SEMICONDUCTOR NANOPARTICLE COMPLEX, SEMICONDUCTOR NANOPARTICLE COMPLEX DISPERSION, SEMICONDUCTOR NANOPARTICLE COMPLEX COMPOSITION, AND SEMICONDUCTOR NANOPARTICLE COMPLEX CURED FILM
A semiconductor nanoparticle composite with a core/shell structure and specific ligands allows high dispersion in polar media, maintaining fluorescence efficiency and heat resistance, addressing dispersion challenges in display technologies.
Patent Information
- Application Number
- JP2023126371
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-13
- Filing Date
- 2023-08-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-08-01
AI Technical Summary
Semiconductor nanoparticles synthesized in nonpolar dispersion media have high hydrophobicity, making them difficult to disperse in polar dispersion media, which are often toxic, and existing methods to disperse them in polar media reduce fluorescence efficiency or require high amounts of dispersants, limiting their application in display and other technologies.
A semiconductor nanoparticle composite with a core/shell structure containing In and P, halogen, and a ligand coordinated to the surface, featuring mercapto fatty acid esters with specific molecular weights and SP values, allowing dispersion in polar media at high mass fractions while maintaining high fluorescence quantum efficiency.
The composite achieves high dispersion in polar media with maintained fluorescence efficiency, heat resistance, and low viscosity, enabling applications in display technologies such as QD films and QD patterning.
Smart Images

Figure 0007574889000005 
Figure 0007574889000006 
Figure 0007574889000001
Abstract
Description
[Technical field]
[0001] The present invention relates to semiconductor nanoparticle composites. [Background technology]
[0002] Semiconductor nanoparticles (quantum dots, QDs) that are small enough to exhibit the quantum confinement effect have a band gap that depends on their particle size. Excitons formed in semiconductor nanoparticles by means of photoexcitation, charge injection, etc. recombine to emit photons with energy according to the band gap, so light emission at a desired wavelength can be obtained by appropriately selecting the composition of the semiconductor nanoparticles and their particle size.
[0003] In the early stages of research into semiconductor nanoparticles, the focus was on elements containing Cd and Pb. However, because Cd and Pb are subject to regulations such as the Restriction of the Use of Certain Hazardous Substances, research has been focused in recent years on non-Cd- and non-Pb-based semiconductor nanoparticles.
[0004] Semiconductor nanoparticles are being used in a variety of applications, including displays, biolabeling, solar cells, etc. For display applications, applications such as QD films, QD patterning, and self-luminous devices (QLEDs) are expected.
[0005] FIG. 2 shows an outline of a device configuration for converting the wavelength from a light source in a conventional display. As shown in FIG. 2, a blue LED 101 is used as a light source, and first, this blue light is converted into white light. For the conversion from blue light to white light, a QD film 102 formed by dispersing semiconductor nanoparticles in a resin and forming it into a film shape with a thickness of about 100 μm is suitably used. The white light obtained by a wavelength conversion layer such as the QD film 102 is further converted into red light, green light, and blue light by a color filter (R) 104, a color filter (G) 105, and a color filter (B) 106, respectively. Note that the polarizing plate is omitted in FIG. 2.
[0006] In recent years, development of a type of display (polarizing plate not shown) that uses QD patterning as a wavelength conversion layer without using a QD film, as shown in FIG. 1, is underway. In the type of display shown in FIG. 1, the blue light from the blue LED 1, which is the light source, is not converted to white light, but is directly converted from blue light to red light or from blue light to green light using QD patterning (7, 8). The QD patterning (7, 8) is formed by patterning semiconductor nanoparticles dispersed in a resin, and the thickness is about 5 μm to 10 μm due to the structural limitations of the display. For blue, blue light from the blue LED 1, which is the light source, is transmitted through a diffusion layer 9 containing a diffusing agent. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2013-136498 A [Non-patent literature]
[0008] [Non-Patent Document 1] Takashi Jin, "Semiconductor Quantum Dots, Their Synthesis and Applications to Life Sciences," Production and Technology, Vol. 63, No. 2, pp. 58-63, 2011 [Non-Patent Document 2] Fabien Dubois et al, “A Versatile Strategy for Quantum Dot Ligand Exchange” J.AM.CHEM.SOC Vol.129, No.3, p.482-483, 2007 [Non-Patent Document 3] Boon-Kin Pong et al, “Modified Ligand-Exchange for Efficient Solubilization of CdSe / ZnS Quantum Dots in Water: A Procedure Guided by Computational Studies” Langmuir Vol.24, No.10, p.5270-5276, 2008 [Non-Patent Document 4] Samsulida Abd. Rahman et al, “Thiolate-Capped CdSe / ZnS Core-Shell Quantum Dots for the Sensitive Detection of Glucose” Sensors Vol.17, No.7, p.1537, 2017 [Non-Patent Document 5] Whitney Nowak Wenger et al, “Functionalization of Cadmium Selenide Quantum Dots with Poly(ethylene glycol): Ligand Exchange, Surface Coverage, and Dispersion Stability” Langmuir, Vol.33, No.33, pp8239-8245, 2017 Summary of the Invention [Problem to be solved by the invention]
[0009] Semiconductor nanoparticles and semiconductor nanoparticle composites are generally prepared as dispersions by dispersing in a dispersion medium, and are applied in various fields. In particular, in display applications, a dispersion in a polar organic dispersion medium such as glycol ethers and glycol ether esters is used, and the dispersion is cured to form a QD film, a QD patterning, or other cured film. In order to increase the wavelength conversion efficiency, it is desirable for the mass fraction of semiconductor nanoparticles in the cured film to be high.
[0010] However, semiconductor nanoparticles and semiconductor nanoparticle composites synthesized in a nonpolar dispersion medium are highly hydrophobic and therefore easily dispersible in a nonpolar dispersion medium, but are difficult to disperse in a polar dispersion medium.
[0011] It is presumed that semiconductor nanoparticles and semiconductor nanoparticle composites synthesized in non-polar dispersion media have small dipole-dipole forces and hydrogen bonding forces. Therefore, among polar dispersion media, semiconductor nanoparticles can be dispersed in toluene and chloroform, which have small dipole-dipole forces and hydrogen bonding forces, just like semiconductor nanoparticles synthesized in organic solvents. However, these polar dispersion media are highly toxic and therefore not practical.
[0012] Ligand exchange method is known as a method for dispersing semiconductor nanoparticles in a polar dispersion medium. The ligand exchange method is a method for replacing the ligand contained in a semiconductor nanoparticle composite obtained by binding a ligand to the surface of a semiconductor nanoparticle with a ligand having a hydrophilic group. The semiconductor nanoparticle composite obtained in this way can be dispersed in a polar dispersion medium. However, the semiconductor nanoparticle composites disclosed in Non-Patent Documents 1 to 5 and Patent Document 1 have a problem that the luminous efficiency is reduced, although the semiconductor nanoparticles can be dispersed in a polar dispersion medium.
[0013] Another known method for making semiconductor nanoparticles dispersible in a polar dispersion medium is the encapsulation method. However, the encapsulation method is a method in which a semiconductor nanoparticle composite obtained by binding a ligand to the surface of the semiconductor nanoparticle is further coated with an amphiphilic polymer, which increases the amount of dispersant relative to the semiconductor nanoparticles, making it difficult to achieve a high mass fraction of the semiconductor nanoparticles. This makes it difficult to apply.
[0014] For these reasons, there is a demand for semiconductor nanoparticle composites that can be dispersed at a high mass fraction in a polar dispersion medium while maintaining a high fluorescence quantum efficiency (QY) of the semiconductor nanoparticles.
[0015] Furthermore, when forming a cured film such as a QD film or QD patterning, any curing method can be used to cure the dispersion. However, when the curing method is thermal curing, heat is applied to the dispersion of the semiconductor nanoparticle composite, and therefore the semiconductor nanoparticles and the semiconductor nanoparticle composite need to be heat resistant.
[0016] In addition, when forming a cured film such as a QD film or QD patterning, any curing method can be used to cure the dispersion, but depending on the curing method (e.g., for inkjet printing), the dispersion may be required to have a low viscosity.
[0017] Therefore, an object of the present invention is to provide a semiconductor nanoparticle composite that can be dispersed at a high mass fraction in a polar dispersion medium while maintaining the high fluorescence quantum efficiency (QY) of the semiconductor nanoparticles. Another object of the present invention is to provide a semiconductor nanoparticle composite that can be dispersed at a high mass fraction in a polar dispersion medium while maintaining the high fluorescence quantum efficiency (QY) of the semiconductor nanoparticles, and that has high heat resistance and is useful in applications where heat resistance is required. Another object of the present invention is to provide a semiconductor nanoparticle composite that can be dispersed at a high mass fraction in a polar dispersion medium while maintaining the high fluorescence quantum efficiency (QY) of the semiconductor nanoparticles, and that has a low viscosity of the dispersion when dispersed in the dispersion medium, and is useful in applications where a low viscosity of the dispersion is required. [Means for solving the problem]
[0018] The above problems are solved by the present invention described below. That is, the semiconductor nanoparticle composite (1) of the present invention is a semiconductor nanoparticle composite in which a ligand is coordinated to the surface of a semiconductor nanoparticle, The semiconductor nanoparticles are core / shell type semiconductor nanoparticles having a core containing In and P and one or more shell layers, the semiconductor nanoparticles further contain a halogen, and in the semiconductor nanoparticles, a molar ratio of the halogen to In is 0.80 to 15.00 in atomic terms; The ligand has the following general formula (1): HS-R1-COO-R2(1) (in general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group), The mercapto fatty acid ester has an SP value of 9.20 or more and a molecular weight of 700 or less, and the average SP value of the entire ligand is 9.10 to 11.00; The present invention provides a semiconductor nanoparticle composite characterized by the above.
[0019] The present invention (2) also provides the semiconductor nanoparticle composite according to (1), wherein the molecular weight of the mercapto fatty acid ester represented by the general formula (1) is 300 or more and 700 or less.
[0020] The present invention (3) also provides the semiconductor nanoparticle composite according to (1), wherein the molecular weight of the mercapto fatty acid ester represented by the general formula (1) is 300 or more and 600 or less.
[0021] The present invention (4) also provides the semiconductor nanoparticle composite according to (2) or (3), wherein the mass ratio of the ligand to the semiconductor nanoparticle (ligand / semiconductor nanoparticle) is 1.00 or less.
[0022] The present invention (5) also provides the semiconductor nanoparticle composite according to (2) or (3), wherein the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is 0.70 or less.
[0023] The present invention (6) also provides the semiconductor nanoparticle conjugate according to any one of (2) to (5), wherein the mass ratio of the ligand to the semiconductor nanoparticle (ligand / semiconductor nanoparticle) is 0.40 or more.
[0024] The present invention (7) also provides the semiconductor nanoparticle composite according to (1), wherein the molecular weight of the mercapto fatty acid ester represented by the general formula (1) is less than 300.
[0025] The present invention (8) also provides the semiconductor nanoparticle composite according to (7), wherein the mass ratio of the ligand to the semiconductor nanoparticle (ligand / semiconductor nanoparticle) is 0.40 or less.
[0026] The present invention (9) also provides a semiconductor nanoparticle composite according to any one of (1) to (8), characterized in that the content of the mercapto fatty acid ester represented by the general formula (1) in the total ligand is 40 mol % or more.
[0027] The present invention (10) also provides a semiconductor nanoparticle composite according to any one of (1) to (8), characterized in that the content of the mercapto fatty acid ester represented by the general formula (1) in the total ligand is 50 mol % or more.
[0028] The present invention (11) also provides a semiconductor nanoparticle composite according to any one of (1) to (8), characterized in that the content of the mercapto fatty acid ester represented by the general formula (1) in the total ligand is 60 mol % or more.
[0029] The present invention (12) also provides the semiconductor nanoparticle composite of any one of (1) to (11), wherein at least one of the shells is formed of ZnSe.
[0030] The present invention (13) also provides the semiconductor nanoparticle composite of any one of (1) to (12), wherein the shell has two or more layers, and the outermost layer of the shell is formed of ZnS.
