Silicon wafer cleaning method, silicon wafer manufacturing method, and silicon wafer

The silicon wafer cleaning method addresses non-uniform native oxide film thickness by offsetting the oxidizing agent supply and adjusting cleaning conditions, resulting in improved film uniformity and semiconductor device yield.

JP7574841B2Active Publication Date: 2024-10-29SUMCO CORP
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2022182395
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-11-15
Publication Date
2024-10-29
Estimated Expiration
2042-11-15

AI Technical Summary

Technical Problem

Existing silicon wafer cleaning methods result in non-uniform thickness of native oxide films, which is a challenge for improving the uniformity and reproducibility of semiconductor devices.

Method used

A method for cleaning silicon wafers involving a surface layer modification step using an oxidizing agent supplied radially offset from the wafer center, followed by an etching step with an etching solution, and a rinsing step, with specific conditions for oxidizing agent and etching solution concentrations, flow rates, and rotation speeds to achieve uniformity.

Benefits of technology

The method enhances the uniformity of native oxide film thickness on silicon wafers, improving the yield and performance of semiconductor devices by ensuring consistent film thickness across the wafer surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574841000003
    Figure 0007574841000003
  • Figure 0007574841000004
    Figure 0007574841000004
  • Figure 0007574841000005
    Figure 0007574841000005
Patent Text Reader

Abstract

To provide a method for cleaning a silicon wafer, a method for manufacturing a silicon wafer, and a silicon wafer having a more uniform native oxide film, which are capable of improving the uniformity of the thickness of a native oxide film on a silicon wafer.SOLUTION: In a silicon wafer cleaning method according to the present invention, in a surface modification step, an oxidizing agent is supplied from a position radially shifted from the center of the silicon wafer. The silicon wafer manufacturing method according to the present invention includes carrying out the silicon wafer cleaning method. In the silicon wafer of the present invention, when a predetermined measurement is carried out, the difference between the maximum value and the minimum value of the thickness of the native oxide film in the radial direction of the silicon wafer is 0.1 or less when the measured thickness of the native oxide film is normalized by the maximum value.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicon wafer cleaning method, a silicon wafer manufacturing method, and a silicon wafer. [Background technology]

[0002] On the surface of silicon wafers, there are oxide films that are formed at room temperature in an air atmosphere, and oxide films that are formed by cleaning with chemical solutions; these are called natural oxide films or chemical oxide films (hereafter referred to as natural oxide films). The thickness of a natural oxide film is about a few tenths of a nanometer (around 0.2 nm) to 2 nm or less. The thickness of a natural oxide film formed in a typical silicon wafer cleaning process is around 5 Å (angstroms). In contrast, an oxide film formed by heat treatment is called a thermal oxide film, and its thickness is 3 nm or more.

[0003] In recent years, semiconductor devices have become more precise, multi-layered, and thin, and thus there is a demand for thinner films for use in semiconductor elements. For example, as a method for improving the gate characteristics of MOS transistors, a method has been disclosed in which the silicon surface is cleaned immediately before the formation of a gate oxide film, the silicon surface is hydrogen-terminated, and then a gate insulating film is formed (e.g., Patent Document 1). In order to improve the yield of the latest semiconductor devices, it is necessary to form an extremely thin silicon oxide film, such as a natural oxide film, uniformly and reproducibly within the surface (e.g., Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-216156 A [Patent Document 2] Patent No. 6791454 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a method for cleaning a silicon wafer, which can improve the uniformity of the thickness of a native oxide film on a silicon wafer, a method for manufacturing a silicon wafer, and a silicon wafer having a more uniform native oxide film. [Means for solving the problem]

[0006] The gist and configuration of the present invention are as follows. (1) A method for cleaning a single silicon wafer, comprising the steps of: a surface modification step of modifying a surface layer of the silicon wafer using an oxidizing agent; an etching step of etching the surface layer of the silicon wafer after the surface layer modification step using an etching solution; A rinsing step of rinsing the surface of the silicon wafer with a rinsing liquid, a supplying step of supplying the oxidizing agent from a position radially shifted from a center of the silicon wafer in the surface modification step; Here, "supplying the oxidant from a position radially shifted from the center of the silicon wafer" means that the intersection of the extension line of the supply pipe supplying the oxidant and the surface of the silicon wafer is radially shifted from the center of the silicon wafer, and the oxidant is supplied from the supply pipe at such a position.

