Silicon carbide semiconductor device and method for manufacturing silicon carbide semiconductor device
The silicon carbide semiconductor device addresses nitrogen concentration and thickness variations in the n-type buffer layer by using a layered structure and proton introduction, enhancing manufacturing efficiency and performance stability.
Patent Information
- Application Number
- JP2020143180
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-08-27
AI Technical Summary
The challenge in silicon carbide semiconductor devices is the difficulty in controlling nitrogen concentration and thickness variations in the high concentration n-type buffer layer, leading to increased manufacturing costs, double Shockley stacking faults, and voltage deterioration due to high nitrogen concentrations.
A silicon carbide semiconductor device with a layered structure and proton or helium introduction to control hole concentration, reducing the need for a high concentration n-type buffer layer, thereby suppressing stacking faults and maintaining consistent impurity concentrations.
The solution effectively reduces manufacturing costs, prevents stacking fault expansion, and maintains consistent performance by controlling hole concentration and reducing proton irradiation damage to the gate insulating film.
Smart Images

Figure 0007574575000001 
Figure 0007574575000002 
Figure 0007574575000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a silicon carbide semiconductor device and a method for manufacturing a silicon carbide semiconductor device. [Background technology]
[0002] Silicon carbide (SiC) is expected to be a next-generation semiconductor material to replace silicon (Si). Compared to conventional semiconductor elements that use silicon carbide as a semiconductor material, semiconductor elements that use silicon carbide as a semiconductor material (hereinafter referred to as silicon carbide semiconductor devices) have various advantages, such as the ability to reduce the resistance of the element in the on-state to one-hundredth of that of conventional semiconductor elements that use silicon as a semiconductor material, and the ability to be used in higher temperature environments (200°C or higher). This is due to the characteristics of the material itself, namely, that the band gap of silicon is about three times larger than that of silicon, and that the dielectric breakdown field strength is nearly one order of magnitude larger than that of silicon.
[0003] Silicon carbide semiconductor devices that have been commercially available to date include Schottky barrier diodes (SBDs) and vertical MOSFETs (metal oxide semiconductor field effect transistors) having a planar gate structure or a trench gate structure.
[0004] The planar gate structure is a MOS gate structure in which a MOS gate is provided in a flat plate shape on the front surface of a semiconductor substrate. The trench gate structure is a MOS gate structure in which a MOS gate is embedded in a trench formed on the front surface of a semiconductor substrate (semiconductor chip), and a channel (inversion layer) is formed along the sidewall of the trench in a direction perpendicular to the front surface of the semiconductor substrate. Therefore, compared to a planar gate structure in which a channel is formed along the front surface of a semiconductor substrate, the unit cell (element constituent unit) density per unit area can be increased, and the current density per unit area can be increased, which is advantageous in terms of cost.
[0005] 9 is a cross-sectional view showing a trench gate structure of a conventional silicon carbide semiconductor device. The structure of the conventional silicon carbide semiconductor device will be described using a trench-type MOSFET 170 as an example. The trench gate structure has an n + The front surface of the silicon carbide substrate 101 is - A silicon carbide epitaxial layer 102 is deposited. - n-type silicon carbide epitaxial layer + The surface side opposite to the silicon carbide substrate side is provided with an n-type high concentration region 105. Within the n-type high concentration region 105, a first p + A first base region 103 is selectively provided. + The n-type base region 103 is disposed at the bottom + A mold area 117 is provided.
[0006] The MOS gate of the trench gate structure includes a p-type base layer 106, a n + Type source region 107, p + The p-type contact region 108, the trench 116, the gate insulating film 109, and the gate electrode 110 are included. + The mold contact region 108 may not be provided.
[0007] An interlayer insulating film 111 is provided on the gate electrode 110, and an n + type source region 107 and p + A source electrode 112 is provided in contact with the contact region 108. + A back surface electrode 113 serving as a drain electrode is provided on the back surface of the silicon carbide substrate 101 .
[0008] In a vertical MOSFET with such a structure, a p-type base layer 106 and an n-type - The parasitic pn diode is formed by the silicon carbide epitaxial layer 102 and the source electrode 112. This parasitic pn diode can be operated by applying a high potential to the source electrode 112. + The p-type contact region 108 and the n-type base layer 106 -The n-type silicon carbide epitaxial layer 102 is + A current flows in the direction toward the silicon carbide substrate 101. In this way, unlike an IGBT, a MOSFET has a built-in parasitic pn diode, making it possible to omit a free wheeling diode (FWD) used in an inverter, which contributes to reducing costs and size. Hereinafter, the parasitic pn diode of a MOSFET will be referred to as a built-in diode.
[0009] Here, p + In the n-type contact region 108, holes (positive holes) which are minority carriers exist, and + A silicon carbide substrate 101 and an n - There are electrons in the silicon carbide epitaxial layer 102. Therefore, when a current flows through the built-in diode, + Holes are injected from the n-type contact region 108, - type silicon carbide epitaxial layer 102 or n + Recombination of electrons and holes occurs in the n-type silicon carbide substrate 101. + If there is a defect in the crystal of the silicon carbide substrate 101, the recombination energy (3 eV) corresponding to the band gap is generated, and + Basal plane dislocations (BPDs), which are a type of crystal defect present in the silicon carbide substrate 101, move, and single Shockley stacking faults (1SSFs) sandwiched between two basal plane dislocations expand.
[0010] As stacking faults expand, they make it difficult for current to flow, causing the on-resistance of the MOSFET and the forward voltage of the built-in diode to rise. If this operation continues, stacking faults will expand cumulatively, causing losses in the inverter circuit to increase over time and increasing the amount of heat generated, which can cause equipment failure.
[0011] For this reason, as shown in Figure 9, - The n-type silicon carbide epitaxial layer 102 and +An n-type boundary layer 120 and a high-concentration n-type buffer layer 121 are provided between the n-type silicon carbide substrate 101 and the n-type boundary layer 120. For example, by forming a highly doped layer such as the highly doped n-type buffer layer 121 doped with nitrogen (N) at a high concentration, a lifetime killer is introduced to prevent the n - This promotes the recombination of holes from the n-type silicon carbide epitaxial layer 102. + The n-type boundary layer 120 controls the concentration of holes reaching the n-type silicon carbide substrate 101, thereby suppressing the occurrence of stacking faults and the expansion of their area. + The n-type boundary layer 120 is doped with, for example, nitrogen at a lower impurity concentration than the n-type silicon carbide substrate 101. + The crystal defects of the n-type silicon carbide substrate 101 are - The barrier 104 is provided to prevent the diffusion of the impurity atoms from reaching the silicon carbide epitaxial layer 102 .
