Flame-retardant materials
A resin-based flame retardant material with low and high melting point inorganic substances forms a flame-retardant film upon heating, addressing insufficient flame retardancy and air permeability in existing materials, achieving effective flame blocking and combustion gas management.
Patent Information
- Application Number
- JP2023120216
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-06-27
- Filing Date
- 2023-07-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2039-06-06
AI Technical Summary
Existing flame retardant materials do not provide sufficient flame retardancy and air permeability, and there is a need for improved materials that can effectively block flames and combustion gases.
A flame retardant material composed of a resin composition containing a binder resin, low melting point inorganic substances, and high melting point inorganic substances that form a flame-retardant film upon heating, with a weight loss of 48% or less and air permeability of 100 seconds or more, using components like glass frit, boron nitride, and silicone resin.
The material exhibits excellent flame retardancy with a weight loss of 48% or less and air permeability of 100 seconds or more, effectively blocking flames and combustion gases, suitable for various applications including transport aircraft and building materials.
Smart Images

Figure 0007571216000001 
Figure 0007571216000002 
Figure 0007571216000003
Abstract
Description
[Technical field]
[0001] The present invention relates to flame retardant materials. [Background technology]
[0002] Flame retardancy is one of the safety requirements for buildings, vehicles, etc. Flame retardant materials have been proposed as materials for imparting such flame retardancy (for example, Patent Documents 1 to 4).
[0003] As a means for imparting flame retardancy to a flame-retardant material, for example, a flame retardant appropriate for the intended use (e.g., halogen-based flame retardants or inorganic flame retardants) may be appropriately selected and mixed into the flame-retardant material, a flame-retardant resin appropriate for the intended use may be used as the main component of the flame-retardant material, or a flame-retardant paint (e.g., inorganic paint) may be applied.
[0004] The present inventors have conducted extensive research into new means for expressing flame retardancy, and as a result have found a new mechanism for expressing flame retardancy, established a means for realizing this mechanism, and are now able to provide a new flame-retardant material. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-186333 [Patent Document 2] Patent No. 4491778 [Patent Document 3] Patent No. 4539349 [Patent Document 4] JP 2014-231597 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a new flame-retardant material having excellent flame retardancy. [Means for solving the problem]
[0007] The flame retardant material of the present invention is A flame-retardant material formed from a resin composition (A) having a binder resin, The weight loss measured by thermogravimetric analysis in an air atmosphere at a temperature increase rate of 50° C. / min. from room temperature to 1000° C. is 48% by weight or less.
[0008] In one embodiment, the weight loss amount is 15% by weight to 35% by weight.
[0009] In one embodiment, the flame-retardant material of the present invention has an air permeability of 100 seconds or more as measured using an Oken-type digital sample-type air permeability / smoothness tester in accordance with JIS-P8117.
[0010] In one embodiment, the air permeability is 3000 seconds or more.
[0011] In one embodiment, the binder resin is at least one selected from a thermoplastic resin, a thermosetting resin, and a rubber.
[0012] In one embodiment, the resin composition (A) contains a low melting point inorganic substance and a high melting point inorganic substance.
[0013] In one embodiment, the low melting point inorganic material is a glass frit.
[0014] In one embodiment, the high melting point inorganic material is at least one selected from boron nitride, alumina, zinc oxide, titanium oxide, silica, barium titanate, calcium carbonate, glass beads, aluminum hydroxide, silicone powder, glass balloons, silica balloons, and talc.
[0015] In one embodiment, the resin composition (A) having the binder resin is a resin composition (B) having a binder resin that generates a high melting point inorganic substance upon heating and a low melting point inorganic substance.
[0016] In one embodiment, the content of the low melting point inorganic substance relative to 100 parts by weight of the binder resin that generates the high melting point inorganic substance by heating is 100 parts by weight to 500 parts by weight in terms of solid content.
[0017] In one embodiment, the total content of the binder resin that generates a high melting point inorganic substance upon heating and the low melting point inorganic substance in the resin composition (B) is 80% by weight to 100% by weight in terms of solid content.
[0018] In one embodiment, the binder resin that generates a high melting point inorganic substance upon heating is a silicone resin.
[0019] In one embodiment, the low melting point inorganic material is a glass frit.
[0020] In one embodiment, the flame-retardant material of the present invention is in the form of a sheet having a thickness of 20 μm to 3000 μm. Effect of the Invention
[0021] According to the present invention, a new flame-retardant material having excellent flame retardancy can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] ≪≪1. Flame-retardant materials≫≫ The flame-retardant material of the present invention is a flame-retardant material formed from a resin composition (A) containing a binder resin. In this specification, the flame-retardant material of the present invention in this embodiment is sometimes referred to as the flame-retardant material (A).
[0023] The resin composition (A) having a binder resin may be a resin composition (B) having a binder resin that generates a high melting point inorganic substance by heating and a low melting point inorganic substance. In this case, the flame-retardant material of the present invention is formed from the resin composition (B) having a binder resin that generates a high melting point inorganic substance by heating and a low melting point inorganic substance. In this specification, the flame-retardant material of the present invention in this embodiment may be referred to as the flame-retardant material (B).
[0024] In this specification, when the term "the flame-retardant material of the present invention" is used, it means that it includes both the flame-retardant material (A) and the flame-retardant material (B). The flame-retardant material may take any suitable form, such as a flame-retardant sheet (the sheet also includes the concept of a tape), a flame-retardant coating agent, a flame-retardant composition, etc., as long as it does not impair the effects of the present invention.
[0025] The flame-retardant material (A) can exhibit excellent flame retardancy by being formed from the resin composition (A).
[0026] The flame-retardant material (B) can exhibit excellent flame retardancy by being formed from the resin composition (B).
[0027] The flame-retardant material of the present invention has a weight loss of 48% or less as measured by thermogravimetric analysis in an air atmosphere, scanning from room temperature to 1000°C at a heating rate of 50°C / min. The weight loss is preferably 1% to 48% by weight, more preferably 5% to 45% by weight, even more preferably 10% to 40% by weight, and particularly preferably 15% to 35% by weight. When the weight loss is within the above range, the flame-retardant material of the present invention can exhibit excellent flame retardancy.
[0028] The flame-retardant material of the present invention has an air permeability measured by an Oken digital sample type air permeability / smoothness tester in accordance with JIS-P8117 of preferably 100 seconds or more, more preferably 500 seconds or more, even more preferably 1000 seconds or more, particularly preferably 2000 seconds or more, and most preferably 3000 seconds or more. If the air permeability is within the above range, the flame-retardant material of the present invention can exhibit better flame retardancy.
