Toner for developing electrostatic images, electrostatic image developer, toner cartridge, process cartridge and image forming apparatus

A toner formulation with controlled alumina and silica particle sizes and ratios, along with specific metal element management, stabilizes charge distribution to prevent image density unevenness in high temperature and humidity environments.

JP7574740B2Active Publication Date: 2024-10-29FUJIFILM BUSINESS INNOVATION CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021087063
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-24
Publication Date
2024-10-29
Estimated Expiration
2041-05-24

AI Technical Summary

Technical Problem

Existing toners experience uneven image density when transitioning from low to high image density in high temperature and high humidity environments due to excessive charging of toner particles, particularly when alumina particles are used as external additives.

Method used

The toner formulation includes alumina particles with a volume average size of 5-80 nm and silica particles with a size of 10-90 nm, with a controlled ratio of silica to alumina content and specific metal element intensities, forming a two-layer structure that stabilizes charging and reduces unevenness.

Benefits of technology

The toner effectively suppresses image density unevenness by maintaining a stable charge distribution, ensuring consistent image quality even in challenging environmental conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574740000005
    Figure 0007574740000005
  • Figure 0007574740000006
    Figure 0007574740000006
  • Figure 0007574740000001
    Figure 0007574740000001
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor with high wear resistance.SOLUTION: An electrostatic charge image development toner provided herein comprises toner particles containing a binder resin, and an external additive containing alumina particles having a volume average particle diameter greater than 5 nm and equal to or less than 80 nm and silica particles having a volume average particle diameter greater than 10 nm and equal to or less than 90 nm. A total Net strength NA of an alkali metal element and an alkali earth metal element of the toner particles is in a range of 0.10 to 1.20 kcps, inclusive, as measured by fluorescent X-ray analysis. A ratio (Ws / Wa) of the content Ws of the silica particles to the content Wa of the alumina particles is greater than 0.5 and less than 35.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner for developing an electrostatic image, an electrostatic image developer, a toner cartridge, a process cartridge and an image forming apparatus. [Background technology]

[0002] Patent Document 1 proposes "a toner having toner particles containing at least a binder resin, a colorant, a release agent, and a resin having sulfur atoms, and an inorganic fine powder mixed with the toner particles, characterized in that (i) the toner particles contain at least one element selected from the group consisting of magnesium, calcium, barium, zinc, aluminum, and phosphorus, and satisfy the following formula: 4≦(total content of the above elements (T): ppm) / (content of sulfur element (S): ppm)≦30, (ii) the weight average particle size (D4) of the toner is 3 μm to 10 μm, and (iii) the average circularity of the toner is 0.950 to 0.995." Patent Document 2 proposes "a toner for developing electrostatic images, the toner having toner particles including toner base particles and an external additive disposed on the surface of the toner base particles, the toner base particles including a crystalline resin as a binder resin, the external additive including alumina particles, and the abundance ratio of aluminum atoms on the surface of the toner particles being 0.8 atom % or more and 5.0 atom % or less." Patent Document 3 proposes "an electrostatic image developer comprising at least an electrostatic image developing toner containing toner particles having an external additive on the surface of toner base particles, and carrier particles, wherein the external additive constituting the toner particles contains at least composite oxide particles mainly composed of alumina and silica, the composite oxide particles contain alumina in the range of 5 to 50 mass % and silica in the range of 50 to 95 mass %, the number average particle size of primary particles of the composite oxide particles is in the range of 7 to 80 nm, and the composite oxide particles have a hydrophobicity of 40 or more." [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-062807 A [Patent Document 2] JP 2019-200345 A [Patent Document 3] JP 2020-038308 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention provides a toner for developing electrostatic images, comprising toner particles containing a binder resin, and an external additive containing alumina particles having a volume average particle size of more than 5 nm and not more than 80 nm, and silica particles having a volume average particle size of 10 nm or more and not more than 90 nm, the toner particles having a total net intensity N A The object of the present invention is to provide a toner for developing electrostatic images which can suppress uneven image density when an image with a high image density is formed after successively forming an image with a low image density under a high temperature and high humidity environment, compared with a case in which the silica particle content Ws to the alumina particle content Wa is less than 0.10 kcps or exceeds 1.30 kcps, or a ratio (Ws / Wa) of the silica particle content Ws to the alumina particle content Wa is 0.5 or less or 35 or more. [Means for solving the problem]

[0005] The above problems are solved by the following means: <1> toner particles containing a binder resin; and an external additive containing alumina particles having a volume average particle size of more than 5 nm and not more than 80 nm and silica particles having a volume average particle size of 10 nm or more and not more than 90 nm, The net intensity N of the total of alkali metal elements and alkaline earth metal elements in the toner particles is measured by fluorescent X-ray analysis. A is 0.10 kcps or more and 1.30 kcps or less, The toner for developing electrostatic images, wherein a ratio (Ws / Wa) of a content Ws of the silica particles to a content Wa of the alumina particles is more than 0.5 and less than 35. <2> The net strength N A is 0.20 kcps or more and 1.00 kcps or less. <1> 2. The toner for developing electrostatic images according to claim 1 . <3> The alkali metal element and the alkaline earth metal element include at least one element selected from the group consisting of Na, Mg, and Ca. <1> or <2> 2. The toner for developing electrostatic images according to claim 1 . <4> The alkali metal element and the alkaline earth metal element include at least one element selected from the group consisting of Na and Mg. <1> or <2> 2. The toner for developing electrostatic images according to claim 1 . <5> The net intensity N of the S element in the toner particles measured by fluorescent X-ray analysis S is 3.0 kcps or more and 6.0 kcps or less. <1> ~ <4> 10. The toner for developing an electrostatic image according to claim 9, <6> The net strength N A For the net strength N S Ratio (N S / N A ) is more than 3 and less than 40 <5> 2. The toner for developing electrostatic images according to claim 1 . <7> The binder resin contains an amorphous polyester resin and a crystalline polyester resin. <1> ~ <6> 10. The toner for developing an electrostatic image according to claim 9, <8> The crystalline polyester resin is a polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol. <7> 2. The toner for developing electrostatic images according to claim 1 . <9> The ratio of the volume average particle diameter of the silica particles to the volume average particle diameter of the alumina particles is 0.2 or more and 2.0 or less. <1> ~ <8> 10. The toner for developing an electrostatic image according to claim 9, <10> In X-ray photoelectron spectroscopy (XPS) before ultrasonic treatment, the ratio of the amount of Si detected to the amount of Al detected is 3.0 to 10.5, In X-ray photoelectron spectroscopy (XPS) after ultrasonic treatment, the amount of Si detected is 2.5 to 8.5 relative to the amount of Al detected. <1> ~ <9> 10. The toner for developing an electrostatic image according to claim 9, <11> The above <1> ~ <10> 2. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1. <12> The above <1> ~ <10> 13. A toner cartridge which contains the toner for developing electrostatic images according to any one of claims 1 to 12 and is detachably mountable to an image forming apparatus. <13> The above <11> and a developing means for developing an electrostatic image formed on a surface of an image carrier by using the electrostatic image developer into a toner image. <14> An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; The above <11> a developing means for developing the electrostatic image formed on the surface of the image carrier into a toner image by using the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising: Effect of the Invention

[0006] <1> , <3> or <4> According to the invention, in a toner for developing an electrostatic image, the toner particles include a binder resin, and an external additive includes alumina particles having a volume average particle size of more than 5 nm and not more than 80 nm, and silica particles having a volume average particle size of 10 nm or more and not more than 90 nm. The net intensity N of the total of alkali metal elements and alkaline earth metal elements in the toner particles measured by fluorescent X-ray analysis is Ais less than 0.10 kcps or more than 1.30 kcps, or the ratio (Ws / Wa) of the silica particle content Ws to the alumina particle content Wa is 0.5 or less or 35 or more. <2> According to the invention, the net strength N A The present invention provides a toner for developing electrostatic images that can suppress uneven image density when a high image density image is formed after successively forming low image density images under a high temperature and high humidity environment, as compared with a case where the toner has a viscosity of less than 0.20 kcps or more than 1.00 kcps. <5> According to the present invention, the net intensity N of the S element in the toner particles measured by fluorescent X-ray analysis S The present invention provides a toner for developing electrostatic images that can suppress uneven image density when a high image density image is formed after successively forming low image density images under a high temperature and high humidity environment, as compared with a case where the static charge density is less than 3.0 kcps or more than 6.0 kcps. <6> According to the invention, the net strength N A For the net strength N S Ratio (N S / N A ) is 3 or less or 40 or more, the toner for developing electrostatic images is provided, which can suppress unevenness in image density when a high-density image is formed after successively forming a low-density image under a high-temperature and high-humidity environment, as compared with the case where the ratio is 3 or less or 40 or more. <7> According to the invention, there is provided a toner for developing electrostatic images, which can suppress unevenness in image density when a high image density image is formed after successively forming low image density images under a high temperature and high humidity environment, compared to when the binder resin contains only an amorphous polyester resin. <8> According to the invention, there is provided a toner for developing electrostatic images, which can suppress unevenness in image density when an image with a high image density is formed after images with a low image density are successively formed under a high temperature and high humidity environment, compared with a case in which the crystalline resin contained in the binder resin is a polymer of an aromatic dicarboxylic acid and a diol having a double bond other than a polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol. <9> According to the invention, there is provided a toner for developing electrostatic images, which can suppress uneven image density when a high image density image is formed after successively forming low image density images under a high temperature and high humidity environment, compared to when the ratio of the volume average particle size of the silica particles to the volume average particle size of the alumina particles is less than 0.2 or exceeds 2.0. <10> According to the invention, there is provided a toner for developing electrostatic images, which comprises toner particles containing a binder resin, and an external additive containing alumina particles having a volume average particle size of more than 5 nm and 80 nm or less, and silica particles having a volume average particle size of 10 nm or more and 90 nm or less, and which can suppress image density unevenness when forming low-density images and then forming high-density images in succession under a high-temperature, high-humidity environment, compared to when the amount of Si detected relative to the amount of Al detected in X-ray photoelectron spectroscopy (XPS) before ultrasonic treatment is less than 3.0 or exceeds 10.5, or when the amount of Si detected relative to the amount of Al detected in X-ray photoelectron spectroscopy (XPS) after ultrasonic treatment is less than 2.5 or exceeds 8.5. <11> ~ <14> According to the invention, in a toner for developing an electrostatic image, the toner particles include a binder resin, and an external additive includes alumina particles having a volume average particle size of more than 5 nm and not more than 80 nm, and silica particles having a volume average particle size of 10 nm or more and not more than 90 nm. The net intensity N of the total of alkali metal elements and alkaline earth metal elements in the toner particles measured by fluorescent X-ray analysis is AThe present invention provides an electrostatic image developer, a toner cartridge, a process cartridge and an image forming apparatus each including an electrostatic image developing toner that can suppress uneven image density when forming an image with a high image density after successively forming images with a low image density in a high temperature and high humidity environment, compared to when using an electrostatic image developing toner having an electrostatic image developing toner in which the viscosity of the electrostatic image is less than 0.10 kcps or more than 1.20 kcps, or a toner in which the ratio (Ws / Wa) of the silica particle content Ws to the alumina particle content Wa is 0.5 or less or 35 or more. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of a process cartridge according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, an embodiment of the present invention will be described in detail. In addition, in numerical ranges described in stages, the upper limit or lower limit value described in a certain numerical range may be replaced with the upper limit or lower limit value of another numerical range described in stages. In addition, in a numerical range, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples. When a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. The term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified.

[0009] "Alkali metal element" refers to Li, Na, K, Rb, Cs, and Fr. "Alkaline earth metal elements" refers to Be, Mg, Ca, Sr, Ba, and Ra.

[0010] <Toner for developing electrostatic images> The toner for developing electrostatic images according to this embodiment (hereinafter, "toner for developing electrostatic images" may also be simply referred to as "toner") has toner particles containing a binder resin, and an external additive containing alumina particles having a volume average particle size of more than 5 nm and not more than 80 nm and silica particles having a volume average particle size of 10 nm or more and not more than 90 nm. In addition, the net intensity N of the total of the alkali metal elements and the alkaline earth metal elements in the toner particles measured by fluorescent X-ray analysis A is 0.10 kcps or more and 1.30 kcps or less, and a ratio (Ws / Wa) of the content Ws of the silica particles to the content Wa of the alumina particles is more than 0.5 and less than 35.

[0011] The toner according to the present embodiment, with the above-mentioned configuration, suppresses unevenness in image density when a high-density image is formed after a low-density image is formed successively under a high-temperature and high-humidity environment. The reason for this is presumed to be as follows.

[0012] Alumina particles are used as an external additive in order to improve the environmental stability of toner charging. Since alumina particles have a lower electrical resistance than other external additives, when low-density images are continuously formed under a high-temperature and high-humidity environment using a toner containing alumina particles, the toner may be easily overcharged. Then, when a high-density image is subsequently formed, image density unevenness may easily occur.

[0013] It is presumed that the toner according to the present embodiment can be achieved by the following mechanism. The toner has an external additive containing alumina particles having a volume average particle size of more than 5 nm and not more than 80 nm, and silica particles having a volume average particle size of 10 nm or more and not more than 90 nm. By setting the volume average particle size of the alumina particles and the silica particles within the above range, a difference in specific gravity is likely to occur between the two particles. Since the alumina particles have a larger specific gravity than the silica particles, the alumina particles adhere to the toner particle surface, and the silica particles adhere thereon. In other words, a two-layer structure of the external additive, a layer of the alumina particles and a layer of the silica particles thereon, is likely to be formed on the toner particle surface. By setting the ratio (Ws / Wa) of the content Ws of the silica particles to the content Wa of the alumina particles to be more than 0.5 and less than 35, the bias in the content of the alumina particles and the silica particles is suppressed, so that the two-layer structure of the external additive is more easily formed. A The net strength in the toner is 0.10 kcps or more and 1.30 kcps or less. A By setting the above range, adsorbed moisture is easily attached to the alkali metal element and alkaline earth metal element present on the surface side of the toner particle. In other words, since the toner particle surface contains a large amount of adsorbed moisture, the external additive is more easily attached to the toner surface, and the two-layer structure of the external additive is easily maintained. For the above reasons, the toner according to the present embodiment has a structure containing a large amount of the silica particles on the outermost surface. Since the silica particles have a relatively high electrical resistance, the toner is unlikely to be excessively charged even when low-density images are continuously formed under a high-temperature and high-humidity environment.

