Semiconductor Device
By employing an oxide semiconductor film with a wurtzite crystal structure, the interface with the gate insulating film is stabilized, addressing the instability issues in transistors, resulting in reliable semiconductor devices suitable for large substrates.
Patent Information
- Application Number
- JP2023001048
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2010-11-30
- Filing Date
- 2023-01-06
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2031-11-23
AI Technical Summary
Transistors using oxide semiconductor films are prone to unstable electrical characteristics due to fluctuations in the interface quality with the gate insulating film, which is affected by manufacturing processes and light irradiation, leading to unreliable performance, especially when large substrates like mother glass are used.
The formation of an oxide semiconductor film with a second crystal structure, such as wurtzite type, which is easily crystallized by heat treatment, is used to improve the interface condition with the gate insulating film, ensuring stable electrical characteristics and reliability. This is achieved by stacking oxide semiconductor films and performing heat treatments at specific temperatures to enhance crystallinity.
The method results in semiconductor devices with stable electrical characteristics and high reliability, allowing for the production of highly reliable transistors even on large substrates, reducing the impact of light irradiation and manufacturing stress.
Smart Images

Figure 0007572469000001 
Figure 0007572469000002 
Figure 0007572469000003
Abstract
Description
[Technical field]
[0001] Semiconductor device having a circuit including a semiconductor element such as a transistor and a manufacturing method thereof For example, power devices mounted on power circuits, memory, thyristors, converters, inverters, etc. semiconductor integrated circuits including image sensors, electro-optical devices such as liquid crystal display panels, The present invention relates to electronic equipment incorporating a light-emitting display device having optical elements as a component.
[0002] In this specification, a semiconductor device is a device that can function by utilizing semiconductor characteristics. This generally refers to electro-optical devices, light-emitting display devices, semiconductor circuits, and electronic devices, all of which are semiconductor devices. be. [Background technology]
[0003] As typified by liquid crystal display devices, transistors formed on glass substrates are amorphous. It is made of amorphous silicon, polycrystalline silicon, etc. Although the resulting transistor has low field-effect mobility, it can be used on large glass substrates. In addition, although the field effect mobility of a transistor using polycrystalline silicon is high, the glass substrate is However, it has a drawback that it is not suitable for large area applications.
[0004] A transistor using an oxide semiconductor is manufactured in place of a transistor using silicon. Technologies that can be applied to electronic and optical devices are attracting attention. For example, oxide semiconductors Then, transistors were fabricated using zinc oxide and In-Ga-Zn-O oxide, and a display device was The technology used for the switching element of the pixel is disclosed in Patent Document 1 and Patent Document 2. do. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-123861 A [Patent Document 2] JP 2007-96055 A Summary of the Invention [Problem to be solved by the invention]
[0006] The electrical characteristics of the transistor are determined by the oxide semiconductor film, which is an active layer, and the The interface between the gate insulating film and the transistor is easily affected by the condition of the interface. In the present invention, the interface between the oxide semiconductor film and the gate insulating film, i.e., the interface on the gate electrode side, is amorphous. If the material is in a crystalline state, the structure is easily affected by factors such as temperature during the manufacturing process, and The electrical characteristics of the transistor tend to become unstable.
[0007] In addition, a transistor using an oxide semiconductor film as a channel can be irradiated with visible light or ultraviolet light. The electrical characteristics change depending on the
[0008] In view of the above problem, one embodiment of the present invention is a method for manufacturing an oxide semiconductor film having a first insulating film and a second insulating film which is in contact with the oxide semiconductor film. Semiconductor device having a transistor with a good interface condition with a gate insulating film and a method for manufacturing the same Another object of the present invention is to provide a transistor using an oxide semiconductor film as a channel. One of the objectives of the present invention is to provide a semiconductor device having high reliability by providing a stable electrical characteristic to the semiconductor device. In addition, large substrates such as mother glass are used to mass-produce highly reliable semiconductor devices. An object of the present invention is to provide a manufacturing process of a semiconductor device that can be manufactured. [Means for solving the problem]
[0009] One embodiment of the present invention is a gate insulating film including an oxide semiconductor film and an insulating film (gate insulating film) in contact with the oxide semiconductor film. In order to improve the interface state with the oxide semiconductor film, a highly crystalline oxide semiconductor film is provided at least near the interface. This allows the creation of a semiconductor device with stable electrical characteristics and high reliability. It can be manufactured.
[0010] In addition, as a method for improving the crystallinity of an oxide semiconductor film, An oxide semiconductor film having a second crystal structure may be provided. The second crystal structure is a wurtzite structure. The oxide semiconductor film that can have the second crystal structure has the first crystal structure. In comparison with a conventional oxide semiconductor film, the oxide semiconductor film is more likely to be crystallized by heat treatment and has higher crystallinity. The crystal structure of 1 is a non-wurtzite structure, a YbFe2O4 type structure, a Yb2Fe3O7 type structure, and others. The crystal structure is selected from any one of the modified structures of the above.
[0011] In addition, an oxide semiconductor film capable of being turned into a first crystal structure by heat treatment and a second crystal structure by heat treatment are formed. The oxide semiconductor film having the above crystal structure is then stacked and subjected to heat treatment. The oxide semiconductor film having the second crystal structure is used as a seed to form a first crystal structure by heat treatment. The oxide semiconductor film having the first crystal structure is formed by crystal growth of the oxide semiconductor film having the first crystal structure. can be.
[0012] The heat treatment is carried out at a temperature of 150° C. to 650° C., preferably 200° C. to 500° C. .
[0013] In addition, instead of heat treatment for crystallization, the oxide was sputtered while being heated. A compound semiconductor film can be formed.
[0014] As a result, for example, in an oxide semiconductor stack in which oxide semiconductor films are stacked, at least By providing a layer having a second oxide semiconductor film, the oxide semiconductor stack can be subjected to heat treatment. By performing the above process, an oxide semiconductor film with high crystallinity can be obtained.
[0015] The thickness of the second oxide semiconductor film is preferably one atomic layer or more and 10 nm or less, more preferably 2 nm or more. The upper limit is 5 nm.
[0016] In the above structure, the oxide semiconductor film is non-single-crystal and the entire oxide semiconductor film is in an amorphous state. (amorphous state) but has crystals with at least a c-axis orientation in the oxide semiconductor film. Yes.
[0017] One embodiment of the present invention is a method for manufacturing a semiconductor device having a transistor, A first oxide semiconductor film is formed, a second oxide semiconductor film is formed, and then a first heat treatment is performed. The oxide semiconductor film having the first crystal structure and the oxide semiconductor film having the second crystal structure are Next, a third oxide semiconductor film is formed over the oxide semiconductor film having the second crystal structure. After the formation of the oxide semiconductor film, a second heat treatment is performed to form an oxide semiconductor film having a third crystal structure. an oxide semiconductor film having a first crystal structure, an oxide semiconductor film having a second crystal structure, A stack of oxide semiconductor films having a third crystal structure is used as a channel region of a transistor. The present invention is characterized in that it is formed by:
[0018] Note that the oxide semiconductor film having the first crystal structure and the oxide semiconductor film having the third crystal structure The crystal structure of the conductive film is YbFe2O4 type structure, Yb2Fe3O7 type structure and non-wurtzite type. The crystal structure of the oxide semiconductor film having the second crystal structure is any one of the following: It has a ruthenium structure.
[0019] The temperature of the first heat treatment and the second heat treatment is 150° C. or higher and 650° C. or lower, preferably 2 The temperature is between 00 and 500 degrees. For this reason, mother glass, which is a large-area substrate, is used as the substrate. It can be used.
[0020] The oxide semiconductor films having the first to third crystal structures are The oxide semiconductor film is non-single-crystal, and the entire oxide semiconductor film is not in an amorphous state. It has a crystalline region oriented along the c-axis, i.e., it has an amorphous region and a crystalline region oriented along the c-axis.
[0021] The oxide semiconductor film having the second crystal structure has a wurtzite crystal structure. Compared with an oxide semiconductor film having a crystal structure and an oxide semiconductor film having a third crystal structure The acid having the second crystal structure is easily crystallized by heat treatment and has high crystallinity. The compound semiconductor film has hexagonal bonds on the ab plane. Layers with rectangular bonds are stacked and bonded in the film thickness direction (c-axis direction), and the c-axis orientation is For this reason, the oxide semiconductor film having the second crystal structure, which has a wurtzite crystal structure, The first oxide semiconductor film and the third oxide semiconductor film are crystal-grown by heating using the above as a seed. As a result, the crystal axis of the oxide semiconductor film having the second crystal structure, which has a wurtzite crystal structure, The oxide semiconductor film having the first crystal structure and the third crystal structure are formed so as to be substantially the same as An oxide semiconductor film having a first crystal structure can be formed. and the oxide semiconductor film having the third crystal structure is an oxide semiconductor film having a second crystal structure. Like the membrane, the bonds in the ab plane form a hexagon. The layers are laminated and bonded in the film thickness direction (c-axis direction), and are c-axis oriented. .
[0022] A gate insulating film is formed on the oxide semiconductor laminate, and a gate electrode is formed on the gate insulating film. By forming a gate electrode, a transistor can be fabricated. Since the oxide semiconductor stack has high crystallinity and high uniformity at the interface, the electrical characteristics are stable. Therefore, a transistor with high reliability can be obtained.
[0023] A gate insulating film is formed on the gate electrode, and the oxide semiconductor laminate is formed on the gate insulating film. As a result, a transistor can be manufactured by forming a gate insulating film. The oxide semiconductor stack has high crystallinity and high uniformity at the interface, and therefore has excellent electrical characteristics. A stable and highly reliable transistor can be obtained.
[0024] In addition, oxides having hexagonal bonds in the ab plane and crystal regions oriented along the c axis By using a stack of semiconductor films in the channel region of a transistor, the transistor can be illuminated with light. The threshold of the transistor is also It is possible to fabricate transistors with stable electrical characteristics and small variations in voltage. can. Effect of the Invention
[0025] According to one embodiment of the present invention, a gate insulating film is provided in contact with an oxide semiconductor film. It is possible to manufacture a semiconductor device having a transistor with a good surface condition. In addition, a semiconductor device having excellent electrical characteristics can be manufactured. Using large substrates, highly reliable semiconductor devices can be mass-produced. [Brief description of the drawings]
[0026] [Figure 1] 1A and 1B are a top view and a cross-sectional view illustrating a semiconductor device according to one embodiment of the present invention. [Diagram 2] 1A to 1C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Diagram 3] 1A to 1C are diagrams illustrating a crystal structure according to an embodiment of the present invention. [Figure 4] 1A to 1C are diagrams illustrating a crystal structure according to an embodiment of the present invention. [Diagram 5] 1 is a HAADF-STEM image illustrating a crystal structure according to an embodiment of the present invention. [Figure 6] 1 is a HAADF-STEM image illustrating a crystal structure according to an embodiment of the present invention. [Figure 7] 1A and 1B are a top view and a cross-sectional view illustrating a semiconductor device according to one embodiment of the present invention. [Figure 8] 1A to 1C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 9] 1A and 1B are a top view and a cross-sectional view illustrating a semiconductor device according to one embodiment of the present invention. [Figure 10] 1A to 1C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 11] 1A and 1B are a top view and a cross-sectional view illustrating a semiconductor device according to one embodiment of the present invention. [Figure 12] 1A to 1C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 13] 1A and 1B are a top view and a cross-sectional view illustrating a semiconductor device according to one embodiment of the present invention. [Figure 14] 1A to 1C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 15] 1A and 1B are a top view and a cross-sectional view illustrating a semiconductor device according to one embodiment of the present invention. [Figure 16] 1A to 1C are cross-sectional views illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention. [Figure 17] 1 is a cross-sectional view illustrating a semiconductor device according to one embodiment of the present invention. [Figure 18] 1A and 1B are a block diagram and a circuit diagram illustrating one embodiment of the present invention. [Figure 19] FIG. 1 is a cross-sectional view showing one embodiment of the present invention. [Figure 20] FIG. 1 is a diagram illustrating an example of an electronic device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] The present invention will be described in detail with reference to the accompanying drawings. The present invention is not limited to the above, and various modifications and variations in form and detail are possible without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that the present invention can be modified in the following manner. The present invention is not limited to the above-described embodiment. In the configuration, the same parts or parts having similar functions are designated by the same reference numerals in different drawings. will be used throughout and a repeated explanation will be omitted.
[0028] In each figure described in this specification, the size, thickness, or area of each component is not clearly indicated. may be exaggerated for clarity and are not necessarily limited to scale .
[0029] In addition, the terms "first," "second," "third," etc., used in this specification are used interchangeably to avoid confusion of components. The number is not limited to the number of the first one. For example, "first one" can be changed to " The terms "second" or "third" can be used interchangeably to explain the present invention.
[0030] (Embodiment 1) In this embodiment, a transistor in which an oxide semiconductor film on an insulating surface is used as a channel and A manufacturing method thereof will be described with reference to FIGS. 1 and 2. FIG. 1B shows the structure of a semiconductor device. FIG. 1A is a cross-sectional view illustrating a structure of a transistor according to one embodiment; It corresponds to a cross-sectional view of the dashed line AB. In FIG. 1(A), a substrate 101, an oxide insulator The film 102, the gate insulating film 107, and the insulating film 109 are omitted. 1A to 1C are cross-sectional views illustrating a manufacturing process of the transistor shown in FIG.
[0031] The transistor shown in FIG. 1B includes an oxide insulating film 102 formed over a substrate 101 and an oxide The oxide semiconductor stack 105 formed on the oxide insulating film 102 and the oxide semiconductor stack 10 A pair of electrodes 106 functioning as a source electrode and a drain electrode formed on the oxide film 5, A gate electrode formed on the oxide insulating film 102, the oxide semiconductor laminate 105, and the pair of electrodes 106. a gate insulating film 107 overlapping with the oxide semiconductor stack 105 via the gate insulating film 107; The gate electrode 108 is covered with a gate insulating film 107. It may have a membrane 109 .
[0032] The oxide semiconductor stack 105 is an oxide semiconductor layer having a first crystal structure in contact with the oxide insulating film 102. a second oxide semiconductor film in contact with the oxide semiconductor film having the first crystal structure; The oxide semiconductor film 105a and the oxide semiconductor film 105b having a crystalline structure are stacked.
[0033] In addition, the oxide semiconductor film 105b having the second crystal structure is used as a seed crystal to grow the oxide semiconductor film 105b having the first crystal structure. The oxide semiconductor film 105a has a crystal growth.
[0034] The oxide semiconductor film 105b having the second crystal structure is a trigonal crystal and / or a hexagonal crystal. do.
[0035] That is, the oxide semiconductor films having the second crystal structure and the first crystal structure are both trigonal and / or hexagonal crystal, a hexagonal lattice image can be seen from the c-axis direction.
[0036] Note that the oxide semiconductor film 105a having the first crystal structure and the oxide semiconductor film 105b having the second crystal structure The semiconductor film 105b is non-single crystal, and the entire oxide semiconductor film is in an amorphous state ( It is not in an amorphous state, but has crystalline regions oriented along the c-axis.
[0037] Next, a manufacturing method of the transistor illustrated in FIG. 1B will be described with reference to FIGS.
[0038] As shown in FIG. 2A, an oxide insulating film 102 is formed on a substrate 101, and then an oxide insulating film 102 is formed on the substrate 101. A first oxide semiconductor film 103a is formed over the oxide semiconductor film 102, and A second oxide semiconductor film 103b is formed thereon.
[0039] The substrate 101 must have at least sufficient heat resistance to withstand subsequent heat treatments. When a glass substrate is used as the substrate 101, a substrate having a distortion point of 730 degrees or more is used. The glass substrate is preferably made of, for example, aluminosilicate glass, aluminophore glass, or the like. Glass materials such as borosilicate glass and barium borosilicate glass are used. It is preferable to use a glass substrate containing more BaO than O3. Board 101 is 8th generation (2160mm x 2460mm), 9th generation (2400mm x 280 0mm, or 2450mm x 3050mm), 10th generation (2950mm x 3400m It is preferable to use mother glass such as mother glass (M) because the processing temperature is high and the processing If the time is long, the glass will shrink significantly, so if you use mother glass for mass production, the manufacturing process The heat treatment is preferably carried out at a temperature of 600° C. or less, and more preferably at a temperature of 450° C. or less.
[0040] Instead of the above glass substrate, an insulating substrate such as a ceramic substrate, a quartz substrate, or a sapphire substrate may be used. A substrate made of an insulating material can be used. Alternatively, crystallized glass can be used. Furthermore, the surface of a semiconductor substrate such as a silicon wafer or the surface of a conductive substrate made of a metal material can be It is also possible to use a substrate having an insulating film formed on its surface.
[0041] When a glass substrate containing impurities such as alkali metals is used as the substrate 101, In order to prevent the intrusion of potassium metal, a nitride insulating film is formed between the substrate 101 and the oxide insulating film 102. A silicon nitride film, an aluminum nitride film, or the like may be formed by CVD. The lithium, sodium, potassium, etc. The alkali metal content is reduced because it is an impurity in the oxide semiconductor film that is formed later. It is preferable.
[0042] The oxide insulating film 102 is formed using an oxide insulating film from which part of oxygen is released by heating. As for the oxide insulating film from which part of the oxygen is released by heating, the oxygen content is higher than that which satisfies the stoichiometric ratio. It is preferable to use an oxide insulating film that contains as much oxygen as possible. The oxide insulating film is heated to form the first oxide semiconductor film 103a and the second oxide semiconductor film 103b. The oxide insulating film 102 can be typically formed of an oxide Silicon, silicon oxynitride, silicon nitride oxide, aluminum oxide, aluminum oxynitride The oxide can be formed of tungsten oxide, gallium oxide, hafnium oxide, yttrium oxide, or the like.