[0029] The flame-retardant material (A) is a material formed from the resin composition (A), and any suitable forming method can be adopted as the forming method as long as it does not impair the effects of the present invention. For example, the resin composition (A) is applied to any suitable substrate (e.g., polyethylene terephthalate film) so that the thickness after drying is a desired thickness, and the substrate is then peeled off to form a sheet-like flame-retardant material (A).
[0030] The flame-retardant material (B) is a material formed from the resin composition (B), and any suitable forming method can be adopted as long as it does not impair the effects of the present invention. For example, the resin composition (B) is applied to any suitable substrate (e.g., polyethylene terephthalate film) so that the thickness after drying is a desired thickness, and the substrate is then peeled off to form a sheet-like flame-retardant material (A).
[0031] The resin composition (A) and the resin composition (B) may be a solvent-based composition, a water-dispersed composition, or a solventless composition (e.g., a hot melt type). For example, they may be coating compositions.
[0032] Examples of a method for applying the resin composition (A) and the resin composition (B) include any appropriate application method such as an applicator, kiss coating, gravure coating, bar coating, spray coating, knife coating, wire coating, dip coating, die coating, curtain coating, dispenser coating, screen printing, and metal mask printing.
[0033] The flame-retardant material of the present invention is formed from a resin composition (A) or a resin composition (B). In this case, the composition of the flame-retardant material of the present invention, which is the resin composition (A) or the resin composition (B), may not be the same as that of the flame-retardant material of the present invention. For example, by applying the resin composition (A) to an arbitrary suitable substrate so that the thickness after drying is a desired thickness and drying by heating, at least a part of the resin composition (A) may undergo a curing reaction. In such a case, the composition of the resin composition (A), which is the material for forming the flame-retardant material (A), is not the same as that of the flame-retardant material (A). For this reason, there is a situation in which it is difficult to define the flame-retardant material of the present invention by its own composition. Therefore, the flame-retardant material of the present invention is defined by defining the resin composition (A) or the resin composition (B), which is the material for forming the flame-retardant material of the present invention.
[0034] When the flame-retardant material of the present invention is in the form of a sheet, its thickness is preferably 20 μm to 3000 μm, more preferably 40 μm to 2000 μm, even more preferably 60 μm to 1000 μm, particularly preferably 80 μm to 500 μm, and most preferably 100 μm to 300 μm. When the thickness is within the above range, the flame-retardant material of the present invention can more effectively exhibit the effects of the present invention. When the flame-retardant material is in the form of a sheet, if its thickness is too small, the flame-retardant material may not be able to exhibit sufficient flame retardancy. When the flame-retardant material is in the form of a sheet, if its thickness is too large, it may be difficult to handle the sheet.
[0035] The flame retardant material of the present invention preferably has a total heat release rate of 30 MJ / m per 10 minutes in a cone calorimeter test according to ISO 5660-1:2002. 2 Below, the maximum heat generation rate is 300kW / m 2 When the result of the cone calorimeter test is within the above range, the flame retardant material of the present invention can exhibit a more excellent flame retardancy.
[0036] When the flame-retardant material of the present invention is in the form of a sheet, it may have a protective layer on the surface thereof, provided that the effect of the present invention is not impaired.
[0037] The main component of the protective layer is preferably a polymer. The protective layer is preferably at least one selected from the group consisting of an ultraviolet-curable hard coat layer, a thermosetting hard coat layer, and an organic-inorganic hybrid hard coat layer. Such a protective layer may be composed of only one layer, or may be composed of two or more layers.
[0038] The ultraviolet-curable hard coat layer may be formed from a resin composition containing an ultraviolet-curable resin. The thermosetting hard coat layer may be formed from a resin composition containing a thermosetting resin. The organic-inorganic hybrid hard coat layer may be formed from a resin composition containing an organic-inorganic hybrid resin.
[0039] More specifically, the curable compound used in the resin as described above may be a monomer, oligomer, polymer, or silazane compound having at least one selected from the group consisting of a silanol group, a precursor of a silanol group (e.g., an alkoxysilyl group or a chlorosilyl group), an acryloyl group, a methacryloyl group, a cyclic ether group, an amino group, and an isocyanate group. From the viewpoint of being less likely to carbonize the surface during combustion, a monomer, oligomer, or polymer having a silanol group is preferred.
[0040] The resin composition capable of forming a hard coat layer may further contain any suitable additive according to purpose. Examples of such additives include photopolymerization initiators, silane coupling agents, release agents, curing agents, curing accelerators, diluents, antiaging agents, modifiers, surfactants, dyes, pigments, discoloration inhibitors, UV absorbers, softeners, stabilizers, plasticizers, defoamers, etc. The type, number and amount of additives contained in the resin composition capable of forming a hard coat layer may be appropriately set according to purpose.
[0041] The thickness of the protective layer may be any appropriate thickness as long as it does not impair the effects of the present invention, and is preferably 0.1 μm to 200 μm, more preferably 0.2 μm to 100 μm, and even more preferably 0.5 μm to 50 μm.
[0042] ≪1-1. Flame retardancy mechanism≫ The mechanism by which the flame retardant material of the present invention exhibits flame retardancy is based on the principle that when the flame retardant material is exposed to high temperatures, a phase change occurs within the flame retardant material to form a flame retardant inorganic coating, which effectively blocks flames, combustion gases, etc. As a result of investigating the components necessary for the formation of a flame retardant inorganic coating by phase change, the following was found.
[0043] In one preferred embodiment, when the three components of the binder resin, the low melting point inorganic substance, and the high melting point inorganic substance are coexisted and exposed to high temperatures, the binder resin is thermally decomposed and disappears or forms a charcoal. After that, when the low melting point inorganic substance melts and becomes liquid, the low melting point inorganic substance becomes a binder component of the high melting point inorganic substance or the charcoal, and forms a coating. Since the liquefied low melting point inorganic substance, the high melting point inorganic substance, and the charcoal are all flame retardant substances, the formed coating is a flame retardant coating.
[0044] In another preferred embodiment, when two components, a binder resin that generates a high melting point inorganic substance by heating and a low melting point inorganic substance, are coexisted and exposed to high temperatures, the binder resin is partially thermally decomposed to form a high melting point inorganic substance as a residue. When the low melting point inorganic substance is then melted and liquefied, the low melting point inorganic substance becomes a binder component of the high melting point inorganic substance and forms a coating. Since the liquefied low melting point inorganic substance and the high melting point inorganic substance are both flame retardant substances, the formed coating is a flame retardant coating.
