Removal method applied to aluminum electrode sheets having oxide layers

The method uses an ionic liquid in a nitrogen atmosphere to remove oxide layers from aluminum electrode sheets, addressing the challenges of moisture and re-oxidation, ensuring effective preparation for subsequent uses.

JP7573697B2Active Publication Date: 2024-10-25APH EPOWER CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023116769
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-11-23
Filing Date
2023-07-18
Publication Date
2024-10-25
Estimated Expiration
2043-07-18

AI Technical Summary

Technical Problem

Existing surface treatments for aluminum electrode sheets leave moisture behind and form oxide layers that are difficult to remove, which can negatively impact subsequent applications.

Method used

A method involving a dipping step in an ionic liquid in a nitrogen atmosphere to effectively remove the oxide layer from aluminum electrode sheets, using aluminum halide and imidazolium chloride, with optional heating, agitation, or vibration steps.

Benefits of technology

The method effectively removes the oxide layer while minimizing exposure to atmospheric conditions, reducing the risk of re-oxidation and moisture retention, thus enhancing the suitability for subsequent applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573697000002
    Figure 0007573697000002
  • Figure 0007573697000003
    Figure 0007573697000003
  • Figure 0007573697000004
    Figure 0007573697000004
Patent Text Reader

Abstract

To provide an oxide layer removal method including a dipping step, which is applied to an aluminum electrode sheet having the oxide layer.SOLUTION: A dipping step includes removing an oxide layer by dipping an aluminum electrode sheet in an ionic liquid so that the aluminum electrode sheet can have an exposed part 120 of aluminum metal. The dipping step is carried out in a nitrogen atmosphere.SELECTED DRAWING: Figure 1B
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a removal method, and in particular to a removal method applied to an aluminum electrode sheet having an oxide layer. [Background technology]

[0002] Generally, aluminum electrode sheets are surface-treated with acidic solutions (e.g., hydrochloric acid, sulfuric acid, nitric acid, etc.). However, this type of surface treatment tends to leave moisture behind, which may have a negative impact on subsequent applications. Furthermore, the above-mentioned surface treatment is often carried out in an atmospheric environment. Summary of the Invention [Problem to be solved by the invention]

[0003] Due to the easily oxidizable nature of the aluminum electrode sheet, even after surface treatment, the oxide layer is likely to form again, making it difficult to effectively remove the oxide layer from the aluminum electrode sheet. [Means for solving the problem]

[0004] The present invention provides a removal method applied to aluminum electrode sheets having an oxide layer, which can effectively remove the oxide layer from the aluminum electrode sheet while reducing the potential for negative impact on subsequent applications.

[0005] The removal method applied to the aluminum electrode sheet having an oxide layer of the present invention includes an immersion step, which includes immersing the aluminum electrode sheet in an ionic liquid to remove the oxide layer and leave the aluminum electrode sheet with exposed portions of aluminum metal, and the immersion step is carried out in a nitrogen atmosphere.

[0006] In one embodiment of the invention, the oxide layer is etched to produce exposed portions of aluminum metal.

[0007] In one embodiment of the invention, the water / oxygen content in the nitrogen atmosphere is less than 100 ppm.

[0008] In one embodiment of the present invention, the amount of oxide layer removed is positively correlated with the immersion time of the immersion step.

[0009] In one embodiment of the invention, the ionic liquid comprises an aluminum halide and an imidazolium chloride.

[0010] In one embodiment of the invention, the amount of aluminum halide used is equal to or greater than the amount of imidazolium chloride used.

[0011] In one embodiment of the present invention, the molar ratio of aluminum halide to imidazolium chloride is between 1-2.

[0012] In one embodiment of the invention, the aluminum halide comprises aluminum chloride.

[0013] In one embodiment of the invention, the imidazolium chloride comprises 1-ethyl-3-methylimidazolium chloride (EMIC) or 1-butyl-3-methylimidazolium chloride (BMIC).

[0014] In one embodiment of the invention, the soaking step further employs a heating step, a stirring step, a vibration step, or a combination thereof. Effect of the Invention

[0015] Based on the above, by performing the immersion step with an ionic liquid in a nitrogen atmosphere, the removal method applied to the aluminum electrode sheet having an oxide layer of the present invention avoids exposing the aluminum electrode sheet to an acidic solution and an atmospheric environment, thereby effectively removing the oxide layer from the aluminum electrode sheet while reducing the possible negative impact on subsequent applications.

