Cr-activated phosphor, wavelength converter, and light-emitting device
The development of a Cr-activated phosphor with a specific formula achieves near-infrared emission when excited by 450 nm light, addressing the emission gap in existing Eu-activated phosphors and enhancing luminescence for diverse applications.
Patent Information
- Application Number
- JP2021047140
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-22
AI Technical Summary
Existing Eu-activated phosphors do not emit light in the range of 600 nm or more and 1000 nm or less when irradiated with light of 450 nm wavelength, and there is a lack of near-infrared emitting phosphors with the Mg1Si1Al3O3N3 crystal structure.
A Cr-activated phosphor with the general formula Mg x SiAl(4-x-y)Cr y O(2+x+3y/2)N(4-x-y) (0≦x≦0.5, 0
The Cr-activated phosphor achieves emission peaks in the near-infrared region with improved luminescence characteristics, suitable for various applications including sensors, inspection, analysis, security, and optical communication.
Smart Images

Figure 0007575316000003 
Figure 0007575316000004 
Figure 0007575316000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a Cr-activated phosphor, a wavelength converter, and a light emitting device. [Background technology]
[0002] Various developments have been made so far regarding phosphors containing crystals whose chemical composition is represented by Mg1Si1Al3O3N3. For example, the technology described in Patent Document 1 is known as this type of technology. Patent Document 1 describes a phosphor in which Eu is dissolved in an inorganic crystal having the same crystal structure as a crystal whose chemical composition is represented by Mg1Si1Al3O3N3, and which emits blue to green fluorescence from 450 nm to 530 nm when irradiated with light from 250 nm to 500 nm (claim 23 of Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-000965 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, the Eu-activated phosphor described in Patent Document 1 does not have an emission peak in the range of 600 nm or more and 1000 nm or less in the emission spectrum when irradiated with light having a wavelength of 450 nm. In addition, it was not known that a phosphor that emits near-infrared light could be obtained by dissolving Cr in an inorganic crystal having the same crystal structure as a crystal with the chemical composition represented by Mg1Si1Al3O3N3. [Means for solving the problem]
[0005] As a result of the research conducted by the inventors with the aim of realizing a near-infrared emitting phosphor, Cr was selected as the activator element, and the phosphor was synthesized according to the general formula: Mg x SiAl (4-x-y) Cry O (2+x+3y / 2) N (4-x-y) (However, by using a compound represented by 0 ≦ x ≦ 0.5, 0 < y ≦ 0.3), when irradiated with light having a wavelength of 450 nm, it has been found that a novel phosphor having an emission peak in the range of 600 nm or more and 1000 nm or less can be realized in the emission spectrum, and the present invention has been completed.
[0006] According to the present invention, a Cr-activated phosphor that emits light having an emission peak in the wavelength range of 600 nm or more and 1000 nm or less when irradiated with light having a wavelength of 450 nm, General formula: Mg x SiAl (4-x-y) Cr y O (2+x+3y / 2) N (4-x-y) (However, 0 ≦ x ≦ 0.5, 0 < y ≦ 0.3) is provided, a Cr-activated phosphor containing a compound represented by the formula.
[0007] Also according to the present invention, a wavelength converter containing the above Cr-activated phosphor is provided.
[0008] Also according to the present invention, a light-emitting device provided with the above wavelength converter is provided.
Advantages of the Invention
[0009] According to the present invention, when irradiated with light having a wavelength of 450 nm, a Cr-activated phosphor having an emission peak in the range of 600 nm or more and 1000 nm or less in the emission spectrum, a wavelength converter using the same, and a light-emitting device are provided.
Brief Description of the Drawings
[0010] [Figure 1] It is a figure which shows the XRD pattern in the phosphors of Example 1, 3, 6, and Comparative Example 1. [Diagram 2] It is a figure which shows the emission spectrum in the phosphors of Example 1, 3, 6, and Comparative Example 1.
Modes for Carrying Out the Invention
[0011] An overview of the Cr-activated phosphor of this embodiment will be described.
[0012] The Cr-activated phosphor is a phosphor that emits light having an emission peak in the wavelength range of 600 nm or more and 1000 nm or less when irradiated with light having a wavelength of 450 nm. This Cr-activated phosphor has the general formula: Mg x SiAl (4-x-y) Cr y O (2+x+3y / 2) N (4-x-y) (However, 0 ≦ x ≦ 0.5, 0 < y ≦ 0.3) and contains a compound represented by.