[0043] When an oxide insulating film contains more oxygen than the stoichiometric ratio, some of the oxygen is removed by heating. The amount of oxygen released at this time is called the Thermal Desorptio Spectroscopy: Thermal Desorption Spectroscopy) analysis was performed to determine the amount of oxygen converted into oxygen atoms. The amount of emitted material is 1.0×10 18 atoms / cm 3 More than 1.0×10 20 a toms / cm 3 More preferably, 3.0×10 20 atoms / cm 3 That's all. .
[0044] Here, we will explain how to measure the amount of released oxygen when converted into oxygen atoms using TDS analysis. , as explained below.
[0045] The amount of gas released during TDS analysis is proportional to the integral value of the spectrum. The amount of gas released is calculated by the ratio of the integral value of the spectrum of the insulating film to the reference value of the standard sample. The standard value of the standard sample is the spectrum of the sample containing the specified atom. is the ratio of the atomic density to the integral value of
[0046] For example, the results of a TDS analysis of a silicon wafer containing a standard sample of hydrogen with a given density, From the results of TDS analysis of the oxide insulating film, the amount of oxygen molecules released from the oxide insulating film (N(O2)) can be calculated using Equation 1. Here, the mass number of 32 detected by TDS analysis is We assume that all the spectra are from oxygen molecules. The mass number of 32 is CH3OH. However, they are unlikely to exist and are not considered here. For oxygen molecules containing oxygen atoms with mass numbers 17 and 18, It is not taken into consideration because its presence in the environment is extremely small.
[0047] N(O2)=N(H2) / S(H2)×S(O2)×α (Math. 1)
[0048] N(H2) is the density of hydrogen molecules desorbed from the standard sample. S(H2) is is the integral value of the spectrum when the standard sample is analyzed by TDS. The value is N(H2) / S(H2). S(O2) is the value obtained by TDS analysis of the oxide insulating film. α is the coefficient that affects the spectral intensity in TDS analysis. For details of the formula 1, please refer to Japanese Patent Application Laid-Open No. 6-275697. The amount of oxygen released from the oxide insulating film was measured using a thermal desorption analyzer EMD-W (Electronics Science Corporation). Using A1000S / W, a standard sample of 1×10 16 atoms / cm 3 The hydrogen atoms of The measurement is performed using a silicon wafer containing the same.
[0049] In addition, some of the oxygen is detected as oxygen atoms in the TDS analysis. The ratio of the oxygen molecules can be calculated from the ionization rate of the oxygen molecules. Since the ionization rate of oxygen molecules is included in the calculation, the amount of oxygen atoms released can be calculated by evaluating the amount of oxygen molecules released. It is possible to estimate even if
[0050] Note that N(O2) is the amount of released oxygen molecules. In the case of an oxide insulating film, When this occurs, the amount of oxygen released is twice the amount of oxygen molecules released.
[0051] The oxide insulating film 102 has a thickness of 50 nm or more, preferably 200 nm or more and 500 nm or less. By making the oxide insulating film 102 thicker, the amount of oxygen released from the oxide insulating film 102 is increased. In addition, the boundary between the oxide insulating film 102 and an oxide semiconductor film to be formed later can be formed It is possible to reduce defects in the surface.
[0052] The oxide insulating film 102 is formed by a sputtering method, a CVD method, or the like. The oxide insulating film from which part of the oxygen is released can be easily formed by using a sputtering method. Therefore, it is preferable.
[0053] When an oxide insulating film that releases some oxygen by heating is formed by a sputtering method, The deposition gas preferably contains a large amount of oxygen, and is preferably a mixture of oxygen and a rare gas. Typically, the oxygen concentration in the deposition gas is set to 6% or more and 100% or less. It is preferable that
[0054] The first oxide semiconductor film 103a is heated to have a trigonal and / or hexagonal crystal structure and a first The insulating film is formed using an oxide semiconductor film that can have a crystalline structure.
[0055] The first oxide semiconductor film 103a is made of an oxide of a quaternary metal, In—Sn—Ga— Zn-O film, In-Ga-Zn-O film, which is an oxide of a ternary metal, In-Sn-Zn- O film, In-Al-Zn-O film, Sn-Ga-Zn-O film, Al-Ga-Zn-O film, S n-Al-Zn-O film, In-Zn-O film, which is an oxide of binary metals, and Sn-Zn-O A film, an Al-Zn-O film, an In-Ga-O film, or the like can be used. The semiconductor may contain SiO2. For example, an In-Ga-Zn-O film is an In-Ga-Zn-O film. The oxide film contains indium (In), gallium (Ga), and zinc (Zn).
[0056] The first oxide semiconductor film 103a is heated to have a trigonal and / or hexagonal crystal structure and a non- Wurtzite type, YbFe2O4 type structure, Yb2Fe3O7 type structure, or any of their modified structures The insulating film is formed using an oxide semiconductor film that can have one of the crystal structures.
[0057] As an example of an oxide semiconductor film having the first crystal structure, an oxide of a ternary metal, In-G The a-Zn-O film has a trigonal and / or hexagonal non-wurtzite crystal structure. The In-Ga-Zn-O film, which is an oxide of InGa-Zn-O, has a YbFe2O4 structure. aZnO4, and In2Ga2ZnO7, which has a Yb2Fe3O7 type structure, and its variants It can take the type structure (M. Nakamura, N. Kimizuka, and T. Mohri, “The Phase Relations in the In 2O3-Ga2ZnO4-ZnO System at 1350 degrees”, J. Soli d State Chem., 1991, Vol. 93, p. 298-315). In the YbFe2O4 type structure, the layer containing Yb is called layer A and the layer containing Fe is called layer B. It has a repeating structure of B|ABB|ABB|, and examples of its modified structure include ABBB The repeating structure of |ABBB| is an example. The Yb2Fe3O7 type structure is It has a repeating structure of ABB|AB|ABB|AB|, and examples of its modified structure include List the repeating structure ABBB|ABB|ABBB|ABB|ABBB|ABB| can be done.
[0058] Note that the first oxide semiconductor film 103a was formed by adding 1×10 17 / cm 3 Below Top 5×10 19 / cm 3 It may contain less than 10000000 nitrogen.
[0059] Note that a metal oxide that can be formed as the first oxide semiconductor film 103a is an energy The energy gap is 2 eV or more, preferably 2.5 eV or more, and more preferably 3 eV or more. In this way, by using an oxide semiconductor with a wide energy gap, The off-state current can be reduced.
[0060] The second oxide semiconductor film 103b is an oxide semiconductor film that can have a second crystal structure by heating. The oxide semiconductor film that can have the second crystal structure is formed using a trigonal crystal structure and / or a hexagonal crystal structure. The first crystal structure of the oxide semiconductor film is crystallized more easily by heat treatment than the first crystal structure of the oxide semiconductor film. It is also highly crystalline.
[0061] The second oxide semiconductor film 103b can be made of zinc oxide, an oxynitride semiconductor, or the like. The oxynitride semiconductor can be formed by adding 5× the metal oxides listed for the first oxide semiconductor film 103a. 10 19 / cm 3The nitrogen can be added by up to 7 atomic %.
[0062] The second oxide semiconductor film 103b is formed in order to cause crystal growth of the first oxide semiconductor film 103a. Since it is used as a seed, the thickness is set to the thickness required for crystal growth. Typically, it is one atomic layer or more, up to 10n The thickness of the second oxide semiconductor film 103b is preferably 2 nm to 5 nm. By making the thickness thinner, the throughput in the film formation process and the heat treatment can be increased.
[0063] The first oxide semiconductor film 103a and the second oxide semiconductor film 103b are each formed by sputtering. The film can be formed by a ring method, a coating method, a printing method, a pulsed laser deposition method, or the like. The first oxide semiconductor film 103a and the second oxide semiconductor film 103b were formed by a quenching method. When forming a film, either an AC sputtering device, a DC sputtering device, or an RF sputtering device can be used. One of the sputtering devices is used.
[0064] Note that the second oxide semiconductor film 103b is formed of an oxynitride semiconductor by a sputtering method. In this case, after the first oxide semiconductor film 103a is formed, the gas to be introduced into the sputtering apparatus is By switching the type of gas, i.e. by introducing nitrogen, an oxynitride semiconductor can be formed. That is, the first oxide semiconductor film 103a and the second oxide semiconductor film 103b are successively formed. This makes it possible to manufacture the device with excellent mass productivity.
[0065] Next, a first heat treatment is performed. The temperature of the first heat treatment is preferably 150° C. or more and 650° C. or less. The heating time of the first heat treatment is 1 minute or more and 2 minutes or less. The time is 4 hours or less. After the temperature of the first heat treatment is gradually increased, the temperature is kept constant. The temperature rise rate from 500 degrees or higher should be between 0.5 degrees / h and 3 degrees / h. Since the crystals of the second oxide semiconductor film 103b gradually grow, the crystallinity can be further improved. can.
[0066] The first heat treatment is performed in a rare gas (typically, argon) atmosphere, an oxygen atmosphere, or a nitrogen atmosphere. Atmosphere, dry air atmosphere, or a mixture of rare gas (typically argon) and oxygen; Alternatively, a mixed atmosphere of rare gas and nitrogen is preferable. A high-purity gas atmosphere in which impurities have been removed to the level of a few ppm or a few ppb. It is preferable that:
[0067] The heat treatment device used in the first heat treatment is not particularly limited, and may be a heat treatment device using a heat generating element such as a resistance heating element. The apparatus may include a device for heating the workpiece by conduction or thermal radiation. For example, Furnaces, GRTA (Gas Rapid Thermal Anneal) equipment, LRTA RTA (Rapid Thermal Anneal) equipment, etc. The LRTA device can be used for halogen-free lamps, metal halide lamps, xenon arc lamps, carbon arc lamps, high pressure The radiation of light (electromagnetic waves) emitted from lamps such as sodium lamps and high-pressure mercury lamps can cause This is a device that heats the object to be treated. The GRTA device is a device that uses high-temperature gas to perform heat treatment. It is located.
[0068] By the first heat treatment, the first oxide semiconductor film 103b is Crystal growth starts toward the second oxide semiconductor film 103a. The second oxide semiconductor film 103b is easily crystallized. Therefore, the second oxide semiconductor film 103b is entirely crystallized and becomes an oxide semiconductor film having a second crystal structure. The first oxide semiconductor is formed on the surface of the second oxide semiconductor film 103b. Since the crystals grow toward the conductive film 103a, the crystals become c-axis oriented crystal regions. The oxide semiconductor film 104b having a crystal structure has a hexagonal shape on the upper surface of the ab-plane. In addition, layers with hexagonal bonds are stacked in the film thickness direction (c-axis direction). It is bonded and c-axis oriented.
[0069] Then, a first heat treatment is performed to form an oxide semiconductor film 104b having a second crystal structure. As a seed, the crystal growth of the first oxide semiconductor film 103a is performed using an oxide having a second crystal structure. The second crystal structure is formed by adsorbing oxygen from the interface with the semiconductor film 104b toward the oxide insulating film 102. The oxide semiconductor film 104b is oriented in the c-axis direction and has the second crystal structure. The oxide semiconductor film 104b is used as a seed to form the oxide semiconductor film 10 having the second crystal structure. The first oxide semiconductor film 103a is grown in a crystal state so that the crystal axis of the first oxide semiconductor film 103a is approximately the same as that of the first oxide semiconductor film 4b. That is, the first oxide semiconductor film 103a can be grown as a crystal with the c-axis aligned. That is, the oxide semiconductor film 104a having the first crystal structure can be ab The layers have hexagonal bonds on the upper plane of the surface. The layers are laminated and bonded in the film thickness direction (c-axis direction) and are c-axis oriented. As a result, the oxide semiconductor film 104a having the first crystal structure with c-axis alignment can be formed. (See Figure 2(B)).
[0070] Note that the first heat treatment causes crystals to grow vertically from the surface of the second oxide semiconductor film 103b. When grown, the oxide semiconductor film 104a having a first crystal structure and the oxide semiconductor film 104b having a second crystal structure are formed. The c-axis of the oxide semiconductor film 104b is approximately perpendicular to the surface.
[0071] In addition, the first oxide semiconductor film 103a and the second oxide semiconductor film 103b are formed by the first heat treatment. The hydrogen contained in the membrane 103b is released (i.e., dehydrogenated or dehydrated), and the oxygen is released. Part of the oxygen contained in the oxide semiconductor insulating film 102 is mixed with the first oxide semiconductor film 103a and the second oxide semiconductor film 103b. The first oxide semiconductor film 103b in the oxide insulating film 102 and the second oxide semiconductor film 103a in the oxide insulating film 102 are Through this process, the first oxide semiconductor film 103a and the second oxide semiconductor film 103b are diffused into the vicinity of the interface. In addition, the oxide insulating film 103b can be formed by the above-mentioned method. By diffusing oxygen to the vicinity of the first oxide semiconductor film 103a in the oxide semiconductor layer 102, Defects at the interface between the insulating film 102 and the first oxide semiconductor film 103a can be reduced. As a result, an oxide semiconductor having a first crystal structure in which the hydrogen concentration and oxygen defects are reduced can be obtained. The oxide semiconductor film 104a having the second crystal structure and the oxide semiconductor film 104b having the second crystal structure can be formed. do.
[0072] Note that the first oxide semiconductor film 103a and the second oxide semiconductor film 103b are formed by a sputtering method. When forming 103b, the leak rate of the processing chamber of the sputtering device is set to 1×10 -10 Pa·m 3 / sec or less, the first oxidation during the film formation by the sputtering method can be prevented. The incorporation of alkali metals, hydrogen, etc. into the oxide semiconductor film 103a and the second oxide semiconductor film 103b It is possible to reduce the amount of impurities mixed in. In addition, the exhaust system uses an adsorption type vacuum pump (e.g. By using a cryopump, impurities such as alkali metals and hydrogen can be prevented from flowing back from the exhaust system. can be reduced.
[0073] In addition, when the first oxide semiconductor film 103a and the second oxide semiconductor film 103b are formed, The gas introduced into the processing chamber of the sputtering device, such as nitrogen gas, oxygen gas, or argon gas, The deposition may be performed by introducing a heated gas such as nitrogen gas. The hydrogen content in the conductive film 103a and the second oxide semiconductor film 103b is reduced. can be done.
[0074] In addition, the first oxide semiconductor film 103a and the second oxide semiconductor film 103b are formed by a sputtering method. Before forming the film 103b, the sputtering device, the target surface or the inside A preheat treatment may be performed to remove moisture or hydrogen. The hydrogen content in the first oxide semiconductor film 103a and the second oxide semiconductor film 103b is reduced. It is possible.
[0075] Through the above steps, the oxide semiconductor film 104a having the first crystal structure and the oxide semiconductor film 104b having the second crystal structure are formed. In addition, the oxide semiconductor film 104b can be formed by adding hydrogen to the oxide semiconductor. If they are included, some of them will become donors and generate electrons as carriers. Similarly, oxygen defects in oxide semiconductors act as donors and generate electrons as carriers. Therefore, the oxide semiconductor film 104a having the first crystal structure and the oxide semiconductor film 104b having the second crystal structure are When the hydrogen concentration or oxygen vacancies in the oxide semiconductor film 104b are reduced, the capacitance in the oxide semiconductor film 104b is reduced. The rear concentration can be reduced, resulting in a negative threshold voltage for the transistors that will be fabricated later. The shift can be reduced.
[0076] <Hexagonal crystal structure> Here, the hexagonal crystal structure will be described below.
[0077] First, the second crystal structure oriented along the c-axis will be described with reference to FIG. Regarding the crystal structure, the structure on the ab plane as viewed from the c-axis direction is shown in Fig. 3(A), and the structure on the ab plane as viewed from the c-axis direction is shown in Fig. 3(B). The vertical structure is shown in FIG.
[0078] Examples of crystals having the second crystal structure include zinc oxide, indium nitride, and gallium nitride. In addition, oxide semiconductors containing nitrogen, i.e., oxynitride semiconductors, also have a c-axis oriented second crystal structure. In some cases, the resulting film has a crystal structure.
[0079] Specifically, nitrogen is 5×10 19 / cm 3 More than 1×10 20 / cm 3 2 more The In-Ga-Zn-O film containing less than 0 atomic percent of In is a film having a second crystal structure oriented along the c-axis. The crystal plane of In-O (crystal plane containing indium and oxygen) and the crystal plane of In-O (crystal plane containing indium The layer is provided between the first surface (the crystal plane containing oxygen) and the second surface (the crystal plane containing Ga and Zn).
[0080] Next, the first crystal structure of the c-axis oriented hexagonal system will be described.
[0081] For example, nitrogen is 1×10 17 / cm 3 5×10 or more 19 / cm 3 Less than In-Ga-Z The nO film has a first crystal structure of the hexagonal system oriented along the c-axis. The In-Ga-Zn-O film having the first crystal structure of the crystal system has the In-O crystal plane on the ab plane. (crystal planes containing indium and oxygen) between the In-O crystal planes The two layers having Ga and Zn are provided on the substrate. In the above, Ga and Zn may be present in one or both layers, and the positions thereof are not limited. I can't.
[0082] The second crystal structure and the first crystal structure are both hexagonal crystal systems, and the atomic structure is in the ab plane. The molecules are arranged in a hexagonal shape. The first crystal structure of the hexagonal system then contacts the second crystal structure, forming a hexagonal A rhombohedral first crystal structure matches the second crystal structure.
