Asymmetric Composites

An asymmetric composite material with differing polymer layers on a porous metal body addresses the limitation of uniform polymer coatings, enhancing functionality and application scope.

JP7575166B2Active Publication Date: 2024-10-29LG CHEM LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023083291
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-08-06
Filing Date
2023-05-19
Publication Date
2024-10-29
Estimated Expiration
2039-08-06

AI Technical Summary

Technical Problem

Existing methods for manufacturing composite materials with porous metal bodies limit application scope by forming polymer layers with identical properties, restricting their versatility.

Method used

The development of an asymmetric composite material with distinct polymer layers on both sides of a porous metal body, allowing for varied properties and expanded application fields.

Benefits of technology

Enables a composite material with enhanced functionality and versatility by incorporating polymer layers with different compositions on opposite sides of the metal foam, optimizing properties for specific applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575166000003
    Figure 0007575166000003
  • Figure 0007575166000004
    Figure 0007575166000004
  • Figure 0007575166000001
    Figure 0007575166000001
Patent Text Reader

Abstract

To provide an asymmetry composite material and a method for preparing the same.SOLUTION: The invention provides: a method for preparing a composite material which comprises a metal porous body (metal foam or the like) and a polymer component, where the polymer component is formed in an asymmetrical structure on both sides of the metal porous body (metal foam or the like); and a composite material prepared in such a manner.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2018-0091348 filed on August 6, 2018, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] This application relates to asymmetric composites and methods for making same. [Background technology]

[0003] Metal foams have a variety of useful properties, such as light weight, energy absorption, thermal insulation, fire resistance, and environmental friendliness, and can be applied in a variety of fields, including lightweight structures, transportation machinery, building materials, and energy absorbing devices.

[0004] Metal foams have a high specific surface area and can improve the flow of fluids such as liquids and gases or electrons, and can therefore be usefully applied to substrates for heat exchangers, catalysts, sensors, actuators, secondary batteries, fuel cells, gas diffusion layers (GDLs), microfluidic flow controllers, and the like.

[0005] In order to expand the application fields of the metal foam or to reinforce the physical properties, a composite material can be produced by combining the metal foam with a resin component. Summary of the Invention [Problem to be solved by the invention]

[0006] The present application aims to provide an asymmetric composite material and a method for producing said asymmetric composite material. [Means for solving the problem]

[0007] The present application relates to an asymmetric composite material and a method for making said asymmetric composite material. The term "composite material" can refer to a material that includes a porous metal body (such as a metal foam) and a polymeric component.

[0008] As shown in FIG. 1, an exemplary asymmetric composite material 10 includes a first polymer layer 1, a metal porous body 3, and a second polymer layer 2 in this order, and the first polymer layer 1 and the second polymer layer 2 may have different components. The phrase "the first polymer layer and the second polymer layer have different components" means that the compositions of a resin component or other additives, which will be described later, are different from each other. Conventionally, a method for manufacturing a composite material in which a resin component is combined with a metal porous body has been widely known. In general, when a metal porous body is coated with a polymer by a dip coating or blade coating method, a polymer layer having the same properties is formed on the surface of the metal porous body, so that the range of application is limited. The present application provides an asymmetric composite material having polymer layers having different properties on both sides of a metal porous body, thereby providing a composite material having various application fields.

[0009] As used herein, the term "metal porous body (e.g., metal foam) or metal skeleton" refers to a porous structure containing metal as a main component. In the above, "containing metal as a main component" refers to a case where the proportion of metal is 55% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, 90% by weight or more, or 95% by weight or more based on the total weight of the metal porous body (e.g., metal foam) or metal skeleton. The upper limit of the proportion of the metal contained as the main component is not particularly limited, and may be, for example, about 100% by weight, 99% by weight, or 98% by weight.

[0010] As used herein, the term "porosity" may refer to a porosity of at least 30%, 40%, 50%, 60%, 70%, 75%, or 80%. The upper limit of the porosity is not particularly limited, and may be, for example, about 99% or less, about 98% or less, 95% or less, 90% or less, 85% or less, 80% or less, or 75% or less. The porosity may be calculated in a known manner by calculating the density of a metal porous body (such as a metal foam).

[0011] The metal porous body (metal foam, etc.) included in the composite material of the present application may be in the form of a film. The composite material of the present application may include the above-mentioned film-shaped metal porous body (metal foam, etc.) and polymer components present on both opposing surfaces of the metal porous body (metal foam, etc.). The opposing surfaces may refer to surfaces facing each other, such as the upper and lower surfaces or both sides of the film-shaped metal porous body (metal foam, etc.). Hereinafter, for convenience, the surface on which the first polymer layer is present among the opposing surfaces of the metal porous body may be referred to as the first surface, and the surface on which the second polymer layer is present as the opposite surface may be referred to as the second surface. In one example, the second polymer layer component may not be present on the first surface, and the first polymer layer component may not be present on the second surface. In one example, the polymer component of the polymer layer may permeate the pores of the metal porous body, for example, the polymer component of the first polymer layer may permeate in a larger amount than the polymer component of the second polymer layer. However, without being limited thereto, the polymer component of the second polymer layer may be infiltrated into the pores of the metal porous body in a larger amount than the polymer component of the first polymer layer, that is, the contents of the first polymer layer component and the second polymer layer component infiltrated into the pores of the metal porous body may be different from each other.

