Light color toner
Antimony-doped tin oxide particles with controlled properties in light-colored toners improve image density and color stability by enhancing conductivity and adherence, addressing issues of existing toners.
Patent Information
- Application Number
- JP2020173265
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-14
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-10-14
AI Technical Summary
Light-colored toners using existing external additives suffer from insufficient image density and color changes due to the addition of these additives.
Incorporating antimony-doped tin oxide particles with a specific number average primary particle diameter and Sb ratio into the toner particles, which enhances electrical conductivity and stability, ensuring appropriate color tone and image density.
The light-colored toner achieves stable image formation with appropriate color tone and excellent image density by using antimony-doped tin oxide particles within a specified range, preventing excessive charging and detachment.
Smart Images

Figure 0007574604000004 
Figure 0007574604000001 
Figure 0007574604000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a light color toner. [Background technology]
[0002] In image formation by electrophotography, a light-colored toner (e.g., yellow toner or light-colored special toner) containing toner particles is used. The toner particles include, for example, toner base particles and an external additive attached to the surface of the toner base particles. As the external additive used in the toner particles, abrasive particles may be used for the purpose of polishing the surface of a photoconductor (e.g., an amorphous silicon photoconductor). As such an external additive, conductive fine particles that have been subjected to a hydrophobic treatment have been proposed (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2007 / 114502 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the light-colored toner using the external additive described in Patent Document 1 does not provide sufficient image density for the images formed. Also, the light-colored toner using the external additive described in Patent Document 1 may have a change in color due to the addition of the external additive.
[0005] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a light-colored toner capable of forming an image having an appropriate color tone and excellent image density. [Means for solving the problem]
[0006] The light-colored toner according to the present invention includes toner particles. The toner particles include toner base particles and an external additive attached to the surface of the toner base particles. The external additive includes specific external additive particles. The specific external additive particles have a number average primary particle diameter of 30 nm or more and 305 nm or less. The specific external additive particles include antimony-doped tin oxide particles. In the antimony-doped tin oxide particles, the mass (M Sb ) and the mass of the tin atom (M Sn ) to the total mass of antimony atoms (M Sb ) ratio (M Sb / (M Sn +M Sb )) is 4 mass % or more and 31 mass % or less. Effect of the Invention
[0007] The light-colored toner according to the present invention can form an image having an appropriate color tone and excellent image density. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a diagram showing an example of a toner particle contained in a light-color toner according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] A preferred embodiment of the present invention will be described below. The toner is an aggregate (e.g., powder) of toner particles. The external additive is an aggregate (e.g., powder) of external additive particles. Unless otherwise specified, the evaluation results (values indicating shape, physical properties, etc.) of the powder (more specifically, the powder of toner particles, the powder of external additive particles, etc.) are the number averages of values measured for each of a considerable number of particles selected from the powder.
[0010] Volume median diameter of powder (D 50 ) unless otherwise specified, the measured value is a value measured based on the Coulter principle (pore electrical resistance method) using a Coulter Counter Multisizer 3 manufactured by Beckman Coulter, Inc.
[0011] Unless otherwise specified, the number average primary particle diameter of a powder is the number average value of the circle equivalent diameters of primary particles (Heywood diameter: diameter of a circle having the same area as the projected area of a primary particle) measured using a scanning electron microscope. The number average primary particle diameter of a powder is, for example, the number average value of the circle equivalent diameters of 100 primary particles. The number average primary particle diameter of particles refers to the number average primary particle diameter of particles in the powder unless otherwise specified.
[0012] Unless otherwise specified, the chargeability refers to the chargeability in triboelectric charging. For example, a standard carrier (standard carrier for negatively charged toner: N-01, standard carrier for positively charged toner: P-01) provided by the Imaging Society of Japan is mixed with the measurement target (e.g., toner) and stirred to triboelectrically charge the measurement target. The charge amount of the measurement target is measured before and after triboelectric charging, for example, with a small suction-type charge amount measuring device (Trek's "MODEL 212HS"), and the greater the change in charge amount before and after triboelectric charging, the stronger the chargeability of the measurement target.
[0013] Unless otherwise specified, the "major component" of a material means the component that is contained in the largest amount in the material on a mass basis.
[0014] Hereinafter, the compound and its derivatives may be collectively referred to by adding "based" after the compound name. When the compound name is followed by "based" to represent the name of a polymer, it means that the repeating unit of the polymer is derived from the compound or its derivative.
[0015] <Light color toner> The light-colored toner according to the embodiment of the present invention includes toner particles. The toner particles include toner base particles and an external additive attached to the surface of the toner base particles. The external additive includes specific external additive particles. The specific external additive particles have a number average primary particle diameter of 30 nm or more and 305 nm or less. The specific external additive particles include antimony-doped tin oxide particles. In the antimony-doped tin oxide particles, the mass (M Sb ) and the mass of the tin atom (M Sn) to the total mass of antimony atoms (M Sb ) ratio (M Sb / (M Sn +M Sb ) (hereinafter, sometimes referred to as Sb ratio) is 4 mass % or more and 31 mass % or less.
[0016] The light-colored toner of the present invention can be suitably used for developing an electrostatic latent image, for example, as a non-magnetic one-component toner having positive charging property. The light-colored toner of the present invention is, for example, a yellow toner or a light-colored special toner (for example, a white toner).
