Die bond material, light emitting device, and method for manufacturing light emitting device

A die-bonding material with a specific curable polysilsesquioxane compound and thermal acid generator addresses adhesion and heat resistance issues, enhancing the reliability of light-emitting devices by providing strong and durable fixation.

JP7575301B2Active Publication Date: 2024-10-29LINTEC CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021037302
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-09
Publication Date
2024-10-29
Estimated Expiration
2041-03-09

AI Technical Summary

Technical Problem

Existing die-bonding materials for light-emitting devices do not provide sufficient adhesion and heat resistance, limiting the performance and reliability of light-emitting devices.

Method used

A die-bonding material containing a specific curable polysilsesquioxane compound, thermal acid generator, and solvent, with a curable polysilsesquioxane compound having a defined molecular structure and composition, is used to enhance adhesion and heat resistance.

Benefits of technology

The die-bonding material provides high adhesive strength and heat resistance, ensuring reliable fixation of light-emitting elements and improving the performance and durability of light-emitting devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575301000036
    Figure 0007575301000036
  • Figure 0007575301000037
    Figure 0007575301000037
  • Figure 0007575301000038
    Figure 0007575301000038
Patent Text Reader

Abstract

To provide a die bond material that is suitably used in fixing a light emitting element at a predetermined position, a light emitting device that has an adhesive member derived from the die bond material, and a method for manufacturing the light emitting device.SOLUTION: There is provided a die bond material that contains the following (A) component, (B) component, and solvent, in which the content of the (B) component exceeds 0 pt.mass and 0.6 pt.mass or less based on 100 pts.mass of the (A) component, and the die bond material has predetermined curing characteristics. Also provided are a light emitting device that has an adhesive member derived from the die bond material, and a method for manufacturing the light emitting device. The (A) component is a curable polysilsesquioxane compound that has a repeating unit indicated by the following formula (a-1), the curable polysilsesquioxane compound satisfying a predetermined requirement related to 29Si-NMR and a mass average molecular weight (Mw). The (B) component is a thermal acid generator.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a die bond material that is suitably used for fixing a light emitting element in a predetermined position, a light emitting device having an adhesive member derived from this die bond material, and a method for manufacturing this light emitting device. [Background technology]

[0002] 2. Description of the Related Art Curable compositions have been improved in various ways depending on the intended use, and have come to be widely used industrially as raw materials for optical parts and molded articles, adhesives, coating agents, and the like. In particular, silicone compound-containing curable compositions have been attracting attention as sealing materials for light-emitting devices and die-bonding materials for light-emitting devices. For example, Patent Documents 1 to 4 describe curable compositions containing a polysilsesquioxane compound as curable compositions that are suitable for use in the production of light-emitting devices. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-359933 A [Patent Document 2] JP 2005-263869 A [Patent Document 3] JP 2006-328231 A [Patent Document 4] WO2017 / 110948 (US2018 / 0355111 A1) Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made with an object to provide a die bond material and a light emitting device with higher performance, and a method for manufacturing the light emitting device. That is, an object of the present invention is to provide a die bond material that is suitable for use in fixing a light emitting element in a predetermined position, a light emitting device having an adhesive member derived from this die bond material, and a method for manufacturing this light emitting device. [Means for solving the problem]

[0005] In order to solve the above problems, the present inventors have conducted extensive research into a die bond material containing a curable polysilsesquioxane compound. As a result, the inventors have found that a die-bonding material containing a specific curable polysilsesquioxane compound, a thermal acid generator, and a solvent is suitable as a material for fixing a light-emitting element, and have completed the present invention.

[0006] Thus, according to the present invention, there are provided the following die bond materials (1) to (9), light emitting devices (10) to (12), and methods for manufacturing light emitting devices (13) to (15).

[0007] [1] A die bond material containing the following components (A), (B), and a solvent, wherein the content of component (B) is more than 0 and 0.6 parts by mass or less per 100 parts by mass of component (A), and when a 0.20 mL sample is placed on a stainless steel plate heated to 100°C and stirred with an automatic curing time measuring device under the following conditions: the impeller rotation speed is 300 rpm, the impeller revolution speed is 120 rpm, and the gap (distance between the stainless steel plate and the impeller) is 0.2 mm, the time from the start of stirring until the stirring torque reaches 0.049 N cm is 200 to 2500 seconds. Component (A): A curable polysilsesquioxane compound having a repeating unit represented by the following formula (a-1), characterized in that the curable polysilsesquioxane compound satisfies the following requirements A1 and A2:

[0008] [ka]

[0009] [R 1 is the formula: Cm H (2m-n+1) F n m represents an integer of 1 to 10, and n represents an integer of 2 or more and (2m+1) or less. D represents a fluoroalkyl group represented by R 1 and Si. [Requirement A1] Curable polysilsesquioxane compounds 29 When Si-NMR is measured, one or more peaks are observed in the region of -62 ppm or more and less than -52 ppm [region (2)], one or more peaks are observed in at least one of the regions of -52 ppm or more and less than -45 ppm [region (1)] and -73 ppm or more and less than -62 ppm [region (3)], and Z2 calculated by the following formula is 20 to 40%.

[0010]

number

[0011] P1: Integral value in region (1) P2: Integral value in region (2) P3: Integral value in region (3) [Requirement A2] The curable polysilsesquioxane compound has a mass average molecular weight (Mw) of 3,500 to 11,000. Component (B): Thermal acid generator [2] The die bonding material according to [1], wherein the proportion of the repeating unit represented by formula (a-1) in the curable polysilsesquioxane compound is 25 mol % or more based on the total repeating units. [3] The die bonding material according to [1] or [2], wherein the curable polysilsesquioxane compound further has a repeating unit represented by the following formula (a-2):

[0012] [ka]

[0013] [R2 represents an unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms. [4] The die bonding material according to [3], wherein the ratio of the repeating unit represented by formula (a-2) in the curable polysilsesquioxane compound is more than 0 mol% and 75 mol% or less with respect to the total repeating units. [5] The curable polysilsesquioxane compound 29 The die bonding material according to any one of [1] to [4], wherein, when Si-NMR is measured, one or more peaks are observed in region (3), and Z3 calculated by the following formula is 60 to 80%.

[0014]

number

[0015] [6] The die bonding material according to any one of [1] to [5], wherein the content of the component (A) is 40 mass % or more and less than 100 mass % of the solid content of the die bonding material. [7] The die bonding material according to any one of [1] to [6], wherein the component (B) is an onium salt-based thermal acid generator. [8] The die bonding material according to any one of [1] to [7], wherein the component (B) satisfies the following requirement B1. [Requirement B1] Regarding component (B), the peak temperature of the maximum endothermic peak obtained by differential scanning calorimetry at a temperature range of 30 to 300°C and a heating rate of 10°C / min (acid generation temperature) is 80 to 180°C. [9] The die bonding material according to any one of [1] to [8], further comprising the following component (C): Component (C): Silane coupling agent

[10] A light emitting device comprising: a pair of lead electrodes; and a molded body molded integrally with the pair of lead electrodes; and a recessed element container, the bottom of the recess being constituted by the pair of lead electrodes; and a light emitting element fixed via an adhesive member onto at least one of the pair of lead electrodes constituting the bottom of the recess; and the adhesive member being a hardened product of the die bond material described in any one of [1] to [9].

[11] The light-emitting device described in

[10] , wherein the adhesive member fixing the light-emitting element has a die shear strength of 650 gf or more when the light-emitting element is pressed from the side at 0.3 mm / sec at 25°C and breaks occur between the light-emitting element and the adhesive member.

[12] The light-emitting device described in

[10] , wherein the adhesive member fixing the light-emitting element has a die shear strength of 300 gf or more when the light-emitting element is pressed from the side at 0.3 mm / sec at 150°C and breaks occur between the light-emitting element and the adhesive member.

[13] The light emitting device according to any one of

[10] to

[12] , wherein the element container has a reflectance maintenance rate (α) of 99.8% or more, which is calculated by the following formula:

[0016]

number

[0017] (R i is the reflectance measured at a wavelength of 450 nm at room temperature (25°C) without heating, and R ii is the reflectance measured at a wavelength of 450 nm after heating at 100°C for 100 minutes and then cooling to room temperature (25°C).

[14] The light emitting device according to any one of

[10] to

[13] , wherein the light emitting element has an emission peak wavelength of 445 nm or more and 465 nm or less.

[15] The light-emitting element is a nitride semiconductor (In x Al y Ga 1-x-y N, 0≦x, 0≦y, x+y≦1).

[16] A method for manufacturing a light emitting device comprising: an element container having a pair of lead electrodes and a molded body molded integrally with the pair of lead electrodes, the element container having a recess, the bottom of the recess being constituted by the pair of lead electrodes; and a light emitting element fixed onto at least one of the pair of lead electrodes constituting the bottom of the recess via an adhesive member, the method comprising: a light emitting element mounting step of fixing the light emitting element to at least one of the pair of lead electrodes using the die bond material described in any one of [1] to [9].

[17] The method for manufacturing a light-emitting device described in

[16] , wherein the light-emitting element mounting process comprises applying the die-bonding material to at least one of the pair of lead electrodes, placing the light-emitting element on the die-bonding material, and hardening the die-bonding material at a temperature of 95°C or higher and 105°C or lower.

[18] The method for producing a light emitting device according to

[16] or

[17] , wherein the light emitting element has an emission peak wavelength of 445 nm or more and 465 nm or less. Effect of the Invention

[0018] According to the present invention, there are provided a die bond material that is suitably used for fixing a light emitting element in a predetermined position, a light emitting device having an adhesive member derived from this die bond material, and a method for manufacturing this light emitting device. [Brief description of the drawings]

[0019] [Figure 1] 1 is a schematic front view of a light emitting device according to an embodiment of the present invention. [Diagram 2] 2 is a schematic cross-sectional view of a light-emitting device according to an embodiment of the present invention taken along the line AA in FIG. [Diagram 3] 2 is a schematic cross-sectional view of a light-emitting device according to an embodiment of the present invention taken along line BB in FIG. [Figure 4] 2 is a schematic bottom view of the light emitting device according to the embodiment of the present invention, shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will be described in detail below by dividing it into the following sections: 1) a die bond material, 2) a light emitting device, and 3) a method for manufacturing a light emitting device.

[0021] 1) Die bond material The die bond material of the present invention contains the following components (A) and (B), and a solvent, in which the content of component (B) is more than 0 parts by mass and not more than 0.6 parts by mass per 100 parts by mass of component (A), and the die bond material has a predetermined curability. Component (A): A curable polysilsesquioxane compound having a repeating unit represented by the above formula (a-1), characterized in that the curable polysilsesquioxane compound (A) satisfies the above requirements A1 and A2. Component (B): Thermal acid generator In the present invention, the term "curable polysilsesquioxane compound" refers to a polysilsesquioxane compound that is converted into a cured product by itself when certain conditions such as heating are satisfied, or a polysilsesquioxane compound that functions as a curable component in a curable composition (die bond material).

[0022] [Component (A)] The component (A) constituting the die bond material of the present invention is a curable polysilsesquioxane compound having a repeating unit represented by the following formula (a-1), and is characterized in that it satisfies the above requirements A1 and A2.

[0023] [ka]

[0024] [R 1 is the formula: C m H (2m-n+1) F n m represents an integer of 1 to 10, and n represents an integer of 2 or more and (2m+1) or less. D represents a fluoroalkyl group represented by R 1and Si.

[0025] In formula (a-1), R 1 is the formula: C m H (2m-n+1) F n The symbol m represents an integer of 1 to 10, and the symbol n represents an integer of 2 or more and (2m+1) or less. The symbol m is preferably an integer of 1 to 5, and more preferably an integer of 1 to 3. R 1 By using a curable polysilsesquioxane compound having the above formula, it is possible to obtain a die bond material having a low refractive index.

[0026] Composition formula: C m H (2m-n+1) F n Examples of the fluoroalkyl group represented by the formula (I) include perfluoroalkyl groups such as CF3, CF3CF2, CF3(CF2)2, CF3(CF2)3, CF3(CF2)4, CF3(CF2)5, CF3(CF2)6, CF3(CF2)7, CF3(CF2)8, and CF3(CF2)9; and hydrofluoroalkyl groups such as CF3CH2CH2, CF3(CF2)3CH2CH2, CF3(CF2)5CH2CH2, and CF3(CF2)7CH2CH2.

[0027] In formula (a-1), D is R 1 and Si. Examples of the linking group for D include arylene groups having 6 to 20 carbon atoms, such as a 1,4-phenylene group, a 1,3-phenylene group, a 1,2-phenylene group, and a 1,5-naphthylene group.

[0028] The curable polysilsesquioxane compound (A) is a compound selected from the group consisting of one type of (R 1 Even if the polymer has two or more (R 1 -D) (copolymer). When the curable polysilsesquioxane compound (A) is a copolymer, the curable polysilsesquioxane compound (A) may be any of a random copolymer, a block copolymer, a graft copolymer, an alternating copolymer, etc., but from the viewpoint of ease of production, etc., a random copolymer is preferred. The structure of the curable polysilsesquioxane compound (A) may be any of a ladder structure, a double-decker structure, a cage structure, a partially cleaved cage structure, a cyclic structure, and a random structure.

