Silica particles, their uses, and method for producing silica particles

Silica particles with internal voids and specific properties address the issue of insufficient hiding and safety in cosmetics, offering lightweight, safe, and effective concealment through enhanced light scattering.

JP7575266B2Active Publication Date: 2024-10-29AGC INC +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020217167
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-25
Publication Date
2024-10-29
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

Conventional silica particles used in cosmetics lack sufficient hiding properties and are not highly safe, as they are dense and may have photocatalytic effects, making them undesirable for skin contact.

Method used

Silica particles with multiple voids having a major axis length of 200 nm or more and 3 μm or less, a pore volume of less than 2.0 cm³/g, and a specific surface area of 1 m²/g or more are produced, featuring a hydrophilic surface and spherical shape, enhancing light scattering and concealment properties.

Benefits of technology

The silica particles achieve reduced apparent density, improved light scattering, and high concealment properties, making them suitable for cosmetics while being safe for skin contact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575266000002
    Figure 0007575266000002
  • Figure 0007575266000003
    Figure 0007575266000003
  • Figure 0007575266000001
    Figure 0007575266000001
Patent Text Reader

Abstract

To provide a novel silica powder having high safety, small apparent density and high concealing property.SOLUTION: A silica powder contains a plurality of voids having a length of a long axis of 200 nm or more and 3 μm or less inside the powder, and a value of {oil absorption amount (cm3 / 100 g) / 100} / pore volume (cm3 / g) is 1.5 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to silica particles, uses thereof, and a method for producing silica particles. [Background technology]

[0002] Particulate silica is used in various fields as a catalyst, a desiccant, an abrasive, and also as a raw material for resin fillers and cosmetics, etc. Types of silica particles include silica having continuous micropores in a mesh pattern inside each particle (porous silica), silica having a structure with one hollow part inside each particle (hollow silica), and silica having substantially no voids inside the particle (solid silica), and are used differently depending on the application.

[0003] For example, Patent Document 1 proposes a spherical metal oxide powder with excellent heat insulation and reduced bulk density, and describes its use as a core material for vacuum insulation materials, various filling applications, additive applications, cosmetic applications, etc. Patent Document 1 cites silica as an example of the metal oxide, and describes a metal oxide powder that is mainly composed of spherical independent particles and has a specific surface area of ​​400 m2 as measured by the BET method. 2 / g or more 1000m 2 / g or less, a pore volume according to the BJH method of 2 mL / g to 8 mL / g, and an oil absorption of 250 mL / 100 g or more.

[0004] Patent Document 2 proposes a method for producing hollow particles made of a dense silica shell, and the dense silica hollow particles have a diameter of 15 to 800 m. 2 It is described that the silica has a BET specific surface area of ​​about 1 / g, a DOP oil absorption of 500 ml or more per 100 g of silica, and a shell thickness of about 2 to 10 nm. Patent Document 2 describes that such hollow dense silica particles can be used as hollow fillers or absorbents.

[0005] In addition, Patent Document 3 describes a method for producing spherical porous inorganic particles capable of reflecting light in the visible light region, and describes the production of porous inorganic particles having macropores of 50 nm or more. Patent Document 3 also describes that the porous inorganic particles can be applied to various fields such as photonic crystals, UV reflecting materials, and CO2 adsorption materials. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2012 / 147812 [Patent Document 2] Special Publication No. 2000-500113 [Patent Document 3] Special Publication No. 2020-525375 Summary of the Invention [Problem to be solved by the invention]

[0007] One of the required properties of inorganic white pigments used in cosmetics is the ability to hide the base. In recent years, in order to improve the texture of the skin, there has been a demand for inorganic white pigments that are pleasant to the touch, highly safe, and have high hiding power. Titanium dioxide, known as an inorganic white pigment with high hiding power, has drawbacks such as an unpleasant feel due to its large particle density and weight, a possible carcinogen, and concerns that it may damage the skin surface due to its photocatalytic properties.

[0008] In contrast, silica particles are expected to be used in cosmetics because their particle size and density can be adjusted and they are highly safe. However, conventional silica particles do not provide sufficient hiding power for the base, and further improvement is needed.

[0009] Therefore, an object of the present invention is to provide novel silica particles which are highly safe, have a small apparent density, and further have high hiding power. [Means for solving the problem]

[0010] The inventors conducted research in light of the above problems and discovered that the above problems could be solved by providing silica particles containing multiple voids with a major axis length of 200 nm or more inside the particles, thereby completing the present invention.

[0011] The present invention relates to the following <1> ~ <12> This is regarding. <1> The particles contain multiple voids with a major axis length of 200 nm to 3 μm, and the oil absorption capacity (cm 3 / 100g) / 100} / pore volume (cm 3 / g) is 1.5 or more. <2> The average circularity is 0.80 or more. <1> The silica particles according to claim 1. <3> The surface is hydrophilic. <1> or <2> The silica particles according to claim 1. <4> The 50% particle size (D 50 ) is 3 to 500 μm. <1> ~ <3> 13. Silica particles according to any one of claims 1 to 12. <5> The pore volume is 2.0 cm 3 / g or less. <1> ~ <4> 13. Silica particles according to any one of claims 1 to 12. <6> The particle strength is 1 MPa or more. <1> ~ <5> 13. Silica particles according to any one of claims 1 to 12. <7> The silica particles are * a * b * In color space, a * When a reddish brown iron (III) oxide powder having a value of 14 to 15 is mixed in a ratio of 30 mass% to obtain a mixed powder, * The value is 6.0 or less. <1> ~ <6> 13. Silica particles according to any one of claims 1 to 12. <8> The above <1> ~ <7> 13. A white pigment comprising the silica particles according to any one of claims 1 to 12. <9> The above <1> ~ <7> A cosmetic comprising the silica particles according to any one of the above. <10> A method for producing silica particles, comprising: forming droplets of an aqueous sodium silicate solution containing template particles, precipitating silica, removing the template particles, and washing and drying the silica from which the template particles have been removed. <11> A method for producing silica particles, comprising the steps of mixing template particles in an aqueous sodium silicate solution to form a dispersed phase, and an organic phase containing a surfactant to form a continuous phase, mixing the dispersed phase and the continuous phase and stirring to emulsify, obtaining an emulsion in which the dispersed phase is converted into droplets, gelling the emulsion to obtain a silica slurry containing silica encapsulating the template particles, adding an acid to the silica slurry to remove the template particles, and washing and drying the silica from which the template particles have been removed. <12> The template particles are at least one selected from the group consisting of magnesium hydroxide, magnesium carbonate, calcium hydroxide, and calcium carbonate. <10> or <11> The method for producing silica particles according to claim 1. Effect of the Invention

