Method for producing electrode molded body

The method addresses non-uniform density and moldability issues in electrode manufacturing by using a mold with supports and pressurization, resulting in improved electrode performance.

JP7572525B2Active Publication Date: 2024-10-23FUJIFILM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023142887
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2023-09-04
Publication Date
2024-10-23
Estimated Expiration
2040-06-26

AI Technical Summary

Technical Problem

Existing methods for manufacturing electrodes in batteries, particularly all-solid-state batteries, face issues with non-uniform density distribution and moldability due to solvent retention or the use of multiple components, leading to decreased battery performance.

Method used

A method involving the use of a mold with a frame-shaped side wall and a support member to mold electrode materials, including steps of supply, molding, and removal, with additional supports and pressurization to ensure uniform density distribution and low solvent content.

Benefits of technology

The method achieves an electrode molded body with excellent moldability and uniform density distribution, reducing solvent retention and improving battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572525000002
    Figure 0007572525000002
  • Figure 0007572525000003
    Figure 0007572525000003
  • Figure 0007572525000004
    Figure 0007572525000004
Patent Text Reader

Abstract

To provide a manufacturing method of a molded body for an electrode that can obtain a molded body for an electrode with excellent moldability when molding an electrode material with a small content of solvent.SOLUTION: A manufacturing method of a molded body for an electrode includes, in this order, the steps of preparing an electrode material including an electrode active material, supplying the electrode material to a mold having a frame-shaped side wall defining a space for accommodating the electrode material, and having a first support disposed on the bottom surface of the mold, molding the electrode material along the internal shape of the mold, and taking out the electrode material from the mold.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing an electrode molded body. [Background technology]

[0002] An electrolytic solution is usually used as an electrolyte contained in a battery such as a lithium ion battery. In recent years, from the viewpoint of safety (e.g., prevention of leakage), the development of an all-solid-state battery in which the electrolytic solution is replaced with a solid electrolyte has been considered.

[0003] In the manufacture of electrodes to be used in batteries as described above, a coating liquid containing an electrode material such as an active material and a solvent is usually used (for example, International Publication No. 2017 / 104405 and Japanese Patent No. 3743706).

[0004] In the manufacture of polarizable electrodes for electric double layer capacitors, a technique is known in which activated carbon powder, carbon black, and a binder are dry-kneaded and then rolled into a sheet-like polarizable electrode (for example, JP-A-4-67610). Summary of the Invention [Problem to be solved by the invention]

[0005] In the method of forming an electrode using a coating liquid (for example, International Publication No. 2017 / 104405 and Japanese Patent No. 3743706), it is usually necessary to dry the coating liquid. If the drying is insufficient, the solvent may remain in the electrode, which may deteriorate the battery performance (for example, discharge capacity and output characteristics). In particular, in an all-solid-state battery, it is preferable that the amount of solvent remaining in the electrode is small.

[0006] On the other hand, in a method of forming an electrode without using a coating liquid (for example, JP-A-4-67610), the density distribution (i.e., mass distribution) of the obtained electrode tends to be non-uniform, so there is room for improvement in formability. An electrode having a non-uniform density distribution may lead to a decrease in battery performance. The above-mentioned problem is not limited to the case where a dry electrode material is used, but may also occur when a wet electrode material is used. In addition, the formability of the electrode tends to decrease as the amount of components used to form the electrode increases.

[0007] The present disclosure has been made in consideration of the above circumstances. An object of one embodiment of the present disclosure is to provide a method for producing an electrode molded body that can obtain an electrode molded body with excellent moldability when molding an electrode material with a low solvent content. [Means for solving the problem]

[0008] The present disclosure includes the following aspects. <1> A method for producing an electrode molded body, comprising the steps of: preparing an electrode material containing an electrode active material; supplying the electrode material to a mold having a frame-shaped sidewall portion defining a space for accommodating the electrode material and having a first support disposed on a bottom surface of the mold; molding the electrode material to conform to an internal shape of the mold; and removing the electrode material from the mold, in this order. <2> In the step of forming the electrode material, the electrode material is formed by directly or indirectly contacting the electrode material with a forming member. <1> 2. A method for producing the electrode molded article according to claim 1 . <3> Between the step of supplying the electrode material and the step of molding the electrode material, a step of disposing a second support on the electrode material supplied to the mold is included. <1> or <2> 2. A method for producing the electrode molded article according to claim 1 . <4> Between the step of forming the electrode material and the step of removing the electrode material, a step of placing a second support on the electrode material supplied to the mold is included. <1> or <2> 2. A method for producing the electrode molded article according to claim 1 . <5> The method includes a step of placing a second support on the electrode material supplied to the mold, and the step of placing the second support and the step of molding the electrode material are carried out simultaneously. <1> or <2> 2. A method for producing the electrode molded article according to claim 1 . <6> The second support is a current collector. <3> ~ <5> 13. A method for producing the electrode molded article according to any one of the above items. <7> Between the step of forming the electrode material and the step of removing the electrode material, a step of disposing the electrode material below the first support in the vertical direction by changing a positional relationship between the first support and the electrode material is included. <1> ~ <6> 13. A method for producing the electrode molded article according to any one of the above items. <8> In the step of removing the electrode material, the electrode material and the first support are removed from the mold. <1> ~ <7> 13. A method for producing the electrode molded article according to any one of the above items. <9> The method includes a step of pressing the electrode material between the step of forming the electrode material and the step of removing the electrode material, or after the step of removing the electrode material. <1> ~ <8> 13. A method for producing the electrode molded article according to any one of the above items. <10> In the step of pressing the electrode material, the electrode material is pressed stepwise using a plurality of rolls. <9> 2. A method for producing the electrode molded article according to claim 1 . <11> The electrode material is supplied to the mold by being discharged from a discharge port having an opening / closing mechanism for controlling the supply of the electrode material. <1> ~ <10> 13. A method for producing the electrode molded article according to any one of the above items. <12> The electrode material is supplied to the mold while the discharge port and the mold are moved relative to each other. <11> 2. A method for producing the electrode molded article according to claim 1 . <13> The content of the liquid component in the electrode material is 30 mass % or less with respect to the total mass of the electrode material. <1> ~ <12> 13. A method for producing the electrode molded article according to any one of the above items. <14> The electrode material contains a conductive additive. <1> ~ <13> 13. A method for producing the electrode molded article according to any one of the above items. <15> The first support is a release material. <1> ~ <14> 13. A method for producing the electrode molded article according to any one of the above items. Effect of the Invention

[0009] According to one embodiment of the present disclosure, it is possible to provide a method for producing an electrode molded body that can obtain an electrode molded body with excellent moldability when molding an electrode material with a low solvent content. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a flow chart showing an example of a method for producing an electrode molded body according to the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of a method for producing an electrode molded article according to the present disclosure. [Diagram 3] FIG. 3 is a schematic plan view of the mold shown in FIG. 2(a). [Figure 4] FIG. 4 is a schematic cross-sectional view showing an example of a method for producing an electrode molded article according to the present disclosure. [Diagram 5] FIG. 5 is a flowchart showing a method for producing the positive electrode sheet in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments, and can be implemented with appropriate modifications within the scope of the purpose of the present disclosure. Components indicated by the same reference numerals in each drawing are the same components. Descriptions of components and reference numerals that are the same in each drawing may be omitted. The dimensional ratios in the drawings do not necessarily represent the actual dimensional ratios.

[0012] In the present disclosure, a numerical range expressed using "~" means a range including the numerical values ​​described before and after "~" as the lower and upper limits. In the numerical ranges described in stages in the present disclosure, the upper or lower limit described in a certain numerical range may be replaced with the upper or lower limit of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit described in a certain numerical range may be replaced with a value shown in the examples. In the present disclosure, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved. In the present disclosure, "(meth)acrylic" means both or either one of acrylic and methacrylic. In the present disclosure, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. In the present disclosure, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous. In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In this disclosure, the term "solid content" refers to components that do not disappear through volatilization or evaporation when a 1 g sample is subjected to a drying treatment at 200° C. for 6 hours in a nitrogen atmosphere. In this disclosure, ordinal numbers (e.g., "first" and "second") are terms used to distinguish components, and do not limit the number of components or the priority of the components.

[0013] <Method of manufacturing electrode molded body> The method for producing an electrode molded body according to the present disclosure includes, in this order, a step of preparing an electrode material containing an electrode active material (hereinafter also referred to as a "preparation step"); a step of supplying the electrode material to a mold having a frame-shaped side wall portion defining a space portion for accommodating the electrode material and a first support disposed on the bottom surface of the mold (hereinafter also referred to as a "supply step"); a step of molding the electrode material along the internal shape of the mold (hereinafter also referred to as a "molding step"); and a step of removing the electrode material from the mold (hereinafter also referred to as a "removal step"). The method for producing an electrode molded body according to the present disclosure includes the above steps, thereby making it possible to obtain an electrode molded body having excellent moldability. In the present disclosure, "excellent moldability" means that the density distribution (i.e., mass distribution) has a high uniformity.

[0014] The reason why the method for producing an electrode molded body according to the present disclosure exhibits the above-mentioned effects is presumed to be as follows. When the electrode material is molded without using a mold, the electrode material may be unevenly distributed due to the movement of the electrode material, resulting in an uneven density distribution of the electrode molded body. On the other hand, in the manufacturing method of the electrode molded body according to the present disclosure, the electrode material is supplied to a mold having a frame-shaped side wall portion defining a space portion for accommodating the electrode material and a first support is arranged on the bottom surface of the mold, and the electrode material is molded along the internal shape of the mold, thereby suppressing uneven distribution of the electrode material that may occur during the molding process. In other words, by molding the electrode material in a state where there is a physical constraint due to the internal shape of the mold (for example, the frame-shaped side wall portion), it is possible to suppress the density distribution of the electrode molded body from becoming uneven due to the movement of the electrode material. Therefore, according to the manufacturing method of the electrode molded body according to the present disclosure, an electrode molded body with excellent moldability can be obtained.

[0015] In addition, in the manufacturing method of the electrode molded body according to the present disclosure, the electrode material can be molded into a desired shape by using a molding die. Since the manufacturing method of the electrode molded body according to the present disclosure does not necessarily require processing (e.g., cutting) the electrode molded body into a desired shape, it is possible to suppress the occurrence of shape defects (e.g., collapse of the cut surface) caused by the above processing.

[0016] The method for producing an electrode molded article according to the present disclosure will be described with reference to the drawings, in which: Fig. 1 is a flow chart showing an example of the method for producing an electrode molded article according to the present disclosure.

[0017] In S110, an electrode material including an electrode active material is prepared (preparation step). The electrode material may be prepared in advance or may be prepared in S110.

[0018] In S120, an electrode material is supplied to the mold (supplying step). In S120, the mold has a frame-shaped side wall portion that defines a space portion for accommodating the electrode material, and a first support is disposed on the bottom surface of the mold.

[0019] In S130, the electrode material is molded according to the internal shape of the mold (molding step). The step in S130 may be performed while the step in S120 is being performed.

[0020] In S140, the electrode material is removed from the mold (removal step).

[0021] Hereinafter, each step of the method for producing an electrode molded article according to the present disclosure will be specifically described.

[0022] <<Preparation process>> The method for producing an electrode molded body according to the present disclosure includes a step of preparing an electrode material containing an electrode active material (preparation step). In the present disclosure, "preparing an electrode material" means making the electrode material usable, and includes preparing an electrode material unless otherwise specified. That is, in the preparation step, a pre-prepared electrode material or a commercially available electrode material may be prepared, or an electrode material may be prepared.

[0023] [Electrode material] The electrode material includes an electrode active material. The electrode material may include components other than the electrode active material as necessary. The components of the electrode material will be described below.

[0024] (electrode active material) An electrode active material is a material capable of inserting and releasing ions of a metal element belonging to Group 1 or Group 2 of the periodic table. Examples of electrode active materials include positive electrode active materials and negative electrode active materials.

[0025] -Cathode active material- The positive electrode active material is not limited, and any known active material used for positive electrodes can be used. The positive electrode active material is preferably a positive electrode active material that can reversibly insert and release lithium ions.

[0026] Examples of the positive electrode active material include transition metal oxides and elements that can be composited with lithium (such as sulfur). Among the above, the positive electrode active material is preferably a transition metal oxide.

