Silicon nitride film etching solution and method for manufacturing semiconductor device using same

The silicon nitride film etching solution with specific compounds addresses the issue of particle generation and selectivity by enhancing solubility and etching selectivity, ensuring efficient and defect-free etching of silicon nitride films.

JP7575901B2Active Publication Date: 2024-10-30OCI CO LTD(KR)
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020156587
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-29
Filing Date
2020-09-17
Publication Date
2024-10-30
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

Current silicon nitride film etching methods, particularly wet etching with phosphoric acid, lead to defects and reduced selectivity due to the etching of both silicon nitride and silicon oxide films, and generate silicon-based particles.

Method used

A silicon nitride film etching solution containing specific compounds represented by Chemical Formulas 1 or 2, which enhance solubility and prevent particle formation, while increasing selectivity to silicon oxide film under various temperature conditions.

Benefits of technology

The solution effectively prevents silicon-based particle growth and enhances etching selectivity, ensuring efficient and defect-free etching of silicon nitride films without significant silicon oxide film etching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575901000018
    Figure 0007575901000018
  • Figure 0007575901000001
    Figure 0007575901000001
  • Figure 0007575901000002
    Figure 0007575901000002
Patent Text Reader

Abstract

To provide a silicon nitride film etching solution which is hardly decomposed at low temperature but easily decomposed under an etching condition at high temperature, and which prevents growth as silicon-based particles and can increase a selection ratio of a silicon nitride film to a silicone oxide film.SOLUTION: The silicon nitride film etching solution comprises a phosphoric acid aqueous solution and at least one of compounds represented by the formula in the figure. In the formula, each X1 is independently selected from nitrogen, oxygen and sulfur; each Y1 is independently selected from hydrogen, halogen, alkoxy group, amine and a hydroxy group; and each a is independently from 1 to 4.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a silicon nitride film etching solution and a method for manufacturing a semiconductor device using the same, and more particularly to a silicon nitride film etching solution that prevents generation of particles and increases a selectivity of a silicon nitride film to a silicon oxide film, and a method for manufacturing a semiconductor device using the same. [Background technology]

[0002] Currently, there are various methods for etching silicon nitride films, and the most commonly used methods are dry etching and wet etching.

[0003] Dry etching is generally an etching method using a gas, and has the advantage of being more isotropic than wet etching, however, dry etching has limitations on the etching pattern, is less productive than wet etching, and is expensive, so wet etching is becoming more widely used.

[0004] Generally, a method using phosphoric acid as an etching solution is well known as a wet etching method. In this case, if only pure phosphoric acid is used to etch a silicon nitride film, as devices become finer, not only the silicon nitride film but also the silicon oxide film may be etched, which may cause various defects and abnormal patterns, so it is necessary to form a protective film on the silicon oxide film to further reduce the etching rate of the silicon oxide film. Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a silicon nitride film etching solution which prevents generation of particles and increases the selectivity of a silicon nitride film to a silicon oxide film under etching conditions.

[0006] Another object of the present invention is to provide a method for manufacturing a semiconductor device using the above-mentioned silicon nitride film etching solution. [Means for solving the problem]

[0007] In order to solve the above-mentioned technical problems, according to one aspect of the present invention, a silicon nitride film etching solution contains an aqueous phosphoric acid solution and at least one of compounds represented by the following Chemical Formula 1 or Chemical Formula 2.

[0008] [ka]

[0009] [ka]

[0010] In the above-mentioned Chemical Formula 1 and Chemical Formula 2, X 1 and X 2 are each independently selected from nitrogen, oxygen, and sulfur; Y 1 and Y 2 are each independently selected from hydrogen, a halogen, an alkoxy group, an amine, and a hydroxy group; a and b each independently represent 1 to 4.

[0011] According to another aspect of the present invention, there is provided a method for manufacturing a semiconductor device using the silicon nitride film etching solution described above. Effect of the Invention

[0012] The silicon nitride film etching solution according to the present invention contains at least one of the compounds represented by Chemical Formula 1 or Chemical Formula 2, and thus the reactivity with water or acid at low temperatures is reduced, thereby making it possible to prevent the growth of silicon-based particles.