[0012] Also, a silicon carbide semiconductor device is known in which protons are injected as a lifetime killer near the interface between a semiconductor substrate of a first conductivity type and a first semiconductor layer of a first conductivity type, thereby reducing the hole density at the interface between the semiconductor substrate of the first conductivity type and the first semiconductor layer of the first conductivity type, and suppressing the growth of crystal defects (see Patent Document 1 below).
[0013] Also, 1×10 17 / cm 3 More than 1×10 18 / cm 3 A silicon carbide semiconductor device is known which comprises a first conductivity type silicon carbide epitaxial layer having an impurity concentration below 1000 nm and a thickness of 1 μm or more and 5 μm or less, and a first conductivity type silicon carbide buffer layer having an impurity concentration three times or more the impurity concentration of the silicon carbide epitaxial layer, and which can suppress stacking faults by the impurity concentration and thickness of the silicon carbide buffer layer (see Patent Document 2 below). [Prior art documents] [Patent documents]
[0014] [Patent Document 1] JP 2019-102493 A [Patent Document 2] Patent No. 6627938 Summary of the Invention [Problem to be solved by the invention]
[0015] However, it is difficult to control the nitrogen concentration in the high-concentration n-type buffer layer 121 by process control, and variations occur in the nitrogen impurity concentration and film thickness. Fig. 10 is a graph showing the concentration gradient of the high-concentration n-type buffer layer of a conventional silicon carbide semiconductor device. In Fig. 10, the horizontal axis represents the depth from the surface S in μm, and the vertical axis represents the nitrogen concentration in atoms / cm. 3 Moreover, graph A is an example of the outer periphery of a semiconductor wafer, and graph B is an example of the center of a semiconductor wafer.
[0016] 10, the nitrogen concentration gradually increases in the depth direction (from the source electrode 112 to the back surface electrode 113) at the peripheral part and the central part of the semiconductor wafer, and the nitrogen concentration is higher at the peripheral part of the semiconductor wafer than at the central part of the semiconductor wafer. Thus, when the nitrogen concentration in the high-concentration n-type buffer layer 121 is formed to be high, the variation in the nitrogen concentration becomes large.
[0017] In addition, the nitrogen concentration of the high-concentration n-type buffer layer 121 is 1.2×10 19 / cm 3 If the concentration exceeds this level, double Shockley stacking faults (2SSF) are likely to occur due to the high nitrogen concentration in the high-concentration n-type buffer layer 121, and the Von (on-state voltage) of the element may deteriorate due to current flow. Furthermore, increasing the thickness of the high-concentration n-type buffer layer 121 increases the epitaxial growth time, increasing the manufacturing cost.
[0018] In this way, increasing the nitrogen concentration in the high-concentration n-type buffer layer 121 increases manufacturing costs, causes concentration variations, and generates 2SSF, while a low nitrogen concentration poses the problem of not being able to sufficiently reduce the concentration of holes reaching the substrate.
[0019] In order to solve the problems associated with the conventional techniques described above, an object of the present invention is to provide a silicon carbide semiconductor device and a method for manufacturing a silicon carbide semiconductor device that can sufficiently reduce the concentration of holes reaching a substrate even when a high-concentration n-type buffer layer is reduced in concentration. [Means for solving the problem]
[0020] In order to solve the above-mentioned problems and achieve the object of the present invention, a silicon carbide semiconductor device according to the present invention has the following features. A first semiconductor layer of a first conductivity type having a lower impurity concentration than the silicon carbide semiconductor substrate is provided on a front surface of a silicon carbide semiconductor substrate of a first conductivity type. A second semiconductor layer of a first conductivity type is provided on a surface of the first semiconductor layer opposite to the silicon carbide semiconductor substrate. A third semiconductor layer of a first conductivity type having a lower impurity concentration than the silicon carbide semiconductor substrate is provided on a surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate. A fourth semiconductor layer of a second conductivity type is provided on a surface of the third semiconductor layer opposite to the silicon carbide semiconductor substrate. A first semiconductor region of a first conductivity type is selectively provided in a surface layer of the fourth semiconductor layer opposite to the silicon carbide semiconductor substrate. A gate electrode is provided via a gate insulating film on at least a part of a surface of the fourth semiconductor layer sandwiched between the first semiconductor region and the third semiconductor layer. A first electrode is provided on the surfaces of the fourth semiconductor layer and the first semiconductor region. A second electrode is provided on the back surface of the silicon carbide semiconductor substrate. The second semiconductor layer has a surface roughness of 1.0×10 13 / cm 3 Above 1.0×10 14 / cm 3 The following concentration of protons was introduced: 1.0×10 18 / cm 3 Above 5.0×10 18 / cm 3 The impurity concentrations are as follows: The second semiconductor layer has a thickness of 1 μm or more and 5 μm or less, and the peak of the proton concentration is located at a position 5 μm or less away from the interface between the first semiconductor layer and the second semiconductor layer toward the first electrode.
[0021] In order to solve the above-mentioned problems and achieve the object of the present invention, a silicon carbide semiconductor device according to the present invention has the following features. A first semiconductor layer of a first conductivity type having a lower impurity concentration than the silicon carbide semiconductor substrate is provided on a front surface of a silicon carbide semiconductor substrate of a first conductivity type. A second semiconductor layer of a first conductivity type is provided on a surface of the first semiconductor layer opposite to the silicon carbide semiconductor substrate. A third semiconductor layer of a first conductivity type having a lower impurity concentration than the silicon carbide semiconductor substrate is provided on a surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate. A fourth semiconductor layer of a second conductivity type is provided on a surface of the third semiconductor layer opposite to the silicon carbide semiconductor substrate. A first semiconductor region of a first conductivity type is selectively provided in a surface layer of the fourth semiconductor layer opposite to the silicon carbide semiconductor substrate. A gate electrode is provided via a gate insulating film on at least a part of a surface of the fourth semiconductor layer sandwiched between the first semiconductor region and the third semiconductor layer. A first electrode is provided on the surfaces of the fourth semiconductor layer and the first semiconductor region. A second electrode is provided on the back surface of the silicon carbide semiconductor substrate. The second semiconductor layer has a surface roughness of 1.0×10 13 / cm 3 Above 1.0×1014 / cm 3 The following concentration of protons was introduced: 1.0×10 18 / cm 3 Above 5.0×10 18 / cm 3 The impurity concentration is as follows: The half width of the proton concentration is 5 μm or more and 10 μm or less.
[0022] In addition, the present invention provides a silicon carbide semiconductor device, comprising: It is characterized in that helium is introduced instead of the protons.