[0031] The present invention (14) also provides the semiconductor nanoparticle composite of any of (1) to (13), characterized in that the shell comprises at least a first shell formed of ZnSe and covering an outer surface of the core, and a second shell formed of ZnS and covering an outer surface of the first shell.
[0032] The present invention (15) also relates to the compound represented by the general formula (1), wherein R2 is any one selected from the group consisting of an oligoethylene glycol group, a polyethylene glycol group, and an alkoxy group. Includes The present invention provides a semiconductor nanoparticle composite according to any one of (1) to (14), characterized in that:
[0033] The present invention (16) also relates to a compound represented by the general formula (1), R on the side not bonded to -COO- 2 of The present invention provides a semiconductor nanoparticle composite according to any one of (1) to (15), characterized in that the terminal group is any one selected from the group consisting of an alkyl group, an alkenyl group, and an alkynyl group.
[0034] The present invention (17) also provides the semiconductor nanoparticle conjugate according to any one of (1) to (16), wherein the ligand further comprises an aliphatic ligand.
[0035] The present invention (18) also provides a semiconductor nanoparticle composite according to (17), characterized in that the aliphatic ligand is one or more selected from the group consisting of aliphatic thiols, aliphatic carboxylic acids, and aliphatic phosphines.
[0036] The present invention (19) also provides the semiconductor nanoparticle composite according to any one of (1) to (18), wherein the quantum efficiency of the semiconductor nanoparticle composite after purification is 80% or more.
[0037] The present invention (20) also provides the semiconductor nanoparticle composite according to any one of (1) to (19), wherein the half width of the emission spectrum of the semiconductor nanoparticle composite is 38 nm or less.
[0038] The present invention (21) also provides a semiconductor nanoparticle composite dispersion liquid in which any one of the semiconductor nanoparticle composites (1) to (20) is dispersed in an organic dispersion medium.
[0039] The present invention (22) also provides a semiconductor nanoparticle composite composition in which any one of the semiconductor nanoparticle composites (1) to (20) is dispersed in a monomer or a prepolymer.
[0040] The present invention (23) also provides a semiconductor nanoparticle composite cured film in which any one of the semiconductor nanoparticle composites (1) to (20) is dispersed in a polymer matrix.
[0041] The present invention (24) also provides a semiconductor nanoparticle composite obtained by contacting a semiconductor nanoparticle which is a core / shell type semiconductor nanoparticle having a core containing In and P and one or more shell layers, and further contains a halogen and has a molar ratio of halogen to In of 0.80 to 15.00 in atomic terms, with a surface modification compound having a bonding group on one end side capable of bonding to the semiconductor nanoparticle, The surface modifying compound is represented by the following general formula (1): HS-R1-COO-R2(1) (in general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group), The mercapto fatty acid ester has an SP value of 9.20 or more and a molecular weight of 700 or less, and the average SP value of the entire surface modifying compound is 9.10 to 11.00; The present invention provides a semiconductor nanoparticle composite characterized by the above.
[0042] The present invention (25) also provides a semiconductor nanoparticle composite according to (24), characterized in that the surface modification compound further comprises an aliphatic group-containing surface modification compound having a binding group capable of binding to the semiconductor nanoparticle at one end and an aliphatic group at the other end.
[0043] In this application, the range indicated by "~" is the range including the numbers on both ends. Effect of the Invention
[0044] According to the present invention, it is possible to obtain a polar semiconductor nanoparticle while maintaining a high fluorescence quantum efficiency (QY). According to the present invention, a semiconductor nanoparticle composite can be provided that can be dispersed at a high mass fraction in a polar dispersion medium while maintaining a high fluorescence quantum efficiency (QY) of the semiconductor nanoparticles, and is also highly heat resistant and useful in applications where heat resistance is required. According to the present invention, a semiconductor nanoparticle composite can be provided that can be dispersed at a high mass fraction in a polar dispersion medium while maintaining a high fluorescence quantum efficiency (QY) of the semiconductor nanoparticles, and is also useful in applications where a low viscosity of the dispersion liquid is required when the semiconductor nanoparticles are dispersed in the dispersion medium. [Brief description of the drawings]
[0045] [Figure 1] FIG. 1 is a schematic diagram showing a QD device. [Diagram 2] FIG. 1 is a schematic diagram showing a QD device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0046] (Semiconductor nanoparticle composite) The semiconductor nanoparticle composite (A) of the present invention is a semiconductor nanoparticle composite in which a ligand is coordinated to the surface of a semiconductor nanoparticle, The semiconductor nanoparticles are core / shell type semiconductor nanoparticles having a core containing In and P and one or more shell layers, the semiconductor nanoparticles further contain a halogen, and a molar ratio of the halogen to In in the semiconductor nanoparticles is 0.80 to 15.00 in atomic terms; The ligand has the following general formula (1): HS-R1-COO-R2(1) (in general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group), The mercapto fatty acid ester has an SP value of 9.20 or more and a molecular weight of 700 or less, and the average SP value of the entire ligand is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the following:
[0047] The semiconductor nanoparticle composite of the present invention is a composite of a semiconductor nanoparticle and a ligand, in which the ligand is coordinated to the surface of the semiconductor nanoparticle. The semiconductor nanoparticle composite of the present invention is obtained by contacting the semiconductor nanoparticle with the ligand.
[0048] In the present invention, the semiconductor nanoparticle composite is a semiconductor nanoparticle composite having light emitting properties. The semiconductor nanoparticle composite of the present invention is a particle that absorbs light of 340 nm to 480 nm and emits light with an emission peak wavelength of 400 nm to 750 nm.
[0049] The full width at half maximum (FWHM) of the emission spectrum of the semiconductor nanoparticle composite of the present invention is preferably 38 nm or less, more preferably 35 nm or less. When the full width at half maximum of the emission spectrum is in the above range, color mixing can be reduced when the semiconductor nanoparticle composite is applied to a display or the like.
[0050] The semiconductor nanoparticle composite of the present invention preferably has a fluorescence quantum efficiency (QY) of 80% or more, more preferably 85% or more. When the semiconductor nanoparticle composite has a fluorescence quantum efficiency of 80% or more, more efficient color conversion can be achieved when the semiconductor nanoparticles are used in applications.
[0051] In the present invention, the optical properties of the semiconductor nanoparticle composite can be measured using a quantum efficiency measurement system. The semiconductor nanoparticle composite is dispersed in a dispersion liquid, and the emission spectrum is measured by applying excitation light. The fluorescence quantum efficiency (QY) and full width at half maximum (FWHM) are calculated from the emission spectrum after reexcitation correction, which is obtained by removing the reexcitation fluorescence emission spectrum of the fluorescence emitted by reexcitation from the emission spectrum obtained here. Examples of dispersion liquids include normal hexane, PGMEA, and chloroform.
[0052] (Semiconductor nanoparticles) The semiconductor nanoparticles constituting the semiconductor nanoparticle composite of the present invention are core / shell type semiconductor nanoparticles having a core containing In and P and one or more shell layers. In the semiconductor nanoparticles, the shell may be at least one layer, and examples of the semiconductor nanoparticles include core / shell type semiconductor nanoparticles consisting of a core and one shell layer, core / shell type semiconductor nanoparticles consisting of a core and two shell layers, and core / shell type semiconductor nanoparticles consisting of a core and three or more shell layers. In particular, by having two or more shell layers, the fluorescence quantum efficiency of the semiconductor nanoparticles can be maintained, and the semiconductor nanoparticle composite can also have high fluorescence quantum efficiency. In addition, the structure of the semiconductor nanoparticles may be such that the shell covers at least a part of the surface of the core, but a structure in which the shell covers the entire surface of the core is preferred, and a structure in which the shell uniformly covers the entire surface of the core is particularly preferred.
[0053] The shell preferably contains a shell having a composition containing Zn and Se, and at least one of the shells is preferably formed of ZnSe. When the semiconductor nanoparticle has two or more shell layers, the outermost shell is preferably a shell having a composition containing Zn and S, and more preferably ZnS.
[0054] In particular, when the shell consists of at least a first shell formed of ZnSe and covering the outer surface of the core particle, and a second shell formed of ZnS and covering the outer surface of the first shell, the fluorescence quantum efficiency can be increased.
[0055] As long as the effects of the present invention are not impaired, the composition in the shell does not necessarily have to be a stoichiometric composition, and each shell may contain elements other than Zn, Se, and S, and the shell may have one or more gradient shells in which the ratio of the elements constituting the shell changes within the shell.
[0056] In the present invention, whether or not the shell covers at least a portion of the core and the element distribution inside the shell can be confirmed by, for example, composition analysis using energy dispersive X-ray spectroscopy with a transmission electron microscope (TEM-EDX).
[0057] The semiconductor nanoparticles according to the semiconductor nanoparticle composite of the present invention contain a halogen. The molar ratio of halogen to In in the semiconductor nanoparticles is 0.80 to 15.00, preferably 1.00 to 15.00, in terms of atoms. The halogen contained in the semiconductor nanoparticles is preferably F, Cl, or Br. By containing halogen in the above range in the semiconductor nanoparticles, high fluorescence quantum efficiency and narrow half width can be obtained, and further, the generation of aggregates can be suppressed during the synthesis of the semiconductor nanoparticle composite described below. Note that the halogen is present at the interface between the core and shell of the semiconductor nanoparticles and / or in the shell of the semiconductor nanoparticles, so that the above-mentioned effects can be more effectively obtained.
[0058] In the semiconductor nanoparticles of the semiconductor nanoparticle composite of the present invention, the molar ratio of P to In is preferably 0.20 to 0.95 in atomic terms, and the molar ratio of Zn to In is preferably 10.00 to 60.00 in atomic terms.
[0059] The elements constituting the semiconductor nanoparticles can be analyzed using a high-frequency inductively coupled plasma emission spectrometer (ICP) or an X-ray fluorescence spectrometer (XRF).
[0060] An example of a method for producing semiconductor nanoparticles will be disclosed below. The core of the semiconductor nanoparticles can be formed by mixing the precursor of In, the precursor of P, and, if necessary, an additive in a solvent and heating the resulting precursor mixture. Coordinating or non-coordinating solvents are used as the solvent. Examples of solvents include 1-octadecene, hexadecane, squalane, oleylamine, trioctylphosphine, and trioctylphosphine oxide. Examples of the precursor of In include, but are not limited to, acetates, carboxylates, and halides containing In. Examples of precursors of P include, but are not limited to, organic compounds and gases containing P. When the precursor is a gas, the core can be formed by injecting the gas into a precursor mixture containing other gases and reacting the gas.
[0061] The semiconductor nanoparticles may contain one or more elements other than In and P, as long as the effect of the present invention is not impaired. In that case, the precursor of the element may be added during the core formation. Examples of additives include dispersants such as carboxylic acids, amines, thiols, phosphines, phosphine oxides, phosphinic acids, and phosphonic acids, but are not limited to these. The dispersant can also serve as a solvent.
[0062] After the core of the semiconductor nanoparticle is formed, a halide can be added as necessary to improve the light emitting properties of the semiconductor nanoparticle.
[0063] In one embodiment, a precursor solution in which an In precursor and, if necessary, a dispersant are added to a solvent is mixed under vacuum, and heated at 100°C to 300°C for 6 to 24 hours, after which a P precursor is added and heated at 200°C to 400°C for 3 to 60 minutes, and then cooled. A halogen precursor is further added and heat-treated at 25°C to 300°C, preferably 100°C to 300°C, more preferably 150°C to 280°C, to obtain a core particle dispersion liquid containing core particles.
[0064] By adding a shell-forming precursor to the synthesized core particle dispersion, the semiconductor nanoparticles can adopt a core / shell structure, thereby increasing the fluorescence quantum efficiency (QY) and stability.
[0065] The elements that make up the shell are thought to form an alloy, heterostructure, or amorphous structure on the surface of the core particle, but it is also possible that some of them migrate to the inside of the core particle by diffusion.
[0066] The added shell-forming element is mainly present near the surface of the core particle and plays a role in protecting the semiconductor nanoparticle from external factors. The core / shell structure of the semiconductor nanoparticle is preferably such that the shell covers at least a part of the core, and more preferably uniformly covers the entire surface of the core particle.