[0012] The silica particles of the present invention contain a plurality of voids with a major axis length of 200 nm to 3 μm inside the particles, resulting in a small apparent density and making the particles light. In addition, the scattering surface of light in the visible light region (400 to 800 nm) increases, improving the scattering of the particles, resulting in particles with high concealing properties. In addition, since the particles are made of silica, they are highly safe. Therefore, they can be suitably used in cosmetics, and when used in cosmetics, they have high concealing properties for the foundation and excellent concealing power for the skin. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 shows a scanning electron microscope image (SEM image) of a cut cross section of the silica particles obtained in Example 4. [Diagram 2] FIG. 2 shows a scanning electron microscope image (SEM image) of the silica particles obtained in Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described below, but the present invention is not limited to the examples in the following description.

[0015] <Silica particles> The silica particles of the present invention contain a plurality of voids with a major axis length of 200 nm or more and 3 μm or less inside the particles, and have an oil absorption capacity (cm 3 / 100g) / 100} / pore volume (cm 3 / g) is 1.5 or more. The presence of voids inside the silica particles can be confirmed, for example, by observing the cross section of the particles with a scanning electron microscope (SEM).

[0016] The length of the major axis of the voids can be found, for example, by photographing a cut surface of a silica particle with an SEM and measuring the longest distance between the openings of the voids in the SEM photograph.

[0017] The silica particles of the present invention contain a plurality of voids with a major axis length of 200 nm or more and 3 μm or less. Visible light is diffused at the interface between silica and air, so if there are voids inside the silica particles, the light is more likely to be scattered, but if the voids are too small, light scattering does not occur. By including voids with a major axis length of 200 nm or more, light scattering can be caused. In addition, taking into consideration the size of silica particles that can be manufactured, the major axis length is set to 3 μm or less. The length of the major axis of the void inside the particle is 200 nm or more, preferably 300 nm or more, and more preferably 400 nm or more, and is 3 μm or less, preferably 2 μm or less, and more preferably 1 μm or less.

[0018] Visible light is scattered at the interface between silica and air, so the more interfaces there are, the more visible light can be scattered, improving concealment. Therefore, by having multiple voids with a major axis length of 200 nm to 3 μm inside the silica particles, the scattering of visible light is improved. The number of voids with a major axis length of 200 nm or more and 3 μm or less needs to be two or more within one particle, and can be appropriately adjusted depending on the size of the silica particle (particle size) and the size of the voids (major axis length).

[0019] In the present invention, the pore volume of the silica particles is 2.0 cm 3 / g or less is preferable. Here, the pore volume means the pore volume derived from pores with a pore diameter of 1 to 100 nm. The apparent particle density is reduced by having pores (voids) with a pore diameter of 1 to 100 nm around voids with a major axis length of 200 nm or more and 3 μm or less. In other words, the silica particles become lighter and have an improved feel, and even if liquid is absorbed, the air phase of the large voids is maintained, so hiding power can be maintained. If the pore volume is too large, the particle strength may decrease, limiting applications, so a pore volume of 2.0 cm or less is preferable. 3 It is preferable that the molecular weight is less than 1 / g. The pore volume is 1.9 cm 3 / g or less is more preferable, and 1.8 cm 3 / g or less is more preferable, and 1.7 cm 3 The lower limit of the pore volume of the silica particles is not particularly limited, but when the silica particles are unsintered, it is preferably 0.9 cm 3 / g or more, and 0.95 cm 3 / g or more is more preferable, and 1.0 cm 3 / g or more is more preferable.

[0020] When the silica particles are sintered, the pores (voids) with a diameter of 1 to 100 nm are shrunk by sintering to reduce the pore volume to 0.3 cm 3 When the number of pores is small, liquid is less likely to penetrate into voids having a major axis length of 200 nm or more and 3 μm or less, and the lightness and hiding power of the silica particles can be maintained.

[0021] The pore volume can be calculated by the nitrogen adsorption method using the BJH method.

[0022] Silica particles have an oil absorption of 30 to 500 cm 3 / 100g. The oil absorption is preferably 30cm 3 When the particle size is 100g or more, the apparent density can be reduced to make the particles lighter. Even if the particle absorbs a small amount of sebum, the particle can maintain high hiding power, making it suitable for use in cosmetics. The oil absorption capacity is 500cm or more.3 If the particle size is less than 100g, high particle strength can be maintained. Oil absorption capacity is 50cm 3 / 100g or more is more preferable, and 100cm 3 / 100g or more is more preferable, 250cm 3 / 100g or more is particularly preferable, and 450cm 3 / 100g or less is more preferable, and 400cm 3 / 100g or less is more preferable, 350cm 3 / 100g or less is particularly preferred.

[0023] Oil absorption can be measured according to JIS K 5101. Specifically, boiled linseed oil is added to the sample while kneading until the entire sample becomes one lump. The oil absorption is expressed as the volume of boiled linseed oil per 100 g of sample when the entire sample becomes one lump. Hereinafter, the oil absorption measured by this method is simply called the oil absorption.

[0024] In the present invention, {oil absorption (cm 3 / 100g) / 100} / pore volume (cm 3 The oil absorption relative to the pore volume per 1 g of silica particles, expressed as (oil absorption / 100) / g (hereinafter referred to as "(oil absorption / 100) / pore volume"), is 1.5 or more. A ratio of (oil absorption / 100) to pore volume greater than 1 indicates that there are many voids inside the particles that can scatter visible light. When the (oil absorption / 100) / pore volume value is 1.5 or more, this indicates that there are particularly many voids inside the particles that can scatter visible light, so that there is more scattering of visible light on the particle surface, and sufficient hiding power can be obtained. The value of (oil absorption / 100) / pore volume is 1.5 or more, preferably 1.6 or more, more preferably 2.0 or more, and is not particularly limited as long as it does not affect the particle strength, but is preferably 500 or less.

