Aqueous dispersions of polymer additives and processes therefor
Aqueous dispersions with controlled coagulum formation using specific polymeric additives enhance corrosion protection and soil removal in coatings, addressing high coagulum issues and improving performance.
Patent Information
- Application Number
- JP2023522816
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-28
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-10-28
AI Technical Summary
Aqueous coating compositions face issues with high coagulum formation when incorporating ethylenically unsaturated siloxane monomers beyond 4.5% by weight, limiting their application and performance, particularly in terms of corrosion protection and soil removal.
Development of aqueous dispersions with low coagulum content (<2,000 ppm) by emulsion polymerization, using specific polymeric additives with structural units of ethylenically unsaturated siloxane monomers, functional groups, and additional monomers, controlled through chain transfer agents and homogenization to minimize coagulum formation.
The solution results in improved corrosion protection and soil removal properties of coatings, achieving better performance with reduced ethylenically unsaturated siloxane monomer concentrations while maintaining effectiveness.
Smart Images

Figure 0007573105000001 
Figure 0007573105000002 
Figure 0007573105000003
Abstract
Description
[Technical field]
[0001] The present invention relates to aqueous dispersions of polymeric additives and processes for preparing same.
[0002] Introduction Aqueous or waterborne coating compositions are becoming more and more important than solvent-based coating compositions to reduce environmental concerns. Aqueous coating compositions are usually formulated using emulsion polymers as binders, which are typically prepared by emulsion polymerization of conventional monomers such as butyl acrylate, 2-ethylhexyl acrylate, styrene, methyl methacrylate, or mixtures thereof. Incorporating more hydrophobic monomers, such as ethylenically unsaturated siloxane monomers, into the polymer backbone of the binder during emulsion polymerization can be one approach to further improve the performance of the coating, such as anticorrosive properties. However, when the ethylenically unsaturated siloxane monomers are included in the binder in an amount greater than 4.5% by weight of the total monomers, large amounts of coagulum (e.g., greater than 2,000 ppm) may be formed in the conventional emulsion polymerization process, which limits the application of the aqueous silicone-acrylic hybrid polymer binder. Aqueous coating compositions can also have other desirable properties, such as stain resistance in outdoor applications.
[0003] It is therefore desirable to provide aqueous dispersions that are particularly suitable for coating compositions and that can provide coatings with improved performance, such as anti-corrosion and stain release properties, without the problems associated with the aforementioned binders. Summary of the Invention
[0004] The present invention provides a novel aqueous dispersion of polymer additives that does not have the above problems. The process for preparing such aqueous dispersion of polymer additives can obtain an aqueous dispersion with low coagulum content, for example, less than 2,000 parts per million (ppm), after filtering through a 44 micrometer sieve. By incorporating a certain amount of the aqueous dispersion of polymer additives into a coating composition, the anticorrosive and stain release properties of the coating made therefrom can be improved.
[0005] In a first aspect, the present invention provides an aqueous dispersion of a polymeric additive having a weight average molecular weight of 2,000 to 25,000 grams per mole (g / mol), the polymeric additive comprising, based on the weight of the polymeric additive: (i) 20% to 85% by weight of structural units of an ethylenically unsaturated siloxane monomer of formula (I), formula (II), or formula (III);
[0006] [ka] (In formula (I), R is an ethylenically unsaturated group, j and k each independently range from 0 to 100, and j+k=5 to 100);
[0007] [ka] (In formula (II), R is an ethylenically unsaturated group, R1 is a hydroxyl, alkyl, aryl, alkoxyl, aryloxy, alkyl ether, or aryl ether group, and m is 1 to 100);
[0008] [ka] (In the formula (III), R is an ethylenically unsaturated group, R1 and R2 are each independently a hydroxyl, alkyl, aryl, alkoxyl, aryloxy, alkyl ether, or aryl ether group, n is 1 to 5, and p is 1 to 100), (ii) 0.1% by weight to 10% by weight of structural units of an ethylenically unsaturated functional monomer having at least one functional group selected from an amide, ureido, carboxyl, carboxylic anhydride, hydroxyl, phosphoric acid, or sulfonic acid group, a salt thereof, or a mixture thereof; (iii) 5% to 79.9% by weight of additional ethylenically unsaturated nonionic monomeric structural units; Including, The coagulum content of the aqueous dispersion is less than 2,000 ppm after filtering through a 44 micrometer sieve.
[0009] In a second aspect, the invention is a process for preparing the aqueous dispersion of the first aspect. The process comprises: The emulsion polymerization of a monomer mixture in the presence of a chain transfer agent, the monomer mixture comprising 20% to 85% by weight of an ethylenically unsaturated siloxane monomer, 0.1% to 10% by weight of an ethylenically unsaturated functional monomer, and 5% to 79.9% by weight of an additional monoethylenically unsaturated nonionic monomer, based on the total weight of the monomer mixture.
[0010] In a second aspect, the invention is a coating composition comprising: (A) 0.8 wt. % to 8 wt. % of an aqueous dispersion of the polymeric additive of the first aspect, based on the total weight of the coating composition; and (B) an emulsion polymer having a weight average molecular weight greater than 25,000 g / mol. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] By "aqueous" dispersion herein is meant that the particles are dispersed in an aqueous medium. By "aqueous medium" herein is meant water and 0-30% by weight, based on the weight of the medium, of a water-miscible compound(s), such as alcohols, glycols, glycol ethers, glycol esters, and the like.
[0012] "Acrylic", as used herein, includes (meth)acrylic acid, alkyl (meth)acrylates, (meth)acrylamides, (meth)acrylonitrile, and modified forms thereof, such as (meth)hydroxyalkyl acrylates. Throughout this document, the fragment "(meth)acrylic" refers to both "methacrylic" and "acrylic". For example, (meth)acrylic acid refers to both methacrylic acid and acrylic acid, and methyl (meth)acrylate refers to both methyl methacrylate and methyl acrylate.
[0013] A "structural unit," also known as a "polymerized unit" of a specified monomer, refers to the remainder of a monomer after polymerization, i.e., the polymerized monomer or the polymerized form of the monomer. For example, the structural unit of methyl methacrylate is:
[0014] [ka] where the dotted lines represent the points of attachment of the structural units to the polymer backbone.
