Nonwoven fabric manufacturing method

The method of embossing with temperature-differentiated rolls and low-speed air-through processing addresses the challenge of suppressing fuzz and maintaining flexibility in nonwoven fabrics, resulting in a fabric with reduced surface fluff and enhanced three-dimensional appearance.

JP7575208B2Active Publication Date: 2024-10-29KAO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020117262
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-07
Publication Date
2024-10-29
Estimated Expiration
2040-07-07

AI Technical Summary

Technical Problem

Existing nonwoven fabric manufacturing methods struggle to achieve both suppression of surface fuzz and maintain a three-dimensional appearance and flexibility, often compromising one for the other by excessive use of high temperatures or air speeds during air-through processing.

Method used

A method involving embossing with a high-temperature and low-temperature roll pair, followed by air-through processing with low-speed hot air, to form thermocompression bonded portions using core-sheath fibers, ensuring the sheath melts while the core remains intact, thereby suppressing fuzz and maintaining flexibility.

Benefits of technology

Produces a nonwoven fabric with reduced fuzz and excellent flexibility, suitable for skin contact, maintaining a clear three-dimensional texture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575208000003
    Figure 0007575208000003
  • Figure 0007575208000004
    Figure 0007575208000004
  • Figure 0007575208000005
    Figure 0007575208000005
Patent Text Reader

Abstract

To provide a nonwoven fabric manufacturing method capable of manufacturing a nonwoven fabric that has less fuzz and is excellent in flexibility.SOLUTION: A nonwoven fabric manufacturing method has an embossing step to sandwich a fiber web 11 containing core-sheath fibers by a pair of rolls formed of a high-temperature embossing roll 21 and a low-temperature roll 31 and form a thermal compression bonded portion 12 on the fiber web 11, and an air-through step to apply air-through processing by blowing a hot blast 42 to the fiber web 11 at air velocity of 1 m / second or less after the embossing step and bond the core-sheath fibers with each other. The temperature of the high-temperature embossing roll 21 is equal to or higher than a melting point of a sheath component of the core-sheath fiber and the temperature of the low-temperature roll 31 is lower than the melting point of the sheath component of the core-sheath fiber.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a nonwoven fabric. [Background technology]

[0002] Regarding the manufacturing method of nonwoven fabrics for use in absorbent articles, many techniques have been proposed for manufacturing nonwoven fabrics having excellent feel. For example, Patent Document 1 describes a method for producing a three-dimensionally shaped nonwoven fabric, in which a web is embossed to form a pressure-bonded portion, and then an air-through process is performed using hot air. In this production method, a general embossing device is used, and heat-extensible fibers that expand in length when heated are used as the constituent fibers of the web. Patent Document 2 also describes a shaped nonwoven fabric having openings. The method for producing this shaped nonwoven fabric uses a shaping roll for thermal compression, which is composed of an upper heated roll that has convex parts (pin rolls) that enable compression hole punching and concave parts that allow the thickness of the nonwoven fabric to remain alternately in the width direction of the roll, and a lower roll that has holes in the part that receives the pin roll. It is described that the temperatures of the upper heated roll and the lower roll are both the same at 115°C, and hole punching and shaping processing are performed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-350836 A [Patent Document 2] JP 2018-90932 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the nonwoven fabric, the uneven surface embossed during the manufacturing process has a three-dimensional appearance and a good texture, and is therefore sometimes used as the surface of an absorbent article or other product that comes into contact with the skin. In this case, if the surface that comes into contact with the skin has too much fiber fuzz, it will cause discomfort to the user. For this reason, in the past, air-through processing was used to blow hot air after embossing, and the temperature and speed of the hot air were increased to suppress the fuzz on the surface. However, excessively high hot air temperature or hot air velocity can impair the apparent three-dimensional appearance and softness of the produced nonwoven fabric, making it difficult to simultaneously suppress surface fuzzing and achieve apparent three-dimensional appearance and softness.