[0029] The proportion of the repeating units represented by formula (a-1) contained in the curable polysilsesquioxane compound (A) is preferably 25 mol % or more, more preferably 25 to 90 mol %, and even more preferably 25 to 85 mol %, based on all repeating units. By using a curable polysilsesquioxane compound (A) in which the proportion of repeating units represented by formula (a-1) is 25 mol % or more based on all repeating units, a die bond material having a lower refractive index can be obtained.

[0030] The curable polysilsesquioxane compound (A) may further have a repeating unit represented by the following formula (a-2) (copolymer).

[0031] [ka]

[0032] In formula (a-2), R 2 represents an unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms.

[0033] R 2 Examples of the unsubstituted alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a s-butyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, an n-octyl group, an n-nonyl group, and an n-decyl group.

[0034] R 2 Examples of the unsubstituted aryl group having 6 to 12 carbon atoms include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group. R 2 Examples of the substituent of the aryl group having 6 to 12 carbon atoms include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, s-butyl, isobutyl, t-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, and isooctyl; halogen atoms such as fluorine, chlorine, and bromine; and alkoxy groups such as methoxy and ethoxy.

[0035] Among these, R 2 As the alkyl group, an unsubstituted alkyl group having 1 to 10 carbon atoms is preferable, an unsubstituted alkyl group having 1 to 6 carbon atoms is more preferable, and an unsubstituted alkyl group having 1 to 3 carbon atoms is particularly preferable, because a cured product having higher adhesive strength and more excellent heat resistance is easily obtained.

[0036] When the curable polysilsesquioxane compound (A) has a repeating unit represented by formula (a-2), the curable polysilsesquioxane compound (A) contains one kind of R 2 Even if it has two or more R 2 The present invention may also have the following structure.

[0037] When the curable polysilsesquioxane compound (A) has a repeating unit represented by formula (a-2), the proportion of the repeating unit is preferably more than 0 mol and not more than 75 mol%, more preferably 10 to 75 mol%, and even more preferably 15 to 75 mol%, based on the total repeating units. By using a curable polysilsesquioxane compound (A) in which the proportion of the repeating unit represented by formula (a-2) falls within the above range, a cured product having higher adhesive strength and more excellent heat resistance can be easily obtained.

[0038] The proportion of the repeating units represented by formula (a-1) or formula (a-2) in the curable polysilsesquioxane compound (A) is, for example, 1 It can be determined by measuring H-NMR.

[0039] The curable polysilsesquioxane compound (A) is soluble in various organic solvents such as ketone solvents such as acetone; aromatic hydrocarbon solvents such as benzene; sulfur-containing solvents such as dimethyl sulfoxide; ether solvents such as tetrahydrofuran; ester solvents such as ethyl acetate; halogen-containing solvents such as chloroform; and mixed solvents consisting of two or more of these. Therefore, the curable polysilsesquioxane compound (A) in a solution state can be dissolved in these solvents. 1 H-NMR can be measured.

[0040] The repeating unit represented by formula (a-1) and the repeating unit represented by formula (a-2) are represented by the following formula (a-3).

[0041] [ka]

[0042] [G is (R 1 -D) or R 2 Represents R 1 ,D.,R. 2 Each has the same meaning as above. 1 / 2 indicates that the oxygen atom is shared with the adjacent repeat unit.

[0043] As shown in formula (a-3), the curable polysilsesquioxane compound (A) has a partial structure, generally referred to as a T site, in which three oxygen atoms are bonded to a silicon atom and one other group (a group represented by G) is bonded to the silicon atom. Examples of the T site contained in the curable polysilsesquioxane compound (A) include those represented by the following formulas (a-4) to (a-6).

[0044] [ka]

[0045] In the formulae (a-4), (a-5) and (a-6), G has the same meaning as above. 3 R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms. 3 Examples of the alkyl group having 1 to 10 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an s-butyl group, an isobutyl group, and a t-butyl group. 3 may be the same or different. In the above formulae (a-4) to (a-6), * denotes a silicon atom bonded thereto.

[0046] The T site represented by the formula (a-4) and the formula (a-5) is a group capable of contributing to a polycondensation reaction (R 3 -O). Therefore, polysilsesquioxane compounds containing many of these T sites have excellent reactivity. Furthermore, die bond materials containing such polysilsesquioxane compounds have excellent curing properties. On the other hand, the T sites represented by formula (a-5) and formula (a-6) are bonded to two or more silicon atoms (adjacent T sites). Therefore, polysilsesquioxane compounds containing many of these T sites tend to have large molecular weights.

[0047] Therefore, the polysilsesquioxane compound containing many T sites, as represented by formula (a-5), has a relatively large molecular weight and is sufficiently reactive. As will be explained below, the curable polysilsesquioxane compound (A) used in the present invention has these properties.

[0048] First, the curable polysilsesquioxane compound (A) satisfies the following requirement A1. [Requirement A1] Curable polysilsesquioxane compounds 29When Si-NMR is measured, one or more peaks are observed in the region of -62 ppm or more and less than -52 ppm [region (2)], one or more peaks are observed in at least one of the regions of -52 ppm or more and less than -45 ppm [region (1)] and -73 ppm or more and less than -62 ppm [region (3)], and Z2 calculated by the following formula is 20 to 40%. Note that "peaks observed in region (1)" refer to peaks whose tops are within the range of region (1). The same applies to "peaks observed in region (2)" and "peaks observed in region (3)."

[0049]

number

[0050] P1: Integral value in region (1) P2: Integral value in region (2) P3: Integral value in region (3)

[0051] In this specification, the terms "integral value in region (1)", "integral value in region (2)", and "integral value in region (3)" refer to values ​​obtained by calculation within the integral ranges of -52 ppm to -45 ppm, -62 ppm to -52 ppm, and -73 ppm to -62 ppm, respectively.

[0052] The peaks observed in regions (1), (2), and (3) are derived from silicon atoms in the T sites represented by formulas (a-4), (a-5), and (a-6), respectively.

[0053] Therefore, a curable polysilsesquioxane compound that satisfies requirement A1 is one that contains 20 to 40% of T sites represented by formula (a-5) relative to the total T sites. As described above, this curable polysilsesquioxane compound has a relatively large molecular weight and sufficient reactivity, and is useful as a curable component of a die bond material.

[0054] In requirement A1, the value of Z2 is preferably 24 to 36%, more preferably 27 to 32%. If Z2 is too small, the curable polysilsesquioxane compound does not have sufficient reactivity, and if Z2 is too large, the storage stability of the die bonding material decreases.

[0055] The curable polysilsesquioxane compound (A) is 29 It is preferred that, when Si-NMR is measured, one or more peaks are observed in region (3) and Z3 calculated by the following formula is 60 to 80%.

[0056]

number

[0057] The curable polysilsesquioxane compound (A) in which Z3 is 60 to 80% contains 60 to 80% of T sites represented by formula (a-6) relative to the total T sites. A curable polysilsesquioxane compound (A) having a Z3 value in the range of 60 to 80% has an excellent balance between molecular weight and reactivity. Since this effect is more easily obtained, the value of Z3 is more preferably from 64 to 76%, and further preferably from 68 to 73%.

[0058] The values ​​of Z2 and Z3 are, for example, 29 Si-NMR is measured to obtain P1 to P3, and the calculation can be performed according to the above formula.

[0059] The curable polysilsesquioxane compound (A) satisfies the above requirement A2. That is, the mass average molecular weight (Mw) of the curable polysilsesquioxane compound (A) is 3,500 to 11,000, preferably 4,000 to 8,000, and more preferably 5,000 to 7,000.

[0060] As described above, curable polysilsesquioxane compounds that satisfy requirement A1 tend to have a relatively large molecular weight. Requirement A2 clarifies the range of the molecular weight. By using a curable polysilsesquioxane compound (A) having a mass average molecular weight (Mw) within the above range as a curable component, a die bond material can be obtained that gives a cured product with high adhesive strength and excellent heat resistance.

[0061] The molecular weight distribution (Mw / Mn) of the curable polysilsesquioxane compound (A) is not particularly limited, but is usually in the range of 1.0 to 10.0, preferably 1.1 to 6.0. By using the curable polysilsesquioxane compound (A) having a molecular weight distribution (Mw / Mn) within the above range as the curable component, it is possible to obtain a die bond material that gives a cured product having superior adhesion and heat resistance. The mass average molecular weight (Mw) and number average molecular weight (Mn) can be determined, for example, as a polystyrene-equivalent value by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent.

[0062] The curable polysilsesquioxane compound (A) can be produced, for example, by polycondensing a compound represented by the following formula (a-7) (hereinafter sometimes referred to as "silane compound (1)"), or the silane compound (1) and a compound represented by the following formula (a-8) (hereinafter sometimes referred to as "silane compound (2)"), in the presence of a polycondensation catalyst.

[0063] [ka]

[0064] In formulas (a-7) and (a-8), R 1 , R 2 , D has the same meaning as above. 4 , R 5 each independently represents an alkyl group having 1 to 10 carbon atoms; 1 , X 2each independently represents a halogen atom, and p and q each independently represent an integer of 0 to 3. 4 , R 5 , and multiple X 1 , X 2 may be the same as or different from each other.

[0065] R 4 , R 5 As the alkyl group having 1 to 10 carbon atoms, R 2 Examples of the alkyl group having 1 to 10 carbon atoms include those exemplified above. X 1 , X 2 Examples of the halogen atom include a chlorine atom and a bromine atom.

[0066] Examples of the silane compound (1) include CF3Si(OCH3)3, CF3CF2Si(OCH3)3, CF3CF2CF2Si(OCH3)3, CF3CF2CF2CF2Si(OCH3)3, CF3CH2CH2Si(OCH3)3, CF3CF2CF2CF2CH2CH2Si(OCH3)3, CF3CF2CF2CF2CF2CF2CH2CH2Si(OCH3)3, CF3CF2CF2CF2CF2CF2CF2CH2CH2Si(OCH3)3, CF3CF2CF2CF2CF2CF2CF2CF2CH2CH2Si(OCH3)3, CF3(C6H4)Si(OCH3)3 (4-(trifluoromethyl)phenyltrimethoxysilane), CF3Si(OCH2CH3)3, CF Fluoroalkyltrialkoxysilane compounds such as 3CF2Si(OCH2CH3)3, CF3CF2CF2Si(OCH2CH3)3, CF3CF2CF2CF2Si(OCH2CH3)3, CF3CF2CF2CF2CH2CH2Si(OCH2CH3)3, CF3CF2CF2CF2CF2CH2CH2Si(OCH2CH3)3, CF3CF2CF2CF2CF2CF2CH2CH2Si(OCH2CH3)3, CF3CF2CF2CF2CF2CF2CF2CF2CH2CH2Si(OCH2CH3)3, CF3CF2CF2CF2CF2CF2CF2CH2CH2Si(OCH2CH3)3, and CF3(C6H4)Si(OCH2CH3)3 (4-(trifluoromethyl)phenyltriethoxysilane); CF3SiCl(OCH3)2, CF3CF2SiCl(OCH3)2, CF3CF2CF2SiCl(OCH3)2, CF3SiBr(OCH3)2, CF3CF2SiBr(OCH3)2, CF3CF2CF2SiBr(OCH3)2, CF3CF2CF2CF2SiCl(OCH3)2, CF3CH2CH2SiCl(OCH3)2, CF3CF2CF2CF2CH2CH2SiCl(OCH3)2, CF3CF2CF2CF2CF2CF2CH2CH2SiCl(OCH3)2, CF3CF2CF2CF2CF2CF2CF2CF2CH2CH2SiCl(OCH3)2, CF3CF2CF2CF2CF2CF2CF2CH2CH2SiCl(OCH3)2, CF3(C6H4)SiCl(OCH3)2(4-(trifluoromethyl)phenylchlorodimethoxysilane), CF3SiCl(OCH2CH3)2, CF3CF2SiCl(OCH2CH3)2, CF3CF2CF2SiCl(O CF3CF2CF2CF2SiCl(OCH2CH3)2, CF3CH2CH2SiCl(OCH2CH3)2, CF3CF2CF2CF2CH2CH2SiCl(OCH2CH3)2, CF3CF2CF2CF2CF2CH2CH2SiCl(OCH2CH3)2, CF3CF2CF2CF2CF2CF2CH2CH2SiCl(OCH2CH3)2, CF3CF2CF2CF2CF2CF2CF2CH2CH2SiCl(OCH2CH3)2, CF3CF2CF2CF2CF2CF2CF2CF2CH2CH2SiCl(OCH2CH3)2, CF3(C6H4)SiCl(OCH2CH3)2 (4-(trifluoromethyl)phenylchlorodiethoxysilane) and other fluoroalkylhalogenodialkoxysilane compounds; CF3SiCl2(OCH3), CF3CF2SiCl2(OCH3), CF3CF2CF2SiCl2(OCH3), CF3CF2CF2CF2SiCl2(OCH3), CF3CH2CH2SiCl2(OCH3), CF3CF2CF2CF2CH2CH2SiCl2(OCH3), CF3CF2CF2CF2CF2CF2CH2CH2SiCl2(OCH3), CF3CF2CF2CF2CF2CF2CF2CH2CH2SiCl2(OCH3), CF3CF2CF2CF2CF2CF2CF2CF2CH2CH2SiCl2(OCH3), CF3(C6H4)SiCl2(OCH3)(4-(trifluoromethyl)phenyldichloromethoxysilane), CF3SiCl2(OCH2CH3), CF3CF2SiC CF3CF2CF2SiCl2(OCH2CH3), CF3CF2CF2CF2SiCl2(OCH2CH3), CF3CH2CH2SiCl2(OCH2CH3), CF3CF2CF2CF2CH2CH2SiCl2(OCH2CH3), CF3CF2CF2CF2CF2CH2CH2SiCl2(OCH2CH3), CF3CF2CF2CF2CF2CF2CH2CH2SiCl2(OCH2CH3), CF3CF2CF2CF2CF2CF2CH2CH2SiCl2(OCH2CH3)2, CF3CF2CF2CF2CF2CF2CF2CF2CH2CH2SiCl2(OCH2CH3), CF3(C6H4)SiCl2(OCH2CH3)(4-(trifluoromethyl)phenyldichloroethoxysilane) and other fluoroalkyldihalogenoalkoxysilane compounds; CF3SiCl3, CF3CF2SiCl3, CF3SiBr3, CF3CF2SiBr3, CF3CF2CF2SiCl3, CF3CF2CF2CF2SiCl3, CF3CH2CH2SiCl3, CF3CF2CF2CF2CH2CH2SiCl3, CF3CF2CF2CF2CF2CF2CH2CH2SiCl3, CF3CF2CF2CF2CF2CF2CF2CH2CH2SiCl3, CF3CF2CF2CF2CF2CF2CF2CF2CH2CH2SiCl3, and CF3(C6H4)SiCl3 (4-trifluoromethylphenyltrichlorosilane). The silane compounds (1) can be used alone or in combination of two or more. Among these, the silane compound (1) is preferably one included in the fluoroalkyltrialkoxysilane compounds.

