Polishing composition, its manufacturing method, and polishing method

The polishing composition with silica particles and specific polishing accelerators enhances the polishing rate of titanium nitride surfaces by embrittling bonds, addressing the inefficiencies of existing technologies.

JP7575878B2Active Publication Date: 2024-10-30FUJIMI INCORPORATED
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020053111
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-24
Publication Date
2024-10-30
Estimated Expiration
2040-03-24

AI Technical Summary

Technical Problem

Existing polishing technologies for titanium nitride surfaces have insufficient polishing rates, necessitating a higher rate for effective processing.

Method used

A polishing composition containing silica particles and a polishing accelerator, such as compounds with aromatic heterocycles or aromatic hydrocarbon rings bonded to OH or COOH groups, enhances the polishing rate of titanium nitride surfaces.

Benefits of technology

The composition significantly improves the polishing rate of titanium nitride surfaces by embrittling Ti-N or Ti-O bonds, achieving higher efficiency and selectivity in polishing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575878000001
    Figure 0007575878000001
  • Figure 0007575878000002
    Figure 0007575878000002
  • Figure 0007575878000003
    Figure 0007575878000003
Patent Text Reader

Abstract

To provide means for polishing a titanium nitride-containing target at a high polishing rate.SOLUTION: The present invention relates to a polishing composition comprising silica particles and a grinding accelerator, which is used to polish a titanium nitride-containing target. The grinding accelerator comprises a compound which includes a heteroaromatic ring, and an OH group or a group of its salt, directly coupled to the heteroaromatic ring, or a compound which includes an aromatic hydrocarbon ring, an OH group or a group of its salt, directly coupled to the aromatic hydrocarbon ring, and a COOH group or a group of its salt, directly coupled to the aromatic hydrocarbon ring.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing composition, a method for producing the same, and a polishing method. [Background technology]

[0002] In recent years, with the trend toward multi-layer wiring on the surface of semiconductor substrates, a so-called chemical mechanical polishing (CMP) technique is used to polish and flatten semiconductor substrates when manufacturing devices. CMP is a method for flattening the surface of an object to be polished (object to be polished) such as a semiconductor substrate by using a polishing composition (slurry) containing abrasive grains such as silica, alumina, ceria, etc., an anticorrosive agent, a surfactant, etc., and the object to be polished (object to be polished) is a film containing silicon, polysilicon, silicon oxide (silicon oxide), silicon nitride, titanium nitride, titanium, tantalum nitride, tantalum, etc., wiring, plugs, etc. made of metals such as copper and tungsten, etc.

[0003] In particular, focusing on the polishing of titanium nitride, Patent Document 1 discloses that titanium and titanium nitride can be polished using a polishing composition containing an oxidizing agent, an abrasive (abrasive grains), and a fluoride-containing additive.

[0004] Furthermore, Patent Document 2 discloses that titanium and titanium nitride can be polished with a polishing composition containing 0.1 mass % or more of colloidal silica and water and having a pH of 6.0 or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-67986 [Patent Document 2] JP 2005-244123 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0006] However, the technique of Patent Document 1 has a problem in that the polishing speed of titanium nitride is not sufficient.

[0007] Furthermore, although the technique of Patent Document 2 is effective in improving the polishing rate for titanium, a higher polishing rate for titanium nitride is required.

[0008] SUMMARY OF THE PRESENT EMBODIMENTS An object of the present invention is to provide a means for polishing an object containing titanium nitride at a high polishing rate. [Means for solving the problem]

[0009] The above object of the present invention can be achieved by the following means: Contains silica particles and an abrasion accelerator; The abrasion accelerator is A compound comprising an aromatic heterocycle and an OH group or a salt group thereof directly bonded to said aromatic heterocycle, or A compound comprising an aromatic hydrocarbon ring, an OH group or a salt group thereof directly bonded to the aromatic hydrocarbon ring, and a COOH group or a salt group thereof directly bonded to the aromatic hydrocarbon ring; The polishing composition is used for polishing an object containing titanium nitride. Effect of the Invention

[0010] According to the present invention, a means can be provided for polishing an object containing titanium nitride at a high polishing rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, the embodiments of the present invention will be described. Note that the present invention is not limited to only the following embodiments. In addition, in this specification, the range "X to Y" means "X or more and Y or less". Furthermore, unless otherwise specified, the operation and measurement of physical properties are performed under the conditions of room temperature (range of 20°C to 25°C) and relative humidity of 40% RH to 50% RH.

[0012] <Polishing composition> One embodiment of the present invention relates to a polishing composition which comprises silica particles and a polishing accelerator, the polishing accelerator being a compound containing an aromatic heterocycle and an OH group or a group of a salt thereof directly bonded to the aromatic heterocycle, or a compound containing an aromatic hydrocarbon ring, an OH group or a group of a salt thereof directly bonded to the aromatic hydrocarbon ring, and a COOH group or a group of a salt thereof directly bonded to the aromatic hydrocarbon ring, the polishing composition being used for polishing an object to be polished which contains titanium nitride.

[0013] Although the mechanism by which the above problems can be solved is not clear in detail, the present inventors speculate as follows.

[0014] A method of increasing electrical conductivity is generally known as a method for polishing a specific object to be polished at a high polishing rate. However, high electrical conductivity may also accelerate the polishing rate of other materials (e.g., a stopper film), which may be undesirable from the viewpoint of increasing the selectivity. However, in the present invention, the above-mentioned polishing accelerator is used in such a manner that the ionized carboxyl group (COO - group) or ionized hydroxyl group (O - The TiN bond or TiO bond is coordinated with the TiN group, and acts to embrittle the TiN bond or TiO bond, accelerating the polishing of titanium nitride. For this reason, the polishing composition of the present invention can significantly improve the polishing rate of a polishing object containing titanium nitride, regardless of the level of electrical conductivity.

