Cables, cable manufacturing methods,
The laminate tape with a maleic anhydride-grafted resin and higher-density polyethylene sheath, along with a waterproofing resin, addresses high-temperature water ingress issues in cables, enhancing water-blocking and environmental resistance.
Patent Information
- Application Number
- JP2020088387
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-20
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-05-20
AI Technical Summary
Conventional cable designs face issues with water ingress and deterioration of transmission characteristics due to high temperatures, especially when bent or twisted, leading to reduced water-stopping properties and potential resin layer softening.
A cable design featuring a laminate tape with a resin layer grafted with maleic anhydride and a thicker wrap portion, combined with a higher-density polyethylene outer sheath, ensures reliable bonding and water-blocking properties by using a higher melt mass flow rate and injecting a waterproofing resin into the wrap portion.
The design maintains excellent water-stopping properties even at high temperatures, prevents buckling, and reduces cable diameter while ensuring high environmental resistance.
Smart Images

Figure 0007575200000002 
Figure 0007575200000003 
Figure 0007575200000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a cable having a laminate tape wound around the outer periphery of a cable core. [Background technology]
[0002] Conventionally, a communication cable or the like is known that includes, for example, a cable core made of an optical fiber or a coated conductor, a laminate tape formed in a tubular shape with a metal layer on the outer periphery of the cable core, and a resin sheath made of polyethylene or the like that coats the outer periphery of the laminate tape. The laminate tape used here is, for example, made of a thin metal layer and a fusion resin layer made of a polyolefin resin laminated on the metal layer.
[0003] The laminate tape is formed into a tube by overlapping both ends in the width direction in the longitudinal direction. A cable core is housed inside the laminate tape, and a cable is formed by extrusion-coating an outer jacket around the outer circumference of the laminate tape. During this process, the heat generated during cable molding melts the fusion resin layer, and the overlapping ends of the fusion layer solidify and are adhesively joined together (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 05-314825 Summary of the Invention [Problem to be solved by the invention]
[0005] By disposing the laminate tape in this manner, the metal layer that constitutes it is possible to prevent water from entering the inside of the cable core, thereby preventing deterioration of the transmission characteristics.
[0006] On the other hand, due to recent abnormal weather and globalization, the highest daytime temperature recorded in Japan is about 41°C, and in some cases it exceeds 50°C overseas. Furthermore, when temperature increases due to sunlight are taken into account, the conventional environmental temperature resistance is no longer sufficient. If the laminate tape is used at temperatures above the environmental temperature resistance, the resin layer of the laminate tape will soften, causing the adhesive to peel off, resulting in a decrease in strength, and problems such as protrusions on the lap of the laminate tape will occur.
[0007] In response to this, there is a method in which a laminate tape is formed using a resin grafted with maleic anhydride, for example, based on a thermoplastic resin with good high-temperature resistance, and the laminate tape is then attached to the cable core vertically to form a polyethylene sheath. However, when such a resin layer with good high-temperature resistance grafted with maleic anhydride is used, there is a problem that the lapped portion is difficult to bond. This may result in a decrease in the water-stopping ability of the cable. In addition, when cables are installed on-site, such as underground, they are often bent or maintained in a bent state. This may result in an insufficient water-stopping effect, especially when bending or twisting is applied at high temperatures.
[0008] The present invention has been made in consideration of such problems, and has an object to provide a cable etc. that has excellent water-stopping properties even at high temperatures. [Means for solving the problem]
[0009] In order to achieve the above-mentioned object, a first invention provides a cable comprising a cable core portion, an outer sheath provided on the outermost periphery of the cable core portion, and a laminate tape disposed inside the outer sheath and wound around the outer periphery of the cable core portion. It is a cable that The laminate tape is constructed by laminating a resin layer and a metal layer, and a wrap portion is formed where both ends of the laminate tape are overlapped and the laminate tape is wrapped around the outer periphery of the cable core portion, and the resin layer is a base resin. Gapothe resin is grafted with propylene and maleic anhydride added thereto, the amount of resin in the wrap portion and its vicinity of the laminate tape is greater than the amount of resin in the portions other than the wrap portion, and the outer jacket is made of polyethylene having a density equal to or greater than medium density polyethylene, Both ends of the cable are held, and at 75°C, one end of the cable is twisted 90 degrees in a certain direction, returned to its original position, and then twisted 90 degrees in the opposite direction to the first direction and returned to its original position. This is counted as one round trip of 90-degree twisting, and after performing eight round trips of 90-degree twisting, no buckling of the laminate tape and no cracks in the outer sheath are observed. The cable is characterized by the above. It is desirable that the wrap length in the circumferential direction of the wrap portion is 7 mm to 15 mm. The polypropylene grafted with the addition of maleic anhydride preferably has a melt mass flow rate of 0.2 g / 10 min to 20 g / 10 min as specified in JIS K 7210-1 (2014).More preferably, the melt mass flow rate is 1.0 g / 10 min to 15 g / 10 min.
[0010] The jacket is preferably made from high density polyethylene.
[0011] It is desirable that the outer cover and the resin layer of the laminate tape are joined continuously in the longitudinal direction.
