Semiconductor device and method for manufacturing floating gate device

A semiconductor device with a floating gate structure using N-doped LaB and organic semiconductors reduces operating voltage, facilitating low-voltage operation and enabling applications in nonvolatile memory and neural calculation elements.

JP7571999B2Active Publication Date: 2024-10-23INSTITUTE OF SCIENCE TOKYO
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021028111
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-10-23
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

Conventional floating gate transistors made of organic semiconductors require high voltages exceeding tens of volts for writing and erasing, and there is a need for lower voltages to accommodate applications in nonvolatile memory and neural calculation elements.

Method used

A semiconductor device with a floating gate device comprising a control gate, a block layer of N-doped LaB, a floating gate containing N-doped LaB, a tunnel layer, a channel layer of organic semiconductor, and an electrode, which can be manufactured using an in-situ process to reduce operating voltage.

Benefits of technology

The device operates at low voltages, enabling applications in nonvolatile memory and neural calculation elements, and allows for the use of flexible or glass substrates due to low-temperature processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571999000001
    Figure 0007571999000001
  • Figure 0007571999000002
    Figure 0007571999000002
  • Figure 0007571999000003
    Figure 0007571999000003
Patent Text Reader

Abstract

To provide floating gate devices that can operate at lower voltages than conventional floating gate devices.SOLUTION: A block layer 120 includes a LaBxNy insulating layer and is formed on a control gate 110. A floating gate 130 includes an N-doped LaB6 metal layer and is formed on a block layer 120, and a tunnel layer 140 includes an N-doped LaB6 metal layer and is formed on the floating gate 130. A channel layer 150 includes an organic semiconductor and is formed on top of the tunnel layer 140.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to floating gate devices. [Background technology]

[0002] In recent years, with the trend toward higher performance and lower power consumption in portable information and communication devices, it has become important to increase the capacity, speed and power consumption of non-volatile memories, such as flash memories, which are semiconductor memories used in integrated circuits.

[0003] A non-volatile memory cell uses a floating gate transistor or a floating gate diode (in this specification, transistors and diodes are collectively referred to as floating gate devices). [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] K. Nagaoka, et al., Vacuum, 170, 108973 (2019). [Non-Patent Document 2] J. Li et al., ACS Appl. Mater. Interfaces, 6, 12815 (2014). [Non-Patent Document 3] SJ Kim et al., J. Mater. Chem. 21, 14516 (2011). [Non-Patent Document 4] SJ Kim et al., Nano Lett. 10, 2884 (2010). [Non-Patent Document 5] D. Son et al., ACS Nano, 9, 5585 (2015). [Non-Patent Document 6] HS Kim et al., Jpn. J. Appl. Phys. 53, 031602 (2014). Summary of the Invention [Problem to be solved by the invention]

[0005] Conventional organic semiconductor floating gate transistors require high voltages of more than 10 V to several tens of V for writing and erasing, and there is a demand for lower voltages (Non-Patent Documents 2 to 6).

[0006] In addition to non-volatile memory, the applications of floating gate devices are expected to expand to include neural computing elements in neural networks and analog memory elements, and low voltage operation is also required for these applications.

[0007] The present disclosure has been made in this context, and one exemplary purpose of an embodiment thereof is to provide a floating gate device that can operate at a lower voltage than conventional floating gate devices. [Means for solving the problem]

[0008] A semiconductor device according to an embodiment of the present disclosure includes a floating gate device. The floating gate device includes a control gate and a LaB x N y The device comprises a block layer including a (lanthanum hexaboride nitride) insulating layer, a floating gate including an N-doped LaB6 (nitrogen-doped lanthanum hexaboride) metal layer formed on the block layer, a tunnel layer including the N-doped LaB6 metal layer formed on the floating gate, a channel layer including an organic semiconductor formed on the tunnel layer, and an electrode formed on the channel layer.

