Resin Sheet

The resin sheet with optimized epoxy resin and inorganic filler composition addresses chipping and adhesion issues, enhancing cuttability and peelability for semiconductor chip packages and circuit boards.

JP7574830B2Active Publication Date: 2024-10-29AJINOMOTO CO INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022123308
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-02
Publication Date
2024-10-29
Estimated Expiration
2042-08-02

AI Technical Summary

Technical Problem

Conventional methods for manufacturing semiconductor chip packages using resin sheets face issues with chipping during cutting and adhesion strength between the resin composition layer and the film layer, leading to poor cuttability and peelability.

Method used

A resin sheet with a resin composition layer containing epoxy resin and inorganic filler, where specific parameters such as mass reduction rate, elongation rate, and tensile modulus are within certain ranges, enhancing both cuttability and peelability.

Benefits of technology

The resin sheet achieves improved cuttability and peelability, reducing chipping and facilitating smooth film layer peeling, while maintaining structural integrity of semiconductor chip packages and circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574830000003
    Figure 0007574830000003
  • Figure 0007574830000004
    Figure 0007574830000004
  • Figure 0007574830000001
    Figure 0007574830000001
Patent Text Reader

Abstract

To provide a resin sheet including a resin composition layer that is superior in both cuttability and peelability.SOLUTION: A resin sheet includes a resin composition layer. The resin composition layer includes (A) an epoxy resin and (B) an inorganic filler. The resin composition layer satisfies the following formula (1): 0.09≤P(a)×P(b) / P(c)≤0.3 (1) (where, P(a) represents the mass reduction rate (%) of the resin composition layer after heating at 190°C for 30 minutes. P(b) represents the elongation (%) measured at a temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes. P(c) represents the tensile elasticity (GPa) measured at a temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin sheet including a resin composition layer. The present invention further relates to a semiconductor chip package and a manufacturing method thereof, a circuit board and a manufacturing method thereof, and a semiconductor device including the semiconductor chip package or the circuit board, which are manufactured using the resin sheet. [Background technology]

[0002] A method for manufacturing a semiconductor chip package such as a wafer level package generally includes a step of forming a cured material layer on a substrate such as a wafer by curing a resin composition. The cured material layer can function as, for example, an insulating layer or a sealing layer. Such a cured material layer may be formed by forming a resin composition layer from a resin composition containing an epoxy resin and an inorganic filler, and curing the resin composition layer. The resin composition layer may also be provided on the substrate by laminating a resin sheet having the resin composition layer and the substrate (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-197656 A Summary of the Invention [Problem to be solved by the invention]

[0004] A method for manufacturing a semiconductor chip package using a resin sheet may include cutting a resin composition layer to fit the shape of a substrate, laminating the resin sheet having the cut resin composition layer to the substrate, and curing the resin composition layer.

[0005] The resin composition layer is usually cut using a blade. For example, a punch blade formed in a desired shape is pressed against the resin composition layer in the thickness direction, and the resin composition layer is cut so as to be punched out in the shape of the punch blade. According to this cutting method, the resin composition layer can be easily cut into a shape that matches the substrate. For example, when a wafer level package is manufactured using a circular wafer as the substrate, the resin composition layer can be easily cut into a circular shape.

[0006] However, when a conventional resin sheet is used, a part of the resin composition layer may be chipped by the above-mentioned cutting. Therefore, the present inventor has studied how to suppress chipping of the resin composition layer during cutting. As a result of the study, the present inventor has found that chipping of the resin composition layer can be suppressed by increasing the amount of solvent in the resin composition layer. That is, when the amount of solvent is large, the compatibility between the inorganic filler in the resin composition layer and the resin component such as epoxy resin is improved, and the flexibility of the resin composition layer is increased, so that chipping can be suppressed.

[0007] However, when the resin composition layer containing an epoxy resin and an inorganic filler contains a large amount of solvent, a resin sheet having a film layer bonded to the resin composition layer may have a problem when peeling off the film layer. Specifically, it is as follows. In order to protect the resin composition layer during storage and transportation and to improve the handling property, the resin sheet may have a film layer bonded to the resin composition layer. This film layer is generally unnecessary in a semiconductor chip package, so it is peeled off during the manufacturing process of the semiconductor chip package. However, when the amount of solvent in the resin composition layer is increased, the adhesive strength between the resin composition layer and the film layer tends to increase. When the adhesive strength becomes excessive, the film layer cannot be peeled off smoothly, and a problem may occur in which a part of the resin composition layer is peeled off together with the film layer.

[0008] In this way, there is a trade-off between the property of suppressing chipping when the resin composition layer is cut and the property of suppressing the adhesive strength between the resin composition layer and the film layer to facilitate peeling of the film layer. In the following description, the property of suppressing chipping of the resin composition layer when the resin composition layer is cut may be referred to as "cuttability". Also, the property of suppressing the adhesive strength between the resin composition layer and the film layer to facilitate peeling of the film layer may be referred to as "peeling property".

[0009] The present invention has been devised in view of the above-mentioned problems, and has an object to provide: a resin sheet having a resin composition layer that is excellent in both cutability and peelability; a method for manufacturing a semiconductor chip package using the resin sheet; a semiconductor chip package having a cured layer formed by curing a resin composition layer that is excellent in both cutability and peelability; a method for manufacturing a circuit board using the resin sheet; a circuit board having a cured layer formed by curing a resin composition layer that is excellent in both cutability and peelability; and a semiconductor device including the semiconductor chip package or circuit board. [Means for solving the problem]

[0010] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved when specific parameters including a mass reduction rate P(a) of a resin composition layer containing an epoxy resin and an inorganic filler due to heating under specific conditions, and an elongation rate P(b) and a tensile modulus P(c) measured after heating the resin composition layer under other specific conditions, are within specific ranges, and have completed the present invention. That is, the present invention includes the following.

[0011] [1] A resin sheet having a resin composition layer, the resin composition layer contains (A) an epoxy resin and (B) an inorganic filler, A resin sheet, wherein the resin composition layer satisfies the following formula (1): 0.09≦P(a)×P(b) / P(c)≦0.3 (1) (In formula (1), P(a) represents the mass loss rate (%) of the resin composition layer upon heating at 190° C. for 30 minutes, P(b) represents the elongation percentage (%) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes, P(c) represents the tensile modulus (GPa) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes. [2] The resin sheet according to [1], wherein the resin composition layer contains an elastomer (C). [3] The resin sheet according to [1] or [2], wherein the resin composition layer contains a curing agent (D). [4] The resin sheet according to [3], wherein the (D) curing agent contains a maleimide resin. [5] The resin sheet according to [3] or [4], wherein the (D) curing agent contains a carbodiimide resin. [6] The resin sheet according to any one of [1] to [5], wherein the resin composition layer has a thickness of 1 μm or more and 150 μm or less. [7] The resin sheet according to any one of [1] to [6], further comprising a film layer in contact with the resin composition layer. [8] A step (I) of cutting the resin composition layer of the resin sheet according to any one of [1] to [7]; A step (II) of laminating a resin sheet having a cut resin composition layer and a substrate; and A method for producing a semiconductor chip package, comprising: a step (III) of curing the resin composition layer. [9] The method for producing a semiconductor chip package according to [8], wherein the substrate comprises a wafer.

[10] The method for producing a semiconductor chip package according to [8] or [9], wherein step (I) includes pressing a blade against the resin composition layer in a thickness direction of the resin composition layer to cut the resin composition layer.

[11] A cured layer is provided by curing a resin composition layer, the resin composition layer contains (A) an epoxy resin and (B) an inorganic filler, A semiconductor chip package, wherein a resin composition layer satisfies the following formula (1): 0.09≦P(a)×P(b) / P(c)≦0.3 (1) (In formula (1), P(a) represents the mass loss rate (%) of the resin composition layer upon heating at 190° C. for 30 minutes, P(b) represents the elongation percentage (%) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes, P(c) represents the tensile modulus (GPa) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes.

[12] A semiconductor device comprising the semiconductor chip package described in

[11] .

[13] A step (I) of cutting the resin composition layer of the resin sheet according to any one of [1] to [7]; A step (II) of laminating a resin sheet having a cut resin composition layer and a substrate; and A method for producing a circuit board, comprising: a step (III) of curing the resin composition layer.

[14] A cured layer is provided by curing a resin composition layer, the resin composition layer contains (A) an epoxy resin and (B) an inorganic filler, A circuit board, wherein a resin composition layer satisfies the following formula (1): 0.09≦P(a)×P(b) / P(c)≦0.3 (1) (In formula (1), P(a) represents the mass loss rate (%) of the resin composition layer upon heating at 190° C. for 30 minutes, P(b) represents the elongation percentage (%) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes, P(c) represents the tensile modulus (GPa) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes.

[15] A semiconductor device comprising the circuit board according to

[14] . Effect of the Invention

[0012] According to the present invention, there can be provided a resin sheet having a resin composition layer that is excellent in both cutability and peelability; a method for manufacturing a semiconductor chip package using the resin sheet; a semiconductor chip package having a cured layer formed by curing a resin composition layer that is excellent in both cutability and peelability; a method for manufacturing a circuit board using the resin sheet; a circuit board having a cured layer formed by curing a resin composition layer that is excellent in both cutability and peelability; and a semiconductor device including the semiconductor chip package or circuit board. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a resin sheet according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view that typically shows a resin sheet after the resin composition layer has been cut in the method for producing a semiconductor chip package according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described in detail below with reference to the following embodiments and examples. However, the present invention is not limited to the following embodiments and examples, and may be modified and implemented as desired without departing from the scope of the claims and their equivalents.

[0015] In the following description, unless otherwise specified, the "planar shape" refers to the shape viewed from the thickness direction.

[0016] In the following description, the "resin component" in the resin composition layer refers to the non-volatile components in the resin composition layer excluding the inorganic filler unless otherwise specified. Also, the "resin component" in the resin composition refers to the non-volatile components in the resin composition excluding the inorganic filler unless otherwise specified.

[0017] [Resin sheet overview] A resin sheet according to one embodiment of the present invention includes a resin composition layer. The resin composition layer contains an epoxy resin (A) and an inorganic filler (B). The resin sheet satisfies the following formula (1). 0.09≦P(a)×P(b) / P(c)≦0.3 (1) (In formula (1), P(a) represents the mass loss rate (%) of the resin composition layer upon heating at 190° C. for 30 minutes, P(b) represents the elongation percentage (%) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes, P(c) represents the tensile modulus (GPa) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes.

[0018] The resin composition layer of the resin sheet according to the present embodiment can be excellent in both cutability and peelability. Therefore, the resin composition layer of the resin sheet according to the present embodiment can suppress chipping of the resin composition layer when cut. In addition, when the resin sheet according to the present embodiment has a film layer provided in contact with the resin composition layer, the film layer can be smoothly peeled off. Conventionally, the cutability and peelability were in a trade-off relationship, but according to the resin sheet according to the present embodiment, it is possible to improve both the cutability and peelability. In addition, when the resin composition layer of the resin sheet according to the present embodiment is cured to obtain a cured layer, it is usually possible to suppress warping of members such as semiconductor chip packages and circuit boards that have the cured layer.

[0019] [Explanation of the relationship expressed by formula (1)] In the following description, the parameters of the resin sheet expressed by the formula "P(a)×P(b) / P(c)" may be referred to as "specific parameters" as appropriate. The specific parameters of the resin sheet "P(a)×P(b) / P(c)" satisfy the relationship of the following formula (1). 0.09≦P(a)×P(b) / P(c)≦0.3 (1) (In formula (1), P(a) represents the mass loss rate (%) of the resin composition layer upon heating at 190° C. for 30 minutes, P(b) represents the elongation percentage (%) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes, P(c) represents the tensile modulus (GPa) measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes.

[0020] In detail, the range of the specific parameter "P(a)×P(b) / P(c)" is usually 0.09 or more, preferably 0.10 or more, more preferably 0.11 or more, more preferably 0.14 or more, and even more preferably 0.16 or more, and is usually 0.30 or less, preferably 0.25 or less, and more preferably 0.20 or less. When the specific parameter "P(a)×P(b) / P(c)" is in the above range, both the cuttability and peelability can be improved.

[0021] P(a) represents the mass reduction rate (%) of the resin composition layer by heating at 190°C for 30 minutes. Therefore, the mass reduction rate P(a) represents the proportion of components removed from the resin composition layer by heating at 190°C for 30 minutes. Usually, all or most of the components removed by heating at 190°C for 30 minutes are solvents as volatile components. In addition, usually, all or most of the solvent contained in the resin composition layer can be volatilized by heating under harsh conditions such as 190°C for 30 minutes. Therefore, the mass reduction rate P(a) represents the amount of solvent contained in the resin composition layer before heating or is correlated with the amount of the solvent. Therefore, the mass reduction rate P(a) can represent the extent of the amount of solvent in the resin composition layer.

[0022] In general, when the amount of solvent in the resin composition layer is large, the compatibility between the (B) inorganic filler, which is one of the causes of the hardness of the resin composition layer, and the (A) resin component such as epoxy resin is improved, and the flexibility of the resin composition layer is improved. Therefore, the flexibility of the resin composition layer is improved when cutting, and the destruction of the resin composition layer when subjected to stress is suppressed, so that the occurrence of chipping can be suppressed. However, when the amount of solvent is large, the adhesive strength between the resin composition layer and the film layer in contact with the resin composition layer tends to be high. If the adhesive strength is excessively large, problems may occur when the film layer is peeled off. On the other hand, when the specific parameter "P(a) x P(b) / P(c)" is within the above range, the above problems can be suppressed and both the cuttability and peelability can be improved.

[0023] From the viewpoint of significantly exerting the effects of the present invention, the range of the mass reduction rate P(a) is preferably 0.6% or more, more preferably 0.8% or more, and particularly preferably 1.0% or more, and is preferably 2.4% or less, more preferably 2.2% or less, and particularly preferably 2.0% or less.

[0024] The mass reduction rate P(a) can be adjusted, for example, by the type and ratio of the solvent contained in the resin composition and the drying conditions (drying temperature, drying time, etc.) when forming the resin composition layer. Specifically, the mass reduction rate P(a) can be adjusted by selecting and appropriately combining multiple types of solvents with different boiling points and adjusting the drying conditions.

[0025] The mass reduction rate P(a) can be obtained by dividing the mass reduction amount ΔM of the resin composition layer by heating at 190° C. for 30 minutes by the mass m0 of the resin composition layer before heating. The mass reduction amount ΔM can be obtained as the difference between the mass of the resin composition layer before heating and the mass of the resin composition layer after heating. In addition, when the resin sheet has an optional layer (e.g., a film layer) other than the resin composition layer and the mass change of the optional layer due to heating is negligibly small, the mass reduction amount ΔM may be obtained as the difference between the mass of the resin sheet before heating and the mass of the resin sheet after heating. The specific method for measuring the mass reduction rate P(a) can be the method described in the examples.

