Use of particulate material comprising particulate synthetic amorphous silicon dioxide as an additive to casting material mixtures, corresponding methods, mixtures and kits

Incorporating particulate synthetic amorphous silicon dioxide with a specific particle size in casting material mixtures enhances moisture resistance and casting weight, addressing the challenge of achieving high quality and stability without relying on lithium or boron compounds.

JP7572970B2Active Publication Date: 2024-10-24HUTTENES-ALBERTUS CHEMISCHE WERKE GMBH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021564550
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-16
Filing Date
2020-05-14
Publication Date
2024-10-24
Estimated Expiration
2040-05-14

AI Technical Summary

Technical Problem

Existing casting material mixtures struggle to achieve a high relative casting weight and good humidity stability while minimizing the use of lithium or boron compounds, which are often necessary for moisture resistance.

Method used

Incorporating particulate synthetic amorphous silicon dioxide with a specific particle size distribution (0.1 to 0.4 μm) as an additive in casting material mixtures, along with refractory mold base materials and water glass, to enhance moisture resistance and casting weight.

Benefits of technology

The solution results in castings with improved moisture resistance and high relative casting weight, achieving a synergistic effect without the need for significant amounts of lithium or boron compounds, ensuring high quality and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572970000008
    Figure 0007572970000008
  • Figure 0007572970000009
    Figure 0007572970000009
  • Figure 0007572970000010
    Figure 0007572970000010
Patent Text Reader

Abstract

The present invention relates to the use of a particulate material comprising, as an individual component or as one of several components, particulate synthetic amorphous silicon dioxide having a particle size distribution with a median value in the range of 0.1 to 0.4 μm, as determined by laser scattering, as an additive to a casting material mixture containing at least the following: a refractory mold base material having an AFS grain size index in the range of 30 to 100, particulate amorphous silicon dioxide having a grain size distribution with a median value in the range of 0.7 to 1.5 μm, as determined by laser scattering, and water glass, for the purpose of increasing the moisture resistance of castings that can be produced by thermal curing of the casting material mixture. The present invention also relates to corresponding methods, mixtures, and kits.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the use of a particulate material comprising particulate synthetic amorphous silicon dioxide as its sole or one of its constituents as an additive to a casting material mixture for increasing the moisture resistance of a casting producible by thermal hardening of the casting material mixture. Further details of the use according to the invention will become apparent from the accompanying claims and the following description. The present invention further relates to a corresponding process for producing a heat-cured casting having improved moisture resistance. In addition, the present invention also relates to a mixture and its use. The present invention further relates to a kit. Respective details will become apparent from the accompanying claims and the following description. [Background technology]

[0002] Lost mold casting is a widely used process for producing near net shape parts. After casting, the mold is broken and the cast part is extracted. Lost molds are negative since they are casting molds; they contain the cavity to be cast, whereby the final cast part is obtained. The internal shape of the future casting is formed by a core. During the production of the mold, a model of the cast part to be produced forms the cavity in the casting material.

[0003] In contrast to the sand casting process, in which the mold (lost mold) is destroyed after casting to extract the cast part, the metal permanent mold, for example made from cast iron or steel, can be reused for the next casting after the cast part is extracted. It is also possible to cast by die casting, in which liquid molten metal is injected into the die casting mold under high pressure and with a high mold filling rate. The aforementioned casting process is also preferred in the context of the present invention. The mold base material used for the mold (in the sand casting process with lost mold) and for the cores is mainly a refractory granular material, for example washed classified silica sand. For the production of the molds, the mold base material is bound with an inorganic or organic binder. The binder creates a certain coherence between the particles of the mold base material so that the mold or the core contains the necessary mechanical stability. The refractory mold base material, premixed with the binder, is preferably in a free-flowing form so that it can be introduced into a suitable cavity and compressed there. The casting material is compressed to increase its strength.

[0004] Molds and cores must meet various requirements: during the actual casting process, they must first have sufficient strength and thermal stability to allow the liquid metal to be contained in the cavity formed by the (partial) mold or molds. After the solidification process starts, the mechanical stability of the cast part is ensured by the solidified metal layer that forms along the walls of the mold.

[0005] The material of the mold would then be expected to change under the effect of the heat given off by the metal, thereby losing its mechanical strength, i.e. the coherence between the individual particles of the refractory material is lost. In the ideal case, the mold and the core would disintegrate again, forming a fine sand which can be easily removed from the cast part and which has accordingly favourable breaking properties.

[0006] DE 10 2013 111 626 A1 discloses a foundry material mixture for the production of moulds or cores, which comprises at least the following: a refractory mould base material, water glass as binder, particulate amorphous silicon dioxide and one or more powdered boron oxide compounds. The document further discloses that the addition of boron compounds to the foundry material mixture improves the humidity stability of the cores and moulds produced therefrom.

[0007] DE 10 2013 106 276 A1 discloses a casting material mixture for the production of moulds and cores for metal processing, which comprises at least one refractory mould base material, particulate amorphous SiO2, water glass and a lithium compound. The document further discloses that the addition of the lithium compound to the casting material mixture improves the humidity stability of the moulds produced therefrom.

[0008] DE 10 2012 020 509 A1 discloses a casting material mixture for the production of moulds and cores intended for metal processing, which comprises at least the following: a refractory mould base material, an inorganic binder and particulate amorphous SiO2 (which can be produced by thermal destruction of ZrSiO4 to form ZrO2 and SiO2).

[0009] DE 10 2012 020 510 A1 discloses a casting material mixture for the production of moulds and cores intended for metal processing, which comprises at least one refractory mould base material, an inorganic binder and particulate amorphous SiO2 (which can be produced by oxidation of silicon metal with an oxygen-containing gas).

[0010] DE 10 2012 020 511 A1 discloses a casting material mixture for the production of moulds and cores intended for metal processing, which comprises at least one refractory mould base material, an inorganic binder and particulate amorphous SiO2 (which can be produced by melting and rapidly re-cooling crystalline quartz).

[0011] EP 1 802 409 B1 discloses a casting material mixture for the production of moulds and cores intended for metal working, comprising at least the following: a refractory mould base material, a binder based on waterglass, which is characterised in that a portion of particulate synthetic amorphous silicon dioxide is added to the casting material mixture.

[0012] WO 2009 / 056320 A1 discloses a casting material mixture for the production of molds intended for metal working, comprising at least: a refractory mould base material; a binder based on waterglass; in which a specific proportion of particulate metal oxide selected from the group of silicon dioxide, aluminium oxide, titanium oxide and zinc oxide; and a specific proportion of at least one surface-active substance are added to the casting material mixture.

[0013] The article "Test Methods for Characterizing the Flowability of Inorganic Core Sand Mixtures - Core Production with Inorganic Binder Systems" by the authors Haanappel and Morsink, published in the specialist journal "Giesserei-Praxis", 4, 2018, p. 35-36, discloses the use of surfactants and powdered additives to improve the flowability of core sand mixtures. Summary of the Invention [Problem to be solved by the invention]

[0014] Thus, the prior art already discloses casting material mixtures containing particulate amorphous SiO2. It is also known that particulate SiO2 from ZrO2 production can be used for casting material mixtures. In addition, it is also known that particulate SiO2 formed in the quartz reduction process (e.g., with coke in an arc furnace) can be used for casting material mixtures. It is also known that the addition of lithium or boron compounds prior to the particulate substrate formulation can improve the humidity stability (moisture resistance) of castings produced therewith.

[0015] Furthermore, there is a need for casting material mixtures whose use can achieve maximum compression and therefore maximum relative casting weight (weight based on the volume of a given object of a planned geometric shape; in the case of a core, this is called the core weight). The use of cores having maximum core weight is advantageous because such casting cores result in cast parts with less chipping, excellent edge sharpening, and higher surface quality.

[0016] More specifically, there is a need for casting material mixtures that make it possible to produce castings (molds or cores) with simultaneously a high relative casting weight (core weight in the case of cores) and good humidity stability.

[0017] More specifically, there is a need for casting material mixtures which make it possible to produce castings (molds or cores) with simultaneously a high relative casting weight (core weight in the case of cores) and good humidity stability, the constituents of which contain very small amounts of lithium or boron compounds (if present), if any.

[0018] In this category, the invention relates to the use of the particulate material of the invention, the process of the invention, the mixture of the invention, the kit of the invention and the use of the mixture of the invention. The embodiments, aspects and properties described in relation to one of these categories or described as preferred are correspondingly or similarly applicable to each of the other categories and vice versa.

[0019] Unless otherwise stated, preferred aspects or embodiments of the invention, as well as their various categories, can be combined with other aspects or embodiments of the invention, as well as their various categories, in particular with other preferred aspects or embodiments. The respective preferred aspects or embodiments can also be combined with one another to in each case still result in preferred aspects or embodiments of the invention. [Means for solving the problem]

[0020] In a main aspect of the present invention, the above-mentioned objects and problems are solved by providing a method for increasing the moisture resistance of castings that can be produced by thermal hardening of a casting material mixture, comprising at least: - Refractory mould base materials with an AFS grain size index in the range of 30-100; - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - Water glass As an additive to a casting material mixture containing This is achieved and solved by the use of a particulate material comprising, as its sole constituent or as one of its multiple constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm as determined by laser scattering.

[0021] The casting material mixture associated with the present invention includes, among other components, a refractory mold base material.

[0022] The point in time of addition of the additive to another constituent in the production of the casting material mixture or of the casting material mixture provided with the additive is arbitrary and can be freely selected, for example, the additive may be added last to an otherwise completed casting material mixture or may first be premixed with one or more of the aforementioned constituents before the final mixing of one or more further constituents into the casting material mixture.

[0023] The term "particulate" preferably refers to a pourable and therefore sieveable solid powder (including particles) or granular material.

[0024] The particulate material preferably comprises, as its sole constituent or as one of its multiple constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm.

[0025] In the context of the present invention, synthetically produced particulate amorphous silicon dioxide refers to amorphous silicon dioxide that: - the target product of a chemical reaction process designed for the industrial synthesis of amorphous silicon dioxide or - A by-product of a chemical reaction process designed for the industrial synthesis of a target product other than amorphous silicon dioxide This means that.

[0026] An example of a reaction process having amorphous silicon dioxide as its target product is the flame hydrolysis of silicon tetrachloride. The amorphous SiO2 ("silicon dioxide") produced by this process is also called "calcined SiO2" ("calcined silicon dioxide") or pyrogenic silica or fumed silica (CAS RN 112945-52-5).

[0027] An example of a reaction process in which amorphous silicon dioxide is formed as a by-product is the reduction of quartz with coke, for example in an arc furnace for the production of silicon or ferrosilicon as the target product. The amorphous SiO2 ("silicon dioxide") thus produced is also called silica dust, silicon dioxide dust or SiO2 fume condensate or "silica fume" or microsilica (CAS RN 69012-64-2).

[0028] Another reaction process by which amorphous silicon dioxide can be produced synthetically is by thermal destruction of ZrSiO4 with coke, for example in an arc furnace, to obtain ZrO and SiO2.

