Liquid crystal polyester resin composition, liquid crystal polyester film using said composition, metal laminate film using said film, and circuit board
A resin composition with polyetherimide and siloxane bonds stabilizes film formation of high-melting-point thermoplastic liquid crystal polyester, addressing viscosity issues and ensuring stable, high-quality films for electronic applications.
Patent Information
- Application Number
- JP2023503933
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-05
- Filing Date
- 2022-03-02
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2042-03-02
AI Technical Summary
Thermoplastic liquid crystal polyester films with melting points of 300°C or higher face challenges in stable film formation due to rapid viscosity decrease under shear stress and temperature fluctuations, leading to hole formation during extrusion processes like inflation extrusion.
A resin composition is developed by blending a small amount of polyetherimide with siloxane bonds in the main chain with thermoplastic liquid crystalline polyester, allowing stable film formation through extrusion molding by maintaining mechanical, electrical, and heat-resistant properties.
The composition suppresses hole formation during extrusion, enhances film-forming processability, and maintains excellent mechanical and electrical properties, suitable for high-speed communication applications.
Smart Images

Figure 0007572535000001 
Figure 0007572535000002 
Figure 0007572535000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal polyester resin composition containing a thermoplastic liquid crystal polyester capable of forming an optically anisotropic molten phase as a main component, a liquid crystal polyester film using the resin composition, and a metal laminate film and a circuit board using the film. [Background technology]
[0002] In recent years, there has been a growing demand in the electronics and electrical fields for smaller and lighter devices, and insulating films with excellent electrical and mechanical properties are in demand. However, conventional raw materials for insulating films, such as polyimide and polyethylene terephthalate, have insufficient electrical properties in the high frequency range, and are highly hygroscopic, which can lead to poor electrical properties and large dimensional changes, making it difficult to create a film that meets the above requirements.
[0003] In contrast, thermoplastic liquid crystal polyesters are useful in the electronics and electrical fields because they exhibit excellent mechanical and electrical properties, low dimensional change, high heat resistance and chemical stability, etc. In particular, thermoplastic liquid crystal polyesters with a melting point of 300°C or higher are useful for printed circuit board applications because they can be used for lead-free solder reflow. However, thermoplastic liquid crystal polyesters have rigid molecular chains that are arranged in an orderly manner even in the molten state, and the molecular chains flow smoothly without entanglement, so the molecular chains tend to be oriented in the direction of the resin flow, and simply forming them into a film does not reach a level where they can be used.
[0004] Patent Document 1 is an invention related to an aromatic resin composition characterized by comprising a wholly aromatic copolyester (liquid crystal polyester) and a polyetherimide, and describes that the mechanical and electrical properties of the wholly aromatic polyester are improved by the polyetherimide. However, the examples in Patent Document 1 only disclose that the resin composition is press-molded into a test piece, and there is no disclosure of continuously molding the resin composition into a film.
[0005] Patent Document 2 is an invention related to a resin composition consisting of a thermotropic liquid crystal polyester and a siloxane polyetherimide copolymer, and discloses that the anisotropy of the mechanical properties of the liquid crystal polyester is reduced by the siloxane polyetherimide copolymer. However, in the examples of Patent Document 2, it is only disclosed that the resin composition is used to prepare a sample piece for various measurements, and there is no disclosure about forming it into a film.
[0006] Patent Document 3 is an invention that aims to improve the edge tear strength without impairing the excellent properties of a thermoplastic liquid crystal polymer (liquid crystal polyester) capable of forming an optically anisotropic melt layer. Patent Document 3 discloses a polymer alloy consisting of a thermoplastic polymer (liquid crystal polyester) capable of forming an optically anisotropic melt layer and an amorphous polymer, and a film consisting of the polymer alloy. Examples of the amorphous polymer include polysulfone, polyethersulfone, polyphenylene sulfide, polycarbonate, polyethylene isophthalate, and polyarylate. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent Publication No. 64-1758 [Patent Document 2] JP 4-246458 [Patent Document 3] Patent Publication No. 2000-290512 Summary of the Invention [Problem to be solved by the invention]
[0008] As a method for producing a film made of a thermoplastic liquid crystal polyester, a production method using an extrusion method such as an inflation extrusion method is known. In Patent Document 3, a film is produced by an inflation extrusion method in an example. In the case of the inflation extrusion method, the orientation of the molecular chain can be controlled to some extent by appropriately adjusting the blow ratio.