[0013] In addition, since the silicon nitride film etching solution according to the present invention contains at least one of the compounds represented by Chemical Formula 1 or Chemical Formula 2, it is easily decomposed under high temperature etching conditions, and can increase the etching selectivity of a silicon nitride film to a silicon oxide film. [Brief description of the drawings]

[0014] [Figure 1] 1A to 1C are cross-sectional views each showing a silicon nitride film removal process using an etching solution according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The advantages and features of the present invention, as well as the methods for achieving them, will become clear with reference to the following examples. However, the present invention is not limited to the following examples, and may be embodied in various different forms. However, the examples are provided to fully disclose the present invention and to fully inform those skilled in the art of the present invention of the scope of the invention, and the present invention is only defined by the scope of the claims.

[0016] The silicon nitride film etching solution according to the present invention will be described in detail below.

[0017] According to one aspect of the present invention, there is provided a silicon nitride film etching solution comprising an aqueous phosphoric acid solution and at least one of compounds represented by the following Chemical Formula 1 or 2.

[0018] [ka]

[0019] [ka]

[0020] In the above-mentioned Chemical Formula 1 and Chemical Formula 2, X 1 and X2 are each independently selected from nitrogen, oxygen, and sulfur; Y 1 and Y 2 are each independently selected from hydrogen, a halogen, an alkoxy group, an amine, and a hydroxy group; a and b each independently represent 1 to 4.

[0021] By alkoxy in this application is meant both an -O-(alkyl) group and an -O-(unsubstituted cycloalkyl) group having one or more ether groups and 1 to 10 carbon atoms, specifically including, but not limited to, methoxy, ethoxy, propoxy, isopropoxy, n-butoxy, tert-butoxy, sec-butoxy, n-pentoxy, n-hexoxy, 1,2-dimethylbutoxy, cyclopropyloxy, cyclobutyloxy, cyclopentyloxy, cyclohexyloxy, and the like.

[0022] By halogen in this application is meant fluoro (-F), chloro (-Cl), bromo (-Br) or iodo (-I).

[0023] Generally, a silicon nitride film etching solution may contain a silicon additive to protect the silicon substrate from the phosphoric acid aqueous solution. However, the silane compound that is mainly used as the silicon additive basically has low solubility in the etching solution containing phosphoric acid. In order to increase the solubility of the silane compound in the etching solution, a silane compound in which a hydrophilic functional group is bonded to a silicon atom is used.

[0024] In this way, when a silane compound in which a hydrophilic functional group is bonded to a silicon atom is used as a silicon additive, the silane compound can have a proper solubility in an etching solution, but it can easily decompose at low temperatures and grow into silicon-based particles. When the silicon-based particles grow, they become the biggest cause of defects in silicon substrates.

[0025] More specifically, a silane compound having a hydrophilic functional group bonded to a silicon atom may undergo a reaction according to the following reaction formula 1.

[0026] [Reaction Scheme 1] TIFF0007575901000005.tif72134

[0027] As shown in Reaction Scheme 1, silane compounds in which hydrophilic functional groups are bonded to silicon atoms can be easily decomposed at low temperatures through an intramolecular rearrangement reaction to form silicon-hydroxy groups (-Si-OH). The silicon-hydroxy groups can generate siloxane (-Si-O-Si-) groups in which silicon atoms and oxygen atoms are alternately bonded to form random chain structures through polymerization. As a result, the silane compounds grow and precipitate as silicon-based particles, which can cause problems with reduced storage safety.

[0028] In addition, in order to ensure the appropriate solubility of the silane compound and to prevent it from being easily decomposed at low temperatures, a silane compound having an alkyl group or a heteroalkyl group bonded to a silicon atom can be used. For example, the silane compound may have a methane, ethane, propane, octane, isopropyl, or t-butyl group bonded to a silicon atom.

