Glass substrates for EUVL and mask blanks for EUVL

By employing a double-sided polisher with reversed rotation and targeted height corrections, the EUVL glass substrate achieves a flatness of less than 10.0 nm, addressing the symmetry issues in conventional polishing methods and improving circuit pattern transfer precision.

JP7574766B2Active Publication Date: 2024-10-29AGC INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021138312
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-30
Filing Date
2021-08-26
Publication Date
2024-10-29
Estimated Expiration
2041-08-26

AI Technical Summary

Technical Problem

Conventional EUVL glass substrates face challenges in achieving flatness of less than 10.0 nm in the central region due to incomplete axial symmetry during final polishing, particularly with 4-fold symmetrical components that cannot be accurately represented by Zernike polynomials.

Method used

The EUVL glass substrate is processed using a double-sided polisher to achieve final polishing with reversed rotation directions of the surface plates, combined with targeted height corrections based on Zernike polynomial expressions, ensuring a maximum height difference of 6.0 nm or less in the central region.

Benefits of technology

This approach effectively suppresses the flatness of the central region to less than 10.0 nm, enhancing the precision of circuit pattern transfer in EUVL mask blanks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574766000012
    Figure 0007574766000012
  • Figure 0007574766000013
    Figure 0007574766000013
  • Figure 0007574766000014
    Figure 0007574766000014
Patent Text Reader

Abstract

To provide a technology that suppresses the flatness of the center region of the main surface of EUVL glass substrate to less than 10.0 nm.SOLUTION: An EUVL glass substrate has a rectangular first main surface in which a conductive film is to be formed, and a rectangular second main surface facing oppositely from the first main surface in which an EUV reflection film and an EUV absorption film are to be formed in this order. When representing the coordinate of the points in the center region of a 142 mm long and 142 mm wide square of the first main surface excluding the rectangular frame-shaped peripheral edge region by (x, y, z (x, y)), the maximum elevation difference in a surface that is a collection of coordinates (x, y, z3 (x, y)) calculated using equations (1) to (3) in the specification is 6.0 nm or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a glass substrate for EUVL (Extreme Ultra-Violet Lithography) and a mask blank for EUVL. [Background technology]

[0002] Conventionally, photolithography technology has been used in the manufacture of semiconductor devices. In photolithography technology, an exposure apparatus irradiates a circuit pattern on a photomask with light, and the circuit pattern is reduced and transferred onto a resist film.

[0003] Recently, in order to enable the transfer of fine circuit patterns, the use of short-wavelength exposure light, for example, ArF excimer laser light, and further EUV (Extreme Ultra-Violet) light, has been considered.

[0004] Here, EUV (extreme ultraviolet) includes soft X-rays and vacuum ultraviolet, and specifically refers to light with a wavelength of about 0.2 nm to 100 nm. At present, EUV with a wavelength of about 13.5 nm is mainly being considered.

[0005] An EUVL photomask is obtained by forming a circuit pattern on an EUVL mask blank.

[0006] The mask blank for EUVL includes a glass substrate, a conductive film formed on a first main surface of the glass substrate, and an EUV reflective film and an EUV absorbing film formed on a second main surface of the glass substrate. The EUV reflective film and the EUV absorbing film are formed in this order.

[0007] The EUV reflective film reflects EUV. The EUV absorbing film absorbs EUV. An opening pattern, which is a circuit pattern, is formed in the EUV absorbing film. The conductive film is attracted to the electrostatic chuck of the exposure tool.

[0008] Mask blanks for EUVL require high flatness to improve the transfer accuracy of circuit patterns. The flatness is mainly determined by the flatness of the glass substrate for EUVL. Therefore, the glass substrate for EUVL also requires high flatness.

[0009] The EUVL mask blank described in Patent Document 1 has a central region and an outer peripheral region on the main surface of the conductive film opposite to the glass substrate. The central region is a square region 142 mm long and 142 mm wide, excluding the rectangular frame-shaped outer peripheral region surrounding the central region. In the central region, the flatness of the component having an order of Legendre polynomial of 3 or more and 25 or less is 20 nm or less.

[0010] Moreover, in the mask blank for EUVL described in Patent Document 2, the difference between the maximum height and the minimum height within a calculation region of the difference data between the composite surface shape and the virtual surface shape is 25 nm or less. The calculation region is an area inside a circle with a diameter of 104 mm. The composite surface shape is obtained by combining the surface shape of the multilayer reflective film and the surface shape of the conductive film. The virtual surface shape is defined by Zernike polynomials expressed in a polar coordinate system. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent No. 6229807 [Patent Document 2] Patent No. 6033987 Summary of the Invention [Problem to be solved by the invention]

[0012] As described above, a high degree of flatness is required for the EUVL glass substrate. Therefore, the central region of the main surface of the EUVL glass substrate is generally subjected to polishing, local processing, and finish polishing in this order. The local processing method is, for example, the GCIB (Gas Cluster Ion Beam) method or the PCVM (Plasma Chemical Vaporization Machining) method.