[0025] The silica particles of the present invention have a specific surface area of ​​1 m2 as determined by the nitrogen adsorption method. 2 / g or more. 2When the SiO2 content is 1 / g or more, the active sites can be increased when the SiO2 content is used as a catalyst support. The specific surface area is 10m 2 / g or more is more preferable, and 50m 2 / g or more is more preferable, and 100m 2 / g or more is particularly preferred, and there is no particular upper limit.

[0026] The specific surface area can be calculated using the BET theory after obtaining an adsorption isotherm by a nitrogen adsorption method.

[0027] The shape of the silica particles of the present invention is not particularly limited, but is preferably spherical. If the silica particles are spherical, they can provide a smooth feeling of use when they come into contact with the skin, making them suitable for use in cosmetics. In addition, in catalyst carrier applications, particularly catalyst carrier applications for polyolefin production, polymer particles of the same shape as the catalyst carrier are generated, so spherical particles are required. Furthermore, spherical particles are also preferred in terms of packing properties.

[0028] The silica particles of the present invention preferably have an average circularity of 0.80 or more. When the average circularity is 0.80 or more, the particle shape becomes close to a sphere, and therefore the particles can be suitably used for various applications. The average circularity of the silica particles is more preferably 0.90 or more, and even more preferably 0.95 or more. There is no particular upper limit to the circularity, and it is most preferably 1.

[0029] The circularity can be calculated by determining the area and perimeter of a particle from an image obtained by a particle image analyzer (e.g., Morphologi4 manufactured by Malvern Instruments) using image analysis software attached to the device, and applying the results to the following formula: The average circularity is the average value of 30,000 particles. Circularity = perimeter of a circle with equal projected area / perimeter of a particle Circumference of a circle with the same projected area: When a particle is observed from directly above, the area of ​​the particle's shadow projected on the plane below is calculated, and a circle with an area equal to this area is calculated, and the length of the contour of that circle is calculated. Particle perimeter: The length of the outline of the particle's shadow projected on a flat surface when the particle is observed from directly above

[0030] The 50% particle size (D 50 In order to obtain the silica particles of the present invention, the 50% particle diameter (D 50 Silica particles with a 50% particle diameter (D ) of less than 3 μm are difficult to manufacture, and those with a diameter of more than 500 μm have limited uses. For example, when used in cosmetics, the particles are too large and may cause a poor feeling when used, so a diameter of 500 μm or less is preferable. 50 ) is preferably within the above range since it can be used for applications in various fields. 50% particle size (D 50 ) is more preferably 5 μm or more, even more preferably 10 μm or more, and particularly preferably 20 μm or more, and is more preferably 300 μm or less, even more preferably 100 μm or less, and particularly preferably 50 μm or less.

[0031] The 50% particle size (D 50 ) can be calculated as a 50% volume equivalent particle diameter by measuring 30,000 particles with a circularity of 0.90 or more using a particle image analyzer (for example, Morphologi4 manufactured by Malvern Instruments).

[0032] The silica particles of the present invention preferably have a particle strength of 1 MPa or more. When the particle strength is 1 MPa or more, the particles have a strength that makes them less likely to collapse, and therefore can be used in a variety of applications. The particle strength is more preferably 1.5 MPa or more, further preferably 2.0 MPa or more, and particularly preferably 2.5 MPa or more, with no particular upper limit.

[0033] The strength of the silica particles can be measured using a microcompression tester (for example, MCT-510, manufactured by Shimadzu Corporation). In the present invention, the particle strength is determined by measuring the compressive strength of 40 silica particles and averaging the results.

[0034] The silica particles of the present invention preferably have a hydrophilic particle surface. If the particle surface is hydrophilic, the silica particles contain little or no organic components, and therefore have no adverse effect on the environment and can be used in various fields.

[0035] The hydrophilicity of the particle surface can be confirmed by a dispersion test in water. For example, 5 g of silica particle powder is added to 100 g of water, and after uniform stirring, the mixture is left to stand for 24 hours. If more than 90% of the silica particles are submerged in the water after 24 hours, the silica particles are deemed to be hydrophilic. The percentage of the submerged silica particles is calculated from the mass of the silica particles obtained by collecting and drying the sedimented particles after standing for 24 hours.

[0036] In addition, the silica particles of the present invention have L * a * b * In color space, a * When a reddish brown iron (III) oxide powder (e.g., special grade, manufactured by Kanto Chemical Co., Ltd.) having a value of 14 to 15 is mixed in a ratio of 30 mass% to obtain a mixed powder, * It is preferable that the value is 6.0 or less. * a * b * The color system was standardized by the International Commission on Illumination (CIE) in 1976.

[0037] The above measurement method can evaluate the shielding ability of silica particles. * A value of 6.0 or less can be evaluated as having high light scattering properties and excellent shielding power. The above a * The value is more preferably 5.0 or less, even more preferably 4.5 or less, and particularly preferably 4.0 or less. * Since a smaller value is more preferable, the lower limit is preferably 0.

[0038] In addition, the powder a *The value can be measured, for example, using a spectrophotometer (for example, SE7700 manufactured by Nippon Denshoku Industries Co., Ltd.) In the measurement using a spectrophotometer, the mixed powder is poured to a thickness of 7.5 mm or more and then the measurement is performed.

[0039] <Method of manufacturing silica particles> The silica particles of the present invention can be obtained by forming an aqueous sodium silicate solution containing template particles into droplets, precipitating silica to produce spherical silica particles containing the template particles, and then removing the template particles from the resulting spherical silica particles containing the template particles. For example, the following method is used.

[0040] A first method for producing silica particles of the present invention includes the steps of mixing a mixture obtained by mixing template particles in an aqueous sodium silicate solution as a dispersed phase and an organic phase containing a surfactant as a continuous phase, mixing the dispersed phase and the continuous phase and emulsifying by stirring to obtain an emulsion in which the dispersed phase is converted into droplets (step (1-1)), gelling the emulsion to precipitate silica, and obtaining a silica slurry containing spherical silica encapsulating the template particles (step (1-2)), adding an acid to the silica slurry to remove the template particles (step (1-3)), and washing and drying the silica from which the template particles have been removed (step (1-4)).