[0026] P(b) represents the elongation percentage (%) of the resin composition layer measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes. Usually, most or all of the volatile components such as the solvent contained in the resin composition layer are dried by heating at 130°C for 30 minutes, but the non-volatile components such as (A) epoxy resin and (B) inorganic filler remain in the resin composition layer. In addition, heating at 130°C for 30 minutes generally does not or hardly causes the reaction of the resin components to proceed. Therefore, the elongation percentage P(b) represents the elongation percentage as a physical property of the non-volatile components contained in the resin composition layer, or has a correlation with the elongation percentage. Therefore, the elongation percentage P(b) can represent the degree of flexibility of the non-volatile components of the resin composition layer excluding volatile components such as the solvent.

[0027] A resin composition layer having a high flexibility of non-volatile components can suppress breakage due to stress. Therefore, even if stress is applied when cutting the resin composition layer, the breakage of the resin composition layer is suppressed, so that the occurrence of chipping can be suppressed. In addition, the flexibility of the non-volatile components of the resin composition layer can contribute to suppression of cohesive failure of the resin composition layer due to stress when peeling off the film layer, and can contribute to suppression of peeling off of a part of the resin composition layer (usually the part near the surface) due to the cohesive failure. On the other hand, a resin composition layer having a flexible non-volatile component tends to have high adhesion strength with the film layer, and therefore the stress when peeling off the film layer tends to be large, so in that sense, peeling off of a part of the resin composition layer is likely to occur. Therefore, both the cutability and the peelability could not be improved by only adjusting the elongation rate P(b). However, when the specific parameter "P(a)×P(b) / P(c)" is in the above range, both the cutability and the peelability can be improved.

[0028] From the viewpoint of significantly exerting the effects of the present invention, the range of the elongation percentage P(b) is preferably 0.8% or more, more preferably 0.9% or more, and is preferably 1.6% or less, more preferably 1.5% or less, and particularly preferably 1.4% or less.

[0029] The elongation percentage P(b) can be adjusted, for example, by the type and ratio of the non-volatile components contained in the resin composition. Specifically, the elongation percentage (b) can be adjusted by appropriately selecting and combining the type and amount of (A) epoxy resin, the amount of (B) inorganic filler, and the types and amounts of (C) elastomer and (D) curing agent.

[0030] The elongation percentage P(b) can be measured at a measurement temperature of 25° C. using a cured product for evaluation obtained by heating the resin composition layer at 130° C. for 30 minutes. The measurement can be performed in accordance with JIS K7127. The specific method for measuring the elongation percentage P(b) can be the method described in the Examples.

[0031] P(c) represents the tensile modulus (GPa) of the resin composition layer measured at a measurement temperature of 25°C after heating the resin composition layer at 130°C for 30 minutes. As described above, most or all of the volatile components such as the solvent contained in the resin composition layer are dried by heating at 130°C for 30 minutes, but the non-volatile components such as (A) epoxy resin and (B) inorganic filler remain in the resin composition layer. In addition, by heating at 130°C for 30 minutes, the reaction of the resin components generally does not proceed or proceeds very little. Therefore, the tensile modulus P(c) represents the tensile modulus as a physical property of the non-volatile components contained in the resin composition layer or has a correlation with the tensile modulus. Therefore, the tensile modulus P(c) can represent the degree of rigidity of the non-volatile components of the resin composition layer excluding volatile components such as the solvent.

[0032] In general, a resin composition layer having a high rigidity of non-volatile components tends to have a low adhesive strength with the film layer. Therefore, the stress applied to the resin composition layer when the film layer is peeled off can be reduced, so that defects can be suppressed when the film layer is peeled off. However, if the rigidity of the non-volatile components of the resin composition layer is high, the brittleness of the resin composition layer increases, and chipping is likely to occur when cutting. In contrast, when the specific parameter "P(a) x P(b) / P(c)" is within the above range, the chipping can be suppressed, and both the cuttability and peelability can be improved.

[0033] From the viewpoint of significantly exerting the effects of the present invention, the range of the tensile modulus P(c) is preferably 8 GPa or more, more preferably 9 GPa or more, and preferably 16 or less, more preferably 15 or less, even more preferably 14 GPa or less, and even more preferably 13 GPa or less.

[0034] The tensile modulus P(c) can be adjusted, for example, by the type and ratio of the non-volatile components contained in the resin composition. Specifically, the tensile modulus P(c) can be adjusted by appropriately selecting and combining the type and amount of (A) epoxy resin, the amount of (B) inorganic filler, and the types and amounts of (C) elastomer and (D) curing agent.

[0035] The tensile modulus P(c) can be measured at a measurement temperature of 25° C. using a cured product for evaluation obtained by heating the resin composition layer at 130° C. for 30 minutes. The measurement can be performed in accordance with JIS K7127. The specific method for measuring the tensile modulus P(c) can be the method described in the Examples.

[0036] [Composition of Resin Composition Layer] A resin sheet according to one embodiment of the present invention includes a resin composition layer containing (A) an epoxy resin and (B) an inorganic filler. The resin composition layer usually contains a resin composition containing the above-mentioned (A) epoxy resin and (B) inorganic filler, and preferably contains only the resin composition. A resin composition containing a combination of (A) an epoxy resin and (B) an inorganic filler has excellent dielectric properties such as dielectric tangent. In addition, a resin sheet having a specific parameter "P(a)×P(b) / P(c)" within the above-mentioned range can have both good cuttability and peelability.

[0037] ((A) Epoxy resin) The epoxy resin (A) as the component (A) is a curable resin having an epoxy group. Examples of the epoxy resin (A) include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidylester type epoxy resin, Examples of the epoxy resin include cresol novolac type epoxy resin, phenol aralkyl type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, isocyanurate type epoxy resin, aliphatic triglycidyl ether type epoxy resin, phenolphthalimidine type epoxy resin, etc. (A) The epoxy resin may be used alone or in combination of two or more kinds.

[0038] From the viewpoint of obtaining a cured layer having excellent heat resistance, the epoxy resin (A) preferably contains an epoxy resin containing an aromatic structure. The aromatic structure is a chemical structure generally defined as aromatic, and also includes polycyclic aromatics and aromatic heterocycles. Examples of epoxy resins containing an aromatic structure include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, bisxylenol type epoxy resins, glycidylamine type epoxy resins having an aromatic structure, glycidylamine type epoxy resins having an aromatic structure, and glycidylamine type epoxy resins having an aromatic structure. Examples of the epoxy resins include ricidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, phenolphthalimidine type epoxy resins, linear aliphatic epoxy resins having an aromatic structure, epoxy resins having a butadiene structure having an aromatic structure, alicyclic epoxy resins having an aromatic structure, heterocyclic epoxy resins, spiro ring-containing epoxy resins having an aromatic structure, cyclohexane dimethanol type epoxy resins having an aromatic structure, naphthylene ether type epoxy resins, trimethylol type epoxy resins having an aromatic structure, and tetraphenylethane type epoxy resins having an aromatic structure.

[0039] The (A) epoxy resin preferably contains an epoxy resin having two or more epoxy groups in one molecule. The proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the non-volatile components of the (A) epoxy resin is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0040] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). (A) Epoxy resin may contain only liquid epoxy resins, or may contain only solid epoxy resins, or may contain a combination of liquid epoxy resins and solid epoxy resins.

[0041] As the liquid epoxy resin, liquid epoxy resin having two or more epoxy groups in one molecule is preferred.As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, epoxy resin having butadiene structure, aliphatic triglycidyl ether type epoxy resin is preferred, and aliphatic triglycidyl ether type epoxy resin is particularly preferred.As the aliphatic triglycidyl ether type epoxy resin, for example, polymethylolalkane triglycidyl ether can be mentioned, and a specific example thereof can be trimethylolpropane triglycidyl ether, etc.

[0042] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", and "604" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycirol type epoxy resin) manufactured by ADEKA Corporation; "EP-3950L" and "EP-3980S" (glycidylamine type epoxy resins) manufactured by ADEKA Corporation; Examples of such epoxy resins include "EP-4088S" (dicyclopentadiene type epoxy resin) manufactured by Company A; "ZX1059" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel Chemical & Material; "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical & Material; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase Chemtex Corporation; "EX-321L" (aliphatic triglycidyl ether type epoxy resin) manufactured by Nagase Chemtex Corporation; "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation; "PB-3600" manufactured by Daicel Corporation, and "JP-100" and "JP-200" (epoxy resin having a butadiene structure) manufactured by Nippon Soda Co., Ltd. These may be used alone or in combination of two or more types.

[0043] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.As the solid epoxy resin, a bixylenol type epoxy resin, a naphthalene type epoxy resin, a naphthalene type 4-functional epoxy resin, a naphthol novolac type epoxy resin, a cresol novolac type epoxy resin, a dicyclopentadiene type epoxy resin, a trisphenol type epoxy resin, a naphthol type epoxy resin, a biphenyl type epoxy resin, a naphthylene ether type epoxy resin, an anthracene type epoxy resin, a bisphenol A type epoxy resin, a bisphenol AF type epoxy resin, a phenol aralkyl type epoxy resin, a tetraphenylethane type epoxy resin, and a phenolphthalimidine type epoxy resin are preferable.

[0044] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation; "EXA-7311" and "EXA-7321" manufactured by DIC Corporation. A-7311-G3, EXA-7311-G4, EXA-7311-G4S, HP6000 (naphthylene ether type epoxy resin); EPPN-502H (trisphenol type epoxy resin) manufactured by Nippon Kayaku; NC7000L (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku; NC3000H, NC3000, NC3000L, NC3000FH, NC3100 (biphenyl type epoxy resin) manufactured by Nippon Steel Chemical & Material; ESN475V (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material. ), "ESN4100V" (naphthalene type epoxy resin); "ESN485" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd. Examples of epoxy resins that can be used include "YX7700" (phenol aralkyl type epoxy resin) manufactured by Osaka Gas Chemicals; "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.These may be used alone or in combination of two or more.

[0045] When a liquid epoxy resin and a solid epoxy resin are used in combination as the (A) epoxy resin, the mass ratio thereof (liquid epoxy resin:solid epoxy resin) is preferably 20:1 to 1:20, more preferably 10:1 to 1:10, and particularly preferably 7:1 to 1:7.

[0046] The epoxy equivalent of the (A) epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 3,000 g / eq., further preferably 80 g / eq. to 2,000 g / eq., and particularly preferably 110 g / eq. to 1,000 g / eq. The epoxy equivalent represents the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.

[0047] The weight average molecular weight (Mw) of the epoxy resin (A) is preferably from 100 to 5,000, more preferably from 250 to 3,000, and further preferably from 400 to 1500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.

[0048] The range of the amount of the epoxy resin (A) in the resin composition layer is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the nonvolatile components in the resin composition layer. The range of the amount of the epoxy resin (A) in the resin composition based on 100% by mass of the nonvolatile components in the resin composition layer is preferably the same as the above-mentioned range of the amount of the epoxy resin (A) in the resin composition layer based on 100% by mass of the nonvolatile components in the resin composition layer. When the amount of the epoxy resin (A) in the resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range is within the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0049] The range of the amount of the epoxy resin (A) in the resin composition layer is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, based on 100% by mass of the resin components in the resin composition layer. The range of the amount of the epoxy resin (A) in the resin composition based on 100% by mass of the resin components in the resin composition is preferably the same as the above-mentioned range of the amount of the epoxy resin (A) in the resin composition layer based on 100% by mass of the resin components in the resin composition layer. When the amount of the epoxy resin (A) in the resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range is within the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0050] ((B) Inorganic filler) The (B) inorganic filler as the (B) component is usually contained in the resin composition and the resin composition layer in the form of particles. An inorganic compound is used as the material of the (B) inorganic filler. Examples of the material of the (B) inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium titanate zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica and alumina are preferred, and silica is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, etc. In addition, spherical silica is preferable as the silica. (B) The inorganic filler may be used alone or in combination of two or more kinds.

[0051] (B) Commercially available inorganic fillers include, for example, "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", "SO-C1", and "SC2050-SXF" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; and "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Corporation.

[0052] From the viewpoint of significantly obtaining the desired effects of the present invention, the average particle size of the (B) inorganic filler is preferably 0.01 μm or more, more preferably 0.05 μm or more, particularly preferably 0.1 μm or more, and is preferably 10 μm or less, more preferably 7 μm or less, and even more preferably 5 μm or less.

[0053] (B) The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the mixture by ultrasonic waves for 10 minutes. The measurement sample can be measured by using a laser diffraction particle size distribution measuring device with blue and red light wavelengths as the light source, and the volume-based particle size distribution of the inorganic filler can be measured by a flow cell method, and the average particle size can be calculated from the obtained particle size distribution as the median diameter. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0054] The range of the specific surface area of ​​the (B) inorganic filler is preferably within 1 m from the viewpoint of significantly obtaining the desired effects of the present invention. 2 / g or more, more preferably 2m 2 / g or more, particularly preferably 3m 2 / g or more. There is no particular upper limit, but it is preferably 60m 2 / g or less, 50m 2 / g or less or 40m 2 The specific surface area can be measured by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0055] (B) The inorganic filler is preferably treated with a surface treatment agent from the viewpoint of improving moisture resistance and dispersibility. Examples of the surface treatment agent include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, titanate coupling agents, etc. The surface treatment agent may be used alone or in any combination of two or more.

[0056] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0057] From the viewpoint of improving the dispersibility of the (B) inorganic filler, the degree of surface treatment with the surface treatment agent is preferably within a specific range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably with 0.2% to 3% by mass of the surface treatment agent, and even more preferably with 0.3% to 2% by mass of the surface treatment agent.

[0058] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin composition, it is more preferable that the content is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0059] (B) The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0060] The range of the amount of the (B) inorganic filler in the resin composition layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 77% by mass or more, and preferably 90% by mass or less, more preferably 86% by mass or less, even more preferably 83% by mass or less, particularly preferably 81% by mass or less, based on 100% by mass of the nonvolatile components in the resin composition. The range of the amount of the (B) inorganic filler in the resin composition based on 100% by mass of the nonvolatile components in the resin composition is preferably the same as the above-mentioned range of the amount of the (B) inorganic filler in the resin composition layer based on 100% by mass of the nonvolatile components in the resin composition layer. When the amount of the (B) inorganic filler in the resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range is within the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured product layer formed using the resin sheet can be effectively suppressed.

[0061] ((C) Elastomer) The resin composition layer and the resin composition according to the present embodiment may contain an elastomer (C) as an optional component. The elastomer (C) as the component (C) does not include those corresponding to the above-mentioned components (A) and (B).

[0062] The (C) elastomer is a resin having flexibility, and is preferably a resin having rubber elasticity or a resin exhibiting rubber elasticity by polymerization with another component. Examples of rubber elasticity include resins exhibiting an elastic modulus of 1 GPa or less when a tensile test is performed at a temperature of 25°C and a humidity of 40% RH according to the Japanese Industrial Standards (JIS K7161). The (C) elastomer is usually an amorphous resin component that can be dissolved in an organic solvent. The (C) elastomer may be used alone or in combination of two or more types at any ratio. The (C) elastomer allows the elongation percentage P(b) and tensile modulus P(c) of the resin composition layer to be adjusted, so that the specific parameter "P(a)×P(b) / P(c)" of the resin sheet can be easily controlled to fall within the above-mentioned range.