[0012] The laminate tape may have a portion in the lap portion where the resin layer is thicker than a portion other than the lap portion.
[0013] A waterproof resin is injected into the lap portion of the laminate tape. At the same time, the waterproof resin is applied to the stepped portion on the outside of the wrap portion, filling the step and forming a smooth surface. It is desirable that
[0014] The waterproof resin is desirably made of the same material as the resin layer of the laminate tape.
[0015] The thickness of the jacket may be 10% or less of the outer diameter of the cable, and the thickness of the jacket may be 8% or less of the outer diameter of the cable.
[0016] According to the first invention, the resin layer of the laminate tape Gapo By using polypropylene and polyethylene with a density equal to or higher than medium density polyethylene for the resin of the sheath, the resin layer of the wrap portion of the laminate can be reliably melted when the sheath is extruded. This allows the wrap portion of the laminate tape to be reliably joined. As a result, the laminate tape can be wrapped around the outer circumference of the cable core with no gaps, ensuring high water impermeability.
[0017] In addition, the base resin Gapo Maleic anhydride is grafted with polypropylene, and by adding 0.1% by mass to 3% by mass of maleic anhydride, a softening temperature of 75°C or higher can be ensured, high environmental temperature resistance can be obtained, and the melt mass flow rate specified in JIS K6922-2 falls within the specified range, making it possible to manufacture with fewer changes to equipment to handle high temperatures, and also resulting in excellent manufacturability. Gapo Reproduction In Grafting maleic anhydride makes it possible to withstand high temperatures, and also makes it possible to ensure that the resin layer and the outer jacket are tightly attached to each other even if the outer jacket is made of medium density polyethylene or higher.
[0018] Furthermore, by making the thickness of the resin layer in the lap portion of the laminate tape thicker than that of the portion other than the lap portion, the lap portion can be bonded more reliably.
[0019] Furthermore, since the outer cover and the resin layer of the laminate tape are continuously joined in the longitudinal direction, higher water stopping properties can be ensured.
[0020] Furthermore, if a waterproofing resin is injected into the lap portion of the laminate tape, the opening of the lap portion can be prevented, and the lap portion can be reliably joined by eliminating any gaps at the joints of the lap portion, thereby ensuring higher watertightness.
[0021] Furthermore, by making the thickness of the outer sheath 10% or less, or even 8% or less, of the outer diameter of the cable, the outer diameter of the cable can be made smaller.
[0022] The second invention is a method for manufacturing a cable according to the first invention, characterized in that after wrapping the laminate tape and before extruding the outer sheath, a waterproof resin is injected between the laminate tapes in the wrap portion, and the outer sheath is extrusion molded at a temperature of 200°C or higher.
[0023] According to the second aspect of the present invention, the lapped portion of the laminate tape can be reliably joined to improve the waterproofing property.
[0024] In particular, by injecting a waterproof resin into the gaps in the lapped portion of the laminate tape before pushing out the outer covering, it is possible to prevent the lapped portion from opening open, thereby ensuring higher waterproofing properties. Effect of the Invention
[0025] According to the present invention, a cable or the like having excellent water blocking properties can be provided. [Brief description of the drawings]
[0026] [Figure 1] FIG. 2 is a cross-sectional view of the laminating tape 1. [Diagram 2] FIG. 2 is a perspective view of a metallic cable 30a using the laminate tape 1. [Diagram 3] FIG. 3 is a cross-sectional view of a metallic cable 30a using the laminate tape 1. [Figure 4] FIG. 4(a) is an enlarged view of part A in FIG. 3, and FIG. 4(b) is a view showing another embodiment of FIG. [Diagram 5] FIG. 5 is a diagram showing still another embodiment of FIG. [Figure 6] FIG. 2 is a perspective view of a metallic cable 30b using the laminate tape 1. [Figure 7] FIG. 3 is a cross-sectional view of a metallic cable 30c using the laminate tape 1. [Figure 8] FIG. 4 is a cross-sectional view of an optical cable 40 using the laminate tape 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a cross-sectional view of a laminate tape 1. The laminate tape 1 has a resin layer 5 and a metal layer 3 laminated on the resin layer 5. The laminate tape 1 is used by being wrapped around the inside of the outer jacket of a cable.
[0028] The metal layer 3 of the laminate tape 1 is not particularly limited, but may be made of aluminum (including aluminum alloys), stainless steel, copper (including copper alloys), or steel. Resin layers 5 may be laminated on both sides of the metal layer 3.
[0029] The resin layer 5 of the laminate tape 1 contains at least one of MDPE, HDPE, polypropylene (PP) as a base resin. By using polypropylene, the softening temperature can be set to 75° C. or higher. The softening temperature of the resin can be measured, for example, according to JIS K7196 (1991).
