Antistatic agent, antistatic agent composition, antistatic resin composition and molded article thereof
The antistatic agent with a polyester-polyether block structure addresses durability and handling issues of conventional agents, ensuring effective antistatic performance and mechanical integrity in thermoplastic resins.
Patent Information
- Application Number
- JP2020150216
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-09-08
AI Technical Summary
Conventional antistatic agents for thermoplastic resins have issues with durability, handling properties, and impair the mechanical properties of the resin, failing to provide sufficient antistatic performance with a small amount of addition, and can lead to surface contamination and electrical issues in precision instruments.
An antistatic agent comprising an aliphatic diol, a dicarboxylic acid derivative, a compound with ethyleneoxy groups and hydroxyl groups, and a polyhydric alcohol, forming a polymer compound with a polyester and polyether block structure, optionally with aromatic sulfonic acid salts, to achieve excellent antistatic performance without compromising mechanical properties.
The antistatic agent provides long-lasting antistatic effects with excellent handling properties and maintains the mechanical properties of the resin, reducing surface contamination and electrical issues in molded products.
Smart Images

Figure 0007575224000001 
Figure 0007575224000002 
Figure 0007575224000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an antistatic agent, an antistatic agent composition, an antistatic resin composition (hereinafter, also simply referred to as a "resin composition"), and a molded article thereof. More specifically, the present invention provides an antistatic agent, an antistatic agent composition, an antistatic resin composition, and a molded article thereof, which can impart an excellent antistatic effect with a small addition amount, have sufficient durability, are excellent in handleability, and do not impair the inherent physical properties of the resin, such as the mechanical properties. [Background technology]
[0002] Synthetic resins such as thermoplastic resins are important materials that are indispensable in modern times because they have excellent properties such as being lightweight and easy to process, as well as being able to design the substrate according to the application. Thermoplastic resins also have excellent electrical insulation properties, so they are frequently used in components of electrical products. However, because thermoplastic resins have such high insulation properties, they have the problem of being easily charged by friction, etc.
[0003] Since electrostatically charged thermoplastic resin attracts surrounding dust and dirt, the appearance of the resin molded product is marred. In addition, among electronic products, for example, precision equipment such as computers may not be able to operate normally due to electrostatic charge. Furthermore, there is also the problem of electric shock. If an electric shock occurs to the human body from the resin, not only will it cause discomfort to the person, but in places where flammable gas or dust is present, it may also induce an explosion.
[0004] In order to solve such problems, synthetic resins have been conventionally treated to prevent static electricity. The most common antistatic treatment method is to add an antistatic agent to synthetic resins. Such antistatic agents include coating-type agents that are applied to the surface of resin molded bodies, and kneading-type agents that are added when the resin is processed and molded. However, coating-type agents have a problem in that they are poorly durable, and that objects that come into contact with the surface are contaminated because a large amount of organic matter is coated on the surface.
[0005] From this viewpoint, kneading-in type antistatic agents have been mainly studied, and for example, polyetheresteramide has been proposed to impart antistatic properties to styrene-based resins (Patent Documents 1 and 2). Also, a block polymer having a structure in which polyester blocks and hydrophilic polymer blocks are repeatedly and alternately bonded has been proposed (Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 11-148072 [Patent Document 2] Japanese Patent Application Publication No. 2004-217929 [Patent Document 3] International Publication No. 2016 / 042936 Summary of the Invention [Problem to be solved by the invention]
[0007] However, in recent years, with the improvement in the performance of precision instruments, etc., the antistatic performance required is higher than ever before. Therefore, there is a demand for the development of an antistatic agent that has higher performance than these conventional antistatic agents, specifically, can impart an excellent antistatic effect with a smaller amount of addition, and further does not impair the inherent physical properties of the resin, such as the mechanical properties.
[0008] Furthermore, some antistatic agents require a long reaction time or a high temperature during production, which can result in problems such as poor economic efficiency and coloration.
[0009] Furthermore, some antistatic agents have poor handling properties, and may cause stickiness or blocking during use.
[0010] Therefore, an object of the present invention is to provide an antistatic agent which can impart an excellent antistatic effect with a small amount of addition, has sufficient durability, is easy to handle, and does not impair the inherent physical properties of the resin, such as mechanical properties, etc. Another object of the present invention is to provide a molded article made of a synthetic resin which is less susceptible to surface contamination due to static electricity or to dust adhesion, and which has the inherent physical properties, such as mechanical properties, of the resin. [Means for solving the problem]
[0011] As a result of intensive research aimed at solving the above problems, the present inventors have found that an antistatic agent having the following structure can impart an excellent antistatic effect with a small amount added, has sufficient durability, is excellent in handleability, and can maintain the inherent physical properties of the resin, such as the mechanical properties, and have completed the present invention.
[0012] That is, the antistatic agent of the present invention is an antistatic agent containing one or more of a polymer compound (E) obtained by a condensation reaction of an aliphatic diol (a1) having 2 to 12 carbon atoms, a dicarboxylic acid derivative (a2), a compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends, and a polyhydric alcohol compound (D) having three or more hydroxyl groups, The dicarboxylic acid derivative (a2) is a mixture of a 1,4-benzenedicarboxylic acid derivative and a 1,3-benzenedicarboxylic acid derivative, and the mixing ratio, by mass, of the 1,4-benzenedicarboxylic acid derivative:1,3-benzenedicarboxylic acid derivative is within the range of 50:50 to 95:5.
[0013] In the antistatic agent of the present invention, it is preferable that the polymer compound (E) is a polymer compound obtained by a condensation reaction of a polyester (a) obtained by reacting an aliphatic diol (a1) having 2 to 12 carbon atoms with a dicarboxylic acid derivative (a2), a compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends, and a polyhydric alcohol compound (D), and the polymer compound (E) has a polyester block (A) constituted by the polyester (a) and a polyether block (B) constituted by the compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends, It is more preferable that the polymer compound (E) has a structure in which a hydroxyl group or an alkyl ester group at an end of the polyester (a), a hydroxyl group at an end of a compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends, and a hydroxyl group of the polyhydric alcohol compound (D) are bonded via an ester bond, the structure being formed by a condensation reaction between the hydroxyl group or the alkyl ester group at an end of the polyester (a), the hydroxyl group at an end of the compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends, and the hydroxyl group of the polyhydric alcohol compound (D). It is even more preferable that the polymer compound (E) has a structure in which a block polymer (C) having hydroxyl groups or alkyl ester groups at both ends, which is formed by repeatedly and alternately bonding the polyester block (A) and the polyether block (B) via ester bonds, and the polyhydric alcohol compound (D) are bonded via an ester bond.
[0014] In the antistatic agent of the present invention, the dicarboxylic acid derivative (a2) of the polymer compound (E) is preferably a mixture of 1,4-benzenedicarboxylic acid dialkyl ester and 1,3-benzenedicarboxylic acid dialkyl ester, and it is more preferable that the dicarboxylic acid derivative (a2) of the polymer compound (E) is a mixture of 1,4-benzenedicarboxylic acid dimethyl ester and 1,3-benzenedicarboxylic acid dimethyl ester.
[0015] In the antistatic agent of the present invention, the aliphatic diol (a1) having 2 to 12 carbon atoms in the polymer compound (E) is preferably at least one of 1,2-ethanediol and 1,4-butanediol. In the antistatic agent of the present invention, the compound (b) having one or more ethyleneoxy groups and hydroxyl groups at both ends in the polymer compound (E) is preferably polyethylene glycol. In the antistatic agent of the present invention, the number average molecular weight of the polyester (a) is preferably 1,000 to 8,000 in terms of polystyrene, the number average molecular weight of the compound (b) having one or more ethyleneoxy groups and hydroxyl groups at both ends is preferably 1,000 to 6,000 in terms of polystyrene, and the number average molecular weight of the block polymer (C) is preferably 5,000 to 30,000 in terms of polystyrene.
[0016] The antistatic agent composition of the present invention is characterized in that it further contains one or more salts of aromatic sulfonic acid in addition to the antistatic agent of the present invention.
[0017] The antistatic resin composition of the present invention is characterized in that it comprises a synthetic resin and the antistatic agent of the present invention blended therein.
[0018] In the antistatic resin composition of the present invention, the synthetic resin is preferably one or more selected from the group consisting of polystyrene resins and copolymers thereof. In addition, in the antistatic resin composition of the present invention, the mass ratio of the synthetic resin to the antistatic agent is preferably in the range of 99 / 1 to 40 / 60.
[0019] Another antistatic resin composition of the present invention is characterized in that it comprises a synthetic resin and the antistatic agent composition of the present invention blended therein.
[0020] In another antistatic resin composition of the present invention, the synthetic resin is preferably one or more selected from the group consisting of polystyrene resins and copolymers thereof. Also, in another antistatic resin composition of the present invention, the mass ratio of the synthetic resin to the antistatic agent composition is preferably in the range of 99 / 1 to 40 / 60.
[0021] The molded article of the present invention is characterized by being made of the antistatic resin composition of the present invention. Effect of the Invention
[0022] According to the present invention, it is possible to provide an antistatic agent that can impart an excellent antistatic effect with a small amount of addition, has sufficient durability, is easy to handle, and does not impair the inherent physical properties of the resin, such as the mechanical properties. Also, according to the present invention, it is possible to provide a synthetic resin composition that has excellent antistatic properties and the inherent physical properties of the resin, such as the mechanical properties. Furthermore, according to the present invention, it is possible to provide a molded product that is less susceptible to surface contamination due to static electricity or dust adhesion, and has the inherent physical properties of the resin, such as the mechanical properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present invention will be described in detail. The antistatic agent of the present invention contains at least one of the following polymer compounds (E) obtained by condensation reaction of an aliphatic diol (a1) having 2 to 12 carbon atoms, a dicarboxylic acid derivative (a2), a compound (b) having one or more ethyleneoxy groups and hydroxyl groups at both ends, and a polyhydric alcohol compound (D) having three or more hydroxyl groups. In the antistatic agent of the present invention, the dicarboxylic acid derivative (a2) is a mixture of a 1,4-benzenedicarboxylic acid derivative and a 1,3-benzenedicarboxylic acid derivative, and the mixing ratio of the 1,4-benzenedicarboxylic acid derivative:1,3-benzenedicarboxylic acid derivative is within the range of 50:50 to 95:5 by mass ratio. The ethyleneoxy group is a group represented by the following general formula (1).
[0024] TIFF0007575224000001.tif9158
[0025] First, the aliphatic diol (a1) having 2 to 12 carbon atoms used in the antistatic agent of the present invention will be described. Examples of the aliphatic diol (a1) having 2 to 12 carbon atoms used in the antistatic agent of the present invention include linear aliphatic diols, branched aliphatic diols, and aliphatic diols containing a cyclic structure having 2 to 12 carbon atoms. In the antistatic agent of the present invention, the aliphatic diol having 2 to 12 carbon atoms may be a mixture of two or more kinds.
[0026] Examples of the aliphatic diol having 2 to 12 carbon atoms include 1,2-ethanediol (ethylene glycol), 1,2-propanediol (propylene glycol), 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 2,2-dimethyl-1,3-propanediol (neopentyl glycol), 2,2-diethyl-1,3-propanediol (3,3-dimethylolpentane), 2-n-butyl-2-ethyl-1,3propanediol (3,3-dimethylolheptane), 3-methyl- Examples of the diol include 1,5-pentanediol, 1,6-hexanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-octadecanediol, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, 1,2-, 1,3- or 1,4-cyclohexanediol, cyclododecanediol, dimer diol, hydrogenated dimer diol, diethylene glycol, dipropylene glycol, triethylene glycol, and polyethylene glycol. Among these aliphatic diols, 1,2-ethanediol (ethylene glycol), 1,4-butanediol, and 1,4-cyclohexanedimethanol are preferred in terms of ease of reaction during production, coloring inhibition, antistatic properties, handling properties, and mechanical properties of molded bodies, and 1,2-ethanediol (ethylene glycol) and 1,4-butanediol are more preferred. In addition, since it is preferable that the aliphatic diol having 2 to 12 carbon atoms has hydrophobic properties, polyethylene glycol, which has hydrophilic properties, is not preferred among the aliphatic diols. However, this does not apply when the diol is used together with other diols. The aliphatic diol (a1) having 2 to 12 carbon atoms used in the antistatic agent of the present invention may be one type or two or more types.
[0027] Next, the dicarboxylic acid derivative (a2) used in the antistatic agent of the present invention will be described. In the antistatic agent of the present invention, the dicarboxylic acid derivative (a2) is a mixture of a 1,4-benzenedicarboxylic acid derivative and a 1,3-benzenedicarboxylic acid derivative, and the mixture ratio of the 1,4-benzenedicarboxylic acid derivative:1,3-benzenedicarboxylic acid derivative is within the range of 50:50 to 95:5 by mass ratio. In the antistatic agent of the present invention, the dicarboxylic acid derivative (a2) is a mixture of a 1,4-benzenedicarboxylic acid derivative and a 1,3-benzenedicarboxylic acid derivative, but may contain other dicarboxylic acid derivatives within a range that does not impair the intended effect of the present invention.
[0028] Examples of the dicarboxylic acid derivative (a2) include dicarboxylic acids themselves, acid anhydrides, esters, alkali metal salts, and acid halides. From the viewpoints of ease of reaction during production and inhibition of coloration, dicarboxylic acid dialkyl esters, i.e., 1,4-benzenedicarboxylic acid dialkyl esters and 1,3-benzenedicarboxylic acid dialkyl esters, are preferred.
[0029] From the viewpoints of ease of reaction during production and inhibition of coloration, the alkyl group constituting the dialkyl ester of 1,4-benzenedicarboxylic acid dialkyl ester and 1,3-benzenedicarboxylic acid dialkyl ester is preferably a methyl group, an ethyl group, a normal propyl group, an isopropyl group, or a normal butyl group, and more preferably a methyl group. That is, 1,4-benzenedicarboxylic acid dimethyl ester and 1,3-benzenedicarboxylic acid dimethyl ester are preferred.
[0030] The mixing ratio of 1,4-benzenedicarboxylic acid dimethyl ester and 1,3-benzenedicarboxylic acid dimethyl ester is within the range of 50:50 to 95:5 by mass, but from the viewpoints of antistatic properties, handling properties, and mechanical properties of the molded body, it is preferably 55:45 to 85:15.
[0031] Next, the compound (b) having one or more ethyleneoxy groups and hydroxyl groups at both ends (hereinafter also referred to as compound (b)) used in the antistatic agent of the present invention will be described. As compound (b), a hydrophilic compound is preferable, a polyether having a group represented by general formula (1) is more preferable, and a polyethylene glycol represented by the following general formula (2) is particularly preferable.
[0032] TIFF0007575224000002.tif11158
[0033] In the general formula (2), m represents a number of 5 to 250. m is preferably a number of 20 to 150 from the viewpoints of ease of reaction during production, inhibition of coloring, antistatic properties, and mechanical properties of molded products.
[0034] Examples of the compound (b) include polyethylene glycol obtained by addition reaction of ethylene oxide, as well as polyethers obtained by addition reaction of ethylene oxide with one or more other alkylene oxides (e.g., propylene oxide, 1,2-, 1,4-, 2,3- or 1,3-butylene oxide, etc.), and these polyethers may be either random or block.