[0016] In order to make the above-mentioned features and advantages of the present invention easier to understand, the following detailed description of the embodiments is given with reference to the accompanying drawings. [Brief description of the drawings]

[0017] [Figure 1A] FIG. 2 is a schematic diagram of an aluminum electrode sheet having an oxide layer that has undergone a 24 hour immersion step in one embodiment of the present invention. [Figure 1B] FIG. 2 is a schematic diagram of an aluminum electrode sheet having an oxide layer that has undergone a 48 hour immersion step in one embodiment of the present invention. [Figure 1C] FIG. 2 is a schematic diagram of an aluminum electrode sheet having an oxide layer that has not been subjected to a dipping step in some embodiments of the present invention. [Figure 1D] FIG. 1D is a schematic diagram of the aluminum electrode sheet of FIG. 1C subjected to a 24 hour immersion step in different molar ratios of aluminum halide and imidazolium chloride. [Figure 1E] FIG. 1D is a schematic diagram of the aluminum electrode sheet of FIG. 1C subjected to a 24 hour immersion step in different molar ratios of aluminum halide and imidazolium chloride. [Diagram 2] FIG. 2 is a schematic diagram of Raman spectra of an aluminum electrode sheet immersed for 0 hours and for 48 hours in one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be described in detail below with reference to the following embodiments, but the embodiments are merely examples and are not intended to limit the scope of the present invention. The present invention is defined by the claims.

[0019] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those skilled in the art. It is understood that terms (such as those defined in commonly used dictionaries) should be interpreted as having a meaning consistent with their meaning in the context of the relevant art, and should not be interpreted as idealized or overly formal unless expressly defined herein.

[0020] FIG. 1A is a schematic diagram of an aluminum electrode sheet having an oxide layer that has undergone a 24-hour immersion step in one embodiment of the present invention. FIG. 1B is a schematic diagram of an aluminum electrode sheet having an oxide layer that has undergone a 48-hour immersion step in one embodiment of the present invention. FIG. 1C is a schematic diagram of an aluminum electrode sheet having an oxide layer that has not undergone a immersion step in some embodiments of the present invention. FIG. 1D and FIG. 1E are schematic diagrams of the aluminum electrode sheet of FIG. 1C that has undergone a 24-hour immersion step in different molar ratios of aluminum halide and imidazolium chloride. FIG. 2 is a schematic diagram of Raman spectra of aluminum electrode sheets with immersion times of 0 hours and 48 hours in one embodiment of the present invention. FIG. 1A and FIG. 1B are images obtained using a digital microscope (50x). Furthermore, the experimental conditions can be, for example, 1.8:1 The experimental conditions included an ionic liquid with a molar ratio of aluminum halide to imidazolium chloride of 100%, a stirring temperature of 60 °C, and times of 24 h (Figure 1A) and 48 h (Figure 1B). In Figure 1D and Figure 1E, the aluminum halide used was aluminum chloride (AlCl 3 ), the imidazolium chloride is 1-ethyl-3-methylimidazolium chloride (EMIC), and the molar ratios of aluminum halide to imidazolium chloride are 1.3:1 and 1.8:1, respectively. Note that other unexplained contents should be obtainable and adjustable by those skilled in the art based on the contents included in the spirit and scope covered by the appended claims.

[0021] 1A, 1B and 2, in this embodiment, the removal method applied to the aluminum electrode sheet 100 having the oxide layer 110 includes a dipping step. The dipping step includes dipping the aluminum electrode sheet 100 into an ionic liquid (not shown) to remove the oxide layer 110 (light colored areas in FIGS. 1A and 1B) so that the aluminum electrode sheet 100 has an exposed portion 120 of aluminum metal (dark colored areas in FIGS. 1A and 1B), and the dipping step is performed in a nitrogen atmosphere. It should be noted that the aluminum electrode sheet 100 is formed by the aluminum metal and the oxide layer 110 formed on its surface. Thus, when the oxide layer 110 is removed, the underlying aluminum metal is exposed, thereby forming the exposed portion 120 of aluminum metal.

