Adhesive Composition

Adhesive compositions using an aqueous polyacid polymer dispersion and hydroxyl group-containing acrylic emulsion address the performance gap of formaldehyde-free binders by providing superior wet and solvent resistance, maintaining stability over time.

JP7572430B2Active Publication Date: 2024-10-23ROHM & HAAS CO
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022525102
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-11-13
Publication Date
2024-10-23
Estimated Expiration
2039-11-13

AI Technical Summary

Technical Problem

Conventional binders used in textiles and nonwovens that contain N-methylolacrylamide (NMA) provide excellent water and solvent resistance but release formaldehyde when heated, while formaldehyde-free crosslinking technologies do not match the performance of NMA-containing binders.

Method used

Adhesive compositions comprising an aqueous polyacid polymer dispersion and a hydroxyl group-containing acrylic emulsion, free of NMA, with a moderate curing temperature, achieving superior wet and solvent resistance.

Benefits of technology

The adhesive compositions exhibit excellent wet strength and solvent resistance, maintaining performance after 30 days of accelerated heat aging, and are suitable for one-component formulations with good storage stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572430000001
    Figure 0007572430000001
  • Figure 0007572430000002
    Figure 0007572430000002
Patent Text Reader

Abstract

An adhesive composition is provided, comprising the following components: (a) an aqueous polyacid polymer dispersion, the polyacid polymer containing 50% to 100% by weight of one or more ethylenically unsaturated mono- or dicarboxylic acids / anhydrides, and (b) a hydroxyl group-containing acrylic copolymer emulsion, the hydroxyl group-containing acrylic copolymer being obtained by polymerizing a monomer mixture containing 0.1 to 10% of a hydroxyl group-containing monomer, 0.1 to 20% by weight of an unsaturated carboxylic acid, and 30 to 90% of an acrylic monomer, wherein the solids weight ratio of components (a) to (b) is 0.1:100 to 10:100, based on the solids of components (a) and (b).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to adhesive compositions, and in particular to adhesive compositions comprising an aqueous dispersion of a polyacid polymer and an acrylic emulsion. [Background technology]

[0002] Traditional binders used in textile and nonwoven applications contain N-methylol acrylamide (NMA) as a functional monomer to provide excellent water (wet strength) and solvent resistance (isopropyl alcohol strength). However, NMA-containing binders release formaldehyde when heated.

[0003] Recently, there have been many research achievements on formaldehyde-free crosslinking technologies, which have achieved excellent water and solvent resistance after curing, but are still not competitive with NMA-containing binders.

[0004] It is expected that new formulations with moderate curing temperatures will be developed to achieve better performance. Summary of the Invention

[0005] The present disclosure provides adhesive compositions, particularly those free of NMA monomers, that have moderate cure temperatures to achieve better performance.

[0006] In a first aspect of the present disclosure, the present disclosure provides a method for the preparation of a composition comprising the following components: (a) an aqueous dispersion of a polyacid polymer, the polyacid polymer containing 50% to 100% by weight of one or more ethylenically unsaturated mono- or dicarboxylic acids / anhydrides; (b) an adhesive composition comprising a hydroxyl group-containing acrylic copolymer emulsion, the hydroxyl group-containing acrylic copolymer being obtained by polymerizing a monomer mixture containing 0.1-10% of a hydroxyl group-containing monomer, 0.1%-20% by weight of an unsaturated carboxylic acid, and 30%-90% of an acrylic monomer; The adhesive composition is provided in which the solids weight ratio of the components (a) and (b) is 0.1:100 to 10:100 based on the solids of the components (a) and (b).

[0007] In a second aspect of the present disclosure, the present disclosure provides an article prepared with an adhesive composition according to the present disclosure.

[0008] In a third aspect of the present disclosure, the present disclosure provides the use of the adhesive composition of the present disclosure for textile / nonwoven fabrics.