[0017] The light-colored toner of the present invention has the above-mentioned configuration, and can form an image having an appropriate color and excellent image density. The reason is explained below. The specific external additive particles contained in the light-colored toner of the present invention include antimony-doped tin oxide particles having a certain range of Sb ratio. The above-mentioned antimony-doped tin oxide particles reduce the electrical resistance of the light-colored toner of the present invention. Therefore, the light-colored toner of the present invention has excellent electric field response and excellent developability when developing an electrostatic latent image on a photoreceptor drum. In addition, the specific external additive particles have a number-average primary particle diameter of 30 nm or more, and are not excessively small particles. Therefore, the specific external additive particles are unlikely to be embedded in the toner mother particles when continuous image formation is performed. Furthermore, the specific external additive particles have a number-average primary particle diameter of 305 nm or less, and are not excessively large particles. Therefore, the specific external additive particles are unlikely to be detached from the toner mother particles when continuous image formation is performed. In this way, the specific external additive particles have a number average primary particle diameter of 30 nm or more and 305 nm or less, so that the specific external additive particles continue to stably adhere to the surface of the toner base particles even when image formation is performed continuously. As a result, the light-colored toner of the present invention can form images with excellent image density.
[0018] In addition, when the Sb ratio of the antimony-doped tin oxide particles is excessively high (for example, when the Sb ratio is more than 31% by mass), the antimony-doped tin oxide particles take on a black color, changing the color of the toner. The phenomenon in which the color of the toner changes due to the antimony-doped tin oxide particles having an excessively high Sb ratio has a small effect on dark color toners (for example, black toner, magenta toner, and cyan toner), but has a large effect on light color toners (especially yellow toner). The light color toner of the present invention suppresses the change in color of the toner due to the antimony-doped tin oxide particles by making the Sb ratio of the antimony-doped tin oxide particles 31% by mass or less. As a result, the light color toner of the present invention has an appropriate color.
[0019] The light-colored toner of the present invention will be described in further detail below. Each of the components described below may be used alone or in combination of two or more, unless otherwise specified.
[0020] [Toner particles] Fig. 1 shows an example of a toner particle 1 contained in a light-colored toner. The toner particle 1 shown in Fig. 1 includes a toner base particle 2 and an external additive attached to the surface of the toner base particle 2. The external additive includes specific external additive particles 3.
[0021] However, the toner particles contained in the light-colored toner of the present invention may have a structure different from that of the toner particle 1 shown in FIG. 1. Specifically, the toner particles may contain only specific external additive particles as an external additive, but may also contain other external additive particles (hereinafter, may be referred to as other external additive particles). The toner particles may also be toner particles having a shell layer (hereinafter, may be referred to as capsule toner particles). In the capsule toner particles, the toner mother particles have, for example, a toner core containing a binder resin and a colorant, and a shell layer covering the surface of the toner core. The details of the toner particles contained in the light-colored toner of the present invention have been described above with reference to FIG. 1.
[0022] The light-colored toner of the present invention has an appropriate color tone. Aand the Lab value of the pellets derived from the toner base particles B The difference between the specific external additive particles and the specific external additive particles can be expressed as ΔE. ΔE is measured by the method described in the Examples or a method based thereon. The light-colored toner of the present invention is preferably such that ΔE is smaller, since the color tone is not changed by the external addition of the specific external additive particles. In the light-colored toner of the present invention, ΔE is preferably 8.5 or less, more preferably 6.0 or less.
[0023] (Specific external additive particles) The specific external additive particles include antimony-doped tin oxide particles. The number-average primary particle diameter of the specific external additive particles is 30 nm or more and 305 nm or less, preferably 60 nm or more and 250 nm or less, and more preferably 100 nm or more and 200 nm or less. By making the number-average primary particle diameter of the specific external additive particles 30 nm or more, it is possible to suppress the specific external additive particles from being embedded in the toner base particles when continuously forming images. By making the number-average primary particle diameter of the specific external additive particles 305 nm or less, it is possible to suppress the specific external additive particles from being detached from the toner base particles when continuously forming images.
[0024] The antimony-doped tin oxide particles are particles containing antimony-doped tin oxide (ATO) as a main component. In the antimony-doped tin oxide particles, the content of antimony-doped tin oxide is preferably 70% by mass or more, more preferably 90% by mass or more, and even more preferably 100% by mass.
[0025] In antimony-doped tin oxide particles, the Sb ratio (M Sb / (M Sn +M Sb)) is 4% by mass or more and 31% by mass or less, preferably 10% by mass or more and 31% by mass or less, and more preferably 20% by mass or more and 28% by mass or less. Here, tin oxide alone does not exhibit electrical conductivity. Tin oxide to which a small amount of antimony is added (Sb ratio is 4% by mass or more and 31% by mass or less) is given properties as a semiconductor and exhibits electrical conductivity. Tin oxide to which a large amount of antimony is added has properties as a simple mixture of tin oxide and antimony and does not exhibit electrical conductivity. From the above, by setting the Sb ratio to 4% by mass or more and 31% by mass or less, the electrical conductivity of the antimony-doped tin oxide particles can be improved. As a result, the light-colored toner of the present invention can form an image with excellent image density. In addition, by setting the Sb ratio to 31% by mass or less, the change in color of the light-colored toner of the present invention due to the antimony-doped tin oxide particles can be suppressed.