[0029] However, the compound remains undecomposed even under high-temperature etching conditions and forms a passivation layer on the silicon oxide film. As a result, the effect of increasing the etching selectivity of the silicon nitride film to the silicon oxide film is weak.

[0030] For example, a silane compound in which an octane group is bonded to a silicon atom can be etched with silicic acid under high-temperature etching conditions. Therefore, it is difficult for the silicon oxide film and silicic acid to combine to form a protective film, and the effect of protecting the silicon oxide film from the phosphoric acid solution and increasing the selectivity of the silicon oxide film to the silicon nitride film is weak.

[0031] The silicon nitride film etching solution according to an embodiment of the present invention has a proper solubility and is not easily decomposed, and is easily decomposed under etching conditions to prevent the growth of silicon-based particles, and contains at least one compound represented by the following Chemical Formula 1 or Chemical Formula 2 in order to increase the selectivity of a silicon nitride film to a silicon oxide film.

[0032] [ka]

[0033] [ka]

[0034] In the above-mentioned Chemical Formula 1 and Chemical Formula 2, X 1 and X 2 are each independently selected from nitrogen, oxygen, and sulfur; Y 1 and Y 2 are each independently selected from hydrogen, a halogen, an alkoxy group, and a hydroxy group; a and b each independently represent 1 to 3.

[0035] In the above Chemical formula 1 and Chemical formula 2, the substituent containing nitrogen, oxygen or sulfur bonded to the silicon atom exhibits polarity. The compounds represented by Chemical formula 1 and Chemical formula 2 contain a silicon atom bonded to the above-mentioned substituent, which is polar, and therefore can ensure the appropriate solubility of the silane compound in the etching solution.

[0036] In addition, the compounds represented by Chemical Formula 1 and Chemical Formula 2 above can suppress the formation of silicon-hydroxyl groups (-Si-OH) bonds, and can suppress the growth of silicon-based particles formed by repeated polymerization of siloxane groups formed by polymerization of silicon-hydroxyl groups.

[0037] In particular, the compounds represented by Chemical Formula 1 and Chemical Formula 2 are easily decomposed under the etching conditions. The etching conditions may be 100° C. or higher. The compounds are decomposed into silicic acid under the etching conditions and bonded with the silicon oxide film to form a protective film, thereby protecting the silicon oxide film from the phosphoric acid solution, increasing the etching rate of the silicon nitride film, and decreasing the etching rate of the silicon oxide film.

[0038] The compound represented by Chemical formula 1 can be decomposed into silicic acid by a rearrangement reaction under etching conditions, and the silicic acid can combine with the silicon oxide film to form a protective film. As a result, by protecting the silicon oxide film from the phosphoric acid solution, the etching selectivity of the silicon oxide film to the silicon nitride film can be increased.

[0039] As an example, the compound represented by Chemical formula 1 may be a compound represented by Chemical formula 3 below.

[0040] [ka]

[0041] In the above formula 3, Y 1 and a are as defined in Chemical Formula 1 above.

[0042] As an example, the compound represented by Chemical formula 2 may be a compound represented by Chemical formula 4 below.

[0043] [ka]

[0044] In the above formula 4, Y 2 and b are as defined in Chemical Formula 2 above.

[0045] The compound represented by Chemical formula 1 is preferably present in the silicon nitride film etching solution at 100 to 500,000 ppm. The compound represented by Chemical formula 1 is more preferably present in the silicon nitride film etching solution at 1,000 to 150,000 ppm. Here, the content of the additive is the amount of the compound represented by Chemical formula 1 dissolved in the silicon nitride film etching solution, and is expressed in ppm.

[0046] For example, the presence of 5,000 ppm of the compound represented by Chemical formula 1 in a silicon nitride film etching solution means that the compound represented by Chemical formula 1 dissolved in the silicon nitride film etching solution is 5,000 ppm.

[0047] When the compound represented by Chemical Formula 1 is present in the silicon nitride film etching solution at less than 100 ppm, the amount of the silicon compound may be insufficient under the etching conditions, and the effect of increasing the etching selectivity of the silicon nitride film to the silicon oxide film may be weak.