[0030] The base resin constituting the resin layer 5 includes at least one of MDPE, HDPE, polypropylene (PP), etc., and is grafted by adding 0.1% by mass to 3% by mass of maleic anhydride. Preferably, 0.1% by mass to 1.5% by mass of maleic anhydride is added to the polyethylene or polypropylene constituting the resin layer 5, more preferably 0.3% by mass to 0.6% by mass or 0.9% by mass to 1.2% by mass of maleic anhydride. In this way, the melt mass flow rate of the MDPE, HDPE, polypropylene (PP), etc. constituting the resin layer 5 can be set to 0.2 g / 10 min to 20 g / 10 min as defined by JIS K 7210-1 (2014). More preferably, the melt mass flow rate of the MDPE, HDPE, polypropylene (PP), etc. constituting the resin layer 5 is 1.0 g / 10 min to 15 g / 10 min.
[0031] If the melt mass-flow rate is too low, the resistance of the extrusion screw increases during extrusion to form the cable jacket, the extrusion speed decreases, and manufacturability deteriorates. On the other hand, if the melt mass-flow rate is too high, there is a risk of problems with shape retention during production. The melt mass-flow rate can be measured, for example, according to JIS K7210-1 (2014).
[0032] Next, a description will be given of an example of a cable using the laminate tape 1. Fig. 2 is a perspective view showing a metallic cable 30a, and Fig. 3 is a cross-sectional view.
[0033] The metallic cable 30a is mainly composed of, from the inside, a plurality of covered conductor wires 31, a pressure winding tape 37, a laminate tape 1, and an outer sheath 17. The covered conductor wire 31 is composed of a conductor and an insulating sheath that covers the conductor.
[0034] The conductor of the coated conductor wire 31 is made of, for example, aluminum or copper, and may be a solid wire as shown in the figure or a twisted wire (not shown). An insulating coating is provided around the conductor. The insulating coating is formed over substantially the entire length of the conductor. The insulating coating is made of an insulating resin. The coated conductor wire 31, including the conductor and insulating coating, may be used as a solid wire, but two may be twisted together to form a pair wire, or four may be twisted together to form a quad wire.
[0035] The multiple covered conductor wires 31 are bundled with a loosely wound string 33. A pressure winding tape 37 is further wound collectively around the outer circumference of the multiple bundles of the multiple covered conductor wires 31. In the metallic cable 30a, the multiple covered conductor wires 31 bundled with the pressure winding tape 37 form the cable core portion 25. The pressure winding tape 37 may be a loosely wound string or the like as long as it is capable of bundling the multiple covered conductor wires 31.
[0036] Here, there are various methods for forming cable core portion 25, such as twisting pair wires and quad wires together to form a unit, and then twisting the unit again, or twisting single core wires, pair wires, and quad wires in a central layer, and then twisting single core wires, pair wires, and quad wires in the first and second layers above that.
[0037] The laminate tape 1 is wound around the outer periphery of the pressure winding tape 37. The laminate tape 1 is wound by longitudinal splicing so that both ends in the width direction are overlapped in the circumferential direction. That is, the laminate tape 1 is wound around the outer periphery of the cable core portion 25 by aligning the axial direction of the cable core portion 25 with the longitudinal direction of the laminate tape 1. At this time, the wrap portion 23 where both ends of the laminate tape 1 are overlapped is formed in a substantially linear shape in the axial direction of the cable core portion 25.
[0038] An outer sheath 17 is provided on the outer periphery of the laminate tape 1. The outer sheath 17 is provided so as to cover the outer periphery of the laminate tape 1. In other words, the laminate tape 1 wound around the outer periphery of the cable core portion 25 is disposed inside the outer sheath 17, and the outer sheath 17 is provided on the outermost periphery of the cable core portion 25.
[0039] The outer jacket 17 is made of medium density polyethylene or higher density (930 kg / m 3 or more), and more preferably high-density polyethylene (942 kg / m 3 The above is the case. Note that carbon black or the like may be added to the outer cover 17.
[0040] Here, low-density polyethylene (LDPE) is generally selected as the material for the outer jacket 17 in order to obtain manufacturability and flexibility. However, if the outer jacket 17 is formed by extrusion using conventional LDPE, the relatively low extrusion temperature suitable for LDPE is insufficient to melt the resin layer 5 of the laminate tape 1, and there is a risk that the resin layer 5 and the metal layer 3 will not be adhesively bonded to each other at the lap portion 23.
[0041] However, if the outer sheath 17 is made of medium-density polyethylene (MDPE) or higher, the temperature suitable for extruding MDPE becomes close to the bonding temperature range of the resin layer 5 of the laminate tape 1, and the resin layer 5 and metal layer 3 can be adhesively bonded at the wrap portion 23, thereby sealing the cable core portion 25.
[0042] Furthermore, when the sheath 17 is made of high density polyethylene (HDPE), it is necessary to extrude the sheath 17 at a higher temperature than when MDPE is extruded, but the same degree of rigidity can be maintained even when the sheath 17 is made thinner. Therefore, the thickness of the sheath 17 can be made 10% or less of the outer diameter of the metallic cable 30a, and more preferably, 8% or less of the outer diameter of the metallic cable 30a. For example, the thickness of a typical sheath is about 2 mm, but it can be made about 1.7 mm. In this way, the metallic cable 30a can be made lighter and easier to bend, improving the workability of the cable.