[0015] The aqueous dispersion of the present invention comprises a polymeric additive. The polymeric additive comprises one or more ethylenically unsaturated siloxane monomers, preferably one or more (meth)acrylate functional siloxane structural units. The ethylenically unsaturated siloxane monomers are represented by formula (I), formula (II), or formula (III):
[0016] [ka] (In formula (I), R is, for example, -CH=CH2, -Rp -OC(=O)CH=CH2 or -R p is an ethylenically unsaturated group containing -OC(=O)C(CH3)=CH2, where R p is a C1-C6 divalent hydrocarbon group, preferably, R is -CH2CH2CH2OC(=O)CH=CH2 or -CH2CH2CH2OC(=O)C(CH3)=CH2, j and k are each independently in the range of 0 to 100, 0 to 80, 0 to 60, 5 to 50, 10 to 40, or 10 to 20, and j+k=5 to 100, for example, 5 to 50, 8 to 50, 10 to 40, 10 to 30, or 10 to 25);
[0017] [ka] (In formula (I), R is, for example, -CH=CH2, -R p -OC(=O)CH=CH2 or -R p is an ethylenically unsaturated group containing -OC(=O)C(CH3)=CH2, where R p is a C1-C6 divalent hydrocarbon group, preferably R is -CH2CH2CH2OC(=O)CH=CH2 or -CH2CH2CH2OC(=O)C(CH3)=CH2, R1 is a hydroxyl, alkyl, aryl, alkoxyl, aryloxy, alkyl ether, or aryl ether group, preferably a hydroxyl group, or an alkyl, alkoxyl, or alkyl ether group having in the range of 1 to 15, 1 to 10, or 1 to 5 carbon atoms, such as -CH3, -OH, -OCH3, or -OCH2CH3, and m is 1 to 100, 5 to 80, 10 to 60, 10 to 40, or 10 to 20);
[0018] [ka] (In formula (III), R is, for example, -CH=CH2, -R p -OC(=O)CH=CH2 or -R pis an ethylenically unsaturated group containing -OC(=O)C(CH3)=CH2, where R p is a C1-C6 divalent hydrocarbon group, preferably, R is -CH2CH2CH2OC(=O)CH=CH2 or -CH2CH2CH2OC(=O)C(CH3)=CH2, R1 and R2 are the same or different and each independently is a hydroxyl, alkyl, aryl, alkoxyl, aryloxy, alkyl ether, or aryl ether group, preferably a hydroxyl group, or an alkyl, alkoxyl, or alkyl ether group having in the range of 1 to 15, 1 to 10, or 1 to 5 carbon atoms, for example, -CH3, -OH, -OCH3, or -OCH2CH3, n is 1 to 5, 1 to 4, 1 to 3, or 1 to 2, and p is 1 to 100, 5 to 80, 5 to 60, 8 to 40, or 8 to 20. Suitable commercially available ethylenically unsaturated siloxane monomers can include, for example, DOWSIL™ 32 methacrylate siloxane monomer available from The Dow Chemical Company (DOWSIL is a trademark of The Dow Chemical Company).
[0019] The polymeric additive of the present invention may comprise structural units of ethylenically unsaturated siloxane monomers in an amount of 20 wt% or more, 21 wt% or more, 22 wt% or more, 23 wt% or more, 24 wt% or more, 25 wt% or more, 26 wt% or more, 27 wt% or more, 28 wt% or more, 29 wt% or more, 30 wt% or more, 31 wt% or more, 32 wt% or more, 33 wt% or more, 34 wt% or more, 35 wt% or more, 36 wt% or more, 37 wt% or more, or even 38 wt% or more, while at the same time being 85 wt% or less, 80 wt% or less, 75 wt% or less, 70 wt% or less, 65 wt% or less, 60 wt% or less, 55 wt% or less, 52 wt% or less, 50 wt% or less, 48 wt% or less, 45 wt% or less, 42 wt% or less, or even 40 wt% or less, based on the weight of the polymeric additive.
[0020] The polymer additive of the present invention comprises structural units of one or more ethylenically unsaturated functional monomers having at least one functional group selected from amide, ureido, carboxyl, carboxylic anhydride, hydroxyl, phosphoric acid, or sulfonic acid groups, salts thereof, or mixtures thereof. Examples of suitable ethylenically unsaturated functional monomers include α,β-ethylenically unsaturated carboxylic acids, including monomers having acids such as methacrylic acid, acrylic acid, itaconic acid, maleic acid, or fumaric acid; or monomers having acid-forming groups that can generate or subsequently be converted into acid groups, such as anhydrides, (meth)acrylic anhydride, or maleic anhydride; sodium styrenesulfonate (SSS), sodium vinylsulfonate (SVS), 2-acrylamido-2-methylpropanesulfonic acid (AMPS), the sodium salt of 2-acrylamido-2-methyl-1-propanesulfonic acid, ... These include ammonium salts, sodium salts of allyl ether sulfonates, acrylamide, methacrylamide, monosubstituted (meth)acrylamides, N-methylacrylamide, N-ethylacrylamide, N-isopropylacrylamide, N-butylacrylamide, N-tertiary butylacrylamide, N-2-ethylhexylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, hydroxy-functional alkyl (meth)acrylates such as hydroxyethyl (meth)acrylate and hydroxypropyl (meth)acrylate, ureido-functional monomers such as hydroxyethyl ethylene urea methacrylate, hydroxyethyl ethylene urea acrylate such as SIPOMER WAM II available from Solvay, methylacrylamidoethyl ethylene urea, or mixtures thereof. Preferred ethylenically unsaturated functional monomers are selected from the group consisting of acrylic acid, sodium styrene sulfonate, acrylamide, methacrylamide, methacrylic acid, or mixtures thereof.The polymeric additive may comprise 0.1 wt% or more, 0.2 wt% or more, 0.3 wt% or more, 0.4 wt% or more, 0.5 wt% or more, 0.6 wt% or more, 0.7 wt% or more, 0.8 wt% or more, 0.9 wt% or more, or even 1.0 wt% or more, and at the same time 10 wt% or less, 9 wt% or less, 8 wt% or less, 7 wt% or less, 6 wt% or less, 5 wt% or less, 4.5 wt% or less, 4 wt% or less, 3.5 wt% or less, 3 wt% or less, 2.5 wt% or less, 2 wt% or less, or even 1.5 wt% or less of structural units of ethylenically unsaturated functional monomers, based on the weight of the polymeric additive.