[0014] Therefore, it is presumed that the toner according to this embodiment suppresses unevenness in image density when a high density image is formed after successively forming low density images in a high temperature and high humidity environment.

[0015] (Toner particles) The toner particles contain a binder resin. The toner particles may also contain a colorant, a release agent, an alkali metal element source, an alkaline earth metal element source, an S element source, and other additives. -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.

[0016] Examples of the binder resin include non-crystalline (also called "non-crystalline") resins and crystalline resins. The "crystalline" nature of a resin refers to the presence of a clear endothermic peak rather than a stepwise change in the amount of endothermic heat in differential scanning calorimetry (DSC); specifically, the half-width of the endothermic peak is within 15°C when measured at a heating rate of 10 (°C / min). On the other hand, the term "amorphous" for a resin refers to a half-width exceeding 15° C., a stepwise change in endothermic heat quantity, or no clear endothermic peak being observed.

[0017] The amorphous resin will now be described. Examples of the amorphous resin include known amorphous resins such as amorphous polyester resin, amorphous vinyl resin (e.g., styrene acrylic resin, etc.), epoxy resin, polycarbonate resin, polyurethane resin, etc. Among these, from the viewpoint of improving the dispersibility of the alkali metal element and the alkaline earth metal element in the toner particles and making the metal element more likely to be present on the toner surface side, amorphous polyester resin and amorphous vinyl resin (particularly styrene acrylic resin) are preferred, and amorphous polyester resin is more preferred. In addition, it is also a preferred embodiment to use an amorphous polyester resin and a styrene-acrylic resin in combination as the amorphous resin. It is also a preferred embodiment to use an amorphous resin having an amorphous polyester resin segment and a styrene-acrylic resin segment (hereinafter also referred to as a "hybrid amorphous resin") as the amorphous resin.

[0018] The amorphous polyester resin may be, for example, a condensation polymer of a polyvalent carboxylic acid and a polyhydric alcohol. The amorphous polyester resin may be a commercially available product or a synthesized product.

[0019] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). Among these, aromatic dicarboxylic acids are preferable as polyvalent carboxylic acids. The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower alkyl esters thereof (e.g., carbon number 1 to 5). The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0020] Examples of polyhydric alcohols include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol, a polyhydric alcohol having a crosslinked or branched structure of three or more may be used in combination with the diol. Examples of the polyhydric alcohol having a trihydric or higher valence include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.

[0021] The amorphous polyester resin can be obtained by a known manufacturing method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.

[0022] Here, the amorphous polyester resin may be a modified amorphous polyester resin in addition to the unmodified amorphous polyester resin described above. The modified amorphous polyester resin is an amorphous polyester resin having a bond group other than an ester bond, or an amorphous polyester resin having a resin component different from the amorphous polyester resin component bonded by a covalent bond or an ionic bond. The modified amorphous polyester resin may be, for example, an amorphous polyester resin having a functional group such as an isocyanate group that reacts with an acid group or a hydroxyl group at the end introduced therein, and a resin having a modified end that is reacted with an active hydrogen compound.

[0023] The styrene-acrylic resin is a copolymer obtained by copolymerizing at least a styrene-based monomer (a monomer having a styrene skeleton) and a (meth)acrylic-based monomer (a monomer having a (meth)acrylic group, preferably a monomer having a (meth)acryloxy group). The styrene-acrylic resin includes, for example, a copolymer of a styrene monomer and a (meth)acrylic acid ester monomer. The acrylic resin portion of the styrene-acrylic resin is a partial structure formed by polymerizing either an acrylic monomer or a methacrylic monomer, or both. In addition, the term "(meth)acrylic" includes both "acrylic" and "methacrylic".

[0024] Specific examples of styrene-based monomers include styrene, alkyl-substituted styrenes (e.g., α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, etc.), halogen-substituted styrenes (e.g., 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, etc.), vinylnaphthalene, etc. The styrene-based monomers may be used alone or in combination of two or more. Of these, as the styrene-based monomer, styrene is preferred from the viewpoints of ease of reaction, ease of reaction control, and availability.

[0025] Specific examples of the (meth)acrylic monomer include (meth)acrylic acid and (meth)acrylic acid esters. Examples of the (meth)acrylic acid esters include (meth)acrylic acid alkyl esters (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, n-lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, n-hexadecyl (meth)acrylate, n-octadecyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, amyl (meth)acrylate, and (meth) Examples of the (meth)acrylic acid monomer include neopentyl acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, etc.), aryl (meth)acrylate esters (e.g., phenyl (meth)acrylate, biphenyl (meth)acrylate, diphenylethyl (meth)acrylate, t-butylphenyl (meth)acrylate, terphenyl (meth)acrylate, etc.), dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, β-carboxyethyl (meth)acrylate, and (meth)acrylamide. The (meth)acrylic acid monomer may be used alone or in combination of two or more. Among these (meth)acrylic esters among the (meth)acrylic monomers, from the viewpoint of fixation, (meth)acrylic acid esters having an alkyl group having 2 to 14 carbon atoms (preferably 2 to 10 carbon atoms, more preferably 3 to 8 carbon atoms) are preferred. Of these, n-butyl (meth)acrylate is preferred, and n-butyl acrylate is particularly preferred.

[0026] The copolymerization ratio of the styrene monomer to the (meth)acrylic monomer (mass basis, styrene monomer / (meth)acrylic monomer) is not particularly limited, but is preferably 85 / 15 to 70 / 30.

[0027] The styrene-acrylic resin may have a crosslinked structure. A preferred example of the styrene-acrylic resin having a crosslinked structure is a copolymer of at least a styrene-based monomer, a (meth)acrylic acid-based monomer, and a crosslinkable monomer.

[0028] The crosslinkable monomer may, for example, be a bifunctional or higher functional crosslinking agent. Examples of bifunctional crosslinking agents include divinylbenzene, divinylnaphthalene, di(meth)acrylate compounds (e.g., diethylene glycol di(meth)acrylate, methylene bis(meth)acrylamide, decanediol diacrylate, glycidyl (meth)acrylate, etc.), polyester type di(meth)acrylate, 2-([1'-methylpropylideneamino]carboxyamino)ethyl methacrylate, etc. Examples of polyfunctional crosslinking agents include tri(meth)acrylate compounds (e.g., pentaerythritol tri(meth)acrylate, trimethylolethane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, etc.), tetra(meth)acrylate compounds (e.g., pentaerythritol tetra(meth)acrylate, oligoester (meth)acrylate, etc.), 2,2-bis(4-methacryloxy, polyethoxyphenyl)propane, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, diaryl chlorendate, etc. Among these, as the crosslinkable monomer, from the viewpoints of suppressing the occurrence of a decrease in image density and suppressing the occurrence of uneven image density, and of fixability, a bifunctional or higher (meth)acrylate compound is preferred, a bifunctional (meth)acrylate compound is more preferred, a bifunctional (meth)acrylate compound having an alkylene group with 6 to 20 carbon atoms is further preferred, and a bifunctional (meth)acrylate compound having a linear alkylene group with 6 to 20 carbon atoms is particularly preferred.

[0029] The copolymerization ratio of the crosslinkable monomer to the total monomers (mass basis, crosslinkable monomer / total monomers) is not particularly limited, but is preferably 2 / 1,000 to 20 / 1,000.

[0030] The method for producing the styrene-acrylic resin is not particularly limited, and various polymerization methods (e.g., solution polymerization, precipitation polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc.) are applied. In addition, the polymerization reaction is carried out by a known operation (e.g., batchwise, semi-continuous, continuous, etc.).

[0031] Hybrid amorphous resin The hybrid amorphous resin is an amorphous resin in which an amorphous polyester resin segment and a styrene-acrylic resin segment are chemically bonded to each other. Examples of the hybrid amorphous resin include a resin having a main chain made of a polyester resin and a side chain made of a styrene-acrylic resin chemically bonded to the main chain; a resin having a main chain made of a styrene-acrylic resin and a side chain made of a polyester resin chemically bonded to the main chain; a resin having a main chain formed by chemically bonding a polyester resin and a styrene-acrylic resin; a resin having a main chain formed by chemically bonding a polyester resin and a styrene-acrylic resin, and at least one of a side chain made of a polyester resin chemically bonded to the main chain and a side chain made of a styrene-acrylic resin chemically bonded to the main chain; and the like.

[0032] The amorphous polyester resin and the styrene-acrylic resin in each segment are as described above, and therefore the description thereof will be omitted.

[0033] The total amount of the polyester resin segment and the styrene-acrylic resin segment in the entire hybrid amorphous resin is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and even more preferably 100 mass%.

[0034] In the hybrid amorphous resin, the proportion of the styrene-acrylic resin segment in the total amount of the polyester resin segment and the styrene-acrylic resin segment is preferably 20% by mass or more and 60% by mass or less, more preferably 25% by mass or more and 55% by mass or less, and even more preferably 30% by mass or more and 50% by mass or less.

[0035] The hybrid amorphous resin is preferably produced by any one of the following methods (i) to (iii). (i) After preparing a polyester resin segment by condensation polymerization of a polyhydric alcohol and a polycarboxylic acid, a monomer constituting a styrene-acrylic resin segment is addition-polymerized. (ii) A styrene-acrylic resin segment is prepared by addition polymerization of an addition-polymerizable monomer, and then a polyhydric alcohol and a polycarboxylic acid are condensation-polymerized. (iii) Polycondensation of a polyhydric alcohol and a polycarboxylic acid and addition polymerization of an addition-polymerizable monomer are carried out in parallel.

[0036] The proportion of the hybrid amorphous resin in the total binder resin is preferably 60% by mass or more and 98% by mass or less, more preferably 65% ​​by mass or more and 95% by mass or less, and even more preferably 70% by mass or more and 90% by mass or less.

[0037] The glass transition temperature (Tg) of the amorphous resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), more specifically, from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."

[0038] The weight average molecular weight (Mw) of the amorphous resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the amorphous resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the amorphous resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.

[0039] The crystalline resin will now be described. Examples of the crystalline resin include known crystalline resins such as crystalline polyester resins and crystalline vinyl resins (e.g., polyalkylene resins, long-chain alkyl (meth)acrylate resins, etc.) Among these, crystalline polyester resins are preferred from the viewpoint of improving the dispersibility of alkali metal elements and alkaline earth metal elements in the toner particles and making the metal elements more likely to be present on the toner surface side.

[0040] The crystalline polyester resin may be, for example, a polycondensate of a polyvalent carboxylic acid and a polyhydric alcohol. The crystalline polyester resin may be a commercially available product or a synthesized product. Here, the crystalline polyester resin is preferably a polycondensate using a polymerizable monomer having a linear aliphatic group rather than a polymerizable monomer having an aromatic group, since the crystalline polyester resin can easily form a crystalline structure.

[0041] Examples of polyvalent carboxylic acids include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower alkyl esters (e.g., carbon number 1 to 5). As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0042] Examples of polyhydric alcohols include aliphatic diols (for example, straight-chain aliphatic diols having 7 to 20 carbon atoms in the main chain). Examples of aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred as aliphatic diols. The polyhydric alcohol may be a trihydric or higher alcohol having a crosslinked or branched structure in combination with the diol. Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.

[0043] Here, the polyhydric alcohol has an aliphatic diol content of 80 mol % or more, preferably 90 mol % or more.

[0044] The crystalline polyester resin can be obtained by a known manufacturing method, for example, in the same manner as the amorphous polyester.

[0045] The melting temperature of the crystalline resin is preferably 50°C or higher and 100°C or lower, more preferably 55°C or higher and 90°C or lower, and even more preferably 60°C or higher and 85°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."

[0046] The weight average molecular weight (Mw) of the crystalline resin is preferably 6,000 or more and 35,000 or less.

[0047] From the viewpoint of improving the dispersibility of the metal elements and making the metal elements more likely to be present on the toner surface side by the interaction between the carboxyl groups derived from the crystalline polyester resin and the alkali metal elements and alkaline earth metal elements in the toner particles, the crystalline polyester resin is preferably a polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol.

[0048] The α,ω-linear aliphatic dicarboxylic acid is preferably an α,ω-linear aliphatic dicarboxylic acid in which the alkylene group connecting the two carboxy groups has 3 or more and 14 or less carbon atoms, more preferably the alkylene group has 4 or more and 12 or less carbon atoms, and even more preferably the alkylene group has 6 or more and 10 or less carbon atoms. Examples of α,ω-linear aliphatic dicarboxylic acids include succinic acid, glutaric acid, adipic acid, 1,6-hexanedicarboxylic acid (commonly known as suberic acid), 1,7-heptanedicarboxylic acid (commonly known as azelaic acid), 1,8-octanedicarboxylic acid (commonly known as sebacic acid), 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid. Of these, 1,6-hexanedicarboxylic acid, 1,7-heptanedicarboxylic acid, 1,8-octanedicarboxylic acid, and 1,10-decanedicarboxylic acid are preferred. The α,ω-linear aliphatic dicarboxylic acids may be used alone or in combination of two or more kinds.

[0049] The α,ω-linear aliphatic diol is preferably an α,ω-linear aliphatic diol in which the alkylene group connecting the two hydroxy groups has 3 to 14 carbon atoms, more preferably the alkylene group has 4 to 12 carbon atoms, and further preferably the alkylene group has 6 to 10 carbon atoms. Examples of the α,ω-linear aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,14-tetradecanediol, and 1,18-octadecanediol. Of these, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are preferred. The α,ω-linear aliphatic diols may be used alone or in combination of two or more kinds.