[0067] Examples of the silane compound (2) include alkyltrialkoxysilane compounds such as methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrippropoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-propyltrippropoxysilane, n-propyltributoxysilane, n-butyltrimethoxysilane, isobutyltrimethoxysilane, n-pentyltrimethoxysilane, n-hexyltrimethoxysilane, and isooctyltriethoxysilane;

[0068] Alkyl halogenoalkoxysilane compounds such as methyl chlorodimethoxysilane, methyl chlorodiethoxysilane, methyl dichloromethoxysilane, methyl bromodimethoxysilane, ethyl chlorodimethoxysilane, ethyl chlorodiethoxysilane, ethyl dichloromethoxysilane, ethyl bromodimethoxysilane, n-propyl chlorodimethoxysilane, n-propyl dichloromethoxysilane, n-butyl chlorodimethoxysilane, and n-butyl dichloromethoxysilane;

[0069] Alkyltrihalogenosilane compounds such as methyltrichlorosilane, methyltribromosilane, ethyltrichlorosilane, ethyltribromosilane, n-propyltrichlorosilane, n-propyltribromosilane, n-butyltrichlorosilane, isobutyltrichlorosilane, n-pentyltrichlorosilane, n-hexyltrichlorosilane, and isooctyltrichlorosilane; and the like. The silane compound (2) can be used alone or in combination of two or more kinds. Among these, as the silane compound (2), those included in the alkyltrialkoxysilane compounds are preferred.

[0070] The method for polycondensing the silane compound is not particularly limited, and any known method can be used. In particular, a curable polysilsesquioxane compound that satisfies the requirements A1 and A2 can be easily obtained by carrying out a polycondensation reaction under relatively mild conditions over a long period of time. Specifically, a polycondensation reaction of a silane compound is carried out at a prescribed temperature in a solvent or without a solvent using an appropriate amount of an acid catalyst to obtain a reaction liquid containing a production intermediate, and then a base is added to neutralize the reaction liquid, and a polycondensation reaction is further carried out to produce the curable polysilsesquioxane compound (A).

[0071] Examples of the solvent include water, aromatic hydrocarbons such as benzene, toluene, and xylene, esters such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, and methyl propionate, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, and alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, s-butyl alcohol, and t-butyl alcohol. These solvents can be used alone or in combination of two or more. When a solvent is used, the amount of the solvent used is usually 0.001 to 10,000 liters, and preferably 0.010 to 0.9 liters, per mol of the total amount of the silane compounds.

[0072] Examples of the acid catalyst include inorganic acids such as phosphoric acid, hydrochloric acid, boric acid, sulfuric acid, and nitric acid, and organic acids such as citric acid, acetic acid, methanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, and p-toluenesulfonic acid. Among these, at least one selected from phosphoric acid, hydrochloric acid, boric acid, sulfuric acid, citric acid, acetic acid, and methanesulfonic acid is preferred. The amount of the acid catalyst used is usually in the range of 0.01 to 2.00 mol %, preferably 0.05 to 1.00 mol %, and more preferably 0.10 to 0.30 mol %, based on the total molar amount of the silane compounds.

[0073] The reaction temperature in the presence of an acid catalyst is usually 20 to 90°C, preferably 25 to 80°C. The reaction time for the reaction in the presence of an acid catalyst is usually 1 to 48 hours, preferably 3 to 24 hours.

[0074] The mass average molecular weight (Mw) of the production intermediate obtained by the reaction in the presence of an acid catalyst is usually 800 to 5,000, and preferably 1,200 to 4,000.

[0075] Examples of the base used to neutralize the reaction solution include aqueous ammonia; organic bases such as trimethylamine, triethylamine, pyridine, 1,8-diazabicyclo[5.4.0]-7-undecene, aniline, picoline, 1,4-diazabicyclo[2.2.2]octane, and imidazole; organic hydroxides such as tetramethylammonium hydroxide and tetraethylammonium hydroxide; metal alkoxides such as sodium methoxide, sodium ethoxide, sodium t-butoxide, and potassium t-butoxide; metal hydrides such as sodium hydride and calcium hydride; metal hydroxides such as sodium hydroxide, potassium hydroxide, and calcium hydroxide; metal carbonates such as sodium carbonate, potassium carbonate, and magnesium carbonate; and metal hydrogen carbonates such as sodium hydrogen carbonate and potassium hydrogen carbonate.

[0076] The amount of the base used for neutralizing the reaction solution is usually in the range of 0.01 to 2.00 mol %, preferably 0.05 to 1.00 mol %, and more preferably 0.10 to 0.70 mol %, based on the total molar amount of the silane compounds. The amount (mol) of the base used to neutralize the reaction solution is preferably 0.5 to 5.0 times, more preferably 0.8 to 3.0 times, and even more preferably 1.0 to 2.0 times the amount (mol) of the acid catalyst used in the previous step. The pH of the reaction solution after neutralization is usually 6.0 to 8.0, preferably 6.2 to 7.0, and more preferably 6.4 to 6.9.

[0077] The reaction temperature after neutralization is usually 40 to 90°C, preferably 50 to 80°C. The reaction time for the reaction after neutralization is usually 20 to 200 minutes, preferably 30 to 150 minutes.

[0078] In the above-mentioned production method, the main purpose of the reaction in the presence of an acid catalyst is hydrolysis, and the main purpose of the reaction after neutralization is dehydration condensation. By carrying out the polycondensation reaction of the silane compound in this manner, the curable polysilsesquioxane compound (A) can be produced efficiently.

[0079] After completion of the reaction, the curable polysilsesquioxane compound (A) can be isolated by carrying out a known purification treatment.

[0080] In the die bond material of the present invention, the curable polysilsesquioxane compound (A) can be used alone or in combination of two or more.

[0081] The content of the curable polysilsesquioxane compound (A) in the die bond material of the present invention is preferably 40 mass % or more and less than 100 mass %, more preferably 48 to 95 mass %, and even more preferably 56 to 90 mass %, based on the total solid content of the die bond material. In the present invention, the term "solid content" refers to components other than the solvent in the die bonding material.

[0082] [(B) component] The component (B) constituting the die bonding material of the present invention is a thermal acid generator. The thermal acid generator refers to a compound that generates an acid component such as a Lewis acid or a Bronsted acid when heated. The die bonding material of the present invention contains a thermal acid generator and therefore has excellent low-temperature curing properties and storage stability. In the present invention, the term "low-temperature curing property" refers to the property of the die bonding material being cured under mild heating conditions.

[0083] The thermal acid generator preferably has a maximum endothermic peak temperature (acid generating temperature) of 80 to 180°C, as determined by differential scanning calorimetry at a temperature range of 30 to 300°C and a heating rate of 10°C / min. A die bond material containing a thermal acid generator having an acid generation temperature of 80° C. or higher under the above conditions has superior storage stability, while a die bond material containing a thermal acid generator having an acid generation temperature of 180° C. or lower under the above conditions has superior low-temperature curing properties. Since these effects are more easily obtained, the acid generation temperature under the above conditions is preferably 90 to 170°C, and more preferably 100 to 160°C.

[0084] The thermal acid generator may be an onium salt-based thermal acid generator, which contains an onium cation component and an anion component. Examples of the onium cation component include an organic sulfonium ion, an organic ammonium ion, an organic phosphonium ion, and an organic iodonium ion.

[0085] The organic sulfonium ion constituting the onium salt-based thermal acid generator includes a cation represented by the following formula (b-1).

[0086] [ka]

[0087] In formula (b-1), R 6 , R 7 , R 8 are each independently a group selected from the group consisting of an unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted aryl group having 6 to 12 carbon atoms, and a substituted aryl group having 6 to 12 carbon atoms.

[0088] R 6 ~R 8 The "unsubstituted alkyl group having 1 to 10 carbon atoms" represented by the following formula (I) preferably has 1 to 6 carbon atoms, and more preferably has 1 to 3 carbon atoms. Examples of the "unsubstituted alkyl group having 1 to 10 carbon atoms" include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a s-butyl group, a t-butyl group, an n-pentyl group, an n-hexyl group, an n-octyl group, an n-nonyl group, and an n-decyl group.

[0089] R 6 ~R 8The number of carbon atoms in the "alkyl group having 1 to 10 carbon atoms and a substituent" represented by the formula (I) is preferably 1 to 6, and more preferably 1 to 3. Note that this carbon number refers to the number of carbon atoms in the portion excluding the substituent (the alkyl group portion). Therefore, R 6 ~R 8 is a "substituted alkyl group having 1 to 10 carbon atoms", R 6 ~R 8 The number of carbon atoms may exceed 10. Examples of the alkyl group in the "substituted alkyl group having 1 to 10 carbon atoms" include the same groups as those exemplified as the "unsubstituted alkyl group having 1 to 10 carbon atoms".

[0090] The number of atoms of the substituent in the "substituted alkyl group having 1 to 10 carbon atoms" (excluding the number of hydrogen atoms) is usually 1 to 30, and preferably 1 to 20. Examples of the substituent in the "substituted alkyl group having 1 to 10 carbon atoms" include aryl groups such as a phenyl group, an o-tolyl group, a m-tolyl group, a p-tolyl group, a 1-naphthyl group, and a 2-naphthyl group.

[0091] R 6 ~R 8 The number of carbon atoms in the "unsubstituted aryl group having 6 to 12 carbon atoms" represented by the following formula is preferably 6. Examples of the "unsubstituted aryl group having 6 to 12 carbon atoms" include a phenyl group, a 1-naphthyl group, and a 2-naphthyl group.

[0092] R 6 ~R 8 The number of carbon atoms in the "aryl group having 6 to 12 carbon atoms and having a substituent" represented by the formula (I) is preferably 6. Note that this number of carbon atoms refers to the number of carbon atoms in the portion excluding the substituent (the aryl group portion). Therefore, R 6 ~R 8 is a "substituted aryl group having 6 to 12 carbon atoms", R 6 ~R 8 The number of carbon atoms may exceed 12. Examples of the aryl group in the "substituted aryl group having 6 to 12 carbon atoms" include the same groups as those exemplified as the "unsubstituted aryl group having 6 to 12 carbon atoms".

[0093] The number of atoms of the substituent in the "substituted aryl group having 6 to 12 carbon atoms" (excluding the number of hydrogen atoms) is usually 1 to 30, and preferably 1 to 20. Examples of the substituent in the "substituted aryl group having 6 to 12 carbon atoms" include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, s-butyl, isobutyl, t-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, and isooctyl; alkoxy groups such as methoxy and ethoxy; hydroxyl; acyloxy groups such as acetyloxy and propionyloxy; and alkylthio groups such as methylthio and ethylthio.