[0063] The (C) elastomer preferably has a high molecular weight. The range of the number average molecular weight (Mn) of the (C) elastomer is preferably 1,000 or more, more preferably 1,500 or more, even more preferably 2,000 or more, even more preferably 3,000 or more, and particularly preferably 5,000 or more. There is no particular upper limit to the number average molecular weight, but it is preferably 1,000,000 or less, more preferably 900,000 or less. The number average molecular weight (Mn) is the number average molecular weight in terms of polystyrene measured using GPC (gel permeation chromatography).

[0064] The (C) elastomer is preferably one or more selected from resins having a glass transition temperature (Tg) of 25° C. or less and resins that are liquid at 25° C. or less. The glass transition temperature of the resin having a glass transition temperature (Tg) of 25° C. or less is preferably 20° C. or less, more preferably 15° C. or less. The lower limit of the glass transition temperature is not particularly limited, but it can usually be −15° C. or more. The resin that is liquid at 25° C. is preferably a resin that is liquid at 20° C. or less, more preferably a resin that is liquid at 15° C. or less. The glass transition temperature can be measured by DSC (differential scanning calorimetry) at a heating rate of 5° C. / min.

[0065] The (C) elastomer is preferably a resin having one or more structures selected from a polybutadiene structure, a polysiloxane structure, a poly(meth)acrylate structure, a polyalkylene structure, a polyalkyleneoxy structure, a polyisoprene structure, a polyisobutylene structure, a polycarbonate structure, and a polystyrene structure in the molecule. The term "(meth)acrylate" includes methacrylate and acrylate, as well as combinations thereof. These structures may be included in the main chain or side chain of the (C) elastomer molecule.

[0066] The (C) elastomer may be, for example, a resin containing a polybutadiene structure. The polybutadiene structure may be contained in the main chain or in the side chain. The polybutadiene structure may be partially or entirely hydrogenated. A resin containing a polybutadiene structure may be called a "polybutadiene resin." Specific examples of polybutadiene resins include "Ricon 130MA8", "Ricon 130MA13", "Ricon 130MA20", "Ricon 131MA5", "Ricon 131MA10", "Ricon 131MA17", "Ricon 131MA20", and "Ricon 184MA6" (polybutadiene containing an acid anhydride group) manufactured by Cray Valley Corporation; "GQ-1000" (polybutadiene having hydroxyl groups and carboxyl groups introduced therein), "G-1000", "G-2000", and "G-3000" (polybutadiene having hydroxyl groups at both ends), "GI-1000", "GI-2000", and "GI-3000" (polybutadiene having hydrogenated hydroxyl groups at both ends) manufactured by Nippon Soda Co., Ltd.; and "FCA-061L" (hydrogenated polybutadiene skeleton epoxy resin) manufactured by Nagase ChemteX Corporation. Specific examples of polybutadiene resins include phenolic hydroxyl group-containing butadiene resins; and polyimide resins having a polybutadiene structure, a urethane structure, and an imide structure in the molecule. The polyimide resins can be produced as linear polyimide resins (polyimides described in JP 2006-37083 A and WO 2008 / 153208 A) using hydroxyl group-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride as raw materials. The content of the butadiene structure in the polyimide resin is preferably 60% by mass to 95% by mass, more preferably 75% by mass to 85% by mass. Details of the polyimide resins can be found in JP 2006-37083 A and WO 2008 / 153208 A, the contents of which are incorporated herein by reference.

[0067] Examples of the (C) elastomer include resins containing a poly(meth)acrylate structure. Resins containing a poly(meth)acrylate structure are sometimes called "poly(meth)acrylic resins." Specific examples of poly(meth)acrylic resins include Teisan Resin manufactured by Nagase ChemteX Corporation; "ME-2000," "W-116.3," "W-197C," "KG-25," and "KG-3000" manufactured by Negami Chemical Industries Co., Ltd.; and "ARUFON UH-2000" manufactured by Toagosei Co., Ltd.

[0068] Examples of the (C) elastomer include resins containing a polycarbonate structure. Resins containing a polycarbonate structure are sometimes called "polycarbonate resins". Specific examples of polycarbonate resins include "FPC0220" and "FPC2136" manufactured by Mitsubishi Gas Chemical Co., Ltd., "T6002" and "T6001" (polycarbonate diols) manufactured by Asahi Kasei Chemicals Corporation, and "C-1090", "C-2090", and "C-3090" (polycarbonate diols) manufactured by Kuraray Co., Ltd. Specific examples of polycarbonate resins include polyimide resins having an imide structure, a urethane structure, and a polycarbonate structure in the molecule. The polyimide resins can be produced as linear polyimide resins using hydroxyl-terminated polycarbonate, a diisocyanate compound, and a tetrabasic acid anhydride as raw materials. The content of the carbonate structure in the polyimide resin is preferably 60% by mass to 95% by mass, more preferably 75% by mass to 85% by mass. For details of the polyimide resin, refer to the description in International Publication No. 2016 / 129541, the contents of which are incorporated herein by reference.

[0069] Examples of the (C) elastomer include resins containing a polysiloxane structure. Resins containing a polysiloxane structure are sometimes called "siloxane resins." Specific examples of siloxane resins include "SMP-2006," "SMP-2003PGMEA," and "SMP-5005PGMEA" manufactured by Shin-Etsu Silicone Co., Ltd., and linear polyimides made from amine-terminated polysiloxanes and tetrabasic acid anhydrides (see International Publication No. 2010 / 053185, JP 2002-12667 A, JP 2000-319386 A, etc.).

[0070] Examples of the (C) elastomer include resins containing a polyalkylene structure or a polyalkyleneoxy structure. A resin containing a polyalkylene structure may be referred to as an "alkylene resin." A resin containing a polyalkyleneoxy structure may be referred to as an "alkyleneoxy resin." The number of carbon atoms in the polyalkylene structure and the polyalkyleneoxy structure is preferably 2 to 15, more preferably 3 to 10, and particularly preferably 5 to 6. Specific examples of alkylene resins and alkyleneoxy resins include "PTXG-1000" and "PTXG-1800" manufactured by Asahi Kasei Fibers Corporation; "EXA-4850-150", "EXA-4816", and "EXA-4822" manufactured by DIC Corporation; "EP-4000", "EP-4003", "EP-4010", and "EP-4011" manufactured by ADEKA Corporation; "BEO-60E" and "BPO-20E" manufactured by New Japan Chemical Co., Ltd.; and "YL7175" and "YL7410" manufactured by Mitsubishi Chemical Corporation.

[0071] (C) Elastomers include, for example, resins containing a polyisoprene structure. Resins containing a polyisoprene structure are sometimes called "isoprene resins." Specific examples of isoprene resins include "KL-610" and "KL613" manufactured by Kuraray Co., Ltd.

[0072] (C) Elastomers include, for example, resins containing a polyisobutylene structure. Resins containing a polyisobutylene structure are sometimes called "isobutylene resins." Specific examples of isobutylene resins include Kaneka Corporation's "SIBSTAR-073T" (styrene-isobutylene-styrene triblock copolymer) and "SIBSTAR-042D" (styrene-isobutylene diblock copolymer).

[0073] Examples of the (C) elastomer include resins containing a polystyrene structure. Resins containing a polystyrene structure are sometimes called "polystyrene resins". The polystyrene resin may be a copolymer containing an arbitrary repeating unit other than the styrene unit in combination with the styrene unit, or may be a hydrogenated polystyrene resin. Examples of the polystyrene resin include styrene-butadiene-styrene block copolymers (SBS), styrene-isoprene-styrene block copolymers (SIS), styrene-ethylene-butylene-styrene block copolymers (SEBS), styrene-ethylene-propylene-styrene block copolymers (SEPS), styrene-ethylene-ethylene-propylene-styrene block copolymers (SEEPS), styrene-butadiene-butylene-styrene block copolymers (SBBS), styrene-butadiene diblock copolymers, hydrogenated styrene-butadiene block copolymers, hydrogenated styrene-isoprene block copolymers, hydrogenated styrene-butadiene random copolymers, and styrene-maleic anhydride copolymers. Specific examples of polystyrene resins include hydrogenated styrene-based thermoplastic elastomers "H1041", "Tuftec H1043", "Tuftec P2000", and "Tuftec MP10" (manufactured by Asahi Kasei Corporation); epoxidized styrene-butadiene thermoplastic elastomers "Epofriend AT501" and "CT310" (manufactured by Daicel Corporation); modified styrene-based elastomers having hydroxyl groups "Septon HG252" (manufactured by Kuraray Co., Ltd.); modified styrene-based elastomers having carboxyl groups "Tuftec N503M", modified styrene-based elastomers having amino groups "Tuftec N501", modified styrene-based elastomers having acid anhydride groups "Tuftec M1913" (manufactured by Asahi Kasei Chemicals Corporation); unmodified styrene-based elastomers "Septon S8104" (manufactured by Kuraray Co., Ltd.); styrene-ethylene / butylene-styrene block copolymers "FG1924" (manufactured by Kraton Corporation), and "EF-40" (manufactured by CRAY VALLEY Co., Ltd.).

[0074] Among the above, the (C) elastomer is preferably a resin containing at least one structure selected from the group consisting of a polybutadiene structure and a poly(meth)acrylate structure in the molecule, from the viewpoint of obtaining particularly good releasability.Furthermore, the (C) elastomer is particularly preferably a resin having a polybutadiene structure in the molecule, from the viewpoint of obtaining particularly good cutting properties.

[0075] The (C) elastomer may have a functional group capable of reacting with the (A) epoxy resin. When the (C) elastomer reacts with the (A) epoxy resin, the mechanical strength of the cured layer obtained by curing the resin composition layer can be increased. The functional group capable of reacting with the (A) epoxy resin includes a functional group that appears upon heating. The functional group capable of reacting with the (A) epoxy resin may be one or more functional groups selected from the group consisting of a hydroxy group, a carboxy group, an acid anhydride group, a phenolic hydroxyl group, an epoxy group, an isocyanate group, and a urethane group. Among these, the functional group is preferably a hydroxy group, an acid anhydride group, a phenolic hydroxyl group, an epoxy group, an isocyanate group, and a urethane group, more preferably a hydroxy group, an acid anhydride group, a phenolic hydroxyl group, and an epoxy group, and particularly preferably a phenolic hydroxyl group. The number average molecular weight (Mn) of the (C) elastomer containing the functional group is preferably greater than 5,000, and therefore the weight average molecular weight (Mw) of the (C) elastomer is also preferably greater than 5,000.

[0076] The range of the amount of the (C) elastomer in the resin composition layer is preferably 1% by mass or more, more preferably 3% by mass or more, even more preferably 5% by mass or more, and preferably 20% by mass or less, more preferably 18% by mass or less, even more preferably 15% by mass or less, and particularly preferably 11% by mass or less, based on 100% by mass of the nonvolatile components in the resin composition layer. The range of the amount of the (C) elastomer in the resin composition based on 100% by mass of the nonvolatile components in the resin composition is preferably the same as the above-mentioned range of the amount of the (C) elastomer in the resin composition layer based on 100% by mass of the nonvolatile components in the resin composition layer. When the amount of the (C) elastomer is within the above-mentioned range in a resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0077] The range of the amount of the (C) elastomer in the resin composition layer is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and preferably 70% by mass or less, more preferably 60% by mass or less, even more preferably 55% by mass or less, and particularly preferably 52% by mass or less, based on 100% by mass of the resin components in the resin composition layer. The range of the amount of the (C) elastomer in the resin composition based on 100% by mass of the resin components in the resin composition is preferably the same as the above-mentioned range of the amount of the (C) elastomer in the resin composition layer based on 100% by mass of the resin components in the resin composition layer. When the amount of the (C) elastomer is within the above-mentioned range in a resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured product layer formed using the resin sheet can be effectively suppressed.

[0078] ((D) Hardener) The resin composition layer and the resin composition according to the present embodiment may contain a (D) curing agent as an optional component. The (D) curing agent as the (D) component does not include those corresponding to the above-mentioned (A) to (C) components. The (D) curing agent can have a function of reacting with the (A) epoxy resin to cure the resin composition.

[0079] Examples of the (D) curing agent include maleimide resins, carbodiimide resins, active ester resins, phenol resins, amine resins, acid anhydride resins, cyanate ester resins, benzoxazine resins, and thiol resins. Among them, maleimide resins, carbodiimide resins, active ester resins, and phenol resins are preferred, and maleimide resins and carbodiimide resins are more preferred. The (D) curing agent may be used alone or in combination of two or more.

[0080] As the maleimide resin, a compound having one or more, preferably two or more, maleimide groups (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl groups) in one molecule can be used. The maleimide resin can react with the epoxy resin (A) in the presence of a suitable catalyst such as an imidazole curing accelerator to form a bond. In addition, the maleimide resin can undergo radical polymerization due to the ethylenic carbon-carbon unsaturated bond contained in the maleimide group, so that the maleimide resin can also bond with itself. When the maleimide resin is used, the warping of a member such as a semiconductor chip package having a cured layer formed using a resin sheet can be effectively suppressed while improving the cuttability and peelability.

[0081] The maleimide resin may be an aliphatic maleimide resin containing an aliphatic amine skeleton, or an aromatic maleimide resin containing an aromatic amine skeleton. Commercially available maleimide resins include, for example, maleimide resins containing an aliphatic skeleton having 36 carbon atoms derived from dimer diamine, such as "BMI-3000J", "BMI-5000", "BMI-1400", "BMI-1500", "BMI-1700", and "BMI-689" (all manufactured by DigiCner Molecules); maleimide resins containing an indane skeleton, as described in the Japan Institute of Invention and Innovation Disclosure Technical Bulletin No. 2020-500211; maleimide resins containing an aromatic ring skeleton directly bonded to the nitrogen atom of the maleimide group, such as "MIR-3000-70MT" (manufactured by Nippon Kayaku Co., Ltd.), "BMI-4000" (manufactured by Daiwa Kasei Co., Ltd.), and "BMI-80" (manufactured by Keiai Kasei Co., Ltd.);

[0082] The range of the amount of the maleimide-based resin in the resin composition layer is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, and is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of the nonvolatile components in the resin composition layer. The range of the amount of the maleimide-based resin in the resin composition based on 100% by mass of the nonvolatile components in the resin composition layer is preferably the same as the above-mentioned range of the amount of the maleimide-based resin in the resin composition layer based on 100% by mass of the nonvolatile components in the resin composition layer. When the amount of the maleimide-based resin in the resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range is within the above-mentioned range, the cutability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0083] The range of the amount of the maleimide-based resin in the resin composition layer is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, based on 100% by mass of the resin components in the resin composition layer. The range of the amount of the maleimide-based resin in the resin composition based on 100% by mass of the resin components in the resin composition layer is preferably the same as the above-mentioned range of the amount of the maleimide-based resin in the resin composition layer based on 100% by mass of the resin components in the resin composition layer. When the amount of the maleimide-based resin in the resin sheet having the specific parameter "P(a)×P(b) / P(c)" in the above-mentioned range is within the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0084] As the carbodiimide resin, a compound having one or more, preferably two or more, carbodiimide groups (-N=C=N-) in one molecule can be used. The carbodiimide resin can react with the (A) epoxy resin to form a bond. In addition, the carbodiimide resin can also react with a hydroxyl group (phenolic hydroxyl group) bonded to an aromatic ring, and can also bond with a phenolic resin. When a carbodiimide resin is used, the cuttability and peelability can be improved, while effectively suppressing warping of a member such as a semiconductor chip package having a cured layer formed using a resin sheet.