[0009] In the present disclosure, polyacid polymer aqueous dispersions can be introduced into hydroxyl-containing acrylic binder systems and cured into networks to provide excellent performance. At 150°C, the self-crosslinking systems showed excellent wet and IPA strength. The formulations according to the present disclosure show very good storage stability. After 30 days of accelerated heat aging in an oven at 50°C, there was no degradation in performance. Thus, the formulations according to the present disclosure are one-component formulations and may be easily handled.

[0010] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention, as claimed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs, and all publications, patent applications, patents, and other references mentioned herein are incorporated by reference.

[0012] As disclosed herein, "and / or" means "and, or alternatively." All ranges are inclusive of their endpoints unless otherwise stated.

[0013] As disclosed herein, the terms "composition," "formulation," or "mixture" refer to a physical blend of different components obtained by simply mixing the different components by physical means.

[0014] As disclosed herein, the term "glass transition temperature" or "Tg" is determined by differential scanning calorimetry (DSC).

[0015] As disclosed herein, all percentages referred to herein are by weight and by temperature in °C unless otherwise specified.

[0016] As disclosed herein, the term "alkyl" or "alkoxy" refers to an alkyl or alkoxy having 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 8 carbon atoms.

[0017] As used herein, the term "(meth)acrylate" refers to an acrylate or a methacrylate.

[0018] As used herein, the term "styrene monomer" means an ethylenically unsaturated monomer substituted with an aromatic group, preferably styrene (Sty) and substituted styrenes, such as alpha-methylstyrene (AMS).

[0019] As used herein, the term "solution" refers to a dispersion of a water-insoluble polymer, which may be prepared by conventional polymerization techniques such as, for example, solution polymerization.

[0020] As used herein, the terms "emulsion," "latex," or "latex composition" refer to a dispersion of water-insoluble polymers that may be prepared by conventional polymerization techniques such as, for example, emulsion polymerization.

[0021] In a first aspect of the present disclosure, the present disclosure provides a method for the preparation of a composition comprising the following components: (a) an aqueous dispersion of a polyacid polymer, the polyacid polymer containing 50% to 100% by weight of one or more ethylenically unsaturated mono- or dicarboxylic acids / anhydrides; (b) an adhesive composition comprising a hydroxyl group-containing acrylic copolymer emulsion, the hydroxyl group-containing acrylic copolymer being obtained by polymerizing a monomer mixture containing 0.1-10% of a hydroxyl group-containing monomer, 0.1%-20% by weight of an unsaturated carboxylic acid, and 30%-90% of an acrylic monomer; The adhesive composition is provided in which the solids weight ratio of the components (a) and (b) is 0.1:100 to 10:100 based on the solids of the components (a) and (b).

[0022] The adhesive composition is aqueous and preferably free of organic solvents, i.e., the adhesive composition contains less than 4%, preferably less than 2%, more preferably less than 1% organic solvent based on the total dry weight of the adhesive composition.

[0023] Polyacid polymer aqueous dispersion The polyacid polymer contains 50% to 100% by weight, preferably 60% to 100% by weight, more preferably 70% to 100% by weight, most preferably 80% to 100% by weight of one or more ethylenically unsaturated mono- or dicarboxylic acids / anhydrides. Suitable ethylenically unsaturated mono- or dicarboxylic acids / anhydrides include, for example, ethylenically unsaturated carboxylic acid monomers such as methacrylic acid, acrylic acid, crotonic acid, fumaric acid, maleic acid, 2-methylmaleic acid, itaconic acid, 2-methylitaconic acid, α,β-methylene glutaric acid, monoalkyl maleates, and monoalkyl fumarates, and ethylenically unsaturated anhydrides such as maleic anhydride, itaconic anhydride, acrylic anhydride, and methacrylic anhydride, and salts thereof. In a preferred embodiment of the present disclosure, the carboxy monomer can be acrylic acid or methacrylic acid or itaconic acid / anhydride or maleic acid / anhydride.