[0041] The second manufacturing method includes spraying a mixed liquid of an aqueous sodium silicate solution containing template particles and an acid for a short time before silica is precipitated, forming droplets in the air, and then precipitating the silica to obtain spherical silica containing the template particles (step (2-1)), removing the template particles from the silica containing the template particles (step (2-2)), and washing and drying the silica from which the template particles have been removed (step (2-3)).

[0042] (First manufacturing method) In step (1-1) of the first manufacturing method, a mixture of template particles and a sodium silicate aqueous solution is used as a dispersed phase, and an organic phase containing a surfactant is used as a continuous phase. The dispersed phase and the continuous phase are mixed and stirred to obtain an emulsion. A water-in-oil (W / O) emulsion is obtained by emulsifying the dispersed and continuous phases with stirring. The dispersed phase breaks into droplets in the continuous phase, and the droplets become droplets of sodium silicate aqueous solution with the template particles present inside.

[0043] The template particles used in the dispersed phase are a material that does not dissolve in an aqueous sodium silicate solution but dissolves in an acid. Examples of template particles include magnesium hydroxide, magnesium carbonate, calcium hydroxide, calcium carbonate, etc., and these may be used alone or in combination of two or more. Among them, at least one selected from the group consisting of magnesium hydroxide and magnesium carbonate is preferred from the viewpoint of being able to dissolve and remove the template particles using sulfuric acid. Sulfuric acid is a non-volatile acid, and is preferred from the viewpoint of safety and equipment protection compared to volatile acids such as hydrochloric acid, nitric acid, and hydrofluoric acid.

[0044] The size of the template particles affects the size of the voids inside the resulting silica particles, so template particles of a desired size may be used. 50 It is preferable to use template particles having a particle size in the range of 200 nm to 3 μm, more preferably 300 nm to 2 μm, and even more preferably 400 nm to 1 μm.

[0045] The sodium silicate aqueous solution preferably has a silicic acid component in a range of 3 to 35 mass % in terms of SiO2 concentration. The silicic acid component in the sodium silicate aqueous solution is mainly contained in the form of SiO2, so it is expressed as a SiO2 concentration converted to SiO2. When the concentration of the silicic acid component in the aqueous sodium silicate solution is within the above range, silica particles can be produced with high production efficiency. The concentration of the silicic acid component in the aqueous sodium silicate solution is more preferably 5% by mass or more, even more preferably 7% by mass or more, and particularly preferably 10% by mass or more, from the viewpoint of high productivity and obtaining particles with high sphericity. Also, from the viewpoint of easily obtaining particles with a small particle size, the concentration is more preferably 30% by mass or less, even more preferably 25% by mass or less, and particularly preferably 20% by mass or less.

[0046] The ratio of silicic acid to sodium in the sodium silicate aqueous solution is preferably SiO2 / Na2O (molar ratio) of 2 to 4. Aqueous sodium silicate solutions having a SiO2 / Na2O (molar ratio) in the above range are easily available, and examples thereof include No. 3 sodium silicate (manufactured by AGC Si-Tech Co., Ltd., SiO2 / Na2O=3), No. 2 sodium silicate (manufactured by AGC Si-Tech Co., Ltd., SiO2 / Na2O=2.5), No. 1 sodium silicate (manufactured by AGC Si-Tech Co., Ltd., SiO2 / Na2O=2), and the like.

[0047] The template particles are preferably mixed in the sodium silicate aqueous solution in the range of 1 to 35% by mass. If the amount of template particles used is too small, each particle may not contain multiple voids with a major axis length of 200 nm to 3 μm, while if the amount is too large, the number of voids inside the silica particles may become too large, resulting in a decrease in particle strength. The amount of the template particles used in the aqueous sodium silicate solution is more preferably 5 to 33% by mass, further preferably 10 to 31% by mass, and particularly preferably 15 to 30% by mass.

[0048] The aqueous sodium silicate solution may contain other components as desired, such as sodium chloride, sodium sulfate, potassium chloride, potassium sulfate, etc., for the purpose of adjusting the pore size distribution.

[0049] The organic phase used in the continuous phase preferably has low solubility in an aqueous sodium silicate solution, and more preferably has no solubility therein. Examples of organic liquids constituting the organic phase include saturated linear hydrocarbons having 9 to 12 carbon atoms, such as n-nonane, n-decane, n-undecane, and n-dodecane; saturated branched hydrocarbons having 9 to 12 carbon atoms, such as isononane, isodecane, isoundecane, and isododecane; aliphatic hydrocarbons having 6 to 8 carbon atoms, such as n-hexane, isohexane, n-heptane, isoheptane, n-octene, and isooctene; alicyclic hydrocarbons having 1 to 8 carbon atoms, such as cyclopentane, cyclohexane, and cyclohexene; benzene, toluene, xylene, ethylbenzene, and propane. Examples of the fluorine-containing compounds include aromatic hydrocarbons such as pyridine, cumene, mesitylene, and tetralin; ethers such as propyl ether and isopropyl ether; esters such as ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-amyl acetate, isoamyl acetate, butyl lactate, methyl propionate, ethyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, and butyl butyrate; and fluorine-containing compounds such as 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether. These may be used alone or in combination of two or more. Among them, saturated linear hydrocarbons having 9 to 12 carbon atoms such as n-decane, n-nonane, n-dodecane, and n-undecane, and saturated branched hydrocarbons such as isononane, isodecane, isoundecane, and isododecane are preferred.

[0050] The flash point of the organic liquid constituting the organic phase is preferably 20 to 80° C., more preferably 30 to 60° C. In addition, non-flammable or flame-retardant organic liquids are preferred. When saturated hydrocarbons with a flash point of less than 20°C are used as the organic liquid, due to the low flash point, fire prevention and work environment measures are necessary. By making the flash point of the organic liquid 20°C or higher, fire prevention can be improved and the work environment can be improved. On the other hand, by making the flash point 80°C or lower, sufficient volatility can be obtained, and it is possible to prevent the organic liquid from adhering to and contaminating the silica particles when the silica particles are recovered from the organic phase.