[0007] (2) The method for cleaning a silicon wafer according to (1) above, wherein the oxidizing agent is ozone water.

[0008] (3) The method for cleaning a silicon wafer according to (1) or (2) above, wherein the etching solution is an aqueous solution of hydrogen fluoride.

[0009] (4) The method for cleaning a silicon wafer according to (1) or (2) above, wherein the rinsing liquid is pure water.

[0010] (5) The method for cleaning a silicon wafer according to any one of (1) to (4) above, wherein the position to which the oxidizing agent is supplied is a position shifted in a radial direction from the center of the silicon wafer within a range of 5 mm to 75 mm.

[0011] (6) The method for cleaning a silicon wafer according to (5) above, wherein the position to which the oxidizing agent is supplied is a position shifted in a radial direction from the center of the silicon wafer within a range of 15 mm to 20 mm.

[0012] (7) The method for cleaning a silicon wafer according to any one of (1) to (6) above, wherein the oxidizing agent is ozone water, the etching liquid is an aqueous solution of hydrogen fluoride, the concentration of the ozone water is within a range of 20 to 30 ppm, and the concentration of the aqueous solution of hydrogen fluoride is within a range of 0.5 to 3.0 mass %.

[0013] (8) The method for cleaning a silicon wafer according to any one of (1) to (7) above, wherein a rotation speed of the silicon wafer in the surface modification step, the etching step, and the rinsing step is within a range of 100 to 500 rpm.

[0014] (9) The method for cleaning a silicon wafer according to any one of the above (1) to (8), comprising a step of measuring a thickness of a native oxide film at intervals of 29.4 mm from the center of the silicon wafer having a diameter of 300 mm by a spectroscopic ellipsometer, and adjusting at least one of a position for supplying the oxidant, a concentration of the oxidant, a concentration of the etching solution, a flow rate of the oxidant, a flow rate of the etching solution, and a rotation speed of the silicon wafer so that a difference between a maximum value and a minimum value of the thickness of the native oxide film in the radial direction of the silicon wafer when the measured thickness of the native oxide film is normalized by the maximum value is 0.1 or less.

[0015] (10) A method for producing a silicon wafer, comprising carrying out the method for cleaning a silicon wafer according to any one of (1) to (9) above.

[0016] (11) A silicon wafer having a native oxide film having a thickness of 2 nm or less formed thereon, characterized in that, when the thickness of the native oxide film is measured at 29.4 mm intervals from the center of the silicon wafer having a diameter of 300 mm to 147 mm from the center using a spectroscopic ellipsometer, the difference between the maximum and minimum thicknesses of the native oxide film in the radial direction of the silicon wafer when the measured thicknesses of the native oxide film are normalized by the maximum thickness is 0.1 or less. Effect of the Invention

[0017] According to the present invention, it is possible to provide a method for cleaning a silicon wafer, a method for manufacturing a silicon wafer, and a silicon wafer having a more uniform native oxide film, which can improve the uniformity of the thickness of a native oxide film on a silicon wafer. [Brief description of the drawings]

[0018] [Figure 1] 1 is a flowchart of a method for cleaning a silicon wafer according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a diagram illustrating a positional relationship between a silicon wafer and supply pipes for an oxidizing agent and an etching solution. [Diagram 3] FIG. 4 is a diagram showing measurement points of the thickness of a native oxide film on a wafer in an embodiment. [Figure 4] FIG. 11 is a diagram showing the measurement results of the thickness of a formed native oxide film. [Diagram 5] FIG. 5 is a diagram showing the result of normalizing the thickness of the native oxide film in FIG. 4 by the maximum value. [Figure 6] FIG. 13 is a diagram showing the results of comparing the uniformity of the thickness of a native oxide film depending on the type of chemical solution. [Figure 7] FIG. 13 is a diagram showing the thickness distribution of a native oxide film when the rotation speed of a silicon wafer during the final treatment with ozone water is changed. [Figure 8] FIG. 8 is a diagram showing the result of normalizing the thickness of the native oxide film in FIG. 7 by the maximum value. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings.