[0021] The polymer additive of the present invention comprises structural units of one or more additional monoethylenically unsaturated nonionic monomers other than the monomers mentioned above. The term "nonionic monomer" in this specification refers to a monomer that does not have an ionic charge at pH=1-14. The additional monoethylenically unsaturated nonionic monomers may include acrylic monomers, styrene monomers, combinations of acrylic monomers and styrene monomers, vinyl ester monomers, or combinations of ethylene monomers and vinyl ester monomers, vinyl silane monomers, or mixtures thereof. Examples of suitable acrylic monomers include alkyl esters of (meth)acrylic acid having 2-30 carbon atoms or 2-18 carbon atoms, such as methyl acrylate, methyl methacrylate, ethyl acrylate, 2-ethylhexyl acrylate, butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, decyl acrylate, isodecyl methacrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate; cyclohexyl (meth)acrylate, metacyclohexyl (meth)acrylate, methyl meth ...methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl methacrylate, methyl meth The monomer may be selected from cycloalkyl (meth)acrylates, including tert-butyl (meth)cyclohexyl (meth)acrylate, dihydrodicyclopentadienyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, (meth)acrylate functional silanes, including (meth)acryloxyalkyltrialkoxysilanes, such as gamma-methacryloxypropyltrimethoxysilane and methacryloxypropyltriethoxysilane; 3-methacryloxypropylmethyldimethoxysilane; 3-methacryloxypropyltrimethoxysilane; 3-methacryloxypropyltriethoxysilane; or mixtures thereof. Examples of suitable styrene monomers include styrene and substituted styrenes. Examples of suitable vinyl silane monomers include vinyl acetate, vinyl butyrate, vinyl versatate, or mixtures thereof. Examples of suitable alkyl alkyl vinyl dialkoxy silanes and vinyl trialkoxy silanes, such as vinyl triethoxy silane and vinyl trimethoxy silane.Preferred additional ethylenically monounsaturated nonionic monomers are butyl acrylate, butyl methacrylate, methyl methacrylate, ethyl acrylate, 2-ethylhexyl acrylate, vinyl acetate, (meth)acrylate functional silanes, styrene, or mixtures thereof. The polymer additive may comprise 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, 30% by weight or more, 35% by weight or more, 40% by weight or more, or even 45% by weight or more, and at the same time 79.9% by weight or less, 79% by weight or less, 78% by weight or less, 75% by weight or less, 72% by weight or less, 70% by weight or less, 68% by weight or less, 65% by weight or less, 62% by weight or less, 60% by weight or less, 59% by weight or less, or even 57% by weight or less of additional monoethylenically unsaturated nonionic monomer structural units, based on the weight of the polymer additive.
[0022] The polymer additive of the present invention may also optionally contain structural units of one or more multiethylenically unsaturated monomers different from the above monomers. Examples of suitable multiethylenically unsaturated monomers include allyl (meth)acrylate, hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, butanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, divinylbenzene, allyl acetate, allyl (meth)acrylamide, allyloxyethyl (meth)acrylate, crotyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenylethyl (meth)acrylate, diallyl maleate, or mixtures thereof. The polymer additive may contain 0-5 wt%, 0-2 wt%, or 0.1 wt% to 1 wt% multiethylenically unsaturated monomer structural units based on the weight of the polymer additive.
[0023] Preferably, the polymeric additive comprises, based on the weight of the polymeric additive, 20% to 50% by weight of structural units of an ethylenically unsaturated siloxane monomer, 1% to 5% by weight of structural units of an ethylenically unsaturated functional monomer, and 45% to 79% by weight of structural units of an additional monoethylenically unsaturated nonionic monomer.
[0024] The polymer additive of the present invention has a molecular weight of 2,000 g / mol or more, 2,100 g / mol or more, 2,200 g / mol or more, 2,500 g / mol or more, 2,800 g / mol or more, 3,000 g / mol or more, 3,200 g / mol or more, 3,500 g / mol or more, 3,800 g / mol or more, 4,000 g / mol or more, 4,200 g / mol or more, 4,500 g / mol or more, 4,800 g / mol or more, 5,000 g / mol or more, 5,200 g / mol or more or less, or even 5,500 g / mol, and at the same time less than or equal to 25,000 g / mol (i.e., ≦25,000 g / mol), less than or equal to 22,000 g / mol, less than or equal to 20,000 g / mol, less than or equal to 18,000 g / mol, less than or equal to 15,000 g / mol, less than or equal to 12,000 g / mol, less than or equal to 10,000 g / mol, less than or equal to 9,500 g / mol, less than or equal to 9,000 g / mol, less than or equal to 8,500 g / mol, or even less than or equal to 8,000 g / mol. w ). M W can be determined by gel permeation chromatography (GPC) analysis, as described in the Examples section below.
[0025] The aqueous dispersion of the polymer additive of the present invention has a low coagulum content. "Low coagulum content" refers to the coagulum content of the aqueous dispersion of less than 2,000 ppm, preferably less than 1,900 ppm, less than 1,800 ppm, less than 1,700 ppm, less than 1,600 ppm, less than 1,500 ppm, less than 1,400 ppm, less than 1,300 ppm, less than 1,200 ppm, less than 1,100 ppm, less than 1,000 ppm, less than 900 ppm, less than 800 ppm, less than 700 ppm, less than 600 ppm, or even less than 500 ppm. The coagulum content can be determined by filtering the aqueous dispersion through a sieve with a mesh size of 44 micrometers (325 mesh) according to the test method described in the following Examples section.
[0026] The aqueous dispersion of the polymeric additive of the present invention can be prepared by emulsion polymerization of a monomer mixture comprising the above-mentioned monomers for forming the structural units of the polymeric additive in the presence of a chain transfer agent. The monomer mixture useful in the present invention comprises an ethylenically unsaturated siloxane monomer, an ethylenically unsaturated functional monomer, an additional monoethylenically unsaturated nonionic monomer, and optionally a multiethylenically unsaturated nonionic monomer. The total concentration of the monomer mixture for preparing the polymeric additive is equal to 100%. The monomer mixture may be emulsified and homogenized, typically by a homogenizer or the like, before polymerization, e.g., before adding the monomer mixture to the reaction vessel. The homogenization process may be carried out for a certain period of time to minimize coagulum formation during polymerization, and thus to obtain an aqueous dispersion with a low coagulum content. For example, the time of the homogenization process may range, for example, from 1 to 5 minutes or from 3 to 5 minutes. Examples of suitable chain transfer agents include 3-mercaptopropionic acid, n-dodecyl mercaptan (nDDM), methyl 3-mercaptopropionate (MMP), butyl 3-mercaptopropionate, benzenethiol, azelaic alkyl mercaptan, or mixtures thereof. The chain transfer agent may be used in an amount effective to control the molecular weight of the polymer additive. For example, the chain transfer agent may be used in an amount of 0.01 wt% or more, 0.1 wt% or more, 0.5 wt% or more, or even 1 wt% or more, and at the same time 5 wt% or less, 4.5 wt% or less, 4 wt% or less, or even 3.5 wt% or less, based on the total weight of the monomer mixture used to prepare the polymer additive.
[0027] Polymerization of the monomer mixture may be carried out by conventional free radical polymerization processes well known in the art. The monomers for preparing the polymeric additive may be added neat, as an emulsion in water, or in one or more portions or continuously, linearly or non-linearly, or combinations thereof, over the reaction period to prepare the polymeric additive. Suitable temperatures for the emulsion polymerization process may be below 95 degrees Celsius (°C), in the range of 50-90°C, or in the range of 70-90°C. The polymerization process to prepare the polymeric additive may use a free radical initiator. The polymerization process may be a thermally initiated or redox initiated emulsion polymerization. Examples of suitable free radical initiators include hydrogen peroxide, tert-butyl hydroperoxide, tert-amyl hydroperoxide, cumene hydroperoxide, ammonium and / or alkali metal persulfates, sodium perborate, superphosphate, and salts thereof; potassium permanganate, and ammonium or alkali metal salts of peroxydisulfate. Free radical initiators may typically be used at levels of 0.01% to 1% by weight or 0.05% to 0.6% by weight based on the total weight of the monomer mixture. The polymerization process may use a redox system that includes the above initiators in combination with a suitable reducing agent. Examples of suitable reducing agents include sodium formaldehyde sulfoxylate, ascorbic acid, isoascorbic acid, alkali metal and ammonium salts of sulfur-containing acids (e.g., sodium sulfite, bisulfite, thiosulfite, hydrosulfite, sulfide, hydrosulfite, or dithionite), acetone bisulfite, glycolic acid, hydroxymethanesulfonic acid, glyoxylic acid hydrate, lactic acid, glyceric acid, malic acid, tartaric acid, and salts of the aforementioned acids. Metal salts of iron, copper, manganese, silver, platinum, vanadium, nickel, chromium, palladium, or cobalt may be used to catalyze the redox reaction. Optionally, a chelating agent for the metal may be used.