[0013] According to the findings of the present inventor, by using a compound having the general formula: Mg x SiAl (4-x-y) Cr y O (2+x+3y / 2) N (4-x-y) (However, 0 ≦ x ≦ 0.5, 0 < y ≦ 0.3), it is possible to appropriately control the doping amount of the activating element Cr in the phosphor, and thus it has been found that a Cr-activated phosphor excellent in emission characteristics in the near-infrared region and / or near the near-infrared region can be realized.
[0014] Although the detailed mechanism is not clear, it is considered that by substituting a part of the elements in the phosphor with Cr elements, the emission peak position can be shifted to the long wavelength side, and a phosphor that emits light in the vicinity of the near-infrared region can be realized. In addition, it is considered that the emission characteristics can be enhanced by appropriately controlling the content of Mg element in the phosphor.
[0015] The Cr-activated phosphor of this embodiment can be excited by blue light to red light having a wavelength of 350 nm to 660 nm.
[0016] The wavelength converter including the Cr-activated phosphor of this embodiment is composed of a member that converts irradiated light (excitation light) and emits light having an emission peak in a wavelength range different from that of the excitation light. The wavelength converter may constitute at least a part of the light emitting device described below. The wavelength converter may emit light having an emission peak in a wavelength range of, for example, 600 nm or more and 1000 nm or less. The wavelength converter may include one or more known phosphors other than the Cr-activated phosphor of this embodiment.
[0017] The wavelength converter may be composed only of a Cr-activated phosphor, or may include a host material in which the Cr-activated phosphor is dispersed. Known host materials can be used, such as glass, resin, and inorganic materials.
[0018] A light emitting device including the wavelength converter of this embodiment can be used for various applications such as sensors, inspection, analysis, security, optical communications, and medical applications, and examples thereof include LED packages, light sources, stationary spectrophotometers, handheld food analyzers, wearable devices, infrared cameras, moisture measuring devices, and gas detectors.
[0019] An example of a light emitting device includes a light emitting element and a wavelength converter including a Cr-activated phosphor that converts light irradiated from the light emitting element and emits light. The shape of such a wavelength converter is not particularly limited, and it may be configured in a plate shape, for example, to seal a part of the light emitting element or the entire light emitting surface.
[0020] The Cr-activated phosphor of this embodiment will be described in detail below.
[0021] When irradiated with light having a wavelength of 450 nm, the Cr-activated phosphor has an emission spectrum with an emission peak in a wavelength range of 600 nm to 1000 nm, preferably 650 nm to 950 nm, and more preferably 680 nm to 900 nm.
[0022] The position of the emission peak depends on the concentration of the Cr element contained in the phosphor, that is, the general formula: Mg xSiAl (4-x-y) Cr y O (2+x+3y / 2) N (4-x-y) (However, it can be controlled by appropriately adjusting y, x, etc. in the range of 0 ≦ x ≦ 0.5, 0 < y ≦ 0.3).
[0023] In the emission spectrum of the Cr-activated phosphor when irradiated with light having a wavelength of 450 nm, the full width at half maximum of the emission peak in the wavelength range of 600 nm or more and 1000 nm or less is, for example, 100 nm or more and 250 nm or less, preferably 110 nm or more and 240 nm or less, more preferably 120 nm or more and 230 nm or less. By setting the full width at half maximum within the above range, the emission intensity at the peak wavelength can be improved.
[0024] In the above general formula, the lower limit of x is, for example, 0.01 or more, preferably 0.02 or more, more preferably 0.05 or more. Thereby, the emission intensity of the emission peak can be increased. On the other hand, the upper limit of x is 0.5 or less, preferably 0.4 or less, more preferably 0.3 or less. Thereby, the shape of the emission peak can be made sharper, and emission without visible light components can be obtained, which is preferable.
[0025] In the above general formula, the lower limit of y is preferably 0.0005 or more, more preferably 0.001 or more. Thereby, light in the vicinity of the near-infrared region can be emitted. On the other hand, the upper limit of y is preferably 0.09 or less, more preferably 0.07 or less. Thereby, the emission intensity at the peak wavelength can be increased.