[0024] One or more ethylenically unsaturated mono- or di-carboxylic acids / anhydrides may be copolymerized with any suitable monomer. In one embodiment of the present disclosure, one or more ethylenically unsaturated mono- or di-carboxylic acids / anhydrides are copolymerized with at least one ethylynically unsaturated monomer, such as an acrylic ester monomer. Suitable acrylic ester monomers include, for example, methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, decyl acrylate, methyl methacrylate, butyl methacrylate, isodecyl methacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate; (meth)acrylamide or substituted (meth)acrylamide; styrene or substituted styrene; butadiene; vinyl acetate or other vinyl ester; acrylonitrile or methacrylonitrile; and the like.

[0025] The polyacid polymer contains 0% to 50% by weight, preferably 0% to 40% by weight, more preferably 0% to 30% by weight, and most preferably 0% to 20% by weight of at least one ethylenically unsaturated monomer.

[0026] The polyacid polymer aqueous dispersion has a total weight solids content of 40% or more, preferably 40% to 60%, and more preferably 45% to 55%.

[0027] In one embodiment, the polyacid polymer has a weight average molecular weight of 2,000 to 1,000,000, preferably 5,000 to 750,000, and most preferably 10,000 to 600,000.

[0028] The polyacid polymer aqueous dispersions can be made by any conventional solution polymerization process, the solution processes of which are well known to those skilled in the art.

[0029] During the solution polymerization process, chain transfer agents such as mercaptans, polymercaptans, and halogen compounds may be used in the polymerization mixture to moderate the molecular weight of the polyacid polymer. Generally, 0% to 10% by weight of C4-C 20 Alkyl mercaptans, mercaptopropionic acid, or esters of mercaptopropionic acid can be used.

[0030] Hydroxyl-containing acrylic copolymer emulsion The hydroxyl group-containing acrylic copolymer emulsion is a latex, which is an aqueous dispersion of particles of a polymer of an ethylenically unsaturated monomer. The hydroxyl group-containing acrylic copolymer is obtained from polymerizing a monomer mixture containing 0.1-10% of a hydroxyl group-containing monomer, 0.1-20% by weight of an unsaturated carboxylic acid, and 30-90% of an acrylic monomer. The latex will typically exhibit a viscosity in the range of about 10-1000 cps at 25°C, more preferably 20-500 cps at 25°C. The solids content in the latex may range from 5-95%. More preferably, it is in the range of 20-80%, even more preferably 30-70%, and even more preferably, it is in the range of 40-60%. In one embodiment, the polymer of the latex has a weight average molecular weight of 5000-2,000,000, more preferably 100,000-2,000,000.

[0031] In one embodiment, suitable examples of hydroxyl group-containing monomers include, but are not limited to, hydroxyalkyl (meth)acrylates, preferably C2-C8 hydroxyalkyl (meth)acrylates, preferably C2-C4 hydroxyalkyl (meth)acrylates, preferably C2-C3 hydroxyalkyl (meth)acrylates. In a further embodiment, the hydroxyl group-containing monomers include hydroxyethyl methacrylate (HEMA), hydroxyethyl acrylate (HEA), hydroxypropyl methacrylate (HPMA) and hydroxypropyl acrylate.

[0032] The monomer mixture contains 0.1 to 10%, preferably 0.5 to 8%, more preferably 0.5 to 5%, and most preferably 0.5 to 2% of a hydroxyl group-containing monomer, based on the weight of the monomer mixture.

[0033] In one embodiment, the unsaturated carboxylic acid comprises one or more α,β-ethylenically unsaturated carboxylic acids. Suitable examples of α,β-ethylenically unsaturated carboxylic acids include, but are not limited to, acid-bearing monomers such as (meth)acrylic acid, itaconic acid, or fumaric acid, or monomers having acid-forming groups that generate or can be subsequently converted into such acid groups (anhydrides, such as (meth)acrylic anhydride, or maleic anhydride), or mixtures thereof.