[0094] Examples of the organic ammonium ion constituting the onium salt-based thermal acid generator include the cation represented by the following formula (b-2).

[0095] [ka]

[0096] In formula (b-2), R 9 , R 10 , R 11 , R 12 are each independently a group selected from the group consisting of an unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted aryl group having 6 to 12 carbon atoms, and a substituted aryl group having 6 to 12 carbon atoms. R 9 ~R 12 As for R 6 ~R 8 Examples of the above-mentioned formulas are the same as those shown in the above formula.

[0097] As the organic phosphonium ion constituting the onium salt-based thermal acid generator, a cation represented by the following formula (b-3) can be mentioned.

[0098] [ka]

[0099] In formula (b-3), R 13 , R 14 , R 15 , R 16 are each independently a group selected from the group consisting of an unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted aryl group having 6 to 12 carbon atoms, and a substituted aryl group having 6 to 12 carbon atoms. R 13 ~R 16 As for R 6 ~R 8 Examples of the above-mentioned formulas are the same as those shown in the above formula.

[0100] As an organic iodonium ion constituting an onium salt-based thermal acid generator, a cation represented by the following formula (b-4) can be mentioned.

[0101] [ka]

[0102] In formula (b-4), R 17 , R 18 are each independently a group selected from the group consisting of an unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted alkyl group having 1 to 10 carbon atoms, an unsubstituted aryl group having 6 to 12 carbon atoms, and a substituted aryl group having 6 to 12 carbon atoms. R 17 , R 18 As for R 6 ~R 8 Examples of the above-mentioned formulas are the same as those shown in the above formula.

[0103] Among these, from the viewpoint of achieving both the curability and storage stability of the die bonding material, the onium cation component is preferably an organic sulfonium ion or an organic ammonium ion, and more preferably an organic sulfonium ion represented by the following formula (b-5).

[0104] [ka]

[0105] In formula (b-5), Ar represents an aryl group having or having no substituent, such as a phenyl group, an o-tolyl group, a m-tolyl group, a p-tolyl group, a 1-naphthyl group, or a 2-naphthyl group.

[0106] Examples of the anion component of the onium salt-based thermal acid generator include a trifluoromethanesulfonate anion, a hexafluorophosphate anion, a hexafluoroantimonate anion, a perfluorobutanesulfonate anion, a tetrakis(pentafluorophenyl)borate anion, and a tetrafluoroborate anion.

[0107] Among these, the anion component is preferably a hexafluorophosphate anion, a hexafluoroantimonate anion, or a tetrakis(pentafluorophenyl)borate anion, because a cured product having excellent optical properties can be easily obtained, and more preferably a hexafluorophosphate anion.

[0108] The thermal acid generators can be used alone or in combination of two or more. The content of the thermal acid generator is usually more than 0 and not more than 0.6 parts by mass, preferably 0.001 to 0.6 parts by mass, and more preferably 0.005 to 0.5 parts by mass, per 100 parts by mass of the polysilsesquioxane compound (A). If the amount of the thermal acid generator is too large, the adhesiveness of the cured product may decrease.

[0109] 〔solvent〕 The solvent constituting the die bonding material of the present invention is not particularly limited as long as it can dissolve or disperse the components of the die bonding material of the present invention. Examples of the solvent include acetates such as diethylene glycol monobutyl ether acetate and 1,6-hexanediol diacetate; tripropylene glycol-n-butyl ether; diglycidyl ethers such as glycerin diglycidyl ether, butanediol diglycidyl ether, diglycidyl aniline, neopentyl glycol glycidyl ether, cyclohexanedimethanol diglycidyl ether, alkylene diglycidyl ether, polyglycol diglycidyl ether, and polypropylene glycol diglycidyl ether; triglycidyl ethers such as trimethylolpropane triglycidyl ether and glycerin triglycidyl ether; and vinylhexene oxides such as 4-vinylcyclohexene monoxide, vinylcyclohexene dioxide, and methylated vinylcyclohexene dioxide. The solvents can be used alone or in combination of two or more.

[0110] The die bond material of the present invention has a solid content of preferably 50% by mass or more and less than 100% by mass, more preferably 60 to 90% by mass, and even more preferably 65 to 85% by mass. By having the solid content within this range, it becomes easier to obtain a die bond material that has excellent workability in the coating process.

[0111] [(C) component] The die bond material of the present invention may contain a silane coupling agent as component (C). By using a die bond material containing a silane coupling agent, it becomes easier to form a cured product with superior adhesiveness. The silane coupling agent refers to a silane compound having a silicon atom, a functional group, and a hydrolyzable group bonded to the silicon atom. The functional group refers to a group that has reactivity with other compounds (mainly organic substances), and examples thereof include groups having a nitrogen atom such as an amino group, a substituted amino group, an isocyanate group, a ureido group, and a group having an isocyanurate skeleton; an acid anhydride group; a vinyl group; an allyl group; an epoxy group; a (meth)acrylic group; a mercapto group; and the like. In the present invention, the silane coupling agent may be used alone or in combination of two or more kinds.

[0112] When the die bonding material of the present invention contains a silane coupling agent, the content thereof is not particularly limited and can be appropriately determined depending on the purpose. The content of the silane coupling agent is usually 95 parts by mass or less, preferably 65 parts by mass or less, and more preferably 35 parts by mass or less, per 100 parts by mass of the curable polysilsesquioxane compound (A).

[0113] As the silane coupling agent, a silane coupling agent having a nitrogen atom in the molecule or a silane coupling agent having an acid anhydride structure in the molecule is preferable.

[0114] Die bonding materials containing a silane coupling agent having a nitrogen atom in the molecule or a silane coupling agent having an acid anhydride structure in the molecule tend to give a cured product having superior heat resistance and adhesiveness.

[0115] Examples of the silane coupling agent having a nitrogen atom in the molecule include a trialkoxysilane compound represented by the following formula (c-1), a dialkoxyalkylsilane compound or a dialkoxyarylsilane compound represented by the following formula (c-2), and the like.

[0116] [ka]

[0117] In the above formula, R arepresents an alkoxy group having 1 to 6 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, or a t-butoxy group. a They may be the same or different. R b represents an alkyl group having 1 to 6 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, or a t-butyl group; or an aryl group having or having no substituent, such as a phenyl group, a 4-chlorophenyl group, a 4-methylphenyl group, or a 1-naphthyl group.

[0118] R c represents an organic group having 1 to 10 carbon atoms and a nitrogen atom. c may further be bonded to another group containing a silicon atom. R c Specific examples of the organic group having 1 to 10 carbon atoms include an N-2-(aminoethyl)-3-aminopropyl group, a 3-aminopropyl group, an N-(1,3-dimethyl-butylidene)aminopropyl group, a 3-ureidopropyl group, and an N-phenyl-aminopropyl group.

[0119] Among the compounds represented by the above formula (c-1) or (c-2), R c Compounds in which is an organic group bonded to another group containing a silicon atom include silane coupling agents having an isocyanurate skeleton (isocyanurate-based silane coupling agents) and silane coupling agents having a urea skeleton (urea-based silane coupling agents).

[0120] Among these, as silane coupling agents having a nitrogen atom in the molecule, isocyanurate-based silane coupling agents and urea-based silane coupling agents are preferred because they tend to give cured products with superior adhesion, and furthermore, those having four or more alkoxy groups bonded to silicon atoms in the molecule are preferred. "Having four or more alkoxy groups bonded to a silicon atom" means that the total number of alkoxy groups bonded to the same silicon atom and alkoxy groups bonded to different silicon atoms is four or more.

[0121] An example of an isocyanurate-based silane coupling agent having four or more alkoxy groups bonded to a silicon atom is a compound represented by the following formula (c-3): An example of an urea-based silane coupling agent having four or more alkoxy groups bonded to a silicon atom is a compound represented by the following formula (c-4):

[0122] [ka]

[0123] In the formula, R a has the same meaning as above. t1 to t5 each independently represent an integer of 1 to 10, preferably an integer of 1 to 6, and particularly preferably 3.

[0124] Among these, as the silane coupling agent having a nitrogen atom in the molecule, it is preferable to use 1,3,5-N-tris(3-trimethoxysilylpropyl)isocyanurate, 1,3,5-N-tris(3-triethoxysilylpropyl)isocyanurate (hereinafter referred to as "isocyanurate compound"), N,N'-bis(3-trimethoxysilylpropyl)urea, N,N'-bis(3-triethoxysilylpropyl)urea (hereinafter referred to as "urea compound"), and combinations of the above-mentioned isocyanurate compounds and urea compounds.

[0125] When the die bonding material of the present invention contains a silane coupling agent having a nitrogen atom in the molecule, its content is not particularly limited, but the mass ratio of the above-mentioned (A) component to the silane coupling agent having a nitrogen atom in the molecule [(A) component: silane coupling agent having a nitrogen atom in the molecule] is preferably 100:0.1 to 100:90, more preferably 100:0.3 to 100:60, more preferably 100:1 to 100:50, even more preferably 100:3 to 100:40, and particularly preferably 100:5 to 100:35. The cured product of the die bonding material containing the component (A) and the silane coupling agent having a nitrogen atom in the molecule in such a ratio exhibits superior heat resistance and adhesiveness.

[0126] Silane coupling agents having an acid anhydride structure in the molecule are organosilicon compounds having both a group having an acid anhydride structure and a hydrolyzable group in one molecule.Specific examples include compounds represented by the following formula (c-5).

[0127] [ka]

[0128] In the formula, Q represents a group having an acid anhydride structure, R d represents an alkyl group having 1 to 6 carbon atoms or a phenyl group having or without a substituent, R e represents an alkoxy group having 1 to 6 carbon atoms or a halogen atom, i and k represent integers of 1 to 3, j represents an integer of 0 to 2, and i+j+k=4. When j is 2, R d may be the same or different. When k is 2 or 3, multiple R e When i is 2 or 3, multiple Q's may be the same or different. Q includes groups represented by the following formulas, and the group represented by (Q1) is particularly preferred.

[0129] [ka]

[0130] In the formula, h represents an integer of 0 to 10.

[0131] Examples of silane coupling agents having an acid anhydride structure in the molecule include tri(C1-6)alkoxysilyl(C2-8)alkyl succinic anhydrides such as 2-(trimethoxysilyl)ethyl succinic anhydride, 2-(triethoxysilyl)ethyl succinic anhydride, 3-(trimethoxysilyl)propyl succinic anhydride, and 3-(triethoxysilyl)propyl succinic anhydride; Di(C1-6)alkoxymethylsilyl(C2-8)alkyl succinic anhydrides, such as 2-(dimethoxymethylsilyl)ethyl succinic anhydride; (C1-6)alkoxydimethylsilyl(C2-8)alkyl succinic anhydrides, such as 2-(methoxydimethylsilyl)ethyl succinic anhydride;

[0132] Trihalogenosilyl (C2-8) alkyl succinic anhydrides, such as 2-(trichlorosilyl)ethyl succinic anhydride and 2-(tribromosilyl)ethyl succinic anhydride; Dihalogenomethylsilyl (C2-8) alkyl succinic anhydrides, such as 2-(dichloromethylsilyl)ethyl succinic anhydride; halogenodimethylsilyl (C2-8) alkyl succinic anhydrides such as 2-(chlorodimethylsilyl)ethyl succinic anhydride; and the like.

[0133] Among these, as the silane coupling agent having an acid anhydride structure in the molecule, tri(C1-6)alkoxysilyl(C2-8)alkyl succinic anhydride is preferred, and 3-(trimethoxysilyl)propyl succinic anhydride or 3-(triethoxysilyl)propyl succinic anhydride is particularly preferred.

[0134] When the die bonding material of the present invention contains a silane coupling agent having an acid anhydride structure in its molecule, its content is not particularly limited, but the mass ratio of the above-mentioned (A) component to the silane coupling agent having an acid anhydride structure in its molecule [(A) component: silane coupling agent having an acid anhydride structure in its molecule] is preferably 100:0.1 to 100:30, more preferably 100:0.3 to 100:20, more preferably 100:0.5 to 100:15, and even more preferably 100:1 to 100:10. The cured product of the die bonding material containing the component (A) and the silane coupling agent having an acid anhydride structure in the molecule in such a ratio exhibits superior adhesiveness.

[0135] The die bonding material of the present invention may contain components other than the above components (A) to (C) to the extent that the object of the present invention is not impaired. Examples of other components include fine particles, antioxidants, ultraviolet absorbers, and light stabilizers.

[0136] By adding fine particles, it may be possible to obtain a die bond material that is excellent in workability in the coating process. Examples of the material of the fine particles include metals, metal oxides, minerals, metal carbonates such as calcium carbonate and magnesium carbonate, metal sulfates such as calcium sulfate and barium sulfate, metal hydroxides such as aluminum hydroxide, metal silicates such as aluminum silicate, calcium silicate and magnesium silicate, inorganic components such as silica, silicone, and organic components such as acrylic polymers. The fine particles used may be surface-modified.

[0137] These fine particles can be used alone or in combination of two or more. The content of the fine particles is not particularly limited, but is usually preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less, based on the (A) component.

