A papermaking additive that enhances the effectiveness of paper strength agents

A polymer with cationic monomers enhances paper strength by improving distribution and adhesion, addressing the inefficacy of amphoteric polyacrylamide enhancers in high-conductivity systems and reducing environmental impact.

JP7571996B2Active Publication Date: 2024-10-23HYMO CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020195619
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-26
Publication Date
2024-10-23
Estimated Expiration
2040-11-26

AI Technical Summary

Technical Problem

Existing amphoteric polyacrylamide-based paper strength enhancers are inhibited in papermaking systems with high electrical conductivity, leading to insufficient performance and environmental issues from increased usage, and existing methods to enhance their effect have adverse effects on equipment and papermaking chemicals.

Method used

A polymer with a specific composition, including cationic monomers, is used in conjunction with paper strength enhancers to promote their effectiveness and reduce the amount needed, improving distribution and adhesion on pulp fibers.

Benefits of technology

The polymer enhances paper strength by uniformizing the distribution of paper strength enhancers, increasing their effectiveness without increasing their use, and improving adhesiveness between pulp fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571996000001
    Figure 0007571996000001
  • Figure 0007571996000002
    Figure 0007571996000002
  • Figure 0007571996000003
    Figure 0007571996000003
Patent Text Reader

Abstract

To provide an additive for paper making, capable of improving the effect of a paper strengthening agent without adversely influencing the environment, a facility or the like, in a paper making process.SOLUTION: A paper strengthening effect can be improved by adding a polymer obtained by polymerizing a monomer component containing a cationic monomer in an amount of 50 to 100 mass%, together with a paper strengthening agent to a paper-making raw material. The polymer is preferably a polymer obtained by polymerizing a monomer component containing a hydrophobic monomer in an amount of more than 0 mass% and not more than 40 mass% relative to the total monomers. The viscosity (at 25°C) of a polymer solution with the polymer dissolved therein in an amount of 1 mass% is, preferably, 15 to 150 mPa-s when measured by a B-type viscometer at a rotation rate of 60 rpm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a papermaking additive that enhances the effect of a paper strength agent in the papermaking process, and a method for enhancing the effect of a paper strength agent. [Background technology]

[0002] Polyacrylamide-based paper strength agents are used as paper strength enhancers that impart strength to paper. Polyacrylamide-based paper strength enhancers are classified into anionic, cationic, and amphoteric types according to their ionicity. Currently, amphoteric paper strength enhancers are the mainstream in terms of performance. Amphoteric polyacrylamide-based paper strength enhancers are made of amphoteric acrylamide-based water-soluble polymers obtained by copolymerizing acrylamide with various polymerization components such as cationic monomers and anionic monomers (Patent Document 1). Amphoteric acrylamide-based water-soluble polymers form polyion complexes. Polyion complexes are formed by electrostatic interactions between cationic and anionic groups. It is known that amphoteric acrylamide-based water-soluble polymers exert a paper strength enhancing effect by forming polyion complexes. In recent years, with the advancement of recycling waste paper and closed systems, fine fibers and dissolved electrolytes have accumulated in the papermaking system, and the electrical conductivity of the papermaking system has tended to increase. As a result, amphoteric paper strength agents in particular are prevented from forming ion complexes, and are unable to exert their full effect. However, increasing the amount of paper strength agents added leads to deterioration of water quality, which is undesirable from an environmental perspective. Therefore, from an environmental perspective, there is a need to improve the effect of paper strength agents without increasing the amount added. As a method for improving the effect of a paper strength agent used in the papermaking process, for example, a method of contacting the paper strength agent with an oxidizing agent at a specific concentration has been disclosed (Patent Document 2). However, this method has undesirable effects such as adverse effects on equipment due to the use of the oxidizing agent and reduced effects of papermaking chemicals such as retention aids.