[0015] It should be noted that the above mechanism is based on speculation, and whether it is correct or not does not affect the technical scope of the present invention.

[0016] Hereinafter, each component that can be contained in the polishing composition, the object to be polished, and the like will be described.

[0017] (Object to be polished) The polishing composition according to one embodiment of the present invention is used to polish an object to be polished that contains titanium nitride (TiN). The object to be polished is not particularly limited as long as the surface to be polished contains titanium nitride, and can be applied to known objects to be polished that are used in the CMP field. Therefore, the form of the object to be polished is not particularly limited, but is preferably a layer that is a flat plate-like member, more preferably a substrate that contains the layer, and even more preferably a semiconductor substrate. For example, a substrate composed of a single layer, a substrate that contains a layer to be polished and other layers (for example, a support layer or other functional layers), etc. can be mentioned.

[0018] The polishing object may be an object whose surface to be polished further includes, in addition to titanium nitride, a component part containing other materials such as a silicon-containing material or a metal. The silicon-containing material is not particularly limited, but may be, for example, a material having a silicon-oxygen bond (e.g., silicon oxide, etc.), a material having a silicon-silicon bond (e.g., polysilicon, etc.), or a material having a silicon-nitrogen bond (e.g., silicon nitride, etc.). The metal is not particularly limited, but may be, for example, copper, aluminum, hafnium, cobalt, nickel, titanium, tungsten, or an alloy thereof. The polishing object may be, for example, a film composed of titanium nitride alone (titanium nitride film), etc.

[0019] (polishing accelerator) The polishing composition according to one embodiment of the present invention contains a polishing accelerator. The polishing accelerator is a compound containing an aromatic heterocycle and an OH group or a salt group thereof directly bonded to the aromatic heterocycle, or a compound containing an aromatic hydrocarbon ring and an OH group or a salt group thereof directly bonded to the aromatic hydrocarbon ring, and a COOH group or a salt group thereof directly bonded to the aromatic hydrocarbon ring. As described above, the polishing accelerator is a compound that reacts with the titanium nitride to be polished by ionizing the carboxyl group (COO - group) or ionized hydroxyl group (O - The titanium nitride-containing polishing agent acts to significantly improve the polishing rate of a polishing object containing titanium nitride by coordinating with the Ti-N bond or Ti-O bond and embrittling the Ti-N bond or Ti-O bond.

[0020] Here, the aromatic heterocycle refers to an aromatic ring having one or more heteroatoms (e.g., nitrogen atom (N), oxygen atom (O), phosphorus atom (P), sulfur atom (S)) as ring-forming atoms, and the remaining ring-forming atoms are carbon atoms (C). The aromatic heterocycle is not particularly limited, but is preferably a monocyclic aromatic heterocycle. The number of heteroatoms is not particularly limited, but is preferably 1 to 3. Examples of the monocyclic aromatic heterocycle having 1 to 3 heteroatoms include, but are not particularly limited to, a furan ring, a pyrrole ring, a thiophene ring, an imidazole ring, a pyrazole ring, an oxazole ring, an isoxazole ring, a thiazole ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a pyridazine ring, a 1,2,3-triazine ring, a 1,2,4-triazine ring, and a 1,3,5-triazine ring. The type of the heteroatom is not particularly limited, but is preferably N.

[0021] As a compound containing an aromatic heterocycle and an OH group or a salt group thereof directly bonded to the aromatic heterocycle, from the viewpoint of improving the polishing rate of a polishing object containing titanium nitride, a compound represented by the following general formula (1) is preferable.

[0022] [ka]

[0023] In the above general formula (1), each Z is independently CR1 or N; In this case, 1 to 3 Z's are N's. Each R1 is independently selected from the group consisting of a hydrogen atom, an OH group or a salt thereof, and a COOH group or a salt thereof; In this case, at least one R1 is an OH group or a salt thereof.

[0024] In the above general formula (1), a compound in which one Z is N and five Z are CR1 is preferred. When one Z is N and five Z are CR1, it is preferred that one or two R1 out of five R1 are OH groups or salt groups, and it is more preferred that one R1 out of five R1 is OH groups or salt groups. When one Z is N and five Z are CR1, it is preferred that all R1 out of five R1 are not COOH groups or salt groups (the compound does not have COOH groups or salt groups), or one R1 is a COOH group or salt group, and it is more preferred that one R1 out of five R1 is a COOH group or salt group.

[0025] Moreover, the aromatic hydrocarbon ring refers to an aromatic ring whose ring-forming element is composed of only carbon atoms. The aromatic hydrocarbon ring is not particularly limited, but more preferably has 6 to 14 ring carbon atoms. The aromatic hydrocarbon ring having 6 to 14 ring carbon atoms is not particularly limited, but examples thereof include a benzene ring, a naphthalene ring, an anthracene ring, a phenalene ring, and a phenanthrene ring. Among these, a benzene ring is preferred from the viewpoint of further improving the polishing speed of a polishing target containing titanium nitride.

[0026] From the viewpoint of improving the polishing rate of a titanium nitride-containing object to be polished, a compound containing an aromatic hydrocarbon ring, an OH group or a salt group thereof directly bonded to the aromatic hydrocarbon ring, and a COOH group or a salt group thereof directly bonded to the aromatic hydrocarbon ring is preferably a compound represented by the following general formula (2):

[0027] [ka]

[0028] In the above general formula (2), each R2 is independently selected from the group consisting of a hydrogen atom, an OH group or a salt thereof, and a COOH group or a salt thereof; In this case, at least one R2 is an OH group or a salt thereof, and at least one R2 is a COOH group or a salt thereof.