[0048] On the other hand, if the compound represented by Chemical formula 1 is present in the silicon nitride film etching solution at a concentration of more than 500,000 ppm, the proportion of water contained in the phosphoric acid aqueous solution in the silicon nitride film etching solution decreases under etching conditions, which may cause particles to be generated at high temperatures and may result in a decrease in the etching selectivity of silicon nitride film to silicon oxide film.

[0049] The silicon substrate is made of silicon nitride (Si x N y ) or silicon oxide (SiO x ) and silicon nitride film (Si x N yIn the case of a silicon substrate including both a silicon oxide film and a silicon nitride film, the silicon oxide film and the silicon nitride film may be laminated alternately or may be laminated in different regions.

[0050] Silicon oxide films are classified into SOD (Spin On Dielectric) films, HDP (High Density Plasma film, thermal oxide film, BPSG (Borophosphate) Silicate Glass) membrane, PSG (Phospho Silicate Glass) membrane, BSG (Boro Silicate Glass) membrane Glass) membrane, PSZ (Polysilazane) membrane, FSG (Fluorinated Silicate) membrane Glass film, LP-TEOS (Low Pressure Tetra Ethyl Ortho Silicate) membrane, PETEOS (Plasma Enhanced Tetra Ethyl Ortho Silicate) membrane, HTO (High Temperature Oxide) membrane, MTO (Medium Temperature Oxide) film, USG (Undopped Silicate Glass) film, SOG (Spin On Glass) film, APL (Advanced Planarization) Layer film, ALD (Atomic Layer) Deposition) film, PE-oxide film (Plasma Enhanced oxide) or O 3 -TEOS(O 3 -Tetra Ethyl Ortho Silicate) and the like may be mentioned.

[0051] In one embodiment, the phosphoric acid aqueous solution is preferably contained in an amount of 60 to 90 parts by weight per 100 parts by weight of the silicon nitride film etching solution.

[0052] If the content of the phosphoric acid aqueous solution is less than 60 parts by weight per 100 parts by weight of the silicon nitride film etching solution, the etching rate of the silicon nitride film may be reduced, so that the silicon nitride film may not be sufficiently etched or the efficiency of the silicon nitride film etching process may be reduced.

[0053] On the other hand, if the content of the phosphoric acid aqueous solution exceeds 90 parts by weight per 100 parts by weight of the silicon nitride film etching solution, the etching selectivity of the silicon oxide film to the silicon nitride film may decrease, and defects in the silicon substrate may occur due to etching of the silicon oxide film.

[0054] The silicon nitride film etching solution according to an embodiment of the present invention may further include a fluorine-containing compound to compensate for the reduced etching rate of the silicon nitride film due to the inclusion of the compound represented by Chemical Formula 1 and to improve the efficiency of the overall etching process.

[0055] In this application, a fluorine-containing compound refers to any compound, in any form, that dissociates fluorine ions.

[0056] In one embodiment, the fluorine-containing compound is at least one selected from hydrogen fluoride, ammonium fluoride, ammonium bifluoride, and ammonium bifluoride.

[0057] In another embodiment, the fluorine-containing compound may be a compound in the form of an ionic bond between an organic cation and a fluorine-based anion.

[0058] For example, the fluorine-containing compound may be a compound in the form of an ionic bond between an alkyl ammonium and a fluorine-based anion. Here, the alkyl ammonium is an ammonium having at least one alkyl group, and may have up to four alkyl groups. The definition of the alkyl group is as described above.

[0059] In yet another example, the fluorine-containing compound may be an ionic liquid in the form of an ionic bond between an organic cation selected from alkylpyrroleum, alkylimidazolium, alkylpyrazolium, alkyloxazolium, alkylthiazolium, alkylpyridinium, alkylpyrimidinium, alkylpyridazinium, alkylpyrazinium, alkylpyrrolidinium, alkylphosphonium, alkylmorpholinium, dialkylimidazolium, and alkylpiperidinium, and a fluorine-based anion selected from fluorophosphate, fluoroalkyl-fluorophosphate, fluoroborate, and fluoroalkyl-fluoroborate.