[0034] The monomer mixture contains from 0.1 to 20%, preferably from 1 to 15%, more preferably from 1.5 to 10%, and most preferably from 1.5 to 8% of the unsaturated carboxylic acid, based on the weight of the monomer mixture.

[0035] In one embodiment, suitable examples of acrylic monomers include (meth)acrylates, such as, but not limited to, alkyl (meth)acrylates, such as, but not limited to, methyl acrylate, ethyl acrylate, butyl acrylate, glycidyl methacrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate, and combinations thereof.

[0036] The monomer mixture comprises 30-90%, preferably 35-85%, more preferably 40-85%, and most preferably 45-85% acrylic monomer, based on the weight of the monomer mixture.

[0037] The monomer mixture may further include one or more additional monomers, such as styrene monomers and vinyl monomers. Examples of styrene monomers may include, for example, styrene, substituted styrenes, or mixtures thereof. Substituted styrenes may include, for example, benzyl acrylate, 2-phenoxyethyl acrylate, butylstyrene, methylstyrene, p-methoxystyrene, or mixtures thereof. A preferred styrene monomer is styrene. Examples of vinyl monomers may include, for example, olefins such as ethylene, propylene, and butadiene; vinyl esters such as vinyl acetate; vinyl alcohol; acrylonitrile; halogenated alkenes such as vinyl chloride; and mixtures thereof.

[0038] The monomer mixture may contain 5% or more, 10% or more, 13% or more, and at the same time 60% or less, 50% or less of styrene monomer by weight of the monomer mixture.

[0039] It will be understood that surfactants can be used as necessary in the disclosed binder composition (e.g., for use in emulsion or dispersion polymerization) to provide stability and also to control particle size. Conventional surfactants include anionic or nonionic emulsifiers or combinations thereof. Typical anionic emulsifiers include, but are not limited to, alkali or ammonium alkyl sulfates, alkali or ammonium alkyl ether sulfates, alkali or ammonium alkyl aryl ether sulfates, alkyl sulfonates, salts of fatty acids, esters of sulfosuccinates, alkyl diphenyl ether disulfonates, and salts or free acids of complex organic phosphates. Typical nonionic emulsifiers include, but are not limited to, polyethers such as ethylene oxide and propylene oxide condensates, including linear and branched alkyl and alkylaryl polyethylene glycol and polypropylene glycol ethers and thioethers, alkylphenoxypoly(ethyleneoxy)ethanols having alkyl groups containing from about 7 to about 18 carbon atoms and having from about 4 to about 100 ethyleneoxy units, and polyoxyalkylene derivatives of hexitols, including sorbitan, sorbide, mannitan, and mannide. Surfactants may be used in the polymer compositions of the present invention at levels of 0.1 to 3 weight percent or greater, based on the total weight of the final composition.

[0040] The acrylic emulsion has a Tg of -80°C to 100°C, preferably -50°C to 80°C, more preferably -45°C to 60°C, and most preferably -40°C to 50°C.

[0041] The solids weight ratio of the polyacid polymer aqueous dispersion and the hydroxyl group-containing acrylic copolymer emulsion is 0.1:100 to 10:100, preferably 0.5:100 to 8:100, more preferably 1:100 to 8:100, and most preferably 2:100 to 7:100, based on the solids of the polyacid polymer aqueous dispersion and the hydroxyl group-containing acrylic copolymer emulsion.