[0009] On the other hand, the melt viscosity of the thermoplastic liquid crystal polyester is highly dependent on shear stress, and a slight increase in shear stress causes a significant decrease in the melt viscosity. Therefore, when the thermoplastic liquid crystal polyester is melt-extruded by the inflation extrusion molding method, the shear stress generated at the die portion causes a sudden decrease in the melt viscosity, making it difficult to maintain the shape of the film, and there is a problem that it is difficult to stably produce the film.
[0010] In addition, the melt viscosity of the thermoplastic liquid crystal polyester is highly dependent on temperature, and a slight increase in temperature around the melting point causes a significant drop in the melt viscosity. This tendency is more pronounced for thermoplastic liquid crystal polyesters with higher melting points, and in particular, thermoplastic liquid crystal polyesters with melting points of 300°C or higher have low melt viscosity around the melting point, so that when a film is produced by extrusion molding such as inflation extrusion molding, holes tend to form in the bubbles extruded from the die, making it difficult to stably produce the film.
[0011] The present invention has been made in consideration of such problems, and an object of the present invention is to provide a liquid crystal polyester resin composition that has excellent mechanical properties, electrical properties, and heat resistance and can be stably formed into a film by extrusion molding such as inflation extrusion molding. [Means for solving the problem]
[0012] The inventors conducted extensive research into a resin composition that would enable stable film formation while maintaining the excellent mechanical properties, electrical properties, and heat resistance of thermoplastic liquid crystal polyesters having a melting point of 300°C or higher. As a result, they discovered that by blending a small amount of polyetherimide having a soft segment containing a siloxane bond in the main chain with a thermoplastic liquid crystal polyester having a melting point of 300°C or higher, stable film formation is possible by extrusion molding such as inflation extrusion molding, and thus completed the present invention.
[0013] According to the present invention, (1) A liquid crystal polyester resin composition comprising a thermoplastic liquid crystal polyester (A) and a polyetherimide (B), wherein the liquid crystal polyester (A) has a melting point of 300° C. or higher, the polyetherimide (B) has a siloxane bond in its main chain, and the blending ratio of the thermoplastic liquid crystal polyester (A) to the polyetherimide (B) is (A):(B)=92-99.5% by weight:0.5-8% by weight, (2) The liquid crystal polyester resin composition according to (1) is provided, characterized in that the thermoplastic liquid crystal polyester (A) contains a structural unit derived from p-hydroxybenzoic acid and a structural unit derived from 6-hydroxy-2-naphthoic acid; (3) The liquid crystal polyester resin composition according to (1) or (2) is provided, which is for use in an inflation extrusion molding method; (4) A liquid crystal polyester film comprising the resin composition according to any one of (1) to (3), (5) The liquid crystal polyester film according to (4) is provided, characterized in that, when F(MD) is the tensile strength in the machine direction of the film and F(TD) is the tensile strength in the width direction of the film, 0.75≦F(TD) / F(MD)≦1.25; (6) The method for producing a liquid crystal polyester film according to (4) or (5) is provided, characterized in that the film is produced by an inflation extrusion method, (7) A metal laminate film is provided, characterized in that a metal layer is laminated on one or both sides of the liquid crystal polyester film according to claim 4 or 5, (8) There is provided a circuit board comprising at least one conductor layer and the thermoplastic liquid crystal polyester film according to (4) or (5). Effect of the Invention
[0014] The liquid crystal polyester resin composition of the present invention contains a polyetherimide having a siloxane bond in the main chain, and thus can suppress the occurrence of holes in the bubbles extruded from the die when forming a film in an extrusion molding method such as inflation extrusion molding, and can stably form a film. In addition, by blending a specific amount of a polyetherimide having a siloxane bond in the main chain, it is possible to maintain the excellent mechanical properties, electrical properties, and heat resistance of a thermoplastic liquid crystal polyester having a melting point of 300 ° C. or more while improving the film forming processability. Therefore, the liquid crystal polyester film made of the liquid crystal polyester resin composition of the present invention and the metal laminate film obtained by laminating the liquid crystal polyester film and a metal layer have excellent mechanical properties, electrical properties, and solder reflow properties, and can be suitably used for applications such as laminates for circuit boards suitable for high-speed communication applications. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below. Note that the present invention is not limited to the following embodiments, and various embodiments can be made within the scope of the effects of the present invention.