[0023] In order to solve the above-mentioned problems and achieve the object of the present invention, a method for manufacturing a silicon carbide semiconductor device according to the present invention has the following features. First, a first step is performed in which a first semiconductor layer of a first conductivity type having a lower impurity concentration than the silicon carbide semiconductor substrate is formed on a front surface of the silicon carbide semiconductor substrate. Next, a first semiconductor layer having a thickness of 1 μm to 5 μm and a thickness of 1.0×10 18 / cm 3 Above 5.0×10 18 / cm 3 A second step of forming a second semiconductor layer of a first conductivity type with an impurity concentration of 1.0×10 or less is performed. Next, a third step of forming a third semiconductor layer of a first conductivity type with an impurity concentration lower than that of the silicon carbide semiconductor substrate is performed on the surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate. Next, a fourth step of forming a fourth semiconductor layer of a second conductivity type on the surface of the third semiconductor layer opposite to the silicon carbide semiconductor substrate is performed. Next, a fifth step of selectively forming a first semiconductor region of a first conductivity type on the surface layer of the fourth semiconductor layer opposite to the silicon carbide semiconductor substrate is performed. Next, a sixth step of forming a gate electrode via a gate insulating film on at least a part of the surface of the fourth semiconductor layer sandwiched between the first semiconductor region and the third semiconductor layer is performed. Next, protons are irradiated to reduce the proton concentration of the second semiconductor layer to 1.0×10 13 / cm 3 Above 1.0×10 14 / cm 3 A seventh step is performed as follows: Next, an eighth step is performed of forming a first electrode on surfaces of the fourth semiconductor layer and the first semiconductor region; Next, a ninth step is performed of forming a second electrode on the back surface of the silicon carbide semiconductor substrate; In the seventh step, the peak of the proton concentration is positioned 5 μm or less toward the first electrode from the interface between the first semiconductor layer and the second semiconductor layer.
[0024] In order to solve the above-mentioned problems and achieve the object of the present invention, a method for manufacturing a silicon carbide semiconductor device according to the present invention has the following features. First, a first step is performed in which a first semiconductor layer of a first conductivity type having a lower impurity concentration than the silicon carbide semiconductor substrate is formed on a front surface of the silicon carbide semiconductor substrate. Next, a 1.0×10 18 / cm 3 Above 5.0×10 18 / cm 3 A second step of forming a second semiconductor layer of a first conductivity type with an impurity concentration of 1.0×10 or less is performed. Next, a third step of forming a third semiconductor layer of a first conductivity type with an impurity concentration lower than that of the silicon carbide semiconductor substrate is performed on the surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate. Next, a fourth step of forming a fourth semiconductor layer of a second conductivity type on the surface of the third semiconductor layer opposite to the silicon carbide semiconductor substrate is performed. Next, a fifth step of selectively forming a first semiconductor region of a first conductivity type on the surface layer of the fourth semiconductor layer opposite to the silicon carbide semiconductor substrate is performed. Next, a sixth step of forming a gate electrode via a gate insulating film on at least a part of the surface of the fourth semiconductor layer sandwiched between the first semiconductor region and the third semiconductor layer is performed. Next, protons are irradiated to reduce the proton concentration of the second semiconductor layer to 1.0×10 13 / cm 3 Above 1.0×10 14 / cm 3 A seventh step is then performed, in which a first electrode is formed on the surfaces of the fourth semiconductor layer and the first semiconductor region. A ninth step is then performed, in which a second electrode is formed on the back surface of the silicon carbide semiconductor substrate. In the seventh step, the half width of the proton concentration is set to 5 μm or more and 10 μm or less.
[0025] In addition, in the method for manufacturing a silicon carbide semiconductor device according to the present invention, in the seventh step, the protons are irradiated from the first electrode side.
[0026] In addition, a method for manufacturing a silicon carbide semiconductor device according to the present invention includes the steps of: The method further includes a step of performing a heat treatment on the first semiconductor region after the fifth step, and the seventh step is performed after the step of performing the heat treatment. It is characterized by:
[0027] In addition, a method for manufacturing a silicon carbide semiconductor device according to the present invention includes the steps of: Helium is introduced in place of the protons. It is characterized by:
[0028] According to the above-mentioned invention, protons are introduced into the high-concentration n-type buffer layer (second semiconductor layer of the first conductivity type). Since protons act as hole lifetime killers, the high-concentration n-type buffer layer can have a lower concentration than conventional ones and a thinner film thickness, and still be capable of recombining holes to the same extent as conventional high-concentration n-type buffer layers. This reduces the manufacturing cost of the high-concentration n-type buffer layer, prevents concentration variations, and prevents the expansion of the 2SSF of the high-concentration n-type buffer layer.
[0029] In addition, the impurities in the high-concentration n-type buffer layer can also act as a lifetime killer for holes, so it is possible to use a high-concentration n-type buffer layer without providing a proton-transporting layer. - This allows the concentration of protons to be kept low compared to when protons are introduced into a silicon carbide epitaxial layer (third semiconductor layer of the first conductivity type). This allows the amount of proton irradiation to be reduced, so damage to the gate insulating film caused by proton irradiation is reduced and a decrease in threshold voltage (Vth) can be suppressed. Effect of the Invention
[0030] Advantageous Effects of Invention The silicon carbide semiconductor device and the method for manufacturing the silicon carbide semiconductor device according to the present invention have the advantage that the concentration of holes reaching the substrate can be sufficiently reduced even when the concentration of a high-concentration n-type buffer layer is reduced. [Brief description of the drawings]
[0031] [Figure 1] 1 is a cross-sectional view showing a structure of a silicon carbide semiconductor device according to an embodiment. [Diagram 2] 1 is a graph showing the relationship between proton irradiation dose and Von fluctuation amount in a silicon carbide semiconductor device according to an embodiment. [Diagram 3]1A to 1C are cross-sectional views showing a state during the manufacture of a silicon carbide semiconductor device according to an embodiment (part 1). [Figure 4] 5A to 5C are cross-sectional views (part 2) illustrating a state during the manufacture of the silicon carbide semiconductor device according to the embodiment. [Diagram 5] 6A to 6C are cross-sectional views (part 3) illustrating a state during the manufacture of a silicon carbide semiconductor device according to an embodiment. [Figure 6] 4 is a cross-sectional view showing a state during the manufacture of a silicon carbide semiconductor device according to an embodiment (part 4). FIG. [Figure 7] 5 is a cross-sectional view showing a state during the manufacture of a silicon carbide semiconductor device according to an embodiment (part 5). FIG. [Figure 8] 6 is a cross-sectional view showing a state during the manufacture of a silicon carbide semiconductor device according to an embodiment (part 6). FIG. [Figure 9] FIG. 1 is a cross-sectional view showing a structure of a conventional silicon carbide semiconductor device. [Figure 10] 1 is a graph showing a concentration gradient of a high-concentration n-type buffer layer of a conventional silicon carbide semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] A silicon carbide semiconductor device and a preferred embodiment of the silicon carbide semiconductor device according to the present invention will be described in detail below with reference to the accompanying drawings. In this specification and the accompanying drawings, in a layer or region prefixed with n or p, electrons or holes are the majority carriers, respectively. In addition, + and - attached to n or p respectively mean that the impurity concentration is higher and lower than that of a layer or region not prefixed with n or p. Note that in the following description of the embodiment and the accompanying drawings, the same reference numerals are attached to similar configurations, and duplicated explanations are omitted. In addition, in this specification, in the notation of Miller indices, "-" means a bar attached to the index immediately following it, and adding "-" before the index represents a negative index. In addition, it is preferable that the description of "same" or "equivalent" includes up to 5% in consideration of manufacturing variations.