[0020] <Silicon wafer cleaning method> Fig. 1 is a flow chart of a method for cleaning a silicon wafer according to one embodiment of the present invention, Fig. 2 is a schematic diagram showing the positional relationship between a silicon wafer and supply pipes for an oxidizing agent and an etching solution.

[0021] The silicon wafer cleaning method of this embodiment is a method for cleaning a single-wafer silicon wafer using a single-wafer spin cleaner. The single-wafer silicon wafer cleaning method here means a method for cleaning a wafer surface by supplying a desired chemical solution from a chemical solution supply nozzle toward the wafer surface while rotating the wafer horizontally around the center of the wafer as the central axis. As shown in FIG. 1, in the method of this embodiment, first, the surface layer of the silicon wafer W is modified using an oxidizing agent (surface modification step: step S101). In this step, as shown in FIG. 2, while rotating the silicon wafer W, an oxidizing agent (ozone water in this example) is supplied to the surface of the silicon wafer W through a supply pipe 1, and is brought into contact with the surface of the silicon wafer W, forming a natural oxide film on the surface of the silicon wafer W. Note that prior to step S101, SC-1 (Standard Clean 1) cleaning or SC-2 (Standard Clean 2) cleaning can be appropriately performed.

[0022] The oxidizing agent is preferably ozone water. The concentration of the ozone water is preferably within the range of 20 to 30 ppm. By setting the concentration of the ozone water to 20 ppm or more, a natural oxide film of sufficient thickness can be formed, while considering the solubility limit of ozone in water, the upper limit of the concentration is about 30 ppm. Here, ppm represents a weight ratio. The flow rate of the ozone water is preferably 0.5 to 1.5 L / min. The treatment time with the ozone water is preferably 15 to 60 seconds.

[0023] 2, in this embodiment, the oxidant (ozone water in this example) is supplied from a position radially shifted (toward the edge of the wafer W) from the center O of the silicon wafer W. More specifically, the position from which the oxidant is supplied is preferably a position radially shifted within a range of 5 mm to 75 mm from the center O of the silicon wafer W, and more preferably a position radially shifted within a range of 15 mm to 20 mm from the center O of the silicon wafer W.

[0024] Next, the surface layer of the silicon wafer W is etched using an etching solution (etching step: step S102). In this step, as shown in FIG. 2, while the silicon wafer W is being rotated, an etching solution (in this example, an aqueous solution of hydrogen fluoride) is supplied to the surface of the silicon wafer W via a supply pipe 2 and brought into contact with the surface of the silicon wafer W. This etches the natural oxide film formed in the surface modification step (step S101). Note that in this step (at least the final etching step if step S102 is performed multiple times), the amount of etching is set to an extent that the natural oxide film remains.

[0025] The etching solution is preferably an aqueous solution of hydrogen fluoride. The concentration of the aqueous solution of hydrogen fluoride is preferably within the range of 0.5 to 3.0 mass %. By setting the concentration of the aqueous solution of hydrogen fluoride to 0.5 mass % or more, a sufficient etching effect can be obtained, while by setting the concentration of the aqueous solution of hydrogen fluoride to 3.0 mass % or less, excessive etching can be suppressed. The flow rate of the aqueous solution of hydrogen fluoride is preferably 0.5 to 1.5 L / min. The treatment time with the aqueous solution of hydrogen fluoride is preferably 1 to 10 seconds.

[0026] 2, in this embodiment, the etching liquid (aqueous solution of hydrogen fluoride in this example) is supplied from the position of the center O of the silicon wafer W (without being shifted in the radial direction). However, the etching liquid may be supplied at a position shifted in the radial direction from the position of the center O of the silicon wafer W.

[0027] In this embodiment, as shown in Fig. 1, after repeating the surface layer modification step (step S101) and the etching step (step S102) a predetermined number of times (e.g., 2 to 4 times), the process proceeds to the rinsing step (step S103) described below. Note that the surface layer modification step (step S101) and the etching step (step S102) do not necessarily have to be repeated. Also, the surface layer modification step (step S101), the etching step (step S102), and the rinsing step (step S103) including the rinsing step (step S103) may be repeated (e.g., 2 to 4 times).