[0005] In view of the above, the present invention relates to a method for producing a nonwoven fabric, which can produce a nonwoven fabric with less fluff and excellent softness. [Means for solving the problem]

[0006] The present invention provides a method for producing a nonwoven fabric, comprising: an embossing step in which a fiber web containing core-sheath fibers is sandwiched between a pair of rolls consisting of a high-temperature embossing roll and a low-temperature roll to form a thermocompression bonded portion in the fiber web; and an air-through step in which hot air having a speed of 1 m / sec or less is blown onto the fiber web after the embossing step to perform an air-through processing and bond the core-sheath fibers to each other by thermal fusion, wherein the temperature of the high-temperature embossing roll is equal to or higher than the melting point of the sheath component of the core-sheath fibers, and the temperature of the low-temperature roll is lower than the melting point of the sheath component of the core-sheath fibers. Effect of the Invention

[0007] According to the method for producing a nonwoven fabric of the present invention, a nonwoven fabric having little fluff and excellent softness can be produced. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic front view showing a preferred embodiment of an apparatus used in a method for producing a nonwoven fabric of the present invention. [Diagram 2] FIG. 2 is an enlarged front view showing a schematic diagram of embossing performed by clamping a fiber web between a pair of rolls. [Diagram 3] Photograph (A) is a drawing substitute photograph showing an image of the surface of nonwoven fabric sample S5 of Example 5, and photograph (B) is a drawing substitute photograph showing an image of the surface of nonwoven fabric sample C2 of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for producing a nonwoven fabric of the present invention will be described below with reference to the drawings.

[0010] The method for producing a nonwoven fabric of the present invention includes an embossing step in which a fiber web 11 containing core-sheath fibers is sandwiched between a pair of rolls consisting of a high-temperature embossing roll 21 and a low-temperature roll 31 having different roll temperatures, to form thermocompression-bonded portions 12 in the fiber web 11. In addition, the manufacturing method of the nonwoven fabric of the present invention includes an air-through process after the embossing process in which hot air 42 having a wind speed of 1 m / sec or less is blown onto the fiber web 11 to perform air-through processing and bond the core-sheath fibers together by thermal fusion.

[0011] The manufacturing method of the nonwoven fabric of the present invention having these steps is carried out, for example, by using a high-temperature embossing roll 21, a low-temperature roll 31, and an air-through machine 41 as shown in Fig. 1. The above-mentioned embossing step is carried out by the high-temperature embossing roll 21 and the low-temperature roll 31, and the above-mentioned air-through step is carried out by the air-through machine 41 located downstream thereof. This produces a nonwoven fabric 10 that has little fuzz, excellent flexibility, and a three-dimensional feel.

[0012] (Embossing process) In the embossing process, rolls with different roll temperatures are used. As shown in Figures 1 and 2, a high-temperature embossing roll 21 and a low-temperature roll 31 arranged opposite to each other rotate while sandwiching a fiber web 11 transported from the upstream side between the two rolls. At this time, the high-temperature embossing roll 21 is heated, and its roll temperature is equal to or higher than the melting point of the sheath component of the core-sheath fiber contained in the fiber web 11. On the other hand, the roll temperature of the low-temperature roll 31 is lower than the melting point of the sheath component of the core-sheath fiber. The "roll temperature" referred to here refers to the roll surface temperature. By performing the embossing process between the high-temperature embossing roll 21 and the low-temperature roll 31 having such a temperature difference, the bulkiness of the fibers between the thermocompression bonded parts 12, 12 formed by the embossing is maintained on the surface 11A of the fiber web 11 that is in contact with the high-temperature embossing roll 21, and fluffing is effectively suppressed. This point will be described in detail below. When the high-temperature embossing roll 21 and the low-temperature roll 31 sandwich the fiber web 11, the heated high-temperature embossing roll 21 presses one surface 11A of the fiber web 11 in the thickness direction with the convex parts 22, as shown in Fig. 2. As a result, the convex parts 22 melt-press the constituent fibers together with heat equal to or higher than the melting point of the sheath component, and form flat thermocompression parts 12 on the surface of the fiber web 11 in the same pattern as the convex parts 22. On the other hand, the recesses 23 present between the protrusions 22, 22 of the high-temperature embossing roll 21 do not press one surface 11A of the fibrous web 11 in the thickness direction, and do not form thermocompression-bonded parts 12. As a result, the part of one surface 11A of the fibrous web 11 facing the recesses 23 maintains the coarse fiber structure of the fibrous web 11 even after embossing, and becomes a bulky part 13 having a sufficient thickness. At this time, the roll temperature of the low-temperature roll 31 is lower than that of the high-temperature embossing roll 21, and is lower than the melting point of the sheath component of the core-sheath fiber. The opposite surface 11B of the fiber web 11 to which the low-temperature roll 31 is applied is not heated to melt the core-sheath fiber. Therefore, in the bulky part 13, heating from the opposite surface 11B side to the inside is suppressed, also due to the low thermal conductivity of the sparse fiber structure. As a result, while the bulky fiber structure of the bulky part 13 is maintained, the high-temperature embossing roll 21 heats and softens the fluffy fibers protruding from the top surface of the bulky part 13 by its roll temperature, and the protrusion can be suppressed. At this time, the fluffy fibers easily enter the spaces between the sparse fibers of the bulky part 13, which is effective in preventing the protrusion. And, the bulky part 13 has high flexibility due to suppressed hardening of the fibers, and has an excellent three-dimensional appearance. In FIG. 1, the projections and recesses on the peripheral surface of the high-temperature embossing roll 21 are omitted.