[0026] The specific external additive particles are prepared, for example, using tin chloride and antimony chloride as raw materials. Therefore, the specific external additive particles may contain residual chlorine atoms derived from the raw materials. Chlorine atoms have high electronegativity. Therefore, the specific external additive particles containing a large amount of chlorine atoms tend to reduce the positive charging property of the toner and slightly reduce the image density of the formed image. From the above, it is preferable that the specific external additive particles do not contain chlorine atoms, or contain chlorine atoms, and the content ratio of chlorine atoms is more than 0.000 mass% and 0.020 mass% or less.
[0027] However, it is preferable that the specific external additive particles contain chlorine atoms in a small amount. The light-colored toner of the present invention contains the specific external additive particles, and therefore has a relatively low electrical resistance. Therefore, the light-colored toner of the present invention may experience a phenomenon in which the charge amount increases due to charge injection caused by the positive bias of the developing roller during development. In a normal environment, even if this phenomenon occurs, the light-colored toner of the present invention does not become excessively charged. However, if the above-mentioned phenomenon occurs in a low-temperature, low-humidity environment in which the charge amount of the toner is likely to increase, the light-colored toner of the present invention may become excessively charged. When the light-colored toner of the present invention is a non-magnetic one-component toner, if the light-colored toner of the present invention becomes excessively charged, the mirror force between the light-colored toner of the present invention and the developing roller becomes excessively high, and the layer thickness of the toner layer on the developing roller increases. On the other hand, if the light-colored toner of the present invention contains a small amount of chlorine atoms, the positive chargeability of the light-colored toner of the present invention is appropriately reduced. As a result, even in a low-temperature, low-humidity environment, it is possible to suppress the light-colored toner of the present invention from becoming excessively charged. From the above, it is preferable that the specific external additive particles contain chlorine atoms in a small amount. Specifically, the content of chlorine atoms in the specific external additive particles is preferably 0.001% by mass or more and 0.020% by mass or less, and more preferably 0.003% by mass or more and 0.010% by mass or less.
[0028] The content of the specific external additive particles in the toner particles is preferably 0.05 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.3 parts by mass or more and 1.0 parts by mass or less, relative to 100 parts by mass of the toner mother particles. By setting the content of the specific external additive particles to 0.05 parts by mass or more and 5.0 parts by mass or less, the image density of the image formed by the light-colored toner of the present invention can be further improved.
[0029] An example of a method for preparing the specific external additive particles will be described. An acid aqueous solution in which tin chloride (e.g., stannic chloride) and antimony chloride (e.g., antimony trichloride) are dissolved in hydrochloric acid, and an alkaline aqueous solution (e.g., an aqueous ammonia solution) are added to water. This results in a suspension containing antimony-doped tin oxide. Thereafter, the solid content contained in the suspension is washed and dried, and then pulverized to obtain the specific external additive particles. When the above-mentioned acid aqueous solution and alkaline aqueous solution are added, the pH and temperature of the suspension may be maintained within a certain range (e.g., pH 6.5 to 9.0, and 60°C to 80°C). In the above-mentioned washing process, the content ratio of chlorine atoms in the specific external additive particles can be adjusted by adjusting the number of washings. Specifically, in the above-mentioned washing process, the content ratio of chlorine atoms in the specific external additive particles is reduced by increasing the number of washings. In addition, in the above-mentioned pulverization process, the number average primary particle diameter of the specific external additive particles can be adjusted by adjusting the pulverization conditions.
[0030] (Other external additive particles) The external additive may contain only specific external additive particles, but preferably further contains other external additive particles.As the other external additive particles, inorganic particles are preferred, silica particles or metal oxide particles (e.g., alumina, titanium oxide, magnesium oxide, zinc oxide) are more preferred, and silica particles or titanium oxide particles are even more preferred.However, as the other external additive particles, organic acid compound particles such as fatty acid metal salts (e.g., zinc stearate) or resin particles may be used.
[0031] The content of the other external additive particles in the toner particles is preferably 0.1 parts by mass or more and 15.0 parts by mass or less, and more preferably 1.0 parts by mass or more and 5.0 parts by mass or less, relative to 100 parts by mass of the toner base particles, from the viewpoint of fully exerting its function while suppressing detachment from the toner base particles.
[0032] (Toner base particles) The toner base particles contain, for example, a binder resin as a main component. The toner base particles may further contain an internal additive (for example, at least one of a colorant, a release agent, a charge control agent, and a magnetic powder) as necessary. The toner base particles can be produced by a pulverization method or an aggregation method, and the pulverization method is preferred.
[0033] (Binding resin) From the viewpoint of providing a light-colored toner having excellent low-temperature fixing property, the toner base particles preferably contain a thermoplastic resin as a binder resin, and more preferably contain a thermoplastic resin in a proportion of 85% by mass or more of the total binder resin. Examples of the thermoplastic resin include styrene resin, acrylic ester resin, olefin resin (e.g., polyethylene resin and polypropylene resin), vinyl resin (e.g., vinyl chloride resin, polyvinyl alcohol, vinyl ether resin, and N-vinyl resin), polyester resin, polyamide resin, and urethane resin. Copolymers of these resins, that is, copolymers in which any repeating unit is introduced into the above resin (e.g., styrene-acrylic ester resin, and styrene-butadiene resin), can also be used as the binder resin.
