Iron oxide magnetic powder and its manufacturing method

The controlled production method for iron-based oxide magnetic powders addresses coercive force variations and particle irregularities, enhancing magnetic recording properties and density by achieving narrow particle size distribution and spherical shape.

JP7575904B2Active Publication Date: 2024-10-30THE UNIV OF TOKYO +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020162743
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-28
Publication Date
2024-10-30
Estimated Expiration
2040-09-28

AI Technical Summary

Technical Problem

Existing iron-based oxide magnetic powders for magnetic recording media suffer from variations in coercive force distribution, particle shape irregularities, and high content of fine and coarse particles, which hinder recording density and stability.

Method used

The production method involves controlling particle size distribution by neutralizing a solution containing trivalent iron ions and metal elements, coating with silicon oxide, and removing excess silicon oxide to achieve particles with an average diameter of 10-20 nm, circularity of 0.955 or more, and reduced fine and coarse particle content.

Benefits of technology

The method results in magnetic powders with improved magnetic recording properties, reduced noise, and enhanced recording density by minimizing fine and coarse particles and ensuring spherical particle shape.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575904000005
    Figure 0007575904000005
  • Figure 0007575904000006
    Figure 0007575904000006
  • Figure 0007575904000007
    Figure 0007575904000007
Patent Text Reader

Abstract

To provide an iron-based oxide magnetic powder suitable for use in magnetic recording media in which the contents of fine particles and coarse particles are sufficiently reduced and the particle shape is close to a true sphere.SOLUTION: A method for producing an iron-based oxide magnetic powder, comprising: a step in which (i) a raw material solution that contains a) trivalent iron ions or b) trivalent iron ions and metal element ions partially replacing Fe-sites, (ii) and an alkaline solution for neutralizing the raw material solution, are added to a reaction system to adjust the pH of the reaction system to 1.0-3.0; a step in which a hydroxycarboxylic acid is added to the obtained reaction solution and then the pH of the reaction system is neutralized to 7.0-10.0; and a step in which the resulting precipitate of iron oxyhydroxide containing substituted metal elements is coated with a silicon oxide and then heated to form particles of ε-iron oxide in which Fe sites are partially replaced with other metal elements; and a step in which the slurry containing the particles is classified.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an iron-based oxide magnetic powder suitable for high-density magnetic recording media, radio wave absorbers, etc., and in particular to a magnetic powder having an average particle size on the order of nanometers, and a method for producing the same. [Background technology]

[0002] ε-Fe2O3 is an extremely rare phase among iron oxides, but nanometer-sized particles have a thermal conductivity of 20 kOe (1.59 × 10 6 Since ε-Fe2O3 exhibits a huge coercive force (Hc) of about 10 ...

[0003] Meanwhile, in the field of magnetic recording, magnetic recording media with a high ratio of the reproduction signal level to particulate noise (C / N ratio: Carrier to Noise Ratio) are being developed, and in order to increase the recording density, there is a demand for finer magnetic particles that make up the magnetic recording layer. However, in general, finer magnetic particles tend to deteriorate their environmental resistance and thermal stability, and there is concern that the magnetic properties of the magnetic particles may decrease under the usage or storage environment. Therefore, by replacing part of the Fe site of ε-Fe2O3 with other metals with excellent heat resistance, it is possible to obtain a magnetic recording medium with the general formula ε-A x B y Fe 2-x-y O3 or ε-A x B y C z Fe 2-x-y-zVarious partial substitution products of ε-Fe2O3 (where A is a divalent metal element such as Co, Ni, Mn, or Zn, B is a tetravalent metal element such as Ti, and C is a trivalent metal element such as In, Ga, or Al) have been developed that have reduced particle size, variable coercive force, and excellent environmental resistance and thermal stability (Patent Document 3).