[0042] Other optional components of the adhesive composition of the present disclosure include, but are not limited to, agents selected from cosolvents, coalescents, pigments or other colorants, fillers, reinforcing agents (e.g., fibers), dispersants, wetting agents, waxes, catalysts, foaming agents, defoamers, UV absorbers, flame retardants, adhesion promoters, antioxidants, biocides, coalescents, or stabilizers. These optional components (if necessary) may be added in any order of addition that does not create incompatibility between the components. Components that are not soluble in the aqueous carrier (e.g., pigments and fillers) may be dispersed in the latex or aqueous carrier or cosolvent using a mixer (optionally a high shear mixer). The pH of the composition may be adjusted by adding an acid or base with stirring. Examples of bases include, but are not limited to, ammonia, diethylamine, triethylamine, dimethylethanolamine, triethanolamine, sodium hydroxide, potassium hydroxide, and sodium acetate. Examples of acids include, but are not limited to, acetic acid, formic acid, hydrochloric acid, nitric acid, and toluenesulfonic acid.

[0043] The adhesive composition of the present disclosure can be used for any purpose. A preferred application is as a binder for textiles / nonwovens. For example, a collection of individual fibers (i.e., fibers that are not spun into yarn) may come into contact with the composition of the present disclosure, for example, by immersion, metering, spraying, or other methods, and the water in the composition of the present disclosure is evaporated or allowed to evaporate to create a textile / nonwoven mat. The resulting textile / nonwoven mat may or may not be heated (i.e., exposed to a temperature above 40°C) either before or during the evaporation of the water. It is contemplated that a continuous volume of polymer adheres to multiple fibers, and thus the polymer acts to bind the fibers together.

[0044] One measure of the effectiveness of a binder is the tensile strength of the textile / nonwoven mat, especially when the mat is exposed to water or organic solvents. Higher tensile strength is desirable.

[0045] The fibers that are bonded together by the composition of the present disclosure can be made of any material. The fibers can be mineral fibers or organic fibers. The organic fibers can be natural or artificial. Some suitable natural organic fibers are made of, for example, cellulose, cellulose derivatives, cotton, hemp, and wool. Some suitable artificial organic fibers are made of, for example, rayon, nylon, polyester, acrylic polymers, and polyolefins. In the practice of the present invention, the fibers can be a mixture of suitable fibers.

[0046] In a second aspect of the present disclosure, the present disclosure provides an article prepared with an adhesive composition according to the present disclosure.

[0047] In a third aspect of the present disclosure, the present disclosure provides the use of the adhesive composition of the present disclosure for textile / nonwoven fabrics.

[0048] In one embodiment, the adhesive composition of the present disclosure may be used to increase the tensile strength of a nonwoven mat, especially when the mat is exposed to water or organic solvents. EXAMPLES

[0049] Some embodiments of the present invention are described herein in the following examples, in which all parts and percentages are by weight unless otherwise specified.However, the scope of the present disclosure is of course not limited to the formulations described in these examples.On the contrary, the examples are merely related to the disclosed invention.

[0050] Raw materials: Abbreviations used: DI Water = deionized water, CD = lateral direction, SC = solids content, BA = butyl acrylate, Sty = styrene, IA = itaconic acid, AA = acrylic acid, HEMA = hydroxyethyl methacrylate, MA = maleic anhydride. A: Polyacid polymer aqueous dispersion (ready-to-use commercial product, from DOW Chemical): A1: Acusol 479N, AA / MA copolymer, 40% solids; A2: Acusol 505N, AA / MA copolymer, 35% solids; A3: Acusol 465, AA / MA copolymer, 40% solids A4: Leukotan 8090, AA homopolymer, 40% solids DS-4: RHODACAL DS-4, surfactant, from Solvay Chemical; IA: itaconic acid, from Sinopharm Chemical Reagent; HEMA: hydroxyethyl methacrylate, from Tokyo Chemical Industry; AA: acrylic acid, from Sinopharm Chemical Reagent; BA: butyl acrylate, from Sinopharm Chemical Reagents; Sty: styrene, from Sinopharm Chemical Reagent; APS: ammonium persulfate, from Sinopharm Chemical Reagent; SBS: sodium bisulfite, from Sinopharm Chemical Reagents; t-BHP: tert-butyl hydroperoxide, 70% aqueous solution, from Tokyo Chemical Industry; FF6: Bruggolite FF6, from Brugmann Chemical; TRITON X-100: A surfactant from DOW Chemical. IPA=isopropanol, from Sinopharm Chemical Reagents. WHATMAN #4 PAPER: A product of Whatman Ltd. Example 1: Preparation of Hydroxyl-Containing Acrylic Copolymer Emulsion (B) BI-1: 5.77g of DS-4 was dissolved in 475g of deionized water (DI water). An emulsified monomer mixture was prepared by slowly adding the following ingredients to the solution with stirring: 6.84g IA, 13.7g HEMA, 34.2g AA, 1107.4g BA, 177.7g Sty.