[0083] On top of the first crystal structure oriented along the c-axis, a second crystal structure with a hexagonal crystal system oriented along the c-axis with the same lattice constant is layered. FIG. 4 shows how the crystal structures of the first and second crystal structures 200 are aligned in a hexagonal crystal system aligned along the c-axis. 4(A) shows a first crystal structure 2001 aligned along the c-axis, and FIG. 4(B) shows a second crystal structure 2001 aligned along the c-axis. The second crystal structure 2000 of the hexagonal crystal system is in contact with the first crystal structure 2001, and the first crystal structure 2001 of the hexagonal crystal system is FIG. 4(C) shows a schematic diagram of the alignment of the crystal structure 2001 of the first crystal structure with the second crystal structure 2000. As shown in.
[0084] In this way, the first crystal structure 2001 of the hexagonal system is in contact with the second crystal structure 2000, The alignment of the first crystal structure 2001 of the system to the second crystal structure 2000 results in a crystalline A layer including a second crystal structure 2000 having a high crystallinity and easy crystallization with a c-axis orientation is used as a seed crystal layer. Then, an oxide semiconductor film is formed in contact with the seed crystal layer. The second crystal structure 2000 contained in the seed crystal layer facilitates crystallization of the oxide semiconductor film. This has the effect of:
[0085] <Seed crystal layer> Next, the seed crystal layer will be described. The seed crystal layer includes a second crystal structure oriented along the c-axis. The seed crystal layer is formed using a material that has higher crystallinity and is easily crystallized as compared with the oxide semiconductor film.
[0086] A second c-axis oriented crystal structure that can be used for the seed crystal layer is described below.
[0087] Examples of compounds that have a c-axis oriented second crystal structure and can be used for the seed crystal layer include Examples include zinc oxide, indium nitride, and gallium nitride. Nitrogen 5×10 19 / cm 3 More than 1×10 20 / cm 3 Contains less than 7 atomic% In some cases, an oxide semiconductor including the oxide semiconductor layer may also be a film including the second crystal structure having a c-axis alignment.
[0088] When a nitrogen-containing oxide semiconductor is used for the seed crystal layer, the nitrogen concentration is 5×10 19 / cm 3 End , preferably 1 x 10 20 / cm 3 Nitrogen is intentionally included so that its content is more than 7 atomic %. The oxide semiconductor film in which nitrogen is intentionally contained in this range is similar to the oxide semiconductor film in which nitrogen is not intentionally contained. Compared to solid semiconductor films, it has a smaller energy gap and allows carriers to flow more easily.
[0089] The second crystal structure, HAADF (high-angle annular dot) with c-axis orientation, In the actual observation image of a dark field STEM, bright spots appear alternately in the diffraction pattern. may be observed.
[0090] Actual HAADF-STEM image obtained by calculation based on the c-axis oriented second crystal structure is shown in Figure 5(A).
[0091] In addition, the HAADF- The actual STEM image is shown in Figure 5(B).
[0092] The actual HAADF-STEM images shown in Fig. 5(A) and Fig. 5(B) each have two periods. It can be confirmed that the crystalline structure has a second crystal structure oriented along the c-axis and has a layer structure having a good adhesion.
[0093] The nitrogen-containing In-Ga-Zn-O film was formed on a quartz glass substrate by sputtering. The target was In:Ga:Zn=1:1:1[a tom ratio] was used, the distance between the substrate and the target was set to 60 mm, and a DC power supply was used to obtain a 0.5 The film was formed at a power of 1000 kW and a pressure of 0.4 Pa. The substrate temperature during film formation was set to 400 degrees. The sputtering gas was nitrogen alone, and was flowed into the film formation chamber at a flow rate of 40 sccm.
[0094] <Oxide semiconductor film> Next, the oxide semiconductor film will be described. The entire conductor film is not in an amorphous state, but is at least hexagonal with a c-axis orientation. The first crystal structure of the system includes crystals that are anisotropically grown from a seed crystal layer. Since the entire conductor film is not in an amorphous state, the electrical characteristics are unstable. The formation of is suppressed.
[0095] A first crystal structure having anisotropy along the c-axis that can be used for an oxide semiconductor film is described. He explains.
[0096] The first crystal structure of the hexagonal system is the YbFe2O4 type structure, the Yb2Fe3O7 type structure, and Examples include the ternary metal oxide I n-Ga-Zn-O has a first crystal structure of a hexagonal system and can be used for an oxide semiconductor film. Note that an In-Ga-Zn-O film that can be used for the oxide semiconductor film is a nitrogen-doped film. 1×10 17 / cm 3 5×10 or more 19 / cm 3 It may also include the following:
[0097] The ternary metal oxide In-Ga-Zn-O contains In, which has a YbFe2O4 type structure. GaZnO4 and In2Ga2ZnO7, which has a Yb2Fe3O7 structure. M. Nakamura, N. Kimizuka, a nd T. Mohri, “The Phase Relations in th e In2O3-Ga2ZnO4-ZnO System at 1350 degrees,” J. Solid State Chem., 1991, Vol.93, p.298-315 It is described in.
[0098] In addition, the oxide semiconductor film includes the In-Sn-Ga-Zn-O film, which is an oxide of a quaternary metal. Ternary metal oxide films such as In-Ga-Zn-O, In-Sn-Zn-O, and In-A l-Zn-O film, Sn-Ga-Zn-O film, Al-Ga-Zn-O film, Sn-Al-Zn -O film, and binary metal oxide films such as In-Zn-O film, Sn-Zn-O film, and Al-Zn In the oxide semiconductor film, a silicon-based film, an In-Ga-O film, an In-Ga-O film, or the like can be used. Here, for example, the In-Ga-Zn-O film may include indium (In), It is an oxide film containing gallium (Ga) and zinc (Zn).
[0099] In the oxide semiconductor film, crystals grow anisotropically from a seed crystal layer. The semiconductor film having the B-structure can have a highly crystalline region in contact with an insulating surface. This reduces the number of interface states due to dangling bonds, resulting in a heterostructure with good interface conditions. It is possible to provide a semiconductor film that
[0100] In addition, the high-angle adiabatic doping factor (HAADF) of the first crystal structure of the c-axis-oriented hexagonal system is In real observation images using a uniaxial dark field (SDF)-STEM, one in three images are bright and dark. Accompanying diffraction patterns may be observed.
[0101] HAADF-STEM calculated based on the first crystal structure of the c-axis-oriented hexagonal system The actual observed image is shown in FIG. 6(A).
[0102] Moreover, an actual HAADF-STEM image of the In-Ga-Zn-O film is shown in Figure 6(B).
[0103] The actual HAADF-STEM images shown in Figure 6(A) and 6(B) are divided into three parts. The first crystal of the c-axis-oriented hexagonal system with one bright and dark region and a nine-periodic layer structure It can be confirmed that it has the structure.
[0104] The In-Ga-Zn-O film was formed by sputtering on a quartz glass substrate at 300 nm. The film was deposited to a thickness of 100 nm. The target was In:Ga:Zn = 1:1:1 [atom ratio] The distance between the substrate and the target was set to 60 mm, and a DC power supply was used with a power of 0.5 kW. The film was formed at a pressure of 0.4 Pa. The substrate temperature during film formation was set to 400°C. The gas used was oxygen alone, and it was flowed into the deposition chamber at a flow rate of 40 sccm.
[0105] Next, a mask is formed over the oxide semiconductor film 104b having the second crystal structure. The oxide semiconductor film 104a having a first crystal structure and the oxide semiconductor film 104b having a second crystal structure are formed by using a mask. The oxide semiconductor film 104b is selectively etched to form an oxide semiconductor film having a first crystal structure. The oxide semiconductor film 105a having the first crystal structure and the oxide semiconductor film 105b having the second crystal structure are formed. The oxide semiconductor film 105a having the first crystal structure and the oxide semiconductor film 105b having the second crystal structure are 05b are collectively referred to as an oxide semiconductor stack 105. After that, the mask is removed.
[0106] The oxide semiconductor film 104a having a first crystal structure and the oxide semiconductor film 104b having a second crystal structure The mask for etching the film 104b is formed by a photolithography process, an inkjet A deposition method, a printing method, or the like can be used as appropriate. The oxide semiconductor film 104a having the second crystal structure and the oxide semiconductor film 104b having the second crystal structure are etched by wet etching. Etching or dry etching can be used as appropriate.
[0107] Next, a pair of electrodes 106 are formed in contact with the oxide semiconductor stack 105. A gate insulating film 107 is formed on the insulating film 102, the oxide semiconductor stack 105, and the pair of electrodes 106. Next, a gate electrode 108 is formed on the gate insulating film 107. An insulating film 109 may be formed over the insulating film 107 and the gate electrode 108 (see FIG. 2C). .).
[0108] The pair of electrodes 106 function as a source electrode and a drain electrode.
[0109] The pair of electrodes 106 may be made of aluminum, chromium, copper, tantalum, titanium, molybdenum, or titanium. or an alloy containing the above-mentioned metal elements, It can be formed by using an alloy of metal elements. One or more of the metallic elements selected from the group consisting of nesium, zirconium, and beryllium The pair of electrodes 106 may have a single-layer structure or a laminated structure of two or more layers. For example, a single layer structure of an aluminum film containing silicon, a titanium film on an aluminum film, A two-layer structure in which a titanium film is laminated on a titanium nitride film, a two-layer structure in which a titanium film is laminated on a titanium nitride film, Two-layer structure with tungsten film laminated, two-layer structure with tungsten film laminated on tantalum nitride film Structure: titanium film, aluminum film laminated on the titanium film, titanium film on top of that There are also three-layer structures that form aluminium, titanium, tantalum, tungsten, etc. A film of an element selected from the group consisting of fluorine, molybdenum, chromium, neodymium, and scandium, or a combination of elements. Alternatively, a nitride film or an alloy film made of a combination of the two electrodes 106 may be used. When copper is used as the electrode, a copper magnesium aluminum layer is formed in contact with the oxide semiconductor stack 105. A copper layer is provided in contact with the copper-magnesium-aluminum alloy layer. can be used.
[0110] The pair of electrodes 106 is made of indium oxide, indium tin oxide, or indium oxide containing tungsten oxide. oxide, indium zinc oxide with tungsten oxide, indium oxide with titanium oxide Indium tin oxide, indium zinc oxide, silicon oxide are added. A light-transmitting conductive material such as indium tin oxide can also be used. A laminate structure of the above-mentioned light-transmitting conductive material and the above-mentioned metal element may also be used.
[0111] The pair of electrodes 106 are formed by a printing method or an inkjet method. After forming a conductive film by a deposition method, a CVD method, a vapor deposition method, or the like, a mask is formed on the conductive film. The conductive film is etched. The mask formed on the conductive film is printed or inkjet printed. A deposition method or a photolithography method can be appropriately used.
[0112] Note that after a conductive film is formed over the oxide semiconductor film 104b having the second crystal structure, A mask having a concave and convex shape is formed by a photomask, and a first crystal structure is formed by using the mask. an oxide semiconductor film 104a having a second crystal structure, an oxide semiconductor film 104b having a second crystal structure, After etching the conductive film, the uneven mask is separated by ashing, and the separated The conductive film is selectively etched using the mask, whereby the oxide semiconductor stack 105 and By this process, the number of photomasks and the number of photoelectrodes can be reduced. The number of lithography steps can be reduced.
[0113] The gate insulating film 107 may be a silicon oxide film, a silicon oxynitride film, a silicon nitride film, or a nitride oxide film. a silicon oxide film, an aluminum oxide film, an aluminum oxynitride film, or a gallium oxide film. The gate insulating film 107 may be formed as a single layer or a multilayer. It is preferable that the portion in contact with the laminated body 105 contains oxygen, and it is particularly preferable that the portion contains an oxide insulating film. The silicon oxide film is formed from an oxide insulating film that releases oxygen when heated, similar to the silicon oxide film 102. By using the above, oxygen can be diffused into the oxide semiconductor stack 105, and the characteristics can be improved. It can be.
[0114] The gate insulating film 107 is made of hafnium silicate (HfSiO x ) membrane, nitrogen added Added hafnium silicate (HfSi x O y N z ) film, nitrogen-doped hafnium Aluminate (HfAl x O y N z ) film, hafnium oxide film, yttrium oxide film, etc. The use of high-k material films can reduce gate leakage. Material film, silicon oxide film, silicon oxynitride film, silicon nitride film, silicon nitride oxide film , an aluminum oxide film, an aluminum oxynitride film, or a gallium oxide film. The gate insulating film 107 may have a thickness of 1 nm to 300 nm. More preferably, it is set to 5 nm or more and 50 nm or less.
[0115] The gate insulating film 107 is formed by a sputtering method, a CVD method, or the like.
[0116] Before forming the gate insulating film 107, the surface of the oxide semiconductor stack 105 is treated with oxygen, The surface of the oxide semiconductor laminate 105 is exposed to plasma of an oxidizing gas such as ozone or dinitrogen monoxide. The surface may be oxidized to reduce oxygen defects.
[0117] The gate electrode 108 may be made of any of a variety of materials including aluminum, chromium, copper, tantalum, titanium, molybdenum, and titanium. a metal element selected from the group consisting of tin, an alloy containing the above-mentioned metal element, and In addition, it can be formed by using an alloy of manganese, magnesium, etc. The present invention may be modified by using one or more metal elements selected from the group consisting of tungsten, zirconium, and beryllium. The gate electrode 108 may have a single-layer structure or a laminated structure of two or more layers. For example, a single-layer structure of an aluminum film containing silicon, a titanium film laminated on an aluminum film, A two-layer structure in which a titanium film is laminated on a titanium nitride film; a two-layer structure in which a tungsten film is laminated on a titanium nitride film; A two-layer structure in which a tungsten film is laminated on a tantalum nitride film; a two-layer structure in which a tungsten film is laminated on a tantalum nitride film; A titanium film is laminated on the titanium film, an aluminum film is laminated on the aluminum film, and a titanium film is formed on the aluminum film. There are also three-layer structures that use aluminum, titanium, tantalum, tungsten, and molybdenum. A film of elements selected from the group consisting of butanol, chromium, neodymium, and scandium, or a combination of multiple elements. Alternatively, an alloy film or a nitride film may be used.
[0118] The gate electrode 108 is made of indium tin oxide or indium oxide containing tungsten oxide. oxide, indium zinc oxide with tungsten oxide, indium oxide with titanium oxide Indium tin oxide, indium zinc oxide, silicon oxide are added. A light-transmitting conductive material such as indium tin oxide can also be used. A laminate structure of the above-mentioned light-transmitting conductive material and the above-mentioned metal element may also be used.
[0119] In addition, between the gate electrode 108 and the gate insulating film, as a material layer in contact with the gate insulating film, Nitrogen-containing In-Ga-Zn-O films, nitrogen-containing In-Sn-O films, and nitrogen-containing In -Ga-O film, In-Zn-O film containing nitrogen, Sn-O film containing nitrogen, It is preferable to provide an In-O film or a metal nitride film (InN, ZnN, etc.). The work function is 5 eV or more, preferably 5.5 eV or more, and the threshold of the electrical characteristics of the transistor is This makes it possible to realize a so-called normally-off switching element. For example, when an In-Ga-Zn-O film containing nitrogen is used, at least an oxide semiconductor A nitrogen concentration higher than that of the laminate 105, specifically, an In-Ga-Zn-O film having a nitrogen concentration of 7 atomic % or more is used. There are.
[0120] The gate electrode 108 is formed by a printing method or an inkjet method. After forming a conductive film by a deposition method, a CVD method, a vapor deposition method, or the like, a mask is formed on the conductive film. The conductive film is etched. The mask formed on the conductive film is printed or inkjet printed. A deposition method or a photolithography method can be appropriately used.
[0121] The insulating film 109 can be formed by appropriately using the insulating films listed for the gate insulating film 107. In addition, when a silicon nitride film is formed as the insulating film 109 by a sputtering method, It is possible to prevent the intrusion of moisture and alkali metals from the outside, and the oxide semiconductor laminate The impurity content of the body 105 can be reduced.
[0122] After the gate insulating film 107 or the insulating film 109 is formed, the insulating film 109 is heated to a temperature of 100° C. In an atmosphere free of moisture (nitrogen atmosphere, oxygen atmosphere, dry air atmosphere (for example, dew point Heat treatment (temperature range 150 degrees or higher) at -40 degrees or lower, preferably at a dew point of -60 degrees or lower 650° C. or less, preferably 200° C. or more and 500° C. or less).
[0123] Through the above steps, trigonal and A transistor having a channel made of an oxide semiconductor stack having a hexagonal crystal structure. It can be made.
[0124] In the oxide semiconductor stack described in this embodiment, a region in the vicinity of the interface with the gate insulating film The high crystallinity and uniformity of the material allow for stable electrical characteristics, resulting in highly reliable transistors. It is also possible to obtain a trigonal structure having hexagonal bonds on the ab plane and oriented along the c axis. The oxide semiconductor stack having crystals with a lattice structure and / or a hexagonal crystal structure is used as a channel region of a transistor. By using this in the region, it is possible to measure the temperature before and after light irradiation of the transistor or the bias-thermal stress (BT) The transistor threshold voltage changes little before and after the test, and the electrical characteristics are stable. Therefore, a transistor having the above characteristics can be manufactured.
[0125] (Embodiment 2) In this embodiment mode, a structure and a manufacturing method of a transistor different from those in Embodiment 1 will be described. 7 and 8. In this embodiment, a stack of an oxide insulating film and an oxide semiconductor The difference from the first embodiment is that a pair of electrodes is provided between the electrodes. The cross-sectional view of the dashed line CD in FIG. 7(A) corresponds to FIG. 7(B). In FIG. 7(A), 1, the oxide insulating film 102, the gate insulating film 117, and the insulating film 119 are omitted. 7B is a cross-sectional view illustrating a manufacturing process of the transistor shown in FIG.