[0004] Since ε-Fe2O3 is obtained as a stable phase with a size on the order of nanometers, a special method is required for its production. The above-mentioned Patent Documents 1 to 3 disclose a method for producing ε-Fe2O3 by using fine crystals of iron oxyhydroxide produced by a liquid phase method as a precursor, coating the precursor with silicon oxide by a sol-gel method, and then heat-treating the precursor. As the liquid phase method, a reverse micelle method using an organic solvent as a reaction medium and a method using only an aqueous solution as a reaction medium are disclosed. However, since the magnetic properties of ε-Fe2O3 or partially substituted ε-Fe2O3 obtained by these methods vary, it has been proposed to improve their magnetic properties by removing the silicon oxide coating after heat treatment and performing a classification process.

[0005] The ε-Fe2O3 or ε-type iron oxide partially substituted with Fe produced by the conventional production methods disclosed in the above Patent Documents 1 to 3 has excellent magnetic properties, but depending on the production conditions, there are cases where variation in coercive force distribution is observed. In response to the problem of variation in coercive force distribution, Patent Document 4 discloses a method for producing an ε-type iron oxide magnetic particle powder containing a substitution metal element, which comprises adding an alkali to an aqueous solution containing trivalent iron ions and ions of metal M partially substituting Fe sites to neutralize the pH to pH 1.0 to 3.0, adding hydroxycarboxylic acid D in an amount of 0.125 to 1.0 in terms of a molar ratio D / Fe to the amount of trivalent iron ions or a molar ratio (D / (Fe+M)) to the total amount of trivalent iron ions and ions of the substitution metal M, further adding an alkali to neutralize the pH to pH 7.0 to 10.0, and covering the resulting iron oxyhydroxide containing the substitution metal element with silicon oxide and heating it. Hydroxycarboxylic acids, which are carboxylic acids that have an OH group in their molecule, form complexes with the trivalent iron ions dissolved in the reaction solution, delaying the reaction that forms iron hydroxide when further alkali is added in the next step, and are said to have the effect of narrowing the distribution of the average particle size of the precursor microparticles containing iron oxyhydroxide that are generated as a result. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2008-174405 A [Patent Document 2] International Publication No. 2008 / 029861 [Patent Document 3] International Publication No. 2008 / 149785 [Patent Document 4] JP 2017-024981 A Summary of the Invention [Problem to be solved by the invention]

[0007] The ε-type iron-based oxide magnetic powder containing substitutional metal elements produced by the manufacturing method disclosed in Patent Document 4 had a narrow particle size distribution and a low content of fine particles that do not contribute to magnetic recording characteristics, and as a result was excellent in that it had a narrow coercive force distribution. However, there was still room for improvement in order to increase the recording density of magnetic recording media. When applying ε-type iron oxide magnetic powder to a magnetic recording medium, it is desirable not only to control the average particle size but also to reduce the proportion of fine particles and coarse particles whose particle size is far from the average value as much as possible. The presence of fine particles, even if their volume ratio in the magnetic powder is small, causes an increase in noise in the electromagnetic conversion characteristic SNR of the magnetic recording medium. In addition, coarse particles have too high a coercive force and cannot be written by a magnetic head, and if their proportion is high, it causes a decrease in magnetic recording density. The ε-type iron oxide magnetic powder containing a substituted metal element manufactured by the manufacturing method disclosed in Patent Document 4 cannot be said to have a sufficiently reduced content of the fine particles and coarse particles, and there are still problems in increasing the recording density of magnetic recording media.

[0008] Furthermore, there is also a problem that the ε-type iron-based oxide magnetic powder containing a substitution metal element produced by the production method disclosed in Patent Document 4 has an irregular particle shape. If the particle shape is irregular, the uneven parts of the particles may interfere with each other and hinder the orientation of the particles when the particles are magnetically oriented during the production of a magnetic recording medium, so it is desirable for the particle shape to be as close to a perfect sphere as possible.