[0050] As the polymer of an α,ω-linear aliphatic dicarboxylic acid and an α,ω-linear aliphatic diol, from the viewpoint of improving the dispersibility of an alkali metal element and an alkaline earth metal element in a toner particle and making the metal element more likely to be present on the toner surface side, a polymer of at least one selected from the group consisting of 1,6-hexanedicarboxylic acid, 1,7-heptanedicarboxylic acid, 1,8-octanedicarboxylic acid, 1,9-nonanedicarboxylic acid, and 1,10-decanedicarboxylic acid and at least one selected from the group consisting of 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol is preferred, and among these, a polymer of 1,10-decanedicarboxylic acid and 1,6-hexanediol is more preferred.

[0051] From the viewpoint of improving the dispersibility of the metal elements by the interaction between the alkali metal elements and the alkaline earth metal elements in the toner particles and making the metal elements more likely to be present on the toner surface side, it is preferable that the binder resin contains an amorphous polyester resin and a crystalline polyester resin.

[0052] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, Examples of the dyes include pigments such as ultramarine blue, chalcoil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate; and dyes such as acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes. The colorant may be used alone or in combination of two or more kinds.

[0053] The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination.

[0054] The content of the colorant is preferably from 1% by mass to 30% by mass, and more preferably from 3% by mass to 15% by mass, based on the total mass of the toner particles.

[0055] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.

[0056] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K 7121-1987 "Method for measuring transition temperature of plastics."

[0057] The content of the release agent is, for example, preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total amount of the toner particles.

[0058] -Source of alkali metal elements- The toner particles have a net intensity of N A From the viewpoint of achieving a viscosity of 0.10 kcps or more and 1.20 kcps or less, it is preferable to contain an alkali metal element source.

[0059] The alkali metal element supply source may be an additive containing an alkali metal element (such as a surfactant or a flocculant). Specifically, the additive containing an alkali metal element may be, for example, a salt containing an alkali metal element. Examples of salts containing an alkali metal element include salts containing lithium element, such as lithium chloride, lithium sulfate, lithium nitrate, etc.; salts containing sodium element, such as sodium chloride, sodium sulfate, sodium nitrate, etc.; salts containing potassium element, such as potassium chloride, potassium sulfate, potassium nitrate, etc.; salts containing rubidium element, such as rubidium chloride, rubidium sulfate, rubidium nitrate, etc.; salts containing cesium element, such as cesium chloride, cesium sulfate, cesium nitrate, etc.; and salts containing francium element, such as francium chloride, francium sulfate, francium nitrate, etc. Examples of the salt containing an alkali metal element include salts containing an alkali metal element sulfonate (eg, sodium alkylbenzenesulfonate such as sodium dodecylbenzenesulfonate).

[0060] -Source of alkaline earth metal elements- The alkaline earth metal element supply source may be an additive containing an alkaline earth metal element (such as a surfactant or a flocculant). Specifically, the additive containing an alkaline earth metal element may be, for example, a salt containing an alkaline earth metal element. Specific examples of salts containing alkaline earth metal elements include salts containing beryllium element, such as beryllium chloride, beryllium sulfate, and beryllium nitrate; salts containing magnesium element, such as magnesium chloride, magnesium sulfate, and magnesium nitrate; salts containing calcium element, such as calcium chloride, calcium sulfate, and calcium nitrate; salts containing strontium element, such as strontium chloride, strontium sulfate, and strontium nitrate; salts containing barium element, such as barium chloride, barium sulfate, and barium nitrate; and salts containing radium element, such as radium chloride, radium sulfate, and radium nitrate. Examples of salts containing an alkaline earth metal element include salts containing an alkaline earth metal element sulfonate (calcium alkylbenzenesulfonate such as calcium dodecylbenzenesulfonate) and metal sulfides (calcium polysulfide).

[0061] The salt containing an alkali metal element is preferably a salt containing a sodium element, such as sodium chloride, sodium sulfate, or sodium nitrate. The salt containing an alkaline earth metal element is preferably a salt containing magnesium element such as magnesium chloride, magnesium sulfate, magnesium nitrate, etc.; and a salt containing calcium element such as calcium chloride, calcium sulfate, calcium nitrate, etc.; and more preferably a salt containing magnesium element such as magnesium chloride, magnesium sulfate, magnesium nitrate, etc.

[0062] The total content of the alkali metal element source and the alkaline earth metal element source in the toner particles is the net strength N A should be added so that the viscosity becomes 0.10 kcps or more and 1.20 kcps or less.

[0063] -S element supply source- Examples of the S element source include additives containing sulfur (surfactants, flocculants, chain transfer agents, initiators, etc.). Specifically, examples of the sulfur source include metal sulfates, metal sulfonates, and metal sulfides. Examples of metal sulfates include alkali metal sulfates (lithium sulfate, sodium sulfate, potassium sulfate, rubidium sulfate, cesium sulfate, francium sulfate, etc.), alkaline earth metal sulfates (beryllium sulfate, magnesium sulfate, calcium sulfate, strontium sulfate, barium sulfate, radium sulfate, etc.), aluminum sulfate, and polyiron (II) sulfate. Examples of the metal sulfonate include metal alkylbenzenesulfonates (such as sodium dodecylbenzenesulfonate and calcium dodecylbenzenesulfonate). The sulfides include calcium polysulfide and the like.

[0064] The content of the S element source in the toner particles is the net strength N S It is preferable to add it so that the viscosity becomes 3.0 kcps or more and 6.0 kcps or less.

[0065] -Other additives- Examples of other additives include well-known additives such as magnetic materials, charge control agents, inorganic powders, etc. These additives are contained in the toner particles as internal additives.

[0066] -Net strength- Net intensity N of the total of alkali metal elements and alkaline earth metal elements in the toner particles measured by X-ray fluorescence analysis A is 0.10 kcps or more and 1.30 kcps or less, and preferably 0.2 kcps or more and 1.00 kcps or less.

[0067] The external additive becomes more easily attached to the toner surface, and the two-layer structure of the external additive is further maintained. In order to achieve this, the net strength N A is preferably 0.20 kcps or more and 1.00 kcps or less, and more preferably 0.20 kcps or more and 0.50 kcps or less.

[0068] Net strength N of alkali metal elements and alkaline earth metal elements A is calculated by measuring the net strength of alkali metal elements and the net strength of alkaline earth metal elements by the following method and adding up these measured values.

[0069] The method for measuring the net strength of alkali metal elements and the net strength of alkaline earth metal elements is as follows. Approximately 0.12 g of toner particles (or toner having toner particles and external additives) is compressed with a compression molding machine under a load of 6 t for 60 seconds to produce a disk with a diameter of 50 mm and a thickness of 2 mm. This disk is used as a sample and qualitative and quantitative elemental analysis is performed under the following conditions using a scanning X-ray fluorescence analyzer (Rigaku ZSX PrimusII) to determine the net intensity (unit: kilo counts per second, kcps) of each of the alkali metal elements and alkaline earth metal elements. The net intensity of the alkali metal elements and the net intensity of the alkaline earth metal elements are then summed to obtain the net intensity N A Calculate. Tube voltage: 40kV ·Tube current: 70mA ·Anti-cathode: Rhodium Measurement time: 15 minutes ·Analysis diameter: 10mm in diameter

[0070] From the viewpoint of making the adsorbed moisture more easily adhered and further maintaining the two-layer structure of the external additive, it is preferable that the alkali metal element and the alkaline earth metal element include at least one selected from the group consisting of Na, Mg, and Ca.

[0071] From the viewpoint of further facilitating adhesion of the adsorbed moisture and further maintaining the two-layer structure of the external additive, it is preferable that the alkali metal element and the alkaline earth metal element include at least one selected from the group consisting of Na and Mg.

[0072] Net intensity of Na element, N, measured by X-ray fluorescence analysis Nis preferably 0.01 kcps or more and 0.20 kcps or less, more preferably 0.02 kcps or more and 0.15 kcps or less, and even more preferably 0.03 kcps or more and 0.10 kcps or less. In addition, from the viewpoint of suppressing uneven density and white spots in the obtained image, the net intensity N M is more preferably 0.15 kcps or more and 1.10 kcps or less, and further preferably 0.20 kcps or more and 1.00 kcps or less.

[0073] Here, the net strength of Na element N N , Net intensity of Mg element N M , and the net intensity of Ca element N C The measurement is the net intensity N of Na element during qualitative and quantitative elemental analysis. N , Net intensity of Mg element N M , and the net intensity of Ca element N C The measurement is performed in the same manner as the measurement of the net strength of alkali metal elements and the net strength of alkaline earth metal elements, except that the above is determined.

[0074] The toner according to the present embodiment has a net intensity N S is preferably 3.0 kcps or more and 6.0 kcps or less, more preferably 3.5 kcps or more and 5.5 kcps or less, and even more preferably 4.0 kcps or more and 5.0 kcps or less.

[0075] Net intensity of S element N S By setting the above range, unevenness in image density can be further suppressed when a low-density image is successively formed and then a high-density image is formed in a high-temperature and high-humidity environment. The reason for this is presumed to be as follows.

[0076] Net intensity of S element N S In order to keep the content within the above range, it is preferable to add a source of S element. The S element has a function of increasing the dispersibility of the alkali metal element and the alkaline earth metal element in the toner particles. S By adding the S element source so that the S content falls within the above range, the dispersibility of the alkali metal element and the alkaline earth metal element in the toner particles is improved. As a result, the alkali metal element and the alkaline earth metal element are more likely to be present on the surface side of the toner particles, and the adsorbed moisture is more likely to adhere to these elements. Therefore, the external additive is more likely to adhere to the toner surface, and the two-layer structure of the external additive is more likely to be maintained. From the above, the net strength of the S element N S It is presumed that by keeping the above range, unevenness in image density can be further suppressed when a high-density image is formed after a low-density image is successively formed in a high-temperature and high-humidity environment.

[0077] Here, the net intensity of the S element, N S The measurement is the net intensity N of the S element during qualitative and quantitative elemental analysis. S The measurement is performed in the same manner as the measurement of the net strength of alkali metal elements and the net strength of alkaline earth metal elements, except that the above is determined.

[0078] Net strength N A Net strength N S Ratio (N S / N A ) is preferably more than 3 and less than 40, more preferably 5 or more and 35 or less, more preferably 10 or more and 30 or less, and even more preferably 15 or more and 25 or less. The ratio (N S / N A ) within the above range improves the dispersibility of the alkali metal element and the alkaline earth metal element in the toner particles while suppressing charge leakage caused by the inclusion of the S element, and it is presumed that this further suppresses unevenness in image density when a high image density image is formed after successively forming low image density images under a high temperature and high humidity environment.

[0079] -Characteristics of toner particles, etc.- The toner particles may be toner particles having a single layer structure, or may be toner particles having a so-called core-shell structure composed of a core portion (core particle) and a coating layer (shell layer) that coats the core portion. Here, the toner particles having a core-shell structure may be composed of, for example, a core containing a binder resin and, if necessary, other additives such as a colorant and a release agent, and a coating layer containing the binder resin.

[0080] The volume average particle size (D50v) of the toner particles is preferably from 2 μm to 10 μm, and more preferably from 4 μm to 8 μm.

[0081] The various average particle sizes and particle size distribution indexes of the toner particles are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant, and this is then added to 100 ml to 150 ml of the electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture diameter of 100 μm. The number of particles sampled is 50,000. Based on the measured particle size distribution, cumulative distributions of volume and number are drawn for each divided particle size range (channel) from the smallest diameter side, and the particle size at 16% of the cumulative size is defined as the volume particle size D16v, the number particle size D16p, the particle size at 50% of the cumulative size as the volume average particle size D50v, the cumulative number average particle size D50p, and the particle size at 84% of the cumulative size as the volume particle size D84v and number particle size D84p. Using these, the volumetric particle size distribution index (GSDv) is (D84v / D16v) 1 / 2 The number size distribution index (GSDp) is (D84p / D16p) 1 / 2 It is calculated as:

[0082] The average circularity of the toner particles is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less.

[0083] The average circularity of toner particles is calculated by (circular equivalent perimeter) / (perimeter) [(perimeter of a circle having the same projected area as the particle image) / (perimeter of the particle projected image)]. Specifically, it is a value measured by the following method. First, the toner particles to be measured are sucked and collected, flattened, and a still image of the particles is captured by instantaneous strobe light emission, and the particle image is analyzed by a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation). The number of samples to be taken in order to calculate the average circularity is 3,500. When the toner contains an external additive, the toner (developer) to be measured is dispersed in water containing a surfactant, and then ultrasonic treatment is performed to obtain toner particles from which the external additive has been removed.

[0084] (External additives) The toner according to the present embodiment contains, as external additives, alumina particles having a volume average particle size of more than 5 nm and not more than 80 nm, and silica particles having a volume average particle size of 10 nm or more and not more than 90 nm.

[0085] -Alumina particles- Alumina particles are aluminum oxide particles represented by Al2O3. The alumina particles have a volume average particle size of more than 5 nm and not more than 80 nm. By setting the volume average particle size of the alumina particles to more than 5 nm, the occurrence of aggregation between the alumina particles is suppressed, and the two-layer structure of the external additive is less likely to collapse. By setting the volume average particle size of the alumina particles to 80 nm or less, the dispersibility on the toner particle surface is improved, and the alumina particles are more likely to adhere to the toner particle surface in a nearly uniform state, which makes it easier to form a two-layer structure of the external additive.

[0086] From the viewpoint of making it easier to form a two-layer structure of the external additive, the volume average particle size of the alumina particles is preferably 10 nm or more and 60 nm or less, more preferably 15 nm or more and 50 nm or less, and even more preferably 18 nm or more and 40 nm or less.