[0085] Specific examples of carbodiimide resins include aliphatic biscarbodiimides such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide); poly(phenylenecarbodiimide), poly(naphthalenecarbodiimide), and the like. Examples of polycarbodiimides include aromatic polycarbodiimides such as poly(methylenediphenylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide].

[0086] Commercially available carbodiimide resins include, for example, "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-05", "Carbodilite V-07", and "Carbodilite V-09" manufactured by Nisshinbo Chemical Inc.; and "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.

[0087] The range of the amount of the carbodiimide resin in the resin composition layer is preferably 0.1% by mass or more, more preferably 0.2% by mass or more, even more preferably 0.5% by mass or more, and preferably 10% by mass or less, more preferably 7% by mass or less, even more preferably 4% by mass or less, and particularly preferably 2% by mass or less, based on 100% by mass of the nonvolatile components in the resin composition layer. The range of the amount of the carbodiimide resin in the resin composition based on 100% by mass of the nonvolatile components in the resin composition layer is preferably the same as the above-mentioned range of the amount of the carbodiimide resin in the resin composition layer based on 100% by mass of the nonvolatile components in the resin composition layer. When the amount of the carbodiimide resin in the resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range is within the above-mentioned range, the cutability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0088] The range of the amount of the carbodiimide resin in the resin composition layer is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less, and particularly preferably 12% by mass or less, based on 100% by mass of the resin components in the resin composition layer. The range of the amount of the carbodiimide resin in the resin composition based on 100% by mass of the resin components in the resin composition layer is preferably the same as the above-mentioned range of the amount of the carbodiimide resin in the resin composition layer based on 100% by mass of the resin components in the resin composition layer. When the amount of the carbodiimide resin in the resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range is within the above-mentioned range, the cutability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0089] As the active ester resin, a compound having one or more active ester groups in one molecule can be used. Among them, as the active ester resin, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferable. The active ester resin is preferably obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester resin obtained from a carboxylic acid compound and a hydroxy compound is preferable, and an active ester resin obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferable. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0090] Preferred specific examples of the active ester resin include active ester resins containing a dicyclopentadiene-type diphenol structure, active ester resins containing a naphthalene structure, active ester resins containing an acetylated product of phenol novolac, and active ester resins containing a benzoylated product of phenol novolac. Among them, active ester resins containing a naphthalene structure and active ester resins containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.

[0091] Commercially available active ester resins include, for example, active ester resins containing a dicyclopentadiene-type diphenol structure such as "EXB9451", "EXB9460", "EXB9460S", "EXB-8000L", "EXB-8000L-65M", "EXB-8000L-65TM", "HPC-8000L-65TM", "HPC-8000", "HPC-8000-65T", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation); and active ester resins containing a naphthalene structure such as "HP-B-8151-62T", "EXB-8100L-65T", "EXB-8150-60T", and "EXB-815 Examples of such active ester resins include "EXB9401" (manufactured by DIC Corporation), which is a phosphorus-containing active ester resin; "DC808" (manufactured by Mitsubishi Chemical Corporation), which is an acetylated product of phenol novolac; "YLH1026", "YLH1030", "YLH1048" (manufactured by Mitsubishi Chemical Corporation), which is a benzoylated product of phenol novolac; and "PC1300-02-65MA" (manufactured by Air Water Corporation), which is an active ester resin containing a styryl group and a naphthalene structure.

[0092] As the phenolic resin, a compound having one or more, preferably two or more, hydroxyl groups (phenolic hydroxyl groups) bonded to an aromatic ring such as a benzene ring or a naphthalene ring in one molecule can be used. From the viewpoint of heat resistance and water resistance, a phenolic resin having a novolac structure is preferred. From the viewpoint of adhesion, a nitrogen-containing phenolic resin is preferred, and a triazine skeleton-containing phenolic resin is more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion, a triazine skeleton-containing phenolic novolac resin is preferred.

[0093] Specific examples of phenol-based resins include "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-375", and "SN-395" manufactured by Nippon Steel Chemical & Material Co., Ltd.; and "LA-7052", "LA-7054", "LA-3018", "LA-3018-50P", "LA-1356", "TD2090", and "TD-2090-60M" manufactured by DIC Corporation.

[0094] The amine resin may be a compound having one or more, preferably two or more, amino groups in one molecule. Examples of the amine resin include aliphatic amines, polyether amines, alicyclic amines, and aromatic amines. Among them, aromatic amines are preferred. The amine resin is preferably a primary amine or secondary amine, and more preferably a primary amine. Specific examples of amine resins include 4,4'-methylenebis(2,6-dimethylaniline), diphenyldiaminosulfone, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)-2,2'-diphenylpropanediamine, 2,2' ... phenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, and the like. Commercially available amine-based resins may be used, and examples thereof include "SEIKACURE-S" manufactured by Seika Corporation; "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd.; and "Epicure W" manufactured by Mitsubishi Chemical Corporation.

[0095] As the acid anhydride resin, a compound having one or more, preferably two or more, acid anhydride groups in one molecule can be used. Specific examples of the acid anhydride resin include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic dianhydride, and the like. Examples of acid anhydrides include anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid. Commercially available acid anhydride resins include, for example, "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by New Japan Chemical Co., Ltd.; "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation; "HN-2200" and "HN-5500" manufactured by Hitachi Chemical Co., Ltd.; and "EF-30", "EF-40", "EF-60", and "EF-80" manufactured by Clay Valley Corporation.

[0096] As the cyanate ester resin, a compound having one or more, preferably two or more, cyanate groups in one molecule can be used. Examples of cyanate ester resins include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester resins include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.

[0097] Specific examples of benzoxazine resins include "JBZ-OD100", "JBZ-OP100D", and "ODA-BOZ" manufactured by JFE Chemical Corporation; "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.; and "HFB2006M" manufactured by Showa Polymer Co., Ltd.

[0098] Specific examples of thiol-based resins include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.

[0099] The active group equivalent of the (D) curing agent is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The active group equivalent represents the mass of the resin per equivalent of the active group.

[0100] In one example, the weight average molecular weight (Mw) of the (D) curing agent may be 100 or more and 5,000 or less.

[0101] When the number of epoxy groups in the (A) epoxy resin is 1, the range of the number of active groups in the (D) curing agent is preferably 0.01 or more, more preferably 0.1 or more, even more preferably 0.2 or more, and preferably 10 or less, more preferably 5 or less, and even more preferably 3 or less. In the resin composition layer or resin composition, the "number of epoxy groups in the (A) epoxy resin" refers to the total value obtained by dividing the mass of the non-volatile component of the (A) epoxy resin present in the resin composition layer or resin composition by the epoxy equivalent. In addition, in the resin composition layer or resin composition, the "number of active groups in the (D) curing agent" refers to the total value obtained by dividing the mass of the non-volatile component of the (D) curing agent present in the resin composition layer or resin composition by the active group equivalent. In a resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range, when the number of active groups of the (D) curing agent is in the above-mentioned range, the cuttability and peelability can be particularly good, and further, warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0102] The range of the amount of the (D) curing agent in the resin composition layer is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, based on 100% by mass of the non-volatile components of the resin composition layer. The range of the amount of the (D) curing agent in the resin composition based on 100% by mass of the non-volatile components of the resin composition layer is preferably the same as the above-mentioned range of the amount of the (D) curing agent in the resin composition layer based on 100% by mass of the non-volatile components of the resin composition layer. When the amount of the (D) curing agent is within the above-mentioned range in a resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0103] The range of the amount of the (D) curing agent in the resin composition layer is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 60% by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, based on 100% by mass of the resin components in the resin composition. The range of the amount of the (D) curing agent in the resin composition based on 100% by mass of the resin components in the resin composition is preferably the same as the above-mentioned range of the amount of the (D) curing agent in the resin composition layer based on 100% by mass of the resin components in the resin composition layer. When the amount of the (D) curing agent is within the above-mentioned range in a resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0104] ((E) Curing Accelerator) The resin composition layer and the resin composition according to the present embodiment may contain a curing accelerator (E) as an optional component. The curing accelerator (E) as the component (E) does not include those corresponding to the above-mentioned components (A) to (D). The curing accelerator (E) functions as a curing catalyst that accelerates the curing of the epoxy resin (A).

[0105] Examples of the (E) curing accelerator include phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, metal-based curing accelerators, and amine-based curing accelerators. Among these, imidazole-based curing accelerators are preferred. The (E) curing accelerators may be used alone or in combination of two or more.

[0106] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutyl phosphonium bromide, tetrabutyl phosphonium chloride, tetrabutyl phosphonium acetate, tetrabutyl phosphonium decanoate, tetrabutyl phosphonium laurate, bis(tetrabutyl phosphonium)pyromellitate, tetrabutyl phosphonium hydrogenhexahydrophthalate, tetrabutyl phosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butyldimethylphosphonium tetraphenylborate; methyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium bromide, propyl triphenyl phosphonium bromide, butyl triphenyl phosphonium bromide, benzyl triphenyl phosphonium chloride, tetraphenyl phosphonium bromide, p-tolyl triphenyl phosphonium tetra-p-tolylborate, tetraphenyl phosphonium bromide, and the like. aromatic phosphonium salts such as tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine Examples of aromatic phosphines include tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.

[0107] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. aromatic dimethylureas such as butylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bisdimethylurea].

[0108] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.

[0109] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct , 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline, and other imidazole compounds and adducts of imidazole compounds and epoxy resins. Commercially available imidazole curing accelerators include, for example, "1B2PZ", "2E4MZ", "2MZA-PW", "2MZ-OK", "2MA-OK", "2MA-OK-PW", "2PHZ", "2PHZ-PW", "Cl1Z", "Cl1Z-CN", "Cl1Z-CNS", and "C11Z-A" manufactured by Shikoku Chemical Industry Co., Ltd.; and "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0110] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0111] Examples of the amine-based curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)-undecene, etc. Commercially available amine-based curing accelerators may be used, such as "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0112] The range of the amount of the (E) curing accelerator in the resin composition layer is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.03% by mass or more, and is preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0.1% by mass or less, based on 100% by mass of the non-volatile components of the resin composition layer. The range of the amount of the (E) curing accelerator in the resin composition based on 100% by mass of the non-volatile components of the resin composition layer is preferably the same as the above-mentioned range of the amount of the (E) curing accelerator in the resin composition layer based on 100% by mass of the non-volatile components of the resin composition layer. When the amount of the (E) curing accelerator is within the above-mentioned range in a resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0113] The range of the amount of the (E) curing accelerator in the resin composition layer is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, even more preferably 0.1% by mass or more, and preferably 5% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less, based on 100% by mass of the resin components in the resin composition layer. The range of the amount of the (E) curing accelerator in the resin composition based on 100% by mass of the resin components in the resin composition is preferably the same as the above-mentioned range of the amount of the (E) curing accelerator in the resin composition layer based on 100% by mass of the resin components in the resin composition layer. When the amount of the (E) curing accelerator is within the above-mentioned range in a resin sheet having the specific parameter "P(a) x P(b) / P(c)" in the above-mentioned range, the cuttability and peelability can be particularly good, and further, the warping of a member such as a semiconductor chip package having a cured material layer formed using the resin sheet can be effectively suppressed.

[0114] ((F) Optional Additives) The resin composition layer and the resin composition according to the present embodiment may further contain an optional additive (F) as an optional non-volatile component in combination with the above-mentioned components (A) to (E). Examples of the optional additive (F) include organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds; leveling agents such as silicone-based leveling agents and acrylic polymer-based leveling agents; thickeners such as bentone and montmorillonite; defoamers such as silicone-based defoamers, acrylic defoamers, fluorine-based defoamers, and vinyl resin-based defoamers; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion improvers such as urea silane; adhesion imparters such as triazole-based adhesion imparters, tetrazole-based adhesion imparters, and triazine-based adhesion imparters; antioxidants such as hindered phenol-based antioxidants; fluorescent brighteners such as stilbene derivatives; fluorine-based anti-oxidants; surfactants such as phosphate-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers. (F) Optional additives may be used alone or in combination of two or more.

[0115] ((G) Solvent) The resin composition layer and the resin composition according to the present embodiment usually contain a volatile component (G) solvent in combination with the non-volatile components such as the above-mentioned components (A) to (F). The amount of the (G) solvent as the (G) component can be reflected in the mass reduction rate P(a) in the specific parameter "P(a) x P(b) / P(c)". For example, the resin composition layer may be manufactured by forming a film of a liquid resin varnish containing an epoxy resin (A), an inorganic filler (B) and a (G) solvent, and drying it. Although most of the (G) solvent is removed by drying, a part of the (G) solvent may remain in the resin composition layer. When the specific parameter "P(a) x P(b) / P(c)" including the mass reduction rate P(a) reflecting the amount of the remaining (G) solvent is in a range that satisfies the formula (1), both the cuttability and the peelability can be improved.

[0116] As the (G) solvent, an organic solvent is usually used. Specific examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, and anisole; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate. Examples of the solvent include ether ester solvents such as ethyl acetate, ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate, ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butylcarbitol), amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, sulfoxide solvents such as dimethyl sulfoxide, nitrile solvents such as acetonitrile and propionitrile, aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The (G) solvent may be used alone or in combination of two or more.

[0117] From the viewpoint of keeping the mass reduction rate P(a) within an appropriate range, the (G) solvent has a preferred boiling point range. In particular, from the viewpoint of suppressing excessive volatilization of the (G) solvent from the resin composition layer to increase the mass reduction rate P(a), the boiling point of the (G) solvent is preferably high. On the other hand, from the viewpoint of shortening the drying time of the resin varnish in the manufacturing process of the resin sheet and suppressing the residue of the (G) solvent after curing of the resin composition layer, the boiling point of the (G) solvent is preferably low. The specific boiling point range of the (G) solvent may be influenced by the combination of the (G) solvents used, but is preferably 30°C or higher, more preferably 40°C or higher, even more preferably 50°C or higher, and preferably 280°C or lower, more preferably 260°C or lower, and particularly preferably 240°C or lower. The boiling point can be measured as the boiling point at 1 atmospheric pressure by the ebullient method or the distillation method.

[0118] The amount of the (G) solvent can be set so that the specific parameter "P(a) x P(b) / P(c)" falls within a range that satisfies formula (1). In one example, the specific range of the amount of the (G) solvent relative to 100% by mass of the resin composition layer can be the same as the range of the mass reduction rate P(a). In another example, the specific range of the amount of the (G) solvent relative to 100% by mass of the resin composition can be the same as the range of the mass reduction rate P(a).

[0119] [Thickness of resin composition layer] The thickness of the resin composition layer can be set according to its application. The specific range of the thickness of the resin composition layer is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and is preferably 150 μm or less, more preferably 120 μm or less, and particularly preferably 100 μm or less.

[0120] [Film layer] The resin sheet according to the present embodiment may further include any layer in combination with the resin composition layer. For example, the resin sheet may include a film layer in contact with the resin composition layer. Usually, the resin composition layer and the film layer are in direct contact. The resin composition layer and the film layer being in "direct" contact means that there is no other layer between the resin composition layer and the film layer, unless otherwise specified.