[0028] Next, a rinse process using a rinse liquid (rinsing process: step S103) is performed. In this process, while rotating the silicon wafer W, a rinse liquid (pure water in this example) is supplied to the surface of the silicon wafer W through a supply pipe (not shown) separate from the supply pipes 1 and 2, to wash away foreign matter on the surface of the silicon wafer W. The rinse liquid is preferably pure water, and more preferably DIW (DeIonized Water). The flow rate of the pure water is preferably 0.5 to 1.5 L / min. The treatment time with the pure water is preferably 1 to 30 seconds. In this embodiment, the pure water is supplied from the position of the center O of the silicon wafer W (without being shifted in the radial direction). However, the pure water may be supplied from the position of the center O of the silicon wafer W shifted in the radial direction.

[0029] In steps S101 to S103, the rotation speed of the silicon wafer W during cleaning is preferably within a range of 100 to 500 rpm.

[0030] The effects of the silicon wafer cleaning method of this embodiment will be described below. The inventors of the present invention conducted extensive research into the cause of the non-uniformity in the thickness of the native oxide film on a silicon wafer, and discovered that in the conventional method of supplying an oxidant (ozone water) from the center O of the silicon wafer W, the rotation of the silicon wafer W generates centrifugal force in the radial direction (from the center to the edge), and the supplied oxidant (ozone water) flows in the radial direction from the center O in a concentric wavy pattern, resulting in a flow that forms a peak in the supply amount, for example, near the point R / 2 (where R is the diameter) or at the outer periphery, and that this is the cause of the non-uniformity in the thickness of the native oxide film within the surface. Therefore, in this embodiment, in the single-wafer cleaning process using an oxidizing agent, an etching solution, and a rinsing solution, in the surface modification step (step S101) using an oxidizing agent, the oxidizing agent (ozone water) is supplied from a position radially shifted from the center O of the silicon wafer W. This prevents the supplied oxidizing agent (ozone water) from flowing radially from the center O in a concentric wavy manner, thereby reducing the peak of the supply amount of the oxidizing agent (ozone water) as described above. Therefore, the silicon wafer cleaning method of this embodiment can improve the uniformity of the thickness of the native oxide film on the silicon wafer W. It is expected that the oxide film of uniform thickness formed in the cleaning process will maintain its uniformity even in the subsequent thermal oxidation process, which is expected to lead to an improvement in the yield in the production of semiconductor devices.

[0031] Here, as described above, the position where the oxidant (ozone water) is supplied is preferably a position shifted in the radial direction from the center of the silicon wafer W within a range of 5 mm to 75 mm. By shifting the position in the radial direction from the center of the silicon wafer W by 5 mm or more, the above-mentioned effect can be obtained more reliably, while by shifting the position in the radial direction from the center of the silicon wafer W by 75 mm or less, the amount of the oxidant (ozone water) supplied to the vicinity of the center O of the silicon wafer W can be prevented from becoming too small, and thus the uniformity of the thickness of the natural oxide film on the silicon wafer W can be improved more reliably. For the same reason, the position where the oxidant (ozone water) is supplied is more preferably a position shifted in the radial direction from the center O of the silicon wafer W within a range of 15 mm to 20 mm.

[0032] Here, at least any one of the position where the oxidant (ozone water) is supplied, the concentration of the oxidant (ozone water), the concentration of the etching solution (aqueous hydrogen fluoride solution), the flow rate of the oxidant (ozone water), the flow rate of the etching solution (aqueous hydrogen fluoride solution), and the rotation speed of the silicon wafer W can also be used as parameters for fine-tuning the uniformity of the thickness of the native oxide film. That is, for example, as an index of the uniformity of the native oxide film, the thickness of the native oxide film is measured at intervals of 29.4 mm from the center of a silicon wafer W having a diameter of 300 mm using a spectroscopic ellipsometer, and the measured thickness of the native oxide film is normalized by the maximum value. The difference between the maximum and minimum values ​​of the thickness of the native oxide film in the radial direction of the silicon wafer W is used, and a target value is set such that the difference between the maximum and minimum values ​​is 0.1 or less. Then, data on the relationship between at least one of the position where the oxidant is supplied, the concentration of the oxidant, the concentration of the etching solution, the flow rate of the oxidant, the flow rate of the etching solution, and the rotation speed of the silicon wafer and the uniformity of the thickness of the native oxide film (e.g., a profile of the amount of variation in the thickness within the surface) is obtained in advance. Based on the current cleaning conditions and the in-plane profile of the native oxide film thickness, a target value for the amount of thickness variation (increase or decrease) in a predetermined region (position) within the silicon wafer surface is determined in order to achieve the target value. Based on the relationship data, correction values ​​for the above cleaning conditions suitable for achieving a target value for the amount of variation in thickness in a predetermined region within the surface of the silicon wafer are determined. Then, by adjusting at least one of the above cleaning conditions by the calculated correction value and then performing subsequent cleaning, the uniformity of the native oxide film on the silicon wafer can be further improved.