[0012] In one example, the metal porous body may include a first region in which the polymer component of the first polymer layer is present and a second region in which the polymer component of the second polymer layer is present. In this specification, the term "polymer component" may mean a resin component described below or other additives contained in the polymer layer, or may mean a polymer solution described below. In a specific example of the present application, the thickness of the first region relative to the thickness of the metal porous body may be within a range of 0.01 to 0.99, 0.05 to 0.95, 0.08 to 0.9, 0.1 to 0.8, 0.2 to 0.7, 0.25 to 0.65, 0.3 to 0.6, 0.35 to 0.55, or 0.4 to 0.5. The thickness of the second region relative to the thickness of the metal porous body may be within a range of 0.01 to 0.99, 0.05 to 0.95, 0.08 to 0.9, 0.1 to 0.8, 0.2 to 0.7, 0.25 to 0.65, 0.3 to 0.6, 0.35 to 0.55, or 0.4 to 0.5. In the present application, the first polymer layer and the second polymer layer having different components may be disposed on both sides of the metal porous body, and the metal porous body may have a polymer component of the first polymer layer and a polymer component of the second polymer layer present together inside the pores, and the thicknesses of the first region and the second region may be adjusted as necessary.

[0013] The metal porous body (metal foam, etc.) in the composite may have a porosity of about 30% to 99%. In one example, when forming the composite in the manner described below, the porosity or pore size of the metal porous body (metal foam, etc.) may be controlled in consideration of the desired asymmetric structure. For example, when forming the asymmetric structure in the manner described below, if the metal porous body (metal foam, etc.) has a small porosity or a small pore size, the degree to which light irradiated from one surface reaches the other surface is small, and conversely, if the porosity or pore size is large, the degree to which light reaches the other surface is large, so that the degree of curing of the photocurable composition on the opposite surface can be controlled. In another example, the porosity may be 40% or more, 50% or more, 60% or more, 70% or more, 75% or more, or 80% or more, or about 95% or less, 90% or less, 85% or less, or 80% or less.

[0014] The metal porous body (such as a metal foam) may be in the form of a film, and the thickness of the film may be within the range of about 5 μm to 5 cm, for example. In other examples, the thickness may be about 4 cm or less, 3 cm or less, 2 cm or less, or 1 cm or less, 9000 μm or less, 8000 μm or less, 7000 μm or less, 6000 μm or less, 5000 μm or less, 4000 μm or less, 3000 μm or less, 2000 μm or less, 1000 μm or less, 900 μm or less, 800 μm or less, 700 μm or less, 600 μm or less, 500 μm or less, 400 μm or less, 300 μm or less, or 200 μm or less, or about 6 μm or more, 7 μm or more, 8 μm or more, 9 μm or more, 10 μm or more, 20 μm or more, 30 μm or more, 40 μm or more, 50 μm or more, 60 μm or more, 70 μm or more, 80 μm or more, 90 μm or more, or 95 μm or more.

[0015] The skeleton of the metal porous body (e.g., metal foam) may be made of various types of metals or metal alloys, and may include or consist of one or more metals or metal alloys selected from the group consisting of, for example, iron, cobalt, nickel, copper, phosphorus, molybdenum, zinc, manganese, chromium, indium, tin, silver, platinum, gold, aluminum, stainless steel, and magnesium.

[0016] Various types of porous metal bodies (e.g., metal foams) are known, and various methods for manufacturing porous metal bodies (e.g., metal foams) are also known. In the present application, such known porous metal bodies (e.g., metal foams) and porous metal bodies (e.g., metal foams) manufactured by the known methods may be applied.

[0017] Known methods for manufacturing a metal porous body (metal foam, etc.) include a method of sintering a composite material of a pore-forming agent such as salt and a metal, a method of coating a support such as a polymer foam with a metal and sintering it in that state, and a slurry method of preparing a binder, a solvent and a dispersant as a slurry, coating, drying and sintering it. The present application can realize a metal foam having a desired pore size, thickness and porosity through the above method. The metal porous body (metal foam, etc.) can also be manufactured by the methods disclosed in the applicant's prior applications, Korean Patent Application Nos. 2017-0086014, 2017-0040971, 2017-0040972, 2016-0162154, 2016-0162153 and 2016-0162152.