[0013] The fiber web to be processed is an aggregate of fibers before the fibers are bonded together. In other words, it is a material before being made into a nonwoven fabric. The fiber web in the present invention may be a single-layer web consisting of only one layer, or a laminated web in which two or more layers are laminated in the thickness direction. In FIG. 1, the fiber web 11 is indicated by a thick line. Fuzz refers to constituent fibers that stand up more than 1 mm in the thickness direction on the surface of the fiber web 11 or nonwoven fabric 10. Such fuzz can occur when the constituent fibers of the fiber web 11 are not sufficiently fused together during the manufacturing process of the nonwoven fabric 10, or when some of the constituent fibers peel off from the surface and become raised during use of the nonwoven fabric 10. By suppressing fuzzing on the surface of the nonwoven fabric, it is possible to obtain a nonwoven fabric 10 that is pleasant to the touch and provides a comfortable sensation to the user of an absorbent article or the like.

[0014] The high-temperature embossing roll 21 has convex portions 22 and concave portions 23 arranged alternately on the roll circumferential surface. Although the convex portions 22 and concave portions 23 are shown in FIG. 1 as being arranged alternately in the roll circumferential direction, this is not limited thereto. They can be appropriately set according to the embossing arrangement in the nonwoven fabric 10 to be manufactured. For example, the convex portions 22 and concave portions 23 may be arranged alternately along the roll axial direction. This alternating arrangement may also be arranged along the roll circumferential direction and a diagonal direction intersecting with the roll axial direction. Furthermore, this alternating arrangement is not limited to any one of the roll circumferential direction, the roll axial direction, and a diagonal direction intersecting with these directions, and may be arranged along a plurality of directions.

[0015] The shape of the low-temperature roll 31 is not particularly limited as long as it exhibits the above-mentioned function. For example, it may be an embossing roll having irregularities on its peripheral surface like the high-temperature embossing roll 21, or a flat roll having a flat peripheral surface. However, from the viewpoint of eliminating the need for engraving the surface of the low-temperature roll 31, eliminating the need for phase matching of the irregularities between the high-temperature embossing roll 21 and the low-temperature roll 31, making the pressing force constant, preventing the fiber web 11 from sticking to the low-temperature roll 31, and smoothing the opposite surface 11B of the nonwoven fabric 10 to be manufactured, it is preferable that the low-temperature roll 31 is a flat roll.