[0033] As a variation of the above fine adjustment, the above fine adjustment can be performed by a method using artificial intelligence. That is, an artificial intelligence model is created by a machine learning unit (processor) of a computer, with the amount of variation in the thickness of the natural oxide film in a predetermined region (position) in the surface as an explanatory variable (input) and at least one of the correction values ​​of each of the above cleaning conditions as an objective variable (output) (sufficient learning data necessary for machine learning is prepared in advance). Then, when the amount of variation in the thickness of the natural oxide film in a predetermined region (position) in the surface (corresponding to a target value that the difference between the maximum and minimum values ​​of the thickness of the natural oxide film in the radial direction of the silicon wafer W is, for example, 0.1 or less) is input in the created artificial intelligence model, at least one of the correction values ​​of each of the above cleaning conditions is output by the machine learning unit. Using the correction value that is the output, at least one of the above cleaning conditions is corrected by the calculated correction value, and then cleaning is performed from the next time onwards. Note that any known algorithm such as a neural network can be used as the machine learning algorithm.

[0034] In the example shown in FIG. 2, when the direction perpendicular to the main surface of the silicon wafer is defined as the up-down direction, the supply pipes 1 and 2 are inclined from the edge side of the silicon wafer in the radial direction toward the center from the top to the bottom (toward the side closer to the silicon wafer). The inclination angle θ1 of the supply pipe 1 with respect to the up-down direction is not particularly limited, but can be 1 to 5°. The inclination angle θ2 of the supply pipe 2 with respect to the up-down direction is not particularly limited, but can be 1 to 5°. These supply pipes 1 and 2 do not necessarily need to be inclined with respect to the up-down direction, and may extend in the up-down direction (without inclination). Even when inclined in the up-down direction, the supply pipes 1 and 2 may be inclined from the inside to the outside in the radial direction of the silicon wafer from the top to the bottom (toward the side closer to the silicon wafer).

[0035] <Silicon wafer manufacturing method> The method for producing a silicon wafer according to one embodiment of the present invention includes carrying out the method for cleaning a silicon wafer according to the above embodiment. As is well known, other steps may include an ingot pulling step, a slicing step, a polishing step, etc. According to the method for producing a silicon wafer according to this embodiment, the uniformity of the thickness of the native oxide film on the silicon wafer W can be improved.

[0036] <Silicon wafer> The silicon wafer according to one embodiment of the present invention is a silicon wafer after the silicon wafer cleaning method according to the above embodiment is carried out, and is a silicon wafer on which a native oxide film having a thickness of 2 nm or less is formed, and when the thickness of the native oxide film is measured at 29.4 mm intervals from the center of a silicon wafer having a diameter of 300 mm to 147 mm using a spectroscopic ellipsometer, the difference between the maximum and minimum thicknesses of the native oxide film in the radial direction of the silicon wafer when the measured thicknesses of the native oxide film are normalized by the maximum value is 0.1 or less. As will be shown in the examples described later, according to the method of this embodiment, a silicon wafer having a native oxide film of a more uniform thickness can be obtained. EXAMPLES

[0037] Examples of the present invention will be described below, but the present invention is not limited to the following examples in any way.