[0027] The transition metal oxide is preferably a transition metal oxide containing at least one transition metal element (hereinafter referred to as "element Ma") selected from the group consisting of Co (cobalt), Ni (nickel), Fe (iron), Mn (manganese), Cu (copper), and V (vanadium).

[0028] When the transition metal oxide contains Li and the element Ma, the molar ratio of Li to the element Ma (amount of substance of Li / amount of substance of element Ma) is preferably 0.3 to 2.2. In the present disclosure, the "amount of substance of element Ma" refers to the total amount of substance of all elements corresponding to the element Ma.

[0029] The transition metal oxide may also contain at least one transition metal element (hereinafter referred to as "element Mb") selected from the group consisting of Group 1 elements other than lithium, Group 2 elements, Al (aluminum), Ga (gallium), In (indium), Ge (germanium), Sn (tin), Pb (lead), Sb (antimony), Bi (bismuth), Si (silicon), P (phosphorus), and B (boron). The content of element Mb (i.e., the total content of all elements corresponding to element Mb) is preferably 0 mol% to 30 mol% with respect to the substance amount of element Ma.

[0030] Examples of the transition metal oxide include transition metal oxides having a layered rock salt structure, transition metal oxides having a spinel structure, lithium-containing transition metal phosphate compounds, lithium-containing transition metal halide phosphate compounds, and lithium-containing transition metal silicate compounds.

[0031] Examples of transition metal oxides having a layered rock salt structure include LiCoO2 (lithium cobalt oxide [LCO]), LiNi2O2 (lithium nickel oxide), LiNi 0.85 Co 0.10 Al 0.05 O2 (Lithium Nickel Cobalt Aluminum Oxide [NCA]), LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (lithium nickel manganese cobalt oxide [NMC]), and LiNi 0.5 Mn 0.5 O2 (lithium manganese nickel oxide).

[0032] Examples of transition metal oxides having a spinel structure include LiCoMnO4, Li2FeMn3O8, Li2CuMn3O8, Li2CrMn3O8, and Li2NiMn3O8.

[0033] Examples of lithium-containing transition metal phosphate compounds include olivine-type iron phosphates (e.g., LiFePO4 and Li3Fe2(PO4)3), iron pyrophosphates (e.g., LiFeP2O7), cobalt phosphates (e.g., LiCoPO4), and monoclinic Nasicon-type vanadium phosphates (e.g., Li3V2(PO4)3 (lithium vanadium phosphate)).

[0034] Examples of lithium-containing transition metal halophosphate compounds include iron fluorophosphates (e.g., LiFePOF), manganese fluorophosphates (e.g., LiMnPOF), and cobalt fluorophosphates (e.g., LiCoPOF).

[0035] Examples of lithium-containing transition metal silicate compounds include Li2FeSiO4, Li2MnSiO4, and Li2CoSiO4.

[0036] The transition metal oxide is preferably a transition metal oxide having a layered rock salt structure, such as LiCoO2 (lithium cobalt oxide [LCO]), LiNi 0.85 Co 0.10 Al 0.05 O2 (nickel cobalt lithium aluminate [NCA]), and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (lithium nickel manganese cobalt oxide [NMC]) and more preferably at least one compound selected from the group consisting of:

[0037] The positive electrode active material may be a commercially available product or may be a synthetic product produced by a known method (e.g., a calcination method). For example, the positive electrode active material obtained by the calcination method may be washed with water, an acidic aqueous solution, an alkaline aqueous solution, or an organic solvent.

[0038] The composition of the positive electrode active material is measured using inductively coupled plasma (ICP) emission spectrometry.

[0039] The shape of the positive electrode active material is not limited, but from the viewpoint of ease of handling, it is preferably in the form of particles.

[0040] The volume average particle diameter of the positive electrode active material is not limited and can be, for example, 0.1 μm to 50 μm. The volume average particle diameter of the positive electrode active material is preferably 0.3 μm to 40 μm, and more preferably 0.5 μm to 30 μm. When the volume average particle diameter of the positive electrode active material is 0.3 μm or more, an aggregate of the electrode material can be easily formed, and the electrode material can be prevented from scattering during handling. When the volume average particle diameter of the positive electrode active material is 40 μm or less, the thickness of the electrode molded body can be easily adjusted, and the generation of voids during the molding process can be prevented.

[0041] The volume average particle diameter of the positive electrode active material is measured by the following method. A dispersion containing 0.1 mass % of the positive electrode active material is prepared by mixing the positive electrode active material with a solvent (e.g., heptane, octane, toluene, or xylene). The dispersion is irradiated with 1 kHz ultrasonic waves for 10 minutes and used as a measurement sample. Using a laser diffraction / scattering type particle size distribution measurement device (e.g., LA-920 manufactured by Horiba, Ltd.), data is collected 50 times under a temperature of 25°C to obtain the volume average particle diameter. A quartz cell is used as the measurement cell. The above measurement is performed using five samples, and the average of the measured values ​​is used as the volume average particle diameter of the positive electrode active material. For other detailed conditions, refer to "JIS Z 8828:2013" as necessary.

[0042] Examples of a method for adjusting the particle size of the positive electrode active material include a method using a pulverizer or a classifier.

[0043] The electrode material may contain one type of positive electrode active material alone, or may contain two or more types of positive electrode active materials.

[0044] The content of the positive electrode active material is preferably 10% by mass to 95% by mass, more preferably 30% by mass to 90% by mass, further preferably 50% by mass to 85% by mass, and particularly preferably 70% by mass to 80% by mass, based on the total solid mass of the electrode material.

[0045] -Negative electrode active material- The negative electrode active material is not limited, and any known active material used for a negative electrode can be used. The negative electrode active material is preferably a negative electrode active material that can reversibly insert and release lithium ions.

[0046] Examples of the negative electrode active material include carbonaceous materials, metal oxides (e.g., tin oxide), silicon oxide, metal composite oxides, lithium alone, lithium alloys (e.g., lithium aluminum alloys), and metals capable of forming alloys with lithium (e.g., Sn, Si, and In). Among the above, the negative electrode active material is preferably a carbonaceous material or a lithium composite oxide from the viewpoint of reliability.

[0047] A carbonaceous material is a material that is substantially composed of carbon. Examples of carbonaceous materials include petroleum pitch, carbon black (e.g., acetylene black), graphite (e.g., natural graphite and artificial graphite (e.g., vapor-grown graphite)), hard carbon, and carbonaceous materials obtained by burning synthetic resins (e.g., polyacrylonitrile (PAN) and furfuryl alcohol resin). Examples of carbonaceous materials include carbon fibers (e.g., polyacrylonitrile-based carbon fibers, cellulose-based carbon fibers, pitch-based carbon fibers, vapor-grown carbon fibers, dehydrated PVA (polyvinyl alcohol)-based carbon fibers, lignin carbon fibers, glassy carbon fibers, and activated carbon fibers). Examples of graphite include mesophase microspheres, graphite whiskers, and tabular graphite. In the present disclosure, "tabular" means a shape having two main planes facing in opposite directions.

[0048] The metal composite oxide is preferably a metal composite oxide capable of absorbing and releasing lithium. From the viewpoint of high current density charge / discharge characteristics, the metal composite oxide capable of absorbing and releasing lithium preferably contains at least one element selected from the group consisting of titanium and lithium.

[0049] The metal oxide and the metal composite oxide are particularly preferably amorphous oxides. Here, "amorphous" means a substance having a broad scattering band with a peak in the region of 20° to 40° in 2θ value in X-ray diffraction method using CuKα radiation. The amorphous oxide may have crystalline diffraction lines. In the amorphous oxide, the strongest intensity of the crystalline diffraction lines observed in the region of 40° to 70° in 2θ value is preferably 100 times or less, more preferably 5 times or less, of the diffraction line intensity of the peak of the broad scattering band observed in the region of 20° to 40° in 2θ value. It is particularly preferable that the amorphous oxide does not have crystalline diffraction lines.

[0050] The metal oxides and composite metal oxides are also preferably chalcogenides, which are reaction products of metal elements and elements of Group 16 of the periodic table.

[0051] Among the compound group consisting of amorphous oxides and chalcogenides, amorphous oxides and chalcogenides of metalloid elements are preferred, and oxides and chalcogenides containing at least one element selected from the group consisting of elements of groups 13 to 15 in the periodic table, Al, Ga, Si, Sn, Ge, Pb, Sb, and Bi are more preferred.

[0052] Preferable examples of amorphous oxides and chalcogenides include Ga2O3, SiO, GeO, SnO, SnO2, PbO, PbO2, Pb2O3, Pb2O4, Pb3O4, Sb2O3, Sb2O4, Sb2O8Bi2O3, Sb2O8Si2O3, Bi2O4, SnSiO3, GeS, SnS, SnS2, PbS, PbS2, Sb2S3, Sb2S5, and SnSiS3. The above compounds may also be composite oxides with lithium (e.g., Li2SnO2).

[0053] It is also preferable that the negative electrode active material further contains titanium. From the viewpoint of excellent rapid charge / discharge characteristics due to small volume fluctuation during the absorption and release of lithium ions, and of enabling an improvement in the life of the lithium ion secondary battery by suppressing electrode deterioration, the negative electrode active material containing titanium is Li4Ti5O 12 (lithium titanate [LTO]) is preferred.

[0054] The negative electrode active material may be a commercially available product or may be a synthetic product produced by a known method (e.g., a calcination method). For example, the negative electrode active material obtained by the calcination method may be washed with water, an acidic aqueous solution, an alkaline aqueous solution, or an organic solvent.

[0055] The negative electrode active material is available, for example, as CGB20 (Nippon Graphite Industries Co., Ltd.).

[0056] The composition of the negative electrode active material is measured by inductively coupled plasma (ICP) emission spectrometry.

[0057] The shape of the negative electrode active material is not limited, but is preferably particulate from the viewpoints of ease of handling and ease of control of uniformity during mass production.

[0058] The volume average particle diameter of the negative electrode active material is preferably 0.1 μm to 60 μm, more preferably 0.3 μm to 50 μm, and particularly preferably 0.5 μm to 40 μm. When the volume average particle diameter of the negative electrode active material is 0.1 μm or more, an aggregate of the electrode material can be easily formed, and the electrode material can be prevented from scattering during handling. When the volume average particle diameter of the negative electrode active material is 60 μm or less, the thickness of the electrode molded body can be easily adjusted, and the generation of voids during the molding process can be prevented. The volume average particle diameter of the negative electrode active material is measured by a method similar to the method for measuring the volume average particle diameter of the positive electrode active material.

[0059] The method for adjusting the particle size of the negative electrode active material includes, for example, a method using a pulverizer or a classifier. In the above method, for example, a mortar, a ball mill, a sand mill, a vibration ball mill, a satellite ball mill, a planetary ball mill, a swirling airflow type jet mill, or a sieve is preferably used. In the pulverization of the negative electrode active material, wet pulverization using water or an organic solvent (e.g., methanol) can also be performed as necessary. The method for adjusting to a desired particle size is preferably classification. In the classification, for example, a sieve or a wind classifier can be used. The classification may be a dry type or a wet type.

[0060] When an amorphous oxide containing Sn, Si, or Ge is used as the negative electrode active material, preferred negative electrode active materials that can be used in combination with the amorphous oxide include, for example, a carbon material capable of absorbing and releasing lithium ions or lithium metal, lithium, a lithium alloy, and a metal capable of alloying with lithium.

[0061] The electrode material may contain one type of negative electrode active material alone, or may contain two or more types of negative electrode active materials.

[0062] The content of the negative electrode active material is preferably 10% by mass to 80% by mass, more preferably 20% by mass to 80% by mass, further preferably 30% by mass to 80% by mass, and particularly preferably 40% by mass to 75% by mass, based on the total solid mass of the electrode material.

[0063] The surfaces of the positive electrode active material and the negative electrode active material may be coated with a surface coating agent. Examples of the surface coating agent include metal oxides containing Ti, Nb, Ta, W, Zr, Si, or Li. Examples of the metal oxides include titanate spinel, tantalum oxides, niobium oxides, and lithium niobate compounds. Specific examples of the compounds include Li4Ti5O 12 , LiTaO3, LiNbO3, LiAlO2, Li2ZrO3, Li2WO4, Li2TiO3, Li2B4O7, Li3PO4, Li2MoO4, and LiBO2.