[0087] Here, the volume average particle size of the alumina particles is measured by the following method. EDX device (manufactured by Horiba, EMAX Evolution X-Max80mm 2 ) is attached to a scanning electron microscope (SEM) (S-4800, manufactured by Hitachi High-Technologies) to capture images at a magnification of 40,000. By EDX analysis, 100 or more primary particles of alumina particles are identified based on the presence of Al. Images of the identified primary particles of alumina particles are imported into an image analyzer (LUZEXIII, manufactured by Nireco Corporation), and the area of ​​each particle is measured by image analysis of the primary particles, and the circle-equivalent diameter is calculated from this area value. This calculation of the circle-equivalent diameter is performed for 100 alumina particles. The 50% diameter (D50v) of the volume-based cumulative frequency of the obtained circle-equivalent diameters is then determined as the volume-average particle diameter of the alumina particles. The magnification of the electron microscope is adjusted so that 10 to 50 alumina particles are captured in one field of view, and the circular equivalent diameter of the primary particles is determined by combining observations of multiple fields of view.

[0088] The average circularity of the alumina particles is preferably 0.75 or more and 1.0 or less, more preferably 0.9 or more and 1.0 or less, and even more preferably 0.92 or more and 0.98 or less. When the average circularity of the alumina particles is within the above range, the alumina particles become closer to a sphere, the adhesive force to the toner particles is easily controlled, and the two-layer structure of the external additive is more easily formed.

[0089] Here, the average circularity of the alumina particles is measured by the following method. First, the circularity of the alumina particles is obtained by observing the primary particles of the alumina particles with a SEM device, and calculating from the planar image analysis of the obtained primary particles according to the following formula, "100 / SF2". Formula: Circularity (100 / SF2) = 4π × (A / I 2 ) (In the formula, I represents the perimeter of the primary particle on the image, and A represents the projected area of ​​the primary particle.) The average circularity of the alumina particles is obtained as the 50% circularity in the cumulative frequency of the circularities of 100 primary particles obtained by the above-mentioned planar image analysis.

[0090] The surfaces of the alumina particles are preferably subjected to a hydrophobic treatment. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, aluminum coupling agents, etc. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, preferably 1 part by mass or more and 50 parts by mass or less, more preferably 5 parts by mass or more and 30 parts by mass or less, and even more preferably 8 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the alumina particles.

[0091] As the hydrophobizing agent, it is preferable to use at least one of a silane coupling agent and a silicone oil. Examples of the silane coupling agent include a compound represented by the following formula (A) and a compound represented by the following formula (B). (R1, R2, R3)-Si-NH-Si-(R1, R2, R3) Formula (A) (R4) 4-n -Si-(OR5) n Formula (B) R1 to R5 are each independently a hydrogen atom, an alkyl group, an aryl group, or an alkoxy group. The alkyl group, the aryl group, and the alkoxy group may have a substituent. R1 to R5 may be the same or different.

[0092] Specifically, the compound represented by formula (A) is preferably hexamethyldisilazane (in the above formula (A), R1, R2 and R3 are each a methyl group) or hexaethyldisilazane (in the above formula (A), R1, R2 and R3 are each an ethyl group), with hexamethyldisilazane being particularly preferred.

[0093] Specifically, as the compound represented by formula (B), it is more preferable that at least one of R1 to R5 in formula (B) is a linear alkyl group having a carbon number of 1 to 12. The linear alkyl group may have a substituent. In the compound represented by the above formula (B), R4 in formula (B) is more preferably a linear alkyl group having 1 to 12 carbon atoms. In the compound represented by the above formula (B), R5 in formula (B) is preferably a methyl group or an ethyl group.

[0094] Examples of silicone oils include organosiloxane oligomers, cyclic compounds such as octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, tetramethylcyclotetrasiloxane, and tetravinyltetramethylcyclotetrasiloxane; linear or branched organosiloxanes; and silicone oils having modified groups. In addition, the silicone oil having a modified group may have, as its type, an alkoxy, carboxy, carbinol, higher fatty acid modified, phenol, epoxy, methacryl, amino, or the like.

[0095] The surface of the alumina particles can be hydrophobized by a known method, such as a dry method or a wet method.

[0096] The dry method is a method of hydrophobizing the surfaces of alumina particles by stirring the alumina particles and a hydrophobizing agent in a reactor such as a fluidized bed. The wet method is a method of hydrophobizing the surfaces of alumina particles by first dispersing the alumina particles in a solvent to form a slurry of the alumina particles, and then adding a hydrophobizing agent to the slurry.

[0097] The method for hydrophobization is preferably a dry method. When the surfaces of alumina particles are hydrophobized by a dry method, the alumina particles and the hydrophobizing agent are stirred and heated at 100° C. or more and 200° C. or less for 0.5 hours or more and 5 hours or less.

[0098] The volume resistivity of alumina particles is 1.0×10 8 Ω cm or more 1.0×10 13 Ω cm or less is preferable, and 1.0×10 9 Ω cm or more 1.0×10 11 Ω·cm or less is more preferable. The volume resistivity of alumina particles is measured as follows. Alumina particles are pressure molded at a surface pressure of 20t to obtain a pellet having a diameter of 20 mm and a thickness of 5.0 mm. The electrical resistance of the pellet is measured at 20°C and 50% RH using a digital ultra-high resistance / microammeter R8340A (manufactured by Advantest Corporation).

[0099] The content of the alumina particles is preferably from 0.05% by mass to 5.0% by mass, more preferably from 0.2% by mass to 2.0% by mass, and even more preferably from 0.4% by mass to 1.0% by mass, based on the toner particles.

[0100] -Silica particles- The external additive includes silica particles. The volume average particle size of the silica particles is 10 nm or more and 90 nm or less. By setting the volume average particle size of the silica particles to 10 nm or more, the thickness of the layer made of the silica particles in the two-layer structure of the external additive increases, making it difficult for the toner to be excessively charged. By setting the volume average particle size of the silica particles to 90 nm or less, the silica particles are less likely to become liberated.

[0101] From the viewpoint of making it easier to form a two-layer structure of the external additive, the volume average particle size of the silica particles is preferably 20 nm or more and 80 nm or less, more preferably 25 nm or more and 70 nm or less, and even more preferably 30 nm or more and 60 nm or less.

[0102] Here, the volume average particle size of the silica particles is measured by the following method. EDX device (manufactured by Horiba, EMAX Evolution X-Max80mm 2 ) is attached to a scanning electron microscope (SEM) (S-4800, manufactured by Hitachi High-Technologies) to capture images at a magnification of 40,000. By EDX analysis, 100 or more primary particles of silica particles are identified based on the presence of Si. Images of the identified primary particles of silica particles are imported into an image analyzer (LUZEXIII, manufactured by Nireco Corporation), and the area of ​​each particle is measured by image analysis of the primary particles, and the circle-equivalent diameter is calculated from this area value. This calculation of the circle-equivalent diameter is performed for 100 silica particles. The 50% diameter (D50v) of the volume-based cumulative frequency of the obtained circle-equivalent diameters is then determined as the volume-average particle diameter of the silica particles. The magnification of the electron microscope is adjusted so that 10 to 50 silica particles are captured in one field of view, and the circular equivalent diameter of the primary particles is determined by combining observations of multiple fields of view.

[0103] The average circularity of the silica particles is preferably 0.75 or more and 1.0 or less, more preferably 0.9 or more and 1.0 or less, and even more preferably 0.92 or more and 0.98 or less. When the average circularity of the silica particles is within the above range, the silica particles become closer to a sphere, the adhesion to the toner particles is easily controlled, and the two-layer structure of the external additive is more easily formed.

[0104] Here, the average circularity of the silica particles is measured by the following method. First, the circularity of the silica particles is obtained by observing the primary particles of the silica particles with an SEM device, and calculating from the planar image analysis of the obtained primary particles according to the following formula, "100 / SF2". Formula: Circularity (100 / SF2) = 4π × (A / I 2 ) (In the formula, I represents the perimeter of the primary particle on the image, and A represents the projected area of ​​the primary particle.) The average circularity of the silica particles is obtained as the 50% circularity in the cumulative frequency of the circularities of 100 primary particles obtained by the above-mentioned planar image analysis.

[0105] The surfaces of the silica particles are preferably subjected to a hydrophobic treatment. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, aluminum coupling agents, etc. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 50 parts by mass or less with respect to 100 parts by mass of the silica particles.

[0106] As the hydrophobizing agent, it is preferable to use at least one of a silane coupling agent and a silicone oil. Specific examples of the silane coupling agent and silicone oil include the hydrophobic treatment agent used for the alumina particles.

[0107] The content of the silica particles is preferably from 0.5% by mass to 5.0% by mass, more preferably from 0.8% by mass to 4.6% by mass, and even more preferably from 1.0% by mass to 4.2% by mass, based on the toner particles.

[0108] -Other external additives- As the external additive, an external additive other than the alumina particles and the silica particles may be used in combination. Other external additives include, for example, inorganic particles, such as TiO2, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, K2O·(TiO2)n, Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, and MgSO4.

[0109] The surface of the inorganic particles as other external additives may be subjected to hydrophobic treatment. The hydrophobic treatment is carried out, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the inorganic particles.

[0110] Other external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate (PMMA), and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles), and the like.

[0111] The amount of the other external additives added is, for example, preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the toner particles.

[0112] -External additive content ratio (Ws / Wa)- In the toner according to the present embodiment, the ratio (Ws / Wa) of the content Ws of the silica particles to the content Wa of the alumina particles is more than 0.5 and less than 35.

[0113] From the viewpoint of making it easier to form a two-layer structure of the external additive, the ratio (Ws / Wa) is preferably 1.5 or more and 25 or less, more preferably 2.0 or more and 15 or less, and further preferably 2.5 or more and 5 or less.

[0114] - Ratio of volume average particle size of external additives - In the toner according to this embodiment, the ratio of the volume average particle diameter of the silica particles to the volume average particle diameter of the alumina particles is preferably 0.2 to 2.0, more preferably 0.4 to 1.8, and even more preferably 0.6 to 1.6. By setting the ratio of the volume average particle size of the silica particles to the volume average particle size of the alumina particles within the above range, the difference in specific gravity between the alumina particles and the silica particles becomes greater, making it easier to achieve a structure in which the alumina particles adhere to the surface of the toner particles and the silica particles then adhere thereon.

[0115] (Toner characteristics) -X-ray photoelectron spectroscopy measurement results before and after ultrasonic treatment- In the toner according to this embodiment, it is preferable that the ratio of the amount of Si detected to the amount of Al detected in X-ray photoelectron spectroscopy (XPS) before ultrasonic treatment is 3.0 or more and 10.5 or less, and that the ratio of the amount of Si detected to the amount of Al detected in X-ray photoelectron spectroscopy (XPS) after ultrasonic treatment is 2.5 or more and 8.5 or less.

[0116] The toner according to the present embodiment, by being configured as described above, can further suppress unevenness in image density when forming an image with a high image density after forming an image with a low image density successively under a high temperature and high humidity environment. The reason for this is presumed to be as follows.

[0117] By controlling the ratio of the detected amount of Si to the detected amount of Al in X-ray photoelectron spectroscopy (XPS) before ultrasonic treatment to 3.0 to 10.5, the toner tends to contain a large amount of silica particles on the outermost surface, i.e., the toner tends to form a layer made of silica particles on the outermost surface. In addition, by setting the ratio of the detected amount of Si to the detected amount of Al in X-ray photoelectron spectroscopy (XPS) after ultrasonic treatment to 2.5 to 8.5, a large amount of alumina particles are likely to be contained inside the layer of silica particles removed by ultrasonic treatment and on the surface of the toner particles. In other words, a layer of alumina particles is likely to be formed inside the layer of silica particles and on the surface of the toner particles. With this configuration, the alumina particles are unlikely to be detached from the surface of the toner particles even if ultrasonic treatment or the like is performed on the toner. In other words, even if an impact or the like is applied to the toner, the alumina particles are likely to be stably adsorbed to the surface of the toner particles. From the above, the above-mentioned composition makes it easy to form and maintain a two-layer structure of an external additive, which is a layer made of the alumina particles and a layer made of the silica particles thereon. In other words, the outermost surface has a structure containing a large amount of the silica particles. Since the silica particles have a relatively high electrical resistance, the toner is less likely to be excessively charged even when low-density images are continuously formed under a high-temperature and high-humidity environment.

[0118] Therefore, it is presumed that the toner according to this embodiment, by having the above-described configuration, will further suppress uneven image density when a high image density image is formed after successively forming low image density images in a high temperature and high humidity environment.

[0119] Here, from the viewpoint of facilitating the formation of a two-layer structure of the external additive, it is more preferable that the ratio of the amount of Si detected to the amount of Al detected in X-ray photoelectron spectroscopy (XPS) before ultrasonic treatment is 3.2 or more and 5.0 or less.

[0120] From the viewpoint of facilitating the formation of a two-layer structure of the external additive, it is more preferable that the ratio of the amount of Si detected to the amount of Al detected in X-ray photoelectron spectroscopy (XPS) after ultrasonic treatment is 2.6 or more and 3.0 or less.

