Coating composition, coating laminate, and method for producing the coating laminate
A two-layer painted laminate is produced using a coating composition with specific resin and catalyst formulations, addressing adhesion, hardness, and weather resistance issues in conventional coatings, achieving enhanced performance and efficiency.
Patent Information
- Application Number
- JP2021052410
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-25
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2041-03-25
AI Technical Summary
Coating films formed from conventional thermosetting resin compositions lack sufficient adhesion, hardness, water resistance, and weather resistance.
A coating composition comprising specific hydroxyl group-containing resins, melamine resins, Lewis acid catalysts, and pigments, with predetermined mass ratios and properties, is used to form a two-layer painted laminate by simultaneously curing a first and second coating layer.
The painted laminate exhibits excellent adhesion, hardness, water resistance, and weather resistance, with improved production efficiency.
Smart Images

Figure 0007574126000008 
Figure 0007574126000001 
Figure 0007574126000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating composition, a coating laminate, and a method for making a coating laminate. [Background technology]
[0002] 2. Description of the Related Art Thermosetting resin compositions containing a polyol and an alkyl-etherified melamine resin have been used in the fields of vehicle paints and home appliance paints.
[0003] As such a thermosetting resin composition, for example, a thermosetting resin composition containing a hydroxyl group-containing resin (A), an alkyl etherified melamine resin (B), a Lewis acid catalyst (C), and a solvent (D) has been proposed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2019 / 202964 Brochure Summary of the Invention [Problem to be solved by the invention]
[0005] On the other hand, coating films formed from such thermosetting resin compositions are required to have even higher adhesion, hardness, water resistance and weather resistance.
[0006] The present invention provides a coating composition, a coating laminate, and a method for producing a coating laminate, which are excellent in adhesion, hardness, water resistance, and weather resistance. [Means for solving the problem]
[0007] The present invention [1] is a coating composition for coating a surface of a substrate, comprising a first coating composition for forming a first coating layer that covers the surface of the substrate, and a second coating composition for forming a second coating layer that covers the surface of the first coating layer, wherein the first coating composition comprises the following components (Ia) to (Id): (Ia) a hydroxyl value of 20 mgKOH / g or more and 80 mgKOH / g or less; A first hydroxyl-containing resin having an acid value of 3 mgKOH / g or more and 50 mgKOH / g or less (excluding the first melamine resin (Ib)). (Ib) A first melamine resin having an average addition number of formaldehyde per 1 mole of melamine of 3 moles or more and 6 moles or less, and modified with an alcohol having 1 to 6 carbon atoms. (Ic) A Lewis acid catalyst consisting of a metal cation with a Pauling electronegativity of 1.31 to 2.02 and a counter anion that is a deprotonated form of nitric acid. (Id) Pigment and the mass ratio of the first hydroxyl-containing resin (Ia) to the first melamine resin (Ib) (first hydroxyl-containing resin (Ia) / first melamine resin (Ib)) is 60 / 40 or more and 95 / 5 or less; The second coating composition includes the following (II-a) to (II-c), (II-a) A second hydroxyl-containing resin having a hydroxyl value of 70 mgKOH / g or more and 180 mgKOH / g or less (excluding the second melamine resin (II-b)). (II-b) A second melamine resin having an average addition number of formaldehyde per 1 mole of melamine of 3 moles or more and 6 moles or less, and modified with an alcohol having 2 to 6 carbon atoms. (II-c) A Lewis acid catalyst consisting of a metal cation with a Pauling electronegativity of 1.31 to 2.02 and a counter anion that is a deprotonated form of nitric acid. and the mass ratio of the second hydroxyl-containing resin (II-a) to the second melamine resin (II-b) (second hydroxyl-containing resin (II-a) / second melamine resin (II-b)) is 60 / 40 or more and 95 / 5 or less.
[0008] The present invention [2] includes the coating composition according to the above [1], wherein the second coating composition further includes the following (II-d): (II-d) A radical scavenger having a base dissociation constant pKb of 6 or more and 14 or less.
[0009] The present invention [3] provides a coating method for a coating composition comprising: a coating layer for coating a surface of the coating layer; and a coating layer for coating a surface of the coating layer, the coating layer being made of a coating composition for coating a surface of the coating layer. The coating composition for coating a coating layer is ... (Ia) a hydroxyl value of 20 mgKOH / g or more and 80 mgKOH / g or less; A first hydroxyl-containing resin having an acid value of 3 mgKOH / g or more and 50 mgKOH / g or less (excluding the first melamine resin (Ib)). (Ib) A first melamine resin having an average addition number of formaldehyde per 1 mole of melamine of 3 moles or more and 6 moles or less, and modified with an alcohol having 1 to 6 carbon atoms. (Ic) A Lewis acid catalyst consisting of a metal cation with a Pauling electronegativity of 1.31 to 2.02 and a counter anion that is a deprotonated form of nitric acid. (Id) Pigment a mass ratio of the first hydroxyl-containing resin (Ia) to the first melamine resin (Ib) (first hydroxyl-containing resin (Ia) / first melamine resin (Ib)) is 60 / 40 or more and 95 / 5 or less; the second coating layer is made of a second coating composition, and the second coating composition contains the following (II-a) to (II-c), (II-a) A second hydroxyl-containing resin having a hydroxyl value of 70 mgKOH / g or more and 180 mgKOH / g or less (excluding the second melamine resin (II-b)). (II-b) A second melamine resin having an average addition number of formaldehyde per 1 mole of melamine of 3 moles or more and 6 moles or less, and modified with an alcohol having 2 to 6 carbon atoms. (II-c) A Lewis acid catalyst consisting of a metal cation with a Pauling electronegativity of 1.31 to 2.02 and a counter anion that is a deprotonated form of nitric acid. The mass ratio of the second hydroxyl-containing resin (II-a) to the second melamine resin (II-b) (second hydroxyl-containing resin (II-a) / second melamine resin (II-b)) is 60 / 40 or more and 95 / 5 or less.
[0010] The present invention [4] includes the coating laminate described in the above [3], in which the substrate is made of resin.
[0011] The present invention [5] includes the coating laminate described in the above [4], wherein the resin is an acrylonitrile-styrene-butadiene copolymer resin.
[0012] The present invention [6] comprises a first step of applying a first coating composition to a surface of a substrate to form an uncured first coating layer, a second step of applying a second coating composition to the surface of the uncured first coating layer after the first step to form an uncured second coating layer, and a third step of simultaneously curing the uncured first coating layer and the uncured second coating layer, wherein the first coating composition comprises the following components (Ia) to (Id): (Ia) a hydroxyl value of 20 mgKOH / g or more and 80 mgKOH / g or less; A first hydroxyl-containing resin having an acid value of 3 mgKOH / g or more and 50 mgKOH / g or less (excluding the first melamine resin (Ib)). (Ib) A first melamine resin having an average addition number of formaldehyde per 1 mole of melamine of 3 moles or more and 6 moles or less, and modified with an alcohol having 1 to 6 carbon atoms. (Ic) A Lewis acid catalyst consisting of a metal cation with a Pauling electronegativity of 1.31 to 2.02 and a counter anion that is a deprotonated form of nitric acid. (Id) Pigment and the mass ratio of the first hydroxyl-containing resin (Ia) to the first melamine resin (Ib) (first hydroxyl-containing resin (Ia) / first melamine resin (Ib)) is 60 / 40 or more and 95 / 5 or less; The second coating composition includes the following (II-a) to (II-c), (II-a) A second hydroxyl-containing resin having a hydroxyl value of 70 mgKOH / g or more and 180 mgKOH / g or less (excluding the second melamine resin (II-b)). (II-b) A second melamine resin having an average addition number of formaldehyde per 1 mole of melamine of 3 moles or more and 6 moles or less, and modified with an alcohol having 2 to 6 carbon atoms. (II-c) A Lewis acid catalyst consisting of a metal cation with a Pauling electronegativity of 1.31 to 2.02 and a counter anion that is a deprotonated form of nitric acid. and a mass ratio of the second hydroxyl-containing resin (II-a) to the second melamine resin (II-b) (second hydroxyl-containing resin (II-a) / second melamine resin (II-b)) is 60 / 40 or more and 95 / 5 or less.
[0013] The present invention [7] includes the method for producing a coated laminate described in the above [6], in which the substrate is made of resin.
[0014] The present invention [8] includes the method for producing a coating laminate described in the above [7], wherein the material of the resin film is an acrylonitrile-styrene-butadiene copolymer resin. Effect of the Invention
[0015] In the coating composition of the present invention, the first coating composition and the second coating composition each have a specific composition, so that a coating laminate having excellent adhesion, hardness, water resistance, and weather resistance can be produced.
[0016] In the coating laminate of the present invention, the first coating layer and the second coating layer are made of a first coating composition and a second coating composition, respectively, each having a specific composition, and therefore have excellent adhesion, hardness, water resistance, and weather resistance.
[0017] In the method for producing a coated laminate of the present invention, the uncured first coating layer and the uncured second coating layer are cured simultaneously, which results in excellent production efficiency. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 shows one embodiment of a method for producing a coating laminate of the present invention. FIG. 1A shows a first step of preparing an object to be coated. FIG. 1B shows a first step of arranging an uncured first coating layer on the surface (one side in the thickness direction) of the object to be coated. FIG. 1C shows a second step of arranging an uncured second coating layer on the surface (one side in the thickness direction) of the uncured first coating layer. FIG. 1D shows a third step of simultaneously curing the uncured first coating layer and the uncured second coating layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] <Coating Composition> The coating composition of the present invention is used to coat the surface of an object 2 to be coated, as will be described in detail later.
