Setting method and manufacturing method
Patent Information
- Application Number
- JP2020052419
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-24
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-03-24
AI Technical Summary
【0014】 本開示の技術によれば、防食鉄筋の製造工程において、樹脂層に落下させて付着させる粒子の落下量の最適化を図ることができる。
Smart Images

Figure 0007571383000005 
Figure 0007571383000006 
Figure 0007571383000007
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a setting method and a manufacturing method, and in particular to a technique suitable for setting the amount of particles that fall and adhere to a resin layer covering a reinforcing bar during the manufacturing process of corrosion-resistant reinforcing bars. [Background technology]
[0002] As an example of rebar for concrete, a corrosion-resistant rebar (or rust-resistant rebar) has been put to practical use in which the surface of a rebar bar is coated with a PVB resin whose main component is polyvinyl butyral (hereinafter, PVB), and particles (e.g., silica sand, etc.) are attached to the PVB resin layer (see, for example, Patent Documents 1 and 2). The silica sand attached to the PVB resin layer forms numerous minute protrusions on the surface of the PVB resin layer, which increases the adhesive strength with concrete. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-043898 A [Patent Document 2] JP 2011-147845 A Summary of the Invention [Problem to be solved by the invention]
[0004] Here, the corrosion-resistant rebar is manufactured by sequentially carrying out the following steps: (1) a first step is to blast the surface of the rebar; (2) a second step is to electrostatically coat the surface of the rebar with a powder whose main component is PVB resin; (3) a third step is to heat and melt the PVB resin layer applied to the rebar using a high-frequency heating device; (4) a fourth step is to allow a predetermined amount of silica sand to fall by gravity from above the rebar to adhere to the PVB resin layer; and (5) a fifth step is to cool the molten PVB resin layer.
[0005] In order to obtain the desired adhesion and anchorage performance to concrete in the corrosion-resistant rebar manufactured in this manner, the amount of silica sand retained in the PVB resin layer is important, and it is particularly desirable to properly control the amount of silica sand that falls in the above-mentioned fourth step.
[0006] In the manufacturing process of corrosion-resistant rebar, the rebar is fed in the axial direction while rotating around its axis, so if the amount of silica sand falling in the above-mentioned fourth step is insufficient, the silica sand will adhere in a spiral shape to the outer periphery of the PVB resin layer, resulting in a product with an undesirable appearance. On the other hand, even if the amount of silica sand falling is increased more than necessary, some of the silica sand will not adhere to the PVB resin layer and will be wasted, which may cause a decrease in manufacturing efficiency. For this reason, in the manufacturing of corrosion-resistant rebar, it is desirable to set the amount of silica sand falling in the above-mentioned fourth step to an optimal amount.
[0007] The technology disclosed herein has been made in consideration of the above circumstances, and aims to optimize the amount of particles that fall onto a resin layer and adhere to it during the manufacturing process of corrosion-resistant rebar. [Means for solving the problem]
[0008] The setting method disclosed herein is a method for setting the drop amount of particles to be dropped onto and adhere to a resin layer in a manufacturing process of a corrosion-resistant rebar having a rebar rod, a resin layer covering at least a portion of the outer periphery of the rebar rod, and particles adhered and held by the resin layer, and is characterized in that it includes a first step of manufacturing the corrosion-resistant rebar by setting the drop amount of the particles to two or more different drop amounts, a second step of measuring the adhesion strength to concrete of each of the corrosion-resistant rebars manufactured with the two or more different drop amounts, and a third step of determining an optimal drop amount of the particles in the manufacturing process based on the relationship between the drop amount set in the first step and the adhesion strength measured in the second step.
[0009] In the third step, it is preferable that the optimum falling amount is the falling amount immediately before the adhesive strength starts to decrease with an increase in the falling amount of the particles.
[0010] In addition, in the second step, it is preferable to further measure the adhesion strength of unpainted reinforcing bar not covered with a resin layer to concrete, and in the third step, the smallest drop amount among the drop amounts showing an adhesion strength higher than the adhesion strength of the unpainted reinforcing bar to concrete is set as the lower limit of the optimal drop amount.
[0011] Furthermore, in the manufacturing process, the reinforcing bar is rotated around its axis while being sent out in the axial direction, thereby causing the particles to adhere to the outer periphery of the resin layer, and in the third step, it is preferable that the smallest falling amount among the falling amounts at which the particles do not adhere in a spiral shape to the outer periphery of the resin layer is set as the lower limit value of the optimal falling amount.