[0045] <1-2. Resin composition (A)> The flame-retardant material (A) is formed from a resin composition (A) containing a binder resin. The binder resin may be of only one kind or of two or more kinds.
[0046] The flame-retardant material (A) preferably has a low melting point inorganic substance and a high melting point inorganic substance. In this case, the resin composition (A) has a binder resin, a low melting point inorganic substance, and a high melting point inorganic substance. The low melting point inorganic substance may be only one type or may be two or more types. The high melting point inorganic substance may be only one type or may be two or more types.
[0047] When the resin composition (A) has a binder resin, a low melting point inorganic substance, and a high melting point inorganic substance, the total content of the binder resin, the low melting point inorganic substance, and the high melting point inorganic substance in the resin composition (A) is preferably 80% by weight to 100% by weight, more preferably 85% by weight to 100% by weight, even more preferably 90% by weight to 100% by weight, particularly preferably 95% by weight to 100% by weight, and most preferably 98% by weight to 100% by weight, in terms of solid content. If the total content of the binder resin, the low melting point inorganic substance, and the high melting point inorganic substance in the resin composition (A) is within the above range in terms of solid content, the flame-retardant material (A) can more effectively exhibit the effects of the present invention. If the total content of the binder resin, the low melting point inorganic substance, and the high melting point inorganic substance in the resin composition (A) is too low in terms of solid content, the flame-retardant material may not be able to exhibit sufficient flame retardancy.
[0048] When the resin composition (A) has a binder resin, a low melting point inorganic substance, and a high melting point inorganic substance, the content ratio of the low melting point inorganic substance to 100 parts by weight of the binder resin in the resin composition (A) is preferably 100 parts by weight to 500 parts by weight, more preferably 110 parts by weight to 400 parts by weight, even more preferably 120 parts by weight to 350 parts by weight, particularly preferably 130 parts by weight to 300 parts by weight, and most preferably 140 parts by weight to 250 parts by weight, in terms of solid content. If the content ratio of the low melting point inorganic substance to 100 parts by weight of the binder resin in the resin composition (A) is within the above range in terms of solid content, the flame-retardant material (A) can more effectively exhibit the effects of the present invention. If the content ratio of the low melting point inorganic substance to 100 parts by weight of the binder resin in the resin composition (A) is outside the above range in terms of solid content, the flame-retardant material may not be able to exhibit sufficient flame retardancy.
[0049] When the resin composition (A) has a binder resin, a low melting point inorganic substance, and a high melting point inorganic substance, the content ratio of the high melting point inorganic substance to 100 parts by weight of the binder resin in the resin composition (A) is preferably 10 parts by weight to 100 parts by weight, more preferably 13 parts by weight to 80 parts by weight, even more preferably 16 parts by weight to 70 parts by weight, particularly preferably 18 parts by weight to 60 parts by weight, and most preferably 20 parts by weight to 50 parts by weight, in terms of solid content. If the content ratio of the high melting point inorganic substance to 100 parts by weight of the binder resin in the resin composition (A) is within the above range in terms of solid content, the flame-retardant material (A) can more effectively exhibit the effects of the present invention. If the content ratio of the high melting point inorganic substance to 100 parts by weight of the binder resin in the resin composition (A) is outside the above range in terms of solid content, the flame-retardant material may not be able to exhibit sufficient flame retardancy.
[0050] The resin composition (A) may contain any other appropriate components in addition to the binder resin, low melting point inorganic substance, and high melting point inorganic substance, as long as the effects of the present invention are not impaired. Such other components may be only one type or may be two or more types. Examples of such other components include solvents, crosslinking agents, pigments, dyes, leveling agents, plasticizers, thickeners, drying agents, defoamers, foaming agents, carbonization promoters, and rust inhibitors.
[0051] <1-2-1. Binder resin> As the binder resin, any suitable binder resin may be adopted as long as it does not impair the effects of the present invention. The binder resin may be one type or two or more types. Such a binder resin is preferably at least one type selected from thermoplastic resins, thermosetting resins, and rubbers, in that the effects of the present invention can be more effectively exhibited.
[0052] As the thermoplastic resin, any appropriate thermoplastic resin may be adopted as long as it does not impair the effects of the present invention. The thermoplastic resin may be one type or two or more types. Examples of such thermoplastic resins include general-purpose plastics, engineering plastics, and super engineering plastics.
[0053] Examples of general-purpose plastics include polyolefins such as polyethylene and polypropylene; vinyl chloride resins such as polyvinyl chloride (PVC) and vinylidene chloride resin (PVDC); acrylic resins such as polymethyl methacrylate; styrene resins such as polystyrene, ABS resin, AS resin, AAS resin, ACS resin, AES resin, MS resin, SMA resin, and MBS resin; polyesters such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate; alkyd resins; and unsaturated polyester resins.
[0054] Examples of engineering plastics include polyamides (nylons) such as nylon 6, nylon 66, nylon 610, nylon 11, and nylon 12; polyethers such as polyacetal (POM) and polyphenylene ether (PPE); and polycarbonates.
[0055] Examples of super engineering plastics include fluorine-based resins such as polyvinylidene fluoride (PVDF); sulfur-containing polymers such as polyphenylene sulfide (PPS) and polyethersulfone (PES); polyimide (PI); polyamide-imide (PAI); polyetherimide (PEI); polyetheretherketone (PEEK); and the like.
[0056] As the thermosetting resin, any suitable thermosetting resin may be adopted as long as it does not impair the effects of the present invention. The thermosetting resin may be one type only, or two or more types. Examples of such thermosetting resins include silicone resins, urethane resins, vinyl ester resins, phenoxy resins, epoxy resins, amino resins such as urea resins, melamine resins, and benzoguanamine resins, phenolic resins, acrylic urethane resins, and acrylic silicone resins.
[0057] As the rubber, any appropriate rubber may be adopted as long as it does not impair the effects of the present invention. The rubber may be one type or two or more types. Examples of such rubber include natural rubber (NR) and synthetic rubber.
[0058] Examples of synthetic rubbers include styrene-isoprene block polymer (SIS), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene rubber (SBR), chloroprene rubber (CR), nitrile rubber (NBR), butyl rubber (IIR), polyisobutylene (PIB), ethylene propylene rubber (e.g., EPM, EPDM, etc.), chlorosulfonated polyethylene (CSM), acrylic rubber (ACM), fluororubber (FKM), epichlorohydrin rubber (CO), urethane rubber (e.g., AU, EU, etc.), and silicone rubber (e.g., FMQ, FMVQ, MQ, PMQ, PVMQ, VMQ, etc.).
