Mn-activated phosphor, wavelength converter, and light-emitting device

The development of a Mn-activated phosphor with specific composition emits near-infrared light when excited by 254 nm light, addressing the emission gap in existing Eu-activated phosphors and enhancing luminescence properties for near-infrared applications.

JP7575315B2Active Publication Date: 2024-10-29DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021047138
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-22
Publication Date
2024-10-29
Estimated Expiration
2041-03-22

AI Technical Summary

Technical Problem

Existing Eu-activated phosphors do not emit light in the range of 600 nm or more and 900 nm or less when irradiated with 254 nm light, and there is a lack of known phosphors that emit near-infrared light with the same crystal structure as Mg1Si1Al3O3N3.

Method used

A Mn-activated phosphor with the general formula Mg1-xSi1Al3+pMn y O2+qN3+z (0.2≦x≦1, 0

Benefits of technology

The Mn-activated phosphor achieves emission peaks in the near-infrared region, offering improved luminescence characteristics and suitability for various devices utilizing near-infrared light.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575315000004
    Figure 0007575315000004
  • Figure 0007575315000005
    Figure 0007575315000005
  • Figure 0007575315000001
    Figure 0007575315000001
Patent Text Reader

Abstract

To provide a Mn-activated phosphor that has an emission peak in the wavelength range of 600 nm or more and 900 nm or less in an emission spectrum when irradiated with light of 254 nm.SOLUTION: A Mn-activated phosphor emits light having an emission peak in the wavelength range of 600 nm or more and 900 nm or less when irradiated with light of 254 nm, the Mn-activated phosphor comprising a compound represented by general formula: Mg1-xSi1Al3+pMnyO2+qN3+z (0.2≤x≤1, 0<y≤0.1, 0.1≤p≤1.5, 0≤q≤1.5, 0.5≤z≤1.5).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a Mn-activated phosphor, a wavelength converter, and a light emitting device. [Background technology]

[0002] Various developments have been made so far regarding phosphors containing crystals whose chemical composition is represented by Mg1Si1Al3O3N3. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a phosphor in which Eu is dissolved in an inorganic crystal having the same crystal structure as a crystal whose chemical composition is represented by Mg1Si1Al3O3N3, and which emits blue to green fluorescence from 450 nm to 530 nm when irradiated with light from 250 nm to 500 nm (claim 23 of Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-000965 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the Eu-activated phosphor described in Patent Document 1 does not have an emission peak in the range of 600 nm or more and 900 nm or less in the emission spectrum when irradiated with light of 254 nm. In addition, it was not known that a phosphor that emits near-infrared light could be obtained by dissolving Mn in an inorganic crystal having the same crystal structure as a crystal with the chemical composition represented by Mg1Si1Al3O3N3. [Means for solving the problem]

[0005] As a result of the investigation aimed at realizing a near-infrared emitting phosphor, the inventor selected Mn element as an activator element and synthesized a phosphor having the general formula: Mg 1-x Si1Al 3+p Mny O 2+q N 3+z (However, by using a compound represented by (where 0.2 ≦ x ≦ 1, 0 < y ≦ 0.1, 0.1 ≦ p ≦ 1.5, 0 ≦ q ≦ 1.5, 0.5 ≦ z ≦ 1.5), it has been found that a novel phosphor having an emission peak in the range of 600 nm or more and 900 nm or less in the emission spectrum can be realized when irradiated with light having a wavelength of 254 nm, and the present invention has been completed.)

[0006] According to the present invention, a Mn-activated phosphor that emits light having an emission peak in the wavelength range of 600 nm or more and 900 nm or less when irradiated with light having a wavelength of 254 nm, General formula: Mg 1-x Si1Al 3+p Mn y O 2+q N 3+z (where 0.1 ≦ x ≦ 1, 0 < y ≦ 0.1, 0.1 ≦ p ≦ 1.5, 0 ≦ q ≦ 2, 0 ≦ z ≦ 1.5) is provided.