[0012] The resin layer may be a resin layer containing polyvinyl butyral as a main component, and the particles may be silica sand.
[0013] The manufacturing method disclosed herein is a method for manufacturing corrosion-resistant rebar using the optimal drop amount set by the setting method, and is characterized in that it includes the steps of coating the outer periphery of the rebar with a resin layer, heating and melting the resin layer, and dropping the particles into the molten resin layer at the optimal drop amount to adhere to the particles. Effect of the Invention
[0014] According to the technology disclosed herein, it is possible to optimize the amount of particles that fall onto a resin layer and adhere to it during the manufacturing process of corrosion-resistant rebar. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a schematic perspective view showing an example of a reinforcing bar used in the corrosion-resistant reinforcing bar according to the present embodiment. [Diagram 2] FIG. 2 is a schematic radial cross-sectional view showing an example of a corrosion-resistant rebar according to the present embodiment. [Diagram 3] FIG. 2 is a flow diagram illustrating an example of a method for manufacturing a corrosion-resistant rebar according to the present embodiment. [Figure 4] FIG. 2 is a schematic diagram showing an example of a manufacturing line for corrosion-resistant rebar according to the present embodiment. [Diagram 5] FIG. 2 is a schematic vertical cross-sectional view of a silica sand deposition device that constitutes a part of the production line according to the present embodiment. [Figure 6] FIG. 4 is a flow diagram illustrating the flow of a setting method according to the present embodiment. [Figure 7] FIG. 2 is a flow chart illustrating the flow of a method for measuring the amount of adhered silica sand according to the present embodiment. [Figure 8] FIG. 2 is a schematic diagram illustrating a method for measuring the amount of silica sand adhesion according to the embodiment. [Figure 9] FIG. 2 is a schematic diagram illustrating a method for measuring the amount of silica sand adhesion according to the embodiment. [Figure 10] FIG. 2 is a schematic diagram illustrating a method for measuring the amount of silica sand adhesion according to the embodiment. [Figure 11] 1 is a graph showing the bond stress and maximum bond stress of each sample. [Figure 12] 1 is a graph showing the relationship between the adhesion stress of each sample and the amount of silica sand falling according to each falling amount condition. [Figure 13] 1 is a graph showing the relationship between the adhesion stress of each sample and the amount of silica sand adhesion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, a setting method and a manufacturing method according to the present embodiment will be described with reference to the accompanying drawings.
[0017] [Corrosion-resistant rebar] FIG. 1 is a schematic oblique view showing an example of a reinforcing bar 11 used in the corrosion-resistant reinforcing bar of this embodiment, and FIG. 2 is a schematic radial cross-sectional view showing an example of the corrosion-resistant reinforcing bar 10 of this embodiment.
[0018] As shown in Fig. 1, the reinforcing bar 11 comprises a substantially cylindrical bar body 12, at least one or more longitudinal ribs 13 extending in the axial direction on the outer circumferential surface of the bar body 12, and a plurality of transverse ribs 14 extending in the circumferential direction on the outer circumferential surface of the bar body 12 and provided at predetermined intervals in the axial direction. The arrangement pattern of the longitudinal ribs 13 and transverse ribs 14 is not limited to the illustrated example, and other arrangement patterns may be used. Furthermore, the reinforcing bar 11 is not limited to a deformed reinforcing bar having ribs, and may be another reinforcing bar such as a round bar.
[0019] As shown in Fig. 2, the corrosion-resistant rebar 10 of this embodiment is manufactured by forming a PVB resin layer 20, mainly composed of PVB resin, on the outer peripheral surface of a rebar bar 11, and adhering and holding silica sand 30 as particles to the PVB resin layer 20. The manufacturing method of the corrosion-resistant rebar 10 will be described in detail below with reference to Figs. 3 to 5.
[0020] [Manufacturing method / production line] Figure 3 is a flow diagram illustrating an example of a manufacturing method for corrosion-resistant rebar 10 in this embodiment, Figure 4 is a schematic diagram showing an example of a manufacturing line 50 for corrosion-resistant rebar 10, and Figure 5 is a schematic vertical cross-sectional view of a silica sand deposition device 54 that constitutes part of the manufacturing line 50.
[0021] As shown in Fig. 3, the corrosion-resistant rebar 10 is manufactured by sequentially carrying out the following steps: (1) a first step of blasting the surface of the rebar bar 11; (2) a second step of heating the rebar bar 11 with a high-frequency heating device; (3) a third step of applying a powder mainly composed of PVB resin to the surface of the rebar bar 11 by electrostatic powder coating; (4) a fourth step of dropping silica sand onto the molten PVB resin layer 20 to cause it to adhere; and (5) a fifth step of cooling and solidifying the molten PVB resin layer 20. Note that the manufacturing method of the corrosion-resistant rebar 10 is not limited to this, and other methods may also be used. For example, the order of the second step and the third step may be reversed.