[0022] Thus, by performing the immersion step using an ionic liquid in a nitrogen atmosphere, the removal method applied to the aluminum electrode sheet 100 having the oxide layer 110 of this embodiment avoids exposing the aluminum electrode sheet 100 to an acidic solution and an atmospheric environment, thereby effectively removing the oxide layer 110 from the aluminum electrode sheet 100 while reducing the possibility of negative effects on subsequent applications (e.g., being placed in an aluminum battery). In this case, the oxide layer 110 is, for example, etched to produce exposed portions 120 of aluminum metal, although the invention is not limited thereto.

[0023] Furthermore, the removal method of the present embodiment is performed in a nitrogen atmosphere (e.g., in a glove box where the atmosphere can be effectively controlled). Thus, re-oxidation of the aluminum metal in an air environment can be avoided, and the oxide layer 110 can be effectively removed from the aluminum electrode sheet 100. Furthermore, since no oxidizing solution (e.g., hydrochloric acid, sulfuric acid, nitric acid, etc.) is used in the surface treatment, no moisture remains, which can reduce the possibility of negative effects on subsequent applications.

[0024] In some embodiments, the water / oxygen content in the nitrogen atmosphere is less than 100 ppm (e.g., any value less than 90 ppm, 70 ppm, 50 ppm, 30 ppm, 10 ppm, 1 ppm, or 100 ppm). In this controlled condition, the possibility of re-oxidation of the aluminum metal can be further reduced, but the invention is not limited thereto.

[0025] In some embodiments, since there is a spontaneous reaction between the ionic liquid and the oxide layer, the longer the immersion time, the greater the reaction amount and area. That is, the longer the immersion time, the greater the amount of oxide layer removed. Thus, the amount of oxide layer removed is positively correlated with the immersion time of the immersion step. For example, as shown in Figures 1A and 1B, most of the oxide layer 110 on the surface of the aluminum electrode sheet 100 is obviously removed according to the immersion time reaching 48 hours, but the present invention is not limited thereto.

[0026] In some embodiments, the ionic liquid comprises an aluminum halide and an imidazolium chloride. For example, the aluminum halide is aluminum chloride (AlCl 3 ), and the imidazolium chloride includes 1-ethyl-3-methylimidazolium chloride (EMIC) or 1-butyl-3-methylimidazolium chloride (BMIC). The ionic liquids mentioned above are AlCl 4 - , Al 2 Cl 7 - , EMI + / BMI + , Al 3 + , Al + and complexes of said ions. In addition, Al 2 Cl 7 - reacts with the oxide layer 110, 2 Cl 7 - The more is generated, the better the removal effect, but the present invention is not limited thereto.

[0027] In some embodiments, the amount of aluminum halide used is equal to or greater than the amount of imidazolium chloride used, and the molar ratio of aluminum halide to imidazolium chloride is between 1 and 2 (e.g., aluminum halide:imidazolium chloride=1:1, aluminum halide:imidazolium chloride=1.2:1, aluminum halide:imidazolium chloride=1.4:1, aluminum halide:imidazolium chloride=1.6:1, aluminum halide:imidazolium chloride=1.8:1, aluminum halide:imidazolium chloride=2:1, or any molar ratio within the ranges described above), but the invention is not limited thereto.

[0028] In some embodiments, the higher the molar ratio of aluminum halide to imidazolium chloride, the better the removal effect. For example, as shown in Figures 1C and 1D, after immersing an aluminum electrode sheet 100 in a solution with a molar ratio of aluminum halide to imidazolium chloride of 1.3:1 for 24 hours, a partially grayish white rust-like exposed portion 120 of aluminum metal appears at the position indicated by the arrow. In comparison, as shown in Figures 1C and 1E, after immersing an aluminum electrode sheet 100 in a solution with a molar ratio of aluminum halide to imidazolium chloride of 1.8:1 for 24 hours, a more pronounced grayish white rust-like exposed portion 120 of aluminum metal appears at the position indicated by the arrow, but the present invention is not limited thereto.