[0138] The antioxidant is added to prevent oxidative deterioration during heating. Examples of the antioxidant include phosphorus-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants.

[0139] Examples of phosphorus-based antioxidants include phosphites, oxaphosphaphenanthrene oxides, etc. Examples of phenol-based antioxidants include monophenols, bisphenols, polymeric phenols, etc. Examples of sulfur-based antioxidants include dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, etc.

[0140] These antioxidants may be used alone or in combination of two or more. The amount of the antioxidant used is usually 10 mass % or less based on the component (A).

[0141] The ultraviolet absorber is added for the purpose of improving the light resistance of the resulting cured product. Examples of the ultraviolet absorbent include salicylic acids, benzophenones, benzotriazoles, and hindered amines. The ultraviolet absorbents can be used alone or in combination of two or more. The amount of the ultraviolet absorber used is usually 10% by mass or less based on the component (A).

[0142] The light stabilizer is added for the purpose of improving the light resistance of the resulting cured product. Examples of the light stabilizer include hindered amines such as poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidine)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidine)imino}]. These light stabilizers may be used alone or in combination of two or more. The amount of the light stabilizer used is usually 20% by mass or less based on the component (A).

[0143] The die bonding material of the present invention can be prepared, for example, by mixing the above-mentioned components (A), (B), and a solvent, as well as other components as desired, in a predetermined ratio, and then degassing the mixture. The mixing method and the degassing method are not particularly limited, and known methods can be used.

[0144] The die bond material of the present invention contains component (A), and therefore has a low refractive index. The refractive index (nD) of the die bonding material of the present invention at 25° C. is preferably 1.410 to 1.430, and more preferably 1.412 to 1.428. The refractive index (nD) of the die bond material can be measured by the method described in the Examples.

[0145] The die bond material of the present invention contains component (B), and therefore has low-temperature curing properties and excellent storage stability.

[0146] The low-temperature curing property of the die bonding material of the present invention can be confirmed, for example, by the method described in the Examples. That is, when a sample of die bond material is placed on a stainless steel plate heated to 100°C and stirred using an automatic curing time measuring device (manufactured by Cyber ​​Corporation, product name "Madoka"), the stirring torque increases. Therefore, by measuring the time it takes for the stirring torque to reach 0.049 N·cm, it is possible to quantify the low-temperature curing property of the die bond material (the curing property of the die bond material under the relatively mild heating condition of 100°C). The time required for the stirring torque to reach 0.049 N·cm is preferably from 200 to 2500 seconds, more preferably from 220 to 2000 seconds, and even more preferably from 240 to 1500 seconds.

[0147] The excellent storage stability of the die bonding material of the present invention can be confirmed, for example, by the method described in the Examples. That is, in a rheometer, a cone plate with a radius of 50 mm and a cone angle of 0.5° is used, and the shear rate is 2 s at 25°C.-1 The viscosity at this time is measured to obtain the initial viscosity, and then the sample is allowed to stand at 25°C for 24 hours, and the viscosity is measured under the same conditions to obtain the viscosity after standing. The storage stability can be quantified by calculating the rate of increase in viscosity from the obtained measured value based on the following formula. [Viscosity increase rate] = [Viscosity after standing] / [Initial viscosity] The viscosity increase rate under the above measurement conditions is preferably 1.40 or less, more preferably 1.25 or less, and even more preferably 1.10 or less.

[0148] As described above, the die bonding material of the present invention has excellent storage stability, and therefore can be stored for a long period of time without freezing or refrigerating.

[0149] The die bonding material of the present invention can be cured by heating. The heating temperature during curing is usually 80 to 140° C., more preferably 90 to 120° C. The heating time is usually 10 minutes to 20 hours, preferably 30 minutes to 15 hours. When the die bond material of the present invention is cured, if the heating temperature is high, it can be cured in a short time, whereas if it is heated for a long time, the heating temperature can be lowered. Thus, the die bond material of the present invention can be cured at a relatively low temperature. Therefore, as described later, when there are surrounding components such as resin components whose heat resistance should be considered, a heating temperature of 95°C to 105°C can be adopted while also taking into consideration productivity, etc.

[0150] The cured product obtained by curing the die bonding material of the present invention preferably has excellent heat resistance and adhesiveness. The heat resistance and adhesiveness of the cured product can be confirmed, for example, as follows. That is, a predetermined amount of the die bond material of the present invention is applied to the mirror surface of a silicon chip, the applied surface is placed on an adherend, pressed, and cured by heat treatment. This is left for 30 seconds on the measurement stage of a bond tester that has been heated to a predetermined temperature (e.g., 100°C), and a stress is applied to the adhesive surface in the horizontal direction (shear direction) from a position 100 μm above the adherend, and the adhesive force between the test piece and the adherend is measured.

[0151] The adhesive strength of the cured product is 15N / 4mm under the measurement conditions described in the examples. 2 More than 25N / 4mm is preferable. 2 More preferably, it is 30N / 4mm or more. 2 More preferably, it is equal to or greater than this. In this specification, "4 mm 2 " means "2mm square," that is, 2mm x 2mm (a square with each side measuring 2mm).

[0152] The die bonding material of the present invention preferably satisfies the following requirement X. [Requirement X] When the solid-state Si nuclear magnetic resonance spectrum of the cured product of the die bond material is measured, a peak is observed in the region of -80 ppm or more and less than -40 ppm, and the half-width of the peak is 500 Hz or more and 900 Hz or less.

[0153] The half-width of a peak is the width of the peak shape cut at half the value of the peak value (height) of the solid-state Si nuclear magnetic resonance spectrum. For example, if the peak values ​​when the peak shape is cut at half the peak value are a (ppm) and b (ppm) respectively (b>a), it can be expressed by the formula: (ba) × M (unit: Hz, M is the resonance frequency). The half width of the peak observed in the region of −80 ppm or more and less than −40 ppm is preferably 500 Hz or more and 900 Hz or less, more preferably 500 Hz or more and 800 Hz or less, further preferably 500 Hz or more and 700 Hz or less, and particularly preferably 500 Hz or more and 600 Hz or less. When the half width of the peak observed in the region of -80 ppm or more and less than -40 ppm is 500 Hz or more and 900 Hz or less, a die bond material that becomes a cured product with superior adhesive strength is easily obtained.

[0154] When multiple overlapping peaks are observed in the region between -80 ppm and -40 ppm, the half-width of each peak can be determined by waveform separation analysis using a Gaussian function or a Lorentz function. In addition, when a solid-state Si nuclear magnetic resonance spectrum of the cured product is measured, if multiple peaks are observed in the region of -80 ppm or more and less than -40 ppm, a die bond material that satisfies the above requirement X is one in which the half-width of at least one peak included in this region is within the above range. The solid-state Si nuclear magnetic resonance spectrum can be measured at room temperature (for example, 25° C.) according to a conventional method.

[0155] The half-width of the peak in the chemical shift region of -80 ppm or more and less than -40 ppm is determined by the (R 1 -D) or R 2 It is affected by the type of component (A) and by components other than component (A). Therefore, a die bond material that satisfies the above-mentioned requirement X can be efficiently obtained by obtaining a curable polysilsesquioxane compound (A), measuring the solid-state Si nuclear magnetic resonance spectrum of the cured product, determining the half-width of the peak in the above-mentioned region, and then appropriately determining the amounts of components other than component (A) to be added depending on the value.

[0156] In addition, as long as a cured product obtained by sufficiently curing a die bond material is used as a measurement sample when measuring a solid-state Si nuclear magnetic resonance spectrum, the chemical shift and half-width of the peak usually do not depend on the curing conditions, etc. In the case of the die bond material of the present invention, for example, a cured product suitable as a measurement sample can be obtained by carrying out a curing reaction at 170° C. for 2 hours. Whether the curing reaction has progressed sufficiently and the sample is suitable for use as a measurement sample can be confirmed, for example, by checking whether there is almost no weight loss due to heating by thermogravimetry with differential thermal analysis (TG-DTA).

[0157] The die bond material of the present invention is suitably used when fixing a light emitting element at a predetermined position. That is, by using the die bond material of the present invention, the light emitting element can be firmly fixed. Furthermore, as described later, by using the die bond material of the present invention, it is possible to obtain the effect of improving the light extraction efficiency of a light emitting device. Details of the method for fixing the light emitting element in a predetermined position using the die bonding material of the present invention will be described in the explanation of the invention of the manufacturing method of the light emitting device.

[0158] 2) Light-emitting device The light-emitting device of the present invention is a light-emitting device comprising: a pair of lead electrodes; a molded body molded integrally with the pair of lead electrodes; and an element container having a recess, the bottom of which is constituted by the pair of lead electrodes; and a light-emitting element fixed via an adhesive member onto at least one of the pair of lead electrodes constituting the bottom of the recess, wherein the adhesive member is a hardened product of the die-bonding material of the present invention.

[0159] Hereinafter, the embodiments of the invention will be described with reference to the drawings as appropriate. However, the light emitting device described below is intended to embody the technical concept of the present invention, and the present invention is not limited to the following unless otherwise specified. Furthermore, the sizes and positional relationships of the components shown in the drawings may be exaggerated for clarity of explanation.

[0160] In the following, the visible wavelength range is defined as the wavelength range of 380 nm or more and 780 nm or less, the blue range is the wavelength range of 420 nm or more and 480 nm or less, the green to yellow range is the wavelength range of 500 nm or more and 590 nm or less, and the red range is the wavelength range of 610 nm or more and 750 nm or less.

[0161] <Embodiment 1> 1 and 4 are respectively a schematic front view and a schematic bottom view of a light emitting device 1100 according to embodiment 1, FIG. 2 is a schematic cross-sectional view taken along line AA in FIG. 1, and FIG. 3 is a schematic cross-sectional view taken along line BB in FIG.

[0162] The light emitting device 1100 according to the first embodiment includes an element receptacle 110 and two light emitting elements 121. The light emitting device 1100 and the element receptacle 110 are long in the horizontal direction (left-right direction in FIG. 1). The element receptacle 110 has a recess 110a. The recess 110a is long in the horizontal direction, similar to the element receptacle 110. The element receptacle 110 includes a first lead electrode 111 and a second lead electrode 112 (a pair of lead electrodes 111, 112), and a molded body 115 molded integrally with the first lead electrode 111 and the second lead electrode 112. The first lead electrode 111 and the second lead electrode 112 are aligned in the horizontal direction. The first lead electrode 111 and the second lead electrode 112 form the bottom of the recess 110a. The molded body 115 forms the side wall of the recess 110a. The two light emitting elements 121 are housed in the recess 110a.

[0163] More specifically, the light emitting device 1100 is a light emitting diode (LED). The recess 110a is provided on one of the side surfaces (front surface) of the element container 110. The molded body 115 contains a white pigment and a filler, and is light reflective due to the white pigment in particular. Therefore, the light emitting area of ​​the light emitting device 1100 (unintended light leakage is not taken into consideration) is approximately aligned with the opening of the recess 110a on the front surface. The first lead electrode 111 and the second lead electrode 112 of the first embodiment are symmetrical with respect to the center of the light emitting device 1100 (element container 110) in the lateral direction. The bottom of the recess 110a is formed by the surface of the molded body 115 and the surfaces of the first lead electrode 111 and the second lead electrode 112. The portions of the first lead electrode 111 and the second lead electrode 112 constituting the bottom of the recess 110a are the first element mounting portion 111a and the second element mounting portion 112a including the bonding area of ​​the light emitting element 121 and the connection area of ​​the wire 150. The two light emitting elements 121 are fixed (mounted) on the first lead electrode 111 (first element mounting portion 111a) and the second lead electrode 112 (second element mounting portion 112a) at the bottom of the recess 110a, respectively, via adhesive members 160. The portion of the second lead electrode 112 includes the connection area of ​​the wire 150. Furthermore, the first lead electrode 111 and the second lead electrode 112 have the first external connection terminal portion 111b and the second external connection terminal portion 112b as portions located outside the molded body 115. The first external connection terminal portion 111b and the second external connection terminal portion 112b are bent so as to fit along the lower surface of the molded body 115. The light emitting device 1100 is mounted by soldering the first external connection terminal 111b and the second external connection terminal 112b to a circuit board or the like. Therefore, the mounting side main surface of the light emitting device 1100 (element container 110) is the lower surface. More specifically, the lower surface of the molded body 115 has regions (left region or right region) on the left and right sides where the first external connection terminal 111b and the second external connection terminal 112b are respectively arranged, and is stepped from the central region of the lower surface of the molded body 115 to the left region or right region. Accordingly, the shape of the front surface of the element container 110 (molded body 115) and the shape of the opening of the recess 110a are formed such that the central region is wider (i.e., the vertical width is larger) on the lower side than the left region or right region.

[0164] The molded body 115 has a reinforcing portion 117 that connects two side walls 1151, 1152 facing each other in the vertical direction of the recess 110a (the up-down direction in FIG. 1). The height of the reinforcing portion 117 is higher than the surfaces of the first lead electrode 111 and the second lead electrode 112 at the bottom of the recess 110a and is lower than the height of the upper surface (front surface) of the light emitting element 121.