[0026] The Cr-activated phosphor may contain a compound satisfying 0 < x + y ≦ 0.8, preferably 0 < x + y ≦ 0.5, more preferably 0 < x + y ≦ 0.3 in the above general formula. Thereby, light in the vicinity of the near-infrared region can be emitted, and the emission intensity of the emission peak can be increased.
[0027] When the Cr-activated phosphor has the composition formula Mg f Si g Al h Oj1 N j2 Cr i is represented by composition ratios f, g, h, j1, j2, and i satisfy 0.00 ≦ f ≦ 0.50, 0.70 ≦ g ≦ 1.30, 0.70 ≦ h ≦ 4.30, 5.70 ≦ j1 + j2 ≦ 6.30, 0.00 < i ≦ 1.30, and 0.70 ≦ h + i ≦ 5.30.
[0028] In the emission spectrum of the Cr-activated phosphor when irradiated with light having a wavelength of 450 nm, let the fluorescence intensity at 600 nm be I 600 and the fluorescence intensity at the emission peak in the wavelength range of 600 nm or more and 1000 nm or less be I MAX . The Cr-activated phosphor may be configured such that I 600 , I MAX satisfy, for example, 1.5 ≦ I MAX / I 600 , preferably 5.0 ≦ I MAX / I 600 , more preferably 10.0 ≦ I MAX / I 600 . This makes it possible to shift the emission peak to the longer wavelength side and make the shape of the emission peak sharper, and it is preferable because emission without visible light components can be obtained. On the other hand, the Cr-activated phosphor may be configured such that I 600 , I MAX satisfy, for example, I MAX / I 600 ≦ 1000.
[0029] For the Cr-activated phosphor, in the volume frequency particle size distribution measured using the laser diffraction scattering method, let the particle diameter at which the cumulative value is 50% be D50, the particle diameter at which the cumulative value is 10% be D10, and the particle diameter at which the cumulative value is 90% be D90.
[0030] D50 is, for example, 1 μm or more and 50 μm or less, preferably 2 μm or more and 40 μm or less, more preferably 3 μm or more and 30 μm or less. By setting it within the above range, the balance of the light-emitting characteristics can be achieved.
[0031] (D90 - D10) / D50 has a lower limit of, for example, 1.0 or more, preferably 1.5 or more, more preferably 2.0 or more. On the other hand, the upper limit of (D90 - D10) / D50 is, for example, 20.0 or less, preferably 10.0 or less, more preferably 7.0 or less. By setting it within the above range, the balance of the light-emitting characteristics can be achieved.
[0032] Hereinafter, the method for manufacturing the Cr-activated phosphor of the present embodiment will be described.
[0033] An example of the method for manufacturing the Cr-activated phosphor may include a mixing step of obtaining a raw material mixture containing each element constituting the composition of the compound represented by the general formula: Mg x SiAl (4-x-y) Cr y O (2+x+3y / 2) N (4-x-y) (where 0 ≤ x ≤ 0.5, 0 < y ≤ 0.3), and a firing step of firing the raw material mixture.
[0034] Examples of the raw material containing the Mg element include a single substance or a mixture of two or more selected from metals, silicides, oxides, carbonates, nitrides, oxynitrides, chlorides, fluorides, and acid fluorides containing Mg. Examples of the raw material containing the Si element include a single substance or a mixture of two or more selected from metals, oxides, carbonates, nitrides, oxynitrides, chlorides, fluorides, and acid fluorides containing Si. Examples of the raw material containing the Al element include a single substance or a mixture of two or more selected from metals, silicides, oxides, carbonates, nitrides, oxynitrides, chlorides, fluorides, and acid fluorides containing Al.
[0035] As the raw material containing Cr, a single substance or a mixture of two or more substances selected from metals, silicides, oxides, carbonates, nitrides, oxynitrides, chlorides, fluorides, and oxyfluorides containing Cr can be used.
[0036] The raw material mixture may contain, for example, Cr nitride or oxide, Mg nitride or oxide, Al nitride or oxide, and silicon oxide or silicon nitride, which can promote the reaction during firing.
[0037] The method for mixing the raw materials is not particularly limited, but examples include a method in which the raw materials are thoroughly mixed using a mixing device such as a mortar, a ball mill, a V-type mixer, or a planetary mill.
[0038] The firing step is a step of firing the above-mentioned raw material mixture in a firing furnace such as an electric furnace. The firing atmosphere in the firing furnace may be a non-oxidizing gas such as argon, helium, hydrogen, nitrogen, etc. These may be used alone or in combination of two or more kinds.