[0067] In one embodiment, a Zn precursor and a Se precursor are added to the aforementioned core particle dispersion liquid, and then the mixture is heated at 150° C. to 300° C., preferably 180° C. to 250° C., and then a Zn precursor and a S precursor are added, and the mixture is heated at 200° C. to 400° C., preferably 250° C. to 350° C. This allows core / shell type semiconductor nanoparticles to be obtained.
[0068] Here, although not particularly limited, examples of Zn precursors that can be used include carboxylates such as zinc acetate, zinc propionate, and zinc myristate, halides such as zinc chloride and zinc bromide, and organic salts such as diethylzinc. As the Se precursor, phosphine selenides such as tributylphosphine selenide, trioctylphosphine selenide, and tris(trimethylsilyl)phosphine selenide, selenols such as benzeneselenol and selenocysteine, and selenium / octadecene solutions can be used. As the S precursor, phosphine sulfides such as tributylphosphine sulfide, trioctylphosphine sulfide, and tris(trimethylsilyl)phosphine sulfide, thiols such as octanethiol, dodecanethiol, and octadecanethiol, and sulfur / octadecene solution can be used.
[0069] The shell precursors may be mixed in advance and added all at once or in multiple portions, or each may be added separately all at once or in multiple portions. When the shell precursors are added in multiple portions, each addition may be heated at a different temperature.
[0070] In the present invention, the method for producing semiconductor nanoparticles is not particularly limited, and in addition to the methods described above, any method may be used, including conventional production methods such as the hot injection method, the homogeneous solvent method, the reverse micelle method, and the CVD method.
[0071] (Ligand) The semiconductor nanoparticle composite of the present invention has a ligand coordinated to the surface of the semiconductor nanoparticle. The coordination described here means that the ligand chemically affects the surface of the semiconductor nanoparticle. The ligand may be bonded to the surface of the semiconductor nanoparticle by a coordinate bond or any other bonding mode (e.g., a covalent bond, an ionic bond, a hydrogen bond, etc.), or may not necessarily be bonded if at least a part of the surface of the semiconductor nanoparticle has a ligand.
[0072] In the semiconductor nanoparticle composite of the present invention, the ligand coordinated to the semiconductor nanoparticle contains a mercapto fatty acid ester represented by the following general formula (1). HS-R1-COO-R2(1)
[0073] In general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group. That is, the mercapto fatty acid ester represented by general formula (1) is a compound in which -SH is bonded to one side of R1 and -COO-R2 is bonded to the other side. In the semiconductor nanoparticle composite of the present invention, the ligand coordinated to the semiconductor nanoparticle may contain one type of mercapto fatty acid ester represented by general formula (1), or may contain two or more types of mercapto fatty acid ester represented by general formula (1).
[0074] By coordinating the mercapto fatty acid ester represented by the general formula (1) to semiconductor nanoparticles, it is possible to obtain a semiconductor nanoparticle composite having a high fluorescence quantum efficiency and a narrow half-value width.
[0075] In the general formula (1), examples of R1 include a methylene group (-CH2-), an ethylene group (-CH2CH2-), a propylene group (-CH2CH2CH2-), a methylethylene group (-CH(CH3)-), and a dimethylmethylene group (-C(CH3)2-).
[0076] In the general formula (1), R2 is not particularly limited as long as it is a hydrophilic group, and examples thereof include hydrophilic groups including groups such as an alkyl group, an alkynyl group, an alkenyl group, an alkoxy group, a hydroxyl group, an aldehyde group, a carboxyl group, an amino group, an imino group, a nitro group, a cyano group, a vinyl group, an aryl group, a halogeno group, a ketone group, an ether bond, an ester bond, and a siloxane bond. R2 is preferably a hydrophilic group having an oligoethylene glycol group, a polyethylene glycol group, or an alkoxy group, and is particularly preferably an oligoethylene glycol group or a polyethylene glycol group. When R2 is an oligoethylene glycol group, a polyethylene glycol group, and Alkoxy group Any one selected from the group consisting of The hydrophilic group allows the semiconductor nanoparticles to be dispersed at a high concentration in a polar solvent. R on the side not bonded to -COO- 2 ofThe terminal group is preferably any one selected from the group consisting of an alkyl group, an alkenyl group, and an alkynyl group. When the terminal group of R2 not bonded to the carboxyl group is any one selected from the group consisting of an alkyl group, an alkenyl group, and an alkynyl group, the interaction between the semiconductor nanoparticle composites is suppressed, and the semiconductor nanoparticles can be dispersed at a high concentration in a polar solvent.
[0077] The molecular weight of the mercapto fatty acid ester represented by general formula (1) is not more than 700. When the molecular weight of the mercapto fatty acid ester represented by general formula (1) is not more than 700, it becomes possible to disperse the semiconductor nanoparticles at a high concentration in a polar solvent.
[0078] In the present invention, the molecular weight of the mercapto fatty acid ester represented by the general formula (1) refers to the average molecular weight of the mercapto fatty acid ester represented by the general formula (1). The average molecular weight of the mercapto fatty acid ester represented by the general formula (1) is measured using a GPC method (gel permeation chromatography), and the number average of the obtained values is taken as the average molecular weight (number average molecular weight Mn).
[0079] Furthermore, the SP value of the mercapto fatty acid ester represented by the general formula (1) is 9.20 or more, preferably 9.20 to 12.00. When the SP value is in the above range, it becomes possible to disperse the semiconductor nanoparticles in a polar solvent. Here, the SP value is determined by calculation using the Y-MB method. In the present invention, when two or more mercapto fatty acid esters represented by the general formula (1) are used as ligands, the SP value of each mercapto fatty acid ester is multiplied by the volume fraction of each mercapto fatty acid ester, and the sum of the SP values is the SP value of the mercapto fatty acid ester. For example, when the mercapto fatty acid ester with SP value A1 is coordinated to the semiconductor nanoparticles in the following manner, P1 volume %, the mercapto fatty acid ester with SP value A2 is coordinated to the semiconductor nanoparticles in the following manner, the mercapto fatty acid ester SP value is expressed by the following formula (2). SP value of mercapto fatty acid ester = Σ(Ai × Pi / 100) (2)
[0080] In the semiconductor nanoparticle composite of the present invention, the ligand may contain a ligand other than the mercapto fatty acid ester represented by general formula (1). Such a ligand other than the mercapto fatty acid ester represented by general formula (1) is not particularly limited as long as it is a compound having a bonding group coordinated to the semiconductor nanoparticles on one end side, and can be used as a compound coordinated to the semiconductor nanoparticles, and can adjust the average SP value of the entire ligand to 9.20 to 11.00, preferably 9.20 to 10.00, when used in combination with the mercapto fatty acid ester represented by general formula (1).
[0081] The SP value of the ligand other than the mercapto fatty acid ester represented by the general formula (1) is not particularly limited, but is preferably 7.50 to 15.00, and particularly preferably 7.50 to 15.00.
[0082] The average SP value of all the ligands coordinated to the semiconductor nanoparticles is 9.20 to 11.00, preferably 9.20 to 10.00. When the average SP value of all the ligands coordinated to the semiconductor nanoparticles is within the above range, it becomes possible to disperse the semiconductor nanoparticles in a polar solvent. The SP value of the ligand can be calculated from the structural formula using the Y-MB method. When there are multiple types of ligands coordinated to the semiconductor nanoparticles, the SP value of each ligand is multiplied by the volume fraction of the ligand, and the sum of the average SP value of all the ligands is taken as the SP value of the ligand. For example, when P1 volume % of the ligands having an SP value of A1 and P2 volume % of the ligands having an SP value of A2 are present in the semiconductor nanoparticles, the SP value of the ligands is calculated by multiplying the SP value of each ligand by the volume fraction of the ligand, and the sum of the average SP value of all the ligands is taken as the SP value of the ligand. When coordinated with P2 volume %, the average SP value of all ligands is expressed by the following equation (3). Average SP value of all ligands = Σ(Ai × Pi / 100) (3)
[0083] As the ligand other than the mercapto fatty acid ester represented by the general formula (1), an aliphatic ligand is preferable. By including an aliphatic ligand as the ligand, the semiconductor nanoparticles can be dispersed at a high concentration in a polar solvent. Furthermore, dispersion is possible in organic solvents having a wider range of SP values. In addition, when applying to the composition and dispersion liquid described later, it becomes possible to expand the selection of dispersion media.
[0084] Examples of the aliphatic ligand include aliphatic thiols, aliphatic carboxylic acids, aliphatic phosphines, aliphatic phosphine oxides, and aliphatic amines, and from the viewpoint of the strength of the coordination force with the semiconductor nanoparticles, at least one selected from the group consisting of aliphatic thiols, aliphatic carboxylic acids, and aliphatic phosphines is preferred. The aliphatic group of the aliphatic ligand may contain a substituent or a heteroatom.
[0085] The content of the mercapto fatty acid ester represented by general formula (1) in the entire ligand is preferably 40 mol% or more, more preferably 50 mol% or more, and even more preferably 60 mol% or more. By setting the content of the mercapto fatty acid ester represented by general formula (1) in the entire ligand within the above range, the semiconductor nanoparticles can be dispersed in a polar solvent at a high concentration and the quantum efficiency can be increased.
[0086] The semiconductor nanoparticle composite (A) of the present invention may include the following first embodiment. The first embodiment of the semiconductor nanoparticle composite (A) of the present invention is a semiconductor nanoparticle composite (A) of the present invention in which the molecular weight of the mercapto fatty acid ester represented by general formula (1) is 300 or more and 700 or less, preferably 300 or more and 600 or less.
[0087] That is, the first embodiment of the semiconductor nanoparticle composite (A) of the present invention is a semiconductor nanoparticle composite in which a ligand is coordinated to the surface of a semiconductor nanoparticle, The semiconductor nanoparticles are core / shell type semiconductor nanoparticles having a core containing In and P and one or more shell layers, the semiconductor nanoparticles further contain a halogen, and in the semiconductor nanoparticles, a molar ratio of the halogen to In is 0.80 to 15.00 in atomic terms; The ligand has the following general formula (1): HS-R1-COO-R2(1) (in general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group), The mercapto fatty acid ester has an SP value of 9.20 or more, and a molecular weight of 300 or more and 700 or less, preferably 300 or more and 600 or less, and the average SP value of the entire ligand is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the above. When the molecular weight of the mercapto fatty acid ester represented by the general formula (1) is within the above range, sufficient steric hindrance is ensured for the semiconductor nanoparticles to disperse in the organic solvent, making it possible to disperse the semiconductor nanoparticles at a higher concentration, and further improving the heat resistance of the semiconductor nanoparticle composite. In the present invention, heat resistance means that when the semiconductor nanoparticle composite is heat-treated at a certain temperature, it can be redispersed after the heat treatment in the solvent in which it was dispersed before the heat treatment.
[0088] In one embodiment of the evaluation of heat resistance, the semiconductor nanoparticle composite is treated in an air atmosphere at 180°C for 1 hour, and then the heat resistance is judged based on whether or not the semiconductor nanoparticle composite can be redispersed in a good solvent for the semiconductor nanoparticle composite. A semiconductor nanoparticle composite that does not have sufficient heat resistance is likely to be redispersed in the heat treatment due to denaturation or elimination of the ligand. Dispersibility in a good solvent decreases significantly after heating.
[0089] In the first embodiment of the semiconductor nanoparticle composite (A) of the present invention, the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is preferably 1.00 or less, more preferably 0.70 or less. When the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is within the above range, it becomes possible to disperse the semiconductor nanoparticles at a high concentration in a polar solvent while maintaining the heat resistance of the semiconductor nanoparticle composite.
[0090] In the first embodiment of the semiconductor nanoparticle composite (A) of the present invention, the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is preferably 0.40 or more. When the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is in the above range, it becomes possible to disperse the semiconductor nanoparticles at a high concentration in a polar solvent while maintaining the heat resistance of the semiconductor nanoparticle composite.
[0091] The semiconductor nanoparticle composite (A) of the present invention may include the following second embodiment. The second embodiment of the semiconductor nanoparticle composite (A) of the present invention is a semiconductor nanoparticle composite (A) of the present invention in which the molecular weight of the mercapto fatty acid ester represented by general formula (1) is less than 300.
