Coating Compositions and Films
A coating composition with specific urea and siloxane bond formation using aliphatic or alicyclic diisocyanates and aminosilane coupling agents addresses the limitations of existing urethane coatings, achieving enhanced scratch, alkali, and solvent resistance while maintaining surface appearance.
Patent Information
- Application Number
- JP2020037652
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-05
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-03-05
AI Technical Summary
Existing urethane coating compositions using polyisocyanate as a curing agent lack sufficient verification of chemical resistance and surface appearance when formed into coating films, particularly in terms of scratch resistance, alkali resistance, and organic solvent resistance.
A coating composition comprising a urea component derived from aliphatic or alicyclic diisocyanates and an aminosilane coupling agent, with specific isocyanate group content and mass ratios, along with compounds containing alkoxysilyl and tertiary amino groups, forms urea and siloxane bonds in the film, enhancing scratch resistance, alkali resistance, and organic solvent resistance.
The resulting coating film exhibits excellent scratch resistance, alkali resistance, and organic solvent resistance, maintaining a good surface appearance.
Smart Images

Figure 0007572151000001 
Figure 0007572151000002 
Figure 0007572151000003
Abstract
Description
[Technical field]
[0001] The present invention relates to coating compositions and films. [Background technology]
[0002] Urethane-based coating compositions using polyisocyanate as a curing agent have excellent chemical resistance, flexibility, etc., when formed into coating films, and are therefore widely used as coatings for automobiles, interior and exterior buildings, home appliances, etc. Furthermore, coating films obtained from polyisocyanates derived from aliphatic diisocyanates do not yellow and have excellent weather resistance, and are therefore used in a wide range of applications.
[0003] In recent years, there has been an increasing demand for paints and coating films with higher functionality in various fields. For example, there is an increasing need to improve the scratch resistance of coating films more than ever before. Furthermore, there is a demand for higher functionality such as chemical resistance without impairing the appearance of conventional coating films. In response to the need for high functionality as described above, various methods have been proposed. For example, in Patent Document 1, a curable resin composition is produced by reacting a part of polyisocyanate with an aminosilane coupling agent and mixing it with polyacrylic polyol, thereby achieving high scratch resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2008 / 074489 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the curable resin composition described in Patent Document 1 has not been sufficiently verified with respect to chemical resistance and surface appearance when formed into a coating film.
[0006] The present invention has been made in consideration of the above circumstances, and provides a coating composition which, when formed into a coating film, has excellent scratch resistance, alkali resistance, organic solvent resistance and surface appearance, and a film using the coating composition. [Means for solving the problem]
[0007] That is, the present invention includes the following aspects. (1) The following component (A): and Ingredients (BC) Contains (A) a urea component derived from a polyisocyanate derived from one or more diisocyanates selected from the group consisting of aliphatic diisocyanates and alicyclic diisocyanates, and an aminosilane coupling agent; (BC) Compounds having an alkoxysilyl group and a tertiary amino group in the same molecule (excluding urea compounds); The content of isocyanate groups in the component (A) is 4% by mass or more and 20% by mass or less relative to the mass of the solid content, The above components ( B.C. The mass ratio of the component (A) to the B.C. ) is 50 / 50 or more and 95 / 5 or less. ( 2 ) further containing an organic solvent, (1 ) The coating composition described herein. ( 3 ) (1) Or (2) A film obtained by curing the coating composition described in 1. Effect of the Invention
[0008] According to the coating composition of the above embodiment, it is possible to provide a coating composition which, when formed into a coating film, has excellent scratch resistance, alkali resistance, organic solvent resistance, and surface appearance. The film of the above embodiment is obtained by curing the coating composition, and has excellent scratch resistance, alkali resistance, organic solvent resistance, and surface appearance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment for carrying out the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment. The present invention can be carried out with appropriate modifications within the scope of the gist of the present invention. As used herein, the term "polyisocyanate" refers to a reaction product in which multiple monomer compounds (monomers) having one or more isocyanate groups (-NCO) are bonded together.
[0010] ≪Paint composition≫ The coating composition of the present embodiment contains the following components (A) to (C). (A) a urea component derived from a polyisocyanate derived from one or more diisocyanates selected from the group consisting of aliphatic diisocyanates and alicyclic diisocyanates, and an aminosilane coupling agent; (B) a compound containing at least one alkoxysilyl group; (C) Compounds containing one or more amine groups
[0011] In the coating composition of this embodiment, the content of isocyanate groups relative to the mass of the solid content of the component (A) is 4% by mass or more and 20% by mass or less, preferably 5% by mass or more and 20% by mass or less, more preferably 6% by mass or more and 20% by mass or less, and even more preferably 10% by mass or more and 20% by mass or less. When the content of isocyanate groups is equal to or more than the above lower limit, urea bonds can be formed when the coating film is formed, and the coating film can have good alkali resistance. On the other hand, when the content of isocyanate groups is equal to or less than the above upper limit, the coating film can have good scratch resistance, organic solvent resistance, and surface appearance.