[0029] The literature frequently refers to amorphous silicon dioxide formed by flame hydrolysis of silicon tetrachloride, for example, as a by-product during the reduction of quartz with coke in an electric arc furnace, as well as amorphous silicon dioxide formed by thermal destruction of ZrSiO4 as "calcined SiO2" ("calcined silicon dioxide") or pyrogenic silica, a term also used in connection with the present application.

[0030] In the context of the present invention, the calcined particulate amorphous silicon dioxide that is particularly preferably used in the context of the present invention includes the type of particulate amorphous silicon dioxide identified by CAS RN 69012-64-2 and CAS RN 112945-52-5.These types of calcined particulate amorphous silicon dioxide that are particularly preferably used in accordance with the present invention can be produced in a manner known per se, in particular by the reduction of quartz with carbon (e.g. coke) in an arc furnace, followed by oxidation to silicon dioxide (preferably during the production of ferrosilicon and silicon).Similarly, SiO2 produced by thermal destruction of ZrSiO4 to obtain ZrO2 from ZrSiO4, and SiO2 obtained by flame hydrolysis of silicon tetrachloride are particularly preferred.

[0031] Particulate amorphous silicon dioxide of the type produced by the reduction of quartz with carbon (e.g., coke) in an electric arc furnace (during the production of ferrosilicon and silicon) contains carbon. Particulate amorphous silicon dioxide of the type produced by the thermal destruction of ZrSiO4 contains zirconium dioxide.

[0032] Particulate amorphous silicon dioxide, which can be produced by the oxidation of silicon metal with an oxygen-containing gas, and by the quenching of molten silicon dioxide, is extremely pure SiO2 containing very few unavoidable impurities.

[0033] Most preferably, the calcined particulate amorphous silicon dioxide preferably used according to the present invention comprises particulate amorphous silicon dioxide of the type identified by CAS RN 69012-64-2. It is preferably produced by the reduction of quartz with carbon (e.g., coke) in an arc furnace (e.g., during the production of ferrosilicon and silicon) or obtained as a by-product (silica fume) during the production process of ferrosilicon and silicon. Likewise, SiO2 produced by thermal destruction of ZrSiO4 to obtain ZrO2 from ZrSiO4 is particularly preferred. These types of particulate amorphous silicon dioxide are also referred to in the art as "microsilica".

[0034] "CAS RN" means CAS Registry Number and CAS Register Number (CAS = Chemical Abstracts Service).

[0035] The use of a particulate material comprising, as its sole constituent or as one of its constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1-0.4 μm as determined by laser scattering, as an additive to a casting material mixture means that said additive is exclusively composed of particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1-0.4 μm as determined by laser scattering, or that said additive comprises other particulate or non-particulate constituents besides particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1-0.4 μm as determined by laser scattering. It is preferred if, apart from particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1-0.4 μm as determined by laser scattering, the additive does not comprise any other particulate constituent which is particulate synthetic amorphous silicon dioxide.

[0036] The median of the particle size distribution is understood to mean the value below which half of the examined particle population has a particle size smaller than that value and the other half of the examined particle population has a particle size larger than that value. This value is preferably ascertained as explained in Example 1 below.

[0037] "Determined by laser scattering" means (here and hereafter) that a sample of the particulate matter to be examined (if necessary) is pre-treated according to the method of Example 1 (see below) and then the particle size distribution of the material thus pre-treated is determined by laser scattering as in Example 1 (see below).

[0038] The mould base material is preferably a refractory mould base material. In this specification, as is commonly understood by those skilled in the art, "refractory" masses, materials and minerals refer to those that can withstand at least a short time the thermal stresses that occur during the casting or solidification of molten iron, usually cast iron. Suitable mould base materials are natural and synthetic mould base materials, such as silica sand, zircon sand or chrome ore sand, olivine, vermiculite, bauxite or fireclay.

[0039] In the context of the present invention, the mould base material preferably represents more than 80% by weight, preferably more than 90% by weight, more preferably more than 95% by weight of the total mass of the casting material mixture. The refractory mould base material is preferably in a free-flowing state. The mould base material used according to the present invention is therefore preferably and usually in granular or particulate form.

[0040] The refractory mould base material has an AFS grain size index in the range of 30 to 100. The AFS grain size index is determined here in accordance with VDG-Merkblatt (information sheet from the “Verein deutscher Giessereifachleute” [Society of German Foundry Experts]) P 34 of October 1999, point 5.2. The AFS grain size index is then calculated according to the following formula:

number

[0041] The particulate amorphous silicon dioxide that may be used, having a particle size distribution, determined by laser scattering, with a median value in the range of 0.7 to 1.5 μm, may be either of the synthetically produced type or of the naturally occurring type, the latter being known, for example, from DE 10 2007 045 649, but which is not preferred since it often contains significant amounts of crystalline constituents and is therefore classified as carcinogenic.

[0042] Water glass can be produced, for example, by dissolving vitreous sodium and potassium silicates in an autoclave or from lithium silicate during a hydrothermal process. According to the invention, it is possible to use water glass containing one, two or more of the mentioned alkali metal ions and / or containing one or even one or more polyvalent cations, for example aluminum. In the context of the present invention, the proportion of water glass in the casting material mixture is preferably in the range of 0.6% to 3% by weight.

[0043] By "enhance moisture resistance" is meant (here and hereafter) that the castings produced when using the present invention have improved moisture resistance (humidity stability) under the specified test conditions, compared to comparable castings with the same composition, geometry and production method, but not containing any synthetic amorphous silicon dioxide with a median particle size distribution in the range of 0.1-0.4 μm. See Example 4 for the determination of moisture stability (humidity resistance).

[0044] The term "thermosetting" is understood to mean that the casting material mixture is subjected to a temperature of more than 100°C, preferably between 100 and 300°C, more preferably between 120 and 250°C, in the step of hardening.

[0045] Thermal curing may also be performed or assisted by microwave irradiation.

[0046] The heat hardening can likewise be carried out or assisted by the passage of a preferably uniform and more preferably homogeneous electric current through or to the formed casting material mixture or by the application of a preferably uniform and more preferably homogeneous electromagnetic field, which preferably heats the casting material mixture uniformly and thereby hardens the mixture particularly homogeneously and ultimately to a high quality. Details are disclosed in DE 102017217098 B3 (Wolfram Bach; Michael Kaftan) and the documents cited therein.

[0047] Heating of the casting material mixture for thermosetting can be carried out, for example, in a mold having a temperature above 100° C., preferably a temperature between 100 and 300° C., more preferably a temperature between 120 and 250° C. The thermosetting is preferably carried out completely or at least partly in a customary mold for the industrial production of castings.

[0048] The casting material mixture can be cured in suitable facilities and / or using suitable devices (e.g., conduits, pumps, etc.), where the thermal curing is assisted by controlled aeration of the molded casting material mixture with ambient air at a controlled temperature. The ambient temperature is preferably heated to 100°C to 250°C, more preferably 110°C to 180°C. This ambient air contains carbon dioxide, which is not equivalent to curing by the CO2 method, which requires, inter alia, a special aeration of the casting material mixture with a CO2-rich gas in the present case, in suitable facilities and / or using suitable devices (e.g., conduits, pumps, etc.). Thus, in connection with the thermal curing considered according to or in combination with the present invention, what is preferably not carried out is the aeration of the casting material mixture with a gas containing CO2 at a high concentration relative to the concentration in air.

[0049] The flow rate and / or volume flow rate of the controlled temperature ambient air in the controlled aeration of the molded casting material mixture with controlled temperature ambient air is preferably adjusted to harden the casting material mixture within a period of time preferred, but at least suitable, for industrial applications.

[0050] The duration of the heat curing, i.e. the heating and controlled aeration of the molded casting material mixture with ambient air at a controlled temperature, may vary according to the requirements of the individual case and may depend, for example, on the size and geometric characteristics of the casting material mixture to be cured or of the casting to be cured.

[0051] In the present invention, hardening by heat curing within a period of less than 5 minutes is preferred; in particular hardening within less than 2 minutes is preferred, although longer times may be necessary for very large castings, depending on the requirements of the individual case.

[0052] The thermal hardening of the casting material mixture is carried out by chemically reacting the constituents of the casting material mixture with one another so as to obtain a mold or a core. The thermal hardening of casting material mixtures comprising solutions or dispersions containing water glass is mainly caused by the condensation of the water glass, i.e. the bonding of the silicate units of the water glass with one another.

[0053] Thermal curing of a casting material mixture does not require that the cure be complete. Thus, thermal curing of a casting material mixture also encompasses incomplete curing of the casting material mixture. This is consistent with the understanding of the term "thermal curing" by those skilled in the art, since for reasons of reaction kinetics, it cannot be expected that all reactive constituents in a generated or provided casting material mixture will react during the rather short duration of the thermal curing process. Those skilled in the art are aware of this phenomenon after curing of, for example, a casting material mixture (which has not been thermally cured).

[0054] The casting material mixture may already be hardened in the mold, but it is also possible to harden the casting material mixture first only in its edge regions so that it has sufficient strength to be removed from the mold, after which the casting material mixture can be further hardened by removing more water (e.g., in a furnace or by evaporation of water under reduced pressure or in a microwave oven).

[0055] The use of the invention is suitable for the production of all castings customary in metal casting, i.e. for example cores and moulds. It is also particularly advantageously possible to produce castings with very thin-walled sections.

[0056] The castings according to the invention which can be produced when using the invention have, inter alia, a promising combination of the property of a relatively high relative casting weight (weight based on the volume of a given object of the planned geometric shape; in the case of a core, this is called the core weight) with a high moisture resistance (humidity stability). According to in-house studies, this relatively high relative casting weight (in the case of a core, the core weight) is made possible and achieved by a positive synergistic effect on the flowability, and therefore compressibility and compaction, of the casting material mixture in the case of the combination of additives used according to the invention (as described above) together with the particulate amorphous silicon dioxide with a particle size distribution in the range of 0.7-1.5 μm, which is also present. The present invention relates to each or all of the above mentioned objects or needs, together with its various aspects (use of a particulate material comprising, as its sole constituent or one of its multiple constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm, as determined by laser scattering, together with particulate amorphous silicon dioxide having a particle size distribution in the range of 0.7 to 1.5 μm, as determined by laser scattering), which are jointly related through a common technical teaching.

[0057] The present invention also provides a process for producing a thermoset casting having improved moisture resistance, comprising: (i) Consists of at least the following: - Refractory mould base materials with an AFS grain size index in the range of 30-100; - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - Water glass preparing a casting material mixture by mixing together (ii) forming the casting material mixture; (iii) heat-curing the molded casting material mixture to obtain a casting. where The present invention also relates to a process in which the constituents of the casting material mixture are further mixed with an additive particulate material comprising, as its sole constituent or as one of its multiple constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution with a median value in the range of 0.1 to 0.4 μm as determined by laser scattering.

[0058] The details concerning the use of the invention and its features are equally applicable.

[0059] The inventive mixing of (at least) the following constituents: a refractory mould base material (having an AFS grain size index in the range of 30-100), particulate amorphous silicon dioxide (having a grain size distribution in the range of 0.7-1.5 μm as determined by laser scattering), water glass and a particulate material as an additive (comprising as its sole or one of its constituents particulate synthetic amorphous silicon dioxide having a grain size distribution in the range of 0.1-0.4 μm as determined by laser scattering) results in a casting material mixture which is subsequently further processed (step (ii)), where the presence of further constituents during the mixing step is not excluded.