[0018] The metal porous body (metal foam, etc.) may also be manufactured by an induction heating method among the methods disclosed in the prior application, and in this case, the metal porous body (metal foam, etc.) may contain at least a conductive magnetic metal. In this case, the metal porous body (metal foam, etc.) may contain the conductive magnetic metal in an amount of 30% by weight or more, 35% by weight or more, 40% by weight or more, 45% by weight or more, or 50% by weight or more by weight. In another example, the proportion of the conductive magnetic metal in the metal porous body (metal foam, etc.) may be about 55% by weight or more, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, 85% by weight or more, or 90% by weight or more. The upper limit of the proportion of the conductive magnetic metal is not particularly limited, and may be, for example, less than about 100% by weight or less than 95% by weight.

[0019] In this application, the term "conductive magnetic metal" may refer to a metal having a certain relative magnetic permeability and conductivity, and capable of generating heat to an extent that the metal can be sintered by induction heating.

[0020] In one example, the conductive metal may be a metal having a relative magnetic permeability of 90 or more. The relative magnetic permeability (μr) is the ratio (μ / μ0) of the magnetic permeability (μ) of the corresponding material to the magnetic permeability (μ0) in a vacuum. The metal may have a relative magnetic permeability of 95 or more, 100 or more, 110 or more, 120 or more, 130 or more, 140 or more, 150 or more, 160 or more, 170 or more, 180 or more, 190 or more, 200 or more, 210 or more, 220 or more, 230 or more, 240 or more, 250 or more, 260 or more, 270 or more, 280 or more, 290 or more, 300 or more, 310 or more, 320 or more, 330 or more, 340 or more, 350 or more, 360 or more, 370 or more, 380 or more, 390 or more, 400 or more, 410 or more, 420 or more, 430 or more, 440 or more, 450 or more, 460 or more, 470 or more, 480 or more, 490 or more, 500 or more, 510 or more, 520 or more, 530 or more, 540 or more, 550 or more, 560 or more, 570 or more, 580 or more, 590 or more, 600 or more, 610 or more, 620 or more, 630 or more, 640 or more, 650 or more, 660 or more, 670 or more, 680 or more, 690 or more, 70 0 or more, 350 or more, 360 or more, 370 or more, 380 or more, 390 or more, 400 or more, 410 or more, 420 or more, 430 or more, 440 or more, 450 or more, 460 or more, 470 or more, 480 or more, 490 or more, 500 or more, 510 or more, 520 or more, 530 or more, 540 or more, 550 or more, 560 or more, 570 or more, 580 or more, or 590 or more. The higher the relative permeability, the higher the heat generated when an electromagnetic field for induction heating is applied, as described below, so the upper limit is not particularly limited. In one example, the upper limit of the relative permeability may be, for example, about 300,000 or less.

[0021] The conductive magnetic metal may have a conductivity of about 8 MS / m or more, 9 MS / m or more, 10 MS / m or more, 11 MS / m or more, 12 MS / m or more, 13 MS / m or more, or 14.5 MS / m or more at 20° C. There is no particular upper limit to the conductivity, and for example, the conductivity may be about 30 MS / m or less, 25 MS / m or less, or 20 MS / m or less.

[0022] Specific examples of such conductive magnetic metals include, but are not limited to, nickel, iron, or cobalt.

[0023] As described above, the composite material of the present application may be an asymmetric composite material. The asymmetric composite material may mean that the first polymer layer and the second polymer layer present on both sides of the metal porous body have different components. The components of the first polymer layer and the second polymer layer mean that the polymer component or resin component described below is different from each other, or other additives are different from each other. In the above, the polymer component and the resin component may be used in the same sense.

[0024] As one example, the resin component contained in the first polymer layer or the second polymer layer may include, for example, a styrene-based resin or elastomer, a polyolefin-based resin or elastomer, other elastomers, a polyoxyalkylene-based resin or elastomer, a polyester-based resin or elastomer, a polyvinyl chloride-based resin or elastomer, a polycarbonate-based resin or elastomer, a polyphenylene sulfide-based resin or elastomer, a mixture of hydrocarbons, a polyamide-based resin or elastomer, an acrylate-based resin or elastomer, an epoxy-based resin or elastomer, a silicone-based resin or elastomer, a fluorine-based resin or elastomer, or a mixture thereof.