[0029] In addition, it can be inferred from the Raman spectrum that the removal method of the present embodiment can effectively remove the oxide layer 110 on the aluminum electrode sheet 100. For example, during the immersion step, aluminum halide is converted to aluminum chloride (AlCl 3 ) and the imidazolium chloride is 1-ethyl-3-methylimidazolium chloride (EMIC), 2 Cl 7 - reacts with the oxide layer 110. Thus, as the immersion time increases, the amount of AlCl 4 - The amount of Al increases2 Cl 7 - decreases. That is, AlCl 4 - and Al 2 Cl 7 - The molar ratio between AlCl and 1-ethyl-3-methylimidazolium chloride increases, and the molar ratio of aluminum chloride to 1-ethyl-3-methylimidazolium chloride (referred to as the AE ratio) decreases. This trend can prove that the oxide layer 110 on the surface of the aluminum electrode sheet 100 has been effectively removed. As shown in FIG. 2 and Table 1, initially, the aluminum electrode sheet 100 was immersed in the ionic liquid with an AE ratio of 1.8 (corresponding to an immersion time of 0 hours) for 48 hours, and the molar ratio between AlCl and 1-ethyl-3-methylimidazolium chloride (referred to as the AE ratio) decreased. 4 - and Al 2 Cl 7 - and the AE ratio decreases as the ratio between the AE ratio increases, but the present invention is not limited thereto.

[0030] [Table 1]

[0031] In some embodiments, the soaking step further employs a heating step, an agitation step, a vibration step, or a combination thereof to improve the removal efficiency. For example, the heating step, the agitation step, and the vibration step may be added at any time during the soaking step (at the beginning of soaking, during soaking, or at the end of soaking). Furthermore, one or more of the heating step, the agitation step, and the vibration step may be used, and the heating step, the agitation step, or the vibration step may be used alone, or a combination of the heating step and the agitation step, a combination of the agitation step, a combination of the heating step and the vibration step, or a combination of the heating step, the agitation step, and the vibration step. When the above-mentioned steps are used, each may be introduced into the soaking step at the same time or at different times, and is not limited by the present invention.

[0032] In some embodiments, a higher temperature for the heating step (e.g., greater than 60° C.) and a longer duration for the stirring or shaking step (e.g., greater than 24 hours) can achieve more effective removal of the oxide layer 110, although the invention is not so limited.

[0033] In summary, by performing the immersion step with an ionic liquid in a nitrogen atmosphere, the removal method applied to the aluminum electrode sheet having an oxide layer of the present invention avoids exposing the aluminum electrode sheet to an acidic solution and an atmospheric environment, thereby effectively removing the oxide layer from the aluminum electrode sheet while reducing the potential negative impact on subsequent applications.

[0034] Although the present invention has been described with reference to the above embodiments, these embodiments are not intended to limit the present invention. Those skilled in the art may make some changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention is defined by the appended claims. [Industrial Applicability]

[0035] The removal method of the present invention can be applied to remove an oxide layer from an aluminum electrode sheet. [Explanation of symbols]

[0036] 100: Aluminum electrode sheet 110: Oxide layer 120: Exposed aluminum metal parts

Claims

1. A removal method applied to an aluminum electrode sheet having an oxide layer, comprising the steps of: Including a soaking step, the immersion step includes immersing the aluminum electrode sheet in an ionic liquid to remove the oxide layer and cause the aluminum electrode sheet to have exposed portions of aluminum metal, the immersion step being performed in a nitrogen atmosphere. Removal method.

2. the oxide layer is etched to produce the exposed portion of the aluminum metal; The removal method according to claim 1 .

3. The water / oxygen content in the nitrogen atmosphere is less than 100 ppm; The removal method according to claim 1 .

4. The amount of removal of the oxide layer is positively correlated with the immersion time of the immersion step. The removal method according to claim 1 .

5. The ionic liquid comprises an aluminum halide and an imidazolium chloride. The removal method according to claim 1 .

6. The amount of the aluminum halide used is equal to or greater than the amount of the imidazolium chloride used. The removal method according to claim 5.

7. the molar ratio of said aluminum halide to said imidazolium chloride is between 1 and 2; The removal method according to claim 5.

8. The aluminum halide includes aluminum chloride. The removal method according to claim 5.

9. The imidazolium chloride includes 1-ethyl-3-methylimidazolium chloride or 1-butyl-3-methylimidazolium chloride. The removal method according to claim 5.

Citation Information

Patent Citations

  • Method for pickling metal with nitric acid

    JP1985121283A

  • Pretreatment of aluminum and aluminum alloy

    JP1987060884A

  • Vacuum degreasing / Washing method

    JP1996197019A

  • Production of aluminum alloy bearing

    JP1998168587A

  • Method for removal of hard coating film in superhard material, and method for production of superhard material

    JP2011179108A