[0051] A surfactant is added to the organic phase as an emulsifier. Examples of the surfactant include anionic surfactants, cationic surfactants, amphoteric surfactants, and nonionic surfactants.

[0052] Examples of the anionic surfactant include sodium fatty acid salts, alkyl sulfates, alkyl benzene sulfonates, and alkyl phosphates. Examples of the cationic surfactant include alkyltrimethylammonium salts, dialkyldimethylammonium salts, and alkylbenzyldimethylammonium salts. Examples of amphoteric surfactants include alkyl dimethylamine oxides and alkyl carboxybetaines. Examples of nonionic surfactants include polyethylene glycol fatty acid esters, polypropylene glycol fatty acid esters, polyethylene glycol alkyl ethers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene alkyl phenyl ethers, and polyoxyethylene alkyl ethers. These surfactants may be used alone or in combination of two or more. Among them, sorbitan fatty acid esters such as sorbitan monooleate, sorbitan dioleate, and sorbitan trioleate are preferred.

[0053] The amount of the surfactant used can be appropriately selected depending on conditions such as the type of surfactant, HLB (Hydrophile-Lipophile Balance) which is an index showing the degree of hydrophilicity or hydrophobicity of the surfactant, the particle size of the target silica particles, etc. Specifically, the surfactant is preferably contained in the organic phase in the range of 0.1 to 5.0% by mass, more preferably 0.1 to 3.0% by mass, and even more preferably 0.1 to 1.0% by mass. By making the content of the surfactant in the organic phase 0.1% by mass or more, it is possible to emulsify uniformly and to make the emulsion more stable. On the other hand, by making the content 5.0% by mass or less, it is possible to prevent the surfactant from adhering to and contaminating the silica particles, which are the final product. When the viscosity of the dispersed phase is low, it is preferable to have a lower concentration of the surfactant in order to emulsify uniformly.

[0054] The emulsion is obtained by adding the dispersed phase to the continuous phase and stirring the mixture. The dispersed phase is preferably added while stirring the continuous phase. As the stirring method, a conventionally known method can be used, and an emulsifying device such as a homogenizer, a homomixer, a colloid mill, an ultrasonic emulsifier, or a homodisper can be used.

[0055] For example, when emulsifying using a homogenizer, the mixture may be stirred and emulsified under emulsification conditions that produce droplets of the desired diameter.

[0056] For example, when emulsifying using a homomixer, emulsification may be carried out by stirring at a speed of 1,000 to 24,000 rpm for 1 to 10 minutes.

[0057] The liquid temperature during emulsification by stirring is preferably 10 to 40°C, more preferably 10 to 35°C, and even more preferably 10 to 30°C.

[0058] In the step (1-2), the emulsion formed in the step (1-1) is gelled to precipitate silica, thereby obtaining a silica slurry containing silica encapsulating template particles. As a method for gelation, for example, an acid may be added under stirring. This lowers the pH of the sodium silicate aqueous solution, and primary silica particles are precipitated. The precipitated primary particles aggregate, and secondary silica particles containing template particles are generated. The acid may be added under conditions such that spherical particles are obtained at the end of gelation, and the pH of the aqueous phase after two-phase separation is near neutral, preferably pH 7 to 10.

[0059] The acid to be used may be either an inorganic acid or an organic acid, with inorganic acids such as sulfuric acid, hydrochloric acid and carbonic acid being more preferred, and carbon dioxide gas being the most preferred for ease of operation.

[0060] The reaction liquid is separated into an aqueous phase in which silica encapsulating template particles is precipitated, and an oil phase, and the oil phase is removed to obtain a silica slurry. The oil phase can be removed by a conventional method, for example, decantation, reduced pressure filtration, pressure filtration, membrane separation, centrifugation, or the like.

[0061] In the step (1-3), an acid is added to the silica slurry obtained in the step (1-2) to remove the template particles.

[0062] Examples of acids that can be used include inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as acetic acid, perchloric acid, hydrobromic acid, trichloroacetic acid, dichloroacetic acid, methanesulfonic acid, and benzenesulfonic acid. Among these, sulfuric acid is preferably used from the viewpoints of safety and equipment protection.

[0063] The acid is preferably added until the pH of the silica slurry becomes equal to or less than 3. This causes the template particles to dissolve and be removed from the silica, forming voids derived from the template particles inside the silica particles. The pH is preferably from 1.5 to 2.5, more preferably from 1.5 to 2.0.

[0064] In step (1-4), the silica from which the template particles have been removed is washed and dried. Examples of the washing liquid for washing the silica include water; and organic solvents such as ethanol, acetone, and diethyl ether.

[0065] The temperature of the cleaning solution is preferably from 10 to 100°C, more preferably from 20 to 90°C, and further preferably from 30 to 80°C.

[0066] After the silica is thoroughly washed, it is dried. The drying may be performed by a conventionally known method. Examples of the drying method include vacuum drying, natural drying, and hot air drying, and for example, a spray dryer, a flash dryer, a tray dryer, a vacuum dryer, a kiln, etc. can be used.

[0067] The drying conditions may be any conditions that allow the washing liquid to be removed and the substrate to be dried, and may be appropriately adjusted depending on the drying method to be used.

[0068] (Second manufacturing method) In step (2-1) of the second manufacturing method, a mixed solution of an aqueous sodium silicate solution containing template particles and an acid is sprayed for a short time before silica precipitates, and the mixture is turned into droplets in the air, after which the silica precipitates, to obtain spherical silica containing the template particles.

[0069] As the template particles, a material that does not dissolve in an aqueous sodium silicate solution but dissolves in an acid is used, as in the first manufacturing method. Examples of the template particles include magnesium hydroxide, magnesium carbonate, calcium hydroxide, calcium carbonate, etc., and these may be used alone or in combination of two or more. Among them, at least one selected from the group consisting of magnesium hydroxide and magnesium carbonate is preferred from the viewpoint of being able to dissolve and remove the template particles using sulfuric acid. Sulfuric acid is a non-volatile acid, and is preferred from the viewpoint of safety and equipment protection compared to volatile acids such as hydrochloric acid, nitric acid, and hydrofluoric acid.