[0009] Another aspect of the present disclosure is a method for fabricating a floating gate device, the method including forming a control gate, depositing LaB x N y forming a first insulating layer comprising: No. 1 On the metal layer, LaB x N yforming a second insulating layer including: forming an organic semiconductor layer on the second insulating layer; thing forming an electrode on the semiconductor layer. Effect of the Invention

[0010] According to an aspect of the present disclosure, a floating gate device that operates at low voltages can be provided. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view of a semiconductor device according to a first embodiment. [Diagram 2] FIG. 2 is a band diagram for the floating gate diode of FIG. 1. [Diagram 3] 3(a) to (h) are diagrams illustrating a method for manufacturing the semiconductor device of FIG. [Figure 4] 4(a) and (b) are diagrams showing the evaluation results of the first sample of the fabricated diode. [Diagram 5] FIG. 13 is a diagram showing the results of program / erase (P / E) measurement of a first sample of the fabricated diode. [Figure 6] FIG. 13 is a diagram showing the results of program / erase (P / E) measurement of a first sample of the fabricated diode. [Figure 7] FIG. 11 is a cross-sectional view of a semiconductor device according to a second embodiment. [Figure 8] 8(a) to 8(h) are diagrams illustrating a method for manufacturing the semiconductor device of FIG. [Figure 9] FIG. 11 is a diagram showing the drain current-drain voltage characteristics (ID-VD characteristics) of a first sample of the fabricated transistor. [Figure 10] FIG. 13 is a diagram showing measurement results of program / erase (P / E) of a first sample of the fabricated transistor. [Figure 11] FIG. 13 is a diagram showing the results of program / erase (P / E) measurement of a second sample of the fabricated transistor. [Figure 12] FIG. 11 is a cross-sectional view of a semiconductor device according to a third embodiment. [Figure 13] FIG. 13 is a band diagram of the floating gate transistor of FIG. [Figure 14] 14(a) to (h) are diagrams illustrating a method for manufacturing the semiconductor device of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] (Overview of the embodiment) A summary of some exemplary embodiments of the present disclosure will be described. This summary is intended to provide a simplified summary of some concepts of one or more embodiments in order to provide a basic understanding of the embodiments as a prelude to the detailed description that follows, and is not intended to limit the scope of the invention or disclosure. Furthermore, this summary is not intended to be a comprehensive overview of all possible embodiments, nor is it intended to limit essential components of the embodiments. For convenience, the term "one embodiment" may be used to refer to one embodiment (example or variant) or multiple embodiments (examples or variants) disclosed in this specification.

[0013] According to one embodiment, a semiconductor device includes a floating gate device. The floating gate device includes a control gate and a LaB x N y The device comprises a block layer including an insulating layer, a floating gate including an N-doped LaB6 metal layer formed on the block layer, a tunnel layer including an N-doped LaB6 metal layer formed on the floating gate, a channel layer including an organic semiconductor formed on the tunnel layer, and an electrode formed on the channel layer.

[0014] According to this configuration, by adopting a stacked structure including an N-doped LaB6 metal layer having low resistivity, a floating gate device with a low operating voltage can be provided. x N yThe laminated structure using an insulating layer allows each layer to be easily thinned, which also reduces the operating voltage. In addition, the insulating layer and metal layer can be formed by an in-situ process, making it easy to manufacture devices with high-quality interface characteristics. In addition, high-temperature processing is required when using Si as the channel layer, but this device allows low-temperature processing, which increases the selection of materials that can be used for the substrate, etc.

[0015] In one embodiment, the organic semiconductor may include pentacene. Organic semiconductors may include a variety of p-type and n-type materials.

[0016] In one embodiment, the control gate may include an N-doped LaB6 metal layer formed on the substrate, allowing the control gate to be formed in the same in-situ process as the insulating and metal layers.

[0017] In one embodiment, the substrate may be a glass substrate or a flexible substrate. The above-mentioned semiconductor device can be subjected to a series of processes including heat treatment at a low temperature of 200° C. or less, so that a glass substrate or a flexible substrate having a low melting point can be used. This makes it possible to provide a semiconductor device having a large area or a flexible shape.

[0018] In one embodiment, the substrate may be a Si substrate, which provides a semiconductor device with a stable shape, similar to conventional Si semiconductor devices.

[0019] In one embodiment, the control gate may include a Si substrate.

[0020] In one embodiment, Floating Gate Device may be a memory element that stores information according to a signal applied to the control gate.

[0021] In one embodiment, the electrodes may include Au.

[0022] In one embodiment, the floating gate device may be a floating gate diode.

[0023] In one embodiment, the floating gate device may be a floating gate transistor.