[0013] In the finish polishing, the EUVL glass substrate is pressed against the platen while rotating the EUVL glass substrate and the platen. The central region of the main surface of the EUVL glass substrate is finish polished approximately axially symmetrically about the center, but is not completely axially symmetrical, and contains axially symmetric components and the remaining distortion components after the finish polishing.

[0014] The distortion components include a four-fold symmetric component rotated around the center of the central region. This four-fold symmetric component is caused by the finish polishing. This four-fold symmetric component is preferably expressed by Zernike polynomials rather than Legendre polynomials. Unlike Legendre polynomials, Zernike polynomials are expressed in polar coordinates and are suitable for removing axially symmetric components.

[0015] However, unlike the Legendre polynomials, the Zernike polynomials can only express circular regions. The main surface of the EUVL glass substrate is rectangular, and its central region is also rectangular, so the four corners of the rectangle cannot be expressed by the Zernike polynomials. Therefore, in the past, it was not possible to accurately grasp the distortion components that occur during finish polishing.

[0016] As a result, it has conventionally been difficult to suppress the flatness of the central region of the main surface of a glass substrate for EUVL to less than 10.0 nm.

[0017] One aspect of the present disclosure provides a technique for suppressing the flatness of a central region of a main surface of a glass substrate for EUVL to less than 10.0 nm. [Means for solving the problem]

[0018] A glass substrate for EUVL according to one embodiment of the present disclosure has a rectangular first main surface on which a conductive film is formed, and a rectangular second main surface facing the opposite direction to the first main surface on which an EUV reflective film and an EUV absorbing film are formed in this order. When the coordinates of a point in a central region of a square 142 mm long and 142 mm wide excluding a peripheral region of the rectangular frame of the first main surface are expressed as (x, y, z(x, y)), the maximum height difference of a surface, which is a set of coordinates (x, y, z3(x, y)) calculated using the following formulas (1) to (3), is 6.0 nm or less.

[0019]

number

[0020] According to one embodiment of the present disclosure, the flatness of the central region of the main surface of the EUVL glass substrate can be suppressed to less than 10.0 nm. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a flowchart showing a method for manufacturing an EUVL mask blank according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a glass substrate for EUVL according to one embodiment. [Diagram 3] FIG. 3 is a plan view showing a glass substrate for EUVL according to one embodiment. [Figure 4] FIG. 4 is a cross-sectional view showing an EUVL mask blank according to an embodiment. [Diagram 5] FIG. 5 is a cross-sectional view showing an example of a photomask for EUVL. [Figure 6] FIG. 6 is a perspective view showing an example of a double-sided polisher, with a part of the double-sided polisher cut away. [Figure 7]FIG. 7 is a diagram showing an example of the height distribution in the central region of the first main surface after finish polishing. [Figure 8] FIG. 8 is a plan view showing an example of an arrangement of a plurality of points set in the central region. [Figure 9] FIG. 9 is a diagram showing the height distribution of the component extracted from the height distribution of FIG. 7 using formula (1). [Figure 10] FIG. 10 is a diagram showing the height distribution of the component extracted from the height distribution of FIG. 7 using equation (2). [Figure 11] FIG. 11 is a diagram showing the height distribution of the component extracted from the height distribution of FIG. 7 using equation (3). [Figure 12] FIG. 12 is a plan view showing the relative rotation direction of the platen with respect to the central region. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding components are denoted by the same reference numerals, and the description may be omitted. In the specification, the symbol "~" indicating a range of values ​​means that the values ​​before and after the symbol are included as the lower and upper limits.

[0023] As shown in Fig. 1, the method for manufacturing an EUVL mask blank has steps S1 to S7. An EUVL mask blank 1 shown in Fig. 4 is manufactured using an EUVL glass substrate 2 shown in Fig. 2 and Fig. 3. Hereinafter, the EUVL mask blank 1 will also be simply referred to as a mask blank 1. Furthermore, the EUVL glass substrate 2 will also be simply referred to as a glass substrate 2.

[0024] As shown in Figures 2 and 3, the glass substrate 2 includes a first main surface 21 and a second main surface 22 facing opposite to the first main surface 21. The first main surface 21 is rectangular. In this specification, a rectangular shape includes a shape with chamfered corners. In addition, a rectangle includes a square. The second main surface 22 faces opposite to the first main surface 21. The second main surface 22 is also rectangular, like the first main surface 21.

[0025] The glass substrate 2 also includes four edge surfaces 23, four first chamfered surfaces 24, and four second chamfered surfaces 25. The edge surfaces 23 are perpendicular to the first main surface 21 and the second main surface 22. The first chamfered surface 24 is formed at the boundary between the first main surface 21 and the edge surfaces 23. The second chamfered surface 25 is formed at the boundary between the second main surface 22 and the edge surfaces 23. In this embodiment, the first chamfered surface 24 and the second chamfered surface 25 are so-called C-chamfered surfaces, but may be R-chamfered surfaces.