[0092] That is, the second embodiment of the semiconductor nanoparticle composite (A) of the present invention is a semiconductor nanoparticle composite in which a ligand is coordinated to the surface of a semiconductor nanoparticle, The semiconductor nanoparticles are core / shell type semiconductor nanoparticles having a core containing In and P and one or more shell layers, the semiconductor nanoparticles further contain a halogen, and in the semiconductor nanoparticles, a molar ratio of the halogen to In is 0.80 to 15.00 in atomic terms; The ligand has the following general formula (1): HS-R1-COO-R2(1) (in general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group), The mercapto fatty acid ester has an SP value of 9.20 or more and a molecular weight of less than 300, preferably 100 or more and less than 300; and the average SP value of the entire ligand is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the above. When the molecular weight of the mercapto fatty acid ester represented by general formula (1) is within the above range, the viscosity of the dispersion can be low even when the semiconductor nanoparticle composite is dispersed at a high mass fraction. In the present invention, the low viscosity of the dispersion when the semiconductor nanoparticle composite is dispersed at a high mass fraction means that the viscosity at 25°C is 30 cp or less when the semiconductor nanoparticle composite is dispersed in isobornyl acrylate so that the mass ratio of the semiconductor nanoparticles is 30.0 mass%.
[0093] In the second embodiment of the semiconductor nanoparticle composite (A) of the present invention, the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is preferably 0.40 or less. When the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is within the above range, it becomes possible to disperse the semiconductor nanoparticles at a high concentration in a polar solvent while suppressing an increase in the viscosity of the dispersion liquid in which the semiconductor nanoparticle composite is dispersed.
[0094] The semiconductor nanoparticle composite (B) of the present invention is a semiconductor nanoparticle composite obtained by contacting a semiconductor nanoparticle which is a core / shell type semiconductor nanoparticle having a core containing In and P and one or more shell layers, and further contains a halogen and has a molar ratio of halogen to In of 0.80 to 15.00 in atomic terms, with a surface modification compound having a bonding group that bonds to the semiconductor nanoparticle on one end side; The surface modifying compound is represented by the following general formula (1): HS-R1-COO-R2(1) (in general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group), The mercapto fatty acid ester has an SP value of 9.20 or more and a molecular weight of 700 or less, and the average SP value of the entire surface modifying compound is 9.10 to 11.00; The semiconductor nanoparticle composite is characterized by the following:
[0095] The semiconductor nanoparticle composite (B) of the present invention is a semiconductor nanoparticle composite obtained by contacting a semiconductor nanoparticle with a surface modification compound having a bonding group that bonds to the semiconductor nanoparticle on one end side. The method for contacting the semiconductor nanoparticle with the surface modification compound is not particularly limited, but an example of the method is adding the surface modification compound to a dispersion of semiconductor nanoparticles. Depending on the bonding strength of the surface modification compound to the semiconductor nanoparticles, heating or stirring may be performed when adding the surface modification compound.
[0096] The semiconductor nanoparticles related to semiconductor nanoparticle composite (B) of the present invention are the same as the semiconductor nanoparticles related to semiconductor nanoparticle composite (A) of the present invention.
[0097] Examples of the binding group in the surface modification compound having a binding group at one end thereof that bonds to a semiconductor nanoparticle include a thiol group, a carboxylic acid group, a phosphine group, a phosphine oxide group, an amine group, etc. Examples of the surface modification compound having a binding group at one end thereof that bonds to a semiconductor nanoparticle include the ligand in the semiconductor nanoparticle composite (A) of the present invention.
[0098] The semiconductor nanoparticle composite (B) of the present invention contains a mercapto fatty acid ester represented by the following general formula (1) as a surface modifying compound having a bonding group on one end thereof that bonds to the semiconductor nanoparticles. HS-R1-COO-R2(1)
[0099] In the semiconductor nanoparticle composite (B) of the present invention, the mercapto fatty acid ester represented by general formula (1), which is a surface modification compound, is the same as the mercapto fatty acid ester represented by general formula (1) in the semiconductor nanoparticle composite (A) of the present invention.
[0100] In the semiconductor nanoparticle composite (B) of the present invention, by using a mercapto fatty acid ester represented by general formula (1) as a surface modification compound, a semiconductor nanoparticle composite with high fluorescence quantum efficiency and narrow half-width can be obtained.
[0101] In the semiconductor nanoparticle composite (B) of the present invention, the molecular weight of the mercapto fatty acid ester represented by general formula (1) is not more than 700. When the molecular weight of the mercapto fatty acid ester represented by general formula (1) is not more than 700, it becomes possible to disperse the semiconductor nanoparticles at a high concentration in a polar solvent.
[0102] In the semiconductor nanoparticle composite (B) of the present invention, the mercapto fatty acid ester represented by general formula (1) has an SP value of 9.20 or more, preferably 9.20 to 12.00. When the SP value is within the above range, it becomes possible to disperse the semiconductor nanoparticles in a polar solvent.
[0103] In the semiconductor nanoparticle composite (B) of the present invention, a surface modifying compound having a bonding group on one end side that bonds to a semiconductor nanoparticle can include a surface modifying compound other than the mercapto fatty acid ester represented by the general formula (1). The surface modification compound other than the mercapto fatty acid ester is not particularly limited as long as it has a bonding group on one end side that bonds to the semiconductor nanoparticles, and can be used as a surface modification compound for semiconductor nanoparticles, and can adjust the average SP value of the entire surface modification compound to 9.20 to 11.00, preferably 9.20 to 10.00, when used in combination with the mercapto fatty acid ester represented by general formula (1).
[0104] The SP value of the surface modifying compound other than the mercapto fatty acid ester represented by the general formula (1) is not particularly limited, but is preferably 7.00 to 15.00, and particularly preferably 7.50 to 15.00.
[0105] The average SP value of all surface modification compounds having a bonding group on one end side capable of bonding to semiconductor nanoparticles is 9.20 to 11.00, preferably 9.20 to 10.00. When the average SP value of all surface modification compounds having a bonding group on one end side capable of bonding to semiconductor nanoparticles is within the above range, it becomes possible to disperse the semiconductor nanoparticles in a polar solvent.
[0106] As a surface modification compound other than the mercapto fatty acid ester represented by the general formula (1), an aliphatic group-containing surface modification compound having a bonding group that bonds to the semiconductor nanoparticles at one end and an aliphatic group at the other end is preferred. By including an aliphatic group-containing surface modification compound as the surface modification compound, the semiconductor nanoparticles can be dispersed at a high concentration in a polar solvent. Furthermore, dispersion is possible in organic solvents with a wider range of SP values. In addition, when applied to the composition and dispersion liquid described later, it becomes possible to expand the selection of dispersion media.
[0107] Examples of the aliphatic group-containing surface modification compound include aliphatic thiols, aliphatic carboxylic acids, aliphatic phosphines, aliphatic phosphine oxides, and aliphatic amines, and from the viewpoint of the strength of the coordination force with the semiconductor nanoparticles, at least one selected from the group consisting of aliphatic thiols, aliphatic carboxylic acids, and aliphatic phosphines is preferred. The aliphatic group of the aliphatic group-containing surface modification compound may contain a substituent or a heteroatom.
[0108] The content of the mercapto fatty acid ester represented by general formula (1) in the entire surface modification compound having a bonding group on one end side that bonds to semiconductor nanoparticles is preferably 40 mol% or more, more preferably 50 mol% or more, and even more preferably 60 mol% or more. By setting the content of the mercapto fatty acid ester represented by general formula (1) in the entire surface modification compound having a bonding group on one end side that bonds to semiconductor nanoparticles within the above range, the semiconductor nanoparticles can be dispersed at a high concentration in a polar solvent and the quantum efficiency can be increased.
[0109] The semiconductor nanoparticle composite (B) of the present invention may be exemplified by the following first embodiment. The first embodiment of the semiconductor nanoparticle composite (B) of the present invention is a semiconductor nanoparticle composite (B) of the present invention in which the molecular weight of the mercapto fatty acid ester represented by general formula (1) is 300 or more and 700 or less, preferably 300 or more and 600 or less.
[0110] That is, the first form of the semiconductor nanoparticle composite (B) of the present invention is a semiconductor nanoparticle composite obtained by contacting a semiconductor nanoparticle which is a core / shell type semiconductor nanoparticle having a core containing In and P and one or more shell layers, and further contains a halogen and has a molar ratio of halogen to In of 0.80 to 15.00 in atomic terms, with a surface modification compound having a bonding group that bonds to the semiconductor nanoparticle on one end side, The surface modifying compound is represented by the following general formula (1): HS-R1-COO-R2(1) (in general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group), The SP value of the mercapto fatty acid ester is 9.20 or more, and the mercapto fatty acid The molecular weight of the ester is 300 or more and 700 or less, preferably 300 or more and 600 or less, and the average SP value of the entire surface modifying compound is 9.10 to 11.00; When the molecular weight of the mercapto fatty acid ester represented by general formula (1) is within the above range, sufficient steric hindrance is ensured for the semiconductor nanoparticles to disperse in the organic solvent, making it possible to disperse the semiconductor nanoparticles at a higher concentration, and further improving the heat resistance of the semiconductor nanoparticle composite.
[0111] In the first embodiment of the semiconductor nanoparticle composite (B) of the present invention, the mass ratio of the surface modification compound to the semiconductor nanoparticles (surface modification compound / semiconductor nanoparticles) is preferably 1.00 or less, and more preferably 0.70 or less. When the mass ratio of the surface modification compound to the semiconductor nanoparticles (surface modification compound / semiconductor nanoparticles) is within the above range, it becomes possible to disperse the semiconductor nanoparticles at a high concentration in a polar solvent while maintaining the heat resistance of the conductor nanoparticle composite.
[0112] In the first embodiment of the semiconductor nanoparticle composite (B) of the present invention, the mass ratio of the surface modification compound to the semiconductor nanoparticles (surface modification compound / semiconductor nanoparticles) is preferably 0.40 or more. When the mass ratio of the surface modification compound to the semiconductor nanoparticles (surface modification compound / semiconductor nanoparticles) is within the above range, it becomes possible to disperse the semiconductor nanoparticles at a high concentration in a polar solvent while maintaining the heat resistance of the semiconductor nanoparticle composite.
[0113] The semiconductor nanoparticle composite (B) of the present invention may include the following second embodiment. The second embodiment of the semiconductor nanoparticle composite (B) of the present invention is a semiconductor nanoparticle composite (B) of the present invention in which the molecular weight of the mercapto fatty acid ester represented by general formula (1) is less than 300.
[0114] That is, the second form of the semiconductor nanoparticle composite (B) of the present invention is a core / shell type semiconductor nanoparticle having a core containing In and P and one or more shell layers, and further containing a halogen, and is a semiconductor nanoparticle composite obtained by contacting a semiconductor nanoparticle having a molar ratio of halogen to In of 0.80 to 15.00 in atomic terms with a surface modification compound having a bonding group that bonds to the semiconductor nanoparticle on one end side, The surface modifying compound is represented by the following general formula (1): HS-R1-COO-R2(1) (in general formula (1), R1 represents an alkylene group having 1 to 3 carbon atoms, and R2 represents a hydrophilic group), The mercapto fatty acid ester has an SP value of 9.20 or more, and a molecular weight of less than 300, preferably 100 or more and less than 300; and the average SP value of the entire surface modifying compound is 9.10 to 11.00; When the molecular weight of the mercapto fatty acid ester represented by general formula (1) is within the above range, the viscosity of the dispersion liquid in which the semiconductor nanoparticle composite is dispersed can be reduced.
[0115] In the second form of the semiconductor nanoparticle composite (B) of the present invention, the mass ratio of the surface modification compound to the semiconductor nanoparticles (surface modification compound / semiconductor nanoparticles) is preferably 0.40 or less. When the mass ratio of the surface modification compound to the semiconductor nanoparticles (surface modification compound / semiconductor nanoparticles) is within the above range, it becomes possible to disperse the semiconductor nanoparticles at a high concentration in a polar solvent while suppressing an increase in the viscosity of the dispersion liquid in which the semiconductor nanoparticle composite is dispersed.