[0022] 4, the production line 50 mainly includes a blasting device 51, a high-frequency heating device 52, an electrostatic coating device 53, a silica sand deposition device 54, and a cooling device 59. In the production line 50, the reinforcing bar 11 is sent out in the axial direction while rotating around the axis by a rotary sending-out mechanism having rollers (not shown) or the like, and passes through each of the devices 51, 52, 53, 54, 59 in order.
[0023] The blasting device 51 performs blasting on the surface of the reinforcing bar 11 to remove oxide scale and to prepare a surface for painting.
[0024] The high-frequency heating device 52 includes a high-frequency heating coil (not shown), and heats the reinforcing bars 11 to a predetermined high temperature (for example, 200 to 250° C.).
[0025] The electrostatic coating device 53 sprays powder paint (powder mainly composed of PVB resin) charged by a high voltage generator (not shown) onto the grounded reinforcing bar 11. During this process, the reinforcing bar 11 is fed axially while rotating, so that a substantially uniform PVB resin layer can be formed over the entire outer periphery of the reinforcing bar 11. The thickness of the PVB resin layer may be, for example, 220±40 μm for civil engineering work and 180±50 μm for architectural work. Note that the thickness is not limited to these values and may be set to an appropriate value depending on the strength, workability, etc.
[0026] The silica sand deposition device 54 has a hopper 55 and a receiving section 56 disposed below the hopper 55. Between the hopper 55 and the receiving section 56, the reinforcing bar 11, whose PVB resin layer has been melted by heat treatment, is fed in the axial direction while rotating. The hopper 55 is disposed so that the bottom 55A is positioned vertically above the reinforcing bar 11. A plurality of through holes 57 are formed in the bottom 55A. These through holes 57 are arranged in series at predetermined intervals along the feeding direction of the reinforcing bar 11.
[0027] That is, as shown in Fig. 5, silica sand fed into the hopper 55 passes through each through-hole 57 and falls toward the reinforcing bar 11 below, thereby allowing the silica sand to adhere to the molten PVB resin layer 20. At this time, the reinforcing bar 11 is fed axially while rotating, so that the silica sand can be adhered to almost the entire outer periphery of the PVB resin layer 20. The part of the silica sand that does not adhere to the PVB resin layer 20 is received by the receiving portion 56 below. The surplus silica sand accumulated in the receiving portion 56 may be fed back into the hopper 55.
[0028] Returning to Fig. 4, the cooling device 59 cools the molten PVB resin layer by air or water, thereby solidifying the PVB resin layer. When the PVB resin layer solidifies, the silica sand is held in the PVB resin layer, completing the corrosion-resistant rebar 10. As shown in Fig. 2, part of the silica sand 30 held in the PVB resin layer 20 protrudes, forming numerous minute protrusions on the surface of the PVB resin layer 20, thereby improving the adhesion and anchorage to concrete.
[0029] Here, the amount of silica sand 30 attached to the PVB resin layer 20 is important for the corrosion-resistant rebar 10 to obtain the desired adhesion strength to concrete. To properly manage the amount of silica sand 30 attached to the PVB resin layer 20, it is desirable to set the amount of silica sand 30 falling to an optimal value in the aforementioned fourth step (silica sand attachment device 54). Through diligent efforts, the inventors have found that there is a predetermined correlation between the amount of silica sand 30 falling set in the fourth step and the adhesion strength of the corrosion-resistant rebar 10 to concrete. A method for setting the optimal amount of falling will be described in detail below.
[0030] [How to set up] FIG. 6 is a flow diagram illustrating the flow of the setting method according to this embodiment.
[0031] As shown in FIG. 6, the setting method of this embodiment is carried out by carrying out the following steps: (1) step S10 (first step of the present disclosure) of setting the silica sand falling amount conditions by setting the hole diameter and number of the through holes 57 to be drilled in the bottom 55A of the hopper 55 in a plurality of appropriate patterns; (2) step S20 of measuring the actual silica sand falling amount for each set falling amount condition; (3) step S30 of measuring the silica sand adhesion amount of the corrosion-resistant rebar prepared for each set falling amount condition; (4) step S40 (second step of the present disclosure) of measuring the adhesion strength (adhesion stress) of the corrosion-resistant rebar prepared for each set falling amount condition to concrete; and (5) step S50 (third step of the present disclosure) of determining the optimal silica sand falling amount from the relationship between the silica sand falling amount measured in step S20 and the adhesion strength measured in step S40.