[0028] In the polymerization process, one or more surfactants may be added before or during the polymerization of the monomers, or a combination thereof. A portion of the surfactants may be added after polymerization. These surfactants may include anionic and / or nonionic emulsifiers. Examples of suitable surfactants include alkali metal or ammonium salts of alkyl, aryl, or alkylaryl sulfates, sulfonates, or phosphates; alkylsulfonic acids; sulfosuccinates; fatty acids; reactive surfactants; ethoxylated alcohols or phenols; and mixtures thereof. The amount of surfactant used typically ranges from 0.1% to 6%, 0.3% to 3%, or 0.5% to 1.5% by weight based on the weight of the monomer mixture used to prepare the polymer additive.
[0029] After the polymerization is completed, the resulting aqueous dispersion containing the polymeric additive may be optionally neutralized with one or more bases as neutralizing agents, for example to a pH value ranging from 6 to 11 or 7 to 9. The bases may partially or completely neutralize the ionic or potentially ionic groups of the polymeric additive. Examples of suitable bases include alkali metal or alkaline earth metal compounds such as sodium hydroxide, potassium hydroxide, calcium hydroxide, zinc oxide, magnesium oxide, sodium carbonate, etc.; primary, secondary, and tertiary amines such as ammonia solution, triethylamine, ethylamine, propylamine, monoisopropylamine, monobutylamine, hexylamine, ethanolamine, diethylamine, dimethylamine, di-n-propylamine, tributylamine, triethanolamine, dimethoxyethylamine, 2-ethoxyethylamine, 3-ethoxypropylamine, dimethylethanolamine, diisopropanolamine, morpholine, ethylenediamine, 2-diethylaminoethylamine, 2,3-diaminopropane, 1,2-propylenediamine, neopentanediamine, dimethylaminopropylamine, hexamethylenediamine, 4,9-dioxadodecane-1,12-diamine, polyethyleneimine, or polyvinylamine; aluminum hydroxide; and mixtures thereof.
[0030] The polymeric additive particles in the aqueous dispersion can have a number average particle size in the range of 50 to 500 nanometers (nm), 60 to 400 nm, or 70 to 300 nm, as determined by a Brookhaven BI-90 Plus Particle Size Analyzer.
[0031] The aqueous dispersion of the polymer additive further comprises water in an amount of, for example, 30% to 90% by weight, 40% to 80% by weight, or 50% to 70% by weight, based on the total weight of the aqueous dispersion.
[0032] The present invention also relates to a coating composition, typically an aqueous coating composition, comprising (A) an aqueous dispersion of a polymer additive and (B) an emulsion polymer. The coating composition of the present invention may comprise the aqueous dispersion of the polymer additive in an amount of 0.8 wt% or more, 0.9 wt% or more, 1.0 wt% or more, 1.1 wt% or more, 1.2 wt% or more, 1.3 wt% or more, 1.4 wt% or more, 1.5 wt% or more, or even 1.6 wt% or more, and at the same time 8 wt% or less, 7.9 wt% or less, 7.8 wt% or less, 7.7 wt% or less, 7.6 wt% or less, 7.5 wt% or less, 7.4 wt% or less, 7.3 wt% or less, 7.2 wt% or less, 7.1 wt% or less, 7 wt% or less, 6.9 wt% or less, 6.8 wt% or less, 6.7 wt% or less, 6.6 wt% or less, 6.5 wt% or less, 6.4 wt% or less, or even 6.3 wt% or less, based on the total weight of the coating composition. Preferably, the aqueous dispersion of the polymeric additive is present in the coating composition in an amount such that the concentration of structural units of the ethylenically unsaturated siloxane monomer is 0.2 wt% or more, 0.22 wt% or more, 0.25 wt% or more, 0.28 wt% or more, 0.3 wt% or more, 0.32 wt% or more, 0.35 wt% or more, 0.38 wt% or more, or even 0.4 wt% or more, and at the same time 1.8 wt% or less, 1.7 wt% or less, 1.6 wt% or less, 1.5 wt% or less, 1.4 wt% or less, 1.3 wt% or less, 1.2 wt% or less, 1.1 wt% or less, 1.0 wt% or less, 0.9 wt% or less, 0.8 wt% or less, 0.78 wt% or less, 0.75 wt% or less, 0.72 wt% or less, or even 0.7 wt% or less, based on the total weight of the coating composition.
[0033] The coating compositions of the present invention further comprise one or more emulsion polymers commonly used as binders, typically in the form of an emulsion or aqueous dispersion. The emulsion polymers useful in the present invention have a weight average molecular weight (M) of more than 25,000 g / mol (i.e., >25,000 g / mol), for example, 30,000 g / mol or more, 60,000 g / mol or more, 80,000 g / mol or more, 100,000 g / mol or more, 200,000 g / mol or more, 300,000 g / mol or more, or even 400,000 g / mol or more. w ) M w can be determined by GPC analysis using polystyrene standards. The emulsion polymer particles can have a particle size of 30 nanometers (nm) to 500 nm, 70 nm to 300 nm, or 70 nm to 250 nm. The particle size of the emulsion polymer can be determined by a Brookhaven BI-90 Plus Particle Size Analyzer.
[0034] The emulsion polymer in the coating composition of the present invention may be selected from acrylic polymers, including acrylic copolymers and styrene-acrylic copolymers, polyurethane-acrylic hybrid polymers, or mixtures thereof. The acrylic polymers useful in the present invention may contain 90% to 99.9% by weight, based on the weight of the acrylic polymer, of structural units of the above-mentioned monoethylenically unsaturated nonionic monomers, such as styrene, butyl acrylate, 2-ethylhexyl acrylate, acetoacetoxyethyl methacrylate (AAEM), or mixtures thereof, and 0.1% to 10% by weight of structural units of the above-mentioned ethylenically unsaturated functional monomers, such as acrylic acid, methacrylic acid, phosphoethyl methacrylate, or mixtures thereof.