[0033] (Embodiment) The semiconductor device according to the present invention is configured using a wide band gap semiconductor. In the embodiment, a silicon carbide semiconductor device fabricated (manufactured) using, for example, silicon carbide (SiC) as a wide band gap semiconductor will be described by taking a trench-type MOSFET 70 as an example. Fig. 1 is a cross-sectional view showing a structure of a silicon carbide semiconductor device according to the embodiment. Fig. 1 shows only an active region of the trench-type MOSFET 70 through which a main current flows.
[0034] As shown in FIG. 1, the silicon carbide semiconductor device according to the embodiment has n + A first main surface (front surface) of a silicon carbide substrate (a silicon carbide semiconductor substrate of a first conductivity type) 1, for example, a (0001) surface (Si surface), is provided with an n-type boundary layer (a first semiconductor layer of a first conductivity type) 20, a high-concentration n-type buffer layer (a second semiconductor layer of a first conductivity type) 21, and an n-type boundary layer (a first semiconductor layer of a first conductivity type) 22. - The semiconductor device is configured using a silicon carbide semiconductor substrate 18 formed by sequentially laminating a p-type silicon carbide epitaxial layer (third semiconductor layer of a first conductivity type) 2 and a p-type base layer (fourth semiconductor layer of a second conductivity type) 6.
[0035] n - The n-type silicon carbide epitaxial layer 2 + An n-type high concentration region 5 may be provided on the surface opposite to the silicon carbide substrate 1 side. + Lower n than silicon carbide substrate 1 - The n-type high concentration drift layer has an impurity concentration higher than that of silicon carbide epitaxial layer 2.
[0036] The n-type boundary layer 20 is + 1.0×10 lower than that of the silicon carbide substrate 1 17 / cm 3 Above 1.0×10 18 / cm 3 The n-type boundary layer 20 has an impurity concentration of 1 μm or more and a thickness of 1 μm or more and 5 μm or less, and is doped with, for example, nitrogen (N). + The crystal defects of the silicon carbide substrate 1 are n -The insulating layer 4 is provided to prevent the electric field from reaching the silicon carbide epitaxial layer 2 .
[0037] The high-concentration n-type buffer layer 21 is a highly doped layer doped with, for example, nitrogen at a high concentration. The high-concentration n-type buffer layer 21 is doped with protons 22 formed by irradiating protons (P). The protons 22 act as lifetime killers of holes, - This promotes the recombination of holes from the n-type silicon carbide epitaxial layer 2. + By controlling the concentration of holes reaching the silicon carbide substrate 1, the occurrence of stacking faults and the expansion of their area can be suppressed. Here, a form in which protons 22 are introduced is shown, but the same effect can be obtained by introducing helium (He) instead of the protons 22.
[0038] Therefore, even if the high-concentration n-type buffer layer 21 has a lower impurity concentration than the conventional one and is made thinner, it can recombine holes to the same extent as the conventional high-concentration n-type buffer layer 121. Therefore, the manufacturing cost of the high-concentration n-type buffer layer 21 can be reduced, the impurity concentration does not vary, and the expansion of the 2SSF of the high-concentration n-type buffer layer 21 can be prevented.
[0039] The impurity concentration of the high-concentration n-type buffer layer 21 is 1.0×10 18 / cm 3 Above 5.0×10 18 / cm 3 This is a concentration range in which it is easy to control the concentration by process. In addition, this concentration is unlikely to cause double Shockley stacking faults (2SSF), and the high-concentration n-type buffer layer 21 can prevent the expansion of both 1SSF from the substrate and 2SSF due to an increase in the nitrogen concentration in the high-concentration n-type buffer layer 21. In addition, by lowering the impurity concentration of the high-concentration n-type buffer layer 21, the nitrogen impurity concentration and film thickness can be made uniform. For example, the surface (n -The difference between the impurity concentration on the surface (contacting the silicon carbide epitaxial layer 2) and the impurity concentration on the back surface can be set to within two times. For example, when the impurity concentration on the front surface is 1.0×10 18 / cm 3 In this case, the impurity concentration on the back surface is 2.0×10 18 / cm 3 The following is the result.
[0040] In addition, since the impurities in the high-concentration n-type buffer layer 21 can also act as a lifetime killer of holes, the high-concentration n-type buffer layer 21 is not provided and the protons 22 are introduced into the n - The concentration of protons 22 can be kept low as compared with the case where protons are introduced into the type silicon carbide epitaxial layer 2. This allows the amount of proton irradiation to be reduced, so that damage to the gate insulating film 9 caused by proton irradiation is reduced and a decrease in the threshold voltage (Vth) can be suppressed.
[0041] Proton 22 is 1.0×10 13 / cm 3 Above 1.0×10 14 / cm 3 2 is a graph showing the relationship between the proton irradiation amount and the Von fluctuation amount in the silicon carbide semiconductor device according to the embodiment. In FIG. 2, the horizontal axis shows the proton irradiation amount (dose amount) in units of / cm 2 The vertical axis shows the amount of variation ΔVon of Von when a test is performed with a voltage of 20V applied to the gate and a source-drain current of 25A, in units of V. Figure 2 shows the minimum (min), maximum (max) and average (average) values of ΔVon obtained from multiple tests.
[0042] As shown in Figure 2, the proton irradiation dose was 1.0 × 10 11 / cm 2 If it exceeds 1.0×10, ΔVon will increase. 11 / cm 2 The dose is 1.0×10 14 / cm 3Therefore, in the embodiment, the peak concentration of protons 22 is 1.0×10 13 / cm 3 Above 1.0×10 14 / cm 3 The following concentrations are preferred:
[0043] In addition, since the starting point of the expansion of the stacking fault exists in the n-type boundary layer 20, the hole concentration at the interface between the n-type boundary layer 20 and the high-concentration n-type buffer layer 21 thereon is 1.0×10 15 / cm 3 It is preferable to adjust the thickness of the high-concentration n-type buffer layer 21 so that the thickness is as follows. For example, the thickness of the high-concentration n-type buffer layer 21 is 1 μm or more and 5 μm or less.