[0060] The combination or order of addition of the individual constituents is arbitrary and can be freely selected.

[0061] Shaping of the casting material mixture (step (ii)) is understood to mean that the casting material mixture or a part of the casting material mixture is transformed into a definite shape. This can be achieved, for example, by introducing the casting material mixture into a mould; more preferably, this means introducing the casting material mixture into a corresponding mould by compressed air.

[0062] Casting is achieved by thermal hardening (step (iii)) of the molded casting material mixture, which has a high moisture resistance due to the presence of an additive (particulate synthetic amorphous silicon dioxide with a median particle size distribution in the range of 0.1-0.4 μm, as determined by laser scattering).

[0063] The casting material mixture comprises at least the following solid constituents: - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - a particulate material as an additive, comprising as its sole or one of several constituents particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; and forming a solid state mixture or suspension by mixing the Here, the process of the invention (as previously described, preferably as specified above as preferred) in which the produced solid state mixture or suspension is mixed with further constituents of the casting material mixture is preferred.

[0064] The particles of the described solid constituents preferably differ not only in their particle size distribution but also in at least one further chemical and / or physical property, particularly preferably in chemical composition, where the presence of one or more further constituents is not excluded, likewise resulting in a solid-state mixture according to the invention.

[0065] Depending on the requirements of the individual case, for the purposes of the present invention it is often advantageous to produce a solid-state mixture from a particulate material which comprises particulate amorphous silicon dioxide having a particle size distribution (determined by laser scattering) with a median value in the range of 0.7 to 1.5 μm and, as its only constituent or one of several constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution (determined by laser scattering) with a median value in the range of 0.1 to 0.4 μm.

[0066] The mixing of the solid-state mixture thus produced with further constituents of the casting material mixture means that the described solid-state mixture is mixed with at least the following constituents: refractory mold base material (having an AFS grain size index in the range of 30-100), particulate amorphous silicon dioxide (having a grain size distribution with a median in the range of 0.7-1.5 μm, as determined by laser scattering), and water glass, which results in the casting material mixture of the invention.

[0067] The present invention also provides at least the following solid constituents for use in the process of the invention (as described above, and preferably as specified above as preferred): - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - a particulate material as an additive, comprising as its sole or one of several constituents particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; It also relates to mixtures containing Here, the mixture is a solid-state mixture or a suspension of solid constituents in a liquid carrier medium, preferably a solid-state mixture.

[0068] The mixtures of the invention, when used in the process of the invention, contribute to increased moisture resistance of the heat set while advantageously having a high relative casting weight (core weight, in the case of cores).

[0069] The mixture of the present invention may further comprise particulate and / or liquid substances. The mixture of the present invention is preferably in the form of a suspension, i.e. a homogeneous mixture of a liquid and particles distributed therein, or a suspension of a solid-state mixture (i.e. no liquid substances are present).

[0070] Consists of at least the following: - Refractory mould base materials with an AFS grain size index in the range of 30-100; - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm; - Water glass, and - a particulate material as an additive, comprising as its sole or one of several constituents particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; Preferred is a mixture of the invention (as previously described, preferably as specified above as preferred), preferably a casting material mixture, comprising:

[0071] Such mixtures of the invention can be used by molding and subsequent thermal curing of the molded mixture to produce castings with particularly high moisture resistance. This high moisture resistance is obtained without the presence of additives / components typically used for this purpose. For example, it is known that the presence of particulate boron oxide compounds or lithium ion-containing water glasses can increase the moisture resistance of the castings. However, such substances have to be additionally introduced and often impair essential parameters of the castings and cast parts formed therefrom, such as the strength, core weight and (surface) quality of the cast parts. Therefore, the presence of such substances is often undesirable and is not necessary for the mixtures of the invention to achieve high moisture resistance. Therefore, further additives / components from the group of particulate boron oxide compounds and / or the group of lithium-containing water glasses are preferably not present in the mixtures of the invention.

[0072] In addition, in the mixture, the proportion of particulate synthetic amorphous silicon dioxide having a particle size distribution with a median in the range of 0.1 to 0.4 μm, determined by laser scattering, is less than 2% by weight, preferably more than 0.015% by weight, more preferably more than 0.02% by weight, based on the total mass of the mixture; and / or The proportion of particulate amorphous silicon dioxide having a particle size distribution with a median in the range of 0.7 to 1.5 μm, determined by laser scattering, is less than 2% by weight, preferably more than 0.015% by weight, more preferably more than 0.02% by weight, based on the total mass of the mixture; and / or the total proportion of particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.1 to 0.4 μm and particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm, is less than 2% by weight, preferably more than 0.3% by weight, based on the total mass of the mixture; and / or The total proportion of amorphous silicon dioxide is less than 2% by weight, preferably more than 0.3% by weight, based on the total mass of the mixture; Mixtures (as previously described, preferably as specified above as preferred), preferably solid state mixtures, are preferred.

[0073] Depending on the requirements of the individual case, it may be preferable to limit the proportion of amorphous silicon dioxide as described (total or having the particle size distribution defined above) in order to achieve a particularly advantageous combination of properties. Here again, the particle size distribution or the respective median of the particle size distribution is determined using laser scattering as described in Example 1.

[0074] In addition: (i) providing or producing a discrete quantity of particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; (ii) providing or producing a quantity of a particulate material comprising, as its sole constituent or as one of its constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm; (iii) mixing the amounts provided or produced in steps (i) and (ii). Preferred are mixtures, preferably casting material mixtures (as previously described, preferably as specified above as preferred), which can be produced by a process comprising:

[0075] Such a preferred (casting material) mixture of the invention therefore comprises two types of particulate amorphous silicon dioxide, which are mixed with one another.

[0076] below: a total mass of particulate amorphous silicon dioxide having a particle size distribution in the range of 0.7 to 1.5 μm as determined by laser scattering; Total mass of particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm as determined by laser scattering Preferred are mixtures (as described above, preferably as specified above as preferred) in which the ratio of is in the range of 20:1 to 1:20, preferably 5:1 to 1:20, more preferably 3:1 to 1:20, particularly preferably 2:1 to 1:20, most preferably 1.5:1 to 1:20.

[0077] Within this preferred range, the humidity stability is increased to a certain degree without significant problems with respect to core weight. Beyond this range, the effect is attenuated.

[0078] below: Particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm median, as determined by laser scattering and / or Particulate amorphous silicon dioxide with a particle size distribution in the range of 0.7 to 1.5 μm median, as determined by laser scattering But the following: - particulate synthetic amorphous silicon dioxide, which contains a proportion of silicon dioxide of at least 90% by weight, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent, preferably producible by reduction of quartz in an electric arc furnace; - particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent, preferably obtainable by thermal destruction of ZrSiO4; - Particulate synthetic amorphous silicon dioxide, which can be produced by oxidizing silicon metal with an oxygen-containing gas; - Particulate synthetic amorphous silicon dioxide, which can be produced by quenching a silicon dioxide melt; and - A mixture of them or independently selected from the group consisting of: The inventive use (as described above, preferably as specified above as preferred), the inventive process (as described above, preferably as specified above as preferred) and the inventive mixture (as described above, preferably as specified above as preferred) are each preferred.

[0079] The configurations described in the following embodiments 14, 15 and 16 are also preferred.

[0080] These species are selected from particulate amorphous silicon dioxide, and independently selected means that the two species are from different groups, or each is from the same group.Thus, the two species of particulate amorphous silicon dioxide can be selected so that they are chemically different and have different particle size distributions.Alternatively, both species may be selected so that they are the same chemical composition, but simply have different particle size distributions.

[0081] Here, the effects and advantages mentioned above in connection with the inventive use, the inventive process and the inventive mixture are achieved to a particular extent.

[0082] below: - the particulate synthetic amorphous silicon dioxide has a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm, contains a proportion of silicon dioxide of at least 90% by weight, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent, and is preferably producible by reduction of quartz in an electric arc furnace; and / or the particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, contains zirconium oxide as a secondary constituent and is preferably a particulate synthetic amorphous silicon dioxide which can be produced by thermal destruction of ZrSiO4; The inventive use (as described above, preferably as specified above as preferred), the inventive process (as described above, preferably as specified above as preferred) and the inventive mixture (as described above, preferably as specified above as preferred) are each preferred.

[0083] This means that in the inventive use (as described above, preferably as specified above as preferred), in the inventive process (as described above, preferably as specified above as preferred) and in the inventive mixture (as described above, preferably as specified above as preferred), both of the specified amorphous silicon dioxide species are selected as described, or only one species is selected as described.

[0084] Here, the effects and advantages mentioned above in connection with the inventive use, the inventive process or the inventive mixture are achieved to a certain extent.

[0085] Preferred are the uses of the invention (as described above, preferably as specified above as preferred), the processes of the invention (as described above, preferably as specified above as preferred) and the mixtures of the invention (as described above, preferably as specified above as preferred) in which one or more constituents have been added to the casting material mixture or mixtures or which are selected from the group consisting of: barium sulfate, boron oxide compounds, graphite, carbohydrates, lithium compounds, phosphorus compounds, hollow microbeads, molybdenum sulfide, platelet-shaped lubricants, surfactants, organosilicon compounds, alumina and alumina-containing compounds.

[0086] The inventive use, the inventive process or the inventive mixture, which has a high moisture resistance of the castings obtained by or which can be produced from the inventive use, the inventive process or the inventive mixture, can be combined with the advantages of the use of one or more constituents of the groups known to those skilled in the art.

[0087] Here, the effects and advantages mentioned above in connection with the inventive use, the inventive process or the inventive mixture are achieved to a certain extent.

[0088] Also: Particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm median, as determined by laser scattering and / or Particulate amorphous silicon dioxide with a particle size distribution in the range of 0.7 to 1.5 μm median, as determined by laser scattering has pozzolanic activity, Also preferred are the uses of the invention (as described above, preferably as specified above as preferred), the processes of the invention (as described above, preferably as specified above as preferred) and the mixtures of the invention (as described above, preferably as specified above as preferred).

[0089] When particulate synthetic amorphous silicon dioxide having a particle size distribution with a median in the range of 0.1 to 0.4 μm, or particulate amorphous silicon dioxide having a particle size distribution with a median in the range of 0.7 to 1.5 μm, has pozzolanic activity, they are capable of reacting with calcium hydroxide in the presence of water.

[0090] Preferably, both particulate synthetic amorphous silicon dioxide having a particle size distribution with a median in the range of 0.1 to 0.4 μm and particulate amorphous silicon dioxide having a particle size distribution with a median in the range of 0.7 to 1.5 μm have pozzolanic activity.

[0091] Preferred are the uses of the invention (as described above, preferably as specified above as preferred), the processes of the invention (as described above, preferably as specified above as preferred) and the mixtures of the invention (as described above, preferably as specified above as preferred), in which the activity of Ra226 in the foundry material mixture or mixture is less than or equal to 1 Bq / g.

[0092] The use of more highly active (casting material) mixtures is increasingly being recognized as unacceptable.

[0093] The above activity is preferably determined by gamma spectrometry according to ISO19581:2017.