[0029] In the above general formula (2), it is preferable that one of the six R2 is an OH group or a salt thereof. It is also preferable that one of the six R2 is a COOH group or a salt thereof.

[0030] In the polishing accelerator, the COOH group or its salt group directly bonded to the aromatic heterocycle or aromatic hydrocarbon ring is converted into an ionized carboxy group (COO - In addition, the OH group or the salt group directly bonded to the aromatic heterocycle or aromatic hydrocarbon ring is preferably present in the form of an ionized hydroxyl group (O - It is particularly preferred that the aryl group is present in the form of a aryl group.

[0031] Thus, a preferred example of the polishing accelerator is a compound represented by the above general formula (1) or the above general formula (2). Among these, a compound represented by the above general formula (1), in which one Z is N, five Z are CR1, one or two R1 of five R1 are OH group or a salt group, one R1 of five R1 is COOH group or a salt group or a hydrogen atom, and the remaining R1 of five R1 is a hydrogen atom is more preferred. Also, a compound represented by the above general formula (2), in which one R2 of six R2 is OH group or a salt group, one R2 of six R2 is COOH group or a salt group, and four R2 of six R2 are hydrogen atoms is more preferred. Further preferred is a compound represented by the above general formula (1), in which one Z is N, five Z are CR1, two of the five R1 are OH groups or salt groups thereof, one of the five R1 is COOH groups or salt groups thereof or a hydrogen atom, and two of the five R1 are hydrogen atoms.

[0032] In the compound represented by the above general formula (1), the positional relationship between the N atom and the OH group or the group of its salt is preferably such that the OH group or the group of its salt is directly bonded to the carbon atom that is a ring-forming atom adjacent to the N atom that is a ring-forming atom (at the ortho position of the N atom). Also, it is preferable that the OH group or the group of its salt is directly bonded to the carbon atom that is adjacent to the N atom that is a ring-forming atom (the carbon atom that is a ring-forming atom further adjacent to the carbon atom that is a ring-forming atom adjacent to the N atom that is a ring-forming atom).

[0033] In a compound represented by the above general formula (1) and in which at least one R1 is a COOH group or a salt group, the positional relationship between the OH group or a salt group and the COOH group or a salt group is preferably such that these groups are directly bonded to adjacent ring-forming atoms. In addition, in a compound represented by the above general formula (1) and in which at least one R1 is a COOH group or a salt group, the positional relationship between the OH group or a salt group and the COOH group or a salt group is preferably such that the COOH group or a salt group is directly bonded to the ring-forming atom adjacent to the ring-forming atom to which the OH group is directly bonded (the ring-forming atom adjacent to the ring-forming atom to which the OH group is directly bonded). In addition, in a compound represented by the above general formula (2), the positional relationship between the OH group or a salt group and the COOH group or a salt group is preferably such that they are directly bonded to adjacent ring-forming atoms. Among these, in the compound represented by the above general formula (1) and in which at least one R1 is a COOH group or a salt group, it is more preferable that the COOH group or a salt group is directly bonded to the ring-forming atom adjacent to the ring-forming atom directly bonded to the OH group (the ring-forming atom adjacent to the ring-forming atom adjacent to the ring-forming atom).

[0034] The OH group or its salt group contained in the polishing accelerator is not particularly limited, but is preferably an OH group. Also, the COOH group or its salt group contained in the polishing accelerator is preferably a COOH group.

[0035] Specific examples of the polishing accelerator are not particularly limited, but from the viewpoint of the effect of improving the polishing rate of a polishing object containing titanium nitride, 1-hydroxypyridine, 2-hydroxypyridine, 3-hydroxypyridine, 2-hydroxynicotinic acid, 4-hydroxynicotinic acid, 5-hydroxynicotinic acid, 6-hydroxynicotinic acid, 2-hydroxyisonicotinic acid, 3-hydroxyisonicotinic acid, 3-hydroxypicolinic acid, 4-hydroxypicolinic acid, 5-hydroxypicolinic acid, 6-hydroxypicolinic acid, salicylic acid, 3-hydroxybenzoic acid, 4-hydroxybenzoic acid, citrazinic acid, 2,3-dihydroxyisonicotinic acid, 2,5-dihydroxyisonicotinic acid, and 3,5-dihydroxyisonicotinic acid are preferred. Among these, 3-hydroxypyridine, 2-hydroxynicotinic acid, 2-hydroxyisonicotinic acid, citrazinic acid, and salicylic acid are more preferable, 3-hydroxypyridine, 2-hydroxyisonicotinic acid, citrazinic acid, and salicylic acid are even more preferable, 3-hydroxypyridine, 2-hydroxyisonicotinic acid, and citrazinic acid are even more preferable, and citrazinic acid is particularly preferable. For 2-hydroxynicotinic acid, 4-hydroxynicotinic acid, 5-hydroxynicotinic acid, 6-hydroxynicotinic acid, 2-hydroxyisonicotinic acid, 3-hydroxyisonicotinic acid, 3-hydroxypicolinic acid, 4-hydroxypicolinic acid, 5-hydroxypicolinic acid, 6-hydroxypicolinic acid, salicylic acid, 3-hydroxybenzoic acid, 4-hydroxybenzoic acid, citrazinic acid, 2,3-dihydroxyisonicotinic acid, 2,5-dihydroxyisonicotinic acid, and 3,5-dihydroxyisonicotinic acid, salt compounds in which the OH group is the salt group and salt compounds in which the COOH group is the salt group are also preferred.