[0035] The coating composition of the present invention may include pigments and / or extenders. As used herein, "pigment" refers to a material that can contribute substantially to the opacity or hiding power of the coating. Such materials typically have a refractive index greater than 1.8. Inorganic pigments typically include metal oxides. Examples of suitable pigments include titanium dioxide (TiO2), zinc oxide, iron oxide, zinc sulfide, zinc phosphate, and anticorrosive pigments such as zinc molybdate, carbon black, barium sulfate, barium carbonate, and mixtures thereof. TiO2 typically exists in two crystalline forms, anastase and rutile. Suitable commercially available TiO2 may include, for example, KRONOS2310 available from Kronos Worldwide, Inc., Ti-Pure R-706 available from Chemours (Wilmington, Del.), TiONA AT1 available from Cristal, and mixtures thereof. TiO2 may also be available in concentrated dispersion form. "Extender" herein refers to a particulate inorganic material having a refractive index of 1.8 or less and greater than 1.3. Examples of suitable extenders include calcium carbonate, clay, calcium sulfate, aluminum silicate, silicates, zeolites, mica, diatomaceous earth, solid or hollow glass, ceramic beads, nepheline syenite, feldspar, diatomaceous earth, calcined diatomaceous earth, talc (hydrated magnesium silicate), silica, alumina, kaolin, pyrophyllite, perlite, baryte, wollastonite, opaque polymers such as ROPAQUE™ Ultra E opaque polymer available from The Dow Chemical Company (ROPAQUE is a trademark of The Dow Chemical Company), and mixtures thereof. The coating composition may have a pigment volume concentration (PVC) of 0-55%, 5-40%, or 10-35%. PVC can be determined according to the following equation:
[0036]
number
[0037] The coating compositions of the present invention may include one or more antifoaming agents. "Antifoaming agent" as used herein refers to a chemical additive that reduces or prevents the formation of foam. The antifoaming agent may be a silicone-based antifoaming agent, a mineral oil-based antifoaming agent, an ethylene oxide / propylene oxide-based antifoaming agent, an alkyl polyacrylate, and mixtures thereof. The antifoaming agent may be present in an amount of 0-5 wt%, 0.05 wt%-3 wt%, or 0.1 wt%-2 wt%, based on the total weight of the coating composition.
[0038] The coating compositions of the present invention may include one or more thickeners, also known as "rheology modifiers". Thickeners may include polyvinyl alcohol (PVA), clay materials, acid derivatives, acid copolymers, urethane associative thickeners (UAT), polyether urea polyurethanes (PEUPU), polyether polyurethanes (PEPU), or mixtures thereof. Examples of suitable thickeners include alkali swellable emulsions (ASE), such as sodium or ammonium neutralized acrylic acid polymers; hydrophobically modified alkali swellable emulsions (HASE), such as hydrophobically modified acrylic acid copolymers; associative thickeners, such as hydrophobically modified ethoxylated urethanes (HEUR); and cellulosic thickeners, such as methylcellulose ethers, hydroxymethylcellulose (HMC), hydroxyethylcellulose (HEC), hydrophobically modified hydroxyethylcellulose (HMHEC), sodium carboxymethylcellulose (SCMC), sodium carboxymethyl 2-hydroxyethylcellulose, 2-hydroxypropylmethylcellulose, 2-hydroxyethylmethylcellulose, 2-hydroxybutylmethylcellulose, 2-hydroxyethylethylcellulose, and 2-hydroxypropylcellulose. Preferably, the thickener is HEUR, HEC, or a mixture thereof. The thickener may be present in an amount of 0 to 8 wt%, 0.05 wt% to 3 wt%, or 0.1 wt% to 1 wt%, based on the total weight of the coating composition.
[0039] The coating compositions of the present invention may include one or more wetting agents. As used herein, "wetting agent" refers to a chemical additive that reduces the surface tension of the coating composition, allowing the coating composition to more easily spread or penetrate onto the surface of a substrate. Wetting agents may be polycarboxylate, anionic, zwitterionic, or nonionic. Wetting agents may be present at 0-5 wt%, 0.05 wt%-3 wt%, or 0.1 wt%-2 wt%, based on the total weight of the coating composition.
[0040] The coating composition of the present invention may include one or more coalescents. As used herein, "coalescent" refers to a slow-evaporating solvent that coalesces polymer particles into a continuous film under ambient conditions. Examples of suitable coalescents include 2-n-butoxyethanol, dipropylene glycol n-butyl ether, propylene glycol n-butyl ether, dipropylene glycol methyl ether, propylene glycol methyl ether, propylene glycol n-propyl ether, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, triethylene glycol monobutyl ether, dipropylene glycol n-propyl ether, n-butyl ether, or mixtures thereof. Preferred coalescents include dipropylene glycol n-butyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, n-butyl ether, or mixtures thereof. The coalescent may be present at 0-30 wt%, 0.5 wt%-20 wt%, or 2 wt%-10 wt%, based on the total weight of the coating composition.
[0041] The coating composition of the present invention may include one or more dispersants. Dispersants may include nonionic, anionic, and cationic dispersants such as polyacids having suitable molecular weights, 2-amino-2-methyl-1-propanol (AMP), dimethylaminoethanol (DMAE), potassium tripolyphosphate (KTPP), trisodium polyphosphate (TSPP), citric acid, and other carboxylic acids. The polyacids used may include homopolymers and copolymers based on polycarboxylic acids (e.g., weight average molecular weights ranging from 1,000 to less than 50,000 as measured by GPC), including those that are hydrophobically or hydrophilically modified, such as polyacrylic acid or polymethacrylic acid or maleic anhydride with various monomers such as styrene, acrylate or methacrylate esters, diisobutylene, and other hydrophilic or hydrophobic comonomers; salts thereof; or mixtures thereof. The dispersants may be present in an amount of 0 to 5 wt%, 0.05 to 3 wt%, or 0.1 to 1 wt%, based on the total weight of the coating composition.
[0042] In addition to the above-mentioned components, the coating composition of the present invention may further include any one or combination of the following additives: buffering agents, neutralizing agents, humectants, mildewcides, biocides, antiskinning agents, colorants, flow agents, antioxidants, plasticizers, leveling agents, adhesion promoters, anti-flash rust additives, anti-corrosion additives, and grinding media. These additives may be present in a total amount of 0-10 wt.% or 0.1 wt.%-2 wt.% based on the total weight of the coating composition. The coating composition may also include water in an amount of 30 wt.%-90 wt.%, 40 wt.%-80 wt.%, or 50 wt.%-70 wt.% of the coating composition.
[0043] The coating composition of the present invention can be prepared by mixing the emulsion polymer with an aqueous dispersion of the polymer additive, and other optional ingredients, such as pigments and / or extenders. The components in the coating composition can be mixed in any order to provide the coating composition of the present invention. Also, any of the above optional ingredients can be added to the composition during or before mixing to form the coating composition. When the coating composition includes pigments and / or extenders, the pigments and / or extenders are preferably mixed with a dispersant to form a slurry of pigments and / or extenders.