[0016] [Liquid crystal polyester resin composition] The liquid crystal polyester resin composition of the present invention comprises a resin composition containing a thermoplastic liquid crystal polyester (A) and a polyetherimide (B) having a siloxane bond in the main chain.
[0017] [Thermoplastic liquid crystal polyester (A)] The thermoplastic liquid crystal polyester (A) is a liquid crystal polyester that exhibits melt anisotropy (a polyester that can form an optically anisotropic molten phase). The melt anisotropy can be confirmed by a conventional polarized light inspection method using crossed polarizers. Specifically, the melt anisotropy can be confirmed by using a polarizing microscope (Olympus Corporation, etc.) to melt a sample placed on a hot stage (Linkam Corporation, etc.) and observing it at a magnification of 150 times under a nitrogen atmosphere. A liquid crystal resin that exhibits optical anisotropy when melted is optically anisotropic and transmits light when inserted between crossed polarizers. If the sample is optically anisotropic, polarized light will transmit even when it is in a molten, stationary liquid state, for example.
[0018] The thermoplastic liquid crystal polyester (A) used in the resin composition of the present invention is a resin having a melting point of 300° C. or more among thermoplastic liquid crystal polyesters. If the melting point is lower than 300° C., the solder reflow property is poor, and therefore, when used for applications such as printed circuit boards, the processing method is limited.
[0019] The thermoplastic liquid crystal polyester (A) used in the resin composition of the present invention preferably contains a constitutional unit derived from p-hydroxybenzoic acid (sometimes referred to as monomer component A) and a constitutional unit derived from 6-hydroxy-2-naphthoic acid (sometimes referred to as monomer component B) as essential units. The thermoplastic liquid crystal polyester (A) may contain a monomer component C other than the monomer components A and B. Examples of the monomer component C include aromatic or aliphatic dicarboxylic acids; aromatic or aliphatic dihydroxy compounds; aromatic hydroxycarboxylic acids; aromatic diamines, aromatic hydroxyamines, or aromatic aminocarboxylic acids; and the like. These may be used alone or in combination of two or more.
[0020] Specific examples of the thermoplastic liquid crystal polyester (A) include a binary polycondensate of p-hydroxybenzoic acid (monomer component A) and 6-hydroxy-2-naphthoic acid (monomer component B); a ternary polycondensate of p-hydroxybenzoic acid (monomer component A), 6-hydroxy-2-naphthoic acid (monomer component B), and terephthalic acid (monomer component C); and a ternary or higher polycondensate of p-hydroxybenzoic acid (monomer component A), 6-hydroxy-2-naphthoic acid (monomer component B), and one or more monomers (monomer component C) selected from the group consisting of terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenol, bisphenol A, hydroquinone, and ethylene terephthalate.
[0021] The blending ratio of each structural unit of the thermoplastic liquid crystal polyester (A) is not particularly limited, but for example, the monomer component A is preferably 20 mol% or more and 90 mol% or less, more preferably 30 mol% or more and 85 mol% or less, and even more preferably 40 mol% or more and 80 mol% or less, based on the total structural units of the thermoplastic liquid crystal polyester (A). Similarly, the monomer component B is preferably 10 mol% or more and 80 mol% or less, more preferably 15 mol% or more and 70 mol% or less, and even more preferably 20 mol% or more and 60 mol% or less, based on the total structural units of the thermoplastic liquid crystal polyester (A).