[0121] FIG. 1 is a cross-sectional view showing a resin sheet according to one embodiment of the present invention. As shown in FIG. 1, a resin sheet 100 according to one embodiment of the present invention may include film layers 120 and 130 in combination with a resin composition layer 110. These film layers 120 and 130 may be provided, for example, to support and protect the resin composition layer 110. Hereinafter, the film layer 120 provided on one side of the resin composition layer 110 may be referred to as a "first film layer" 120, and the film layer 130 provided on the other side of the resin composition layer 110 may be referred to as a "second film layer" 130.

[0122] Examples of the first film layer 120 include a film made of a plastic material, a metal foil, and a release paper, with a film made of a plastic material and a metal foil being preferred.

[0123] When a film made of a plastic material is used as the first film layer 120, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"); polycarbonate (hereinafter sometimes abbreviated as "PC"); acrylic polymers such as polymethyl methacrylate (hereinafter sometimes abbreviated as "PMMA"); polyolefins such as polypropylene; cyclic polyolefins; triacetyl cellulose (hereinafter sometimes abbreviated as "TAC"); polyether sulfide (hereinafter sometimes abbreviated as "PES"); polyether ketone; polyimide; and the like. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0124] When a metal foil is used as the first film layer 120, examples of the metal foil include copper foil and aluminum foil. Among them, copper foil is preferable. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0125] The surface of the first film layer 120 that is to be bonded to the resin composition layer 110 may be subjected to a matte treatment, a corona treatment, an antistatic treatment, or the like.

[0126] As the first film layer 120, a film layer with a release layer (not shown) may be used, which has a release layer on the surface to be bonded to the resin composition layer 110. Examples of the release agent used in the release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. Examples of commercially available release agents include alkyd resin-based release agents such as "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation. Examples of film layers with a release layer include "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited.

[0127] The thickness range of the first film layer 120 is preferably 5 μm or more, more preferably 10 μm or more, and is preferably 75 μm or less, more preferably 60 μm or less. When a film layer with a release layer is used, it is preferable that the thickness of the entire film layer with the release layer is in the above range.

[0128] The second film layer 130 may be, for example, the same film layer as the first film layer 120. The second film layer 130 may be thinner than the first film layer 120, and the thickness of the second film layer 130 may be in the range of 1 μm to 40 μm, for example. When the first film layer 120 and the second film layer 130 are used in combination, one of the first film layer 120 and the second film layer 130 may function as a support for supporting the resin composition layer 110, and the other may function as a cover film layer for protecting the resin composition layer 110.

[0129] [Shape of resin sheet] There is no limitation on the shape of the resin sheet according to this embodiment. The resin sheet may have, for example, a sheet shape or a long shape. Unless otherwise specified, the "long" shape refers to a film or sheet shape having a length of 10 times or more than the width. The length is preferably 20 times or more than the width, and specifically, may be a length that can be wound into a roll and stored or transported. There is no particular limit on the upper limit of the length, and it may be, for example, 100,000 times or less than the width.

[0130] [Manufacturing method of resin sheet] The resin sheet can be manufactured, for example, by a manufacturing method including a step of preparing a resin composition and a step of applying the resin composition to a suitable support surface. In this case, the surface of a film layer can be used as the support surface. Among them, a manufacturing method including a step of dissolving the resin composition in a (G) solvent to prepare a liquid resin varnish and a step of applying the resin varnish to a support surface is preferred. By using the (G) solvent, the viscosity can be adjusted to improve the applicability. When a resin varnish is used, the resin varnish is usually dried after application to form a resin composition layer.

[0131] The resin composition can be produced, for example, by mixing the above-mentioned components. The above-mentioned components may be mixed partially or entirely at the same time, or may be mixed in sequence. In the process of mixing each component, the temperature may be appropriately set, and thus heating and / or cooling may be performed temporarily or throughout. In addition, stirring or shaking may be performed in the process of mixing each component.

[0132] The resin composition and the resin varnish can be applied using a coating device such as a die coater.

[0133] Drying may be performed by heating, blowing hot air, or the like. Drying conditions are preferably set so as to obtain a specific parameter "P(a) x P(b) / P(c)" that satisfies formula (1). For example, when using a resin varnish containing 30% by mass to 60% by mass of an organic solvent, a desired resin composition layer can often be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0134] The method for producing a resin sheet may include a step of laminating a resin composition layer and a film layer after obtaining the resin composition layer. For example, the method for producing a resin sheet may include a step of forming a resin composition layer on a surface of a first film layer, and a step of laminating the formed resin composition layer and a second film layer.

[0135] [Characteristics of resin sheet] The resin sheet according to the present embodiment can have excellent cuttability. Therefore, when cutting the resin composition layer of the resin sheet, chipping of the resin composition layer can be suppressed. In one example, when a cuttability evaluation test is performed to punch out the resin sheet using a 10 cm square cutter to obtain a sample sheet having a square planar shape, chipping at the corners of the resin composition layer of the sample sheet can be reduced. Specifically, of the four corners of the sample sheet, chipping of the resin composition layer can be eliminated, preferably at one or more corners, and more preferably at all four corners. The cuttability evaluation test can be specifically performed by a method described in the examples described later.

[0136] The resin sheet according to the present embodiment can have excellent peelability. Therefore, when the resin sheet has a film layer, the adhesive strength of the resin composition layer and the film layer can be suppressed, and the film layer can be peeled off smoothly. In one example, a peelability evaluation test is performed in which the resin sheet having the resin composition layer and the film layer is laminated with a substrate, and then the film layer is peeled off in the vertical direction at a speed of 50 mm / min. When this peelability evaluation test is performed, the magnitude of the force (load) required to peel off the film layer can be preferably 0.09 kgf / cm or less, more preferably 0.06 kgf / cm or less. Specifically, the peelability evaluation test can be performed by a method described in the examples described later.

[0137] A cured layer is obtained by curing the resin composition layer of the resin sheet according to this embodiment. This cured layer usually contains the cured product of the above-mentioned resin composition, and preferably contains only the cured product of the above-mentioned resin composition. When the resin composition layer is cured, heat is usually applied to the resin composition layer. Therefore, among the components contained in the resin composition layer, volatile components such as (G) solvent can be volatilized by heat during curing, but non-volatile components such as components (A) to (F) do not volatilize by heat during curing. Therefore, the cured product of the resin composition can contain the non-volatile components of the resin composition or their reaction products.

[0138] The cured layer can be provided on members such as semiconductor chip packages and circuit boards. In this case, the cured layer obtained from the resin sheet according to this embodiment can usually suppress warping of the members. In one example, a warpage evaluation test is performed in which a cured layer having a thickness of 140 μm is formed on the entire surface of one side of a 12-inch silicon wafer (thickness 775 μm) using a resin sheet to produce a sample laminate. When this warpage evaluation test is performed, the amount of warpage of the sample laminate can be preferably 1.0 mm or less, more preferably 0.6 mm or less. Specifically, the warpage evaluation test can be performed by the method described in the examples below.

[0139] The cured layer obtained by curing the resin composition layer preferably has excellent dielectric properties. For example, the relative dielectric constant of the cured layer is preferably 4.0 or less, more preferably 3.6 or less, and particularly preferably 3.4 or less. The lower limit of the relative dielectric constant is not particularly limited, and may be, for example, 1.5 or more, 2.0 or more, etc. Also, for example, the dielectric tangent of the cured layer is preferably 0.0100 or less, more preferably 0.0090 or less, even more preferably 0.0080 or less, and particularly preferably 0.0070 or less. The lower limit of the dielectric tangent is not particularly limited, and may be, for example, 0.0010 or more. In one example, the relative dielectric constant and dielectric tangent of the cured layer can be measured under the conditions of a measurement frequency of 5.8 GHz and a measurement temperature of 23 ° C. by a cavity resonance perturbation method using an Agilent Technologies "HP8362B" using a cured layer obtained by heating the resin composition layer at 190 ° C. for 90 minutes.

[0140] The above-mentioned resin sheet can be used, for example, as a resin sheet for forming an encapsulating layer. In this case, the resin composition layer can be suitably used as a resin composition layer for an encapsulating layer. Among them, the resin composition layer of the resin sheet is preferably used as a resin composition layer for encapsulating a semiconductor (a resin composition layer for semiconductor encapsulation), and more preferably used as a resin composition layer for encapsulating a semiconductor chip (a resin composition layer for semiconductor chip encapsulation).

[0141] The resin sheet may also be used for purposes other than forming an encapsulating layer, for example, as a resin sheet for forming an insulating layer. In this case, the resin composition layer can be suitably used as a resin composition layer for forming an insulating layer of a semiconductor chip package (a resin composition layer for forming an insulating layer of a semiconductor chip package) and a resin composition layer for forming an insulating layer of a circuit board (including a printed wiring board) (a resin composition layer for forming an insulating layer of a circuit board). The insulating layer may include an interlayer insulating layer and a rewiring formation layer.

[0142] Examples of semiconductor chip packages include FC-CSP, MIS-BGA package, ETS-BGA package, Fan-out type WLP (Wafer Level Package), Fan-in type WLP, Fan-out type PLP (Panel Level Package), and Fan-in type PLP.

[0143] Furthermore, the resin composition layer of the resin sheet can be used in a wide range of applications in which a resin composition layer is used, such as a solder resist, a die bonding material, a hole filling resin, and a component embedding resin.

[0144] <Method of manufacturing semiconductor chip package> The above-mentioned resin sheet can be used to manufacture a semiconductor chip package. A step (I) of cutting the resin composition layer of the resin sheet; A step (II) of laminating a resin sheet having a cut resin composition layer and a substrate; A step (III) of curing the resin composition layer; Includes.

[0145] (Step (I): Cutting step of resin composition layer) The method for producing a semiconductor chip package according to this embodiment includes a step (I) of cutting the resin composition layer of the resin sheet.

[0146] The step (I) preferably includes pressing a blade against the resin composition layer in the thickness direction to cut the resin composition layer. In one example, the resin composition layer may be cut using a die cutter equipped with a cylindrical roll rotatably provided in the circumferential direction and a blade provided on the circumferential surface of the roll. When using a die cutter, the resin sheet is conveyed in the same direction as the rotation direction of the die cutter while rotating the die cutter in the circumferential direction so as to contact the blade of the die cutter. The blade of the die cutter can press the resin composition layer of the conveyed resin sheet in the thickness direction, enter into the resin composition layer, and cut so as to punch out the resin composition layer. In another example, the resin composition layer may be cut using a punching blade having a desired planar shape as viewed from the thickness direction of the resin composition layer. When a punching blade is used, the resin composition layer can be pressed in the thickness direction with the punching blade and cut so as to punch out the resin composition layer. As shown in these examples, the above-mentioned resin sheet can effectively suppress chipping of the resin composition layer when the resin composition layer is cut so as to be punched out by a blade.

[0147] FIG. 2 is a cross-sectional view showing the resin sheet 100 after cutting the resin composition layer 110 in the manufacturing method of a semiconductor chip package according to one embodiment of the present invention. As shown in FIG. 2, the resin composition layer 110 having a planar shape corresponding to the shape of the blade can be obtained by the above-mentioned cutting. Hereinafter, among the cut parts of the resin composition layer 110, the part laminated with the substrate (not shown) may be referred to as the "effective resin composition layer" 111, and the other parts may be referred to as the "peripheral resin composition layer" 112. When the above-mentioned resin sheet 100 is used, it is possible to suppress the generation of chips in the resin composition layer 110 by cutting. Therefore, it is possible to obtain the effective resin composition layer 111 having the intended shape with high certainty.

[0148] 2 shows an example in which the resin composition layer 110 is entirely cut in the thickness direction, the resin composition layer 110 may be partially cut in the thickness direction. When at least a portion of the resin composition layer 110 in the thickness direction is cut to form an incision in at least a portion of the resin composition layer 110 in the thickness direction, the peripheral resin composition layer 112 can be smoothly removed in step (V) described later.

[0149] When the resin sheet 100 has a film layer, the film layer may be cut in step (I). For example, when the second film layer 130 is between the resin composition layer 110 and a blade (not shown), not only the resin composition layer 110 but also the second film layer 130 is usually cut in step (I). At this time, the second film layer 130 may be cut in its entirety in the thickness direction. Hereinafter, as shown in FIG. 2, among the cut parts of the second film layer 130, the part covering the effective resin composition layer 111 may be referred to as a "main part" 131, and the other parts may be referred to as a "peripheral part" 132.

[0150] In step (I), the film layer does not have to be cut. For example, when a first film layer 120 is provided on the side opposite to the blade (not shown) with respect to the resin composition layer 110, the first film layer 120 does not have to be cut. As shown in FIG. 2, the blade may partially enter the first film 120 and partially cut the first film layer 120 in the thickness direction.

[0151] Here, an example is shown in which a long resin sheet 100 having a second film layer 130, a resin composition layer 110, and a first film layer 120 in this order from the blade side is used. In this case, the resin composition layer 110 and the second film layer 130 are preferably cut. The first film layer 120 may not be cut, and may be partially cut in the thickness direction. However, the operation in step (I) is not limited to that shown in this example. For example, the resin composition layer 110 of a resin sheet not having the second film layer 130 may be cut by performing step (I) after the second film layer 130 is peeled off in step (IV) described later.

[0152] The effective resin composition layer 111 obtained by cutting the resin composition layer 110 in step (I) usually has a planar shape corresponding to the substrate (not shown) to be laminated with the effective resin composition layer 111. For example, the effective resin composition layer 111 may have the same planar shape as the substrate, may have a planar shape larger than the substrate, or may have a planar shape smaller than the substrate. As a specific example, when a wafer having a circular planar shape is used as the substrate, the resin composition layer 110 may be cut so as to obtain the effective resin composition layer 111 having a circular planar shape.

[0153] (Step (IV): Film Layer Peeling Step) The method for producing a semiconductor chip package according to this embodiment may include a step (IV) of peeling off a film layer before the step (II). For example, a method for producing a semiconductor chip package using a resin sheet having a first film layer and a second film layer usually includes a step (IV) of peeling off one or both of the first resin sheet and the second film layer before the step (II). From the viewpoint of supporting and protecting the effective resin composition layer during transportation, it is preferable that the step (IV) peels off only one of the first resin sheet and the second film layer.

[0154] The step (IV) of peeling off the film layer may be performed before or after the step (I). By cutting the resin composition layer while supporting the resin composition layer with the film layer, chipping of the resin composition layer can be effectively suppressed, so that the step (IV) of peeling off the film layer is preferably performed after the step (I).

[0155] An example of a method for peeling off the first film layer is a method in which, while the second film layer and the resin composition layer are adsorbed by a vacuum adsorption machine, the first film layer is pulled away from the resin composition layer to peel it off.

[0156] On the other hand, a method for peeling off the second film layer can be, for example, a method in which the first film layer and the resin composition layer are adsorbed by a vacuum adsorption machine, and the second film layer is pulled away from the resin composition layer to peel it off.