[0059] <1-2-2. Low melting point inorganic substances> As the low melting point inorganic substance, any appropriate low melting point inorganic substance may be adopted within a range that does not impair the effects of the present invention. The low melting point inorganic substance may be only one type, or may be two or more types. Such a low melting point inorganic substance is preferably an inorganic substance that melts at a temperature of 1100°C or less. As such a low melting point inorganic substance, glass frit is preferably used in terms of the effect of the present invention being more effectively exhibited. The glass frit is preferably at least one type selected from phosphate-based glass frit, borosilicate-based glass frit, and bismuth-based glass frit in terms of the effect of the present invention being more effectively exhibited.
[0060] The yield point of the glass frit is preferably 300° C. to 700° C., more preferably 300° C. to 650° C., and further preferably 300° C. to 600° C. When the yield point of the glass frit is within the above range, the flame-retardant material (A) can more effectively exhibit the effects of the present invention.
[0061] The average particle size of the glass frit is preferably 0.1 μm to 50 μm, more preferably 0.5 μm to 45 μm, further preferably 1 μm to 40 μm, particularly preferably 2 μm to 35 μm, and most preferably 3 μm to 30 μm. When the average particle size of the glass frit is within the above range, the flame-retardant material (A) can more effectively exhibit the effects of the present invention.
[0062] <1-2-3. High melting point inorganic substances> As the high melting point inorganic substance, any suitable high melting point inorganic substance may be adopted within a range that does not impair the effects of the present invention. The high melting point inorganic substance may be only one type, or may be two or more types. Such a high melting point inorganic substance is preferably an inorganic substance that does not melt at a temperature of 1100°C or less. In terms of being able to more effectively exhibit the effects of the present invention, such a high melting point inorganic substance is preferably at least one type selected from boron nitride, alumina, zinc oxide, titanium oxide, silica, barium titanate, calcium carbonate, glass beads, aluminum hydroxide, silicone powder, glass balloons, silica balloons, and talc.
[0063] The average particle size of the high melting point inorganic substance is preferably 0.01 μm to 50 μm, more preferably 0.05 μm to 40 μm, even more preferably 0.1 μm to 35 μm, particularly preferably 0.5 μm to 30 μm, and most preferably 1 μm to 25 μm. When the average particle size of the high melting point inorganic substance is within the above range, the flame retardant material (A) can more effectively exhibit the effects of the present invention.
[0064] ≪1-3. Resin composition (B)≫ The flame-retardant material (B) is formed from a resin composition (B) having a binder resin that generates a high melting point inorganic substance upon heating and a low melting point inorganic substance. That is, the resin composition (B) has a binder resin that generates a high melting point inorganic substance upon heating and a low melting point inorganic substance. The binder resin that generates a high melting point inorganic substance upon heating may be only one type or may be two or more types. The low melting point inorganic substance may be only one type or may be two or more types. The high melting point inorganic substance may be only one type or may be two or more types.
[0065] The total content of the binder resin that generates a high melting point inorganic substance by heating and the low melting point inorganic substance in the resin composition (B) is preferably 80% by weight to 100% by weight, more preferably 85% by weight to 100% by weight, even more preferably 90% by weight to 100% by weight, particularly preferably 95% by weight to 100% by weight, and most preferably 98% by weight to 100% by weight, in terms of solid content. If the total content of the binder resin that generates a high melting point inorganic substance by heating and the low melting point inorganic substance in the resin composition (B) is within the above range in terms of solid content, the flame-retardant material (B) can more effectively exhibit the effects of the present invention. If the total content of the binder resin that generates a high melting point inorganic substance by heating and the low melting point inorganic substance in the resin composition (B) is too low in terms of solid content, the flame-retardant material may not be able to exhibit sufficient flame retardancy.
[0066] The content ratio of the low melting point inorganic substance relative to 100 parts by weight of the binder resin that generates a high melting point inorganic substance by heating in the resin composition (B) is preferably 100 parts by weight to 500 parts by weight, more preferably 110 parts by weight to 450 parts by weight, even more preferably 120 parts by weight to 400 parts by weight, particularly preferably 130 parts by weight to 350 parts by weight, and most preferably 140 parts by weight to 300 parts by weight, in terms of solid content. If the content ratio of the low melting point inorganic substance relative to 100 parts by weight of the binder resin that generates a high melting point inorganic substance by heating in the resin composition (B) is within the above range in terms of solid content, the flame-retardant material (B) can more effectively exhibit the effects of the present invention. If the content ratio of the low melting point inorganic substance relative to 100 parts by weight of the binder resin that generates a high melting point inorganic substance by heating in the resin composition (B) is outside the above range in terms of solid content, the flame-retardant material may not be able to exhibit sufficient flame retardancy.
[0067] The resin composition (B) may contain any other appropriate components in addition to the binder resin that generates a high melting point inorganic substance by heating and the low melting point inorganic substance, as long as the effects of the present invention are not impaired. Such other components may be only one type or may be two or more types. Examples of such other components include solvents, crosslinking agents, high melting point inorganic substances, pigments, dyes, leveling agents, plasticizers, thickeners, drying agents, defoamers, foaming agents, carbonization promoters, and rust inhibitors.
[0068] <1-3-1. Binder resin that produces high melting point inorganic substances when heated> As the binder resin that generates a high melting point inorganic substance by heating, any suitable binder resin that generates a high melting point inorganic substance by heating can be adopted within a range that does not impair the effects of the present invention. The binder resin that generates a high melting point inorganic substance by heating may be only one type, or may be two or more types. The binder resin that generates a high melting point inorganic substance by heating is preferably a silicone resin, since the effects of the present invention can be more effectively exhibited.
[0069] As the silicone resin, any appropriate silicone resin can be used as long as it does not impair the effects of the present invention. Examples of such silicone resins include addition reaction type silicones, condensation reaction type silicones, silicone resins, and silicone rubbers.
[0070] When silicone resin is used as a binder resin that generates a high melting point inorganic substance by heating, when the silicone resin is exposed to high temperatures, a part of the silicone is thermally decomposed to form silica as a residue. After that, when the low melting point inorganic substance melts and becomes liquid, the low melting point inorganic substance becomes a binder component of silica and forms a coating. Since the liquefied low melting point inorganic substance and silica are both flame retardant substances, the formed coating becomes a flame retardant coating.
[0071] <1-3-2. Low melting point inorganic substances> For the low melting point inorganic substance contained in the resin composition (B), the explanation in the section <1-2-2. Low melting point inorganic substance> can be cited.