[0022] When the thermoplastic liquid crystal polyester (A) contains the monomer component C, the blending ratio of each structural unit of the thermoplastic liquid crystal polyester (A) is not particularly limited, but for example, the monomer component A is preferably 15 mol% or more and 90 mol% or less, more preferably 20 mol% or more and 85 mol% or less, based on the total structural units. Similarly, the monomer component B is preferably 5 mol% or more and 60 mol% or less, more preferably 15 mol% or more and 50 mol% or less, based on the total structural units of the thermoplastic liquid crystal polyester (A). Similarly, the monomer component C is preferably 0.5 mol% or more and 60 mol% or less, more preferably 1 mol% or more and 50 mol% or less, based on the total structural units of the thermoplastic liquid crystal polyester (A).
[0023] The melting point of the thermoplastic liquid crystal polyester (A) is not particularly limited as long as it is 300°C or higher, but from the viewpoint of heat resistance and moldability, it is preferably 300°C or higher and 400°C or lower, more preferably 305°C or higher and 370°C or lower, even more preferably 310°C or higher and 360°C or lower, and particularly preferably 315°C or higher and 345°C or lower. The melting point of the thermoplastic liquid crystal polyester (A) is determined by heating a sample at a rate of 10°C / min using a differential scanning calorimeter (DSC) to completely melt it, then cooling the molten product to 30°C at a rate of 10°C / min, and heating it again at a rate of 10°C / min, at the position of the endothermic peak that appears when the sample is heated at a rate of 10°C / min to 30°C.
[0024] [Polyetherimide (B) having siloxane bonds in the main chain] Polyetherimide (B) having a siloxane bond in the main chain is a non-crystalline thermoplastic resin in which a siloxane group is introduced into polyetherimide to impart the flexibility of a silicone elastomer. Polyetherimide is a resin having an imide bond and an ether bond in the molecule, and is represented, for example, by the following general formula (1). <General formula (1)> [ka] (In the formula, n represents the degree of polymerization, and is preferably 10 or more, more preferably 10 or more and 200 or less, and even more preferably 10 or more and 100 or less.)
[0025] The polyetherimide (B) having a siloxane bond in the main chain is a silicone-modified polyetherimide obtained by block copolymerizing a polyetherimide represented by general formula (1) with a siloxane group represented by the following general formula (2). <General formula (2)> [ka] (In the formula, m represents the degree of polymerization, and is preferably 1 or more, more preferably 1 or more and 20 or less, and even more preferably 1 or more and 10 or less.)
[0026] The silicone-modified polyetherimide may be a synthetic product or a commercially available product, such as SILTEM manufactured by SHPP Japan LLC. TM STM1500, SILTEM TM STM1600, SILTEM TM Examples include STM1700.
[0027] The glass transition temperature of the silicone-modified polyetherimide is not particularly limited, but is preferably 190°C or higher, more preferably 195°C or higher, and even more preferably 200°C or higher. If the glass transition temperature of the silicone-modified polyetherimide is within the above range, a liquid crystal polyester resin composition having excellent heat resistance can be obtained. The glass transition temperature of the silicone-modified polyetherimide is determined by heating a sample at a rate of 10°C / min using a differential scanning calorimeter (DSC) to completely melt the sample, then cooling the melt to 30°C at a rate of 10°C / min, and heating the sample again at a rate of 10°C / min. The intersection of the original baseline and the tangent at the inflection point at the position where the baseline shifts is the glass transition temperature.
[0028] The liquid crystal polyester resin composition of the present invention contains the above-mentioned thermoplastic liquid crystal polyester (A) and the polyetherimide (B) having a siloxane bond in the main chain in a ratio of (A):(B)=92-99.5% by weight:0.5-8% by weight. Preferably, (A):(B)=94-99.5% by weight:0.5-6% by weight, more preferably (A):(B)=96-99.5% by weight:0.5-4% by weight. From the viewpoint of obtaining particularly excellent mechanical properties, preferably, (A):(B)=94-96% by weight:4-6% by weight. If the blending ratio of the polyetherimide (B) having a siloxane bond in the main chain is less than the above range, the film forming processability of the liquid crystal polyester resin composition by extrusion molding cannot be improved, and stable film formation cannot be performed. If the proportion of the polyetherimide (B) having a siloxane bond in the main chain is more than the above range, the mechanical properties of the liquid crystal polyester film made of the liquid crystal polyester resin composition are significantly deteriorated.