[0036] The amount (concentration) of the polishing accelerator is not particularly limited, but is preferably 0.01 mmol / L or more, more preferably 0.1 mmol / L or more, and even more preferably 1 mmol / L or more, based on the total volume of the polishing composition. In this range, the polishing speed of the polishing object containing titanium nitride is further improved. In addition, the amount (concentration) of the polishing accelerator is not particularly limited, but is preferably 100 mmol / L or less, more preferably 50 mmol / L or less, and even more preferably 30 mmol / L or less, based on the total volume of the polishing composition. In this range, the polishing accelerator acts more effectively. It is presumed that the reason for this is that the dispersibility of the abrasive grains is further improved without excessive increase in electrical conductivity.

[0037] (Abrasive grain) The polishing composition according to one embodiment of the present invention contains silica particles as abrasive grains. The abrasive grains act to improve the polishing rate by mechanically polishing the object to be polished.

[0038] The silica particles are not particularly limited, but from the viewpoint of dispersion stability and defect performance, fumed silica or colloidal silica is preferred, and colloidal silica is more preferred. The colloidal silica can be produced by a sodium silicate method or a sol-gel method, and colloidal silica produced by any method can be suitably used. However, from the viewpoint of reducing metal impurities, colloidal silica produced by the sol-gel method is preferred. Colloidal silica produced by the sol-gel method is preferred because it contains less metal impurities and corrosive ions such as chloride ions that have the property of diffusing in semiconductors. The production of colloidal silica by the sol-gel method can be carried out using a conventionally known method, and specifically, colloidal silica can be obtained by hydrolysis and condensation reaction using a hydrolyzable silicon compound (e.g., alkoxysilane or its derivative) as a raw material.

[0039] The silica particles may be surface-modified or unmodified. An example of a preferred silica particle is a colloidal silica having an unmodified surface.

[0040] The shape of silica particles is not particularly limited, and may be spherical or non-spherical.Specific examples of non-spherical shapes include polygonal prisms such as triangular prisms and square prisms, cylinders, bales of cylinders whose central parts are more bulging than their ends, donuts whose central parts are penetrating disks, plates, so-called cocoon shapes with a constriction in the central part, so-called association-type spheres in which a plurality of particles are integrated, so-called confetti-shaped shapes with a plurality of protrusions on the surface, and rugby ball shapes, and various other shapes are not particularly limited.

[0041] The average primary particle diameter of the silica particles is not particularly limited, but is preferably 5 nm or more, more preferably 7 nm or more, even more preferably 10 nm or more, and particularly preferably 25 nm or more. In this range, the polishing speed of the polishing object containing titanium nitride is improved. In addition, the average primary particle diameter of the silica particles is not particularly limited, but is preferably 120 nm or less, more preferably 80 nm or less, and even more preferably 50 nm or less. In this range, the frequency of defects on the polishing surface of the polishing object containing titanium nitride can be further reduced. In addition, the polishing efficiency of the polishing object containing titanium nitride is improved. The value of the average primary particle diameter of the silica particles can be calculated based on the specific surface area of ​​the silica particles measured by the BET method (BET specific surface area) assuming that the shape of the silica particles is a true sphere. More specifically, the average primary particle diameter of the silica particles can be calculated from the specific surface area of ​​the silica particles measured by the BET method using "Flow Sorb II 2300" manufactured by Micromeritics and the density of the silica particles.

[0042] The average secondary particle diameter of the silica particles is not particularly limited, but is preferably 10 nm or more, more preferably 20 nm or more, even more preferably 30 nm or more, and particularly preferably 50 nm or more. In this range, the polishing speed of the polishing object containing titanium nitride is improved. In addition, the average secondary particle diameter of the silica particles is not particularly limited, but is preferably 250 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, and particularly preferably 100 nm or less. In this range, the frequency of defects on the polishing surface of the polishing object containing titanium nitride can be further reduced. In addition, the polishing efficiency of the polishing object containing titanium nitride is improved. The value of the average secondary particle diameter of the silica particles can be calculated by a dynamic light scattering method represented by a laser diffraction scattering method, for example, using a dynamic light scattering particle size / particle size distribution device UPA-UTI151 manufactured by Nikkiso Co., Ltd.

[0043] The size of the silica particles (average primary particle size, average secondary particle size) can be appropriately controlled by selecting a method for producing the silica particles, for example.

[0044] The silica particles may be used alone or in combination of two or more kinds.

[0045] The amount (concentration) of silica particles added is not particularly limited, but is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.1% by mass or more, based on the total mass of the polishing composition. In this range, the contact frequency between the silica particles and the object to be polished increases, and the polishing speed of the object to be polished is further improved. In addition, the amount (concentration) of silica particles added is not particularly limited, but is preferably 30% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the polishing composition. In this range, it leads to cost reduction, and the aggregation of silica particles is suppressed, and the polishing speed of the object to be polished is further improved.

[0046] The polishing composition according to one embodiment of the present invention may contain other abrasive grains in addition to silica grains. The other abrasive grains may be any of inorganic grains other than silica grains, organic grains, and organic-inorganic composite grains. Examples of inorganic grains other than silica grains include grains made of metal oxides such as alumina grains, ceria grains, and titania grains, silicon nitride grains, silicon carbide grains, and boron nitride grains. Examples of organic grains include polymethylmethacrylate (PMMA) grains.