[0043] In the metallic cable 30a, the laminate tape 1 functions as a moisture permeation prevention layer. That is, the wrap portion 23 of the laminate tape 1 is adhesively bonded, and the resin layer 5 of the laminate tape 1 and the jacket 17 are continuously bonded in the longitudinal direction, thereby making it possible to restrict the path of moisture penetration.
[0044] The outer covering 17 may be one layer or two or more layers, in which case the laminate tape 1 can be used by being disposed as the inner layer of any of the outer coverings 17. The laminate tape 1 may also be used in two or more layers, and a metal exterior suitable for the purpose may be applied as another layer in addition to the laminate tape 1.
[0045] In the metallic cable 30a, a tear cord 35 is disposed between the laminate tape 1 and the cable core portion 25. By pulling out the tear cord 35, the laminate tape 1 and the outer sheath 17 can be torn apart, and the covered conductor wire 31 inside can be taken out.
[0046] In the metallic cable 30a, the number of coated conductor wires 31 constituting the cable core portion 25 and the number of bundles are not limited to those shown in the figure. Also, the metallic cable 30a may be a composite cable further including optical fibers or the like.
[0047] As described above, the laminate tape 1 has a wrap portion 23. Fig. 4(a) is an enlarged view of part A in Fig. 3, which is an enlarged view of the wrap portion 23. The laminate tape 1 is wrapped around the outer periphery of the cable core portion 25 with the resin layer 5 on the outside. That is, the jacket 17 and the resin layer 5 are adhesively bonded. In the wrap portion 23, the metal layer 3 at the outer end of the wrap portion 23 and the resin layer 5 at the inner end are adhesively bonded.
[0048] Here, the wrap length (B in the figure) of the wrap portion 23 in the circumferential direction is preferably 1 mm or more and 2.0 times or less the outer diameter of the metallic cable 30a, and more preferably 1.5 times or less the outer diameter. For example, the length of the wrap portion is about 7 mm to 20 mm. If the wrap length is too short, there is a risk of deterioration of the water impermeability due to the opening of the wrap portion 23 when bending the metallic cable 30a. On the other hand, if the wrap length is too long, the moisture permeation prevention layer becomes thick, which also affects flexibility.
[0049] As shown in Fig. 4(b), the resin layer 5 may have a thicker portion at least on one end of the laminate tape 1. In this way, the thickness of the resin layer 5 on the inside of the wrap portion 23 of the laminate tape 1 (C in the figure) can be made thicker than the thickness of the resin layer 5 in areas other than the wrap portion 23. Although a method of making the entire resin layer thick is also conceivable, making areas other than the wrap portion thick would lead to increased material costs, so it is better to make only the wrap portion thicker.
[0050] For example, when the ends of the laminate tape 1 are joined at the wrap portion 23, if the thickness of the resin layer 5 is about 50 μm, it is not possible to absorb the irregularities on the outer periphery of the cable core portion 25, and there is a risk that the end of the laminate tape 1 will float. For this reason, by making the thickness of the resin layer 5 in the wrap portion 23 thicker (for example, about 100 μm), it is possible to prevent gaps from being generated in the wrap portion 23.
[0051] 5, waterproof resin 27 may be injected into the lap portion 23 of the laminate tape 1. By injecting waterproof resin 27 from the outer periphery of the lap portion 23 into the gap of the lap portion 23 of the laminate tape 1, the total thickness of the resin in the vicinity of the lap portion 23 (resin layer 5 + waterproof resin 27) can be made thicker than the thickness of the resin layer 5 in the portion other than the lap portion 23. In other words, by making the amount of resin in the lap portion 23 and its vicinity of the laminate tape 1 greater than the amount of resin outside the lap portion 23, the opening of the lap portion 23 as described above can be suppressed, and the lap portion 23 can be reliably joined. Note that, as shown in FIG. 4(b), the thickness of the resin layer 5 of the lap portion 23 may be made thick, and waterproof resin 27 may be further injected.
[0052] Furthermore, when the waterproof resin 27 is injected into the wrap portion 23, the waterproof resin 27 is also applied to the stepped portion on the outside of the wrap portion 23, so that the steps at the end of the wrap portion 23 can be filled and smoothed out. This ensures that the outer cover 17 and the resin layer 5 are bonded together, preventing the occurrence of gaps. The waterproof resin 27 can be made of the same material as the resin layer 5, for example.
[0053] Next, a method for manufacturing the metallic cable 30a will be described. An insulating coating is formed around the conductor by extrusion, for example, to form the coated conductor 31. Next, the coated conductor 31 is twisted and assembled into pair wires, quad wires, and units, or multi-layered pair wires and quad wires, and bundled with a loosely wound string 33 as necessary. A plurality of bundles are collectively wrapped with a pressure winding tape 37 to form the cable core section 25. The pressure winding tape 37 may be a loosely wound string or the like, and may be any tape capable of bundling the assembled cores. A laminate tape 1 in which a resin layer 5 and a metal layer 3, etc., have been bonded together is supplied, and a forming machine or the like is used to vertically wind the pressure winding tape 37 (cable core section 25) around the outer periphery to form a moisture permeation prevention layer.