[0029] The liquid crystal polyester resin composition of the present invention may contain other resin components other than the above-mentioned thermoplastic liquid crystal polyester (A) and polyetherimide (B) having a siloxane bond in the main chain, within a range that does not impair the effects of the present invention. Examples of other resin components include thermoplastic resins such as polyarylate, polyphenylene sulfide, polyphenylene ether, polyether ether ketone, polyetherimide, cycloolefin polymer, polyamide, polyamideimide, polyimide, and epoxy group-containing olefin copolymer. The liquid crystal polyester resin composition of the present invention may also contain additives such as lubricants, antioxidants, and fillers.
[0030] [Method of manufacturing liquid crystal polyester film] The present invention also proposes a film made of the above-mentioned resin composition and a method for producing the film. The liquid crystal polyester film of the present invention is obtained by blending the above-mentioned thermoplastic liquid crystal polyester (A) and the polyetherimide (B) having a siloxane bond in the main chain by a known method and forming a film. Since the resin composition of the present invention has a low blending ratio of the polyetherimide (B) having a siloxane bond in the main chain, it is preferable to melt-knead and granulate the resin composition prior to film formation in order to provide a stable kneaded state.
[0031] The equipment for melt kneading is not particularly limited, and examples thereof include various known extruders such as a batch kneader, a kneader, a co-kneader, a Banbury mixer, a roll mill, a single-screw or twin-screw extruder, etc. Among these, a single-screw extruder or a twin-screw extruder is preferably used because of its excellent kneading ability and productivity.
[0032] The resin composition of the present invention is preferably formed into a film by an extrusion molding method such as a T-die extrusion method or an inflation extrusion method, since a sudden decrease in melt viscosity of the resin composition due to shear stress can be suppressed by blending a small amount of polyetherimide (B) having a siloxane bond in the main chain. Among them, in consideration of the balance of mechanical properties of the film, it is preferable to form the film by the inflation extrusion molding method.
[0033] An example of the inflation extrusion molding method is a method in which the above-mentioned resin composition is fed into a melt extruder equipped with a die having an annular slit, the molten resin composition is extruded upward or downward in a bubble shape from the annular slit of the extruder, and air or an inert gas is blown into the inside of the bubble made of the molten resin composition to expand and stretch the bubble in a direction (TD) perpendicular to the flow direction (MD) to obtain a film. The cylinder temperature of the melt extruder is usually 280 to 400°C, preferably 320 to 380°C. The interval between the annular slits is usually 0.1 to 5 mm, preferably 0.2 to 2 mm. The diameter of the annular slit is usually 20 to 1000 mm, preferably 25 to 600 mm.
[0034] In the inflation extrusion molding method, the blow ratio is preferably 1.5 or more, more preferably 2.0 or more, even more preferably 4.0 or more, and particularly preferably 4.5 or more. The upper limit of the blow ratio is not particularly limited, but for example, the blow ratio is 10 or less. The draft ratio is preferably 1.5 to 20, more preferably 1.5 to 10. Here, the blow ratio is the stretch ratio in the TD direction, and the draft ratio is the stretch ratio in the MD direction. When the blow ratio and the draft ratio are in the above range, the anisotropy of the tensile modulus and tensile strength of the obtained film (the difference between the MD direction and the TD direction) can be improved. However, in the inflation extrusion molding method, increasing the blow ratio to improve the anisotropy of the film works in the direction of destabilizing the shape retention of the bubble made of the resin composition in a molten state, so that the bubble is likely to vibrate or have holes. In particular, when a liquid crystal polyester having a melting point of more than 300°C is expanded and stretched by inflation extrusion molding so that the blow ratio is 4.0 or more, holes are frequently formed in the bubbles, making it difficult to form a film. In contrast, the resin composition of the present invention contains a small amount of polyetherimide (B) having a siloxane bond in the main chain, which can suppress a sudden decrease in the melt viscosity of the resin composition due to shear stress, etc., and therefore, even if the blow ratio is 4.0 or more, holes are suppressed from being formed in the bubbles, and the film can be stably formed while improving the anisotropy of the film.