[0035] Further examples of compound (b) include compounds having a structure in which ethylene oxide is added to an active hydrogen atom-containing compound, and compounds having a structure in which ethylene oxide and one or more other alkylene oxides (e.g., propylene oxide, 1,2-, 1,4-, 2,3- or 1,3-butylene oxide, etc.) are added. These may be either randomly or block-added.
[0036] Examples of the active hydrogen atom-containing compound include glycols, dihydric phenols, primary monoamines, secondary diamines, and dicarboxylic acids.
[0037] As the glycol, aliphatic glycols having 2 to 20 carbon atoms, alicyclic glycols having 5 to 12 carbon atoms, aromatic glycols having 8 to 26 carbon atoms, and the like can be used.
[0038] Examples of aliphatic glycols include ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,3-hexanediol, 1,4-hexanediol, 1,6-hexanediol, 2,5-hexanediol, 1,2-octanediol, 1,8-octanediol, 1,10-decanediol, 1,18-octadecanediol, 1,20-eicosanediol, diethylene glycol, triethylene glycol, and thiodiethylene glycol.
[0039] Examples of alicyclic glycols include 1-hydroxymethyl-1-cyclobutanol, 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1-methyl-3,4-cyclohexanediol, 2-hydroxymethylcyclohexanol, 4-hydroxymethylcyclohexanol, 1,4-cyclohexanedimethanol, and 1,1'-dihydroxy-1,1'-dicyclohexyl.
[0040] Examples of aromatic glycols include dihydroxymethylbenzene, 1,4-bis(β-hydroxyethoxy)benzene, 2-phenyl-1,3-propanediol, 2-phenyl-1,4-butanediol, 2-benzyl-1,3-propanediol, triphenylethylene glycol, tetraphenylethylene glycol, and benzopinacol.
[0041] As the dihydric phenol, a phenol having 6 to 30 carbon atoms can be used, and examples thereof include catechol, resorcinol, 1,4-dihydroxybenzene, hydroquinone, bisphenol A, bisphenol F, bisphenol S, dihydroxydiphenyl ether, dihydroxydiphenyl thioether, binaphthol, and alkyl (having 1 to 10 carbon atoms) or halogen-substituted derivatives thereof.
[0042] Examples of the primary monoamine include aliphatic primary monoamines having 1 to 20 carbon atoms, such as methylamine, ethylamine, n-propylamine, isopropylamine, n-butylamine, s-butylamine, isobutylamine, n-amylamine, isoamylamine, n-hexylamine, n-heptylamine, n-octylamine, n-decylamine, n-octadecylamine, and n-icosylamine.
[0043] Examples of the secondary diamine that can be used include aliphatic secondary diamines having 4 to 18 carbon atoms, heterocyclic secondary diamines having 4 to 13 carbon atoms, alicyclic secondary diamines having 6 to 14 carbon atoms, aromatic secondary diamines having 8 to 14 carbon atoms, and secondary alkanol diamines having 3 to 22 carbon atoms.
[0044] Examples of the aliphatic secondary diamine include N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N'-dibutylethylenediamine, N,N'-dimethylpropylenediamine, N,N'-diethylpropylenediamine, N,N'-dibutylpropylenediamine, N,N'-dimethyltetramethylenediamine, N,N'-diethyltetramethylenediamine, N,N'-dibutyltetramethylenediamine, N,N'-dimethylhexamethylenediamine, N,N'-diethylhexamethylenediamine, N,N'-dibutylhexamethylenediamine, N,N'-dimethyldecamethylenediamine, N,N'-diethyldecamethylenediamine, and N,N'-dibutyldecamethylenediamine.
[0045] Examples of the heterocyclic secondary diamine include piperazine and 1-aminopiperidine.
[0046] Examples of alicyclic secondary diamines include N,N'-dimethyl-1,2-cyclobutanediamine, N,N'-diethyl-1,2-cyclobutanediamine, N,N'-dibutyl-1,2-cyclobutanediamine, N,N'-dimethyl-1,4-cyclohexanediamine, N,N'-diethyl-1,4-cyclohexanediamine, N,N'-dibutyl-1,4-cyclohexanediamine, N,N'-dimethyl-1,3-cyclohexanediamine, N,N'-diethyl-1,3-cyclohexanediamine, and N,N'-dibutyl-1,3-cyclohexanediamine.
[0047] Examples of aromatic secondary diamines include N,N'-dimethyl-phenylenediamine, N,N'-dimethyl-xylylenediamine, N,N'-dimethyl-diphenylmethanediamine, N,N'-dimethyl-diphenyletherdiamine, N,N'-dimethyl-benzidine, and N,N'-dimethyl-1,4-naphthalenediamine.
[0048] Examples of secondary alkanol diamines include N-methyldiethanolamine, N-octyldiethanolamine, N-stearyldiethanolamine, and N-methyldipropanolamine.
[0049] As the dicarboxylic acid, a dicarboxylic acid having 2 to 20 carbon atoms can be used, such as an aliphatic dicarboxylic acid, an aromatic dicarboxylic acid, or an alicyclic dicarboxylic acid.
[0050] Examples of aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, methylsuccinic acid, dimethylmalonic acid, β-methylglutaric acid, ethylsuccinic acid, isopropylmalonic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanediacid, dodecanediacid, tridecanediacid, tetradecanediacid, hexadecanedioic acid, octadecanedioic acid, and icosanediacid.
[0051] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, phenylmalonic acid, homophthalic acid, phenylsuccinic acid, β-phenylglutaric acid, α-phenyladipic acid, β-phenyladipic acid, biphenyl-2,2'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, naphthalenedicarboxylic acid, sodium 3-sulfoisophthalate, and potassium 3-sulfoisophthalate.
[0052] Examples of alicyclic dicarboxylic acids include 1,3-cyclopentanedicarboxylic acid, 1,2-cyclopentanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanediacetic acid, 1,3-cyclohexanediacetic acid, 1,2-cyclohexanediacetic acid, and dicyclohexyl-4,4'-dicarboxylic acid.
[0053] These active hydrogen atom-containing compounds can be used either individually or in combination of two or more.
[0054] In the antistatic agent of the present invention, the compound (b) may be used alone or in combination of two or more kinds.
[0055] Next, the polyhydric alcohol compound (D) having 3 or more hydroxyl groups used in the antistatic agent of the present invention will be described. The polyhydric alcohol compound (D) used in the antistatic agent of the present invention is not particularly limited as long as it has 3 or more hydroxyl groups.
[0056] For example, trihydric alcohols such as glycerin, 1,2,3-butanetriol, 1,2,4-butanetriol, 2-methyl-1,2,3-propanetriol, 1,2,3-pentanetriol, 1,2,4-pentanetriol, 1,3,5-pentanetriol, 2,3,4-pentanetriol, 2-methyl-2,3,4-butanetriol, trimethylolethane, 2,3,4-hexanetriol, 2-ethyl-1,2,3-butanetriol, trimethylolpropane, 4-propyl-3,4,5-heptanetriol, 2,4-dimethyl-2,3,4-pentanetriol, triethanolamine, triisopropanolamine, and 1,3,5-tris(2-hydroxyethyl)isocyanurate. tetrahydric alcohols such as pentaerythritol, 1,2,3,4-pentane tetrol, 2,3,4,5-hexane tetrol, 1,2,4,5-pentane tetrol, 1,3,4,5-hexane tetrol, diglycerin, ditrimethylolpropane, sorbitan, N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine, and N,N,N',N'-tetrakis(2-hydroxyethyl)ethylenediamine; pentahydric alcohols such as adonitol, arabitol, xylitol, and triglycerin; hexahydric alcohols such as dipentaerythritol, sorbitol, mannitol, iditol, inositol, dulcitol, talose, and allose; and tripentaerythritol. There is no particular restriction on the molecular weight of the polyhydric alcohol compound, and high molecular weight polyhydric alcohols such as polypentaerythritol and polyvinyl alcohol can be used, as well as synthetic polyhydric alcohols such as polyester polyols. In the present invention, the polyhydric alcohol compound (D) having three or more hydroxyl groups may be used alone or in combination of two or more kinds.
[0057] In the antistatic agent of the present invention, the polyhydric alcohol compound (D) having three or more hydroxyl groups is preferably pentaerythritol, dipentaerythritol, glycerin, diglycerin, trimethylolpropane, or ditrimethylolpropane, from the viewpoints of ease of reaction and suppression of coloration during production, antistatic properties and handleability, and mechanical properties of a molded body, and is more preferably glycerin or diglycerin.
[0058] In addition, from the viewpoints of ease of reaction and suppression of coloration during production, antistatic properties and handleability, and mechanical properties of molded bodies, the polymer compound (E) in the antistatic agent of the present invention is preferably a polymer compound obtained by a condensation reaction of polyester (a) obtained by reacting an aliphatic diol (a1) having 2 to 12 carbon atoms with a dicarboxylic acid derivative (a2), a compound (b), and a polyhydric alcohol compound (D) having 3 or more hydroxyl groups.
[0059] From the viewpoints of ease of reaction during production, suppression of coloration, antistatic properties and handleability, and mechanical properties of molded products, it is preferable that the polymer compound (E) in the antistatic agent of the present invention has a polyester block (A) composed of a polyester (a) obtained by reacting an aliphatic diol (a1) having 2 to 12 carbon atoms with a dicarboxylic acid derivative (a2), and a polyether block (B) composed of a compound (b), and has a structure formed by bonding via an ester bond formed by a condensation reaction of a hydroxyl group or alkyl ester group at the end of the polyester (a), a hydroxyl group at the end of the compound (b), and a hydroxyl group of a polyhydric alcohol compound (D) having 3 or more hydroxyl groups.
[0060] From the viewpoints of ease of reaction and suppression of coloration during production, antistatic properties and handleability, and mechanical properties of molded bodies, it is preferable that the polymer compound (E) in the antistatic agent of the present invention has a structure in which a block polymer (C) having hydroxyl groups or alkyl ester groups at both ends, which is formed by repeatedly and alternately bonding a polyester block (A) and a polyether block (B) via ester bonds, and a polyhydric alcohol compound (D) having three or more hydroxyl groups are bonded via ester bonds.
[0061] The polyester (a) in the antistatic agent of the present invention preferably comprises an aliphatic diol (a1) having 2 to 12 carbon atoms and a dialkyl dicarboxylate (a2), and more preferably has a structure in which a residue obtained by removing a hydroxyl group from an aliphatic diol having 2 to 12 carbon atoms and a residue obtained by removing an alkyl group from a dialkyl dicarboxylate are bonded via an ester bond. The terminals of the polyester (a) are either hydroxyl groups or alkyl ester groups, and in the antistatic agent of the present invention, both terminals may be hydroxyl groups, both terminals may be alkyl ester groups, or one terminal may be a hydroxyl group and the remaining terminal may be an alkyl ester group, but from the viewpoints of ease of reaction during production and suppression of coloration, it is preferable that both terminals are hydroxyl groups.
[0062] The degree of polymerization of the polyester (a) is preferably from 2 to 50 from the viewpoints of ease of reaction during production, inhibition of coloration, antistatic properties, handling properties, and mechanical properties of molded articles.
[0063] The polyester (a) in the antistatic agent of the present invention is preferably obtained by a condensation reaction between an aliphatic diol (a1) having 2 to 12 carbon atoms and a dialkyl dicarboxylate (a2). In the antistatic agent of the present invention, the condensation reaction includes a polycondensation reaction. In addition, in the antistatic agent of the present invention, the condensation reaction includes an esterification reaction and an ester exchange reaction.
[0064] In the condensation reaction, a catalyst for promoting the esterification reaction (including the transesterification reaction) may be used, and as the catalyst, a conventionally known catalyst such as dibutyltin oxide, tetraalkyl titanate, zirconium acetate, zinc acetate, etc. In order to suppress oxidation of the product during the reaction, an antioxidant such as a phenol-based antioxidant may be added to the reaction system.
[0065] A preferred polyester (a), which has hydroxyl groups at both ends, can be obtained by condensation reaction of (a1) and (a2). In this case, the reaction ratio of (a1) to (a2) is preferably such that (a1) is used in excess so that both ends have hydroxyl groups, and it is preferably used in a molar excess of 1 molar to (a2).
[0066] The polyester (a) having alkyl ester groups at both ends can be obtained by a condensation reaction of (a1) and (a2). In this case, the reaction ratio of (a1) to (a2) is preferably such that (a2) is used in excess, preferably 1 molar excess over (a1), so that both ends have alkyl ester groups.
[0067] The dicarboxylic acid dialkyl ester (a2) constituting the polyester (a) may be a derivative thereof (e.g., dicarboxylic acid itself, acid anhydride, ester other than alkyl ester, alkali metal salt, acid halide, etc.) so long as it finally becomes the polyester (a), and when the polyester (a) is obtained using a derivative, both ends are finally treated to give hydroxyl groups or alkyl ester groups, and the reaction for obtaining the block polymer (C) having a structure having carboxyl groups at both ends may proceed as is. However, from the viewpoint of reactivity, it is preferable to use a dicarboxylic acid dialkyl ester.
[0068] In the antistatic agent of the present invention, the compound (b) preferably undergoes a condensation reaction with the polyester (a) to form an ester bond and form a block polymer (C) structure, and the hydroxyl groups at both ends of the compound (b) may be protected or modified, or may be in the form of a precursor.
[0069] The block polymer (C) having hydroxyl groups or alkyl ester groups at both ends in the antistatic agent of the present invention has a structure in which a polyester block (A) composed of the above polyester (a) and a polyether block (B) composed of the compound (b) are repeatedly and alternately bonded via ester bonds. An example of such a block polymer (C) is a structure represented by the following general formula (3) or (4).
[0070] TIFF0007575224000003.tif25161
[0071] TIFF0007575224000004.tif28161
[0072] In the general formulae (3) and (4), (A) represents a block composed of a polyester (a) having hydroxyl groups or alkyl ester groups at both ends, (B) represents a block composed of a compound (b) having one or more ethyleneoxy groups and hydroxyl groups at both ends, and t represents the number of repeating units, which is preferably a number from 1 to 10, more preferably a number from 1 to 7, and most preferably a number from 1 to 5, from the viewpoints of ease of reaction during production, inhibition of coloring, antistatic properties, handleability, and mechanical properties of molded products. 1 represents an alkylene group having 2 to 12 carbon atoms in the aliphatic diol (a1) having 2 to 12 carbon atoms constituting the polyester (a), R 2 represents an alkyl group of the dicarboxylic acid dialkyl ester (a2) constituting the polyester (a).
[0073] The block polymer (C) having hydroxyl groups or alkyl ester groups at both ends can be obtained by a condensation reaction between a polyester (a) having hydroxyl groups or alkyl ester groups at both ends and a compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends. For example, when the end is a hydroxyl group, the reaction can be carried out by an ester exchange reaction. In that case, an aliphatic diol (e.g., 1,2-ethanediol, 1,4-butanediol) is ester exchanged and eliminated. For example, when the end is an alkyl ester group, the reaction can be carried out by an ester exchange reaction. In that case, an alcohol corresponding to the alkyl group (e.g., methanol in the case of a methyl ester) is ester exchanged and eliminated.
[0074] However, as long as the structure is equivalent to a structure in which blocks (A) and blocks (B) are repeatedly and alternately bonded via ester bonds, it is not necessarily required to synthesize the compound from polyester (a) and compound (b).
[0075] The reaction ratio of polyester (a) to compound (b) is adjusted so that X moles of compound (b) and X+1 moles of polyester (a) are used, whereby a block polymer (C) having hydroxyl groups or alkyl ester groups at both ends can be preferably obtained.