[0016] (Air-through process) The fiber web 11 that has been embossed in the embossing step is then transported to an air-through machine 41. In the air-through step, as shown in FIG. 1, while the fiber web 11 passes through the inside of the air-through machine 41, hot air 42 is blown onto the fiber web 11 in an air-through manner. That is, the hot air 42 heated to a predetermined temperature is blown onto the fiber web 11 so as to penetrate the fiber web 11 in the thickness direction. The hot air 42 is blown onto the fiber web 11 at a wind speed of 1 m / sec or less, which is lower than that of conventional air-through processing. This air-through step using the blowing of the low-speed hot air 42 can be realized from the beginning because the aforementioned unique embossing step has been performed first to effectively suppress fuzzing. As shown in Fig. 1, the hot air 42 is preferably blown against the one side 11A of the fibrous web 11 against which the above-mentioned high-temperature embossing roll 21 is applied. This makes it possible to fix the state by heat fusion while further suppressing fuzzing. Since the hot air 42 blows at a low speed, even if the one side 11A on which the bulky portions 13 of the fibrous web 11 are arranged is placed up, the hot air 42 can be blown gently without crushing the bulky portions 13. In this way, the bulky parts 13, which have maintained their coarse fiber structure in the embossing process and have been suppressed from fuzzing, are not crushed by the hot air 42, and the intersections between the constituent fibers of the fiber web 11 are bonded by heat fusion to form a nonwoven fabric. This makes it possible to suitably manufacture a nonwoven fabric 10 that has little fuzzing and excellent flexibility. Moreover, by going through these processes, the thickness of the bulky parts 13 is maintained large, the unevenness is clearly defined, and a nonwoven fabric 10 that has an excellent three-dimensional appearance can be manufactured. The nonwoven fabric 10 thus manufactured is preferably used with the surface 11A that has been subjected to the high-temperature embossing roll 21 as the use surface, since it is less likely to fuzz and is less likely to cause irritation to the skin. For example, when the nonwoven fabric 10 is used in a portion that comes into contact with the skin, such as a top sheet of an absorbent article, the surface 11A of the nonwoven fabric 10 can be used with the surface that comes into contact with the skin, providing the user with a soft, comfortable, and secure feel.

[0017] Next, the materials and devices used in the method for producing the nonwoven fabric of the present invention will be described in detail.

[0018] (Sheath-core fiber) The fiber web 11 used in the present invention contains core-sheath fibers as constituent fibers. By using core-sheath fibers, it is possible to use a component with a lower melting point on the outside (sheath) of the fiber than on the inside (core), and it is possible to adjust the degree to which the fiber melts in the embossing process or air-through process. In addition, since the fibers are bonded to each other by thermal fusion in the sheath portion, the degree of freedom of fiber movement is increased, and a nonwoven fabric 10 with excellent flexibility can be produced. As long as the effects of the present invention are achieved, the fiber web 11 may contain fibers other than core-sheath fibers as constituent fibers.

[0019] The components used in the core-sheath fiber are not particularly limited as long as they can achieve the effects of the present invention. For example, as a component constituting the sheath, polyethylene resin is preferred from the viewpoint of productivity, and examples thereof include low-density polyethylene (hereinafter also referred to as LDPE, melting point: 115°C), high-density polyethylene (hereinafter also referred to as HDPE, melting point: 135°C), linear low-density polyethylene (hereinafter also referred to as LLDPE, melting point: 125°C), etc., and the density is 0.935 g / cm 3 More than 0.965g / cm 3 HDPE having a melting point of 160°C or less is preferred. The component constituting the core is not particularly limited as long as it has a melting point higher than that of the component constituting the sheath. Examples of the component constituting the core include polyolefin resins such as polypropylene (hereinafter also referred to as PP, melting point: 160°C), and polyester resins such as polyethylene terephthalate (hereinafter also referred to as PET, melting point: 255°C) and polybutylene terephthalate (hereinafter also referred to as PBT, melting point: 250°C), with PP and PET being preferred. Nylon (melting point: 225°C) and polyamide resins (melting point: 225°C) can also be used. The melting points of each resin are representative values. In the present invention, it is preferable to use a core-sheath fiber that combines any two of these components. In this case, a fiber with a high melting point is used as the core component, and a fiber with a low melting point is used as the sheath component. In addition, from the viewpoint of easily producing a nonwoven fabric by thermal fusion, the difference in melting point between the core component and the sheath component is preferably 20°C or more, more preferably 25°C or more.