[0165] The reinforcing portion 117 is located at approximately the center of the lateral direction of the recess 110a and on a separation region 1150 separating the first lead electrode 111 and the second lead electrode 112, and is continuous with the separation region 1150. In detail, the reinforcing portion 117 is located between the two light emitting elements 121, and a part of the reinforcing portion 117 covers the peripheral portion of the first lead electrode 111 and the second lead electrode 112 at the bottom of the recess 110a. The vicinity of the separation region 1150 of the molded body 115 is a portion where damage such as cracking of the molded body 115 is likely to occur, so that the reinforcing portion 117 can reinforce the vicinity of the separation region 1150 of the molded body 115. This allows the first lead electrode 111 and the second lead electrode 112 to be firmly held by the molded body 115.

[0166] Reinforcing portion 117 can appropriately suppress blocking of light from light emitting element 121, hardly affecting the light distribution of light emitting device 1100, and can effectively increase the mechanical strength of molded body 115 to suppress deformation. Therefore, it is possible to obtain element container 110 that is resistant to deformation due to external forces, heating during reflow solder mounting, and / or temperature changes due to heat generated by light emitting element 121 and wavelength converting material 140 (described later), and that easily obtains a desired light distribution.

[0167] The light emitting device 1100 is preferably of a side-emitting type (side-view type).

[0168] The light emitting device 1100 includes a sealing member 130. The sealing member 130 is filled in the recess 110a. The sealing member 130 contains a wavelength conversion material 140 that converts the light emitted by the light emitting element 121 into light of a different wavelength. The wavelength conversion material 140 contains a first phosphor that emits green to yellow light and a second phosphor that emits red light. In this case, it is preferable that the light emitting element 121 is an element that emits blue light. With this configuration, light emission with excellent color reproducibility or color rendering is possible.

[0169] Furthermore, the second phosphor preferably contains a manganese-activated fluoride phosphor, which is capable of emitting light with a narrow spectral half-width in the red range.

[0170] The base material of the sealing member 130 is preferably a silicone-based resin containing a phenyl group. The silicone-based resin is a thermosetting resin having excellent heat resistance and light resistance, and the heat resistance is further enhanced by containing a phenyl group. The silicone-based resin containing a phenyl group has a relatively high gas barrier property among silicone-based resins, so that it is easy to suppress the deterioration of the manganese-activated fluoride phosphor due to moisture. In addition, it is easy to suppress the deterioration of the first lead electrode 111 and the second lead electrode 112 and the wire 150 described later due to corrosive gases such as sulfur-containing gas. Note that, in order to suppress the deterioration due to moisture and heat, it is preferable that the manganese-activated fluoride phosphor is present more on the rear side than the front side in the sealing member 130, that is, on the bottom side of the recess 110a.

[0171] The light emitting device 1100 includes a wire 150 that connects the first lead electrode 111 and the second lead electrode 112 to the light emitting element 121. The wire 150 is housed in the recess 110a and sealed in the sealing member 130. From the viewpoint of enhancing light reflectivity, the wire 150 preferably contains silver. That is, the wire 150 preferably has at least a surface made of silver or a silver alloy, and is more preferably a silver wire or a silver alloy wire. Furthermore, from the viewpoint of preventing breakage, the silver-containing wire 150 is preferably a gold wire having a silver or silver alloy coating on its surface, or a silver alloy wire containing gold.

[0172] The molded body 115 has a gate mark 115a at the rear molded portion covering the rear surfaces of the first lead electrode 111 and the second lead electrode 112. Such a molded body 115 is mainly molded by an injection molding method. In the injection molding method, a resin with a relatively high melt viscosity is forcefully injected into a cavity of a mold from a gate. Therefore, the front surfaces of the first lead electrode 111 and the second lead electrode 112, particularly the first element mounting portion 111a and the second element mounting portion 112a, are pressed against the mold by the pressure of the resin, and the occurrence of burrs on the first element mounting portion 111a and the second element mounting portion 112a is suppressed. In addition, by covering both the front and rear surfaces of the first lead electrode 111 and the second lead electrode 112 in this way, the first lead electrode 111 and the second lead electrode 112 can be firmly held by the molded body 115. For example, thermoplastic resin and unsaturated polyester resin are suitable for such a configuration of molded body 115 because they are relatively difficult to adhere to first lead electrode 111 and second lead electrode 112. The "gate mark" is a protrusion formed on molded body 115 as a mark of a gate, which is an injection port for resin into a cavity of a mold. The front molded portion of molded body 115 mainly constitutes the side wall surrounding recess 110a.

[0173] Hereinafter, each component of the light emitting device according to one embodiment of the present invention will be described.

[0174] (Light emitting device 1100) The light emitting device is configured by housing a light emitting element in an element container and electrically connecting the light emitting element to a pair of lead electrodes, and is preferably further sealed with a sealing member. The light emitting device may be, for example, a light emitting diode (LED).

[0175] (Element container 110) The element container is a container that contains a light-emitting element and has electrodes (terminals) for supplying power to the light-emitting element from the outside. The element container is composed of at least a pair of lead electrodes and a molded body. The element container may be, for example, what is called a "package."

[0176] (First lead electrode 111, second lead electrode 112) A pair of lead electrodes (first lead electrode and second lead electrode) constitute a pair of positive and negative electrodes (terminals) in the element container. In one element container, at least one pair of lead electrodes is sufficient, but there may be multiple pairs. The lead electrode is a base material made of a flat plate of zinc, iron, copper, lead, phosphorus, or an alloy thereof, which is subjected to various processes such as pressing (including punching), etching, and rolling. The lead electrode may be composed of a laminate of these metals or alloys, but it is convenient to compose it as a single layer. In particular, a copper alloy (phosphor bronze, copper containing iron, etc.) containing copper as the main component is preferable. In addition, a light-reflecting film such as nickel, palladium, gold, silver, or an alloy thereof may be provided on the surface, and silver or a silver alloy having excellent light reflectivity is preferable. In particular, a silver or silver alloy film (e.g., a plating film) using a sulfur-based gloss agent has a smooth surface and can obtain extremely high light reflectivity.

[0177] (Molded body 115) The molded body forms a base of a container in the element container. The molded body constitutes a part of the outer shape of the element container. From the viewpoint of light reflectivity, the light reflectance of the molded body at the emission peak wavelength of the light emitting element is preferably 75% or more, and more preferably 90% or more. Furthermore, the molded body is preferably white. Before curing, the molded body passes through a state having fluidity, that is, a liquid state (including a sol state or a slurry state). The molded body can be molded by injection molding, transfer molding, or the like.

[0178] (Base material for molded body) Thermosetting resins or thermoplastic resins can be used as the base material of the molded body. The resins shown below include modified resins and hybrid resins. An example of a thermosetting resin is an unsaturated polyester resin. A thermoplastic resin is also preferable as the base material of the molded body. Generally, a thermoplastic resin is cheaper than a thermosetting resin, but has poor heat resistance and light resistance and is easily deformed. Examples of the thermoplastic resin include polyamide resins such as 9C nylon (registered trademark) resin and 9T nylon (registered trademark) resin. From the viewpoints of light reflectivity, mechanical strength, thermal expansion and contraction, the molded body preferably contains the following white pigment and filler in the base material, but is not limited thereto.

[0179] (White pigment) Examples of the white pigment include titanium oxide. Titanium oxide is preferable because it has a relatively high refractive index and excellent light-hiding properties. The shape of the white pigment is not particularly limited, and may be amorphous (crushed), but is preferably spherical from the viewpoint of fluidity. The particle size of the white pigment (hereinafter, "particle size" is defined, for example, as the average particle size D50) is not particularly limited, and is, for example, 0.01 μm to 1 μm, and preferably 0.1 μm to 0.5 μm. The content of the white pigment in the molded body is not particularly limited, and is preferably high from the viewpoint of the light reflectivity of the molded body, but is preferably 20% by mass to 70% by mass, and more preferably 30% by mass to 60% by mass, taking into account the influence on fluidity. The mass % represents the ratio of the weight of each material to the total weight of all constituent materials.

[0180] (Filler for Molded Body) Examples of the filler include calcium silicate (wollastonite). Calcium silicate (wollastonite) is preferred as a reinforcing agent, and is suitable for thin or small molded bodies because of its relatively small diameter. Specifically, the average fiber diameter of the reinforcing agent is not particularly limited, and is, for example, 0.05 μm or more and 100 μm or less, preferably 0.1 μm or more and 50 μm or less, more preferably 1 μm or more and 30 μm or less, and even more preferably 2 μm or more and 15 μm or less. The average fiber length of the reinforcing agent is not particularly limited, and is, for example, 0.1 μm or more and 1 mm or less, preferably 1 μm or more and 200 μm or less, more preferably 3 μm or more and 100 μm or less, and even more preferably 5 μm or more and 50 μm or less. The average aspect ratio (average fiber length / average fiber diameter) of the reinforcing agent is not particularly limited, and is, for example, 2 to 300 or less, preferably 2 to 100 or less, more preferably 3 to 50 or less, and even more preferably 5 to 30 or less. The shape of the filler is not particularly limited, and may be amorphous (crushed), but from the viewpoint of its function as a reinforcing agent, it is preferably fibrous (needle-like) or plate-like (scale-like), and from the viewpoint of fluidity, it is preferably spherical. The content of the filler in the molded product is not particularly limited, and may be appropriately determined in consideration of the thermal expansion coefficient, mechanical strength, etc. of the molded product, but is preferably 10% by mass to 80% by mass, more preferably 30% by mass to 60% by mass (of which, the reinforcing agent is preferably 5% by mass to 30% by mass, more preferably 5% by mass to 20% by mass).

[0181] (Light emitting element 121) A semiconductor light-emitting element can be used as the light-emitting element. A light-emitting element often has a substrate, but it is sufficient if it has at least an element structure made of various semiconductors and a pair of positive and negative (pn) electrodes. In particular, nitride semiconductors (In x Al y Ga 1-x-yN, 0≦x, 0≦y, x+y≦1) is preferred. The emission peak wavelength of the light-emitting element is preferably in the range of 445 nm to 465 nm in terms of light emission efficiency, color mixing with light from other light sources, excitation efficiency of wavelength conversion substances, etc. In the case of a light-emitting element having a pair of positive and negative electrodes provided on the same side, each electrode is connected to a pair of lead electrodes by wires (face-up mounting). The number of light-emitting elements mounted in one element container may be one or more. Multiple light-emitting elements can be connected in series or parallel by wires.

[0182] (Sealing member 130) The sealing member is a member that seals the light-emitting element to protect it from dust, moisture, external forces, etc. The sealing member may be any member that has electrical insulation properties and is translucent to the light emitted from the light-emitting element (preferably has a light transmittance of 70% or more, more preferably 85% or more at the emission peak wavelength of the light-emitting element). The sealing member preferably contains at least a wavelength conversion substance in its base material, but is not limited thereto.

[0183] (Base material for sealing components) The base material of the sealing member may be a silicone-based resin or a modified silicone resin containing a phenyl group.

[0184] (Wavelength conversion material 140) The wavelength conversion material absorbs at least a part of the primary light emitted from the light emitting element and emits secondary light having a wavelength different from the primary light. This allows a light emitting device to emit a mixed color light (e.g., white light) of the primary light and the secondary light having a visible wavelength. The wavelength conversion material may be one of the specific examples shown below, or two or more of them may be combined.

[0185] (First phosphor) The first phosphor emits green to yellow light. From the viewpoints of luminous efficiency, color mixing relationship with light from other light sources, etc., the emission peak wavelength of the first phosphor preferably falls within the green region (range of 500 nm or more and 560 nm or less), and more preferably within the range of 520 nm or more and 560 nm or less. Specifically, yttrium aluminum garnet-based phosphors (e.g., Y3(Al,Ga)5O 12 :Ce), lutetium aluminum garnet-based phosphors (e.g., Lu3(Al,Ga)5O 12 :Ce), silicate-based phosphors (e.g., (Ba,Sr)2SiO4:Eu), chlorosilicate-based phosphors (e.g., Ca8Mg(SiO4)4Cl2:Eu), β-sialon-based phosphors (e.g., Si 6-Z Al Z O Z N 8-Z :Eu(0 < Z < 4.2)), etc. can be mentioned.

[0186] (The second phosphor) The second phosphor emits red light. From the viewpoints of luminous efficiency, color mixing relationship with light from other light sources, etc., the emission peak wavelength of the second phosphor preferably falls within the range of 620 nm or more and 670 nm or less. Specifically, nitrogen-containing calcium aluminosilicate (CASN or SCASN)-based phosphors (e.g., (Sr,Ca)AlSiN3:Eu), etc. can be mentioned. Further, the fluoride phosphor activated with manganese is a phosphor represented by the general formula (I): A2[M 1-a Mn a F6] (wherein, in the above general formula (I), A is at least one selected from the group consisting of K, Li, Na, Rb, Cs, and NH4, M is at least one element selected from the group consisting of Group 4 elements and Group 14 elements, and a satisfies 0 < a < 0.2). A representative example of this fluoride phosphor is potassium fluorosilicate-based phosphor (e.g., K2SiF6:Mn).