[0026] The glass of the glass substrate 2 is preferably quartz glass containing TiO2. Quartz glass has a smaller linear expansion coefficient and smaller dimensional change due to temperature change than general soda-lime glass. Quartz glass may contain 80% to 95% by mass of SiO2 and 4% to 17% by mass of TiO2. When the TiO2 content is 4% to 17% by mass, the linear expansion coefficient is approximately zero near room temperature, and there is almost no dimensional change near room temperature. Quartz glass may contain a third component or impurities other than SiO2 and TiO2.

[0027] The size of the glass substrate 2 in plan view is, for example, 152 mm in length and 152 mm in width. The length and width may be greater than or equal to 152 mm.

[0028] The glass substrate 2 has a central region 27 and a peripheral region 28 on the first main surface 21. The central region 27 is a square region 142 mm long and 142 mm wide excluding the peripheral region 28 which has a rectangular frame shape surrounding the central region 27, and is a region which is processed to a desired flatness by steps S1 to S4. The four sides of the central region 27 are parallel to the four end faces 23. The center of the central region 27 coincides with the center of the first main surface 21.

[0029] Although not shown, the second main surface 22 of the glass substrate 2 also has a central region and a peripheral region, similar to the first main surface 21. The central region of the second main surface 22, like the central region of the first main surface 21, is a square region 142 mm long and 142 mm wide, and is a region that is processed to a desired flatness by steps S1 to S4 in FIG.

[0030] First, in step S1, the first main surface 21 and the second main surface 22 of the glass substrate 2 are polished. In this embodiment, the first main surface 21 and the second main surface 22 are polished simultaneously by a double-sided polisher 9 described later, but may be polished sequentially by a single-sided polisher (not shown). In step S1, the glass substrate 2 is polished while a polishing slurry is supplied between the polishing pad and the glass substrate 2.

[0031] The polishing pad may be, for example, a urethane-based polishing pad, a nonwoven fabric-based polishing pad, or a suede-based polishing pad. The polishing slurry contains an abrasive and a dispersion medium. The abrasive is, for example, cerium oxide particles. The dispersion medium is, for example, water or an organic solvent. The first main surface 21 and the second main surface 22 may be polished multiple times with abrasives of different materials or particle sizes.

[0032] The abrasive used in step S1 is not limited to cerium oxide particles, and may be, for example, silicon oxide particles, aluminum oxide particles, zirconium oxide particles, titanium oxide particles, diamond particles, silicon carbide particles, or the like.

[0033] Next, in step S2, the surface shapes of the first main surface 21 and the second main surface 22 of the glass substrate 2 are measured. To measure the surface shapes, for example, a non-contact measuring machine such as a laser interference type is used so as not to scratch the surface. The measuring machine measures the surface shapes of the central region 27 of the first main surface 21 and the central region of the second main surface 22.

[0034] Next, in step S3, the first main surface 21 and the second main surface 22 of the glass substrate 2 are locally processed to improve the flatness with reference to the measurement result of step S2. The first main surface 21 and the second main surface 22 are locally processed in that order. The order may be any order, and is not particularly limited. The method of local processing is, for example, the GCIB method or the PCVM method. The method of local processing may also be a polishing method using a magnetic fluid, a polishing method using a rotary polishing tool, or the like.

[0035] Next, in step S4, the first main surface 21 and the second main surface 22 of the glass substrate 2 are finish-polished. In this embodiment, the first main surface 21 and the second main surface 22 are polished simultaneously by a double-sided polisher 9 described below, but they may be polished sequentially by a single-sided polisher (not shown). In step S4, the glass substrate 2 is polished while a polishing slurry is supplied between the polishing pad and the glass substrate 2. The polishing slurry contains an abrasive. The abrasive is, for example, colloidal silica particles.

[0036] Next, in step S5, a conductive film 5 shown in FIG. 4 is formed in the central region 27 of the first main surface 21 of the glass substrate 2. The conductive film 5 is used to attach the EUVL photomask to an electrostatic chuck of an exposure tool. The conductive film 5 is made of, for example, chromium nitride (CrN). The conductive film 5 is formed by, for example, sputtering.

[0037] Next, in step S6, an EUV reflective film 3 shown in FIG. 4 is formed in the central region of the second main surface 22 of the glass substrate 2. The EUV reflective film 3 reflects EUV. The EUV reflective film 3 may be, for example, a multilayer reflective film in which high refractive index layers and low refractive index layers are alternately stacked. The high refractive index layers are made of, for example, silicon (Si), and the low refractive index layers are made of, for example, molybdenum (Mo). The EUV reflective film 3 is formed by a sputtering method such as ion beam sputtering or magnetron sputtering.