[0025] Examples of the styrene-based resin or elastomer include styrene-ethylene-butadiene-styrene block copolymer (SEBS), styrene-isoprene-styrene block copolymer (SIS), acrylonitrile-butadiene-styrene block copolymer (ABS), acrylonitrile-styrene-acrylate block copolymer (ASA), styrene-butadiene-styrene block copolymer (SBS), styrene-based homopolymer, or a mixture thereof. Examples of the olefin-based resin or elastomer include high-density polyethylene-based resin or elastomer, low-density polyethylene-based resin or elastomer, polypropylene-based resin or elastomer, or a mixture thereof. Examples of the elastomer include ester-based thermoplastic elastomer, olefin-based elastomer, silicone-based elastomer, acrylic-based elastomer, or a mixture thereof. Among them, polybutadiene resin or elastomer, polyisobutylene resin or elastomer, or the like can be used as the olefin-based thermoplastic elastomer. Examples of the polyoxyalkylene resin or elastomer include polyoxymethylene resin or elastomer, polyoxyethylene resin or elastomer, or a mixture thereof. Examples of the polyester resin or elastomer include polyethylene terephthalate resin or elastomer, polybutylene terephthalate resin or elastomer, or a mixture thereof. Examples of the polyvinyl chloride resin or elastomer include polyvinylidene chloride. Examples of the hydrocarbon mixture include hexatriacotane or paraffin. Examples of the polyamide resin or elastomer include nylon. Examples of the acrylate resin or elastomer include polybutyl(meth)acrylate.Examples of the epoxy resin or elastomer include bisphenol types such as bisphenol A type, bisphenol F type, bisphenol S type, and water additives thereof; novolac types such as phenol novolac type and cresol novolac type; nitrogen-containing ring types such as triglycidyl isocyanurate type and hydantoin type; alicyclic types; aliphatic types; aromatic types such as naphthalene type and biphenyl type; glycidyl types such as glycidyl ether type, glycidyl amine type and glycidyl ester type; dicyclo types such as dicyclopentadiene type; ester types; ether ester types, and mixtures thereof. Examples of the silicon resin or elastomer include polydimethylsiloxane. Examples of the fluorine-based resin or elastomer include polytrifluoroethylene resin or elastomer, polytetrafluoroethylene resin or elastomer, polychlorotrifluoroethylene resin or elastomer, polyhexafluoropropylene resin or elastomer, polyvinylidene fluoride, polyvinyl fluoride, polyethylene propylene fluoride, and mixtures thereof.

[0026] The resins or elastomers listed above may be used by grafting with, for example, maleic anhydride, or may be used by copolymerizing with other resins or elastomers or monomers for producing resins or elastomers listed above, or may be used by modifying with other compounds, such as carboxyl-terminated butadiene-acrylonitrile copolymers.

[0027] Meanwhile, more specifically, when the polymer layer is a cured product of a curable composition, the resin component may include a polymer that is cured by irradiation with light or application of heat. The term "thermosetting resin" means a resin that can be cured through application of appropriate heat or aging process, and the term "photocurable resin" means a resin that can be cured by irradiation with electromagnetic waves. The curable resin may also be a dual-curing resin having both the properties of thermosetting and photocuring. In this specification, the irradiation with light may include irradiation with microwaves, infrared rays (IR), ultraviolet rays (UV), X-rays, and gamma rays, as well as particle beams such as an alpha-particle beam, a proton beam, a neutron beam, and an electron beam.

[0028] Examples of such curable compositions include acrylic curable compositions, epoxy curable compositions, isocyanate curable compositions, urethane curable compositions, polyester curable compositions, polyamic acid curable compositions, polyamide curable compositions, phthalonitrile curable compositions, and silicone curable compositions. Each of the compositions can be cured to form an acrylic polymer component, an epoxy polymer component, an isocyanate polymer component, a urethane polymer component, a polyester polymer component, a polyamic acid polymer component, a polyamide polymer component, a phthalonitrile resin polymer component, or a silicone polymer component, and such compositions are widely known in the polymer composition industry. In the present application, an appropriate component can be selected from such known components and used, and if necessary, a composite polymer can be formed using two or more of the above components.

[0029] The composition as described above generally includes a polymer component, an oligomer component, and / or a monomer component having a functional group that can be cured by irradiation with light or application of heat, and includes an initiator capable of initiating a curing reaction by irradiation with light and / or application of heat, such as a radical initiator or a cationic initiator, or other curing agent, etc. Examples of the functional group that can be cured by irradiation with light or application of heat include, but are not limited to, functional groups containing a radically polymerizable double bond, such as an acryloyl group or a methacryloyl group, cationic polymerizable functional groups, such as a glycidyl group, an alicyclic epoxy group, an oxetanyl group, etc., or hydrogen atoms bonded to silicon atoms, alkenyl groups such as a vinyl group, an isocyanate group, a carboxyl group, a hydroxyl group, an epoxy group, an aziridine group, etc.

[0030] In one example, the resin component in the first or second polymer layer may have a weight average molecular weight (Mw) that allows the polymer layer to be molded into a film shape. For example, the resin component may have a weight average molecular weight of about 100,000 to 2,000,000, 120,000 to 1,500,000, or 150,000 to 1,000,000. In this specification, the term "weight average molecular weight" refers to a converted value relative to standard polystyrene measured by GPC (Gel Permeation Chromatograph). However, it is not necessary for the resin component to have the weight average molecular weight mentioned above. For example, when the molecular weight of the resin component is not at a level that allows the resin component to form a film, a separate binder resin may be added to the composition.