[0064] (Inorganic solid electrolyte) From the viewpoint of improving battery performance (e.g., discharge capacity and output characteristics), the electrode material preferably contains an inorganic solid electrolyte. Here, the term "solid electrolyte" refers to a solid electrolyte capable of transferring ions therein.

[0065] Inorganic solid electrolytes are not electrolytes that contain an organic substance as the main ion-conducting material, and are therefore clearly distinguished from organic solid electrolytes (e.g., polymer electrolytes such as polyethylene oxide (PEO) and organic electrolyte salts such as lithium bis(trifluoromethanesulfonyl)imide (LiTFSI)). In addition, inorganic solid electrolytes are solid in the steady state, and are not dissociated or liberated into cations or anions. Therefore, they are also clearly distinguished from inorganic electrolyte salts that are dissociated or liberated into cations or anions in electrolyte solutions and polymers (e.g., LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI), and LiCl).

[0066] There are no limitations on the inorganic solid electrolyte as long as it has ionic conductivity of a metal element belonging to Group 1 or 2 of the periodic table, and it is common for the inorganic solid electrolyte to have no electronic conductivity.

[0067] When the electrode molded article obtained by the method for producing an electrode molded article according to the present disclosure is used in a lithium ion battery, the inorganic solid electrolyte preferably has ionic conductivity for lithium ions.

[0068] Examples of inorganic solid electrolytes include sulfide-based inorganic solid electrolytes and oxide-based inorganic solid electrolytes. Among the above, the inorganic solid electrolyte is preferably a sulfide-based inorganic solid electrolyte from the viewpoint of forming a good interface between the active material and the inorganic solid electrolyte.

[0069] -Sulfide-based inorganic solid electrolyte- The sulfide-based inorganic solid electrolyte preferably contains a sulfur atom (S), has the ionic conductivity of a metal element belonging to Group 1 or Group 2 of the periodic table, and has electronic insulation properties.

[0070] The sulfide-based inorganic solid electrolyte more preferably contains at least Li, S, and P and has lithium ion conductivity. The sulfide-based inorganic solid electrolyte may contain elements other than Li, S, and P as necessary.

[0071] An example of the sulfide-based inorganic solid electrolyte is an inorganic solid electrolyte having a composition represented by the following formula (A).

[0072] L a1 M b1 P c1 S d1 A e1 :Formula (A)

[0073] In formula (A), L represents at least one element selected from the group consisting of Li, Na, and K, and is preferably Li.

[0074] In formula (A), M represents at least one element selected from the group consisting of B, Zn, Sn, Si, Cu, Ga, Sb, Al, and Ge, and is preferably B, Sn, Si, Al, or Ge, and more preferably Sn, Al, or Ge.

[0075] In formula (A), A represents at least one element selected from the group consisting of I, Br, Cl, and F, and is preferably I or Br, and more preferably I.

[0076] In formula (A), a1 represents an integer of 1 to 12, preferably an integer of 1 to 9, and more preferably an integer of 1.5 to 4.

[0077] In formula (A), b1 represents an integer of 0 to 1, and more preferably an integer of 0 to 0.5.

[0078] In formula (A), c1 represents 1.

[0079] In formula (A), d1 represents an integer of 2 to 12, preferably an integer of 3 to 7, and more preferably an integer of 3.25 to 4.5.

[0080] In formula (A), e1 represents an integer of 0 to 5, preferably an integer of 0 to 3, and more preferably an integer of 0 to 1.

[0081] In formula (A), it is preferable that b1 and e1 are 0, it is more preferable that b1 and e1 are 0 and the ratio of a1, c1, and d1 (i.e., a1:c1:d1) is 1 to 9:1:3 to 7, and it is particularly preferable that b1 and e1 are 0 and the ratio of a1, c1, and d1 (i.e., a1:c1:d1) is 1.5 to 4:1:3.25 to 4.5.

[0082] The composition ratio of each element can be controlled, for example, by adjusting the blending amounts of raw material compounds when producing the sulfide-based inorganic solid electrolyte.

[0083] The sulfide-based inorganic solid electrolyte may be non-crystalline (glass), crystallized (glass ceramic), or only partially crystallized. Examples of the sulfide-based inorganic solid electrolyte include Li-PS-based glass containing Li, P, and S, and Li-PS-based glass ceramic containing Li, P, and S. Among the above, the sulfide-based inorganic solid electrolyte is preferably Li-PS-based glass.

[0084] The lithium ion conductivity of sulfide-based inorganic solid electrolytes is 1×10 -4 S / cm or more is preferable, and 1×10 -3 The upper limit of the lithium ion conductivity of the sulfide-based inorganic solid electrolyte is not limited. The lithium ion conductivity of the sulfide-based inorganic solid electrolyte is, for example, 1×10 -1 It is practical to have a value of less than S / cm.

[0085] The sulfide-based inorganic solid electrolyte can be produced, for example, by (1) a reaction between lithium sulfide (LiS) and a phosphorus sulfide (e.g., diphosphorus pentasulfide (P2S5)), (2) a reaction between lithium sulfide and at least one of elemental phosphorus and elemental sulfur, or (3) a reaction between lithium sulfide and a phosphorus sulfide (e.g., diphosphorus pentasulfide (P2S5)) and at least one of elemental phosphorus and elemental sulfur.

[0086] In the production of Li-PS-based glass and Li-PS-based glass ceramics, the molar ratio of Li2S to P2S5 (Li2S:P2S5) is preferably 65:35 to 85:15, and more preferably 68:32 to 77:23. By setting the molar ratio of Li2S to P2S5 in the above range, the lithium ion conductivity can be further increased.

[0087] Examples of sulfide-based inorganic solid electrolytes include compounds obtained by using a raw material composition containing Li2S and sulfides of elements of groups 13 to 15. Examples of raw material compositions include Li2S-P2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2O5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, Li2S-GeS2-ZnS, Li2S- Ga2S3, Li2S-GeS2-Ga2S3, Li2S-GeS2-P2S5, Li2S-GeS2-Sb2S5, Li2S-GeS2-Al2S3, Li2S-SiS2, Li2S-Al2S3, Li2S-S iS2-Al2S3, Li2S-SiS2-P2S5, Li2S-SiS2-P2S5-LiI, Li2S-SiS2-LiI, Li2S-SiS2-Li4SiO4, Li2S-SiS2-Li3PO4, and Li 10 GeP2S 12 Among the above, the raw material composition is preferably Li2S-P2S5, Li2S-GeS2-Ga2S3, Li2S-SiS2-P2S5, Li2S-SiS2-Li4SiO4, Li2S-SiS2-Li3PO4, Li2S-LiI-Li2O-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-GeS2-P2S5, or Li 10 GeP2S 12 It is preferable that Li2S-P2S5, Li 10 GeP2S 12 , or Li2S-P2S5-SiS2, more preferably.

[0088] Examples of the method for producing a sulfide-based inorganic solid electrolyte material using the above-mentioned raw material composition include an amorphization method. Examples of the amorphization method include a mechanical milling method and a melt quenching method. Among the above, the mechanical milling method is preferred from the viewpoint of enabling processing at room temperature and simplifying the manufacturing process.

[0089] -Oxide-based inorganic solid electrolyte- The oxide-based inorganic solid electrolyte preferably contains oxygen atoms (O), has the ionic conductivity of a metal element belonging to Group 1 or 2 of the periodic table, and has electronic insulation properties.

[0090] The ionic conductivity of oxide-based inorganic solid electrolytes is 1×10 -6 S / cm or more is preferable, and 5×10 -6 More preferably, it is 1×10 -5 It is particularly preferable that the ionic conductivity of the oxide-based inorganic solid electrolyte is 1×10 S / cm or more. There is no upper limit to the ionic conductivity of the oxide-based inorganic solid electrolyte. -1 It is practical to have a value of less than S / cm.

[0091] Examples of oxide-based inorganic solid electrolytes include Li xa La ya TiO3 (hereinafter referred to as "LLT"; xa satisfies 0.3≦xa≦0.7, and ya satisfies 0.3≦ya≦0.7); Li xb La yb Zr zb M bb mb O nb (M bb is at least one element selected from the group consisting of Al, Mg, Ca, Sr, V, Nb, Ta, Ti, Ge, In, and Sn; xb satisfies 5≦xb≦10, yb satisfies 1≦yb≦4, zb satisfies 1≦zb≦4, mb satisfies 0≦mb≦2, and nb satisfies 5≦nb≦20; Li xc B yc M cczc O nc (M cc is at least one element selected from the group consisting of C, S, Al, Si, Ga, Ge, In, and Sn. xc satisfies 0 ≦ xc ≦ 5, yc satisfies 0 ≦ yc ≦ 1, zc satisfies 0 ≦ zc ≦ 1, and nc satisfies 0 ≦ nc ≦ 6.); Li xd (Al,Ga) yd (Ti,Ge) zd Si ad P md O nd (xd satisfies 1 ≦ xd ≦ 3, yd satisfies 0 ≦ yd ≦ 1, zd satisfies 0 ≦ zd ≦ 2, ad satisfies 0 ≦ ad ≦ 1, md satisfies 1 ≦ md ≦ 7, and nd satisfies 3 ≦ nd ≦ 13.); Li (3-2xe) M ee xe D ee O(xe satisfies 0 ≦ xe ≦ 0.1, M ee represents a divalent metal atom, D ee represents a halogen atom or a combination of two or more halogen atoms.); Li xf Si yf O zf (xf satisfies 1 ≦ xf ≦ 5, yf satisfies 0 < yf ≦ 3, zf satisfies 1 ≦ zf ≦ 10.); Li xg S yg O zg (xg satisfies 1 ≦ xg ≦ 3, yg satisfies 0 < yg ≦ 2, zg satisfies 1 ≦ zg ≦ 10.); Li3BO3; Li3BO3 - Li2SO4; Li2O - B2O3 - P2O5; Li2O - SiO2; Li6BaLa2Ta2O 12 ; Li3PO (4-3 / 2w) N w (w satisfies w < 1.); Li having a LISICON (Lithium super ionic conductor) type crystal structure 3.5 Zn 0.25 GeO4; La having a perovskite type crystal structure 0.55 Li 0.35 TiO3; LiTi2P3O having a NASICON (Natrium super ionic conductor) type crystal structure 12 ; Li1+xh+yh (Al,Ga) xh (Ti,Ge) 2-xh S yh P 3-yh O 12 (xh satisfies 0≦xh≦1, and yh satisfies 0≦yh≦1); and Li7La3Zr2O having a garnet-type crystal structure. 12 (hereinafter referred to as "LLZ").

[0092] As the oxide-based inorganic solid electrolyte, a phosphorus compound containing Li, P, and O is also preferred. Examples of the phosphorus compound containing Li, P, and O include lithium phosphate (Li3PO4), LiPON in which part of the oxygen in lithium phosphate is replaced with nitrogen, and LiPOD1 (D1 is at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zr, Nb, Mo, Ru, Ag, Ta, W, Pt, and Au).

[0093] As an oxide-based inorganic solid electrolyte, LiA 1 ON(A 1 is at least one element selected from the group consisting of Si, B, Ge, Al, C, and Ga.) is also preferred.

[0094] Among the above, oxide-based inorganic solid electrolytes include LLT, Li xb La yb Zr zb M bb mb O nb (M bb , xb, yb, zb, mb, and nb are as defined above. ), LLZ, Li3BO3, Li3BO3-Li2SO4, or Li xd (Al,Ga) yd (Ti,Ge) zd S ad P md O nd (xd, yd, zd, ad, md, and nd are as described above), and LLT, LLZ, LAGP (Li 1.5 Al 0.5 Ge 1.5(PO4)3), or LATP ([Li 1.4 Ti2Si 0.4 P 2.6 O 12 ]-AlPO4), more preferably, LLZ.

[0095] The inorganic solid electrolyte is preferably in the form of particles.

[0096] The volume average particle size of the inorganic solid electrolyte is preferably 0.01 μm or more, more preferably 0.1 μm or more, and is preferably 100 μm or less, more preferably 50 μm or less.