[0012] The content of isocyanate groups can be calculated, for example, by the following method. First, (A) urea component: 1 g or more and 3 g or less (Wg) is precisely weighed out. Next, 20 mL of toluene is added to (A) urea component and dissolved. Next, 10 mL of 2N di-n-butylamine toluene solution is added to the toluene solution containing (A) urea component, and after mixing, the mixture is left at room temperature for 15 minutes. Next, 70 mL of isopropyl alcohol is added to this mixture and mixed. This liquid is titrated with 1N hydrochloric acid solution (factor F) as an indicator, and the titration value obtained is "V2mL". The same operation is performed without (A) urea component, and the titration value obtained is "V1mL". Using these titration values, the isocyanate group content relative to the solid content in the urea component is calculated from the following formula. The solid content of the urea component obtained in the synthesis example is examined, and those whose value is 98 mass% or more are directly subjected to measurement. On the other hand, for those having an isocyanate group content of less than 98% by mass, the value obtained by multiplying Wg by the proportion of solid content is introduced into the following formula instead of Wg to calculate the isocyanate group content relative to the solid content in the urea component. The solid content can be calculated using the method shown in the examples described later.
[0013] Isocyanate group content (mass%) = (V1-V2) x F x 42 / (W x 1000) x 100
[0014] In the coating composition of this embodiment, the mass ratio (A) / (B) of component (A) to component (B) is 50 / 50 or more and 95 / 5 or less, preferably 60 / 40 or more and 90 / 10 or less, and more preferably 70 / 30 or more and 85 / 15 or less. The greater the mass of component (A), the more excellent the alkali resistance of the coating film when formed, while the greater the mass of component (B), the more excellent the scratch resistance of the coating film when formed.
[0015] The mass ratio (A) / (B) of component (A) to component (B) can be calculated, for example, from the blending amounts of each component.
[0016] Furthermore, as described later, when a compound (BC) containing an alkoxysilyl group and an amino group in the same molecule (hereinafter sometimes abbreviated as "(BC) alkoxysilyl group- and amino group-containing compound") is used instead of the (B) amino group-containing compound and the (C) alkoxysilyl group-containing compound, (A) / (B) can be calculated by dividing the amount of the (A) urea component by the amount of the (BC) alkoxysilyl group- and amino group-containing compound.
[0017] When the coating composition of this embodiment is formed into a coating film, two types of bonds are formed: a urea bond formed by the isocyanate group of component (A), and a siloxane bond formed by the silanol group generated from the alkoxysilyl group of component (A) and component (B). When the coating film is formed, the urea bond is formed, which can improve the alkali resistance and surface appearance. When the coating film is formed, the siloxane bond is formed, which can improve the scratch resistance. In addition, the two types of bonds, the urea bond and the siloxane bond, are formed, which can improve the organic solvent resistance. Therefore, according to the coating composition of this embodiment, a coating film excellent in scratch resistance, alkali resistance, organic solvent resistance, and surface appearance can be obtained. Next, each component contained in the coating composition of the present embodiment will be described in detail below.
[0018] <(A) Urea component> The (A) urea component is derived from a polyisocyanate and an aminosilane coupling agent, that is, it contains a urea compound that is a reaction product between a polyisocyanate and an aminosilane coupling agent. The (A) urea component can contain, in addition to the urea compound, an unreacted polyisocyanate and an unreacted aminosilane coupling agent.
[0019] [Urea compound] A urea compound is a compound having one or more urea bonds in one molecule. In general, a urea bond is a bond represented by formula (I). In formula (I), the wavy line represents a bond.
[0020] [ka]
[0021] The urea bond in the urea compound is formed by an addition reaction between an isocyanate group of the polyisocyanate and an amino group of the aminosilane coupling agent.
[0022] Next, the polyisocyanate and the aminosilane coupling agent used in the production of the urea compound will be described in detail below.
[0023] (Polyisocyanate) The polyisocyanate is derived from one or more diisocyanates selected from the group consisting of (a) aliphatic diisocyanates and (b) cycloaliphatic diisocyanates, i.e., the polyisocyanate is a reaction product of the above component (a) and one or more diisocyanates selected from the group consisting of the above component (b).
[0024] In this specification, the term "derivation" includes a prepolymerization reaction of component (a), a prepolymerization reaction of component (b), and a prepolymerization reaction of a mixture of components (a) and (b). Examples of the "prepolymerization reaction" include a reaction to generate a uretdione group by cyclizing dimerization of two isocyanate groups, a reaction to generate an isocyanurate group or an iminooxadiazinedione group by cyclizing trimerization of three isocyanate groups, a reaction to generate a biuret group by reacting three isocyanate groups with one water molecule, a reaction to generate an oxadiazinetrione group by reacting two isocyanate groups with one molecule of carbon dioxide, a reaction to generate a urethane group by reacting one isocyanate group with one hydroxyl group, a reaction to generate an allophanate group by reacting two isocyanate groups with one hydroxyl group, a reaction to generate an acylurea group by reacting one isocyanate group with one carboxyl group, and a reaction to generate a urea group by reacting one isocyanate group with one primary or secondary amine. These can be used alone or in combination of two or more.
[0025] (1) Component (a): Aliphatic diisocyanate Aliphatic diisocyanates are diisocyanate compounds that contain saturated hydrocarbon groups that do not contain a cyclic structure. Polyisocyanates derived from aliphatic diisocyanates tend to have low viscosity. Examples of the aliphatic diisocyanate include 1,4-diisocyanatobutane, 1,5-diisocyanatopentane, ethyl (2,6-diisocyanato)hexanoate, 1,6-diisocyanatohexane (hereinafter sometimes abbreviated as "HDI"), 1,9-diisocyanatononane, 1,12-diisocyanatododecane, 2,2,4- or 2,4,4-trimethyl-1,6-diisocyanatohexane, etc. Among these, as the aliphatic diisocyanate, HDI is particularly preferred because it is easily available industrially and has excellent weather resistance and coating film flexibility.