[0116] (Regarding purification) The semiconductor nanoparticle composite of the present invention can be separated and purified from the reaction solution as necessary. As a purification method, the semiconductor nanoparticle composite is aggregated using a poor solvent, and then the semiconductor nanoparticle composite is separated and purified from the reaction solution. A method for isolating the body-nanoparticle complex is used.
[0117] In one embodiment, the semiconductor nanoparticle composites can be precipitated from the dispersion by adding a polarity-reversing solvent such as acetone. The precipitated semiconductor nanoparticle composites can be collected by filtration or centrifugation, while the supernatant containing unreacted starting materials and other impurities can be discarded or reused. The precipitated semiconductor nanoparticle composites can then be washed with additional dispersion medium and dispersed again. This purification process can be repeated, for example, 2-4 times, or until the desired purity is reached.
[0118] In the present invention, in addition to the methods described above, any method such as coagulation, liquid-liquid extraction, distillation, electrodeposition, size exclusion chromatography and / or ultrafiltration may be used alone or in combination as a method for purifying the semiconductor nanoparticle composite.
[0119] (Semiconductor nanoparticle composite dispersion) The semiconductor nanoparticle composite of the present invention can be dispersed in a polar dispersion medium to form a semiconductor nanoparticle composite dispersion liquid. In the present invention, the state in which the semiconductor nanoparticle composite is dispersed in a dispersion medium refers to a state in which the semiconductor nanoparticle composite does not precipitate or does not remain as visible turbidity (cloudiness) when the semiconductor nanoparticle composite and the dispersion medium are mixed. Note that the semiconductor nanoparticle composite dispersed in the dispersion medium is referred to as a semiconductor nanoparticle composite dispersion liquid.
[0120] The semiconductor nanoparticle composite of the present invention disperses in organic dispersion media having an SP value of 8.50 or more, and further in organic dispersion media having an SP value of 9.00 or more and organic dispersion media having an SP value of 10.00 or more, to form a semiconductor nanoparticle composite dispersion liquid.
[0121] The SP value here is a value calculated from the Hansen solubility parameter in the same manner as in the method for determining the SP value of the polar ligand. The Hansen solubility parameter is described in a handbook, for example, "Hansen Solubility Parameters: A User's Guide to Solubility Parameters" in the "Hansen Solubility Parameters" section. The dispersion medium can be determined by using the values in “The Handbook of Polymerization”, 2nd edition, C. M. Hansen (2007), or the program in Practice (HSPiP) provided by Hanson and Abbot et al. (2nd edition). For organic dispersion media not described in the Handbook, the dispersion medium can be determined by calculation using the Y-MB method.
[0122] In the present invention, examples of the organic dispersion medium for the semiconductor nanoparticle composite dispersion of the present invention include alcohols such as methanol, ethanol, isopropyl alcohol, and normal propyl alcohol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone; esters such as methyl acetate, ethyl acetate, isopropyl acetate, normal propyl acetate, normal butyl acetate, and ethyl lactate; ethers such as diethyl ether, dipropyl ether, dibutyl ether, and tetrahydrofuran; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, and propylene glycol. Glycol ethers such as propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, propylene glycol dimethyl ether, dipropylene glycol dimethyl ether, propylene glycol diethyl ether, and dipropylene glycol diethyl ether; and glycol ether esters such as ethylene glycol acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate (PGMEA), and dipropylene glycol monoethyl ether acetate. By dispersing the semiconductor nanoparticle composite of the present invention in these organic dispersion media, the semiconductor nanoparticle composite can be used while maintaining its dispersibility when applied to dispersion in cured films or resins, as described below.
[0123] In particular, in the semiconductor nanoparticle composite of the present invention, it is possible to select polar organic dispersion media such as alcohols, glycol ethers, and glycol ether esters as the organic dispersion medium. By dispersing the semiconductor nanoparticle composite of the present invention in these organic dispersion media, the semiconductor nanoparticle composite can be used while maintaining its dispersibility when applied to dispersion in a cured film or resin, which will be described later. In particular, PGMEA and PGME are commonly used as dilution solvents in the field of photoresists, and if the semiconductor nanoparticle composite can be dispersed in PGMEA and PGME, the semiconductor nanoparticle composite can be widely applied to the photoresist field.
[0124] By adopting the above-mentioned configuration, the semiconductor nanoparticle composite of the present invention can be dispersed in an organic dispersion medium at a high mass fraction, and as a result, the mass fraction of the semiconductor nanoparticles in the semiconductor nanoparticle composite dispersion can be made 20 mass% or more, further 30 mass% or more, and even 35 mass% or more.
[0125] Furthermore, in the present invention, a monomer can be selected as a dispersion medium for the semiconductor nanoparticle composite dispersion of the present invention. The monomer is not particularly limited, but is preferably a (meth)acrylic monomer that allows a wide range of applications for the semiconductor nanoparticles. According to the application of the semiconductor nanoparticle composite dispersion, the (meth)acrylic monomer may be selected from methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, isoamyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, 3,5,5-trimethylcyclohexanol (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, methoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, methoxytriethylene glycol acrylate, 2-ethylhexyl diglycol acrylate, methoxypolyethylene glycol acrylate, methoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, methoxytriethylene glycol acrylate, 2-ethylhexyl diglycol acrylate, methoxypolyethylene glycol acrylate, methoxyethyl (meth) ... Dipropylene glycol acrylate, phenoxyethyl (meth)acrylate, 2-phenoxydiethylene glycol (meth)acrylate, 2-phenoxypolyethylene glycol (meth)acrylate (n≒2), tetrahydrofurfuryl (meth)acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, dicyclopentanyloxyl ether ethyl (meth)acrylate, isobornyloxylethyl (meth)acrylate, adamantyl (meth)acrylate, dimethyladamantyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, benzyl (meth)acrylate, ω-carboxy-polycaprolactone (n≒2) monoacrylate, 2-hydroxy-3-phenoxypropyl acrylate, 2-hydroxy-3-phenoxyethyl (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, (3-ethyloxetan-3-yl)methyl (meth)acrylate, o-phenylphenol ethoxy (meth)acrylate, dimethylamino (meth)acrylate, diethylamino (meth)acrylate, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, glycidyl (meth)acrylate, 2-(meth)acryloyloxyethyl phosphate, acryloylmorpholine, dimethylacrylamide, dimethylaminopropylacrylamide, isopropylacrylamide, diethylacrylamide, hydroxyethylacrylamide, and N-acryloyloxyethyl phthalate. The acrylic monomer is selected from (meth)acrylic monomers such as acryloyloxyethylhexahydrophthalimide. These may be used alone or in combination of two or more. In particular, the acrylic monomer is preferably one or a mixture of two or more selected from lauryl (meth)acrylate and 1,6-hexadiol di(meth)acrylate depending on the application of the semiconductor nanoparticle composite dispersion liquid.
[0126] In the present invention, a prepolymer can be selected as the dispersion medium of the semiconductor nanoparticle composite dispersion of the present invention. The prepolymer is not particularly limited, but examples thereof include acrylic resin prepolymer, silicone resin prepolymer, and epoxy resin prepolymer.
[0127] (Semiconductor nanoparticle composite composition) In the present invention, a monomer or prepolymer can be selected as the dispersion medium of the semiconductor nanoparticle composite dispersion of the present invention to form a semiconductor nanoparticle composite composition. That is, the semiconductor nanoparticle composite composition of the present invention is a semiconductor nanoparticle composite composition in which the semiconductor nanoparticle composite of the present invention is dispersed in a monomer or prepolymer. The monomer or prepolymer is not particularly limited, but examples thereof include radical polymerizable compounds containing ethylenically unsaturated bonds, siloxane compounds, epoxy compounds, isocyanate compounds, and phenol derivatives. Examples of the monomer include the monomers used as the dispersion medium described above. Examples of the prepolymer include the prepolymers used as the dispersion medium described above.
[0128] Furthermore, the semiconductor nanoparticle composite composition of the present invention may contain a crosslinking agent, which is selected from polyfunctional (meth)acrylates, polyfunctional silane compounds, polyfunctional amines, polyfunctional carboxylic acids, polyfunctional thiols, polyfunctional alcohols, polyfunctional isocyanates, etc., depending on the type of monomer in the semiconductor nanoparticle composite composition of the present invention.
[0129] Furthermore, the semiconductor nanoparticle composite composition of the present invention may further contain various organic solvents that do not affect curing, such as aliphatic hydrocarbons such as pentane, hexane, cyclohexane, isohexane, heptane, octane, and petroleum ether, alcohols, ketones, esters, glycol ethers, glycol ether esters, aromatic hydrocarbons such as benzene, toluene, xylene, and mineral spirits, and alkyl halides such as dichloromethane and chloroform. The above organic solvents can be used not only for diluting the semiconductor nanoparticle composite composition, but also as organic dispersion media. That is, it is also possible to disperse the semiconductor nanoparticle composite of the present invention in the above organic solvent to obtain a semiconductor nanoparticle composite dispersion liquid.
[0130] Furthermore, the semiconductor nanoparticle composite composition of the present invention may contain appropriate initiators, scattering agents, catalysts, binders, surfactants, adhesion promoters, antioxidants, ultraviolet absorbers, anti-aggregation agents, dispersants, and the like, depending on the type of monomer in the semiconductor nanoparticle composite composition.
[0131] Furthermore, in order to improve the optical properties of the semiconductor nanoparticle composite composition of the present invention or the semiconductor nanoparticle composite cured film of the present invention described later, the semiconductor nanoparticle composite composition may contain a scattering agent. The scattering agent is a metal oxide such as titanium oxide or zinc oxide, and the particle size thereof is preferably 100 nm to 500 nm. From the viewpoint of the scattering effect, the particle size of the scattering agent is more preferably 200 nm to 400 nm. By including a scattering agent, the absorbance is improved by about two times. The content of the scattering agent in the semiconductor nanoparticle composite composition of the present invention is preferably 2 mass % to 30 mass % relative to the composition, and more preferably 5 mass % to 20 mass % from the viewpoint of maintaining the patternability of the composition.
[0132] Due to the configuration of the semiconductor nanoparticle composite of the present invention, The mass fraction of the semiconductor nanoparticles can be 30 mass% or more. By setting the mass fraction of the semiconductor nanoparticles in the semiconductor nanoparticle composite composition to 30 mass% to 95 mass%, the semiconductor nanoparticle composite and semiconductor nanoparticles can be dispersed at a high mass fraction in the cured film described below.
[0133] When the semiconductor nanoparticle composite composition of the present invention is formed into a 10 μm film, the absorbance of the film with respect to light having a wavelength of 450 nm from the normal direction is preferably 1.0 or more, more preferably 1.3 or more, and even more preferably 1.5 or more. This allows efficient absorption of backlight light, thereby making it possible to reduce the thickness of the cured film described below and to miniaturize the device to which the composition is applied.
[0134] (Diluted Composition) The diluted composition is obtained by diluting the aforementioned semiconductor nanoparticle composite composition of the present invention with an organic solvent.
[0135] The organic solvent for diluting the semiconductor nanoparticle composite composition is not particularly limited, and examples thereof include aliphatic hydrocarbons such as pentane, hexane, cyclohexane, isohexane, heptane, octane, and petroleum ether, alcohols, ketones, esters, glycol ethers, glycol ether esters, aromatic hydrocarbons such as benzene, toluene, xylene, and mineral spirits, and alkyl halides such as dichloromethane and chloroform. Among these, glycol ethers and glycol ether esters are preferred from the viewpoints of solubility in a wide range of resins and uniformity of the coating when applied.
[0136] (Cured film of semiconductor nanoparticle composite) The semiconductor nanoparticle composite cured film of the present invention refers to a film containing the semiconductor nanoparticle composite of the present invention and being cured. The semiconductor nanoparticle composite cured film of the present invention can be obtained by curing the above-mentioned semiconductor nanoparticle composite composition or diluted composition into a film.