[0072] ≪≪2.Applications≫≫ Since the flame-retardant material of the present invention can exhibit excellent flame retardancy, it can be used as interior parts (interior parts for transport aircraft) for transport aircraft such as railway cars, airplanes, automobiles, ships, elevators, escalators, etc., exterior parts for transport aircraft, building materials, display parts, home appliance parts, electronic circuit parts, etc. It can also be suitably used as a lighting cover, particularly as a lighting cover for interior parts for transport aircraft. EXAMPLES
[0073] The present invention will be described in more detail below with reference to examples and comparative examples. However, the present invention is not limited thereto. In the following description, "parts" and "%" are by weight unless otherwise specified.
[0074] <Combustion test> A sheet of flame-retardant material or materials cut to a width of 15 mm and a length of 50 mm was exposed to a flame from a gas burner for 10 seconds. The shape and strength of the flame-retardant material or materials after exposure to flame were evaluated according to the following criteria. (shape) ◯: The sheet shape is maintained and there is no deformation. △: The sheet shape is maintained, but there is some deformation. ×: The sheet shape cannot be maintained. (strength) 〇: The sheet shape is maintained when dropped from a height of 10 cm. ×: The sheet shape cannot be maintained when dropped from a height of 10 cm.
[0075] <Weight loss measurement> The sample was placed in a TGA (thermobalance) measuring device and measured by scanning from room temperature to 1000°C at a heating rate of 50°C / min in an air atmosphere to determine the amount of weight loss at 1000°C.
[0076] <Air permeability measurement> Measurements were taken using Asahi Seiko Co., Ltd.'s Oken-type digital sample-type air permeability and smoothness tester (model: EG.6) using a test method based on JIS-P8117.
[0077] [Synthesis Example 1] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Nippon Zeon Co., Ltd.), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (A-1).
[0078] [Synthesis Example 2] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of aluminum hydroxide (product name: BF013, manufactured by Nippon Light Metal Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (B-1).
[0079] [Synthesis Example 3] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of talc (product name: Imported talc, manufactured by Maruo Calcium Corporation), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (C-1).
[0080] [Synthesis Example 4] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of calcium carbonate (product name: heavy calcium carbonate, manufactured by Maruo Calcium Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (D-1).
[0081] [Synthesis Example 5] To a container equipped with a stirrer, 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Nippon Zeon Co., Ltd.), 20 parts by weight of glass beads (product name: CF0018WB15-01, manufactured by Nippon Frit Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene were added and mixed by stirring to obtain a synthetic rubber composition (E-1).
[0082] [Synthesis Example 6] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of titanium oxide (product name: TITONE R-42, manufactured by Sakai Chemical Industry Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (F-1).
[0083] [Synthesis Example 7] Into a container equipped with a stirrer, 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of aluminum oxide (product name: TITONE R-42, manufactured by Sakai Chemical Industry Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene were added and mixed by stirring to obtain a synthetic rubber composition (G-1).
[0084] [Synthesis Example 8] To a container equipped with a stirrer, 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of silicone powder (product name: KMP-600, manufactured by Shin-Etsu Chemical Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene were added and mixed by stirring to obtain a synthetic rubber composition (H-1).
[0085] [Synthesis Example 9] A container equipped with a stirrer was charged with 80 parts by weight of natural rubber (product name: Natural Rubber (INT No.1 RSS), manufactured by Toyota Tsusho Corporation), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene, and the mixture was stirred to obtain a natural rubber composition (A-1).
[0086] [Synthesis Example 10] Into a container equipped with a stirrer, 266 parts by weight of acrylic rubber (product name: SK Dyne 1429DTB, solid content concentration: 30%, manufactured by Soken Chemical Industries, Ltd.), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 114 parts by weight of toluene were added and mixed by stirring to obtain an acrylic rubber composition (A-1).
[0087] [Synthesis Example 11] A container equipped with a stirrer was charged with 80 parts by weight of vinyl chloride resin (product name: Shin-Etsu PVC TK-1300, manufactured by Shin-Etsu Chemical Co., Ltd.), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene, and the mixture was stirred to obtain a vinyl chloride resin composition (A-1).
[0088] [Synthesis Example 12] A container equipped with a stirrer was charged with 160 parts by weight of nylon resin (product name: AQ Nylon P-95, solid content concentration: 50%, manufactured by Toray Industries, Inc.), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 220 parts by weight of distilled water, and the mixture was stirred to obtain a nylon resin composition (A-1).
[0089] [Synthesis Example 13] A container equipped with a stirrer was charged with 195 parts by weight of a fluororesin (product name: Obligato SS0057, solid content concentration: 41%, manufactured by AGC Coatec), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of a phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 185 parts by weight of toluene, and the mixture was stirred to obtain a fluororesin composition (A-1).
[0090] [Synthesis Example 14] Into a container equipped with a stirrer, 200 parts by weight of an epoxy resin (trade name: jER1256B40, solid content concentration: 40%, manufactured by Mitsubishi Chemical Corporation), 40 parts by weight of a curing agent (trade name: IBMI12, manufactured by Mitsubishi Chemical Corporation), 20 parts by weight of silica (trade name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of a phosphate-based glass frit (trade name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 180 parts by weight of MEK were added and mixed by stirring to obtain an epoxy resin composition (A-1).
[0091] [Synthesis Example 15] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Nippon Zeon Co., Ltd.), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (A-2).
[0092] [Synthesis Example 16] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of aluminum hydroxide (product name: BF013, manufactured by Nippon Light Metals Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (B-2).
[0093] [Synthesis Example 17] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of talc (product name: Imported talc, manufactured by Maruo Calcium Corporation), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (C-2).
[0094] [Synthesis Example 18] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of calcium carbonate (product name: heavy calcium carbonate, manufactured by Maruo Calcium Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (D-2).
[0095] [Synthesis Example 19] To a container equipped with a stirrer, 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Nippon Zeon Co., Ltd.), 20 parts by weight of glass beads (product name: CF0018WB15-01, manufactured by Nippon Frit Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene were added and mixed by stirring to obtain a synthetic rubber composition (E-2).
[0096] [Synthesis Example 20] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of titanium dioxide (product name: TITONE R-42, manufactured by Sakai Chemical Industry Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (F-2).
[0097] [Synthesis Example 21] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of aluminum oxide (product name: TITONE R-42, manufactured by Sakai Chemical Industry Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (G-2).
[0098] [Synthesis Example 22] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Zeon Corporation), 20 parts by weight of silicone powder (product name: KMP-600, manufactured by Shin-Etsu Chemical Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (H-2).
[0099] [Synthesis Example 23] A container equipped with a stirrer was charged with 80 parts by weight of natural rubber (product name: Natural Rubber (INT No.1 RSS), manufactured by Toyota Tsusho Corporation), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 700 parts by weight of toluene, and the mixture was stirred to obtain a natural rubber composition (A-2).