[0054] As described above, when the laminate tape 1 is formed into a cylindrical shape, the two ends of the laminate tape 1 overlap each other to form the lap portion 23. In this state, the laminate tapes 1 are not fused to each other in the lap portion 23, so there is a risk that the overlapping portions will open up slightly and create gaps. If the jacket is extruded in this state, the lap portion 23 will be formed with air remaining in the gaps, and there is a risk that the joining of the resin layer 5 and the metal layer 3 of the lap portion 23 will be incomplete.
[0055] Therefore, it is desirable to inject the waterproof resin 27 between the laminate tapes 1 in the lap portion 23 before extruding the outer sheath 17 after winding the laminate tape 1 so as to fill such gaps. For example, after winding the laminate tape 1, a nozzle or needle is placed on the outer joint of the lap portion 23, and the waterproof resin 27 is injected from there. Also, if necessary, after injecting the waterproof resin 27, the lap portion 23 is pressed from the outer periphery to make it even. The applied thickness of the waterproof resin 27 is about 1 mm or less. That is, the waterproof resin 27 is injected in an amount such that a part of the waterproof resin 27 protrudes from the lap portion 23. In this way, the lap portion 23 can be sealed and partially bonded in advance before extruding the outer sheath 17. Also, the step formed in the lap portion 23 can be made somewhat gentler.
[0056] Next, the outer jacket 17 is extruded and integrated onto the outer periphery of the moisture barrier layer formed by the laminate tape 1. Since the outer jacket 17 is made of medium density polyethylene or high density polyethylene, it is extruded at a temperature higher than the extrusion temperature of conventional polyethylene. For example, it is desirable to extrude the outer jacket 17 at a temperature of 200°C or higher. In this manner, the resin layer 5, the metal layer 3, and the waterproof resin 27 are reliably adhesively bonded together. In this manner, the metallic cable 30a is manufactured.
[0057] As described above, according to this embodiment, the resin layer 5 is a resin in which maleic anhydride is grafted onto a thermoplastic resin with good high-temperature resistance, and therefore has a high softening temperature, and can reliably maintain the bonding of the wrap portion 23 even at high temperatures. Furthermore, by using medium-density polyethylene or high-density polyethylene for the outer jacket 17, the resin layer 5 containing maleic acid and the metal layer 3 are reliably bonded and sealed, thereby improving water-stopping properties. Furthermore, the outer jacket 17 and the resin layer 5 are reliably bonded continuously in the longitudinal direction, so buckling of the laminate tape 1 can be suppressed.
[0058] Furthermore, by making the resin layer 5 of the wrap portion 23 thicker, the wrap portion 23 can be joined more reliably. For example, since the outer peripheral surface of the cable core portion 25 is not necessarily flat (a completely uniformly curved surface), some unevenness also occurs in the resin layer 5 when the laminate tape 1 is wound around it. If the outer jacket 17 is extruded in this state, there is a risk that a gap will remain between the resin layer 5 and the metal layer 3, which face each other in the wrap portion 23. In contrast, by making the resin layer 5 thicker, the resin layer 5 acts as a cushion when the outer jacket 17 is extruded, and the wrap portion 23 can be joined more reliably.
[0059] The same effect can be obtained by injecting waterproof resin 27 into wrap portion 23. Injecting waterproof resin 27 can also smooth out the steps in wrap portion 23, thereby preventing air pockets from forming when jacket 17 is extruded.
[0060] In addition, since the outer sheath 17 is made of medium-density polyethylene or high-density polyethylene, the thickness of the outer sheath 17 can be made thinner, making the cable lighter and easier to bend, although this reduces flexibility somewhat, thereby improving the ease of installation of the cable.
[0061] Next, a second embodiment will be described. Fig. 6 is a perspective view showing a metallic cable 30b. In the following description, the same components as those in the metallic cable 30a are denoted by the same reference numerals as in Figs. 1 to 5, and duplicated description will be omitted.
[0062] The metallic cable 30b has a configuration similar to that of the metallic cable 30a, but is different in that the laminate tape 1 is corrugated. The corrugated shape of the laminate tape 1 is formed such that peaks and valleys are repeated in the longitudinal direction of the cable core portion 25, and the peaks and valleys are each continuous in the circumferential direction. The metallic cable 30b may be smooth without being corrugated.
[0063] The corrugated shape of the laminate tape 1 may be formed during the production of the laminate tape 1 by feeding and winding the corrugated laminate tape 1 around the outer periphery of the cable core portion 25, or the corrugation process may be performed simultaneously when the laminate tape 1 is formed.
[0064] In this way, the laminate tape 1 can be corrugated as necessary before use. Even in this case, the thickness of the resin layer 5 may be increased in the wrap portion 23, or a waterproof resin 27 may be injected. The wrap portion 23 is formed in this manner, which also applies to the other embodiments described below.