[0121] The procedure for X-ray photoelectron spectroscopy measurements before and after ultrasonic treatment is as follows. The test method is as follows: first, ultrasonic treatment is performed on the toner according to the following procedure. 0.1 L of a 0.2 mass% aqueous surfactant solution, Contaminon N (Fujifilm Wako Pure Chemical Industries), which is an aqueous dispersion medium, is placed in an ultrasonic treatment device (Ultrasonic Generator model US-300TCVP (manufactured by Nippon Seiki Co., Ltd.)), 5 g of toner particles are added thereto, and ultrasonic vibrations with an output of 20 W and a frequency of 20 kHz are applied for 1 minute. Then, the floating external additives are removed and collected, and the toner particles are taken out and sieved through a mesh to separate the liberated external additives from the toner particles. The toner particles after sieving are called the toner after ultrasonic treatment. Thereafter, the toner before and after the ultrasonic treatment are subjected to X-ray photoelectron spectroscopy analysis to calculate the detected amount of Si and the detected amount of Al in each toner. The detected amount of Si is calculated by calculating the atomic weight of Si relative to the total atomic weight in the measurement area. The detected amount of Al is calculated by calculating the atomic weight of Al relative to the total atomic weight in the measurement area. The XPS measurement conditions are as follows. ·X-ray photoelectron spectrometer: JPS-9000MX manufactured by JEOL Ltd. ·X-ray source: MgKα ray Acceleration voltage: 10.0 kV ·Emission current: 20mA Photoelectron energy analyzer pass energy: 30V The weight of each atom in the measurement region is calculated using a relative photosensitivity factor provided by JASCO Corporation, and background correction and area are calculated according to the analysis application software provided by JEOL Ltd.

[0122] -Other toner characteristics- In the toner according to this embodiment, the maximum endothermic peak temperature during the first temperature rise measured by a differential scanning calorimeter (DSC) is preferably 58° C. or more and 75° C. or less. By setting the maximum endothermic peak temperature of the toner to 58° C. or more and 75° C. or less, the low-temperature fixability of the toner is improved.

[0123] The maximum endothermic peak temperature during the first temperature rise of the toner is measured by a differential scanning calorimeter (DSC) as follows. A PerkinElmer DSC-7 differential scanning calorimeter is used, and the melting points of indium and zinc are used to correct the temperature of the detector, and the heat of fusion of indium is used to correct the amount of heat. An aluminum pan is used for the sample, and an empty pan is set as a control, and the temperature is raised from room temperature to 150°C at a rate of 10°C / min. Then, the temperature at which the maximum endothermic peak is obtained in the obtained endothermic curve is determined.

[0124] (Toner manufacturing method) The toner according to the exemplary embodiment is obtained by producing toner particles and then externally adding an external additive to the toner particles.

[0125] The toner particles may be produced by any of a dry production method (e.g., a kneading and pulverizing method, etc.) and a wet production method (e.g., an aggregation and coalescence method, a suspension polymerization method, a dissolution suspension method, etc.). There is no particular limitation on these production methods, and any known production method may be used. Among these, it is preferable to obtain the toner particles by the aggregation and coalescence method.

[0126] Specifically, for example, when toner particles are produced by the aggregation and coalescence method, The toner particles are manufactured through a process including a step of preparing a resin particle dispersion in which resin particles to be a binder resin are dispersed (resin particle dispersion preparation process), a step of aggregating the resin particles (or other particles, if necessary) in the resin particle dispersion (in a dispersion after mixing other particle dispersions, if necessary) to form aggregated particles (aggregated particle formation process), and a step of heating the aggregated particle dispersion in which the aggregated particles are dispersed, fusing and coalescing the aggregated particles, and forming toner particles (fusion and coalescence process).

[0127] Here, in order to set the net intensity of each of the above elements in the toner particles within the above range, a source of each of the above elements is added during the production process of the toner particles.

[0128] Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described, but the colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may be used.

[0129] -Resin particle dispersion preparation process- First, a resin particle dispersion in which resin particles serving as a binder resin are dispersed, as well as a colorant particle dispersion in which colorant particles are dispersed and a release agent particle dispersion in which release agent particles are dispersed are prepared.

[0130] Here, the resin particle dispersion liquid is prepared, for example, by dispersing resin particles in a dispersion medium with the aid of a surfactant.

[0131] The dispersion medium used in the resin particle dispersion liquid is, for example, an aqueous medium. Examples of the aqueous medium include water such as distilled water and ion-exchanged water, alcohols, etc. These may be used alone or in combination of two or more kinds.

[0132] Examples of the surfactant include anionic surfactants such as sulfate salts, sulfonates, phosphates, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Among these, anionic surfactants and cationic surfactants are particularly preferred. The nonionic surfactants may be used in combination with anionic surfactants or cationic surfactants. The surfactant may be used alone or in combination of two or more kinds.

[0133] In the resin particle dispersion, examples of the method for dispersing the resin particles in the dispersion medium include general dispersion methods using, for example, a rotary shear type homogenizer, a ball mill having a media, a sand mill, a dyno mill, etc. Depending on the type of resin particles, the resin particles may be dispersed in the resin particle dispersion using, for example, a phase inversion emulsification method. The phase inversion emulsification method is a method in which the resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, a base is added to the organic continuous phase (O phase) to neutralize it, and then an aqueous medium (W phase) is added to effect conversion of the resin from W / O to O / W (so-called phase inversion), resulting in a discontinuous phase, and the resin is dispersed in particulate form in the aqueous medium.

[0134] The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably from 0.01 μm to 1 μm, more preferably from 0.08 μm to 0.8 μm, and even more preferably from 0.1 μm to 0.6 μm. The volume average particle size of the resin particles is measured by using a particle size distribution obtained by measurement using a laser diffraction particle size distribution measuring device (e.g., LA-700 manufactured by Horiba, Ltd.), subtracting the cumulative distribution from the small particle size side for the volume of the divided particle size range (channel), and measuring the particle size at which the cumulative distribution is 50% of all particles as the volume average particle size D50v. The volume average particle sizes of particles in other dispersions are also measured in the same manner.

[0135] The content of the resin particles in the resin particle dispersion is, for example, preferably from 5% by mass to 50% by mass, and more preferably from 10% by mass to 40% by mass.

[0136] In addition, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared in the same manner as the resin particle dispersion. That is, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion are the same for the colorant particles dispersed in the colorant particle dispersion and the release agent particles dispersed in the release agent particle dispersion.

[0137] -Agglomerated particle formation process- Next, the colorant particle dispersion and the release agent particle dispersion are mixed together with the resin particle dispersion. Then, in the mixed dispersion, the resin particles, the colorant particles, and the release agent particles are hetero-aggregated to form aggregated particles containing the resin particles, the colorant particles, and the release agent particles and having a diameter close to that of the target toner particles.

[0138] Specifically, for example, an aggregating agent is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic (e.g., pH 2 or more and 5 or less), a dispersion stabilizer is added as necessary, and then the mixed dispersion is heated to a temperature of the glass transition temperature of the resin particles (specifically, for example, a temperature of the glass transition temperature of the resin particles -30°C or more and the glass transition temperature -10°C or less), and the particles dispersed in the mixed dispersion are aggregated to form aggregated particles. In the aggregated particle formation process, for example, the above-mentioned aggregating agent may be added to the mixed dispersion at room temperature (e.g., 25°C) while stirring the mixed dispersion with a rotary shear homogenizer, the pH of the mixed dispersion may be adjusted to an acidic state (e.g., pH 2 or more and 5 or less), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.

[0139] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved. If necessary, an additive that forms a complex or a similar bond with the metal ions of the flocculant may be used, and a chelating agent is preferably used as this additive.

[0140] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide. The chelating agent may be a water-soluble chelating agent, such as oxycarboxylic acid (e.g., tartaric acid, citric acid, gluconic acid, etc.), iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), ethylenediaminetetraacetic acid (EDTA), etc. The amount of the chelating agent added is, for example, preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, relative to 100 parts by mass of the resin particles.

[0141] -Fusion / coalescence process- Next, the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition temperature of the resin particles (for example, a temperature 10 to 30° C. higher than the glass transition temperature of the resin particles) to fuse and coalesce the aggregated particles, thereby forming toner particles.

[0142] Through the above steps, toner particles are obtained. Note that, after obtaining an aggregated particle dispersion liquid in which aggregated particles are dispersed, the toner particles may be manufactured through a process of further mixing the aggregated particle dispersion liquid with a resin particle dispersion liquid in which resin particles are dispersed, and aggregating the aggregated particles so that the resin particles are further attached to the surfaces of the aggregated particles to form second aggregated particles, and a process of heating the second aggregated particle dispersion liquid in which the second aggregated particles are dispersed to fuse and coalesce the second aggregated particles to form toner particles having a core / shell structure.

[0143] After the fusion and coalescence process, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process, and drying process to obtain toner particles in a dried state. In the washing step, it is preferable to carry out sufficient replacement washing with ion-exchanged water from the viewpoint of electrostatic charge. In addition, the solid-liquid separation step is not particularly limited, but it is preferable to carry out suction filtration, pressure filtration, etc. from the viewpoint of productivity. In addition, in the drying step, there is no particular limit to the method, but it is preferable to carry out freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc. from the viewpoint of productivity.

[0144] The toner according to the present embodiment is produced, for example, by adding an external additive to the obtained toner particles in a dry state and mixing them. The mixing may be performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.

[0145] <Electrostatic image developer> The electrostatic image developer according to this embodiment contains at least the toner according to this embodiment. The electrostatic image developer according to the present embodiment may be a one-component developer containing only the toner according to the present embodiment, or may be a two-component developer in which the toner is mixed with a carrier.

[0146] The carrier is not particularly limited, and may be any known carrier, such as a coated carrier in which the surface of a core material made of magnetic powder is coated with a coating resin, a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin, or a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material and are coated with a coating resin.

[0147] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt, and magnetic oxides such as ferrite and magnetite.

[0148] Examples of the coating resin and matrix resin include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin containing an organosiloxane bond or a modified product thereof, fluororesin, polyester, polycarbonate, phenolic resin, and epoxy resin. The coating resin and the matrix resin may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate.

[0149] Here, in order to coat the surface of the core material with a coating resin, a method of coating with a coating layer forming solution in which the coating resin and, if necessary, various additives are dissolved in an appropriate solvent can be mentioned. The solvent is not particularly limited and may be selected taking into consideration the coating resin to be used, the suitability for application, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer, a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material, a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air, and a kneader coater method in which the core material of a carrier and the solution for forming a coating layer are mixed in a kneader coater and the solvent is removed.

[0150] In the two-component developer, the mixture ratio (mass ratio) of the toner and the carrier is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100.

[0151] <Image forming device / image forming method> An image forming apparatus / image forming method according to this embodiment will be described. The image forming apparatus according to the present embodiment includes an image carrier, a charging means for charging the surface of the image carrier, an electrostatic image forming means for forming an electrostatic image on the surface of the charged image carrier, a developing means for containing an electrostatic image developer and developing the electrostatic image formed on the surface of the image carrier as a toner image with the electrostatic image developer, a transfer means for transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing means for fixing the toner image transferred to the surface of the recording medium. The electrostatic image developer according to the present embodiment is used as the electrostatic image developer.

[0152] In the image forming apparatus according to this embodiment, an image forming method (the image forming method according to this embodiment) is carried out, which includes a charging step of charging the surface of an image carrier, an electrostatic image forming step of forming an electrostatic image on the surface of the charged image carrier, a developing step of developing the electrostatic image formed on the surface of the image carrier as a toner image using the electrostatic image developer according to this embodiment, a transfer step of transferring the toner image formed on the surface of the image carrier to the surface of a recording medium, and a fixing step of fixing the toner image transferred to the surface of the recording medium.

[0153] The image forming apparatus according to the present embodiment may be any of known image forming apparatuses, such as a direct transfer type apparatus in which a toner image formed on the surface of an image holder is directly transferred to a recording medium; an intermediate transfer type apparatus in which a toner image formed on the surface of an image holder is primarily transferred to the surface of an intermediate transfer body, and the toner image transferred to the surface of the intermediate transfer body is then secondarily transferred to the surface of a recording medium; an apparatus equipped with a cleaning means for cleaning the surface of the image holder before charging after the transfer of the toner image; and an apparatus equipped with a discharging means for irradiating the surface of the image holder with discharging light to discharge it before charging after the transfer of the toner image. In the case of an intermediate transfer type device, the transfer means has, for example, an intermediate transfer body onto whose surface a toner image is transferred, a primary transfer means which primarily transfers the toner image formed on the surface of the image carrier onto the surface of the intermediate transfer body, and a secondary transfer means which secondarily transfers the toner image transferred onto the surface of the intermediate transfer body onto the surface of a recording medium.

[0154] In the image forming apparatus according to the present embodiment, for example, a portion including the developing means may have a cartridge structure (process cartridge) that is detachably attached to the image forming apparatus. As the process cartridge, for example, a process cartridge including a developing means that contains the electrostatic image developer according to the present embodiment is preferably used.

[0155] An example of an image forming apparatus according to the present embodiment will be described below, but the present invention is not limited to this. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.

[0156] FIG. 1 is a schematic diagram showing the configuration of an image forming apparatus according to the present embodiment. The image forming apparatus shown in Fig. 1 includes first to fourth electrophotographic image forming units 10Y, 10M, 10C, and 10K (image forming means) that output images of each color of yellow (Y), magenta (M), cyan (C), and black (K) based on color-separated image data. These image forming units (hereinafter sometimes simply referred to as "units") 10Y, 10M, 10C, and 10K are arranged in parallel at predetermined distances from each other in the horizontal direction. These units 10Y, 10M, 10C, and 10K may be process cartridges that are detachable from the image forming apparatus.

[0157] Above each of the units 10Y, 10M, 10C, and 10K in the drawing, an intermediate transfer belt 20 is provided as an intermediate transfer body extending through each unit. The intermediate transfer belt 20 is provided wound around a drive roll 22 and a support roll 24 that are arranged from left to right in the drawing at a distance from each other and contact the inner surface of the intermediate transfer belt 20, and is adapted to run in a direction from the first unit 10Y to the fourth unit 10K. Note that a force is applied to the support roll 24 in a direction away from the drive roll 22 by a spring or the like (not shown), and tension is applied to the intermediate transfer belt 20 wound around them. In addition, an intermediate transfer body cleaning device 30 is provided on the image carrier side of the intermediate transfer belt 20, facing the drive roll 22. Further, the developing devices (developing means) 4Y, 4M, 4C, and 4K of the units 10Y, 10M, 10C, and 10K are supplied with toner including four colors of toner, yellow, magenta, cyan, and black, contained in toner cartridges 8Y, 8M, 8C, and 8K, respectively.