[0076] In the reaction, after completion of the synthesis reaction of polyester (a), the compound (b) may be added to the reaction system and reacted as it is without isolating polyester (a).
[0077] The condensation reaction may be carried out using a catalyst for promoting the reaction, and examples of the catalyst that can be used include conventionally known catalysts such as dibutyltin oxide, tetraalkyl titanate, zirconium acetate, zinc acetate, etc. In order to suppress oxidation of the product during the reaction, an antioxidant such as a phenol-based antioxidant may be added to the reaction system.
[0078] From the viewpoints of ease of reaction during production, suppression of coloration, antistatic properties and handleability, and mechanical properties of molded bodies, the polymer compound (E) according to the present invention preferably has a structure in which a block polymer (C) having a structure having hydroxyl groups or alkyl ester groups at both terminals and a polyhydric alcohol compound (D) having three or more hydroxyl groups are bonded via an ester bond formed between the hydroxyl groups or alkyl ester groups at the terminals of the block polymer (C) and the hydroxyl groups of the polyhydric alcohol compound (D).
[0079] Moreover, the polymer compound (E) may further contain an ester bond formed by a hydroxyl group or an alkyl ester group of the polyester (a) and a hydroxyl group of the polyhydric alcohol compound (D).
[0080] The polymer compound (E) can be obtained by subjecting the hydroxyl group or alkyl ester group of the block polymer (C) to a condensation reaction with the hydroxyl group of the polyhydric alcohol compound (D).
[0081] For example, when the block polymer (C) has a hydroxyl group at the end as in general formula (3), it may be reacted by transesterification. In that case, an aliphatic diol (e.g., 1,2-ethanediol, 1,4-butanediol) is transesterified and eliminated. Also, when the block polymer (C) has an alkyl ester group at the end as in general formula (4), it may be reacted by transesterification. In that case, an alcohol corresponding to the alkyl group (e.g., methanol in the case of a methyl ester) is transesterified and eliminated.
[0082] The number of hydroxyl groups in the polyhydric alcohol compound (D) to be reacted is preferably 0.5 to 5 equivalents, more preferably 0.5 to 2.0 equivalents, of the number of hydroxyl groups or alkyl ester groups in the block polymer (C) to be reacted. The reaction may be carried out in various solvents or in a molten state.
[0083] In the reaction, after completion of the synthesis reaction of the block polymer (C), the polyhydric alcohol compound (D) may be added to the reaction system and reacted as is without isolating the block polymer (C). In this case, the hydroxyl groups or alkyl ester groups of the unreacted polyester (a) used in excess when synthesizing the block polymer (C) may react with some of the hydroxyl groups of the polyhydric alcohol compound (D) to form ester bonds.
[0084] A preferred polymer compound (E) of the present invention does not necessarily have to be synthesized from a block polymer (C) having a structure having hydroxyl groups or alkyl ester groups at both terminals and a polyhydric alcohol compound (D) having three or more hydroxyl groups, as long as it has a structure equivalent to a structure in which the block polymer (C) has a structure having hydroxyl groups or alkyl ester groups at both terminals and the polyhydric alcohol compound (D) having three or more hydroxyl groups and is bonded via an ester bond formed by the hydroxyl groups or alkyl ester groups of the block polymer (C) and the hydroxyl groups of the polyhydric alcohol (D).
[0085] In the antistatic agent of the present invention, the number average molecular weight of the polyester (a) constituting the polyester block (A) in the polymer compound (E) is preferably 1,000 to 8,000, more preferably 1,000 to 6,000, and even more preferably 1,000 to 5,000, in terms of polystyrene, from the viewpoints of ease of reaction during production, suppression of coloration, antistatic properties and handling properties, and mechanical properties of molded products. If the number average molecular weight is less than 1,000, the storage stability may be poor, and if it exceeds 8,000, the reaction to obtain the polymer compound (E) may take a long time, which may result in poor economic efficiency, or the obtained polymer compound may be colored due to a long-term reaction.
[0086] The method for measuring the number average molecular weight in terms of polystyrene is preferably gel permeation chromatography (GPC), and the measuring method is described below.
[0087] <Method for measuring number average molecular weight based on polystyrene conversion> The number average molecular weight (hereinafter also referred to as "Mn") was measured by gel permeation chromatography under the following conditions: Equipment: GPC equipment manufactured by JASCO Corporation Solvent: Chloroform Reference material: Polystyrene Detector: Differential refractometer (RI detector) Column stationary phase: Showa Denko Co., Ltd. Shodex LF-804 Column temperature: 40℃ Sample concentration: 1mg / 1mL Flow rate: 0.5mL / min. Injection volume: 100μL
[0088] The number average molecular weight of the compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends constituting the polyether block (B) in the polymer compound (E) is calculated from the measured hydroxyl value, and from the viewpoints of ease of reaction during production, inhibition of coloration, antistatic properties, handleability, and mechanical properties of molded products, is preferably 1,000 to 6,000, more preferably 1,000 to 5,000, and even more preferably 1,000 to 4,000. The method for measuring the hydroxyl value and the method for calculating the number average molecular weight from the hydroxyl value are described below.
[0089] <Calculation method of number average molecular weight from hydroxyl value> The hydroxyl value was measured by the following hydroxyl value measurement method, and the number average molecular weight (hereinafter also referred to as "Mn") was determined by the following formula. Number average molecular weight = (56110 x 2) / hydroxyl value <Hydroxyl value measurement method> Reagent A (acetylating agent) (1) Triethyl phosphate 1560mL (2) Acetic anhydride, 193 mL (3) Perchloric acid (60%) 16g Mix the above reagents in the order of (1) → (2) → (3). Reagent B Mix pyridine and pure water in a volume ratio of 3:1. Reagent C Add 2 to 3 drops of phenolphthalein solution to 500 mL of isopropyl alcohol and neutralize with 1N KOH aqueous solution.
[0090] First, weigh out 2 g of sample into a 200 mL Erlenmeyer flask, add 10 mL of triethyl phosphate, and heat to dissolve. Add 15 mL of Reagent A, plug with a stopper, and shake vigorously. Add 20 mL of Reagent B, plug with a stopper, and shake vigorously. Add 50 mL of Reagent C. Titrate with 1N KOH aqueous solution and calculate using the formula below.
[0091] Hydroxyl value [mgKOH / g] = 56.11 × f × (TB) / S f: Factor of 1N-KOH solution B: Blank titration volume [mL] T: Test titer [mL] S: Sample amount [g]
[0092] Furthermore, the number average molecular weight of the block polymer (C) having hydroxyl groups or alkyl ester groups at both ends in the polymer compound (E) is preferably 5,000 to 30,000, more preferably 6,000 to 26,000, and more preferably 7,000 to 22,000, in terms of ease of reaction during production, coloring suppression, antistatic properties, handleability, and mechanical properties of the molded product, in terms of polystyrene. If the number average molecular weight is less than 5,000, the storage stability may be poor, and if it exceeds 30,000, the reaction to obtain the polymer compound (E) may take a long time, which may result in poor economic efficiency, or the obtained polymer compound may be colored due to a long reaction time. The method for measuring the number average molecular weight in terms of polystyrene is preferably gel permeation chromatography (GPC), and the measuring method is as described above.
[0093] From the viewpoint of antistatic properties, the antistatic agent of the present invention is preferably formed into an antistatic agent composition further comprising one or more salts of aromatic sulfonic acid.
[0094] Examples of salts of aromatic sulfonic acid include salts consisting of an alkali metal cation and an aromatic sulfonic acid anion. Examples of alkali metals constituting the cation include lithium, sodium, potassium, cesium, rubidium, etc., and examples of aromatic sulfonic acids constituting the anion include aromatic sulfonic acids having 1 to 30 carbon atoms such as p-toluenesulfonic acid, dodecylbenzenesulfonic acid, and alkylnaphthalenesulfonic acid. Among them, from the viewpoint of antistatic properties, salts of lithium, sodium, and potassium are more preferable, and salts of sodium are most preferable.
[0095] Specific examples of alkali metal salts of aromatic sulfonic acid include lithium p-toluenesulfonate, sodium p-toluenesulfonate, potassium p-toluenesulfonate, lithium dodecylbenzenesulfonate, sodium dodecylbenzenesulfonate, potassium dodecylbenzenesulfonate, lithium alkylnaphthalenesulfonate, sodium alkylnaphthalenesulfonate, potassium alkylnaphthalenesulfonate, etc. Among these, sodium p-toluenesulfonate, sodium dodecylbenzenesulfonate, sodium alkylnaphthalenesulfonate, etc. are preferred. Among these, sodium dodecylbenzenesulfonate is preferred from the viewpoint of antistatic properties.
[0096] Also, salts of aromatic sulfonic acids using organic cations instead of alkali metal cations may be used.
[0097] Examples of organic cations include amidinium cations, guanidinium cations, and tertiary ammonium cations.
[0098] Examples of amidinium cations include the following:
[0099] [1] Imidazolinium cation 1,2,3,4-tetramethylimidazolinium, 1,3,4-trimethyl-2-ethylimidazolinium, 1,3-dimethylimidazolinium, 1,3-dimethyl-2,4-diethylimidazolinium, 1,2-dimethyl-3,4-diethylimidazolinium, 1-methyl-2,3,4-triethylimidazolinium, 1,2,3,4-tetraethylimidazolinium, 1,2,3-trimethylimidazolinium, 1,3-dimethyl-2-ethylimidazolinium, 1-ethyl-2,3-dimethylimidazolinium, 1,2,3-triethylimidazolinium, 4-cyano-1,2,3-trimethylimidazolinium, 3-cyanomethyl-1,2-dimethylimidazolinium, 2-cyanomethyl-1,3-dimethylimidazolinium Imidazolinium, 4-acetyl-1,2,3-trimethylimidazolinium, 3-acetylmethyl-1,2-dimethylimidazolinium, 4-methylcarboxymethyl-1,2,3-trimethylimidazolinium, 3-methylcarboxymethyl-1,2-dimethylimidazolinium, 4-methoxy-1,2,3-trimethylimidazolinium, 3-methoxymethyl-1,2-dimethylimidazolinium, 4-formyl-1,2,3-trimethylimidazolinium, 3-formylmethyl-1,2-dimethylimidazolinium, 3-hydroxyethyl-1,2-dimethylimidazolinium, 4-hydroxymethyl-1,2,3-trimethylimidazolinium, 2-hydroxyethyl-1,3-dimethylimidazolinium, and the like.
[0100] [2] Imidazolium cation 1,3-Dimethylimidazolium, 1,3-Diethylimidazolium, 1-Ethyl-3-methylimidazolium, 1,2,3-Trimethylimidazolium, 1,2,3,4-Tetramethylimidazolium, 1,3-Dimethyl-2-Ethylimidazolium, 1,2-Dimethyl-3-Ethyl-imidazolium, 1,2,3-Triethylimidazolium, 1,2,3,4-Tetraethylimidazolium, 1,3-Dimethyl-2-Phenylimidazolium, 1,3-Dimethyl-2-Benzylimidazolium, 1-Benzyl-2,3-Dimethyl-imidazolium, 4-Cyano-1,2,3-Trimethylimidazolium, 3-Cyanomethyl-1,2-Dimethylimidazolium, 2-Cyanomethyl-1,3-Dimethyl -imidazolium, 4-acetyl-1,2,3-trimethylimidazolium, 3-acetylmethyl-1,2-dimethylimidazolium, 4-methylcarboxymethyl-1,2,3-trimethylimidazolium, 3-methylcarboxymethyl-1,2-dimethylimidazolium, 4-methoxy-1,2,3-trimethylimidazolium, 3-methoxymethyl-1,2-dimethylimidazolium, 4-formyl-1,2,3-trimethylimidazolium, 3-formylmethyl-1,2-dimethylimidazolium, 3-hydroxyethyl-1,2-dimethylimidazolium, 4-hydroxymethyl-1,2,3-trimethylimidazolium, 2-hydroxyethyl-1,3-dimethylimidazolium, etc.
[0101] [3] Tetrahydropyrimidinium cation 1,3-Dimethyl-1,4,5,6-tetrahydropyrimidinium, 1,2,3-Trimethyl-1,4,5,6-tetrahydropyrimidinium, 1,2,3,4-Tetramethyl-1,4,5,6-tetrahydropyrimidinium, 1,2,3,5-Tetramethyl-1,4,5,6-tetrahydropyrimidinium, 8-Methyl-1,8-diazabicyclo[5,4,0]-7-undecenium, 5-Methyl-1,5-diazabicyclo[4,3,0]- 5-Nonenium, 4-Cyano-1,2,3-trimethyl-1,4,5,6-tetrahydropyrimidinium, 3-Cyanomethyl-1,2-dimethyl-1,4,5,6-tetrahydropyrimidinium, 2-Cyanomethyl-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, 4-Acetyl-1,2,3-trimethyl-1,4,5,6-tetrahydropyrimidinium, 3-Acetylmethyl-1,2-dimethyl-1,4,5,6-tetrahydropyrimidinium Dropyrimidinium, 4-methylcarboxymethyl-1,2,3-trimethyl-1,4,5,6-tetrahydropyrimidinium, 3-methylcarboxymethyl-1,2-dimethyl-1,4,5,6-tetrahydropyrimidinium, 4-methoxy-1,2,3-trimethyl-1,4,5,6-tetrahydropyrimidinium, 3-methoxymethyl-1,2-dimethyl-1,4,5,6-tetrahydropyrimidinium, 4-formyl-1,2,3 -trimethyl-1,4,5,6-tetrahydropyrimidinium, 3-formylmethyl-1,2-dimethyl-1,4,5,6-tetrahydropyrimidinium, 3-hydroxyethyl-1,2-dimethyl-1,4,5,6-tetrahydropyrimidinium, 4-hydroxymethyl-1,2,3-trimethyl-1,4,5,6-tetrahydropyrimidinium, 2-hydroxyethyl-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium and the like.
[0102] [4] Dihydropyrimidinium cation 1,3-Dimethyl-1,4- or -1,6-dihydropyrimidinium, [These are referred to as 1,3-dimethyl-1,4(6)-dihydropyrimidinium, and the same expression will be used hereinafter.] 1,2,3-trimethyl-1,4(6)-dihydropyrimidinium, 1,2,3,4-tetramethyl-1,4(6)-dihydropyrimidinium, 1,2,3,5-tetramethyl-1,4(6)-dihydropyrimidinium, 8-methyl-1,8-diazabicyclo[5,4,0]-7,9(10)-undecadienium, 5-methyl-1,5-diazabicyclo[4,3,0]-5,7(8)-nonadienium , 4-cyano-1,2,3-trimethyl-1,4(6)-dihydropyrimidinium, 3-cyanomethyl-1,2-dimethyl-1,4(6)-dihydropyrimidinium, 2-cyanomethyl-1,3-dimethyl-1,4(6)-dihydropyrimidinium, 4-acetyl-1,2,3-trimethyl-1,4(6)-dihydropyrimidinium, 3-acetylmethyl-1,2-dimethyl-1,4(6)-dihydropyrimidinium 4-methylcarboxymethyl-1,2,3-trimethyl-1,4(6)-dihydropyrimidinium, 3-methylcarboxymethyl-1,2-dimethyl-1,4(6)-dihydropyrimidinium, 4-methoxy-1,2,3-trimethyl-1,4(6)-dihydropyrimidinium, 3-methoxymethyl-1,2-dimethyl-1,4(6)-dihydropyrimidinium, 4-formyl-1,2,3- Trimethyl-1,4(6)-dihydropyrimidinium, 3-formylmethyl-1,2-dimethyl-1,4(6)-dihydropyrimidinium, 3-hydroxyethyl-1,2-dimethyl-1,4(6)-dihydropyrimidinium, 4-hydroxymethyl-1,2,3-trimethyl-1,4(6)-dihydropyrimidinium, 2-hydroxyethyl-1,3-dimethyl-1,4(6)-hydropyrimidinium and the like.