[0026] (2) Component (b): Alicyclic diisocyanate Alicyclic diisocyanates are diisocyanate compounds that contain one or more saturated hydrocarbon rings. Examples of alicyclic diisocyanates include 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane (hereinafter sometimes abbreviated as "hydrogenated XDI"), 1,3- or 1,4-diisocyanatocyclohexane, 3,5,5-trimethyl-1-isocyanato-3-(isocyanatomethyl)cyclohexane (hereinafter sometimes abbreviated as "IPDI"), 4-4'-diisocyanato-dicyclohexylmethane (hereinafter sometimes abbreviated as "hydrogenated MDI"), and 2,5- or 2,6-diisocyanatomethylnorbornane.
[0027] (Aminosilane coupling agent) The aminosilane coupling agent is a silane coupling agent that contains at least one of a primary amino group and a secondary amino group in the molecule of the silane coupling agent.
[0028] Examples of the aminosilane coupling agent include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-methyl-3-(trimethoxysilyl)propylamine, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, and N-(6-aminohexyl)-3-aminopropyltrimethoxysilane. silane, 3-aminopropyl diethoxymethylsilane, 3-tert-butylaminopropyl trimethoxysilane, 3-cyclohexylaminopropyl trimethoxysilane, N-methyl-3-amino-2-methylpropyl trimethoxysilane, N-ethyl-3-amino-2-methylpropyl methyl dimethoxysilane, N-ethyl-3-amino-2-methylpropyl trimethoxysilane, N-ethyl-3-amino-2-methylpropyl diethoxymethylsilane, N-ethyl-3-amino-2-methylpropyl triethoxysilane ethoxysilane, N-butyl-3-amino-2-methylpropyltrimethoxysilane, 3-(N-methyl-2-amino-1-methyl-1-ethoxy)propyltrimethoxysilane, N-ethyl-4-amino-3,3-dimethylbutyldimethoxymethylsilane, N-ethyl-4-amino-3,3-dimethylbutyltrimethoxysilane, bis-(3-trimethoxysilyl-2-methylpropyl)amine, N-(3-trimethoxysilylpropyl)-3-amino-2-methylpropyltrimethoxysilane, N-phenyl-3-a Aminopropyltrimethoxysilane, 3-trimethoxysilylpropyl-3-[N-(3-trimethoxysilyl)-propylamino]-2-propionic acid methyl ester, 3-triethoxysilylpropyl-3-[N-(3-triethoxysilyl)-propylamino]-2-propionic acid methyl ester, 3-trimethoxysilylpropyl-3-[N-(3-triethoxysilyl)-propylamino]-2-propionic acid methyl ester, N-ethyl-4-amino-3,3-dimethylbutyldimethoxymethylsilane, N-ethyl-4-amino-3,Examples of the aminosilane coupling agent include 3-dimethylbutyltrimethoxysilane, N-(3-trimethoxysilyl)propyl-3-[N-(3-trimethoxysilyl)propylamino]propionamide, N-(3-triethoxysilyl)propyl-3-[N-(3-triethoxysilyl)propylamino]propionamide, N-(3-trimethoxysilyl)propyl-3-[N-(3-triethoxysilyl)propylamino]propionamide, N,N-bis[(3-trimethoxysilyl)propyl]amine, N,N-bis[(3-triethoxysilyl)propyl]amine, N,N-bis[(3-tripropoxysilyl)propyl]amine, and N,N-bis[(3-trimethoxysilyl)-2-methylpropyl]amine. These aminosilane coupling agents may be used alone or in combination of two or more.
[0029] The aminosilane coupling agent may contain, as an organic reactive group other than the amino group, a vinyl group, an epoxy group, a (meth)acrylic group, a mercapto group, an isocyanate group, a ketimine group, a styryl group, or the like.
[0030] (A) Method for producing urea component The (A) urea component is a compound derived from a polyisocyanate derived from one or more diisocyanates selected from the group consisting of aliphatic diisocyanates and alicyclic diisocyanates, and an aminosilane coupling agent. Specifically, the urea component (A) is obtained by reacting the polyisocyanate with the aminosilane coupling agent for 30 minutes to 3 hours at a temperature of about 50° C. to 200° C. The compounding ratio of the polyisocyanate to the aminosilane coupling agent can be, for example, 30 / 70 to 70 / 30 in molar ratio.
[0031] <(B) Compound containing an alkoxysilyl group> The (B) compound containing an alkoxysilyl group (hereinafter, sometimes abbreviated as "(B) alkoxysilyl group-containing compound") is a monomer, oligomer, or polymer having a Si-OR group in the molecule. Here, "R" in Si-OR is a hydrocarbon group, and is preferably an alkyl group, an aryl group, a vinyl group, or a styryl group. Examples of such (B) alkoxysilyl group-containing compounds include tetramethoxysilane, trimethoxymethylsilane, dimethyldimethoxysilane, methoxytrimethylsilane, tetraethoxysilane, triethoxymethylsilane, diethoxydimethylsilane, ethoxytrimethylsilane, triethoxyphenylsilane, diethoxymethylphenylsilane, ethenyltriethoxysilane, triethoxyphenylvinylsilane, 1,4,6,9-tetraoxa-5-silaspiro[4,4]nonane, and 3-glycidoxypropyltriethoxysilane. These (B) alkoxysilyl group-containing compounds may be used alone or in combination of two or more.