[0032] The details of each of these steps S10 to S50 will be specifically described below based on examples. Among the steps S10 to S50, S20, S30, and S40 are in no particular order. Furthermore, the present disclosure is not limited to the following examples. EXAMPLES
[0033] [Setting the drop amount conditions and measuring the drop amount: steps S10 and S20] In step S10, a plurality of drop amount conditions are set by setting appropriate patterns of diameters and numbers of through holes 57 drilled in bottom 55A of hopper 55. The diameters and numbers of through holes 57 set in this test are shown in Table 1. As shown in Table 1, a total of five types of drop amount conditions were set in this test: very small amount, small amount, medium amount, large amount, and very large amount.
[0034] [Table 1] The very small amount is provided with one through hole 57 having a hole diameter of φ: 1.5 mm on the bottom 55A of the hopper 55. The small amount is provided with two through holes 57 having a hole diameter of φ: 2.0 mm arranged at a predetermined interval in the feed direction of the reinforcing bar 11 on the bottom 55A of the hopper 55. The medium amount is provided with three through holes 57 having a hole diameter of φ: 2.0 mm arranged at a predetermined interval in the feed direction of the reinforcing bar 11 on the bottom 55A of the hopper 55. The large amount is provided with five through holes 57 having a hole diameter of φ: 3.5 mm arranged at a predetermined interval in the feed direction of the reinforcing bar 11 on the bottom 55A of the hopper 55. The extremely large quantity has a total of 13 through holes 57 with a hole diameter φ of 1.5 to 3.5 mm arranged on the bottom 55A of the hopper 55 with the minimum spacing between adjacent holes 57 in the discharge direction of the reinforcing bars 11 so that they do not interfere with each other.
[0035] For each of these five types, silica sand was charged into the hopper 55, and the actual amount of silica sand falling m, specifically, the mass of silica sand falling per unit time (1 minute) from the through-hole 57 of the hopper 55, was measured. No. 8 silica sand was used as the silica sand charged into the hopper 55. This No. 8 silica sand has a particle size distribution in which particles with a particle size of less than 0.15 mm and a particle size of 0.05 mm or more account for 70% or more. The measurement results of the amount of silica sand falling m are shown in Table 2 below.
[0036] [Table 2] From the amount of silica sand falling per unit time m shown in Table 2, the amount of silica sand falling per 1 m of reinforcing bar A1 and the amount of silica sand falling per 1 m of reinforcing bar A2 are 2 Specifically, the amount of silica sand falling A1 was calculated based on the following formula (1), and the amount of silica sand falling A2 was calculated based on the following formula (2).
[0037] A1=m / a ·····································(1) A2=m / (a×l) (2) However, A1: Reinforcement bar: Amount of silica sand falling per 1m (g / m) A2: Steel bar: 1m 2Amount of silica sand falling per unit (g / m 2 ) m: Amount of material falling from the hopper (g / min) a: Axial feeding speed of the reinforcing bar (m / min) l: Nominal circumference of the rebar (cm) In the manufacturing line, the feed speed a varies depending on the diameter of the rebar bar that is the base material, and is set to a faster speed as the rebar diameter becomes smaller. This is because the thickness of the PVB resin film coated by electrostatic coating in the second process is approximately constant (for example, about 220±40 μm) regardless of the rebar diameter, and if a base material with a small rebar diameter is fed at a slow speed, the PVB resin layer will be burned in the third process where the PVB resin layer is melted. The relationship between each rebar diameter (name) and the feed speed a is shown in Table 3.
[0038] [Table 3] In this test, D19 (nominal circumference: 6.0 cm) reinforcing bars were used as the base material, as specified in JIS G 3112:2010 (reinforced concrete steel bars). Therefore, the feed speed a substituted into the above formulas (1) and (2) is 2.2, and the nominal circumference l is 6.0. The feed speed a can be set to an appropriate value depending on the film thickness of the PVB resin layer to be coated, the heat capacity of the high-frequency heating device 52, etc.
[0039] The silica sand falling amounts A1 and A2 calculated by the above formulas (1) and (2) are summarized in Table 4. In Table 4, the evaluation results in the right column are the evaluation results obtained by visually observing the appearance of the actually manufactured corrosion-resistant rebar 10. The evaluation was performed as follows: a case in which silica sand was attached almost uniformly to the entire outer periphery of the PVB resin layer 20 was rated as good, and a case in which silica sand was attached in a spiral or sparse shape to the outer periphery of the PVB resin layer 20 was rated as poor.