[0024] A method for fabricating a floating gate device according to one embodiment includes forming a control gate, depositing LaB x N y forming a first insulating layer comprising: No. 1 On the metal layer, LaB x N y forming a second insulating layer including: forming an organic semiconductor layer on the second insulating layer; thing forming an electrode on the semiconductor layer.

[0025] This makes it possible to provide a semiconductor device that operates at a low voltage.

[0026] In one embodiment, the steps of forming the first insulating layer, forming the first metal layer, and forming the second insulating layer may be performed in-situ by switching the atmospheric gas using a sputtering method with an N-doped LaB6 target, thereby reducing the manufacturing time and / or manufacturing cost.

[0027] In one embodiment, the atmospheric gas in the step of forming the first metal layer may be a rare gas, and the atmospheric gas in the step of forming the first insulating layer and the second insulating layer may be a mixed gas of the rare gas and nitrogen. Specifically, the atmospheric gas in the step of forming the first insulating layer and the second insulating layer may be Ar / N2, and the atmospheric gas in the step of forming the first metal layer may be Ar. The atmospheric gas in the step of forming the first insulating layer and the second insulating layer may be Kr / N2, and the atmospheric gas in the step of forming the first metal layer may be Kr. The atmospheric gas in the step of forming the first insulating layer and the second insulating layer may be Xe / N2, and the atmospheric gas in the step of forming the first metal layer may be Xe. Ar is more advantageous than Kr and Xe in terms of cost, and Kr and Xe can reduce damage compared to Ar.

[0028] In one embodiment, forming the control gate may include forming a second metal layer comprising N-doped LaB6 on the substrate.

[0029] In one embodiment, the steps of forming the first insulating layer, the first metal layer, and the second insulating layer may be performed at a temperature of 200° C. or less, which allows the selection of a material with a low melting point for the base substrate.

[0030] (Embodiment) Hereinafter, the present disclosure will be described with reference to the drawings based on preferred embodiments. The same or equivalent components, parts, and processes shown in each drawing will be given the same reference numerals, and duplicated descriptions will be omitted as appropriate. In addition, the embodiments are illustrative and do not limit the invention, and all features and combinations thereof described in the embodiments are not necessarily essential to the invention.

[0031] In this specification, "a state in which component A is connected to component B" includes a case in which component A and component B are directly physically connected to each other, and a case in which component A and component B are indirectly connected to each other via other components that do not substantially affect the electrical connection state between them or that do not impair the function or effect achieved by their combination.

[0032] Similarly, "a state in which component C is provided between components A and B" includes not only the case in which components A and C, or components B and C, are directly connected to each other, but also the case in which they are indirectly connected to each other via other components that do not substantially affect the electrical connection between them or that do not impair the functions or effects achieved by their combination.

[0033] In addition, the dimensions of the components in each drawing are shown enlarged or reduced as appropriate to facilitate understanding.

[0034] (Embodiment 1) 1.1 Device structure 1 is a cross-sectional view of a semiconductor device 100 according to embodiment 1. The semiconductor device 100 includes a floating gate diode 102, which is a floating gate device.

[0035] The floating gate diode 102 has a laminated structure including a back electrode 104, an upper electrode 106, a control gate (CG) 110, a block layer (BL) 120, a floating gate (FG) 130, a tunnel layer (TL) 140, and a channel layer (CH) 150.

[0036] The control gate 110 is + The substrate is a Si(100) substrate, and a back electrode 104 is formed on the bottom surface thereof. The back electrode 104 is preferably made of Al, but is not limited to this, and any material that can make contact with the material (Si) of the control gate 110 may be selected, and metals other than Al, such as W or TiN, may also be used.

[0037] The blocking layer 120 is a LaB x N y The insulating layer includes:

[0038] The floating gate 130 comprises a metal layer of N-doped LaB6 formed on the blocking layer 120.

[0039] The tunnel layer 140 comprises an N-doped LaB6 metal layer formed on the floating gate 130 .

[0040] The channel layer 150 includes a thin film of an organic semiconductor formed on the tunnel layer, the organic semiconductor being, but not limited to, a polycyclic aromatic hydrocarbon, with pentacene being preferred.

[0041] The upper electrode 106 is formed on the channel layer 150. The upper electrode 106 is preferably made of Au, but is not limited to this and any material that can make contact with the organic semiconductor of the channel layer 150 may be selected, and metals other than Au, such as Ag and Pt, may also be used.