[0032] <(C) Compound containing an amino group> Examples of the (C) compound containing an amino group (hereinafter sometimes abbreviated as "(C) amino group-containing compound") include primary amines, secondary amines, and tertiary amines. As the (C) amino group-containing compound, amines having a high boiling point are preferred in order to prevent scattering during the curing process. Examples of such (C) amino group-containing compounds include tripropylamine, N,N-diisopropylethylamine, diisopropylamine, normal butylamine, diphenylamine, aniline, carbazole, di-n-propylamine, isopropylethylamine, piperidine, and piperazine. These (C) amino group-containing compounds may be used alone or in combination of two or more. The (C) amino group-containing compound may have an alkyl group, an aryl group, a thiol group, a silyl group, an alkoxy group, or the like in the molecule. Also, a polyamine having a plurality of amino groups in one molecule may be used.
[0033] <(BC) Compounds containing an amino group and an alkoxysilyl group> The coating composition of this embodiment preferably contains (BC) a compound containing an alkoxysilyl group and an amino group in the same molecule (hereinafter sometimes abbreviated as "(BC) alkoxysilyl group- and amino group-containing compound") instead of (B) the amino group-containing compound and (C) the alkoxysilyl group-containing compound. In addition, in the (BC) alkoxysilyl group- and amino group-containing compound, the amino group is preferably a tertiary amino group, since this makes it easier to adjust the reaction rates of the hydrolysis reaction from alkoxysilane to silanol and the dehydration condensation reaction between silanols. (BC) Examples of the alkoxysilyl group- and amino group-containing compounds include N,N-dimethyl-3-(trimethoxysilyl)propylamine ([3-(N,N-dimethylamino)propyl]trimethoxysilane), N,N-dimethyl-3-(triethoxysilyl)propylamine, N,N-dimethyl-3-(tripropoxysilyl)propylamine, N,N-dimethyl-3-(tributoxysilyl)propylamine, N,N-diethyl-3-(trimethoxysilyl)propylamine, N,N-diethyl-3-(triethoxysilyl)propylamine, N,N-diethyl-3-(trippropoxysilyl)propylamine, N,N -diethyl-3-(tributoxysilyl)propylamine, N,N-dipropyl-3-(trimethoxysilyl)propylamine, N,N-dipropyl-3-(triethoxysilyl)propylamine, N,N-dipropyl-3-(tripropoxysilyl)propylamine, N,N-dipropyl-3-(tributoxysilyl)propylamine, N,N-dibutyl-3-(trimethoxysilyl)propylamine, N,N-dibutyl-3-(triethoxysilyl)propylamine, N,N-dibutyl-3-(tripropoxysilyl)propylamine, N,N-dibutyl-3-(tributoxysilyl)propylamine, etc. These (BC) alkoxysilyl group- and amino group-containing compounds may be used alone or in combination of two or more.
[0034] <(D) Organic solvent> The coating composition of this embodiment may contain (D) an organic solvent in addition to the above components (A) to (C). By containing an organic solvent, the coating composition of this embodiment has a lower viscosity and therefore improved handleability.
[0035] The organic solvent may be any solvent that does not have a functional group that reacts with an isocyanate group or a urea bond and is compatible with the coating composition of this embodiment. Examples of such organic solvents include ester compounds, ether compounds, ketone compounds, aromatic compounds, polyethylene glycol dialkyl ether compounds, and polyethylene glycol dicarboxylate compounds. Examples of ester compounds include butyl acetate, isobutyl acetate, pentyl acetate, methoxypropyl acetate, 3-methoxybutyl acetate, 2-ethylbutyl acetate, 2-ethylhexyl acetate, cyclohexyl acetate, butyl propionate, butyl butyrate, dioctyl adipate, and diisopropyl glutarate. Examples of ether compounds include diisopropyl ether, dibutyl ether, dioxane, and diethoxyethane. Examples of ketone compounds include 2-pentanone, 3-pentanone, 2-hexanone, methyl isobutyl ketone, 2-heptanone, 4-heptanone, diisobutyl ketone, isophorone, cyclohexanone, and methylcyclohexanone. Examples of aromatic compounds include benzene, toluene, xylene, ethylbenzene, butylbenzene, p-cymene, etc. Examples of polyethylene glycol dialkyl ether compounds include diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, diethylene glycol dibutyl ether, etc. Examples of polyethylene glycol dicarboxylate compounds include diethylene glycol diacetate, etc.
[0036] <(E) Paint Additives> In addition to the above components (A) to (D), the coating composition of this embodiment may contain various known and commonly used (E) coating additives. Examples of coating additives include thickeners, leveling agents, thixotropic agents, defoamers, freeze stabilizers, matting agents, crosslinking reaction catalysts, antiskinning agents, dispersants, wetting agents, light stabilizers, antioxidants, UV absorbers, fillers, plasticizers, lubricants, reducing agents, preservatives, antifungal agents, deodorants, yellowing inhibitors, antistatic agents, and charge regulators. These additives can be appropriately selected and used within a range that does not impair the effects of the coating composition of this embodiment. In particular, known compounds can be used as crosslinking reaction catalysts, and it is advantageous in terms of reaction to use a metal complex having a chelating ligand. The compound that forms the chelating ligand is an organic compound having at least two functional groups that can be coordinated to a metal atom or metal ion. These functional groups are electron donors that provide electrons to a metal atom or metal ion as an electron acceptor. Essentially, any organic compound can be used as long as it does not negatively affect or prevent the coating composition from crosslinking to a cured product upon curing of the coating composition.