[0038] Finally, in step S7, an EUV absorbing film 4 shown in FIG. 4 is formed on the EUV reflective film 3 formed in step S6. The EUV absorbing film 4 absorbs EUV. The EUV absorbing film 4 is formed of a single metal, an alloy, a nitride, an oxide, an oxynitride, or the like containing at least one element selected from tantalum (Ta), chromium (Cr), and palladium (Pd), for example. The EUV absorbing film 4 is formed by, for example, a sputtering method.

[0039] In this embodiment, steps S6 to S7 are performed after step S5, but may be performed before step S5.

[0040] The above steps S1 to S7 provide the mask blank 1 shown in Fig. 4. The mask blank 1 has a first main surface 11 and a second main surface 12 facing opposite to the first main surface 11, and has, from the first main surface 11 side to the second main surface 12 side, a conductive film 5, a glass substrate 2, an EUV reflective film 3, and an EUV absorbing film 4, in this order.

[0041] Although not shown, the mask blank 1 has a central region and a peripheral region on the first main surface 11, similar to the glass substrate 2. The central region is a square region measuring 142 mm in length and 142 mm in width, excluding a rectangular frame-shaped peripheral region surrounding the central region. The mask blank 1 also has a central region and a peripheral region on the second main surface 12, similar to the glass substrate 2. The central region is a square region measuring 142 mm in length and 142 mm in width, excluding a rectangular frame-shaped peripheral region surrounding the central region.

[0042] In addition to the conductive film 5, the glass substrate 2, the EUV reflective film 3, and the EUV absorbing film 4, the mask blank 1 may include another film.

[0043] For example, the mask blank 1 may further include a low-reflection film. The low-reflection film is formed on the EUV absorbing film 4. Then, a circuit pattern 41 is formed on both the low-reflection film and the EUV absorbing film 4. The low-reflection film is used for inspecting the circuit pattern 41, and has lower reflection characteristics with respect to inspection light than the EUV absorbing film 4. The low-reflection film is formed of, for example, TaON or TaO. For example, a sputtering method is used as a method for forming the low-reflection film.

[0044] The mask blank 1 may further include a protective film. The protective film is formed between the EUV reflective film 3 and the EUV absorbing film 4. The protective film protects the EUV reflective film 3 so that the EUV reflective film 3 is not etched when the EUV absorbing film 4 is etched to form a circuit pattern 41 in the EUV absorbing film 4. The protective film is formed of, for example, Ru, Si, TiO2, or the like. The protective film is formed by, for example, a sputtering method.

[0045] 5, the EUVL photomask is obtained by forming a circuit pattern 41 in an EUV absorbing film 4. The circuit pattern 41 is an opening pattern, and is formed by photolithography and etching. Therefore, the mask blank 1 may include a resist film used to form the circuit pattern 41.

[0046] Incidentally, the mask blank 1 is required to have a high degree of flatness in order to improve the transfer accuracy of the circuit pattern 41. The flatness is mainly determined by the flatness of the glass substrate 2. Therefore, the glass substrate 2 is also required to have a high degree of flatness.

[0047] Therefore, as described above, polishing (step S1), local processing (step S3), and finish polishing (step S4) are performed on the glass substrate 2 in this order. In the finish polishing, the glass substrate 2 is pressed against a surface plate while rotating the glass substrate 2 and the surface plate. In the finish polishing, for example, a double-sided polisher 9 shown in FIG. 6 is used.

[0048] The double-sided polisher 9 has a lower platen 91, an upper platen 92, a carrier 93, a sun gear 94, and an internal gear 95. The lower platen 91 is arranged horizontally, and a lower polishing pad 96 is attached to the upper surface of the lower platen 91. The upper platen 92 is arranged horizontally, and an upper polishing pad 97 is attached to the lower surface of the upper platen 92. The carrier 93 holds the glass substrate 2 horizontally between the lower platen 91 and the upper platen 92. Each carrier 93 holds one glass substrate 2 at a time, but may hold multiple substrates at a time. The carrier 93 is arranged radially outside the sun gear 94 and radially inside the internal gear 95. A plurality of carriers 93 are arranged around the sun gear 94 at intervals. The sun gear 94 and the internal gear 95 are arranged concentrically and mesh with the outer peripheral gear 93a of the carrier 93.

[0049] The double-sided polisher 9 is, for example, a 4-way type, and the lower surface plate 91, the upper surface plate 92, the sun gear 94, and the internal gear 95 rotate about the same vertical rotation center line. The lower surface plate 91 and the upper surface plate 92 rotate in opposite directions, and press the lower polishing pad 96 against the lower surface of the glass substrate 2, and press the upper polishing pad 97 against the upper surface of the glass substrate 2. At least one of the lower surface plate 91 and the upper surface plate 92 supplies polishing slurry to the glass substrate 2. The polishing slurry is supplied between the glass substrate 2 and the lower polishing pad 96 to polish the lower surface of the glass substrate 2. The polishing slurry is also supplied between the glass substrate 2 and the upper polishing pad 97 to polish the upper surface of the glass substrate 2.