[0044] The peak value of the concentration of protons 22 in the high-concentration n-type buffer layer 21 is about 5 μm from the interface between the n-type boundary layer 20 and the high-concentration n-type buffer layer 21. - It is preferable that the protons 22 are introduced on the side of the high-concentration n-type silicon carbide epitaxial layer 2. The half-width of the concentration of the protons 22 (the region where the concentration is more than half of the peak value) is preferably 5 μm or more and 10 μm or less. As a result, since the protons 22 are introduced mainly in the high-concentration n-type buffer layer 21, the n - Therefore, an increase in the resistance of the silicon carbide epitaxial layer 2 can be suppressed.
[0045] For example, current density 1100A / cm 3 When the current was applied at a temperature of 175°C, the peak concentration of protons 22 was 1.0 x 10 14 / cm 3 If the layer in which the lifetime is reduced by the protons 22 (for example, the region in which the concentration of the protons 22 is half or more of the peak value) is 9 μm or more, the nitrogen concentration of the high-concentration n-type buffer layer 21 is 1.0×10 18 / cm 3 Even if the film thickness is 1 μm, the hole concentration at the interface between the n-type boundary layer 20 and the high-concentration n-type buffer layer 21 thereon is 1.0×10 15 / cm 3In this way, by making the high-concentration n-type buffer layer 21 thinner than before, the epitaxial growth time can be shortened, and the manufacturing cost can be reduced.
[0046] n + A back surface electrode 13 serving as a drain electrode is provided on a second main surface (back surface, i.e., the back surface of the silicon carbide semiconductor base 18) of the silicon carbide substrate 1. A drain electrode pad (not shown) is provided on the surface of the back surface electrode 13.
[0047] A trench structure is formed on the first main surface side (p-type base layer 6 side) of the silicon carbide semiconductor substrate 18. Specifically, the trench 16 is formed in the n-type + The n-type high concentration region 5 (or the n-type high concentration region 5 when the n-type high concentration region 5 is not provided) is formed by penetrating the p-type base layer 6 from the surface opposite to the silicon carbide substrate 1 side (the first main surface side of the silicon carbide semiconductor base 18). - The gate electrode 10 is formed on the bottom and side walls of the trench 16 along the inner wall of the trench 16. The gate electrode 10 is formed on the inside of the gate insulating film 9 in the trench 16. The gate electrode 10 is insulated from the n-type high concentration region 5(2) and the p-type base layer 6 by the gate insulating film 9. A part of the gate electrode 10 may protrude from the upper side of the trench 16 (the side where the source electrode 12 described later is provided) to the source electrode 12 side. The gate insulating film 9 is preferably formed on the m-plane. For example, when a trench structure is formed, the side wall of the trench 16 is preferably an m-plane.
[0048] n-type high concentration region 5(2) + In the surface layer on the opposite side to the silicon carbide substrate 1 side (the first main surface side of the silicon carbide semiconductor base 18), a first p + A second p-type base region 3 is provided in the n-type high concentration region 5(2) and in contact with the bottom of the trench 16. + A mold base region 4 is provided. +The second base region 4 is provided at a position facing the bottom of the trench 16 in the depth direction (the direction from the source electrode 12 to the drain electrode 13). + The width of the mold base region 4 is equal to or greater than the width of the trench 16. The bottom of the trench 16 is the second p + The p-type base region 4 may be connected to the p-type base layer 6 and the second p + It may be located within the n-type high concentration region 5 ( 2 ) sandwiched between the n-type base regions 4 .
[0049] Also, n - In the silicon carbide epitaxial layer 2, a first p + A region deeper than the n-type base region 3 has a peak impurity concentration higher than that of the n-type high concentration region 5(2). + The mold region 17 is provided. + This refers to a position closer to the back surface electrode 13 than the mold base region 3 .
[0050] Inside the p-type base layer 6, an n-type + A p-type source region (first semiconductor region of a first conductivity type) 7 is selectively provided. + A contact region 8 may be selectively provided. + Type source region 7 and p + The mold contact regions 8 abut each other.
[0051] The interlayer insulating film 11 is provided on the entire first main surface side of the silicon carbide semiconductor substrate 18 so as to cover the gate electrode 10 embedded in the trench 16. The source electrode 12 is connected to the n-type semiconductor layer 14 via a contact hole opened in the interlayer insulating film 11. + The p-type source region 7 and the p-type base layer 6 are in contact with each other. + When the n-type contact region 8 is provided, the source electrode 12 is + Type source region 7 and p +The source electrode 12 is in contact with the type contact region 8. The source electrode 12 is electrically insulated from the gate electrode 10 by an interlayer insulating film 11. A source electrode pad (not shown) is provided on the source electrode 12. A barrier metal 14 may be provided between the source electrode 12 and the interlayer insulating film 11 to prevent diffusion of metal atoms from the source electrode 12 to the gate electrode 10 side, for example.
[0052] (Method of Manufacturing Silicon Carbide Semiconductor Device According to an Embodiment) Next, a method for manufacturing a silicon carbide semiconductor device according to an embodiment will be described. Figures 3 to 8 are cross-sectional views showing states during the manufacturing process of a silicon carbide semiconductor device according to an embodiment.
[0053] First, n-type silicon carbide + A silicon carbide substrate 1 is prepared. + The silicon carbide substrate 1 has a size of, for example, 5.0×10 18 / cm 3 And this n + On the first main surface of the silicon carbide substrate 1, an n-type boundary layer 20 made of silicon carbide is epitaxially grown to a thickness of, for example, about 5 μm while being doped with an n-type impurity, for example, nitrogen atoms (N). The impurity concentration of the n-type boundary layer 20 is, for example, 1.0×10 18 / cm 3 The setting may be made so as to be about the same.
[0054] Next, on the surface of the n-type boundary layer 20, a high-concentration n-type buffer layer 21 made of silicon carbide is epitaxially grown to a thickness of, for example, 1 μm to 5 μm while being doped with an n-type impurity, for example, nitrogen atoms (N). The impurity concentration of the high-concentration n-type buffer layer 21 is, for example, 1.0×10 18 / cm 3 Above 5.0×10 18 / cm 3 It may be set as follows:
[0055] Next, the surface of the high-concentration n-type buffer layer 21 is doped with n-type impurities, such as nitrogen atoms (N), while -The silicon carbide epitaxial layer 2a is epitaxially grown to a thickness of, for example, about 30 μm. The state up to this point is shown in FIG.
[0056] Next, the bottom n - A mask (not shown) having a desired opening is formed on the surface of the silicon carbide epitaxial layer 2a by photolithography, for example, an oxide film. Then, using this oxide film as a mask, n-type impurities, for example, nitrogen atoms, may be ion-implanted by ion implantation. As a result, the lower n - The n-type silicon carbide epitaxial layer 2a includes + A mold area 17 is formed.