[0020] The coating composition includes a first coating composition and a second coating composition. More specifically, the first coating composition and the second coating composition are compositions for forming the first coating layer 3 and the second coating layer 4, respectively. In other words, a mixture of the first coating composition and the second coating composition does not form the first coating layer 3 or the second coating layer 4.
[0021] <First coating composition> The first coating composition, which will be described in detail later, is a composition for forming a first coating layer that covers the surface of the body 2 to be coated.
[0022] The first coating composition includes (Ia) a first hydroxyl-containing resin, (Ib) a first melamine resin, (Ic) a Lewis acid catalyst, and (Id) a pigment.
[0023] <First hydroxyl group-containing resin> The first hydroxyl-containing resin is a resin having a predetermined acid value and a predetermined hydroxyl value. Examples of the first hydroxyl-containing resin include hydroxyl-containing acrylic resin, hydroxyl-containing polyester resin, hydroxyl-containing epoxy resin, and hydroxyl-containing urethane resin, and preferably, hydroxyl-containing acrylic resin. Note that the first hydroxyl-containing resin does not include the first melamine resin described later.
[0024] In the first hydroxyl-containing resin, the hydroxyl-containing acrylic resin is a polymerization product of the first polymerization component.
[0025] The first polymerization component is a monomer component. More specifically, the first polymerization component is a polymerizable component (monomer component) capable of radical polymerization (vinyl polymerization).
[0026] The first polymerization component contains a (meth)acrylic acid ester, an acidic group-containing vinyl monomer, a hydroxyl group-containing vinyl monomer, and, if necessary, a copolymerizable monomer copolymerizable therewith.
[0027] Examples of the (meth)acrylic acid ester include alkyl esters of (meth)acrylic acid having 1 to 12 carbon atoms. Examples of the alkyl ester of (meth)acrylic acid having 1 to 12 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, and benzyl (meth)acrylate. Of these, preferred are alkyl esters of (meth)acrylic acid having 1 to 8 carbon atoms, more preferred are alkyl esters of (meth)acrylic acid having 1 to 6 carbon atoms, and even more preferred are methyl methacrylate and n-butyl acrylate. The (meth)acrylic acid ester includes an acrylic acid ester and / or a methacrylic acid ester.
[0028] The (meth)acrylic acid esters can be used alone or in combination of two or more kinds.
[0029] The acidic group-containing vinyl monomer is blended into the first polymerization component from the viewpoint of dispersing the pigment (described later). Examples of the acidic group-containing vinyl monomer include a carboxyl group-containing vinyl monomer and a sulfonic acid group-containing vinyl monomer.
[0030] The carboxyl group-containing vinyl monomer may be a monocarboxylic acid, a dicarboxylic acid, or a salt thereof. The monocarboxylic acid may be, for example, (meth)acrylic acid. The dicarboxylic acid may be, for example, itaconic acid, maleic acid, fumaric acid, itaconic anhydride, maleic anhydride, and fumaric anhydride.
[0031] Examples of the sulfonic acid group-containing vinyl monomer include sulfonic acid or a salt thereof. Examples of the sulfonic acid include allyl sulfonic acid, methallyl sulfonic acid, and acrylamido t-butyl sulfonic acid. Examples of the salt of the sulfonic acid include, for example, an alkali metal salt (e.g., sodium salt, potassium salt) and an ammonium salt of the above sulfonic acid. Specific examples include sodium allyl sulfonate, sodium methallyl sulfonate, and ammonium methallyl sulfonate.
[0032] The acidic group-containing vinyl monomer is preferably a carboxyl group-containing vinyl monomer, more preferably a monocarboxylic acid, further preferably (meth)acrylic acid, particularly preferably methacrylic acid.
[0033] The acidic group-containing vinyl monomers can be used alone or in combination of two or more kinds.
[0034] Examples of hydroxyl group-containing vinyl monomers include hydroxymethyl(meth)acrylate, 2-hydroxyethyl(meth)acrylate, and 2-hydroxypropyl(meth)acrylate, preferably 2-hydroxyethyl(meth)acrylate, and more preferably 2-hydroxyethyl(meth)acrylate.
[0035] Examples of the copolymerizable monomer include functional group-containing vinyl monomers (excluding acidic group-containing vinyl monomers and hydroxyl group-containing vinyl monomers; the same applies below), vinyl esters, aromatic vinyl monomers, N-substituted unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, α-olefins, and dienes.
[0036] Examples of functional group-containing vinyl monomers include amino group-containing vinyl monomers, cyano group-containing vinyl monomers, glycidyl group-containing vinyl monomers, and acetoacetoxy group-containing vinyl monomers.
[0037] Examples of amino group-containing vinyl monomers include 2-aminoethyl (meth)acrylate, 2-(N-methylamino)ethyl (meth)acrylate, and 2-(N,N-dimethylamino)ethyl (meth)acrylate.
[0038] An example of the cyano group-containing vinyl monomer is (meth)acrylonitrile.
[0039] An example of the glycidyl group-containing vinyl monomer is glycidyl (meth)acrylate.
[0040] An example of an acetoacetoxy group-containing vinyl monomer is acetoacetoxyethyl (meth)acrylate.
[0041] Examples of vinyl esters include vinyl acetate and vinyl propionate.
[0042] Aromatic vinyl monomers include, for example, styrene and α-methylstyrene.
[0043] An example of the N-substituted unsaturated carboxylic acid amide is N-methylol (meth)acrylamide.
[0044] An example of the heterocyclic vinyl compound is vinylpyrrolidone.
[0045] Examples of vinylidene halide compounds include vinylidene chloride and vinylidene fluoride.
[0046] Examples of α-olefins include ethylene and propylene.
[0047] An example of the dienes is butadiene.
[0048] Additionally, the copolymerizable monomer may include a crosslinkable vinyl monomer.
[0049] Examples of crosslinkable vinyl monomers include compounds containing two or more vinyl groups. Examples of compounds containing two or more vinyl groups include methylene bis(meth)acrylamide, divinylbenzene, polyethylene glycol chain-containing di(meth)acrylate, trimethylolpropane tetraacrylate, pentaerythritol triacrylate, and pentaerythritol tetraacrylate.
[0050] The copolymerizable monomers can be used alone or in combination of two or more kinds.
[0051] In the first polymerization component, the mixing ratio of the (meth)acrylic acid ester relative to 100 parts by mass of the first polymerization component is, for example, 70 parts by mass or more, preferably 80 parts by mass or more, and for example, 95 parts by mass or less, preferably 90 parts by mass or less.
[0052] The mixing ratio of the acidic group-containing vinyl monomer is, for example, 0.1 parts by mass or more, preferably 1 part by mass or more, and for example, 10 parts by mass or less, preferably 5 parts by mass or less, and more preferably 3 parts by mass or less, relative to 100 parts by mass of the first polymerization component.
[0053] When the mixing ratio of the acidic group-containing vinyl monomer is within the above-mentioned range, the acid value (described later) of the first hydroxyl group-containing resin can be adjusted to a predetermined range described later.
[0054] The mixing ratio of the hydroxyl group-containing vinyl monomer is, for example, 3 parts by mass or more, preferably 10 parts by mass or more, and for example, 20 parts by mass or less, preferably 15 parts by mass or less, and more preferably 12 parts by mass or less, relative to 100 parts by mass of the first polymerization component.
[0055] When the blending ratio of the hydroxyl group-containing vinyl monomer is within the above-mentioned range, the hydroxyl value (described later) of the first hydroxyl group-containing resin can be adjusted to a predetermined range described later.
[0056] The mixing ratio of the copolymerizable monomer relative to 100 parts by mass of the first polymerization component is, for example, 0.1 parts by mass or more and, for example, 10 parts by mass or less.
[0057] The first polymerization component preferably does not contain a copolymerizable monomer, and contains a (meth)acrylic acid ester, an acidic group-containing vinyl monomer, and a hydroxyl group-containing vinyl monomer, and more preferably the first polymerization component consists of a (meth)acrylic acid ester, an acidic group-containing vinyl monomer, and a hydroxyl group-containing vinyl monomer.
[0058] The hydroxyl-containing acrylic resin is obtained by polymerizing the first polymerization component.
[0059] The polymerization method is not particularly limited, and examples of the polymerization method include bulk polymerization and solution polymerization, and preferably includes solution polymerization.
[0060] When solution polymerization is employed as the polymerization method, the first polymerization component and, if necessary, a polymerization initiator are mixed in a solvent and polymerized.
[0061] The solvent may be a known solvent, such as an alkyl ester (e.g., butyl acetate) or an alcohol (isobutanol).
[0062] In addition, commercially available products can also be used as the solvent, such as the T-Sol series (aromatic hydrocarbons, manufactured by ENEOS Corporation).
[0063] The solvents can be used alone or in combination of two or more kinds.
[0064] The polymerization initiator may, for example, be a peroxide-based radical polymerization initiator (eg, t-butylperoxy-2-ethylhexanoate).