[0187] (Filler for the sealing member) Examples of the filler for the sealing member include silicon dioxide (silica). Silica is preferable as a reducer of the thermal expansion coefficient of the sealing member. The shape of the filler for the sealing member is not particularly limited, and may be amorphous (crushed), but is preferably spherical from the viewpoint of fluidity.

[0188] (Wire 150) The wire is a conducting wire that connects the electrode of the light-emitting element to the lead electrode, and specifically, a metal wire of gold, copper, silver, platinum, aluminum, palladium, or an alloy thereof can be used.

[0189] (Adhesive member 160) The adhesive member is a member for fixing the light emitting element to the lead electrode. In the light emitting device of the present invention, the adhesive member is a cured product of the die bond material of the present invention.

[0190] 3) Manufacturing method of light-emitting device The manufacturing method of the light-emitting device of the present invention is a manufacturing method of a light-emitting device comprising an element container having a pair of lead electrodes and a molded body molded integrally with the pair of lead electrodes, and having a recess, the bottom of the recess being constituted by the pair of lead electrodes, and a light-emitting element fixed via an adhesive member onto at least one of the pair of lead electrodes constituting the bottom of the recess, the manufacturing method of the light-emitting device including a light-emitting element mounting step of fixing the light-emitting element to at least one of the pair of lead electrodes using the die bond material of the present invention. The light emitting device obtained by this manufacturing method is similar to the light emitting device of the present invention described above, and a detailed description thereof will be omitted.

[0191] In the method for producing the light emitting device of the present invention, known methods can be appropriately used for the steps other than the step of mounting the light emitting element.

[0192] The mounting process of the light-emitting element can be carried out, for example, by applying the die-bonding material to at least one of the pair of lead electrodes, placing the light-emitting element on the die-bonding material (coating), and curing the die-bonding material at a temperature of 95°C or higher and 105°C or lower.

[0193] The amount of the die-bonding material of the present invention to be applied is not particularly limited, and is usually an amount that results in a coating film of the die-bonding material having a thickness of 0.5 to 5 μm, preferably 1 to 3 μm.

[0194] The heating temperature when the die bond material is heat cured varies depending on the die bond material used, but is preferably 95° C. to 105° C. The heating time is usually 10 minutes to 20 hours, preferably 30 minutes to 15 hours. By setting the heating temperature within the range of 95° C. to 105° C., deterioration of the surrounding members can be prevented and the light emitting device can be manufactured efficiently. EXAMPLES

[0195] Examples of the present invention will be described in detail below. It should be noted that the present invention is not limited to the following examples.

[0196] (average molecular weight measurement) The mass average molecular weight (Mw) and number average molecular weight (Mn) of the curable polysilsesquioxane compounds obtained in the Production Examples were measured using the following apparatus and conditions, expressed as standard polystyrene equivalent values. Device name: HLC-8220GPC, manufactured by Tosoh Corporation Column: TSKgel GMHXL, TSKgel GMHXL, and TSKgel 2000HXL connected in sequence Solvent: Tetrahydrofuran Injection volume: 80μl Measurement temperature: 40℃ Flow rate: 1ml / min Detector: Differential refractometer

[0197] (IR spectrum measurement) The IR spectrum of the curable polysilsesquioxane compound obtained in the Production Examples was measured using a Fourier transform infrared spectrophotometer (Spectrum 100, manufactured by PerkinElmer).

[0198] ( 29Si-NMR measurement) In order to investigate the repeating units and their amounts in the curable polysilsesquioxane compounds obtained in the manufacturing examples, 29 Si-NMR measurements were carried out. Equipment: Bruker Biospin AV-500 29 Si-NMR resonance frequency: 99.352MHz Probe: 5mmφ solution probe Measurement temperature: room temperature (25℃) Sample rotation speed: 20kHz Measurement method: Inverse gate decoupling method 29 Si flip angle: 90° 29 Si 90°Pulse width: 8.0μs Repeat time: 5s Accumulation count: 9200 times Observation width: 30kHz

[0199] ( 29 Si-NMR sample preparation method) In order to shorten the relaxation time, Fe(acac)3 was added as a relaxation reagent and measurements were performed. Curable polysilsesquioxane compound concentration: 30% by mass Fe(acac)3 concentration: 0.7% by mass Measurement solvent: acetone Internal standard: TMS

[0200] (Waveform processing analysis) For each peak in the spectrum after Fourier transformation, the chemical shift was determined from the peak top position and integrated.

[0201] (Measurement of acid generation temperature of thermal acid generator) Differential scanning calorimetry was performed on each thermal acid generator using a differential scanning calorimeter (manufactured by TA Instruments; product name: DSC Q2000Auto) under the conditions of an initial temperature of 30°C, a measurement temperature range of 30 to 300°C, and a heating rate of 10°C / min. From the obtained DSC curve, the peak temperature (°C) of the maximum endothermic peak was calculated to obtain the acid generation temperature of each thermal acid generator.

[0202] <Production Example 1> A 300 mL eggplant-shaped flask was charged with 17.0 g (77.7 mmol) of 3,3,3-trifluoropropyltrimethoxysilane and 32.33 g (181.3 mmol) of methyltriethoxysilane, and then an aqueous solution obtained by dissolving 0.0675 g of 35 mass % hydrochloric acid (the amount of HCl was 0.65 mmol, 0.25 mol % relative to the total amount of the silane compounds) in 14.0 g of distilled water was added with stirring, and the entire volume was stirred at 30° C. for 2 hours, then heated to 70° C. and stirred for 20 hours. While continuing to stir the contents, a mixed solution of 0.0394 g of 28% by mass ammonia water (NH3 amount: 0.65 mmol) and 46.1 g of propyl acetate was added thereto to adjust the pH of the reaction liquid to 6.9, and the mixture was stirred at 70° C. for 40 minutes. After the reaction solution was cooled to room temperature, 50 g of propyl acetate and 100 g of water were added thereto and separated to obtain an organic layer containing a reaction product. Magnesium sulfate was added to this organic layer and dried. After removing the magnesium sulfate by filtration, the organic layer was concentrated with an evaporator, and the obtained concentrate was then vacuum dried to obtain a curable polysilsesquioxane compound (1) [curable PSQ (A1)]. The mass average molecular weight (Mw) of the curable PSQ (A1) was 5,500, and the molecular weight distribution was 3.40. The IR spectrum data of the curable PSQ (A1) is shown below. Si-CH3: 1272cm -1 ,1409cm -1 ,Si-O:1132cm -1 ,CF:1213cm -1 Also, 29 As a result of Si-NMR spectrum measurement, the peak integral ratio of T1, T2, and T3 was 2:27:71.

[0203] The compounds used in the examples and comparative examples are shown below. (Component A) Curable PSQ(A1)

[0204] (Component B and Comparative Compound) Thermal acid generator (B1): Compound represented by the following formula (acid generation temperature: 150°C)

[0205] [ka]

[0206] Thermal acid generator (B2): Compound represented by the following formula (acid generation temperature: 125°C)

[0207] [ka]

[0208] Thermal acid generator (B3): Compound represented by the following formula (acid generation temperature: 125°C)

[0209] [ka]

[0210] Hardening accelerator (X1): Hydrochloric acid Curing accelerator (X2): Ti complex

[0211] (C component) Silane coupling agent (C1): 1,3,5-N-tris[3-(trimethoxysilyl)propyl]isocyanurate Silane coupling agent (C2): 3-(trimethoxysilyl)propylsuccinic anhydride

[0212] Example 1 To 100 parts by mass of the curable PSQ (A1), a mixed solvent of diethylene glycol monobutyl ether acetate: tripropylene glycol-n-butyl ether = 40:60 (mass ratio), 30 parts by mass of the silane coupling agent (C1), and 3 parts by mass of the silane coupling agent (C2) were added, and the entire volume was stirred. To this, 0.05 parts by mass of the thermal acid generator (B1) (added as a 10% by mass ethyl acetate solution) was added, and the entire volume was thoroughly mixed to obtain a die bond material.

[0213] (Examples 2 to 6, Comparative Examples 1 to 3) A die bond material was obtained in the same manner as in Example 1, except that the components in Example 1 were changed to those shown in Table 1.

[0214] [Table 1]

[0215] The die bond materials obtained in the examples and comparative examples were subjected to the following measurements and tests. The results are shown in Table 2.

[0216] [Refractive index measurement] The die bond material was discharged onto a horizontal surface, and the measurement surface of a pen refractometer (PEN-RI, manufactured by ATAGO) was pressed against the surface at 25° C. to measure the refractive index (nD).

[0217] [Curing evaluation] The hardening time of the die bond material was measured by the following method using an automatic hardening time measuring device "Madoka" (manufactured by Cyber ​​Corporation). 0.20 mL of the sample was placed on a stainless steel plate heated to 100°C and stirred. The stirring torque increased over time, so the time (seconds) until the stirring torque reached 0.049 N cm was measured. The stirring conditions were as follows: Rotation speed of the agitator: 300 rpm Rotational speed of the stirring blade: 120 rpm Gap (distance between heating plate and stirring blade): 0.2mm

[0218] [Evaluation of Viscosity Increase Rate] Using a rheometer (Anton Paar, MCR301) with a cone plate of 50 mm radius and 0.5° cone angle, the shear rate was 2 s at 25°C. -1 The viscosity at that time (initial viscosity) was measured. The sample was allowed to stand at 25°C for 24 hours, and then the viscosity was measured under the same conditions. From the obtained measured values, the rate of increase in viscosity was calculated based on the following formula. [Viscosity increase rate] = [Viscosity after standing] / [Initial viscosity]

[0219] [Adhesive strength evaluation] A square with a side length of 2 mm (area of ​​4 mm 2 The die bond materials obtained in the Examples and Comparative Examples were applied to the mirror surface of a silicon chip of 1.0 mm2 each to a thickness of approximately 2 μm, and the applied surface was placed on an adherend (silver-plated copper plate) and pressed. The material was then heat-treated at 100°C for 2 hours to harden it, yielding an adherend with a test piece attached. This adherend with the test piece attached was left for 30 seconds on the measurement stage of a bond tester (Dage, Series 4000) that had been preheated to 100°C, and a stress was applied to the adhesive surface in the horizontal direction (shear direction) at a speed of 200 μm / s from a position 100 μm above the adherend, and the adhesive strength (N / 4 mm2) between the test piece and adherend at 100°C was measured. 2 ) was measured.

[0220] [Solid Si-NMR measurement] The die bond material obtained in Example 3 was heated at 170° C. for 2 hours to be cured, and the cured product was subjected to solid-state Si-NMR measurement under the following conditions. The results are shown in Table 3. Equipment: Bruker Biospin AV-500 29 Si-NMR resonance frequency: 99.352MHz Probe: 7.0mmφ CP-MAS probe External standard: hexamethylcyclotrisiloxane (-9.66 ppm) Measurement temperature: 25℃ Sample rotation speed: 4kHz Measurement method: Pulse program hpdec (high power decoupling) 29 Si 90° pulse width: 5.5μs Repeat time: 600s Number of times accumulated: 128 times Observation width: 30kHz Broadening factor: 20Hz

[0221] <Data Processing Method> In the solid-state Si-NMR measurements, the measurement data was taken with a time domain size of 1024, zero-filled to 8192 points, and Fourier transformed.

[0222] <Waveform separation analysis method> For each peak in the spectrum after Fourier transformation, an optimization calculation was performed by the nonlinear least squares method, with the chemical shift, height, half-width, and Gaussian and Lorentzian waveform component ratio of the peak shape as variable parameters.

[0223] [Table 2]

[0224] [Table 3]

[0225] <Example 6> The light emitting device of Example 6 is a side-emitting type LED having the structure of light emitting device 1100 of the example shown in Figures 1 to 4. The size of this light emitting device (element container) is 4.2 mm in width (width in the left-right direction), 1.0 mm in depth (width in the front-back direction), and 0.6 mm in thickness (width in the up-down direction).

[0226] The element container 110 is formed by molding a molded body 115 integrally with a first lead electrode 111 (negative electrode) and a second lead electrode 112 (positive electrode). The element container 110 has a recess 110a on the front surface, which is 3.6 mm wide, 0.46 mm long (narrow portions 0.36 mm wide), and 0.3 mm deep.