[0070] The size of the template particles is the same as in the first manufacturing method, and template particles of a desired size may be used. 50 It is preferable to use template particles having a particle size in the range of 200 nm to 3 μm, more preferably 300 nm to 2 μm, and even more preferably 400 nm to 1 μm.

[0071] The sodium silicate aqueous solution may be the same as that used in the first production method, and the silicic acid component preferably has a SiO2 concentration in the range of 3 to 35 mass % calculated as SiO2. When the concentration of the silicic acid component in the aqueous sodium silicate solution is within the above range, silica particles can be produced with high production efficiency. The concentration of the silicic acid component in the aqueous sodium silicate solution is more preferably 5% by mass or more, even more preferably 7% by mass or more, and particularly preferably 10% by mass or more, from the viewpoint of high productivity and obtaining particles with high sphericity. Also, from the viewpoint of easily obtaining particles with a small particle size, the concentration is more preferably 30% by mass or less, even more preferably 25% by mass or less, and particularly preferably 20% by mass or less.

[0072] Moreover, the ratio of silicic acid to sodium in the aqueous sodium silicate solution, in terms of SiO2 / Na2O (molar ratio), is preferably 2 to 4. The above-mentioned commercially available products having a SiO2 / Na2O (molar ratio) in the above range are easily available.

[0073] The template particles are preferably mixed in the sodium silicate aqueous solution in the range of 1 to 35% by mass. If the amount of template particles used is too small, each particle may not contain multiple voids with a major axis length of 200 nm to 3 μm, while if the amount is too large, the number of voids inside the silica particles may become too large, resulting in a decrease in particle strength. The amount of the template particles used in the aqueous sodium silicate solution is more preferably 5 to 33% by mass, further preferably 10 to 31% by mass, and particularly preferably 15 to 30% by mass.

[0074] The aqueous sodium silicate solution may contain other components as desired, such as sodium chloride, sodium sulfate, potassium chloride, potassium sulfate, etc., for the purpose of adjusting the pore size distribution.

[0075] The acid may be either an inorganic acid or an organic acid, with inorganic acids such as sulfuric acid, hydrochloric acid, and carbonic acid being more preferred.

[0076] The acid to be mixed with the aqueous sodium silicate solution containing the template particles is added to the aqueous sodium silicate solution containing the template particles so that the pH of the aqueous solution becomes approximately neutral, preferably 7-10.

[0077] In the second manufacturing method, the mixture of the aqueous sodium silicate solution containing the template particles and the acid is sprayed in a short time before silica is precipitated. Examples of the method for spraying the mixture in a short time to form droplets include a spray method, ultrasonic atomization, and a method of colliding large droplets with a high-speed fluid to form fine particles.

[0078] Methods for precipitating silica after it has been converted into droplets include extending the residence time in air, increasing the temperature for drying, and spraying into an acidic gas.

[0079] As a result, spherical silica particles containing the template particles are obtained.

[0080] Next, an acid is added to the spherical silica particles containing the template particles therein to remove the template particles (step 2-2).

[0081] The acids that can be used are the same as those in the first production method, and examples thereof include inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid, and organic acids such as acetic acid, perchloric acid, hydrobromic acid, trichloroacetic acid, dichloroacetic acid, methanesulfonic acid, and benzenesulfonic acid. Among these, it is preferable to use sulfuric acid from the viewpoints of safety and equipment protection.

[0082] The acid is preferably added until the pH of the silica slurry becomes equal to or less than 3. This causes the template particles to dissolve and be removed from the silica, resulting in voids derived from the template particles being formed inside the silica particles. The pH is preferably from 1.5 to 2.5, more preferably from 1.5 to 2.0.

[0083] In the next step, the silica from which the template particles have been removed is washed and dried (step 2-3).

[0084] Examples of the washing liquid for washing the silica include water; and organic solvents such as ethanol, acetone, and diethyl ether.

[0085] The temperature of the cleaning solution is preferably from 10 to 100°C, more preferably from 20 to 90°C, and further preferably from 30 to 80°C.

[0086] After the silica is thoroughly washed, it is dried. Drying is the same as in the first manufacturing method, and may be performed by a conventionally known method. Examples of drying methods include vacuum drying, natural drying, and hot air drying, and for example, a spray dryer, an airflow dryer, a tray dryer, a vacuum dryer, a kiln, etc. can be used.

[0087] The drying conditions may be any conditions that allow the washing liquid to be removed and the substrate to be dried, and may be appropriately adjusted depending on the drying method to be used.

[0088] The manufacturing method of the present invention may further include a step of calcining the silica particles obtained in step (1-4) of the first manufacturing method and step (2-3) of the second manufacturing method. Calcining the silica particles can increase the strength of the silica particles. After calcination, all the silica particles become amorphous.

[0089] The temperature for firing the silica particles is preferably 800° C. or higher, more preferably 850° C. or higher, and even more preferably 900° C. or higher, from the viewpoint of increasing particle strength, and is preferably 1100° C. or lower, from the viewpoints of leaving voids of 200 nm or more in the particles, preventing the generation of crystalline silica, and preventing fusion between particles.

[0090] The calcination time is preferably 1 hour or more, more preferably 2 hours or more, and even more preferably 3 hours or more from the viewpoint of increasing the particle strength, and is preferably 6 hours or less, more preferably 5 hours or less, and even more preferably 4 hours or less from the viewpoint of leaving voids of 200 nm or more in the particles, preventing the generation of crystalline silica, and preventing the particles from fusing together.

[0091] <Applications of silica particles> The silica particles of the present invention can be used as materials in various fields, such as cosmetics, catalyst supports, and heat insulating materials.

[0092] In cosmetics, the silica particles have high hiding power in dry powder, so that it is expected to have improved performance as a cosmetic material that can be used in dry powder form, such as finishing powder, loose foundation, and pressed foundation. The silica particles of the present invention have relatively small voids around them, so that they have excellent hiding power even when sweat or sebum is present. In addition, the silica particles of the present invention are light particles with a high void ratio, so that they can be used in mascara, which requires lightness, and can be expected to provide a new feel due to the added lightness. In addition, they can be used as a white pigment because they scatter visible light.

[0093] In catalyst supporting applications, when polymer polymerization is carried out while the support is being disintegrated, this leads to easy disintegration, and the reaction rate can be improved.

