500°C. On the other hand, an inert gas is passed through a liquid borate ester and then introduced into the reaction tube, thereby introducing the borate ester into the reaction tube. On the other hand, ammonia gas is directly introduced into the reaction tube. Examples of the inert gas include rare gases such as helium, neon, and argon, and nitrogen gas. The borate ester may be, for example, an alkyl borate ester, and is preferably trimethyl borate.
[0027] The molar ratio of the amount of ammonia introduced to the amount of borate ester introduced (ammonia / borate ester) may be, for example, 1 or more and 10 or less.
[0028] The introduced boric acid ester and ammonia react in the heated reaction tube to generate a precursor of boron nitride particles. This precursor contains amorphous boron nitride and may be, for example, a white powder. Some of the generated precursor adheres to the inside of the reaction tube, but most of the precursor is transported by the inert gas and unreacted ammonia gas to a collection vessel attached to the end of the reaction tube and collected.
[0029] The time (reaction time) for reacting the borate ester with ammonia in the first step is preferably within 30 seconds. The reaction time is the time during which the borate ester and ammonia remain in the part (heated part) of the reaction tube heated to 750 to 1400°C, and can be adjusted by the gas flow rate when the borate ester and ammonia are introduced and the length of the reaction tube installed in the resistance heating furnace (the length of the heated part of the reaction tube).
[0030] In the second step, the precursor obtained in the first step is placed in another reaction tube (e.g., an alumina tube) installed in a resistance heating furnace, and nitrogen gas and ammonia gas are introduced separately into the reaction tube. The gas introduced at this time may be only ammonia gas. The flow rates of the nitrogen gas and ammonia gas may be appropriately adjusted so that the reaction time is a desired value. For example, the higher the flow rate of ammonia gas, the shorter the reaction time.
[0031] The reaction tube is then heated to 1000 to 1600°C. The heating time may be, for example, 1 hour or more and 10 hours or less. This allows the crystallization of boron nitride in the precursor to proceed, and boron nitride particles are obtained. However, all of the boron nitride in the precursor is not crystallized, and low-crystalline boron nitride remains inside the boron nitride particles.
[0032] This manufacturing method does not include a step of heating the boron nitride particles obtained in the second step at 1800°C or higher after the second step (a step that has been conventionally performed to promote crystal growth of boron nitride). That is, in this manufacturing method, the desired boron nitride particles are obtained in an incompletely crystal-grown state after the heating in the second step. This manufacturing method may not include a step of heating the boron nitride particles obtained in the second step at 1700°C or higher, 1600°C or higher, 1500°C or higher, 1400°C or higher, 1300°C or higher, 1200°C or higher, 1100°C or higher, 1000°C or higher, 900°C or higher, 800°C or higher, 700°C or higher, 600°C or higher, 500°C or higher, 400°C or higher, 300°C or higher, 200°C or higher, 100°C or higher, 50°C or higher, 40°C or higher, or 30°C or higher after the second step.
[0033] The above-mentioned boron nitride particles are preferably used for heat dissipation members, for example. When the boron nitride particles are used for heat dissipation members, they are used in the form of a resin composition mixed with a resin, for example. That is, another embodiment of the present invention is a resin composition containing a resin and the above-mentioned boron nitride particles. This resin composition is preferably used as a heat dissipation member.
[0034] The content of the above-mentioned boron nitride particles, based on the total volume of the resin composition, is preferably 30 vol. % or more, more preferably 40 vol. % or more, and even more preferably 50 vol. % or more, from the viewpoint of improving the thermal conductivity of the resin composition and making it easier to obtain excellent heat dissipation performance, and is preferably 85 vol. % or less, more preferably 80 vol. % or less, and even more preferably 70 vol. % or less, from the viewpoint of suppressing the generation of voids during molding and the deterioration of insulation and mechanical strength.
[0035] Examples of resins include epoxy resins, silicone resins, silicone rubber, acrylic resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyimides, polyamideimides, polyetherimides, polybutylene terephthalate, polyethylene terephthalate, polyphenylene ether, polyphenylene sulfide, wholly aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS (acrylonitrile-butadiene-styrene) resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins.
[0036] The resin content may be 15 vol.% or more, 20 vol.% or more, or 30 vol.% or more, and may be 70 vol.% or less, 60 vol.% or less, or 50 vol.% or less, based on the total volume of the resin composition.
[0037] The resin composition may further contain a curing agent that cures the resin. The curing agent is appropriately selected depending on the type of resin. For example, when the resin is an epoxy resin, the curing agent may be a phenol novolac compound, an acid anhydride, an amino compound, or an imidazole compound. The content of the curing agent may be, for example, 0.5 parts by mass or more or 1.0 parts by mass or more, and 15 parts by mass or less or 10 parts by mass or less, relative to 100 parts by mass of the resin.