[0037] Examples of the metal include one or more metals selected from the group consisting of the 3rd to 4th main groups, the 3rd to 6th subgroups, the 1st subgroup, the 2nd subgroup, and the lanthanoids of the periodic table of the elements. Among them, one or more metals selected from the group consisting of boron, aluminum, gallium, silicon, germanium, tin, zinc, titanium, zirconium, hafnium, vanadium, niobium, tantalum, molybdenum, tungsten, and cerium are preferred, and one or more metals selected from the group consisting of aluminum, silicon, titanium, and zirconium are more preferred.
[0038] Examples of the metal compound include oxides, oxide hydrates, sulfates, hydroxides, and phosphates, with oxides, oxide hydrates, and hydroxides being preferred.
[0039] As the catalyst, for example, a chelate complex of tin and zirconium can be used as the catalyst. Among them, a chelate of one or more metals selected from the group consisting of tin, aluminum, zirconium, titanium and boron is preferred. Specific examples of such metal chelates include dibutyltin dilaurate, aluminum methyl-acetoacetate, zirconium ethylacetoacetate, etc., and among them, an alcoholate or ester of one or more metals selected from the group consisting of tin, aluminum, zirconium, titanium and boron is preferred. More specific examples of the catalyst include tin naphthenate, tin benzoate, tin octanoate, tin butyrate, dibutyltin dilaurate, dibutyltin diacetate, dibutyltin oxide, lead octanoate, etc.
[0040] <Method of producing coating composition> The coating composition of this embodiment is a moisture-curing coating composition that can be cured by the action of moisture in the air without blending a resin component as a main component. Therefore, for example, the above-mentioned component (B) and the above-mentioned component (C), or the above-mentioned component (BC), and (E) a coating additive as necessary, are added to the above-mentioned component (A) or its solvent dilution. Then, as necessary, (D) an organic solvent is further added to adjust the viscosity. Then, the coating composition can be obtained by stirring by hand or using a stirring device such as a mixer.
[0041] <Usage> The coating composition of this embodiment has excellent adhesion to substrates such as metals, plastics, and old coatings. In addition, coatings obtained from the coating composition of this embodiment are less likely to develop blisters (swelling of coatings) when immersed in water. Therefore, the coating composition of this embodiment can be used as a raw material for coatings for metal parts, coatings for plastic parts, inks, adhesives, sealants, elastomers, films, foams, plastic materials, and the like. In particular, the coating composition of this embodiment is suitable for coatings for metal parts, coatings for plastic parts, sealants, adhesives, or films.
[0042] <Film> The film of this embodiment is formed by curing the above-mentioned coating composition. As described above, the film of this embodiment has two types of bonds: a urea bond formed by the isocyanate group of component (A), and a siloxane bond formed by the silanol group generated from the alkoxysilyl group of component (A) and component (B). By having the urea bond, it is possible to improve the alkali resistance. By having the siloxane bond, it is possible to improve the scratch resistance. In addition, by having two types of bonds, the urea bond and the siloxane bond, it is possible to improve the organic solvent resistance. Therefore, the film of this embodiment is excellent in scratch resistance, alkali resistance, organic solvent resistance, and surface appearance.
[0043] The film of this embodiment can be obtained by applying the coating composition to a substrate or the like, curing the composition at room temperature of about 20° C. to 30° C., and heating the composition at 50° C. to 150° C. Specifically, the alkoxysilyl groups of the aminosilane coupling agent in the coating composition react with each other due to moisture in the air to become silanol groups, which then cure by forming siloxane bonds, while the isocyanates react with each other with moisture in the air to form urea bonds, and the isocyanates react with partially eliminated alcohols to form urethane bonds, thereby obtaining a film.
[0044] Examples of the coating method include known methods such as reverse roll coating, gravure coating, kiss coating, die coater, roll brush, spray coating, air knife coating, wire bar coating, pipe doctor method, impregnation coating, curtain coating, roll coating, curtain flow coating, spray coating, bell coating, and electrostatic coating.
[0045] The thickness of the film is not particularly limited, but is preferably from 0.2 μm to 500 μm, more preferably from 1 μm to 500 μm, further preferably from 5 μm to 300 μm, and particularly preferably from 5 μm to 100 μm. EXAMPLES
[0046] The present embodiment will be described in more detail below with reference to specific examples and comparative examples. However, the present embodiment is not limited in any way by the following examples and comparative examples as long as the gist of the present embodiment is not exceeded.