[0040] [Table 4] Here, we will consider the reasons why the medium, large and very large amounts were rated as good, while the very small and small amounts were rated as unacceptable.
[0041] In the silica sand adhering device 54 shown in FIG. 5, the silica sand 30 falling from the hopper 55 toward the PVB resin layer 20 adheres to the portion of the outer peripheral surface of the PVB resin layer 20 located vertically below the through-holes 57. For this reason, when the number of through-holes 57 is small, such as in the case of a very small amount or a small amount, the falling amount of the silica sand 30 is insufficient relative to the delivery speed a, and the silica sand adheres in a spiral shape to the outer peripheral surface of the PVB resin layer 20. If the delivery speed a is set slow to prevent such spiral adhesion, as described above, the PVB resin layer will be burned in the third step. On the other hand, for the medium amount, large amount, and very large amount, the falling amount of the silica sand 30 is sufficiently secured relative to the delivery speed a, and it is considered that the silica sand was able to be adhered approximately uniformly to the entire outer peripheral surface of the PVB resin layer 20. In other words, it was confirmed that from the viewpoint of the product appearance, it is desirable to set the optimal falling amount to be equal to or greater than the medium amount.
[0042] [Measurement of silica sand adhesion amount: Step S30] In step S30, the amount of silica sand 30 adhering to the PVB resin layer 20 is measured for each of the corrosion-resistant rebars 10 fabricated under the five types of drop amount conditions described above. In this test, the amount of silica sand 30 adhering was measured according to the procedure shown in FIG.
[0043] Specifically, as shown in FIG. 7 , the amount of silica sand adhesion is determined by (1) step S31 of preparing a measurement sample, (2) step S32 of measuring the length of the measurement sample, (3) step S33 of dissolving the resin layer by immersing the measurement sample in an organic solvent and leaving it to stand, (4) step S34 of drying the filter paper and measuring the dry mass of the filter paper alone, (5) step S35 of filtering out the silica sand by injecting the dissolving liquid into the filter paper and filtering it, (6) step S36 of drying the filter paper and silica sand and measuring the total dry mass of the filter paper and silica sand, and (7) measuring the mass of the silica sand obtained by subtracting the dry mass of the filter paper alone from the total dry mass per 1 m of the outer circumferential surface of the corrosion-resistant rebar 10. 2 The measurement was performed by sequentially performing step S31 and step S37, which converts the measured amount of adhesion into an amount of adhesion per unit. Details of each of steps S31 to S37 will be specifically described below.
[0044] (Preparation of measurement sample: Step S31) In step S31, the corrosion-resistant rebar with silica sand attached and held to the PVB resin layer is cut to a predetermined length to prepare measurement samples (preferably multiple pieces). For the base material rebar, any rebar designated in Table 4 of JIS G 3122:2010 can be used. The cutting method is not particularly limited, but from the viewpoint of preventing thermal melting of the PVB resin layer, it is desirable to select a cutting method that does not generate heat on the cut surface (or that suppresses the generation of heat). An example of a cutting method that does not generate heat is cutting with a band saw or the like.
[0045] The axial length of the measurement sample is not particularly limited, but the maximum length is preferably set to a length that fits within the container used in step S33 described below, taking into consideration the capacity (height) of the container. Furthermore, in the case where the reinforcing bar is a deformed reinforcing bar as shown in Fig. 1, if the measurement sample is made too short, it will be easily affected by the ribs 13, 14 (particularly the horizontal rib 14). From this perspective, it is preferable that the minimum length of the measurement sample is set to an appropriate length that includes multiple horizontal ribs 14.
[0046] (Measurement of the length of the measurement sample: Step S32) In step S32, as shown in Fig. 8, the axial length L of the measurement sample S created in the above-mentioned step S31 is measured. The axial length L is desirably measured to an accuracy of 0.01 mm using a caliper (e.g., a micrometer). Here, the cut surfaces formed at both ends of the measurement sample S may not be perpendicular to the axial direction, and there is a possibility that the accuracy cannot be guaranteed by measuring only one point. From this viewpoint, it is preferable to measure lengths L1, L2 at at least two points perpendicular to the radial direction, and to determine the axial length L of the measurement sample S as the average value (L = (L1 + L2) / 2) of these lengths.
[0047] It should be noted that step S32 can also be performed using the reinforcing bars 11 from which the PVB resin has been dissolved and removed after completion of step S35 described below.