[0103] The guanidinium cations include the following:
[0104] [1] Guanidinium cation with an imidazolinium skeleton 2-Dimethylamino-1,3,4-trimethylimidazolinium, 2-Diethylamino-1,3,4-trimethylimidazolinium, 2-Diethylamino-1,3-dimethyl-4-ethylimidazolinium, 2-Dimethylamino-1-methyl-3,4-diethylimidazolinium, 2-Diethylamino-1-methyl-3,4-diethylimidazolinium, 2-Diethylamino-1,3,4-tetraethylimidazolinium, 2-Dimethylamino-1,3-dimethylimidazolinium, 2-Diethyla 1,5-Dihydro-1,2-dimethyl-2H-imido[1,2a]imidazolinium, 1,5-Dihydro-1,2-dimethyl-2H-imido[1,2a]imidazolinium, 1,5,6,7-Tetrahydro-1,2-dimethyl-2H-pyrimido[1,2a]imidazolinium, 1,5,6,7-Tetrahydro-1,2-dimethyl-2H-pyrimido[1,2a]imidazolinium, 1,5-Dihydro-1,2-dimethyl -2H-pyrimido[1,2a]imidazolinium, 2-dimethylamino-4-cyano-1,3-dimethylimidazolinium, 2-dimethylamino-3-cyanomethyl-1-methylimidazolinium, 2-dimethylamino-4-acetyl-1,3-dimethylimidazolinium, 2-dimethylamino-3-acetylmethyl-1-methylimidazolinium, 2-dimethylamino-4-methylcarboxymethyl-1,3-dimethylimidazolinium, 2-dimethylamino-3-methylcarboxymethyl- 1-methylimidazolinium, 2-dimethylamino-4-methoxy-1,3-dimethylimidazolinium, 2-dimethylamino-3-methoxymethyl-1-methylimidazolinium, 2-dimethylamino-4-formyl-1,3-dimethylimidazolinium, 2-dimethylamino-3-formylmethyl-1-methylimidazolinium, 2-dimethylamino-3-hydroxyethyl-1-methylimidazolinium, 2-dimethylamino-4-hydroxymethyl-1,3-dimethylimidazolinium and the like.
[0105] [2] Guanidinium cation with an imidazolium skeleton 2-Dimethylamino-1,3,4-trimethylimidazolium, 2-Diethylamino-1,3,4-trimethylimidazolium, 2-Diethylamino-1,3-dimethyl-4-ethylimidazolium, 2-Dimethylamino-1-methyl-3,4-diethylimidazolium, 2-Diethylamino-1-methyl-3,4-diethylimidazolium, 2-Diethylamino-1,3,4-tetraethylimidazolium, 2-Dimethylamino-1,3-dimethylimidazolium, 2-Diethyla 1,5-Dihydro-1,2-dimethyl-2H-imido[1,2a]imidazolium, 1,5-Dihydro-1,2-dimethyl-2H-imido[1,2a]imidazolium, 1,5,6,7-Tetrahydro-1,2-dimethyl-2H-pyrimido[1,2a]imidazolium, 1,5,6,7-Tetrahydro-1,2-dimethyl-2H-pyrimido[1,2a]imidazolium, 1,5-Dihydro-1,2-dimethyl-2H-pyrimido[1,2a]imidazolium -2H-pyrimido[1,2a]imidazolium, 2-dimethylamino-4-cyano-1,3-dimethylimidazolium, 2-dimethylamino-3-cyanomethyl-1-methylimidazolium, 2-dimethylamino-4-acetyl-1,3-dimethylimidazolinium, 2-dimethylamino-3-acetylmethyl-1-methylimidazolium, 2-dimethylamino-4-methylcarboxymethyl-1,3-dimethylimidazolium, 2-dimethylamino-3-methylcarboxymethyl -1-methylimidazolium, 2-dimethylamino-4-methoxy-1,3-dimethylimidazolium, 2-dimethylamino-3-methoxymethyl-1-methylimidazolium, 2-dimethylamino-4-formyl-1,3-dimethylimidazolium, 2-dimethylamino-3-formylmethyl-1-methylimidazolium, 2-dimethylamino-3-hydroxyethyl-1-methylimidazolium, 2-dimethylamino-4-hydroxymethyl-1,3-dimethylimidazolium, and the like.
[0106] [3] Guanidinium cation with a tetrahydropyrimidinium skeleton 2-Dimethylamino-1,3,4-trimethyl-1,4,5,6-tetrahydropyrimidinium, 2-Diethylamino-1,3,4-trimethyl-1,4,5,6-tetrahydropyrimidinium, 2-Diethylamino-1,3-dimethyl-4-ethyl-1,4,5,6-tetrahydropyrimidinium, 2-Dimethylamino-1-methyl-3,4-diethyl-1,4,5,6-tetrahydropyrimidinium, 2-Diethylamino-1-methyl-3,4-diethyl-1,4,5,6-tetrahydropyrimidinium, 2-Diethylamino- 1,3,4-Tetraethyl-1,4,5,6-tetrahydropyrimidinium, 2-Dimethylamino-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, 2-Diethylamino-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, 2-Dimethylamino-1-ethyl-3-methyl-1,4,5,6-tetrahydropyrimidinium, 2-Diethylamino-1,3-diethyl-1,4,5,6-tetrahydropyrimidinium, 1,3,4,6,7,8-Hexahydro-1,2-dimethyl-2H-imide [1,2 a]pyrimidinium, 1,3,4,6-tetrahydro-1,2-dimethyl-2H-imido[1,2a]pyrimidinium, 1,3,4,6,7,8-hexahydro-1,2-dimethyl-2H-pyrimido[1,2a]pyrimidinium, 1,3,4,6-tetrahydro-1,2-dimethyl-2H-pyrimido[1,2a]pyrimidinium, 2-dimethylamino-4-cyano-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-3-cyanomethyl-1-methyl-1,4,5,6-tetrahydropyrimidinium 2-dimethylamino-4-acetyl-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-3-acetylmethyl-1-methyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-4-methylcarboxymethyl-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-3-methylcarboxymethyl-1-methyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-4-methoxy-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-3-methoxymethyl-1-methyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-4-formyl-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-3-formylmethyl-1-methyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-3-hydroxyethyl-1-methyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-4-hydroxymethyl-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, etc.
[0107] [4] Guanidinium cation with a dihydropyrimidinium skeleton 2-Dimethylamino-1,3,4-trimethyl-1,4(6)-dihydropyrimidinium, 2-Diethylamino-1,3,4-trimethyl-1,4(6)-dihydropyrimidinium, 2-Diethylamino-1,3-dimethyl-4-ethyl-1,4(6)-dihydropyrimidinium, 2-Dimethylamino-1-methyl-3,4-diethyl-1,4(6)-dihydropyrimidinium, 2-Diethylamino-1-methyl-3,4-diethyl-1,4(6)-dihydropyrimidinium, 2-Diethylamino-1,3,4-tetraethyl-1,4(6)-di Hydropyrimidinium, 2-dimethylamino-1,3-dimethyl-1,4(6)-dihydropyrimidinium, 2-diethylamino-1,3-dimethyl-1,4(6)-dihydropyrimidinium, 2-dimethylamino-1-ethyl-3-methyl-1,4(6)-dihydropyrimidinium, 2-diethylamino-1,3-diethyl-1,4(6)-dihydropyrimidinium, 1,6,7,8-tetrahydro-1,2-dimethyl-2H-imido[1,2a]pyrimidinium, 1,6-dihydro-1,2-dimethyl-2H-imido[1,2a]pyrimidinium 1,6,7,8-tetrahydro-1,2-dimethyl-2H-pyrimido[1,2a]pyrimidinium, 1,6-dihydro-1,2-dimethyl-2H-pyrimido[1,2a]pyrimidinium, 2-dimethylamino-4-cyano-1,3-dimethyl-1,4(6)-dihydropyrimidinium, 2-dimethylamino-3-cyanomethyl-1-methyl-1,4(6)-dihydropyrimidinium, 2-dimethylamino-4-acetyl-1,3-dimethyl-1,4(6)-dihydropyrimidinium, 2-dimethylamino-3-acetylmethyl-1-methyl -1,4(6)-dihydropyrimidinium, 2-dimethylamino-4-methylcarboxymethyl-1,3-dimethyl-1,4(6)-dihydropyrimidinium, 2-dimethylamino-3-methylcarboxymethyl-1-methyl-1,4(6)-dihydropyrimidinium, 2-dimethylamino-4-methoxy-1,3-dimethyl-1,4(6)-dihydropyrimidinium, 2-dimethylamino-3-methoxymethyl-1-methyl-1,4(6)-dihydropyrimidinium, 2-dimethylamino-4-formyl-1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-3-formylmethyl-1-methyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-3-hydroxyethyl-1-methyl-1,4,5,6-tetrahydropyrimidinium, 2-dimethylamino-4-hydroxymethyl-1,3-dimethyl-1,4(6)-dihydropyrimidinium, etc.
[0108] Of these, imidazoliniums are preferred, and 1,2,3,4-tetramethylimidazolinium, 1,2,3-trimethylimidazolinium, and 1-ethyl-2,3-dimethylimidazolinium are particularly preferred.
[0109] Tertiary ammonium cations include methyldilauryl ammonium and the like.
[0110] These cations may be used alone or in combination of two or more.
[0111] The aromatic sulfonic acid salt may be blended with the polymer compound (E) used in the antistatic agent of the present invention, or may be blended with the polymer compound (E) in a synthetic resin such as a thermoplastic resin. From the viewpoint of antistatic properties, the blending amount of the aromatic sulfonic acid salt is preferably 1 to 20 parts by mass, more preferably 3 to 15 parts by mass, per 100 parts by mass of the polymer compound (E).
[0112] To obtain the antistatic agent composition of the present invention, the antistatic agent of the present invention, one or more salts of aromatic sulfonic acid, and other optional components may be mixed, if necessary, and various mixers may be used for mixing. Heat may be used during mixing. Examples of mixers that can be used include a tumbler mixer, a Henschel mixer, a ribbon blender, a V-type mixer, a W-type mixer, a super mixer, and a Nauta mixer. In addition, one or more salts of aromatic sulfonic acid may be added to the reaction system during the synthesis reaction of the polymer compound (E).
[0113] Furthermore, the antistatic agent of the present invention may be used as an antistatic agent composition having antistatic properties by blending an alkali metal salt other than the salt of aromatic sulfonic acid within a range that does not impair the effects of the present invention.
[0114] Examples of alkali metal salts other than aromatic sulfonic acid salts include salts of organic acids or inorganic acids, and examples of alkali metals include lithium, sodium, potassium, cesium, rubidium, etc. Examples of organic acids include aliphatic monocarboxylic acids having 1 to 18 carbon atoms, such as formic acid, acetic acid, propionic acid, butyric acid, and lactic acid; aliphatic dicarboxylic acids having 1 to 12 carbon atoms, such as oxalic acid, malonic acid, succinic acid, fumaric acid, maleic acid, and adipic acid; aromatic carboxylic acids such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, and salicylic acid; and aliphatic sulfonic acids having 1 to 20 carbon atoms, such as methanesulfonic acid and trifluoromethanesulfonic acid. Examples of inorganic acids include hydrochloric acid, hydrobromic acid, sulfuric acid, sulfurous acid, phosphoric acid, phosphorous acid, polyphosphoric acid, nitric acid, and perchloric acid. Among them, from the viewpoint of antistatic properties and safety to living bodies and the environment, salts of lithium, sodium, and potassium are preferred, and sodium is more preferred.
[0115] Specific examples of alkali metal salts other than aromatic sulfonic acid salts include lithium acetate, sodium acetate, potassium acetate, lithium chloride, sodium chloride, potassium chloride, lithium phosphate, sodium phosphate, potassium phosphate, lithium sulfate, sodium sulfate, lithium perchlorate, sodium perchlorate, and potassium perchlorate.
[0116] The alkali metal salt other than the aromatic sulfonic acid salt may be blended into the antistatic agent of the present invention, or may be blended into a synthetic resin together with the antistatic agent of the present invention and used. From the viewpoint of antistatic properties, the blending amount thereof is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and most preferably 3.0 to 12 parts by mass, relative to 100 parts by mass of the antistatic agent of the present invention.
[0117] Furthermore, the antistatic agent of the present invention may be used as an antistatic agent composition having antistatic properties by blending an ionic liquid other than the salt of aromatic sulfonic acid within a range that does not impair the effects of the present invention.
[0118] Examples of ionic liquids include room-temperature molten salts having a melting point of 100°C or less, at least one of the cations or anions constituting the ionic liquid being an organic ion, and having an initial conductivity of 1 to 200 ms / cm, preferably 10 to 200 ms / cm, such as those described in WO 95 / 15572.
[0119] Examples of the cations constituting the ionic liquid include cations selected from the group consisting of amidinium, pyridinium, pyrazolium and guanidinium cations. Among these, examples of the amidinium cation include the following:
[0120] (1) Imidazolinium cation Examples of the imidazolinium include those having 5 to 15 carbon atoms, such as 1,2,3,4-tetramethylimidazolinium and 1,3-dimethylimidazolinium;
[0121] (2) Imidazolium cation Examples of the imidazolium derivatives include those having 5 to 15 carbon atoms, such as 1,3-dimethylimidazolium and 1-ethyl-3-methylimidazolium;
[0122] (3) Tetrahydropyrimidinium cation Examples of the aryl group include those having 6 to 15 carbon atoms, such as 1,3-dimethyl-1,4,5,6-tetrahydropyrimidinium and 1,2,3,4-tetramethyl-1,4,5,6-tetrahydropyrimidinium;
[0123] (4) Dihydropyrimidinium cation Examples of the alkyl group include those having 6 to 20 carbon atoms, such as 1,3-dimethyl-1,4-dihydropyrimidinium, 1,3-dimethyl-1,6-dihydropyrimidinium, 8-methyl-1,8-diazabicyclo[5,4,0]-7,9-undecadienium, and 8-methyl-1,8-diazabicyclo[5,4,0]-7,10-undecadienium.
[0124] The pyridinium cation may be one having 6 to 20 carbon atoms, such as 3-methyl-1-propylpyridinium and 1-butyl-3,4-dimethylpyridinium.
[0125] The pyrazolium cation may be one having 5 to 15 carbon atoms, such as 1,2-dimethylpyrazolium or 1-n-butyl-2-methylpyrazolium.