[0007] Also according to the present invention, a wavelength converter containing the above Mn-activated phosphor is provided.

[0008] Also according to the present invention, a light-emitting device including the above wavelength converter is provided.

Advantages of the Invention

[0009] According to the present invention, a Mn-activated phosphor having an emission peak in the range of 600 nm or more and 900 nm or less in the emission spectrum when irradiated with light having a wavelength of 254 nm, a wavelength converter using the same, and a light-emitting device are provided.

Brief Description of the Drawings

[0010] [Figure 1] It is a diagram showing the XRD patterns of the phosphors of Example 1, 4, Comparative Example 1, and 2. [Diagram 2] It is a diagram showing the emission spectra of the phosphors of Example 1, 4, Comparative Example 1, and 2.

Embodiments for Carrying Out the Invention

[0011] The Mn-activated phosphor of this embodiment will be outlined.

[0012] The Mn-activated phosphor is a phosphor that emits light having an emission peak in the wavelength range of 600 nm or more and 900 nm or less when irradiated with light having a wavelength of 254 nm. This Mn-activated phosphor has the general formula: Mg 1-x Si1Al 3+p Mn y O 2+q N 3+z (However, 0.2 ≦ x ≦ 1, 0 < y ≦ 0.1, 0.1 ≦ p ≦ 1.5, 0 ≦ q ≦ 1.5, 0.5 ≦ z ≦ 1.5) and contains a compound represented by.

[0013] According to the findings of the present inventor, by using a compound having the general formula: Mg 1-x Si1Al 3+p-y Mn y O 2+q N 3+z (However, 0.2 ≦ x ≦ 1, 0 < y ≦ 0.1, 0.1 ≦ p ≦ 1.5, 0 ≦ q ≦ 1.5, 0.5 ≦ z ≦ 1.5), it is possible to appropriately control the activation amount of the activation element Mn in the phosphor, so that an Mn-activated phosphor excellent in emission characteristics in the near-infrared region and / or near the near-infrared region can be realized.

[0014] Although the detailed mechanism is not clear, it is considered that by substituting a part of the elements in the phosphor with Mn elements, the emission peak position can be shifted to the long wavelength side, and a phosphor that emits light in the vicinity of the near-infrared region can be realized. Also, it is considered that the emission characteristics can be enhanced by appropriately controlling the content of Mg element in the phosphor.

[0015] The Mn-activated phosphor of this embodiment can be excited by UV light of 200 nm to 300 nm or blue light of 420 nm to 530 nm.

[0016] The wavelength converter including the Mn-activated phosphor of this embodiment is composed of a member that converts irradiated light (excitation light) and emits light having an emission peak in a wavelength range different from that of the excitation light. The wavelength converter may constitute at least a part of the light emitting device described below. The wavelength converter may emit light having an emission peak in a wavelength range of, for example, 600 nm or more and 900 nm or less. The wavelength converter may include one or more known phosphors other than the Mn-activated phosphor of this embodiment.

[0017] The wavelength converter may be composed only of a Mn-activated phosphor, or may include a base material in which the Mn-activated phosphor is dispersed. Examples of the base material include glass, resin, and inorganic materials.

[0018] A light emitting device including the wavelength converter of this embodiment can be used for various applications such as sensors, inspection, analysis, security, optical communications, and medical applications, and examples thereof include LED packages, light sources, stationary spectrophotometers, handheld food analyzers, wearable devices, infrared cameras, moisture measuring devices, and gas detectors.

[0019] An example of a light emitting device includes a light emitting element and a wavelength converter including a Mn-activated phosphor that converts light irradiated from the light emitting element and emits light. The shape of such a wavelength converter is not particularly limited, and it may be configured in a plate shape, for example, to seal a part of the light emitting element or the entire light emitting surface.

[0020] The Mn-activated phosphor of this embodiment will be described in detail below.