[0038] The boron nitride particles may be distributed in a form housed in a container, for example. That is, another embodiment of the present invention is a container comprising the above-mentioned boron nitride particles and a container for housing the boron nitride particles. The container may have any shape capable of housing the boron nitride particles, and may be, for example, a bag, a box, a bottle, a can, or the like. EXAMPLES
[0039] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.
[0040] [Example 1] (Preparation of boron nitride particles) First, in the first step, a reaction tube (quartz tube) installed in a resistance heating furnace was heated to 1150°C. Meanwhile, nitrogen gas was passed through trimethyl borate and then introduced into the reaction tube, thereby introducing trimethyl borate into the reaction tube. Meanwhile, ammonia gas was directly introduced into the reaction tube. The molar ratio of the amount of ammonia introduced to the amount of trimethyl borate introduced (ammonia / trimethyl borate) was set to 4.5. Thus, trimethyl borate and ammonia were reacted to obtain a precursor (white powder) of boron nitride particles. The reaction time was 10 seconds.
[0041] In the second step, the precursor obtained in the first step was placed in another reaction tube (alumina tube) installed in a resistance heating furnace, and nitrogen gas and ammonia gas were introduced into the reaction tube at a flow rate of 10 L / min and 15 L / min, respectively. The reaction tube was then heated at 1500°C for 2.5 hours. As a result, boron nitride particles were obtained.
[0042] (Observation of boron nitride particles and evaluation of crystallinity) The boron nitride particles obtained under the following conditions were observed using a transmission electron microscope (TEM; "JEM-2100" manufactured by JEOL Ltd.). Objective lens aperture: φ120μm Focusing lens aperture: φ150μm Recording medium: AMETEK "OrisusSC1000A1" Bining:2 Exposure time: 0.5 seconds In addition, "GMS3" manufactured by AMETEK was used as image analysis software for TEM observation and FFT analysis described later.
[0043] A TEM bright-field image (magnification: 100,000 times) of the entire obtained boron nitride particle is shown in Figure 1. Also, a TEM dark-field image of the peripheral region S of the boron nitride particle shown in Figure 1 observed at 400,000 times is shown in Figure 2.
[0044] Next, FFT analysis was performed on the 8.556 nm square area S1 in Figure 2, and an FFT image of 256 × 256 pixels was obtained. The obtained FFT pattern was analyzed in the 1 to 4 nm range in the reciprocal lattice space, as shown in Figures 3(a) and 3(b). -1 In other words, it was confirmed that the region S1 in the peripheral portion S of the boron nitride particle is composed of highly crystalline boron nitride.
[0045] As shown in Fig. 4, other regions S2 to S5 in the peripheral portion S of the boron nitride particle were also subjected to FFT analysis in the same manner as for the region S1. As a result, as shown in Figs. 4 and 5, -1 In other words, it was confirmed that the regions S2 to S5 in the peripheral region S of the boron nitride particle are also composed of highly crystalline boron nitride.
[0046] FIG. 6 shows a TEM dark-field image of the central portion C of the boron nitride particle shown in FIG. 1, observed at 400,000 times. As shown in FIG. 6, regions C1 to C4 in the central portion C of the boron nitride particle were also subjected to FFT analysis in the same manner as region S1. As a result, as shown in FIGS. 6 and 7, the 1 to 4 nm -1 No bright spots (peaks) due to the periodicity derived from the h-BN (0002) plane were confirmed within this range. In other words, it was confirmed that the regions C1 to C4 in the center C of the boron nitride particle are composed of low-crystalline boron nitride.
[0047] 3(b), 5 and 7 are graphs showing the intensities after background subtraction by the B-spline method. Also, from the graphs shown in FIG. 3(b), 5 and 7, for each of the regions S1 to S5 and C1 to C4, the intensities of 1 to 4 nm in the reciprocal lattice space are -1 The maximum intensity (relative intensity) Smax in the range of 4 nm in reciprocal space and the noise intensity -1 Exceeding 6nm -1The standard deviation (N) in the following range and the ratio (Smax / N) were calculated. The results are shown in Table 1.
[0048] [Table 1]
[0049] As described above, it was found that the peripheral part of the obtained boron nitride particles contains highly crystalline boron nitride (dominated by the area where the above-mentioned bright spots (peaks) can be confirmed), and the central part contains low-crystalline boron nitride (dominated by the area where the above-mentioned bright spots (peaks) cannot be confirmed). In addition, the diameter of the central part was approximately 40 nm, and the thickness of the peripheral part was approximately 50 nm.