[0042] 2 is a band diagram of the floating gate diode 102 of FIG 1. The Au of the upper electrode 106 has a work function φ M Pentacene has a LUMO level of 3.2 eV and a HOMO level of 5 eV.

[0043] LaB x N y The band structure of the insulating layer has not been clarified in detail at present. However, the tunnel layer 140 and the block layer 120 are x N y Since it exhibits electrical properties similar to those of h-BN (hexagonal boron nitride), it is assumed to have the band structure of h-BN and is shown to have a forbidden band of 6.42 eV.

[0044] The configuration of the semiconductor device 100 has been described above.

[0045] 1.2 Manufacturing method 3(a) to (h) are diagrams illustrating a method for manufacturing the semiconductor device 100 of FIG.

[0046] First, as shown in FIG. 3(a), n + The -Si(100) substrate is chemically cleaned. The cleaning may be a combination of SPM (sulfuric acid / hydrogen peroxide) cleaning and DHF (dilute hydrofluoric acid) cleaning.

[0047] 3(b) to (d), a LaB layer that will become a block layer 120, a floating gate 130, and a tunnel layer 140 is formed on the control gate 110. x N y layer (first insulating film), N-doped LaB6 (metal film), LaB x N y A laminate structure of a layer (second insulating film) is formed. This laminate structure can be formed in-situ by RF sputtering at room temperature.

[0048] Specifically, by using N-doped LaB6 as a target and switching the atmospheric gas between Ar / N2 and Ar, it is possible to selectively form a metal film in an Ar atmosphere and an insulating film in an Ar / N2 atmosphere.

[0049] After the formation of the laminated structure of FIG. 3(d), metallization is performed, and then a heat treatment (for example, a PMA (Post-Metallization-Anneal) treatment) is performed as shown in FIG. 3(e).

[0050] 3(f), a thin film of pentacene that will become the channel layer 150 is formed on the tunnel layer 140. The channel layer 150 can be formed by thermal evaporation.

[0051] 3(g), the Au top electrode 106 is formed on the channel layer 150. The top electrode 106 can be formed by thermal evaporation.

[0052] 3(h), an Al back electrode 104 is formed on the back surface of the control gate 110. The back electrode 104 can be formed by thermal evaporation.

[0053] The above is the method for manufacturing the semiconductor device 100. According to this manufacturing method, the atmospheric gas is switched by an in-situ process, and LaB x N y and N-doped LaB6 can be selectively formed to create a layered structure, which is advantageous in terms of manufacturing cost and time.

[0054] 1.3 Sample evaluation Next, a sample of the semiconductor device 100 that was actually fabricated (called a diode sample) and its evaluation will be described.

[0055] (1) First sample The thicknesses of the layers of the first diode sample thus fabricated are as follows: Block layer (BL) 10nm Floating gate (FG) 20nm Tunnel layer (TL) 5nm Channel layer (CH) 10nm The upper electrode had a diameter of φ100 μm.

[0056] The conditions for forming each layer are as follows.

[0057] As described above, the stacked structure of the block layer (BL), floating gate (FG), and tunnel layer (TL) was formed by an in-situ process using a plasma sputtering method with an N-doped LaB6 target (N: 0.4%).

[0058] The conditions for forming each layer are as follows. Block layer (BL) 0.47 Pa (Ar / N2 gas flow ratio: 10 / 7 sccm) Floating gate (FG) 0.35 Pa (Ar gas flow rate: 10 sccm) Tunnel layer (TL) 0.47 Pa (Ar / N2 gas flow ratio: 10 / 7 sccm)

[0059] The heat treatment process after the formation of the laminated structure was carried out at 400°C / 1 min in N2 (1 SLM).

[0060] The channel layer (CH) was prepared by dissolving pentacene at room temperature at 5×10 -6 The films were deposited by thermal evaporation at a growth rate of 0.3 nm / min at Torr.

[0061] The evaluation results of the first sample of the diode fabricated under the above conditions will be described below.