[0158] Since the first to fourth units 10Y, 10M, 10C, and 10K have the same configuration, the first unit 10Y that forms a yellow image and is disposed upstream in the direction in which the intermediate transfer belt travels will be described here as a representative example. Note that by assigning reference numerals of magenta (M), cyan (C), and black (K) instead of yellow (Y) to parts equivalent to those of the first unit 10Y, descriptions of the second to fourth units 10M, 10C, and 10K will be omitted.

[0159] The first unit 10Y has a photoconductor 1Y that acts as an image carrier. Around the photoconductor 1Y, a charging roll (an example of a charging means) 2Y that charges the surface of the photoconductor 1Y to a predetermined potential, an exposure device (an example of an electrostatic image forming means) 3 that exposes the charged surface to a laser beam 3Y based on a color-separated image signal to form an electrostatic image, a developing device (an example of a developing means) 4Y that supplies charged toner to the electrostatic image to develop it, a primary transfer roll 5Y (an example of a primary transfer means) that transfers the developed toner image onto an intermediate transfer belt 20, and a photoconductor cleaning device (an example of a cleaning means) 6Y that removes toner remaining on the surface of the photoconductor 1Y after the primary transfer are arranged in this order. The primary transfer roll 5Y is disposed inside the intermediate transfer belt 20 and is provided at a position facing the photoconductor 1Y. Furthermore, a bias power supply (not shown) that applies a primary transfer bias is connected to each of the primary transfer rolls 5Y, 5M, 5C, and 5K. Each bias power supply varies the transfer bias applied to each primary transfer roll under the control of a control unit (not shown).

[0160] Hereinafter, an operation of forming a yellow image in first unit 10Y will be described. First, prior to operation, the surface of the photoconductor 1Y is charged to a potential of −600V to −800V by the charging roll 2Y. The photoconductor 1Y has a conductivity (for example, a volume resistivity at 20° C. of 1×10 -6The photosensitive layer is formed by laminating a photosensitive layer on a substrate having a resistivity of Ωcm or less. This photosensitive layer is usually highly resistive (the resistance of ordinary resins), but when irradiated with a laser beam 3Y, the resistivity of the portion irradiated with the laser beam changes. A laser beam 3Y is output to the charged surface of the photoreceptor 1Y via an exposure device 3 in accordance with image data for yellow sent from a control unit (not shown). The laser beam 3Y is irradiated onto the photosensitive layer on the surface of the photoreceptor 1Y, and an electrostatic charge image of a yellow image pattern is formed on the surface of the photoreceptor 1Y.

[0161] An electrostatic image is an image formed on the surface of the photoconductor 1Y by electrostatic charging. The laser beam 3Y reduces the resistivity of the irradiated parts of the photosensitive layer, causing the charged charges on the surface of the photoconductor 1Y to flow, while the charges remain in the parts not irradiated by the laser beam 3Y. This is a so-called negative latent image. The electrostatic image formed on the photoconductor 1Y is rotated to a predetermined developing position as the photoconductor 1Y travels. Then, at this developing position, the electrostatic image on the photoconductor 1Y is made visible as a toner image (developed image) by the developing device 4Y.

[0162] The developing device 4Y contains an electrostatic image developer including at least yellow toner and a carrier, for example. The yellow toner is triboelectrically charged by being stirred inside the developing device 4Y, and is held on a developer roll (an example of a developer holder) with a charge of the same polarity (negative polarity) as the charge on the photoconductor 1Y. As the surface of the photoconductor 1Y passes through the developing device 4Y, the yellow toner electrostatically adheres to the discharged latent image portion on the surface of the photoconductor 1Y, and the latent image is developed with the yellow toner. The photoconductor 1Y on which the yellow toner image has been formed continues to travel at a predetermined speed, and the toner image developed on the photoconductor 1Y is transported to a predetermined primary transfer position.

[0163] When the yellow toner image on the photoconductor 1Y is transported to the primary transfer, a primary transfer bias is applied to the primary transfer roll 5Y, and an electrostatic force from the photoconductor 1Y to the primary transfer roll 5Y acts on the toner image, and the toner image on the photoconductor 1Y is transferred onto the intermediate transfer belt 20. The transfer bias applied at this time has a polarity (+) opposite to the polarity (-) of the toner, and in the first unit 10Y, for example, it is controlled to +10 μA by a control unit (not shown). On the other hand, the toner remaining on the photoconductor 1Y is removed and collected by the photoconductor cleaning device 6Y.

[0164] Further, the primary transfer bias applied to the primary transfer rolls 5M, 5C, and 5K subsequent to the second unit 10M is also controlled in accordance with the first unit. In this manner, the intermediate transfer belt 20 onto which the yellow toner image has been transferred by the first unit 10Y is conveyed successively through the second to fourth units 10M, 10C, and 10K, where the toner images of the respective colors are transferred in a superimposed manner.

[0165] The intermediate transfer belt 20 onto which the four color toner images have been transferred in multiple layers through the first to fourth units reaches a secondary transfer section that is composed of the intermediate transfer belt 20, a support roll 24 that contacts the inner surface of the intermediate transfer belt, and a secondary transfer roll (an example of a secondary transfer means) 26 arranged on the image bearing surface side of the intermediate transfer belt 20. Meanwhile, a recording paper (an example of a recording medium) P is fed at a predetermined timing into the gap between the secondary transfer roll 26 and the intermediate transfer belt 20 via a supply mechanism, and a secondary transfer bias is applied to the support roll 24. The transfer bias applied at this time has a (-) polarity that is the same as the (-) polarity of the toner, and an electrostatic force from the intermediate transfer belt 20 toward the recording paper P acts on the toner image, so that the toner image on the intermediate transfer belt 20 is transferred onto the recording paper P. The secondary transfer bias at this time is determined according to the resistance detected by a resistance detection means (not shown) that detects the resistance of the secondary transfer section, and is voltage-controlled.

[0166] Thereafter, the recording paper P is sent to a pressure contact portion (nip portion) of a pair of fixing rolls in a fixing device (one example of a fixing means) 28, where the toner image is fixed onto the recording paper P, forming a fixed image.

[0167] The recording paper P onto which the toner image is transferred can be, for example, plain paper used in electrophotographic copying machines, printers, etc. In addition to the recording paper P, other examples of the recording medium include overhead projector sheets, etc. To further improve the smoothness of the image surface after fixing, it is preferable that the surface of the recording paper P is also smooth. For example, coated paper in which the surface of ordinary paper is coated with resin or the like, art paper for printing, etc. are preferably used.

[0168] After the color image has been fixed, the recording paper P is conveyed toward the discharge section, and the series of color image forming operations is completed.

[0169] <Process cartridge / toner cartridge> The process cartridge according to this embodiment will be described. The process cartridge according to this embodiment is a process cartridge that contains the electrostatic image developer according to this embodiment, is equipped with a developing means that develops an electrostatic image formed on the surface of an image carrier using the electrostatic image developer into a toner image, and is detachably attached to an image forming apparatus.

[0170] In addition, the process cartridge according to this embodiment is not limited to the above configuration, and may be configured to include a developing device and, as necessary, at least one other means selected from an image carrier, a charging means, an electrostatic image forming means, and a transfer means.

[0171] An example of a process cartridge according to the present embodiment will be described below, but the present invention is not limited to this example. Note that only the main parts shown in the drawings will be described, and descriptions of the rest will be omitted.

[0172] FIG. 2 is a schematic diagram showing the process cartridge according to the present embodiment. The process cartridge 200 shown in FIG. 2 is configured by, for example, a housing 117 having a mounting rail 116 and an opening 118 for exposure, and integrally combining and holding a photoconductor 107 (an example of an image carrier), a charging roll 108 (an example of a charging means) provided around the photoconductor 107, a developing device 111 (an example of a developing means), and a photoconductor cleaning device 113 (an example of a cleaning means), which are assembled into a cartridge. In FIG. 2, 109 denotes an exposure device (an example of an electrostatic image forming means), 112 denotes a transfer device (an example of a transfer means), 115 denotes a fixing device (an example of a fixing means), and 300 denotes recording paper (an example of a recording medium).

[0173] Next, the toner cartridge according to this embodiment will be described. The toner cartridge according to the present embodiment is a toner cartridge that contains the toner according to the present embodiment and is detachably attached to an image forming apparatus. The toner cartridge contains replenishment toner to be supplied to a developing unit provided in the image forming apparatus.

[0174] 1 is an image forming apparatus having a configuration in which toner cartridges 8Y, 8M, 8C, and 8K can be attached and detached, and the developing devices 4Y, 4M, 4C, and 4K are connected to the toner cartridges corresponding to the respective developing devices (colors) through toner supply pipes (not shown). When the toner contained in the toner cartridge becomes low, the toner cartridge is replaced. EXAMPLES

[0175] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the embodiments of the present invention are not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" are based on mass.

[0176] <Synthesis of amorphous polyester resin (A)> Terephthalic acid: 68 parts Fumaric acid: 32 parts Ethylene glycol: 42 parts 1,5-Pentanediol: 47 parts The above materials were placed in a flask equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 220°C over 1 hour under a nitrogen gas flow, and 1 part of titanium tetraethoxide was added for a total of 100 parts of the above materials. The temperature was raised to 240°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at 240°C for 1 hour, after which the reaction product was cooled. In this way, an amorphous polyester resin (A) with a weight average molecular weight of 97,000 and a glass transition temperature of 60°C was obtained.

[0177] <Preparation of amorphous polyester resin particle dispersion (A1)> In a vessel equipped with a temperature control means and a nitrogen substitution means, 40 parts of ethyl acetate and 25 parts of 2-butanol were added to prepare a mixed solvent, and then 100 parts of amorphous polyester resin (A) were gradually added and dissolved, and 10% aqueous ammonia solution (equivalent to 3 times the amount by mole relative to the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the vessel was substituted with dry nitrogen, the temperature was kept at 40°C, and 400 parts of ion-exchanged water was dropped into the mixed liquid while stirring, to perform emulsification. After the dropwise addition, the emulsion was returned to 25°C, and a resin particle dispersion in which resin particles with a volume average particle size of 195 nm were dispersed was obtained. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and an amorphous polyester resin particle dispersion (A1) was obtained.

[0178] <Preparation of cyan colorant-containing amorphous polyester resin particle dispersion (C1)> 250 parts of amorphous polyester resin (A) and 50 parts of CI Pigment Blue 15:3 (phthalocyanine pigment, Dainichi Seika Kabushiki Kaisha, Cyanine Blue 4937) were put into a Henschel mixer and mixed for 120 seconds at a screw rotation speed of 600 rpm to obtain raw material (A). 200 parts of raw material (A) and 0.2 parts of 50% aqueous sodium hydroxide solution were put into the raw material inlet of a twin-screw extruder (TEM-58SS, Toshiba Machine Co., Ltd.), and 40 parts of anionic surfactant (TaycaPower, Tayca Co., Ltd., solid content 12%, sodium dodecylbenzenesulfonate) were put into the fourth barrel of the twin-screw extruder, and kneaded at a barrel setting temperature of 95°C and a screw rotation speed of 240 rpm. 150 parts of ion-exchanged water at a temperature of 95°C was fed from the fifth barrel of the twin-screw extruder, 150 parts by mass of ion-exchanged water at a temperature of 95°C from the seventh barrel, and 15 parts of ion-exchanged water at a temperature of 95°C from the ninth barrel, and the raw material (A) was kneaded at an average feed rate of 200 kg / h to obtain a resin particle dispersion in which resin particles with a volume average particle size of 180 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and a cyan colorant (CI Pigment Blue 15:3)-containing amorphous polyester resin particle dispersion (C1) was obtained.

[0179] <Preparation of Magenta Colorant-Containing Amorphous Polyester Resin Particle Dispersion (M1)> A magenta colorant (CI Pigment Red 269)-containing amorphous polyester resin particle dispersion (M1) was obtained in the same manner as the cyan colorant (CI Pigment Blue 15:3)-containing amorphous polyester resin particle dispersion (C1), except that the colorant was changed from CI Pigment Blue 15:3 to CI Pigment Red 269 (quinacridone pigment, manufactured by Nippon Ink Chemicals, SYMULER FAST RED 1022).

[0180] <Preparation of Yellow Colorant-Containing Amorphous Polyester Resin Particle Dispersion (Y1)> A yellow colorant (CI Pigment Yellow 74)-containing amorphous polyester resin particle dispersion (Y1) was obtained in the same manner as the cyan colorant (CI Pigment Blue 15:3)-containing amorphous polyester resin particle dispersion (C1), except that the colorant was changed from CI Pigment Blue 15:3 to CI Pigment Yellow 74 (monoazo pigment, Dainichi Seika Chemicals, Seika Fast Yellow 2054).

[0181] <Preparation of Black Colorant-Containing Amorphous Polyester Resin Particle Dispersion (K1)> A black colorant (carbon black)-containing amorphous polyester resin particle dispersion (K1) was obtained in the same manner as the cyan colorant (CI Pigment Blue 15:3)-containing amorphous polyester resin particle dispersion (C1), except that the colorant was changed from CI Pigment Blue 15:3 to carbon black (Regal 330, manufactured by Cabot Corporation).

[0182] <Preparation of amorphous polyester resin particle dispersions containing various colorants (C2 / M2 / Y2 / K2)> The following various colorant-containing amorphous polyester resin particle dispersions were obtained in the same manner as in the cyan colorant (CI Pigment Blue 15:3)-containing amorphous polyester resin particle dispersion (C1), except that the amount of anionic surfactant (TaycaPower, manufactured by Tayca Corporation, solid content 12%, sodium dodecylbenzenesulfonate) added to the fourth barrel of the twin-screw extruder was changed from 40 parts to 60 parts. Amorphous polyester resin particle dispersion (C2) containing cyan colorant (CI Pigment Blue 15:3) · Magenta colorant (CI Pigment Red 269)-containing amorphous polyester resin particle dispersion (M2) Amorphous polyester resin particle dispersion (Y2) containing yellow colorant (CI Pigment Yellow 74) A black colorant (carbon black)-containing amorphous polyester resin particle dispersion (K2) was obtained.