[0035] The thickness of the liquid crystal polyester film of the present invention is not particularly limited, but is, for example, 0.5 μm or more and 1000 μm or less. Taking into consideration the handling property and productivity during melt extrusion, the thickness is preferably 5 μm or more and 500 μm or less, more preferably 20 μm or more and 300 μm or less, and even more preferably 30 μm or more and 200 μm or less.
[0036] The liquid crystal polyester film of the present invention preferably has a tensile strength of 180 MPa or more in the machine direction (MD direction) and the width direction (TD direction). The tensile strength is more preferably 200 MPa or more, and even more preferably 220 MPa or more. The upper limit of the tensile strength is not particularly limited, but is preferably, for example, 500 MPa or less, more preferably 400 MPa or less, and even more preferably 350 MPa or less. If the tensile strength is within the above range, the film has excellent handleability when processed into a laminate for a circuit board suitable for high-speed communication applications, and can suppress defects and cracks that occur at the ends of the film.
[0037] The liquid crystal polyester film of the present invention preferably has low anisotropy in the machine direction (MD) and width direction (TD). In particular, the tensile strength F(TD) in the width direction of the film relative to the tensile strength F(MD) in the machine direction of the film (i.e., F(TD) / F(MD)) is preferably 0.5 to 1.5, more preferably 0.75 to 1.25, even more preferably 0.85 to 1.25, and particularly preferably 0.90 to 1.20. If the tensile strength F(TD) in the width direction of the film relative to the tensile strength F(MD) in the machine direction of the film is within the above range, the anisotropy of the mechanical and electrical properties of the film is small, and it can be suitably used for applications such as laminates for circuit boards suitable for high-speed communication applications.
[0038] The liquid crystal polyester film of the present invention can be further subjected to a heat treatment to relax the orientation of the molecular chains and improve the film dimensional stability. The heat treatment can be a conventionally known method, for example, a contact heat treatment, a non-contact heat treatment, etc., and the type is not particularly limited.
[0039] [Metal laminate film] The liquid crystal polyester film of the present invention may be used as a metal laminate film by laminating a metal layer thereon. When laminating the metal layer, the surface of the liquid crystal polyester film on which the metal layer is to be laminated may be subjected to corona discharge treatment, ultraviolet irradiation treatment or plasma treatment in order to increase adhesive strength.
[0040] Examples of the method for laminating a metal layer on the liquid crystal polyester film of the present invention include (1) a method for attaching a liquid crystal polyester film to a metal foil by heat and pressure bonding, (2) a method for attaching a liquid crystal polyester film and a metal foil with an adhesive, and (3) a method for forming a metal layer on a liquid crystal polyester film by vapor deposition. Among them, the lamination method (1) is a method for pressing the liquid crystal polyester film to a metal foil at a temperature near the flow start temperature of the liquid crystal polyester film using a press or a heated roll, and is recommended because it can be easily performed. Examples of the adhesive used in the lamination method (2) include hot melt adhesives and polyurethane adhesives. Among them, epoxy group-containing ethylene copolymers are preferably used as adhesives. Examples of the lamination method (3) include ion beam sputtering, high frequency sputtering, direct current magnetron sputtering, and glow discharge. Among them, high frequency sputtering is preferably used.
[0041] Examples of metals used in the metal layer include gold, silver, copper, copper alloys, nickel, nickel alloys, aluminum, aluminum alloys, iron, and iron alloys. Copper is preferred for tab tapes and circuit boards, and aluminum is preferred for capacitors. Examples of the structure of the metal laminate film thus obtained include a two-layer structure of a liquid crystal polyester film and a metal layer, a three-layer structure in which metal layers are laminated on both sides of a liquid crystal polyester film, and a five-layer structure in which liquid crystal polyester films and metal layers are alternately laminated. The laminate may be heat-treated as necessary for the purpose of developing high strength. The thickness of the metal layer is not particularly limited, but is preferably 1.5 to 1000 μm, more preferably 2 to 500 μm, even more preferably 5 to 150 μm, and particularly preferably 7 to 100 μm. If the thickness is thinner than this range, the mechanical strength is poor, and if the thickness is thicker than the above range, the handling and processability are poor.