[0062] 4(a) and (b) are diagrams showing the evaluation results of the first sample of the fabricated diode. The evaluation was performed at room temperature, with the top electrode 106 grounded (0 V) and the back electrode 104 applied with a pulsed gate voltage V G The following changes were made:

[0063] FIG. 4(a) shows the CV characteristics, with the horizontal axis representing the applied gate voltage V G The vertical axis indicates the capacitance per unit area. The CV characteristics are G The measurements were performed by changing the frequency from 10 kHz to 100 kHz to 1 MHz. The maximum capacitance was 0.76 μF / cm at 100 kHz. 2 It was.

[0064] The hysteresis is negligible at 46 mV and no frequency dispersion is observed between the 10 kHz and 100 kHz results, suggesting excellent interface properties between the pentacene channel layer and the N-doped LaB6 tunnel layer 140.

[0065] FIG. 4(b) shows the JV characteristics (current-voltage characteristics), where the horizontal axis is the applied gate voltage V G The vertical axis indicates the current density. The current density is V G = 7.2 x 10 at -3V -3 A / cm 2 This indicates that the insulating properties are good.

[0066] 5 is a diagram showing the results of program / erase (P / E) measurement of the first sample of the fabricated diode, where the horizontal axis indicates voltage and the vertical axis indicates capacitance, and the results are shown when operated at 1 MHz.

[0067] The square plots show the initial voltage-capacitance characteristics, the circle plots show the voltage-capacitance characteristics after programming, and the triangle plots show the voltage-capacitance characteristics after erasing.

[0068] Program voltage and time (V PGM / t PGM ) are -4V and 10ms, respectively, and the erase voltage and time (V ERS / t ERS ) is 4V, 10ms. The memory window at this time is 1V.

[0069] The program voltage and erase voltage of ±4V can be said to be much smaller than those of conventional organic semiconductor floating gate diodes, which indicates that the floating gate diode 102 according to the first embodiment can be suitably used as a floating gate memory element.

[0070] (2) Second sample Next, we will explain the second sample, which was produced under different conditions. The second sample has the same size and layer structure as the first sample, but differs from the first sample in that the heat treatment was performed under the conditions of 200°C / 1min (N2:1SLM).

[0071] 6 is a diagram showing the results of program / erase (P / E) measurement of the first sample of the fabricated diode, where the horizontal axis indicates voltage and the vertical axis indicates capacitance, and the results are shown when operated at 1 MHz.

[0072] For the second sample obtained by heat treatment at 200°C, a memory window of 0.5 V was obtained by applying a program voltage of -4 V for 10 ms and an erase voltage of 4 V for 10 ms, demonstrating that it can be used as a memory element operating at low voltages.

[0073] (Embodiment 2) 2.1 Device structure 7 is a cross-sectional view of a semiconductor device 200 according to embodiment 2. The semiconductor device 200 includes a floating gate transistor 202. The layer structure of the floating gate transistor 202 is substantially the same as that of the floating gate diode 102 in FIG. 1, but a source electrode 206 and a drain electrode 208 are formed instead of the upper electrode 106.

[0074] The band structure of the floating gate transistor 202 of the semiconductor device 200 is omitted since it is similar to the band diagram (FIG. 2) of the floating gate diode 102 of FIG.

[0075] The above is the configuration of the semiconductor device 200.

[0076] 2.2 Manufacturing method 8(a) to 8(h) are diagrams illustrating a method for manufacturing the semiconductor device 200 of Fig. 2. The method for manufacturing the semiconductor device 200 is basically the same as the method for manufacturing the semiconductor device 100 of Fig. 1.

[0077] First, as shown in FIG. 8(a), n + The -Si(100) substrate is chemically cleaned. The cleaning may be a combination of SPM (sulfuric acid / hydrogen peroxide) cleaning and DHF (dilute hydrofluoric acid) cleaning.

[0078] 8(b) to (d), a LaB layer that will become a block layer 120, a floating gate 130, and a tunnel layer 140 is formed on the control gate 110. x N y layer (first insulating film), N-doped LaB6 (metal film), LaB x N y A laminate structure of a layer (second insulating film) is formed. This laminate structure can be formed in-situ by RF sputtering at room temperature.

[0079] After the laminated structure of FIG. 8(d) is formed, a heat treatment is performed as shown in FIG. 8(e).

[0080] 8(f), a thin film of pentacene that will become the channel layer 150 is formed on the tunnel layer 140. The channel layer 150 can be formed by thermal evaporation.