[0137] The semiconductor nanoparticle composite cured film of the present invention contains the semiconductor nanoparticles according to the semiconductor nanoparticle composite of the present invention, ligands coordinated to the surfaces of the semiconductor nanoparticles, and a polymer matrix. In other words, the semiconductor nanoparticle composite cured film of the present invention is a cured film in which the semiconductor nanoparticle composite of the present invention is dispersed in a polymer matrix.
[0138] Examples of the polymer matrix include, but are not limited to, (meth)acrylic resin, silicone resin, epoxy resin, silicone resin, maleic acid resin, butyral resin, polyester resin, melamine resin, phenolic resin, and polyurethane resin. The semiconductor nanoparticle composite cured film of the present invention may be obtained by curing the above-mentioned semiconductor nanoparticle composite composition of the present invention. The semiconductor nanoparticle composite cured film of the present invention may further contain a crosslinking agent.
[0139] The method for curing the film is not particularly limited, but the film can be cured by a curing method suitable for the composition constituting the film, such as heat treatment or ultraviolet treatment.
[0140] The semiconductor nanoparticles and the ligands coordinated to the surfaces of the semiconductor nanoparticles contained in the semiconductor nanoparticle composite cured film of the present invention preferably constitute the semiconductor nanoparticle composite of the present invention described above. By configuring the semiconductor nanoparticle composite contained in the semiconductor nanoparticle composite cured film of the present invention as described above, it is possible to disperse the semiconductor nanoparticle composite in the cured film at a higher mass fraction. The mass fraction of the semiconductor nanoparticles in the semiconductor nanoparticle composite cured film is desirably 30 mass% or more, and more desirably 40 mass% or more. However, if the content is 70 mass % or more, the composition constituting the film will become less, making it difficult to cure and form the film.
[0141] The semiconductor nanoparticle composite cured film of the present invention contains semiconductor nanoparticle composites at a high mass fraction, and therefore the absorbance of the semiconductor nanoparticle composite cured film can be increased. When the semiconductor nanoparticle composite cured film of the present invention has a thickness of 10 μm, the absorbance of the semiconductor nanoparticle composite cured film is preferably 1.0 or more, more preferably 1.3 or more, and even more preferably 1.5 or more, for light with a wavelength of 450 nm from the normal direction of the semiconductor nanoparticle composite cured film.
[0142] Furthermore, since the semiconductor nanoparticle composite cured film of the present invention contains a semiconductor nanoparticle composite having high luminescence properties, it is possible to provide a semiconductor nanoparticle composite cured film having high luminescence properties. The fluorescence quantum efficiency of the semiconductor nanoparticle composite cured film of the present invention is preferably 70% or more, and more preferably 80% or more.
[0143] In order to miniaturize devices to which the semiconductor nanoparticle composite cured film of the present invention is applied, the thickness of the semiconductor nanoparticle composite cured film of the present invention is preferably 50 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less.
[0144] (Semiconductor nanoparticle composite patterned film and display element) The semiconductor nanoparticle composite patterned film can be obtained by forming the above-mentioned semiconductor nanoparticle composite composition or dilution composition into a film pattern. The method for forming the semiconductor nanoparticle composite composition and dilution composition into a pattern is not particularly limited, and examples thereof include spin coating, bar coating, inkjet, screen printing, and photolithography.
[0145] The display element uses the semiconductor nanoparticle composite patterned film. For example, by using the semiconductor nanoparticle composite patterned film as a wavelength conversion layer, a display element having excellent fluorescent quantum efficiency can be provided.
[0146] It will be understood that the structures and / or methods described herein are presented as examples, and that numerous variations are possible, and that these specific examples or examples should not be taken in a limiting sense. A particular procedure or method described herein may represent one of many process methods. Thus, various acts illustrated and / or described may be performed in the order illustrated and / or described, or may be omitted. Similarly, the order of the methods described above may be altered.
[0147] The subject matter of the present disclosure includes all novel and non-obvious combinations and subcombinations of the various methods, systems, and structures disclosed herein, as well as other features, functions, acts, and / or properties, and all equivalents thereof. EXAMPLES
[0148] EXAMPLES The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these.
[0149] (Ligand) The ligands used in the examples and comparative examples were prepared as follows. In the following, PEG refers to a polyethylene glycol chain, and "-(CH2CH2O)n The structure is represented by "-CH3". <Preparation of single ligand> (Method for preparing 1,1-dimethyl-3-oxobutyl mercaptopropionate) In a flask, 4.2 g of 3-mercaptopropionic acid (40 mmol), 4.7 g of diacetone alcohol (40 mmol), 5.4 g of 1-hydroxybenzotriazole (40 mmol), 100 mL of methylene chloride, and 7.7 g of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (40 mmol) were mixed under a nitrogen atmosphere. The solution was reacted at room temperature for 60 minutes, and then the reaction solution was transferred to a separatory funnel and washed with saturated sodium bicarbonate water, water, and saturated saline in that order. The resulting organic phase was dried using magnesium sulfate, filtered, and concentrated by evaporation. The concentrate was purified by column chromatography using hexane and ethyl acetate as the developing solvent to obtain the desired ligand (1,1-dimethyl-3-oxobutyl mercaptopropionate).
[0150] (Preparation method of thioglycolic acid PEG ester (molecular weight 470)) In a flask, 3.7 g of thioglycolic acid (40 mmol), 19.2 g of methoxy PEG-OH (molecular weight 400, 48 mmol), and 0.2 g of concentrated sulfuric acid were mixed under a nitrogen atmosphere. The solution was stirred at 60°C and the pressure was reduced to 30 mmHg or less, and reacted for 24 hours. After cooling the reaction solution to room temperature, it was dissolved in toluene and washed with saturated sodium bicarbonate water, water, and saturated saline in that order. The resulting organic phase was dried over magnesium sulfate, and then the organic phase was filtered and concentrated by evaporation to obtain the desired ligand (thioglycolic acid PEG ester, molecular weight 470).
[0151] (Preparation method of thioglycolic acid PEG ester (molecular weight 760)) Methoxy PEG-OH (molecular weight 400, 48 mmol) was changed to methoxy PEG-OH (molecular weight 690, 48 mmol), and the same preparation as above was carried out to obtain thioglycolic acid PEG ester with a molecular weight of 760.
[0152] (Preparation method of 3-mercaptopropionic acid PEG ester (molecular weight 550)) In a flask, 4.2 g of 3-mercaptopropionic acid (40 mmol), 21.6 g of methoxy PEG-OH (molecular weight 450, 48 mmol), and 0.2 g of concentrated sulfuric acid were mixed under a nitrogen atmosphere. The solution was stirred at 60°C and the pressure was reduced to 30 mmHg or less, and reacted for 24 hours. After cooling the reaction solution to room temperature, it was dissolved in toluene and washed with saturated sodium bicarbonate water, water, and saturated saline in that order. The organic phase obtained was dried using magnesium sulfate, and then filtered and concentrated by evaporation to obtain the desired ligand (3-mercaptopropionic acid PEG ester, molecular weight 550).
[0153] (Preparation method of 3-mercaptopropionic acid PEG ester (molecular weight 640)) Methoxy PEG-OH (molecular weight 450, 48 mmol) was changed to methoxy PEG-OH (molecular weight 550, 48 mmol), and the same preparation as above was carried out to obtain 3-mercaptopropionic acid PEG ester with a molecular weight of 760.
[0154] (Preparation method of 2-[2-(2-acetoxyethoxy)ethoxy]ethyl 3-mercaptopropionate) In a flask, 2.1 g of 3-mercaptopropionic acid (20 mmol), 1.2 g of acetic acid (20 mmol), 7.2 g of triethylene glycol (48 mmol), 100 mL of toluene, and 0.2 g of concentrated sulfuric acid were mixed under a nitrogen atmosphere. A Dean-Stark apparatus was attached to the flask, and the solution was reacted for 24 hours while stirring at 110°C. After cooling the reaction solution to room temperature, it was washed in turn with saturated sodium bicarbonate water, water, and saturated saline. The resulting organic phase was dried over magnesium sulfate, filtered, and concentrated by evaporation. The concentrate was purified by column chromatography using hexane and ethyl acetate as the developing solvent to obtain the desired ligand (2-[2-(2-acetoxyethoxy)ethoxy]ethyl 3-mercaptopropionate).
[0155] (Method for preparing 6-mercaptohexanoic acid PEG ester) In a flask, 5.9 g of 6-mercaptohexanoic acid (40 mmol), 19.2 g of methoxy PEG-OH (molecular weight 400, 48 mmol), and 0.2 g of concentrated sulfuric acid were mixed under a nitrogen atmosphere. The solution was stirred at 60°C and the pressure was reduced to 30 mmHg or less, and reacted for 24 hours. After cooling the reaction solution to room temperature, it was dissolved in toluene and washed with saturated sodium bicarbonate water, water, and saturated saline in that order. The organic phase obtained was dried using magnesium sulfate, and then the organic phase was filtered and concentrated by evaporation to obtain the desired ligand (6-mercaptohexanoic acid PEG ester, molecular weight 530).
[0156] (Preparation method of 2-[2-(2-levulinoxyethoxy)ethoxy]ethyl 3-mercaptopropionate) In a flask, 2.1 g of 3-mercaptopropionic acid (20 mmol), 2.3 g of levulinic acid (20 mmol), 6.0 g of triethylene glycol (40 mmol), 5.4 g of 1-hydroxybenzotriazole (40 mmol), 100 mL of methylene chloride, and 7.7 g of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (40 mmol) were mixed under a nitrogen atmosphere. The solution was reacted at room temperature for 60 minutes, and then the reaction solution was transferred to a separatory funnel and washed with saturated sodium bicarbonate water, water, and saturated saline in that order. The resulting organic phase was dried using magnesium sulfate, filtered, and concentrated by evaporation. The concentrate was purified by column chromatography using hexane and ethyl acetate as the developing solvent to obtain the desired ligand (2-[2-(2-levulinoxyethoxy)ethoxy]ethyl 3-mercaptopropionate).
[0157] (Method for preparing 2-[2-[2-(2-hexyloxyethoxy)ethoxy]ethoxy]ethyl 3-mercaptopropionate) In a flask, 4.2 g of 3-mercaptopropionic acid (40 mmol), 13.4 g of tetraethylene glycol monohexyl ether (48 mmol), 100 mL of toluene, and 0.2 g of concentrated sulfuric acid were mixed under a nitrogen atmosphere. A Dean-Stark apparatus was attached to the flask, and the solution was reacted for 24 hours while stirring at 110°C. After cooling the reaction solution to room temperature, it was washed in turn with saturated sodium bicarbonate water, water, and saturated saline. The resulting organic phase was dried over magnesium sulfate, filtered, and concentrated by evaporation. The concentrate was purified by column chromatography using hexane and ethyl acetate as the developing solvent to obtain the desired ligand (3-mercaptopropionic acid 2-[2-[2-(2-hexyloxyethoxy)ethoxy]ethoxy]ethyl).
[0158] [Example 1] An InP-based semiconductor nanoparticle composite was prepared according to the following method. (Preparation of core particles) Indium acetate (0.3 mmol) and zinc oleate (0.6 mmol) were added to a mixture of oleic acid (0.9 mmol), 1-dodecanethiol (0.1 mmol), and octadecene (10 mL), and the mixture was heated to about 120°C under vacuum (<20 Pa) and reacted for 1 hour. The mixture reacted under vacuum was placed in a nitrogen atmosphere at 25°C, tris(trimethylsilyl)phosphine (0.2 mmol) was added, and the mixture was heated to about 300°C and reacted for 10 minutes. The reaction solution was cooled to 25°C, octanoic acid chloride (1.1 mmol) was poured in, and the mixture was heated at about 250°C for 30 minutes, and then cooled to 25°C to obtain a dispersion of InP-based semiconductor nanoparticles.
[0159] (Precursor for shell formation) In preparing the shell, the following precursors were first prepared. (Preparation of Zn precursor solution) 40 mmol of zinc oleate was mixed with 75 mL of octadecene and heated at 110° C. for 1 hour under vacuum to prepare a Zn precursor with [Zn]=0.4 M. (Preparation of Se precursor (trioctylphosphine selenide)) 22 mmol of selenium powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain trioctylphosphine selenide with [Se] = 2.2 M. (Preparation of S precursor (trioctylphosphine sulfide)) 22 mmol of sulfur powder and 10 mL of trioctylphosphine were mixed in nitrogen and stirred until completely dissolved to obtain trioctylphosphine sulfide ([S] = 2.2 M).