[0051] A solution containing 50.42g DS-4 and 370g deionized water was placed in a 5-necked 3 liter round bottom flask equipped with a thermocouple, cooling condenser, stirrer and heated to 70°C under nitrogen. 27.4g itaconic acid (IA) in 255g DI water at 60°C was charged to the flask. Then 82.8g emulsified monomer mixture was charged into the flask. Then 3.72g ammonium persulfate (APS) in 25g DI water and 1.86g sodium bisulfite (SBS) in 20g DI water were charged into the flask. When the exothermic peak occurred and the temperature was 70°C, the remaining emulsified monomer mixture, a solution of APS (2.48g in 50g DI water) and a solution of SBS (1.24g in 50g DI water) were fed in 120 minutes. The polymerization reaction temperature was maintained at 69-71°C. After the addition was completed, the vessel containing the emulsified monomer mixture and the feed tube leading to the flask were rinsed with 90 g of DI water and the rinse was returned to the flask. The flask was then held at 70° C. for 15 minutes. A solution of t-BHP (70%, 1.05 g in 5 g DI water) and FF6 (0.9 g) in 5 g DI water was then charged. After 15 minutes, a solution of t-BHP (70%, 3.98 g in 38 g DI water) and FF6 (3.38 g in 42 g DI water) was added slowly over 60 minutes and the reaction was then cooled to room temperature. 15 g of ammonia solution was added to adjust the pH value to 6.5-7.5. The solids content is 45%.

[0052] Emulsion BI-1 was prepared containing a copolymer containing 81 wt% BA, 13 wt% Sty, 2.5 wt% AA, 2.5 wt% IA, 1 wt% HEMA based on the dry weight of the copolymer. Tg=-25°C.

[0053] BI-2: Emulsion BI-2 was prepared following the same process as emulsion BI-1, except that 5.77g of DS-4 was dissolved in 475g of deionized water (DI water), and the emulsion monomer mixture was prepared by slowly adding the following ingredients to the solution with stirring: 6.84g of IA, 34.2g of AA, 615.2g of butyl acrylate, 670g of styrene. Tg=30°C.

[0054] BI-3: Emulsion BI-3 was prepared following the same process as emulsion BI-1, except that 5.77g of DS-4 was dissolved in 475g of deionized water (DI water), and the emulsion monomer mixture was prepared by slowly adding the following ingredients to the solution with stirring: 6.84g of IA, 34.2g of AA, 806.6g of butyl acrylate, 478.5g of styrene. Tg=0°C.

[0055] BC-1: Emulsion BC-1 was prepared following the same process as emulsion BI-1, except that 5.77g of DS-4 was dissolved in 475g of DI water, and the emulsion monomer mixture was prepared by slowly adding the following ingredients to the solution with stirring: 6.84g of IA, 34.2g of glacial acrylic acid, 1107.4g of butyl acrylate, 191.4g of styrene. No HEMA was added. Tg=-25°C.

[0056] BC-2: Emulsion BC-2 was a ready-to-use commercial product (ECONEXT 919, from DOW Chemical), Tg=-25°C, no HEMA. Examples of the invention and comparative examples The above raw materials were blended according to the following Table 1. The raw materials were stirred for 15 minutes to obtain a curable aqueous composition.