[0094] In addition, when used as a heat insulating material, the silica particles of the present invention have a high porosity, so that high heat insulating performance can be expected. EXAMPLES

[0095] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the following description, the same components are used as common components. Moreover, Examples 1 to 5 are working examples, Examples 6 to 8 are comparative examples, and Example 9 is the iron (III) oxide used in the test.

[0096] (Example 1) The dispersed phase was prepared by diluting No. 3 sodium silicate (AGC Si-Tech Co., Ltd., sodium silicate aqueous solution, SiO2 / Na2O (molar ratio) = 3) with distilled water to adjust the SiO2 concentration to 24 mass%, and stirring and mixing this with magnesium hydroxide template particles (Konoshima Chemical Co., Ltd., Magseeds X-6F, 50% particle size 0.8 μm). As the continuous phase, n-decane (Tosoh Corporation, HC-250, C 10 H 22 ) in which 0.7% by mass of sorbitan monooleate (Ionet S80, manufactured by Sanyo Chemical Industries, Ltd.) was dissolved in advance as a surfactant was used. The continuous phase of n-decane containing surfactant was stirred with a homogenizer (Microtech Nithion Co., Ltd., Hiscotron, generator shaft NS-30UG / 20P) while the dispersed phase of sodium silicate slurry containing magnesium hydroxide was added and emulsified by stirring at 8,000 rpm for 5 minutes. The resulting emulsion was stirred with a three-one motor while carbon dioxide gas was blown in at a rate of 1.0 L / min for 20 minutes to precipitate silica. Thereafter, the aqueous phase containing silica gel obtained by removing the oil phase was stirred at room temperature while sulfuric acid was added until the pH reached 2 to remove the template. The slurry after template removal was filtered and washed with warm water, and dried with a spray dryer (Mini Spray Dryer B290, manufactured by Nippon Buchi Co., Ltd.) to obtain silica particles of Example 1.

[0097] (Example 2) The silica particles obtained in Example 1 were heated to 1050° C. at a heating rate of 5° C. / min and calcined for 4 hours. Thereafter, the silica particles were cooled to room temperature to obtain silica particles of Example 2.

[0098] (Example 3) The silica particles obtained in Example 1 were heated to 1100° C. at a heating rate of 5° C. / min and calcined for 4 hours. Thereafter, the particles were cooled to room temperature to obtain silica particles of Example 3.

[0099] (Example 4) Silica particles of Example 4 were obtained in the same manner as in Example 1, except that magnesium carbonate (Magthermo MS-S, 50% particle size 1.5 μm, manufactured by Konoshima Chemical Co., Ltd.) was used as the template particles.

[0100] (Example 5) The silica particles obtained in Example 4 were heated to 1000° C. at a heating rate of 5° C. / min and calcined for 4 hours. Thereafter, the particles were cooled to room temperature to obtain silica particles of Example 5.

[0101] (Example 6) A commercially available porous silica called "Sunsphere H-121" manufactured by AGC Si-Tech Co., Ltd. was used.

[0102] (Example 7) A commercially available porous silica called "Sunsphere H-122" manufactured by AGC Si-Tech Co., Ltd. was used.

[0103] A commercially available non-porous silica, "Sunsphere NP-100" manufactured by AGC Si-Tech Co., Ltd., was used.

[0104] (Example 9) Commercially available iron(III) oxide powder (Kanto Chemical Co., Ltd., special grade, reddish brown powder) was used.

[0105] The physical properties of the silica particles of Examples 1 to 8 were measured as follows. The results are shown in Table 1. Note that Example 9 is the material used for the chromaticity evaluation.

[0106] <Size and number of voids inside particles> The silica particle powder was intentionally broken by crushing it between two glass slides, and the broken surface of the particle was observed using a tabletop scanning electron microscope (JCM-7000, manufactured by JEOL Ltd.). The length of the major axis at the opening of the void was measured to confirm whether there were multiple voids of 200 nm to 3 μm. If there were multiple voids of 200 nm to 3 μm, the particle was evaluated as having voids, and if there was no void or only one void of 200 nm to 3 μm, the particle was evaluated as having no voids. As for the silica particles of Example 4, an SEM photograph of a cut surface is shown in FIG. 1, and an SEM photograph of the appearance is shown in FIG.

[0107] <Average circularity> The circularity was calculated by obtaining the area and perimeter of a particle from an image obtained by a particle image analyzer (e.g., Morphologi4 manufactured by Malvern Instruments) using image analysis software attached to the device, and applying the results to the following formula: The average circularity of 30,000 silica particles was determined. Circularity = perimeter of a circle with equal projected area / perimeter of a particle Circumference of a circle with the same projected area: When a particle is observed from directly above, the area of ​​the particle's shadow projected on the plane below is calculated, and a circle with an area equal to this area is calculated, and the length of the contour of that circle is calculated. Particle perimeter: The length of the outline of the particle's shadow projected on a flat surface when the particle is observed from directly above

[0108] <50% particle size (D 50 )(μm)> 50% particle size (D 50 ) was calculated as the 50% volume equivalent particle diameter by measuring 30,000 particles with a circularity of 0.90 or more using a particle image analyzer (Malvern Instruments, Morphologi4).

[0109] <Specific surface area (m 2 / g)> The specific surface area was determined by analyzing the results of measurements by nitrogen adsorption method at relative pressures of 0 to 0.99 using an automatic specific surface area / pore distribution measuring device (Tristar II 3020 series, manufactured by Shimadzu Corporation) using the BET method.

[0110] <Pore volume (cm 3 / g)> The pore volume was determined by analyzing the results of measurements at relative pressures of 0 to 0.99 by the nitrogen adsorption method using an automatic specific surface area / pore distribution measuring device (Tristar II 3020 series, manufactured by Shimadzu Corporation) in the same manner as for the specific surface area, using the BJH method.

[0111] <Oil absorption amount (cm 3 / 100g)> The oil absorption was measured in accordance with JIS K 5101. The sample, which was made up of silica particles, was kneaded until the entire sample was formed into a single mass, while boiled linseed oil was added to the sample. When the entire sample had formed a single mass, the volume of boiled linseed oil per 100 g of sample was determined.