[0126] The transistor shown in FIG. 7B includes an oxide insulating film 102 formed over a substrate 101 and an oxide A pair of electrodes functioning as a source electrode and a drain electrode formed on the oxide insulating film 102. 116, an oxide insulating film 102, and a pair of electrodes functioning as a source electrode and a drain electrode. The oxide semiconductor laminate 115 covers the pair of electrodes 116, the oxide insulating film 102, and the pair of electrodes 116. 1, a gate insulating film 117 formed on the oxide semiconductor stack 115, and a gate insulating film 1 A gate electrode 118 overlaps with the oxide semiconductor stack 115 with the gate electrode 17 interposed therebetween. An insulating film 119 may be provided to cover the gate insulating film 117 and the gate electrode 118. In the opening of the insulating film 119, a pair of wirings 120 contacting the pair of electrodes 116 may be provided. good.
[0127] The oxide semiconductor stack 115 includes a first insulating film 114 and a second insulating film 115a. The oxide semiconductor film 115a having a crystal structure and the oxide semiconductor film 115b having a first crystal structure are and an oxide semiconductor film 115b having a second crystal structure which is in contact with the oxide semiconductor film 115a. It is characterized by:
[0128] In addition, the oxide semiconductor film 115b having the second crystal structure is used as a seed crystal to grow the oxide semiconductor film 115b having the first crystal structure. The oxide semiconductor film 115a has a crystal growth.
[0129] Similarly to Embodiment 1, the oxide semiconductor film having the second crystal structure and the first crystal structure is Both are trigonal and / or hexagonal, so a hexagonal lattice image can be seen from the c-axis direction. .
[0130] Note that the oxide semiconductor film 115a having the first crystal structure and the oxide semiconductor film 115b having the second crystal structure The semiconductor film 115b is non-single crystal, and the entire oxide semiconductor film is in an amorphous state ( It is not in an amorphous state, but has crystals oriented along the c-axis.
[0131] Next, a manufacturing method of the transistor shown in FIG. 7B will be described with reference to FIGS.
[0132] As shown in FIG. 8A, an oxide insulating film 102 is formed on a substrate 101 in the same manner as in the first embodiment. Next, a pair of electrodes 116 is formed over the oxide insulating film 102. A first oxide semiconductor film 113a and a second oxide semiconductor film 113b are formed on the electrode 116 and the oxide insulating film 102. A semiconductor film 113b is formed.
[0133] The pair of electrodes 116 is formed using the same material and method as the pair of electrodes 106 described in Embodiment 1. It can be formed by using appropriate materials.
[0134] The first oxide semiconductor film 113a and the second oxide semiconductor film 113b have the same structure as those described in Embodiment 1. The first oxide semiconductor film 103a and the second oxide semiconductor film 103b are formed using the same materials and processes. It can be formed by using an appropriate manufacturing method.
[0135] Next, a first heat treatment is performed in the same manner as in the first embodiment. Crystal growth starts from the surface of the first oxide semiconductor film 113b toward the first oxide semiconductor film 113a. The second oxide semiconductor film 113b is an oxide semiconductor film 114b having a second crystal structure. The oxide semiconductor film 114b having the second crystal structure has crystals aligned along the c-axis. do.
[0136] Then, a first heat treatment is performed to form an oxide semiconductor film 114b having a second crystal structure. The crystal growth of the first oxide semiconductor film 113a is performed by using an oxide having a second crystal structure as a seed. The oxide insulating film 102 is then formed by adsorbing the first crystal structure on the oxide insulating film 102. In addition, an oxide semiconductor film 114a having a first crystal structure is formed. The film 114a has crystals oriented along the c-axis (see FIG. 8(B)).
[0137] Through the above steps, the oxide semiconductor film 114a having the first crystal structure and the oxide semiconductor film 114b having the second crystal structure are obtained. In this way, the oxide semiconductor film 114b can be formed.
[0138] Next, a mask is formed over the oxide semiconductor film 114b having the second crystal structure. The oxide semiconductor film 114a having a first crystal structure and the oxide semiconductor film 114b having a second crystal structure are formed by using a mask. The oxide semiconductor film 114b is selectively etched to form an oxide semiconductor film having a first crystal structure. The oxide semiconductor film 115a having the first crystal structure and the oxide semiconductor film 115b having the second crystal structure are formed. The oxide semiconductor film 115a having the first crystal structure and the oxide semiconductor film 115b having the second crystal structure are 15b are collectively referred to as an oxide semiconductor stack 115. After that, the mask is removed.
[0139] Next, a gate electrode was formed on the oxide insulating film 102, the pair of electrodes 116, and the oxide semiconductor stack 115. Next, a gate electrode 118 is formed on the gate insulating film 117. .
[0140] Thereafter, an insulating film 119 is formed on the gate insulating film 117 and the gate electrode 118. Next, After forming a mask on the insulating film 119, the gate insulating film 117 and a part of the insulating film 119 are etched. Then, the pair of electrodes 116 are connected through the openings. A wiring 120 may be formed (see FIG. 8C).
[0141] The gate insulating film 117 is formed using a material and a method similar to those of the gate insulating film 107 described in Embodiment 1. The method can be appropriately used to form the film.
[0142] The gate electrode 118 is formed using the same material and method as the gate electrode 108 described in Embodiment 1. It can be formed by using appropriate materials.
[0143] The insulating film 119 is formed using a material and a method similar to those of the insulating film 109 described in Embodiment 1. It can be formed by:
[0144] The wiring 120 can be formed by appropriately using a material and a manufacturing method similar to those of the pair of electrodes 116. can.
[0145] Through the above steps, trigonal and and / or a transistor having an oxide semiconductor stack having a hexagonal crystal structure in a channel region. It is possible to create a data.
[0146] In the oxide semiconductor stack described in this embodiment, a region in the vicinity of the interface with the gate insulating film The high crystallinity and uniformity of the material allow for stable electrical characteristics, resulting in highly reliable transistors. It is also possible to obtain a trigonal structure having hexagonal bonds on the ab plane and oriented along the c axis. The oxide semiconductor stack having crystals with a lattice structure and / or a hexagonal crystal structure is used as a channel region of a transistor. By using it in the region, light irradiation or bias-thermal stress (BT) test for transistors can be performed. The amount of change in the threshold voltage of the transistor is small before and after the change, and stable electrical characteristics are maintained. It is possible to manufacture a transistor having such a structure.
[0147] Note that this embodiment mode can be appropriately combined with other embodiment modes.
[0148] (Embodiment 3) In this embodiment, a transistor including an oxide semiconductor film as a channel and a manufacturing method thereof will be described. 9 and 10. FIG. 9B shows one mode of the structure of a semiconductor device. FIG. 9(A) is a cross-sectional view illustrating a structure of a certain transistor, and is a top view of the transistor. 9A corresponds to a cross-sectional view taken along line 9A-B. In FIG. 9B, the gate insulating film 107 and the insulating film 109 are omitted. 1A to 1C are cross-sectional views illustrating a manufacturing process of a transistor.
[0149] The transistor shown in FIG. 9B includes an oxide insulating film 102 formed over a substrate 101 and an oxide The oxide semiconductor stack 105 formed on the oxide insulating film 102 and the oxide semiconductor stack 10 A pair of electrodes 106 functioning as a source electrode and a drain electrode formed on the oxide film 5, A gate electrode formed on the oxide insulating film 102, the oxide semiconductor laminate 105, and the pair of electrodes 106. a gate insulating film 107 overlapping with the oxide semiconductor stack 105 via the gate insulating film 107; The gate electrode 108 is covered with a gate insulating film 107. It may have a membrane 109 .
[0150] The oxide semiconductor stack 105 is an oxide semiconductor layer having a first crystal structure in contact with the oxide insulating film 102. a second oxide semiconductor film in contact with the oxide semiconductor film having the first crystal structure; The oxide semiconductor film 105b having a crystal structure and the oxide semiconductor film 105 having a second crystal structure a third oxide semiconductor film 105c having a crystal structure in contact with the gate insulating film 107 and the second oxide semiconductor film 105b; The present invention is characterized in that the above are laminated.
[0151] That is, the oxide semiconductor film 105b having the second crystal structure is provided above and below the oxide semiconductor film 105b having the first crystal structure. The oxide semiconductor film 105a and the oxide semiconductor film 105c having the third crystal structure are included.
[0152] In addition, the oxide semiconductor film 105b having the second crystal structure is used as a seed crystal to grow the oxide semiconductor film 105b having the first crystal structure. and an oxide semiconductor film 105c having a third crystal structure. Each of them is characterized by crystal growth.
[0153] The oxide semiconductor film 105a having a first crystal structure and the oxide semiconductor film 105b having a third crystal structure The crystal structure of the film 105c is trigonal and / or hexagonal, and has a YbFe2O4 type structure, Yb It has either a 2Fe3O7 type structure or a non-wurtzite type structure. is a trigonal and / or hexagonal non-wurtzite crystal structure.
[0154] The crystal structure of the oxide semiconductor film 105b having the second crystal structure is trigonal and / or It has a wurtzite structure, which is a hexagonal crystal structure.
[0155] That is, the oxide semiconductor film having the first crystal structure to the oxide semiconductor film having the third crystal structure Since both films are trigonal and / or hexagonal, a hexagonal lattice image can be confirmed from the c-axis direction. can.
[0156] Note that the oxide semiconductor film 105a having the first crystal structure and the oxide semiconductor film 105b having the second crystal structure The oxide semiconductor film 105b having the third crystal structure and the oxide semiconductor film 105c having the third crystal structure are each a non-crystalline semiconductor film. The oxide semiconductor film is crystalline, and the entire oxide semiconductor film is not in an amorphous state, but has a c-axis orientation. In other words, it has an amorphous region and a crystalline region with a c-axis orientation.
[0157] Next, a manufacturing method of the transistor shown in FIG. 9B will be described with reference to FIGS.
[0158] As shown in FIG. 10A, similarly to the first embodiment, an oxide insulating film 102 is formed on a substrate 101. After the formation of the first oxide semiconductor film 103a, the first oxide semiconductor film 103a is formed over the oxide insulating film 102. A second oxide semiconductor film 103b is formed over the oxide semiconductor film 103a.
[0159] The oxide insulating film 102 is formed using an oxide insulating film from which part of oxygen is released by heating. As for the oxide insulating film from which part of the oxygen is released by heating, the oxygen content is higher than that which satisfies the stoichiometric ratio. It is preferable to use an oxide insulating film that contains as much oxygen as possible. The oxide insulating film is heated to form the first oxide semiconductor film 103a and the second oxide semiconductor film 103b. The oxide insulating film 102 can be typically formed of an oxide Silicon, silicon oxynitride, silicon nitride oxide, aluminum oxide, aluminum oxynitride The oxide can be formed of tungsten oxide, gallium oxide, hafnium oxide, yttrium oxide, or the like.
[0160] The oxide insulating film 102 has a thickness of 50 nm or more, preferably 200 nm or more and 500 nm or less. By increasing the thickness of the oxide insulating film 102, the amount of oxygen released from the oxide insulating film 102 can be increased. At the same time, the oxide insulating film 102 can be formed at the interface with the oxide semiconductor film to be formed later. It is possible to reduce defects in the
[0161] The oxide insulating film 102 is formed by a sputtering method, a CVD method, or the like. The oxide insulating film from which part of the oxygen is released can be easily formed by using a sputtering method. Therefore, it is preferable.
[0162] When an oxide insulating film that releases some oxygen by heating is formed by a sputtering method, The deposition gas preferably contains a large amount of oxygen, and is preferably a mixture of oxygen and a rare gas. Typically, the oxygen concentration in the deposition gas is set to 6% or more and 100% or less. It is preferable that
[0163] The first oxide semiconductor film 103a is heated to have a trigonal and / or hexagonal crystal structure and a non- Wurtzite type, YbFe2O4 type structure, Yb2Fe3O7 type structure, or any of their modified structures The insulating film is formed using an oxide semiconductor film that can have one of the crystal structures.
[0164] As an example of an oxide semiconductor film having the first crystal structure, an oxide of a ternary metal, In-G The a-Zn-O film has a trigonal and / or hexagonal non-wurtzite crystal structure. The In-Ga-Zn-O film, which is an oxide of InGa-Zn-O, has a YbFe2O4 structure. aZnO4, and In2Ga2ZnO7, which has a Yb2Fe3O7 type structure, and its variants It can take the type structure (M. Nakamura, N. Kimizuka, and T. Mohri, “The Phase Relations in the In 2O3-Ga2ZnO4-ZnO System at 1350 degrees”, J. Soli d State Chem., 1991, Vol.93, p.298-315).
[0165] The first oxide semiconductor film 103a is made of an oxide of a quaternary metal, In—Sn—Ga— Zn-O film, In-Ga-Zn-O film, which is an oxide of a ternary metal, In-Sn-Zn- O film, In-Al-Zn-O film, Sn-Ga-Zn-O film, Al-Ga-Zn-O film, S n-Al-Zn-O film, In-Zn-O film, which is an oxide of binary metals, and Sn-Zn-O A film, an Al-Zn-O film, an In-Ga-O film, or the like can be used. The semiconductor may contain SiO2. For example, an In-Ga-Zn-O film is an In-Ga-Zn-O film. The oxide film contains indium (In), gallium (Ga), and zinc (Zn). The oxide semiconductor film 103a is formed by adding 1×10 17 / cm 3 5×10 or more 19 / cm 3 It may contain less than 10000000 nitrogen.
[0166] Note that a metal oxide that can be formed in the first oxide semiconductor film 103a has an energy The gap is 2 eV or more, preferably 2.5 eV or more, and more preferably 3 eV or more. In this way, by using an oxide semiconductor with a wide energy gap, The leakage current can be reduced.
[0167] The second oxide semiconductor film 103b is an oxide semiconductor film that can have a wurtzite crystal structure by heating. The oxide semiconductor film that can have a wurtzite crystal structure is a trigonal and / or hexagonal crystal structure, It is easily oxidized and has high crystallinity.
[0168] The second oxide semiconductor film 103b can be made of zinc oxide, an oxynitride semiconductor, or the like. The oxynitride semiconductor can be formed by adding 5× the metal oxides listed for the first oxide semiconductor film 103a. 10 19 / cm 3 More than 1×1020 / cm 3 Addition of nitrogen of 7 atomic % or less It can be formed as follows.
[0169] The second oxide semiconductor film 103b is a semiconductor film including the first oxide semiconductor film 103a and a semiconductor film to be formed later. The third oxide semiconductor film 103c is used as a seed for crystal growth. The thickness may be set to a value within a range of, typically, one atomic layer to 10 nm, and preferably, 2 nm to 5 nm. The thickness of the second oxide semiconductor film 103b can be reduced by reducing the thickness of the film formation process and the heating process. The processing throughput can be increased.
[0170] The first oxide semiconductor film 103a and the second oxide semiconductor film 103b are each formed by sputtering. The film can be formed by a ring method, a coating method, a printing method, a pulsed laser deposition method, or the like. The first oxide semiconductor film 103a and the second oxide semiconductor film 103b were formed by a quenching method. When forming a film, either an AC sputtering device, a DC sputtering device, or an RF sputtering device can be used. One of the sputtering devices is used.
[0171] Note that the second oxide semiconductor film 103b is formed of an oxynitride semiconductor by a sputtering method. In this case, after the first oxide semiconductor film 103a is formed, the gas to be introduced into the sputtering apparatus is By switching the type of gas, i.e. by introducing nitrogen, an oxynitride semiconductor can be formed. That is, the first oxide semiconductor film 103a and the second oxide semiconductor film 103b are successively formed. This makes it possible to manufacture the device with excellent mass productivity.
[0172] Next, a first heat treatment is performed in the same manner as in the first embodiment.
[0173] By the first heat treatment, the first oxide semiconductor film 103b is Crystal growth starts toward the second oxide semiconductor film 103a. The second oxide semiconductor film 103b is easily crystallized. Therefore, the second oxide semiconductor film 103b is entirely crystallized and has a wurtzite crystal structure. The second oxide semiconductor film 102 is formed as an oxide semiconductor film 104b having the crystal structure of the second oxide semiconductor film 102. Since crystals grow from the surface of 3b toward the first oxide semiconductor film 103a, the c-axis oriented That is, the oxide semiconductor film 104b having the second crystal structure has a crystal structure in the ab plane. In addition, the layer having the hexagonal bonds has a thickness of They are stacked and bonded in the c-axis direction and are c-axis oriented.
[0174] By continuing the first heat treatment, the oxide semiconductor film 104b having the second crystal structure is grown. As a result, the crystal growth of the first oxide semiconductor film 103a becomes an oxide semiconductor having a second crystal structure. The second crystal structure is formed by adsorbing the oxide insulating film 102 on the oxide insulating film 102. Since the oxide semiconductor film 104b has a c-axis orientation, the oxide semiconductor film 104b has the second crystal structure. The oxide semiconductor film 104b is used as a seed to form the oxide semiconductor film 104b having the second crystal structure. The crystal of the first oxide semiconductor film 103a can be grown so that the crystal axis of the first oxide semiconductor film 103a is substantially the same as that of the first oxide semiconductor film 103b. That is, the first oxide semiconductor film 103a can be grown as a crystal with the c-axis orientation. That is, the oxide semiconductor film 104a having the first crystal structure has a crystal structure in the ab-plane. In the plane of the film, the layers have hexagonal bonds. The layers are laminated and bonded in the c-axis direction, and are c-axis oriented. It is possible to form an oxide semiconductor film 104a having a first oriented crystal structure (FIG. 1 See 0(B). ).