[0047] However, in the polishing composition according to one embodiment of the present invention, the amount (concentration) of other abrasive grains added is preferably as small as possible, and it is particularly preferable that the polishing composition does not substantially contain other abrasive grains. In this specification, the term "does not substantially contain other abrasive grains" refers to the amount (concentration) of other abrasive grains added being less than 0.001% by mass relative to the total mass of the polishing composition.

[0048] (Oxidizing agent) The polishing composition according to one embodiment of the present invention preferably further contains an oxidizing agent, which acts to improve polishing characteristics by oxidizing the surface of the object to be polished, such as increasing the polishing speed of the object to be polished or improving the surface quality of the object to be polished after polishing.

[0049] The oxidizing agent is not particularly limited, but examples thereof include hydrogen peroxide, sodium peroxide, barium peroxide, ozone water, silver (II) salt, iron (III) salt, permanganic acid, chromic acid, dichromate, peroxodisulfuric acid, peroxolinic acid, peroxosulfuric acid, peroxoboric acid, performic acid, peracetic acid, perbenzoic acid, perphthalic acid, hypochlorous acid, hypobromous acid, hypoiodous acid, chloric acid, chlorous acid, perchloric acid, bromic acid, iodic acid, periodic acid, persulfuric acid, dichloroisocyanuric acid, and salts thereof. Among these, hydrogen peroxide is preferred from the viewpoint of handling and safety. The oxidizing agent can be used alone or in combination of two or more.

[0050] The amount (concentration) of the oxidizing agent to be added is not particularly limited, but is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.1% by mass or more, based on the total mass of the polishing composition. In this range, the oxidation reaction of titanium nitride proceeds more sufficiently, and the polishing speed of the polishing object containing titanium nitride is improved. In addition, the amount (concentration) of the oxidizing agent to be added is not particularly limited, but is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, based on the total mass of the polishing composition. In this range, the effect of the decrease in the abrasive grain concentration due to the addition of the oxidizing agent is smaller, and the polishing speed of the polishing object containing titanium nitride can be maintained better.

[0051] (pH adjuster) The polishing composition according to one embodiment of the present invention preferably further contains a pH adjuster, which adjusts the pH of the polishing composition to an appropriate range, thereby improving the chemical polishing effect on the surface to be polished, thereby increasing the polishing rate, or improving the dispersion stability of the polishing composition.

[0052] The pH adjuster is not particularly limited as long as it is a compound having a pH adjusting function, and for example, an acid or a basic compound can be used. Here, the basic compound refers to a compound having a function of increasing the pH of the polishing composition by being added to the polishing composition.

[0053] The acid may be either an inorganic acid or an organic acid. The inorganic acid is not particularly limited, but examples thereof include sulfuric acid, nitric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. The organic acid is not particularly limited, but examples thereof include carboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylpentanoic acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, and lactic acid.

[0054] The basic compound is not particularly limited, but examples thereof include hydroxides of alkali metals or Group 2 elements, ammonia, etc. Specific examples of hydroxides of alkali metals include potassium hydroxide (KOH), sodium hydroxide (NaOH), etc. Specific examples of hydroxides of Group 2 elements include calcium hydroxide (Ca(OH)2).

[0055] Among these, from the viewpoint of adjusting the pH value to the optimum range described later, basic compounds are preferred. In addition, hydroxides of alkali metals or Group 2 elements and ammonia are more preferred, hydroxides of alkali metals or Group 2 elements are even more preferred, and hydroxides of alkali metals are even more preferred. In addition, potassium hydroxide and sodium hydroxide are particularly preferred, and potassium hydroxide is the most preferred.

[0056] The pH adjusters may be used alone or in combination of two or more kinds.

[0057] The amount (concentration) of the pH adjuster to be added may be appropriately selected so as to give the desired pH value of the polishing composition, and it is preferable to add an amount so as to give a preferred pH value of the polishing composition described below.

[0058] (pH) The pH of the polishing composition according to one embodiment of the present invention is not particularly limited. However, the lower limit of the pH is preferably 1 or more. In this range, the possibility of deteriorating consumables such as the polishing apparatus and the polishing pad in contact with it is further reduced. Furthermore, the lower limit of the pH is more preferably more than 7, more preferably 8 or more, even more preferably 9 or more, and particularly preferably 9.5 or more. In this range, the polishing rate of the polishing object containing titanium nitride is further improved. The reason for this is presumed to be that under alkaline conditions in the above range, the carboxyl group or hydroxyl group in the polishing accelerator is more easily ionized than under acidic conditions, and the coordination of the polishing accelerator to titanium nitride is also easier. In addition, the upper limit of the pH is preferably 12 or less, more preferably 11 or less. In this range, corrosion is less likely to occur, and the composition can be applied to polishing objects containing a wider variety of materials other than titanium nitride. In addition, safety is further improved, handling is easier, and the stability of the polishing composition is further improved. The pH value of the polishing composition can be evaluated using a pH meter (manufactured by Horiba, Ltd., product name: LAQUA (registered trademark)).

[0059] (Electrical conductivity adjuster) The polishing composition according to one embodiment of the present invention preferably further contains an electrical conductivity adjuster. The electrical conductivity adjuster adjusts the electrical conductivity of the polishing composition to an appropriate range, thereby synergistically enhancing the effect of the polishing accelerator or improving the dispersion stability of the polishing composition. The reason for this is unclear, but it is speculated that the addition of the electrical conductivity adjuster increases the electrical conductivity, thereby increasing the oxidation rate or degree of the titanium element by the oxidizing agent, making it easier to form an embrittled film (oxide film).