[0044] The coating composition of the present invention can provide improved corrosion resistance to coatings made therefrom. The present invention also provides a method of improving the corrosion resistance of a substrate susceptible to corrosion, such as a metal. The method includes applying the coating composition to a metal substrate and drying or allowing the coating composition to dry to form a coating. Improved corrosion resistance means a blister rating of "6F" or higher and a surface rust rating of "7S" or even higher, preferably "7P", "9S", "9P", or "10", for a coating having a thickness of 40-50 micrometers (μm) after at least 300 hours of exposure to salt spray according to ASTM B117-2011. The coating composition can provide good stain release properties to the coating, as indicated by a stain release score of 65 or higher according to the GB / T 9780-2013 test method. Compared to binders containing structural units of ethylenically unsaturated siloxane monomers, the aqueous dispersion of the polymeric additive of the present invention can provide greater efficiency in improving the corrosion resistance and stain release properties of coating compositions containing same. For example, to achieve comparable corrosion resistance and stain release properties, the coating compositions of the present invention require a lower concentration of ethylenically unsaturated siloxane monomer structural units, based on the weight of the coating composition, than a coating composition that includes a binder that includes ethylenically unsaturated siloxane monomer structural units.
[0045] The present invention also relates to a method of producing a coating on a substrate, preferably an exterior surface, comprising applying a coating composition to the substrate and drying or allowing the applied coating composition to dry to produce a coating. The coating composition of the present invention can be applied to and adhered to a variety of substrates. Examples of suitable substrates include wood, metal, plastic, foam, stone, elastomeric substrates, glass, fabric, concrete, or cementitious substrates. The coating composition, preferably containing pigments, is suitable for a variety of applications, such as marine protective coatings, general industrial finishes, metal protective coatings, automotive coatings, traffic coatings, exterior insulation finish systems (EIFS), wood coatings, coil coatings, plastic coatings, can coatings, architectural coatings, and civil engineering coatings. The coating composition is particularly suitable for metal protective coatings and architectural coatings. The coating composition can be used as a primer, a topcoat, a one-coat direct-to-metal coating, or in combination with other coatings to form multi-layer coatings.
[0046] The present invention also provides a method for improving the corrosion resistance of a metal substrate, comprising providing a coating composition, applying the coating composition to a metal substrate, and drying or allowing the coating composition to dry to form a coating having improved corrosion resistance as defined above. The present invention also relates to a coated metal article comprising a coating having improved corrosion resistance as defined above.
[0047] The coating composition of the present invention may be applied to a substrate by conventional means, including brushing, dipping, rolling, and spraying. The coating composition is preferably applied by spraying. Standard spraying techniques and equipment for spraying, such as air atomized spraying, air atomization, airless spraying, high volume low pressure spraying, and electrostatic spraying, such as electrostatic bell application, and either manual or automatic methods can be used. After the coating composition of the present invention is applied to a substrate, the coating composition can be dried or dried at room temperature (23±2° C.) or at elevated temperatures, for example, from 35° C. to 60° C., to form a film (i.e., coating). EXAMPLES
[0048] Some embodiments of the invention will now be described in the following examples in which all parts and percentages are by weight unless otherwise specified. The following materials are used in the examples: DOWSIL32 additive (DC-32), available from The Dow Chemical Company, is a methacrylate siloxane monomer having the following structure:
[0049] [ka] (In the formula, j+k=12~25).
[0050] DISPONIL Fes993 surfactant (solids content 29%-31%) available from BASF is the sodium salt of an aliphatic polyglycol ether sulfate.
[0051] HITENOL AR1025 (25% solids content) available from Dai-ichi Kogyo Seiyaku Co., Ltd. is the ammonium salt of polyoxyethylene styrenated propenyl phenyl ether sulfate.
[0052] NATROSOL 250 HBR thickener is available from Ashland Aqualon Company.
[0053] ACRYSOL™ RM-8W thickener, available from The Dow Chemical Company, is a non-ionic urethane rheology modifier.
[0054] OROTAN™ 681 (35% solids content) and OROTAN 1288 dispersants (45% solids content), and TRITON™ EF-406 nonionic surfactant (70% solids content), are all available from The Dow Chemical Company.
[0055] AMP-95 neutralizer is available from Sinopharm.
[0056] Nopco NXZ Defoamer is available from Cognis Corporation.
[0057] Surfynol TG non-ionic wetting agent and Tego Airex 902W defoamer are both available from Evonik.
[0058] Ti-Pure R-706 pigment, available from DuPont, is a titanium dioxide pigment.
[0059] Kaolin clay (DB-80) is available from Shanxi Jinyang Calcinated Kaolin Ltd.
[0060] CC-700 extender is available from Guangfu Building Materials Group (China).
[0061] Wash clay available from HuILi (China) is used as the bulking agent.
[0062] Binder 1, Binder 2, and Binder 3 are all available from The Dow Chemical Company. Binder 1 is a 100% acrylic emulsion (solids content: 49.0% and M w : 340,000-360,000 g / mol); Binder 2 is a styrene-acrylic emulsion (solid content: 47.0%, M w : 340,000-360,000 g / mol); Binder 3 is a styrene-acrylic emulsion (solid content: 47.5%, M w :90,000~110,000g / mol).
[0063] ROPAQUE™ Ultra E opaque polymer is available from The Dow Chemical Company.
[0064] Texanol ester alcohol, available from Eastman, is used as a coalescent.
[0065] Propylene glycol is used as an antifreeze agent.
[0066] Sodium nitrite (15%) is used as a flash rust inhibitor additive.
[0067] ACRYSOL, OROTAN, TRITON, and ROPAQUE are all trademarks of The Dow Chemical Company.
[0068] The following standard analytical equipment and methods are used in the examples and for determining the properties and characteristics described herein.
[0069] GPC analysis GPC analysis was typically performed on an Agilent 1200. Samples were dissolved in tetrahydrofuran (THF) / formic acid (FA) (5%) at a concentration of 2 milligrams (mg) / mL to form a sample solution, which was then filtered through a 0.45 μm polytetrafluoroethylene (PTFE) filter before GPC analysis. GPC analysis was performed using the following conditions:
[0070] Columns: one precolumn and two mixed B columns (7.8 x 300 mm); column temperature: 35 °C; mobile phase: THF / FA (5%); flow rate: 1.0 mL / min; injection volume: 100 μm; detector: Agilent refractive index detector, 35 °C; and calibration curve: PL polystyrene (PS) Narrow standards (part number: 2010-0101) with PS equivalent molecular weight ranging from 2329000 to 162 g / mol.
[0071] Coagulum content of aqueous dispersions of polymer additives The aqueous dispersion samples were filtered through a 44 micrometer sieve. The residue remaining on the sieve was washed with water and placed in a 150°C oven for 20 minutes. The coagulum content is determined by dividing the dry weight of the residue on the sieve by the original wet weight of the aqueous polymer dispersion. The lower the coagulum content, the more stable the polymerization process is when preparing the aqueous dispersion.