[0097] The volume average particle diameter of the inorganic solid electrolyte is measured by the following method. A dispersion containing 1 mass% of the inorganic solid electrolyte is prepared by mixing the inorganic solid electrolyte with water (heptane is used when measuring the volume average particle diameter of a substance unstable in water). The dispersion is irradiated with 1 kHz ultrasound for 10 minutes and used as the measurement sample. Using a laser diffraction / scattering type particle size distribution measuring device (e.g., LA-920 manufactured by Horiba, Ltd.), data is collected 50 times under the condition of a temperature of 25°C to obtain the volume average particle diameter. A quartz cell is used as the measurement cell. The above measurement is performed using five samples, and the average of the measured values ​​is used as the volume average particle diameter of the inorganic solid electrolyte. For other detailed conditions, refer to "JIS Z 8828:2013" as necessary.

[0098] The electrode material may contain a single type of inorganic solid electrolyte, or may contain two or more types of inorganic solid electrolytes.

[0099] When the electrode material contains an inorganic solid electrolyte, the content of the inorganic solid electrolyte is preferably 1% by mass or more, more preferably 5% by mass or more, and particularly preferably 10% by mass or more, based on the total solid mass of the electrode material, from the viewpoints of reducing the interface resistance and maintaining the battery characteristics (e.g., improving cycle characteristics). From the same viewpoint, the content of the inorganic solid electrolyte is preferably 90% by mass or less, more preferably 70% by mass or less, and particularly preferably 50% by mass or less, based on the total solid mass of the electrode material.

[0100] (binder) From the viewpoint of improving the adhesion between the electrode materials, it is preferable that the electrode material contains a binder. The binder is not limited as long as it is an organic polymer, and a known binder used as a binder in the positive or negative electrode of a battery material can be used. Examples of the binder include fluorine-containing resin, hydrocarbon-based thermoplastic resin, acrylic resin, and urethane resin.

[0101] Examples of fluorine-containing resins include polytetrafluoroethylene (PTFE), polyvinylene difluoride (PVdF), and a copolymer of polyvinylene difluoride and hexafluoropropylene (PVdF-HFP).

[0102] Examples of the hydrocarbon thermoplastic resin include polyethylene, polypropylene, styrene butadiene rubber (SBR), hydrogenated styrene butadiene rubber (HSBR), butylene rubber, acrylonitrile butadiene rubber, polybutadiene, and polyisoprene.

[0103] Examples of acrylic resins include polymethyl(meth)acrylate, polyethyl(meth)acrylate, polyisopropyl(meth)acrylate, polyisobutyl(meth)acrylate, polybutyl(meth)acrylate, polyhexyl(meth)acrylate, polyoctyl(meth)acrylate, polydodecyl(meth)acrylate, polystearyl(meth)acrylate, poly2-hydroxyethyl(meth)acrylate, poly(meth)acrylic acid, polybenzyl(meth)acrylate, polyglycidyl(meth)acrylate, polydimethylaminopropyl(meth)acrylate, and copolymers of monomers that form the above resins.

[0104] The binder may also be a copolymer of a vinyl monomer, such as a methyl (meth)acrylate-styrene copolymer, a methyl (meth)acrylate-acrylonitrile copolymer, or a butyl (meth)acrylate-acrylonitrile-styrene copolymer.

[0105] The weight average molecular weight of the binder is preferably 10,000 or more, more preferably 20,000 or more, and particularly preferably 50,000 or more.The weight average molecular weight of the binder is preferably 1,000,000 or less, more preferably 200,000 or less, and particularly preferably 100,000 or less.

[0106] The moisture concentration in the binder is preferably 100 ppm or less on a mass basis.

[0107] The metal concentration in the binder is preferably 100 ppm or less on a mass basis.

[0108] The electrode material may contain a single binder or may contain two or more binders.

[0109] When the electrode material contains a binder, the content of the binder is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and particularly preferably 1% by mass or more, based on the total solid mass of the electrode material, from the viewpoint of reducing and maintaining the interface resistance. From the viewpoint of battery performance, the content of the binder is preferably 10% by mass or less, more preferably 5% by mass or less, and particularly preferably 3% by mass or less, based on the total solid mass of the electrode material.

[0110] When the electrode material contains an electrode active material, an inorganic solid electrolyte, and a binder, the ratio of the total mass of the active material and the inorganic solid electrolyte to the mass of the binder ([mass of active material+mass of inorganic solid electrolyte] / [mass of binder]) is preferably 1,000 to 1, more preferably 500 to 2, and particularly preferably 100 to 10.

[0111] (Conductive assistant) From the viewpoint of improving the electronic conductivity of the active material, the electrode material preferably contains a conductive assistant. The conductive assistant is not limited, and a known conductive assistant can be used. In particular, when the electrode material contains a positive electrode active material, the electrode material preferably contains a conductive assistant.

[0112] Examples of the conductive assistant include graphite (e.g., natural graphite and artificial graphite), carbon black (e.g., acetylene black, ketjen black, and furnace black), amorphous carbon (e.g., needle coke), carbon fibers (e.g., vapor-grown carbon fibers and carbon nanotubes), other carbonaceous materials (e.g., graphene and fullerene), metal powders (e.g., copper powder and nickel powder), metal fibers (e.g., copper fibers and nickel fibers), and conductive polymers (e.g., polyaniline, polypyrrole, polythiophene, polyacetylene, and polyphenylene derivatives).

[0113] Among the above, the conductive assistant is preferably at least one type of conductive assistant selected from the group consisting of carbon fibers and metal fibers.

[0114] Examples of the shape of the conductive assistant include fibrous, needle-like, cylindrical, dumbbell-like, disk-like, and elliptical sphere-like shapes. Among the above, the conductive assistant is preferably fibrous in terms of improving the electronic conductivity of the active material.

[0115] The aspect ratio of the conductive assistant is preferably 1.5 or more, and more preferably 5 or more. When the aspect ratio of the conductive assistant is 1.5 or more, the electronic conductivity of the electrode active material can be improved, and therefore the output characteristics of the battery can be improved.

[0116] The aspect ratio of the conductive assistant is preferably equal to or less than 10,000, more preferably equal to or less than 5,000, and particularly preferably equal to or less than 1,000. Furthermore, the aspect ratio of the conductive assistant is preferably equal to or less than 500, more preferably equal to or less than 300, and particularly preferably equal to or less than 100. By making the aspect ratio of the conductive assistant equal to or less than 10,000, the dispersibility of the conductive assistant can be improved, and a short circuit caused by the conductive assistant penetrating through the electrode molded body can be efficiently prevented.

[0117] The aspect ratio of the conductive assistant is measured by the following method. SEM images of three arbitrary fields of view taken at 1000 to 3000 magnifications using a scanning electron microscope (SEM) (e.g., XL30 manufactured by PHILIPS) are converted into BMP (bitmap) files. Images of 50 conductive assistants are captured using image analysis software (e.g., "A-zo-kun", an integrated application of IP-1000PC manufactured by Asahi Engineering Co., Ltd.). The maximum and minimum values ​​of the length of each conductive assistant are read in a state where each conductive assistant is observed without overlapping. The "maximum length of the conductive assistant" refers to the length (i.e., the major axis length) of the line segment with the maximum length among the line segments from a certain point to another point on the periphery of the conductive assistant. The "minimum length of the conductive assistant" refers to the length (i.e., the minor axis length) of the line segment with the minimum length among the line segments from a certain point to another point on the periphery of the conductive assistant that are perpendicular to the line segment showing the maximum length. Of the maximum length values ​​(major axis lengths) of each of the 50 conductive assistants, the average value (A) of 40 values ​​excluding the top 5 and bottom 5 is calculated. Next, of the minimum length values ​​(minor axis lengths) of each of the 50 conductive assistants, the average value (B) of 40 values ​​excluding the top 5 and bottom 5 is calculated. The aspect ratio of the conductive assistant is calculated by dividing the average value (A) by the average value (B).

[0118] The minor axis length of the conductive assistant is preferably 10 μm or less, more preferably 8 μm or less, and particularly preferably 5 μm or less.

[0119] The minor axis length of the conductive assistant is preferably 1 nm or more, more preferably 3 nm or more, and particularly preferably 5 nm or more.

[0120] The minor axis length of the conductive assistant is the minimum value of the lengths of 50 conductive assistants calculated in the method for measuring the aspect ratio of the conductive assistant.

[0121] The average minor axis length of the conductive assistant is preferably 8 μm or less, more preferably 5 μm or less, and particularly preferably 3 μm or less.

[0122] The average minor axis length of the conductive assistant is preferably 1 nm or more, more preferably 2 nm or more, and particularly preferably 3 nm or more.

[0123] The average minor axis length of the conductive additive is the average value of the minor axis lengths of each conductive additive, excluding the top 10% (i.e., top 5) and bottom 10% (i.e., bottom 5) of the minimum lengths (minor axis lengths) of 50 conductive additives calculated using the method for measuring the aspect ratio of the conductive additive.

[0124] The electrode material may contain one type of conductive assistant, or may contain two or more types of conductive assistants.

[0125] When the electrode material contains a conductive assistant, the content of the conductive assistant is preferably more than 0 mass % and not more than 10 mass %, more preferably 0.5 mass % to 8 mass %, and particularly preferably 1 mass % to 7 mass %, relative to the total solid mass of the electrode material, from the viewpoint of improving the electronic conductivity of the active material.

[0126] (Lithium salts) From the viewpoint of improving battery performance, the electrode material preferably contains a lithium salt. The lithium salt is not limited, and any known lithium salt can be used.

[0127] As the lithium salt, the lithium salts described in paragraphs 0082 to 0085 of JP-A No. 2015-088486 are preferred.

[0128] The electrode material may contain a single type of lithium salt, or may contain two or more types of lithium salts.

[0129] When the electrode material contains a lithium salt, the content of the lithium salt is preferably 0.1% by mass to 10% by mass with respect to the total solid mass of the electrode material.

[0130] (Dispersant) The electrode material preferably contains a dispersant, which can suppress aggregation when the concentration of either the electrode active material or the inorganic solid electrolyte is high.

[0131] The dispersant is not limited, and any known dispersant can be used. As the dispersant, a compound consisting of a low molecular weight or oligomer having a molecular weight of 200 or more and less than 3,000, and having a functional group shown in the following functional group group (I) and an alkyl group having 8 or more carbon atoms or an aryl group having 10 or more carbon atoms in the same molecule is preferable.

[0132] The functional group group (I) is at least one functional group selected from the group consisting of an acidic group, a group having a basic nitrogen atom, a (meth)acryloyl group, a (meth)acrylamide group, an alkoxysilyl group, an epoxy group, an oxetanyl group, an isocyanate group, a cyano group, a sulfanyl group, and a hydroxy group, preferably at least one functional group selected from the group consisting of an acidic group, a group having a basic nitrogen atom, an alkoxysilyl group, a cyano group, a sulfanyl group, and a hydroxy group, more preferably at least one functional group selected from the group consisting of a carboxy group, a sulfonic acid group, a cyano group, an amino group, and a hydroxy group.

[0133] The electrode material may contain a single dispersant, or may contain two or more dispersants.

[0134] When the electrode material contains a dispersant, the content of the dispersant is preferably 0.2 mass % to 10 mass %, and more preferably 0.5 mass % to 5 mass %, relative to the total solid mass of the electrode material, from the viewpoint of preventing aggregation and achieving good battery performance.

[0135] (liquid component) The electrode material may contain a liquid component, such as an electrolyte.

[0136] The electrolyte is not limited and may be any known electrolyte, for example, an electrolyte containing a lithium salt compound and a carbonate compound.

[0137] An example of the lithium salt compound is lithium hexafluorophosphate. The electrolyte may contain one type of lithium salt compound alone, or may contain two or more types of lithium salt compounds.

[0138] Examples of carbonate compounds include ethyl methyl carbonate, ethylene carbonate, and propylene carbonate. The electrolyte may contain one type of carbonate compound alone, or may contain two or more types of carbonate compounds.

[0139] The content of the electrolyte in the electrode material is preferably 30% by mass or less, more preferably 20% by mass or less, and particularly preferably 15% by mass or less, based on the total mass of the electrode material. By making the content of the electrolyte in the electrode material 30% by mass or less, it is possible to suppress the electrolyte from seeping out when the electrode material is molded.

[0140] From the viewpoint of improving battery performance, the content of the electrolyte in the electrode material is preferably 0.01 mass % or more, and more preferably 0.1 mass % or more, based on the total mass of the electrode material.