[0050] For example, the lower surface plate 91, the sun gear 94, and the internal gear 95 rotate in the same direction in a plan view. The rotational directions of these are opposite to the rotational direction of the upper surface plate 92. The carrier 93 rotates on its axis while revolving. The revolution direction of the carrier 93 is the same as the rotational direction of the sun gear 94 and the internal gear 95. On the other hand, the rotational direction of the carrier 93 is determined by the product of the rotation speed and pitch circle diameter of the sun gear 94 and the product of the rotation speed and pitch circle diameter of the internal gear 95. If the product of the rotation speed and pitch circle diameter of the internal gear 95 is larger than the product of the rotation speed and pitch circle diameter of the sun gear 94, the rotational direction of the carrier 93 and the revolution direction of the carrier 93 will be the same direction. On the other hand, if the product of the rotation speed and pitch circle diameter of the internal gear 95 is smaller than the product of the rotation speed and pitch circle diameter of the sun gear 94, the rotation direction of the carrier 93 and the revolution direction of the carrier 93 are opposite to each other.

[0051] The first main surface 21 and the second main surface 22 of the glass substrate 2 are finish-polished by the double-sided polisher 9 in an approximately axially symmetric manner about their respective centers. The first main surface 21 and the second main surface 22 tend to be polished in a plane-symmetric manner with respect to the central plane in the plate thickness direction of the glass substrate 2. The first main surface 21 and the second main surface 22 tend to be both polished into a convex curved surface, or both polished into a concave curved surface. Note that for the finish polishing, a single-sided polisher (not shown) may be used as described above.

[0052] FIG. 7 shows an example of the height distribution of the central region 27 of the first main surface 21 after finish polishing. Here, the height distribution after tilt correction is shown. The central region 27 shown in FIG. 7 is a convex curved surface in which the height at the center is higher than the heights at the four corners. The units of the values ​​indicating the height in FIG. 7 are nm, and the larger the value, the higher the height. Note that the height distribution of the central region of the second main surface 22 after finish polishing is similar to the height distribution in FIG. 7, and is therefore not shown.

[0053] 7 was measured using an UltraFlat200Mask manufactured by Corning Tropel Inc. In order to eliminate the influence of gravity, the glass substrate 2 was stood substantially vertically and supported so that neither the first main surface 21 nor the second main surface 22 of the glass substrate 2 was in contact with other members such as a stage, and the height distribution was measured.

[0054] As is clear from Fig. 7, central region 27 of first main surface 21 after finish polishing is not completely axially symmetric, but contains axially symmetric components and the remaining distortion components. The distortion components will be described in detail later, but contain four-fold symmetric components rotated around the center of central region 27 as shown in Fig. 9. These four-fold symmetric components are generated by finish polishing.

[0055] The four-fold symmetric components are preferably expressed by Zernike polynomials rather than Legendre polynomials because, unlike Legendre polynomials, Zernike polynomials are expressed in polar coordinates and are suitable for removing axially symmetric components.

[0056] However, unlike the Legendre polynomials, the Zernike polynomials can only express circular regions. The central region 27 is rectangular, and the four corners of the rectangle cannot be expressed by the Zernike polynomials. Therefore, in the past, it was not possible to accurately grasp the distortion components generated by the finish polishing.

[0057] Therefore, in this embodiment, the coordinates of a point in the central area 27 of a square 142 mm in length and 142 mm in width are expressed as (x, y, z(x, y)), and the distortion components are obtained using the following equations (1) to (3).

[0058]

number

[0059] Fig. 8 shows an example of the arrangement of multiple points set in the central region 27. In Fig. 8, the X-axis direction is the horizontal direction, and the Y-axis direction is the vertical direction. The origin, which is the intersection of the X-axis and the Y-axis, is the center of the central region 27.

[0060] As is clear from FIG. 8, z1(x, y) in formula (1) is the average value of the heights of four points that are four-fold symmetric about the origin. FIG. 9 shows the height distribution of a surface, which is a set of coordinates (x, y, z1(x, y)). In FIG. 9, the units of the values ​​indicating height are nm, and the larger the value, the higher the height. The height distribution shown in FIG. 9 further includes a four-fold symmetric component rotated about the origin in addition to the axially symmetric component. This four-fold symmetric component rotates, for example, in the counterclockwise direction, as shown by the dashed line in FIG. 9.