[0065] The mixing ratio of the polymerization initiator is appropriately set depending on the purpose and application.
[0066] As for the polymerization conditions, the polymerization temperature is, for example, 70° C. or more and, for example, 120° C. or less, and the polymerization time is, for example, 1 hour or more and, for example, 12 hours or less.
[0067] This gives a hydroxyl group-containing acrylic resin.
[0068] The hydroxyl value of the first hydroxyl-containing resin is 20 mgKOH / g or more, preferably 40 mgKOH / g or more, and 80 mgKOH / g or less, preferably 60 mgKOH / g or less.
[0069] When the hydroxyl value is equal to or greater than the lower limit, the crosslink density is improved, so that a first coating layer 3 having excellent water resistance can be obtained.
[0070] Furthermore, when the hydroxyl value is equal to or less than the upper limit, an increase in cure shrinkage of the first coating layer 3 can be suppressed, so that a first coating layer 3 having excellent adhesion can be obtained.
[0071] Although details will be described later, the hydroxyl value of the first hydroxyl-containing resin is preferably set to be smaller than the hydroxyl value of the second hydroxyl-containing resin (described later).
[0072] The hydroxyl value can be determined, for example, by JIS K 0070-1992 (acetylation method) (the same applies below).
[0073] The acid value of the first hydroxyl-containing resin is 3 mgKOH / g or more, preferably 7 mgKOH / g or more, and 50 mgKOH / g or less, preferably 30 mgKOH / g or less, more preferably 20 mgKOH / g or less.
[0074] When the acid value is equal to or higher than the lower limit, a first coating composition having excellent pigment dispersibility can be obtained.
[0075] When the acid value is equal to or less than the upper limit, a first coating layer 3 having excellent water resistance can be obtained.
[0076] The acid value can be determined, for example, by JIS K 0070-1992 (potentiometric titration method) (the same applies below).
[0077] The weight average molecular weight (Mw) of the first hydroxyl group-containing resin in terms of polystyrene, measured by gel permeation chromatography (GPC), is, for example, 5,000 or more, preferably 8,000 or more, more preferably 10,000 or more, and for example, 200,000 or less, preferably 100,000 or less, more preferably 80,000 or less, even more preferably 40,000 or less, particularly preferably 30,000 or less, and most preferably 25,000 or less.
[0078] If the weight average molecular weight is within the above range, a first coating layer 3 that is excellent in paintability, appearance, strength, hardness and abrasion resistance can be formed.
[0079] The glass transition temperature of the first hydroxyl group-containing resin is, for example, -30°C or higher, preferably -20°C or higher, more preferably 0°C or higher, even more preferably 5°C or higher, and for example, 80°C or lower, preferably 60°C or lower, more preferably 50°C or lower, even more preferably 30°C or lower.
[0080] If the glass transition temperature is within the above range, a first coating layer 3 having excellent coatability, hardness and water resistance can be formed.
[0081] The method for measuring the glass transition temperature will be described in detail in the Examples below (the same applies hereinafter).
[0082] <First melamine resin> The first melamine resin is an alkyl-etherified melamine resin obtained by modifying (alkyl-etherifying) at least a portion of the methylol groups of a melamine resin obtained from melamine and formaldehyde with an alcohol.
[0083] Formaldehyde can be prepared as an aqueous solution, or solid paraformaldehyde can be used as formaldehyde.
[0084] When formaldehyde is prepared as an aqueous solution, its concentration is, for example, 80% or more and, for example, 99% or less.
[0085] In the first melamine resin, the alcohol is an alcohol having 1 to 6 carbon atoms. On the other hand, when the alcohol is an alcohol having 7 or more carbon atoms, the alcohol does not volatilize during heat curing, and the curability of the first coating composition decreases, resulting in a problem that the hardness and water resistance decrease. Examples of the alcohol having 1 to 6 carbon atoms include linear monohydric alcohols having 1 to 6 carbon atoms and branched monohydric alcohols having 1 to 6 carbon atoms. Examples of the linear monohydric alcohols having 1 to 6 carbon atoms include methanol, ethanol, n-propanol, n-butanol, n-pentanol, and n-hexanol. Examples of the branched monohydric alcohols having 1 to 6 carbon atoms include isopropanol, isobutanol, sec-butanol, and tert-butanol.
[0086] The alcohol is preferably a linear monohydric alcohol having 1 to 6 carbon atoms, more preferably a linear monohydric alcohol having 1 to 4 carbon atoms, further preferably methanol, ethanol, and n-butanol, and particularly preferably ethanol.
[0087] The alcohols can be used alone or in combination of two or more kinds.
[0088] To obtain the first melamine resin, first, melamine and formaldehyde are subjected to a methylolation reaction to obtain a melamine resin.
[0089] To carry out a methylolation reaction between melamine and formaldehyde, melamine and formaldehyde are mixed together. Specifically, formaldehyde is mixed so that the average addition number of formaldehyde per 1 mole of melamine is 3 moles or more, preferably 4 moles or more and 6 moles or less.
[0090] When the average addition number is equal to or greater than the lower limit, the crosslink density can be improved, and water resistance can be improved.
[0091] On the other hand, if the average number of additions is less than the lower limit, the water resistance decreases.
[0092] The average number of additions may be, for example, 13 This can be calculated by C-NMR analysis (same below).
[0093] When formaldehyde is added to all three amino groups of melamine, the average number of formaldehyde added is 6 moles.
[0094] In the methylolation reaction, alcohol is preliminarily mixed together with melamine and formaldehyde. The mixing ratio of the alcohol is, for example, 4 mol or more, preferably 6 mol or more, and for example, 8 mol or less, per mol of melamine.
[0095] After the methylolation reaction, an acid catalyst is added, and at least a portion of the methylol groups of the melamine resin is modified with an alcohol (alkyl etherification).
[0096] Examples of the acid catalyst include organic acids and inorganic acids. Examples of the organic acids include formic acid, oxalic acid, and paratoluenesulfonic acid. Examples of the inorganic acids include phosphoric acid, hydrochloric acid, sulfuric acid, and nitric acid. Examples of the acid catalyst include preferably organic acids, more preferably paratoluenesulfonic acid.
[0097] The acid catalysts can be used alone or in combination of two or more kinds.
[0098] The mixing ratio of the acid catalyst is appropriately set depending on the purpose and application.
[0099] As for reaction conditions, the reaction temperature is, for example, 60° C. or higher and, for example, 120° C. or lower, and the reaction time is, for example, 1 hour or higher and, for example, 12 hours or lower.
[0100] A neutralizing agent (eg, sodium hydroxide) is then added to neutralize the reaction product.
[0101] This results in a first melamine resin. The first melamine resin is a melamine resin in which the average number of formaldehyde added per 1 mole of melamine is 3 to 6 moles, and the melamine resin is modified with an alcohol having 1 to 6 carbon atoms.
[0102] The first melamine resin has a weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography (GPC) of, for example, 800 or more, preferably 1000, more preferably 1100 or more, even more preferably 1800 or more, and for example, 15000 or less, preferably 7000 or less, more preferably 5000 or less, even more preferably 2500 or less.
[0103] If the weight average molecular weight is within the above range, a first coating layer 3 excellent in mechanical properties, smoothness, and appearance can be formed.
[0104] <Lewis acid catalyst> The Lewis acid catalyst consists of a cation and a counter anion.
[0105] The cation is a metal cation having a Pauling electronegativity of 1.31 or more and 2.02 or less. More specifically, the Pauling electronegativity is 1.31 or more, preferably 1.50 or more, more preferably 1.60 or more, and 2.02 or less, preferably 1.80 or less.
[0106] If the electronegativity is equal to or higher than the above lower limit, a first coating layer 3 excellent in water resistance, hardness, and weather resistance can be formed.
[0107] When the electronegativity is equal to or less than the upper limit, the water resistance, hardness, and weather resistance are excellent.
[0108] Examples of metals having a Pauling electronegativity of 1.31 or more and 2.02 or less include magnesium, manganese, aluminum, cobalt, nickel, tin, zinc, copper, and bismuth, and preferably include manganese, aluminum, nickel, and zinc, and more preferably include aluminum.
[0109] The counter anion is the deprotonated form of nitric acid.
[0110] Specific examples of such Lewis acid catalysts include magnesium nitrate, manganese nitrate, aluminum nitrate, cobalt nitrate, nickel nitrate, tin nitrate, zinc nitrate, copper nitrate, and bismuth sulfate, and preferably, manganese nitrate, aluminum nitrate, and nickel nitrate, and more preferably, aluminum nitrate.
[0111] <Pigments> Examples of the pigment include color pigments, luster pigments, and extender pigments.
[0112] Examples of color pigments include titanium oxide, zinc oxide, carbon black, cadmium red, molybdenum red, chrome yellow, chromium oxide, Prussian blue, cobalt blue, azo pigments, phthalocyanine pigments, quinacridone pigments, isoindoline pigments, threne pigments, and perylene pigments.
[0113] Examples of the luster pigment include aluminum powder, aluminum paste, mica powder, and mica powder coated with titanium oxide.
[0114] Examples of extender pigments include talc, clay, kaolin, baryta, barium sulfate, barium carbonate, calcium carbonate, and alumina white.
[0115] As the pigment, preferably, a glittering pigment is used, from the viewpoint of improving dispersibility by an acidic group-containing vinyl monomer (preferably, a carboxyl group-containing vinyl monomer), and more preferably, an aluminum paste is used.