[0094] At least the following: - as or in the first component of the kit, an amount of particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; - as or in a second component of the kit, a quantity of particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.1 to 0.4 μm; A kit for producing a mixture (as described above, preferably as specified above as preferred) comprising Preferred are kits in which the first and second components of the kit are spatially separated from each other.

[0095] The use of a kit according to the invention for producing a mixture according to the invention according to one of the following embodiments 4, 6, 8, 10, 12, 16, 19, 22 or 28 or for carrying out a process according to the invention according to one of the following embodiments 2, 3, 15, 18, 21 or 24 is preferred.

[0096] Here too, the effects and advantages mentioned above in connection with the inventive use, the inventive process or the inventive mixture are achieved.

[0097] The use of the mixture (as previously described, preferably as specified above as preferred) in the manufacture of moulds or cores for metalworking is preferred. The cores thus produced are subsequently used for the outer parts of moulds, preferably selected from the group consisting of metal permanent moulds (e.g. die casting moulds) and lost moulds (e.g. sand moulds).

[0098] Here too, the effects and advantages listed above in connection with the inventive uses and the inventive mixtures are achieved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0099] Preferred embodiments of the present invention will be specifically described below.

[0100] 1. Aimed at increasing the moisture resistance of castings that can be produced by thermal hardening of casting material mixtures, comprising at least: - Refractory mould base materials with an AFS grain size index in the range of 30-100; - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - Water glass As an additive to a casting material mixture containing 1. Use of a particulate material comprising, as its sole constituent or as one of several constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm.

[0101] 2. A process for producing a thermoset casting having improved moisture resistance, comprising: (i) Consists of at least the following: - Refractory mould base materials with an AFS grain size index in the range of 30-100; - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - Water glass preparing a casting material mixture by mixing together (ii) forming the casting material mixture; (iii) heat-curing the molded casting material mixture to obtain a casting. where A process in which the constituents of the casting material mixture are further mixed with an additive particulate material having as its sole or one of multiple constituents particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm as determined by laser scattering.

[0102] 3. The casting material mixture comprises at least the following solid constituents: - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - a particulate material as an additive, comprising as its sole or one of several constituents particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; and forming a solid state mixture by mixing the The process of embodiment 2, wherein the produced solid state mixture is mixed with additional constituents of the casting material mixture.

[0103] 4. A mixture for use in the process according to any of aspects 2 and 3, comprising at least the following solid constituents: - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - a particulate material as an additive, comprising as its sole or one of several constituents particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; Including, The mixture herein is a solid state mixture or a suspension of solid constituents in a liquid carrier medium, preferably a casting material mixture.

[0104] 5. The following: (i) producing or providing particulate amorphous silicon dioxide, either as a pure substance or as a component of a solid state mixture or as a component of a suspension of solid components in a liquid carrier medium, having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; and separately (ii) producing or providing a particulate material comprising, as its sole constituent or as one of a plurality of constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm, either as a pure substance or as a constituent of a solid state mixture or as a constituent of a suspension of solid constituents in a liquid carrier medium, followed by (iii) mixing the substances produced or provided in steps (i) and (ii) (each independently a pure substance, a solid state mixture, or a suspension). 5. A process for producing the mixture of claim 4, comprising:

[0105] 6. Consists of at least the following: - Refractory mould base materials with an AFS grain size index in the range of 30-100; - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm; - Water glass, and - a particulate material as an additive, comprising as its sole or one of several constituents particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; 5. The mixture according to embodiment 4, preferably a casting material mixture for producing a casting, comprising:

[0106] 7. Below: (i) producing or (preferably) providing particulate amorphous silicon dioxide, either as a pure substance or as a component of a solid state mixture or as a component of a suspension of the solid components in a liquid carrier medium, having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; (ii) producing or (preferably) preparing a particulate material comprising, as its sole constituent or as one of several constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm, either as a pure substance or as a constituent of a solid state mixture or as a constituent of a suspension of solid constituents in a liquid carrier medium; (iii) producing or (preferably) providing a refractory mould base material having an AFS grain size index in the range of 30 to 100; (iv) producing or (preferably) providing water glass; (v) mixing the substances produced or prepared in steps (i) to (iv) (preferably, the substances produced or prepared in steps (i) and (ii) are first mixed with each other, and then the resulting premix is ​​mixed with a further substance). 7. A process for producing the mixture of embodiment 6, comprising:

[0107] 8. In the mixture, the proportion of particulate synthetic amorphous silicon dioxide having a particle size distribution with a median in the range of 0.1 to 0.4 μm, determined by laser scattering, is less than 2% by weight, preferably more than 0.015% by weight, more preferably more than 0.02% by weight, based on the total mass of the mixture; and / or The proportion of particulate amorphous silicon dioxide having a particle size distribution with a median in the range of 0.7 to 1.5 μm, determined by laser scattering, is less than 2% by weight, preferably more than 0.015% by weight, more preferably more than 0.02% by weight, based on the total mass of the mixture; and / or the total proportion of particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.1 to 0.4 μm and particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm, is less than 2% by weight, preferably more than 0.3% by weight, based on the total mass of the mixture; and / or The total proportion of amorphous silicon dioxide is less than 2% by weight, preferably more than 0.3% by weight, based on the total mass of the mixture; 7. A mixture, preferably a casting material mixture, according to embodiment 6.

[0108] 9. Below: (i) producing or providing, as a component of a solid state mixture or as a component of a suspension of the solid component in a liquid carrier medium, particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; (ii) producing or providing, as a component of a solid state mixture or as a component of a suspension of the solid components in a liquid carrier medium, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm; (iii) producing or providing a further liquid or particulate substance or mixture of substances; (iv) mixing the constituents produced or prepared in steps (i) to (iii) in corresponding amounts (see embodiment 6); 9. A process for producing the mixture of embodiment 8, comprising:

[0109] 10. The following: (i) providing or producing a discrete quantity of particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; (ii) providing or producing a quantity of a particulate material having, as its only constituent or as one of its constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm; (iii) mixing the amounts provided or produced in steps (i) and (ii), preferably producible by a process according to any of aspects 5, 7 and 9. 9. The mixture, preferably a casting material mixture, of any of the preceding aspects 4, 6 and 8, producible by a process comprising:

[0110] 11. The following: (i) providing or producing a discrete quantity of particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; (ii) providing or producing a quantity of a particulate material having, as its only constituent or as one of its constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm; (iii) mixing the amounts provided or produced in steps (i) and (ii). 11. A process for producing the mixture of any of embodiments 4, 6, 8 or 10, comprising:

[0111] 12. The following: a total mass of particulate amorphous silicon dioxide having a particle size distribution in the range of 0.7 to 1.5 μm as determined by laser scattering; Total mass of particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm as determined by laser scattering In the mixture according to any one of aspects 4, 6, 8 or 10, the ratio of is in the range of 20:1 to 1:20, preferably in the range of 5:1 to 1:20, more preferably in the range of 3:1 to 1:20, particularly preferably in the range of 2:1 to 1:20, and most preferably in the range of 1.5:1 to 1:20.

[0112] 13. The following: (i) providing or producing, as a constituent of a solid state mixture or as a constituent of a suspension of solid constituents in a liquid carrier medium, a quantity of particulate material comprising, as its sole constituent or as one of a plurality of constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm; (ii) providing or producing, as a component of a solid state mixture or as a component of a suspension of the solid component in a liquid carrier medium, a discrete quantity of particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; (iii) mixing the amounts of substances produced or provided in steps (i) and (ii), such that the amounts of said substances in the resulting mixture are: - a total mass of particulate amorphous silicon dioxide having a particle size distribution in the range of 0.7 to 1.5 μm, determined by laser scattering; - total mass of particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm as determined by laser scattering; is in the range of 20:1 to 1:20, preferably 5:1 to 1:20, more preferably 3:1 to 1:20, particularly preferably 2:1 to 1:20, and most preferably 1.5:1 to 1:20. 11. A process for producing the mixture of any of embodiments 4, 6, 8 or 10, comprising:

[0113] 14. Particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm, as determined by laser scattering. and / or Particulate amorphous silicon dioxide with a particle size distribution in the range of 0.7 to 1.5 μm median, as determined by laser scattering But the following: - particulate synthetic amorphous silicon dioxide, preferably produced by reduction of quartz in an electric arc furnace (in this case typically obtained as a by-product), which contains a proportion of silicon dioxide of at least 90% by weight, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent; - particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent, preferably produced by thermal destruction of ZrSiO4; - Particulate synthetic amorphous silicon dioxide produced by oxidizing silicon metal with an oxygen-containing gas; - Particulate synthetic amorphous silicon dioxide produced by quenching a silicon dioxide melt; and - A mixture of them 2. The use according to embodiment 1, wherein said compound is selected from the group consisting of:

[0114] 15. Particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm, as determined by laser scattering. and / or Particulate amorphous silicon dioxide with a particle size distribution in the range of 0.7 to 1.5 μm median, as determined by laser scattering But the following: - particulate synthetic amorphous silicon dioxide, which contains at least 90% by weight of silicon dioxide, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent, and which is preferably produced by reduction of quartz in an electric arc furnace; - particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent, preferably produced by thermal destruction of ZrSiO4; - Particulate synthetic amorphous silicon dioxide produced by oxidizing silicon metal with an oxygen-containing gas; - Particulate synthetic amorphous silicon dioxide produced by quenching a silicon dioxide melt; and - A mixture of them 4. The process according to any of aspects 2 and 3, wherein said first and second nucleotide sequences are selected from the group consisting of:

[0115] 16. Particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm, as determined by laser scattering. and / or Particulate amorphous silicon dioxide with a particle size distribution in the range of 0.7 to 1.5 μm median, as determined by laser scattering But the following: - particulate synthetic amorphous silicon dioxide, which contains at least 90% by weight of silicon dioxide, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent, and which can be obtained preferably by reduction of quartz in an electric arc furnace; - particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent, preferably obtainable by thermal destruction of ZrSiO4; - Particulate synthetic amorphous silicon dioxide, which can be produced by oxidizing silicon metal with an oxygen-containing gas; - Particulate synthetic amorphous silicon dioxide, which can be produced by quenching a silicon dioxide melt; and - A mixture of them 13. The mixture according to any of aspects 4, 6, 8, 10 or 12, wherein said mixture is selected, or independently selected, from the group consisting of:

[0116] 17. - A particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1-0.4 μm, containing at least 90% by weight of silicon dioxide, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent, and is preferably produced by reduction of quartz in an electric arc furnace; and / or 15. The process of any of aspects 1 or 14, wherein the particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm contains zirconium oxide as a secondary constituent and is preferably a particulate synthetic amorphous silicon dioxide produced by thermal destruction of ZrSiO4.

[0117] 18. - A particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1-0.4 μm, containing at least 90% by weight of silicon dioxide, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent, and is preferably produced by reduction of quartz in an electric arc furnace; and / or The process of any of aspects 2, 3 or 15, wherein the particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm contains zirconium oxide as a secondary constituent, and is preferably a particulate synthetic amorphous silicon dioxide produced by thermal destruction of ZrSiO4.