[0031] In the specific example of the present application, the first polymer layer or the second polymer layer may include the above-mentioned resin component and the corresponding curing agent or initiator, which may be appropriately combined according to the desired physical properties in the technical field of interest by a general engineer. For example, one side of the metal porous body may include a polymer component having adhesive properties, and the other side may include a polymer component having adhesive properties. In addition, without being limited thereto, a polymer layer having electrical conductivity may be formed on one side of the metal porous body, and a polymer layer having electrical insulation may be formed on the other side. In addition, a polymer layer having excellent tensile properties may be formed on one side of the metal porous body, and a polymer layer having excellent compressive properties may be formed on the other side. The above examples may be designed by a general engineer in consideration of the physical properties required depending on the application of the metal porous body.

[0032] In one example, the first polymer layer may be an electrically conductive layer having a surface resistance of 10 Ω / □ or less as measured according to JIS K 7194, and the second polymer layer may be an electrically insulating layer having a surface resistance of 1000 Ω / □ or more as measured according to JIS K 7194. In one example, the electrically conductive layer may have a surface resistance in the range of 0.01 to 9 Ω / □ or 0.1 to 5 Ω / □, and the electrically insulating layer may have a surface resistance in the range of 1000 to 5000 Ω / □ or 1500 to 4000 Ω / □. In one example, the first polymer layer may have a peel strength from a copper metal plate (peel speed: 0.3 m / min, peel angle: 180°) of 0.1 to 100 g / mm or 1 to 90 g / mm, and the second polymer layer may have a peel strength from a copper metal plate (peel speed: 0.3 m / min, peel angle: 180°) of 10 to 1000 g / mm or more than 100 g / mm and 1000 g / mm or less. In one example, the first polymer layer may have a tensile modulus at 25° C. in the range of 0.01 MPa to 10 MPa or 0.1 MPa to 5 MPa, and the second polymer layer may have a tensile modulus at 25° C. in the range of 100 MPa to 1000 MPa or 300 MPa to 800 MPa. In the present application, a composite material can be configured so that the first polymer layer and the second polymer layer satisfy the desired physical properties depending on the application of the composite material and according to the needs.

[0033] In the specific example of the present application, the first or second polymer layer may further include a radical initiator depending on the type of resin component. The radical initiator may be a photoinitiator or a thermal initiator. The specific type of photoinitiator may be appropriately selected in consideration of the curing speed and the possibility of yellowing. For example, a benzoin-based, hydroxyketone-based, aminoketone-based, or phosphine oxide-based photoinitiator may be used, and specifically, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2 ... Pyridine ketone, benzophenone, p-phenylbenzophenone, 4,4'-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyl dimethyl ketal, acetophenone dimethyl ketal, p-dimethylaminobenzoic acid ester, oligo[2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone], and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide can be used.

[0034] The radical initiator may be contained in an amount of 0.2 to 20 parts by weight, 0.5 to 18 parts by weight, 1 to 15 parts by weight, or 2 to 13 parts by weight relative to 100 parts by weight of the resin component.

[0035] In the embodiment of the present application, the first or second polymer layer may further include a curing agent depending on the type of the resin component. For example, the first or second polymer layer may further include a curing agent capable of reacting with the above-mentioned resin component to form a crosslinked structure.

[0036] An appropriate type of curing agent can be selected and used depending on the type of the resin component or the functional group contained in the resin.

[0037] As an example, when the resin component is an epoxy resin, the curing agent may be one or more of epoxy resin curing agents known in the art, such as, for example, an amine curing agent, an imidazole curing agent, a phenolic curing agent, a phosphorus curing agent, or an acid anhydride curing agent, but is not limited thereto.

[0038] As one example, the curing agent may be an imidazole compound that is in a solid phase at room temperature and has a melting point or decomposition temperature of 80° C. or higher. Examples of such compounds include, but are not limited to, 2-methylimidazole, 2-heptadecylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, and 1-cyanoethyl-2-phenylimidazole.

[0039] The content of the curing agent may be selected depending on the composition of the composition, for example, the type and ratio of the resin component. For example, the curing agent may be included in an amount of 1 to 20 parts by weight, 1 to 10 parts by weight, or 1 to 5 parts by weight, based on 100 parts by weight of the resin component. However, the weight ratio may be changed depending on the type and ratio of the resin component or the functional group of the resin, or the crosslink density to be realized.

[0040] When the resin component is a resin that can be cured by irradiation with active energy rays, for example, a cationic photopolymerization initiator can be used as the initiator.

[0041] As the cationic photopolymerization initiator, an ionized cationic initiator of an onium salt or an organometallic salt series, or an organic silane or latent sulfonic acid series or a non-ionized cationic photopolymerization initiator can be used. Examples of the onium-based initiator include diaryliodonium salts, triarylsulfonium salts, and aryldiazonium salts. Examples of the organometallic salt-based initiator include iron arene. Examples of the organosilane-based initiator include o-nitrobenzyl triaryl silyl ether, triaryl silyl peroxide, and acyl silane. Examples of the latent sulfuric acid-based initiator include, but are not limited to, α-sulfonyloxyketone and α-hydroxymethylbenzoin sulfonate.