[0141] The electrode material may contain, as a liquid component, a solvent (hereinafter, simply referred to as "solvent") other than the solvent contained as a component of the electrolyte solution. Examples of the solvent include alcohol compound solvents, ether compound solvents, amide compound solvents, amino compound solvents, ketone compound solvents, aromatic compound solvents, aliphatic compound solvents, and nitrile compound solvents.

[0142] Examples of alcohol compound solvents include methyl alcohol, ethyl alcohol, 1-propyl alcohol, 2-propyl alcohol, 2-butanol, ethylene glycol, propylene glycol, glycerin, 1,6-hexanediol, cyclohexanediol, sorbitol, xylitol, 2-methyl-2,4-pentanediol, 1,3-butanediol, and 1,4-butanediol.

[0143] Examples of ether compound solvents include alkylene glycol alkyl ethers (e.g., ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol, dipropylene glycol, propylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol, polyethylene glycol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, diethylene glycol monobutyl ether, and diethylene glycol monobutyl ether), dimethyl ether, diethyl ether, diisopropyl ether, dibutyl ether, tetrahydrofuran, and dioxane.

[0144] Examples of amide compound solvents include N,N-dimethylformamide, 1-methyl-2-pyrrolidone, 2-pyrrolidinone, 1,3-dimethyl-2-imidazolidinone, 2-pyrrolidinone, ε-caprolactam, formamide, N-methylformamide, acetamide, N-methylacetamide, N,N-dimethylacetamide, N-methylpropanamide, and hexamethylphosphoric triamide.

[0145] Amino compound solvents include, for example, triethylamine, diisopropylethylamine, and tributylamine.

[0146] Examples of ketone compound solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone.

[0147] Aromatic solvents include, for example, benzene, toluene, and xylene.

[0148] Aliphatic solvents include, for example, hexane, heptane, octane, and decane.

[0149] Nitrile compound solvents include, for example, acetonitrile, propylonitrile, and isobutyronitrile.

[0150] The solvent is preferably at least one solvent selected from the group consisting of nitrile compound solvents, aromatic compound solvents, and aliphatic compound solvents, more preferably at least one solvent selected from the group consisting of isobutyronitrile, toluene, and heptane, and particularly preferably at least one solvent selected from the group consisting of toluene and heptane.

[0151] The boiling point of the solvent at normal pressure (i.e., 1 atm) is preferably 50° C. or higher, and more preferably 70° C. or higher. The boiling point of the solvent is preferably 250° C. or lower, and more preferably 220° C. or lower.

[0152] The electrode material may contain a single solvent or may contain two or more solvents.

[0153] The content of the solvent (including the solvent contained as a component of the electrolyte; the same applies hereinafter in this paragraph) in the electrode material is preferably 30 mass% or less, more preferably 20 mass% or less, and particularly preferably 15 mass% or less, based on the total mass of the electrode material. By making the content of the solvent in the electrode material 30 mass% or less, deterioration of the battery performance can be suppressed, and also, the exudation of the solvent when the electrode material is molded can be suppressed. There is no lower limit for the content of the solvent in the electrode material. The content of the solvent in the electrode material may be 0 mass% or more, or may exceed 0 mass%.

[0154] The content of the liquid component in the electrode material is preferably 30% by mass or less, more preferably 20% by mass or less, and particularly preferably 15% by mass or less, based on the total mass of the electrode material. By making the content of the liquid component in the electrode material 30% by mass or less, it is possible to suppress the liquid component from seeping out when the electrode material is molded. In addition, when the liquid component contains a solvent, it is possible to suppress deterioration of the battery performance. There is no lower limit for the content of the liquid component in the electrode material. The content of the liquid component in the electrode material may be 0% by mass or more, or may exceed 0% by mass.

[0155] In addition to the above, the following materials can also be used as the electrode material. (1) The granule described in paragraphs 0029 to 0037 of JP2017-104784A. (2) The positive electrode mixture paint described in paragraph 0054 of JP2016-059870A. (3) Composite particles described in paragraphs 0017 to 0070 of JP2016-027573A. (4) Composite particles described in paragraphs 0020 to 0033 of Japanese Patent No. 6402200. (5) The electrode composition described in paragraphs 0040 to 0065 of JP2019-046765A. (6) Materials described in paragraphs 0080 to 0114 of JP2017-054703A (for example, active materials, positive electrode slurries, and negative electrode slurries). (7) The powder described in JP 2014-198293 A. (8) The active material, binder, and composite particles described in paragraphs 0024 to 0025, 0028, and 0030 to 0032 of JP2016-062654A.

[0156] (Method of preparing electrode material) The electrode material can be prepared, for example, by mixing the electrode active material and, if necessary, the above-mentioned components other than the electrode active material. Examples of the mixing method include a method using a ball mill, a bead mill, a planetary mixer, a blade mixer, a roll mill, a kneader, or a disk mill.

[0157] <<Supply process>> The method for producing an electrode molded body according to the present disclosure includes a step of supplying an electrode material to a mold having a frame-shaped side wall portion defining a space portion for accommodating an electrode material and having a first support disposed on a bottom surface of the mold (supply step). The electrode material supplied to the mold is disposed on the first support in the mold.

[0158] An example of the supplying step will be described with reference to the drawings. For example, as shown in Fig. 2(a) to (c), an electrode material 40 is supplied to a forming mold 20 arranged on a conveyor belt 10A. Fig. 3 is a schematic plan view of the forming mold shown in Fig. 2(a).

[0159] FIG. 2(a) shows a mold 20 disposed on a conveyor belt 10A.

[0160] The conveyor belt 10A is capable of conveying the forming mold 20. The surface of the conveyor belt 10A also functions as the bottom surface of the forming mold 20.

[0161] Although not shown in FIG. 2(a), the transport belt 10A is disposed as a belt of a belt conveyor in a loop shape along the outer periphery of a head pulley and a tail pulley disposed at both ends of the belt conveyor.

[0162] The forming die 20 is a die for forming the electrode material. As shown in Fig. 3, the forming die 20 is arranged in a belt shape (i.e., a band shape) in the longitudinal direction of the conveyor belt 10A. The arrow shown in Fig. 3 indicates the conveying direction. The arrow shown in Fig. 3 is parallel to the longitudinal direction of the conveyor belt 10A.

[0163] The forming die 20 is fixed to the conveyor belt 10A by suction. The forming die 20 may be fixed to the conveyor belt 10A by using an adhesive.

[0164] The mold 20 has a frame-shaped side wall 20A that defines a space (recess) for accommodating the electrode material. The space of the mold is defined by the side wall 20A of the mold 20 and the conveyor belt 10A.

[0165] 3, a plurality of spaces are provided in the molding die 20. The number of spaces in the molding die 20 may be one.

[0166] 2(b) shows the first support 30 disposed on the bottom surface of the molding die 20. The first support 30 may be disposed on the molding die 20 at least before the electrode material 40 is supplied to the molding die 20.

[0167] 2(c) shows the electrode material 40 supplied to the molding die 20. The electrode material 40 supplied to the molding die 20 is placed on the first support 30.

[0168] The supplying step may be carried out through the steps shown in Figures 4(a) to (c), which show the same steps as those shown in Figures 2(a) to (c), except that instead of the molding die 20, a molding die 21 having a frame-shaped side wall portion 21A and a bottom portion 21B is used.

[0169] The supplying step will be specifically described below.

[0170] [Mold] The molding die is a die for molding the electrode material, and has a frame-shaped side wall portion that defines a space capable of accommodating the electrode material (see, for example, FIG. 2(a)).

[0171] In the present disclosure, the term "frame-like" refers to a state in which an inner wall surface is disposed along the periphery of a space when the casting mold is viewed from above (see, for example, FIG. 3).

[0172] The shape of the space (referring to the internal shape of the mold; the same applies below) is not limited and may be determined according to the desired shape of the electrode molded body. For example, when the electrode material is molded into a flat plate, the shape of the space is preferably flat.

[0173] Examples of the shape of the space when viewed in a plane include a rectangular shape and a circular shape. For example, when the electrode material is molded into a rectangular shape, the shape of the space when viewed in a plane is preferably a rectangular shape.

[0174] The width of the space when viewed from above is not limited and may be determined according to the width of the intended electrode molded article. The width of the space when viewed from above may be appropriately determined within the range of, for example, 50 mm to 2,000 mm.

[0175] The length of the space when viewed from above is not limited and may be determined according to the length of the intended electrode molded article. The length of the space when viewed from above may be appropriately determined within the range of, for example, 100 mm to 2,000 mm.

[0176] The height of the space is not limited and may be determined according to the desired height (i.e., thickness) of the electrode molded article. The height of the space may be appropriately determined, for example, within a range of more than 0 mm and 5 mm or less.

[0177] The mold may have one space, or may have two or more spaces (see, for example, FIG. 3).

[0178] The frame-shaped side wall portion can function as a physical constraint to suppress uneven distribution of the electrode material supplied to the mold. For example, the frame-shaped side wall portion can restrict the movement of the electrode material that causes uneven density distribution of the electrode molded body. By using a mold having a frame-shaped side wall portion, an electrode molded body with excellent moldability can be obtained.

[0179] Examples of materials for the sidewall include resin and metal.

[0180] Metals include, for example, stainless steel, copper, and aluminum.

[0181] Examples of the resin include fluororesin, silicone resin, polypropylene, polyethylene terephthalate, and polyethylene.

[0182] The material of the side wall is preferably a resin from the viewpoint of improving moldability. The material of the side wall is preferably a fluororesin or a silicon resin from the viewpoints of improving the releasability of the electrode material, preventing contamination of the mold, and improving the durability of the mold, more preferably polytetrafluoroethylene (PTFE) or a tetrafluoroethylene-ethylene copolymer (ETFE), and particularly preferably polytetrafluoroethylene.

[0183] The inner peripheral shape of the side wall portion when viewed in a plan view is not limited as long as it is frame-shaped, and may be determined according to the shape of the target electrode molded body. Examples of the inner peripheral shape of the side wall portion when viewed in a plan view include a rectangular shape and a circular shape. For example, when the electrode material is molded into a rectangular shape, the inner peripheral shape of the side wall portion when viewed in a plan view is preferably a rectangular shape. In other words, the side wall portion preferably has four inner wall surfaces in which adjacent surfaces intersect each other at right angles.

[0184] The structure of the side wall portion may be separable or inseparable (e.g., an integrated structure) as long as it can define a space capable of containing an electrode material. In addition, the side wall portion may be made of a single member or may be made of multiple members.

[0185] The mold may have only a side wall, or may have a bottom in addition to the side wall. Specifically, the mold may have a bottom and a frame-shaped side wall that define a space capable of accommodating an electrode material (see, for example, FIG. 4(a)).

[0186] When the mold has a bottom, the sidewall is preferably disposed in contact with the bottom, and more preferably in contact with the bottom and in a direction perpendicular to the bottom.

[0187] When the mold has a bottom, the bottom may be a part that can be separated from the side wall, or it may be a part that cannot be separated from the side wall (e.g., a part that is integrated with the side wall), as long as it can define a space that can accommodate the electrode material.

[0188] Examples of the material of the bottom include the resin and metal used as the material of the sidewall. The preferred material of the bottom is the same as the preferred material of the sidewall. The material of the bottom is preferably the same as the material of the sidewall.

[0189] The shape of the bottom is not limited and may be determined according to the shape of the intended electrode molded article. For example, when the electrode material is molded into a flat plate, the bottom is preferably flat.

[0190] The thickness of the mold is not limited and may be appropriately determined within the range of, for example, 0 mm to 5 mm. From the viewpoint of moldability and performance depending on the thickness of the product, the thickness of the mold is preferably within the range of 0.01 mm to 2 mm, more preferably within the range of 0.1 mm to 1 mm, and particularly preferably within the range of 0.2 mm to 1.0 mm.

[0191] The mold is preferably in the form of a belt (i.e., band) (see, for example, FIG. 3). The mold is in the form of a belt, which can improve productivity. The belt-shaped mold preferably has two or more spaces. When the belt-shaped mold has two or more spaces, it is preferable that a recess is disposed between each space. By disposing a recess between each space, excess electrode material can be collected, which can prevent contamination due to scattering of the electrode material.

[0192] The method for producing the mold is not limited, and a known method can be used. Examples of the method for producing the mold include casting and injection molding. The mold can also be obtained by removing a portion corresponding to the space from the base material of the mold. The mold can also be obtained by joining and combining a plurality of members together.

