Metal film deposition method
The method addresses plating solution seepage in porous film apparatuses by sandwiching and pressurizing the porous membrane with a holding member, ensuring uniform metal film formation and reducing excess solution, enhancing process efficiency.
Patent Information
- Application Number
- JP2021077971
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-30
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-04-30
AI Technical Summary
The existing film forming apparatus using a porous film is prone to plating solution seepage due to pressurization, leading to inefficiencies and difficulty in managing the metal film formation process.
A method involving a porous membrane impregnated with plating solution, where the film-forming surface is pressed against an object, using a holding member to sandwich the porous film and apply pressure to impregnate the solution, while utilizing a biasing member to ensure contact with the mounting table, preventing seepage and optimizing film formation.
The method effectively prevents plating solution seepage, ensuring uniform metal film formation and reducing excess solution on non-coated surfaces, thereby improving process efficiency and minimizing waste.
Smart Images

Figure 0007571656000001 
Figure 0007571656000002 
Figure 0007571656000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming a metal film on a surface of a substrate. [Background technology]
[0002] As an example of this type of technology, Patent Document 1 discloses a film formation device having an anode, a porous membrane provided between the anode and a body to be formed so as to be in contact with the body to be formed, a liquid storage chamber that defines a solution storage space between the anode and the porous membrane, and a power supply unit that applies a voltage between the anode and the body to be formed, wherein the porous membrane is made of polyolefin chains that do not have ion-exchange functional groups.
[0003] Using this film-forming device, a plating solution is contained in the liquid storage chamber, and with the porous membrane and the cathode in contact with each other, a voltage is applied between the anode and the body to be coated, thereby allowing a metal coating to be formed on the film-forming area of the body to be coated. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-97764 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when a porous membrane is used in the film-forming apparatus shown in Patent Document 1, the plating solution in the liquid storage chamber is pressurized when a metal film is formed, so there is a risk that the plating solution will seep out to the parts of the porous membrane that are not in contact with the object to be formed.
[0006] The present invention has been made in consideration of these points, and its object is to provide a method for forming a metal film that can prevent plating solution from seeping out from portions of the porous film that are not in contact with the substrate to be coated. [Means for solving the problem]
[0007] In view of the above problems, the method for forming a metal film according to the present invention is a method for forming a metal film, which comprises pressing a porous film impregnated with a plating solution containing metal ions against a body to be coated, to form a metal film made of a metal derived from the metal ions on a surface of the body to be coated that comes into contact with the plating solution, and is characterized by including at least the steps of: sandwiching the porous film between a mounting table having a accommodating recess for accommodating the body to be coated so that the surface to be coated of the body to be coated is exposed, and a clamping member having a liquid retaining hole for retaining the plating solution at a position opposite to the surface to be coated of the body to be coated placed on the mounting table, so that the surface to be coated comes into contact with the porous film; pressurizing the plating solution held in the liquid retaining hole to impregnate the porous film with the plating solution; and stopping pressurization of the plating solution and forming the metal film on the surface to be coated with the plating solution impregnated in the porous film. Effect of the Invention
[0008] According to the present invention, in the step of sandwiching the porous film, the porous film is sandwiched between the mounting table containing the film-forming object and the clamping member so that the film-forming surface is in contact with the porous film. As a result, the part of the porous film that is not in contact with the film-forming surface is in contact with the surface of the mounting table and functions like a sealant, so that even if the plating solution is pressurized, it is possible to prevent the plating solution from seeping out of the porous film. [Brief description of the drawings]
[0009] [Figure 1A] FIG. 2 is a schematic cross-sectional view illustrating a clamping step in the method for forming a metal coating according to the first embodiment of the present invention. [Figure 1B] 1B is a schematic cross-sectional view illustrating a pressurizing step and a film-forming step in the film-forming method of a metal film in the film-forming apparatus shown in FIG. 1A. [Figure 1C] 1B is a schematic cross-sectional view for explaining a film forming process in the film forming apparatus shown in FIG. 1A for forming a metal film. FIG. [Figure 2A] 1B is a cross-sectional view of a main part of a film forming apparatus for a metal film according to a modified example of FIG. 1A. [Figure 2B] 2B is a schematic cross-sectional view for explaining a pressurizing step in the film forming apparatus shown in FIG. 2A for forming a metal film. FIG. [Figure 3A] 1B is a schematic cross-sectional view for explaining a film formation apparatus for carrying out a film formation method which is comparative to that of FIG. 1A. [Figure 3B] 3B is a schematic cross-sectional view for explaining a film forming method using the film forming apparatus shown in FIG. 3A. [Figure 4A] 2B is a schematic cross-sectional view for explaining a film formation apparatus for carrying out a film formation method which is comparative to that of FIG. 2A. [Figure 4B] 4B is a schematic cross-sectional view for explaining a film forming method using the film forming apparatus shown in FIG. 4A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The method for forming a metal film according to the present embodiment will be described below. First, a film forming apparatus used in the method for forming a metal film according to the first embodiment will be described with reference to Figs. 1A to 4B.