[0034] The content of the binder resin in the toner base particles is preferably from 60% by mass to 95% by mass, and more preferably from 75% by mass to 90% by mass.
[0035] From the viewpoint of improving the low-temperature fixing property of the light-colored toner of the present invention, the binder resin is preferably a polyester resin. The polyester resin is obtained by polycondensation of one or more polyhydric alcohols and one or more polycarboxylic acids. Examples of the alcohol for synthesizing the polyester resin include dihydric alcohols (e.g., diol compounds and bisphenol compounds) and trihydric or higher alcohols. Examples of the carboxylic acid for synthesizing the polyester resin include dicarboxylic acids and trihydric or higher carboxylic acids. In place of the polycarboxylic acid, a polycarboxylic acid derivative capable of forming an ester bond by polycondensation (e.g., anhydrides of polycarboxylic acids and polycarboxylic acid halides) may be used.
[0036] Examples of diol compounds include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 2-butene-1,4-diol, 1,5-pentanediol, 2-pentene-1,5-diol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, 1,4-benzenediol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.
[0037] Examples of bisphenol compounds include bisphenol A, hydrogenated bisphenol A, ethylene oxide adducts of bisphenol A (eg, polyoxyethylene(2,2)-2,2-bis(4-hydroxyphenyl)propane), and propylene oxide adducts of bisphenol A.
[0038] Examples of trihydric or higher alcohols include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, diglycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene.
[0039] Examples of divalent carboxylic acids include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, cyclohexanedicarboxylic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, succinic acid, alkylsuccinic acids (more specifically, n-butylsuccinic acid, isobutylsuccinic acid, n-octylsuccinic acid, n-dodecylsuccinic acid, isododecylsuccinic acid), and alkenylsuccinic acids (more specifically, n-butenylsuccinic acid, isobutenylsuccinic acid, n-octenylsuccinic acid, n-dodecenylsuccinic acid, isododecenylsuccinic acid).
[0040] Examples of trivalent or higher carboxylic acids include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxylpropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, and empol trimer acid.
[0041] The polyester resin is preferably a condensation polymer of a bisphenol A ethylene oxide adduct, terephthalic acid, and trimellitic anhydride.
[0042] (Coloring agent) The toner base particles preferably contain a colorant. As the colorant, a known pigment or dye can be used according to the color of the light-colored toner of the present invention. From the viewpoint of forming a high-quality image using the light-colored toner of the present invention, the content of the colorant is preferably 1 part by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the binder resin.
[0043] The toner base particles may contain a color colorant, such as a yellow colorant.
[0044] The toner base particles may contain a white colorant, such as titanium dioxide, zinc oxide (zinc white), lithopone, and white lead.
[0045] The toner base particles preferably contain a yellow colorant.
[0046] As the yellow colorant, for example, one or more compounds selected from the group consisting of condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and arylamide compounds can be used. As the yellow colorant, for example, CI Pigment Yellow (3, 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 191, and 194), Naphthol Yellow S, Hansa Yellow G, and CI Vat Yellow can be mentioned.
[0047] (Release agent) The toner base particles may contain a release agent. The release agent is used, for example, for the purpose of imparting offset resistance to the light-colored toner of the present invention. From the viewpoint of imparting sufficient offset resistance to the light-colored toner of the present invention, the content of the release agent is preferably 1 part by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the binder resin.
[0048] Examples of the release agent include aliphatic hydrocarbon waxes, oxides of aliphatic hydrocarbon waxes, vegetable waxes, animal waxes, mineral waxes, ester waxes mainly composed of fatty acid esters, and waxes in which a part or all of the fatty acid esters are deoxidized. Examples of the aliphatic hydrocarbon waxes include low molecular weight polyethylene, low molecular weight polypropylene, polyolefin copolymers, polyolefin waxes, microcrystalline waxes, paraffin waxes, and Fischer-Tropsch waxes. Examples of the oxides of aliphatic hydrocarbon waxes include oxidized polyethylene waxes and block copolymers of oxidized polyethylene waxes. Examples of the vegetable waxes include candelilla wax, carnauba wax, Japan wax, jojoba wax, and rice wax. Examples of the animal waxes include beeswax, lanolin, and spermaceti. Examples of the mineral waxes include ozokerite, ceresin, and petrolatum. Examples of the ester waxes mainly composed of fatty acid esters include montan acid ester wax and castor wax. An example of the wax in which the fatty acid esters are partially or completely deoxidized is deoxidized carnauba wax. As the release agent, carnauba wax is preferred.
[0049] When the toner base particles contain a release agent, a compatibilizer may be added to the toner base particles in order to improve the compatibility between the binder resin and the release agent.
[0050] (Charge control agent) The toner base particles may contain a charge control agent. The charge control agent is used, for example, for the purpose of providing a toner having better charge stability or better charge rise characteristics. The charge rise characteristics of a toner are an index of whether or not the toner can be charged to a predetermined charge level in a short time. By incorporating a positively chargeable charge control agent in the toner base particles, the cationic nature of the toner base particles can be enhanced.