[0116] The pigments can be used alone or in combination of two or more kinds.
[0117] <Preparation of first coating composition> The first coating composition is obtained by mixing a first hydroxyl-containing resin, a first melamine resin, a Lewis acid catalyst, and a pigment.
[0118] Furthermore, when a solvent is used in preparing the first hydroxyl-containing resin and the first melamine resin, the first coating composition contains the solvent.
[0119] If necessary, known additives can be blended into the first coating composition.
[0120] In the first coating composition, the mass ratio of the first hydroxyl-containing resin (Ia) to the first melamine resin (Ib) (first hydroxyl-containing resin (Ia) / first melamine resin (Ib)) is 60 / 40 or more, preferably 70 / 30 or more, and for example, 95 / 5 or less.
[0121] If the mass ratio is equal to or greater than the lower limit, a first coating layer 3 excellent in water resistance, hardness, and weather resistance can be formed.
[0122] If the mass ratio is equal to or less than the upper limit, a first coating layer 3 excellent in water resistance, hardness, and weather resistance can be formed.
[0123] The mixing ratio of the first hydroxyl group-containing resin is, for example, 50 parts by mass or more, preferably 60 parts by mass or more, and more preferably 70 parts by mass or more, and for example, 90 parts by mass or less, preferably 80 parts by mass or less, per 100 parts by mass of the total amount of the first hydroxyl group-containing resin, the first melamine resin, the Lewis acid catalyst, and the pigment (hereinafter, the first component).
[0124] The blending ratio of the first melamine resin is, per 100 parts by mass of the first component, for example, 5 parts by mass or more, preferably 10 parts by mass or more, preferably 15 parts by mass or more, and for example, 40 parts by mass or less, preferably 30 parts by mass or less, and more preferably 20 parts by mass or less.
[0125] The mixing ratio of the Lewis acid catalyst is, per 100 mass of the total amount of the first hydroxyl group-containing resin and the first melamine resin, for example, 0.01 parts by mass or more, preferably 0.1 parts by mass or more, and for example, 5 parts by mass or less, preferably 4 parts by mass or less.
[0126] The mixing ratio of the Lewis acid catalyst is, per 100 parts by mass of the first component, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and for example, 10 parts by mass or less, preferably 5 parts by mass or less, and more preferably 1 part by mass or less.
[0127] When the blending ratio of the Lewis acid catalyst is within the above range, a first coating composition having excellent storage stability and low-temperature curing property can be obtained.
[0128] The blending ratio of the pigment, relative to 100 parts by mass of the total amount of the first hydroxyl group-containing resin, the first melamine resin, and the Lewis acid catalyst, is, for example, 1 part by mass or more, preferably 2 parts by mass or more, more preferably 5 parts by mass or more, and for example, 200 parts by mass or less, preferably 100 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, and particularly preferably 10 parts by mass or less.
[0129] The mixing ratio of the pigment is, for example, 0.5 parts by mass or more, preferably 3 parts by mass or more, and for example, 10 parts by mass or less, preferably 5 parts by mass or less, relative to 100 parts by mass of the first component.
[0130] Although described in detail below, the first coating layer 3 is obtained by applying a first coating composition to the surface (one surface in the thickness direction) of the body 2 to be coated and then curing the composition.
[0131] <Second Coating Composition> The second coating composition is a composition for forming the second coating layer 4 that covers the surface of the first coating layer 3, which will be described in detail later.
[0132] The second coating composition comprises (II-a) a second hydroxyl-containing resin, (II-b) a second melamine resin, (II-c) a Lewis acid catalyst, and, optionally, (II-d) a radical scavenger.
[0133] <Secondary hydroxyl group-containing resin> The second hydroxyl-containing resin is a resin having a predetermined hydroxyl value. More specifically, the second hydroxyl-containing resin has a hydroxyl value different from that of the first hydroxyl-containing resin. In addition, as described below, when the second coating layer 4 is a clear layer, the second coating composition does not contain a pigment, so that the dispersibility of the pigment is not required. Therefore, in such a case, the second hydroxyl-containing resin does not need an acid value.
[0134] The second hydroxyl-containing resin may be the same as the resin exemplified as the first hydroxyl-containing resin, and preferably is a hydroxyl-containing acrylic resin. Note that the second hydroxyl-containing resin does not include the second melamine resin described below.
[0135] In the second hydroxyl-containing resin, the hydroxyl-containing acrylic resin is the polymerization product of the second polymerization component.
[0136] The second polymerization component is a monomer component. More specifically, the second polymerization component is a polymerizable component (monomer component) capable of radical polymerization (vinyl polymerization).
[0137] The second polymerization component includes a (meth)acrylic acid ester, a hydroxyl group-containing vinyl monomer, and optionally an acid group-containing vinyl monomer, and optionally a copolymerizable monomer that can be copolymerized with them. As described above, the second hydroxyl group-containing resin may not require an acid value. Therefore, the acid group-containing vinyl monomer is an optional component.
[0138] The (meth)acrylic acid ester is the same as that exemplified for the first hydroxyl group-containing resin, and preferably, an alkyl ester of (meth)acrylic acid having 1 to 8 carbon atoms, more preferably, an alkyl ester of (meth)acrylic acid having 1 to 6 carbon atoms, and further preferably, methyl methacrylate and n-butyl acrylate.
[0139] The hydroxyl group-containing vinyl monomer is the same as that exemplified for the first hydroxyl group-containing resin, and preferably, 2-hydroxyethyl (meth)acrylate, more preferably, 2-hydroxyethyl methacrylate, is used.
[0140] Examples of the acidic group-containing vinyl monomer include those exemplified for the first hydroxyl group-containing resin, and preferably, the acidic group-containing vinyl monomer is a carboxyl group-containing vinyl monomer, more preferably, the monocarboxylic acid, even more preferably, the (meth)acrylic acid, and particularly preferably, the methacrylic acid.
[0141] The copolymerizable monomers are the same as those exemplified for the first hydroxyl group-containing resin.
[0142] In the second polymerization component, the blending ratio of the (meth)acrylic acid ester is, for example, 60 parts by mass or more, preferably 70 parts by mass or more, and for example, 95 parts by mass or less, preferably 90 parts by mass or less, more preferably 80 parts by mass or less, relative to 100 parts by mass of the second polymerization component. The blending ratio of the (meth)acrylic acid ester in the second polymerization component is preferably set to be smaller than the blending ratio of the (meth)acrylic acid ester in the first polymerization component.
[0143] The mixing ratio of the hydroxyl group-containing vinyl monomer relative to 100 parts by mass of the second polymerization component is, for example, 12 parts by mass or more, preferably 20 parts by mass or more, more preferably 25 parts by mass or more, and for example, 40 parts by mass or less, preferably 30 parts by mass or less.
[0144] When the blending ratio of the hydroxyl-containing vinyl monomer is within the above-mentioned range, the hydroxyl value (described later) of the second hydroxyl-containing resin can be adjusted to a predetermined range described later.
[0145] The mixing ratio of the hydroxyl-containing vinyl monomer in the second polymerization component is preferably set to be greater than the mixing ratio of the hydroxyl-containing vinyl monomer in the first polymerization component, thereby making it possible to make the hydroxyl value of the second hydroxyl-containing resin greater than the hydroxyl value of the first hydroxyl-containing resin.
[0146] The mixing ratio of the acidic group-containing vinyl monomer relative to 100 parts by mass of the second polymerization component is, for example, 0.1 parts by mass or more and, for example, 8 parts by mass or less, preferably 5 parts by mass or less.
[0147] When the mixing ratio of the acidic group-containing vinyl monomer is within the above-mentioned range, the acid value (described later) of the second hydroxyl group-containing resin can be adjusted to a predetermined range described later.
[0148] The mixing ratio of the acidic group-containing vinyl monomer in the second polymerization component is preferably set to be smaller than the mixing ratio of the acidic group-containing vinyl monomer in the first polymerization component, thereby making it possible to make the acid value of the second hydroxyl-containing resin smaller than the acid value of the first hydroxyl-containing resin.
[0149] The mixing ratio of the copolymerizable monomer relative to 100 parts by mass of the second polymerization component is, for example, 0.1 parts by mass or more and, for example, 10 parts by mass or less.
[0150] The second polymerization component preferably does not contain a copolymerizable monomer, but contains a (meth)acrylic acid ester, a hydroxyl group-containing vinyl monomer, and an acidic group-containing vinyl monomer, and more preferably consists of a (meth)acrylic acid ester, a hydroxyl group-containing vinyl monomer, and an acidic group-containing vinyl monomer.
[0151] The hydroxyl-containing acrylic resin is obtained by polymerizing the second polymerization component.
[0152] In the polymerization, the polymerization method, polymerization conditions, type of solvent, and type of polymerization initiator are the same as those exemplified for the first hydroxyl group-containing resin.
[0153] This gives a hydroxyl group-containing acrylic resin.
[0154] The hydroxyl value of the second hydroxyl-containing resin is 70 mgKOH / g or more, preferably 90 mgKOH / g or more, more preferably 110 mgKOH / g or more, and is 180 mgKOH / g or less, preferably 140 mgKOH / g or less.