[0193] [First support] The first support is disposed on the bottom surface of the mold. By using the first support, moldability can be improved, and further, the electrode material can be easily removed from the mold in the removal step.

[0194] In the present disclosure, the "bottom surface of the mold" means the surface of a member capable of defining the bottom surface of the space in the mold. The bottom surface of the mold may be the surface of a member independent of the mold (specifically, the side wall portion) as long as the space can be defined in the mold, or may be the surface of a part of the mold (e.g., the bottom portion). That is, in an embodiment of the present disclosure, as long as the space can be defined in the mold, the surface of a member independent of the mold is regarded as the bottom surface of the mold. For example, as shown in FIG. 2(a), the surface of the conveyor belt 10A, which is a member independent of the mold 20, is regarded as the bottom surface of the mold 20. Also, for example, as shown in FIG. 4(a), the surface of the bottom portion 21B, which is a part of the mold 21, is the bottom surface of the mold 21.

[0195] The first support may be, for example, a release material. Examples of the release material include release paper, surface-treated metals (e.g., aluminum and stainless steel (commonly referred to as "SUS"), films having a coating layer, and papers having a coating layer. The coating layer may be formed by, for example, a silicone coating or a fluorine coating.

[0196] From the viewpoint of improving the releasability of the electrode material, the first support is preferably a release material, and more preferably release paper.

[0197] The first support preferably has a flat plate shape from the viewpoint of its ability to conform to the bottom surface of the mold and the shape of the electrode material.

[0198] From the viewpoint of shape conformability, the average thickness of the first support is preferably 5 μm or more, more preferably 10 μm or more, and particularly preferably 20 μm or more. From the viewpoint of flexibility and light weight, the average thickness of the first support is preferably 500 μm or less, more preferably 300 μm or less, and particularly preferably 200 μm or less. The average thickness of the first support is the arithmetic average of the thicknesses measured at three points by cross-sectional observation. A known microscope (e.g., a scanning electron microscope) can be used for cross-sectional observation.

[0199] The size of the first support is not limited and may be determined according to the size of the bottom surface of the mold. The size of the first support in plan view is preferably smaller than the size of the bottom surface of the mold. When the size of the first support is smaller than the size of the bottom surface of the mold, the electrode material can be easily removed from the mold in the removal step. From the same viewpoint, the ratio of the area of ​​the first support to the area of ​​the bottom surface of the mold in plan view is preferably 99.9% to 90%, more preferably 99.8% to 95%, and particularly preferably 99.5% to 97%.

[0200] [Supply method] The method for supplying the electrode material to the mold is not limited, and any known method can be used. For example, a method using a supplying device can be used as the method for supplying the electrode material to the mold.

[0201] Feeding devices include, for example, screw feeders, disk feeders, rotary feeders, and belt feeders.

[0202] As a method for supplying the electrode material to the mold, a method of supplying the electrode material to the mold by discharging the electrode material from a discharge port can be mentioned. When a supplying device is used, the electrode material may be discharged from the discharge port by using the supplying device.

[0203] In the supply step, the discharge port preferably has an opening / closing mechanism for controlling the supply of the electrode material from the viewpoint of preventing contamination due to scattering of the electrode material. Here, the "opening / closing mechanism" means a movable mechanism that can open and close the flow path of the electrode material. Examples of the valve body used in the opening / closing mechanism include a plate-shaped valve body and a spherical valve body.

[0204] When the electrode material is supplied using a supply device, it is also preferable that the opening and closing mechanism is disposed in a flow path from the supply device to the discharge port.

[0205] In the supplying step, it is preferable to supply the electrode material to the mold while moving the discharge port and the mold relatively. By supplying the electrode material by the above method, the dispersibility of the electrode material in the mold can be improved, so that an electrode molded body having excellent moldability can be obtained.

[0206] In the present disclosure, "moving the discharge port and the mold relatively" includes moving the discharge port relative to the mold, moving the mold relative to the discharge port, and moving each of the discharge port and the mold. When moving each of the discharge port and the mold, for example, the discharge port and the mold may be moved in a direction away from each other along the same directional axis. When moving each of the discharge port and the mold, the discharge port and the mold may be moved in a direction perpendicular to each other. For example, it is possible to combine moving the discharge port in the width direction of the mold (for example, TD: Transverse Direction) and moving the mold in a direction perpendicular to the width direction of the mold (for example, MD: Machine Direction).

[0207] In the supplying step, it is preferable to move the casting mold relative to the discharge port in order to improve productivity.

[0208] When the mold is moved in the supplying step, the means for transporting the mold is not limited and any known transport means can be used. Examples of the means for transporting the mold include a belt conveyor, a linear motion guide, and a cross roller table.

[0209] From the viewpoint of stability, the supply amount of the electrode material is preferably 0.01 kg / min to 100 kg / min, more preferably 0.1 kg / min to 10 kg / min, and particularly preferably 0.5 kg / min to 5 kg / min.

[0210] <<Forming process>> The method for producing an electrode molded body according to the present disclosure includes a step of molding an electrode material along the internal shape of a mold (hereinafter, also referred to as a "molding step"). By including the molding step in the method for producing an electrode molded body according to the present disclosure, the density distribution of the electrode material can be made uniform, so that an electrode molded body with excellent moldability can be obtained.

[0211] An example of the molding process will be described with reference to the drawings. For example, as shown in FIG. 2(d), the electrode material 40 can be molded along the internal shape of the mold 20 by applying pressure to the electrode material 40 via the second support 50.

[0212] 2(d), for example, a roll (not shown) serving as a molding member is brought into contact with the second support 50, so that the electrode material 40 can be pressed via the second support 50. The electrode material 40 may be directly pressed without using the second support 50.

[0213] FIG. 4( d ) shows the same process as FIG. 2( d ), except that a mold 21 is used instead of the mold 20 .

[0214] The molding process will be specifically described below.

[0215] In the present disclosure, "molding the electrode material to conform to the internal shape of the mold" means shaping the electrode material into a shape that corresponds to the inner surface of the mold, in other words, the shape of the space in the mold.

[0216] The method of forming the electrode material is not limited as long as it can form the electrode material along the internal shape of the mold, and a known method can be used. For example, the method of forming the electrode material includes a method of applying an external force to the electrode material in the mold. By applying an external force to the electrode material in the mold, the electrode material can be formed along the internal shape of the mold.

[0217] Specific examples of the method for shaping the electrode material include a method of applying pressure in the depth direction of the electrode material, a method of vibrating the electrode material, and a method of flattening the surface of the electrode material.

[0218] In the molding step, it is preferable to mold the electrode material by directly or indirectly contacting the electrode material with the molded member. Here, "indirectly contacting the electrode material with the molded member" means that the electrode material and the molded member are contacted via another member (e.g., a second support described later) disposed between the electrode material and the molded member.

[0219] The molding member is a member for molding the electrode material. The molding member is not limited as long as it can mold the electrode material along the internal shape of the mold. The molding member may be, for example, a part of a device, or may be a single-use item. The molding member is preferably a member having a surface that contacts the electrode material. Here, in the case where the electrode material and the molding member are indirectly contacted, the "surface that contacts the electrode material" means a surface that contacts another member disposed between the electrode material and the molding member. Examples of the molding member include a roll, a press, a scraper, and a plate-like member (for example, a squeegee). Among the above, the molding member is preferably a roll from the viewpoint of continuity.

[0220] The molding member preferably has a vibration means. By having the molding member have the vibration means, moldability can be improved. As the vibration means, for example, a general vibration device can be mentioned.

[0221] The surface of the molded member preferably has an uneven shape, which can improve moldability.

[0222] The molding member may be used alone or in combination of two or more kinds.

[0223] When the electrode material is molded using a molding member, the molding member may be in contact with only the electrode material, or may be in contact with both the electrode material and the mold.

[0224] When the electrode material is molded using a molding member, the electrode material may be pressed using the molding member, or the molding member may be moved along the surface of the electrode material while the electrode material and the molding member are in contact with each other. The electrode material may be moved while the electrode material and the molding member are in contact with each other.

[0225] When the electrode material is pressed using a molding member, the pressure is preferably from 1 MPa to 1 GPa, more preferably from 5 MPa to 500 MPa, and particularly preferably from 10 MPa to 300 MPa.

[0226] When the electrode material is molded using a molding member, it is preferable to mold the electrode material by moving the molding member and the mold relatively while directly or indirectly contacting the electrode material and the molding member. By molding the electrode material by the above method, an electrode molded body having excellent moldability can be obtained, and productivity can be improved. When the electrode material is molded by the above method, it is also preferable to pressure mold the electrode material.

[0227] In the present disclosure, "moving the molding member and the mold relatively" includes moving the molding member relative to the mold, moving the mold relative to the molding member, and moving each of the molding member and the mold. From the viewpoint of improving productivity, it is preferable to move the mold relative to the molding member. When moving each of the molding member and the mold, it is preferable to move each of the molding member and the mold in a direction away from each other along the same directional axis.

[0228] The molding step may be performed while the supplying step is being performed. That is, in the method for producing an electrode molded body according to the present disclosure, the electrode material may be molded along the internal shape of the mold while being supplied to the mold.

[0229] <<Coating process>> The method for producing an electrode molded article according to the present disclosure preferably includes a step of placing a second support on the electrode material supplied to the mold (hereinafter, also referred to as a "coating step"). By including the coating step in the method for producing an electrode molded article according to the present disclosure, moldability can be improved and contamination due to scattering of the electrode material can also be prevented.

[0230] An example of the coating step will be described with reference to the drawings. For example, in Fig. 1, the coating step may be performed between S120 and S130, between S130 and S140, or simultaneously with S130.

[0231] For example, as shown in FIG. 2(d), a second support 50 can be placed on the electrode material 40 supplied to the mold 20.

[0232] FIG. 4( d ) shows the same process as FIG. 2( d ), except that a mold 21 is used instead of the mold 20 .

[0233] The coating step will be specifically described below.

[0234] From the viewpoints of improving moldability and preventing contamination due to scattering of the electrode material, the method for producing an electrode molded body according to the present disclosure preferably includes a step (covering step) of placing a second support on the electrode material supplied to the mold between the step of supplying the electrode material (supplying step) and the step of molding the electrode material (molding step).

[0235] From the viewpoints of improving moldability and preventing contamination due to scattering of the electrode material, the method for producing an electrode molded body according to the present disclosure also preferably includes a step (covering step) of placing a second support on the electrode material supplied to the mold between the step of molding the electrode material (molding step) and the step of removing the electrode material (removal step).

[0236] The method for producing an electrode molded body according to the present disclosure includes a step of placing a second support on the electrode material supplied to the mold (covering step) from the viewpoints of improving moldability, preventing contamination due to scattering of the electrode material, and improving productivity, and it is also preferable to simultaneously carry out the step of placing the second support (covering step) and the step of molding the electrode material (molding step). Here, "simultaneously carrying out the covering step and the molding step" means that the electrode material is molded along the internal shape of the mold while the second support is placed on the electrode material supplied to the mold. In the above method, the electrode material can be molded via the second support.

[0237] Examples of materials for the second support include resin, metal, and paper.

[0238] The second support is preferably a current collector, which allows the electrode material to be easily disposed on the current collector and also improves productivity.

[0239] The current collector is not limited, and any known current collector can be used.

[0240] Examples of the positive electrode current collector include aluminum, aluminum alloy, stainless steel, nickel, and titanium. The positive electrode current collector is preferably aluminum or an aluminum alloy. It is also preferable that the positive electrode current collector is aluminum or stainless steel having a coating layer containing carbon, nickel, titanium, or silver on the surface.

[0241] Examples of the negative electrode current collector include aluminum, copper, a copper alloy, stainless steel, nickel, and titanium. The negative electrode current collector is preferably aluminum, copper, a copper alloy, or stainless steel, and more preferably copper or a copper alloy. The negative electrode current collector is also preferably aluminum, copper, a copper alloy, or stainless steel having a coating layer containing carbon, nickel, titanium, or silver on the surface.

[0242] The current collector is preferably an aluminum foil or a copper foil. An aluminum foil is usually used as a current collector for a positive electrode. A copper foil is usually used as a current collector for a negative electrode.

[0243] The second support may be meshed or punched. The second support may be a porous body, a foam, or a molded body of fibers. The surface of the second support may have irregularities due to a surface treatment.

[0244] The second support preferably has a flat plate shape.