[0051] Examples of the positively charged charge control agent include azine compounds, direct dyes, acid dyes, alkoxylated amines, alkylamides, quaternary ammonium salt compounds, and resins containing quaternary ammonium cationic groups. As the charge control agent, quaternary ammonium salts are preferred.
[0052] Examples of the azine compound include pyridazine, pyrimidine, pyrazine, 1,2-oxazine, 1,3-oxazine, 1,4-oxazine, 1,2-thiazine, 1,3-thiazine, 1,4-thiazine, 1,2,3-triazine, 1,2,4-triazine, 1,3,5-triazine, 1,2,4-oxadiazine, 1,3,4-oxadiazine, 1,2,6-oxadiazine, 1,3,4-thiadiazine, 1,3,5-thiadiazine, 1,2,3,4-tetrazine, 1,2,4,5-tetrazine, 1,2,3,5-tetrazine, 1,2,4,6-oxatriazine, 1,3,4,5-oxatriazine, phthalazine, quinazoline, and quinoxaline.
[0053] Examples of direct dyes include Azin Fast Red FC, Azin Fast Red 12BK, Azin Violet BO, Azin Brown 3G, Azin Light Brown GR, Azin Dark Green BH / C, Azin Deep Black EW, and Azin Deep Black 3RL.
[0054] Acid dyes include, for example, Nigrosine BK, Nigrosine NB, and Nigrosine Z.
[0055] Examples of quaternary ammonium salts include benzyldecylhexylmethylammonium chloride, decyltrimethylammonium chloride, 2-(methacryloyloxy)ethyltrimethylammonium chloride, and dimethylaminopropylacrylamide methyl chloride quaternary salt.
[0056] From the viewpoint of providing a light-colored toner having further excellent charging stability, the content of the charge control agent is preferably 0.1 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the binder resin.
[0057] [Manufacturing method of light-colored toner] The light-colored toner of the present invention can be produced, for example, by a production method including a step of preparing toner base particles and a step of adding an external agent.
[0058] (Toner Base Particle Preparation Process) In the toner base particle preparation step, the toner base particles are prepared by, for example, an aggregation method or a pulverization method.
[0059] The aggregation method includes, for example, an aggregation step and a coalescence step. In the aggregation step, fine particles containing components constituting the toner base particles are aggregated in an aqueous medium to form aggregated particles. In the coalescence step, components contained in the aggregated particles are coalesced in the aqueous medium to form the toner base particles.
[0060] Next, the pulverization method will be described. The pulverization method allows the toner base particles to be prepared relatively easily and also allows the production cost to be reduced. When the toner base particles are prepared by the pulverization method, the preparation process of the toner base particles includes, for example, a melt-kneading process and a pulverization process. The preparation process of the toner base particles may further include a mixing process before the melt-kneading process. In addition, the preparation process of the toner base particles may further include at least one of a fine pulverization process and a classification process after the pulverization process.
[0061] In the mixing step, the binder resin and the internal additives added as necessary are mixed to obtain a mixture. In the melting and kneading step, the toner materials are melted and kneaded to obtain a molten and kneaded product. For example, the mixture obtained in the mixing step is used as the toner material. In the pulverizing step, the obtained molten and kneaded product is cooled, for example, to room temperature (25°C), and then pulverized to obtain a pulverized product. If it is necessary to reduce the diameter of the pulverized product obtained in the pulverizing step, a step of further pulverizing the pulverized product (fine pulverizing step) may be performed. In addition, if the particle size of the pulverized product is to be uniform, a step of classifying the obtained pulverized product (classifying step) may be performed. Through the above steps, the pulverized product, that is, toner base particles, is obtained.
[0062] (External addition process) In the external addition step, the above-mentioned toner base particles and the external additive are mixed using a mixer, and the external additive is attached to the surface of the toner base particles. This results in the light-colored toner of the present invention. The external additive includes specific external additive particles and other external additive particles that are used as necessary. As an example of the mixer, an FM mixer (manufactured by Nippon Coke & Engineering Co., Ltd.) can be mentioned. EXAMPLES
[0063] The present invention will be described in more detail below using examples, but the present invention is not limited to the scope of the examples.
[0064] [Preparation of external additive particles] The external additive particles (a) to (n) were prepared by the following method.