[0057] Next, n + The mask used for ion implantation to form the type region 17 is removed. Next, a mask for ion implantation having a predetermined opening is formed, for example, from an oxide film by photolithography. Then, p-type impurities such as aluminum are implanted into the opening of the oxide film to form a lower first p-type region with a depth of about 0.5 μm. + The base region 3a and the second p + A type base region 4 is formed. + When the type region 17 is formed, n + Type region 17 n + A lower first p + The base region 3a is + It is formed so as to overlap the mold region 17 .
[0058] Next, a part of the ion implantation mask is removed, and n-type impurities such as nitrogen are ion-implanted into the opening, forming a lower n - A lower n-type high concentration region 5a having a depth of, for example, about 0.5 μm may be formed in a part of the surface region of the silicon carbide epitaxial layer 2a. The impurity concentration of the lower n-type high concentration region 5a is, for example, 1×10 17 / cm 3 The state up to this point is shown in Figure 4.
[0059] Next, the bottom n -An upper n-type epitaxial layer 2a is formed on the surface of the silicon carbide epitaxial layer 2a. The upper n-type epitaxial layer 2a is doped with n-type impurities such as nitrogen. - The upper n-type silicon carbide epitaxial layer 2b is formed to a thickness of about 0.5 μm. - The impurity concentration of the silicon carbide epitaxial layer 2b is 3×10 15 / cm 3 The lower n - The silicon carbide epitaxial layer 2a and the upper n - The silicon carbide epitaxial layer 2b is formed of n - This results in a silicon carbide epitaxial layer 2 .
[0060] Next, the top n - An ion implantation mask having a predetermined opening is formed on the surface of the silicon carbide epitaxial layer 2b by photolithography, for example, using an oxide film. Then, p-type impurities such as aluminum are implanted into the opening of the oxide film to form an upper first p-type impurity layer having a depth of about 0.5 μm. + The mold base region 3b is a lower first p + The upper portion 1p is formed so as to overlap the mold base region 3a. + The mold base region 3b and the lower part 1p + The base region 3a forms a continuous region, and the first p + This forms the mold base region 3. + The impurity concentration of the base region 3b is set to, for example, 5×10 18 / cm 3 Set it so that it is about the same.
[0061] Next, a part of the ion implantation mask may be removed, and an n-type impurity such as nitrogen may be ion-implanted into the opening to form an upper n-type high concentration region 5b having a depth of, for example, about 0.5 μm in a part of the surface region of the second silicon carbide epitaxial layer 2. The impurity concentration of the upper n-type high concentration region 5b may be set to, for example, 1×10 17 / cm 3 The upper n-type heavily doped region 5b and the lower n-type heavily doped region 5a are formed so that at least a portion of them are in contact with each other to form the n-type heavily doped region 5. However, there are cases where the n-type heavily doped region 5 is formed over the entire surface of the substrate, and cases where it is not formed. The state up to this point is shown in FIG.
[0062] Next, n - On the surface of the silicon carbide epitaxial layer 2, a p-type base layer 6 is formed by epitaxial growth to a thickness of about 1.1 μm. The impurity concentration of the p-type base layer 6 is 4×10 17 / cm 3 After the p-type base layer 6 is formed by epitaxial growth, p-type impurities such as aluminum may be further ion-implanted into the p-type base layer 6.
[0063] Next, a predetermined region constituting a MOS gate is formed on the first main surface layer (surface layer of the p-type base layer 6) of the silicon carbide semiconductor substrate 18. Specifically, an ion implantation mask having a predetermined opening is formed on the surface of the p-type base layer 6 by photolithography, for example, from an oxide film. N-type impurities such as nitrogen (N) and phosphorus (P) are ion-implanted into this opening, and n-type impurities are implanted into a portion of the surface of the p-type base layer 6. + Next, the n-type source region 7 is formed. + The ion implantation mask used for forming the p-type source region 7 is removed, and a mask for ion implantation having a predetermined opening is formed in the same manner, and p-type impurities such as boron are ion-implanted into a portion of the surface of the p-type base layer 6 to form p + A contact region 8 may be formed. + The impurity concentration of the p-type contact region 8 is set to be higher than the impurity concentration of the p-type base layer 6.
[0064] Next, a heat treatment (activation anneal) is performed to activate the entire region formed by ion implantation. For example, the heat treatment (anneal) is performed in an inert gas atmosphere at about 1700° C. to form the first p + Mold base region 3, second p + Type base region 4, n + Type source region 7, p + Type contact region 8 and n + An activation process is carried out on the mold region 17. As described above, each ion implantation region may be activated collectively by one heat treatment, or each ion implantation may be activated by a heat treatment. The state up to this point is shown in FIG.
[0065] Next, a trench forming mask having a predetermined opening is formed by photolithography on the surface of the p-type base layer 6, for example, using an oxide film. Next, a trench 16 is formed by dry etching, penetrating the p-type base layer 6 and reaching the n-type high concentration region 5(2). The bottom of the trench 16 is connected to the second p-type high concentration region 5(2) formed in the n-type high concentration region 5(2). + This may extend to the mold base region 4. The trench mask is then removed.
[0066] Next, n + Type source region 7 and p + A gate insulating film 9 is formed along the surface of the contact region 8 and the bottom and sidewalls of the trench 16. This gate insulating film 9 may be formed by thermal oxidation at a temperature of about 1000° C. in an oxygen atmosphere. Alternatively, this gate insulating film 9 may be formed by a method of deposition by a chemical reaction such as high temperature oxidation (High Temperature Oxide: HTO).
[0067] Next, a polycrystalline silicon layer doped with, for example, phosphorus atoms is provided on the gate insulating film 9. This polycrystalline silicon layer may be formed so as to fill the trench 16. This polycrystalline silicon layer is patterned by photolithography and left inside the trench 16 to form the gate electrode 10. The state up to this point is shown in FIG.
[0068] Next, the first main surface side (p +Particle beam irradiation 23 is performed from the side of the silicon carbide semiconductor substrate 21 (the side of the silicon carbide base region 6). The particle beam irradiation 23 is performed by irradiating protons. Alternatively, helium may be irradiated instead of protons. The particle beam irradiation 23 is performed so that protons 22 are introduced into the high concentration n-type buffer layer 21. Since the protons 22 disappear at a temperature of 500° C. or higher, the particle beam irradiation 23 is performed after the activation annealing. Here, the particle beam irradiation 23 is performed after the formation of the gate electrode 10, but since the annealing for converting nickel formed on the silicon carbide semiconductor substrate surface in the contact hole of the interlayer insulating film 11 into nickel silicide is also performed at about 1000° C., it is sufficient to perform the particle beam irradiation 23 after the annealing for forming nickel silicide.