[0118] 19. - A particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm, contains a proportion of silicon dioxide of at least 90% by weight, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent, and can be produced by reduction of quartz, preferably in an electric arc furnace; and / or 17. The mixture according to any of embodiments 4, 6, 8, 10, 12 or 16, wherein the particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm, contains zirconium oxide as a secondary constituent and is preferably a particulate synthetic amorphous silicon dioxide which can be produced by thermal destruction of ZrSiO4.

[0119] 20. The use of any of aspects 1, 14 or 17, wherein one or more constituents are added to the casting material mixture and are selected from the group consisting of: barium sulfate, boron oxide compounds, graphite, carbohydrates, lithium compounds, phosphorus compounds, hollow microbeads, molybdenum sulfide, platelet-shaped lubricants, surfactants, organosilicon compounds, alumina and alumina-containing compounds.

[0120] 21. The process of any of aspects 2, 3, 15, or 18, wherein one or more constituents are added to the casting material mixture and are selected from the group consisting of barium sulfate, boron oxide compounds, graphite, carbohydrates, lithium compounds, phosphorus compounds, hollow microbeads, molybdenum sulfide, platelet shaped lubricants, surfactants, organosilicon compounds, alumina, and alumina-containing compounds.

[0121] 22. The mixture of any of aspects 4, 6, 8, 10, 12, 16, or 19, wherein one or more constituents are added to the casting material mixture and are selected from the group consisting of barium sulfate, boron oxide compounds, graphite, carbohydrates, lithium compounds, phosphorus compounds, hollow microbeads, molybdenum sulfide, platelet-shaped lubricants, surfactants, organosilicon compounds, alumina, and alumina-containing compounds.

[0122] 23. Particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm as determined by laser scattering. and / or Particulate amorphous silicon dioxide with a particle size distribution in the range of 0.7 to 1.5 μm median, as determined by laser scattering 21. The process of any one of embodiments 1, 14, 17, or 20, wherein said process has pozzolanic activity.

[0123] twenty four. Particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm median, as determined by laser scattering and / or Particulate amorphous silicon dioxide with a particle size distribution in the range of 0.7 to 1.5 μm median, as determined by laser scattering 22. The mixture of any one of aspects 2, 3, 15, 18 or 21, wherein said mixture has pozzolanic activity.

[0124] 25. Particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm, as determined by laser scattering. and / or Particulate amorphous silicon dioxide with a particle size distribution in the range of 0.7 to 1.5 μm median, as determined by laser scattering 23. The mixture of any of aspects 4, 6, 8, 10, 12, 16, 19, or 22, wherein said mixture has pozzolanic activity.

[0125] 26. The use according to any one of aspects 1, 14, 17, 20 or 23, wherein the activity of Ra226 in the foundry material mixture is 1 Bq / g or less.

[0126] 27. The process of any one of aspects 2, 3, 15, 18, or 21, wherein the activity of Ra226 in the casting material mixture is less than or equal to 1 Bq / g.

[0127] 28. The mixture of any of the preceding embodiments 4, 6, 8, 10, 12, 16, 19, or 22, wherein the activity of Ra226 in the mixture is 1 Bq / g or less.

[0128] 29. A kit for producing a mixture according to any of the preceding aspects 4, 6, 8, 10, 12, 16, 19, 22 or 28, or for carrying out a process according to any of aspects 2, 3, 15, 18, 21 or 24, comprising: At least the following: - as or in the first component of the kit, an amount of particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; - as or in a second component of the kit, a quantity of particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.1 to 0.4 μm; Including, A kit, wherein the first and second components of the kit are spatially separated from each other.

[0129] 30. Use of a mixture according to any of the preceding aspects 4, 6, 8, 10, 12, 16, 19, 22 or 29 in the manufacture of moulds or cores for metalworking, wherein the produced cores are preferably used for the outer parts of moulds selected from the group consisting of metal permanent moulds (e.g. die casting moulds) and lost moulds (e.g. sand moulds).

[0130] below: - Particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm, as determined by laser scattering and - Particulate amorphous silicon dioxide having a particle size distribution in the range of 0.7 to 1.5 μm, as determined by laser scattering but have different chemical compositions; The uses, mixtures and processes according to the invention are preferred. [Brief description of the drawings]

[0131] [Figure 1] 3 shows the results of the determination of the core weight of the test bars (see Example 3) and the results of the determination of the moisture resistance of the test bars (Example 4). The X-axis shows the percentage of the granulated RW filler in the total amount of granulated RW filler and RW filler Q1 Plus in the casting material mixture. The Y-axis shows the core weight (grams) determined according to Example 3. The Z-axis shows the moisture resistance (%) determined according to Example 4. The black circles show the measured values ​​of the core weight of the test bars, which have been confirmed experimentally (according to Example 3). The dashed and dotted lines show the progression of the measurement points in a schematic way. The dashed lines show the linear correlation expected by the skilled person between the percentage of the granulated RW filler in the total amount of granulated RW filler and RW filler Q1 Plus in the casting material mixture and the core weight (linear combination based on the values ​​of the pure materials). The crosses show the measured values ​​of the moisture resistance of the test bars, which have been confirmed experimentally (according to Example 4). The solid lines show the progression of the measurement points in a schematic way. The dashed line shows the linear correlation (linear combination based on the values ​​of the pure materials) expected by a person skilled in the art between the proportion of granulated RW filler in the total amount of granulated RW filler and RW filler Q1 Plus in the casting material mixture and moisture resistance. [Diagram 2]The results of the determination of the core weight of the test bars (made from mixtures 1.1, 1.2 and 1.3, see Table 5, Example 6) and the results of the determination of the residual strength after 3 hours of the test bars (made from mixtures 1.1, 1.2 and 1.3, see Table 5, Example 6) are shown. The X-axis here and in Figures 3, 4 and 5 shows the proportion (%) of the RW filler Q1 Plus in the total mass of Elkem Microsilica® 971 and the RW filler Q1 Plus in the casting material mixture. The Y-axis here and in Figures 3, 4 and 5 shows the core weight (g) determined according to item 6.5 of Example 6. The Z-axis here and in Figures 3, 4 and 5 shows the residual strength (%) after 3 hours determined according to item 6.7 of Example 6. The filled circles here and in Figures 3, 4 and 5 show the measured values ​​of the core weight of the test bars, which were confirmed by experiment (according to Example 6). The dashed lines show here and in Figures 3, 4 and 5 the linear correlation expected by a person skilled in the art between the percentage of RW filler Q1 Plus in the total mass of Elkem Microsilica® 971 and RW filler Q1 Plus in the casting material mixture and the core weight (linear combination based on the values ​​of the pure materials). The cross symbols show here and in Figures 3, 4 and 5 the experimentally confirmed (according to Example 6) residual strength values ​​after 3 hours. The dashed lines show here and in Figures 3, 4 and 5 the linear correlation expected by a person skilled in the art between the percentage of RW filler Q1 Plus in the total mass of Elkem Microsilica® 971 and RW filler Q1 Plus in the casting material mixture and the moisture resistance (linear combination based on the values ​​of the pure materials). [Diagram 3] The results of the determination of the core weight of the test bars (made from mixtures 2.1, 2.2 and 2.3, see Table 5, Example 6) and the determination of the residual strength after 3 hours of the test bars (made from mixtures 2.1, 2.2 and 2.3, see Table 5, Example 6) are shown. [Figure 4]The results of the determination of the core weight of the test bars (made from mixtures 3.1, 3.2 and 3.3, see Table 5, Example 6) and the determination of the residual strength after 3 hours of the test bars (made from mixtures 3.1, 3.2 and 3.3, see Table 5, Example 6) are shown. [Diagram 5] The results of the determination of the core weight of the test bars (made from mixtures 4.1, 4.2 and 4.3, see Table 5, Example 6) and the determination of the residual strength after 3 hours of the test bars (made from mixtures 4.1, 4.2 and 4.3, see Table 5, Example 6) are shown. [Figure 6] 5 shows the results of the determination of the core weight of the test bars (made from mixtures 5.1, 5.2 and 5.3, see Table 5, Example 6). The X-axis shows the percentage of granulated RW filler in the total mass of Elkem Microsilica® 971 and granulated RW filler in the foundry material mixture. The Y-axis shows the core weight (g) determined according to item 6.5 of Example 6. The filled circles show the measured values ​​of the core weight of the test bars, which were confirmed by experiment (according to Example 6). The dashed line shows the linear correlation (linear combination based on the values ​​of the pure materials) expected by a person skilled in the art between the percentage of granulated RW filler in the total mass of Elkem Microsilica® 971 and granulated RW filler in the foundry material mixture and the core weight. EXAMPLES

[0132] Example 1 - Determination of particle size distribution by laser scattering The choice of materials in this example is merely exemplary, and laser scattering according to the procedures of this example can also be used to determine the particle size distribution or median value of other particulate silicon dioxide species used in accordance with the present invention.

[0133] 1.1 Sample preparation: As an example, silica fume particles (CAS number: 65012-64-2), which are commercially available (RW Silicium GmbH) and have the granular powder form from the Si production, granulated RW filler ["RW-Fueller gesiebt"], and the granular powder form from the ZrO2 production, RW filler Q1 Plus ["RW-Fueller Q1 plus"], were experimentally determined using laser scattering.

[0134] In each case, about a teaspoon of granular amorphous silicon dioxide was mixed with about 100 mL of demineralized water, and the resulting mixture was stirred for 30 seconds with a magnetic stirrer (IKAMAG RET) at a stirrer speed of 500 revolutions per minute. The samples were then sonicated with an ultrasonic probe (Hielscher; model: UP200HT) equipped with an S26d7 sonotrode (Hielscher) pre-adjusted to 100% amplitude, which was immersed in the sample. The sonication was continuous (not pulsed). For the silica fume particles examined from the Si production, i.e., the granulated RW filler, and for the silica fume particles from the ZrO2 production, i.e., the RW filler Q1 Plus, optimal sonication times of 300 seconds (for the granulated RW filler) or 240 seconds (RW filler Q1 Plus) were selected, which had been previously confirmed as described in Example 1, item 1.3.

[0135] 1.2 Laser scattering measurements: The measurements were carried out using a Horiba LA-960 instrument (hereafter LA-960). For the measurements, the circulation speed was set to 6, the stirrer speed to 8, the data recording of the sample to 30,000, the convergence factor to 15, the distribution mode to volume, the refractive index (R) to 1.50-0.01i (1.33 in the case of demineralized water dispersion medium), and the refractive index (B) to 1.50-0.01i (1.33 in the case of demineralized water dispersion medium). The laser scattering measurements were carried out at room temperature (20°C-25°C).

[0136] The measurement chamber of the LA-960 was filled with demineralized water up to about three-quarters full (maximum filling level). The agitator was then started at the set speed and the circulation was switched on to degas the water. A zero measurement was then performed using the specified parameters.

[0137] Next, a disposable pipette was used to take a 0.5-3.0 mL sample from the center of the sample prepared according to item 1.1 of Example 1 immediately after sonication. The entire contents of the pipette were then introduced into the measurement chamber such that the transmittance of the red laser was 80%-90% and the transmittance of the blue laser was 70%-90%. Afterwards, the measurement was started. The measured values ​​were automatically evaluated based on the specified parameters.