[0100] [Synthesis Example 24] Into a container equipped with a stirrer, 266 parts by weight of acrylic rubber (product name: SK Dyne 1429DTB, solid content concentration: 30%, manufactured by Soken Chemical Industries, Ltd.), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 114 parts by weight of toluene were added and mixed with stirring to obtain an acrylic rubber composition (A-2).
[0101] [Synthesis Example 25] A container equipped with a stirrer was charged with 80 parts by weight of vinyl chloride resin (product name: Shin-Etsu PVC TK-1300, manufactured by Shin-Etsu Chemical Co., Ltd.), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene, and the mixture was stirred to obtain a vinyl chloride resin composition (A-2).
[0102] [Synthesis Example 26] A vessel equipped with a stirrer was charged with 160 parts by weight of nylon resin (product name: AQ Nylon P-95, solid content concentration: 50%, manufactured by Toray Industries, Inc.), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 220 parts by weight of distilled water, and the mixture was stirred to obtain a nylon resin composition (A-2).
[0103] [Synthesis Example 27] A container equipped with a stirrer was charged with 195 parts by weight of a fluororesin (product name: Obligato SS0057, solid content concentration: 41%, manufactured by AGC Coatec), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of a borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 185 parts by weight of toluene, and the mixture was stirred to obtain a fluororesin composition (A-2).
[0104] [Synthesis Example 28] Into a container equipped with a stirrer, 200 parts by weight of an epoxy resin (trade name: jER1256B40, solid content concentration: 40%, manufactured by Mitsubishi Chemical Corporation), 40 parts by weight of a curing agent (trade name: IBMI12, manufactured by Mitsubishi Chemical Corporation), 20 parts by weight of silica (trade name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), 200 parts by weight of a borosilicate glass frit (trade name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 180 parts by weight of MEK were added and mixed by stirring to obtain an epoxy resin composition (A-2).
[0105] [Synthesis Example 29] Into a container equipped with a stirrer, 100 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Nippon Zeon Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 300 parts by weight of toluene were added and mixed by stirring to obtain a synthetic rubber composition (I).
[0106] [Synthesis Example 30] A container equipped with a stirrer was charged with 80 parts by weight of synthetic rubber (product name: Quintac3520, manufactured by Nippon Zeon Co., Ltd.), 20 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 100 parts by weight of toluene, and the mixture was stirred to obtain a synthetic rubber composition (J).
[0107] Example 1 The synthetic rubber composition (A-1) obtained in Synthesis Example 1 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (1). The results are shown in Tables 1 and 2.
[0108] Example 2 The synthetic rubber composition (B-1) obtained in Synthesis Example 2 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (2). The results are shown in Tables 1 and 2.
[0109] Example 3 The synthetic rubber composition (C-1) obtained in Synthesis Example 3 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (3). The results are shown in Tables 1 and 2.
[0110] Example 4 The synthetic rubber composition (D-1) obtained in Synthesis Example 4 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (4). The results are shown in Tables 1 and 2.
[0111] Example 5 The synthetic rubber composition (E-1) obtained in Synthesis Example 5 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (5). The results are shown in Tables 1 and 2.
[0112] Example 6 The synthetic rubber composition (F-1) obtained in Synthesis Example 6 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (6). The results are shown in Tables 1 and 2.
[0113] Example 7 The synthetic rubber composition (G-1) obtained in Synthesis Example 7 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (7). The results are shown in Tables 1 and 2.
[0114] Example 8 The synthetic rubber composition (H-1) obtained in Synthesis Example 8 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (8). The results are shown in Tables 1 and 2.
[0115] Example 9 The natural rubber composition (A-1) obtained in Synthesis Example 9 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (9). The results are shown in Tables 1 and 2.
[0116] Example 10 The acrylic rubber composition (A-1) obtained in Synthesis Example 10 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (10). The results are shown in Tables 1 and 2.
[0117] Example 11 The vinyl chloride resin composition (A-1) obtained in Synthesis Example 11 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (11). The results are shown in Tables 1 and 2.
[0118] Example 12 The nylon resin composition (A-1) obtained in Synthesis Example 12 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (12). The results are shown in Tables 1 and 2.
[0119] Example 13 The fluororesin composition (A-1) obtained in Synthesis Example 13 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (13). The results are shown in Tables 1 and 2.
[0120] Example 14 The epoxy resin composition (A-1) obtained in Synthesis Example 14 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (14). The results are shown in Tables 1 and 2.
[0121] Example 15 The synthetic rubber composition (A-2) obtained in Synthesis Example 15 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (15). The results are shown in Tables 1 and 2.
[0122] Example 16 The synthetic rubber composition (B-2) obtained in Synthesis Example 16 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (16). The results are shown in Tables 1 and 2.
[0123] Example 17 The synthetic rubber composition (C-2) obtained in Synthesis Example 17 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (17). The results are shown in Tables 1 and 2.
[0124] Example 18 The synthetic rubber composition (D-2) obtained in Synthesis Example 18 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (18). The results are shown in Tables 1 and 2.
[0125] Example 19 The synthetic rubber composition (E-2) obtained in Synthesis Example 19 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (19). The results are shown in Tables 1 and 2.
[0126] Example 20 The synthetic rubber composition (F-2) obtained in Synthesis Example 20 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (20). The results are shown in Tables 1 and 2.
[0127] Example 21 The synthetic rubber composition (G-2) obtained in Synthesis Example 21 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (21). The results are shown in Tables 1 and 2.
[0128] Example 22 The synthetic rubber composition (H-2) obtained in Synthesis Example 22 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (22). The results are shown in Tables 1 and 2.
[0129] Example 23 The natural rubber composition (A-2) obtained in Synthesis Example 23 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (23). The results are shown in Tables 1 and 2.
[0130] Example 24 The acrylic rubber composition (A-2) obtained in Synthesis Example 24 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (24). The results are shown in Tables 1 and 2.
[0131] Example 25 The vinyl chloride resin composition (A-2) obtained in Synthesis Example 25 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (25). The results are shown in Tables 1 and 2.
[0132] Example 26 The nylon resin composition (A-2) obtained in Synthesis Example 26 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (26). The results are shown in Tables 1 and 2.
[0133] Example 27 The fluororesin composition (A-2) obtained in Synthesis Example 27 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (27). The results are shown in Tables 1 and 2.
[0134] Example 28 The epoxy resin composition (A-2) obtained in Synthesis Example 28 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating in a hot air circulation oven at 80° C. for 2 minutes and at 110° C. for 2 minutes, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (28). The results are shown in Tables 1 and 2.