[0039] The calcination temperature in the calcination step is selected from the viewpoints of reducing unreacted raw materials after the calcination step and suppressing decomposition of the main component. The lower limit of the firing temperature in the firing step is preferably 1000° C. or higher, more preferably 1200° C. or higher, and even more preferably 1500° C. or higher. On the other hand, the upper limit of the firing temperature is preferably 2200° C. or lower, more preferably 2000° C. or lower, and even more preferably 1900° C. or lower.
[0040] The pressure of the firing atmosphere gas is selected depending on the firing temperature, but is usually in the range of 0.1 MPa to 10 MPa, and is preferably 0.5 MPa to 1 MPa in consideration of industrial productivity.
[0041] The calcination time in the calcination step is selected from an appropriate time range from the viewpoints of reducing unreacted materials and improving productivity. The lower limit of the firing time is preferably 0.5 hours or more, more preferably 1 hour or more, and even more preferably 2 hours or more, and the upper limit of the firing time is preferably 48 hours or less, more preferably 24 hours or less, and even more preferably 10 hours or less.
[0042] As a result of the above, the raw material mixture (calcined product) is obtained after the calcination step.
[0043] The method for producing a Cr-activated phosphor of this embodiment may further include a pulverizing step of pulverizing the raw material mixture (fired product) after the firing step to obtain a pulverized product.
[0044] The state of the fired product obtained by the firing process varies depending on the raw material composition and firing conditions, from powder to lumps. The fired product can be made into powder of a specified size by the crushing process and / or classification process. In addition to the above, a process known in the field of phosphors may be added.
[0045] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES
[0046] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.
[0047] [Examples 1 to 6] (Production of Cr-activated phosphor) Silicon nitride (Si3N4), aluminum nitride (AlN), aluminum oxide (Al2O3), magnesium oxide (MgO), and chromium oxide (Cr2O3) were weighed according to the design composition shown in Table 1, and mixed in a mortar to obtain a raw material mixture. x SiAl (4-x-y) Cr y O (2+x+3y / 2) N (4-x-y)Represents x and y. The resulting raw material mixture was placed in an electric furnace and fired in a nitrogen atmosphere at 1700° C. and 0.8 MPa for 4 hours. The obtained fired product was pulverized in a mortar and then sieved (classified) with a sieve having an opening of 150 μm, and the part that passed through the sieve was collected to obtain a powdered Cr-activated phosphor (phosphor particles).
[0048] As a result of powder X-ray diffraction measurement (XRD measurement) using Cu-Kα radiation, a peak attributed to Mg1Si1Al3O3N3 was confirmed for all of the Cr-activated phosphors obtained in Examples 1 to 6, and it was confirmed that the crystal structure of the main phase was the same as Mg1Si1Al3O3N3. In addition, for the Cr-activated phosphors obtained in Examples 5 and 6, although the crystal structure of the main phase was the same as Mg1Si1Al3O3N3, a diffraction peak of small intensity attributed to β-SiAlON was confirmed, and it was confirmed that a trace amount of β-SiAlON was contained as a subphase. The XRD patterns of Examples 1, 3, and 6 and Comparative Example 1 are shown in FIG.
[0049] [Table 1]
[0050] [Comparative Example 1] A powdered Eu-activated phosphor (phosphor particles) represented by Mg1Si1Al3O3N3:Eu was obtained in the same manner as in Example 1, except that chromium oxide (Cr2O3) was changed to europium oxide (Eu2O3).
[0051] [Table 2]
[0052] (D10, D50, D90) The particle size distribution of the powdered Cr-activated phosphor was measured using a particle size measuring device (LS 13 320, manufactured by Beckman Coulter) using a laser diffraction / scattering method.