[0065] Next, a third embodiment will be described. Fig. 7 is a cross-sectional view showing a metallic cable 30c. The metallic cable 30c has an inner sheath 39. In the metallic cable 30c, similar to the metallic cables 30a and 30b, a plurality of covered conductor wires 31 are bundled with a loosely wrapped string 33, and a pressure winding tape 37 is wound around the outer periphery of the bundle. The pressure winding tape 37 may be a loosely wrapped string or the like as long as it can bundle a plurality of bundles. In addition, a first laminate tape 1 is wound vertically around the outer periphery of the pressure winding tape 37 (cable core portion 25) to form a lap portion 23.
[0066] In the metallic cable 30c, an inner sheath 39 is formed around the outer periphery of the first laminate tape 1. The inner sheath 39 is formed by, for example, extrusion. The second laminate tape 1 is further wound around the outer periphery of the inner sheath 39.
[0067] The outer sheath 17 is provided on the outer periphery of the second laminate tape 1 on the outside, which is the outermost periphery of the metallic cable 30c. That is, the second laminate tape 1 is disposed inside the outer sheath 17. The outer sheath 17 is provided so as to cover the outer periphery of the second laminate tape 1, and is bonded to the resin layer 5 of the second laminate tape 1. That is, the metallic cable 30c has two resin layers, the outer sheath 17 and the inner sheath 39, and the laminate tape 1 is wound in two layers on the inner side of each of the outer sheath 17 and the inner sheath 39. Note that when the metallic cable 30c has two resin layers, the outer sheath 17 and the inner sheath 39, the laminate tape 1 may be a single layer only on the inner side of either the outer sheath 17 or the inner sheath 39, and in this case, an exterior suitable for the purpose may be provided on the inner side of the outer sheath 17 or the inner sheath 39 where the laminate tape 1 is not disposed. As an example of the exterior, it may be wrapped in iron or stainless steel to protect it from bird and animal damage.
[0068] In this manner, when providing the inner sheath 39, tear strings 35a, 35b are disposed between the first laminate tape 1 on the inner periphery side and the holding winding tape 37 (cable core portion 25) and between the inner sheath 39 and the second laminate tape 1 on the outer periphery side, respectively. In this manner, by pulling out the tear string 35b, the outer laminate tape 1 and the outer jacket 17 can be torn apart to expose the inner sheath 39. Furthermore, by further pulling out the tear string 35a, the inner laminate tape 1 and the inner sheath 39 can be torn apart to allow the covered conductor wire 31 inside to be taken out.
[0069] In this embodiment, the cable core part 25 is up to the pressure winding tape 37, but the cable core part 25 may include the inner sheath 39. In either case, the laminate tape 1 is wound around the outer periphery of the cable core part. The inside of the inner sheath 39 may be made of only resin without the laminate tape 1.
[0070] In this manner, by applying the laminate tape 1 to the metallic cables 30a, 30b, and 30c, it is possible to obtain metallic cables that are not only waterproof but also have excellent environmental resistance.
[0071] Furthermore, by providing an inner sheath 39 and providing tear cords 35a, 35b at respective locations like the metallic cable 30c, the outer jacket 17 etc. and the inner sheath 39 etc. can be torn separately, making the tearing operation easy and preventing breakage of the tear cords, etc.
[0072] Next, a fourth embodiment will be described. Fig. 8 is a cross-sectional view showing an optical cable 40. The optical cable 40 is composed of a tension member 41, a spacer 43, an optical fiber ribbon 47, an inner sheath 39, a laminate ribbon 1, an outer jacket 17, and the like.
[0073] The spacer 43 is made of a flexible resin. A plurality of grooves 45 are provided on the outer periphery of the spacer 43, and the grooves 45 are formed in a spiral shape in one direction relative to the longitudinal direction of the spacer 43, or in an SZ shape in both directions, and are repeated continuously. A tension member 41 is provided in the center of the spacer 43. A plurality of optical fiber ribbons 47 are housed in the grooves 45. The optical fiber ribbon 47 is, for example, an optical fiber ribbon in which optical fibers adjacent to each other in the longitudinal direction are bonded with a UV resin.
[0074] A pressure winding tape 49 is wound around the outer periphery of the spacer 43 by longitudinal wrapping or spiral winding. An inner sheath 39 is provided around the outer periphery of the pressure winding tape 49 (cable core portion 25). The inner sheath 39 is formed, for example, by extrusion molding. A protective tape 53 is wound around the outer periphery of the inner sheath 39. The inner sheath 39 and the protective tape 53 are made of resin, and the inner sheath 39 and the protective tape 53 are not bonded to each other.
[0075] The laminate tape 1 is wound around the outer periphery of the protective tape 53. As described above, the laminate tape 1 is wound vertically with the resin layer 5 on the outer periphery and the lapped portion 23 provided.
[0076] In this embodiment, the cable core portion 25 is up to the pressure winding tape 49, but the cable core portion may include the inner sheath 39 and the protective tape 53, or may include only the inner sheath 39 without using the protective tape 53. As described above, in either case, the laminate tape 1 is wound around the outer periphery of the cable core portion. That is, in the present invention, the laminate tape 1 being wound around the outer periphery of the cable core portion includes the provision of other components such as the protective tape 53 between the cable core portion and the laminate tape 1. Furthermore, as in the metallic cable described above, the laminate tape 1 may be smooth or may be corrugated, and the layer to which the laminate tape 1 is not applied may be provided with an exterior suitable for the purpose.