[0175] Note that the first heat treatment causes crystals to grow vertically from the surface of the second oxide semiconductor film 103b. When grown, the oxide semiconductor film 104a having a first crystal structure and the oxide semiconductor film 104b having a second crystal structure are formed. The c-axis of the oxide semiconductor film 104b is approximately perpendicular to the surface.
[0176] In addition, the first oxide semiconductor film 103a and the second oxide semiconductor film 103b are formed by the first heat treatment. The hydrogen contained in the membrane 103b is released (i.e., dehydrogenated or dehydrated), and the oxygen is released. Part of the oxygen contained in the oxide semiconductor insulating film 102 is mixed with the first oxide semiconductor film 103a and the second oxide semiconductor film 103b. The first oxide semiconductor film 103b in the oxide insulating film 102 and the second oxide semiconductor film 103a in the oxide insulating film 102 are Through this process, the first oxide semiconductor film 103a and the second oxide semiconductor film 103b are diffused into the vicinity of the interface. In addition, the oxide insulating film 103b can be formed by the above-mentioned method. By diffusing oxygen to the vicinity of the first oxide semiconductor film 103a in the oxide semiconductor layer 102, Defects at the interface between the insulating film 102 and the first oxide semiconductor film 103a can be reduced. As a result, an oxide semiconductor having a first crystal structure in which the hydrogen concentration and oxygen defects are reduced can be obtained. The oxide semiconductor film 104a having the second crystal structure and the oxide semiconductor film 104b having the second crystal structure can be formed. do.
[0177] Next, as shown in FIG. 10C, The third oxide semiconductor film 103c is formed. The third insulating film can be formed using the same material and method as the nitride semiconductor film 103a. The thickness of the oxide semiconductor film 103c is determined by the practitioner depending on the device to be manufactured. For example, the first oxide semiconductor film 103a, the second oxide semiconductor film 103b, and The total thickness of the oxide semiconductor film 103c and the second oxide semiconductor film 103b is greater than or equal to 10 nm and less than or equal to 200 nm.
[0178] Note that the first to third oxide semiconductor films 103a to 103c are formed by a sputtering method. 103c, when forming one or more of the films, the leak rate of the processing chamber of the sputtering device 1×10 -10 Pa·m 3 / sec or less, during the film formation by sputtering In the first oxide semiconductor film 103a to the third oxide semiconductor film 103c, It is possible to reduce the inclusion of impurities such as silicon metals and hydrogen. By using an air pump (such as a cryopump), alkali metals and hydrogen can be removed from the exhaust system. It is possible to reduce the backflow of impurities such as those mentioned above.
[0179] In addition, at least one of the first oxide semiconductor film 103a to the third oxide semiconductor film 103c When forming the above film, the gas introduced into the processing chamber of the sputtering device, such as nitrogen gas or oxygen, Alternatively, a gas such as nitrogen gas or argon gas may be introduced in a heated state to form a film. At least one of the first oxide semiconductor film 103a to the third oxide semiconductor film 103c The hydrogen content can be reduced.
[0180] The first to third oxide semiconductor films 103a to 103b are formed by a sputtering method. 103c, before depositing any one or more of the sputtering equipment, the surface of the target, or In order to remove moisture or hydrogen contained therein, a preheat treatment may be performed. As a result, any one of the first to third oxide semiconductor films 103a to 103c The hydrogen content contained in the above can be reduced.
[0181] Next, a second heat treatment is performed. The temperature of the second heat treatment is preferably 150° C. or more and 650° C. or less. Preferably, the temperature is 200° C. or higher and 500° C. or lower. The heating time of the second heat treatment is 1 minute or longer. 24 hours or less.
[0182] In the second heat treatment, the atmosphere can be the same as that in the first heat treatment. In addition, the heating device may be the same as that used in the first heating treatment.
[0183] By performing the second heat treatment, an acid having a second crystal structure having a wurtzite crystal structure is obtained. Crystal growth starts from the oxide semiconductor film 104b toward the third oxide semiconductor film 103c. The oxide semiconductor film 104b having the second crystal structure is c-axis oriented. The third oxide semiconductor film 103c is formed by using the oxide semiconductor film 104b having the above structure as a seed. Similarly to the first oxide semiconductor film 103a, the oxide semiconductor film 10 has a second crystal structure. The third oxide semiconductor film 103c is grown so that the crystal axis of the third oxide semiconductor film 103c is substantially aligned with the crystal axis of the third oxide semiconductor film 103b. That is, the third oxide semiconductor film 103c can be grown as a crystal with its c-axis oriented. That is, the oxide semiconductor film 104c having the third crystal structure has an ab-plane In addition, the layers with hexagonal bonds are called membranes. The layers are laminated and bonded in the thickness direction (c-axis direction) and are c-axis oriented. An oxide semiconductor film 104c having a third crystal structure in which the c-axis is aligned can be formed. In addition, since the crystals grow using the oxide semiconductor film 104b having the second crystal structure as a seed, The crystal growth of the third oxide semiconductor film 103c is promoted, and an oxide semiconductor having a third crystal structure is formed. The surface of the body membrane 104c has high crystallinity and high uniformity (see FIG. 10(D)).
[0184] Note that the second heat treatment removes oxide semiconductor film 104b having the second crystal structure from the surface of the oxide semiconductor film 104b. When the crystal grows vertically from the first crystal structure, the c-axis of the oxide semiconductor film 104c having the third crystal structure is The direction is approximately perpendicular to the surface of the oxide semiconductor film 104b having the second crystal structure.
[0185] In addition, the second heat treatment can be performed to form the third oxide semiconductor film 10 in a similar manner to the first heat treatment. The hydrogen contained in 3c is released (i.e., dehydrogenated or dehydrated). As a result, the hydrogen concentration It is possible to form the oxide semiconductor film 104c having the third crystal structure in which the crystallinity is reduced. .
[0186] Through the above steps, an oxide semiconductor having a first crystal structure, which is a trigonal and / or hexagonal structure, is obtained. A conductive film 104a, an oxide semiconductor film 104b having a second crystal structure, and a semiconductor film 104b having a third crystal structure It is possible to form an oxide semiconductor film 104c having the first crystal structure. an oxide semiconductor film 104a having a second crystal structure, an oxide semiconductor film 104b having a third crystal structure, The hydrogen concentration and oxygen defects in the oxide semiconductor film 104c having the above structure can be reduced. When hydrogen is contained in an oxide semiconductor, some of it acts as a donor and is transported as a carrier. Similarly, oxygen defects in oxide semiconductors also act as donors, resulting in the generation of electrons. Therefore, the oxide semiconductor film having the first crystal structure 104a, an oxide semiconductor film 104b having a second crystal structure, and an oxide semiconductor film 104c having a third crystal structure. When the hydrogen concentration or oxygen vacancies in the oxide semiconductor film 104c are reduced, the capacitance in the oxide semiconductor film 104c is reduced. The rear concentration can be reduced, resulting in a negative threshold voltage for the transistors that will be fabricated later. For these reasons, the oxide semiconductor having the first crystal structure can reduce the phase shift. The oxide semiconductor film 104a having the second crystal structure, the oxide semiconductor film 104b having the third crystal structure, and the oxide semiconductor film 104c having the second crystal structure are By reducing the hydrogen concentration and the amount of oxygen defects in the oxide semiconductor film 104c to be formed later, In this way, it is possible to reduce the negative shift in the threshold voltage of the transistor to be treated.
[0187] Next, similarly to the first embodiment, a mass was formed on the oxide semiconductor film 104c having the third crystal structure. After the mask is formed, the oxide semiconductor film 104a having the first crystal structure is formed using the mask. The oxide semiconductor film 104b having the second crystal structure and the oxide semiconductor film 104b having the third crystal structure The conductive film 104c is selectively etched to form the oxide semiconductor film 10 having the first crystal structure. 5a, an oxide semiconductor film 105b having a second crystal structure, and an oxide semiconductor film 105c having a third crystal structure. The oxide semiconductor film 105c having the first crystal structure is formed. a, an oxide semiconductor film 105b having a second crystal structure, and an oxide semiconductor film 105c having a third crystal structure. The oxide semiconductor film 105c and the oxide semiconductor film 105b are collectively referred to as the oxide semiconductor stack 105. After that, the mask is removed. Remove.
[0188] Next, a pair of electrodes 106 are formed in contact with the oxide semiconductor stack 105. A gate insulating film 107 is formed on the insulating film 102, the oxide semiconductor stack 105, and the pair of electrodes 106. Next, a gate electrode 108 is formed on the gate insulating film 107. An insulating film 109 may be formed on the insulating film 107 and the gate electrode 108 (see FIG. 10(E)). Light. ).
[0189] The pair of electrodes 106 is formed using the same material and method as the pair of electrodes 106 described in Embodiment 1. It can be formed by using appropriate materials.
[0190] Note that after a conductive film is formed over the oxide semiconductor film 104c having the third crystal structure, A mask having a concave and convex shape is formed by a photomask, and a first crystal structure is formed by using the mask. an oxide semiconductor film 104a having a second crystal structure, an oxide semiconductor film 104b having a second crystal structure, and After the oxide semiconductor film 104c having the third crystal structure and the conductive film are etched, The uneven mask is separated by ashing, and the conductive film is selectively formed by the separated mask. By etching the oxide semiconductor layer 105, the oxide semiconductor layer 105 and the pair of electrodes 106 are formed. This process reduces the number of photomasks and photolithography steps. It is possible.
[0191] The gate insulating film 107 is formed using a material and a method similar to those of the gate insulating film 107 described in Embodiment 1. The method can be appropriately used to form the film.
[0192] Before forming the gate insulating film 107, the surface of the oxide semiconductor stack 105 is treated with oxygen, The surface of the oxide semiconductor laminate 105 is exposed to plasma of an oxidizing gas such as ozone or dinitrogen monoxide. The surface may be oxidized to reduce oxygen defects.
[0193] The gate electrode 108 is formed using the same material and method as the gate electrode 108 described in Embodiment 1. It can be formed by using appropriate materials.
[0194] After the gate insulating film 107 or the insulating film 109 is formed, the insulating film 109 is heated to a temperature of 100° C. In an atmosphere free of moisture (nitrogen atmosphere, oxygen atmosphere, dry air atmosphere (for example, dew point Heat treatment (temperature range 150 degrees or higher) at -40 degrees or lower, preferably at a dew point of -60 degrees or lower 650° C. or less, preferably 200° C. or more and 500° C. or less).
[0195] Through the above steps, trigonal and and / or a transistor having an oxide semiconductor stack having a hexagonal crystal region in a channel. It is possible to create a data.
[0196] In the oxide semiconductor stack described in this embodiment, a region in the vicinity of the interface with the gate insulating film The high crystallinity and uniformity of the material allow for stable electrical characteristics, resulting in highly reliable transistors. It is also possible to obtain a trigonal structure having hexagonal bonds on the ab plane and oriented along the c axis. The oxide semiconductor stack having a crystal region with a crystalline structure and / or a hexagonal crystal structure is used as a channel of a transistor. By using it in the transistor area, it is possible to measure the temperature before and after light irradiation or bias-thermal stress (B T) The change in the threshold voltage of the transistor was small even before and after the test, and stable electrical characteristics were obtained. It is possible to fabricate transistors having advantageous characteristics.
[0197] In addition, oxynitride semiconductors have a smaller energy gap than oxide semiconductors, and the carrier Therefore, in the transistor, the oxide semiconductor film having the third crystal structure By reducing the thickness of the oxide semiconductor film 105c, the oxide semiconductor film 105b having the second crystal structure becomes a crystal semiconductor film. As a result, the gate insulating film 107 and the buried channel type transistor are formed. and the oxide semiconductor film 105c having the third crystal structure. Therefore, a transistor having the above characteristics can be manufactured.
[0198] (Embodiment 4) In this embodiment mode, a structure and a manufacturing method of a transistor different from those in Embodiment 3 will be described. In this embodiment, the oxide insulating film and the oxide semiconductor film are The difference from the third embodiment is that a pair of electrodes is provided between the layers. The cross-sectional view of the dashed line CD in FIG. 11(A) corresponds to FIG. 11(B). The substrate 101, the oxide insulating film 102, the gate insulating film 117, and the insulating film 119 are omitted. 12A to 12C are cross-sectional views illustrating a manufacturing process of the transistor illustrated in FIG.
[0199] The transistor shown in FIG. 11B includes an oxide insulating film 102 formed over a substrate 101 and A pair of electrodes functioning as a source electrode and a drain electrode are formed on the oxide insulating film 102. a pair of insulating films 102 and 116 functioning as a source electrode and a drain electrode; The oxide semiconductor laminate 115 covers the electrode 116, the oxide insulating film 102, and the pair of electrodes 11 6, and a gate insulating film 117 formed on the oxide semiconductor stack 115, and a gate insulating film A gate electrode 118 overlaps with the oxide semiconductor stack 115 with a gate electrode 117 interposed therebetween. The gate insulating film 117 and the gate electrode 118 may be covered with an insulating film 119. In the opening of the insulating film 119, a pair of wirings 120 contacting the pair of electrodes 116 are provided. Good too.
[0200] The oxide semiconductor stack 115 includes a first insulating film 114 and a second insulating film 115a. The oxide semiconductor film 115a having a crystal structure and the oxide semiconductor film 115b having a first crystal structure are an oxide semiconductor film 115b having a second crystal structure in contact with an oxide semiconductor film 115a; the oxide semiconductor film 115b and the gate insulating film 117, The semiconductor layer 115 is characterized in that it is laminated with a nitride semiconductor film 115c.
[0201] That is, the oxide semiconductor film 115b having the second crystal structure is provided above and below the oxide semiconductor film 115b having the first crystal structure. The oxide semiconductor film 115a and the oxide semiconductor film 115c having the third crystal structure are included.
[0202] In addition, the oxide semiconductor film 115b having the second crystal structure is used as a seed crystal to grow the oxide semiconductor film 115b having the first crystal structure. and an oxide semiconductor film 115c having a third crystal structure. Each of them is characterized by crystal growth.
[0203] The oxide semiconductor film 115a having a first crystal structure and the oxide semiconductor film 115b having a third crystal structure The crystal structure of the film 115c is trigonal and / or hexagonal and non-wurtzite, YbFe 2O4 type structure, Yb2Fe3O7 type structure, or a modified structure thereof. A non-wurtzite structure is a crystal structure that is not a trigonal and / or hexagonal wurtzite structure.
[0204] The crystal structure of the oxide semiconductor film 115b having the second crystal structure is trigonal and / or It has a wurtzite structure, which is a hexagonal crystal structure.
[0205] Similarly to Embodiment 3, the oxide semiconductor films 115a to 115b having the first crystal structure and the third crystal structure are Since the oxide semiconductor film 115c having the above-mentioned structure is a trigonal crystal and / or a hexagonal crystal, the c-axis A hexagonal lattice image can be seen from any direction.
[0206] Note that the oxide semiconductor film 115a having the first crystal structure and the oxide semiconductor film 115b having the second crystal structure The oxide semiconductor film 115b having the third crystal structure and the oxide semiconductor film 115c having the third crystal structure are non-crystalline. The oxide semiconductor film is crystalline, and the entire oxide semiconductor film is not in an amorphous state, but has a c-axis orientation. In other words, it has an amorphous region and a crystalline region with a c-axis orientation.
[0207] Next, a manufacturing method of the transistor shown in FIG. 11B will be described with reference to FIGS.
[0208] As shown in FIG. 12A, similarly to the first embodiment, an oxide insulating film 102 is formed on a substrate 101. Next, a pair of electrodes 116 is formed over the oxide insulating film 102. A first oxide semiconductor film 113a and a second oxide semiconductor film 113b are formed over the electrode 116 and the oxide insulating film 102. Then, a compound semiconductor film 113b is formed.
[0209] The pair of electrodes 116 is formed using the same material and method as the pair of electrodes 106 described in Embodiment 1. It can be formed by using appropriate materials.
[0210] The first oxide semiconductor film 113a and the second oxide semiconductor film 113b have the same structure as those described in Embodiment 1. The first oxide semiconductor film 103a and the second oxide semiconductor film 103b are formed using the same materials and processes. It can be formed by using an appropriate manufacturing method.
[0211] Next, a first heat treatment is performed in the same manner as in the first embodiment. Crystal growth starts from the surface of the first oxide semiconductor film 113b toward the first oxide semiconductor film 113a. The second oxide semiconductor film 113b has a second crystal structure having a wurtzite crystal structure. The oxide semiconductor film 114b having the second crystal structure is formed. 14b has c-axis oriented crystals.
[0212] Then, a first heat treatment is performed to form an oxide semiconductor film 114b having a second crystal structure. The crystal growth of the first oxide semiconductor film 113a is performed by using an oxide having a second crystal structure as a seed. The oxide insulating film 102 is then formed by adsorbing the first crystal structure on the oxide insulating film 102. In addition, an oxide semiconductor film 114a having a first crystal structure is formed. Film 114a has c-axis oriented crystalline domains.
[0213] Next, a third oxide semiconductor film 113 is formed on the oxide semiconductor film 114b having the second crystal structure. The third oxide semiconductor film 113c is formed as described in Embodiment 3 (see FIG. 12B). The third oxide semiconductor film 103c shown in FIG. 1 is formed by using a material and a method similar to those of the third oxide semiconductor film 103c shown in FIG. can be done.