[0081] 8(g), a source electrode 206 and a drain electrode 208 made of Au are formed on the channel layer 150. The source electrode 206 and the drain electrode 208 can be formed by thermal evaporation.

[0082] 8(h), an Al back electrode 204 is formed on the back surface of the control gate 110. The back electrode 204 can be formed by thermal evaporation.

[0083] The above is the method for manufacturing the semiconductor device 200. According to this manufacturing method, the atmospheric gas is switched by an in-situ process, and LaB x N y and N-doped LaB6 can be selectively formed to create a layered structure, which is advantageous in terms of manufacturing cost and time.

[0084] Next, a sample of the semiconductor device 200 that was actually fabricated and its evaluation will be described.

[0085] 2.3 Sample evaluation (1) First sample The thicknesses of the layers of the fabricated first sample of the transistor are as follows: Block layer (BL) 10nm Floating gate (FG) 20nm Tunnel layer (TL) 5nm Channel layer (CH) 10nm Moreover, the source electrode 206 and the drain electrode 208 each had a diameter of φ100 μm, and the element size (channel length / channel width) of the transistor was L / W=320 μm / 100 μm.

[0086] The conditions for forming each layer are as follows.

[0087] As described above, the stacked structure of the block layer (BL), floating gate (FG), and tunnel layer (TL) was formed by an in-situ process using a plasma sputtering method with an N-doped LaB6 target (N: 0.4%).

[0088] The conditions for forming each layer are as follows. Block layer (BL) 0.47 Pa (Ar / N2 gas flow ratio: 10 / 7 sccm) Floating gate (FG) 0.35 Pa (Ar gas flow rate: 10 sccm) Tunnel layer (TL) 0.47 Pa (Ar / N2 gas flow ratio: 10 / 7 sccm)

[0089] The heat treatment process was carried out at 400 °C / 1 min in N2 (1 SLM).

[0090] The channel layer (CH) was prepared by dissolving pentacene at room temperature at 5×10 -6 The films were deposited by thermal evaporation at a growth rate of 0.3 nm / min at Torr.

[0091] The evaluation results of the first sample of the transistor manufactured under the above conditions will be described below.

[0092] Figure 9 shows the drain current-drain voltage characteristics (I D -V D The horizontal axis shows the drain voltage V D The vertical axis is the drain current I D Shows.

[0093] The evaluation was performed at room temperature, with the source electrode 206 grounded (0 V) and the drain electrode 208 applied with a drain voltage V D is applied to the rear electrode 204, and a gate voltage V G The gate voltage V G was changed in 1 V steps in the range of 0 to -2 V.

[0094] The subthreshold slope (SS) is 549 mV / dec, and the mobility μ satis 1.03 × 10 -3 cm 2 / (V s).

[0095] FIG. 10 shows the measurement results of program / erase (P / E) of the first sample of the fabricated transistor. FIG. 10 shows the drain current-gate voltage characteristics (I D -V G The square plots show the characteristics in the initial state before programming, the circle plots show the characteristics after programming, and the triangle plots show the characteristics after erasing.

[0096] For programming / erasing, the source electrode 206 and the drain electrode 208 are grounded (0 V), and a pulse voltage V pulse As with the first sample of the diode described above, the program voltage and time (V PGM / t PGM ) are -4V and 10ms, respectively, and the erase voltage and time (V ERS / t ERS ) are 4V and 10ms respectively.

[0097] Through programming and erasing, the threshold voltage Vth of the floating gate transistor 202 shifts from -1.01V to -0.53V, and therefore the memory window is 0.48V.

[0098] (2) Second sample Next, we will explain the second sample, which was produced under different conditions. The second sample has the same size and layer structure as the first sample, but differs from the first sample in that the heat treatment was performed under the conditions of 200°C / 1min (N2:1SLM).

[0099] FIG. 11 shows the results of program / erase (P / E) measurement of the second sample of the fabricated transistor. FIG. 11 shows the drain current-gate voltage characteristics (I D -V GThe square plots show the initial state characteristics before programming, the circle plots show the characteristics after programming, and the triangle plots show the characteristics after erasing. Programming and erasing were performed under the same conditions as the first sample, and the program voltage and time (V PGM / t PGM ) are -4V and 10ms, respectively, and the erase voltage and time (V ERS / t ERS ) are 4V and 10ms respectively.