[0060] The electrical conductivity adjuster is not particularly limited as long as it is a compound having an electrical conductivity adjusting function, and for example, a salt compound can be used.

[0061] Examples of the salt compound include salts of acids and salts of basic compounds. Among these, salts of acids are preferred. The salts of acids may be organic acid salts or inorganic acid salts, but more preferred are inorganic acid salts. The inorganic acid salts are not particularly limited, but include, for example, nitrates such as potassium nitrate and ammonium nitrate, phosphates such as diammonium hydrogen phosphate and ammonium dihydrogen phosphate, and sulfates such as ammonium sulfate. Among these, sulfates are more preferred, and ammonium sulfate is particularly preferred. As mentioned above, the salt compound may be a salt of a basic compound, and examples of the salt of a basic compound are not particularly limited, but include, for example, potassium chloride, sodium chloride, potassium bromide, potassium iodide, and ammonium citrate. The salt compounds may be used alone or in combination of two or more.

[0062] The amount (concentration) of the electrical conductivity adjuster to be added may be appropriately selected so as to obtain the desired electrical conductivity of the polishing composition, and it is preferable to add an amount so as to obtain a preferred electrical conductivity value of the polishing composition described below.

[0063] (Electrical Conductivity) The electrical conductivity (EC) of the polishing composition according to one embodiment of the present invention is not particularly limited. However, the lower limit of the electrical conductivity is preferably 0.1 mS / cm or more, more preferably 0.5 mS / cm or more, and even more preferably 1 mS / cm or more. In this range, the polishing rate of the titanium nitride film is improved. This is presumably because the increase in electrical conductivity increases the oxidation rate or the degree of oxidation of the titanium element by the oxidizing agent, and the formation of an embrittled film (oxide film) is more likely to proceed. In addition, the upper limit of the electrical conductivity is preferably less than 10 mS / cm. In this range, the dispersion stability of the polishing composition is further improved. In addition, the upper limit of the electrical conductivity is more preferably less than 7 mS / cm, more preferably 6 mS / cm or less, and particularly preferably 5 mS / cm or less. In this range, the polishing rate of the titanium nitride film can be improved while maintaining good dispersion stability of the abrasive grains. The reason for this is presumably that the electrical conductivity is not excessively high, and the electrical double layer of the abrasive grains is not excessively compressed, so that the aggregation of the abrasive grains caused by the decrease in the repulsive force between the abrasive grains is suppressed. From these viewpoints, an example of a preferred range of electrical conductivity is 1 mS / cm or more and 6 mS / cm or less. The electrical conductivity of the polishing composition can be evaluated by a tabletop electrical conductivity meter (manufactured by Horiba, Ltd., model number: DS-71).

[0064] The electrical conductivity can be improved by, for example, increasing the amount of an acid, a basic compound, or a salt compound thereof. Specifically, the electrical conductivity may be controlled by the amount of each component other than the electrical conductivity regulator, or by further adding an electrical conductivity regulator.

[0065] (dispersion medium) The polishing composition according to one embodiment of the present invention preferably further contains a dispersion medium (solvent). The dispersion medium acts to disperse or dissolve each component.

[0066] The dispersion medium is not particularly limited, but preferably contains water. The content of water in the dispersion medium is not particularly limited, but is preferably 50% by mass or more, more preferably 90% by mass or more, and even more preferably water alone, with respect to the total mass of the dispersion medium. From the viewpoint of preventing contamination of the object to be cleaned and inhibition of the action of other components, the water is preferably water that contains as few impurities as possible, and is preferably water with a total content of transition metal ions of 100 ppb or less. Here, the purity of the water can be increased, for example, by removing impurity ions using an ion exchange resin, removing foreign matter with a filter, distillation, or other operations. Specifically, the water is preferably deionized water (ion-exchanged water), pure water, ultrapure water, distilled water, or the like.

[0067] In addition, the dispersion medium may be an organic solvent or a mixed solvent of water and an organic solvent, if the dispersion medium can improve the dispersibility or solubility of each component. The organic solvent is not particularly limited, and a known organic solvent can be used. When a mixed solvent of water and an organic solvent is used, it is preferable that the organic solvent is miscible with water. When an organic solvent is used, after preparing a mixed solvent by mixing water and an organic solvent, each component may be added to the mixed solvent and mixed, or each component may be dispersed or dissolved in the organic solvent and then mixed with water. The organic solvent may be used alone or in combination of two or more kinds.

[0068] (Other ingredients) The polishing composition according to one embodiment of the present invention may further contain other components within a range that does not impair the effects of the present invention. The other components are not particularly limited, and may be appropriately selected from various components used in known polishing compositions, including, for example, a wetting agent, a surfactant, a chelating agent, a preservative, an antifungal agent, a dissolved gas, a reducing agent, etc.

[0069] <Method of manufacturing the polishing composition> Another aspect of the present invention relates to a method for producing a polishing composition used for polishing an object to be polished that contains titanium nitride, the method comprising mixing silica particles with a polishing accelerator, the polishing accelerator being a compound containing an aromatic heterocycle and an OH group or a salt group thereof directly bonded to the aromatic heterocycle, or a compound containing an aromatic hydrocarbon ring, an OH group or a salt group thereof directly bonded to the aromatic hydrocarbon ring, and a COOH group or a salt group thereof directly bonded to the aromatic hydrocarbon ring.

[0070] The mixing method for mixing each component is not particularly limited, and a known method can be used as appropriate. The mixing temperature is not particularly limited, but is generally preferably 10 to 40°C, and may be heated to increase the dissolution rate. The mixing time is also not particularly limited.