[0020] (Temperature of hot embossing roll) As described above, the temperature of the high-temperature embossing roll 21 is equal to or higher than the melting point of the sheath component of the core-sheath fiber. By using the high-temperature embossing roll 21 whose peripheral surface is heated to a temperature equal to or higher than the melting point of the sheath component, the sheath component can be melted when the fiber web 11 is pressed with the convex portions 22, and the thermocompression bonded portions 12 can be efficiently formed. In addition, the heat of the high-temperature embossing roll 21 can soften the constituent fibers of the fiber web 11. From the viewpoints of efficient formation of the thermocompression bonded parts 12 and softening of the constituent fibers of the fiber web 11, the temperature of the hot embossing roll 21 is preferably 136° C. or higher, more preferably 138° C. or higher, and even more preferably 140° C. or higher. Moreover, from the viewpoints of maintaining the flexibility of the obtained nonwoven fabric 10, the temperature of the hot embossing roll 21 is preferably 145° C. or lower, more preferably 144° C. or lower, and even more preferably 143° C. or lower. From the viewpoints of efficient formation of the thermocompression bonded parts 12 and softening of the constituent fibers of the fiber web 11, the difference between the temperature of the high-temperature embossing roll 21 and the melting point of the sheath component of the core-sheath fiber is preferably 1° C. or more, more preferably 2° C. or more, and even more preferably 5° C. or more. Moreover, from the viewpoint of maintaining the flexibility of the obtained nonwoven fabric 10, the difference is preferably 10° C. or less, more preferably 8° C. or less, and even more preferably 6° C. or less.

[0021] (Low temperature roll) As described above, the temperature of the low-temperature roll 31 is lower than the melting point of the sheath component of the core-sheath fiber. By keeping the temperature of the peripheral surface of the low-temperature roll 31 below a certain level, it is possible to prevent the fiber web 11 from sticking to the low-temperature roll 31 due to melting of the sheath component. As a result, a step of peeling the fiber web 11 from the low-temperature roll 31 after the embossing step is not required, and excessive stretching and width shrinkage of the fiber web 11 can be prevented. Furthermore, the production efficiency of the nonwoven fabric 10 can be improved. From the viewpoint of obtaining a nonwoven fabric 10 having excellent flexibility, the temperature of the low-temperature roll 31 is preferably 112° C. or higher, more preferably 114° C. or higher, and even more preferably 116° C. or higher. Moreover, from the viewpoint of preventing the fiber web 11 from sticking to the low-temperature roll 31, the temperature of the low-temperature roll 31 is preferably 120° C. or lower, more preferably 118° C. or lower, and even more preferably 116° C. or lower. From the viewpoint of preventing the fiber web 11 from sticking to the low-temperature roll 31, the difference between the temperature of the low-temperature roll 31 and the melting point of the sheath component of the core-sheath fiber is preferably 15°C or more, more preferably 18°C ​​or more, and even more preferably 21°C or more.

[0022] (The difference between the temperature of the hot embossing roll and the temperature of the cold roll) From the viewpoint of obtaining a nonwoven fabric 10 having excellent flexibility and suppressing fuzzing on the surface of the nonwoven fabric 10, the difference in temperature between the high-temperature embossing roll 21 and the low-temperature roll 31 is preferably 18° C. or more, more preferably 20° C. or more, and even more preferably 21° C. or more. Moreover, from the viewpoint of preventing the fiber web 11 from sticking to the low-temperature roll 31, the difference is preferably 28° C. or less, more preferably 26° C. or less, and even more preferably 24° C. or less.