[0048] (Dissolving the resin layer: Step S33) 9, the measurement sample S is placed in a container 500, and an organic solvent is poured into the container 500 until the measurement sample S is completely immersed. After the organic solvent is poured, the opening of the container 500 is closed and sealed with a cap 510 to prevent the organic solvent from evaporating or dissipating. After the container 500 is sealed, the measurement sample S is left to stand in a stable temperature environment, such as a room, until the PVB resin layer of the measurement sample S is completely dissolved.
[0049] Here, the type of organic solvent is not particularly limited as long as it is a solvent capable of dissolving the PVB resin, but from the viewpoint of resin solubility and ease of handling, it is preferable to use alcohol, particularly isopropyl alcohol (isopropanol). The concentration of the alcohol may be adjusted as appropriate, but the purity is preferably 98% by mass or more. The temperature at which it is left standing may be room temperature (for example, about 23°C). The time for which it is left standing is not particularly limited, but when isopropyl alcohol is used, it is preferably at least 4 hours or more, and more preferably 12 hours or more. Examples of solvents that can dissolve PVB resin include alcohols such as methanol, ethanol, propanol, isopropanol, butanol, isobutanol, diacetone alcohol, and benzyl alcohol; glycols such as 1-methoxy-2-propanol, 3-methoxy-1-butanol, and carbitol; ethers such as dioxane and THF; cellosolves such as methyl cellosolve, ethyl cellosolve, and butyl cellosolve; esters such as methoxypropyl acetate, ethyl butyrate, n-butyl glycolate, and DBE; and ketones such as methyl ethyl ketone (MEK) and cyclohexanone.
[0050] In the illustrated example, the measurement sample S is placed vertically in the container 500, but it may be placed horizontally depending on the shape of the container 500. When placed horizontally, the measurement sample S may be supported at both ends by a support means and suspended in the organic solvent.
[0051] (Drying the filter paper and measuring the dry mass: Step S34) In step S34, the filter paper is placed in a drying facility such as a drying oven or an electric oven, and the mass of the filter paper after drying (hereinafter referred to as the single dry mass mA) is measured. The filter paper is preferably dried until the mass loss is less than about 0.01 g. In this case, it is preferable that the drying temperature is 90° C. or higher, and the drying time is 30 minutes or longer. Note that step S34 does not need to be started after the end of step S33, and may be performed in parallel with step S33 before the end of step S33.
[0052] (Filtration of the solution and filtration of the silica sand: Step S35) 10, in step S35, the filter paper 600 is set in a filtering device 610 (e.g., a funnel), and the solution in which the PVB resin is dissolved is filtered through the filter paper 600 to separate the silica sand from the solution. At this time, simply tilting the container 500 may result in silica sand that has settled on the bottom side of the container 500 or silica sand adhering to the surface of the measurement sample S remaining therein, and the remaining silica sand may not be collected by the filter paper 600. In order to reliably collect such remaining silica sand, it is preferable to wash the container 500 and the measurement sample S with a cleaning liquid and pour the cleaning liquid into the filter paper 600.
[0053] If distilled water is used as the cleaning solution, the PVB resin in the solution will solidify again, making it impossible to filter the silica sand. For this reason, it is preferable to use the same organic solvent (isopropyl alcohol in this embodiment) as the cleaning solution used in step S33 described above.
[0054] (Drying process of filter paper and silica sand, measurement of dry mass: Step S36) In step S36, the filter paper and the silica sand collected on the filter paper are placed in a drying facility such as a drying oven or an electric furnace, and the total mass of the filter paper and silica sand after drying (hereinafter referred to as the total dry mass mB) is measured. It is preferable to dry the filter paper and silica sand until the mass loss is less than about 0.01 g. At this time, it is preferable to set the heating temperature to 90°C or higher, and the drying time to 30 minutes or more.
[0055] (Calculation and conversion of mass of silica sand: Step S37) In step S37, the mass m of the silica sand attached to the measurement sample S is calculated according to the following formula (3), which subtracts the individual dry mass mA obtained in step S34 from the total dry mass mB obtained in step S36.
[0056] m=mB-mA (3) Where, m: mass of silica sand (g) mA: Single unit dry mass (g) mB: Total dry mass (g) Next, the mass m of the obtained silica sand is calculated by the following formula (4): 2 Convert this into the adhesion amount M per unit.