[0065] (External additive particles (a)) Two liters of water were added to the reaction vessel. The temperature of the water was kept at 70°C by heating and then keeping the reaction vessel warm. Separately, an acid solution was prepared by dissolving 825g of stannic chloride (SnCl4·5H2O) and 175g of antimony trichloride (SbCl3) in 1L of 2.4N hydrochloric acid. Ammonia aqueous solution (ammonia concentration 1mol / L) and the above-mentioned acid solution were dropped in parallel over one hour into a reaction vessel containing water at 70°C. In the parallel dropping, the amount of ammonia aqueous solution added was adjusted so that the pH of the contents of the reaction vessel was maintained at pH7-8. The contents of the reaction vessel became a suspension by the parallel dropping. Next, the suspension in the reaction vessel was suction filtered. In the suction filtration, a 2L Buchner funnel, a 1.1L funnel (manufactured by Asahi Seisakusho Co., Ltd.), and filter paper (Advantec Toyo Co., Ltd. "No. 131") were used. Next, the filter cake remaining on the filter paper was washed by pouring 1 L of water from above (washing operation). This washing operation was performed a total of six times. The conductivity of the washed filter cake was measured using an electric conductivity meter ("ES-51" manufactured by Horiba, Ltd.), and was 10 μS / cm. The washed filter cake was dried at 110°C for 12 hours, and then fired at 700°C for 2 hours in an electric furnace. Then, the fired filter cake was pulverized using a pulverizer ("CPY+DSF" impact plate type supersonic jet pulverizer manufactured by Nippon Pneumatic Mfg. Co., Ltd.). In the pulverization of the fired filter cake, a ceramic flat plate was used as the impact plate, the material supply rate was 7.0 kg / hour, and the pulverization pressure was 0.5 MPa. As a result, external additive particles (a) were obtained.
[0066] (External additive particles (b) to (l)) The external additive particles (b) to (l) were prepared in the same manner as the preparation of the external additive particles (a), except for the following changes: In the preparation of the external additive particles (b) to (l), the amounts of stannic chloride and antimony trichloride added, the number of filtrations in the washing operation, and the grinding conditions were changed as shown in Table 1 below.
[0067] (External additive particles (m)) Two liters of water and 100 g of titanium oxide particles (AEROXIDE (registered trademark) P25 manufactured by Nippon Aerosil Co., Ltd.) were put into a reaction vessel, and the titanium oxide particles were dispersed in the water. The reaction vessel was heated and then kept warm to maintain the temperature of the dispersion at 70°C. Separately, an acid solution was prepared by dissolving 413 g of stannic chloride (SnCl4·5H2O) and 88 g of antimony trichloride (SbCl3) in 1 L of 2.4 N hydrochloric acid. An aqueous ammonia solution (ammonia concentration 1 mol / L) and the above-mentioned acid solution were dropped in parallel over 1 hour into the reaction vessel containing the dispersion at 70°C. In the parallel dropping, the amount of the aqueous ammonia solution added was adjusted so that the pH of the contents of the reaction vessel was maintained at pH 7 to 8. The parallel dropping turned the contents of the reaction vessel into a suspension. Next, the suspension in the reaction vessel was suction filtered. In the suction filtration, a 2L Buchner funnel, a 1.1L funnel (manufactured by Asahi Seisakusho Co., Ltd.), and filter paper ("No. 131" manufactured by Advantec Toyo Co., Ltd.) were used. Next, the filter cake remaining on the filter paper was washed by pouring 1L of water from above (washing operation). This washing operation was performed a total of six times. The conductivity of the washed filter cake was measured using an electric conductivity meter ("ES-51" manufactured by Horiba, Ltd.), and was 10 μS / cm. The washed filter cake was dried at 110°C for 12 hours and then fired at 700°C for 2 hours in an electric furnace. The fired filter cake was then pulverized using a pulverizer ("CPY+DSF" impact plate type supersonic jet pulverizer manufactured by Nippon Pneumatic Mfg. Co., Ltd.). In the pulverization of the fired filter cake, a ceramic flat plate was used as the impact plate, the material supply rate was 6.0 kg / hour, and the pulverization pressure was 0.5 MPa. In this way, external additive particles (m) were obtained.
[0068] (External additive particles (n)) Titanium oxide particles ("AEROXIDE (registered trademark) P25" manufactured by Nippon Aerosil Co., Ltd.) were used as the external additive particles (n).
[0069] [Table 1]
[0070] (X-ray fluorescence analysis) The external additive particles (a) to (n) are analyzed by fluorescent X-rays, and the Sb ratio (M Sb / (M Sn +M Sb ))" and the content of chlorine atoms were calculated. The results are shown in Table 2 below. The conditions for the X-ray fluorescence analysis were as follows. Note that, to create a calibration curve for the X-ray fluorescence analysis, multiple types of calibration curve samples were used, each of which was a mixture of tin oxide (SnO2), antimony pentoxide, and sodium chloride in a specific blending ratio.
[0071] (X-ray fluorescence analysis conditions) Sample: Cylindrical pellets made by compressing additive particles at a pressure of 20 MPa for 3 seconds -Analysis equipment: Scanning X-ray fluorescence analyzer (Rigaku Corporation "ZSX") X-ray tube (X-ray source): Rh (rhodium) Excitation conditions: Tube voltage 50 kV, tube current 50 mA Measurement area (X-ray irradiation range): diameter 30 mm Measurement elements: antimony, chlorine, tin
[0072] (Particle size measurement) A cross-sectional image (magnification: 30,000 times) of the light-colored toner was taken using a scanning electron microscope ("JSM-6700F" manufactured by JEOL Ltd.). Based on the cross-sectional image, the circle-equivalent diameters of 100 external additive particles (specifically, any of the external additive particles (a) to (n)) were analyzed using image analysis software ("WinROOF" manufactured by Mitani Shoji Co., Ltd.), and the average value was taken as the number-average primary particle diameter. The results are shown in Table 2 below.