[0023] (Proportion of the area of ​​the convex parts) From the viewpoint of appropriately forming the bulky parts 13 in the fiber web 11 to obtain a nonwoven fabric 10 having excellent flexibility, it is preferable that the area occupied by the convex parts 22 on the peripheral surface of the high-temperature embossing roll 21 is equal to or less than a certain amount. Specifically, the ratio of the area of ​​the convex parts 22 on the peripheral surface of the high-temperature embossing roll 21 is preferably 14% or less, more preferably 12% or less, and even more preferably 10% or less. Moreover, from the viewpoint of appropriately forming the thermocompression-bonded parts 12 in the fiber web 11, the ratio is preferably 6% or more, more preferably 7% or more, and even more preferably 8% or more. The ratio of the area of ​​the protrusions 22 on the peripheral surface of the high-temperature embossing roll 21 can be found by dividing the area occupied by the protrusions 22 on the peripheral surface of the high-temperature embossing roll 21 by the sum of the area occupied by the protrusions 22 and the area occupied by the recesses 23. When the protrusions 22 are repeated in a certain pattern, the ratio may be found using the smallest repeating unit.

[0024] (Hot air speed) As described above, the speed of the hot air 42 is 1 m / sec or less. By keeping the speed of the hot air 42 at a certain level or less, the thickness of the fiber web 11 can be maintained in the air-through process, and the nonwoven fabric 10 having an excellent texture and a three-dimensional feel can be produced. Conventionally, in order to sufficiently suppress fuzzing on the surface of the nonwoven fabric produced, the hot air speed in the air-through processing has generally been set to about 1.2 to 2 m / sec. However, in the present invention, as described above, by softening the fiber web 11 in advance with the heat of the high-temperature embossing roll 21 in the embossing step, fuzzing can be sufficiently suppressed even with hot air having a low speed of 1 m / sec or less. From the viewpoint of producing a nonwoven fabric 10 having excellent flexibility, the speed of the hot air 42 is preferably 1.0 m / sec or less, more preferably 0.8 m / sec or less, and even more preferably 0.6 m / sec or less. Moreover, from the viewpoint of suppressing fluffing on the surface of the nonwoven fabric, the speed of the hot air 42 is preferably 0.3 m / sec or more, more preferably 0.35 m / sec or more, and even more preferably 0.4 m / sec or more.

[0025] (Hot air temperature) From the viewpoint of producing a nonwoven fabric 10 having excellent flexibility, the temperature of the hot air 42 is preferably 140° C. or less, more preferably 138° C. or less, and even more preferably 136° C. or less. Moreover, from the viewpoint of sufficiently fusing the constituent fibers of the fiber web 11, the temperature of the hot air 42 is preferably 132° C. or more, more preferably 133° C. or more, and even more preferably 134° C. or more.

[0026] (Applications of nonwoven fabric) The nonwoven fabric 10 produced by the present invention can be used in a variety of articles, including, preferably, absorbent articles, such as diapers for adults and children, sanitary napkins, incontinence pads, panty liners, and absorbent pads. Absorbent articles generally have a top sheet on the skin contact side, a back sheet on the non-skin contact side, and an absorbent disposed between the top sheet and the back sheet. The top sheet has the function of allowing excreted liquid to pass from the skin contact side to the non-skin contact side (liquid permeability). The back sheet has the function of preventing excreted liquid from passing from the skin contact side to the non-skin contact side (liquid impermeability). The absorbent has the function of absorbing and retaining excreted liquid. Of these components, the nonwoven fabric 10 produced by the present invention can be suitably used as a topsheet. This allows the user to feel the softness and good texture of the nonwoven fabric 10. In particular, it is preferable to incorporate the nonwoven fabric 10 into an absorbent article so that the surface to which hot air 42 has been blown to suppress fuzzing becomes the surface to be used. EXAMPLES

[0027] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0028] Example 1 A fiber web consisting of core-sheath fibers with a core component of PET resin (melting point: 256°C) and a sheath component of HDPE resin (melting point: 135°C) was embossed using a pair of rolls to form thermocompression bonded parts. The pair of rolls used consisted of a high-temperature embossing roll with a temperature of 137°C and a convex area ratio of 9.6%, and a low-temperature roll with a flat peripheral surface and a temperature of 116°C. The embossed fiber web was transported to the inside of the air-through machine by a transport net, and the air-through processing was performed by blowing hot air against the surface pressed by the convex part of the high-temperature embossing roll to fuse the constituent fibers of the fiber web together. The hot air speed was 0.5 m / s and the hot air temperature was 136°C. In this manner, a nonwoven fabric sample S1 of Example 1 was obtained.