[0003] [Patent Document 1] JP 2012-251252 A [Patent Document 2] Patent No. 6664627 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention aims to provide a papermaking additive that can improve the effect of a paper strength agent without adversely affecting the environment, facilities, etc. in the papermaking process. [Means for solving the problem]

[0005] As a result of intensive research to solve the above problems, it was discovered that by using a polymer having a specific composition together with a paper strength agent, the paper strength enhancing effect of the paper strength agent is promoted and the amount of paper strength agent used can be reduced. Effect of the Invention

[0006] According to the present invention, by using a polymer having a specific composition together with a paper strength agent, the paper strength increasing effect of the paper strength agent is promoted, and the amount of paper strength agent used can be reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The present invention will be described in detail below. The polymer of the present invention can be obtained by any method such as aqueous solution polymerization, emulsion polymerization, dispersion polymerization, suspension polymerization, etc. The aqueous solution polymerization will be described below. The polymer of the present invention can be obtained by polymerizing a monomer component having a cationic monomer as an essential component. The polymerization can be carried out by adding a monomer mixture, water, a radical polymerization initiator, and optionally a surfactant to a predetermined reaction vessel, stirring and heating the mixture in an inert gas atmosphere such as nitrogen gas, to obtain the target polymer.

[0008] Among the cationic monomers, examples of the tertiary amino group-containing cationic monomers include dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylamide, diethylaminopropyl (meth)acrylamide, and salts thereof. Examples of the quaternary ammonium base-containing cationic monomer include (meth)acryloyloxyethyl trimethyl ammonium chloride, (meth)acryloyloxyethyl dimethyl benzyl ammonium chloride, (meth)acryloylaminopropyl trimethyl ammonium chloride, (meth)acryloylaminopropyl dimethyl benzyl ammonium chloride, (meth)acryloyloxy 2-hydroxypropyl trimethyl ammonium chloride, etc. Also included are diallyl methyl amine, diallyl benzyl amine, diallyl dimethyl ammonium chloride, diallyl methyl benzyl ammonium chloride, etc. Two or more of these may be used in combination. The content of the cationic monomer is 50 to 100% by mass, preferably 60 to 100% by mass, and more preferably 60 to 99% by mass, based on the total monomers.

[0009] The polymer in the present invention may further contain a nonionic monomer, a hydrophobic monomer, etc. as a polymerization component.

[0010] Examples of nonionic monomers include acrylamide, dimethylacrylamide, diethylacrylamide, isopropylacrylamide, hydroxyethylacrylamide, vinylpyrrolidone, vinylformamide, glycerol (meth)acrylate, hydroxyethyl (meth)acrylate, etc. Two or more of these may be used in combination. The amount of the nonionic monomer is 0 to 50% by mass, preferably 0 to 30% by mass, based on the total amount of the monomers.

[0011] In the present invention, the hydrophobic monomer means a monomer having a solubility of 2% by mass or less in water at 20° C. Examples of hydrophobic monomers include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, octyl (meth)acrylate, stearyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, styrene, ethylstyrene, etc. Two or more of these may be combined. The amount of the hydrophobic monomer is 0 to 50% by mass, preferably 0 to 40% by mass, and more preferably 1 to 40% by mass, based on the total amount of the monomers.

[0012] Furthermore, an anionic monomer and a crosslinking monomer may be contained to the extent that the effect is not impaired. Examples of the anionic monomer include (meth)acrylic acid, itaconic acid, maleic acid, styrenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid, and salts thereof, etc. Two or more of these may be used in combination. Examples of the crosslinkable monomer include methylenebisacrylamide, ethylene glycol di(meth)acrylate, N-methylolacrylamide, triallyl isocyanate, and divinylbenzene. Two or more of these may be combined. The addition rate of the crosslinkable monomer is preferably 1% by mass or less based on the total monomers.