[0073] [Table 2]
[0074] Among the external additive particles (a) to (n), the external additive particles (a), (c) to (d), (g) to (h), and (j) to (l) were specific external additive particles.
[0075] [Preparation of binder resin] 1.0 mol of polyoxyethylene (2,2)-2,2-bis(4-hydroxyphenyl)propane, 4.5 mol of terephthalic acid, 0.5 mol of trimellitic anhydride, and 4 g of dibutyltin oxide were charged into a reaction vessel. The contents of the reaction vessel were reacted at 230°C for 8 hours under a nitrogen atmosphere. Thereafter, the pressure in the reaction vessel was reduced to 8.3 kPa, and the unreacted components in the reaction vessel were distilled off under reduced pressure. Thereafter, the contents of the reaction vessel (polyester resin) were washed and then dried. As a result, a polyester resin with a softening point of 120°C was obtained. This polyester resin was used as a binder resin.
[0076] [Preparation of toner base particles] Using an FM mixer ("FM-20B" manufactured by Nippon Coke & Engineering Co., Ltd.), 100 parts by mass of the above-mentioned polyester resin as a binder resin, 4 parts by mass of Pigment Yellow 74 ("Seika Fast Yellow 7040Y" manufactured by Dainichiseika Chemicals Co., Ltd.) as a yellow colorant, 10 parts by mass of Carnauba wax ("Carnauba No. 1" manufactured by Kato Yoko Co., Ltd.) as a wax, and 3 parts by mass of a quaternary ammonium salt compound ("FCA210PS" manufactured by Fujikura Kasei Co., Ltd.) as a charge control agent were mixed. The mixture obtained was then melt-kneaded at 150°C using a twin-screw extruder ("TEM45" manufactured by Toshiba Machine Co., Ltd.). The kneaded product obtained after cooling was coarsely pulverized with a Feather Mill (registered trademark) ("350 x 600" manufactured by Hosokawa Micron Corporation). The coarsely pulverized product obtained was finely pulverized with an airflow type pulverizer ("Jet Mill IDS-2" manufactured by Nippon Pneumatic Mfg. Co., Ltd.). The resulting finely pulverized material was classified using an elbow jet classifier (Nippon Steel Mining Co., Ltd., "Elbow Jet EJ-LABO Model"). This resulted in toner base particles with a volume median diameter of 7 μm. The volume median diameter of the toner base particles was measured using a particle sizer (Beckman Coulter, Inc., "Coulter Counter Multisizer 3").
[0077] [External Addition Treatment] 100.0 parts by mass of the toner base particles, 1.5 parts by mass of silica particles ("AEROSIL (registered trademark) REA90" manufactured by Nippon Aerosil Co., Ltd.) as an external additive, and external additive particles of the type and mass parts shown in Table 3 below were mixed in an FM mixer ("FM-10" manufactured by Nippon Coke and Engineering Co., Ltd.). As a result, light-colored toners (yellow toners) of Examples 1 to 8 and Comparative Examples 1 to 7 were obtained. In Comparative Example 5, only silica particles were used as the external additive.
[0078] <Evaluation> The light-colored toners of Examples 1 to 8 and Comparative Examples 1 to 7 were evaluated for color tone, image density of formed images, and fixability by the following methods. The evaluation results are shown in Table 3 below.
[0079] [Evaluation machine] A monochrome printer ("HL-1218W" manufactured by Brother Industries, Ltd.) was used as the evaluation machine. A light-colored toner (specifically, any of the light-colored toners of Examples 1 to 8 and Comparative Examples 1 to 7) was put into the development device of the evaluation machine. The development device of the evaluation machine also functioned as a toner container. In other words, the evaluation machine was a monochrome printer with a development device replacement system. As the printing paper, "Multi Paper Super White+ (registered trademark)" manufactured by Askul Corporation was used.
[0080] [Image Density] Using the evaluation machine, a pattern image with a printing rate of 5% was continuously formed on 1,500 sheets of printing paper under conditions of a temperature of 23°C and a humidity of 50%. Then, a solid image was formed on the above-mentioned printing paper (toner loading amount: 0.7 mg / cm 2 The image density (ID) of the formed solid image was measured with a reflection densitometer ("RD914" manufactured by X-Rite). The image density was evaluated according to the following criteria.
[0081] (Image Density Evaluation Criteria) A (very good): ID is 1.3 or higher B (Good): ID is 1.1 or more and less than 1.3 C (bad): ID is less than 1.1
[0082] [Color] 0.2 g of the light-colored toners of Examples 1 to 8 and Comparative Examples 1 to 7 and 0.2 g of the above-mentioned toner base particles were each placed in a molding machine (Labo Dice φ20 manufactured by LabNect Co., Ltd.) and pressed (15 MPa) with a hydraulic press machine (Labo Press LP-100 manufactured by LabNect Co., Ltd.) to form pellets (diameter 20 mm). Lab values of pellets derived from each toner A and the Lab value of the pellets derived from the toner base particles B The Lab value for each light-colored toner was measured using a reflection densitometer (SpectroEye (registered trademark) manufactured by X-Rite). A and Lab value B The difference between the two values, ΔE, was calculated. Whether each light-colored toner had an appropriate color tone was evaluated based on ΔE. In detail, light-colored toners with a large ΔE were evaluated as not having an appropriate color tone because the color tone was changed by the external additive particles, based on the following criteria.