[0061] As is clear from FIG. 8, z2(x, y) in formula (2) is the average value of the heights of eight points that are line-symmetric about four reference lines L1 to L4 that pass through the origin. Reference line L1 is the X-axis, reference line L2 is the Y-axis, and reference lines L3 and L4 are diagonals of the central region 27. The height distribution of the surface, which is a collection of coordinates (x, y, z2(x, y)), is shown in FIG. 10. The units of the values ​​indicating the height in FIG. 10 are nm, and the larger the value, the higher the height. The height distribution shown in FIG. 10 contains only components that are almost axisymmetric.

[0062] z3(x,y) in equation (3) is the difference between z1(x,y) in equation (1) and z2(x,y) in equation (2). The height distribution of the surface, which is a set of coordinates (x,y,z3(x,y)), is shown in Figure 11. The units of the values ​​indicating height in Figure 11 are nm, and the larger the value, the higher the height. The height distribution shown in Figure 11 is the difference between the height distribution shown in Figure 9 and the height distribution shown in Figure 10, and mainly contains four-fold symmetric components rotated around the origin.

[0063] Next, with reference to Fig. 12, the reason why the height distribution shown in Fig. 11 occurs due to finish polishing will be described. The arrows shown in Fig. 12 indicate the relative rotation direction of a surface plate (e.g., lower surface plate 91 or upper surface plate 92) with respect to central region 27. In other words, the arrows shown in Fig. 12 indicate the rotation direction of the surface plate in a coordinate system fixed to central region 27.

[0064] At the four corners of the central region 27, polishing progresses easily in an area A1 on the upstream side in the rotation direction of the platen, while polishing progresses less easily in an area A2 on the downstream side in the rotation direction of the platen. As a result, it is believed that the height distribution shown in FIG. 11 occurs during the finish polishing.

[0065] The inventor has found through experiments etc. that if the maximum height difference Δz3 (Δz3≧0) of the surface, which is a set of coordinates (x, y, z3(x, y)), is 6.0 nm or less, the flatness PV (PV≧0) of the central region 27 can be suppressed to less than 10.0 nm.

[0066] In the present disclosure, the flatness PV of the central region 27 refers to the maximum height difference of the remaining components after excluding the components expressed by a quadratic function from all components of the height distribution of the central region 27. The quadratic function is expressed by the following formula (4).

[0067]

number

[0068] The components of the quadratic function are components that can be automatically corrected in the exposure apparatus, and therefore do not affect the transfer accuracy of the circuit pattern 41. Therefore, the components of the quadratic function are excluded from all components of the height distribution of the central region 27 when calculating the flatness PV of the central region 27.

[0069] In order to suppress Δz3 to 6.0 nm or less, the present inventor first performs the processes of steps S1 to S4 on another glass substrate 2 in advance, and calculates the height difference z at each point of the central region 27 before and after the finish polishing using the following formula (5). dif (x, y) was calculated. Then, z was calculated using the following formula (6). 4_dif (x,y) was calculated.

[0070]

number

[0071] In the above formula (6), z 4_dif (x,y) is the average value of four points that are four-fold symmetric around the origin. Therefore, z in the above formula (6) 4_dif (x, y) is a four-fold symmetric component among the distortion components, and corresponds to z3(x, y) in the above formula (3).

[0072] The inventors calculated z 4_dif It was found that by correcting the target height of each point of the central region 27 in the local processing (step S3) using (x, y), Δz3 can be suppressed to 6.0 nm or less. As a result, a glass substrate 2 with a PV of less than 10.0 nm was obtained.

[0073] Here, the corrected target height is determined by subtracting the target height set based on the measurement result in step S2 from the target height calculated in advance by z 4_dif (x, y). In other words, the corrected target processing amount is calculated by subtracting the target processing amount set based on the measurement result of step S2 from the target processing amount calculated in advance z 4_difThe z used for these corrections is calculated by adding (x, y). 4_dif (x, y) is preferably the average value of a plurality of glass substrates 2. 4_dif The average value of (x, y) is obtained for each processing condition of the finish polishing (for example, type of abrasive, type of polishing pad, polishing pressure, rotation speed, etc.).

[0074] Furthermore, the present inventors have noticed that the distortion components caused by the finish polishing (step S4) are due to the relative rotation of the surface plate with respect to the glass substrate 2, and have found that Δz3 can be suppressed to 4.0 nm or less by reversing the rotation direction of the surface plate during the finish polishing. As a result, a glass substrate 2 with a PV of less than 8.0 nm could be obtained.

[0075] Specifically, during the finish polishing (step S4), the rotation directions of the lower platen 91 and the upper platen 92 are reversed. At that time, the rotation directions of the sun gear 94 and the internal gear 95 are also reversed. As long as the rotation directions are reversed, the rotation speeds may be the same. As described above, a single-sided polishing machine may be used in the finish polishing.

[0076] If the rotation direction of the platen is reversed during the finish polishing, the direction of the arrows in Fig. 12 is reversed, and the areas that are polished well and the areas that are polished poorly are interchanged. In the finish polishing, the time that the platen rotates clockwise and the time that the platen rotates counterclockwise are set to be approximately the same. As a result, Δz3 can be suppressed to 4.0 nm or less.