[0245] From the viewpoints of self-supporting property, transportability, and penetration resistance, the average thickness of the second support is preferably 1 μm to 500 μm, more preferably 3 μm to 300 μm, and particularly preferably 5 μm to 200 μm. The average thickness of the second support is the arithmetic average of the thicknesses measured at three points by cross-sectional observation. A known microscope (e.g., a scanning electron microscope) can be used for cross-sectional observation.

[0246] <<Displacement process>> The method for producing an electrode molded body according to the present disclosure preferably includes a step of changing the positional relationship between the first support and the electrode material (hereinafter, also referred to as a "displacement step"). By including the displacement step in the method for producing an electrode molded body according to the present disclosure, the electrode material can be disposed at a position where it can be easily removed from the mold.

[0247] An example of the displacement step will be described with reference to the drawings. For example, in Fig. 1, the displacement step is preferably performed between S130 and S140.

[0248] 2(e), the positional relationship between the first support 30 and the electrode material 40 can be changed by inverting the first support 30 and the electrode material 40 upside down. For example, the first support 30 and the electrode material 40 can be inverted upside down by inverting the conveying direction of the conveyor belt 10 by 180 degrees in a U-shape at the end of the belt conveyor (not shown).

[0249] FIG. 4( e ) shows the same process as FIG. 2( e ), except that a mold 21 is used instead of the mold 20 .

[0250] The displacement step will now be described in detail.

[0251] In the present disclosure, "changing the positional relationship between the first support and the electrode material" means changing the positional relationship between the first support and the electrode material in an arbitrary coordinate system (for example, a three-dimensional orthogonal coordinate system).

[0252] From the viewpoint of improving formability and improving the releasability of the electrode material, the method for producing an electrode molded body according to the present disclosure preferably includes a displacement step between the step of molding the electrode material (molding step) and the step of removing the electrode material (removal step).

[0253] When the manufacturing method of the electrode molded body according to the present disclosure includes a coating step, it is preferable that the manufacturing method of the electrode molded body according to the present disclosure includes a displacement step between the coating step and the removal step, from the viewpoints of improving moldability and improving releasability of the electrode material.

[0254] In the displacement step, it is preferable to arrange the electrode material vertically below the first support by changing the positional relationship between the first support and the electrode material. By arranging the electrode material vertically below the first support, the electrode material can be easily removed from the mold in the removal step.

[0255] In the present disclosure, "the electrode material is disposed below the first support in the vertical direction" means that the electrode material is disposed below the lower surface of the first support in a cross-sectional view perpendicular to a horizontal plane, in other words, the first support and the electrode material are disposed at a position where a virtual line extending in the vertical direction (i.e., the direction of gravity) is drawn with respect to the first support and the electrode material, and the virtual line extends in the vertical direction and passes through the first support and the electrode material in this order. For example, when the downward direction in FIG. 2(e) is the vertical direction, the electrode material 40 is disposed below the first support in the vertical direction. In FIG. 2(e), for example, even when the first support 30 and the electrode material 40 are rotated within a range of 1 degree to 89 degrees, it can be said that the electrode material 40 is disposed below the first support in the vertical direction.

[0256] The method for changing the positional relationship between the first support and the electrode material is not limited, and any known method can be used. When the mold is disposed on a transport member (e.g., a belt and a roll), the positional relationship between the first support and the electrode material can be changed by changing the transport direction of the transport member. In addition, the positional relationship between the first support and the electrode material can also be changed by rotating the mold.

[0257] <<Pressure process>> The method for producing an electrode molded body according to the present disclosure preferably includes a step of pressurizing the electrode material (hereinafter also referred to as a "pressurizing step"). By including the pressurizing step in the method for producing an electrode molded body according to the present disclosure, the density distribution of the electrode material can be made more uniform, so that an electrode molded body with excellent moldability can be obtained. In addition, the pressurizing step can also serve as a consolidation step, so that the density of the obtained electrode molded body can be increased.

[0258] An example of the pressurizing step will be described with reference to the drawings. For example, in Fig. 1, the pressurizing step may be performed between S130 and S140, or may be performed after S140.

[0259] For example, as shown in FIG. 2(f), the electrode material 40 can be pressed using a conveyor belt 10A and a conveyor belt 10B.

[0260] In FIG. 2(f), the electrode material 40 may be pressed using a pair of rolls (not shown) instead of the conveyor belt 10A and the conveyor belt 10B, or the electrode material 40 may be pressed using a roll (not shown) instead of the conveyor belt 10B.

[0261] FIG. 4( f ) shows the same process as FIG. 2( f ), except that a mold 21 is used instead of the mold 20 .

[0262] The pressurizing step will be specifically described below.

[0263] The pressurizing step may be performed before or after the removal step. The method for producing an electrode molded body according to the present disclosure preferably includes a pressurizing step between the molding step and the removal step, or after the removal step.

[0264] When the method for producing an electrode molded article according to the present disclosure includes a covering step, the method for producing an electrode molded article according to the present disclosure preferably includes a pressurizing step between the covering step and the removal step.

[0265] The method for applying pressure to the electrode material is not limited, and any known method can be used. For example, a method using a pressure member can be used as the method for applying pressure to the electrode material.

[0266] Pressure members include, for example, rolls, belts, and presses.

[0267] The pressure applying member may be used alone or in combination of two or more. In the pressure applying step, for example, a pair of rolls may be used, a combination of a roll and a belt may be used, or two belts may be used.

[0268] In the pressing step, it is preferable to pressurize the electrode material stepwise using a plurality of rolls. By pressing the electrode material stepwise using a plurality of rolls, the density distribution of the electrode material can be made more uniform, so that an electrode molded body having excellent formability can be obtained. For example, the electrode material can be pressed stepwise by using a plurality of rolls in which the gap between the rolls is adjusted to be narrower stepwise.

[0269] The pressure is preferably from 1 MPa to 1 GPa, more preferably from 5 MPa to 500 MPa, and particularly preferably from 10 MPa to 300 MPa.

[0270] In the pressing step, from the viewpoint of improving formability, it is preferable to pressurize the electrode material under heated conditions.

[0271] <<Removal process>> The method for producing an electrode molded article according to the present disclosure includes a step of removing the electrode material from the mold (hereinafter also referred to as the "removal step").

[0272] An example of the removal step will be described with reference to the drawings. For example, as shown in Fig. 2(g), an electrode molded body 60 can be obtained by removing the electrode material from the molding die 20.

[0273] As shown in FIG. 2(g), a conveyor belt 10B can be used as a member for receiving the electrode material taken out from the forming mold 20 (a receiving member to be described later).

[0274] For example, in Fig. 2(f), the electrode material 40 may be pressed from the direction of the conveyor belt 10A. In Fig. 2(f), the electrode material may be attracted toward the conveyor belt 10B. By each of the above-mentioned methods, the conveyor belt 10A and the first support 30 can be easily separated from each other, and therefore the electrode material can be easily removed from the molding die.

[0275] FIG. 4( g ) shows a similar process to that of FIG. 2( g ), except that the electrode material is removed from a mold 21 instead of from mold 20 .

[0276] The removal step will now be described in detail.

[0277] In the present disclosure, "removing the electrode material from the mold" means obtaining the electrode material by separating the mold from the electrode material, and is not limited to removing the electrode material contained in the mold to the outside of the mold. For example, in the removal step, the electrode material may be separated from the mold, or the mold may be separated from the electrode material. There is no limitation on the method for removing the electrode material from the mold, and a known method can be used. Examples of the method for removing the electrode material from the mold include a method that utilizes the electrode material's own weight, a method that pushes out the electrode material, and a method that uses a tool (e.g., a spatula). The electrode material may also be removed from the mold by disassembling the mold.

[0278] An example of a method for extruding the electrode material is a method in which air is pumped into a molding die to extrude the electrode material.

[0279] In the removal step, it is preferable to remove the electrode material from the mold in a direction in which the electrode material is arranged with reference to the first support. The above method allows the electrode material to be easily removed. Here, "removing the electrode material from the mold in a direction in which the electrode material is arranged with reference to the first support" is not limited to removing only the electrode material, but also includes removing the electrode material and the second support when a second support is used in the manufacturing method of an electrode molded body according to the present disclosure.

[0280] In the removal step, it is preferable to remove the electrode material and the first support from the mold. By removing the electrode material and the first support from the mold, the releasability of the electrode material can be improved, and further, the surface of the electrode material can be protected in the process of removing the electrode material, so that an electrode molded body having excellent moldability can be obtained. When a second support is used in the manufacturing method for an electrode molded body according to the present disclosure, it is preferable to remove the electrode material, the first support, and the second support from the mold.

[0281] When the electrode material and the first support are removed from the mold, the first support after the removal step may be used as a protector when cutting the second support, or as a so-called interleaf paper. Furthermore, after the removal step, the first support may be peeled off as appropriate.

[0282] In the removal step, it is preferable to remove the electrode material from the mold and place the electrode material on a receiving member. By placing the electrode material on the receiving member, scattering of the electrode material can be prevented, and an electrode molded body with excellent moldability can be obtained. Here, "placing the electrode material on the receiving member" is not limited to placing the electrode material in contact with the receiving member, and includes placing the second support and the electrode material on the receiving member in this order when a second support is used in the manufacturing method of an electrode molded body according to the present disclosure.

[0283] The receiving member is not limited as long as it can accommodate the electrode material taken out from the mold. Examples of the receiving member include a resin film, a metal foil, and a metal plate. Also, as shown in FIG. 2(g) and FIG. 4(g), a conveying member can be used as the receiving member.

[0284] In the removal step, it is also preferable to remove the electrode material from the mold by sucking or adsorbing the electrode material (meaning the second support when a second support is used) onto the receiving member. The above method allows the electrode material to be easily removed from the mold. Here, "sucking or adsorbing the electrode material onto the receiving member" is not limited to directly sucking or adsorbing the electrode material onto the receiving member, and includes indirectly sucking or adsorbing the electrode material onto the receiving member via the second support when a second support is used in the manufacturing method for an electrode molded body according to the present disclosure.

[0285] In the removal step, it is preferable to remove the electrode material from the mold by pushing out the electrode material in a direction in which the electrode material is to be disposed relative to the first support, or by sucking or adsorbing the electrode material to a receiving member, and it is more preferable to remove the electrode material from the mold by pushing out the electrode material in a direction in which the electrode material is to be disposed relative to the first support, and by sucking or adsorbing the electrode material to a receiving member.

[0286] <<Transportation method>> In the method for producing an electrode molded body according to the present disclosure, the method for transporting the mold may be, for example, a method using a transport member. For example, by placing the mold on the transport member, the above steps can be carried out while the mold is being transported.

[0287] In the manufacturing method of the electrode molded body according to the present disclosure, the mold is preferably arranged on a conveying member. By carrying out each of the above steps using the mold arranged on the conveying member, productivity can be improved. When using the mold arranged on the conveying member, for example, by carrying out each of the above steps along the conveying direction, the electrode molded body can be obtained.

[0288] The transport member may be, for example, a belt or a roll.

[0289] The transport member may be used alone or in combination of two or more kinds.

[0290] <<Molded body for electrode>> The electrode molded article obtained by the method for producing an electrode molded article according to the present disclosure has excellent moldability and can be used as various electrodes. The electrode molded article is preferably an electrode molded article for an all-solid-state secondary battery.

[0291] The shape of the electrode molded article is not limited and may be appropriately determined depending on the application. The shape of the electrode molded article is preferably a flat plate shape.

[0292] From the viewpoint of improving battery performance (e.g., discharge capacity and output characteristics), the average thickness of the electrode molded body is preferably 0.01 mm to 2 mm, more preferably 0.05 mm to 1.5 mm, and particularly preferably 0.1 mm to 1 mm. The average thickness of the electrode molded body is the arithmetic mean of the thicknesses measured at three points by cross-sectional observation. A known microscope (e.g., a scanning electron microscope) can be used for cross-sectional observation. EXAMPLES

[0293] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited to these examples.

[0294] <Preparation of sulfide-based inorganic solid electrolyte (Li-PS-based glass)> The sulfide-based inorganic solid electrolyte was prepared with reference to "T. Ohtomo, A. Hayashi, M. Tatsumisago, Y. Tsuchida, S. Hama, K. Kawamoto, Journal of Power Sources, 233, (2013), pp. 231-235, and A. Hayashi, S. Hama, H. Morimoto, M. Tatsumisago, T. Minami, Chem. Lett., (2001), pp. 872-873".