[0011] 1. About the deposition equipment As shown in FIG. 1, the film forming apparatus 1 of this embodiment is a metal film forming apparatus that presses a porous membrane 50 impregnated with a plating solution L containing metal ions against a film-forming body W to form a metal film made of a metal derived from the metal ions on a film-forming surface F of the film-forming body W that is in contact with the plating solution L.
[0012] 1A, the film forming apparatus 1 includes a mounting table 16 on which a film-formed object W is placed, and a storage recess 16a for storing the film-formed object W is formed in the mounting table 16 so that a film-formed surface F of the film-formed object W is exposed. A biasing member 28 such as a spring is disposed in the storage recess 16a, and the biasing member 28 biases the film-formed object W toward the porous membrane 50.
[0013] In this embodiment, the biasing member 28 is set so that, during film formation, the film-formed object W is compressed and deformed until it becomes substantially flush with the surface of the mounting table 16. Therefore, the height of the film-formed object W and the spring constant of the biasing member 28 are set so that the depth of the accommodating recess 16a coincides with the sum of the height of the film-formed object W and the compressively deformed biasing member 28.
[0014] The film forming apparatus 1 includes an apparatus main body 10, and the apparatus main body 10 has a porous membrane 50 attached at a position facing a mounting table 16, and a liquid storage chamber 11 is formed to store the plating solution L so that the plating solution L is sealed by the porous membrane 50. The mounting table 16 is capable of being raised and lowered freely relative to the apparatus main body 10. The mounting table 16 can be raised and lowered by a commonly known device such as a linear motion device such as a linear guide.
[0015] Here, a plating solution L is contained in the liquid containing chamber 11 of the device main body 10, and when a metal film is formed on the film-forming body W by electroless plating, for example, an electroless plating solution is contained as the plating solution L. Furthermore, when a metal film is formed by electrolytic plating, an anode (not shown) is disposed in the liquid containing chamber 11 at a position facing the film-forming body W. The film-forming body W is used as the cathode, and a power source (not shown) is connected to the anode and the film-forming body W (cathode), and a voltage is applied between them during film formation.
[0016] Furthermore, in this embodiment, a housing 18 may be disposed so as to surround the mounting table 16, and a suction pump 30 may be connected to the housing 18 for creating a negative pressure inside the housing 18 by sucking air therein during film formation. This allows the porous film 50 to be formed on the film-formation target body W. The liquid containing chamber 11 is provided with a pressure pump 19 for pressurizing the plating solution L contained in the liquid containing chamber 11.
[0017] The porous membrane 50 is a porous membrane in which fine pores through which the plating solution permeates are formed in the thickness direction, and has a pore diameter of about 20 to 100 nm, and has a porous structure (i.e., an ion cluster structure). The pores of the porous structure are very small, and the average pore diameter is, for example, 0.1 μm or more and 100 μm or less. The solid electrolyte membrane can be impregnated with the electroless plating solution by applying pressure. When electrolytic plating is performed, the porous membrane 50 is a solid electrolyte membrane through which metal ions permeate, and examples of the material include fluorine-based resins such as Nafion (registered trademark) manufactured by DuPont, hydrocarbon-based resins, polyamic acid resins, and resins having an ion exchange function such as Selemion (CMV, CMD, CMF series) manufactured by Asahi Glass Co., Ltd., but are not particularly limited thereto. The thickness of the porous membrane 50 is preferably 10 μm or more and 200 μm or less, and more preferably 20 μm or more and 160 μm or less.
[0018] The metal ions contained in the plating solution L are, for example, metal ions such as copper ions, nickel ions, silver ions, or gold ions. In the case of an electroless plating solution, the electroless plating solution is preferably a so-called displacement type electroless plating solution. The electroless plating solution contains, for example, a metal compound and a complexing agent, and may contain additives as necessary. Examples of additives include a pH buffer or a stabilizer. In the case of an electrolytic plating solution, the plating solution is preferably an electrolytic solution in which the metal to be the metal film is dissolved in the form of ions by sulfuric acid, nitric acid, or the like.
[0019] 1B, the film-forming surface F of the film-forming body W is a conductive surface to serve as a cathode, and is formed with grooves R. In the case of electroless plating, a catalyst such as palladium may be applied to the film-forming surface F.
[0020] In this embodiment, the apparatus further includes a clamping member 12. The clamping member 12 has a liquid holding hole 13 formed in a position facing a film-forming surface F of a film-forming body W placed on a mounting table 16, in which the plating liquid L of the liquid storage chamber 11 is held.
[0021] In this embodiment, the clamping member 12 is disposed closer to the liquid storage chamber 11 than the porous membrane 50 so as to be in contact with the porous membrane 50. The liquid retention hole 13 allows the plating solution L in the liquid storage chamber 11 to pass through toward the porous membrane 50, and has an opening on the porous membrane 50 side having a size corresponding to the membrane formation surface F, and the plating solution L comes into contact with the porous membrane 50 through this opening.