[0021] When irradiated with light having a wavelength of 254 nm, the Mn-activated phosphor has an emission spectrum with an emission peak in a wavelength range of 600 nm to 900 nm, preferably 680 nm to 900 nm, and more preferably 700 nm to 850 nm.

[0022] The position of the emission peak depends on the concentration of Mn element contained in the phosphor, that is, the general formula: Mg 1-x Si1Al 3+p Mny O 2+q N 3+z (However, it can be controlled by appropriately adjusting y, 1 - x, etc. in the range of (where 0.2 ≤ x ≤ 1, 0 < y ≤ 0.1, 0.1 ≤ p ≤ 1.5, 0 ≤ q ≤ 1.5, 0.5 ≤ z ≤ 1.5).

[0023] When the Mn - activated phosphor is irradiated with light having a wavelength of 254 nm, the full width at half - maximum of the emission peak in the wavelength range of 600 nm or more and 900 nm or less in the emission spectrum of the Mn - activated phosphor is, for example, 100 nm or more and 170 nm or less, preferably 110 nm or more and 160 nm or less, more preferably 120 nm or more and 150 nm or less. By setting the full width at half - maximum within the above range, the emission intensity at the peak wavelength can be improved.

[0024] In the above general formula, the lower limit of 1 - x is, for example, 0.01 or more, preferably 0.02 or more, more preferably 0.05 or more. Thereby, the emission intensity of the emission peak can be increased. On the other hand, the upper limit of 1 - x is 0.90 or less, preferably 0.50 or less, more preferably 0.30 or less. Thereby, the shape of the emission peak can be made sharper, and emission without visible light components can be obtained, which is preferable.

[0025] In the above general formula, the lower limit of y is preferably 0.005 or more, more preferably 0.01 or more. The peak position can be within a desired range. On the other hand, the upper limit of y is preferably 0.09 or less, more preferably 0.07 or less. Thereby, light in the vicinity of the near - infrared region can be emitted.

[0026] The Mn - activated phosphor may contain a compound satisfying 0 < 1 - x + y ≤ 1.0, preferably 0 < 1 - x + y ≤ 0.9, more preferably 0 < 1 - x + y ≤ 0.5 in the above general formula. Thereby, light in the vicinity of the near - infrared region can be emitted, and the emission intensity of the emission peak can be increased.

[0027] The Mn - activated phosphor has a composition formula Mg f Si g Alh O j1 N j2 Mn i represented by the composition ratios f, g, h, j1, j2 and i are 0.00 ≦ f ≦ 0.88, 0.70 ≦ g ≦ 1.30, 0.70 ≦ h ≦ 4.50, 5.50 ≦ j1 + j2 ≦ 7.50, 0.00 < i ≦ 1.30, and it may be configured to satisfy 0.70 ≦ h + i ≦ 5.30.

[0028] When the phosphor activated by Mn is irradiated with light having a wavelength of 254 nm, in the emission spectrum of the phosphor activated by Mn, let the fluorescence intensity at 650 nm be I 650 and the fluorescence intensity at the emission peak in the wavelength range of 600 nm or more and 900 nm or less be I MAX and. The phosphor activated by Mn is such that I 650 , I MAX is, for example, 1.5 ≦ I MAX / I 650 , preferably 5.0 ≦ I MAX / I 650 , more preferably 10.0 ≦ I MAX / I 650 It may be configured to satisfy. As a result, it is possible to shift the emission peak to the longer wavelength side or make the shape of the emission peak sharper, and it is preferable because emission containing no visible light component can be obtained. On the other hand, the phosphor activated by Mn is such that I 650 , I MAX is, for example, I MAX / I 650 ≦ 1000.

[0029] Regarding the phosphor activated by Mn, in the volume frequency particle size distribution measured using the laser diffraction scattering method, let the particle diameter at which the cumulative value is 50% be D50, the particle diameter at which the cumulative value is 10% be D10, and the particle diameter at which the cumulative value is 90% be D90.