[0077] In addition, when the rotation direction of the platen is reversed during the finish polishing, the target height or the target processing amount in the local processing is corrected by z 4_dif Instead of (x, y), use z in the following formula (7): 8_dif Use (x,y).

[0078]

number

[0079] In addition, z is the average of 8 points. 8_dif Although (x, y) does not include the four-fold symmetric components shown in Fig. 11, this is not a problem because the four-fold symmetric components shown in Fig. 11 can be reduced by reversing the rotation direction of the platen during the finish polishing.

[0080] When the rotation direction of the surface plate is reversed during the finish polishing, the target height after correction is determined by subtracting the target height set based on the measurement result of step S2 from the target height calculated in advance by z 8_dif (x, y). In other words, the corrected target processing amount is calculated by subtracting the target processing amount set based on the measurement result of step S2 from the target processing amount calculated in advance z 8_dif The z used for these corrections is calculated by adding (x, y). 8_dif (x, y) is preferably the average value of a plurality of glass substrates 2. 8_dif The average value of (x, y) is obtained for each processing condition of the finish polishing (for example, type of abrasive, type of polishing pad, polishing pressure, rotation speed, etc.).

[0081] The above has been described with respect to the central region 27 of the first main surface 21 of the glass substrate 2, but the same applies to the central region of the second main surface 22 of the glass substrate 2. In the central region of the second main surface 22 as well, if Δz3 is suppressed to 6.0 nm or less, PV can be suppressed to less than 10.0 nm.

[0082] Furthermore, the flatness of the first main surface 11 of the mask blank 1 is determined by the flatness of the first main surface 21 of the glass substrate 2. Therefore, in the central region of the first main surface 11, if Δz3 is controlled to 6.0 nm or less, PV can also be controlled to 15.0 nm or less, preferably less than 10.0 nm.

[0083] Furthermore, the flatness of the second main surface 12 of the mask blank 1 is determined by the flatness of the second main surface 22 of the glass substrate 2. Therefore, in the central region of the second main surface 12, if Δz3 is controlled to 6.0 nm or less, PV can also be controlled to 15.0 nm or less, preferably less than 10.0 nm. EXAMPLES

[0084] In Examples 1 to 7, steps S1 to S4 shown in FIG. 1 were carried out under the same conditions except for the following conditions to prepare glass substrates 2, and Δz3 and PV were measured for central region 27 of first main surface 21. In Examples 1 to 3, the rotation direction of the platen was reversed during the finish polishing, and the z 8_dif The target height of the local processing was corrected using the average value of (x, y). In addition, in Examples 4 and 5, the rotation direction of the platen was kept in one direction during the finish polishing, and the z 4_dif The target height of the local processing was corrected using the average value of (x, y). On the other hand, in Examples 6 and 7, the rotation direction of the platen was kept in one direction during the finish polishing, and the z 4_dif The target height of the local processing was set using the measurement results of step S2 without using the average value of (x, y). Examples 1 to 5 are working examples, and Examples 6 and 7 are comparative examples. The results are shown in Table 1.

[0085] [Table 1] As is clear from Table 1, in Examples 1 to 3, the rotation direction of the platen was reversed during the finish polishing, and the z 8_dif Since the target height of the local processing was corrected using the average value of (x, y), Δz3 was suppressed to 4.0 nm or less, and PV was suppressed to less than 8.0 nm. In addition, in Examples 4 and 5, the rotation direction of the platen was kept in one direction during the finish polishing, and the z 4_dif Since the target height of the local processing was corrected using the average value of (x, y), Δz3 was suppressed to 6.0 nm or less, and PV was suppressed to less than 10.0 nm. On the other hand, in Examples 6 and 7, the rotation direction of the platen was kept in one direction during the finish polishing, and the z 4_difSince the target height for local processing was set using the measurement results of step S2 without using the average value of (x, y), Δz3 became larger than 6.0 nm, and PV became 10.0 nm or more.

[0086] Next, the mask blank 1 for EUVL was produced using the glass substrate 2 of Examples 1 to 7. First, a CrN film was formed as a conductive film by ion beam sputtering on the first main surface 21 (the surface on which Δz3 and PV were measured) of the glass substrate 2 by ion beam sputtering. Next, a multilayer reflective film (EUV reflective film) was formed on the second main surface 22 of the glass substrate 2 by ion beam sputtering. The multilayer reflective film was formed by alternately laminating 40 periods of a Si film of about 4 nm and a Mo film of about 3 nm, and then laminating a Si film of about 4 nm at the end. Next, a Ru film of 2.5 nm was formed as a protective film by sputtering on the multilayer reflective film. Next, a TaN film of 75 nm and a TaON film of 5 nm were formed as an absorbing film (EUV absorbing film) on the protective film by sputtering. In this manner, an EUVL mask blank 1 was obtained, which had a conductive film 5, a glass substrate 2, an EUV reflective film 3, and an EUV absorbing film 4 in this order.