[0155] When the hydroxyl value is equal to or greater than the lower limit, the crosslink density is improved, making it possible to obtain the second coating layer 4 having excellent water resistance.
[0156] Furthermore, when the hydroxyl value is equal to or less than the upper limit, an increase in cure shrinkage of the first coating layer 3 can be suppressed, so that a second coating layer 4 having excellent adhesion can be obtained.
[0157] As will be described in detail later, the hydroxyl value of the second hydroxyl-containing resin is preferably set to be greater than the hydroxyl value of the first hydroxyl-containing resin.
[0158] The acid value of the second hydroxyl group-containing resin is, for example, 0 mgKOH / g or more, preferably 0.5 mgKOH / g or more, more preferably 1 mgKOH / g or more, and for example, 50 mgKOH / g or less, preferably 30 mgKOH / g or less, more preferably 20 mgKOH / g, even more preferably 10 mgKOH / g or less, and particularly preferably 5 mgKOH / g or less.
[0159] When the acid value of the second hydroxyl-containing resin is within the above range, a second coating composition having excellent compatibility and curability can be obtained.
[0160] In addition, the acid value of the second hydroxyl-containing resin is preferably set to be smaller than the acid value of the first hydroxyl-containing resin.
[0161] The weight average molecular weight (Mw) of the secondary hydroxyl group-containing resin, measured by gel permeation chromatography (GPC) in terms of polystyrene, is, for example, 5,000 or more, preferably 8,000 or more, more preferably 10,000 or more, and for example, 200,000 or less, preferably 100,000 or less, more preferably 80,000 or less, even more preferably 40,000 or less, and particularly preferably 25,000 or less.
[0162] If the weight average molecular weight is within the above range, it is possible to form a second coating layer 4 that is excellent in paintability, appearance, strength, hardness and abrasion resistance.
[0163] The glass transition temperature of the second hydroxyl group-containing resin is, for example, -30°C or higher, preferably -20°C or higher, more preferably 0°C or higher, even more preferably 5°C or higher, and for example, 80°C or lower, preferably 60°C or lower, more preferably 30°C or lower, even more preferably 20°C or lower.
[0164] If the glass transition temperature is within the above range, a second coating layer 4 having excellent coatability, hardness and water resistance can be formed.
[0165] <Second melamine resin> The second melamine resin is an alkyl-etherified second melamine resin obtained by modifying (alkyl-etherifying) at least a portion of the methylol groups of a melamine resin obtained from melamine and formaldehyde with an alcohol.
[0166] As the formaldehyde, the same formaldehyde as exemplified for the first melamine resin can be used.
[0167] In the second melamine resin, the alcohol is an alcohol having 2 to 6 carbon atoms. On the other hand, when the alcohol is an alcohol having 7 or more carbon atoms, the alcohol does not volatilize during heat curing, and the curability of the second coating composition decreases, resulting in a problem that the hardness and water resistance decrease. Examples of the alcohol having 2 to 6 carbon atoms include linear monohydric alcohols having 2 to 6 carbon atoms and branched monohydric alcohols having 2 to 6 carbon atoms. Examples of the linear monohydric alcohols having 2 to 6 carbon atoms include ethanol, n-propanol, n-butanol, n-pentanol, and n-hexanol. Examples of the branched monohydric alcohols having 2 to 6 carbon atoms include isopropanol, isobutanol, sec-butanol, and tert-butanol.
[0168] The alcohol is preferably a linear monohydric alcohol having 2 to 6 carbon atoms, more preferably a linear monohydric alcohol having 2 to 4 carbon atoms, still more preferably ethanol and n-butanol, and particularly preferably n-butanol. That is, particularly preferably, the alcohol in the second melamine resin is selected to have a larger carbon number than the alcohol in the first melamine resin. This improves water resistance.
[0169] The alcohols can be used alone or in combination of two or more kinds.
[0170] The second melamine resin can be obtained in the same manner as the first melamine resin described above.
[0171] In this method, the average number of formaldehyde added per mole of melamine is 3 moles or more, preferably 4 moles or more and 6 moles or less, which provides excellent water resistance, hardness, and weather resistance.
[0172] When the average number of additions is equal to or greater than the lower limit, the crosslink density can be improved, and the second coating layer 4 having excellent water resistance, hardness, and weather resistance can be formed.
[0173] In this method, the blending ratio of the alcohol, the acid catalyst, and the reaction conditions are the same as those exemplified for the first melamine resin.
[0174] This results in a second melamine resin. The second melamine resin is a melamine resin in which the average number of formaldehyde added per 1 mole of melamine is 3 to 6 moles, and the melamine resin is modified with an alcohol having 2 to 6 carbon atoms.
[0175] The second melamine resin has a weight average molecular weight (Mw) in terms of polystyrene measured by GPC of, for example, 800 or more, preferably 1000, more preferably 1100 or more, even more preferably 1800 or more, and for example, 15000 or less, preferably 7000 or less, more preferably 5000 or less, even more preferably 2500 or less.
[0176] If the weight average molecular weight is within the above range, it is possible to form a second coating layer 4 that is excellent in mechanical properties, smoothness, and appearance.
[0177] <Lewis acid catalyst> Examples of the Lewis acid catalyst include those exemplified for the first melamine resin and Lewis acid catalysts, and preferred examples include manganese nitrate, aluminum nitrate, nickel nitrate, and zinc nitrate, and more preferred examples include aluminum nitrate.
[0178] <Radical scavenger> The radical scavenger is used as a radical chain inhibitor that captures active radical species generated during the deterioration process of the second coating layer 4.
[0179] Examples of the radical scavenger include hindered piperidines. Also, known polymerizable light stabilizers can be used as the radical scavenger.
[0180] The base dissociation constant pKb of the radical scavenger is, for example, 6 or more, preferably 7.5 or more, more preferably 8.5 or more, and for example, 14 or less.
[0181] If the base dissociation constant pKb is within the above range, the acid-base reaction with the Lewis acid catalyst can be suppressed, and active radical species generated during the deterioration process of the second coating layer 4 can be captured to an extent that does not impair the catalytic activity.
[0182] Commercially available radical scavengers can also be used, including Tinuvin 249 (pKb=8.0), Tinuvin 152 (pKb=7.0 and 9.4), Tinuvin 123 (pKb=9.6) (all manufactured by BASF), HOSTAVIN 3058LIQ (manufactured by Clariant), and Adeka STAB LA-81 (manufactured by ADEKA).
[0183] <Preparation of second coating composition> The second coating composition is obtained by mixing a second hydroxyl-containing resin, a second melamine resin, a Lewis acid catalyst, and, if necessary, a radical scavenger.
[0184] Furthermore, when a solvent is used in preparing the second hydroxyl-containing resin and the second melamine resin, the second coating composition contains the solvent.
[0185] Furthermore, the second coating composition may contain known additives (for example, an ultraviolet absorbing agent) if necessary.
[0186] The ultraviolet absorbing agent is preferably one that can suppress coloring caused by complex formation with Lewis acid catalyst. Such ultraviolet absorbing agents include, for example, cyanoacrylate-based ultraviolet absorbing agents and triazine-based ultraviolet absorbing agents. Cyanoacrylate-based ultraviolet absorbing agents include, for example, Uvinul 3030, Uvinul 3035, Uvinul 3039C (manufactured by BASF), and SEESORB 501, SEESORB 502 (manufactured by Shipro Chemicals). Examples of triazine-based ultraviolet absorbers include ADK STAB LA-46 and ADK STAB LA-F70 (manufactured by ADEKA CORPORATION), Tinvin 400, Tinvin 405, Tinvin 460, Tinvin 477, and Tinvin 479 (manufactured by BASF SE), KEMISORB 102 (manufactured by Chemipro Chemical Co., Ltd.), EVERSORB 40, EVERSORB 41FD, and EVERSORB 45 (manufactured by Everlight Chemical Co., Ltd.).
[0187] In the second coating composition, the mass ratio of the second hydroxyl-containing resin (II-a) to the second melamine resin (II-b) (second hydroxyl-containing resin (II-a) / second melamine resin (II-b)) is 60 / 40 or more, preferably 70 / 30 or more, and for example, 95 / 5 or less.
[0188] If the mass ratio is equal to or greater than the lower limit, a second coating layer 4 having excellent water resistance, hardness, and weather resistance can be formed.
[0189] When the mass ratio is equal to or less than the upper limit, a second coating layer 4 having excellent water resistance, hardness, and weather resistance can be formed.
[0190] The mixing ratio of the second hydroxyl group-containing resin is, for example, 50 parts by mass or more, preferably 60 parts by mass or more, more preferably 70 parts by mass or more, and for example, 90 parts by mass or less, preferably 80 parts by mass or less, per 100 parts by mass of the total amount of the second hydroxyl group-containing resin, the second melamine resin, the Lewis acid catalyst, and the radical scavenger (hereinafter, the second component).
[0191] The blending ratio of the second melamine resin is, per 100 parts by mass of the second component, for example, 5 parts by mass or more, preferably 10 parts by mass or more, preferably 15 parts by mass or more, and for example, 40 parts by mass or less, preferably 30 parts by mass or less, and more preferably 20 parts by mass or less.
[0192] The mixing ratio of the Lewis acid catalyst is, relative to 100 mass of the total amount of the second hydroxyl group-containing resin and the second melamine resin, for example, 0.01 part by mass or more, preferably 0.1 part by mass or more, and for example, 5 parts by mass or less, preferably 4 parts by mass or less.