[0057] M=α×Ms (4) However, M: 1m 2 Amount of silica sand attached per unit (g) α : 1m 2 Conversion factor per α=1 / D D: Total outer surface area of the measurement sample S (m 2 ) D = d × L d: Nominal circumference of the rebar sample (m) L: Axial length of the measurement sample (m) Ms: Total mass of filtered silica sand (g) Ms = Σm By measuring the amount of silica sand adhesion based on the above measurement method, it is possible to effectively eliminate the influence of the heavy reinforcing bar 11 and reliably improve the measurement accuracy compared to a method of comparing the actual measurement sample S with a separately prepared sample coated only with PVB resin. In addition, since there is no need to separately prepare a sample coated only with PVB resin, it is also possible to effectively reduce the time and effort.
[0058] [Measurement of adhesion strength (adhesion stress): Step S40] Returning to FIG. 6, in step S40, multiple anticorrosive rebars are prepared based on the above-mentioned drop amount conditions, and the bond strength of these anticorrosive rebars to concrete is measured. In this test, a specimen was prepared by embedding the base end of the anticorrosive rebar in a concrete block, and a pull-out test of the anticorrosive rebar was performed on the specimen to measure the bond stress to concrete. The pull-out test was performed with reference to the Japan Society of Civil Engineers standard JSCE-E516 "Adhesion strength test method for epoxy resin coated rebars."
[0059] In addition to the test samples prepared under the five types of drop amount conditions mentioned above, the bond stress with concrete was also measured for comparison purposes using unpainted rebars that were not coated with resin, epoxy resin-coated rebars that were coated only with epoxy resin, and PVB resin-coated rebars that were coated only with PVB resin.
[0060] Here, when the base material is a deformed reinforcing bar as shown in Figure 1, the maximum bond stress depends not only on the bond strength between the reinforcing bar and the concrete, but also on the strength of the concrete itself due to the influence of the ribs 13, 14 (particularly the horizontal rib 14). In other words, the point at which the concrete breaks down will be measured as the maximum bond stress, and there is a possibility that the bond performance of the silica sand will not be evaluated correctly. From this perspective, in this test, a comparison was made by measuring the bond stress at a slippage of 0.002D (D: nominal diameter of the reinforcing bar) and the maximum bond stress.
[0061] The test results are shown in Figures 11, 12 and 13. Figure 11 is a graph showing the bond stress and maximum bond stress of each sample.
[0062] As shown in Figure 11, the bond stress of epoxy resin coated rebars and PVB resin coated rebars, which are coated only with resin, was lower than that of unpainted rebars. On the other hand, it was confirmed that even if the amount was very small, if there was a small amount of silica sand attached to the PVB resin layer, the bond stress would be higher than that of unpainted rebars.
[0063] FIG. 12 is a graph showing the relationship between the adhesion stress of each sample and the amount of silica sand falling (measured in step S20 described above) according to each falling amount condition.
[0064] As shown in Figure 12, the bond stress with the concrete increases with an increase in the amount of silica sand dropped, but for extremely large amounts, the bond stress is lower than for large amounts. In other words, even if the drop amount condition is set to an extremely large amount, the bond stress with the concrete does not necessarily reach its highest value. This is presumably because, even when the drop amount condition is set to an extremely large amount, the amount of silica sand that can actually adhere to the surface of the PVB resin layer is less than when the drop amount condition is set to a large amount.
[0065] FIG. 13 is a graph showing the relationship between the adhesion stress of each sample and the amount of silica sand adhesion (measured in step S30 described above).
[0066] As shown in Figure 13, when the falling amount condition was set to an extremely large amount, even though the amount of silica sand falling was large, the amount of silica sand adhering to the PVB resin layer was less than when the falling amount condition was set to a large amount.
[0067] From the above, it was confirmed that there is a relationship between the amount of silica sand falling and the adhesion stress (adhesion strength): the adhesion stress increases as the amount of silica sand falling increases, but when the amount of silica sand falling exceeds a certain threshold amount, the actual amount of silica sand adhesion decreases, and the adhesion stress also decreases. In other words, it was confirmed that if the amount of silica sand falling that corresponds to the peak value at which the adhesion stress with concrete is the highest is obtained by experiment, etc., the obtained amount of silica sand falling can be set as the optimal amount of silica sand falling in the manufacturing process.
[0068] If the optimum drop amount thus obtained is used as the drop amount of silica sand in the aforementioned manufacturing process (step 4), it becomes possible to stably manufacture anticorrosive rebars that can exhibit the desired adhesive performance to concrete. In addition, in the manufacturing process, it becomes possible to effectively reduce the amount of surplus silica sand that falls without adhering to the PVB resin layer, which also makes it possible to improve manufacturing efficiency.