[0042] In one example, the cationic initiator may be an ionizing cationic photoinitiator.

[0043] In one example, the first or second polymer layer may further include inorganic particles as necessary. The specific type of inorganic particles (or fillers) used in the present application is not particularly limited, and for example, one or a mixture of two or more of clay, talc, alumina, calcium carbonate, zirconia, silica, etc. may be used.

[0044] The inorganic particles of the present application may be contained in an amount of 1 to 70 parts by weight or 25 to 50 parts by weight relative to 100 parts by weight of the resin component. The inorganic particles may have an average particle size measured by a D50 particle size analyzer within a range of 5 to 100 nm or 8 to 40 nm. The inorganic particles may have a refractive index within a range of 1.2 to 2.0 or 1.4 to 1.7. The first or second polymer layer of the present application contains the inorganic particles, so that a cured product having the desired physical properties can be produced.

[0045] In one example, the first or second polymer layer may further include conductive particles, if necessary. The conductive particles may include a conductive metal, for example, silver, copper, nickel, gold, aluminum, or graphite. The conductive particles may be single conductive metal particles, or may be a form in which a first conductive metal particle is coated with a second conductive metal. For example, the conductive particles may include one or more of graphite powder, copper powder, silver powder, nickel powder, silver-coated copper powder (Ag-coated Cu powder), gold-coated copper powder, silver-coated nickel powder (Ag-coated Ni powder), and gold-coated nickel powder. The conductive particles may have a spherical, dendrite-type, rod-type, needle-type, flake-type, or rugby ball-type shape. Specifically, the conductive particles may be dendrite-type, and in this case, the polymer layer has excellent conductivity compared to the content of the conductive particles. When the conductive particles are contained, the conductive particles may be contained in an amount of 3 to 50 parts by weight or 5 to 30 parts by weight relative to 100 parts by weight of the resin component.

[0046] In addition to the above-mentioned components, the polymer layer may contain various additives depending on the intended use and the manufacturing process of the composite material described below. For example, the first or second polymer layer may contain a tackifier, a multifunctional active energy ray curable material, a crosslinking agent, a filler, etc. in an appropriate range of content depending on the desired physical properties.

[0047] In one example, the first polymer layer or the second polymer layer may have a thickness in the range of 5 to 100 μm, 8 to 80 μm, 12 to 60 μm, 15 to 40 μm, or 18 to 28 μm. The thickness of the first polymer layer and the thickness of the second polymer layer may be different from each other or the same. In the composite material of the present application, the thicknesses may be the same or the thickness of the first polymer layer may be thicker than the thickness of the second polymer layer depending on the physical properties of the two polymer layers described above. In the present application, on the other hand, the thickness of the second polymer layer may be thicker than the thickness of the first polymer layer.

[0048] The composite material of the present application may be used as a heat insulating material, a heat dissipating material, a sound insulating material, a lightweight material, a structural material, or an electrode material, etc.

[0049] The present application also relates to a method for producing an asymmetric composite material. The above-mentioned asymmetric composite material can be produced by the following production method.

[0050] The manufacturing method may include a step of applying a first polymer layer to one side of a metal porous body having a resin layer attached to the other side. The other side of the metal porous body may refer to a side of the metal porous body (such as a metal foam) to which the resin layer is not attached. The resin layer may be, but is not limited to, an adhesive layer. In addition, the step of applying the first polymer layer may include coating a first polymer layer solution containing a polymer component of the first polymer layer.

[0051] In one example, as shown in FIG. 2, when one surface of a metal porous body (metal foam, etc.) 3 is attached to a resin layer 11, at least a part of the resin layer 11 penetrates into the pores of the metal porous body (metal foam, etc.) 3 due to the porosity of the metal porous body (metal foam, etc.). Then, when a first polymer layer 1 is applied to the surface of the metal porous body (metal foam, etc.) 3 where the resin layer 11 does not exist, the first polymer layer 1 does not penetrate into at least the pores where the resin layer 11 exists. Of course, by adjusting the viscosity of the first polymer layer 1, the degree of penetration into the pores can be adjusted so that the first polymer layer 1 does not penetrate into some of the pores where the resin layer 11 does not exist. In this state, the manufacturing method of the present application can include a step of curing or crosslinking the first polymer layer 1. In FIG. 2, reference numeral 12 denotes a base film or a release film that supports the resin layer 11.

[0052] In the method of the present application, in order to adjust the degree of penetration of the resin layer into the pores of the porous metal body, a porous metal body (such as a metal foam) may be placed on the resin layer, and the porous metal body may be pressurized to attach the adhesive layer. That is, such pressure can cause the adhesive layer to penetrate into more pores, thereby adjusting the structure of the asymmetric film.

[0053] In addition, the thickness of the resin layer can be controlled in other ways to control the degree of pore penetration of the resin layer, thereby controlling the structure of the asymmetric film.