[0157] In addition, as shown in the example of Fig. 2, when the second film layer is cut in step (I), the second film layer after cutting includes a main portion covering the effective resin composition layer and a peripheral portion covering the peripheral resin composition layer. Therefore, when step (IV) is performed after step (I), step (IV) may include peeling off the main portion of the second film layer, or may include peeling off the peripheral portion of the second film layer. The peeling off of the main portion and the peripheral portion of the second film layer may be performed simultaneously or sequentially.

[0158] The peeling method of the main part of the second film layer can be, for example, an adhesive tape method, a vacuum suction method, etc. For example, in the adhesive tape method, an adhesive tape is generally attached to the main part of the second film layer, and then the adhesive tape is peeled off. At this time, the main part of the second film layer can be peeled off together with the peeled adhesive tape.

[0159] The peripheral portion of the second film layer can be peeled off by, for example, the adhesive tape method, the vacuum suction method, etc., as in the case of the main portion. In addition, when a long resin sheet is used, the peripheral portion of the second film layer can be formed continuously in the conveying direction of the resin sheet. Therefore, the peripheral portion of the second film layer can be peeled off by mechanically pulling the peripheral portion. For example, the peripheral portion of the second film layer can be peeled off continuously by pulling the peripheral portion of the second film layer away from the resin composition layer.

[0160] When the above-mentioned resin sheet is used, since the adhesive strength between the resin composition layer and the film layer is low, the film layer can be smoothly separated from the resin composition layer. Therefore, the effective resin composition layer is prevented from being partially or entirely fixed to the film layer. Therefore, the occurrence of a defect in which the effective resin composition layer is partially or entirely peeled off together with the film layer is prevented, and the film layer can be smoothly peeled off.

[0161] (Step (V): Peeling off peripheral resin composition layer) The method for producing a semiconductor chip package according to this embodiment may include a step (V) of peeling off the peripheral resin composition layer. The method for producing a semiconductor chip package usually includes a step (V) of peeling off the peripheral resin composition layer after the step (I).

[0162] The peripheral resin composition layer may be peeled off after step (IV) or may be peeled off simultaneously with a part or the whole of step (IV). For example, the peripheral resin composition layer may be peeled off simultaneously with peeling off the first film layer in step (IV). As a specific example, the first film layer and the peripheral resin composition layer may be peeled off by pulling them away from the effective resin composition layer while the main part of the second film layer and the effective resin composition layer are adsorbed by a vacuum adsorption machine.

[0163] Also, for example, the peripheral resin composition layer may be peeled off at the same time as peeling off the peripheral portion of the second film layer in step (IV). As a specific example, the peripheral portion of the second film layer and the peripheral resin composition layer may be pulled away from the effective resin composition layer to peel off the peripheral portion of the second film layer and the peripheral resin composition layer.

[0164] Furthermore, for example, the peripheral resin composition layer may be peeled off separately from the peeling of the peripheral portions of the first film layer and the second film layer.

[0165] When the above-mentioned resin sheet is used, since the adhesive strength between the resin composition layer and the film layer is low, the peripheral resin composition layer can be smoothly separated from the film layer. Therefore, the peripheral resin composition layer is prevented from being partially or entirely fixed to the film layer. Therefore, the peripheral resin composition layer can be smoothly peeled off.

[0166] (Step (II): Lamination step) The method for manufacturing a semiconductor chip package according to the present embodiment includes a step (II) of laminating a resin sheet having an effective resin composition layer as a cut resin composition layer with a substrate. This lamination is performed so that the effective resin composition layer of the resin sheet and the substrate are bonded. This lamination can form an effective resin composition layer on the substrate.

[0167] The substrate preferably includes, for example, a substrate or a wafer. Examples of the substrate include a glass substrate; a metal substrate such as copper, titanium, stainless steel, or cold-rolled steel plate (SPCC); a substrate such as an FR-4 substrate in which glass fibers are impregnated with epoxy resin or the like and then heat-cured; a substrate made of bismaleimide triazine resin such as BT resin; and a polyimide substrate. Examples of the wafer include a semiconductor wafer such as a silicon wafer, a gallium arsenide (GaAs) wafer, an indium phosphide (InP) wafer, a gallium phosphide (GaP) wafer, a gallium nitride (GaN) wafer, a gallium telluride (GaTe) wafer, a zinc selenium (ZnSe) wafer, or a silicon carbide (SiC) wafer; a glass wafer; or a pseudo wafer. Examples of the pseudo wafer include, for example, a plate-shaped member having a molded resin and electronic components embedded in the molded resin.

[0168] The substrate or wafer itself may be used as the substrate. Alternatively, the substrate or wafer may be combined with any member and used as the substrate. For example, a composite member having a temporary fixing film formed on the substrate or wafer may be used as the substrate. When a composite member having a temporary fixing film is used as the substrate, the substrate can be easily peeled off in a later step. The temporary fixing film is preferably a film that can be peeled off from the semiconductor chip and can temporarily fix the semiconductor chip. An example of a commercially available temporary fixing film is "Riva Alpha" manufactured by Nitto Denko Corporation.

[0169] A semiconductor chip may be provided on the substrate. For example, when the substrate is provided with a temporary fixing film, the semiconductor chip may be temporarily fixed on the temporary fixing film. The temporary fixing of the semiconductor chip may be performed using, for example, a device such as a flip chip bonder or a die bonder. The layout and number of the semiconductor chips may be appropriately set according to the shape and size of the temporary fixing film, the number of semiconductor chip packages to be produced, and the like. For example, the semiconductor chips may be temporarily fixed by arranging them in a matrix shape of multiple rows and multiple columns. When the semiconductor chip is provided on the substrate, lamination is usually performed so that the semiconductor chip is embedded in the effective resin composition layer.

[0170] The resin sheet and the substrate can be laminated, for example, by thermocompression bonding the resin sheet to the substrate. Examples of the member for thermocompression bonding the resin sheet to the substrate (hereinafter sometimes referred to as "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (such as a SUS roll). It is preferable to press the thermocompression bonding member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the substrate.

[0171] The substrate and the resin sheet may be laminated, for example, by a vacuum lamination method. The lamination conditions may be, for example, as follows. The heat-pressure bonding temperature is preferably in the range of 60°C to 160°C, more preferably 80°C to 140°C. The heat-pressure bonding pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably 0.29MPa to 1.47MPa. The heat-pressure bonding time is preferably in the range of 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. The lamination is preferably carried out under reduced pressure conditions of 13hPa or less.

[0172] The lamination can be carried out by a commercially available vacuum laminator. Examples of commercially available vacuum laminators include the vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., the vacuum applicator manufactured by Nikko Materials Co., Ltd., the batch type vacuum pressure laminator, and the fully automatic LC tape laminator manufactured by Lintec Co., Ltd. When using a wafer as the substrate, it is preferable to use a diaphragm type laminator in order to prevent the wafer from cracking.

[0173] (Process (VI): Smoothing process) The method for manufacturing a semiconductor chip package according to this embodiment may include a step (VI) of smoothing the effective resin composition layer after laminating the resin sheet and the substrate in the step (II) and before curing the effective resin composition layer in the step (III). Specifically, the effective resin composition layer may be smoothed by performing a smoothing treatment in which a thermocompression member is pressed against the resin sheet under normal pressure (atmospheric pressure). The pressing conditions for the smoothing treatment may be the same as the conditions for the thermocompression bonding in the above step (II). Moreover, the lamination in the step (II) and the smoothing treatment in the step (VI) may be performed consecutively using a vacuum laminator.

[0174] (Step (VII): Film Layer Peeling Step) When the resin sheet laminated to the substrate in step (II) includes a film layer, the method for manufacturing a semiconductor chip package according to this embodiment may include a step (VII) of peeling off the film layer after step (II). For example, when a resin sheet including a first film layer and a second film layer is used as in the example shown in FIG. 2, the resin sheet laminated to the substrate may include one of the first film layer and the second film layer in step (II). Thus, the method for manufacturing a semiconductor chip package may include a step (VII) including peeling off one of the first film layer and the second film layer. The step (VII) of peeling off the film layer may be performed before or after step (III).

[0175] The method for peeling off the film layer in step (VII) is not particularly limited, and may be the same as the method for peeling off the film layer in step (IV). When the above-mentioned resin sheet is used, the adhesive strength between the resin composition layer and the film layer is low, so that the occurrence of a defect in which a part or all of the resin composition layer peels off together with the film layer is suppressed, and the film layer can be peeled off smoothly.

[0176] (Process (III): hardening process) The method for producing a semiconductor chip package according to the present embodiment includes a step (II) of laminating a resin sheet and a substrate, and a step (III) of curing an effective resin composition layer as a resin composition layer laminated on the substrate. The effective resin composition layer is usually cured by thermal curing.

[0177] The thermal curing conditions for the effective resin composition layer may vary depending on the type of resin composition, but the curing temperature is usually in the range of 120°C to 240°C (preferably in the range of 150°C to 220°C, more preferably in the range of 170°C to 200°C), and the curing time is in the range of 5 minutes to 120 minutes (preferably in the range of 10 minutes to 100 minutes, more preferably in the range of 15 minutes to 90 minutes).

[0178] Before the effective resin composition layer is thermally cured, the effective resin composition layer may be subjected to a preliminary heating treatment in which the effective resin composition layer is heated at a temperature lower than the curing temperature. For example, prior to thermally curing the effective resin composition layer, the resin composition layer may be preheated at a temperature of usually 50°C or more and less than 120°C (preferably 60°C or more and 110°C or less, more preferably 70°C or more and 100°C or less) for usually 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes).

[0179] By curing the effective resin composition layer, a cured layer containing the cured product of the resin composition can be formed on the substrate. Thus, a semiconductor chip package having a cured layer can be obtained by the above-mentioned manufacturing method. Usually, the obtained semiconductor chip package contains a cured layer and a semiconductor chip. And, the semiconductor chip package manufactured using the above-mentioned resin sheet can usually suppress warpage.

[0180] In the semiconductor chip package, the cured layer can function as, for example, a sealing layer, an insulating layer, a solder resist layer, etc. In one example, when a semiconductor chip is provided on a substrate, a semiconductor chip package can be obtained that includes a semiconductor chip and a cured layer as a sealing layer that seals the semiconductor chip. Examples of such semiconductor chip packages include Fan-out type WLP, Fan-in type WLP, Fan-out type PLP, Fan-in type PLP, etc.

[0181] (Optional process) The method for manufacturing a semiconductor chip package according to this embodiment may further include any optional steps in combination with the steps described above.

[0182] For example, the method for manufacturing the semiconductor chip package described above includes the steps of: A step of temporarily fixing the semiconductor chip on the substrate; forming an encapsulation layer on the semiconductor chip; peeling off the substrate; A step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material has been peeled off; A process of forming a rewiring layer as a conductor layer on the rewiring formation layer. The method may be carried out as a production method including the steps of:

[0183] Also, for example, a method for manufacturing a semiconductor chip package includes: A process of forming a rewiring formation layer as an insulating layer on a substrate. A step of forming a rewiring layer as a conductor layer on the rewiring formation layer; A step of mounting a semiconductor chip on the rewiring formation layer so as to be electrically connected to the rewiring layer; forming an encapsulation layer on the semiconductor chip; The method may be carried out as a production method including the steps of:

[0184] In the manufacturing methods according to these examples, the above-mentioned cured layer can be preferably applied to the sealing layer and the rewiring formation layer. Therefore, the step of forming the sealing layer and the step of forming the rewiring formation layer may be performed by a method including the above-mentioned steps (I) to (III) and, if necessary, steps (IV) to (VII). In that case, the manufacturing method of the semiconductor chip package may further include any step required for making the above-mentioned cured layer function as the sealing layer or the rewiring formation layer. Furthermore, the manufacturing method of the semiconductor chip package may include any step other than the steps of forming the sealing layer and the rewiring formation layer. Hereinafter, these optional steps will be described.

[0185] The method for producing a semiconductor chip package may include, as an optional step, a step of forming holes such as via holes and through holes in the cured material layer. For example, when the cured material layer is used as an insulating layer such as a rewiring formation layer, a hole may be formed in the cured material layer for interlayer connection between a conductor layer provided on one side of the cured material layer and a conductor layer provided on the other side. Examples of the method for forming the hole include laser irradiation, etching, mechanical drilling, etc. In addition, the method for producing a semiconductor chip package preferably includes a desmear step of removing smears in the hole after the hole is formed.

[0186] The method for manufacturing a semiconductor chip package may include, as an optional step, a step of performing a roughening treatment on the cured material layer. The roughening treatment usually roughens the surface of the cured material layer, including the inside of the hole. Therefore, when the cured material layer is used as an insulating layer such as a rewiring formation layer, the roughening treatment can increase the adhesion strength between the cured material layer and the conductor layer. The roughening treatment may be either a dry or wet roughening treatment. An example of the dry roughening treatment is a plasma treatment. An example of the wet roughening treatment is a method in which a swelling treatment using a swelling liquid, a roughening treatment using an oxidizing agent, and a neutralization treatment using a neutralizing liquid are performed in this order.

[0187] The manufacturing method of the semiconductor chip package may include, as an optional step, a step of forming a conductor layer on the cured layer. The conductor layer may be used, for example, as wiring. As a specific example, when the cured layer is used as a rewiring formation layer, the conductor layer may be formed as a rewiring layer. The conductor material used for the conductor layer is not particularly limited. The conductor material contained in the conductor layer may be, for example, a material containing one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. As the conductor material, a single metal may be used, or an alloy may be used. As the alloy, for example, an alloy of two or more metals selected from the above group (for example, nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy) may be used. Among them, from the viewpoint of versatility, cost and ease of patterning of the conductor layer formation, chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper as a single metal; and an alloy of nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy as an alloy; are preferable. Among them, single metals such as chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper; and nickel-chromium alloys; are more preferable, and single metal copper is particularly preferable. The conductor layer may have a single-layer structure, or may have a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated.

[0188] Examples of the method for forming the conductor layer include plating, sputtering, and vapor deposition. For example, the surface of the cured layer may be plated by an appropriate method such as a semi-additive method or a full-additive method to form a conductor layer having a desired wiring pattern. The material of the conductor layer to be formed may be a single metal or an alloy. In addition, the conductor layer may have a single-layer structure including only one layer, or a multi-layer structure including two or more layers of different types of materials.

[0189] Here, an example of an embodiment in which a conductor layer is formed on a cured material layer will be described in detail. A plating seed layer is formed on the surface of the cured material layer by electroless plating. Then, a mask pattern is formed on the formed plating seed layer, exposing a part of the plating seed layer in accordance with a desired wiring pattern. After forming an electrolytic plating layer on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by a process such as etching, and a conductor layer having a desired wiring pattern can be formed.

[0190] Furthermore, the above-mentioned formation of the cured material layer and the formation of the conductor layer may be repeated to alternately stack the cured material layers and the conductor layers (build up).

[0191] The method for manufacturing a semiconductor chip package according to this embodiment may include, as an optional step, a step of polishing the cured material layer. In one example, the method for manufacturing a semiconductor chip package may include a step of polishing the surface of the cured material layer opposite to the substrate. In another example, when the substrate is peeled off as described below, the method for manufacturing a semiconductor chip package may include a step of polishing the surface of the cured material layer exposed by peeling off the substrate. The smoothness of the surface of the cured material layer can be improved by polishing. Examples of the polishing method include a chemical mechanical polishing method using a chemical mechanical polishing device, a mechanical polishing method such as a buff, and a surface grinding method using a rotating grinding wheel.