[0100] For the second sample of the transistor obtained by heat treatment at 200°C, a memory window of 0.3 V was obtained by applying a program voltage of -4 V for 10 ms and an erase voltage of 4 V for 10 ms, demonstrating that it can be used as a low-voltage memory element.

[0101] It can be said that the program and erase voltages of ±4 V are significantly smaller than the operating voltages of conventional organic floating gate transistors, which are ±16 V to ±90 V. In addition, since there is room for optimization of the layer thickness and other aspects of the sample created this time, it is believed that in the future it will be possible to further reduce the operating voltage and further widen the memory window.

[0102] (Embodiment 3) 3.1 Device structure 12 is a cross-sectional view of a semiconductor device 300 according to embodiment 3. The semiconductor device 300 includes a floating gate transistor 302, which is a floating gate device.

[0103] The floating gate transistor 302 has a different control gate (CG) structure compared to the floating gate transistor 202 described in the second embodiment, while the block layer 320, floating gate 330, tunnel layer 340, and channel layer 350 are similar to those of the floating gate transistor 202 in the second embodiment.

[0104] 12, a metal layer of N-doped LaB6 is used as the material of the control gate 310. The control gate CG is connected to a metal wiring (not shown) and a gate terminal is drawn out.

[0105] The control gate 310 is formed on the substrate 301. As described in the second embodiment, the floating gate device described in this disclosure can undergo a series of processes, including heat treatment, at a low temperature of 200° C. or less. This means that a material with a melting point lower than 400° C. can be used. Therefore, a flexible substrate may be used for the substrate 301. In this case, all layers of the floating gate transistor 302 have flexibility, so that a semiconductor device 300 with a flexible shape can be provided. Alternatively, a glass substrate may be used for the substrate 301. In this case, a semiconductor device 300 with a large area can be provided.

[0106] The substrate 301 may be made of a material such as a Si substrate or a glass substrate on which the control gate 310 can be formed by a sputtering method described later. In the second embodiment, a Si(100) substrate is used as the control gate layer, but in the third embodiment, when the substrate 301 is a Si substrate, the Si substrate serves simply as a support member. Alternatively, when the floating gate transistor 302 is used as a memory element, a peripheral circuit is required. When a Si substrate is used as the substrate 301, transistors constituting the peripheral circuit can be integrated on the Si substrate.

[0107] FIG. 13 is a band diagram for the floating gate transistor 302 of FIG.

[0108] 3.2 Manufacturing method 14(a) to (h) are diagrams illustrating a manufacturing method of the semiconductor device 300 of FIG.

[0109] First, chemically clean the substrate 301. When a flexible substrate is used as the substrate 301, an organic solvent may be used for cleaning.

[0110] 14(b) to (e), a control gate 310, a block layer 320, a floating gate 330, and an N-doped LaB6 (first metal film) that will become a tunnel layer 340 are formed on the substrate 301. x N y layer (first insulating film), N-doped LaB6 (second metal film), LaB x N y A laminated structure of a layer (second insulating film) is formed. This laminated structure can be formed in-situ by RF sputtering at room temperature. In RF sputtering, N-doped LaB6 is used as the target, and the atmospheric gas is switched between Ar and Ar / N2, allowing the insulating film and the metal film to be selectively formed alternately.

[0111] After the laminated structure of FIG. 14(e) is formed, a heat treatment is performed as shown in FIG. 14(f).

[0112] 14(g), a thin film of pentacene that will become the channel layer 350 is formed on the tunnel layer 340. The channel layer 350 can be formed by thermal evaporation.

[0113] 14(g), a source electrode 306 and a drain electrode 308 made of Au are formed on the channel layer 350. The source electrode 306 and the drain electrode 308 can be formed by thermal evaporation.

[0114] The above is the method for manufacturing the semiconductor device 300. According to this manufacturing method, the atmospheric gas is switched by an in-situ process, and LaB x N y and N-doped LaB6 are selectively formed to form a laminated structure. In the third embodiment, it becomes possible to form the control gate (CG) by an in-situ process.

[0115] (Application) In this way, the floating gate device (102, 202, 302) capable of low voltage operation can be used as a non-volatile memory cell by utilizing the change in capacitance or threshold voltage.