[0060] Compared with hydrogen fluoride or ammonium fluoride, which are commonly used as fluorine-containing compounds in silicon nitride film etching solutions, the fluorine-containing compounds provided in the form of ionic liquids have a high boiling point and decomposition temperature, and therefore have the advantage that there is little risk of the composition of the etching solution being changed due to decomposition during the etching process performed at high temperatures.

[0061] According to another aspect of the present invention, there is provided a method for manufacturing a semiconductor device using the silicon nitride film etching solution described above.

[0062] According to this manufacturing method, a semiconductor element can be manufactured by performing a selective etching process for a silicon nitride film on a silicon substrate including at least a silicon nitride film using the above-mentioned etching solution.

[0063] A silicon substrate used in the manufacture of a semiconductor device may include a silicon nitride film, or may include both a silicon oxide film and a silicon nitride film. In addition, in the case of a silicon substrate including both a silicon oxide film and a silicon nitride film, the silicon oxide film and the silicon nitride film may be laminated alternately or may be laminated in different regions.

[0064] The method for manufacturing a semiconductor device according to the present invention can be applied to the manufacturing process of a NAND device. More specifically, the above-mentioned etching solution can be used in a process step that requires selective removal of a silicon nitride film without damaging a silicon oxide film in a stacked structure for forming a NAND.

[0065] As an example, FIG. 1 is a schematic cross-sectional view illustrating a process for removing a silicon nitride film using an etching solution according to the present invention.

[0066] Referring to FIG. 1, a mask pattern layer 30 is formed on a laminated structure 20 in which silicon nitride films 11 and silicon oxide films 12 are alternately laminated on a silicon substrate 10, and then a trench 50 is formed by an anisotropic etching process.

[0067] Also, referring to FIG. 1, an etching solution according to the present invention is injected through the trench 50 region formed in the stacked structure 20, thereby etching the silicon nitride film 11 so that only the silicon oxide film 12 and the mask pattern layer 30 remain.

[0068] That is, the present invention uses an etching solution having an improved etching selectivity for silicon nitride film with respect to silicon oxide film, thereby minimizing etching of silicon oxide film 12 in stacked structure 20 and completely and selectively removing silicon nitride film 11 in a sufficient time. Then, a semiconductor device can be manufactured through a subsequent process including a step of forming a gate electrode in the region where silicon nitride film 11 has been removed.

[0069] Specific examples of the present invention are presented below. However, the examples described below are merely for the purpose of specifically illustrating or explaining the present invention, and the present invention should not be limited thereby.

[0070] Working Example Etching solution production In Example 1, the compound represented by Chemical formula 1 was added to an aqueous phosphoric acid solution, and in Example 2, the compound represented by Chemical formula 2 was added to an aqueous phosphoric acid solution to prepare an etching solution with an initial concentration of 500 ppm.

[0071] The etching solution compositions according to Examples 1 and 2 are as shown in Table 1.

[0072] [Table 1]

[0073] The etching solution compositions of Comparative Examples 1 to 3 are as shown in Table 2.

[0074] [Table 2]

[0075] Experimental Example Measurement of the average diameter of silicon-based particles The average diameter of silicon-based particles present in the etching solutions of Examples 1-2 and Comparative Examples 2-3 was measured over time at room temperature (25°C). The average diameter of silicon-based particles was measured using a PAS (particle size analyzer). The average diameters of the measured silicon-based particles are shown in Table 3 below.

[0076] [Table 3]

[0077] As shown in Table 3 above, it can be confirmed that the etching solutions of Examples 1 and 2 contain almost no silicon-based particles even after the passage of time.

[0078] On the other hand, as shown in Table 3 above, in the etching solutions of Comparative Examples 2 and 3, it can be confirmed that silicon-based particles having a diameter of 5 μm or more are present as time passes.