[0054] The type of the resin layer that can be applied in the present application is not particularly limited, and a known type of resin layer or adhesive layer can be used. For example, the method can be carried out using an adhesive sheet or adhesive film having the adhesive layer formed on one side. In this case, the adhesive that can be applied includes, but is not limited to, known acrylic adhesives, silicone adhesives, urethane adhesives, and epoxy adhesives.

[0055] The manufacturing method of the present application may include a step of curing or crosslinking the first polymer layer 1. The method of curing or crosslinking in the above process is not particularly limited, and a suitable method such as light irradiation or heat application may be applied depending on the type of resin component of the applied polymer layer. If necessary, a step of removing uncured or uncrosslinked composition after the curing or crosslinking may be further performed.

[0056] In the above-mentioned method, by controlling the curing or crosslinking conditions, for example, the degree or direction of light irradiation, the degree of heat application, the thickness of the adhesive layer, the thickness of the polymer layer and / or the thickness of the metal porous body (metal foam, etc.), the porosity or pore size of the metal porous body (metal foam, etc.), the shape of the corresponding asymmetric structure can be variously adjusted.

[0057] In one example, the process may form the first polymer layer on at least one of the first and second surfaces of a porous structure (e.g., a metal foam) to a thickness in the range of about 1 nm to 2 cm.

[0058] In the manufacturing method of the present application, a step of removing uncured or uncrosslinked polymer layer components after the curing or crosslinking may be further carried out.

[0059] The above-mentioned asymmetric structure can be formed by this process. The step of removing the uncured or uncrosslinked polymer layer components can be called developing. This developing process can be performed in a known manner, for example, the developing process can be performed using a treating agent known to be capable of removing the uncured or uncrosslinked composition. Known treating agents include developers such as ethanol, basic water, N-methylpyrrolidone, methylene chloride, chloroform, toluene, ethylene glycol, or propylene glycol monomethyl ether acetate. The developing process can be performed by applying the developer in a suitable manner, for example, at a pressure of about 2 bar or more and at a temperature range of 20°C to 50°C using a spray developing method.

[0060] In the method of the present application, a step of removing the resin layer may be further performed after the curing or crosslinking step. The method of removing the resin layer is not particularly limited. Since the resin layer has a characteristic of being attached to the adherend by application of pressure and being removed by peeling, an appropriate removal method may be selected depending on the type of the applied resin layer.

[0061] If necessary, in the present application, the above step may be followed by a step of washing off residual resin layer, which may be carried out in a manner similar to the above-mentioned developing step.

[0062] The manufacturing method of the present application may further include, after the step of removing the resin layer 11, a step of applying a second polymer layer 2 to one surface of the metal porous body 3 from which the resin layer 11 has been removed. The second polymer layer 2 may be applied in the same manner as the application of the first polymer layer 1 described above. In addition, the manufacturing method of the present application may further include a step of curing or crosslinking the second polymer layer 2, and the curing or crosslinking may be carried out depending on the type of resin component. Effect of the Invention

[0063] The present application provides a composite material including a metal porous body (e.g., metal foam) and a polymer component, and a method for manufacturing the composite material in which the polymer component is formed in an asymmetric structure on both sides of the metal porous body (e.g., metal foam), and a composite material manufactured by such a method. [Brief description of the drawings]

[0064] [Figure 1] FIG. 2 is a cross-sectional view of an asymmetric composite of the present application. [Diagram 2] FIG. 2 is an exemplary diagram for explaining a method for manufacturing an asymmetric composite material according to the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0065] The present application will be described in detail below through examples and comparative examples, but the scope of the present application is not limited to the following examples.

[0066] <Example 1> As the metal porous body, a copper metal foam in the form of a film having a thickness of 100 μm and a porosity of about 75% was used. The metal foam was placed on an adhesive layer of an adhesive sheet (based on PET) having an acrylic adhesive layer having a thickness of 10 μm, and then pressed with a load of about 3 kg. Then, polydimethylsiloxane (PDMS, Sylgard184) was coated to a thickness of 20 μm on the opposite side of the side that contacted the adhesive layer of the pressed copper foam using a film applicator, and heated in an oven at 120° C. for 20 minutes to form a first polymer layer. After curing, the adhesive sheet (PET-adhesive layer) was removed to prepare a composite material. Thereafter, to form a second polymer layer on the surface of the composite from which the adhesive sheet was removed, epoxy resin (KUKDO CHEMICAL, resin YD-128 + hardener G640) was coated to a thickness of 20 μm using a film applicator, and heated in an oven at 80° C. for 60 minutes to prepare an asymmetric composite.

[0067] <Example 2> An asymmetric composite was prepared in the same manner as in Example 1, except that a thermosetting acrylic resin (LG Chem) was coated to a thickness of 20 μm using a film applicator as the second polymer layer and heated in an oven at 80° C. for 60 minutes.