[0069] Here, the optimal drop amount does not necessarily have to be a single point corresponding to the peak value of the bond stress, but may be set within a predetermined range. Specifically, the lower limit of the optimal drop amount may be the amount of silica sand drop that provides a higher bond stress than unpainted rebar and does not result in spiral-shaped silica sand adhesion on the surface. In this embodiment, the intermediate amount corresponds to the lower limit of the optimal drop amount. Moreover, the upper limit of the optimal drop amount may be the amount of silica sand drop just before the bond stress with the concrete (or the amount of silica sand adhesion) begins to drop below a predetermined threshold value. In this embodiment, the amount just before the extremely large amount corresponds to the upper limit of the optimal drop amount.
[0070] In addition, the optimum drop amount does not need to be found by performing an experiment every time, but rather, by performing a number of experiments in advance under different conditions (feed speed, melting temperature, etc.), the optimum drop amount under these different conditions can be constructed as a database, and the optimum drop amount under conditions for which no experiment has been performed can be calculated based on a model formula (linear approximation formula, etc.) obtained from the database. If such a database is constructed, it can be used when changing the production line or installing a new production line.
[0071] In addition, the resin layer covering the reinforcing bar 11 may be a resin layer other than PVB, and the particles may be particles other than silica sand. [Explanation of symbols]
[0072] 10. Corrosion-resistant steel bars 11 Steel bars 20 PVB resin layer (resin layer) 30 Silica sand (particles) 50 production lines 51 Blast treatment equipment 52 High frequency heating device 53 Electrostatic painting equipment 54 Silica sand deposition device 55 Hopper 56 Receiving part 57 Through hole 59 Cooling device
Claims
1. A method for setting the amount of particles that are dropped onto and adhere to the resin layer in a manufacturing process for a corrosion-resistant reinforcing bar having a reinforcing bar, a resin layer that covers at least a part of the outer periphery of the reinforcing bar, and particles that are adhered to and held by the resin layer, comprising: A first step of preparing the corrosion-resistant rebar by setting the particle drop amount to two or more different drop amounts; A second step of measuring the adhesion strength of each of the plurality of anticorrosive rebars produced by the two or more different drop amounts to concrete; The relationship between the drop amount set in the first step and the adhesion strength measured in the second step and a third step of determining an optimal drop amount of the particles in the manufacturing process based on the relationship, In the third step, the optimum falling amount is the falling amount immediately before the adhesion strength starts to decrease with respect to an increase in the falling amount of the particles. A setting method comprising:
2. In the second step, the adhesive strength of the unpainted reinforcing bar not coated with the resin layer to the concrete is further measured, In the third step, the smallest drop amount among the drop amounts that show a higher adhesion strength than the adhesion strength of the unpainted reinforcing bar to the concrete is set as the lower limit of the optimal drop amount. The setting method according to claim 1 .
3. In the manufacturing process, the reinforcing bar is fed in the axial direction while rotating around the axis, so that the particles are attached to the outer periphery of the resin layer, In the third step, the smallest amount of falling that does not cause the particles to adhere in a spiral shape to the outer periphery of the resin layer is set as the lower limit of the optimal amount of falling. The setting method according to claim 1 .
4. In the manufacturing process, the reinforcing bar is fed in the axial direction while rotating around the axis, so that the particles are attached to the outer periphery of the resin layer, In the third step, the smallest amount of falling that exhibits a higher adhesion strength than the adhesion strength of the unpainted reinforcing bar to the concrete and does not cause the particles to adhere in a spiral shape to the outer periphery of the resin layer is set as the lower limit of the optimal amount of falling. The setting method according to claim 2 .
5. The resin layer is a resin layer containing polyvinyl butyral as a main component, and the particles are silica sand. The setting method according to any one of claims 1 to 4.
6. A method for manufacturing a corrosion-resistant rebar using the optimal drop amount set by the setting method according to any one of claims 1 to 5, A step of coating the outer periphery of the reinforcing bar with the resin layer; heating and melting the resin layer; and dropping the particles at the optimum drop amount onto the molten resin layer to cause the particles to adhere to the resin layer. A manufacturing method comprising the steps of:
Citation Information
Patent Citations
Production of concrete reinforcing material made of frp
JP1994297591A
Highly durable and corrosion resistant steel, and method and apparatus for producing the same
JP2011147845A
Manufacturing apparatus for reinforcing-bar with corrosion-proof film
JP2014087725A
Rust-proof deformed bar
JP2017043898A