[0050] (Measurement of average circularity) First, a scanning electron microscope (SEM) was used to take an SEM image (magnification: 10,000 times, image resolution: 1280 x 1024 pixels) of the obtained boron nitride particles. The obtained SEM image was analyzed using image analysis software (e.g., "MacView" manufactured by Mountec Co., Ltd.) to calculate the projected area (S) and perimeter (L) of the boron nitride particles. Next, the projected area (S) and perimeter (L) were calculated using the following formula: Circularity = 4πS / L 2 The circularity was calculated according to the formula: The average circularity was calculated from the circularities of 100 randomly selected boron nitride particles. The average circularity of the obtained boron nitride particles was 0.94.
[0051] (Measurement of average particle size) Using distilled water as a dispersion medium for dispersing boron nitride particles and sodium hexametaphosphate as a dispersant, a 0.125% by mass aqueous solution of sodium hexametaphosphate was prepared. The boron nitride particles obtained at a ratio of 0.1 g / 80 mL were added to this aqueous solution, and ultrasonic dispersion was performed once for 1 minute and 30 seconds at an AMPLITUDE of 80% using an ultrasonic homogenizer ("US-300E" manufactured by Nippon Seiki Seisakusho) to prepare a dispersion of boron nitride particles. The dispersion was taken while stirring at 60 rpm, and the volume-based particle size distribution was measured using a laser diffraction scattering particle size distribution measuring device ("LS-13 320" manufactured by Beckman Coulter, Inc.). At this time, 1.33 was used as the refractive index of water, and 1.7 was used as the refractive index of boron nitride particles. From the measurement results, the average particle size was calculated as the particle size (median diameter, d50) at the cumulative value of 50% of the cumulative particle size distribution. The average particle size of the obtained boron nitride particles was 510 nm.
[0052] [Comparative Example 1] Comparative boron nitride particles were obtained in the same manner as in Example 1, except that after the second step of Example 1, the boron nitride particles were placed in a boron nitride crucible and heated in an induction heating furnace under a nitrogen atmosphere at 2000°C for 5 hours. That is, in Comparative Example 1, comparative boron nitride particles were obtained by a conventional manufacturing method.
[0053] <Measurement of thermal conductivity> The thermal conductivity of the boron nitride particles obtained in Example 1 and the comparative boron nitride particles obtained in Comparative Example 1 was measured by the following procedure. A resin composition was obtained by mixing 100 parts by mass of naphthalene-type epoxy resin (DIC Corporation, "HP4032") and 10 parts by mass of imidazoles (Shikoku Kasei Corporation, "2E4MZ-CN") as a curing agent with 40% by volume of boron nitride particles. This resin composition was applied to a PET sheet to a thickness of 1.0 mm, and then degassed at a reduced pressure of 500 Pa for 10 minutes. Then, the mixture was cooled to 150°C and pressurized at 160 kg / cm. 2 The mixture was heated and pressed for 60 minutes under the above conditions to produce a 0.5 mm thick sheet. A measurement sample with a size of 10 mm x 10 mm was cut out from the obtained sheet, and the thermal diffusivity A (m 2 / sec) was measured. The specific gravity B (kg / m 3 ) was measured by Archimedes' law. The specific heat capacity C (J / (kg K)) of the measurement sample was also measured using a differential scanning calorimeter (Rigaku Corporation, "ThermoPlusEvoDSC8230"). Using these physical property values, the thermal conductivity H (W / (m K)) was calculated from the formula H=A×B×C.
[0054] As a result, the boron nitride particles obtained in Example 1 exhibited a thermal conductivity of 1.13 W / (m K), while the comparative boron nitride particles obtained in Comparative Example 1 exhibited a thermal conductivity of 1.12 W / (m K). Thus, in Example 1, boron nitride particles having a thermal conductivity equivalent to that of Comparative Example 1 were obtained, despite the omission of the step of Comparative Example 1 of heating at 2000°C for 5 hours in a nitrogen atmosphere (a step carried out in conventional manufacturing methods).
Claims
1. a core portion including low crystalline boron nitride; a peripheral portion disposed so as to surround the central portion and including highly crystalline boron nitride; The average circularity is 0.8 or more, The average particle size is 0.15 μm or more, Boron nitride particles are used to form heat dissipation components.
2. A resin composition comprising a resin and the boron nitride particles according to claim 1.
3. A container comprising the boron nitride particles according to claim 1 and a container for containing the boron nitride particles.
Citation Information
Patent Citations
Hexagonal nanometer boron nitride microsphere and its synthesis process and application
CN1931719A
Boron nitride spherical nanoparticle and method of producing the same
JP2010180066A
Metal-deposited crystalline boron nitride composite material, method for producing the same and use of the same
JP2011056438A
Organoboron route and process for preparation of boron nitride
US20020155052A1
Spherical boron nitride particles and production method thereof
WO2015122379A1