[0072] Salt spray resistance test The coating composition was applied to Q-panels (cold-rolled steel) by a 150 μm applicator. The resulting coating film was dried for 7 days at 23° C. and 50% relative humidity (RH). Salt spray resistance properties were tested by exposing the as-prepared coated panels to a salt spray environment (5% sodium chloride fog) according to ASTM B117-2011. Prior to exposure, the exposed cold-rolled steel was covered with tape (3M Plastic Tape #471). A scribe mark made with a razor blade was inscribed on the bottom half of the panel obtained above just prior to exposure. The panel was exposed to the salt spray environment for a specified time and then removed from the salt spray environment. The surface of the panel was first cleaned with deionized (DI) water and then scored. The results were presented as blister / rust scores.
[0073] Blister scoring was performed according to ASTM D714-02(2009) and included numbers and / or one or more letters as shown in Table 1. The letters F, M, MD, or D are a qualitative designation of the density of the blisters. The numbers refer to the size of the blisters, with 2 being the largest size, 8 being the smallest size, and 10 being no blisters. The higher the number, the smaller the size of the blisters. The rust rating was determined by ASTM D610-2001 as shown in Tables 2 and 3. Panels with blister density ratings of "6F" or higher and "7S" or higher are acceptable ratings for the extent of rust and indicate good corrosion resistance of the coating.
[0074] [Table 1]
[0075] [Table 2]
[0076] [Table 3]
[0077] Stain removal rating A film of the test coating composition was drawn down on a black vinyl scrub chart using a 150 μm applicator and dried at constant temperature (25° C.) and humidity (50%) for 7 days before applying the stain. The stain removal properties were evaluated according to GB / T 9780-2013 (Test method for dirt pick-up resistance and stain removal of architectural coating and paint films). Each stain (vinegar, black tea, blue-black ink, water-soluble black, alcohol-soluble black, and a mixture of petrolatum and carbon black, respectively) was then applied evenly to a test area having a width of 25 millimeters (mm) and the length of the chart cross section. The liquid stain was applied on top of gauze to prevent runoff from the test area. The stain was kept on the panel and allowed to absorb for 2 hours before being wiped off with a dry tissue. The panel was then placed on a scrub tester under a weight of 1.5 kilograms (kg) at a scrub speed of 37 cycles / min using 1% Aomo powder solution. The panels were scrubbed for 200 cycles, then removed from the tester, rinsed thoroughly under running water, and hung to dry. Finally, each cleaned soiled area was evaluated by measuring the change in reflectance (X).
[0078]
number
[0079] According to the X of different stains, you can get the score (R) for each stain removal ability from the following table:
[0080] [Table 4]
[0081] The total stain removal performance score (R') was calculated as follows:
[0082]
number
[0083] A higher score indicates better stain removal performance. A total stain removal score of at least 60 is acceptable.
[0084] Synthesis of Polymer Additive (PA) Dispersion 1 ("PA Dispersion 1") A 3-liter, 5-neck flask equipped with a mechanical stirrer, nitrogen (N2) sweep, thermocouple, and condenser was charged with water (420.00 g) and Fes993 surfactant (1.95 g). The resulting solution in the flask was heated to 86° C. An initiator solution (0.65 g sodium persulfate (SPS) dissolved in 5.00 g water) was added. After 2 minutes (min), a finely stirred monomer emulsion was fed by a homogenizer containing 2-ethylhexyl acrylate (EHA, 96.00 g), DC-32 (120.00 g), ethyl acrylate (EA, 75.00 g), methacrylic acid (MAA, 9.00 g), n-dodecyl mercaptan (nDDM, 9.81 g), and Fes993 surfactant (18.30 g) in water (130.00 g). Simultaneously, initiators including SPS (0.53 g) and water (60.00 g) were co-fed over a period of 90 minutes while maintaining the flask temperature at about 86° C. After the end of the feeds, the reaction was held for 5 minutes. After cooling to 60° C., a chaser system including ferrous sulfate solution (4.00 g, 0.2% aqueous solution) and tert-butyl hydroperoxide (t-BHP, 1.18 g) in water (5.00 g), and isoascorbic acid (IAA, 0.58 g) in water (5.00 g) was added. After holding for 15 minutes, the same chaser system as above was charged again. Finally, the resulting dispersion was cooled to ambient temperature and filtered through a 325 mesh size screen (i.e., 44 micrometer sieve) to obtain PA Dispersion 1 with a total solids content of 30%.
[0085] Synthesis of PA dispersion A PA Dispersion A was prepared similarly to the synthesis of PA Dispersion 1 above, except that a monomer emulsion containing EHA (96.00 g), EA (195.00 g), MAA (9.00 g), nDDM (9.81 g), and Fes993 surfactant (18.30 g) in water (130.00 g) was used.
[0086] Synthesis of PA dispersion B PA Dispersion B was prepared similarly to the synthesis of PA Dispersion 1 above, except that a monomer emulsion containing EHA (180.00 g), DC-32 (30.00 g), EA (75.00 g), MAA (15.00 g), nDDM (9.81 g), and Fes993 surfactant (18.30 g) in water (130.00 g) was used.
[0087] Synthesis of PA dispersion 2 PA Dispersion 2 was prepared similarly to the synthesis of PA Dispersion 1 above, except that a monomer emulsion containing EHA (150.00 g), DC-32 (60.00 g), EA (75.00 g), MAA (15.00 g), nDDM (9.81 g), and Fes993 surfactant (18.30 g) in water (130.00 g) was used.
[0088] Synthesis of PA dispersion 3 PA Dispersion 3 was prepared similarly to the synthesis of PA Dispersion 1 above, except that a monomer emulsion containing EHA (126.00 g), DC-32 (90.00 g), EA (75.00 g), MAA (9.00 g), nDDM (9.81 g), and Fes993 surfactant (18.30 g) in water (130.00 g) was used.
[0089] Synthesis of PA dispersion 4 PA Dispersion 4 was prepared similarly to the synthesis of PA Dispersion 1 above, except that a monomer emulsion containing EHA (102.00 g), DC-32 (120.00 g), EA (75.00 g), MAA (3.00 g), nDDM (9.81 g), and Fes993 surfactant (18.30 g) in water (130.00 g) was used.
[0090] Synthesis of PA dispersion D PA Dispersion D was prepared similarly to the synthesis of PA Dispersion 1 above, except that the monomer emulsion containing EHA (180.00 g), DC-32 (30.00 g), EA (75.00 g), MAA (15.00 g), nDDM (9.81 g), and Fes993 surfactant (18.30 g) in water (130.00 g) was not stirred with a homogenizer before being fed to the flask.
[0091] Synthesis of PA dispersion C PA Dispersion C was prepared similarly to the synthesis of PA Dispersion 1 above, except that a monomer emulsion containing EHA (60.00 g), DC-32 (60.00 g), EA (45.00 g), MAA (135.00 g), nDDM (9.81 g), and Fes993 surfactant (18.30 g) in water (130.00 g) was used.