[0069] The particle beam irradiation 23 may be performed from the back side of the silicon carbide semiconductor substrate. In this case, the influence of the particle beam irradiation 23 on the gate electrode 10 can be reduced. However, the particle beam irradiation 23 from the back side has a disadvantage that n + Since the thickness of the n-type silicon carbide substrate 1 is large, it is difficult to adjust the peak position of the proton concentration, and further, the half-value width of the concentration of protons 22 in the high-concentration n-type buffer layer 21 is widened, so that the particle beam irradiation 23 is preferably performed from the first main surface side of the silicon carbide semiconductor base. The state up to this point is shown in FIG.
[0070] Next, for example, phosphorus glass is deposited to a thickness of about 1 μm so as to cover the gate insulating film 9 and the gate electrode 10, forming an interlayer insulating film 11. Next, a barrier metal 14 made of titanium (Ti) or titanium nitride (TiN) may be formed so as to cover the interlayer insulating film 11. The interlayer insulating film 11 and the gate insulating film 9 are patterned by photolithography. + Type source region 7 and p + A contact hole is formed exposing the mold contact region 8. Thereafter, a heat treatment (reflow) is performed to flatten the interlayer insulating film 11.
[0071] Next, the interlayer insulating film 11 is selectively removed, and a nickel (Ni) or Ti film is formed on the surface of the silicon carbide semiconductor substrate 18. Next, the surface is protected and n +A Ni or Ti film is formed on the back side of the silicon carbide substrate 1. Next, a heat treatment at about 1000° C. is performed to bond the front side of the silicon carbide semiconductor base 18 and the n-type silicon carbide substrate 1. + An ohmic electrode is formed on the rear surface side of the silicon carbide substrate 1 .
[0072] Next, a conductive film that will become the source electrode 12 is provided on the interlayer insulating film 11 so as to contact the ohmic electrode portion formed in the contact hole, and n + Type source region 7 and p + The contact region 8 is brought into contact with a source electrode 12 .
[0073] Next, n + A back electrode 13 made of, for example, a nickel (Ni) film is formed on the second main surface of the silicon carbide substrate 1. Then, a heat treatment is performed at a temperature of, for example, about 970° C. to form an n-type silicon carbide substrate. + The silicon carbide substrate 1 and the back surface electrode 13 are connected to each other by ohmic contact.
[0074] Next, an electrode pad to become a source electrode pad (not shown) is deposited on the source electrode 12 on the front surface of the silicon carbide semiconductor substrate 18 and in the opening of the interlayer insulating film 11 by, for example, a sputtering method. The thickness of the portion of the electrode pad on the interlayer insulating film 11 may be, for example, 5 μm. The electrode pad may be made of, for example, aluminum containing 1% silicon (Al-Si). Next, the source electrode pad is selectively removed.
[0075] Next, for example, titanium (Ti), nickel (Ni) and gold (Au) are deposited in this order as a drain electrode pad (not shown) on the surface of the back electrode 13. In this manner, the silicon carbide semiconductor device shown in FIG.
[0076] As described above, according to the embodiment, protons are introduced into the high-concentration n-type buffer layer. Since protons act as hole lifetime killers, the high-concentration n-type buffer layer can have a lower concentration than conventional ones and a thinner film thickness, and still recombine holes to the same extent as conventional high-concentration n-type buffer layers. This reduces the manufacturing cost of the high-concentration n-type buffer layer, prevents concentration variations, and prevents the expansion of the 2SSF of the high-concentration n-type buffer layer.
[0077] In addition, the impurities in the high-concentration n-type buffer layer can also act as a lifetime killer for holes, so it is possible to use a high-concentration n-type buffer layer without providing a proton-transporting layer. - This allows the proton concentration to be kept low compared to when doping a silicon carbide epitaxial layer, which reduces the amount of proton irradiation, thereby minimizing damage to the gate insulating film caused by proton irradiation and suppressing a decrease in threshold voltage (Vth).
[0078] The present invention can be modified in various ways without departing from the spirit of the present invention, and in each of the above-mentioned embodiments, for example, the dimensions and impurity concentration of each part are set in various ways according to the required specifications. In addition, each of the above-mentioned embodiments has been described using a trench gate type vertical MOSFET as an example, but it is also applicable to a PiN diode, an IGBT (Insulated Gate Bipolar Transistor), etc. In addition, in each of the embodiments, the first conductivity type is n-type and the second conductivity type is p-type, but the present invention is similarly valid even if the first conductivity type is p-type and the second conductivity type is n-type. [Industrial Applicability]
[0079] INDUSTRIAL APPLICABILITY As described above, the silicon carbide semiconductor device and the method for manufacturing a silicon carbide semiconductor device according to the present invention are useful for power semiconductor devices used in power conversion devices such as inverters, power supply devices for various industrial machines, automobile igniters, and the like. [Explanation of symbols]
[0080] 1, 101 n + Silicon carbide substrate 2, 102 n - Silicon carbide epitaxial layer 2a bottom n - Silicon carbide epitaxial layer 2b Top n - Silicon carbide epitaxial layer 3, 103 1st p. + Type-based regions 3a Lower 1st p. + Type-based regions 3b Upper 1st p. + Type-based regions 4, 104 2nd p. + Type-based regions 5, 105 n-type high concentration region 5a Lower n-type high concentration region 5b Upper n-type high concentration region 6, 106 p-type base layer 7, 107 n + Type Source Area 8, 108 p. + Mold Contact Area 9, 109 Gate insulating film 10, 110 Gate electrode 11, 111 Interlayer insulating film 12, 112 Source electrode 13, 113 Back electrode 14, 114 Barrier metal 16, 116 Trench 17, 117 n + type area 18 Silicon carbide semiconductor substrate 20, 120 n-type boundary layer 21, 121 Highly doped n-type buffer layer 22 Protons 23 Particle Beam Irradiation 70, 170 Trench MOSFET
Claims
1. a first conductivity type silicon carbide semiconductor substrate; a first semiconductor layer of a first conductivity type provided on a front surface of the silicon carbide semiconductor substrate and having a lower impurity concentration than the silicon carbide semiconductor substrate; a second semiconductor layer of a first conductivity type provided on a surface of the first semiconductor layer opposite to the silicon carbide semiconductor substrate; a third semiconductor layer of a first conductivity type having an impurity concentration lower than that of the silicon carbide semiconductor substrate, the third semiconductor layer being provided on a surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate; a fourth semiconductor layer of a second conductivity type provided on a surface of the third semiconductor layer opposite to the silicon carbide semiconductor substrate; a first semiconductor region of a first conductivity type selectively provided in a surface layer of the fourth semiconductor layer on a side opposite to the silicon carbide semiconductor substrate; a gate electrode provided via a gate insulating film on at least a portion of a surface of the fourth semiconductor layer sandwiched between the first semiconductor region and the third semiconductor layer; a first electrode provided on a surface of the fourth semiconductor layer and the first semiconductor region; A second electrode provided on a back surface of the silicon carbide semiconductor substrate; Equipped with The second semiconductor layer is 1.0×10 13 / cm 3 Above 1.0 x 10 14 / cm 3 The following concentration of protons was introduced: 1.0×10 18 / cm 3 Above 5.0 x 10 18 / cm 3 The impurity concentration is as follows: The second semiconductor layer has a thickness of 1 μm or more and 5 μm or less, a peak of the proton concentration is located at a position 5 μm or less away from the interface between the first semiconductor layer and the second semiconductor layer toward the first electrode side,