[0071] In addition, the preferred aspects (type, characteristics, structure, amount added, etc.) of each component in the method for producing a polishing composition are the same as those of each component in the above-mentioned polishing composition. In addition, the preferred characteristics and other various features of the produced polishing composition are the same as those in the above-mentioned polishing composition.

[0072] <Polishing method> Another aspect of the present invention relates to a polishing method, comprising polishing an object containing titanium nitride by using the above polishing composition or by producing a polishing composition by the above production method, and using the polishing composition produced.

[0073] The object to be polished in the polishing method is the same as that described above for the polishing composition.

[0074] The polishing device and polishing conditions are not particularly limited, and known devices and conditions can be appropriately used.

[0075] The polishing device may be a general polishing device equipped with a holder for holding the object to be polished, a motor capable of changing the rotation speed, and a polishing platen to which a polishing pad (polishing cloth) can be attached. Either a single-sided polishing device or a double-sided polishing device may be used as the polishing device. As the polishing pad, general nonwoven fabric, polyurethane, porous fluororesin, etc. may be used without any particular restrictions. The polishing pad is preferably provided with grooves for collecting the polishing liquid.

[0076] The polishing conditions are not particularly limited, and appropriate conditions can be appropriately set according to the characteristics of the polishing composition and the object to be polished. The polishing load (polishing pressure, processing pressure) is not particularly limited, but generally, it is preferably 0.1 psi or more and 10 psi or less per unit area, more preferably 0.5 psi or more and 8 psi or less, and even more preferably 1 psi or more and 6 psi or less. In this range, it is possible to obtain a high polishing rate while suppressing the substrate damage caused by the load and the occurrence of defects such as scratches on the surface. The rotation speed of the platen and the carrier are not particularly limited, but generally, it is preferably 10 rpm or more and 500 rpm or less, more preferably 20 rpm or more and 300 rpm or less, and even more preferably 30 rpm or more and 200 rpm or less. The method of supplying the polishing composition is not particularly limited, and a method of continuously supplying the composition with a pump or the like (flowing) may be adopted. The supply amount of the polishing composition (flow rate of the polishing composition) may be a supply amount that covers the entire object to be polished, and is not particularly limited, but generally, it is preferably 100 mL / min or more and 5000 mL / min or less. The polishing time is not particularly limited and may be appropriately set so as to obtain the desired polishing result, but is generally preferably 5 seconds or more and 180 seconds or less. In addition, the polishing is preferably performed using in-situ dressing. Here, in-situ dressing refers to a technique of polishing and dressing the pad. In-situ dressing can further improve the uniformity of the polishing rate relative to the polishing time and further improve the controllability of polishing. As the in-situ dressing member, it is preferable to use a conditioner such as a diamond dresser.

[0077] After polishing, the polished object may be washed with water and then dried on the surface by using a spin dryer or air blower to remove water droplets adhering to the surface.

[0078] <Method of manufacturing semiconductor substrate> Another aspect of the present invention relates to a method for producing a semiconductor substrate, comprising a step (polishing step) of polishing a titanium nitride-containing polishing object by the above-mentioned polishing method. That is, this aspect is a method for producing a semiconductor substrate, comprising polishing a substrate material used for forming a titanium nitride-containing polishing object, a semiconductor substrate, by using the above-mentioned polishing composition, or by producing a polishing composition by the above-mentioned production method, and using the produced polishing composition.

[0079] In addition, in the manufacturing method, for other steps, steps that can be adopted in known manufacturing methods for semiconductor substrates can be appropriately adopted. EXAMPLES

[0080] The present invention will be described in more detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. Unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively. In the following examples, unless otherwise specified, the operations were performed under the conditions of room temperature (25°C) / relative humidity 40-50%RH.

[0081] <Preparation of Polishing Composition> (Polishing composition 1) Polishing composition 1 was prepared by adding abrasive grains (colloidal silica (unmodified); average primary particle diameter: 35 nm, average secondary particle diameter: 66.1 nm), hydrogen peroxide (H2O2) as an oxidizing agent, 2-hydroxynicotinic acid as a polishing accelerator, ammonium sulfate as an electrical conductivity adjuster, and KOH as a pH adjuster to pure water as a dispersion medium.

[0082] Here, the amount of abrasive grains added was 2 mass% relative to the total mass of the polishing composition prepared. The amount of hydrogen peroxide added as an oxidizing agent was 0.12 mass% relative to the total mass of the polishing composition prepared. Here, hydrogen peroxide was added using a 31 mass% concentration hydrogen peroxide aqueous solution, and the amount of hydrogen peroxide contained therein was added to achieve the above-mentioned amount. The amount of 2-hydroxynicotinic acid added as a polishing accelerator was 10 mmol / L relative to the total volume of the polishing composition prepared. The amount of KOH added as a pH adjuster was an amount that would result in a pH of 10.0 for the polishing composition prepared. The amount of ammonium sulfate added as an electrical conductivity adjuster was an amount that would result in an electrical conductivity of 5.0 mS / cm for the polishing composition prepared.

[0083] The pH of the polishing composition 1 prepared above was measured. The pH of the polishing composition (liquid temperature: 25° C.) was measured with a pH meter (manufactured by Horiba, Ltd., model number: LAQUA (registered trademark)).