[0214] Next, a second heat treatment is performed in the same manner as in the third embodiment. The second crystal structure of the oxide semiconductor film 114b has a ruthenium-type crystal structure. Crystal growth starts from the first oxide semiconductor film 113c toward the third oxide semiconductor film 113c. 3c becomes an oxide semiconductor film 114c having a third crystal structure. The oxide semiconductor film 114c having the above structure has crystal regions with c-axis alignment (see FIG. 12C). Light. ).
[0215] Through the above steps, an oxide semiconductor having a first crystal structure, which is a trigonal and / or hexagonal structure, is obtained. A conductive film 114a, an oxide semiconductor film 114b having a second crystal structure, and a semiconductor film 114b having a third crystal structure It is possible to form the oxide semiconductor film 114c having the above structure.
[0216] Next, a mask is formed over the oxide semiconductor film 114c having the third crystal structure. The oxide semiconductor film 114a having a first crystal structure and the oxide semiconductor film 114b having a second crystal structure are formed by using a mask. The oxide semiconductor film 114b and the oxide semiconductor film 114c having the third crystal structure are selectively The oxide semiconductor film 115a having the first crystal structure and the oxide semiconductor film 115b having the second crystal structure are then etched. an oxide semiconductor film 115b having a third crystal structure, and an oxide semiconductor film 115c having a third crystal structure. Note that the oxide semiconductor film 115a having the first crystal structure and the oxide semiconductor film 115b having the second crystal structure are formed. an oxide semiconductor film 115b having a third crystal structure, and an oxide semiconductor film 115c having a third crystal structure. The resulting structure is collectively referred to as an oxide semiconductor stack 115. After that, the mask is removed.
[0217] Next, a gate electrode was formed on the oxide insulating film 102, the pair of electrodes 116, and the oxide semiconductor stack 115. Next, a gate electrode 118 is formed on the gate insulating film 117. .
[0218] Thereafter, an insulating film 119 is formed on the gate insulating film 117 and the gate electrode 118. Next, After forming a mask on the insulating film 119, the gate insulating film 117 and a part of the insulating film 119 are etched. Then, the pair of electrodes 116 are connected through the openings. A wiring 120 may be formed (see FIG. 12(D)).
[0219] The gate insulating film 117 is formed using a material and a method similar to those of the gate insulating film 107 described in Embodiment 1. The method can be appropriately used to form the film.
[0220] The gate electrode 118 is formed using the same material and method as the gate electrode 108 described in Embodiment 1. It can be formed by using appropriate materials.
[0221] The insulating film 119 is formed using a material and a method similar to those of the insulating film 109 described in Embodiment 1. It can be formed by:
[0222] The wiring 120 can be formed by appropriately using a material and a manufacturing method similar to those of the pair of electrodes 116. can.
[0223] Through the above steps, trigonal and A transistor having an oxide semiconductor stack having a hexagonal crystal region in a channel region. A dialyzer can be created.
[0224] In the oxide semiconductor stack described in this embodiment, a region in the vicinity of the interface with the gate insulating film The high crystallinity and uniformity of the material allow for stable electrical characteristics, resulting in highly reliable transistors. It is also possible to obtain a trigonal structure having hexagonal bonds on the ab plane and oriented along the c axis. The oxide semiconductor stack having a crystal region with a crystalline structure and / or a hexagonal crystal structure is used as a channel of a transistor. By using it in the transistor area, it is possible to measure the temperature before and after light irradiation or bias-thermal stress (B T) The change in the threshold voltage of the transistor was small even before and after the test, and stable electrical characteristics were obtained. It is possible to fabricate transistors having advantageous characteristics.
[0225] Note that this embodiment mode can be appropriately combined with other embodiment modes.
[0226] (Embodiment 5) In this embodiment mode, a structure and a manufacturing method of a transistor different from those in Embodiments 1 to 4 will be described. A method for forming a semiconductor device using the oxide insulating film and a semiconductor device using the oxide insulating film will be described with reference to FIGS. The present embodiment differs from the first to fourth embodiments in that a gate electrode is provided between the gate insulating film and the gate insulating film. That is, in the first to fourth embodiments, a top-gate transistor is used. However, in this embodiment, a bottom-gate transistor will be described. 13(B) is a cross-sectional view taken along dashed line EF in FIG. 13(A), which is a top view. In FIG. 3(A), a substrate 101, an oxide insulating film 102, a gate insulating film 127, and an insulating film 129 is omitted. FIG. 14 illustrates a manufacturing process of the transistor shown in FIG. FIG.
[0227] The transistor shown in FIG. 13B includes an oxide insulating film 102 formed over a substrate 101 and A gate electrode 128 formed on the oxide insulating film 102, and a gate insulating film 102 and a gate A gate insulating film 127 covers the electrode 128, and the gate electrode 128 is formed by interposing the gate insulating film 127 therebetween. When the oxide semiconductor stack 125 and the source electrode 111 are overlapped with each other, The gate insulating film 1 has a pair of electrodes 126 functioning as a gate electrode and a drain electrode. 27, an insulating film 129 may be provided to cover the oxide semiconductor stack 125 and the pair of electrodes 126. stomach.
[0228] The oxide semiconductor laminate 125 is an oxide semiconductor layer having a first crystal structure in contact with the gate insulating film 127. a second oxide semiconductor film in contact with the oxide semiconductor film having the first crystal structure; The oxide semiconductor film 125c having a crystalline structure is stacked on the oxide semiconductor film 125b.
[0229] In addition, the oxide semiconductor film 125b having the first crystal structure is used as a seed crystal to grow a semiconductor film having a second crystal structure. The oxide semiconductor film 125c has a feature that crystal growth is performed.
[0230] The oxide semiconductor film 125b having the first crystal structure is one of a trigonal crystal and / or a hexagonal crystal. It has a wurtzite crystal structure.
[0231] The oxide semiconductor film 125c having the second crystal structure is a trigonal crystal and / or a hexagonal crystal. Crystals with either the bFe2O4 type structure, the Yb2Fe3O7 type structure, or the non-wurtzite type structure It has a structure.
[0232] The oxide semiconductor film having the first crystal structure and the oxide semiconductor film having the second crystal structure are Both are trigonal and / or hexagonal, so a hexagonal lattice image can be seen from the c-axis direction. .
[0233] The oxide semiconductor film 125b having a first crystal structure and the oxide semiconductor film 125b having a second crystal structure Each of the oxide semiconductor films 125c is non-single crystal, and the entire oxide semiconductor film is in an amorphous state (amorphous state). The crystal regions are not in a fast state, but have c-axis oriented crystalline regions. It has crystalline regions.
[0234] Note that the oxide semiconductor stack 125 is an oxide semiconductor film having a first crystal structure. The oxide semiconductor film 125b having the second crystal structure and the oxide semiconductor film 125c having the second crystal structure were used. As shown in the third and fourth embodiments, the oxide semiconductor stack may have a three-layer structure. .
[0235] Next, a manufacturing method of the transistor shown in FIG. 13B will be described with reference to FIGS.
[0236] As shown in FIG. 14A, similarly to the first embodiment, an oxide insulating film 102 is formed on a substrate 101. Next, a gate electrode 128 is formed over the oxide insulating film 102. A gate insulating film 127 is formed on the insulating film 102 and the gate electrode 128. The first oxide semiconductor film 123 b is formed over the insulating film 127 .
[0237] The gate electrode 128 and the gate insulating film 127 are the same as those of the gate electrode 1 shown in the first embodiment. The insulating film 108 and the gate insulating film 107 can be formed by using the same material and manufacturing method as those of the insulating film 108 and the gate insulating film 107. do.
[0238] The first oxide semiconductor film 123b has the same structure as the second oxide semiconductor film 103b described in Embodiment 1. The same materials and manufacturing methods can be used appropriately to form the same.
[0239] Next, a first heat treatment is performed in the same manner as in the first embodiment. Crystal growth begins from the surface of the compound semiconductor film 123b toward the gate insulating film 127, and a first The oxide semiconductor film 124b has a crystalline structure. The semiconductor film 124b has a crystal region oriented along the c-axis.
[0240] Next, a second oxide semiconductor film 123 is formed on the oxide semiconductor film 124b having the first crystal structure. The second oxide semiconductor film 123c is formed as described in Embodiment 3 (see FIG. 14B). The third oxide semiconductor film 103c can be formed by using a material and a method similar to those of the third oxide semiconductor film 103c shown in FIG. This can be done.
[0241] Next, a second heat treatment is performed in the same manner as in the third embodiment. From the interface with the oxide semiconductor film 124b toward the second oxide semiconductor film 123c Crystal growth starts, and the second oxide semiconductor film 123c becomes an oxide semiconductor film having a second crystal structure. The oxide semiconductor film 124c having the second crystal structure is a It has axially aligned crystal domains (see FIG. 14(C)).
[0242] Through the above steps, the oxide semiconductor film 124b having the first crystal structure and the oxide semiconductor film 124b having the second crystal structure are obtained. It is possible to form the oxide semiconductor film 124c having the above structure.
[0243] Next, a mask is formed over the oxide semiconductor film 124c having the second crystal structure. The oxide semiconductor film 124b having a first crystal structure and the oxide semiconductor film 124c having a second crystal structure are formed using a mask. The oxide semiconductor film 124c is selectively etched to obtain an oxide semiconductor film having a first crystal structure. A semiconductor film 125b and an oxide semiconductor film 125c having a second crystal structure are formed. The oxide semiconductor film 125b having the first crystal structure and the oxide semiconductor film 125c having the second crystal structure are The oxide semiconductor film 125c and the oxide semiconductor film 125b are collectively referred to as the oxide semiconductor stack 125. After that, the mask is removed. Remove.
[0244] Next, similarly to the first embodiment, a pair of electrodes 126 is formed.
[0245] Next, an insulating film is formed on the gate insulating film 127, the pair of electrodes 126, and the oxide semiconductor stack 125. A film 129 may be formed (see FIG. 14(D)).
[0246] The insulating film 129 is formed using a material and a method similar to those of the insulating film 109 described in Embodiment 1. It can be formed by:
[0247] Through the above steps, trigonal and A transistor having an oxide semiconductor stack having a hexagonal crystal region in a channel region. A dialyzer can be created.
[0248] Note that in this embodiment, a channel etching type transistor is used. The present invention can be applied to a channel protection type transistor.
[0249] The oxide semiconductor laminate has high crystallinity and uniformity in the region near the interface with the gate insulating film. Since the conductivity type is also high, a transistor having stable electrical characteristics and high reliability can be obtained. Also, trigonal and / or hexagonal crystals having hexagonal bonds in the ab plane and oriented along the c axis By using an oxide semiconductor stack having a crystal structure for a channel region of a transistor, Before and after light exposure to the transistor, and before and after bias-thermal stress (BT) testing The amount of change in the threshold voltage of a transistor is small, and the transistor has stable electrical characteristics. It is possible to create a star.
[0250] In addition, oxynitride semiconductors have a smaller energy gap than oxide semiconductors, and the carrier Therefore, the oxide semiconductor having the first crystal structure in contact with the gate insulating film 127 is easily oxidized. By forming the semiconductor film 125b from an oxynitride semiconductor film, a transistor having good electrical characteristics can be obtained. It is possible to create a data.
[0251] Note that this embodiment mode can be appropriately combined with other embodiment modes.
[0252] (Embodiment 6) In this embodiment mode, a structure and a manufacturing method of a transistor different from those in Embodiments 1 to 5 will be described. The method will be described with reference to FIGS. 15 and 16. In this embodiment, a bottom gate type In addition, a pair of electrodes is provided between the gate insulating film and the oxide semiconductor stack. The difference from the fifth embodiment is that the dashed line in FIG. The cross-sectional view of GH corresponds to FIG. 15(B). In FIG. 15(A), a substrate 101, an oxide The insulating film 102, the gate insulating film 137, and the insulating film 139 are omitted. 5A to 5C are cross-sectional views illustrating a manufacturing process of the transistor shown in FIG.
[0253] The transistor shown in FIG. 15B includes an oxide insulating film 102 formed over a substrate 101 and A gate electrode 138 formed on the oxide insulating film 102, and the oxide insulating film 102 and the gate A gate insulating film 137 that covers the electrode 138 and a gate insulating film 138 that functions as a source electrode and a drain electrode are provided. A pair of electrodes 136, a gate insulating film 137, and an oxide semiconductor stack in contact with the pair of electrodes 136 The gate insulating film 137, the oxide semiconductor stack 135, and a pair of An insulating film 139 may be provided to cover the electrode 136 .
[0254] The oxide semiconductor laminate 135 is an oxide semiconductor layer having a first crystal structure in contact with the gate insulating film 137. a second oxide semiconductor film in contact with the oxide semiconductor film having the first crystal structure; The oxide semiconductor film 135c having a crystalline structure is stacked on the oxide semiconductor film 135b.
[0255] In addition, the oxide semiconductor film 135b having the first crystal structure is used as a seed crystal to grow a semiconductor film having a second crystal structure. The oxide semiconductor film 135c has a feature that crystals are grown.
[0256] The oxide semiconductor film 135b having the first crystal structure is one of a trigonal crystal and / or a hexagonal crystal. It has a wurtzite crystal structure.
[0257] The oxide semiconductor film 135c having the second crystal structure is a trigonal crystal and / or a hexagonal crystal. Crystals with either the bFe2O4 type structure, the Yb2Fe3O7 type structure, or the non-wurtzite type structure It has a structure.
[0258] The oxide semiconductor film having the first crystal structure and the oxide semiconductor film having the second crystal structure are Both are trigonal and / or hexagonal, so a hexagonal lattice image can be seen from the c-axis direction. .
[0259] The oxide semiconductor film 135b having the first crystal structure and the oxide semiconductor film 135b having the second crystal structure Each of the oxide semiconductor films 135c is non-single crystal, and the entire oxide semiconductor film is in an amorphous state (amorphous state). The crystal regions are not in a fast state, but have c-axis oriented crystalline regions. It has crystalline regions.
[0260] Here, the oxide semiconductor stack 135 is an oxide semiconductor film having a first crystal structure. The oxide semiconductor film 135b having the second crystal structure and the oxide semiconductor film 135c having the second crystal structure were used. As shown in the third and fourth embodiments, the oxide semiconductor stack may have a three-layer structure. .
[0261] Next, a manufacturing method of the transistor shown in FIG. 15B will be described with reference to FIGS.
[0262] As shown in FIG. 16A, similarly to the first embodiment, an oxide insulating film 102 is formed on a substrate 101. Next, a gate electrode 138 is formed over the oxide insulating film 102. A gate insulating film 137 is formed on the insulating film 102 and the gate electrode 138. Next, the gate A pair of electrodes 136 are formed on the insulating film 137. Next, the gate insulating film 137 and the pair of electrodes 136 are A first oxide semiconductor film 133 b is formed over the electrode 136 .
[0263] The gate electrode 138, the gate insulating film 137, and the first oxide semiconductor film 133b are , the gate electrode 108, the gate insulating film 107, and the second oxide semiconductor The film can be formed by appropriately using a material and a manufacturing method similar to those of the film 103b.
[0264] Next, a first heat treatment is performed in the same manner as in the first embodiment. Crystal growth begins from the surface of the compound semiconductor film 133b toward the gate insulating film 137, and the first The oxide semiconductor film 133b becomes an oxide semiconductor film 134b having the first crystal structure. The oxide semiconductor film 134b having the first crystal structure has crystal regions which are c-axis aligned.
[0265] Next, a second oxide semiconductor film 133 is formed on the oxide semiconductor film 134b having the first crystal structure. The second oxide semiconductor film 133c is formed as described in Embodiment 3 (see FIG. 16B). The third oxide semiconductor film 103c can be formed by using a material and a method similar to those of the third oxide semiconductor film 103c shown in FIG. This can be done.
[0266] Next, a second heat treatment is performed in the same manner as in the third embodiment. From the interface with the oxide semiconductor film 134b toward the second oxide semiconductor film 133c having the structure Crystal growth starts, and the second oxide semiconductor film 133c becomes an oxide semiconductor film having a second crystal structure. The oxide semiconductor film 134c having the second crystal structure is It has axially aligned crystal domains (see FIG. 16(C)).
[0267] Through the above steps, the oxide semiconductor film 134b having the first crystal structure and the oxide semiconductor film 134b having the second crystal structure are obtained. It is possible to form the oxide semiconductor film 134c having the above structure.
[0268] Next, a mask is formed over the oxide semiconductor film 134c having the second crystal structure. The oxide semiconductor film 134b having a first crystal structure and the oxide semiconductor film 134b having a second crystal structure are formed using a mask. The oxide semiconductor film 134c is selectively etched to obtain an oxide semiconductor film having a first crystal structure. A semiconductor film 135b and an oxide semiconductor film 135c having a second crystal structure are formed. The oxide semiconductor film 135b having the first crystal structure and the oxide semiconductor film 135b having the second crystal structure are The oxide semiconductor film 135c and the oxide semiconductor film 135b are collectively referred to as the oxide semiconductor stack 135. After that, the mask is removed. Remove.
[0269] Next, an insulating film is formed on the oxide insulating film 102, the pair of electrodes 136, and the oxide semiconductor stack 135. A film 139 may be formed (see FIG. 16(D)).
[0270] The insulating film 139 is formed using a material and a method similar to those of the insulating film 109 described in Embodiment 3. It can be formed by:
[0271] Through the above steps, trigonal and and / or a transistor having an oxide semiconductor stack having a hexagonal crystal structure in a channel region. It is possible to create a data.
[0272] Note that in this embodiment, a channel etching type transistor is used. The present invention can be applied to a channel protection type transistor.