[0126] The guanidinium cations include the following: (1) Guanidinium cation with an imidazolinium skeleton Examples of the imidazolium salt include those having 8 to 15 carbon atoms, such as 2-dimethylamino-1,3,4-trimethylimidazolinium and 2-diethylamino-1,3,4-trimethylimidazolinium;
[0127] (2) Guanidinium cation with an imidazolium skeleton Examples of the imidazolium derivatives include those having 8 to 15 carbon atoms, such as 2-dimethylamino-1,3,4-trimethylimidazolium and 2-diethylamino-1,3,4-trimethylimidazolium;
[0128] (3) Guanidinium cation having a tetrahydropyrimidinium skeleton Examples of the alkyl group include those having 10 to 20 carbon atoms, such as 2-dimethylamino-1,3,4-trimethyl-1,4,5,6-tetrahydropyrimidinium and 2-diethylamino-1,3-dimethyl-4-ethyl-1,4,5,6-tetrahydropyrimidinium;
[0129] (4) Guanidinium cation having a dihydropyrimidinium skeleton Examples thereof include those having 10 to 20 carbon atoms, such as 2-dimethylamino-1,3,4-trimethyl-1,4-dihydropyrimidinium, 2-dimethylamino-1,3,4-trimethyl-1,6-dihydropyrimidinium, 2-diethylamino-1,3-dimethyl-4-ethyl-1,4-dihydropyrimidinium, and 2-diethylamino-1,3-dimethyl-4-ethyl-1,6-dihydropyrimidinium.
[0130] These cations may be used alone or in combination of two or more. Among these, from the viewpoints of frictional electrification voltage and surface resistivity, the amidinium cation is preferred, the imidazolium cation is more preferred, and the 1-ethyl-3-methylimidazolium cation is particularly preferred.
[0131] In the ionic liquid, examples of organic or inorganic acids constituting the anion include the following. Examples of organic acids include carboxylic acids, sulfuric esters, aliphatic sulfonic acids, and phosphoric esters; examples of inorganic acids include superacids (e.g., borofluoroacid, tetrafluoroboric acid, perchloric acid, hexafluorophosphoric acid, hexafluoroantimonic acid, and hexafluoroarsenic acid), phosphoric acid, and boric acid. These organic and inorganic acids may be used alone or in combination of two or more.
[0132] Among organic acids and inorganic acids, preferred from the viewpoint of the antistatic properties of the ionic liquid are acids that form conjugate bases of super strong acids, anions other than the conjugate bases of super strong acids, and mixtures thereof, in which the Hamett acidity function (-H0) of the anions constituting the ionic liquid is 12 to 100.
[0133] Examples of anions other than the conjugate base of a super strong acid include halogen (such as fluorine, chlorine and bromine) ions and poly(n=1 to 25)fluoroalkanesulfonic acid (such as undecafluoropentanesulfonic acid) ions.
[0134] In addition, examples of the super strong acid include protonic acids and those derived from a combination of a protonic acid and a Lewis acid, and mixtures thereof. Examples of the protonic acid as the super strong acid include bis(trifluoromethylsulfonyl)imide acid, bis(pentafluoroethylsulfonyl)imide acid, tris(trifluoromethylsulfonyl)methane, perchloric acid, fluorosulfonic acid, alkane (having 1 to 30 carbon atoms)sulfonic acid (e.g., methanesulfonic acid, dodecanesulfonic acid, etc.), poly(n=1 to 30)fluoroalkane (having 1 to 30 carbon atoms)sulfonic acid (e.g., trifluoromethanesulfonic acid, pentafluoroethanesulfonic acid, heptafluoropropanesulfonic acid, nonafluorobutanesulfonic acid, undecafluoropentanesulfonic acid, and tridecafluorohexanesulfonic acid), borofluoric acid, and tetrafluoroboric acid. Among these, preferred from the viewpoint of ease of synthesis are borofluoroacid, trifluoromethanesulfonic acid, bis(trifluoromethanesulfonyl)imidic acid and bis(pentafluoroethylsulfonyl)imidic acid.
[0135] Examples of protonic acids used in combination with the Lewis acid include hydrogen halides (e.g., hydrogen fluoride, hydrogen chloride, hydrogen bromide, and hydrogen iodide), perchloric acid, fluorosulfonic acid, methanesulfonic acid, trifluoromethanesulfonic acid, pentafluoroethanesulfonic acid, nonafluorobutanesulfonic acid, undecafluoropentanesulfonic acid, tridecafluorohexanesulfonic acid, and mixtures thereof. Among these, hydrogen fluoride is preferred from the viewpoint of the initial conductivity of the ionic liquid. Examples of Lewis acids include boron trifluoride, phosphorus pentafluoride, antimony pentafluoride, arsenic pentafluoride, tantalum pentafluoride, and mixtures thereof. Among these, boron trifluoride and phosphorus pentafluoride are preferred from the viewpoint of the initial conductivity of the ionic liquid.
[0136] The combination of the protonic acid and the Lewis acid is arbitrary, and examples of super strong acids formed by these combinations include tetrafluoroboric acid, hexafluorophosphoric acid, hexafluorotantalic acid, hexafluoroantimonic acid, hexafluorotantalum sulfonic acid, tetrafluoroboric acid, hexafluorophosphoric acid, chlorotrifluoroboric acid, hexafluoroarsenic acid, and mixtures thereof.
[0137] Of these anions, from the viewpoint of the antistatic properties of the ionic liquid, preferred are the conjugate bases of super strong acids (super strong acids composed of protonic acids and super strong acids composed of a combination of a protonic acid and a Lewis acid), and more preferred are the conjugate bases of super strong acids composed of protonic acids and super strong acids composed of a protonic acid, boron trifluoride and / or phosphorus pentafluoride.
[0138] Among ionic liquids, from the viewpoint of antistatic properties, preferred are ionic liquids having an amidinium cation, more preferred are ionic liquids having a 1-ethyl-3-methylimidazolium cation, and particularly preferred is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide.
[0139] The ionic liquid may be blended with the antistatic agent of the present invention, or may be blended with a synthetic resin together with the antistatic agent of the present invention. The blending amount of the ionic liquid is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and most preferably 1 to 12 parts by mass, relative to 100 parts by mass of the antistatic agent of the present invention, from the viewpoint of antistatic properties and their durability.
[0140] The antistatic agent of the present invention may be used as an antistatic agent composition having antistatic properties by blending a salt of a Group 2 element within a range that does not impair the effects of the present invention. Examples of the salt of the Group 2 element include salts of organic acids or inorganic acids, and examples of the Group 2 element include beryllium, magnesium, calcium, strontium, barium, etc. Examples of the organic acid include aliphatic monocarboxylic acids having 1 to 18 carbon atoms such as formic acid, acetic acid, propionic acid, butyric acid, and lactic acid; aliphatic dicarboxylic acids having 1 to 12 carbon atoms such as oxalic acid, malonic acid, succinic acid, fumaric acid, maleic acid, and adipic acid; aromatic carboxylic acids such as benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, and salicylic acid; and aliphatic sulfonic acids having 1 to 20 carbon atoms such as methanesulfonic acid and trifluoromethanesulfonic acid. Examples of the inorganic acid include hydrochloric acid, hydrobromic acid, sulfuric acid, sulfurous acid, phosphoric acid, phosphorous acid, polyphosphoric acid, nitric acid, and perchloric acid.
[0141] The salt of the Group 2 element may be blended in the antistatic agent of the present invention, or may be blended in a synthetic resin together with the antistatic agent of the present invention. The blending amount of the salt of the Group 2 element is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and most preferably 3.0 to 12 parts by mass, based on 100 parts by mass of the antistatic agent of the present invention.
[0142] The antistatic agent of the present invention may be used as an antistatic agent composition having antistatic properties by blending a surfactant within a range that does not impair the effects of the present invention. As the surfactant, a nonionic, anionic, cationic or amphoteric surfactant can be used. Examples of the nonionic surfactant include polyethylene glycol type nonionic surfactants such as higher alcohol ethylene oxide adducts, fatty acid ethylene oxide adducts, higher alkylamine ethylene oxide adducts, and polypropylene glycol ethylene oxide adducts; polyhydric alcohol type nonionic surfactants such as polyethylene oxide, fatty acid esters of glycerin, fatty acid esters of pentaerythritol, fatty acid esters of sorbitol or sorbitan, alkyl ethers of polyhydric alcohols, and fatty amides of alkanolamines; examples of the anionic surfactant include carboxylates such as alkali metal salts of higher fatty acids; sulfate ester salts such as higher alcohol sulfate ester salts, higher alkyl ether sulfate ester salts, sulfonates such as alkyl sulfonates and paraffin sulfonates; and phosphate ester salts such as higher alcohol phosphate ester salts; examples of the cationic surfactant include quaternary ammonium salts such as alkyl trimethyl ammonium salts. Examples of amphoteric surfactants include amino acid type amphoteric surfactants such as higher alkylaminopropionate salts, betaine type amphoteric surfactants such as higher alkyldimethylbetaine and higher alkyldihydroxyethylbetaine, and the like. These can be used alone or in combination of two or more kinds.
[0143] The surfactant may be blended in the antistatic agent of the present invention, or may be blended in a synthetic resin together with the antistatic agent of the present invention. The blending amount of the surfactant is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and most preferably 1 to 10 parts by mass, based on 100 parts by mass of the antistatic agent of the present invention.
[0144] Furthermore, the antistatic agent of the present invention may be used as an antistatic agent composition having antistatic properties by blending a polymeric antistatic agent within a range that does not impair the effects of the present invention. As the polymeric antistatic agent, for example, a polymeric antistatic agent such as a known polyetheresteramide can be used, and as the known polyetheresteramide, for example, a polyetheresteramide consisting of a polyoxyalkylene adduct of bisphenol A described in JP-A-7-10989 can be mentioned. In addition, a block polymer having a repeating structure with 2 to 50 bond units between a polyolefin block and a hydrophilic polymer block can be used, and for example, a block polymer described in US Pat. No. 6,552,131 can be mentioned.
[0145] The polymer-type antistatic agent may be blended with the antistatic agent of the present invention, or may be blended with a synthetic resin together with the antistatic agent of the present invention. The blending amount of the polymer-type antistatic agent is preferably 0 to 50 parts by mass, more preferably 5 to 20 parts by mass, based on 100 parts by mass of the antistatic agent of the present invention.
[0146] Furthermore, the antistatic agent of the present invention may be blended with a compatibilizer to the extent that the effect of the present invention is not impaired, to form an antistatic agent composition having antistatic properties. Blending with a compatibilizer can improve the compatibility of the antistatic agent of the present invention with other components and synthetic resins. Examples of such compatibilizers include modified vinyl polymers having at least one functional group (polar group) selected from the group consisting of carboxyl groups, epoxy groups, amino groups, hydroxyl groups, and polyoxyalkylene groups, such as the polymers described in JP-A-3-258850, modified vinyl polymers having sulfonyl groups described in JP-A-6-345927, and block polymers having a polyolefin portion and an aromatic vinyl polymer portion. More preferred compatibilizers include acid anhydride-modified polyolefins such as maleic anhydride-modified polyethylene, maleic anhydride-modified polypropylene, itaconic anhydride-modified polyethylene, and itaconic anhydride-modified polypropylene.
[0147] The compatibilizer may be blended with the antistatic agent of the present invention, or may be blended with a synthetic resin together with the antistatic agent of the present invention. The blending amount of the compatibilizer is preferably 0.1 to 15 parts by mass, more preferably 1 to 10 parts by mass, based on 100 parts by mass of the antistatic agent of the present invention.
[0148] In addition to the antistatic agent of the present invention and the above-mentioned components, other components may be blended as optional components in the antistatic agent composition of the present invention, so long as the effects of the present invention are not impaired. These other components may be blended directly into the antistatic agent composition, or may be blended into a synthetic resin such as a thermoplastic resin when the antistatic agent of the present invention or the antistatic agent composition of the present invention is blended into the synthetic resin to be used as a resin composition having antistatic properties.
[0149] Next, the antistatic resin composition of the present invention will be described. The resin composition of the present invention is obtained by blending the antistatic agent of the present invention or the antistatic agent composition of the present invention with a synthetic resin. The synthetic resin is preferably a thermoplastic resin.
[0150] Examples of thermoplastic resins include α-olefin polymers such as polypropylene, high density polyethylene, low density polyethylene, linear low density polyethylene, cross-linked polyethylene, ultra-high molecular weight polyethylene, polybutene-1, poly-3-methylpentene, and poly-4-methylpentene, or polyolefin resins such as ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-propylene copolymer, and copolymers thereof; halogen-containing resins such as polyvinyl chloride, polyvinylidene chloride, chlorinated polyethylene, chlorinated polypropylene, polyvinylidene fluoride, chlorinated rubber, vinyl chloride-vinyl acetate copolymer, vinyl chloride-ethylene copolymer, vinyl chloride-vinylidene chloride copolymer, vinyl chloride-vinylidene chloride-vinyl acetate terpolymer, vinyl chloride-acrylic acid ester copolymer, vinyl chloride-maleic acid ester copolymer, and vinyl chloride-cyclohexylmaleimide copolymer; petroleum resin, coumarone resin, polystyrene, polyvinyl acetate, acrylic resin, styrene, and / or the like. or copolymers of α-methylstyrene with other monomers (e.g., maleic anhydride, phenylmaleimide, methyl methacrylate, butadiene, acrylonitrile, etc.) (e.g., AS resin, ABS (acrylonitrile butadiene styrene copolymer) resin, ACS resin, SBS resin, MBS resin, heat-resistant ABS resin, etc.); polymethyl methacrylate, polyvinyl alcohol, polyvinyl formal, polyvinyl butyral; aromatic polyesters such as polyalkylene terephthalates such as polyethylene terephthalate, polybutylene terephthalate, and polycyclohexane dimethylene terephthalate, polyalkylene naphthalates such as polyethylene naphthalate and polybutylene naphthalate, and linear polyesters such as polytetramethylene terephthalate; degradable aliphatic polyesters such as polyhydroxybutyrate, polycaprolactone, polybutylene succinate, polyethylene succinate, polylactic acid, polymalic acid, polyglycolic acid, polydioxane, and poly(2-oxetanone);Examples of the thermoplastic resins include polyamides such as polyphenylene oxide, polycaprolactam, and polyhexamethylene adipamide, polycarbonate, polycarbonate / ABS resin, branched polycarbonate, polyacetal, polyphenylene sulfide, polyurethane, cellulose resin, polyimide resin, polysulfone, polyphenylene ether, polyether ketone, polyether ether ketone, and liquid crystal polymer, and blends thereof.
[0151] The thermoplastic resin may be an elastomer such as isoprene rubber, butadiene rubber, acrylonitrile-butadiene copolymer rubber, styrene-butadiene copolymer rubber, fluororubber, silicone rubber, olefin-based elastomer, styrene-based elastomer, polyester-based elastomer, nitrile-based elastomer, nylon-based elastomer, vinyl chloride-based elastomer, polyamide-based elastomer, or polyurethane-based elastomer. In the resin composition of the present invention, these thermoplastic resins may be used alone or in combination of two or more kinds. The thermoplastic resin may be alloyed.
[0152] These thermoplastic resins can be used regardless of the molecular weight, degree of polymerization, density, softening point, proportion of insoluble matter in a solvent, degree of stereoregularity, presence or absence of catalyst residue, types and blending ratios of raw monomers, types of polymerization catalysts (e.g., Ziegler catalysts, metallocene catalysts, etc.), polymerization methods (e.g., bulk polymerization, suspension polymerization, etc.), etc.
[0153] Among these thermoplastic resins, from the viewpoints of antistatic properties and mechanical properties of molded products, one or more types selected from the group consisting of polystyrene-based resins and copolymers thereof are preferred, and specifically, ABS resin is preferred.