[0295] Specifically, in a glove box under an argon atmosphere (dew point: -70°C), 2.42 g of lithium sulfide (Li2S, Aldrich, purity: >99.98%) and 3.9 g of diphosphorus pentasulfide (P2S5, Aldrich, purity: >99%) were weighed out, and then the lithium sulfide and diphosphorus pentasulfide were mixed for 5 minutes using an agate mortar. The molar ratio of Li2S to P2S5 (Li2S:P2S5) was 75:25. 66 zirconia beads with a diameter of 5 mm were placed in a 45 mL zirconia container (manufactured by Fritsch), and then the entire amount of the mixture of lithium sulfide and diphosphorus pentasulfide was placed in, and the container was completely sealed under an argon atmosphere. The container was attached to a Fritsch planetary ball mill P-7 (trade name), and mechanical milling was performed for 20 hours at a temperature of 25°C and a rotation speed of 510 rpm (revolutions per minute), to obtain 6.2 g of a yellow powder sulfide solid electrolyte material (Li-PS-based glass). The above process was repeated 10 times to obtain 62 g of a solid electrolyte material.

[0296] <Example 1> [Preparation of positive electrode material (P-1)] 180 zirconia beads with a diameter of 5 mm were put into a 45 mL zirconia container (manufactured by Fritsch), and then 3.0 g of the Li-PS glass prepared above was put into it. The container was attached to a planetary ball mill P-7 manufactured by Fritsch, and mixed for 2 hours at a temperature of 25°C and a rotation speed of 300 rpm. Next, 6.8 g of LCO (LiCoO2, manufactured by Nippon Chemical Industry Co., Ltd.) as an active material and Li-100 (0.2 g) manufactured by Denka Co., Ltd. as a conductive assistant were put into the container, and then the container was attached to a planetary ball mill P-7, and mixed for 10 minutes at a temperature of 25°C and a rotation speed of 100 rpm to obtain a positive electrode material (P-1). The above process was repeated 10 times to obtain the required amount of positive electrode material.

[0297] [Preparation of negative electrode material (N-1)] 180 zirconia beads with a diameter of 5 mm were put into a 45 mL zirconia container (manufactured by Fritsch), and then 4.0 g of the prepared Li-PS glass was put into it. The container was attached to a planetary ball mill P-7 manufactured by Fritsch, and mixed for 2 hours at a temperature of 25°C and a rotation speed of 300 rpm. Next, 5.0 g of CGB20 (trade name, manufactured by Nippon Graphite Industries Co., Ltd.) as an active material and 1.0 g of the prepared conductive assistant were put into the container, and then the container was attached to a planetary ball mill P-7, and mixed for 15 minutes at a temperature of 25°C and a rotation speed of 200 rpm to obtain a negative electrode material (N-1). The above steps were repeated 10 times to obtain the required amount of negative electrode material.

[0298] [Preparation of positive electrode sheet] The positive electrode material (P-1) was put into the powder receiving port of a screw feeder (AS ONE Corporation powder measuring feeder (screw type), PSF-100SA) (S210 in FIG. 5). Next, release paper (first support) precut to a size of 44.9 mm x 49.9 mm was placed inside a fluororesin frame belt (molding mold, thickness: 1.0 mm, inner dimensions of hollow frame (hereinafter simply referred to as "frame") 45 mm x 50 mm) wound around an adsorbent porous stainless steel belt conveyor. The release paper was adsorbed to the belt conveyor by reduced pressure.

[0299] While the frame belt was being transported using the belt conveyor, a screw feeder was operated to supply the positive electrode material (P-1) to a thickness of 0.6 mm inside the frame of the frame belt (S220 in FIG. 5).

[0300] An aluminum foil (second support, current collector) having a thickness of 20 μm was placed on the frame belt, and then, using a φ90 mm stainless steel roll and a rubber roll made of NBR (nitrile butadiene rubber), the positive electrode material (P-1) was pressed evenly through the aluminum foil, thereby compacting the positive electrode material (P-1) within the frame without any gaps (S230 and S240 in FIG. 5).

[0301] The conveying direction was reversed 180 degrees in a U-shape at the end of the belt conveyor, thereby turning the release paper and the positive electrode material (P-1) upside down (S250 in FIG. 5). During the reversing process, the positive electrode material (P-1) was conveyed while being nipped from the upper surface to the lower surface of the belt conveyor.

[0302] After the inversion, compressed air was blown from the inside of the belt conveyor to push the release paper out of the frame, thereby extruding a flat plate of the positive electrode material (P-1) onto the aluminum foil (S260 in FIG. 5).

[0303] After the excess aluminum foil was cut off with a Thomson blade, the sheet was pressed at 10 MPa for 1 minute to obtain a positive electrode sheet (electrode compact) (S270 in FIG. 5). The layer structure of the positive electrode sheet was positive electrode layer / aluminum foil.

[0304] [Preparation of negative electrode sheet] A negative electrode sheet (electrode molded body) was produced in the same manner as the positive electrode sheet, except that the positive electrode material (P-1) was changed to the negative electrode material (N-1) and the aluminum foil (second support, current collector) was changed to a copper foil (second support, current collector) having a thickness of 20 μm. The layer structure of the negative electrode sheet was negative electrode layer / copper foil.

[0305] [Preparation of solid electrolyte sheet] 180 zirconia beads with a diameter of 5 mm were put into a 45 mL zirconia container (manufactured by Fritsch), and then 1.0 g of the Li-PS glass prepared above and 1.5 g of isobutyronitrile were put into the container. The container was attached to a Fritsch planetary ball mill P-7, and the mixture was stirred at a temperature of 25°C and a rotation speed of 300 rpm for 2 hours to obtain a solid electrolyte composition. The obtained solid electrolyte composition was applied onto an aluminum foil of 20 μm using an applicator, and then dried at 80°C for 1 hour and then at 120°C for 1 hour to obtain a solid electrolyte sheet. The layer structure of the solid electrolyte sheet was solid electrolyte layer / aluminum foil. After the solid electrolyte layer was sufficiently solidified, the aluminum foil was peeled off to extract only the solid electrolyte layer. The thickness of the solid electrolyte layer was 30 μm.

[0306] [Preparation of all-solid-state secondary batteries] The solid electrolyte layer was placed opposite the negative electrode layer of the negative electrode sheet, and pressed at 10 MPa for 1 minute to produce a negative electrode sheet with a solid electrolyte.

[0307] A positive electrode sheet and a negative electrode sheet with a solid electrolyte were placed in a stainless steel case of any size having a spacer and a washer, so that the positive electrode layer of the positive electrode sheet and the solid electrolyte layer of the negative electrode sheet with a solid electrolyte faced each other. Through the above operations, an all-solid-state secondary battery was obtained. The layer structure of the obtained all-solid-state secondary battery was copper foil / negative electrode layer / solid electrolyte layer / positive electrode layer / aluminum foil.

[0308] <Example 2> The electrolyte used was a lithium hexafluorophosphate solution (1.0M LiPF6in EC / EMC=50 / 50 (v / v)) manufactured by Aldrich. "EC" means ethylene carbonate. "EMC" means ethyl methyl carbonate.

[0309] A positive electrode sheet, a negative electrode sheet, a solid electrolyte sheet, and an all-solid-state secondary battery were each produced in the same manner as in Example 1, except that a positive electrode material (P-2) prepared by kneading a positive electrode material (P-1) and an electrolytic solution (amount added: an amount that was 10 mass% relative to the total mass of the positive electrode material (P-2) to be obtained) was used as the positive electrode material, and a negative electrode material (N-2) prepared by kneading a negative electrode material (N-1) and an electrolytic solution (amount added: an amount that was 25 mass% relative to the total mass of the negative electrode material (N-2) to be obtained) was used as the negative electrode material.

[0310] <Comparative Example 1> A positive electrode sheet, a negative electrode sheet, a solid electrolyte sheet, and an all-solid-state secondary battery were produced in the same manner as in Example 1, except that in the production of the positive electrode sheet and the negative electrode sheet, a fluororesin frame belt (molding die) was not used and the end portions were cut off using a Thomson blade.

[0311] <Evaluation> [Electrode layer mass distribution] The mass of the positive electrode sheet (20 sheets) cut into 1 cm squares was measured using an electronic balance to evaluate the mass variation (σ) of the positive electrode layer in the positive electrode sheet. The mass variation (σ) of the negative electrode layer in the negative electrode sheet was evaluated using the same method as above. The evaluation results are shown in Table 1. The smaller the value of the variation (σ), the better the moldability.

[0312] [Table 1]

[0313] In the "Mold" column of Table 1, "-" means that no mold was used.

[0314] From Table 1, it was found that, regarding the mass distribution of the positive electrode layer and the mass distribution of the negative electrode layer, the variations in Examples 1 and 2 were smaller than those in Comparative Example 1. This result shows that the moldability of Examples 1 and 2 is superior to that of Comparative Example 1.

[0315] The disclosure of Japanese Patent Application No. 2019-122367, filed on June 28, 2019, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. Preparing an electrode material including an electrode active material; A step of supplying the electrode material to a mold that has a frame-shaped side wall portion that defines a space portion for accommodating the electrode material and has a first support disposed on a bottom surface of the mold, the mold being disposed on a conveyor belt; forming the electrode material along an internal shape of the mold; removing the electrode material from the mold; in this order, a step of disposing a second support on the electrode material supplied to the mold either between the step of supplying the electrode material and the step of molding the electrode material, or between the step of molding the electrode material and the step of removing the electrode material; The second support is a current collector. A method for producing an electrode molded body.

2. Preparing an electrode material including an electrode active material; A step of supplying the electrode material to a mold that has a frame-shaped side wall portion that defines a space portion for accommodating the electrode material and has a first support disposed on a bottom surface of the mold, the mold being disposed on a conveyor belt; forming the electrode material along an internal shape of the mold; removing the electrode material from the mold; in this order, The method includes a step of placing a second support on the electrode material supplied to the mold, and the step of placing the second support and the step of molding the electrode material are performed simultaneously; The second support is a current collector. A method for producing an electrode molded body.

3. 3. The method for producing an electrode molded body according to claim 1, wherein the surface of the conveyor belt is the bottom surface of the mold.

4. The method for producing an electrode molded body according to any one of claims 1 to 3, wherein in the step of molding the electrode material, the electrode material is molded by directly or indirectly contacting the electrode material with a molding member.

5. 5. The method for producing an electrode molded body according to claim 1, further comprising, between the step of molding the electrode material and the step of removing the electrode material, a step of disposing the electrode material below the first support in a vertical direction by changing a positional relationship between the first support and the electrode material.

6. In the step of removing the electrode material, the electrode material and the first support are removed from the mold. The method for producing the electrode molded article according to any one of claims 1 to 5.

7. The method for producing an electrode molded body according to any one of claims 1 to 6, further comprising a step of pressurizing the electrode material between the step of molding the electrode material and the step of removing the electrode material, or after the step of removing the electrode material.

8. The method for producing an electrode molded body according to claim 7 , wherein in the step of pressing the electrode material, the electrode material is pressed stepwise using a plurality of rolls.

9. The method for producing an electrode molded body according to any one of claims 1 to 8, wherein the electrode material is supplied to the molding die by discharging the electrode material from a discharge port having an opening / closing mechanism for controlling the supply of the electrode material.

10. The method for producing an electrode molded body according to claim 9 , wherein the electrode material is supplied to the mold while the discharge port and the mold are moved relatively to each other.

11. The method for producing an electrode molded body according to any one of claims 1 to 10, wherein the content of a liquid component in the electrode material is 30 mass % or less with respect to the total mass of the electrode material.

12. The method for producing an electrode molded body according to any one of claims 1 to 11, wherein the electrode material contains a conductive assistant.

13. The method for producing an electrode molded body according to any one of claims 1 to 12, wherein the first support is a release material.

Citation Information

Patent Citations

  • Manufacturing equipment and manufacturing method for electrode of power type lithium ion battery

    CN102694149A

  • Semiconductor memory device

    JP1984103371A

  • Manufacture of flat cell positive electrode body

    JP1988029445A

  • Apparatus and method for manufacturing fuel cell body

    JP2000277129A

  • Process for producing electrode laminate and electrode laminate

    WO2011064842A1