[0138] For silica fume particles (sized RW filler) examined from the Si production, the particle size distribution was determined to have a median of 0.23 micrometers, rounded to three decimal places.

[0139] For silica fume particles (sized RW filler Q1 Plus) examined from the ZrO2 production, the particle size distribution was determined to have a median of 0.84 micrometers, rounded to three decimal places.

[0140] 1.3 Determination of optimal sonication time: The optimal sonication time, which varies depending on the type of sample, was confirmed by carrying out a series of measurements with different sonication times for various types of particulate silicon dioxide.This was carried out by starting with 10 seconds, extending by 10 seconds for each additional sample, and measuring the particle size distribution of each immediately after the end of sonication using laser scattering (LA-960) as described in item 1.2 of example 1.As the time of sonication is increased, the median value observed in the particle size distribution first falls, and then finally rises again at longer sonication times.For the sonication described in item 1.1 of example 1, the sonication time selected is the time when the lowest median value of the particle size distribution is determined for each particle type in these series of measurements; this sonication time is the "optimal" sonication time.

[0141] Example 2 - Preparation of test bars This example describes the manufacture of test bars (castings) by way of example; the dimensions of the test bars are merely exemplary and the choice of materials used is merely illustrative of the different materials that may be used in accordance with the present invention.

[0142] 2.1 Production of the casting mixture For the purposes of this example, RW filler (having a particle size distribution with a median of 0.23 micrometers, determined by laser scattering, rounded to three decimal places; as an example of a particulate synthetic amorphous silicon dioxide with a particle size distribution with a median in the range of 0.1 to 0.4 μm, determined by laser scattering) and Q1 Plus (having a particle size distribution with a median of 0.84 micrometers, determined by laser scattering, rounded to three decimal places; as an example of a particulate amorphous silicon dioxide with a particle size distribution with a median in the range of 0.7 to 1.5 μm, determined by laser scattering) were mixed together in dry form; the amounts added are evident from Table 1. The powder mixture obtained from the sized RW filler and the RW filler Q1 Plus was mixed by hand with H31 sand (quartz sand; manufactured by Quarzwerke GmbH, AFS particle size index 46).

[0143] A liquid binder based on water glass having a solids content of 36.2% by weight, a molar coefficient of about 2.1 and a Na2O:K2O ratio (molar) of about 7.7, containing 2.0% by weight of HOESCH EHS 40 (from Hoesch; ethylhexyl sulfate, active ingredient content 40.0% to 44.0%; CAS number 126-92-1) was then added and all the constituents were mixed together using a Bull mixer (model: RN 10 / 20, from Morek Multiserver) at 220 revolutions per minute for 120 seconds.

[0144] By way of example, non-invention and invention mixtures were prepared using the weight proportions of the components used as specified in Table 1.

[0145] [Table 1]

[0146] 2.2 Test bar production The casting material mixtures produced according to item 2.1 of Example 2 were molded into test bars with dimensions of 22.4 mm x 22.4 mm x 185 mm. For this purpose, the respective casting material mixtures were introduced into a mold for test bars at a temperature of 180° C. using compressed air (4 bar) and an injection time of 3 seconds. The test bars were subsequently heat-cured at 180° C. for 30 seconds while being further aerated with heated ambient air at an aeration pressure of 2 bar and an aeration and aeration hose temperature of 180° C. The mold was then opened and the hardened test bars were removed, stored and allowed to cool.

[0147] Example 3 - Determination of Core Weight This example describes, by way of example only, the determination of core weight for a test bar (casting).

[0148] Test bars made according to Example 2 using mix numbers 1, 2, 3, 5, 7, 9, 11, 12, 13 after a cooling time of about 1 hour were weighed on an electronic laboratory balance. The results are shown in Table 2, where each value of the core weight corresponds to the average value from nine individual measurements. The mix numbers in Table 2 correspond to the mix numbers in Table 1, so that in this respect the same mix numbers refer to casting material mixes of the same composition.

[0149] [Table 2]

[0150] Example 4 - Determination of moisture resistance This example describes, purely by way of example, the determination of the moisture resistance (humidity stability) of test bars (castings).

[0151] 4.1 Determination of 1-hour intensity The test bars (mixtures no. 1, 3, 4, 5, 6, 7, 8, 9, 10, 11, 13) produced according to Example 2 were introduced, after a cooling time of about 1 hour, into a Georg Fischer strength testing apparatus equipped with a three-point bending apparatus (manufactured by Morek Multiserw) and the force at which the test bars broke was measured. The readings (N / cm 2 ) was the 1-hour intensity.

[0152] 4.2 Determination of absolute residual strength after 22 hours in a temperature and humidity controlled cabinet The test bars produced according to example 2 (mixture number according to example 4.1) were, after a cooling time of 1 hour, stored for 22 hours under controlled conditions of 30° C. and 75% relative humidity in a temperature and humidity controlled cabinet (VC 0034, from Voetsch).

[0153] The absolute residual strength was then determined by introducing each test bar into a Georg Fischer strength testing apparatus equipped with a three-point bending fixture (Morek Multiserw) and measuring the force that caused the test bar to break. Readings (N / cm 2) indicates the absolute residual strength. For cores that were already broken before 22 hours, 0 N / cm 2 An absolute residual strength of was assumed.

[0154] 4.3 Determination of moisture resistance To determine the moisture resistance for each mix number, the sum of six measurements of absolute residual strength (Example 4.2) was averaged and divided by the average of three measurements of 1-hour strength (Example 4.1). The value thus obtained was multiplied by 100%; the result is the moisture resistance. The moisture resistance values ​​thus determined are reported in Table 3. The mix numbers in Table 3 correspond to those in Table 1, so that the same mix number refers to a casting material mix of the same composition.

[0155] [Table 3]

[0156] Example 5 - Synergy The results from Example 3, Table 2, and Example 4, Table 3 are summarized below in Table 4. Table 4 is accompanied by a diagram in Figure 1 which was generated from this table.

[0157] [Table 4]

[0158] From Table 4 and the accompanying Figure 1 it is generally clear that advantageous values ​​for the ratio of the total mass of particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm, i.e. material RW filler Q1 Plus (having a particle size distribution with a median of 0.84 μm rounded to three decimal places), to the total mass of particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.1 to 0.4 μm, i.e. granulated RW filler (having a particle size distribution with a median of 0.23 μm rounded to three decimal places, determined by laser scattering), are in the range of 20:1 to 1:20. This is because within this range there is a significant double synergy, which is manifested in an unexpectedly high (synergistically increased) moisture resistance and at the same time an unexpectedly high (synergistically increased) relative casting weight (in this case the core weight) (each measured value being higher than the predicted value). Preferably, these values ​​are in the range of 5:1 to 1:20, more preferably 3:1 to 1:20, particularly preferably 2:1 to 1:20, most preferably 1.5:1 to 1:20. It is therefore particularly preferred that the proportion of particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm, determined by laser scattering (in this example this is a sized RW filler having a particle size distribution with a median of 0.23 μm, rounded to three decimal places), based on the total mass of the two types used, is at least 40% by weight.

[0159] The corresponding castings therefore ensure, firstly, high storage stability (in particular stability against the action of moisture) and, secondly, a high degree of compaction of the formed casting material mixture, which results in a high-quality surface that is almost free of defects in the thermoset castings obtained therefrom, which in turn achieves a high-quality surface that is almost free of defects in the metal casting parts produced by the method of the invention, which are in contact with the thermoset castings during the casting process.

[0160] Example 6 - Comparative Study: 6.1 General guidelines for understanding the test This example concerns comparative testing on a total of 15 different casting material mixtures, as exemplified in Table 5. More specifically, the inventive experiments were compared with non-inventive experiments carried out according to WO 2009 / 056320 A1.

[0161] Tests according to the invention were carried out with the casting material mixtures 1.3, 2.3, 3.3 and 4.3 shown in Table 5. All other casting material mixtures were not according to the invention.

[0162] In all the casting material mixtures examined, the same silica sand and the same alkali metal water glass were used in each case in the same amounts; see Table 5 and the accompanying footnote 1 for details of the alkali metal water glass composition.

[0163] The particulate synthetic amorphous silicon dioxide having a particle size distribution with a median value ranging from 0.1 to 0.4 μm, as determined by laser scattering, used in all ten casting material mixtures 1.1, 1.3, 2.1, 2.3, 3.1, 3.3, 4.1, 4.3, 5.1 and 5.3 was Elkem Microsilica® 971 U. As noted in footnote 5 for Table 5, the median value of the particle size distribution (rounded to three decimal places) was 0.20 μm according to the method from Example 1. The optimal sonication time identified (see item 1.3 in Example 1) was 1020 seconds.

[0164] In all eight casting material mixtures 1.2, 1.3, 2.2, 2.3, 3.2, 3.3, 4.2, and 4.3, the particulate amorphous silicon dioxide used was RW filler Q1 Plus, having a particle size distribution with a median in the range of 0.7 to 1.5 μm, as determined by laser scattering; according to example 1.2, this material had a particle size distribution with a median of 0.84 micrometers, rounded to the nearest tenth.

[0165] In the two casting material mixtures 5.2 and 5.3 (in the casting material mixture 5.3, in addition to Elkem Microsilica® 971 U), the particulate synthetic amorphous silicon dioxide used was a granular RW filler, having a particle size distribution with a median in the range of 0.1 to 0.4 μm, as determined by laser scattering; according to example 1.2, this material had a particle size distribution with a median of 0.23 micrometers, rounded to three decimal places.

[0166] No surfactant was used in casting material mixtures 1.1-1.3; a total of three different surfactants, all in the same amounts, were used in further casting material mixtures. See footnotes 2, 3, and 4 in Table 5 for surfactant material details.

[0167] Tests were carried out on five groups of casting material mixtures (1.1-1.3, 2.1-2.3, 3.1-3.3, 4.1-4.3 and 5.1-5.3): - The first test in each group (casting material mixtures 1.1, 2.1, 3.1, 4.1, 5.1) concerns in each case casting material mixtures which contain only Elkem Microsilica® 971 U as the only particulate synthetic amorphous silicon dioxide. - the second test in each group concerned foundry material mixes which in each case did not contain Elkem Microsilica® 971 U and contained either the RW filler Q1 Plus (foundry material mixes 1.2, 2.2, 3.2, 4.2) or a granulated RW filler (foundry material mix 5.2) as the only particulate synthetic amorphous silicon dioxide. - the third test in each group concerns in each case foundry material mixes which, in addition to Elkem Microsilica® 971 U, contain either the RW filler Q1 Plus (foundry material mixes 1.3, 2.3, 3.3, 4.3) or a granulated RW filler (foundry material mix 5.3).

[0168] In the casting material mixtures 1.3, 2.3, 3.3 and 4.3, in each case two types of particulate synthetic amorphous silicon dioxide were used, one of which (Elkem Microsilica® 971 U) had a particle size distribution in the range of 0.1-0.4 μm as determined by laser scattering, and the other (RW filler Q1 Plus) had a particle size distribution in the range of 0.7-1.5 μm as determined by laser scattering.