[0038] In this embodiment, a p-type epitaxial silicon wafer (hereinafter simply referred to as silicon wafer) having a diameter of 300 mm was used as a sample. First, a cleaning process was performed for 15 seconds using ozone water with an ozone concentration of 20 ppm, with the wafer rotating at 300 rpm. Next, a cleaning process was performed for 4 seconds for the purpose of etching the oxide film, with the silicon wafer rotating at 300 rpm, using an aqueous solution of hydrogen fluoride with a concentration of 1%. The etching process with the aqueous solution of hydrogen fluoride at this time was performed under conditions such that the oxide film was not completely removed. Next, a cleaning process was performed for 30 seconds using ozone water with an ozone concentration of 20 ppm, with the wafer rotating at 300 rpm, for oxide film formation, and thus a set of cleaning with ozone water and cleaning with an aqueous solution of hydrogen fluoride was repeated three times. Then, cleaning with DIW (pure water) was performed for 30 seconds. In all cleaning processes, the flow rate of the chemical solution was 1.0 L / min. For epitaxial silicon wafers, the supply pipe was inclined from top to bottom (towards the side closer to the silicon wafer) from the edge side in the radial direction of the silicon wafer towards the center, with an inclination angle of 4° in the vertical direction. Tests were conducted under three conditions for the position of the supply pipe during treatment with ozone water: at the center of the wafer, and shifted 15 mm and 20 mm in the radial direction from the center of the wafer. The thickness of the native oxide film on the wafer after single-wafer cleaning was measured using a spectroscopic ellipsometer at a total of 121 measurement points spaced 29.4 mm apart from the center of the wafer. The measurement points are shown in Figure 3 as dots.

[0039] FIG. 4 is a diagram showing the measurement results of the thickness of the formed native oxide film. As shown in FIG. 4, an oxide film of about 3 to 4 Å was formed on the wafer. FIG. 5 is a diagram showing the result of normalizing the thickness of the native oxide film in FIG. 4 by the maximum value. The horizontal axis of FIG. 4 and FIG. 5 is the measurement point (mm) represented by the radial distance from the center of the wafer, and the radial distance (mm) of the supply pipe from the center of the wafer. The vertical axis of FIG. 5 shows the value of the thickness of the native oxide film normalized by the maximum value. It can be said that the lower the standard deviation of the in-plane distribution of the thickness of the native oxide film, the higher the uniformity of the in-plane distribution. From this, it can be seen that the uniformity of the thickness of the native oxide film in the silicon wafer surface is higher when the position of the ozone water supply pipe is shifted in the radial direction of the wafer than when the position of the ozone water supply pipe is at the center position of the wafer.

[0040] With reference to Figure 5, the relationship between the standard deviation of the oxide film thickness in the radial direction of the wafer and the difference between the maximum and minimum values ​​is shown in Table 1 below. From Table 1, it can be seen that the standard deviation and the difference between the maximum and minimum values ​​are reduced by shifting the position of the ozone water supply pipe in the radial direction of the wafer, that is, the uniformity of the oxide film thickness within the silicon wafer surface is improved. Also, when the distance from the center in the circumferential direction of the wafer is 15 mm, the results are similar to when the distance from the center in the circumferential direction of the wafer is 20 mm.

[0041] [Table 1]

[0042] As described in the embodiment, the cleaning conditions of the silicon wafer can be adjusted by using the difference between the maximum and minimum thicknesses of the native oxide film on the wafer as an index. For example, when the difference between the maximum and minimum thicknesses of the native oxide film on a silicon wafer cleaned under certain cleaning conditions is 0.1 or more, the in-plane distribution of the native oxide film is checked, and if the thickness of the native oxide film is thick around R / 2 (where R is the diameter) or at the outer periphery of the silicon wafer, the cleaning conditions to be adjusted can be, for example, by lowering the rotation speed of the silicon wafer during the final ozone water treatment, which is considered to improve the uniformity of the thickness of the native oxide film.

[0043] Next, the effect of shifting the supply position from the center of the wafer was examined depending on the type of chemical liquid. Figure 6 shows the results of comparing the uniformity of the thickness of the natural oxide film according to the type of chemical liquid. The conventional example shows the result when ozone water, hydrogen fluoride solution, and pure water are all supplied from the center of the wafer, the inventive example shows the result when ozone water is shifted 20 mm from the center of the wafer in the radial direction, and the hydrogen fluoride solution and pure water are supplied from the center of the wafer, and the comparative example shows the result when the hydrogen fluoride solution is shifted 20 mm from the center of the wafer, and the ozone water and pure water are supplied from the center of the wafer. Comparing these, it can be seen that the uniformity of the thickness of the natural oxide film of the inventive example was better than that of the conventional example and the comparative example. That is, good results were obtained when the supply position of ozone water was shifted from the center of the silicon wafer in the radial direction. Although the detailed mechanism is unknown, the inventors believe that the change in the liquid film due to the hydraulic jump that occurs when a chemical liquid such as ozone water is discharged affects the variation in the reaction speed of the chemical liquid in the radial direction of the wafer. Furthermore, the inventors believe that the removal and formation of native oxide films is not uniformly achieved by the treatment with ozone water and an aqueous solution of hydrogen fluoride, but rather that the uniformity of the oxide film is ensured by the balance of the two chemical solutions.