[0077] An outer jacket 17 is provided on the outer periphery of the laminate tape 1, which is the outermost periphery of the optical cable 40. That is, the laminate tape 1 is disposed inside the outer jacket 17. The outer jacket 17 is provided so as to cover the outer periphery of the laminate tape 1, and is bonded to the resin layer 5 of the laminate tape 1.
[0078] In the optical cable 40, a tear string is also arranged between the laminate tape 1 and the cable core portion 25. In the illustrated example, a tear string 35a is arranged between the holding winding tape 49 (cable core portion 25) and the inner sheath 39, and further, a tear string 35b is arranged between the protective tape 53 and the laminate tape 1. By pulling out the tear string 35b, the laminate tape 1 and the outer jacket 17 can be torn apart to expose the internal protective tape 53, etc. Furthermore, by further pulling out the tear string 35a, the internal sheath 39 and the protective tape 53 can be torn apart to take out the optical fiber ribbon 47.
[0079] In the optical cable 40, the shape, number, and depth of the grooves 45 and the configuration of the optical fiber ribbon 47 are not limited to the illustrated example. Also, the inner sheath 39 and the protective tape 53 are not necessarily required.
[0080] In this way, by applying the laminate tape 1 to the optical cable 40, it is possible to obtain an optical cable that is excellent in environmental resistance as well as ensures water-proofing. It is also possible to further improve water-proofing by forming a resin layer 5 so that the wrap portion 23 of the laminate tape 1 can be easily attached.
[0081] In addition, by wrapping protective tape 53 between the tear cord 35b and the inner sheath 39, it is possible to prevent the tear cord 35b from digging into or adhering to the inner sheath 39, making it difficult to pull out.
[0082] In this way, the laminate tape 1 can be suitably applied to various types of cables. EXAMPLES
[0083] Next, several samples were produced by changing the resin layer and jacket of the cable shown in Figure 1, and the appearance abnormalities and the presence or absence of buckling of the laminate tape after a twisting test were evaluated. The laminate tape used had a metal layer made of 150μm stainless steel and a resin layer made of 100μm low-density polyethylene. The cable had an overall diameter of about 23mm, and was cut into 1.5m lengths for evaluation. The conditions and results are shown in Table 1.
[0084] [Table 1]
[0085] The presence or absence of grafting of maleic anhydride indicates the presence or absence of grafting by adding maleic anhydride to the base resin HDPE. As for "resin amount in the lapped part is greater than that in the lapped area", as mentioned above, the case where the resin layer in the lapped part is thick (waterproofing resin injection) is marked as "○", and the case where there is no change in the resin thickness in the lapped part is marked as "×".
[0086] The twisting test was carried out at 75°C. First, both ends of the cable were held, and the other end was twisted 90 degrees in one direction, returned to its original position, then twisted 90 degrees in the opposite direction and returned to its original position. This counted as one full round of 90-degree twisting, and the test was carried out with 8 rounds of 90-degree twisting. As with the appearance abnormalities, if there was no buckling of the laminate tape or cracks in the outer sheath, it was marked as ◯, and if there was buckling of the laminate tape or cracks in the outer sheath, it was marked as ×.
[0087] In Examples 1 to 7, the outer covering was medium density polyethylene (MDPE) or high density polyethylene (HDPE), and the base resin of the laminate tape was medium density polyethylene (MDPE), high density polyethylene (HDPE), or polypropylene (PP) with 1% grafted maleic anhydride, so the external appearance abnormality and the twist test were passed (○).
[0088] On the other hand, in the cable in which the laminate tape used a resin layer formed from a resin without added maleic anhydride and the jacket was formed by extruding HDPE as in Comparative Example 1, lifting was observed at the lapped portion of the laminate tape, and furthermore buckling was observed in some places. This is thought to be because the laminate tape and the jacket were not continuously joined in the longitudinal direction of the cable.
[0089] If the laminate tape and the jacket are not continuously joined in the longitudinal direction of the cable, either the laminate tape or the jacket must resist the twisting force, which places an excessive load on the laminate tape, making it more likely for the laminate tape to lift or buckle at the wrapped portion. In contrast, if the laminate tape and the jacket are continuously joined in the longitudinal direction of the cable, both the laminate tape and the jacket can resist the twisting force. For this reason, Comparative Example 1 failed the twisting test (×).
[0090] In addition, in Comparative Example 2, the outer covering was made of low-density polyethylene and the extrusion temperature was low, so that the twist test was unsuccessful (×).
[0091] In addition, in Comparative Example 3, the amount of resin in the wrap portion was the same as in other portions without any increase in the waterproof resin, and therefore the twist test was failed (×). This is because when the cable is twisted, peeling may occur at the wrap portion because no waterproof resin is injected. This twist test is an acceleration test assuming that the cable is installed while being twisted in the usage environment, and peeling of the wrap portion is considered to occur when stress is continuously applied to the wrap portion of the laminate tape for a long period of time, causing the adhesive portion to become unable to withstand it. For this reason, when the cable core is attached vertically with the laminate tape, by forming an outer sheath in a state where the wrap portion is filled with the same resin as the resin layer of the laminate tape, peeling at the wrap portion is considered to be prevented even when the cable is bent for a long period of time.