[0029] (Examples 2 to 8) Nonwoven fabric samples S2 to S8 of Examples 2 to 8 were obtained in the same manner as in Example 1, except that the temperatures of the hot embossing roll and the cold roll were as shown in Table 1.

[0030] (Comparative Examples 1 to 4) Nonwoven fabric samples C1 to C4 of Comparative Examples 1 to 4 were obtained in the same manner as in Example 1, except that the temperatures of the hot embossing roll and the cold roll were as shown in Table 2.

[0031] Comparative Example 5 A nonwoven fabric sample C5 of Comparative Example 5 was obtained in the same manner as in Example 2, except that the temperature of the high-temperature embossing roll and the wind speed of the hot air were as shown in Table 2. Comparative Example 6 A nonwoven fabric sample C6 of Comparative Example 6 was obtained in the same manner as in Example 3, except that the temperature of the low-temperature roll was set as shown in Table 2.

[0032] (Fuzziness evaluation) Nonwoven fabric samples S1 to S8 of Examples 1 to 8 and nonwoven fabric samples C1 to C6 of Comparative Examples 1 to 6 were folded in half with the surface facing the high-temperature embossing roll facing outward, and the folded portion was photographed from the thickness direction using a digital camera against a black background. The number of fluffs rising more than 1 mm above the nonwoven fabric surface (a reference line connecting the portions of the bulky portion that were most recessed toward the low-temperature roll) and the maximum fluff height were measured for two random 10 cm sections. The length of the section to be measured and the fluff height were measured based on the graduations on a scale photographed together with the nonwoven fabric sample. Based on the measurement results, the fuzzing of each nonwoven fabric sample was quantified on the following five-point scale and evaluated as the average value of the two points. The higher the value, the more fuzzing is suppressed. 5: No fuzz is observed on the nonwoven surface. 4: The number of fluffs is 2 or less, and the maximum fluff height is less than 5 mm. 3: The number of fibers is 3 and the maximum fiber height is less than 5 mm. 2: The number of fibers is 4 and the maximum fiber height is less than 5 mm. 1: The number of fibers is 5 or more, or the maximum fiber height is 5 mm or more. FIG. 3 shows images taken of the surface of nonwoven fabric sample S5 of Example 5 and the surface of nonwoven fabric sample C2 of Comparative Example 2.

[0033] (Flexibility assessment) The softness of each of the nonwoven fabric samples S1 to S8 of Examples 1 to 8 and the nonwoven fabric samples C1 to C6 of Comparative Examples 1 to 6 was evaluated as follows. Specifically, a 10 cm x 10 cm evaluation sample was cut out from the nonwoven fabric sample, and the surface of the evaluation sample facing the high-temperature embossing roll was used as the evaluation target surface. The evaluation sample was placed on a table with the evaluation target surface facing up, and the evaluation sample was evaluated for flexibility by touching the evaluation sample from the front. The evaluation of flexibility was performed by four adult males who are skilled in flexibility evaluation. Specifically, the flexibility was evaluated in three stages as follows, with the nonwoven fabric sample S1 of Example 1, which has excellent flexibility, as the standard (2 points). The average of the scores of the four people was rounded off to the nearest integer digit to obtain the flexibility score. 3: Better than nonwoven fabric sample S1 of Example 1. 2: Equivalent to nonwoven fabric sample S1 of Example 1. 1: Inferior to nonwoven fabric sample S1 of Example 1.

[0034] (Evaluation of detachability of fiber web) For each of Examples 1 to 8 and Comparative Examples 1 to 6, the degree of adhesion of the fiber web to the low-temperature roll immediately after embossing was visually observed, and the releasability was evaluated according to the following three-level scale. A higher value indicates higher releasability. 3: Almost no sticking to the outer circumference of the low-temperature roll. 2: Although there is some sticking around the outer circumference of the low-temperature roll, no tension adjustment is required. 1: There is sticking on the outer circumference of the low-temperature roll, and tension adjustment is required. The results are shown in Tables 1 and 2.