[0047] <Methods for measuring and evaluating the physical properties of coating compositions> [Physical Properties 1] (Isocyanate group content (NCO%)) The urea component obtained in the synthesis example (before dilution with a solvent): 1 g or more and 3 g or less was precisely weighed (Wg). Next, 20 mL of toluene was added to the urea component and dissolved. Next, 10 mL of a 2N toluene solution of di-n-butylamine was added to the toluene solution containing the urea component, and after mixing, the mixture was left at room temperature for 15 minutes. Next, 70 mL of isopropyl alcohol was added to this mixture and mixed. This liquid was titrated with a 1N hydrochloric acid solution (factor F) as an indicator, and the titration value obtained was designated as "V2mL". The same operation was performed without the urea component, and the titration value obtained was designated as "V1mL". Using these titration values, the isocyanate group content (NCO%) relative to the solid content in the urea component was calculated from the following formula. The solid content of the urea component obtained in the synthesis example was examined by the method described below, and those whose value was 98 mass% or more were directly subjected to measurement. On the other hand, for those with a solid content of less than 98% by mass, the value obtained by multiplying Wg by the proportion of solid content was introduced into the following formula to calculate the isocyanate group content relative to the solid content in the urea component.
[0048] Isocyanate group content (mass%) = (V1-V2) x F x 42 / (W x 1000) x 100
[0049] [Physical Properties 2] (Solids) When the urea component obtained in the synthesis example was used as a sample and diluted with a solvent, the mass of an aluminum cup was precisely weighed (W0g). Approximately 1 g of sample was placed in the cup, and the mass of the cup before drying by heating was precisely weighed (W1g). The cup containing the sample was heated in a dryer at 105°C for 3 hours. After the cup was cooled to room temperature after heating, the mass of the cup was precisely weighed again (W2g). Using the precisely weighed masses, the mass % of the dry residue in the sample was calculated as solids using the following formula.
[0050] Solid content (mass%)=(W2-W0) / (W1-W0)×100
[0051] [Physical Properties 3] ((A) / (B)) The mass ratio (A) / (B) was calculated by dividing the blend amount of the urea component (A) by the blend amount of the compound containing at least one alkoxysilyl group (B).
[0052] [Preparation of coating film] The coating compositions obtained in the examples and comparative examples were applied to a thickness of approximately 30 μm to 40 μm, dried for one day in an atmosphere of 23°C / 50% RH, and then baked at 120°C for one hour to obtain a coating film.
[0053] [Rating 1] (Scratch resistance) The coating compositions obtained in the Examples and Comparative Examples were applied to an electrodeposited plate to a thickness of about 30 μm to 40 μm, dried for one day in an atmosphere of 23° C. / 50% RH, and then baked for one hour at 120° C. to obtain a coating film. The obtained coating film was rubbed back and forth 20 times with a brass brush bearing a load of 1 kg, and the gloss retention of the coating film surface before and after rubbing was calculated in %, and the scratch resistance was evaluated according to the following evaluation criteria.
[0054] (Evaluation Criteria) ◎: 95% or more ○: Less than 95% 90% or more ×: Less than 90%
[0055] [Rating 2] (Alkaline resistance) The coating compositions obtained in the examples and comparative examples were applied to a glass plate to a thickness of 30 μm to 40 μm, dried for one day under an atmosphere of 23° C. / 50% RH, and then baked at 120° C. for one hour to obtain a coating film. A rubber ring was placed on the obtained coating film, and a 10% by mass aqueous solution of sodium hydroxide was dropped onto the center portion. After immersion at 23° C. for 24 hours, the alkali resistance was evaluated according to the following evaluation criteria based on the state of blisters formed between the glass substrate and the coating film.
[0056] (Evaluation Criteria) ○: No change in appearance ×: Cloudiness, dissolution, or blister swelling.
[0057] [Rating 3] (Organic solvent resistance) The coating compositions obtained in the examples and comparative examples were applied to a glass plate to a thickness of 30 μm to 40 μm, dried for one day under an atmosphere of 23° C. / 50% RH, and then baked at 120° C. for one hour to obtain a coating film. Cotton moistened with xylene or ethanol was placed on the obtained coating film. Organic solvent resistance was evaluated according to the following evaluation criteria from the state of the coating film appearance after leaving it in xylene for 10 minutes or ethanol for 5 minutes at 23° C.
[0058] (Evaluation Criteria) ○: No traces of either xylene or ethanol △: Whitening, swelling, or elution in either xylene or ethanol ×: Whitening, swelling, and elution occurred in both xylene and ethanol.
[0059] [Rating 4] (Surface appearance) The coating compositions obtained in the Examples and Comparative Examples were applied to a glass plate to a thickness of about 30 μm to 40 μm, dried for one day in an atmosphere of 23° C. / 50% RH, and then baked for one hour at 120° C. to obtain a coating film. The obtained coating film was visually observed and the surface appearance was evaluated according to the following evaluation criteria.
[0060] (Evaluation Criteria) ◎: Smooth, colorless, transparent film ○: Colorless and transparent film with unevenness in some areas ×: Film with uniform unevenness, or whitening or bumps ××: No film formed
[0061] <(A) Synthesis of urea component> The urea component (A) used in the examples and comparative examples was produced according to the following synthesis procedure.
[0062] [Synthesis Example 1] (Synthesis of urea component P-a1) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 40.9 parts by mass of HDI isocyanurate type polyisocyanate (Duranate TPA-100, manufactured by Asahi Kasei Corporation) (hereinafter, sometimes referred to as "polyisocyanate A-1") was added, and 19.1 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Kasei Co., Ltd.) was added dropwise while stirring, and the mixture was stirred at 60°C for 1 hour to carry out a urea reaction. The isocyanate group content relative to the solid content in the obtained urea component was 11.8% by mass. Then, 40.0 parts by mass of butyl acetate was mixed to obtain a homogeneous solution. The obtained homogeneous solution of the urea component was a pale yellow liquid, and the solid content was 60% by mass.