[0092] The properties of the resulting aqueous dispersions of the polymer additives are shown in Table 5. As shown in Table 5, PA Dispersions 1-4 all exhibited lower coagulum content compared to PA Dispersion C, which contained higher levels of acid structural units, and PA Dispersion D, which was prepared by not utilizing the homogenization process.
[0093] [Table 5]
[0094] Coating compositions of Examples (Ex) 1 to 8 and Comparative Examples (Comp) A to C The obtained polymer additive dispersions (e.g., PA Dispersions 1-4, A and B) were used to prepare coating compositions based on the formulations shown in Table 6. All ingredients in the grinding stage for preparing each coating composition were added sequentially and mixed uniformly for 30 minutes using a high-speed disperser at about 1,000 revolutions per minute (rpm) to form a grind. The ingredients in the premix in the letdown stage were mixed first, followed by the addition of the grind. Then, the PA dispersions were added at the end of the letdown stage based on the type and dosage shown in Table 7. Then, ACRYSOL RM-8W and water were further added to obtain the coating compositions. The water load was adjusted to maintain the total weight of each coating composition at 1,000 g. The obtained coating compositions were evaluated for salt spray resistance, and the results are shown in Table 7.
[0095] [Table 6]
[0096] As shown in Table 7, the coating compositions of Examples 1-8 containing 1.67% to 6.67% of PA Dispersion 1, 2, 3, or 4 (by weight based on the total weight of each coating composition) provided coatings with much better salt spray resistance than Comparative Example A after 300 hours of salt spray exposure. In contrast, Comparative Example B, which contained 10% of a polymer additive containing DC-32 structural units, exhibited poorer salt spray resistance compared to Comparative Example A and Example 1. The coating composition of Comparative Example C, which contained 8.89% of PA Dispersion 3, had poorer salt spray resistance compared to Comparative Example A.
[0097] [Table 7]
[0098] Coating Compositions of Examples 9-13 and Comparative Examples D and E The above obtained polymer additive dispersions (e.g., PA Dispersions 1, 4, and A) were used to prepare coating compositions based on the formulations shown in Table 8. All ingredients in the grinding step for preparing each coating composition were added sequentially and mixed uniformly for 30 minutes using a high-speed disperser at about 1,000 revolutions per minute (rpm) to form a mill base, followed by sequentially adding other ingredients including binder (binder 1 or 2) and PA dispersion in the dilution step to obtain the coating composition. The dosage and type of binder and PA dispersion are shown in Table 9. The obtained coating compositions were evaluated for stain removal resistance, and the results are shown in Table 9.
[0099] [Table 8]
[0100] As shown in Table 9, the coating compositions of Examples 9 and 10 containing the acrylic silicone hybrid polymer additive provided coatings with improved stain resistance compared to the coating composition of Comparative Example D. In particular, when 2.0% (by weight of the total coating composition) of PA Dispersion 1 was included, the total score for stain removal of the resulting coating composition of Example 10 was improved by 5 points compared to Comparative Example D. Furthermore, coating compositions containing Binder 2 and 1% to 2.0% of a polymer additive dispersion (PA Dispersion 1 or 4) also showed improved stain removal properties compared to the coating composition of Comparative Example E (Examples 11-13).
[0101] [Table 9]
Claims
1. 1. An aqueous dispersion of a polymeric additive having a weight average molecular weight of 2,000 to 25,000 g / mol, said polymeric additive comprising, based on the weight of said polymeric additive: (i) 20% to 85% by weight of structural units of an ethylenically unsaturated siloxane monomer of formula (I). 【Chemistry 1】 (In formula (I), R is an ethylenically unsaturated group, j and k each independently range from 0 to 100, and j+k=5 to 100), (ii) 0.1% to 10% by weight of structural units of an ethylenically unsaturated functional monomer having at least one functional group selected from an amide, ureido, carboxyl, carboxylic anhydride, hydroxyl, phosphoric acid, or sulfonic acid group, a salt thereof, or a mixture thereof; (iii) 5% to 79.9% by weight of additional ethylenically unsaturated nonionic monomer structural units; An aqueous dispersion, wherein the coagulum content of said aqueous dispersion is less than 2,000 ppm after filtering through a 44 micrometer sieve.
2. The ethylenically unsaturated siloxane monomer is represented by formula (I) where R is -CH=CH 2 , -R p -OC(=O)CH=CH 2 , or -R p -OC(=O)C(CH 3 ) = CH 2 Wherein R p is C 1 -C 6 2. The aqueous dispersion of claim 1, having a structure represented by:
3. 3. The aqueous dispersion of claim 1 or 2, wherein the polymeric additive comprises from 20% to 50% by weight of structural units of the ethylenically unsaturated siloxane monomer, based on the weight of the polymeric additive.
4. 4. The aqueous dispersion of claim 1, wherein the polymeric additive comprises from 1% to 5% by weight, based on the weight of the polymeric additive, of structural units of the ethylenically unsaturated functional monomer.
5. 5. The aqueous dispersion according to claim 1, wherein the polymer additive has a weight average molecular weight of 5,000 to 10,000 g / mol.
6. 6. The aqueous dispersion of any one of claims 1 to 5, wherein the additional monoethylenically unsaturated nonionic monomer is selected from the group consisting of acrylic monomers, styrene monomers, combinations of acrylic and styrene monomers, vinyl ester monomers, combinations of ethylene and vinyl ester monomers, vinyl silane monomers, or mixtures thereof.
7. A process for preparing the aqueous dispersion according to any one of claims 1 to 6, comprising the steps of: emulsion polymerization of a monomer mixture in the presence of a chain transfer agent, the monomer mixture comprising: 20% to 85% by weight of an ethylenically unsaturated siloxane monomer; 0.1% to 10% by weight of an ethylenically unsaturated functional monomer; and 5% to 79.9% by weight of an additional monoethylenically unsaturated nonionic monomer, based on the total weight of the monomer mixture; A process wherein the monomer mixture is emulsified and homogenized prior to polymerization.
8. 7. A coating composition comprising: (A) 0.8 wt. % to 8 wt. % of an aqueous dispersion of the polymer additive of any one of claims 1 to 6, based on a total weight of the coating composition; and (B) an emulsion polymer having a weight average molecular weight greater than 25,000 g / mol.
9. 9. The coating composition of claim 8, wherein the structural units of the ethylenically unsaturated siloxane monomer in the polymeric additive are present in an amount of 0.2 to 1.8 weight percent based on the total weight of the coating composition.
10. 9. The coating composition of claim 8 comprising 1% to 7% by weight of said polymeric additive dispersion, based on the weight of said coating composition.
Citation Information
Patent Citations
Preparation of aqueous resin dispersion
JP1993140255A
Production of diorganopolysiloxane / Acrylic ester copolymer emulsion
JP1993287217A
Production of water-base resin dispersion, and coating agent comprising same
JP1997012655A
Paper coating agent
JP1997208647A
Resin composite for thermal transfer recording and image receptive body