[0030] D50 is, for example, 1 μm or more and 50 μm or less, preferably 2 μm or more and 40 μm or less, more preferably 3 μm or more and 30 μm or less. By setting it within the above range, the balance of the light emission characteristics can be achieved.

[0031] The lower limit of (D90 - D10) / D50 is, for example, 1.0 or more, preferably 1.5 or more, more preferably 2.0 or more. On the other hand, the upper limit of (D90 - D10) / D50 is, for example, 20.0 or less, preferably 10.0 or less, more preferably 7.0 or less. By setting it within the above range, the balance of the light emission characteristics can be achieved.

[0032] Hereinafter, the method for manufacturing the Mn-activated phosphor of the present embodiment will be described.

[0033] An example of the method for manufacturing the Mn-activated phosphor may include a mixing step of obtaining a raw material mixture containing each element constituting the composition of a compound represented by the general formula: Mg 1-x Si1Al 3+p Mn y O 2+p N 3+p (where 0.2 ≤ x ≤ 1, 0 < y ≤ 0.1, 0.1 ≤ p ≤ 1.5, 0 ≤ q ≤ 1.5, 0.5 ≤ z ≤ 1.5), and a firing step of firing the raw material mixture.

[0034] Examples of the raw material containing Mg element include a single substance or a mixture of two or more selected from metals, silicides, oxides, carbonates, nitrides, oxynitrides, chlorides, fluorides, and acid fluorides containing Mg. Examples of the raw material containing Si element include a single substance or a mixture of two or more selected from metals, oxides, carbonates, nitrides, oxynitrides, chlorides, fluorides, and acid fluorides containing Si. Examples of the raw material containing Al element include a single substance or a mixture of two or more selected from metals, silicides, oxides, carbonates, nitrides, oxynitrides, chlorides, fluorides, and acid fluorides containing Al.

[0035] As the raw material containing Mn element, a single substance or a mixture of two or more substances selected from metals, silicides, oxides, carbonates, nitrides, oxynitrides, chlorides, fluorides, and oxyfluorides containing Mn is used.

[0036] The raw material mixture may contain, for example, Mn nitride or oxide, Mg nitride or oxide, Al nitride or oxide, and silicon oxide or silicon nitride, which can promote the reaction during firing.

[0037] The method for mixing the raw materials is not particularly limited, but examples include a method in which the raw materials are thoroughly mixed using a mixing device such as a mortar, a ball mill, a V-type mixer, or a planetary mill.

[0038] The firing step is a step of firing the above-mentioned raw material mixture in a firing furnace such as an electric furnace. The firing atmosphere in the firing furnace may be a non-oxidizing gas such as argon, helium, hydrogen, nitrogen, etc. These may be used alone or in combination of two or more kinds.

[0039] The calcination temperature in the calcination step is selected from the viewpoints of reducing unreacted raw materials after the calcination step and suppressing decomposition of the main component. The lower limit of the firing temperature in the firing step is preferably 1000° C. or higher, more preferably 1200° C. or higher, and even more preferably 1500° C. or higher. On the other hand, the upper limit of the firing temperature is preferably 2200° C. or lower, more preferably 2000° C. or lower, and even more preferably 1900° C. or lower.

[0040] The pressure of the firing atmosphere gas is selected depending on the firing temperature, but is usually in the range of 0.1 MPa to 10 MPa, and is preferably 0.5 MPa to 1 MPa in consideration of industrial productivity.

[0041] The calcination time in the calcination step is selected from an appropriate time range from the viewpoints of reducing unreacted materials and improving productivity. The lower limit of the firing time is preferably 0.5 hours or more, more preferably 1 hour or more, and even more preferably 2 hours or more, and the upper limit of the firing time is preferably 48 hours or less, more preferably 24 hours or less, and even more preferably 10 hours or less.

[0042] As a result of the above, the raw material mixture (calcined product) is obtained after the calcination step.

[0043] The method for producing a Mn-activated phosphor of this embodiment may further include a pulverization step of pulverizing the raw material mixture (fired product) after the firing step to obtain a pulverized product.