[0193] The mixing ratio of the Lewis acid catalyst is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and for example, 10 parts by mass or less, preferably 5 parts by mass or less, and more preferably 1 part by mass or less, per 100 parts by mass of the second component.
[0194] When the blending ratio of the Lewis acid catalyst is within the above range, a second coating composition having excellent storage stability and low-temperature curing property can be obtained.
[0195] The mixing ratio of the radical scavenger is, for example, 0.1 part by mass or more, preferably 0.5 part by mass or more, and for example, 10 parts by mass or less, preferably 5 parts by mass or less, and more preferably 1 part by mass or less, per 100 parts by mass of the second component.
[0196] Although described in detail below, the second coating layer 4 is obtained by applying a second coating composition to the surface (one surface in the thickness direction) of the first coating layer 3 and curing it.
[0197] <Method of manufacturing a coating laminate (method of using a coating composition)> The coating composition is used to coat the surface of the substrate 2. By coating the substrate 2, a coating laminate is produced.
[0198] With reference to FIG. 1, one embodiment of the method for producing a coating laminate of the present invention will be described.
[0199] In Fig. 1, the up-down direction of the paper is the up-down direction (thickness direction), the upper side of the paper is the upper side (one side in the thickness direction), and the lower side of the paper is the lower side (the other side in the thickness direction). The left-right direction and the depth direction of the paper are surface directions perpendicular to the up-down direction. Specifically, they follow the directional arrows in each figure.
[0200] The manufacturing method of the coating laminate 1 comprises a first step of applying a first coating composition to the surface (one side in the thickness direction) of the body 2 to form an uncured first coating layer 3; after the first step, a second step of applying a second coating composition to the surface (one side in the thickness direction) of the uncured first coating layer 3 to form an uncured second coating layer 4; and a third step of simultaneously curing the uncured first coating layer 3 and the uncured second coating layer 4.
[0201] In the first step, an uncured first coating layer 3 is disposed on the surface (one surface in the thickness direction) of the body 2 to be coated.
[0202] In the first step, as shown in FIG. 1A, first, an object to be coated 2 is prepared.
[0203] The object 2 is an object to be coated, the surface (one surface in the thickness direction) of which is imparted with various physical properties by the first coating layer 3 and the second coating layer 4.
[0204] In FIG. 1A, the object to be coated 2 has a flat plate shape, but the shape of the object to be coated 2 is not particularly limited, and various shapes can be selected.
[0205] The object 2 to be coated may be, for example, a resin or a metal.
[0206] Examples of the resin include polyester resin, (meth)acrylic resin (including acrylic resin and / or methacrylic resin), polyolefin resin, polycarbonate resin, polyamide resin, polyimide resin, acrylonitrile-styrene-butadiene copolymer resin (ABS resin), polystyrene resin, polyvinylidene chloride, styrene-acrylonitrile copolymer resin, and cellulose acetate. Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of the (meth)acrylic resin include polymethyl methacrylate resin (PMMA). Examples of the polyolefin resin include polyethylene resin and polypropylene resin.
[0207] Examples of metals include iron, aluminum, zinc, and stainless steel.
[0208] From the viewpoints of workability and light weight, the material of the body 2 to be coated is preferably a resin, and more preferably an acrylonitrile-styrene-butadiene copolymer resin (ABS resin).
[0209] In particular, the first coating layer 3 and the second coating layer 4 are formed from a first coating composition containing a first melamine resin and a second coating composition containing a second melamine resin, respectively, and therefore can be cured at a low temperature (for example, 60°C or higher and 100°C or lower). Therefore, even a resin with low heat resistance can be selected as the coated body 2.
[0210] Next, to place an uncured first coating layer 3 on the surface (one side in the thickness direction) of the substrate 2, a first coating composition is applied to the surface (one side in the thickness direction) of the substrate 2 as shown in FIG. 1B, and if the first coating composition contains a solvent, it is dried as necessary.
[0211] This makes it possible to dispose the uncured first coating layer 3 on the surface (one side in the thickness direction) of the body 2. In other words, the surface (one side in the thickness direction) of the body 2 can be covered with the uncured first coating layer 3.
[0212] In the second step, an uncured second coating layer 4 is disposed on the surface (one surface in the thickness direction) of the uncured first coating layer 3.
[0213] To place an uncured second coating layer 4 on the surface (one side in the thickness direction) of the uncured first coating layer 3, as shown in FIG. 1C, a second coating composition is applied to the surface (one side in the thickness direction) of the uncured first coating layer 3, and if the first coating composition contains a solvent, it is dried as necessary.
[0214] This makes it possible to dispose the uncured second coating layer 4 on the surface (one side in the thickness direction) of the uncured first coating layer 3. In other words, the surface (one side in the thickness direction) of the uncured first coating layer 3 can be covered with the uncured second coating layer 4.
[0215] In the third step, the uncured first coating layer 3 and the uncured second coating layer 4 are cured simultaneously.
[0216] Specifically, as shown in FIG. 1D, the uncured first coating layer 3 and the uncured second coating layer 4 are heated, for example, at a temperature of 60° C. or higher and 100° C. or lower, to simultaneously cure the uncured first coating layer 3 and the uncured second coating layer 4.
[0217] This results in a coating laminate 1. As shown in FIG. 1D, in the coating laminate 1, the surface (one side in the thickness direction) of the object 2 is covered with the first coating layer 3 (after curing), and the surface (one side in the thickness direction) of the first coating layer 3 (after curing) is covered with the second coating layer 4 (after curing). That is, the coating laminate 1 includes the object 2, the first coating layer 3 that covers the surface (one side in the thickness direction) of the object 2, and the second coating layer 4 that covers the surface (one side in the thickness direction) of the first coating layer 3. Specifically, the coating laminate 1 includes the object 2, the first coating layer 3 that is directly disposed on the surface (one side in the thickness direction) of the object 2, and the second coating layer 4 that is directly disposed on the surface (one side in the thickness direction) of the first coating layer 3.
[0218] The first coating layer 3 has a film shape and is disposed over the entire lower surface of the second coating layer 4 so as to be in contact with the lower surface of the second coating layer 4.
[0219] The first coating layer 3 is formed from a first coating composition as described above.
[0220] The first coating layer 3 is a paint layer containing a pigment and also a primer layer.
[0221] The first coating layer 3 has a thickness of, for example, 5 μm or more and, for example, 40 μm or less.
[0222] The second coating layer 4 has a film shape. The second coating layer 4 is disposed over the entire upper surface of the first coating layer 3 so as to be in contact with the upper surface of the first coating layer 3. The second coating layer 4 is the uppermost layer of the coating laminate 1.
[0223] The second coating layer 4 is formed from a second coating composition as described above.
[0224] The second coating layer 4 is a protective layer (top coat layer) and is preferably a clear layer that does not contain a pigment.
[0225] The second coating layer 4 has a thickness of, for example, 5 μm or more and, for example, 40 μm or less.
[0226] Furthermore, the ratio of the thickness of the first coating layer 3 to the thickness of the second coating layer 4 (thickness of the first coating layer 3 / thickness of the second coating layer 4) is, for example, 0.1 or more, preferably 0.3 or more, and for example, 1.5 or less, preferably 1.0 or less.
[0227] <Action and effect> In the coating composition, the first coating composition and the second coating composition each have a specific composition, so that a coating laminate 1 having excellent adhesion, hardness, water resistance, and weather resistance can be produced.
[0228] Specifically, in the coating laminate 1, adhesion is ensured particularly by the first coating layer 3, while hardness, water resistance, and weather resistance are ensured particularly by the second coating layer 4. This makes it possible to ensure adhesion, hardness, water resistance, and weather resistance in the entire first coating layer 3 and second coating layer 4.
[0229] Specifically, the hydroxyl value of the first hydroxyl-containing resin in the first coating layer 3 (first coating composition) is set to be relatively smaller than the hydroxyl value of the second hydroxyl-containing resin in the second coating layer 4 (second coating composition).
[0230] Thereby, the first coating layer 3 having a low cross-link density ensures adhesion, while the second coating layer 4 having a high cross-link density ensures hardness, water resistance, and weather resistance.
[0231] In the method for producing the coating laminate 1, the uncured first coating layer 3 and the uncured second coating layer 4 are cured simultaneously, which results in excellent production efficiency.
[0232] In the coating laminate 1, the first coating layer 3 and the second coating layer 4 are made of a first coating composition and a second coating composition, respectively, having a predetermined composition, and therefore have excellent adhesion, hardness, water resistance, and weather resistance.
[0233] The coating composition can be suitably used, in particular, as a precoat paint (coating agent). The coating composition and the coating laminate 1 obtained by using the coating composition can be used in various industrial applications such as home appliance applications and vehicle applications, and can be suitably used, in particular, in vehicle applications (for example, the exterior of motorcycles). EXAMPLES
[0234] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are based on mass unless otherwise specified. In addition, the specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit value (numerical value defined as "less than or equal to" or "less than") or lower limit value (numerical value defined as "more than or equal to" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".
[0235] 1.Details of ingredients The trade names and abbreviations of the components used in each Production Example, each Example, and each Comparative Example are described in detail below.