2. A first conductivity type silicon carbide semiconductor substrate; a first semiconductor layer of a first conductivity type provided on a front surface of the silicon carbide semiconductor substrate and having a lower impurity concentration than the silicon carbide semiconductor substrate; a second semiconductor layer of a first conductivity type provided on a surface of the first semiconductor layer opposite to the silicon carbide semiconductor substrate; a third semiconductor layer of a first conductivity type having an impurity concentration lower than that of the silicon carbide semiconductor substrate, the third semiconductor layer being provided on a surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate; a fourth semiconductor layer of a second conductivity type provided on a surface of the third semiconductor layer opposite to the silicon carbide semiconductor substrate; a first semiconductor region of a first conductivity type selectively provided in a surface layer of the fourth semiconductor layer on a side opposite to the silicon carbide semiconductor substrate; a gate electrode provided via a gate insulating film on at least a portion of a surface of the fourth semiconductor layer sandwiched between the first semiconductor region and the third semiconductor layer; a first electrode provided on a surface of the fourth semiconductor layer and the first semiconductor region; A second electrode provided on a back surface of the silicon carbide semiconductor substrate; Equipped with the second semiconductor layer has protons introduced therein at a concentration of 1.0×10 13 / cm 3 or more and 1.0×10 14 / cm 3 or less, and has an impurity concentration of 1.0×10 18 / cm 3 or more and 5.0×10 18 / cm 3 or less; A silicon carbide semiconductor device, wherein a half width of the proton concentration is 5 μm or more and 10 μm or less.
3. A silicon carbide semiconductor device as described in claim 1 or 2, characterized in that helium is introduced instead of the protons.
4. A method for manufacturing a semiconductor device comprising the steps of: forming a first semiconductor layer of a first conductivity type on a front surface of a silicon carbide semiconductor substrate of a first conductivity type, the first semiconductor layer having a lower impurity concentration than the silicon carbide semiconductor substrate; a second step of forming a second semiconductor layer of a first conductivity type on a surface of the first semiconductor layer opposite to the silicon carbide semiconductor substrate, the second semiconductor layer having a thickness of 1 μm to 5 μm and an impurity concentration of 1.0×10 18 / cm 3 to 5.0×10 18 / cm 3 ; a third step of forming a third semiconductor layer of a first conductivity type having an impurity concentration lower than that of the silicon carbide semiconductor substrate on a surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate; a fourth step of forming a fourth semiconductor layer of a second conductivity type on a surface of the third semiconductor layer opposite to the silicon carbide semiconductor substrate; a fifth step of selectively forming a first semiconductor region of a first conductivity type in a surface layer of the fourth semiconductor layer on a side opposite to the silicon carbide semiconductor substrate; a sixth step of forming a gate electrode via a gate insulating film on at least a part of a surface of the fourth semiconductor layer sandwiched between the first semiconductor region and the third semiconductor layer; a seventh step of irradiating the second semiconductor layer with protons to set the proton concentration in the second semiconductor layer to 1.0×10 13 / cm 3 or more and 1.0×10 14 / cm 3 or less; an eighth step of forming a first electrode on a surface of the fourth semiconductor layer and the first semiconductor region; a ninth step of forming a second electrode on a back surface of the silicon carbide semiconductor substrate; Including, a proton concentration peak is set at a position 5 μm or less away from the interface between the first semiconductor layer and the second semiconductor layer toward the first electrode, in the seventh step.
5. A first step of forming a first semiconductor layer of a first conductivity type having a lower impurity concentration than a silicon carbide semiconductor substrate on a front surface of the silicon carbide semiconductor substrate; a second step of forming a second semiconductor layer of a first conductivity type having an impurity concentration of 1.0×10 18 / cm 3 or more and 5.0×10 18 / cm 3 or less on a surface of the first semiconductor layer opposite to the silicon carbide semiconductor substrate; a third step of forming a third semiconductor layer of a first conductivity type having an impurity concentration lower than that of the silicon carbide semiconductor substrate on a surface of the second semiconductor layer opposite to the silicon carbide semiconductor substrate; a fourth step of forming a fourth semiconductor layer of a second conductivity type on a surface of the third semiconductor layer opposite to the silicon carbide semiconductor substrate; a fifth step of selectively forming a first semiconductor region of a first conductivity type in a surface layer of the fourth semiconductor layer on a side opposite to the silicon carbide semiconductor substrate; a sixth step of forming a gate electrode via a gate insulating film on at least a part of a surface of the fourth semiconductor layer sandwiched between the first semiconductor region and the third semiconductor layer; a seventh step of irradiating the second semiconductor layer with protons to set the proton concentration in the second semiconductor layer to 1.0×10 13 / cm 3 or more and 1.0×10 14 / cm 3 or less; an eighth step of forming a first electrode on a surface of the fourth semiconductor layer and the first semiconductor region; a ninth step of forming a second electrode on a back surface of the silicon carbide semiconductor substrate; Including, a half-width of the concentration of the protons being set to 5 μm or more and 10 μm or less in the seventh step.
6. A method for manufacturing a silicon carbide semiconductor device as described in claim 4 or 5, characterized in that in the seventh step, the protons are irradiated from the first electrode side.
7. A method for manufacturing a silicon carbide semiconductor device described in any one of claims 4 to 6, further comprising a step of performing heat treatment on the first semiconductor region after the fifth step, and the seventh step is performed after the step of performing the heat treatment.
8. A method for manufacturing a silicon carbide semiconductor device according to claim 4, wherein helium is introduced instead of the protons.
Citation Information
Patent Citations
Silicon carbide semiconductor substrate and silicon carbide semiconductor device using the same
JP2009088223A
Semiconductor device and method for manufacturing the same
JP2018166196A
Silicon carbide semiconductor device and silicon carbide semiconductor device manufacturing method
JP2019102493A
Silicon carbide semiconductor substrate, method for manufacturing silicon carbide semiconductor substrate, semiconductor device, and method for manufacturing semiconductor device
JP6627938B2