[0053] (Emission spectrum) For the Cr-activated phosphors of Examples 1 to 6 and the Eu-activated phosphor of Comparative Example 1, emission spectra were obtained using a spectrofluorometer as follows. First, a powdered Cr-activated phosphor was filled in a solid sample holder (a synthetic quartz cell) attached to a photometer, and then, using a spectrofluorophotometer (Fluorolog-3, manufactured by Horiba, Ltd.) equipped with a cut filter (a filter that absorbs light with a wavelength of 490 nm or less), a Xe lamp was used as a light source to measure the emission spectrum when irradiated with excitation light with a wavelength of 450 nm. Note that, only in the case of Comparative Example 1, a lamp that emits light with a wavelength of 365 nm was used as the excitation light, and a filter that absorbs light with a wavelength of 390 nm or less was used as the cut filter. The emission spectra of Examples 1, 3, and 6, and Comparative Example 1 are shown in FIG. 2. In the emission spectra of each Example, the maximum emission intensity (I MAX ) was normalized as 1.00, and in the emission spectrum of Comparative Example 1, the maximum value of the emission intensity was normalized as 1.00. Furthermore, for the Cr-activated phosphors of Examples 1 to 6, the peak position and half-width of the emission peak were measured from the obtained emission spectrum. From the obtained emission spectrum, the maximum emission intensity (I MAX ), and the fluorescence intensity at 600 nm I 600 I MAX / I 600 was calculated.
[0054] Based on the presence or absence of an emission peak in the wavelength range of 600 nm or more and 1000 nm or less in the above emission spectrum, it was judged whether emission in that range was present (◯) or not (×). Emission in the near infrared region in the wavelength range of 600 nm or more and 1000 nm or less was confirmed in the Cr-activated phosphors of Examples 1 to 6, but was not confirmed in the Eu-activated phosphor of Comparative Example 1. On the other hand, emission in the wavelength range of 400 nm or more and less than 500 nm was confirmed only for the Eu-activated phosphor of Comparative Example 1.
[0055] The Cr-activated phosphor of the present invention exhibits an emission peak in the wavelength range of 600 nm or more and 1000 nm or less when excited by excitation light with a wavelength of 450 nm, and thus exhibits excellent emission characteristics. It was therefore demonstrated that a Cr-activated phosphor suitable for various devices utilizing near-infrared light can be realized.
Claims
1. A Cr-activated phosphor that emits light having an emission peak in a wavelength range of 600 nm to 1000 nm when irradiated with light having a wavelength of 450 nm, General formula: Mg x SiAl (4-x-y) Cr y O (2+x+3y/2) N (4-x-y) (wherein 0≦x≦0.5, 0<y≦0.3)
2. 2. The Cr-activated phosphor of claim 1 , A Cr-activated phosphor having an emission spectrum when irradiated with light having a wavelength of 450 nm, in which the half width of an emission peak in a wavelength range of 600 nm to 1000 nm is 100 nm to 250 nm.
3. 3. The Cr-activated phosphor according to claim 1, In the emission spectrum when light with a wavelength of 450 nm is irradiated, the fluorescence intensity at 600 nm is expressed as I 600 , the fluorescence intensity at the emission peak in the wavelength range of 600 nm to 1000 nm is I MAX Then, I 600 , I MAX However, 1.5≦I MAX / I 600 A Cr-activated phosphor that satisfies the above requirement.
4. The Cr-activated phosphor according to any one of claims 1 to 3, A Cr-activated phosphor comprising a compound that satisfies 0<x+y≦0.8 in the above general formula.
5. The Cr-activated phosphor according to any one of claims 1 to 4, A Cr-activated phosphor, in which D50, the particle diameter at which the cumulative value is 50%, is 1 μm or more and 50 μm or less in a volume frequency particle size distribution measured by a laser diffraction scattering method.
6. 6. The Cr-activated phosphor of claim 5, In the volume frequency particle size distribution measured by a laser diffraction scattering method, when the particle diameter at which the cumulative value is 10% is defined as D10 and the particle diameter at which the cumulative value is 90% is defined as D90, A Cr-activated phosphor, wherein (D90-D10) / D50 is 1.0 or more and 20.0 or less.
7. A wavelength converter comprising the Cr-activated phosphor according to any one of claims 1 to 6.
8. A light emitting device comprising the wavelength converter according to claim 7.
Citation Information
Patent Citations
Manganese-chromium-codoped silicon-aluminium oxynitride alkaline-earth salt luminescent material, preparation method and application thereof
CN104140813A
Nitrogen oxide blue-green phosphor and preparation method thereof
CN110452691A
Phosphor comprising oxynitride glass as matrix material
JP2001214162A
Phosphor, method for manufacturing the same, light emitting device, image display device, pigment, and ultraviolet absorber
JP2015000965A
Oxynitride fluorescent powder with transition metal as light-emitting center, and preparation method therefor
WO2021243521A1