[0013] In the polymerization, a surfactant can be used when a hydrophobic monomer is used. A surfactant is a substance having a hydrophilic group and a hydrophobic group in the molecule. Neutral surfactants include polyoxyalkylene alkyl ethers, polyoxyethylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monooleate and polyoxyethylene sorbitan trioleate, polyoxyethylene alkyl ethers such as polyoxyethylene cetyl ether, polyoxyethylene oleyl ether and polyoxyethylene lauryl ether, sorbitan fatty acid esters such as sorbitan monooleate and sorbitan monostearate, and polyoxyethylene higher alcohol ethers such as pentaoxyethylene oleyl alcohol ether. Anionic surfactants include sodium dodecyl sulfate, sodium dodecylbenzenesulfonate, and naphthalenesulfonate-formaldehyde condensates. Cationic surfactants include dodecyltrimethylammonium chloride, stearyltrimethylammonium chloride, and distearyldimethylammonium chloride. Two or more of these can also be combined. Polymerization in water in the presence of a surfactant acts to finely disperse the hydrophobic monomer, promoting copolymerization. If the amount of the surfactant is small, the effect of finely dispersing the monomer is small, and if the amount is too large, it may cause foaming when dissolved or used. The surfactant addition rate is 0.01% by mass to 5% by mass, preferably 0.05% by mass to 3% by mass, and more preferably 0.1% by mass to 1% by mass, based on the total monomer.

[0014] In the present invention, a chain transfer agent can be used. Examples of the chain transfer agent include alkyl mercaptans, thioglycolic acid and its esters, isopropyl alcohol, allyl alcohol, allylamine, sodium hypophosphite, etc. Also included are monomers such as methallylsulfonates, such as sodium methallylsulfonate, potassium methallylsulfonate, and ammonium methallylsulfonate.

[0015] Examples of the polymerization initiator include azo-based polymerization initiators such as 2,2'-azobis[2-(5-methyl-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, and 2,2'-azobis-2-amidinopropane dihydrochloride. Other examples include persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate, and peroxides such as hydrogen peroxide and benzoyl peroxide. These can be used alone, but can also be used as redox-based polymerization initiators in combination with reducing agents such as sulfites and hydrogen sulfites. The addition rate of the polymerization initiator is 0.01% by mass to 2% by mass, preferably 0.1% by mass to 1% by mass, based on the total monomers.

[0016] The polymerization concentration is 10% by mass to 80% by mass in terms of monomer concentration, and preferably 15% by mass to 60% by mass. The polymerization reaction is usually carried out at a temperature of 30° C. to 100° C. for a time of 0.5 to 20 hours.

[0017] The obtained polymer preferably has a viscosity of 5 to 200 mPa·s in a 1% by mass aqueous solution of the polymer. More preferably, it is 15 to 170 mPa·s. The viscosity is measured with a B-type viscometer at 60 rpm and 25°C. If the viscosity is lower than this range, the paper strength enhancing effect is insufficient. If the viscosity is higher than this range, the solubility decreases and handling becomes difficult. As the B-type viscometer, a general-purpose product such as the B8M model or TVB-10M model manufactured by Toki Sangyo Co., Ltd. is appropriately used. If the viscosity is 100 mPa·s or less, a No. 1 rotor is used.

[0018] The effect of enhancing the effect of the polymeric paper strength agent in the present invention will now be described. It is believed that the cationic group portion of the strength agent interacts with the carboxyl group of the pulp to exert the paper strength enhancing effect. However, the distribution of the carboxyl group of the pulp is not uniform, and the strength agent is preferentially distributed in the area with a high density of carboxyl groups, and the distribution of the strength agent on the pulp is also uneven, and it is believed that the paper strength enhancing effect cannot be fully exerted. It is believed that by adding the polymer with a high density of cationic groups in the present invention, the polymer is preferentially adsorbed to the area with a high density of carboxyl groups, uniformizing the distribution of the strength agent on the pulp and promoting the paper strength enhancing effect. It is known that cationic polymers copolymerized with hydrophobic monomers form micelles in water. Cationic polymers copolymerized with hydrophobic monomers are believed to effectively block localized carboxymethyl groups on the pulp, uniformly distribute the paper strength agent on the pulp, and further promote the paper strength enhancement effect. In addition, micellar cationic polymers have an increased cationic group density, which is believed to contribute to improving the adhesion between pulps.