[0160] Using each of the precursors obtained as described above, a shell was formed on the surface of the InP-based semiconductor nanoparticles (core) as follows. (Shell formation) The core dispersion was heated to 200°C. At 250°C, 6.0mL of Zn precursor solution and 2.0mL of trioctylphosphine selenide were added and reacted for 30 minutes to form a ZnSe shell on the surface of the InP-based semiconductor nanoparticles. Furthermore, 4.0mL of Zn precursor solution and 1.8mL of trioctylphosphine sulfide were added, and the temperature was raised to 280°C and reacted for 1 hour to form a ZnS shell. The obtained semiconductor nanoparticles were observed by STEM-EDS and were confirmed to have a core / shell structure. Dehydrated acetone was added to the solution in which the synthesized core / shell-structured semiconductor nanoparticles were dispersed, causing the semiconductor nanoparticles to aggregate. After centrifugation (4000 rpm, 10 minutes), the supernatant was removed and the semiconductor nanoparticles were redispersed in hexane. This process was repeated to obtain purified semiconductor nanoparticles.
[0161] (composition analysis) Elemental analysis of the semiconductor nanoparticles was performed using an inductively coupled plasma optical emission spectrometer (ICP) and an X-ray fluorescence spectrometer (XRF). In the ICP measurement, the purified semiconductor nanoparticles were dissolved in nitric acid, heated, and then diluted with water and measured using an ICP optical emission spectrometer (Shimadzu Corporation, ICPS-8100) with a calibration curve method. In the XRF measurement, a filter paper was soaked in the dispersion liquid, placed in a sample holder, and quantitative analysis was performed using an X-ray fluorescence spectrometer (Rigaku Corporation, ZSX100e). The molar ratio of halogen to In in the semiconductor nanoparticles is shown in Table 1.
[0162] (Preparation of semiconductor nanoparticle composites) In a flask, the purified semiconductor nanoparticles were dispersed in 1-octadecene to prepare a semiconductor nanoparticle 1-octadecene dispersion liquid. 10.0 g of the prepared semiconductor nanoparticle 1-octadecene dispersion liquid was placed in a flask, 3.6 g of thioglycolic acid PEG ester (molecular weight 470) as a mercapto fatty acid ester and 0.4 g of dodecanethiol as a non-polar ligand were added, and the mixture was stirred at 110°C for 60 minutes in a nitrogen atmosphere and cooled to 25°C to obtain a semiconductor nanoparticle composite. The reaction solution containing the semiconductor nanoparticle composite was transferred to a centrifuge tube and centrifuged at 4000G for 20 minutes, resulting in separation into a transparent 1-octadecene phase and a semiconductor nanoparticle composite phase. The 1-octadecene phase was removed, and the remaining semiconductor nanoparticle composite phase was collected. 5.0 mL of acetone was added to the obtained semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of normal hexane was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the transparent supernatant was removed and the precipitate was collected. This operation was repeated several times to obtain a purified semiconductor nanoparticle composite.
[0163] <Analysis> (Measurement of molecular weight of ligand) The molecular weight of the ligand was measured by the GPC method using a liquid chromatograph (LC-20: Shimadzu Corporation). First, the ligand was dissolved in THF (tetrahydrofuran) to obtain an eluent. The eluent was then placed in a column (KF-801, KF-803, KF-805: Shodex). The syneresis liquid was injected, and the number average molecular weight was calculated from the molecular weight distribution curve obtained. col READY_CAL SET Mp 102-40,000: Aldrich) was used.
[0164] (Fluorescence quantum efficiency measurement) The optical properties of the semiconductor nanoparticle composite were measured using a fluorescence quantum efficiency measurement system (QE-2100, manufactured by Otsuka Electronics). The semiconductor nanoparticle composite obtained by synthesis was dispersed in a dispersion medium, and a single light of 450 nm was applied as excitation light to obtain an emission spectrum. The fluorescence quantum efficiency (QY) and full width at half maximum (FWHM) were calculated from the emission spectrum after re-excitation correction, which was obtained by removing the re-excitation fluorescence emission spectrum of the portion of the fluorescence emitted by re-excitation from the emission spectrum obtained here. Propylene glycol monomethyl ether acetate (PGMEA) was used as the dispersion medium. The results obtained are shown in Table 2.
[0165] ( 1 H-NMR measurement) The purified semiconductor nanoparticle complex was analyzed for the ligands coordinated to the semiconductor nanoparticles using a nuclear magnetic resonance (NMR) device (JNM-LA400 manufactured by JEOL Ltd.). In all measurements, deuterated chloroform was used as the solvent and tetramethylsilane was used as the internal standard substance for chemical shifts. 1 H-NMR was measured. From the semiconductor nanoparticle composite obtained in Example 1, signals due to the alkyl group of dodecanethiol were observed around 0.8 to 1.6 ppm, and signals due to the polyethylene glycol skeleton were observed around 3.5 to 4.0 ppm. From the area ratio of these signals, the abundance ratio of each ligand was calculated. Based on the abundance ratio of each ligand, the average SP value of all ligands and the ratio of mercapto fatty acid ester to all ligands were calculated. The obtained results are shown in Tables 1 and 3.
[0166] (Thermogravimetric analysis) The purified semiconductor nanoparticle composite was heated to 550°C by differential thermogravimetry (DTA-TG), held for 10 minutes, and cooled. The residual mass after analysis was taken as the mass of the semiconductor nanoparticles, and the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) in the semiconductor nanoparticle composite was determined from this value. The results are shown in Tables 1 and 3.
[0167] (Dispersibility test) With reference to the above mass ratio, an organic dispersion medium was added to the semiconductor nanoparticle composite so that the semiconductor nanoparticle concentrations were 20.0 mass%, 30.0 mass%, and 35.0 mass%, respectively, and the dispersion state at that time was confirmed. Those that were dispersed were marked with "○", and those in which precipitation or turbidity was observed were marked with "×" in Tables 2 and 4. Propylene glycol monomethyl ether acetate (PGMEA) was used as the dispersion medium.
[0168] (Filterability test) A filterability test was conducted on the samples that could be used to prepare a semiconductor nanoparticle composite PGMEA dispersion with a semiconductor nanoparticle concentration of 20.0% by mass. 1 mL of the 20% by mass semiconductor nanoparticle composite PGMEA solution was weighed into a syringe and filtered using a PTFE syringe filter with a mesh size of 0.45 μm (filter diameter 13 mm). Samples that could be filtered using one syringe filter are marked with "◯", and samples that became clogged during the process are marked with "×" in Tables 2 and 4.
[0169] (Heat resistance test) 50 mg of the semiconductor nanoparticle composite was weighed into a sample tube and heated at 180°C for 60 minutes in an air atmosphere. The sample was air-cooled to room temperature, and 1 mL of chloroform was added to check the dispersion state at that time. Dispersed samples were marked with a "○", and precipitates and turbidity were observed. Those that were not satisfactory are marked with an "X" in Tables 2 and 4.
[0170] (Viscosity measurement) The semiconductor nanoparticle composite was dispersed in isobornyl acrylate so that the concentration of the semiconductor nanoparticles was 30.0% by mass to prepare a dispersion. The viscosity of the obtained dispersion was then measured at 25° C. using a TA Instruments AR-2000 rheometer. The measurement was performed at 0.1 s -1 After pre-shearing for 1 minute, -1 From 1000s -1 The shear rate was changed from 100s to 100s. -1 The viscosity at 30 cp or less was marked with "◎", that at more than 30 cp and less than 60 cp was marked with "◯", and that at more than 60 cp was marked with "×", and these are shown in Tables 2 and 4. Note that a hyphen (-) is entered for samples from which a 30 mass % semiconductor nanoparticle composite isobornyl acrylate dispersion could not be prepared.
[0171] Example 2 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 3.2 g of 3-mercaptopropionic acid PEG ester (molecular weight 550) was used as the mercapto fatty acid ester and 0.8 g of oleic acid was used as the aliphatic ligand.
[0172] Example 3 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 3.2 g of thioglycolic acid PEG ester (molecular weight 470) was used as the mercapto fatty acid ester and 0.8 g of ethylhexyl 3-mercaptopropionate was used instead of the aliphatic ligand.
[0173] Example 4 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 6.4 g of 3-mercaptopropionic acid PEG ester (molecular weight 640) was used as the mercapto fatty acid ester and 0.8 g of dodecanethiol was used as the aliphatic ligand.
[0174] Example 5 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 2.8 g of thioglycolic acid PEG ester (molecular weight 470) was used as the mercapto fatty acid ester and 1.2 g of dodecanethiol was used as the aliphatic ligand.
[0175] Example 6 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 2.4 g of thioglycolic acid PEG ester (molecular weight 470) was used as the mercapto fatty acid ester and 1.6 g of dodecanethiol was used as the aliphatic ligand.
[0176] Example 7 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 0.45 mmol of octanoic acid chloride was used when preparing the dispersion of core particles, and 3.6 g of 3-mercaptopropionic acid PEG ester (molecular weight 550) was used as the mercapto fatty acid ester and 0.4 g of dodecanethiol was used as the aliphatic ligand when preparing the semiconductor nanoparticle composite.
[0177] Example 8 The same procedure was carried out except that 2.5 mmol of octanoic acid chloride was used in the preparation of the dispersion of the core particles, 3.8 g of 3-mercaptopropionic acid PEG ester was used as the mercapto fatty acid ester, and 0.2 g of dodecanethiol was used as the aliphatic ligand in the preparation of the semiconductor nanoparticle composite. In the same manner as in Example 1, a semiconductor nanoparticle composite was obtained.
[0178] Example 9 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 3.6 g of 2-[2-[2-(2-hexyloxyethoxy)ethoxy]ethoxy]ethyl 3-mercaptopropionate was used as the mercapto fatty acid ester and 0.4 g of dodecanethiol was used as the aliphatic ligand.
[0179] Example 10 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 3.8 g of 2-[2-(2-levulinoxyethoxy)ethoxy]ethyl 3-mercaptopropionate was used as the mercapto fatty acid ester and 0.2 g of dodecanethiol was used as the aliphatic ligand.
[0180] Example 11 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 3.6 g of 1,1-dimethyl-3-oxobutyl 3-mercaptopropionate was used as the mercapto fatty acid ester and 0.4 g of trioctylphosphine was used as the aliphatic ligand.
[0181] Example 12 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 0.45 mmol of octanoic acid chloride was used when preparing the dispersion of core particles, and 3.2 g of 3-methoxybutyl 3-mercaptopropionate as the mercapto fatty acid ester and 0.8 g of dodecanethiol as the aliphatic ligand were used when preparing the semiconductor nanoparticle composite.
[0182] Example 13 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 2.5 mmol of octanoic acid chloride was used when preparing the dispersion of core particles, and 3.2 g of 1,1-dimethyl-3-oxobutyl 3-mercaptopropionate as the mercapto fatty acid ester and 0.8 g of dodecanethiol as the aliphatic ligand were used when preparing the semiconductor nanoparticle composite.
[0183] Example 14 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the step of preparing the semiconductor nanoparticle composite, 2.8 g of 3-methoxybutyl 3-mercaptopropionate was used as the mercapto fatty acid ester and 1.2 g of dodecanethiol was used as the aliphatic ligand.
[0184] Example 15 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 3.8 g of 2-[2-(2-acetoxyethoxy)ethoxy]ethyl 3-mercaptopropionate was used as the mercapto fatty acid ester and 0.05 g of dodecanethiol was used as the aliphatic ligand.
[0185] Example 16 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the step of preparing the semiconductor nanoparticle composite, 2.8 g of 3-methoxybutyl 3-mercaptopropionate was used as the mercapto fatty acid ester and 1.2 g of benzenethiol was used instead of the aliphatic ligand.