[0044] Next, we also carried out a verification in which the rotation speed of the silicon wafer during the final supply of ozone water was changed when the supply position of the ozone water was fixed at 15 mm from the center of the wafer. The rotation speeds were 100 rpm, 150 rpm, 200 rpm, and 300 rpm. Figure 7 shows the thickness distribution of the native oxide film when the rotation speed of the silicon wafer during the final treatment with ozone water was changed. It can be seen that by lowering the rotation speed during the final supply of ozone water, a better in-plane distribution of the thickness of the native oxide film could be obtained.

[0045] FIG. 8 is a diagram showing the result of normalizing the thickness of the native oxide film in FIG. 7 by the maximum value. Table 2 below shows the relationship between the standard deviation of the thickness of the native oxide film in the wafer radial direction and the difference between the maximum value and the minimum value with respect to FIG. 8. It can be seen from Table 2 that the standard deviation and the difference between the maximum value and the minimum value are further reduced compared to the previous invention example by lowering the rotation speed of the silicon wafer at the time of the final ozone water supply from the reference value (POR: Point of Reference), and therefore it can be said that the uniformity of the thickness of the native oxide film within the silicon wafer surface is very high. This is considered to be because the centrifugal force is reduced by lowering the rotation speed of the silicon wafer in the final ozone water treatment, which increases the oxidation reaction near the outer periphery, and the outer periphery is raised, resulting in further improved in-plane uniformity.

[0046] [Table 2] [Explanation of symbols]

[0047] 1: Supply tube 2: Supply pipe

Claims

1. A method for cleaning a single silicon wafer, comprising the steps of: a surface layer modification step of modifying a surface layer of the silicon wafer using ozone water having a concentration in the range of 20 to 30 ppm; an etching step of etching the surface layer of the silicon wafer after the surface modification step using an aqueous solution of hydrogen fluoride having a concentration in the range of 0.5 to 3.0 mass %; A rinsing step of rinsing the surface of the silicon wafer with pure water, In the surface modification step, the ozone water is supplied from a fixed position radially shifted from the center of the silicon wafer within a range of 5 mm to 75 mm, The method for cleaning a silicon wafer, wherein a rotation speed of the silicon wafer in the surface modification step, the etching step, and the rinsing step is within a range of 100 to 500 rpm.

2. 2. The silicon wafer cleaning method according to claim 1, wherein the position to which the ozone water is supplied is shifted in a radial direction from the center of the silicon wafer within a range of 15 mm to 20 mm.

3. 3. The method for cleaning a silicon wafer according to claim 1, further comprising the steps of: measuring a thickness of a native oxide film at intervals of 29.4 mm from the center of the silicon wafer having a diameter of 300 mm using a spectroscopic ellipsometer; and adjusting at least one of a position where the ozone water is supplied, a concentration of the ozone water, a concentration of the aqueous solution of hydrogen fluoride, a flow rate of the ozone water, a flow rate of the aqueous solution of hydrogen fluoride, and a rotation speed of the silicon wafer so that a difference between a maximum value and a minimum value of the thickness of the native oxide film in the radial direction of the silicon wafer when the measured thickness of the native oxide film is normalized by a maximum value is 0.1 or less.

4. A method for producing a silicon wafer, comprising carrying out the method for cleaning a silicon wafer according to claim 1 or 2.

Citation Information

Patent Citations

  • Method for measuring surface roughness of semiconductor substrate

    JP1994163662A

  • Deposition of oxide on surface of silicon wafer

    JP1995066195A

  • Formation of silicon nitride oxide film and manufacture of p type semiconductor element

    JP2000216156A

  • Method for cleaning wafer

    JP2002203824A

  • Substrate processing equipment and method therefor

    JP2004079755A