[0063] [Synthesis Example 2] (Synthesis of urea component P-a2) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 54.9 parts by mass of polyisocyanate A-1 was added, and 5.1 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise while stirring, and the mixture was stirred at 60°C for 1 hour to carry out a urea reaction. The isocyanate group content relative to the solid content in the obtained urea component was 20.0% by mass. Then, 40.0 parts by mass of butyl acetate was mixed to obtain a homogeneous solution. The obtained homogeneous solution of the urea component was a pale yellow liquid, and the solid content was 60% by mass.
[0064] [Synthesis Example 3] (Synthesis of urea component P-a3) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 50.5 parts by mass of polyisocyanate A-1 was added, and 9.5 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise while stirring, and the mixture was stirred at 60°C for 1 hour to carry out a urea reaction. The isocyanate group content relative to the solid content in the obtained urea component was 17.4% by mass. Then, 40.0 parts by mass of butyl acetate was mixed to obtain a homogeneous solution. The obtained homogeneous solution of the urea component was a pale yellow liquid, and the solid content was 60% by mass.
[0065] [Synthesis Example 4] (Synthesis of urea component P-a4) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 43.4 parts by mass of HDI biuret type polyisocyanate (Duranate 24A-100, manufactured by Asahi Kasei Corporation) (hereinafter, sometimes referred to as "polyisocyanate A-2") was added, and 16.6 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Kasei Co., Ltd.) was added dropwise while stirring, and the mixture was stirred at 60°C for 1 hour to carry out a urea reaction. The isocyanate group content relative to the solid content in the obtained urea component was 13.6% by mass. Then, 40.0 parts by mass of butyl acetate was mixed to obtain a homogeneous solution. The obtained homogeneous solution of the urea component was a pale yellow liquid, and the solid content was 60% by mass.
[0066] [Synthesis Example 5] (Synthesis of urea component P-a5) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 52.3 parts by mass of HDI elastic adduct type polyisocyanate (Duranate E402-100, manufactured by Asahi Kasei Corporation) (hereinafter, sometimes referred to as "polyisocyanate A-3") was added, and 7.7 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Kasei Co., Ltd.) was dropped while stirring, and the mixture was stirred at 60 ° C for 1 hour to perform a urea reaction. After that, 40.0 parts by mass of butyl acetate was mixed, and then the mixture and urea component P-a1 were mixed in a mass ratio of 20:80 to obtain a homogeneous solution. The isocyanate group content relative to the solid content in the obtained homogeneous solution of the urea component was 9.1% by mass. The obtained homogeneous solution of the urea component was a pale yellow liquid, and the solid content was 60% by mass.
[0067] [Synthesis Example 6] (Synthesis of urea component P-a6) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 46.3 parts by mass of HDI multifunctional polyisocyanate (Duranate MFA-100, manufactured by Asahi Kasei Corporation) (hereinafter, sometimes referred to as "polyisocyanate A-4") was added, and 13.7 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Kasei Co., Ltd.) was added dropwise while stirring, and the mixture was stirred at 60°C for 1 hour to carry out a urea reaction. The isocyanate group content relative to the solid content in the obtained urea component was 11.2% by mass. Then, 40.0 parts by mass of butyl acetate was mixed to obtain a homogeneous solution. The obtained homogeneous solution of the urea component was a pale yellow liquid, and the solid content was 60% by mass.
[0068] [Synthesis Example 7] (Synthesis of urea component P-a7) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 31.8 parts by mass of polyisocyanate A-4 was added, 28.2 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise while stirring, and the mixture was stirred at 60°C for 1 hour to carry out a urea reaction. The isocyanate group content relative to the solid content in the obtained urea component was 4.0% by mass. Then, 40.0 parts by mass of butyl acetate was mixed to obtain a homogeneous solution. The obtained homogeneous solution of the urea component was a pale yellow liquid, and the solid content was 60% by mass.
[0069] [Synthesis Example 8] (Synthesis of urea component P-b1) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 25.0 parts by mass of polyisocyanate A-1 was added, and 35.0 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise while stirring, and the mixture was stirred at 60°C for 1 hour to carry out a urea reaction. The isocyanate group content relative to the solid content in the obtained urea component was 2.4% by mass. Then, 40.0 parts by mass of butyl acetate was mixed to obtain a homogeneous solution. The obtained homogeneous solution of the urea component was a pale yellow liquid with a solid content of 60% by mass.
[0070] [Synthesis Example 9] (Synthesis of urea component P-b2) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 57.8 parts by mass of polyisocyanate A-1 was added, and 2.2 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise while stirring, and the mixture was stirred at 60°C for 1 hour to carry out a urea reaction. The isocyanate group content relative to the solid content in the obtained urea component was 21.7% by mass. Then, 40.0 parts by mass of butyl acetate was mixed to obtain a homogeneous solution. The obtained homogeneous solution of the urea component was a pale yellow liquid, and the solid content was 60% by mass.