[0227] The molded body 115 contains a white pigment of titanium oxide (40% by mass) and a filler of fibrous calcium silicate (wollastonite; 10% by mass) in a base material of polyamide resin. The molded body 115 is molded by injection molding, and has a gate mark 115a at approximately the center of the rear surface (of the rear molded part). The first lead electrode 111 and the second lead electrode 112 are small metal pieces having a thickness of 0.11 mm, which are silver-plated with a sulfur-based brightener on a base body of a copper alloy. The sidewall surface of the recess 110a is formed by the surface of the molded body 115, and the bottom of the recess 110a is formed by the surface of the molded body 115 and the surfaces of the first lead electrode 111 and the second lead electrode 112. The parts of the first lead electrode 111 and the second lead electrode 112 that form the bottom of this recess 110a are the first element mounting part 111a and the second element mounting part 112a. Moreover, the first lead electrode 111 and the second lead electrode 112 have a first external connection terminal portion 111b and a second external connection terminal portion 112b as portions located outside the molded body 115. The first external connection terminal portion 111b and the second external connection terminal portion 112b extend from the lower surface of the molded body 115 and are bent along the lower surface, and are further bent along the left end surface or the right end surface. The molded body 115 has a reinforcing portion 117 connecting two side walls 1151, 1152 facing each other in the vertical direction of the recess 110a. The reinforcing portion 117 is located on a separation region 1150 separating the first lead electrode 111 and the second lead electrode 112, and is located approximately in the center of the horizontal direction of the recess 110a. The reinforcing portion 117 has a rectangular shape (a linear shape with width) when viewed from the front, and a trapezoidal shape when viewed in cross section.

[0228] Two light emitting elements 121 (first light emitting element 121 and second light emitting element 121) are accommodated in the recess 110a of the element container. The light emitting element 121 is a semiconductor light emitting element having a length of 0.24 mm, a width of 0.85 mm, and a thickness of 0.12 mm, and is capable of emitting blue light (emission peak wavelength of about 455 nm) and is configured by sequentially stacking an n-type layer, an active layer, and a p-type layer of a nitride semiconductor on a sapphire substrate. The first light emitting element 121 and the second light emitting element 121 are fixed on the first element mounting portion 111a and the second element mounting portion 112a, respectively, via adhesive members 160. The n-electrode of the first light emitting element 121 and the first element mounting portion 111a, the p-electrode of the first light emitting element 121 and the n-electrode of the second light emitting element 121, and the p-electrode of the second light emitting element 121 and the second element mounting portion 112a are connected by wires 150, respectively. In the light emitting device of the present invention, adhesive member 160 is a hardened product of the die bond material of Example 3. Wire 150 is a silver-gold alloy wire (approximately 80% silver / approximately 20% gold) with a wire diameter of 25 μm.

[0229] The recess 110a of the element container is filled with a sealing member 130 so as to cover the light emitting element 121. The sealing member 130 is made of a methyl-phenyl silicone resin as a base material, and contains a wavelength conversion material 140 made of a first phosphor that is a β-sialon phosphor capable of emitting green light (peak emission wavelength of about 540 nm) and a second phosphor that is a potassium fluorosilicate phosphor capable of emitting red light (peak emission wavelength of about 630 nm). The front surface of the sealing member 130 is substantially flush with the front surface of the molded body 115 (slightly concave due to curing shrinkage). A large amount of the wavelength conversion material 140 is present in the sealing member 130 on the bottom side of the recess 110a.

[0230] <Evaluation 1: Evaluation of heat resistance of the resin that constitutes the molded body of the element container (change in resin reflectance)> The following experiment was carried out to examine the heat resistance of the resin constituting the molded body of the element container. A thin film plate (4 mm thick) of polyamide resin containing titanium oxide and fibrous wollastonite (titanium oxide content 40% by mass, wollastonite content 10% by mass) was used as a sample, and the initial reflectance (Ri ) was measured at room temperature (25°C). Next, the initial reflectance (R i The sample was heated in an oven at 100°C for 100 minutes, 135°C for 100 minutes, or 150°C for 100 minutes with the surface on which the reflectance at a wavelength of 450 nm (R ii The reflectance retention rate (α) was calculated according to the following formula. The results are shown in Table 3.

[0231]

number

[0232] [Table 4]

[0233] In order to manufacture a light-emitting device having the desired performance, it is preferable that the reflectance maintenance rate (α) of the element container is 99.8% or more when heated during the manufacturing process of the light-emitting device. The above experiment shows that for element containers made of polyamide resin, if the heating temperature during the mounting process of the light-emitting element can be lowered to about 100°C, the deterioration can be suppressed.

[0234] <Evaluation 2: Die shear strength of adhesive material> In evaluation 2, the effect was confirmed using a light emitting device in the manufacturing process according to Example 6, which had been subjected to the process of fixing the light emitting element on the lead electrode by the die bond material of Example 3. In this example, for the sake of explanation, it may be referred to as a light emitting device in the manufacturing process according to Example 6. In this specification, the light emitting device in the manufacturing process refers to a state in which the die bond material is applied to the lead electrode, the light emitting element is placed on the die bond material (coated material), and then the die bond material is cured (mounted). The curing conditions of the die bond material at this time are 100°C for 400 minutes (Reference Example 1), 100°C for 500 minutes (Example 7), 100°C for 600 minutes (Example 8), and 100°C for 800 minutes (Example 9). The die shear strength of the obtained samples was measured at a stage temperature set to 25°C or 150°C. The measurement device used was a bonding tester PTR1000 (manufactured by Rhesca), and a sensor for 2 kgf was used. The shear speed was 0.3 mm / sec, the tool height was 35 μm, and the light-emitting element was pressed from the side to measure the strength (die shear strength) at the time when breakage occurred between the light-emitting element and the adhesive member. The average measured values ​​(n=24) are shown in Table 5. The light emitting device used in Evaluation 2 was a roughly rectangular parallelepiped with dimensions of 0.24 mm in length, 0.85 mm in width, and 0.12 mm in thickness.

[0235] [Table 5]

[0236] As described above, when the die bonding material of Example 3 is cured at 100° C., an adhesive member having sufficient strength can be obtained by setting the heating time to 500 minutes or more.

[0237] From the above experimental results, it has been found that by hardening the die-bonding material having low-temperature hardening properties under appropriate conditions, it is possible to obtain an adhesive member having sufficient strength while suppressing deterioration of the surrounding resin members, etc. As a result, it is possible to obtain a light-emitting device that maintains its luminous flux. [Industrial Applicability]

[0238] The light emitting device according to one embodiment of the present invention can be used in backlight devices for liquid crystal displays, various lighting fixtures, large displays, various display devices such as for advertisements and destination guidance, projector devices, and further image reading devices in digital video cameras, facsimiles, copy machines, scanners, etc. [Explanation of symbols]

[0239] 110: Element container (110a: recess) 111...First lead electrode 112...Second lead electrode 111a...first element mounting portion 112a...second element mounting section 111b...First external connection terminal section 112b...Second external connection terminal section 115... Molded body (115a... gate mark, 1150... separation region, 1151, 1152... side wall, 117... reinforcement part) 121...Light emitting element 130...Sealing member 140...Wavelength conversion material 150…Wire 160...Adhesive material 1100...Light emitting device

Claims

1. A die bonding material comprising the following component (A), component (B), and a solvent: The content of the (B) component is more than 0 parts by mass and 0.6 parts by mass or less per 100 parts by mass of the (A) component, A die bond material in which, when 0.20 mL of a sample is placed on a stainless steel plate heated to 100°C using an automatic curing time measuring device and stirred with a stirring blade under the following conditions: the stirring blade rotation speed is 300 rpm, the stirring blade revolution speed is 120 rpm, and the gap (distance between the stainless steel plate and the stirring blade) is 0.2 mm, the time from the start of stirring until the stirring torque reaches 0.049 N cm is 200 to 2500 seconds. Component (A): A curable polysilsesquioxane compound having a repeating unit represented by the following formula (a-1), which satisfies the following requirements A1 and A2: 【number】 [R 1 is the composition formula: C m H (2m-n+1) F n m is an integer of 1 to 10, and n is an integer of 2 or more and (2m+1) or less. D is a fluoroalkyl group represented by the formula: 1 and Si, or a single bond. [Requirement A1] Curable polysilsesquioxane compounds 29 When Si-NMR is measured, one or more peaks are observed in a region of -62 ppm or more and less than -52 ppm [region (2)], one or more peaks are observed in at least one of a region of -52 ppm or more and less than -45 ppm [region (1)] and a region of -73 ppm or more and less than -62 ppm [region (3)], and Z2 calculated by the following formula is 20 to 40%. [0010] P1: integral value in region (1) P2: integral value in region (2) P3: integral value in region (3) [Requirement A2] The curable polysilsesquioxane compound has a mass average molecular weight (Mw) of 3,500 to 11,000. Component (B): Thermal acid generator

2. 2. The die bonding material according to claim 1, wherein the curable polysilsesquioxane compound has a repeating unit represented by formula (a-1) in a proportion of 25 mol % or more based on all repeating units.

3. The die bonding material according to claim 1 or 2, wherein the curable polysilsesquioxane compound further has a repeating unit represented by the following formula (a-2): [Case 2] [R 2 represents an unsubstituted alkyl group having 1 to 10 carbon atoms, or a substituted or unsubstituted aryl group having 6 to 12 carbon atoms.

4. The die bonding material according to claim 3, wherein the ratio of the repeating unit represented by formula (a-2) in the curable polysilsesquioxane compound is more than 0 mol% and 75 mol% or less with respect to all repeating units.

5. The curable polysilsesquioxane compound 29 The die bond material according to any one of claims 1 to 4, wherein when Si-NMR is measured, one or more peaks are observed in the region (3), and Z3 calculated by the following formula is 60 to 80%. [0025]

6. The die bonding material according to any one of claims 1 to 5, wherein the content of the component (A) is 40 mass% or more and less than 100 mass% of the solid content of the die bonding material.

7. The die bonding material according to any one of claims 1 to 6, wherein the component (B) is an onium salt-based thermal acid generator.

8. The die bonding material according to any one of claims 1 to 7, wherein the component (B) satisfies the following requirement B1. [Requirement B1] With respect to component (B), the peak temperature of the maximum endothermic peak (acid generation temperature) obtained by differential scanning calorimetry at a temperature range of 30 to 300°C and a heating rate of 10°C / min is 80 to 180°C.

9. The die bonding material according to any one of claims 1 to 8, further comprising the following component (C): Component (C): Silane coupling agent

10. An element container including a pair of lead electrodes and a molded body integrally molded with the pair of lead electrodes, the element container having a recess, the bottom of the recess being formed by the pair of lead electrodes; a light emitting element fixed via an adhesive member onto at least one of the pair of lead electrodes that form a bottom of the recess; Equipped with A light emitting device, wherein the adhesive member is a cured product of the die bond material according to any one of claims 1 to 9.

11. The light-emitting device according to claim 10, wherein the adhesive member fixing the light-emitting element has a die shear strength of 650 gf or more measured when the light-emitting element is pressed from the side at 0.3 mm / sec at 25°C and breakage occurs between the light-emitting element and the adhesive member.

12. The light-emitting device according to claim 10, wherein the adhesive member fixing the light-emitting element has a die shear strength of 300 gf or more when the light-emitting element is pressed from the side at 0.3 mm / sec at 150°C and breaks occur between the light-emitting element and the adhesive member.

13. 13. The light emitting device according to claim 10, wherein the element container has a reflectance maintenance rate (α) of 99.8% or more, which is calculated by the following formula: [0030] (R i is the reflectance measured at a wavelength of 450 nm at room temperature (25° C.) without heating, and R iiis the reflectance measured at a wavelength of 450 nm after heating at 100° C. for 100 minutes and then cooling to room temperature (25° C.).

14. 14. The light emitting device according to claim 10, wherein the light emitting element has an emission peak wavelength of 445 nm or more and 465 nm or less.

15. The light emitting element is a nitride semiconductor (In x A y G 1-x-y The light emitting device according to any one of claims 10 to 14, wherein N, 0≦x, 0≦y, x+y≦1).

16. An element container including a pair of lead electrodes and a molded body integrally molded with the pair of lead electrodes, the element container having a recess, the bottom of the recess being formed by the pair of lead electrodes; a light emitting element fixed via an adhesive member onto at least one of the pair of lead electrodes that form a bottom of the recess; A method for manufacturing a light emitting device comprising: A method for manufacturing a light emitting device, comprising: a light emitting element mounting step of fixing the light emitting element to at least one of the pair of lead electrodes using the die bond material according to any one of claims 1 to 9.

17. The light emitting element mounting step includes: The die bond material is applied to at least one of the pair of lead electrodes, The light emitting element is disposed on the die bond material; The method for manufacturing a light emitting device according to claim 16, wherein the die bond material is cured at a temperature of 95° C. or more and 105° C. or less.

18. 18. The method for manufacturing a light emitting device according to claim 16, wherein the light emitting element has an emission peak wavelength of 445 nm or more and 465 nm or less.

Citation Information

Patent Citations

  • Sealing material for optical element

    JP2004359933A

  • Resin composition for sealing optical semiconductor

    JP2005263869A

  • Resin composition for encapsulating optical element

    JP2006328231A

  • Die bonding material, light-emitting device and method for manufacturing light-emitting device

    JP2020176212A

  • Curable composition, method for producing curable composition, cured product, use of curable composition, and optical device