[0183] <Preparation of amorphous polyester resin particle dispersions containing various colorants (C3 / M3 / Y3 / K3)> The following various colorant-containing amorphous polyester resin particle dispersions were obtained in the same manner as in the cyan colorant (CI Pigment Blue 15:3)-containing amorphous polyester resin particle dispersion (C1), except that the amount of anionic surfactant (TaycaPower, manufactured by Tayca Corporation, solid content 12%, sodium dodecylbenzenesulfonate) added to the fourth barrel of the twin-screw extruder was changed from 40 parts to 20 parts. · Cyan colorant (CI Pigment Blue 15:3)-containing amorphous polyester resin particle dispersion (C3) · Magenta colorant (CI Pigment Red 269)-containing amorphous polyester resin particle dispersion (M3) Amorphous polyester resin particle dispersion (Y3) containing yellow colorant (CI Pigment Yellow 74) · Amorphous polyester resin particle dispersion containing black colorant (carbon black) (K3)

[0184] <Preparation of amorphous polyester resin particle dispersions containing various colorants (C4 / M4 / Y4 / K4)> The following various colorant-containing amorphous polyester resin particle dispersions were obtained in the same manner as in the cyan colorant (CI Pigment Blue 15:3)-containing amorphous polyester resin particle dispersion (C1), except that the amount of anionic surfactant (TaycaPower, manufactured by Tayca Corporation, solid content 12%, sodium dodecylbenzenesulfonate) added to the fourth barrel of the twin-screw extruder was changed from 40 parts to 5 parts. · Amorphous polyester resin particle dispersion (C4) containing cyan colorant (CI Pigment Blue 15:3) · Magenta colorant (CI Pigment Red 269)-containing amorphous polyester resin particle dispersion (M4) Amorphous polyester resin particle dispersion (Y4) containing yellow colorant (CI Pigment Yellow 74) · Amorphous polyester resin particle dispersion containing black colorant (carbon black) (K4)

[0185] <Preparation of Crystalline Polyester Resin Particle Dispersion (B1)> 1,10-Decanedicarboxylic acid: 260 parts 1,6-Hexanediol: 167 parts Dibutyltin oxide (catalyst): 0.3 parts The above materials were placed in a heated and dried three-necked flask, the air in the three-necked flask was replaced with nitrogen gas to create an inert atmosphere, and the mixture was stirred and refluxed at 180°C for 5 hours by mechanical stirring. Next, the temperature was gradually raised to 230°C under reduced pressure and stirred for 2 hours, and when the mixture became viscous, it was air-cooled to stop the reaction. Thus, a crystalline polyester resin with a weight average molecular weight of 12500 and a melting temperature of 73°C was obtained. 90 parts of the crystalline polyester resin, 1.8 parts of anionic surfactant (TaycaPower, manufactured by Tayca Co., Ltd., solid content 12%, sodium dodecylbenzenesulfonate) and 210 parts of ion-exchanged water were mixed, heated to 120°C, and dispersed using a homogenizer (Ultra Turrax T50 manufactured by IKA Co., Ltd.), and then dispersed for 1 hour using a pressure discharge type Gaulin homogenizer to obtain a resin particle dispersion in which resin particles with a volume average particle size of 195 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, thereby obtaining a crystalline polyester resin particle dispersion (B1).

[0186] (Preparation of Crystalline Polyester Resin Particle Dispersion (B2)) Terephthalic acid: 235 parts 1,4-Butenediol: 123 parts Dibutyltin oxide (catalyst): 0.3 parts The above ingredients were placed in a heated and dried three-neck flask, and the air in the container was turned into an inert atmosphere with nitrogen gas by reducing the pressure, and the mixture was stirred and refluxed at 175°C for 4 hours by mechanical stirring. The temperature was then gradually increased to 230°C under reduced pressure and stirred for 2 hours, and when the mixture became viscous, it was air-cooled to stop the reaction. The molecular weight measurement (polystyrene equivalent) of the obtained "crystalline polyester resin (B2)" showed that the weight average molecular weight (Mw) was 12700 and the melting temperature was 69°C. 90 parts of the obtained resin was mixed with 1.5 parts of an anionic surfactant (TaycaPower, manufactured by Tayca Corporation, solids content 12%, sodium dodecylbenzenesulfonate) and 200 parts of ion-exchanged water, heated to 120°C, thoroughly dispersed using an IKA Ultra-Turrax T50, and then dispersed for 1 hour using a pressure-discharge type Gaulin homogenizer to obtain a crystalline polyester resin particle dispersion (B2) having a volume average particle size of 195 nm and a solids content of 20 parts by mass.

[0187] <Preparation of styrene acrylic resin particle dispersion (S1)> Styrene: 375 parts n-Butyl acrylate: 25 parts Acrylic acid: 2 parts Dodecanethiol: 24 parts Carbon tetrabromide: 4 parts The mixture obtained by mixing and dissolving the above materials was dispersed and emulsified in a flask in a surfactant solution in which 6 parts of a nonionic surfactant (manufactured by Sanyo Chemical Industries, Nonipol 400) and 10 parts of an anionic surfactant (manufactured by TaycaPower, Tayca Co., Ltd., solid content 12%, sodium dodecylbenzenesulfonate) were dissolved in 550 parts of ion-exchanged water. Next, an aqueous solution in which 4 parts of ammonium persulfate were dissolved in 50 parts of ion-exchanged water was added over a period of 20 minutes while stirring the flask. Next, after nitrogen replacement, the flask was heated in an oil bath while stirring the contents until the temperature reached 70°C, and the temperature was maintained at 70°C for 5 hours to continue emulsion polymerization. Thus, a resin particle dispersion in which resin particles having a volume average particle size of 150 nm were dispersed was obtained. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and a styrene acrylic resin particle dispersion (S1) was obtained.

[0188] <Preparation of release agent particle dispersion (W1)> Ester wax (Nippon Oil & Fats Co., Ltd., WEP-8, melting temperature 79°C): 100 parts Anionic surfactant: 1 part (TaycaPower, manufactured by Tayca Corporation, sodium dodecylbenzenesulfonate) Ion-exchanged water: 350 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a pressure discharge Gaulin homogenizer to obtain a release agent particle dispersion in which release agent particles with a volume average particle size of 220 nm were dispersed. Ion-exchanged water was added to this release agent particle dispersion to adjust the solid content to 20%, and this was used as release agent particle dispersion (W1).

[0189] [Preparation of toner particles] <Preparation of toner particles of each color (C1 / M1 / Y1 / K1)> Ion-exchanged water: 200 parts Cyan colorant-containing amorphous polyester resin particle dispersion (C1): 145 parts Styrene acrylic resin particle dispersion (S1): 30 parts Release agent particle dispersion (W1): 10 parts The above materials were placed in a round stainless steel flask, and 0.1N (0.1mol / L) nitric acid was added to adjust the pH to 3.5, after which an aqueous magnesium chloride solution in which 6 parts of magnesium chloride were dissolved in 30 parts of ion-exchanged water was added. The materials were dispersed at 30°C using a homogenizer (IKA Ultra Turrax T50), and then heated to 45°C in a heating oil bath and maintained until the volume average particle size reached 4.5μm.

[0190] Next, 30 parts of the amorphous polyester resin particle dispersion (A1) and 15 parts of the crystalline polyester resin particle dispersion (B1) were added and held for 30 minutes. These two dispersions were added at 30 minute intervals a total of four times. Next, 40 parts of the amorphous polyester resin particle dispersion (A1) was added, and the pH was adjusted to 9.0 with a 1N aqueous sodium hydroxide solution. Next, while continuing stirring, the temperature was increased to 85°C at a rate of 0.05°C / min, and after being held at 85°C for 3 hours, it was cooled to 30°C at a rate of 15°C / min (first cooling). Next, it was heated to 85°C at a rate of 0.2°C / min (reheating), held for 30 minutes, and then cooled to 30°C at a rate of 0.5°C / min (second cooling). Next, the solid content was filtered off, washed with ion-exchanged water, and dried to obtain cyan toner particles (C1) having a volume average particle size of 5.8 μm.

[0191] In the preparation of cyan toner particles (C1), the cyan colorant-containing amorphous polyester resin particle dispersion (C1) was changed to a magenta colorant-containing amorphous polyester resin particle dispersion (M1), a yellow colorant-containing amorphous polyester resin particle dispersion (Y1), or a black colorant-containing amorphous polyester resin particle dispersion (K1), and the rest of the process was repeated to obtain magenta toner particles (M1), yellow toner particles (Y1), and black toner particles (K1).

[0192] <Preparation of toner particles of each color (C2 / M2 / Y2 / K2)> Each color toner particle (C2 / M2 / Y2 / K2) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. -Cyan colorant-containing amorphous polyester resin particle dispersion (C1) has been changed to various colorant-containing amorphous polyester resin particle dispersions (C2 / M2 / Y2 / K2). The amount of magnesium chloride added in the production of toner particles has been changed from 6 parts to 4 parts.

[0193] <Preparation of toner particles of each color (C3 / M3 / Y3 / K3)> Each color toner particle (C3 / M3 / Y3 / K3) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. The amount of magnesium chloride added in the production of toner particles has been changed from 6 parts to 20 parts.

[0194] <Preparation of toner particles of each color (C4 / M4 / Y4 / K4)> Each color toner particle (C4 / M4 / Y4 / K4) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. -Cyan colorant-containing amorphous polyester resin particle dispersion (C1) has been changed to various colorant-containing amorphous polyester resin particle dispersions (C3 / M3 / Y3 / K3). The amount of nonionic surfactant (TaycaPower, Tayca Corporation, solid content 12%, sodium dodecylbenzenesulfonate) was changed to 0.5 parts.

[0195] <Preparation of toner particles of each color (C5 / M5 / Y5 / K5)> Each color toner particle (C5 / M5 / Y5 / K5) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. -Cyan colorant-containing amorphous polyester resin particle dispersion (C1) has been changed to various colorant-containing amorphous polyester resin particle dispersions (C4 / M4 / Y4 / K4). The amount of nonionic surfactant (TaycaPower, Tayca Corporation, 12% solids, sodium dodecylbenzenesulfonate) was changed to 3 parts.

[0196] <Preparation of toner particles of each color (C6 / M6 / Y6 / K6)> Each color toner particle (C6 / M6 / Y6 / K6) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. -Cyan colorant-containing amorphous polyester resin particle dispersion (C1) has been changed to various colorant-containing amorphous polyester resin particle dispersions (C2 / M2 / Y2 / K2). The amount of magnesium chloride added in the production of toner particles has been changed from 6 parts to 2 parts.

[0197] <Preparation of toner particles of each color (C7 / M7 / Y7 / K7)> Each color toner particle (C7 / M7 / Y7 / K7) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. -Cyan colorant-containing amorphous polyester resin particle dispersion (C1) has been changed to various colorant-containing amorphous polyester resin particle dispersions (C2 / M2 / Y2 / K2). The amount of magnesium chloride added in the production of toner particles has been changed from 6 parts to 30 parts.

[0198] <Preparation of toner particles of each color (C8 / M8 / Y8 / K8)> Toner particles of each color (C8 / M8 / Y8 / K8) were obtained in the same manner as the toner particles of each color (C1 / M1 / Y1 / K1), except that the crystalline polyester resin particle dispersion liquid (B1) was not added in the preparation of the toner particles of each color (C1 / M1 / Y1 / K1).

[0199] <Preparation of toner particles of each color (C9 / M9 / Y9 / K9)> In producing each color toner particle (C1 / M1 / Y1 / K1), each color toner particle (C9 / M9 / Y9 / K9) was obtained in the same manner as in producing each color toner particle (C1 / M1 / Y1 / K1), except that the crystalline polyester resin particle dispersion liquid (B1) was changed to the crystalline polyester resin particle dispersion liquid (B2).

[0200] <Preparation of toner particles of each color (C10 / M10 / Y10 / K10)> Each color toner particle (C10 / M10 / Y10 / K10) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. The amount of nonionic surfactant (TaycaPower, Tayca Corporation, solid content 12%, sodium dodecylbenzenesulfonate) was changed to 6 parts.

[0201] <Preparation of toner particles of each color (C11 / M11 / Y11 / K11)> Each color toner particle (C11 / M11 / Y11 / K11) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. The amount of nonionic surfactant (TaycaPower, Tayca Corporation, 12% solids, sodium dodecylbenzenesulfonate) was changed to 7 parts.

[0202] <Preparation of toner particles of each color (C12 / M12 / Y12 / K12)> Each color toner particle (C12 / M12 / Y12 / K12) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. The amount of nonionic surfactant (TaycaPower, Tayca Corporation, solid content 12%, sodium dodecylbenzenesulfonate) was changed to 0.2 parts.

[0203] <Preparation of toner particles of each color (C13 / M13 / Y13 / K13)> Each color toner particle (C13 / M13 / Y13 / K13) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. -Cyan colorant-containing amorphous polyester resin particle dispersion (C1) has been changed to various colorant-containing amorphous polyester resin particle dispersions (C2 / M2 / Y2 / K2). The amount of magnesium chloride added in the production of toner particles has been changed from 6 parts to 23 parts.

[0204] <Preparation of toner particles of each color (C14 / M14 / Y14 / K14)> Each color toner particle (C14 / M14 / Y14 / K14) was obtained in the same manner as in the preparation of the cyan toner particle (C1), except for the following changes. -Cyan colorant-containing amorphous polyester resin particle dispersion (C1) has been changed to various colorant-containing amorphous polyester resin particle dispersions (C2 / M2 / Y2 / K2). The amount of magnesium chloride added in the production of toner particles has been changed from 6 parts to 2.5 parts.