[0135] Comparative Example 1 The synthetic rubber composition (I) obtained in Synthesis Example 29 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a material (C1). The results are shown in Tables 1 and 2.
[0136] Comparative Example 2 The synthetic rubber composition (J) obtained in Synthesis Example 30 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a material (C2). The results are shown in Tables 1 and 2.
[0137] [Table 1]
[0138] [Table 2]
[0139] [Synthesis Example 31] To a container equipped with a stirrer, 50 parts by weight of silicone resin (product name: KE-1950-50A, manufactured by Shin-Etsu Chemical Co., Ltd.), 50 parts by weight of silicone resin (product name: KE-1950-50B, manufactured by Shin-Etsu Chemical Co., Ltd.), 200 parts by weight of phosphate-based glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and 128 parts by weight of toluene were added and mixed by stirring to obtain a silicone resin composition (S-1).
[0140] [Synthesis Example 32] To a container equipped with a stirrer, 50 parts by weight of silicone resin (product name: KE-1950-50A, manufactured by Shin-Etsu Chemical Co., Ltd.), 50 parts by weight of silicone resin (product name: KE-1950-50B, manufactured by Shin-Etsu Chemical Co., Ltd.), 200 parts by weight of borosilicate glass frit (product name: CY5600, manufactured by Nippon Frit Co., Ltd.), and 128 parts by weight of toluene were added and mixed by stirring to obtain a silicone resin composition (S-2).
[0141] Example 29 The silicone resin composition (S-1) obtained in Synthesis Example 31 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (29). The results are shown in Tables 3 and 4.
[0142] Example 30 The silicone resin composition (S-2) obtained in Synthesis Example 32 was applied onto a polyethylene terephthalate film (thickness: 50 μm, product name: Lumirror S10, manufactured by Toray Industries, Inc.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 80° C. for 2 minutes and at 110° C. for 2 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (30). The results are shown in Tables 3 and 4.
[0143] [Table 3]
[0144] [Table 4]
[0145] [Synthesis Example 33] Into a container equipped with a stirrer, 100 parts by weight of an epoxy-based paint (product name: Mild Rust Guard, manufactured by SK Chemical Co., Ltd.), 10 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 100 parts by weight of glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.) were added and mixed by stirring to obtain a coating composition (A-1).
[0146] [Synthesis Example 34] Into a container equipped with a stirrer, 100 parts by weight of an epoxy-based paint (product name: Mild Rust Guard, manufactured by SK Chemical Co., Ltd.), 10 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 200 parts by weight of glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.) were added and mixed by stirring to obtain a coating composition (A-2).
[0147] [Synthesis Example 35] Into a container equipped with a stirrer, 100 parts by weight of an epoxy-based paint (product name: Mild Rust Guard, manufactured by SK Chemical Industries, Ltd.), 10 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 300 parts by weight of glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.) were added and mixed by stirring to obtain a coating composition (A-3).
[0148] [Synthesis Example 36] A container equipped with a stirrer was charged with 100 parts by weight of a urethane paint (product name: Retan ECO Bake, manufactured by Kansai Paint Co., Ltd.), 10 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 100 parts by weight of glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and the mixture was stirred to obtain a coating composition (B-1).
[0149] [Synthesis Example 37] A container equipped with a stirrer was charged with 100 parts by weight of a urethane paint (product name: Retan ECO Bake, manufactured by SK Chemical Co., Ltd.), 10 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 200 parts by weight of glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and the mixture was stirred to obtain a coating composition (B-2).
[0150] [Synthesis Example 38] A container equipped with a stirrer was charged with 100 parts by weight of a urethane paint (product name: Retan ECO Bake, manufactured by SK Chemical Co., Ltd.), 10 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 300 parts by weight of glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and the mixture was stirred to obtain a coating composition (B-3).
[0151] [Synthesis Example 39] A container equipped with a stirrer was charged with 100 parts by weight of a fluorine-based paint (product name: Super Odefresh F, manufactured by Nippon Paint Co., Ltd.), 10 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 100 parts by weight of glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and the mixture was stirred to obtain a coating composition (C-1).
[0152] [Synthesis Example 40] A container equipped with a stirrer was charged with 100 parts by weight of a fluorine-based paint (product name: Super Odefresh F, manufactured by Nippon Paint Co., Ltd.), 10 parts by weight of silica (product name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 200 parts by weight of glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.), and the mixture was stirred to obtain a coating composition (C-2).
[0153] [Synthesis Example 41] To a container equipped with a stirrer, 100 parts by weight of an acrylic paint (trade name: Nippe Roadline 1000, manufactured by Nippon Paint Co., Ltd.), 10 parts by weight of silica (trade name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 100 parts by weight of glass frit (trade name: VY0053M, manufactured by Nippon Frit Co., Ltd.) were added and mixed by stirring to obtain a coating composition (D-1).
[0154] [Synthesis Example 42] Into a container equipped with a stirrer, 100 parts by weight of an acrylic paint (trade name: Nippe Roadline, manufactured by Nippon Paint Co., Ltd.), 10 parts by weight of silica (trade name: AEROSIL RX 200, manufactured by Nippon Aerosil Co., Ltd.), and 200 parts by weight of glass frit (trade name: VY0053M, manufactured by Nippon Frit Co., Ltd.) were added and mixed by stirring to obtain a coating composition (D-2).
[0155] [Synthesis Example 43] In a container equipped with a stirrer, 100 parts by weight of a silicone-based paint (product name: Super Odefresh Si, manufactured by Nippon Paint Co., Ltd.) and 100 parts by weight of a glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.) were added and mixed by stirring to obtain a coating composition (E-1).
[0156] [Synthesis Example 44] In a container equipped with a stirrer, 100 parts by weight of a silicone-based paint (product name: Super Odefresh Si, manufactured by Nippon Paint Co., Ltd.) and 200 parts by weight of a glass frit (product name: VY0053M, manufactured by Nippon Frit Co., Ltd.) were added and mixed by stirring to obtain a coating composition (E-2).
[0157] Example 31 The coating composition (A-1) obtained in Synthesis Example 33 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (31). The results are shown in Tables 5 and 6.
[0158] Example 32 The coating composition (A-2) obtained in Synthesis Example 34 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (32). The results are shown in Tables 5 and 6.
[0159] Example 33 The coating composition (A-3) obtained in Synthesis Example 35 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (33). The results are shown in Tables 5 and 6.