[0084] Furthermore, the electrical conductivity of the polishing composition (polishing composition without electrical conductivity adjuster) prepared in the same manner except that no electrical conductivity adjuster was added in the preparation of the above-mentioned polishing composition was measured.The electrical conductivity (EC) of the polishing composition 1 (polishing composition after the addition of electrical conductivity adjuster) prepared above was also measured.The electrical conductivity of the polishing composition (liquid temperature: 25°C) before and after the addition of the electrical conductivity adjuster was measured using a tabletop electrical conductivity meter (manufactured by Horiba Ltd., model number: DS-71).

[0085] (Polishing composition 2-7) Each polishing composition was prepared in the same manner as for Polishing Composition 1, except that the type and amount (concentration) of each component was changed as shown in Table 1 below.

[0086] <Polishing method> (Polishing equipment and polishing conditions) The surface of the object to be polished was polished using each of the polishing compositions prepared above under the following equipment and conditions. The object to be polished was a TiN blanket wafer, which was a TiN film (titanium nitride film) having a thickness of 2500 Å formed on the surface of a substrate: [Polishing Equipment and Polishing Conditions] Polishing device: EJ-380IN-CH (Engis Japan Co., Ltd.) Polishing pad: IC1010 (manufactured by Nitta Haas Corporation) Grinding pressure (processing pressure): 2.25 psi Polishing platen rotation speed: 60 rpm Supply rate of polishing composition: 100 mL / min Polishing time: 30sec Conditioner (In-situ dressing component): Diamond dresser (SDT-100, manufactured by Noritake Co., Ltd.).

[0087] <Evaluation> (Measurement of polishing speed) The above-mentioned object to be polished was polished using each polishing composition, and the polishing speed (Å / min) of the TiN film was measured. The polishing speed of the TiN film was calculated by dividing the difference in thickness (Å) of a TiN blanket wafer (30 mm×30 mm) before and after polishing, measured using a sheet resistance measuring device based on the principle of the DC four-point probe method, by the polishing time (min). The evaluation results are shown in Table 1 below.

[0088] [Table 1]

[0089] From the results in Table 1 above, it was confirmed that the polishing compositions 1 to 5 according to the examples, which contain the polishing accelerator of the present invention, have a significantly high removal rate for the TiN film.

[0090] On the other hand, it was confirmed that polishing composition 6 of the comparative example, which does not contain a polishing accelerator, and polishing composition 7 of the comparative example, which contains a comparative compound having a structure different from the polishing accelerator of the present invention, have an inferior polishing rate for the TiN film compared to polishing compositions 1 to 5 of the examples.

Claims

1. Contains silica particles and an abrasion accelerator; The polishing accelerator is a compound containing an aromatic heterocycle and an OH group or a salt group thereof directly bonded to the aromatic heterocycle, A polishing composition used for polishing an object containing titanium nitride.

2. The polishing composition according to claim 1, wherein the polishing accelerator is a compound represented by the following general formula (1): 【Chemistry 1】 In the above general formula (1), each Z is independently CR 1 or N, In this case, 1 to 3 Z's are N; Each R 1 are each independently selected from the group consisting of a hydrogen atom, an OH group or a salt thereof, and a COOH group or a salt thereof; In this case, at least one R 1 is an OH group or a salt thereof.

3. The polishing accelerator is a compound represented by the general formula (1), in which one Z is N and five Z are CR. 1 In this case, the five R 1 One or two of the R 1 is an OH group or a salt thereof, and five of the R 1 One of the R 1 is a COOH group or a salt thereof, or a hydrogen atom, and five of the R 1 The remaining R 1 The polishing composition according to claim 2 , wherein is a compound in which is a hydrogen atom.

4. The polishing composition according to claim 3, wherein the polishing accelerator is at least one selected from the group consisting of 2-hydroxypyridine, 3-hydroxypyridine, 2-hydroxynicotinic acid, 4-hydroxynicotinic acid, 5-hydroxynicotinic acid, 6-hydroxynicotinic acid, 2-hydroxyisonicotinic acid, 3-hydroxyisonicotinic acid, 3-hydroxypicolinic acid, 4-hydroxypicolinic acid, 5-hydroxypicolinic acid, 6-hydroxypicolinic acid, citrazinic acid, 2,3-dihydroxyisonicotinic acid, 2,5-dihydroxyisonicotinic acid, 3,5-dihydroxyisonicotinic acid, and salts thereof.

5. The polishing composition according to any one of claims 1 to 4, having a pH of more than 7.

6. 6. The polishing composition according to claim 1, having an electrical conductivity of 1 mS / cm or more and 6 mS / cm or less.

7. The polishing composition according to any one of claims 1 to 6, further comprising an inorganic acid salt.

8. The polishing composition according to any one of claims 1 to 7, further comprising an oxidizing agent.

9. Mixing silica particles with an abrasion accelerator; The polishing accelerator is a compound containing an aromatic heterocycle and an OH group or a salt group thereof directly bonded to the aromatic heterocycle; A method for producing a polishing composition used for polishing an object to be polished that contains titanium nitride.

10. A polishing method comprising: using the polishing composition according to any one of claims 1 to 8; or producing a polishing composition by the production method of claim 9; and polishing an object to be polished containing titanium nitride with the polishing composition produced.

11. A method for producing a semiconductor substrate, comprising: polishing a substrate material by the polishing method according to claim 10, the substrate material being an object to be polished that contains titanium nitride.

Citation Information

Patent Citations

  • Slurry for chemical and physical grinding containing fluoride additive and its use

    JP1998067986A

  • Composite and method for polishing titanium-containing composites

    JP2001500188A

  • Polishing composition

    JP2005244123A

  • Polishing solution for metal

    JP2009295747A

  • Chemical mechanical polishing liquid and polishing method

    JP2011176208A