[0083] (Change in color) A (particularly good): ΔE is less than 6.0 B (Good): ΔE is 6.0 or more and less than 8.5 C (Failure): ΔE is 8.5 or more
[0084] [Fixation] Using the evaluation machine, a solid image was formed on printing paper under conditions of a temperature of 10°C and a humidity of 10% RH (toner loading amount: 0.7 mg / cm 2 ). The occurrence of offset was judged by subjecting the printing paper (evaluation paper) on which a solid image was formed to the following folding and rubbing test. In the folding and rubbing test, the evaluation paper was folded so that the side on which the solid image was formed was on the inside and the crease passed through the center of the solid image. Next, the folded evaluation paper was rubbed back and forth five times on the crease while applying a load of 1 kg using a brass weight (1 kg) covered with cotton cloth. Next, the evaluation paper was unfolded, and the length of peeling of the light-colored toner in the folded part of the evaluation paper where the solid image was fixed (peeling length) was measured. Fixability was evaluated according to the following criteria.
[0085] (Evaluation Criteria for Fixation) A (very good): Less than 0.07 mm B (Good): 0.07mm or more and less than 0.10mm C (defective): 0.10mm or more
[0086] [Table 3]
[0087] The light-colored toners of Examples 1 to 8 each contained toner particles. The toner particles included toner base particles and an external additive attached to the surface of the toner base particles. The external additive contained specific external additive particles. The specific external additive particles had a number average primary particle diameter of 30 nm or more and 305 nm or less. The specific external additive particles contained antimony-doped tin oxide particles. In the antimony-doped tin oxide particles, the Sb ratio was 4 mass % or more and 31 mass % or less. The light-colored toners of Examples 1 to 8 were able to form images having appropriate color meanings and excellent image density and fixing properties.
[0088] On the other hand, the light-colored toners of Comparative Examples 1 to 7 did not have the above-mentioned configuration, and therefore at least one of the color, image density and fixability of the formed image was poor.
[0089] Specifically, the external additive particles (b) used in the light-colored toner of Comparative Example 1 were antimony-doped tin oxide particles with an Sb ratio of less than 4% by mass. It is considered that the external additive particles (b) had a relatively high electrical resistance, and therefore the image density of the formed image was insufficient.
[0090] The external additive particles (e) used in the light-colored toner of Comparative Example 2 were antimony-doped tin oxide particles with an Sb ratio of more than 31% by mass. Since the external additive particles (e) were black, it was determined that the light-colored toner of Comparative Example 2 did not have an appropriate color.
[0091] The number average primary particle diameter of the external additive particles (f) and (i) used in the light-colored toners of Comparative Examples 3 and 4 was less than 30 nm or more than 305 nm. It is considered that the image density of the formed images was insufficient because the external additive particles (f) and (i) were embedded in the toner base particles or detached from the toner base particles during continuous image formation.
[0092] The light-colored toner of Comparative Example 5 did not use specific external additive particles. The external additive particles (m) and (n) used in the toners of Comparative Examples 6 and 7 were conductive titanium oxide particles or titanium oxide particles. It is considered that the external additive particles (m) and (n) have relatively high electrical resistance. It is also considered that the external additive particles (m) aggregate on the surface of the toner base particles because ATO acts as an aggregating agent, and are easily detached from the surface of the toner base particles. Therefore, it is considered that the image density of the images formed by the light-colored toners of Comparative Examples 5 to 7 was insufficient. [Industrial Applicability]
[0093] The light-colored toner of the present invention can be used to form images in, for example, a copier, a printer, or a multifunction machine. [Explanation of symbols]
[0094] 1 Toner particles 2. Toner base particles 3. Specific external additive particles
Claims
1. A light-color toner which is a non-magnetic one-component toner containing toner particles and is a yellow toner or a white toner, The toner particles include a toner base particle and an external additive attached to a surface of the toner base particle, The external additive contains specific external additive particles, The specific external additive particles have a number average primary particle diameter of 30 nm or more and 305 nm or less, The specific external additive particles include antimony-doped tin oxide particles, In the antimony-doped tin oxide particles, the content of antimony-doped tin oxide is 90 mass % or more, and the mass of antimony atoms (M Sb ) and the mass of a tin atom (M Sn ) to the total mass of antimony atoms (M Sb ) ratio (M Sb / (M Sn +M Sb ) is 4% by mass or more and 31% by mass or less.
2. The specific external additive particles are Does not contain chlorine atoms 2. The light-color toner according to claim 1, further comprising a chlorine atom, the chlorine atom content being more than 0.000% by mass and not more than 0.020% by mass.
3. 3. The light-color toner according to claim 2, wherein the specific external additive particles contain chlorine atoms, and the content of chlorine atoms is from 0.001% by mass to 0.020% by mass.
4. The toner base particles contain a binder resin and a colorant, 4. The light-colored toner according to claim 1, wherein the colorant comprises a yellow colorant.
Citation Information
Patent Citations
Developing method
JP1987184473A
Electrostatic latent image developing toner
JP1992024646A
Liquid crystal optical element
JP1994202084A
Developing sleeve and developing device
JP1996160737A
Two-component developer
JP2020129029A