[0236] MMA: Methyl methacrylate n-BA: n-butyl acrylate HEMA: 2-hydroxyethyl methacrylate MAC: Methacrylic acid PBO: t-Butyl peroxy-2-ethylhexanoate, trade name "Perbutyl O", manufactured by NOF Corporation T-SOL100: Aromatic hydrocarbons, manufactured by ENEOS Corporation Tinuvin123: Radical scavenger, base dissociation constant pKb=9.6, manufactured by BASF Tinuvin 249: base dissociation constant pKb = 8.0, manufactured by BASF Tinuvin 292: base dissociation constant pKb = 5.1, manufactured by BASF Tinuvin 144: base dissociation constant pKb = 5.5, manufactured by BASF Tinuvin 405: UV absorber, manufactured by BASF Tinuvin 384: UV absorber, manufactured by BASF
[0237] 2. Production of first hydroxyl group-containing resin or second hydroxyl group-containing resin Manufacturing Example 1 A four-neck flask equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet tube was charged with 51 g of T-SOL100 and 51 g of iso-butanol, and the temperature was raised to 100°C while degassing with nitrogen. Next, a solution containing 50 g of MMA, 41.5 g of n-BA, 7.0 g of HEMA, 1.5 g of MAC, and 2.0 g of PBO was added dropwise over 4 hours, and the mixture was aged for 1 hour to obtain a first hydroxyl group-containing resin (I-a1). The solid content was 50% by mass.
[0238] Manufacturing Example 2 to Manufacturing Example 9 A first hydroxyl-containing resin was obtained in the same manner as in Production Example 1. However, the compounding recipe was changed according to Table 1.
[0239] Manufacturing Example 10 to Manufacturing Example 13 A secondary hydroxyl group-containing resin was obtained in the same manner as in Production Example 1. However, the compounding recipe was changed according to Table 2.
[0240] 3. Manufacturing of the first melamine resin or the second melamine resin Manufacturing Example 14 A four-neck flask equipped with a stirrer, a thermometer, a reflux condenser and a nitrogen inlet tube was charged with 126 g (1.0 mol) of melamine, 196 g (6.0 mol) of paraformaldehyde with a formalin concentration of 92% and 519 g (7.0 mol) of n-butanol, and the temperature was raised to the reflux temperature. A methylolation reaction was carried out at the reflux temperature for 1 hour. 0.45 g (0.53 mmol) of a 20% aqueous solution of paratoluenesulfonic acid was added, and an alkylation reaction was carried out for 3 hours while dehydrating under reflux. Thereafter, the reaction product was neutralized with 0.16 g (0.80 mmol) of a 20% sodium hydroxide solution. Next, the solvent was distilled off under reduced pressure, and the mixture was diluted with n-butanol until the solid content concentration was 60% by mass. This resulted in a first melamine resin (I-b1).
[0241] Manufacturing Example 15 to Manufacturing Example 19 A first melamine resin was obtained in the same manner as in Production Example 14. However, the compounding recipe was changed according to Table 3.
[0242] Manufacturing Example 20 to Manufacturing Example 24 A second melamine resin was obtained in the same manner as in Production Example 14. However, the compounding recipe was changed according to Table 4.
[0243] In addition, as the first melamine resin (I-b5), a product name "Cymel 370" (manufactured by Daicel-Allnex Corporation, solvent: isobutanol, solid content: 88%, average number of formaldehyde added per 1 mol of melamine was 5.8 mol, and melamine resin (methylated melamine resin) modified with methanol) was prepared.
[0244] In addition, as the second melamine resin (II-b3'), a product name "Cymel 303" (manufactured by Daicel Allnex Corporation, solid content: 98%, average number of formaldehyde added per 1 mol of melamine is 5.9 mol, and melamine resin (methylated melamine resin) modified with methanol) was prepared.
[0245] 4. Manufacturing of coating laminate Examples 1 to 24 and Comparative Examples 1 to 21
[0246] <Preparation of first coating composition> A first coating composition was prepared by mixing a first hydroxyl-containing resin, a first melamine resin, a Lewis acid catalyst, and a pigment according to the formulations shown in Tables 5 to 7. In Tables 5 to 7, the values of the first hydroxyl-containing resin, the first melamine resin, the Lewis acid catalyst, and the pigment are the values of the solid content.
[0247] <Preparation of second coating composition> A second coating composition was prepared by mixing a second hydroxyl-containing resin, a second melamine resin, a Lewis acid catalyst, a radical scavenger, and an ultraviolet absorber according to the formulations shown in Tables 5 to 7. In Tables 5 to 7, the values of the second hydroxyl-containing resin, the second melamine resin, the Lewis acid catalyst, the radical scavenger, and the ultraviolet absorber are the values of the solid content.
[0248] <Production of coating laminate> [1st step] A 2 mm thick ABS resin was prepared as the object to be coated.
[0249] Next, the first coating composition was applied to one surface in the thickness direction of the body to be coated, and dried at 25° C. to provide an uncured first coating layer.
[0250] [Second process] A second coating composition was applied to one surface in the thickness direction of the uncured first coating layer, and dried at 25° C. to form an uncured second coating layer.
[0251] [3rd step] The uncured first coating layer and the uncured second coating layer were heated at 70° C. for 20 minutes and cured simultaneously.
[0252] In this way, a coating laminate was obtained. In the coating laminate, the first coating layer had a thickness of 20 μm, and the second coating layer had a thickness of 20 μm.
[0253] 5. Evaluation <Acid value> The acid value of the first hydroxyl-containing resin and the second hydroxyl-containing resin of each production example was measured according to JIS K 0070-1992 (potentiometric titration method). The results are shown in Tables 1 and 2.
[0254] <Hydroxyl value> The hydroxyl values of the first hydroxyl-containing resin and the second hydroxyl-containing resin of each production example were measured according to JIS K 0070-1992 (acetylation method). The results are shown in Tables 1 and 2.
[0255] <Weight average molecular weight> The weight average molecular weight of the first hydroxyl-containing resin, the second hydroxyl-containing resin, the first melamine resin, and the second melamine resin of each production example was measured based on the GPC method under the following measurement conditions. The results are shown in Tables 1 to 4. Detector: Differential refractometer (RI) Columns: TSKgel G7000 x 1, TSKgel G4000 x 2, TSKgel G2000 x 1 (all manufactured by Tosoh Corporation) Mobile phase: tetrahydrofuran (THF) Column temperature: 25℃ Flow rate: 0.6ml / min Sample concentration: 20 mg / mL (tetrahydrofuran solution) Injection volume: 10μl
[0256] The weight average molecular weight was calculated using a calibration curve prepared from monodisperse standard polystyrene.
[0257] <Glass transition temperature> For the first hydroxyl-containing resin and the second hydroxyl-containing resin of each Production Example, calculations were made according to the FOX formula shown in the following formula (1). 1 / Tg=W1 / Tg1+W2 / Tg2+···+W n / Tg n (1)
[0258] In the above formula (1), Tg is the glass transition temperature (K) of n types of the first or second polymerization components (monomers), W1, W2, W n is the mass fraction of each monomer, W1+W2+···+W n = 1. Also, Tg1, Tg2, Tg n is the glass transition temperature (K) of the homopolymer of each monomer.
[0259] For the glass transition temperature of the homopolymer of the monomer, values described in literature can be used, such as those described in the Mitsubishi Rayon Co., Ltd. Acrylic Ester Catalog (1997 edition) and Kyozo Kitaoka, "New Polymer Library 7: Introduction to Synthetic Resins for Paints," Polymer Publishing Association, pp. 168-169. The results are shown in Tables 1 and 2.
[0260] <Average number of formaldehyde molecules added> For the first melamine resin and the second melamine resin in each production example, the average number of formaldehyde added per 1 mole of melamine is 13 The results were measured by C-NMR, and are shown in Tables 3 and 4.
[0261] <Pigment dispersibility> Each of the first coating compositions was allowed to stand at 25° C. for 24 hours. Thereafter, the state of the first coating composition was visually observed. The pigment dispersibility was evaluated based on the following criteria. The results are shown in Tables 5 to 7. [standard] ⊚: No pigment sedimentation was observed. ◯: Sedimentation of the pigment was observed, but the pigment could be redispersed by stirring. ×: Sedimentation of the pigment was observed, and the pigment did not disperse even with stirring.
[0262] <Metal corrosivity> A zinc phosphate-treated steel sheet was immersed in each of the first coating composition and the second coating composition maintained at 40°C for 24 hours, and the state of the zinc phosphate-treated steel sheet after removal was visually observed. Metal corrosivity was evaluated based on the following criteria. The results are shown in Tables 5 to 7. [standard] ◯: No coloring was observed on the steel sheet. ×: Coloring due to rust was observed on the steel sheet.
[0263] <Adhesion> In accordance with JIS K5400 8.5.2:1990, the coating laminates of each Example and Comparative Example were cut with a knife in a grid pattern with a width of 1 mm vertically and horizontally so as to reach the substrate. An adhesive tape was then adhered to the surface, and the coating state after instantaneous peeling was visually observed. The adhesion was evaluated based on the following criteria. The results are shown in Tables 5 to 7. [standard] ◯: No peeling or chipping of the coating was observed. ×: Peeling and chipping of the coating film were observed over the entire surface.