[0154] The mass ratio of the synthetic resin to the antistatic agent of the present invention or the antistatic agent composition of the present invention in the resin composition of the present invention is preferably in the range of 99 / 1 to 40 / 60, more preferably in the range of 90 / 10 to 60 / 40, from the viewpoints of antistatic properties and mechanical properties of a molded product.
[0155] The method of blending the antistatic agent of the present invention into a synthetic resin is not particularly limited, and any method that is commonly used can be used. For example, the antistatic agent of the present invention may be blended by mixing and kneading using a roll mixer, bumper mixer, extruder, kneader, etc. The antistatic agent of the present invention may be added to a synthetic resin as is, or may be added after impregnating the carrier, if necessary. To impregnate the carrier, the agent may be heated and mixed as is, or may be diluted with an organic solvent, if necessary, and then impregnated into the carrier, and the solvent may be removed. As such a carrier, those known as fillers or bulking agents for synthetic resins, or flame retardants and light stabilizers that are solid at room temperature can be used, and examples thereof include calcium silicate powder, silica powder, talc powder, alumina powder, titanium oxide powder, or carriers whose surfaces have been chemically modified, and flame retardants and antioxidants that are solid, as listed below. Among these carriers, carriers whose surfaces have been chemically modified are preferred, and silica powder whose surfaces have been chemically modified are more preferred. These carriers preferably have an average particle size of 0.1 to 100 μm, and more preferably 0.5 to 50 μm.
[0156] The method of blending the antistatic agent of the present invention with a synthetic resin may involve kneading the block polymer (C) and the polyhydric alcohol compound (D) having three or more hydroxyl groups into the synthetic resin simultaneously to synthesize the antistatic agent of the present invention and blending it therein, or at the same time, one or more salts of aromatic sulfonic acids may be kneaded in at the same time. Alternatively, the antistatic agent of the present invention may be blended with a synthetic resin during molding such as injection molding to obtain a molded product, and at that time, one or more salts of aromatic sulfonic acids may be blended in at that time. Furthermore, a masterbatch of the antistatic agent of the present invention and a synthetic resin may be produced in advance, and this masterbatch may be blended, and at that time, one or more salts of aromatic sulfonic acids may be blended in at that time.
[0157] If necessary, various additives such as a phenol-based antioxidant, a phosphorus-based antioxidant, a thioether-based antioxidant, an ultraviolet absorber, and a hindered amine-based light stabilizer can be further added to the resin composition of the present invention, thereby stabilizing the resin composition of the present invention.
[0158] These various additives such as antioxidants may be blended in the antistatic agent composition of the present invention before blending with the synthetic resin. Furthermore, they may be blended during the production of the polymer compound (E) which is the antistatic agent of the present invention. In particular, the antioxidant is preferably blended during the production of the polymer compound (E) since it can prevent the polymer compound (E) from being deteriorated by oxidation during the production.
[0159] Examples of the phenol-based antioxidants include 2,6-di-tert-butyl-p-cresol, 2,6-diphenyl-4-octadecyloxyphenol, distearyl (3,5-di-tert-butyl-4-hydroxybenzyl)phosphonate, 1,6-hexamethylenebis[(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid amide], 4,4'-thiobis(6-tert-butyl-m-cresol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-butyl-m-cresol, ... 2,2'-ethylidenebis(6-tert-butyl-m-cresol), 2,2'-ethylidenebis(4,6-di-tert-butylphenol), 2,2'-ethylidenebis(4-sec-butyl-6-tert-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-tris(2,6-dimethyl-3-hydroxy-4-tert-butylbenzyl)isocyanurate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, diethyl)-2,4,6-trimethylbenzene, 2-tert-butyl-4-methyl-6-(2-acryloyloxy-3-tert-butyl-5-methylbenzyl)phenol, stearyl (3,5-di-tert-butyl-4-hydroxyphenyl)propionate, tetrakis [3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate methyl]methane, thiodiethylene glycol bis [(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 1,6-hexamethylene bis [(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] 〕, bis[3,3-bis(4-hydroxy-3-tert-butylphenyl)butyric acid]glycol ester, bis[2-tert-butyl-4-methyl-6-(2-hydroxy-3-tert-butyl-5-methylbenzyl)phenyl]terephthalate, 1,3,5-tris[(3,5-ditert-butyl-4-hydroxyphenyl)propionyloxyethyl]isocyanurate, 3,9-bis[1,1-dimethyl-2-{(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, triethylene glycol bis[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate], etc. The amount of these phenol-based antioxidants added is preferably 0.001 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the synthetic resin.
[0160] Examples of phosphorus-based antioxidants include trisnonylphenyl phosphite, tris[2-tert-butyl-4-(3-tert-butyl-4-hydroxy-5-methylphenylthio)-5-methylphenyl]phosphite, tridecyl phosphite, octyldiphenyl phosphite, di(decyl)monophenyl phosphite, di(tridecyl)pentaerythritol diphosphite, di(nonylphenyl)pentaerythritol diphosphite, bis(2,4-ditert-butylphenyl)pentaerythritol diphosphite, bis(2,6-ditert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,4,6-tritert-butylphenyl)pentaerythritol diphosphite, bis(2,4-dicumylphenyl)pentaerythritol diphosphite, tetra(tridecyl)isopropylidenediphenol diphosphite, tetra(tridecyl)-4,4'-n-butylidenebis(2- tert-butyl-5-methylphenol) diphosphite, hexa(tridecyl)-1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane triphosphite, tetrakis(2,4-ditert-butylphenyl) biphenylene diphosphonite, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, 2,2'-methylenebis(4,6-tert-butylphenyl)-2-ethylhexyl phosphite, 2 ,2'-methylenebis(4,6-tert-butylphenyl)-octadecyl phosphite, 2,2'-ethylidenebis(4,6-di-tert-butylphenyl)fluorophosphite, tris(2-[(2,4,8,10-tetrakis-tert-butyldibenzo[d,f][1,3,2]dioxaphosphepin-6-yl)oxy]ethyl)amine, phosphite of 2-ethyl-2-butylpropylene glycol and 2,4,6-tri-tert-butylphenol, etc. The amount of these phosphorus-based antioxidants to be added is preferably 0.001 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the synthetic resin.
[0161] Examples of thioether-based antioxidants include dialkylthiodipropionates such as dilauryl thiodipropionate, dimyristyl thiodipropionate, and distearyl thiodipropionate, and pentaerythritol tetra(β-alkylthiopropionic acid) esters. The amount of these thioether-based antioxidants added is preferably 0.001 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the synthetic resin.
[0162] Examples of the ultraviolet absorber include 2-hydroxybenzophenones such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 5,5'-methylenebis(2-hydroxy-4-methoxybenzophenone); 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, and 2-(2'-hydroxy-3',5'- 2-(2'-hydroxyphenyl)benzotriazoles such as 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-dicumylphenyl)benzotriazole, 2,2'-methylenebis(4-tert-octyl-6-(benzotriazolyl)phenol), 2-(2'-hydroxy-3'-tert-butyl-5'-carboxyphenyl)benzotriazole; phenyl Benzoates such as ricinate, resorcinol monobenzoate, 2,4-ditert-butylphenyl-3,5-ditert-butyl-4-hydroxybenzoate, 2,4-ditert-amylphenyl-3,5-ditert-butyl-4-hydroxybenzoate, hexadecyl-3,5-ditert-butyl-4-hydroxybenzoate; substituted oxanilides such as 2-ethyl-2'-ethoxyoxanilide, 2-ethoxy-4'-dodecyloxanilide; ethyl-α-cyano-β,β-diphenylacrylate, methyl and triaryl triazines such as 2-(2-hydroxy-4-octoxyphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine, 2-(2-hydroxy-4-methoxyphenyl)-4,6-diphenyl-s-triazine, and 2-(2-hydroxy-4-propoxy-5-methylphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine. The amount of these ultraviolet absorbers added is preferably 0.001 to 30 parts by mass, more preferably 0.05 to 10 parts by mass, relative to 100 parts by mass of the synthetic resin.
[0163] Examples of the hindered amine light stabilizer include 2,2,6,6-tetramethyl-4-piperidyl stearate, 1,2,2,6,6-pentamethyl-4-piperidyl stearate, 2,2,6,6-tetramethyl-4-piperidyl benzoate, bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1-octoxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)- 1,2,3,4-butane tetracarboxylate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butane tetracarboxylate, bis(2,2,6,6-tetramethyl-4-piperidyl)·bis(tridecyl)-1,2,3,4-butane tetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)·bis(tridecyl)-1,2,3,4-butane tetracarboxylate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)-2-butyl-2-(3,5-ditert-butyl) 1,2,2,6,6-Pentamethyl-4-piperidyl methacrylate, Poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}], 1,2,3,4-butanecarboxylic acid / 2,2-bis(hydroxymethyl)-1,3-propanediol / 3-hydroxy-2,2-dimethylpropanal / 1,2,2,6,6 -Pentamethyl-4-piperidinyl ester polycondensate, bis(1,2,2,6,6-pentamethyl-4-piperidyl) decanedioate / methyl 1,2,2,6,6-pentamethyl-4-piperidyl sebacate mixture, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, 1-(2-hydroxyethyl)-2,2,6,6-tetramethyl-4-piperidinol / diethyl succinate polycondensate, 1,6-bis(2,2,6,6-tetramethyl-4-piperidylamino)hexane / dibromoethane polycondensate, 1,6-bis(2,2,6,6-tetramethyl-4-piperidylamino)hexane / 2,4-dichloro-6-morpholino-s-triazine polycondensate, 1,6-bis(2,2,6,6-tetramethyl-4-piperidylamino)hexane / 2,4-dichloro-6-tert-octylamino-s-triazine polycondensate, 1,5,8,12-tetrakis[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidyl)amino)-s-triazine-6-yl]-1 ,5,8,12-Tetraazadodecane, 1,5,8,12-Tetrakis[2,4-bis(N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino)-s-triazin-6-yl]-1,5,8,12-tetraazadodecane, 1,6,11-Tris[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidyl)amino)-s-triazin-6-ylamino]undecane, 1,6,11-Tris[ 2,4-bis(N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidyl)amino)-s-triazin-6-ylamino]undecane, 3,9-bis[1,1-dimethyl-2-{tris(2,2,6,6-tetramethyl-4-piperidyloxycarbonyl)butylcarbonyloxy}ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane, 3,9-bis[1,1-dimethyl-2-{tris(1,2,2,6, Examples of the hindered amine compounds include bis(1-undecyloxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate, 2,2,6,6-tetramethyl-4-piperidylhexadecanoate, and 2,2,6,6-tetramethyl-4-piperidyloctadecanoate. The amount of these hindered amine light stabilizers added is preferably 0.001 to 30 parts by mass, and more preferably 0.05 to 10 parts by mass, relative to 100 parts by mass of the synthetic resin.
[0164] In addition, when a polyolefin resin is used as the synthetic resin, it is preferable to further add a known neutralizing agent to neutralize the residual catalyst in the polyolefin resin as necessary within a range that does not impair the effects of the present invention. Examples of the neutralizing agent include fatty acid metal salts such as calcium stearate, lithium stearate, and sodium stearate, and fatty acid amide compounds such as ethylene bis(stearamide), ethylene bis(12-hydroxystearamide), and stearic acid amide, and these neutralizing agents may be used in combination.
[0165] To the resin composition of the present invention, other additives may be further added, as necessary, within the scope of not impairing the effects of the present invention, such as nucleating agents such as metal salts of aromatic carboxylates, metal salts of alicyclic alkyl carboxylates, aluminum p-tert-butylbenzoate, aromatic metal salts of phosphates, and dibenzylidene sorbitols, metal soaps, hydrotalcites, triazine ring-containing compounds, metal hydroxides, phosphate-based flame retardants, condensed phosphate-based flame retardants, inorganic phosphorus-based flame retardants, (poly)phosphate-based flame retardants, halogen-based flame retardants, silicon-based flame retardants, antimony oxides such as antimony trioxide, other inorganic flame retardant assistants, other organic flame retardant assistants, fillers, pigments, lubricants, foaming agents, and the like.
[0166] Examples of triazine ring-containing compounds include melamine, ammeline, benzguanamine, acetoguanamine, phthalodiguanamine, melamine cyanurate, melamine pyrophosphate, butylenediguanamine, norbornenediguanamine, methylenediguanamine, ethylenedimelamine, trimethylenedimelamine, tetramethylenedimelamine, hexamethylenedimelamine, and 1,3-hexylenedimelamine.
[0167] Examples of metal hydroxides include magnesium hydroxide, aluminum hydroxide, calcium hydroxide, barium hydroxide, zinc hydroxide, and Kismer 5A (magnesium hydroxide: manufactured by Kyowa Chemical Industry Co., Ltd.).
[0168] Examples of the phosphate ester-based flame retardants include trimethyl phosphate, triethyl phosphate, tributyl phosphate, tributoxyethyl phosphate, trischloroethyl phosphate, trisdichloropropyl phosphate, triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, trixylenyl phosphate, octyl diphenyl phosphate, xylenyl diphenyl phosphate, trisisopropylphenyl phosphate, 2-ethylhexyl diphenyl phosphate, t-butylphenyl diphenyl phosphate, bis-(t-butylphenyl)phenyl phosphate, tris-(t-butylphenyl)phosphate, isopropylphenyl diphenyl phosphate, bis-(isopropylphenyl)diphenyl phosphate, and tris-(isopropylphenyl)phosphate.
[0169] Examples of the condensed phosphate ester flame retardant include 1,3-phenylene bis(diphenyl phosphate), 1,3-phenylene bis(dixylenyl phosphate), bisphenol A bis(diphenyl phosphate), and the like.
[0170] Examples of the (poly)phosphate-based flame retardant include ammonium salts and amine salts of (poly)phosphoric acids, such as ammonium polyphosphate, melamine polyphosphate, piperazine polyphosphate, melamine pyrophosphate, and piperazine pyrophosphate.
[0171] Examples of other inorganic flame retardant auxiliary agents include inorganic compounds such as titanium oxide, aluminum oxide, magnesium oxide, hydrotalcite, talc, and montmorillonite, and surface-treated products thereof, and various commercially available products such as TIPAQUE R-680 (titanium oxide: manufactured by Ishihara Sangyo Kaisha), Kyowamag 150 (magnesium oxide: manufactured by Kyowa Chemical Industry Co., Ltd.), DHT-4A (hydrotalcite: manufactured by Kyowa Chemical Industry Co., Ltd.), and Alcamizer 4 (zinc-modified hydrotalcite: manufactured by Kyowa Chemical Industry Co., Ltd.) can be used. Examples of other organic flame retardant auxiliary agents include pentaerythritol.
[0172] In addition, additives that are usually used in synthetic resins, such as crosslinking agents, anti-fogging agents, plate-out inhibitors, surface treatment agents, plasticizers, lubricants, flame retardants, fluorescent agents, anti-fungal agents, bactericides, foaming agents, metal deactivators, release agents, pigments, processing aids, antioxidants, light stabilizers, etc., may be blended into the resin composition of the present invention, as necessary, within a range that does not impair the effects of the present invention.
[0173] The additives to be blended in the resin composition of the present invention may be added directly to the synthetic resin, or may be blended in the antistatic agent or antistatic agent composition of the present invention and then added to the synthetic resin.