[0019] The location where the polymer in the present invention is added is the vicinity of the location where the paper strength agent is added. Generally, the paper strength agent is added to the raw paper material before papermaking where the pulp dry solids concentration is 2.0 mass% or more upstream of the papermaking process, such as a refiner, a raw material blending chest, a mixing chest, a machine chest, or a seed box. In this case, the polymer in the present invention is also added to the raw paper material. In the papermaking process, the high-concentration papermaking raw material transferred from the upstream with a pulp dry solids concentration of 2.0% by mass or more is diluted with white water or fresh water just before the papermaking machine to a papermaking raw material with a pulp dry solids concentration of less than 2.0% by mass. Generally, it is diluted to 0.5 to 1.5% by mass, and these are called inlet raw materials or headbox raw materials. In some cases, a paper strength agent is added to these raw materials (hereinafter referred to as inlet raw materials), and in this case, the polymer of the present invention is also added to the papermaking raw material. In this case, the addition location of the process is before or after the fan pump or before or after the screen, which is the shearing process. The order of addition of the paper strength enhancer may be before or after the paper strength enhancer, or they may be added simultaneously. In view of the mechanism of the paper strength promotion effect in the present invention, it is preferable to add the paper strength enhancer before or simultaneously with the addition of the paper strength enhancer.

[0020] The types of paper to which the polymer-based papermaking additive of the present invention is applied include newsprint, wood-free printing paper, medium-quality printing paper, gravure printing paper, PPC paper, coated base paper, lightly coated paper, packaging paper, liner and core raw paper boards, etc. Among these, liner and core raw paper boards, etc., which require a stronger effect of the paper strength enhancer, are preferred. The addition rate is 1% by mass to 100% by mass (polymer pure content) of the paper strength enhancer (pure content). The polymer pure content is 0.003 to 1% by mass, preferably 0.005 to 0.5% by mass, based on the pulp dry solid content. In addition, it can be used in combination with other papermaking chemicals such as sizing agents, aluminum sulfate, pitch control agents, retention aids, and drainage aids.

[0021] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. EXAMPLES

[0022] (Production Example 1) In a 500mL four-neck flask, 62.5g of 80% by mass methacryloyloxyethyltrimethylammonium chloride, 187.5g of demineralized water, and 0.1g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of a 1% by mass aqueous solution of the obtained polymer was 16.4 mPa·s. The results are shown in Table 1.

[0023] (Production Example 2) In a 500mL four-neck flask, 10.0g of styrene, 50.0g of 80% by mass methacryloyloxyethyl trimethylammonium chloride, 189.1g of demineralized water, 0.5g of sodium dodecyl sulfate, and 0.01g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of a 1% by mass aqueous solution of the obtained polymer was 20.2 mPa·s. The results are shown in Table 1.

[0024] (Production Example 3) In a 500mL four-neck flask, 50.0g of 50% acrylamide, 31.8g of 80% methacryloyloxyethyl trimethylammonium chloride, 167.3g of demineralized water, 0.05g of sodium hypophosphite, and 0.05g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of a 1% by mass aqueous solution of the obtained polymer was 42.0mPa·s. The results are shown in Table 1.

[0025] (Production Example 4) In a 500mL four-neck flask, 30.0g of 50% acrylamide, 43.9g of 80% methacryloyloxyethyltrimethylammonium chloride, 175.1g of demineralized water, 0.05g of sodium hypophosphite, and 0.05g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of the 1% by mass aqueous solution of the obtained polymer was 24.0mPa·s. The results are shown in Table 1.

[0026] (Production Example 5) In a 500mL four-neck flask, 0.5g of dodecyl methacrylate, 61.9g of 80% by mass methacryloyloxyethyl trimethylammonium chloride, 187.3g of demineralized water, 0.5g of sodium dodecyl sulfate, and 0.05g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of a 1% by mass aqueous solution of the obtained polymer was 26.5 mPa·s. The results are shown in Table 1.

[0027] (Production Example 6) In a 500mL four-neck flask, 0.5g of dodecyl methacrylate, 1.0g of styrene, 60.6g of 80% by mass methacryloyloxyethyl trimethylammonium chloride, 187.2g of demineralized water, 0.5g of sodium dodecyl sulfate, and 0.05g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of the 1% by mass aqueous solution of the obtained polymer was 112.0mPa·s. The results are shown in Table 1.