[0273] The oxide semiconductor laminate has high crystallinity and uniformity in the region near the interface with the gate insulating film. Since the conductivity type is also high, a transistor having stable electrical characteristics and high reliability can be obtained. Also, trigonal and / or hexagonal crystals having hexagonal bonds in the ab plane and oriented along the c axis The oxide semiconductor stack having the crystal region of the above structure is used for a channel region of a transistor. Before and after light irradiation to the transistor, or before and after bias-thermal stress (BT) testing Even if the transistor is turned on, the amount of change in the threshold voltage of the transistor is small, and the transistor has stable electrical characteristics. It is possible to fabricate a transistor.
[0274] Note that this embodiment mode can be appropriately combined with other embodiment modes.
[0275] (Embodiment 7) In this embodiment, in any of the first to sixth embodiments, a semiconductor device having a plurality of gate electrodes is A transistor will be described. Here, the transistor described in Embodiment 5 will be used. However, the present invention can be appropriately applied to the first to fourth embodiments and the sixth embodiment. do.
[0276] As in the fifth embodiment, an oxide insulating film 102 is formed on a substrate 101 as shown in FIG. A first gate electrode 148a and a first gate insulating film 147a are formed on the oxide insulating film 102. Next, an oxide semiconductor having a first crystal structure is formed on the first gate insulating film 147a. The oxide semiconductor film 125c having the second crystal structure and the conductive film 125b are stacked. A compound semiconductor laminate 125, a pair of electrodes 126, and a second gate insulating film 147b are formed. .
[0277] Next, a region on the second gate insulating film 147b that overlaps with the oxide semiconductor stack 125 is Next, a second gate electrode 148b is formed in the second gate insulating film 147b. An insulating film 129 may be formed as a protective film on the gate electrode 148b.
[0278] The first gate electrode 148a and the second gate electrode 148b are the same as those shown in the first embodiment. It can be formed in the same manner as the electrode 108 .
[0279] The first gate insulating film 147a and the second gate insulating film 147b are the same as those in the first embodiment. It can be formed in the same manner as the gate insulating film 107 .
[0280] The first gate electrode 148a and the second gate electrode 148b may be connected to each other. In this case, the first gate electrode 148a and the second gate electrode 148b have the same potential. The channel region is disposed on the first gate electrode 148a side of the oxide semiconductor laminate 125 and the second gate Since the second insulating layer 144 is formed on the side of the gate electrode 148b, the on-current and the field effect mobility of the transistor are improved. It is possible.
[0281] Alternatively, the first gate electrode 148a and the second gate electrode 148b are not connected and are different. In this case, the threshold voltage of the transistor can be controlled. do.
[0282] In this embodiment, the pair of electrodes 126 is connected to the oxide semiconductor stack 125 and the second gate electrode 126. The first gate insulating film 147a and the oxide semiconductor stacked film 147b are formed between the first gate insulating film 147a and the oxide semiconductor stacked film 147b. It may be formed between the bodies 125 .
[0283] Through the above steps, a transistor having a plurality of gate electrodes can be manufactured.
[0284] (Embodiment 8) In this embodiment, at least a part of the driver circuit and a transistor disposed in the pixel portion are formed on the same substrate. A method for manufacturing a display device having a transistor will be described below.
[0285] The transistors disposed in the pixel portion are formed according to any one of the embodiments 1 to 7. The transistors described in any of the embodiments 1 to 7 are n-channel transistors. Therefore, among the driver circuits, the driver circuits that can be configured with n-channel transistors A part of the transistors is formed on the same substrate as the transistors in the pixel portion.
[0286] FIG. 18A shows a block diagram of an active matrix display device. A pixel portion 5301, a first scanning line driver circuit 5302, a second scanning line driver circuit 5303, and a second scanning line driver circuit 5304 are provided on a substrate 5300. The pixel portion 5301 includes a driver circuit 5303 and a signal line driver circuit 5304. A signal line driver circuit 5304 is arranged so as to extend from the signal line driver circuit 5305, and a plurality of scanning lines are arranged in the first scanning line driver circuit 5306. The scanning line driver circuit 5302 and the second scanning line driver circuit 5303 are arranged to extend from each other. At the intersections of the lines and the signal lines, pixels each having a display element are arranged in a matrix. The display device substrate 5300 is made of FPC (Flexible Printed Circuit). A timing control circuit (also called a controller or control IC) is connected to the timing control circuit via a connection such as an IRCuit. The NI PXIe-4100 is connected to the
[0287] In FIG. 18A, a first scanning line driver circuit 5302, a second scanning line driver circuit 5303, a signal The signal line driver circuit 5304 is formed on the same substrate 5300 as the pixel portion 5301. This reduces the number of external components such as drive circuits, and therefore reduces costs. In addition, when a driving circuit is provided outside the substrate 5300, it becomes necessary to extend the wiring, and the wiring The number of connections increases. If a driver circuit is provided on the same board 5300, the number of connections between the wiring can be reduced. This can reduce the amount of damage, thereby improving reliability and yield.
[0288] FIG. 18B shows one example of the circuit configuration of the pixel section. The pixel structure of the panel is shown.
[0289] This pixel structure has multiple pixel electrodes in one pixel, and each pixel electrode has a transistor. Each transistor is configured to be driven by a different gate signal. That is, in a pixel with a multi-domain design, the voltage applied to each pixel electrode is The signal is independently controlled.
[0290] The gate wiring 602 of the transistor 628 and the gate wiring 603 of the transistor 629 are , are separated so that different gate signals can be applied. On the other hand, The functioning source or drain electrode 616 is connected to transistor 628 and transistor 62 9. Transistor 628 and transistor 629 are the same as those in the first embodiment. The transistors in the seventh embodiment can be used as appropriate.
[0291] The first pixel electrode and the second pixel electrode have different shapes and are separated by a slit. The second pixel electrode is formed so as to surround the outside of the first pixel electrode that spreads in a V shape. The timing of the voltages applied to the first pixel electrode and the second pixel electrode is controlled by the transistor 628. The alignment of the liquid crystal is controlled by changing the polarity of the transistor 629. The transistor 628 is connected to the gate wiring 602, and the transistor 629 is connected to the gate wiring 603. By applying different gate signals to the gate wiring 602 and the gate wiring 603, The operation timing of the transistor 628 and the transistor 629 can be made different.
[0292] In addition, a capacitance wiring 690 is provided, and the gate insulating film is used as a dielectric. A capacitance electrode electrically connected to the pixel electrode of No. 2 and a storage capacitance are formed.
[0293] The first pixel electrode, the liquid crystal layer, and the counter electrode are overlapped to form a first liquid crystal element 651. In addition, the second pixel electrode, the liquid crystal layer, and the counter electrode are overlapped, so that the second liquid crystal pixel A first liquid crystal element 651 and a second liquid crystal element 652 are formed in one pixel. It is a multi-domain structure in which 2 is provided.
[0294] Note that the pixel configuration shown in FIG. 18(B) is not limited to this. The pixels are now equipped with new switches, resistors, capacitors, transistors, sensors, logic circuits, etc. Any of the above may be added.
[0295] In addition, in this embodiment, the form of the liquid crystal display panel of the VA type is shown, but it is not particularly limited. It can be applied to various types of liquid crystal display devices. For example, the method of improving the viewing angle characteristics In the IPS mode, an electric field is applied to the liquid crystal layer in a direction parallel to the main surface of the substrate. It can be applied to
[0296] For example, a liquid crystal display panel using the IPS method that exhibits a blue phase without using an alignment film is used. The blue phase is one of the liquid crystal phases, and is generated when the temperature of the cholesteric liquid crystal is increased. The blue phase is a phase that appears just before the transition from the cholesteric phase to the isotropic phase. Since it only appears in a certain temperature range, liquid crystals mixed with chiral agents are used to improve the temperature range. The composition is used in the liquid crystal layer of a liquid crystal element. The response speed of the crystal composition is short (less than 1 msec) and it is optically isotropic, so no alignment process is required. and the viewing angle dependency is small.
[0297] In addition, in order to improve the video characteristics of liquid crystal display devices, multiple LEDs (light emitting diodes) are used as backlights. A surface light source is formed by using a diode) light source or multiple EL light sources, etc., and a surface light source is formed. A driving technology that drives each light source independently and intermittently within one frame period (for example, field Three or more types of LEDs may be used as a surface light source. Alternatively, a white LED may be used. As a surface light source, three or more types of light sources each having a different color may be used. (For example, if you use R (red), G (green), and B (blue)), you do not need to use a color filter. In addition, when using a white LED as a surface light source, A color filter is provided to display color. Since multiple LEDs can be controlled independently, the liquid crystal layer It is also possible to synchronize the LED emission timing with the switching timing of the optical modulation. It is possible to turn off some of the LEDs, which is particularly useful for black areas that occupy the entire screen. In the case of image display in which the ratio of the pixels is high, the power consumption can be reduced.
[0298] FIG. 18C shows one example of the circuit configuration of the pixel section. 4 shows the pixel structure of the display panel.
[0299] In an organic EL element, electrons and holes are released from a pair of electrodes by applying a voltage to the light-emitting element. are injected into a film containing a light-emitting organic compound, causing a current to flow. The rears (electrons and holes) recombine to form an excited state in the light-emitting organic compound. When the excited state returns to the ground state, light is emitted. Such a light-emitting element is called a current-excitation type light-emitting element.
[0300] FIG. 18C shows a pixel configuration to which digital time gray scale driving can be applied as a semiconductor device. FIG.
[0301] The configuration of a pixel to which digital time gray scale driving can be applied and the operation of the pixel will be described. In this study, two n-channel transistors using an oxide semiconductor film for the channel region were used in one pixel. The form in which they are used is shown below.
[0302] The pixel 6400 includes a switching transistor 6401, a driving transistor 6402, The switching transistor 64 has a light emitting element 6404 and a capacitor element 6403. 01, the gate electrode is connected to the scanning line 6406, and the first electrode (the source electrode and the drain electrode) is connected to the scanning line 6406. The second electrode (the other of the source electrode and the drain electrode) is connected to a signal line 6405. ) is connected to the gate electrode of the driving transistor 6402. 402, the gate electrode is connected to the power supply line 6407 via the capacitance element 6403, and the first electrode The first electrode is connected to a power line 6407, and the second electrode is connected to a first electrode (pixel electrode) of the light emitting element 6404. The second electrode of the light emitting element 6404 corresponds to a common electrode 6408. 408 is electrically connected to a common potential line formed on the same substrate.
[0303] A low power supply potential is set to the second electrode (common electrode 6408) of the light emitting element 6404. Note that the low power supply potential is a low power supply potential with respect to the high power supply potential set to the power supply line 6407. Potential < High power supply potential. For example, GND, 0V, etc. are set as low power supply potential. The potential difference between the high power supply potential and the low power supply potential is applied to the light emitting element 6404. In order to make the light emitting element 6404 emit light by passing a current through the light emitting element 6404, a high power supply potential and the low power supply potential is set to be equal to or higher than the forward threshold voltage of the light emitting element 6404. Each potential is set.
[0304] The capacitor 6403 is omitted by substituting the gate capacitance of the driving transistor 6402. It is also possible to set the gate capacitance of the driving transistor 6402 as follows: A capacitance may be formed between the gate electrode and the second electrode.
[0305] In the case of a voltage input voltage driving method, the gate electrode of the driving transistor 6402 is In this case, the driving transistor 6402 is in two states, either fully on or off. In other words, the driving transistor 6402 is operated in a linear region. In order to operate the driving transistor 6402 in a linear region, the voltage of the power supply line 6407 is higher than that of the driving transistor 6402. A voltage higher than the voltage at the gate electrode of the driving transistor 6402 is applied to the gate electrode of the driving transistor 6402. A voltage equal to or higher than (power supply line voltage+Vth of driving transistor 6402) is applied to 5.
[0306] In addition, when analog gray scale driving is performed instead of digital time gray scale driving, the input of the signal is different. By doing so, the same pixel configuration as in FIG. 18(C) can be used.
[0307] When analog gradation driving is performed, the gate electrode of the driving transistor 6402 is connected to the light emitting element 64 A voltage equal to or higher than the forward voltage of 04 plus the Vth of the driving transistor 6402 is applied. The forward voltage of 6404 refers to the voltage required to achieve the desired brightness. Incidentally, the driving transistor 6402 is designed to operate in the saturation region. By inputting a video signal, a current can be passed through the light emitting element 6404. In order to operate the transistor 6402 in the saturation region, the potential of the power supply line 6407 is set to The gate potential of the transistor 6402 is set higher than that of the transistor 6403. Analog gray scale driving can be performed by passing a current according to a video signal through the element 6404 .
[0308] Note that the pixel configuration shown in FIG. 18C is not limited to this. The pixels are now equipped with new switches, resistors, capacitors, sensors, transistors, logic circuits, etc. may be added.
[0309] Next, the configuration of the light-emitting element will be described with reference to the cross-sectional structure of a pixel shown in FIG. The cross-sectional structure of a pixel is shown in FIG. 1, taking the case where the light-emitting element driving transistor is an n-channel type as an example. The semiconductor device shown in FIG. 19(A), FIG. 19(B), and FIG. The light-emitting element driving transistors 7011, 7021, and 7001 are the same as those in the first embodiment. The transistor can be manufactured in a manner similar to that of the transistor shown in the seventh embodiment.
[0310] At least one of the first electrode and the second electrode of the light-emitting element is made of a conductive film that transmits visible light. The structure that focuses on the direction of light emission is as follows: The light emitting element and the transistor are formed on the substrate without being sandwiched between the substrate and the light emitting element. The top emission structure extracts light from the side on which the light emitting element is formed, and the light emitting element is emitted through the substrate on which the light emitting element is formed. A bottom emission structure that emits light on the side where no optical element is formed, and a substrate on which a light emitting element is formed There is a double-sided emission structure in which light is emitted from one side of the substrate and from the other side of the substrate through the substrate. The pixel configuration shown in 18(C) can be applied to any light emitting element of any emission structure.
[0311] The light emitting element having a bottom emission structure will be described with reference to FIG. The element emits light in the direction shown by the arrow in FIG.
[0312] In FIG. 19A, a light-emitting element driving transistor 7011 is an n-channel transistor shown in Embodiment 1. However, the present invention is not limited to this embodiment.
[0313] In FIG. 19A, a source electrode or a drain electrode of a light-emitting element driving transistor 7011 is An EL layer 7014, a second electrode 7015, and a third electrode 7016 are disposed on a first electrode 7017 having a light-transmitting property and electrically connected to the first electrode. The electrodes 7015 are laminated in this order.
[0314] The first electrode 7017 is formed using a conductive film that transmits visible light. Examples of the indium oxide include tungsten oxide and indium oxide including tungsten oxide. Indium zinc oxide, indium oxide with titanium oxide, indium tin oxide with titanium oxide Indium tin oxide (ITO), indium zinc oxide, silicon oxide Indium tin oxide doped with 5n is also available. A thin metal film having a thickness of about 20 nm to 30 nm can also be used. An aluminum film can be used by being laminated on another light-transmitting conductive film.
[0315] The second electrode 7015 is preferably made of a material that efficiently reflects light emitted from the EL layer 7014. This is because the light extraction efficiency can be improved. For example, a conductive film that transmits visible light may be used on the side in contact with the EL layer 7014, and A light-shielding film 7016 can be laminated on the side of the light-shielding film 7016. A metal film that efficiently reflects the light emitted by the EL layer is preferable, but a black pigment may be added. Resins and the like can also be used.
[0316] One of the first electrode 7017 and the second electrode 7015 functions as an anode, and the other functions as a cathode. The electrode that functions as the anode is preferably made of a material with a large work function, and the cathode is preferably made of a material with a large work function. For the electrodes functioning as poles, a material having a small work function is preferred.
[0317] Materials with a large work function include, for example, ZrN, Ti, W, Ni, Pt, Cr, etc., and I TO, In-Zn-O, etc. can be used. Materials with small work functions include Li Alkaline metals such as Ca and Cs, and alkaline earth metals such as Mg, Ca, and Sr, and In addition to alloys containing Mg (Mg:Ag, Al:Li, etc.), rare earth metals such as Yb and Er are used. It is possible.
[0318] When comparing power consumption, the first electrode 7017 is made to function as a cathode and the second electrode Using 7015 as the anode can suppress the voltage rise in the drive circuit and reduce power consumption. This is preferable.
[0319] The EL layer 7014 may include at least a light-emitting layer. The layer may be laminated. In the case of a structure having a plurality of layers, the layer may be laminated in the order of the hole from the anode side. The structure is a laminate of an injection layer, a hole transport layer, a light emitting layer, an electron transport layer, and an electron injection layer. It is not necessary to provide all of these layers in the EL layer 7014. In addition, the intermediate layer may be a charge generating layer or an electron relay layer. Other configurations may be added as appropriate.
[0320] In addition, the light-emitting element 7012 includes a partition wall 7019 that covers an edge portion of the first electrode 7017. 7019 is suitable for organic resin films such as polyimide, acrylic, polyamide, and epoxy, as well as inorganic insulating films. In particular, the side of the partition wall 7019 is curved continuously. It is preferable to form the inclined surface using a photosensitive resin material so that the inclined surface has a certain degree of efficiency. When a photosensitive resin material is used for the partition wall 7019, a process of forming a resist mask is performed. The partition wall can be formed of an inorganic insulating film. By using this for the partition walls, the amount of moisture contained in the partition walls can be reduced.