[0186] (Example 17) In the shell formation reaction, after the ZnSe shell was formed, the Zn precursor solution and trisulfide were The mixture was cooled to room temperature without adding octylphosphine. Furthermore, in the step of preparing the semiconductor nanoparticle composite, 3.2 g of 1,1-dimethyl-3-oxobutyl 3-mercaptopropionate was used as the mercapto fatty acid ester, and 0.8 g of dodecanethiol was used as the aliphatic ligand, and a semiconductor nanoparticle composite was obtained in the same manner as in Example 1.
[0187] Comparative Example 1 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the process of preparing the semiconductor nanoparticle composite, 9.6 g of thioglycolic acid PEG ester (molecular weight 760) was used as the mercapto fatty acid ester and 0.8 g of dodecanethiol was used as the aliphatic ligand.
[0188] Comparative Example 2 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 4.5 mmol of octanoic acid chloride was used when preparing the dispersion of core particles, and 3.6 g of thioglycolic acid PEG ester (molecular weight 470) was used as the mercapto fatty acid ester and 0.4 g of dodecanethiol was used as the aliphatic ligand when preparing the semiconductor nanoparticle composite.
[0189] Comparative Example 3 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that in the step of preparing the semiconductor nanoparticle composite, 3.2 g of 6-mercaptohexanoic acid PEG ester was used as the mercapto fatty acid ester and 0.8 g of dodecanethiol was used as the aliphatic ligand.
[0190] Comparative Example 4 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 2.0 g of thioglycolic acid PEG ester (molecular weight 470) was used as the mercapto fatty acid ester and 2.0 g of dodecanethiol was used as the aliphatic ligand in the process of producing the semiconductor nanoparticle composite. Chloroform was used as the solvent for measuring the fluorescence quantum yield.
[0191] Comparative Example 5 In the process of preparing the semiconductor nanoparticle composite, mercapto fatty acid ester was not added, and 4.0 g of dodecanethiol was used as an aliphatic ligand. The mixture was stirred at 110°C for 60 minutes under a nitrogen atmosphere, and cooled to 25°C to obtain a semiconductor nanoparticle composite. The reaction solution containing the semiconductor nanoparticle composite was transferred to a centrifuge tube, 100 mL of acetone was added, and the mixture was centrifuged at 4000G for 20 minutes, resulting in separation into a transparent supernatant and a semiconductor nanoparticle composite phase. The supernatant was removed, and the remaining semiconductor nanoparticle composite phase was collected. 5.0 mL of normal hexane was added to the obtained semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of acetone was added to the obtained dispersion, and the mixture was centrifuged at 4000G for 20 minutes. After centrifugation, the transparent supernatant was removed, and the precipitate was collected. This operation was repeated several times. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1 except for the above. Normal hexane was used as a solvent for measuring the fluorescence quantum yield.
[0192] Comparative Example 6 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 0.2 mmol of octanoic acid chloride was used when preparing the dispersion of core particles, and 3.2 g of 3-methoxybutyl 3-mercaptopropionate as the mercapto fatty acid ester and 0.8 g of dodecanethiol as the aliphatic ligand were used when preparing the semiconductor nanoparticle composite.
[0193] Comparative Example 7 In the process of preparing the semiconductor nanoparticle composite, 3.2 g of ethylhexyl 3-mercaptopropionate as the mercapto fatty acid ester and 0.8 g of dodecanethiol as the aliphatic ligand were used, and the mixture was stirred at 110°C for 60 minutes in a nitrogen atmosphere and then cooled to 25°C. A semiconductor nanoparticle composite was obtained. The reaction solution containing the semiconductor nanoparticle composite was transferred to a centrifuge tube, 100 mL of acetone was added, and the mixture was centrifuged at 4000 G for 20 minutes, resulting in separation into a transparent supernatant and a semiconductor nanoparticle composite phase. The supernatant was removed, and the remaining semiconductor nanoparticle composite phase was collected. 5.0 mL of normal hexane was added to the obtained semiconductor nanoparticle composite phase to prepare a dispersion. 50 mL of acetone was added to the obtained dispersion, and the mixture was centrifuged at 4000 G for 20 minutes. After centrifugation, the transparent supernatant was removed, and the precipitate was collected. This operation was repeated several times. A semiconductor nanoparticle composite was obtained in the same manner as in Example 1 except for the above. Chloroform was used as a solvent for measuring the fluorescence quantum yield.
[0194] Comparative Example 8 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 3.2 g of 2-hydroxyethyl 3-mercaptopropionate was used as the mercapto fatty acid ester and 0.8 g of trioctylphosphine was used as the aliphatic ligand in the step of producing the semiconductor nanoparticle composite. This semiconductor nanoparticle composite was not dispersed in chloroform or PGMEA, and fluorescence quantum yield measurement could not be performed.
[0195] Comparative Example 9 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that 4.5 mmol of octanoic acid chloride was used when preparing the dispersion of core particles, and 3.6 g of 3-methoxybutyl 3-mercaptopropionate as the mercapto fatty acid ester and 0.4 g of dodecanethiol as the aliphatic ligand were used when preparing the semiconductor nanoparticle composite.
[0196] Comparative Example 10 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that octanoic acid chloride was not added when preparing the dispersion liquid of the core particles.
[0197] Comparative Example 11 A semiconductor nanoparticle composite was obtained in the same manner as in Example 1, except that when preparing the dispersion of core particles, 0.3 mmol of indium chloride was added instead of indium acetate, and octanoyl chloride was not added. The indium chloride added during the preparation of the core particle dispersion generates hydrogen chloride as a by-product during synthesis, and it was found that the halogen content in the final semiconductor nanoparticles is lower than that in the case where a halogen precursor is added during the preparation of the core particle dispersion.
[0198] The meanings of the abbreviations shown in Tables 1 to 4 are as follows: MPAE: Mercapto fatty acid ester QD: Semiconductor nanoparticles DDT: Dodecanethiol TOP: Trioctylphosphine EHMP: Ethylhexyl 3-mercaptopropionate PGMEA: Propylene glycol monomethyl ether acetate
[0199] [Table 1]
[0200] [Table 2]
[0201] [Table 3]
[0202] [Table 4]
[0203] As can be seen from the above results, in Examples 1 to 17, the semiconductor nanoparticle composites had high fluorescence quantum efficiency (QY), and were excellent in dispersibility in polar dispersion media, allowing dispersion at a high mass fraction. On the other hand, Comparative Example 5, which does not use a mercapto fatty acid ester, Comparative Example 1, which has a too large molecular weight of the mercapto fatty acid ester, Comparative Examples 3 and 7, which have a too low SP value of the mercapto fatty acid ester, Comparative Example 4, which has a too low average SP of the entire ligand, and Comparative Example 8, which has a too high average SP of the entire ligand, all have poor dispersibility in a polar dispersion medium and are difficult to disperse at a high mass fraction. In addition, Comparative Examples 2, 6, 9, 10, and 11 have low fluorescence quantum efficiency and also low filterability because the halogen / In ratio of the semiconductor nanoparticles is outside the range specified in the present invention.
[0204] Moreover, Examples 1 to 10, in which the molecular weight of the mercapto fatty acid ester represented by general formula (1) is in the range of 300 to 700, are excellent in heat resistance, and it was found that the semiconductor nanoparticle composites of the present invention using a mercapto fatty acid ester represented by general formula (1) having a molecular weight of 300 to 700 are particularly suitable for applications in which heat resistance is important. Note that, although the viscosity of the dispersion liquid when dispersed in a dispersion medium in Examples 1 to 10 is higher than that in Examples 11 to 17, in which a mercapto fatty acid ester represented by general formula (1) having a molecular weight of less than 300 is used, the dispersion liquid can be used except for applications in which a low viscosity of the dispersion medium is particularly required.
[0205] Furthermore, in Examples 11 to 17, in which the molecular weight of the mercapto fatty acid ester represented by general formula (1) is in the range of 300 or less, the viscosity of the dispersion liquid when dispersed in a dispersion medium is low. From this, it was found that the semiconductor nanoparticle composites of the present invention, in which the mercapto fatty acid ester represented by general formula (1) having a molecular weight of less than 300 as in Examples 11 to 17, do not have the heat resistance of Examples 1 to 10, in which the mercapto fatty acid ester represented by general formula (1) having a molecular weight of 300 to 700 is used, are suitable for applications in which low viscosity of the dispersion liquid is more important than heat resistance. [Explanation of symbols]
[0206] 1, 101 Blue LED 3, 103 LCD 7, 8 QD patterning 9 Diffusion Layer 11 cores 12. Shell 102 QD Film 104 Color Filter(R) 105 Color Filter (G) 106 Color Filter (B)
Claims
1. A semiconductor nanoparticle composite in which a ligand is coordinated to a surface of a semiconductor nanoparticle, The semiconductor nanoparticles are core / shell type semiconductor nanoparticles having a core containing In and P and one or more shell layers, the semiconductor nanoparticles further contain a halogen, and in the semiconductor nanoparticles, a molar ratio of the halogen to In, calculated on an atomic basis, is 0.80 to 15.00; The ligand has the following general formula (1): HS-R 1 -COO-R 2 (1) (In general formula (1), R 1 represents an alkylene group having 1 to 3 carbon atoms; R 2 represents a hydrophilic group; The mercapto fatty acid ester has an SP value of 9.20 or more and a molecular weight of less than 300; the average SP value of the entire ligand is 9.10 to 11.00; and the mass ratio of the ligand to the semiconductor nanoparticles (ligand / semiconductor nanoparticles) is 0.40 or less; A semiconductor nanoparticle composite comprising:
2. 2. The semiconductor nanoparticle composite according to claim 1, wherein the content of the mercapto fatty acid ester represented by general formula (1) in the total amount of the ligands is 40 mol % or more.
3. 3. The semiconductor nanoparticle composite according to claim 1, wherein at least one of the shells is formed of ZnSe.
4. 4. The semiconductor nanoparticle composite according to claim 1, wherein the shell has two or more layers, and the outermost layer of the shell is formed of ZnS.
5. R in the general formula (1) 2 The semiconductor nanoparticle composite according to any one of claims 1 to 4, characterized in that: contains any one selected from the group consisting of an oligoethylene glycol group, a polyethylene glycol group, and an alkoxy group.
6. The semiconductor nanoparticle composite according to any one of claims 1 to 5, characterized in that the terminal group of R 2 not bonded to -COO- in the general formula (1) is any one selected from the group consisting of alkyl groups, alkenyl groups and alkynyl groups.
7. 7. The semiconductor nanoparticle composite according to claim 1, wherein the ligand further comprises an aliphatic ligand.
8. The semiconductor nanoparticle composite according to claim 7, wherein the aliphatic ligand is one or more selected from the group consisting of aliphatic thiols, aliphatic carboxylic acids and aliphatic phosphines.
9. A semiconductor nanoparticle composite described in any one of claims 1 to 8, characterized in that the shell consists at least of a first shell covering the outer surface of the core formed of ZnSe, and a second shell covering the outer surface of the first shell formed of ZnS.
10. The semiconductor nanoparticle composite according to claim 1, wherein the quantum efficiency of the purified semiconductor nanoparticle composite is 80% or more.
11. The semiconductor nanoparticle composite according to claim 1, wherein the half width of the emission spectrum of the semiconductor nanoparticle composite is 38 nm or less.
12. A semiconductor nanoparticle composite dispersion liquid in which the semiconductor nanoparticle composite according to any one of claims 1 to 11 is dispersed in a polar organic dispersion medium.
13. A semiconductor nanoparticle composite composition comprising the semiconductor nanoparticle composite according to any one of claims 1 to 11 dispersed in a monomer or a prepolymer.
14. A cured film of a semiconductor nanoparticle composite comprising the semiconductor nanoparticle composite according to any one of claims 1 to 11 dispersed in a polymer matrix.
Citation Information
Patent Citations
Quantum dot solid film and preparation method thereof
CN106479503A
Ultrafine semiconductor particle
JP2002121549A
Thin film-like molding containing semiconductor crystal grain, and its use
JP2002162501A
Titanium compound containing quantum dots and production method, and photoelectric conversion element using the titanium compound containing quantum dots
JP2013136498A
Quantum dot material and method for manufacturing same
WO2017188300A1