[0042] [Circuit board] The circuit board of the present invention includes at least one conductor layer and at least one insulator (or dielectric) layer, and the form is not particularly limited as long as the liquid crystal polyester film of the present invention is used as the insulator (or dielectric), and it can be used as various high-frequency circuit boards by known or conventional means. The circuit board may also be a circuit board (or a semiconductor element mounting board) on which a semiconductor element (e.g., an IC chip) is mounted.
[0043] The conductor layer used in the circuit board of the present invention is formed, for example, from at least a metal having electrical conductivity, and a circuit pattern is formed on this conductor layer by using a known circuit processing method. The conductor forming the conductor layer may be various metals having electrical conductivity, such as gold, silver, copper, iron, nickel, aluminum, or alloy metals thereof. In addition, a circuit pattern may be formed on the metal layer portion of the above-mentioned metal laminate film. EXAMPLES
[0044] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. Evaluations in the examples were performed by the following methods.
[0045] (Film-forming: Bubble holes) When a film was produced by inflation extrusion molding, the appearance of bubbles of molten resin extruded from a die was visually observed and evaluated according to the following criteria. ○: No holes in the bubble △: Small holes appear in the bubble (air leaks from inside the bubble, making the bubble shape unstable) ×: Holes in the bubble occur, film production is not possible (Tensile strength) In accordance with ASTM D882, samples cut to a size of 190 mm x 15 mm were measured using an autograph AGS-500NX (Shimadzu Corporation) at a tensile speed of 12.5 mm / min and a chuck distance of 125 mm. The measurement temperature was 23°C. Measurements were performed in both the machine direction (MD) and the width direction (TD) of the film.
[0046] The following resins were used in the examples and comparative examples. LCP: Liquid crystal polyester consisting of a constitutional unit derived from p-hydroxybenzoic acid, a constitutional unit derived from 6-hydroxy-2-naphthoic acid, and a constitutional unit derived from terephthalic acid (LAPEROS (registered trademark) C950RX manufactured by Polyplastics Co., Ltd., melting point: 320°C) PEI-SS: Siloxane modified polyetherimide (SILTEM manufactured by SHPP Japan LLC) TM STM-1700, glass transition temperature: 197℃) PEI: Polyetherimide (ULTEM manufactured by SHPP Japan LLC) TM 1000, glass transition temperature: 217℃) PSU: Polysulfone (Ultrason (registered trademark) S2010, manufactured by BASF Japan, glass transition temperature: 187°C) PPSU: Polyphenylene sulfone (Ultrason (registered trademark) P3010, manufactured by BASF Japan, glass transition temperature: 220°C) PES: Polyethersulfone (Ultrason® E2010, manufactured by BASF Japan, glass transition temperature: 225°C)
[0047] <Example 1> 99% by weight of LCP and 1% by weight of PEI-SS were dry-blended, fed to a melt extruder equipped with a die with a circular slit (diameter 25 mm), melt-extruded from the circular slit of the extruder at a discharge rate of 3 kg / h, stretched under conditions of a draft ratio of 2 and a blow ratio of 5, and a liquid crystal polyester film with a thickness of 50 μm was obtained by inflation extrusion molding. The film formability and tensile strength of the obtained film are shown in Table 1.
[0048] <Examples 2 and 3, Comparative Examples 1 to 8> Except for changing the liquid crystal polyester resin composition as shown in Table 1, the liquid crystal polyester films of Examples 2 and 3 and Comparative Examples 1 to 8 were obtained in the same manner as in Example 1. The film formability and tensile strength of the obtained films are shown in Table 1.
[0049] [Table 1]
[0050] The liquid crystal polyester films of Examples 1 to 3 containing 1, 3, and 5% by weight of siloxane-modified polyetherimide as an amorphous polymer were capable of stable film formation without holes in the bubbles of molten resin extruded from a die at a stretching ratio exceeding 4.0 in blow ratio. In addition, the liquid crystal polyester films of Examples 1 to 3 maintained the excellent mechanical properties, electrical properties, and heat resistance of thermoplastic liquid crystal polyesters having a melting point of 300°C or more, and showed small anisotropy in tensile strength.