[0071] [Synthesis Example 10] (Synthesis of urea component P-b3) The inside of a four-neck flask equipped with a stirrer, a thermometer, and a cooling tube was replaced with nitrogen, 20.9 parts by mass of polyisocyanate A-1 was added, and 39.1 parts by mass of N,N-bis[(3-trimethoxysilyl)propyl]amine (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise while stirring, and the mixture was stirred at 60°C for 1 hour to carry out a urea reaction. The isocyanate group content relative to the solid content in the obtained urea component was 0% by mass. Then, 40.0 parts by mass of butyl acetate was mixed to obtain a homogeneous solution. The obtained homogeneous solution of the urea component was a pale yellow liquid, and the solid content was 60% by mass.
[0072] The compositions and physical property measurement results of the urea components (A) obtained in Synthesis Examples 1 to 10 are shown in Table 1.
[0073] [Table 1]
[0074] <Production of Coating Composition> [Examples 1 to 10 and Comparative Examples 1 to 6] (Production of Coating Compositions S-a1 to S-a10 and S-b1 to S-b6) Coating compositions S-a1 to S-a10 and S-b1 to S-b6 with a solid content of 50 mass% were produced by blending various components so as to obtain the compositions shown in Tables 2 and 3. In Comparative Example 4, the polyol was blended immediately before the production of the coating film.
[0075] In Tables 2 and 3, the details of each component are as follows. ((B) Alkoxysilyl Group-Containing Compound) B-1: 3-glycidoxypropyltriethoxysilane
[0076] ((C) Amine Group-Containing Compound) C-1: N,N-diisopropylethylamine
[0077] ((BC) Alkoxysilyl Group and Amine Group-Containing Compounds) BC-1: [3-(N,N-dimethylamino)propyl]trimethoxysilane
[0078] ((D) Organic Solvent) D-1: Butyl acetate
[0079] ((E) Paint Additives) E-1: Dibutyltin dilaurate (Neostan U-100, manufactured by Nitto Kasei Co., Ltd.)
[0080] (Polyol) Setalux1767 (Allnex)
[0081] The evaluation results of the coating films using each coating composition are shown in Tables 2 and 3.
[0082] [Table 2]
[0083] [Table 3]
[0084] As can be seen from Tables 2 and 3, the coating compositions S-a1 to S-a10 (Examples 1 to 10), which contained a urea component (A) with an isocyanate group content of 4% by mass or more and 20% by mass or less and had an (A) / (B) ratio of 50 / 50 or more and 94.3 / 5.7 or less, were all good in terms of scratch resistance, alkali resistance, organic solvent resistance, and surface appearance when formed into coating films. Furthermore, paint composition S-a1 (Example 1) containing component (BC) tended to have better scratch resistance when formed into a coating film than paint composition S-a3 (Example 3) containing components (B) and (C).
[0085] On the other hand, in the coating compositions S-b1 and S-b3 (Comparative Examples 1 and 3) which contained a urea component (A) with an isocyanate group content of less than 4 mass% and in which the (A) / (B) ratio was 76.9 / 23.1, the coating films had good scratch resistance, organic solvent resistance, and surface appearance, but the coating films had poor alkali resistance. In addition, in the coating composition S-b2 (Comparative Example 2) containing a urea component (A) with an isocyanate group content of more than 20 mass% and with an (A) / (B) ratio of 76.9 / 23.1, the scratch resistance, alkali resistance, organic solvent resistance and surface appearance of the coating film were all poor. In addition, in the coating compositions S-b4 and S-b5 (Comparative Examples 4 and 5) containing a urea component (A) with an isocyanate group content of 11.8 mass% and in which the (A) / (B) ratio was greater than 95 / 5, the coating films formed had good alkali resistance and surface appearance, but the scratch resistance and organic solvent resistance of the coating films formed were poor. In addition, in the coating composition S-b6 (Comparative Example 6) containing urea component (A) with an isocyanate group content of 17.4 mass% and in which (A) / (B) was less than 50 / 50, the coating film had good scratch resistance, but the coating film had poor alkali resistance, organic solvent resistance, and surface appearance. [Industrial Applicability]
[0086] According to the coating composition of the present embodiment, it is possible to provide a coating composition which, when formed into a coating film, has excellent abrasion resistance, alkali resistance, organic solvent resistance, and surface appearance. The film of the present embodiment is obtained by curing the coating composition, and has excellent abrasion resistance, alkali resistance, organic solvent resistance, and surface appearance.
Claims
1. Contains the following components (A) and (BC), (A) a urea component derived from a polyisocyanate derived from one or more diisocyanates selected from the group consisting of aliphatic diisocyanates and alicyclic diisocyanates, and an aminosilane coupling agent; (BC) A compound having an alkoxysilyl group and a tertiary amino group in the same molecule (excluding urea compounds); The content of isocyanate groups relative to the mass of the solid content of the component (A) is 4% by mass or more and 20% by mass or less, A coating composition, wherein the mass ratio (A) / (BC) of the component (A) to the component (BC) is 50 / 50 or more and 95 / 5 or less.
2. The coating composition of claim 1 further comprising an organic solvent.
3. A film obtained by curing the coating composition according to claim 1 or 2.
Citation Information
Patent Citations
Primer composition
JP1990145660A
Hybrid paint composition
JP2000169793A
Nonaqueous thermosetting 2k coating agent
JP2003041188A
Primer composition for sealing material
JP2007070571A
Paint, and a coating film formed from said paint having high scratch resistance, weather resistance, and good optical properties.
JP2012511058A