[0057] A 28 cm x 46 cm piece of WHATMAN paper was immersed in 300 mL of the formulated composition. The treated paper was padded with a Mathis padder and then dried and cured at 150°C for 3 minutes. The polymer loading in the paper was controlled at 14-16%. The cured paper was cut into 1 inch x 4 inch pieces, with the 4 inch direction being the cross-machine (CD) direction of the paper. The tensile strength of the samples was tested dry (untreated), wet (after 30 minutes immersion in 0.1 wt% Triton X-100 / water solution), and IPA (after 30 minutes immersion in isopropanol) on an Instron tensile tester. Wet strength reflects resistance to water and IPA strength reflects resistance to solvents. The results are shown in Table 2 below. [Table 1] [Table 2]

[0058] Compared to Comparatives 1-3, Inventions 1-1-3-4, having Component A in the formulation, showed a 10%-25% improvement in wet strength and a 40%-90% improvement in IPA strength. By comparing Comparative 1 to Comparatives 4 or 5, and Invention 1-1 to Comparatives 4-1 or 5-1, both wet strength and IPA strength increased when Component B contained a hydroxyl group-containing monomer. Comparing Invention 3-3 to Invention 3-3-a, it was found that the performance of the invention formulations remained stable after 30 days of 50°C heat aging.

[0059] Glass transition temperature (Tg) A dried sample of the polymer was placed in an aluminum crucible and the sample was then tested by a DSC Q2000 from TA Instruments following this program. 1. Heat from -80℃ to 120℃ at 20℃ / min to erase the thermal history; 2.Cool down to -80℃; 3. Heat from -80°C to 120°C at 10°C / min.

[0060] The half-height point of the transition was determined as the glass transition temperature (Tg). The present application also relates to the following aspects: (1) The following ingredients: (a) an aqueous dispersion of a polyacid polymer, the polyacid polymer comprising 50% to 100% by weight of one or more ethylenically unsaturated mono- or dicarboxylic acids / anhydrides; Polyacid polymer aqueous dispersion, (b) an adhesive composition comprising a hydroxyl group-containing acrylic copolymer emulsion, the hydroxyl group-containing acrylic copolymer being obtained by polymerizing a monomer mixture containing 0.1-10% of a hydroxyl group-containing monomer, 0.1%-20% by weight of an unsaturated carboxylic acid, and 30%-90% of an acrylic monomer; An adhesive composition, wherein the solids weight ratio of the components (a) and (b) is 0.1:100 to 10:100 based on the solids of the components (a) and (b). (2) The adhesive composition according to claim 1, wherein the ethylenically unsaturated mono- or dicarboxylic acid / anhydride comprises methacrylic acid, acrylic acid, crotonic acid, fumaric acid, maleic acid, 2-methylmaleic acid, itaconic acid, 2-methylitaconic acid, α,β-methylene glutaric acid, monoalkyl maleates, monoalkyl fumarates, maleic anhydride, itaconic anhydride, acrylic anhydride, methacrylic anhydride, and salts thereof. (3) The adhesive composition of claim 1, wherein the one or more ethylenically unsaturated mono- or dicarboxylic acids / anhydrides are copolymerized with methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, decyl acrylate, methyl methacrylate, butyl methacrylate, isodecyl methacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, (meth)acrylamide, substituted (meth)acrylamide, styrene, substituted styrene, butadiene, vinyl acetate, acrylonitrile and / or methacrylonitrile. (4) The adhesive composition according to claim 1, wherein the hydroxyl group-containing monomer comprises a hydroxyalkyl (meth)acrylate. (5) The adhesive composition of claim 1, wherein the hydroxyl group-containing monomer comprises hydroxyethyl methacrylate (HEMA), hydroxyethyl acrylate (HEA), hydroxypropyl methacrylate (HPMA) and hydroxypropyl acrylate. (6) The adhesive composition of claim 1, wherein the unsaturated carboxylic acid comprises (meth)acrylic acid, itaconic acid, fumaric acid, (meth)acrylic anhydride, maleic anhydride, or a mixture thereof. (7) The adhesive composition of claim 1, wherein the acrylic monomer comprises methyl acrylate, ethyl acrylate, butyl acrylate, glycidyl methacrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and combinations thereof. (8) The adhesive composition according to claim 1, wherein the monomer mixture contains a styrene monomer or a vinyl monomer. (9) An article prepared using the adhesive composition according to claim 1. (10) Use of the adhesive composition according to claim 1 for textiles / nonwoven fabrics.