[0035] [Table 1]

[0036] [Table 2]

[0037] As shown in Tables 1 and 2, nonwoven fabric samples S1 to S8 of Examples 1 to 8, which were produced by setting the temperature of the high-temperature embossing roll to the melting point of the sheath component or higher, the temperature of the low-temperature roll to less than the melting point of the sheath component, and the hot air speed to 1 m / sec or less, had less fuzz on the surface than nonwoven fabric samples C1 to C5 of Comparative Examples 1 to 5, which were produced by setting the temperature of the high-temperature embossing roll to less than the melting point of the sheath component. Furthermore, nonwoven fabric samples S1 to S8 of Examples 1 to 8 were superior in softness to nonwoven fabric sample C5 of Comparative Example 5, which was produced by setting the hot air speed to more than 1 m / sec, and nonwoven fabric sample C6 of Comparative Example 6, which was produced by setting the temperature of the low-temperature roll to the same temperature as the melting point of the sheath component. In addition, among the nonwoven fabric samples S1 to S8 of Examples 1 to 8, nonwoven fabric samples S1 to S6 of Examples 1 to 6, in which the temperature of the low-temperature roll was 120°C or lower (the difference between the temperature of the low-temperature roll and the melting point of the sheath component was 15°C or more), showed good peelability of the fiber web immediately after the embossing process and had excellent manufacturing efficiency of the nonwoven fabric. [Explanation of symbols]

[0038] 10. Nonwoven Fabrics 11 Fiber web 11A One side of the fiber web 11B Reverse surface of fiber web 12 Thermocompression section 13 Bulky part 21 High temperature embossing roll 22 Convex 23 Recess 31 Low temperature roll 41 Air-through machine 42 Hot air

Claims

1. an embossing step of sandwiching a fiber web containing core-sheath fibers between a pair of rolls consisting of a high-temperature embossing roll and a low-temperature roll to form a thermocompression bonded portion and a bulky portion in the fiber web; and an air-through process in which hot air having a wind speed of 1 m / sec or less is blown onto the fiber web after the embossing process to perform an air-through process, thereby bonding the core-sheath fibers together by heat fusion while maintaining the bulky portion. The core component of the sheath-core fiber is polypropylene, polyethylene terephthalate or nylon, and the sheath component of the sheath-core fiber is high-density polyethylene, and the core-sheath fiber does not contain a thermally extensible fiber, the temperature of the high-temperature embossing roll is equal to or higher than the melting point of the sheath component of the core-sheath fiber, and the difference between the temperature of the high-temperature embossing roll and the melting point of the sheath component of the core-sheath fiber is 1° C. or more and 8° C. or less; the temperature of the low-temperature roll is lower than the melting point of the sheath component of the core-sheath fiber, and the difference between the temperature of the low-temperature roll and the melting point of the sheath component of the core-sheath fiber is 15° C. or more; A method for producing a nonwoven fabric, wherein the difference in temperature between the high-temperature embossing roll and the low-temperature roll is 18°C ​​or more and 28°C or less.

2. The method for producing a nonwoven fabric according to claim 1 , wherein the area ratio of the protrusions to the peripheral surface of the high-temperature embossing roll is 14% or less.

3. The method for producing a nonwoven fabric according to claim 1 or 2, wherein the temperature of the hot air is 140° C. or less.

4. The method for producing a nonwoven fabric according to any one of claims 1 to 3, wherein the low-temperature roll is a flat roll.

5. The method for producing a nonwoven fabric according to any one of claims 1 to 4, wherein the surface of the fiber web that is contacted with the high-temperature embossing roll becomes a surface to be used in the nonwoven fabric.

6. The method for producing a nonwoven fabric according to any one of claims 1 to 5, wherein in the air-through step, the hot air is blown onto a surface of the fiber web against which the high-temperature embossing roll is brought into contact.

Citation Information

Patent Citations

  • Three-dimensionally shaped nonwoven fabric

    JP2005350836A

  • Nonwoven fabric

    JP2011102456A

  • Nonwoven fabric

    JP2012001866A

  • Thermally extensible fiber and nonwoven fabric using the same

    JP2013122104A

  • Shaped nonwoven fabric

    JP2018090932A