[0087] Δz3 and PV were measured for the central region of the first main surface 11 (the surface on the conductive film 5 side) of the EUVL mask blank 1 produced using the glass substrate 2 of Examples 1 to 7. The results are shown in Table 2.

[0088] [Table 2] As shown in Table 2, in Examples 1 to 5, Δz3 was suppressed to 6.0 nm or less and PV was suppressed to 15.0 nm or less in the central region of the first main surface 11 of the EUVL mask blank 1. In Examples 6 and 7, Δz3 was greater than 6.0 nm and PV was greater than 15.0 nm in the central region of the first main surface 11 of the EUVL mask blank 1.

[0089] Although the EUVL glass substrate and the EUVL mask blank according to the present disclosure have been described above, the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure. [Explanation of symbols]

[0090] 2. Glass substrate 21 1st main surface 22 Second main surface 27 Central area 28 Periphery 3 EUV reflective film 4. EUV absorbing film 5 Conductive Film

Claims

1. A glass substrate for EUVL having a rectangular first main surface on which a conductive film is formed, and a rectangular second main surface facing opposite to the first main surface on which an EUV reflective film and an EUV absorbing film are formed in this order, a glass substrate for EUVL, wherein when the coordinates of a point in a central region of a square of 142 mm in length and 142 mm in width, excluding a peripheral region of the rectangular frame of the first main surface, are expressed as (x, y, z(x, y)), a maximum height difference of a surface which is a set of coordinates (x, y, z3(x, y)) calculated using the following formulas (1) to (3) is 6.0 nm or less. [0010] In the above coordinates (x, y, z(x, y)), x indicates the horizontal coordinate, y indicates the vertical coordinate, and z indicates the height coordinate, with the horizontal, vertical, and height directions being perpendicular to each other.

2. A glass substrate for EUVL having a rectangular first main surface on which a conductive film is formed, and a rectangular second main surface facing opposite to the first main surface on which an EUV reflective film and an EUV absorbing film are formed in this order, a glass substrate for EUVL, in which when the coordinates of a point in a central region of a square having a length of 142 mm and a width of 142 mm, excluding a peripheral region of the rectangular frame of the second main surface, are expressed as (x, y, z(x, y)), a maximum height difference of a surface which is a set of coordinates (x, y, z3(x, y)) calculated using the following formulas (1) to (3) is 6.0 nm or less. [0025] In the above coordinates (x, y, z(x, y)), x indicates the horizontal coordinate, y indicates the vertical coordinate, and z indicates the height coordinate, with the horizontal, vertical, and height directions being perpendicular to each other.

3. A mask blank for EUVL having a rectangular first main surface and a rectangular second main surface facing opposite to the first main surface, and having, from a side of the first main surface to a side of the second main surface, a conductive film, a glass substrate, an EUV reflective film, and an EUV absorbing film, in this order, a mask blank for EUVL, wherein when the coordinates of a point in a central region of a square of 142 mm in length and 142 mm in width, excluding a peripheral region of the first main surface in a rectangular frame shape, are expressed as (x, y, z(x, y)), a maximum height difference of a surface which is a set of coordinates (x, y, z3(x, y)) calculated using the following formulas (1) to (3) is 6.0 nm or less. [0030] In the above coordinates (x, y, z(x, y)), x indicates the horizontal coordinate, y indicates the vertical coordinate, and z indicates the height coordinate, with the horizontal, vertical, and height directions being perpendicular to each other.

4. A mask blank for EUVL having a rectangular first main surface and a rectangular second main surface facing opposite to the first main surface, and having, from a side of the first main surface to a side of the second main surface, a conductive film, a glass substrate, an EUV reflective film, and an EUV absorbing film, in this order, a mask blank for EUVL, wherein when the coordinates of a point in a central region of a square of 142 mm in length and 142 mm in width, excluding a peripheral region of the second main surface in the shape of a rectangular frame, are expressed as (x, y, z(x, y)), a maximum height difference of a surface which is a set of coordinates (x, y, z3(x, y)) calculated using the following formulas (1) to (3) is 6.0 nm or less. [0045] In the above coordinates (x, y, z(x, y)), x indicates the horizontal coordinate, y indicates the vertical coordinate, and z indicates the height coordinate, with the horizontal, vertical, and height directions being perpendicular to each other.

Citation Information

Patent Citations

  • Keyless opening and closing apparatus of car door lock

    JP1985033987A

  • boiler

    JP1987029807A

  • Mask blank substrate, mask blank, exposure mask, method for manufacturing semiconductor device and method for manufacturing mask blank substrate

    JP2006126816A

  • Manufacturing method of glass substrate for mask blank