Claims

1. The following ingredients: (a) an aqueous dispersion of a polyacid polymer, the polyacid polymer containing 50% to 100% by weight of one or more ethylenically unsaturated mono- or dicarboxylic acids / anhydrides, the ethylenically unsaturated mono- or dicarboxylic acids / anhydrides including methacrylic acid, acrylic acid, crotonic acid, fumaric acid, maleic acid, 2-methylmaleic acid, itaconic acid, 2-methylitaconic acid, α,β-methylene glutaric acid, monoalkyl maleates, monoalkyl fumarates, maleic anhydride, itaconic anhydride, acrylic anhydride, methacrylic anhydride, and salts thereof; (b) a hydroxyl group-containing acrylic copolymer emulsion, the hydroxyl group-containing acrylic copolymer containing 0.1-10% of a hydroxyl group-containing monomer, 0.1%-20% by weight of an unsaturated carboxylic acid, and 30%-90% of an acrylic monomer; An adhesive composition comprising a hydroxyl-containing acrylic copolymer emulsion obtained by polymerizing a monomer mixture, the acrylic monomer is selected from the group consisting of methyl acrylate, ethyl acrylate, butyl acrylate, glycidyl methacrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and combinations thereof; The adhesive composition, wherein the solids weight ratio of components (a) and (b) is from 0.1:100 to 10:100, based on the solids of components (a) and (b).

2. 2. The adhesive composition of claim 1, wherein the one or more ethylenically unsaturated mono- or dicarboxylic acids / anhydrides are copolymerized with methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, decyl acrylate, methyl methacrylate, butyl methacrylate, isodecyl methacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, (meth)acrylamide, substituted (meth)acrylamide, styrene, substituted styrene, butadiene, vinyl acetate, acrylonitrile and / or methacrylonitrile.

3. The adhesive composition of claim 1 , wherein the hydroxyl-containing monomer comprises a hydroxyalkyl (meth)acrylate.

4. 2. The adhesive composition of claim 1, wherein the hydroxyl group-containing monomers include hydroxyethyl methacrylate (HEMA), hydroxyethyl acrylate (HEA), hydroxypropyl methacrylate (HPMA) and hydroxypropyl acrylate.

5. 2. The adhesive composition of claim 1, wherein the unsaturated carboxylic acid comprises (meth)acrylic acid, itaconic acid, fumaric acid, (meth)acrylic anhydride, maleic anhydride, or mixtures thereof.

6. 2. The adhesive composition of claim 1, wherein said monomer mixture comprises a styrene monomer or a vinyl monomer different from said ethylenically unsaturated mono- or dicarboxylic acid / anhydride.

7. 13. An article prepared with the adhesive composition of claim 1.

8. 2. Use of the adhesive composition according to claim 1 on textile / nonwoven fabrics.

Citation Information

Patent Citations

  • Coating agent composition

    JP1992117470A

  • Production of copolymer latex, copolymer latex, and paper coating composition obtained therefrom

    JP1994298815A

  • Aqueous emulsion composition and adhesive composition

    JP2003342335A

  • Curable aqueous composition and use thereof as heat-resistant nonwoven fabric binder

    JP2005068399A

  • Aqueous binder for inorganic fiber heat-insulating / sound-absorbing material, and inorganic fiber heat-insulating / sound-absorbing material