[0022] In the film forming method using the comparative film forming apparatus 9 shown in FIG. 3A, the film-formed object W protrudes from the accommodation recess 16a of the mounting table 16. The accommodation recess 16a is not provided with a biasing member such as a spring. When a metal film is to be formed on the film-formed surface F of the film-formed object W in the state shown in FIG. 3A, as shown in FIG. 3B, a gap is formed between the mounting table 16 and the porous film 50, and the exuded plating solution enters these gaps. As a result, a metal film can be formed on the surface of the groove R of the film-formed object W by the exudation of the plating solution L. However, in this case, even if a metal film can be formed on the surface of the groove R, a large amount of the plating solution L exudes onto the mounting table 16, and the plating solution L must be wiped off.
[0023] Therefore, in the film forming method of this embodiment, the following sandwiching step, impregnation step, and film forming step are performed. First, in the sandwiching step, as shown in FIG. 1A, the porous membrane 50 is sandwiched between the mounting table 16 having the accommodation recess 16a for accommodating the film-formed body W so that the film-formed surface F of the film-formed body W is exposed, and the sandwiching member 12 having the liquid holding hole 13 for holding the plating solution L at a position facing the film-formed surface F of the film-formed body W placed on the mounting table 16, so that the film-formed surface F contacts the porous membrane 50. At this time, the biasing member 28 is compressed and deformed, so that the film-formed surface F contacts the plating solution L through the porous membrane 50, and the surface of the mounting table 16 contacts the sandwiching member 12 through the porous membrane 50.
[0024] 1B, in the impregnation step, the pressure pump 19 is driven to pressurize the plating solution L in the liquid storage chamber 11, thereby pressurizing the plating solution L held in the liquid holding hole 13. This causes the plating solution L in the liquid holding hole 13 to impregnate the porous membrane 50.
[0025] Here, the portion of the porous membrane 50 that is not in contact with the deposition surface F contacts the surface of the mounting table 16 and functions like a sealant, so that even if the plating solution is pressurized, it is possible to prevent the plating solution from seeping out of the porous membrane, as shown in Fig. 1B. As a result, in the impregnation step, the biasing member 28 is further compressed and deformed by the liquid pressure of the plating solution L that has passed through the porous membrane 50, and the deposition target W is pressed down. As a result, the plating solution is also filled into the grooves R formed on the deposition target surface F of the deposition target W.
[0026] 1C, in the film formation step, the pressurization of the plating solution L by the pressure pump 19 is stopped, and a metal film is formed on the film formation surface F by the plating solution L impregnated in the porous membrane 50. In this way, according to the present embodiment, leakage of the plating solution L onto the mounting table 16 can be suppressed, and therefore the work of wiping off the plating solution L from the mounting table 16 can be reduced.
[0027] Furthermore, as shown in Fig. 4A, in a comparative film forming method using a film forming apparatus 9, if the heights of the objects W (WA, WB) to be filmed are different during film formation, the taller object WA protrudes from the surface of the mounting table 16. Therefore, when attempting to form a metal film on the objects WA, WB, pressing the porous film 50 against the objects WA, WB causes excessive stress to act on the portion of the porous film 50 that contacts the film formation surface F of the taller object WA compared to the shorter object WB. This may cause damage to the portion of the porous film 50 to which the excessive force acts, as shown in Fig. 4B.
[0028] However, in this embodiment, even if the objects WA and WB have different heights and the protrusion amounts L1, L2 from the mounting table 16 are different as shown in Fig. 2A, the biasing member 28 may be set to compress and deform the object W to be coated until it becomes substantially flush with the surface of the mounting table 16 (until they become the same surface) during film formation, as shown in Fig. 2B. This makes it possible to form a metal film on the surfaces F of the objects WA and WB to be coated while suppressing damage to the porous film 50.
[0029] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments, and various design modifications can be made without departing from the spirit of the present invention as described in the claims. [Explanation of symbols]
[0030] 1: film forming apparatus, 10: apparatus body, 11: liquid storage chamber, 12: clamping member, 13: liquid holding hole, 16: mounting table, F: film forming surface, L: plating solution, W: film forming body
Claims
[Claim 1] A method for forming a metal film, comprising pressing a porous film impregnated with a plating solution containing metal ions against a film-forming body, thereby forming a metal film made of a metal derived from the metal ions on a film-forming surface of the film-forming body that is in contact with the plating solution, the method comprising: a step of sandwiching the porous film between a mounting table having a recess for accommodating the film-formed body so that the film-formed surface of the film-formed body is exposed, and a sandwiching member having a liquid holding hole for holding the plating solution formed at a position facing the film-formed surface of the film-formed body placed on the mounting table, so that the film-formed surface is in contact with the porous film; pressurizing the plating solution held in the solution holding hole to impregnate the porous membrane with the plating solution; a step of stopping pressurization of the plating solution and forming the metal coating on the film-forming surface using the plating solution impregnated in the porous membrane; A method for forming a metal film comprising at least the steps of:
Citation Information
Patent Citations
Film forming apparatus for forming metal film
CN111719176A
Film forming device of forming metallic film
JP2019056142A
Film forming device, and method of forming metal film using the same
JP2020097764A
Apparatus for forming metal film
JP2020152987A
Film forming apparatus for metal coating film and film forming method therefor
WO2015072481A1