[0174] The resin composition of the present invention can be molded to obtain a resin molded product having antistatic properties. The molding method is not particularly limited, and examples thereof include extrusion processing, calendar processing, injection molding, rolling, compression molding, blow molding, and rotational molding, and molded products of various shapes such as resin plates, sheets, films, bottles, fibers, and irregular shapes can be produced.
[0175] The molded article obtained from the resin composition of the present invention has excellent antistatic properties and mechanical properties.
[0176] The resin composition of the present invention and molded articles using the same can be used in a wide range of industrial fields, including electricity, electronics, communications, agriculture, forestry, fisheries, mining, construction, food, textiles, clothing, medicine, coal, petroleum, rubber, leather, automobiles, precision instruments, wood, building materials, civil engineering, furniture, printing, and musical instruments.
[0177] More specifically, the resin composition of the present invention and its molded article are used in applications such as office and office automation equipment, such as printers, personal computers, word processors, keyboards, PDAs (personal digital assistants), telephones, copiers, facsimiles, ECRs (electronic cash registers), calculators, electronic organizers, cards, holders, and stationery; home appliances, such as washing machines, refrigerators, vacuum cleaners, microwave ovens, lighting equipment, game consoles, irons, and kotatsu; AV equipment, such as TVs, VTRs, video cameras, radio cassette players, tape recorders, minidiscs, CD players, speakers, and liquid crystal displays; electric and electronic parts and communication equipment, such as connectors, relays, capacitors, switches, printed circuit boards, coil bobbins, semiconductor encapsulating materials, LED encapsulating materials, electric wires, cables, transformers, deflection yokes, distribution boards, and clocks; interior and exterior materials for automobiles, plate-making films, adhesive films, bottles, food containers, food packaging films, plastic wrap films for pharmaceuticals and medicines, product packaging films, agricultural films, agricultural sheets, and greenhouse films.
[0178] Furthermore, the resin composition of the present invention and its molded article can be used in a wide variety of applications, including seats (padding, outer material, etc.), belts, ceiling coverings, convertible tops, armrests, door trims, rear package trays, carpets, mats, sun visors, wheel covers, mattress covers, airbags, insulation materials, handrails, handrail straps, wire covering materials, electrical insulation materials, paints, coating materials, covering materials, flooring materials, corner walls, carpets, wallpaper, wall covering materials, exterior materials, interior materials, roofing materials, deck materials, wall materials, pillars, etc. It can be used for a variety of purposes, including materials for automobiles, vehicles, ships, aircraft, buildings, houses, and construction materials such as lumber, flooring, fence materials, frames and moldings, window and door shapes, shingles, paneling, terraces, balconies, soundproofing boards, heat insulating boards, window materials, etc., as well as civil engineering materials, clothing, curtains, sheets, nonwoven fabrics, plywood, synthetic fiber boards, carpets, entrance mats, sheets, buckets, hoses, containers, glasses, bags, cases, goggles, skis, rackets, tents, musical instruments, and other daily necessities and sporting goods. EXAMPLES
[0179] The present invention will be described in more detail below using examples, but the present invention is not limited to these.
[0180] Polymer compound (E) was produced according to the following production example. In the following production example, the number average molecular weight of compound (b) was calculated by the following <Method for calculating number average molecular weight from hydroxyl value>, and the number average molecular weights of compounds other than compound (b) were calculated by the following <Method for measuring number average molecular weight in terms of polystyrene>.
[0181] <Calculation method of number average molecular weight from hydroxyl value> The hydroxyl value was measured by the following hydroxyl value measurement method, and the number average molecular weight (hereinafter also referred to as "Mn") was determined by the following formula. Number average molecular weight = (56110 x 2) / hydroxyl value <Hydroxyl value measurement method> Reagent A (acetylating agent) (1) Triethyl phosphate 1560mL (2) Acetic anhydride, 193 mL (3) Perchloric acid (60%) 16g Mix the above reagents in the order of (1) → (2) → (3). Reagent B Mix pyridine and pure water in a volume ratio of 3:1. Reagent C Add 2 to 3 drops of phenolphthalein solution to 500 mL of isopropyl alcohol and neutralize with 1N KOH aqueous solution.
[0182] First, weigh out 2 g of sample into a 200 mL Erlenmeyer flask, add 10 mL of triethyl phosphate, and heat to dissolve. Add 15 mL of Reagent A, plug with a stopper, and shake vigorously. Add 20 mL of Reagent B, plug with a stopper, and shake vigorously. Add 50 mL of Reagent C. Titrate with 1N KOH aqueous solution and calculate using the formula below.
[0183] Hydroxyl value [mgKOH / g] = 56.11 × f × (TB) / S f: Factor of 1N-KOH solution B: Blank test titration volume [mL] T: Test titer [mL] S: Sample amount [g]
[0184] <Method for measuring number average molecular weight based on polystyrene conversion> The number average molecular weight was measured by gel permeation chromatography under the following conditions: Equipment: GPC equipment manufactured by JASCO Corporation Solvent: Chloroform Reference material: Polystyrene Detector: Differential refractometer (RI detector) Column stationary phase: Showa Denko Co., Ltd. Shodex LF-804 Column temperature: 40℃ Sample concentration: 1mg / 1mL Flow rate: 0.5mL / min. Injection volume: 100μL
[0185] [Production Example 1] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 95:5 (mass ratio) A separable flask was charged with 401 g of 1,4-benzenedicarboxylic acid dimethyl ester, 21 g of 1,3-benzenedicarboxylic acid dimethyl ester, 230 g of 1,4-butanediol, and 0.5 g of tetraisopropoxy titanate, and the mixture was heated gradually from 160°C to 190°C at normal pressure for 4 hours. Polymerization was then carried out at 210°C under reduced pressure for 1 hour to obtain polyester (A)-1 having hydroxyl groups at both ends. The number average molecular weight Mn of polyester (A)-1 was 2,880 in terms of polystyrene.
[0186] Next, 400 g of the obtained polyester (A)-1, 305 g of polyethylene glycol having a number average molecular weight of 3,300 as compound (b)-1 having hydroxyl groups at both ends, 0.5 g of an antioxidant (Adeka STAB AO-50), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 200°C for 4 hours under reduced pressure to obtain block polymer (C)-1 having a structure having hydroxyl groups at both ends. The number average molecular weight Mn of this block polymer (C)-1 was 15,000 in terms of polystyrene.
[0187] 1.3 g of glycerin (hydroxyl group amount: 0.04 mol) as a polyhydric alcohol compound (D)-1 was added to 300 g (terminal hydroxyl group amount: 0.04 mol) of the obtained block polymer (C)-1 having a structure with hydroxyl groups at both ends, and the mixture was polymerized under reduced pressure at 220°C for 2 hours to obtain an antistatic agent (E)-1 of the present invention.
[0188] [Production Example 2] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio) A separable flask was charged with 317 g of 1,4-benzenedicarboxylic acid dimethyl ester, 105 g of 1,3-benzenedicarboxylic acid dimethyl ester, 230 g of 1,4-butanediol, and 0.5 g of tetraisopropoxy titanate, and the mixture was heated gradually from 160°C to 190°C at normal pressure for 4 hours. The mixture was then polymerized at 210°C under reduced pressure for 1 hour to obtain polyester (A)-2 having hydroxyl groups at both ends. The number average molecular weight Mn of polyester (A)-2 was 2,880 in terms of polystyrene.
[0189] Next, 400 g of the obtained polyester (A)-2, 305 g of polyethylene glycol having a number average molecular weight of 3,300 as compound (b)-1 having hydroxyl groups at both ends, 0.5 g of an antioxidant (Adeka STAB AO-50), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 200°C for 4 hours under reduced pressure to obtain block polymer (C)-2 having a structure with hydroxyl groups at both ends. The number average molecular weight Mn of this block polymer (C)-2 was 15,000 in terms of polystyrene.
[0190] To 300 g (terminal hydroxyl group amount: 0.04 mol) of the obtained block polymer (C)-2 having a structure with hydroxyl groups at both ends, 1.3 g of glycerin (hydroxyl group amount: 0.04 mol) was added as a polyhydric alcohol compound (D)-1, and the mixture was polymerized under reduced pressure at 220°C for 2 hours, to obtain an antistatic agent (E)-2 of the present invention.
[0191] [Production Example 3] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 55:45 (mass ratio) A separable flask was charged with 232 g of 1,4-benzenedicarboxylic acid dimethyl ester, 190 g of 1,3-benzenedicarboxylic acid dimethyl ester, 230 g of 1,4-butanediol, and 0.5 g of tetraisopropoxy titanate, and the mixture was heated gradually from 160°C to 190°C at normal pressure for 4 hours. The mixture was then polymerized at 210°C under reduced pressure for 1 hour to obtain polyester (A)-3 having hydroxyl groups at both ends. The number average molecular weight Mn of polyester (A)-3 was 2,880 in terms of polystyrene.
[0192] Next, 400 g of the obtained polyester (A)-3, 305 g of polyethylene glycol having a number average molecular weight of 3,300 as compound (b)-1 having hydroxyl groups at both ends, 0.5 g of an antioxidant (Adeka STAB AO-50), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 200°C for 4 hours under reduced pressure to obtain block polymer (C)-3 having a structure having hydroxyl groups at both ends. The number average molecular weight Mn of this block polymer (C)-3 was 15,000 in terms of polystyrene.
[0193] 1.3 g of glycerin (hydroxyl group amount: 0.04 mol) as a polyhydric alcohol compound (D)-1 was added to 300 g (terminal hydroxyl group amount: 0.04 mol) of the obtained block polymer (C)-3 having a structure having hydroxyl groups at both ends, and the mixture was polymerized under reduced pressure at 220°C for 2 hours to obtain an antistatic agent (E)-3 of the present invention.
[0194] [Production Example 4] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio) To 300 g (terminal hydroxyl group amount: 0.04 mol) of the block polymer (C)-2 having a structure with hydroxyl groups at both ends shown in Production Example 2, 1.7 g of diglycerol (hydroxyl group amount: 0.04 mol) was added as the polyhydric alcohol compound (D)-2, and the mixture was polymerized under reduced pressure at 220° C. for 2 hours, to obtain an antistatic agent (E)-4 of the present invention.
[0195] [Production Example 5] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio) To 300 g (terminal hydroxyl group amount: 0.04 mol) of the block polymer (C)-2 having a structure with hydroxyl groups at both ends shown in Production Example 2, 1.4 g of pentaerythritol (hydroxyl group amount: 0.04 mol) was added as a polyhydric alcohol compound (D)-3, and the mixture was polymerized under reduced pressure at 220°C for 2 hours, to obtain an antistatic agent (E)-5 of the present invention.
[0196] [Production Example 6] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio)
[0197] To 300 g (terminal hydroxyl group amount: 0.04 mol) of the block polymer (C)-2 having a structure with hydroxyl groups at both ends shown in Production Example 2, 1.7 g of dipentaerythritol (hydroxyl group amount: 0.04 mol) was added as a polyhydric alcohol compound (D)-4, and the mixture was polymerized under reduced pressure at 220° C. for 2 hours, to obtain an antistatic agent (E)-6 of the present invention.
[0198] [Production Example 7] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio) To 300 g (terminal hydroxyl group amount: 0.04 mol) of the block polymer (C)-2 having a structure with hydroxyl groups at both ends shown in Production Example 2, 3.4 g of diglycerol (hydroxyl group amount: 0.08 mol) as a polyhydric alcohol compound (D)-1 was added, and the mixture was polymerized under reduced pressure at 220° C. for 3 hours, to obtain an antistatic agent (E)-7 of the present invention.
[0199] [Production Example 8] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio) 0.9 g of diglycerol (0.02 mol of hydroxyl group) as a polyhydric alcohol compound (D)-1 was added to 300 g (0.04 mol of terminal hydroxyl group) of the block polymer (C)-2 having a structure with hydroxyl groups at both ends shown in Production Example 2, and the mixture was polymerized under reduced pressure at 220°C for 3 hours, to obtain an antistatic agent (E)-8 of the present invention.
[0200] [Production Example 9] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio) A separable flask was charged with 294 g of 1,4-benzenedicarboxylic acid dimethyl ester, 98 g of 1,3-benzenedicarboxylic acid dimethyl ester, 138 g of 1,2-ethanediol, and 0.5 g of tetraisopropoxy titanate, and the mixture was heated gradually from 160°C to 190°C at normal pressure for 6 hours. The mixture was then polymerized at 210°C under reduced pressure for 1 hour to obtain polyester (A)-4 with hydroxyl groups at both ends. The number average molecular weight Mn of polyester (A)-4 was 2,750 in terms of polystyrene.
[0201] Next, 400 g of the obtained polyester (A)-4, 320 g of polyethylene glycol having a number average molecular weight of 3,300 as compound (b)-1 having hydroxyl groups at both ends, 0.5 g of an antioxidant (Adeka STAB AO-50), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 200°C for 4 hours under reduced pressure to obtain block polymer (C)-4 having a structure having hydroxyl groups at both ends. The number average molecular weight Mn of this block polymer (C)-4 was 14,500 in terms of polystyrene.
[0202] 1.3 g of glycerin (hydroxyl group amount: 0.04 mol) as a polyhydric alcohol compound (D)-1 was added to 300 g (terminal hydroxyl group amount: 0.04 mol) of the obtained block polymer (C)-4 having a structure having hydroxyl groups at both ends, and the mixture was polymerized under reduced pressure at 220°C for 4 hours to obtain an antistatic agent (E)-9 of the present invention.
[0203] [Production Example 10] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio) A separable flask was charged with 198 g of 1,4-benzenedicarboxylic acid dimethyl ester, 66 g of 1,3-benzenedicarboxylic acid dimethyl ester, 225 g of 1,4-cyclohexanedimethanol, and 0.5 g of tetraisopropoxy titanate, and the mixture was heated gradually from 160°C to 190°C at normal pressure for 3 hours. The mixture was then polymerized at 210°C under reduced pressure for 1 hour to obtain polyester (A)-5 having hydroxyl groups at both ends. The number average molecular weight Mn of polyester (A)-5 was 2,800 in terms of polystyrene.
[0204] Next, 400 g of the obtained polyester (A)-5, 314 g of polyethylene glycol having a number average molecular weight of 3,300 as compound (b)-1 having hydroxyl groups at both ends, 0.5 g of an antioxidant (Adeka STAB AO-50), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 200°C for 4 hours under reduced pressure to obtain block polymer (C)-5 having a structure with hydroxyl groups at both ends. The number average molecular weight Mn of this block polymer (C)-5 was 15,800 in terms of polystyrene.
[0205] 1.2 g of glycerin (hydroxyl group amount: 0.04 mol) as a polyhydric alcohol compound (D)-1 was added to 300 g (terminal hydroxyl group amount: 0.04 mol) of the obtained block polymer (C)-5 having a structure having hydroxyl groups at both ends, and the mixture was polymerized under reduced pressure at 220°C for 1 hour to obtain an antistatic agent (E)-10 of the present invention.
[0206] [Production Example 11] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio) A separable flask was charged with 306 g of 1,4-benzenedicarboxylic acid dimethyl ester, 102 g of 1,3-benzenedicarboxylic acid dimethyl ester, 246 g of 1,4-butanediol, and 0.5 g of tetraisopropoxy titanate, and the mixture was heated gradually from 160°C to 190°C at normal pressure for 4 hours. The mixture was then polymerized at 210°C under reduced pressure for 1 hour to obtain polyester (A)-6 having hydroxyl groups at both ends. The number average molecular weight Mn of polyester (A)-6 was 1,900 in terms of polystyrene.