[0068] <Example 3> An asymmetric composite was prepared in the same manner as in Example 1, except that a coating solution in which polydimethylsiloxane (PDMS, Sylgard 184) and copper powder (particle size 10 μm, dendritic type) were mixed in a weight ratio of 90:10 was coated to a thickness of 20 μm using a film applicator as the second polymer layer, and heated in an oven at 120° C. for 20 minutes.

[0069] <Example 4> An asymmetric composite was prepared in the same manner as in Example 1, except that a coating solution in which polydimethylsiloxane (PDMS, Sylgard 184) and graphite powder (particle size 5 μm, flake type) were mixed in a weight ratio of 90:10 was coated to a thickness of 20 μm using a film applicator as the second polymer layer, and heated in an oven at 120° C. for 20 minutes.

[0070] <Example 5> As the first polymer layer, a coating solution in which polydimethylsiloxane (PDMS, Sylgard 184) and copper powder (particle size 10 μm, dendritic type) were mixed in a weight ratio of 90:10 was coated to a thickness of 20 μm using a film applicator and heated in an oven at 120 ° C for 20 minutes to form a first polymer layer, and as the second polymer layer, a coating solution in which polydimethylsiloxane (PDMS, Sylgard 184) and copper powder (particle size 10 μm, dendritic type) were mixed in a weight ratio of 70:30 was coated to a thickness of 20 μm using a film applicator and heated in an oven at 120 ° C for 20 minutes to form a second polymer layer. An asymmetric composite was prepared in the same manner as in Example 1, except that.

[0071] <Comparative Example 1> A composite was manufactured in the same manner as in Example 1, except that the adhesive sheet having an acrylic adhesive layer was not applied to the metal foam. Specifically, polydimethylsiloxane (PDMS, Sylgard184) was coated on one side of the copper metal foam in Example 1 to a thickness of 20 μm using a film applicator, and heated in an oven at 120° C. for 20 minutes to form a first polymer layer. After curing, epoxy resin (KUKDO CHEMICAL, resin YD-128 + hardener G640) was coated on the opposite side of the copper foam to a thickness of 20 μm using a film applicator to form a second polymer layer, and heated in an oven at 80° C. for 60 minutes to manufacture a composite.

[0072] <Experimental Example 1 - Measurement of surface resistance> The surface resistance of the polymer layers of the composite materials produced in Examples 3 to 5 was measured according to a standard test method using a Mitsubishi Chemical MCP-HT450 surface resistance tester. The surface resistance was measured under an environment of 23°C and 50% relative humidity.

[0073] <Experimental Example 2 - Measurement of peeling force> The first polymer layer or the second polymer layer of the composite material prepared in Example 1 and Example 2 was stored at 25°C and 50% relative humidity for 3 days, and then the peel force of the first or second polymer layer against the copper plate (peel speed: 5 mm / sec, peel angle: 180 degrees) was measured.

[0074] The measurement was performed under constant temperature and humidity conditions, and the peel force was measured using a texture analyzer according to ASTM3330.

[0075] [Table 1]

[0076] The second polymer layer of Example 1 is not removable and has no adhesive properties after curing.

[0077] [Table 2]

[0078] In Comparative Example 1, when polydimethylsiloxane (PDMS, Sylgard184) is coated as the first polymer layer, the liquid polydimethylsiloxane is applied to the first surface of the copper foam (the surface of the copper foam to which the first polymer layer is applied) and then penetrates into the pores and penetrates to the second surface (the surface opposite the first surface), resulting in the first polymer layer being formed on both sides of the metallic copper foam. Then, even if a second polymer layer is applied, the second polymer layer is formed on the first polymer layer already formed on the second surface. [Explanation of symbols]

[0079] 1: First polymer layer 2: Second polymer layer 3: Porous metal 11: Resin layer 12: Substrate or release film

Claims

1. 1. A method for manufacturing an asymmetric composite material, comprising: Providing a metal porous body having a first surface on which a resin layer is present and a second surface opposite to the first surface; applying a first polymer layer to a second surface of the metal porous body; curing or crosslinking the first polymeric layer after applying the first polymeric layer; removing the resin layer after curing or crosslinking the first polymer layer; applying a second polymer layer to the first surface of the metal porous body after removing the resin layer; The method, wherein the first polymeric layer and the second polymeric layer have different compositions.

2. The method of claim 1 , wherein the resin layer is an adhesive layer.

3. The method of claim 1 or 2, wherein applying the first polymeric layer comprises applying a first polymeric layer solution.

4. The method of claim 1 , further comprising cleaning any remnants of the resin layer after removing the resin layer.

5. 5. The method of claim 1, further comprising curing or crosslinking the second polymeric layer after applying the second polymeric layer.

Citation Information

Patent Citations

  • JP1987121928U

  • Induction heater

    JP1998165311A

  • Structural panels for exposed surfaces

    JP2019011039A

  • Laminate Materials and Dilatant Compounds for Ballistic Shielding

    US20120189808A1

  • Foamed core sandwich construction

    US3711363A