[0192] The method for producing a semiconductor chip package may include, as an optional step, a step of mounting a semiconductor chip on a cured material layer. As a specific example, the method for producing a semiconductor chip package may include a step of mounting a semiconductor chip on a cured material layer so as to be conductively connected to a conductor layer such as a rewiring layer formed on the cured material layer. This step usually includes bonding a semiconductor chip to the cured material layer so as to be conductively connected between a terminal electrode of the semiconductor chip and the conductor layer. Examples of the bonding method include a method of bonding the semiconductor chip and the cured material layer via an insulating adhesive, a method of pressing the semiconductor chip to the cured material layer, a method of bonding the semiconductor chip by reflow, and the like, but other methods may also be used.

[0193] The method for producing a semiconductor chip package according to this embodiment may include, for example, a step of peeling off the substrate as an optional step. As a specific example, when a substrate including a temporary fixing film is used, the substrate can be peeled off. Examples of a method for peeling off the substrate include a method of heating, foaming or expanding the temporary fixing film to peel it off. In the method of heating, foaming or expanding the temporary fixing film to peel it off, the heating conditions are usually 100° C. to 250° C. for 1 second to 90 seconds or 5 minutes to 15 minutes. In addition, examples of a method for peeling off the substrate include a method of irradiating the temporary fixing film with ultraviolet light through the substrate to reduce the adhesive strength of the temporary fixing film to peel it off. In the method of irradiating ultraviolet light to reduce the adhesive strength of the temporary fixing film to peel it off, the irradiation amount of ultraviolet light is usually 10 mJ / cm. 2 ~1000mJ / cm 2 It is.

[0194] The method for manufacturing a semiconductor chip package according to the present embodiment may include, as an optional step, a step of forming a solder resist layer on a conductor layer such as a rewiring layer. Any material having insulating properties may be used as the material for the solder resist layer. Among them, from the viewpoint of ease of manufacturing the semiconductor chip package, a photosensitive resin composition and a thermosetting resin composition are preferred. The solder resist layer may be formed by a cured layer obtained by curing the resin composition layer of the above-mentioned resin sheet.

[0195] The method for manufacturing the semiconductor chip package according to the present embodiment may include, as an optional step, a bumping process for forming bumps, which may be performed by a method such as solder balls or solder plating.

[0196] The method for manufacturing the semiconductor chip package according to this embodiment may include, as an optional step, for example, a step of dicing the semiconductor chip packages into individual pieces.

[0197] Here, a more specific example of the method for producing a semiconductor chip package will be described. In a specific example, a cured material layer is formed as a rewiring formation layer on a substrate by a method including the above-mentioned steps (I) to (III), and a conductor layer is formed as a rewiring layer on the cured material layer. Only one layer of each of the cured material layer and the conductor layer may be formed, or two or more layers may be formed for build-up. Thereafter, a semiconductor chip is mounted on the cured material layer, and a sealing layer is formed to seal the chip. The sealing layer may be produced using the above-mentioned resin sheet. Then, the substrate may be peeled off and diced as necessary to obtain a semiconductor chip package.

[0198] In another specific example, a semiconductor chip is provided on a substrate, and a cured layer is formed as a sealing layer on the substrate by a method including the above-mentioned steps (I) to (III). Then, the substrate is peeled off. A rewiring formation layer and a rewiring layer are formed on the surface exposed by peeling off the substrate. The rewiring formation layer may be formed using the above-mentioned resin sheet. Also, the rewiring formation layer and the rewiring layer may each be formed in one layer, or two or more layers may be formed for build-up. Then, dicing may be performed to obtain a semiconductor chip package.

[0199] In the production methods according to these specific examples, one or more of the above steps may be carried out in combination.

[0200] (Method of manufacturing a semiconductor chip package using a circuit board) The semiconductor chip package may be manufactured by a method including a step of manufacturing a circuit board by a method for manufacturing a circuit board described later, and a step of mounting a semiconductor chip on the circuit board. Since the method for manufacturing a circuit board described later includes steps (I), (II), and (III), the method including the method for manufacturing a circuit board can also manufacture a semiconductor chip package using the above-mentioned resin sheet. The obtained semiconductor chip package usually includes a cured layer and a semiconductor chip.

[0201] The process of mounting a semiconductor chip on a circuit board usually includes bonding the semiconductor chip to the circuit board so that the terminal electrodes of the semiconductor chip and the circuit wiring of the circuit board are conductively connected. The bonding conditions between the circuit board and the semiconductor chip can be, for example, the conditions used in flip-chip mounting of the semiconductor chip. Also, for example, the semiconductor chip and the circuit board may be bonded via an insulating adhesive.

[0202] An example of a bonding method is a method of bonding a semiconductor chip to a circuit board. The bonding conditions are that the bonding temperature is usually in the range of 120°C to 240°C (preferably in the range of 130°C to 200°C, more preferably in the range of 140°C to 180°C), and the bonding time is usually in the range of 1 second to 60 seconds (preferably in the range of 5 seconds to 30 seconds).

[0203] Another example of the bonding method is a method of bonding a semiconductor chip to a circuit board by reflow. The reflow conditions may be in the range of 120°C to 300°C.

[0204] After the semiconductor chip is bonded to the circuit board, the semiconductor chip may be filled with a molded underfill material.

[0205] <Manufacturing method of circuit board> A circuit board can be manufactured by using the above-mentioned resin sheet. A step (I) of cutting the resin composition layer of the resin sheet; A step (II) of laminating a resin sheet having a cut resin composition layer and a substrate; A step (III) of curing the resin composition layer; Includes.

[0206] In the method for producing a circuit board according to the present embodiment, the step (I) of cutting the resin composition layer of the resin sheet can be performed in the same manner as the step (I) of the method for producing a semiconductor chip package described above. According to the step (I) of the method for producing a circuit board according to the present embodiment, it is possible to obtain the same advantages as the step (I) of the method for producing a semiconductor chip package.

[0207] The method for producing a circuit board according to this embodiment may include a step (IV) of peeling off the film layer and a step (V) of peeling off the peripheral resin composition layer, similar to the method for producing a semiconductor chip package described above. The steps (IV) and (V) in the method for producing a circuit board may be performed in the same manner as the steps (IV) and (V) in the method for producing a semiconductor chip package described above. The steps (IV) and (V) in the method for producing a circuit board according to this embodiment can provide the same advantages as the steps (IV) and (V) in the method for producing a semiconductor chip package.

[0208] The method for manufacturing a circuit board according to the present embodiment includes a step (II) of laminating a resin sheet having an effective resin composition layer as a cut resin composition layer and a substrate. This lamination is performed so that the effective resin composition layer of the resin sheet and the substrate are bonded. This lamination allows the effective resin composition layer to be formed on the substrate.

[0209] Examples of the substrate include glass epoxy substrates, metal substrates, polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. The substrate may have a metal layer such as copper foil on the surface as a part of the substrate. For example, a substrate having peelable metal layers (first metal layer and second metal layer) on both surfaces may be used. When such a substrate is used, a conductor layer as a wiring layer that can function as circuit wiring is usually formed on the surface of the second metal layer opposite to the first metal layer. Examples of materials for the metal layer include copper foil, copper foil with carrier, and the above-mentioned materials for the conductor layer, and copper foil is preferred. Examples of substrates having a metal layer include "Micro Thin" ultra-thin copper foil with carrier manufactured by Mitsui Mining & Smelting Co., Ltd. The substrate may have a conductor layer on one or both sides, and this conductor layer may be patterned. When manufacturing a circuit board, an intermediate product on which an insulating layer and / or a conductor layer should be further formed is also included in the above-mentioned "substrate". When manufacturing a circuit board with built-in components as the circuit board, a substrate with built-in components may be used.

[0210] The resin sheet and the substrate can be laminated, for example, by heat-pressing the resin sheet to the substrate. The specific lamination method and conditions can be the same as those in step (II) of the above-mentioned method for producing a semiconductor chip package.

[0211] The method for producing a circuit board according to this embodiment may include a step (VI) of smoothing the effective resin composition layer and a step (VII) of peeling off the film layer, similar to the method for producing a semiconductor chip package described above. Steps (VI) and (VII) in the method for producing a circuit board may be performed in the same manner as steps (VI) and (VII) in the method for producing a semiconductor chip package described above. Steps (VI) and (VII) in the method for producing a circuit board according to this embodiment can provide the same advantages as steps (VI) and (VII) in the method for producing a semiconductor chip package.

[0212] The method for producing a circuit board according to this embodiment includes step (III) of curing the effective resin composition layer as the resin composition layer laminated on the substrate after laminating the resin sheet and the substrate in step (II). Step (III) of the method for producing a circuit board according to this embodiment can be performed in the same manner as step (III) of the method for producing a semiconductor chip package described above. By curing the effective resin composition layer, a cured layer containing a cured product of the resin composition can be formed on the substrate. Thus, a circuit board having a cured layer can be obtained by the above-mentioned production method. A circuit board produced using the above-mentioned resin sheet can usually be suppressed from warping.

[0213] In the circuit board, the cured material layer can function as, for example, an insulating layer, a sealing layer, a solder resist layer, or the like.

[0214] The method for manufacturing a circuit board according to this embodiment may further include any optional steps in combination with the steps described above.

[0215] The method for producing a circuit board may include, for example, a step of polishing the cured layer. The method for producing a circuit board may include, for example, a step of forming holes such as via holes and through holes in the cured layer. In addition, a desmearing step may be performed after the holes are formed. The method for producing a circuit board may include, for example, a step of performing a roughening treatment on the cured layer. The method for producing a circuit board may include, for example, a step of forming a conductor layer on the cured layer. These optional steps may be performed in the same manner as described in the method for producing a semiconductor chip package described above.

[0216] The method for producing a circuit board may include, for example, a step of peeling off the substrate. As a specific example, the step of peeling off the substrate can be carried out when a substrate having a peelable metal layer is used. When the substrate is removed, it is possible to produce a circuit board having a cured layer and a conductor layer embedded in the cured layer.

[0217] The method for manufacturing a circuit board may, for example, be to manufacture a circuit board having a multi-layer structure, such as a multi-layer printed wiring board, by repeatedly carrying out the above-mentioned steps.

[0218] In the method for manufacturing the circuit board, the same steps as those described in the method for manufacturing the semiconductor chip package may be performed.

[0219] <Semiconductor device> The semiconductor device includes the above-mentioned semiconductor chip package or circuit board. Examples of the semiconductor device include various semiconductor devices used in electrical products (e.g., computers, mobile phones, smartphones, tablet devices, wearable devices, digital cameras, medical devices, televisions, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, aircraft, etc.). EXAMPLES

[0220] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the following description, the terms "parts" and "%" used to express amounts refer to "parts by mass" and "% by mass", respectively, unless otherwise specified. Furthermore, the operations described below were carried out in the atmosphere at room temperature and normal pressure (25°C and 1 atm) unless otherwise specified.

[0221] <List of ingredients> The raw materials of the resin compositions used in the following Examples and Comparative Examples are as follows.

[0222] (A) Component: Aliphatic triglycidyl ether (Nagase ChemteX "EX-321L", epoxy equivalent 130g / eq.) Phenolphthalimidine type epoxy resin (Nippon Kayaku Co., Ltd. "WHR991S", epoxy equivalent 265g / eq.)

[0223] (B) Ingredients: Inorganic filler 1: Spherical silica (average particle size 1 μm, specific surface area 4.5 m) surface-treated with an aminosilane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.) 2 / g, Admatechs "SO-C4")

[0224] (C) Ingredients: Hydroxyl-containing acrylic polymer (Toagosei Co., Ltd. "ARUFON UH-2000", weight average molecular weight 11,000, glass transition temperature -55°C)

[0225] (D) Ingredients: Bisphenol A diphenyl ether bismaleimide ("BMI-4000" manufactured by Daiwa Chemical Industry Co., Ltd., maleimide group equivalent weight 285 g / eq., toluene solution with solid content of 50% by mass) Carbodiimide resin (Nisshinbo Chemical's "V-03", active group equivalent of approximately 216 g / eq., toluene solution with 50% solids by mass) Active ester resin (DIC "HPC-8000-65T", active group equivalent weight approx. 223 g / eq., toluene solution with solid content of 65% by mass) Phenol novolac resin (DIC "TD-2090-60M", hydroxyl equivalent of approximately 105 g / eq., MEK solution with 60% solids)

[0226] (E) Ingredients: Imidazole-based curing accelerator (Shikoku Chemical Industry Co., Ltd. "1B2PZ", 1-benzyl-2-phenylimidazole, MEK solution with 5% solids by mass)

[0227] <Production Example 1. Production of Elastomer 1> In a reaction vessel, 50 g of bifunctional hydroxyl-terminated polybutadiene (number average molecular weight: 5047 (GPC method), hydroxyl equivalent = 1800 g / eq., solid content 100 mass%: "G-3000" manufactured by Nippon Soda Co., Ltd.), 23.5 g of aromatic hydrocarbon mixed solvent ("IPZOL 150" manufactured by Idemitsu Petrochemical Co., Ltd.), and 0.005 g of dibutyltin laurate were mixed and dissolved uniformly. When the mixture became uniform, the temperature was raised to 50°C, and 4.8 g of toluene-2,4-diisocyanate (isocyanate equivalent: 87.08 g / eq.) was added while further stirring, and the reaction was carried out for about 3 hours. Next, the reaction mixture was cooled to room temperature, and 8.96 g of benzophenonetetracarboxylic dianhydride (acid anhydride equivalent: 161.1 g / eq.), 0.07 g of triethylenediamine, and 40.4 g of ethyl diglycol acetate (manufactured by Daicel Corporation) were added thereto, and the mixture was heated to 130° C. with stirring and reacted for about 4 hours. -1 The disappearance of the NCO peak was confirmed. The disappearance of the NCO peak was regarded as the end point of the reaction, and the reaction mixture was cooled to room temperature and filtered through a 100 mesh filter cloth to obtain an elastomer 1 (non-volatile content 50 mass%) having an imide structure, a urethane structure, and a polybutadiene structure. The number average molecular weight of the obtained elastomer 1 was 13,700.

[0228] <Example 1> A resin solution was obtained by dissolving 4 parts of an aliphatic triglycidyl ether ("EX-321L" manufactured by Nagase ChemteX Corporation, epoxy equivalent 130 g / eq.) and 2 parts of a phenolphthalimidine type epoxy resin ("WHR991S" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 265 g / eq.) in 8 parts of MEK with heating while stirring. This resin solution was cooled to room temperature. Then, 20 parts of elastomer 1 (non-volatile content 50% by mass), 2 parts of active ester resin (DIC Corporation's "HPC-8000-65T", active group equivalent of about 223 g / eq., toluene solution with solid content of 65% by mass), 1.5 parts of phenol novolac resin (DIC Corporation's "TD-2090-60M", hydroxyl group equivalent of about 105 g / eq., MEK solution with solid content of 60%), bisphenol A diphenyl ether bismaleimide (Daiwa Chemical Industry Co., Ltd.'s "BMI-4000", maleimide) were added to the resin solution. A mixture of 8 parts of a carbodiimide resin (Nisshinbo Chemical Co., Ltd.'s "V-03", active group equivalent of about 216 g / eq., solid content of 50% by mass in toluene solution), 2 parts of a carbodiimide resin (Nisshinbo Chemical Co., Ltd.'s "V-03", active group equivalent of about 216 g / eq., solid content of 50% by mass in toluene solution), 1 part of an imidazole curing accelerator (Shikoku Kasei Kogyo Co., Ltd.'s "1B2PZ", 1-benzyl-2-phenylimidazole, solid content of 5% by mass in MEK solution), 85 parts of inorganic filler 1, and 10 parts of MEK were mixed and uniformly dispersed in a high-speed rotating mixer to obtain a mixture. The mixture was then filtered through a cartridge filter (ROKITECHNO's "SHP020") to produce a resin varnish.