[0079] Measurement of etching rate of silicon oxide film and silicon nitride film The silicon nitride film etching solutions according to Examples 1-2 and Comparative Examples 1-3 were used to etch a silicon oxide film (thermal oxide layer) and a silicon nitride film having a thickness of 500 Å at 175° C. by immersing them in the heated etching solutions for 10 minutes.

[0080] The thicknesses of the silicon oxide and silicon nitride films before and after etching were measured by ellipsometry (Nano-View, SE The etching rate was calculated by dividing the difference in thickness of the silicon oxide film and the silicon nitride film before and after etching by the etching time (10 minutes).

[0081] The measured etch rates are shown in Table 4 below.

[0082] [Table 4]

[0083] As shown in Table 4 above, the etching solutions of Examples 1 and 2 can reduce the etching rate of a silicon oxide film compared to the etching solutions of Comparative Examples 1 to 3, and this can be confirmed to improve the etching selectivity ratio of a silicon oxide film to a silicon nitride film.

[0084] Although one embodiment of the present invention has been described above, a person having ordinary knowledge in the technical field can modify and change the present invention in various ways by adding, changing, deleting or adding components within the scope of the concept of the present invention described in the claims, and this can also be said to be within the scope of the rights of the present invention. [Explanation of symbols]

[0085] 10 Silicon substrate 11 Silicon nitride film 12 Silicon oxide film 20 Laminated structure 30 Mask Pattern Layer 50 Trench

Claims

1. an aqueous solution of phosphoric acid; and At least one of the compounds represented by the following formula 1 or 2 is included: Silicon nitride etching solution: 【Chemistry 1】 【Chemistry 2】 In the above formula 1 and formula 2, X 1 and X 2 are each independently selected from oxygen and sulfur; Y 1 and Y 2 are each independently selected from an alkoxy group and a hydroxy group; a and b each independently represent 1 to 4.

2. The compound represented by Chemical Formula 1 is characterized in that it is a compound represented by Chemical Formula 3 below, or is characterized in that it is a compound represented by Chemical Formula 3: The silicon nitride film etching solution according to claim 1: 【Chemistry 3】 In the above formula 3, Y 1 and a are as defined in Chemical Formula 1 above.

3. The compound represented by Chemical Formula 2 is a compound represented by Chemical Formula 4: The silicon nitride film etching solution according to claim 1: 【Chemistry 4】 In the above formula 4, Y 2 and b are as defined in Chemical Formula 2 above.

4. The silicon nitride film etching solution contains the compound represented by Chemical Formula 1 in an amount of 100 to 500,000 ppm. The silicon nitride film etching solution according to claim 1 .

5. The silicon nitride film etching solution further includes at least one fluorine-containing compound selected from hydrogen fluoride, ammonium fluoride, ammonium bifluoride, and ammonium bifluoride; The silicon nitride film etching solution according to claim 1 .

6. The silicon nitride film etching solution further includes a fluorine-containing compound having an ionic bond between an organic cation and a fluorine-based anion. The silicon nitride film etching solution according to claim 1 .

7. The organic cation is at least one selected from alkylimidazolium, dialkylimidazolium, alkylpyridinium, alkylpyrrolidinium, alkylphosphonium, alkylmorpholinium, and alkylpiperidinium; The silicon nitride film etching solution according to claim 6.

8. The fluorine-based anion is at least one selected from the group consisting of fluorophosphate, fluoroalkyl-fluorophosphate, fluoroborate, and fluoroalkyl-fluoroborate; The silicon nitride film etching solution according to claim 6.

9. A method for manufacturing a semiconductor device, comprising an etching step using the silicon nitride film etching solution according to claim 1.

Citation Information

Patent Citations

  • Insulation layer etchant composition and method of forming pattern using the same

    CN110157434A

  • Removal of mems sacrificial layers using supercritical fluid / chemical formulations

    JP2007513522A

  • Etching composition and method for manufacturing semiconductor device using same

    JP2018538692A

  • Compositions and methods for etching silicon nitride-containing substrates

    WO2019051053A1