[0028] (Production Example 7) In a 500mL four-neck flask, 20.0g of styrene, 24.7g of dimethylaminoethyl methacrylate, 15.8g of 35% by mass hydrochloric acid, 187.2g of demineralized water, 0.5g of sodium dodecyl sulfate, and 0.05g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of a 1% by mass aqueous solution of the obtained polymer was 23.4mPa·s. The results are shown in Table 1.

[0029] (Production Example 8) In a 500mL four-neck flask, 1.0g of 2-ethylhexyl acrylate, 61.3g of 80% by mass methacryloyloxyethyl trimethylammonium chloride, 187.3g of demineralized water, 0.5g of sodium dodecyl sulfate, and 0.05g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of the 1% by mass aqueous solution of the obtained polymer was 155.5mPa·s. The results are shown in Table 1.

[0030] (Production Example 9) In a 500mL four-neck flask, 0.5g of stearyl methacrylate, 2.5g of styrene, 59.0g of 80% by mass methacryloyloxyethyl trimethylammonium chloride, 188.2g of demineralized water, 0.5g of sodium dodecyl sulfate, and 0.05g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of a 1% by mass aqueous solution of the obtained polymer was 164.0mPa·s. The results are shown in Table 1.

[0031] (Production Example 10) In a 500mL four-neck flask, 2.5g of dodecyl methacrylate, 5.1g of styrene, 53.1g of 80% by mass methacryloyloxyethyl trimethylammonium chloride, 188.2g of demineralized water, 0.5g of sodium dodecyl sulfate, and 0.05g of 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride (VA-044, manufactured by Wako Pure Chemical Industries) were charged and nitrogen gas was passed through while stirring at 150 rpm. After 30 minutes, the temperature was raised to 50°C and maintained for 3 hours. Then, the temperature was maintained at 70°C for 2 hours. After cooling, an aqueous polymer solution was obtained. The viscosity of the 1% by mass aqueous solution of the obtained polymer was 67.5mPa·s. The results are shown in Table 1.

[0032] (Table 1) TIFF0007571996000001.tif4289Cationic monomer; DMM: dimethylaminoethyl methacrylate, DMC: methacryloyloxyethyl trimethyl ammonium chloride Hydrophobic monomer; St: styrene, DDM: dodecyl methacrylate, 2EHA: 2-ethylhexyl acrylate, SMA: stearyl methacrylate Nonionic monomer; AAM: acrylamide Viscosity of 1% by mass aqueous solution: measured using a B-type viscometer at 60 rpm and 25°C.

[0033] In addition, commercially available paper strength agents 1 to 3 were prepared. Their compositions and physical properties are shown in Table 2.

[0034] (Table 2) TIFF0007571996000002.tif2789

[0035] Example 1 As a paper stock, waste cardboard was beaten with a Niagara beater to a degree of beating of 300 mL. This was used as a pulp slurry with a pulp concentration of 1% by mass (pH 7.3, electrical conductivity 117.1 mS / m). To 500 mL of this pulp slurry, 0.01% by mass of the polymer sample production example 1 of the present invention in Table 1 and 0.3% by mass of the paper strength enhancer 1 in Table 2 were added based on the pulp solid content, and the mixture was stirred at 800 rpm for 1 minute, and then paper was made on a TAPPI standard paper machine (using an 80 mesh wire), pressed for 5 minutes at a pressure of 410 kPa, and dried for 3 minutes at 105°C using a rotating drum wire. The mixture was conditioned for 24 hours under conditions of a temperature of 23°C and a humidity of 50%, and the basis weight was 80 g / cm. 2The paper was obtained. The burst strength and compression strength of the obtained paper were measured and expressed as specific burst strength and specific compression strength, respectively. The burst strength was measured using a Mullen burst tester (manufactured by Kumagai Riki Kogyo Co., Ltd.) in accordance with JIS P 8131, and the compression strength was measured using a short span compression tester (Compressive Strength Tester STFI, manufactured by L&W Co., Ltd.) in accordance with JIS P 8126. The same tests were also carried out for Production Examples 2 to 4. The results are shown in Table 3.