[0264] <Water resistance> The coated laminates of each of the Examples and Comparative Examples were immersed in warm water maintained at 40° C. for 8 hours, and then removed and visually observed. Water resistance was evaluated based on the following criteria. The results are shown in Tables 5 to 7. [standard] ◎: No abnormalities such as whitening were observed. ○: Slight bleaching was observed, but the bleaching disappeared within 12 hours. ×: Significant whitening occurred, and the whitening did not disappear.
[0265] <Pencil hardness> In accordance with JIS K 5600-5-4, a pencil lead was placed at an angle of about 45° against the coating laminate of each Example and Comparative Example, and the pencil lead was moved forward at a uniform speed of about 10 mm while being pressed against the test coating plate surface hard enough not to break the lead. The hardness symbol of the hardest pencil that did not cause any scratches on the coating film was recorded as the pencil hardness. The results are shown in Tables 5 to 7.
[0266] <Gloss> The 60 degree gloss of the coated test pieces was measured in accordance with JIS K 5600-4-7. The gloss was evaluated based on the following criteria. The results are shown in Tables 5 to 7. [standard] ◯: The 60 degree gloss value was 90 or more. ×: The 60 degree gloss value was less than 90.
[0267] <Weather resistance> In accordance with JIS D 0205, the coating laminates of each of the Examples and Comparative Examples were tested for 500 hours at a black panel temperature of 63±3°C, and the change in color difference (ΔE) from the coating test piece at 0 hours of testing was measured. Weather resistance was evaluated based on the following criteria. The results are shown in Tables 5 to 7. [standard] ◎:0≦ΔE≦1.5 ○:1.5<ΔE≦3.0 ×:3.0<ΔE
[0268] [Table 1]
[0269] [Table 2]
[0270] [Table 3]
[0271] [Table 4]
[0272] [Table 5]
[0273] [Table 6]
[0274] [Table 7] [Explanation of symbols]
[0275] 1. Paint laminate 2 Object to be painted 3 First coating layer 4 Second Coating Layer
Claims
1. A coating composition for coating a surface of an object to be coated, comprising: a first coating composition for forming a first coating layer that covers the surface of the substrate; and a second coating composition for forming a second coating layer that covers a surface of the first coating layer; The first coating composition includes the following components (I-a) to (I-d): (I-a) a hydroxyl value of 20 mgKOH / g or more and 80 mgKOH / g or less; A first hydroxyl-containing resin having an acid value of 3 mgKOH / g or more and 50 mgKOH / g or less (excluding the first melamine resin (I-b)). (I-b) A first melamine resin in which the average number of formaldehyde added per 1 mol of melamine is 3 mol or more and 6 mol or less, and which is modified with an alcohol having 1 to 6 carbon atoms. (I-c) A Lewis acid catalyst comprising a cation made of a metal having a Pauling electronegativity of 1.31 or more and 2.02 or less and a counter anion which is a deprotonated form of nitric acid. (I-d) Pigment and the mass ratio of the first hydroxyl-containing resin (Ia) to the first melamine resin (Ib) (first hydroxyl-containing resin (Ia) / first melamine resin (Ib)) is 60 / 40 or more and 95 / 5 or less; The second coating composition includes the following (II-a) to (II-c): (II-a) A second hydroxyl-containing resin having a hydroxyl value of 70 mgKOH / g or more and 180 mgKOH / g or less (excluding the second melamine resin (II-b)). (II-b) A second melamine resin in which the average number of formaldehyde added per 1 mol of melamine is 3 mol or more and 6 mol or less, and which is modified with an alcohol having 2 to 6 carbon atoms. (II-c) A Lewis acid catalyst comprising a cation made of a metal having a Pauling electronegativity of 1.31 or more and 2.02 or less and a counter anion which is a deprotonated form of nitric acid. and the mass ratio of the second hydroxyl-containing resin (II-a) to the second melamine resin (II-b) (second hydroxyl-containing resin (II-a) / second melamine resin (II-b)) is 60 / 40 or more and 95 / 5 or less; A coating composition, wherein the first hydroxyl-containing resin has a hydroxyl value that is less than the hydroxyl value of the second hydroxyl-containing resin.
2. The coating composition according to claim 1 , wherein the second coating composition further comprises the following (II-d): (II-d) A radical scavenger having a base dissociation constant pKb of 6 or more and 14 or less.
3. A coating method for a coating composition comprising: a coating object; a first coating layer that coats a surface of the coating object; and a second coating layer that coats a surface of the first coating layer, the first coating layer comprises a first coating composition; The first coating composition includes the following components (I-a) to (I-d): (I-a) a hydroxyl value of 20 mgKOH / g or more and 80 mgKOH / g or less; A first hydroxyl-containing resin having an acid value of 3 mgKOH / g or more and 50 mgKOH / g or less (excluding the first melamine resin (I-b)). (I-b) A first melamine resin in which the average number of formaldehyde added per 1 mol of melamine is 3 mol or more and 6 mol or less, and which is modified with an alcohol having 1 to 6 carbon atoms. (I-c) A Lewis acid catalyst comprising a cation made of a metal having a Pauling electronegativity of 1.31 or more and 2.02 or less and a counter anion which is a deprotonated form of nitric acid. (I-d) Pigment and the mass ratio of the first hydroxyl-containing resin (Ia) to the first melamine resin (Ib) (first hydroxyl-containing resin (Ia) / first melamine resin (Ib)) is 60 / 40 or more and 95 / 5 or less; the second coating layer comprises a second coating composition; The second coating composition includes the following (II-a) to (II-c): (II-a) A second hydroxyl-containing resin having a hydroxyl value of 70 mgKOH / g or more and 180 mgKOH / g or less (excluding the second melamine resin (II-b)). (II-b) A second melamine resin in which the average number of formaldehyde added per 1 mol of melamine is 3 mol or more and 6 mol or less, and which is modified with an alcohol having 2 to 6 carbon atoms. (II-c) A Lewis acid catalyst comprising a cation made of a metal having a Pauling electronegativity of 1.31 or more and 2.02 or less and a counter anion which is a deprotonated form of nitric acid. and the mass ratio of the second hydroxyl-containing resin (II-a) to the second melamine resin (II-b) (second hydroxyl-containing resin (II-a) / second melamine resin (II-b)) is 60 / 40 or more and 95 / 5 or less; A coating laminate, wherein the hydroxyl value of the first hydroxyl-containing resin is smaller than the hydroxyl value of the second hydroxyl-containing resin.
4. The coating laminate according to claim 3 , wherein the object to be coated is a resin.
5. 5. The coating laminate according to claim 4, wherein the resin is an acrylonitrile-styrene-butadiene copolymer resin.
6. A first step of applying a first coating composition to a surface of an object to be coated to provide an uncured first coating layer; a second step, subsequent to the first step, of disposing an uncured second coating layer on the surface of the uncured first coating layer by applying a second coating composition; and a third step of simultaneously curing the uncured first coating layer and the uncured second coating layer, The first coating composition includes the following components (I-a) to (I-d): (I-a) a hydroxyl value of 20 mgKOH / g or more and 80 mgKOH / g or less; A first hydroxyl-containing resin having an acid value of 3 mgKOH / g or more and 50 mgKOH / g or less (excluding the first melamine resin (I-b)). (I-b) A first melamine resin in which the average number of formaldehyde added per 1 mol of melamine is 3 mol or more and 6 mol or less, and which is modified with an alcohol having 1 to 6 carbon atoms. (I-c) A Lewis acid catalyst comprising a cation made of a metal having a Pauling electronegativity of 1.31 or more and 2.02 or less and a counter anion which is a deprotonated form of nitric acid. (I-d) Pigment and the mass ratio of the first hydroxyl-containing resin (Ia) to the first melamine resin (Ib) (first hydroxyl-containing resin (Ia) / first melamine resin (Ib)) is 60 / 40 or more and 95 / 5 or less; The second coating composition includes the following (II-a) to (II-c): (II-a) A second hydroxyl-containing resin having a hydroxyl value of 70 mgKOH / g or more and 180 mgKOH / g or less (excluding the second melamine resin (II-b)). (II-b) A second melamine resin in which the average number of formaldehyde added per 1 mol of melamine is 3 mol or more and 6 mol or less, and which is modified with an alcohol having 2 to 6 carbon atoms. (II-c) A Lewis acid catalyst comprising a cation made of a metal having a Pauling electronegativity of 1.31 or more and 2.02 or less and a counter anion which is a deprotonated form of nitric acid. and the mass ratio of the second hydroxyl-containing resin (II-a) to the second melamine resin (II-b) (second hydroxyl-containing resin (II-a) / second melamine resin (II-b)) is 60 / 40 or more and 95 / 5 or less; A method for producing a coating laminate, wherein the hydroxyl value of the first hydroxyl-containing resin is smaller than the hydroxyl value of the second hydroxyl-containing resin.
7. The method for producing a coated laminate according to claim 6, wherein the object to be coated is a resin.
8. The method for producing a coated laminate according to claim 7, wherein the material of the resin film is an acrylonitrile-styrene-butadiene copolymer resin.
Citation Information
Patent Citations
Method for multiple-layer top coating
JP1999207255A
Method for formation of multi-layered coating film and coated article
JP2009028607A
Formation method of laminate coating film
JP2015112565A
Thermosetting resin composition, coating material for pre-coated metal, cured product, and laminate