[0092] In Comparative Example 4, the base resin of the resin layer of the laminate tape was low-density polyethylene (LDPE), and in Comparative Example 5, the base layer of the resin layer of the laminate tape was ethylene-vinyl acetate copolymer (EVA), so during the twist test, the base resin of the resin layer of the laminate tape softened, the wrap portion peeled off, and the outer coating was damaged. In addition, in Comparative Example 6, when the outer resin was low-density polyethylene (LDPE) and the base resin of the resin layer of the laminate tape was also low-density polyethylene (LDPE) and the extrusion temperature was set at 230°C, the base resin of the resin layer of the laminate tape softened during the twist test, causing the wrap portion to peel off and damaging the outer resin.
[0093] Although the embodiment of the present invention has been described above with reference to the attached drawings, the technical scope of the present invention is not limited to the above-described embodiment. It is clear that a person skilled in the art can think of various modifications or alterations within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.
[0094] For example, it goes without saying that the configurations of the respective embodiments described above can be combined with each other. [Explanation of symbols]
[0095] 1. Laminated tape 3……Metal layer 5: Resin layer 17……Outer cover 23....Rap section 25………Cable core section 27……Waterproof resin 30a, 30b, 30c...Metallic cable 31....Covered conductor 33………Coarsely wound cord 35, 35a, 35b………Tear cord 37………Pressing tape 39………Inner sheath 40...Optical cable 41...Tension member 43...Spacer 45……groove 47: Optical fiber ribbon 49………Pressing tape 53...Protective tape
Claims
1. A cable core portion, an outer sheath provided on the outermost circumference of the cable core portion; a laminate tape disposed inside the outer sheath and wound around an outer periphery of the cable core portion; A cable comprising: the laminate tape is configured by laminating a resin layer and a metal layer, and a wrap portion is formed in which both ends of the laminate tape are overlapped, and the laminate tape is wrapped around an outer periphery of the cable core portion; The resin layer has a base resin of polypropylene, to which maleic anhydride has been added and grafted, the amount of resin in the lap portion and in the vicinity of the lap portion of the laminate tape is greater than the amount of resin in other portions than the lap portion; The outer jacket is made of polyethylene having a density equal to or greater than medium density polyethylene, A cable characterized in that, after a twist test in which both ends of the cable are held, one end of the cable is twisted 90 degrees in a certain direction at 75°C, returned to its original position, and then twisted 90 degrees in the opposite direction to the first direction and returned to its original position, one round trip of 90 degrees twist is counted, and no buckling of the laminate tape or cracks are generated in the outer sheath after the twist test, which consists of eight round trips of 90 degrees twist.
2. An optical cable as described in claim 1, characterized in that the wrap length in the circumferential direction of the wrap portion is 7 mm to 15 mm.
3. A cable as described in claim 1 or claim 2, characterized in that the polypropylene grafted with the addition of maleic anhydride has a melt mass-flow rate, as defined in JIS K 7210-1 (2014), of 0.2 g / 10 min or more and 20 g / 10 min or less.
4. A cable as described in claim 3, characterized in that the melt mass flow rate is 1.0 g / 10 min or more and 15 g / 10 min or less.
5. 5. The cable according to claim 1, wherein the outer jacket is made of high density polyethylene.
6. 6. The cable according to claim 1, wherein the outer jacket and the resin layer of the laminate tape are joined continuously in the longitudinal direction.
7. The cable according to any one of claims 1 to 6, characterized in that in the wrap portion of the laminate tape, a portion is formed in which the thickness of the resin layer is thicker than the thickness of the resin layer in portions other than the wrap portion.
8. A cable as described in any one of claims 1 to 7, characterized in that a waterproof resin is injected into the wrap portion of the laminate tape, and the waterproof resin is applied to any stepped portion on the outside of the wrap portion, filling in the steps and forming a smooth slope.
9. 9. The cable according to claim 8, wherein the waterproof resin is made of the same material as the resin layer of the laminate tape.
10. 10. The cable according to claim 1, wherein the thickness of the outer jacket is 10% or less of the outer diameter of the cable.
11. The thickness of the outer jacket is 8% or less of the outer diameter of the cable. A cable according to any one of claims 1 to 10.
12. A method for producing a cable according to any one of claims 1 to 11, comprising the steps of: After the laminating tape is wound, and before the outer covering is extruded, a waterproofing resin is injected between the laminating tapes in the lap portion; A method for producing a cable, comprising extrusion molding the outer sheath at a temperature of 200°C or higher.
Citation Information
Patent Citations
Kotaino netsushoriro
JP1976020710A
Preparation laminate sheathed cable
JP1978141483A
JP1979015781U
Waterrproof cable manufacture
JP1979021586A
JP1979093789U