[0044] The state of the fired product obtained by the firing process varies depending on the raw material composition and firing conditions, from powder to lumps. The fired product can be made into powder of a specified size by the crushing process and / or classification process. In addition to the above, a process known in the field of phosphors may be added.

[0045] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES

[0046] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.

[0047] [Examples 1 to 4, Comparative Example 1] (Manufacturing of Mn-activated phosphors) According to the design composition shown in Table 1, silicon nitride (Si3N4), aluminum nitride (AlN), aluminum oxide (Al2O3), magnesium oxide (MgO), and manganese oxide (MnO2) were weighed and mixed in a mortar to obtain a raw material mixture. The resulting raw material mixture was placed in an electric furnace and fired in a nitrogen atmosphere at 1700° C. and 0.8 MPa for 2 hours. The obtained fired product was pulverized in a mortar and then sieved (classified) with a sieve having an opening of 150 μm, and the sieved portion was collected to obtain a powdered Mn-activated phosphor (phosphor particles).

[0048] [Table 1]

[0049] The content (wt%) of each element in the obtained Mn-activated phosphors of Examples 1 to 4 and Comparative Example 1 was measured by ICP emission spectrometry. The results are shown in Table 2.

[0050] [Table 2]

[0051] [Comparative Example 2] A powdered Eu-activated phosphor (phosphor particles) represented by Mg1Si1Al3O3N3:Eu was obtained in the same manner as in Comparative Example 1, except that manganese oxide (MnO2) was changed to europium oxide (Eu2O3).

[0052] [Table 3]

[0053] Powder X-ray diffraction measurements (XRD measurements) using Cu-Kα radiation were performed on the Mn-activated phosphors obtained in Examples 1 to 4 and Comparative Example 1, and the Eu-activated phosphor obtained in Comparative Example 2. As a result, peaks attributed to Mg1Si1Al3O3N3 were confirmed in the XRD patterns of all the phosphors. The XRD patterns in Examples 1 and 4 and Comparative Examples 1 and 2 are shown in FIG.

[0054] (D10, D50, D90) The particle size distribution of the Mn-activated phosphors of Examples 1 to 4 and Comparative Example 1 was measured using a particle size measuring device (LS 13 320, manufactured by Beckman Coulter) that employs a laser diffraction / scattering method.

[0055] (Emission spectrum) For the Mn-activated phosphors of Examples 1 to 4 and Comparative Example 1, and the Eu-activated phosphor of Comparative Example 2, emission spectra were obtained using a spectrofluorometer as follows. First, a powdered Mn-activated phosphor was filled into a solid sample holder (a synthetic quartz cell) attached to a photometer, and then, using a spectrofluorophotometer (Fluorolog-3, manufactured by Horiba, Ltd.) equipped with a cut filter (a filter that absorbs light with a wavelength of 290 nm or less), a Xe lamp was used as a light source to measure the emission spectrum when irradiated with excitation light with a wavelength of 254 nm. Note that, only in the case of Comparative Example 2, a lamp that emits light with a wavelength of 365 nm was used as the excitation light, and a filter that absorbs light with a wavelength of 390 nm or less was used as the cut filter. The emission spectra of Examples 1 and 4 and Comparative Examples 1 and 2 are shown in FIG. 2. In the emission spectra of each Example and Comparative Example 1, the maximum emission intensity (I MAX ) was normalized as 1.00, and in the emission spectrum of Comparative Example 2, the maximum value of the emission intensity was normalized as 1.00. Furthermore, for the Mn-activated phosphors of Examples 1 to 4 and Comparative Example 1, the peak position and half-width of the emission peak were measured from the obtained emission spectrum. MAX ), and fluorescence intensity at 650 nm I 650 I MAX / I 650 was calculated.