[0207] Next, 400 g of the obtained polyester (A)-6, 239 g of polyethylene glycol having a number average molecular weight of 1,700 as compound (b)-2 having hydroxyl groups at both ends, 0.5 g of an antioxidant (Adeka STAB AO-50), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 200°C for 4 hours under reduced pressure to obtain block polymer (C)-6 having a structure with hydroxyl groups at both ends. The number average molecular weight Mn of this block polymer (C)-6 was 9,000 in terms of polystyrene.
[0208] To 300 g (terminal hydroxyl group amount: 0.07 mol) of the obtained block polymer (C)-6 having a structure having hydroxyl groups at both ends, 2.0 g of glycerin (hydroxyl group amount: 0.07 mol) as a polyhydric alcohol compound (D)-1 was added, and the mixture was polymerized under reduced pressure at 220°C for 2 hours, to obtain an antistatic agent (E)-11 of the present invention.
[0209] [Production Example 12] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 75:25 (mass ratio) A separable flask was charged with 281 g of 1,4-benzenedicarboxylic acid dimethyl ester, 94 g of 1,3-benzenedicarboxylic acid dimethyl ester, 164 g of 1,4-butanediol, and 0.5 g of tetraisopropoxy titanate, and the mixture was heated gradually from 160°C to 190°C at normal pressure for 4 hours. The mixture was then polymerized at 210°C under reduced pressure for 1 hour to obtain polyester (A)-7 having methyl ester groups at both ends. The number average molecular weight Mn of polyester (A)-7 was 2,900 in terms of polystyrene.
[0210] Next, 400 g of the obtained polyester (A)-7, 303 g of polyethylene glycol having a number average molecular weight of 3,300 as compound (b)-1 having hydroxyl groups at both ends, 0.5 g of an antioxidant (Adeka STAB AO-50), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 200°C for 4 hours under reduced pressure to obtain block polymer (C)-7 having a structure with methyl ester groups at both ends. The number average molecular weight Mn of this block polymer (C)-7 was 15,000 in terms of polystyrene.
[0211] To 300 g (terminal hydroxyl group amount: 0.04 mol) of the obtained block polymer (C)-7 having a structure having hydroxyl groups at both ends, 1.3 g of glycerin (hydroxyl group amount: 0.04 mol) as a polyhydric alcohol compound (D)-1 was added, and the mixture was polymerized under reduced pressure at 220°C for 2 hours, to obtain an antistatic agent (E)-12 of the present invention.
[0212] [Comparative Production Example 1] A separable flask was charged with 422 g of 1,4-benzenedicarboxylic acid dimethyl ester, 230 g of 1,4-butanediol, and 0.5 g of tetraisopropoxy titanate, and the mixture was heated gradually from 160°C to 190°C at normal pressure for 4 hours. The mixture was then polymerized at 210°C under reduced pressure for 1 hour to obtain comparative polyester-1 with hydroxyl groups at both ends. The number average molecular weight Mn of comparative polyester-1 was 2,880 in terms of polystyrene.
[0213] Next, 400 g of the obtained comparative polyester-1, 305 g of polyethylene glycol having a number average molecular weight of 3,300 as compound (b)-1 having hydroxyl groups at both ends, 0.5 g of an antioxidant (3-(3,5-di-tert-butyl-4-hydroxyphenyl) stearyl propionate; "ADEKA STAB AO-50" manufactured by ADEKA CORPORATION), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 200°C for 4 hours under reduced pressure to obtain a comparative block polymer-1 having a structure having hydroxyl groups at both ends. The number average molecular weight Mn of this comparative block polymer-1 was 15,000 in terms of polystyrene.
[0214] 1.3 g of glycerin (hydroxyl group amount: 0.04 mol) as polyhydric alcohol compound (D)-1 was added to 300 g (terminal hydroxyl group amount: 0.04 mol) of the obtained comparative block polymer-1 having a structure with hydroxyl groups at both ends, and the mixture was polymerized under reduced pressure at 220°C for 2 hours to obtain a comparative antistatic agent-1.
[0215] [Comparative Production Example 2] A separable flask was charged with 303 g of 1,4-cyclohexanedimethanol, 141 g of adipic acid, and 187 g of 1,3-benzenedicarboxylic acid dimethyl ester, and polymerized for 4 hours at normal pressure while gradually increasing the temperature from 160°C to 210°C. Then, 0.6 g of tetraisopropoxy titanate was charged, and polymerized for 3 hours at 210°C under reduced pressure to obtain comparative polyester-2 with hydroxyl groups at both ends. The number average molecular weight Mn of comparative polyester-2 was 2,800 in terms of polystyrene.
[0216] Next, 400 g of the obtained comparative polyester-2, 300 g of polyethylene glycol having a number average molecular weight of 3,300 as compound (b)-3 having hydroxyl groups at both ends, 0.5 g of an antioxidant (Adeka STAB AO-60), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 210°C for 7 hours under reduced pressure to obtain a comparative block polymer-2 having a structure with carboxyl groups at both ends. The number average molecular weight Mn of this comparative block polymer-2 having a structure with hydroxyl groups at both ends was 15,000 in terms of polystyrene.
[0217] To 300 g of the obtained comparative block polymer-2 (terminal hydroxyl group amount 0.04 mol) having a structure with hydroxyl groups at both ends, 1.3 g of glycerin (hydroxyl group amount 0.04 mol) was added as a polyhydric alcohol compound (D), and the mixture was polymerized under reduced pressure at 220°C for 6 hours to obtain a comparative antistatic agent-2.
[0218] [Comparative Production Example 3] 1,4-benzenedicarboxylic acid dimethyl ester: 1,3-benzenedicarboxylic acid dimethyl ester = 45:55 (mass ratio)
[0219] A separable flask was charged with 190g of 1,4-benzenedicarboxylic acid dimethyl ester, 232g of 1,3-benzenedicarboxylic acid dimethyl ester, 230g of 1,4-butanediol, and 0.5g of tetraisopropoxy titanate, and the mixture was heated gradually from 160°C to 190°C at normal pressure for 4 hours. The mixture was then polymerized at 210°C under reduced pressure for 1 hour to obtain comparative polyester-3 with hydroxyl groups at both ends. The number average molecular weight Mn of comparative polyester-3 was 2,880 in terms of polystyrene.
[0220] Next, 400 g of the obtained comparative polyester-3, 305 g of polyethylene glycol having a number average molecular weight of 3,300 as compound (b)-1 having hydroxyl groups at both ends, 0.5 g of an antioxidant (Adeka STAB AO-50), and 0.5 g of tetraisopropoxy titanate were charged and polymerized at 200°C for 4 hours under reduced pressure to obtain a comparative block polymer-3 having a structure having hydroxyl groups at both ends. The number average molecular weight Mn of this comparative block polymer-3 was 15,000 in terms of polystyrene.
[0221] 1.3 g of glycerin (hydroxyl group amount: 0.04 mol) as polyhydric alcohol compound (D)-1 was added to 300 g (terminal hydroxyl group amount: 0.04 mol) of the obtained comparative block polymer-3 having a structure with hydroxyl groups at both ends, and the mixture was polymerized under reduced pressure at 220°C for 2 hours to obtain a comparative antistatic agent-3.
[0222] [Examples 1 to 34, Comparative Examples 1 to 14] Using the resin compositions of each of the Examples and Comparative Examples blended based on the compounding amounts (parts by mass) shown in Tables 1 to 8 below, test pieces for surface resistivity and test pieces for physical property measurement were obtained according to the test piece preparation conditions shown below. Using the test pieces for surface resistivity obtained, the surface resistivity (SR value) was measured according to the following, and antistatic properties and their durability were evaluated. Furthermore, the test pieces for physical property measurement obtained were used to measure the flexural modulus and Charpy impact strength as mechanical properties. The respective results are shown in Tables 1 to 8.
[0223] <ABS Resin Composition Test Specimen Preparation Conditions> The antistatic resin composition blended based on the compounding amounts shown in the following table was granulated using a twin-screw extruder (PCM30 with 60 mesh) manufactured by Ikegai Corporation at 230°C and a rate of 6 kg / hour to obtain pellets. The obtained pellets were molded using a horizontal injection molding machine (NEX80: manufactured by Nissei Plastic Industrial Co., Ltd.) under processing conditions of a resin temperature of 230°C and a mold temperature of 50°C to obtain test specimens for surface resistivity (100 mm × 100 mm × 3 mm) and test specimens for physical property measurement (80 mm × 10 mm × 4 mm).
[0224] <Surface Resistivity (SR Value)> The obtained test specimens were stored immediately after molding processing under conditions of a temperature of 25°C and a humidity of 50%RH. After 1 day and 30 days of storage after molding processing, the surface resistivity (Ω / □) was measured under the same atmosphere using an R8340 resistance meter manufactured by Advantest Corporation under conditions of an applied voltage of 100V and an applied time of 1 minute. The measurement was performed at 5 points for each of the 5 test specimens, and the average value was obtained.
[0225] <Water Resistance to Wiping> After the surface of the obtained test specimen was wiped 50 times with a wet wipe in running water, it was stored for 2 hours under conditions of a temperature of 25°C and a humidity of 50%. Then, under the same atmosphere, the surface specific resistance value (Ω / □) was measured using an R8340 resistance meter manufactured by Advantest Corporation under conditions of an applied voltage of 100V and an applied time of 1 minute. The measurement was performed at 5 points, and the average value was obtained.
[0226] <Flexural Modulus> Measured in accordance with ISO178.
[0227] <Charpy Impact Strength> Measured in accordance with ISO179-1 (notched).
[0228] <ABS Resin> Resin - 1: Product name GA - 101 manufactured by Japan A & L Co., Ltd. (ABS resin manufactured by suspension polymerization method with MFR 23) Resin-2: Versalis SpA Product name F332 (MFR14, ABS resin produced by bulk polymerization method)
[0229] [Table 1] *1: Nippon A&L Co., Ltd. Product name: GA-101 (ABS resin manufactured by suspension polymerization method) Melt flow rate = 23g / 10min (ISO1133, 220℃ x 10.00kg) *2: Versalis SpA product name F332 (ABS resin manufactured by bulk polymerization method) Melt flow rate = 14g / 10min (ISO1133, 220℃ x 10.00kg) *3: Sodium dodecylbenzenesulfonate *4: Polyether ester amide antistatic agent (BASF, product name Irgastat P-20) *5: Blocking occurred during the processing of the test specimen, making it impossible to evaluate, and handling was poor.
[0230] [Table 2]
[0231] [Table 3]
[0232] [Table 4]
[0233] [Table 5]
[0234] [Table 6]
[0235] [Table 7]
[0236] [Table 8]
[0237] It can be seen from Tables 1 to 8 that by using the antistatic agent of the present invention, it is possible to impart sustained antistatic performance to a resin without impairing the inherent physical properties of the resin and while maintaining good handling properties.
Claims
1. An antistatic agent comprising at least one polymer compound (E) obtained by a condensation reaction of an aliphatic diol (a1) having 2 to 12 carbon atoms, a dicarboxylic acid derivative (a2), a compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends, and a polyhydric alcohol compound (D) having three or more hydroxyl groups, the dicarboxylic acid derivative (a2) is a mixture of a 1,4-benzenedicarboxylic acid derivative and a 1,3-benzenedicarboxylic acid derivative, and the mixing ratio of the 1,4-benzenedicarboxylic acid derivative: the 1,3-benzenedicarboxylic acid derivative is within a range of 50:50 to 95:5 in terms of mass ratio; the polymer compound (E) is a polymer compound obtained by a condensation reaction of a polyester (a) obtained by reacting the aliphatic diol (a1) having 2 to 12 carbon atoms with a dicarboxylic acid derivative (a2), a compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends, and a polyhydric alcohol compound (D); the polymer compound (E) has a polyester block (A) constituted by the polyester (a) and a polyether block (B) constituted by the compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends, An antistatic agent characterized by having a structure formed by a condensation reaction between a hydroxyl group or an alkyl ester group at the end of the polyester (a), a hydroxyl group at the end of a compound (b) which has one or more ethyleneoxy groups and has hydroxyl groups at both ends, and a hydroxyl group of the polyhydric alcohol compound (D), which are bonded via an ester bond.
2. 2. The antistatic agent according to claim 1, wherein the polymer compound (E) has a structure in which a block polymer (C) having a hydroxyl group or an alkyl ester group at both ends, which block polymer (C) is formed by repeatedly and alternately bonding a block (A) of the polyester (a) and a block (B) of the polyether via ester bonds, and the block polymer (C) is bonded to the polyhydric alcohol compound (D) via ester bonds.
3. 3. The antistatic agent according to claim 1, wherein the dicarboxylic acid derivative (a2) of the polymer compound (E) is a mixture of a 1,4-benzenedicarboxylic acid dialkyl ester and a 1,3-benzenedicarboxylic acid dialkyl ester.
4. 3. The antistatic agent according to claim 1, wherein the dicarboxylic acid derivative (a2) of the polymer compound (E) is a mixture of 1,4-benzenedicarboxylic acid dimethyl ester and 1,3-benzenedicarboxylic acid dimethyl ester.
5. The antistatic agent according to any one of claims 1 to 4, wherein the aliphatic diol (a1) having 2 to 12 carbon atoms in the polymer compound (E) is at least one of 1,2-ethanediol and 1,4-butanediol.
6. 6. The antistatic agent according to claim 1, wherein the compound (b) having one or more ethyleneoxy groups and hydroxyl groups at both ends of the polymer compound (E) is polyethylene glycol.
7. The antistatic agent according to any one of claims 2 to 6, wherein the polyester (a) has a number average molecular weight of 1,000 to 8,000 in terms of polystyrene, the compound (b) having one or more ethyleneoxy groups and having hydroxyl groups at both ends has a number average molecular weight of 1,000 to 6,000 in terms of polystyrene, and the block polymer (C) has a number average molecular weight of 5,000 to 30,000 in terms of polystyrene.
8. 8. An antistatic agent composition comprising the antistatic agent according to claim 1 further comprising at least one salt of an aromatic sulfonic acid.
9. 8. An antistatic resin composition comprising a synthetic resin and the antistatic agent according to claim 1 blended therewith.
10. 10. The antistatic resin composition according to claim 9, wherein the synthetic resin comprises at least one resin selected from the group consisting of polystyrene resins and copolymers thereof.
11. 11. The antistatic resin composition according to claim 9, wherein a mass ratio of the synthetic resin to the antistatic agent is in the range of 99 / 1 to 40 / 60.
12. 9. An antistatic resin composition comprising a synthetic resin and the antistatic agent composition according to claim 8 blended therewith.
13. 13. The antistatic resin composition according to claim 12, wherein the synthetic resin comprises at least one resin selected from the group consisting of polystyrene-based resins and copolymers thereof.
14. 14. The antistatic resin composition according to claim 12, wherein a mass ratio of the synthetic resin to the antistatic agent composition is in the range of 99 / 1 to 40 / 60.
15. A molded article comprising the antistatic resin composition according to any one of claims 9 to 14.
Citation Information
Patent Citations
Sheet or web carrying antistatic layer
JP1987280287A
Antistatic agent
JP1999148072A
Antistatic agent and antistatic resin composition
JP2000336346A
Block polymer and destaticizing agent containing the same
JP2002080600A
Antistatic resin composition and its shaped article
JP2004217929A