[0169] In casting material mix 5.3, two particulate synthetic amorphous silicon dioxides were used, each of which had a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm.

[0170] 6.2 Production of the casting mixture For the preparation of the foundry material mixtures detailed in Table 5, the alkali metal water glass and any surfactant (surface-active substance) were added to the initially packed H32 silica sand. The mixture was stirred for 1 minute at 200 revolutions per minute using a Bull mixer (model: RN 10 / 20, manufactured by Morek Multiserw). Granular amorphous silicon dioxide was then added and the resulting mixture was stirred for another minute with the Bull mixer.

[0171] [Table 5]

[0172] 6.3 Test bar production The casting material mixtures of the respective compositions specified in table 5, produced according to item 6.2, were molded into test bars with dimensions of 22.4 mm x 22.4 mm x 185 mm. For this purpose, the respective casting material mixtures were introduced by compressed air (2 bar) into a mold for test bars at a temperature of 180°C and were kept in the mold for a further 50 seconds. In order to accelerate the hardening of the mixture, hot air (3 bar, 150°C) was passed through the mold for the last 20 seconds. The mold was then opened and the test bars (22.4 mm x 22.4 mm x 185 mm) were taken out.

[0173] The test bars were used for the tests according to the following items 6.4 to 6.7; non-inventive test bars based on the group of casting material mixtures 5.1 to 5.3 were used only for the test according to 6.5 (determination of the core weight).

[0174] 6.4 Determination of heat resistance Immediately after removal from the mould, the test bars produced according to item 6.3 were introduced into a Georg Fischer strength testing machine equipped with a three-point bending apparatus (manufactured by Morek Multiserw). 10 seconds after the mould was opened, the force at which the test bars broke was measured. The readings (N / cm 2 ) indicates high temperature strength. Table 6 shows the results of the high temperature strength measurements; the reported values ​​are in each case the median from three measurements.

[0175] 6.5 Determination of core weight After a cooling time of approximately 1 hour, the test bars produced according to section 6.3 were weighed on a laboratory electronic balance. The results are shown in Table 6, where each core weight value corresponds to the median value from nine individual measurements.

[0176] 6.6 Determination of 1-hour intensity The test bars manufactured according to item 6.3, after removal from the mould, were placed horizontally on a frame so that they were located on the frame only in the region of both ends of their entire length and the test bars extended over a section of about 16 cm without the contact surfaces touching each other. After a cooling time of 1 hour after removal from the mould, the test bars were introduced into a Georg Fischer strength testing machine equipped with a three-point bending apparatus (manufactured by Morek Multiserw) and the force causing the breakage of the test bars was measured. The readings (N / cm 2 ) indicates 1 hour strength. The results are shown in Table 6, where the reported values ​​are in each case the median from three measurements.

[0177] 6.7 Determination of residual strength after 3 hours and relative residual strength after 3 hours After removal from the mould, the test bars produced according to section 6.3 were allowed to cool for 1 hour under ambient laboratory conditions as described in section 6.6, then mounted on the same frame and stored in a temperature and humidity controlled cabinet (VC 0034, Voetsch) under controlled conditions of 30° C. and 75% relative humidity for three hours (3h).

[0178] Each test bar was then placed in a Georg Fischer strength testing apparatus equipped with a three-point bending fixture (Morek Multiserw) and the (absolute) residual strength after 3 hours was determined by measuring the force that caused the test bar to break. The readings (N / cm 2 ) indicates the (absolute) residual strength after 3 hours. For cores that have already broken before 3 hours have elapsed, 0 N / cm 2 The absolute residual strengths of the samples were reported. The results are shown in Table 6, where the reported values ​​are in each case the median values ​​from three measurements.

[0179] For the determination of the relative residual strength after 3 hours, each absolute residual strength value after 3 hours was divided by the corresponding value of the 1 hour strength. The values ​​thus obtained were multiplied by 100%; the respective result is the relative residual strength after 3 hours. The results are reported in Table 6.

[0180] 6.8 Results: Selected results of measurements from 6.4-6.7 are shown in Figures 2-6 (see above description of figures). Additionally, the results of all measurements from 6.4-6.7 are summarized in Table 6; for clarity, the measurements in the table have been rounded to two decimal places. The numbers of the casting material mixtures shown in Table 6 correspond to those in Table 5.

[0181] [Table 6]

[0182] From table 6 and from figures 2 to 5, which correspond to the groups of three casting material mixtures (1.1-1.3 to 4.1-4.3), it is clear that in both cases, Elkem Microsilica® 971 U (particulate amorphous silicon dioxide having a particle size distribution with a median of 0.20 micrometers, i.e. in the range of 0.1-0.4 μm, as determined by laser scattering) in combination with the RW filler Q1 Plus (particulate amorphous silicon dioxide having a particle size distribution with a median of 0.84 micrometers, i.e. in the range of 0.7-1.5 μm, as determined by laser scattering), the core weights of the test bars produced are surprisingly high, i.e. higher than the linear combination of the values ​​of the test bars containing Elkem Microsilica® 971 U alone or the RW filler Q1 Plus alone (in each case the linear combination shown by the dashed line).

[0183] In both cases, a significant double synergistic effect was observed, manifested in unexpectedly high (synergistically enhanced) relative cast object weights (core weights) and at the same time unexpectedly high (synergistically enhanced) relative residual strengths after 3 hours.

[0184] From table 6 and from figure 6 corresponding to the group of three casting material mixtures 5.1 to 5.3, it is clear that for casting material mixture 5.3, i.e. in the case of the combination of Elkem Microsilica® 971 U (particulate amorphous silicon dioxide having a particle size distribution with a median of 0.20 micrometers, i.e. in the range of 0.1 to 0.4 μm, as determined by laser scattering) with a granulated RW filler (particulate amorphous silicon dioxide having a similar particle size distribution with a median of 0.23 micrometers, i.e. in the range of 0.1 to 0.4 μm, as determined by laser scattering), the core weight of the test bars produced is not higher than the linear combination (in each case the linear combination shown by the dashed line) of the values ​​of the test bars containing Elkem Microsilica® 971 U alone (casting material mixture 5.1) or the RW filler Q1 Plus alone (casting material mixture 5.2); no double synergistic effect can be observed.

[0185] The surprising advantages of the present invention are evident, in particular, in comparison with the experiments carried out according to WO 2009 / 056320 A1 with non-inventive casting material mixtures 1.1, 2.1, 3.1, 4.1, 5.1: the core weights of the casting material mixtures according to the invention are in each case significantly higher; at the same time, the relative residual strength after 3 hours does not decrease to an extent that is significant for industrial practice (double synergistic effect). Preferred aspects of the present invention are as follows. [1] The purpose of the present invention is to increase the moisture resistance of castings that can be produced by thermal hardening of a casting material mixture, comprising at least the following: - Refractory mould base materials with an AFS grain size index in the range of 30-100; - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - Water glass As an additive to the casting material mixture comprising: 1. Use of a particulate material comprising, as its sole constituent or as one of several constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm. [2] A process for producing a thermoset casting having improved moisture resistance, comprising: (i) Consists of at least the following: - Refractory mould base materials with an AFS grain size index in the range of 30-100; - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - Water glass preparing a casting material mixture by mixing together (ii) forming the casting material mixture; (iii) heat-curing the molded casting material mixture to obtain a casting. Including, 13. The process of claim 12, wherein the constituents of the casting material mixture are further mixed with an additive particulate material comprising, as its sole or one of multiple constituents, particulate synthetic amorphous silicon dioxide having a median particle size distribution in the range of 0.1 to 0.4 μm as determined by laser scattering. [3] The casting material mixture comprises at least the following solid constituents: - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - a particulate material as an additive, comprising as its sole or one of several constituents particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; to create a solid state mixture or suspension by mixing The process according to claim 2, wherein the solid-state mixture or suspension produced is mixed with further constituents of the casting material mixture. [4] A mixture for use in the process according to [2] or [3], comprising at least the following solid constituents: - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm as a median, and - a particulate material as an additive, comprising as its sole or one of several constituents particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; Including, A mixture, wherein said mixture is a solid state mixture or a suspension of solid constituents in a liquid carrier medium, preferably a solid state mixture. [5] Consists of at least the following: - Refractory mould base materials with an AFS grain size index in the range of 30-100; - particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, in the range of 0.7 to 1.5 μm; - Water glass, and - a particulate material as an additive, comprising as its sole or one of several constituents particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; The mixture according to [4] above, [6] In the mixture, the proportion of particulate synthetic amorphous silicon dioxide having a particle size distribution with a median in the range of 0.1 to 0.4 μm, determined by laser scattering, is less than 2% by weight, preferably more than 0.015% by weight, more preferably more than 0.02% by weight, based on the total mass of the mixture; and / or the proportion of particulate amorphous silicon dioxide having a particle size distribution with a median in the range of 0.7 to 1.5 μm, determined by laser scattering, is less than 2% by weight, preferably more than 0.015% by weight, more preferably more than 0.02% by weight, based on the total mass of the mixture; and / or the total proportion of particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.1 to 0.4 μm and particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm, is less than 2% by weight, preferably more than 0.3% by weight, based on the total mass of the mixture; and / or The total proportion of amorphous silicon dioxide is less than 2% by weight, preferably more than 0.3% by weight, based on the total mass of the mixture; The mixture described in [5] above. [7] The following: (i) providing or producing a discrete quantity of particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; (ii) providing or producing a quantity of a particulate material comprising, as its only constituent or as one of a plurality of constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm; (iii) mixing the amounts provided or produced in steps (i) and (ii). The mixture according to any one of [4] to [6] above, which can be produced by a process comprising: [8] The following: a total mass of particulate amorphous silicon dioxide having a particle size distribution in the range of 0.7 to 1.5 μm as determined by laser scattering; Total mass of particulate synthetic amorphous silicon dioxide having a particle size distribution in the range of 0.1 to 0.4 μm as determined by laser scattering The mixture according to any one of the above [4] to [7], wherein the ratio of is in the range of 20:1 to 1:20, preferably 5:1 to 1:20, more preferably 3:1 to 1:20, particularly preferably 2:1 to 1:20, and most preferably 1.5:1 to 1:20. [9] The particulate synthetic amorphous silicon dioxide having a particle size distribution with a median value in the range of 0.1 to 0.4 μm as determined by laser scattering. and / or The particulate amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median value in the range of 0.7 to 1.5 μm. But the following: - a particulate synthetic amorphous silicon dioxide which contains silicon dioxide in a proportion of at least 90% by weight, based on the total mass of said particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent, and which can be preferably produced by reduction of quartz in an electric arc furnace; - Contains zirconium oxide as a secondary constituent, preferably ZrSiO 4 Particulate synthetic amorphous silicon dioxide, which can be produced by the thermal decomposition of; - Particulate synthetic amorphous silicon dioxide, which can be produced by oxidizing silicon metal with an oxygen-containing gas; - Particulate synthetic amorphous silicon dioxide, which can be produced by quenching a silicon dioxide melt; and - A mixture of them The use according to [1], the process according to [2] or [3], or the mixture according to any one of [4] to [8], wherein the compound is selected from the group consisting of:

[10] - the particulate synthetic amorphous silicon dioxide has a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm, contains a proportion of silicon dioxide of at least 90% by weight, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent, and is preferably producible by reduction of quartz in an electric arc furnace; and / or said particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.7 to 1.5 μm, contains zirconium oxide as a secondary constituent, and preferably ZrSiO 4 The use according to [1] or [9], the process according to [2], [3] or [9], or the mixture according to any one of [4] to [9], wherein the particulate synthetic amorphous silicon dioxide is a particulate synthetic amorphous silicon dioxide that can be produced by thermal decomposition of the above.