[0051] On the other hand, the liquid crystal polyester films of Comparative Examples 1 and 2 containing 10 and 15% by weight of siloxane-modified polyetherimide were able to be stably formed without holes in the bubbles of the molten resin extruded from the die at a stretch ratio exceeding 4.0 in blow ratio, but showed a significant decrease in tensile strength and a relatively large anisotropy in tensile strength compared to the liquid crystal polyester film of Comparative Example 4 not containing an amorphous polymer. Also, the liquid crystal polyester film of Comparative Example 3 containing 50% by weight of siloxane-modified polyetherimide was unable to be formed into a film because holes were frequently generated at a stretch ratio exceeding 4.0 in blow ratio.
[0052] The liquid crystal polyester film of Comparative Example 4, which was made only of a thermoplastic liquid crystal polyester having a melting point exceeding 300°C, showed that at a stretching ratio exceeding a blow ratio of 4.0, small holes were generated in the bubbles of molten resin extruded from the die, and the air inside the bubbles made the bubble shape unstable.
[0053] The liquid crystal polyester film of Comparative Example 5, which contained 5% by weight of non-siloxane-modified polyetherimide as an amorphous polymer, was capable of stable film formation without holes in the bubbles of molten resin extruded from the die at a stretching ratio exceeding 4.0 in blow ratio, but showed a significantly lower tensile strength and a relatively large anisotropy in tensile strength compared to the liquid crystal polyester film of Comparative Example 4, which did not contain an amorphous polymer.
[0054] The liquid crystal polyester films of Comparative Examples 6 to 8, which contained 5% by weight each of polysulfone, polyphenylene sulfone, and polyether sulfone as amorphous polymers, showed results in which small holes were generated in the bubbles of molten resin extruded from the die at a stretching ratio exceeding a blow ratio of 4.0, and the air inside the bubbles made the bubble shape unstable. [Industrial Applicability]
[0055] As described above, the liquid crystal polyester film obtained by the present invention is used for electrical insulation of motors and transformers, element formation film of flexible solar cells, etc. by taking advantage of its excellent electrical properties, dimensional stability, heat resistance, etc. It can also be used in the acoustic field, such as surface protection films and diaphragms. The metal laminate film of the present invention can also be used for circuit boards, capacitors, electromagnetic wave shielding materials, etc. The circuit board of the present invention may be used for various transmission lines and antennas (for example, microwave or millimeter wave antennas), and may also be used for antenna devices in which an antenna and a transmission line are integrated.
Claims
1. A liquid crystal polyester resin composition comprising a thermoplastic liquid crystal polyester (A) and a polyetherimide (B), wherein the thermoplastic liquid crystal polyester (A) has a melting point of 300°C or higher, the polyetherimide (B) has a siloxane bond in its main chain, and the blending ratio of the thermoplastic liquid crystal polyester (A) to the polyetherimide (B) is (A):(B)=92-99.5% by weight:0.5-8% by weight, and a liquid crystal polyester film comprising the resin composition.
2. The liquid crystal polyester film according to claim 1, characterized in that the thermoplastic liquid crystal polyester (A) contains a structural unit derived from p-hydroxybenzoic acid and a structural unit derived from 6-hydroxy-2-naphthoic acid.
3. 3. The liquid crystal polyester film according to claim 1, which is an inflation film.
4. The liquid crystal polyester film according to any one of claims 1 to 3, characterized in that, when F(MD) is the tensile strength in the machine direction of the film and F(TD) is the tensile strength in the width direction of the film, 0.75≦F(TD) / F(MD)≦1.
25.
5. 5. A metal laminate film, comprising the liquid crystal polyester film according to claim 1, and a metal layer laminated on one or both sides of the liquid crystal polyester film.
6. A circuit board comprising at least one conductor layer and the thermoplastic liquid crystal polyester film according to claim 1 .
Citation Information
Patent Citations
Aromatic resin composition
JP1989001758A
Liquid crystal polyester composition
JP1992246458A
Polymer alloy and its film
JP2000290512A
Liquid crystalline resin composition and method for producing the same
JP2007138143A
Cited By
Laminate board, multilayer board, and manufacturing method of laminate board
JP2024160919A
Laminate, multilayer board, and manufacturing method of laminate
US12679927B2