[0321] A color filter layer 7033 is provided between the light emitting element 7012 and the substrate 7010. (See FIG. 19A). By applying a structure for emitting white light to the light-emitting element 7012, The light emitted by the light emitting element 7012 passes through the color filter layer 7033 and enters the insulating film 7032. The light passes through the gate insulating film 7031, the oxide insulating film 7030, and the substrate 7010. do.
[0322] A plurality of types of color filter layers 7033 may be formed. For example, a red color filter layer may be formed for each pixel. A filter layer, a blue color filter layer, a green color filter layer, etc. can be provided. The color filter layer 7033 is formed by a droplet discharge method such as an ink-jet method, a printing method, Alternatively, they may be formed by an etching method using photolithography technology.
[0323] The color filter layer 7033 is covered with an overcoat layer 7034, which is a protective insulating layer. In FIG. 19A, the overcoat layer 7034 is thin. As shown in the figure, the overcoat layer 7034 is made of a resin material such as an acrylic resin, and is colored. It has the function of flattening unevenness caused by the -filter layer 7033.
[0324] In addition, an insulating film 7032, a color filter layer 7033, an overcoat layer 7034, and a protective film The contact hole formed in the protective insulating film 7035 and reaching the drain electrode is Place it so that it overlaps with 019.
[0325] Next, a light emitting element having a dual emission structure will be described with reference to FIG. The light emitting element emits light in the direction shown by the arrow in FIG.
[0326] In FIG. 19B, a light-emitting element driving transistor 7021 is an n-channel transistor shown in Embodiment 1. However, the present invention is not limited to this embodiment.
[0327] In FIG. 19B, the source electrode or the drain electrode of the light-emitting element driving transistor 7021 is An EL layer 7024, a second electrode 7025, and a third electrode 7026 are disposed on a first electrode 7027 having a light-transmitting property and electrically connected to the first electrode. The electrodes 7025 are laminated in this order.
[0328] The first electrode 7027 and the second electrode 7025 are formed using a conductive film that transmits visible light. The conductive film that transmits light can be used for the first electrode 7017 in FIG. Therefore, the detailed description of the first electrode 7017 is incorporated herein by reference. do.
[0329] Either the first electrode 7027 or the second electrode 7025 functions as an anode. The electrode that functions as the anode is preferably made of a material with a large work function. Preferably, the electrode functioning as the cathode is made of a material having a small work function.
[0330] The EL layer 7024 may be composed of a single layer or may be composed of multiple layers. The layer 7024 may have a structure and material that can be used for the EL layer 7014 in FIG. Therefore, the description of the EL layer 7014 is incorporated in the detailed description.
[0331] In addition, the light-emitting element 7022 includes a partition wall 7029 that covers an edge portion of the first electrode 7027. 7029 is a diagram showing a structure and material that can be used for the partition wall 7019 in FIG. Therefore, the detailed description will be referred to the description of the partition wall 7019.
[0332] In the case of the element structure shown in FIG. 19B, the light emitted from the light-emitting element 7022 is As shown by the arrows, the light is emitted to both the second electrode 7025 side and the first electrode 7027 side. One of the lights emitted to the electrode 7027 side passes through the insulating film 7042, the gate insulating film 7041, the oxide The light is emitted through the insulating film 7040 and the substrate 7020 .
[0333] In the structure of FIG. 19B, when a full-color display is performed, for example, the light-emitting element 70 22 is a green light emitting element, one of the adjacent light emitting elements is a red light emitting element, and the other The light-emitting element is a blue light-emitting element. In addition to the three types of light-emitting elements, a white element is also added, making a total of four. A light-emitting display device capable of full-color display may be manufactured using a variety of light-emitting elements.
[0334] Next, a light emitting element having a top emission structure will be described with reference to FIG. The light emitting element emits light in the direction shown by the arrow in FIG.
[0335] In FIG. 19C, a light-emitting element driving transistor 7001 is an n-channel transistor shown in Embodiment 1. However, the present invention is not limited to this embodiment.
[0336] In FIG. 19C, the source electrode or drain electrode of the light-emitting element driving transistor 7001 is An EL layer 7004 and a second electrode 7005 are disposed on a first electrode 7003 electrically connected to the are layered in order.
[0337] The first electrode 7003 is preferably made of a material that efficiently reflects light emitted from the EL layer 7004. This is because the light extraction efficiency can be improved. For example, a conductive film that transmits visible light may be used on the side in contact with the EL layer 7004, and A light-shielding film can be laminated on the side of the substrate. A metal film that efficiently reflects the emitted light is preferable, but a resin with black pigment added, for example, can also be used. It can also be used.
[0338] The second electrode 7005 is formed using a conductive film that transmits visible light. The material that can be used for the first electrode 7017 in FIG. 19(A) can be applied. Therefore, the detailed description will be given with reference to the description of the first electrode 7017.
[0339] Either the first electrode 7003 or the second electrode 7005 functions as an anode. The electrode that functions as the anode is preferably made of a material with a large work function. Preferably, the electrode functioning as the cathode is made of a material having a small work function.
[0340] The EL layer 7004 may be composed of a single layer, or may be composed of multiple layers stacked together. The layer 7004 may have a structure and material that can be used for the EL layer 7014 in FIG. Therefore, the description of the EL layer 7014 is incorporated in the detailed description.
[0341] In addition, the light-emitting element 7002 includes a partition wall 7009 that covers an edge portion of the first electrode 7003. 7009 is a diagram showing a structure and material that can be used for the partition wall 7019 in FIG. Therefore, the detailed description will be referred to the description of the partition wall 7019.
[0342] In FIG. 19C, the source electrode of the light-emitting element driving transistor 7001 or The drain electrode is provided on a gate insulating film 7051, a protective insulating film 7052, and an insulating film 7055. The first electrode 7003 is electrically connected to the first electrode 7003 through a contact hole formed in the first electrode 7003. Film 7053 is available in polyimide, acrylic, benzocyclobutene, polyamide, epoxy, etc. Resin materials can be used. In addition to the above resin materials, low-dielectric constant materials (low-k materials) can also be used. In addition, insulating materials made of these materials can be used. The planarization insulating film 7053 may be formed by stacking a plurality of films. The method for forming the 53 is not particularly limited, and may be a sputtering method, a SOG method, a spin coater method, or the like, depending on the material. Coating, dip, spray coating, droplet ejection method (inkjet method, screen printing, off Set printing, etc. can be used.
[0343] In the structure of FIG. 19C, when a full-color display is performed, for example, the light-emitting element 70 02 is a green light emitting element, one adjacent light emitting element is a red light emitting element, and the other The light-emitting element is a blue light-emitting element. In addition to the three types of light-emitting elements, a white element is also added, making a total of four. A light-emitting display device capable of full-color display may be manufactured using a variety of light-emitting elements.
[0344] In the structure of FIG. 19(C), all the light emitting elements are white light emitting elements. In addition, a sealing substrate having a color filter or the like is disposed above the light emitting element 7002. A light-emitting display device capable of full color display may be manufactured. By forming a material and combining it with color filters and color conversion layers, full color display is achieved. It is possible to do so.
[0345] Of course, a single-color display may be used. For example, a lighting device may be formed using white light. Alternatively, monochromatic light may be used to form an area color type light emitting device.
[0346] If necessary, an optical film such as a polarizing film, eg, a circular polarizing plate, may be provided.
[0347] In addition, a transistor for controlling the driving of a light-emitting element (a transistor for driving a light-emitting element) and a light-emitting element In the above example, the transistor for driving the light emitting element and the light emitting element are electrically connected. A current control transistor may be connected between them.
[0348] Note that the semiconductor device described in this embodiment mode is not limited to the configuration shown in FIG. Various modifications based on the technical concept of the present invention are possible.
[0349] (Embodiment 9) The semiconductor device disclosed in this specification can be applied to various electronic devices (including game machines). The electronic device can be, for example, a television device (television or television receivers), computer monitors, digital cameras, digital video cameras digital photo frames, mobile phones (also called mobile phones or mobile phone devices), ), portable game machines, personal digital assistants, audio playback devices, pachinko machines and other large game machines, etc. The electronic devices including the display device described in the above embodiment will be described. Reveal.
[0350] FIG. 20A shows a portable information terminal, which includes a main body 3001, a housing 3002, a display unit 300 The display unit 3003b has a touch input function. The panel is a keyboard panel that can be used to input commands by touching the keyboard button 3004 displayed on the display unit 3003b. By touching the display unit 3003a, screen operations and character input can be performed. The panel may be configured as a panel having an input function. The transistor is used as a switching element to produce a liquid crystal panel or an organic light-emitting diode as shown in the eighth embodiment. By manufacturing a panel and applying it to the display units 3003a and 3003b, a portable information terminal can be realized. It can be said that it is the end.
[0351] The portable information terminal shown in FIG. 20(A) displays various information (still images, videos, text images, etc.). ), calendar, date or time display function, The ability to manipulate or edit the information displayed, and to process it using various software (programs) In addition, the rear and side of the housing can have external connection terminals ( It may also be configured to include an earphone jack, a USB terminal, a recording medium insertion portion, etc.
[0352] The portable information terminal shown in FIG. 20(A) can also be configured to transmit and receive information wirelessly. You can wirelessly purchase and download the desired book data from the electronic book server. It is also possible to configure it in this way.
[0353] The portable information terminal shown in FIG. 20A has two display units 3003a and 3003b. One of them can be removed, and the figure when it is removed is shown in FIG. The display unit 3003a is also a panel with a touch input function, making it even lighter when carried around. It is possible to hold the housing 3002 with one hand and operate it with the other hand, which is convenient. It is.
[0354] Furthermore, the housing 3002 shown in FIG. 20B is provided with an antenna, a microphone function, and a wireless function. It may also be used as a mobile phone.
[0355] FIG. 20C shows one form of a mobile phone. Mobile phone 500 shown in FIG. 5 includes a display unit 5001 built into the housing, as well as a display panel attached to a hinge 5002. The display device 5003 includes a panel 5003, operation buttons 5004, a speaker, a microphone, etc.
[0356] In a mobile phone 5005 shown in FIG. 20C, a display panel 5003 slides to display a display It overlaps with 5001 and functions as a light-transmitting cover. The filter 5003 is a filter that is attached to the substrate side and the surface opposite to the substrate as shown in FIG. 19(B) of the eighth embodiment. This is a display panel that uses light-emitting elements with a dual-side emission structure that extracts light from the
[0357] In addition, since the display panel 5003 uses light-emitting elements with a dual-side emission structure, the display unit 5001 The display can be displayed in a state where it is overlapped with the other, and the user can display both and see both displays. The display panel 5003 is transparent, and the other side of the display panel can be seen through. For example, a map is displayed on the display unit 5001, and the user's location point is displayed. By displaying the status on the display panel 5003, it is possible to provide an easily recognizable status. Cut.
[0358] In addition, when the mobile phone 5005 is provided with an image pickup element and used as a video phone, You can talk to multiple people while displaying your hands, so you can hold video conferences, etc. For example, the face of one or more people is displayed on the display panel 5003, and the display unit 50 By displaying another face on 01, the user can have a conversation while looking at the faces of two or more people. This can be done.
[0359] In addition, when a touch input button 5006 displayed on the display panel 5003 is touched with a finger or the like, You can also use it to make calls, send emails, and perform other operations. By sliding the display panel 5003 and touching the operation button 5004 with a finger, This can be done more.
[0360] FIG. 20D shows one embodiment of a television device 9600. The display unit 9603 is incorporated in the housing 9601 of the device 600. It is possible to display images. Also, here we have the Stand 9605 with a built-in CPU. In the embodiment 1 to the embodiment 7, the housing 9601 is supported by the By applying the transistor to the display portion 9603, a television set 9600 can be obtained. It is possible.
[0361] The television device 9600 can be operated using an operation switch on the housing 9601 or a separate remote control. The remote control can also be operated by the remote control. A display unit for displaying the output information may be provided.
[0362] The television device 9600 includes a receiver and a modem. It can receive more general television broadcasts, and can also be connected to a modem via wired or wireless connection. By connecting to a network, communication can be one-way (sender to receiver) or two-way. It is also possible to communicate information (between a sender and a receiver, or between receivers).
[0363] The television device 9600 also includes an external connection terminal 9604 and a storage medium playback / recording unit 96 02, external memory slot. The external connection terminal 9604 is for connecting USB cables, etc. It can be connected to various cables, enabling data communication with a personal computer, etc. In the storage medium playback / recording unit 9602, a disk-shaped recording medium is inserted and recorded on the recording medium. It is possible to read data stored in the external memory and write data to the recording medium. Displays images and videos stored in the external memory 9606 inserted in the slot. It is also possible to display it on the display unit 9603.
[0364] As described above, the configurations, methods, etc. described in this embodiment may be used in conjunction with the configurations, methods, etc. described in other embodiments. They can be used in any suitable combination. [Explanation of symbols]
[0365] 101 Substrate 102 Oxide insulating film 103a Oxide semiconductor film 103b Oxide semiconductor film 103c Oxide semiconductor film 104a Oxide semiconductor film 104b Oxide semiconductor film 104c Oxide semiconductor film 105 Oxide semiconductor laminate 105a Oxide semiconductor film 105b Oxide semiconductor film 105c Oxide semiconductor film 106 Electrode 107 Gate insulating film 108 Gate electrode 109 Insulating film 113a Oxide semiconductor film 113b Oxide semiconductor film 113c Oxide semiconductor film 114a Oxide semiconductor film 114b Oxide semiconductor film 114c Oxide semiconductor film 115 Oxide semiconductor laminate 115a Oxide semiconductor film 115b Oxide semiconductor film 115c Oxide semiconductor film 116 Electrode 117 Gate insulating film 118 Gate electrode 119 Insulating film 120 Wiring 123b Oxide semiconductor film 123c Oxide semiconductor film 124b Oxide semiconductor film 124c Oxide semiconductor film 125 Oxide semiconductor laminate 125b Oxide semiconductor film 125c Oxide semiconductor film 126 electrode 127 Gate insulating film 128 Gate electrode 129 Insulating Film 133b Oxide semiconductor film 133c Oxide semiconductor film 134b Oxide semiconductor film 134c Oxide semiconductor film 135 Oxide semiconductor laminate 135b Oxide semiconductor film 135c Oxide semiconductor film 136 Electrode 137 Gate insulating film 138 Gate electrode 139 Insulating Film 147a Gate insulating film 147b Gate insulating film 148a Gate electrode 148b Gate electrode 602 Gate wiring 603 Gate wiring 616 Source electrode or drain electrode 628 Transistor 629 Transistor 651 Liquid crystal element 652 Liquid crystal element 690 Capacitance wiring 2000 Crystal Structure 2001 Crystal structure 3001 Main unit 3002 Case 3003a Display section 3003b Display section 3004 Keyboard Buttons 5001 Display section 5002 Hinge 5003 Display Panel 5004 Operation button 5005 Mobile phone 5006 Touch input button 5300 Board 5301 Pixel unit 5302 Scanning line driver circuit 5303 Scanning line driver circuit 5304 Signal line driver circuit 6400 pixels 6401 Switching transistor 6402 Driving transistor 6403 Capacitor 6404 Light emitting element 6405 Signal Line 6406 scan lines 6407 Power line 6408 Common electrode 7001 Light emitting device driving transistor 7002 Light emitting element 7003 Electrode 7004 EL layer 7005 Electrode 7009 Bulkhead 7010 Substrate 7011 Light emitting device driving transistor 7012 Light emitting element 7014 EL layer 7015 Electrode 7016 Membrane 7017 Electrode 7019 Bulkhead 7020 Substrate 7021 Light emitting device driving transistor 7022 Light emitting element 7024 EL layer 7025 Electrode 7027 Electrode 7029 Bulkhead 7030 Oxide insulating film 7031 Gate insulating film 7032 Insulating film 7033 Color filter layer 7034 Overcoat layer 7035 Protective insulating film 7040 Oxide insulating film 7041 Gate insulating film 7042 Insulating film 7051 Gate insulating film 7052 Protective insulating film 7053 Flattening insulating film 7055 Insulating film 9600 Television Equipment 9601 Case 9602 Storage media playback and recording unit 9603 Display section 9604 External connection terminal 9605 Stand 9606 External Memory
Claims
1. A first insulating film; an oxide semiconductor stack on the first insulating film; a second insulating film on the oxide semiconductor stack; a gate electrode; the oxide semiconductor stack is disposed in a channel region of a transistor; the oxide semiconductor stack includes a first oxide semiconductor film that contains indium, gallium, and zinc and has a first crystal structure; and a second oxide semiconductor film that has a region in contact with an upper surface of the first oxide semiconductor film, contains a different number of types of metal elements from the first oxide semiconductor film, and has a second crystal structure different from the first crystal structure, The second oxide semiconductor film has a region having higher crystallinity than the first oxide semiconductor film.
2. A gate electrode; a first insulating film on the gate electrode; an oxide semiconductor stack on the first insulating film; a second insulating film on the oxide semiconductor stack, the oxide semiconductor stack is disposed in a channel region of a transistor; the oxide semiconductor stack includes a first oxide semiconductor film that contains indium, gallium, and zinc and has a first crystal structure; and a second oxide semiconductor film that has a region in contact with an upper surface of the first oxide semiconductor film, contains a different number of types of metal elements from the first oxide semiconductor film, and has a second crystal structure different from the first crystal structure, The second oxide semiconductor film has a region having higher crystallinity than the first oxide semiconductor film.
Citation Information
Patent Citations
Thin film transistor and its manufacturing method
JP2003298062A
Semiconductor device and method for manufacturing the same
JP2007096055A
Semiconductor device and its manufacturing method
JP2007123861A
Thin film transistor and manufacturing method thereof
JP2010040552A
Semiconductor device and method of manufacturing the same
JP2010153802A