[11] The use according to any one of [1] or [9] to

[10] , the process according to any one of [2] to [3] and [9] to

[10] , or the mixture according to any one of [3] to

[10] , wherein one or more constituents are added to the casting material mixture or mixture, or are selected from the group consisting of barium sulfate, boron oxide compounds, graphite, carbohydrates, lithium compounds, phosphorus compounds, hollow microbeads, molybdenum sulfide, platelet-shaped lubricants, surfactants, organosilicon compounds, alumina and alumina-containing compounds.

[12] The particulate synthetic amorphous silicon dioxide having a particle size distribution with a median value in the range of 0.1 to 0.4 μm as determined by laser scattering. and / or The particulate amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median value in the range of 0.7 to 1.5 μm. The use according to any one of [1] or [9] to

[11] above, the process according to any one of [2] to [3] or [9] to

[11] above, or the mixture according to any one of [3] to

[11] above, wherein the use according to any one of [1] or [9] to

[11] above has pozzolanic activity.

[13] The use according to any one of [1] or [9] to

[12] , the process according to any one of [2] to [3] or [9] to

[12] , or the mixture according to any one of [3] to

[12] , wherein the activity of Ra226 in the casting material mixture or the mixture is 1 Bq / g or less.

[14] A kit for producing the mixture according to any one of [4] to

[13] , At least the following: - as or in the first component of the kit, an amount of particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; - as or in a second component of said kit, an amount of particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.1 to 0.4 μm; Including, A kit, wherein the first and second components of the kit are spatially separated from each other.

[15] Use of the mixture according to any one of [4] to

[13] above in the manufacture of molds or cores for metal processing.

Claims

1. The object of the present invention is to increase the moisture resistance of castings which can be produced by thermal hardening of a casting material mixture, comprising at least: - a refractory mould base material having an AFS grain size index in the range from 30 to 100; particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.7 to 1.5 μm; and - Water glass As an additive to the casting material mixture comprising: Use of a particulate material comprising, as its sole constituent or as one of several constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm.

2. 1. A process for producing a thermoset casting having improved moisture resistance, comprising: (i) At least the following components: - a refractory mould base material having an AFS grain size index in the range from 30 to 100; particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.7 to 1.5 μm; and - Water glass preparing a casting material mixture by mixing together (ii) forming the casting material mixture; (iii) heat-curing the molded casting material mixture to obtain a casting. Including, 13. The process of claim 12, wherein the constituents of the casting material mixture are further mixed with an additive particulate material comprising, as its sole or one of its multiple constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution with a median value in the range of 0.1 to 0.4 μm as determined by laser scattering.

3. The casting material mixture comprises at least the following solid constituents: particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.7 to 1.5 μm; and - a particulate material as an additive, comprising, as its sole constituent or as one of its several constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; to create a solid state mixture or suspension by mixing 3. The process of claim 2, wherein the solid state mixture or suspension produced is mixed with further constituents of the casting material mixture.

4. A mixture for use in the process according to claim 2 or 3, comprising at least the following solid constituents: particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.7 to 1.5 μm; and - a particulate material as an additive, comprising, as its sole constituent or as one of its several constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; Including, A mixture wherein the mixture is a solid state mixture or a suspension of solid constituents in a liquid carrier medium.

5. Consists of at least the following: - a refractory mould base material having an AFS grain size index in the range from 30 to 100; particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; - Water glass, and - a particulate material as an additive, comprising, as its sole constituent or as one of its several constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; The mixture of claim 4 comprising:

6. In the mixture, the proportion of particulate synthetic amorphous silicon dioxide having a particle size distribution with a median in the range of 0.1 to 0.4 μm, as determined by laser scattering, is less than 2% by weight, based on the total mass of the mixture; and / or the proportion of particulate amorphous silicon dioxide having a particle size distribution with a median in the range of 0.7 to 1.5 μm, as determined by laser scattering, is less than 2% by weight, based on the total mass of the mixture; and / or the combined proportion of particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.1 to 0.4 μm and particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm, is less than 2% by weight, based on the total mass of the mixture; and / or The total proportion of amorphous silicon dioxide is less than 2% by weight, based on the total mass of the mixture; The mixture according to claim 5.

7. below: (i) providing or producing a discrete quantity of particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; (ii) providing or producing a quantity of a particulate material comprising, as its sole constituent or as one of a plurality of constituents, particulate synthetic amorphous silicon dioxide having a particle size distribution with a median in the range of 0.1 to 0.4 μm as determined by laser scattering; (iii) mixing the amounts provided or produced in steps (i) and (ii). The mixture according to any one of claims 4 to 6, which can be produced by a process comprising:

8. below: a total mass of particulate amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; A total mass of particulate synthetic amorphous silicon dioxide having a particle size distribution with a median value in the range of 0.1 to 0.4 μm as determined by laser scattering.

8. The mixture according to claim 4, wherein the ratio of is in the range of 20:1 to 1:

20.

9. The particulate synthetic amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm. and / or The particulate amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm. but the following: - a particulate synthetic amorphous silicon dioxide which contains silicon dioxide in a proportion of at least 90% by weight, based on the total mass of said particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent; - Particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent; particulate synthetic amorphous silicon dioxide, which can be produced by oxidizing silicon metal with an oxygen-containing gas; - particulate synthetic amorphous silicon dioxide, which can be produced by quenching a silicon dioxide melt; and - Mixtures thereof 2. The use of claim 1, wherein said compound is selected from the group consisting of:

10. - said particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm, contains a proportion of silicon dioxide of at least 90% by weight, based on the total mass of said particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent; and / or Use according to claim 1 or 9, wherein the particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.7 to 1.5 μm is a particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent.

11. 11. The use according to any of claims 1 and 9 to 10, wherein one or more constituents are added to the casting material mixture or are selected from the group consisting of barium sulfate, boron oxide compounds, graphite, carbohydrates, lithium compounds, phosphorus compounds, hollow microbeads, molybdenum sulfide, platelet shaped lubricants, surfactants, organosilicon compounds, alumina and alumina containing compounds.

12. The particulate synthetic amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm. and / or The particulate amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm. The use according to any one of claims 1 and 9 to 11, wherein said compound has pozzolanic activity.

13. The use according to any one of claims 1 and 9 to 12, wherein the activity of Ra226 in the foundry material mixture is less than or equal to 1 Bq / g.

14. The particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm. and / or The particulate amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm. but the following: - a particulate synthetic amorphous silicon dioxide which contains silicon dioxide in a proportion of at least 90% by weight, based on the total mass of said particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent; - Particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent; particulate synthetic amorphous silicon dioxide, which can be produced by oxidizing silicon metal with an oxygen-containing gas; - particulate synthetic amorphous silicon dioxide, which can be produced by quenching a silicon dioxide melt; and - Mixtures thereof 4. The process of claim 2 or 3, wherein said first and second aryl groups are selected or independently selected from the group consisting of:

15. - the particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm, contains a proportion of silicon dioxide of at least 90% by weight, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent; and / or - the process according to any one of claims 2, 3 and 14, wherein the particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm, is a particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent.

16. The process of any of claims 2-3 and 14-15, wherein one or more constituents are added to the casting material mixture or are selected from the group consisting of barium sulfate, boron oxide compounds, graphite, carbohydrates, lithium compounds, phosphorus compounds, hollow microbeads, molybdenum sulfide, platelet shaped lubricants, surfactants, organosilicon compounds, alumina and alumina containing compounds.

17. The particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm. and / or The particulate amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm. The process according to any one of claims 2 to 3 and 14 to 16, wherein said process has pozzolanic activity.

18. The process of claim 2, 3, or 14, wherein the activity of Ra226 in the casting material mixture is 1 Bq / g or less.

19. The particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm. and / or The particulate amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm. but the following: - a particulate synthetic amorphous silicon dioxide which contains silicon dioxide in a proportion of at least 90% by weight, based on the total mass of said particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent; - Particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent; particulate synthetic amorphous silicon dioxide, which can be produced by oxidizing silicon metal with an oxygen-containing gas; - particulate synthetic amorphous silicon dioxide, which can be produced by quenching a silicon dioxide melt; and - Mixtures thereof 9. The mixture of any one of claims 4 to 8, wherein the mixture is selected from the group consisting of:

20. - the particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.1 to 0.4 μm, contains a proportion of silicon dioxide of at least 90% by weight, based on the total mass of the particulate synthetic amorphous silicon dioxide, and at least carbon as a secondary constituent; and / or 20. The mixture according to any one of claims 4 to 8 and 19, wherein the particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm is a particulate synthetic amorphous silicon dioxide containing zirconium oxide as a secondary constituent.

21. The mixture of any of claims 4 to 8 and 19 to 20, wherein one or more constituents are added to the mixture or are selected from the group consisting of barium sulfate, boron oxide compounds, graphite, carbohydrates, lithium compounds, phosphorus compounds, hollow microbeads, molybdenum sulfide, platelet shaped lubricants, surfactants, organosilicon compounds, alumina and alumina containing compounds.

22. The particulate synthetic amorphous silicon dioxide having a particle size distribution, as determined by laser scattering, with a median in the range of 0.1 to 0.4 μm. and / or The particulate amorphous silicon dioxide has a particle size distribution, as determined by laser scattering, with a median in the range of 0.7 to 1.5 μm. The mixture according to any one of claims 4 to 8 and 19 to 21, wherein said mixture has pozzolanic activity.

23. A mixture described in any of claims 4 to 8 and 19 to 22, wherein the activity of Ra226 in the mixture is 1 Bq / g or less.

24. A kit for producing the mixture according to any one of claims 4 to 8 and 19 to 23, comprising: At least the following: - as or in the first component of said kit, an amount of particulate amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median in the range of 0.7 to 1.5 μm; - as or in a second component of said kit, an amount of particulate synthetic amorphous silicon dioxide having a particle size distribution, determined by laser scattering, with a median value in the range of 0.1 to 0.4 μm; Including, A kit wherein the first and second components of the kit are spatially separated from each other.

25. Use of the mixture according to any one of claims 4 to 8 and 19 to 23 in the manufacture of moulds or cores for metalworking.

Citation Information

Patent Citations

  • Mixture of molding material, mold for casting, and method for producing mold for casting

    JP2008307604A

  • Mold material, mold and method for manufacturing the same

    JP2013094834A

  • Molding material mixtures containing metal oxides of aluminum and zirconium in particulate form

    US20150306658A1

  • Mould material mixtures on the basis of inorganic binders, and method for producing moulds and cores for metal casting

    WO2014059969A2

  • Coated sand, method for producing same, and method for producing casting mold using same

    WO2018097180A1