[0116] The applications of floating gate devices are not limited to non-volatile memories (digital memory elements), but can also be used as analog memory elements that utilize the continuous capacitance and threshold changes according to the gate voltage, or as D / A converters.Floating gate devices can also be used as neural computing elements in neural networks, and are expected to be applied to neurodevices that mimic the human brain by performing weighting calculations on input signals.

[0117] The embodiments merely illustrate the principles and applications of the present invention, and many modifications and changes in arrangement are permitted to the embodiments without departing from the spirit of the present invention defined in the claims. [Explanation of symbols]

[0118] 100 Semiconductor device 102 Floating Gate Diode 104 Back electrode 106 Upper electrode 110 Control Gate 120 Block Layer 130 Floating Gate 140 Tunnel Layer 150 channel layer 200 Semiconductor device 202 Floating Gate Transistor 204 Back electrode 206 Source Electrode 208 Drain electrode 210 Control Gate 220 Block Layer 230 Floating Gate 240 Tunnel Layer 250 channel layer 300 Semiconductor device 301 Substrate 302 Floating Gate Transistor 306 Source Electrode 308 Drain electrode 310 Control Gate 320 Block Layer 330 Floating Gate 340 Tunnel Layer 350 channel layer

Claims

1. Equipped with a floating gate device, The floating gate device comprises: A control gate; A LaB formed on the control gate. x N y a block layer including an insulating layer; An N-doped LaB layer is formed on the blocking layer. 6 a floating gate including a metal layer; An N-doped LaB 6 a tunnel layer including a metal layer; a channel layer including an organic semiconductor formed on the tunnel layer; an electrode formed on the channel layer; A semiconductor device comprising:

2. 2. The semiconductor device according to claim 1, wherein the organic semiconductor includes pentacene.

3. The control gate is an N-doped LaB 6 3. The semiconductor device according to claim 1, further comprising a metal layer.

4. 4. The semiconductor device according to claim 3, wherein the substrate is a glass substrate or a flexible substrate.

5. 4. The semiconductor device according to claim 3, wherein the substrate is a Si substrate.

6. 3. The semiconductor device according to claim 1, wherein the control gate includes a Si substrate.

7. 5. The semiconductor device according to claim 1, wherein the floating gate device is a memory element that stores information corresponding to a signal applied to the control gate.

8. 6. The semiconductor device according to claim 1, wherein the electrode contains Au.

9. 9. The semiconductor device according to claim 1, wherein the floating gate device is a floating gate diode.

10. 9. The semiconductor device according to claim 1, wherein the floating gate device is a floating gate transistor.

11. 1. A method for manufacturing a floating gate device, comprising the steps of: forming a control gate; On the control gate, LaB x N y forming a first insulating layer comprising: On the first insulating layer, N-doped LaB 6 forming a first metal layer comprising: On the first metal layer, LaB x N y forming a second insulating layer comprising: forming an organic semiconductor layer on the second insulating layer; forming an electrode on the organic semiconductor layer; A manufacturing method comprising:

12. The steps of forming the first insulating layer, forming the first metal layer, and forming the second insulating layer are each performed by using N-doped LaB 6 12. The method according to claim 11, wherein the step of sputtering is performed in situ by switching the atmospheric gas.

13. The atmospheric gas in the step of forming the first metal layer includes one selected from the group consisting of Ar, Kr, and Xe; 13. The method according to claim 12, wherein the atmospheric gas in the steps of forming the first insulating layer and the second insulating layer is a mixed gas of the selected one and nitrogen.

14. The step of forming the control gate may include forming an N-doped LaB 6 14. The method of claim 11, further comprising forming a second metal layer comprising:

15. 15. The method according to claim 11, wherein the steps of forming the first insulating layer, the first metal layer, and the second insulating layer are performed at a temperature of 200[deg.] C. or less.

Citation Information

Patent Citations

  • Semiconductor memory device

    JP1994013626A

  • Field-effect transistor, semiconductor memory, display element, image display device, and system

    JP2011151370A

  • Low voltage flexible organic / transparent transistor for selective gas sensing, photodetecting and CMOS device applications

    US20060231882A1

  • Organic semiconductor element and CMIS semiconductor device provided with same

    WO2015044980A1