[0056] Based on the presence or absence of an emission peak in the wavelength range of 600 nm or more and 900 nm or less in the above emission spectrum, it was judged whether emission in that range was present (◯) or not (×). Emission in the wavelength range of 600 nm or more and 900 nm or less was confirmed in the Mn-activated phosphors of Examples 1 to 4 and Comparative Example 1, but not in the Eu-activated phosphor of Comparative Example 2. On the other hand, emission in the wavelength range of 400 nm or more and less than 500 nm was confirmed only for the Eu-activated phosphor of Comparative Example 2.

[0057] When irradiated with light having a wavelength of 254 nm, the Mn-activated phosphors of Examples 1 to 4 exhibited emission peaks in the wavelength range of 600 nm or more and 900 nm or less, and showed superior emission characteristics compared to Comparative Example 1. From these examples, it is clear that it is possible to realize a Mn-activated phosphor suitable for various devices that utilize near-infrared light.

Claims

1. A Mn-activated phosphor that emits light having an emission peak in a wavelength range of 600 nm to 900 nm when irradiated with light having a wavelength of 254 nm, General formula: Mg 1-x S 1 A 3+p Mn y O 2+q N 3+z (wherein 0.2≦x≦1, 0<y≦0.1, 0.1≦p≦1.5, 0≦q≦1.5, and 0.5≦z≦1.5).

2. 2. The Mn-activated phosphor of claim 1, A Mn-activated phosphor, in which, in an emission spectrum when irradiated with light having a wavelength of 254 nm, the half-width of an emission peak in a wavelength range of 600 nm to 900 nm is 100 nm to 170 nm.

3. 3. The Mn-activated phosphor according to claim 1, In the emission spectrum when light with a wavelength of 254 nm is irradiated, the fluorescence intensity at 650 nm is I 650 , the fluorescence intensity at the emission peak in the wavelength range of 600 nm to 900 nm is I MAX Then, I 650 , I MAX However, 1.5≦I MAX / I 650 A Mn-activated phosphor that satisfies the above requirement.

4. The Mn-activated phosphor according to any one of claims 1 to 3, A Mn-activated phosphor comprising a compound that satisfies the above general formula: 0<1-x+y≦1.

0.

5. The Mn-activated phosphor according to any one of claims 1 to 4, The Mn-activated phosphor has the formula Mg f S g A h O j1 N j2 Mn i It is expressed as The composition ratios f, g, h, j1, j2 and i are 0.00≦f≦0.88, 0.70≦g≦1.30, 0.70≦h≦4.50, 5.50≦j1+j2≦7.50, 0.00<i≦1.30, and A Mn-activated phosphor configured to satisfy 0.70≦h+i≦5.

30.

6. The Mn-activated phosphor according to any one of claims 1 to 5, A Mn-activated phosphor, in which a particle diameter D50 at which a cumulative value reaches 50% in a volume frequency particle size distribution measured by a laser diffraction scattering method is 1 μm or more and 50 μm or less.

7. 7. The Mn-activated phosphor of claim 6, In the volume frequency particle size distribution measured by a laser diffraction scattering method, when the particle diameter at which the cumulative value reaches 10% is defined as D10 and the particle diameter at which the cumulative value reaches 90% is defined as D90, A Mn-activated phosphor, in which (D90-D10) / D50 is 1.0 or more and 20.0 or less.

8. A wavelength converter comprising the Mn-activated phosphor according to any one of claims 1 to 7.

9. A light emitting device comprising the wavelength converter according to claim 8.

Citation Information

Patent Citations

  • Manganese-chromium-codoped silicon-aluminium oxynitride alkaline-earth salt luminescent material, preparation method and application thereof

    CN104140813A

  • Red long-afterglow nitride luminescent material and preparation method thereof

    CN110055061A

  • Phosphor, method for manufacturing the same, light emitting device, image display device, pigment, and ultraviolet absorber

    JP2015000965A

  • Phosphor, method for producing same and light-emitting device

    WO2006016711A1

  • Phosphor, method for producing same, and light-emitting device

    WO2007099862A1