[0160] Example 34 The coating composition (B-1) obtained in Synthesis Example 36 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (34). The results are shown in Tables 5 and 6.
[0161] Example 35 The coating composition (B-2) obtained in Synthesis Example 37 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (35). The results are shown in Tables 5 and 6.
[0162] Example 36 The coating composition (B-3) obtained in Synthesis Example 38 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (36). The results are shown in Tables 5 and 6.
[0163] Example 37 The coating composition (C-1) obtained in Synthesis Example 39 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRF, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (37). The results are shown in Tables 5 and 6.
[0164] Example 38 The coating composition (C-2) obtained in Synthesis Example 40 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRF, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (38). The results are shown in Tables 5 and 6.
[0165] Example 39 The coating composition (D-1) obtained in Synthesis Example 41 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (39). The results are shown in Tables 5 and 6.
[0166] Example 40 The coating composition (D-2) obtained in Synthesis Example 42 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (40). The results are shown in Tables 5 and 6.
[0167] Example 41 The coating composition (E-1) obtained in Synthesis Example 43 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (41). The results are shown in Tables 5 and 6.
[0168] Example 42 The coating composition (E-2) obtained in Synthesis Example 44 was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the coating was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a flame-retardant material (42). The results are shown in Tables 5 and 6.
[0169] Comparative Example 3 An epoxy paint (product name: Mild Rust Guard, manufactured by SK Chemicals) was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, manufactured by Mitsubishi Chemical Corporation) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the film was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain material (C3). The results are shown in Tables 5 and 6.
[0170] Comparative Example 4 A urethane paint (product name: Retan ECO Bake, Kansai Paint Co., Ltd.) was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, Mitsubishi Chemical Co., Ltd.) using a Tester Sangyo Co., Ltd. applicator so that the thickness after drying would be 100 μm, and then the film was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain material (C4). The results are shown in Tables 5 and 6.
[0171] Comparative Example 5 A fluorine-based paint (product name: Super Ode Fresh F, Nippon Paint Co., Ltd.) was applied to a polyethylene terephthalate film (thickness: 50 μm, product name: Diafoil MRS, Mitsubishi Chemical Co., Ltd.) using an applicator manufactured by Tester Sangyo Co., Ltd., so that the thickness after drying would be 100 μm, and then the film was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain a material (C5). The results are shown in Tables 5 and 6.
[0172] Comparative Example 6 An acrylic paint (trade name: Nippe Roadline 1000, manufactured by Nippon Paint Co., Ltd.) was applied to a polyethylene terephthalate film (thickness: 50 μm, trade name: Diafoil MRS, manufactured by Mitsubishi Chemical Co., Ltd.) using an applicator manufactured by Tester Sangyo Co., Ltd. so that the thickness after drying would be 100 μm, and then the film was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain material (C6). The results are shown in Tables 5 and 6.
[0173] Comparative Example 7 Silicone paint (trade name: Super Ode Fresh Si, Nippon Paint) was applied to a polyethylene terephthalate film (thickness: 50 μm, trade name: Diafoil MRS, Mitsubishi Chemical) using a Tester Sangyo applicator so that the thickness after drying would be 100 μm, and then the film was dried by heating at 100° C. for 30 minutes in a hot air circulation oven, and the polyethylene terephthalate film was peeled off to obtain material (C7). The results are shown in Tables 5 and 6.
[0174] [Table 5]
[0175] [Table 6] [Industrial Applicability]
[0176] The flame-retardant material of the present invention can be suitably used, for example, as interior components for transport vehicles such as railway cars, aircraft, automobiles, ships, elevators, and escalators (interior components for transport vehicles), exterior components for transport vehicles, building materials, display components, home appliance components, electronic circuit components, and lighting covers.
Claims
1. A flame-retardant material formed from a resin composition (A) having a binder resin, The resin composition (A) further contains a low melting point inorganic substance and a high melting point inorganic substance, the low melting point inorganic material is a glass frit, the total content of the binder resin, the low melting point inorganic substance, and the high melting point inorganic substance is 80% by weight to 100% by weight; the content ratio of the low melting point inorganic substance relative to 100 parts by weight of the binder resin is 100 parts by weight to 500 parts by weight; the content ratio of the high melting point inorganic substance relative to 100 parts by weight of the binder resin is 10 parts by weight to 80 parts by weight, The low melting point inorganic substance is an inorganic substance that melts at a temperature of 1100° C. or less, The high melting point inorganic substance is an inorganic substance that does not melt at a temperature of 1100° C. or less, The flame-retardant material has a weight loss of 48% or less as measured by thermogravimetric analysis in which the material is scanned from room temperature to 1000° C. at a heating rate of 50° C. / min in an air atmosphere; the binder resin is at least one selected from a thermoplastic resin, a thermosetting resin, and a rubber, and the thermosetting resin is at least one selected from a urethane resin, a vinyl ester resin, a phenoxy resin, an epoxy resin, an amino resin, a phenolic resin, and an acrylic urethane resin; Flame retardant material.
2. The flame retardant material according to claim 1, wherein the weight loss is from 15% to 35% by weight.
3. 3. The flame-retardant material according to claim 1, which has an air permeability of 100 seconds or more as measured by an Oken type digital sample type air permeability / smoothness tester in accordance with JIS-P8117.
4. The flame retardant material according to claim 3, wherein the air permeability is 3000 seconds or more.
5. The flame-retardant material according to any one of claims 1 to 4, wherein the high-melting point inorganic substance is at least one selected from the group consisting of boron nitride, alumina, zinc oxide, titanium oxide, silica, barium titanate, calcium carbonate, glass beads, aluminum hydroxide, silicone powder, glass balloons, silica balloons, and talc.
6. The flame-retardant material according to any one of claims 1 to 5, which is in the form of a sheet having a thickness of 20 µm to 3000 µm.
7. 7. The flame-retardant material according to claim 1, wherein the content of the high-melting point inorganic substance is 20 parts by weight to 100 parts by weight based on 100 parts by weight of the binder resin.
8. A flame-retardant material described in any one of claims 1 to 7, in sheet form and further having a protective layer.
9. 9. The flame-retardant material according to claim 1, wherein the glass frit is at least one selected from the group consisting of a phosphate-based glass frit, a borosilicate-based glass frit, and a bismuth-based glass frit.
Citation Information
Patent Citations
Heat-resistant coating material
JP1994212113A
Fire retardant decorative material and fire retardant paint composition
JP1995186333A
Flame-retardant resin composition and method of making resin flame-retardant
JP1995309970A
Fire resistant polymer composition
JP2006504859A
Fire proof resin foaming laminate
JP2009208355A