[0229] As the first film layer, a polyethylene terephthalate film ("Lumirror R80" manufactured by Toray Industries, Inc., thickness 38 μm, softening point 130° C.) that had been subjected to release treatment with an alkyd resin-based release agent ("AL-5" manufactured by Lintec Corporation) was prepared. A resin varnish was applied onto this first film layer using a die coater so that the thickness of the resin composition layer after drying would be 70 μm, and the resin sheet including the first film layer and the resin composition layer was obtained by drying at 85° C. to 100° C. The drying time was set so that the mass reduction rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass reduction rate by heating at 190° C.> described later would be the value in Table 1.

[0230] <Example 2> The amount of inorganic filler 1 was changed to 93 parts. In addition, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass loss rate by heating at 190°C> described later would be the value in Table 1. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0231] <Example 3> The amount of inorganic filler 1 was changed to 110 parts. In addition, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass loss rate by heating at 190°C> described later would be the value in Table 1. A resin varnish and a resin sheet were produced in the same manner as in Example 1 except for the above points.

[0232] <Example 4> The amount of inorganic filler 1 was changed to 75 parts. In addition, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass loss rate by heating at 190°C> described later would be the value in Table 1. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0233] <Example 5> The amount of aliphatic triglycidyl ether "EXL-321L" was changed to 2 parts. The amount of elastomer 1 (non-volatile content 50% by mass) was also changed to 26 parts. Furthermore, the drying time after application of the resin varnish was changed so that the mass reduction rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass reduction rate by heating at 190°C> described later would be the value in Table 1. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0234] <Example 6> The amount of phenolphthalimidine type epoxy resin "WHR991S" was changed to 3 parts. The amount of elastomer 1 (non-volatile component 50% by mass) was changed to 14 parts. The amount of phenol novolac resin "TD-2090-60M" (solid content 60%) was changed to 2 parts. The drying time after application of the resin varnish was changed so that the mass reduction rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass reduction rate by heating at 190°C> described later would be the value in Table 1. A resin varnish and a resin sheet were produced in the same manner as in Example 1 except for the above items.

[0235] <Example 7> 20 parts of Elastomer 1 (non-volatile content 50% by mass) was changed to 8 parts of a hydroxyl-containing acrylic polymer ("ARUFON UH-2000" manufactured by Toagosei Co., Ltd., weight average molecular weight 11,000, glass transition temperature -55°C). In addition, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass loss rate by heating at 190°C> described later would be the value in Table 1. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0236] <Example 8> The amount of active ester resin "HPC-8000-65T" (solid content 65% by mass) was changed to 1.2 parts. The amount of carbodiimide resin "V-03" (solid content 50% by mass) was changed to 3 parts. Furthermore, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown below in <Measurement of mass loss rate by heating at 190°C> became the value in Table 1. Apart from the above, the resin varnish and resin sheet were produced in the same manner as in Example 1.

[0237] <Example 9> The phenol novolac resin "TD-2090-60M" was not used, and the amount of carbodiimide resin "V-03" (solid content 50 mass%) was changed to 8 parts. In addition, the drying time after application of the resin varnish was changed so that the mass reduction rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass reduction rate by heating at 190°C> described later would be the value in Table 1. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0238] <Example 10> The amount of active ester resin "HPC-8000-65T" (solid content 65% by mass) was changed to 3 parts, and carbodiimide resin "V-03" was not used. In addition, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass loss rate by heating at 190°C> described later would be the value in Table 1. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0239] <Example 11> Bisphenol A diphenyl ether bismaleimide "BMI-4000" was not used, and the amount of MEK mixed at the end was changed to 14 parts. In addition, the drying time after application of the resin varnish was changed so that the mass reduction rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass reduction rate by heating at 190°C> described later would be the value in Table 1. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0240] <Comparative Example 1> The amount of elastomer 1 (50% by mass of non-volatile components) was changed to 36 parts. In addition, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass loss rate by heating at 190°C> described later would be the value in Table 2. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0241] <Comparative Example 2> The amount of elastomer 1 (50% by mass of non-volatile components) was changed to 4 parts. In addition, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass loss rate by heating at 190°C> described later would be the value in Table 2. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0242] <Comparative Example 3> The amount of inorganic filler 1 was changed to 120 parts. In addition, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass loss rate by heating at 190°C> described later would be the value in Table 2. A resin varnish and a resin sheet were produced in the same manner as in Example 1 except for the above points.

[0243] <Comparative Example 4> The amount of inorganic filler 1 was changed to 63 parts. In addition, the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown in <Measurement of mass loss rate by heating at 190°C> described later would be the value in Table 2. A resin varnish and a resin sheet were produced in the same manner as in Example 1, except for the above points.

[0244] <Comparative Example 5> A resin varnish and a resin sheet were produced in the same manner as in Example 1, except that the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown below in <Measurement of mass loss rate by heating at 190°C> would be the value in Table 2.

[0245] <Comparative Example 6> A resin varnish and a resin sheet were produced in the same manner as in Example 1, except that the drying time after application of the resin varnish was changed so that the mass loss rate P(a) of the resin composition layer measured by the method shown below in <Measurement of mass loss rate by heating at 190°C> would be the value in Table 2.

[0246] <Measurement of mass loss rate by heating at 190℃> The resin sheet was cut into 10 cm squares, placed in a desiccator together with thoroughly dried silica gel, and left for 30 minutes, after which the mass M0 was measured. The mass of the first film layer contained in the resin sheet was subtracted from this mass M0 to obtain the mass m0 (=M0-mass of the first film layer) of the resin composition layer before heating. The resin sheet was heated at 190°C for 30 minutes, and after cooling for 30 minutes in a desiccator together with silica gel as before, the mass M1 was measured again. The mass reduction amount ΔM due to heating was obtained by subtracting the mass M1 from the mass M0. Since the first film layer used in the above-mentioned examples and comparative examples does not contain components such as solvents that volatilize upon heating at 190°C for 30 minutes, the mass reduction amount ΔM represents not only the mass reduction amount of the resin sheet but also the mass reduction amount of the resin composition layer. The mass reduction amount ΔM was divided by the mass m0 of the resin composition layer before heating to calculate the mass reduction rate P(a) [%] of the resin composition layer.

[0247] <Measurement of elongation and elastic modulus after heating at 130℃> The resin sheet was heated at 130°C for 30 minutes, and the first film layer was peeled off to obtain a cured product for evaluation. This cured product for evaluation was cut into a dumbbell shape No. 1 to obtain a test piece. The test piece was subjected to tensile strength measurement using a tensile tester "RTC-1250A" manufactured by Orientec Co., Ltd., and the elongation percentage [%] and tensile modulus [GPa] at 25°C were obtained. The measurement was performed in accordance with JIS K7127. This operation was performed three times, and the average value was calculated. The average value of the elongation percentage [%] was adopted as parameter P(b), and the average value of the tensile modulus was adopted as parameter P(c).

[0248] <Cutting performance evaluation test> An OPP film (biaxially oriented polypropylene film, Oji F-Tex Co., Ltd. "MA-411", thickness 15 μm) was prepared as the second film layer. The resin sheet and the second film layer were laminated at 40 ° C. using a roll laminator so that the resin composition layer and the second film layer were bonded to each other, to obtain a multilayer sample sheet having a layer structure of the first film layer / resin composition layer / second film layer. This multilayer sample sheet was punched out using a 10 cm square cutter manufactured by Dumbbell Co., Ltd. The square multilayer sample sheet obtained by punching was observed, and the chipping ease (cutting ability) of the resin composition layer was evaluated. Since chipping of the resin composition layer due to punching is likely to occur at the corners where the cutter blade contacts, the less chipping at the corners of the resin composition layer, the better the cutting ability.

[0249] Cutting ability evaluation criteria: "◯": No chipping in the resin composition layer at any of the four corners of the multilayer sample sheet. "△": The resin composition layer was chipped at one to three corners of the multilayer sample sheet. "X": The resin composition layer was chipped at all four corners of the multilayer sample sheet.

[0250] <Removability evaluation test> A glass cloth-based epoxy resin double-sided copper-clad laminate with copper foil on the surface (copper foil thickness 18 μm, substrate thickness 0.8 mm, Panasonic "R-1766") was prepared. Both sides were roughened by etching using a microetching agent (Mec "CZ8101") so that the copper etching amount was 2 μm. The copper-clad laminate obtained in this way is called a "roughened copper-clad laminate".

[0251] The resin sheet was laminated onto the roughened copper-clad laminate using a batch-type vacuum pressure laminator (Nikko Materials' two-stage build-up laminator "CVP700"). This lamination was performed so that the resin composition layer of the resin sheet and the roughened copper-clad laminate were bonded. This lamination was also performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing for 30 seconds at 100°C and a pressure of 0.74 MPa.

[0252] A cut was made in the first film layer of the resin sheet, surrounding an area of ​​10 mm in width and 100 mm in length. One end of this area was peeled off and held with a gripper (Autocom type testing machine "AC-50C-SL" manufactured by TSE Corporation), and the load (kgf / cm) when 20 mm was peeled off in the vertical direction at a speed of 50 mm / min at room temperature was measured to determine the peel strength as the adhesion strength between the first film layer and the resin composition layer.

[0253] The peel strength indicates the strength of the force required to peel off the resin composition layer and the first film layer. Therefore, the smaller the peel strength, the smaller the adhesion strength between the resin composition layer and the film layer, and therefore the smoother the peeling of the film layer. Therefore, the smaller the peel strength, the more effectively the resin composition layer can be prevented from causing defects due to the peeling of the film layer, and therefore the better the peelability.

[0254] Peelability evaluation criteria: "○": Peel strength is 0.06kgf / cm or less. "△": Peel strength is 0.07kgf / cm~0.09kgf / cm. "X": Peel strength is 0.1kgf / cm or more.

[0255] <Warpage evaluation test> The resin sheet was laminated on the entire surface of one side of a 12-inch silicon wafer (thickness 775 μm) using a batch-type vacuum pressure laminator. This lamination was performed so that the resin composition layer and the silicon wafer were bonded. The first film layer of the resin sheet was peeled off to expose the resin composition layer. A resin sheet was similarly laminated on the surface of this exposed resin composition layer, and the first film layer was peeled off. By the above lamination, two resin composition layers (total thickness 140 μm) were formed on one side of the 12-inch silicon wafer. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 100° C. and a pressure of 0.74 MPa for 30 seconds.

[0256] The sample was heated in an oven at 100°C for 30 minutes, and then further heated at 190°C for 90 minutes to cure the resin composition layer, thereby obtaining a sample laminate having a layer structure of "silicon wafer / cured layer". The obtained sample laminate was placed on the top surface of a horizontal table. The end of the sample laminate was pressed against the top surface of the table. The distance between the end of the silicon wafer on the opposite side to the pressed end and the top surface of the table was measured as the amount of warping. The amount of warping was evaluated according to the following criteria. The smaller the amount of warping, the more effectively the warping was suppressed.

[0257] Warpage evaluation criteria: "○": Warpage is between 0 mm and 0.6 mm. "△": The amount of warping is greater than 0.6 mm and less than 1.0 mm. "X": The amount of warping is greater than 1.0 mm.

[0258] <Result> The results of the above examples and comparative examples are shown in the following table, where the amount of each component represents parts by weight of non-volatile components.

[0259] [Table 1]

[0260] [Table 2]

[0261] Experiments similar to those of Examples 1 to 11 described above were conducted by changing the thickness of the resin composition layer in the range of 1 μm to 150 μm, and it was confirmed that these experiments also resulted in similar results to those of Examples 1 to 11, although to different degrees. It has also been confirmed that, even when components (C) to (G) are not contained in Examples 1 to 11, the same results as in Examples 1 to 11 are obtained, although to a different extent. [Explanation of symbols]

[0262] 100 Resin sheet 110 Resin composition layer 111 Effective resin composition layer 112 Peripheral resin composition layer 120 First Film Layer 130 Second Film Layer 131 Main part of second film layer 132 Peripheral portion of second film layer

Claims

1. A resin sheet having a resin composition layer, The resin composition layer contains (A) an epoxy resin and (B) an inorganic filler, A resin sheet, wherein the resin composition layer satisfies the following formula (1): 0.09≦P(a)×P(b) / P(c)≦0.3 (1) (In formula (1), P(a) represents the mass reduction rate (%) of the resin composition layer upon heating at 190° C. for 30 minutes, P(b) represents the elongation percentage (%) measured at a measurement temperature of 25° C. after heating the resin composition layer at 130° C. for 30 minutes, P(c) represents the tensile modulus (GPa) measured at a measurement temperature of 25° C. after heating the resin composition layer at 130° C. for 30 minutes.

2. The resin sheet according to claim 1 , wherein the resin composition layer comprises an elastomer (C).

3. The resin sheet according to claim 1 , wherein the resin composition layer comprises a curing agent (D).

4. The resin sheet according to claim 3 , wherein the curing agent (D) comprises a maleimide-based resin.

5. The resin sheet according to claim 3 , wherein the curing agent (D) comprises a carbodiimide resin.

6. The resin sheet according to claim 1 , wherein the resin composition layer has a thickness of 1 μm or more and 150 μm or less.

7. The resin sheet according to claim 1 , further comprising a film layer in contact with the resin composition layer.

8. The resin sheet according to claim 1 , wherein P(a) is 0.6% or more.

9. A step (I) of cutting the resin composition layer of the resin sheet according to any one of claims 1 to 8; A step (II) of laminating a resin sheet having a cut resin composition layer and a substrate; and A method for producing a semiconductor chip package, comprising: (III) curing the resin composition layer.

10. The method of claim 9 , wherein the substrate comprises a wafer.

11. The method for producing a semiconductor chip package according to claim 9 , wherein step (I) comprises pressing a blade against the resin composition layer in a thickness direction thereof to cut the resin composition layer.

12. A step (I) of cutting the resin composition layer of the resin sheet according to any one of claims 1 to 8; A step (II) of laminating a resin sheet having a cut resin composition layer and a substrate; and A method for producing a circuit board, comprising: a step (III) of curing the resin composition layer.

Citation Information

Patent Citations

  • Speaker system

    JP2000138996A

  • Resin composition, resin film, production method of resin film, method for manufacturing semiconductor device, and semiconductor device

    JP2017197656A

  • Resin material and multilayer printed wiring board