[0036] Comparative Example 1 Using the same pulp slurry as in Example 1, the same test as in Example 1 was carried out without using the polymer sample of the present invention. The results are shown in Table 3.

[0037] (Table 3) TIFF0007571996000003.tif5189

[0038] It was found that the effect of the paper strength agent was enhanced by the use of the polymer sample of the present invention in combination with the paper strength agent, compared to the use of the paper strength agent alone. The polymer sample preparation example 2 obtained by using a cationic monomer and a hydrophobic monomer was the most effective.

[0039] Example 2 Using the same pulp slurry as in Example 1, tests similar to those in Example 1 were carried out using Polymer Sample Production Examples 5 to 7 of the present invention. The results are shown in Table 4.

[0040] Comparative Example 2 Using the same pulp slurry as in Example 1, the same test as in Example 1 was carried out without using the polymer sample of the present invention. The results are shown in Table 4.

[0041] (Table 4) TIFF0007571996000004.tif4689

[0042] Compared to the addition of a paper strength agent alone, the use of the polymer sample of the present invention in combination with the paper strength agent was found to have an effect of enhancing the effect of the paper strength agent. It was found that the effect tends to be greater when the hydrophobic monomer content is high and the viscosity of the 1% by mass aqueous solution is high.

[0043] Example 3 Using the same pulp slurry as in Example 1, a test similar to that in Example 1 was carried out using the polymer sample production example 8 of the present invention. The effective addition ratio of the paper strength agent and the polymer sample of the present invention was investigated. The results are shown in Table 5.

[0044] Comparative Example 3 Using the same pulp slurry as in Example 1, tests similar to those in Example 1 were carried out using the paper strength agent alone or the polymer sample of the present invention alone. The results are shown in Table 5.

[0045] (Table 5) TIFF0007571996000005.tif4389

[0046] In a comparison of the same total addition rate, the effect of enhancing paper strength was observed when a small amount of the polymer sample of the present invention was used in combination, compared to the addition of a paper strength enhancer alone.

[0047] Example 4 Using the same pulp slurry as in Example 1, tests similar to those in Example 1 were carried out using paper strength agents 2 and 3. The results are shown in Table 6.

[0048] Comparative Example 4 Using the same pulp slurry as in Example 1, the same test as in Example 1 was carried out without using the polymer sample of the present invention. The results are shown in Table 6.

[0049] (Table 6) TIFF0007571996000006.tif4289

[0050] Addition of a small amount of the polymer sample of the present invention to any of the paper strength agents was found to have a significant effect of promoting the paper strength agent.

Claims

1. The papermaking additive is a polymer obtained by polymerizing a monomer component containing 30% by mass to 100% by mass of a cationic monomer based on the total monomers, and the method for enhancing the effect of a paper strength agent is characterized in that the papermaking additive is added to a papermaking raw material prior to papermaking in an amount of 1% by mass to 100% by mass (pure polymer content) of the paper strength agent (pure content) before or simultaneously with the addition of the paper strength agent.

2. 2. The method for enhancing the effect of a paper strength agent according to claim 1, wherein the polymer is obtained by polymerizing a monomer component containing a hydrophobic monomer.

3. The method for enhancing the effect of a paper strength agent according to claim 2, characterized in that the polymer is obtained by polymerizing a monomer component containing more than 0% by mass to 50% by mass of hydrophobic monomers relative to the total monomers.

4. The method for enhancing the effect of a paper strength agent according to any one of claims 1 to 3, characterized in that the viscosity (25°C) of a 1% by mass aqueous solution of the polymer is 5 to 200 mPa·s when measured with a B-type viscometer at a rotation speed of 60 rpm.

Citation Information

Patent Citations

  • Additive for making paper

    JP2002115199A

  • Service system for providing local information

    JP2003324523A

  • Organic coagulant and method for treating waste water or sludge

    JP2007029766A

  • Polymer flocculant

    JP2008296154A

  • Powder type paper-strengthening agent, manufacturing method of powder type paper-strengthening agent, paper-strengthening agent solution and paper

    JP2020147875A