[0205] [Preparation of silica particles] Commercially available silica particles were used as an external additive. Silica particles (1): Nippon Aerosil Co., Ltd., RY50, volume average particle size 40 nm Silica particles (2): Tokuyama Corporation, PM20, volume average particle size 12 nm Silica particles (3): TGC243, manufactured by Kabat, volume average particle size 85 nm Silica particles (4): H30TD, manufactured by Wacker-Chemie, volume average particle size 7 nm Silica particles (5): UFP-80HH, manufactured by Denka Co., Ltd., volume average particle size 100 nm

[0206] [Preparation of alumina particles] (Alumina particles (1)) Aluminum trichloride (AlCl3) was evaporated in an evaporator at 200°C. The chloride vapor was passed into the mixing chamber of the burner by argon gas at a feed rate of 200 kg / h. Here, the argon gas containing the chloride vapor was mixed with 100 Nm of hydrogen. 3 / h and air 450Nm 3 / h and fed to the flame through a central tube (diameter 7 mm). The burner temperature was 230°C and the tube discharge velocity was approximately 30 m / s. Hydrogen 0.05 Nm 3 / h was fed as a jacket-type gas through an outer tube. The gas was burned in the reaction chamber and cooled to about 110 °C in the downstream agglomeration zone, which caused agglomeration of primary particles of alumina. The resulting aluminium oxide particles were separated in a filter or cyclone from the simultaneously produced hydrochloric acid-containing gas, and the powder with moist air was treated at about 600 °C to remove the adhesive chlorides and obtain alumina powder. The obtained alumina powder was placed in a reaction vessel, and while the powder was stirred with a rotary blade under a nitrogen atmosphere, 20 g of decylsilane diluted with 60 g of hexane was added to 100 g of the alumina powder. After heating and stirring at 200°C for 120 minutes, the mixture was cooled with cooling water and dried under reduced pressure to obtain alumina particles (1) having a volume average particle size of 8 nm.

[0207] (Alumina particles (2)) Alumina particles (2) having a volume average particle size of 20 nm were obtained in the same manner as in the production of alumina particles (1), except that in the production of alumina particles (1), aluminum trichloride vapor was passed at 100 kg / h and argon gas was passed into the mixing chamber of the burner at a supply rate of 100 kg / h.

[0208] (Alumina particles (3)) Alumina particles (3) having a volume average particle size of 80 nm were obtained in the same manner as in the production of alumina particles (1), except that in the production of alumina particles (1), aluminum trichloride vapor was passed at a rate of 50 kg / h and argon gas was passed into the mixing chamber of the burner at a supply rate of 75 kg / h.

[0209] (Alumina particles (4)) Alumina particles (4) having a volume average particle size of 5 nm were obtained in the same manner as in the production of alumina particles (1), except that in the production of alumina particles (1), aluminum trichloride vapor was passed at 300 kg / h and argon gas was passed into the mixing chamber of the burner at a supply rate of 300 kg / h.

[0210] (Alumina particles (5)) Alumina particles (5) having a volume average particle size of 100 nm were obtained in the same manner as in the production of alumina particles (1), except that in the production of alumina particles (1), aluminum trichloride vapor was passed at a rate of 50 kg / h and argon gas was passed into the mixing chamber of the burner at a supply rate of 20 kg / h.

[0211] [Creating the carrier] After 500 parts of spherical magnetite powder particles (volume average particle diameter 0.55 μm) were stirred with a Henschel mixer, 5 parts of a titanate-based coupling agent were added, and the mixture was heated to 100 ° C and stirred for 30 minutes. Next, 6.25 parts of phenol, 9.25 parts of 35% formalin, 500 parts of magnetite particles treated with a titanate-based coupling agent, 6.25 parts of 25% ammonia water, and 425 parts of water were added to a four-neck flask and stirred, and reacted at 85 ° C for 120 minutes while stirring. Next, the mixture was cooled to 25 ° C, 500 parts of water were added, and the supernatant liquid was removed and the precipitate was washed with water. The washed precipitate was heated and dried under reduced pressure to obtain a carrier (CA) with an average particle size of 35 μm.

[0212] <Example 1> [External addition of additives] 100 parts of cyan toner particles (C1) and 0.5 parts of alumina particles (1) were mixed and mixed for 30 seconds at a rotation speed of 10,000 rpm using a sample mill, and after a 30-second pause, 1.7 parts of silica particles (1) were added and mixed for 30 seconds at a rotation speed of 10,000 rpm. The mixture was sieved using a vibrating sieve with a mesh size of 45 μm to obtain toner (C1). The volume average particle diameter of toner (C1) was 5.8 μm.

[0213] [Mixing toner and carrier] Cyan toner (C1) and carrier (CA) were placed in a V blender in a ratio of toner (C1):carrier (CA)=5:95 (mass ratio) and stirred for 20 minutes to obtain a cyan developer (C1).

[0214] [Preparation of various developers] A magenta developer (M1) was obtained in the same manner as for the cyan developer (C1), except that magenta toner particles (M1) were used instead of the cyan toner particles (C1). A yellow developer (Y1) was obtained in the same manner as for the cyan developer (C1), except that the yellow toner particles (Y1) were used instead of the cyan toner particles (C1). A black developer (K1) was obtained in the same manner as for the cyan developer (C1), except that the black toner particles (K1) were used instead of the cyan toner particles (C1). The resulting set of developers of each color was used as the developer set of Example 1.

[0215] <Examples 2 to 16 and Comparative Examples 1 to 8> A developer set of each example was obtained in the same manner as in Example 1, except that the type of toner particles used and the type and amount of external additives added were changed as shown in Table 1.

[0216] [Measurement of the volume average particle size of toner particles] Of the developer sets of each example, the volume average particle size of the toner particles in the cyan developer was measured according to the method described above. The results are shown in Table 1. The "volume average particle size" of the toner particles in the developers of the other colors was almost the same as the "volume average particle size" of the toner particles in the cyan developer.

[0217] [Measurement of net intensity of each element] Of the developer sets of each example, the net intensity of the following elements was measured for the toner particles in the cyan developer according to the method described above. The results are shown in Table 2. Note that the "net intensity of each element" of the toner particles in the developers of the other colors was almost the same as the "net intensity of each element" of the toner particles in the cyan developer. Net strength of S element N S (In the table, “S(N S )" ·Net strength N of alkali metal elements and alkaline earth metal elements A (In the table, "ALKALI(N A ) 」 (denoted as) Net strength of Na element N N (In the table, “Na(N N )" Net strength of Mg element N M (In the table, “Mg(N M )" Net strength of Ca element N C (In the table, “Ca(N C )" ·Net strength N of alkali metal elements and alkaline earth metal elements other than Na, Mg, and Ca A-NMC ((In the table, “ALKALI-(Na+Mg+Ca)(N A-NMC )"

[0218] <Image Density Unevenness Evaluation> The developer set of each example was housed in a developing device of a modified DocuCentreColor400 (manufactured by Fuji Xerox Co., Ltd.). Using this modified machine, 10,000 sheets of four-color band chart images with an image density of 20% were output per day on A4 size J paper (manufactured by Fuji Xerox Co., Ltd.) in an environment of 28.5°C and 85% RH. After outputting a total of 20,000 sheets, the transfer belt member was removed, and the deteriorated transfer belt member was set in the modified DocuCenterColor400 (manufactured by Fuji Xerox Co., Ltd.) in place of the removed transfer belt member. The environment was changed to 10°C and 10% RH, and the product was left standing for 24 hours or more. Thereafter, a 1×290 mm band chart, 20×20 mm secondary color (red, green, blue) patch images, and 20×20 mm tertiary color (process black) patch images were printed on 7,000 sheets of A4 size 45 paper (manufactured by Ricoh Co., Ltd., basis weight 52 gsm) in one day. The images on the printed paper were visually checked every 1,000 sheets and evaluated according to the following evaluation criteria. A to C were considered to be within the acceptable range. -Evaluation criteria- A: There is no problem with the image quality. B: Slight unevenness in image density is observed around the tertiary color patches, but there is no problem with image quality. C: In addition to the tertiary color, slight unevenness in image density is observed around the secondary color patches, but there is no problem with the image quality. D: Image density unevenness is observed in the tertiary color. E: In addition to the tertiary color, image density unevenness is observed around the secondary color patches.

[0219] The "particle size ratio (Si / Al)" in the tables indicates the ratio of the volume average particle size of silica particles to the volume average particle size of alumina particles.

[0220] [Table 1-1]

[0221] [Table 1-2]

[0222] [Table 2-1]

[0223] [Table 2-2]

[0224] From the above results, it is understood that the toner of this embodiment can suppress unevenness in image density when a high density image is formed after successively forming low density images under a high temperature and high humidity environment. [Explanation of symbols]

[0225] 1Y, 1M, 1C, 1K Photoconductor (an example of an image carrier) 2Y, 2M, 2C, 2K Charging roll (an example of a charging means) 3 Exposure device (an example of an electrostatic image forming means) 3Y, 3M, 3C, 3K laser beam 4Y, 4M, 4C, 4K developing device (an example of developing means) 5Y, 5M, 5C, 5K Primary transfer roll (an example of a primary transfer means) 6Y, 6M, 6C, 6K Photoconductor cleaning device (an example of a cleaning means) 8Y, 8M, 8C, 8K toner cartridges 10Y, 10M, 10C, 10K Image forming units 20 Intermediate transfer belt (an example of an intermediate transfer body) 22 Driving Roll 24 Support roll 26 Secondary transfer roll (an example of a secondary transfer means) 28 Fixing device (an example of a fixing means) 30 Intermediate transfer body cleaning device P Recording paper (an example of a recording medium) 107 Photoconductor (an example of an image carrier) 108 Charging roll (an example of charging means) 109 Exposure device (an example of electrostatic image forming means) 111 Developing device (an example of developing means) 112 Transfer device (an example of a transfer means) 113 Photoconductor cleaning device (an example of a cleaning means) 115 Fixing device (an example of fixing means) 116 Mounting Rail 117 Cabinet 118 Exposure Aperture 200 Process Cartridge 300 Recording paper (an example of a recording medium)

Claims

1. Toner particles containing a binder resin; and an external additive containing alumina particles having a volume average particle size of more than 5 nm and not more than 80 nm and silica particles having a volume average particle size of 10 nm or more and not more than 90 nm, The net strength N of the total of alkali metal elements and alkaline earth metal elements in the toner particles measured by fluorescent X-ray analysis A is 0.10 kcps or more and 1.30 kcps or less, The toner for developing electrostatic images, wherein a ratio (Ws / Wa) of a content Ws of the silica particles to a content Wa of the alumina particles is more than 0.5 and less than 35.

2. The net strength N A 2. The toner for developing electrostatic images according to claim 1, wherein the viscosity is from 0.20 kcps to 1.00 kcps.

3. 3. The toner for developing electrostatic images according to claim 1, wherein the alkali metal element and the alkaline earth metal element include at least one element selected from the group consisting of Na, Mg, and Ca.

4. 3. The toner for developing electrostatic images according to claim 1, wherein the alkali metal element and the alkaline earth metal element include at least one selected from the group consisting of Na and Mg.

5. The net intensity N of the S element in the toner particles measured by fluorescent X-ray analysis S 5. The toner for developing electrostatic images according to claim 1, wherein the viscosity is 3.0 kcps or more and 6.0 kcps or less.

6. The net strength N A The net strength N S The ratio (N S / N A 6. The toner for developing electrostatic images according to claim 5, wherein the molecular weight ratio (Mw) is more than 3 and less than 40.

7. 7. The toner for developing electrostatic images according to claim 1, wherein the binder resin comprises an amorphous polyester resin and a crystalline polyester resin.

8. 8. The toner for developing electrostatic images according to claim 7, wherein the crystalline polyester resin is a polymer of an α,ω-straight-chain aliphatic dicarboxylic acid and an α,ω-straight-chain aliphatic diol.

9. 9. The toner for developing electrostatic images according to claim 1, wherein a ratio of a volume average particle size of the silica particles to a volume average particle size of the alumina particles is 0.2 or more and 2.0 or less.

10. In X-ray photoelectron spectroscopy (XPS) before ultrasonic treatment, the ratio of the amount of Si detected to the amount of Al detected is 3.0 to 10.5, The toner for developing electrostatic images according to any one of claims 1 to 9, wherein the ratio of detected amount of Si to detected amount of Al in X-ray photoelectron spectroscopy (XPS) after ultrasonic treatment is 2.5 or more and 8.5 or less.

11. 11. An electrostatic image developer comprising the toner for developing electrostatic images according to claim 1.

12. A toner cartridge which contains the toner for developing electrostatic images according to any one of claims 1 to 10 and is detachably mountable to an image forming apparatus.

13. 12. A process cartridge detachably mountable to an image forming apparatus, comprising: a developing unit that contains the electrostatic image developer according to claim 11 and develops an electrostatic image formed on a surface of an image carrier by the electrostatic image developer into a toner image.

14. An image carrier; a charging means for charging the surface of the image carrier; an electrostatic image forming means for forming an electrostatic image on the charged surface of the image carrier; a developing unit that contains the electrostatic image developer according to claim 11 and develops the electrostatic image formed on the surface of the image carrier into a toner image by the electrostatic image developer; a transfer means for transferring the toner image formed on the surface of the image carrier to a surface of a recording medium; a fixing means for fixing the toner image transferred onto the surface of the recording medium; An image forming apparatus comprising:

Citation Information

Patent Citations

  • Toner

    JP2005062807A

  • Toner and developer for developing electrostatic latent image, toner cartridge, process cartridge and image forming apparatus

    JP2011209313A

  • Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

    JP2016070991A

  • Toner for two-component developer and image forming method using the same

    JP2017167440A

  • Toner for developing electrical static charge image and two-component developer for developing electrical static charge image