[0112] <Particle strength (MPa)> The particle strength was determined by measuring the compressive strength of 40 silica particles per sample using a microcompression tester (MCT-510, manufactured by Shimadzu Corporation) and calculating the average value.

[0113] <Particle surface properties> 5g of silica particle powder was added to 100g of water, stirred uniformly, and then left to stand for 24 hours. If 90% or more of the silica particles had sunk in the water after 24 hours, the silica particles were deemed to be hydrophilic and rated as "hydrophilic." If less than 90% of the silica particles had sunk after 24 hours, they were rated as "not hydrophilic." The percentage of sunk silica particles was calculated from the mass of the silica particles obtained by collecting and drying the sunk particles after leaving them to stand for 24 hours.

[0114] * Value, L * Value, WB value (-)> The powder of silica particles was mixed with the iron (III) oxide powder (a * The mixed powder was placed in a round measuring cell (diameter 35 mm × height 15 mm) to a volume of more than half, and the color difference was measured using a spectrophotometer (SE7700, manufactured by Nippon Denshoku Industries Co., Ltd.). a * The value indicates the strength of the color, with the larger the + value, the stronger the redness, and the larger the - value, the stronger the greenness. If the value is 6.0 or less, it can be determined that the color (redness) of the iron (III) oxide is suppressed. * The value indicates the brightness of the color, the larger it is, the brighter it is, and the smaller it is, the darker it is. The WB value indicates the whiteness, the larger it is, the whiter it is, and the smaller it is, the blacker it is.

[0115] [Table 1] ​

[0116] The silica particles of Examples 1 to 5 had a plurality of voids of 200 nm to 3 μm inside the particles, and the value of (oil absorption amount / 100) / pore volume was 1.5 or more. As can be seen from Table 1, in the evaluation using the silica particles of Examples 1 to 5, * The value was 6.0 or less, and the redness of iron (III) oxide was suppressed. This indicates that the silica particles of Examples 1 to 5 have higher visible light scattering properties and are superior in shielding properties for the base compared to the silica particles of Examples 6 to 8.

Claims

1. The particle contains a plurality of voids with a major axis length of 200 nm to 3 μm, and the oil absorption capacity (cm 3 / 100g) / 100} / pore volume (cm 3 / g) is 1.5 or more, and the surface is hydrophilic, When the silica particles are mixed with 30% by mass of reddish-brown iron (III) oxide powder having an a* value of 14 or more and 15 or less in the L*a*b* color system to obtain a mixed powder, the a* value of the mixed powder is 6.0 or less.

2. A silica particle containing a plurality of voids with a major axis length of 200 nm or more and 3 μm or less inside the particle, having a value of {oil absorption (cm3 / 100g) / 100} / pore volume (cm3 / g) of 1.5 or more and said pore volume being less than 2.0 cm3 / g, When the silica particles are mixed with 30% by mass of reddish-brown iron (III) oxide powder having an a* value of 14 or more and 15 or less in the L*a*b* color system to obtain a mixed powder, the a* value of the mixed powder is 6.0 or less.

3. A silica particle containing a plurality of voids with a major axis length of 200 nm or more and 3 μm or less inside the particle, having a value of {oil absorption (cm3 / 100g) / 100} / pore volume (cm3 / g) of 1.5 or more and a particle strength of 1 MPa or more, When the silica particles are mixed with 30% by mass of reddish-brown iron (III) oxide powder having an a* value of 14 or more and 15 or less in the L*a*b* color system to obtain a mixed powder, the a* value of the mixed powder is 6.0 or less.

4. The pore volume is 2.0 cm 3 The silica particles according to claim 1 or 3, wherein the surface area is less than 1 / g.

5. 3. The silica particles according to claim 1 or 2, having a particle strength of 1 MPa or more.

6. 4. The silica particle according to claim 2 or 3, which has a hydrophilic surface.

7. The silica particles according to any one of claims 1 to 6, having an average circularity of 0.80 or more.

8. The 50% particle size (D) in the cumulative particle size distribution based on the volume of silica particles 50 8. The silica particles according to claim 1, wherein the average particle diameter is 3 to 500 μm.

9. Silica particles according to claim 1, wherein the value of {oil absorption (cm 3 / 100 g) / 100} / pore volume (cm 3 / g) is 2.0 or more.

10. A white pigment comprising the silica particles according to any one of claims 1 to 9.

11. A cosmetic comprising the silica particles according to any one of claims 1 to 9.

12. A method for producing silica particles, comprising the steps of: mixing a mixture of template particles in an aqueous sodium silicate solution as a dispersed phase; mixing and stirring an organic phase containing a surfactant as a continuous phase; mixing the dispersed phase and the continuous phase to emulsify the mixture; obtaining an emulsion in which the dispersed phase is converted into droplets; gelling the emulsion to obtain a silica slurry containing silica encapsulating the template particles; adding an acid to the silica slurry until the pH of the silica slurry becomes 3 or less to remove the template particles; and washing and drying the silica from which the template particles have been removed, the template particle is at least one selected from the group consisting of magnesium hydroxide and magnesium carbonate, and the 50% particle diameter (D50) of the template particle is 200 nm to 3 μm; The sodium silicate aqueous solution has a silicic acid component with a SiO 2 concentration calculated as SiO 2 of 3 to 35 mass %, and a ratio of silicic acid to sodium in the sodium silicate aqueous solution is SiO 2 / Na 2 O (molar ratio) of 2 to 4; the template particles are mixed in the sodium silicate aqueous solution in an amount of 1 to 35% by mass, the organic phase is one or more of saturated linear hydrocarbons having 9 to 12 carbon atoms and saturated branched hydrocarbons having 9 to 12 carbon atoms, and the organic phase contains 0.1 to 5.0 mass % of the surfactant.

Citation Information

Patent Citations

  • Method for producing hollow silica particles

    JP2000500113A

  • Porous silica particle having surface smoothness, manufacturing process of the porous silica particle, and cosmetic mixed with the porous silica particle

    JP2009137806A

  • Amorphous silica

    JP2010184856A

  • Spherical shape oxide powder, and production method thereof

    JP2014088307A

  • Method for manufacturing spherical silica

    JP2015113277A