[0009] In view of the above problems, the present invention provides an iron-based oxide magnetic powder consisting of ε-iron oxide particles in which part of the Fe sites is substituted with other metal elements, the content of fine particles and coarse particles being sufficiently reduced and the particle shape being nearly spherical, suitable for use in magnetic recording media, and a method for producing the iron-based oxide magnetic powder. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention provides (1) Provided is an iron-based oxide magnetic powder consisting of epsilon-iron oxide particles in which some of the Fe sites have been substituted with other metal elements, the powder having an average particle size measured by a transmission electron microscope of 10 nm or more and 20 nm or less, the percentage of particles having a particle size of 8 nm or less being 3% or less, the percentage of particles having a particle size of 20 nm or more being 25% or less, the average circularity of the particles observed by a transmission electron microscope being 0.955 or more, and the coefficient of variation of particle sizes measured by a transmission electron microscope being 19% or less. (2) The metal element substituting a portion of the Fe sites is preferably one or more of Ga, Co, and Ti. (3) The metal element substituting a portion of the Fe site may be one or more of Ga, Co, Ti, Ni, Mn, Cr, Nd, Dy and Gd.

[0011] In the present invention, (4) A method for producing an iron-based oxide magnetic powder comprising particles of ε-iron oxide or ε-iron oxide in which a part of the Fe site is substituted with another metal element, the particles having an average particle diameter of 10 nm or more and 20 nm or less as measured by a transmission electron microscope, A raw solution preparation step of preparing an aqueous solution containing trivalent iron ions or trivalent iron ions and ions of a metal element that substitutes a part of the Fe site (hereinafter referred to as a raw solution) and an alkaline aqueous solution for neutralizing the raw solution; a first neutralization step of continuously or intermittently adding and mixing the raw material solution and the aqueous alkaline solution to a reaction system to adjust the pH of the reaction system to 1.0 or more and 3.0 or less; adding a hydroxycarboxylic acid to the aqueous solution after the first neutralization step; a second neutralization step of adding an alkali to the aqueous solution containing the hydroxycarboxylic acid to neutralize the pH to 7.0 or more and 10.0 or less to obtain a slurry containing a precipitate of iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element; a step of adding a silicon compound having a hydrolyzable group to a slurry containing the iron oxyhydroxide or the iron oxyhydroxide containing a substitution metal element, and coating the iron oxyhydroxide or the iron oxyhydroxide containing a substitution metal element with a hydrolysis product of the silicon compound; heating the iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element coated with the hydrolysis product of a silicon compound to obtain epsilon iron oxide coated with silicon oxide or epsilon iron oxide in which a portion of the Fe site is substituted with another metal element; removing the silicon oxide from the silicon oxide-coated ε-iron oxide or the ε-iron oxide having a portion of the Fe sites substituted with another metal element to obtain a slurry containing the ε-iron oxide or the ε-iron oxide having a portion of the Fe sites substituted with another metal element; adding a quaternary ammonium salt having a concentration of 0.009 mol / kg to 1.0 mol / kg as a surface modifier to a slurry containing the ε-iron oxide or the ε-iron oxide in which a part of the Fe sites is substituted with another metal element, and adjusting the pH to 11.0 to 14.0; a step of subjecting the slurry containing the surface modifier to a dispersion treatment to obtain a dispersion slurry of ε-iron oxide particles or ε-iron oxide particles in which a part of the Fe sites is substituted with another metal element; a step of classifying a slurry containing the dispersed particles of the ε-iron oxide or the ε-iron oxide having a part of the Fe sites substituted with another metal element; The present invention provides a method for producing an iron-based oxide magnetic powder, comprising the steps of: (5) The first neutralization step described in the above item (4) is preferably a step in which the raw material solution and the aqueous alkaline solution containing 0.4 equivalents or more and 0.9 equivalents or less of alkali relative to the sum of the amounts of acid radicals contained in the raw material solution are added continuously or intermittently to a reaction system not containing trivalent iron ions and ions of metal elements substituting a part of the Fe sites, and mixed to adjust the pH of the reaction system to 1.0 or more and 3.0 or less. (6) The first neutralization step described in (4) above may be a step in which, when the raw material solution and the aqueous alkali solution are each continuously or intermittently added to a reaction system already containing trivalent iron ions, or trivalent iron ions and ions of a metal element substituting a portion of the Fe sites, the amount of trivalent iron ions and ions of a metal element already contained in the reaction system is 50 mol % or less of the sum of the amount of the trivalent iron ions and ions of a metal element substituting a portion of the Fe sites and the amount of the trivalent iron ions and ions of a metal element substituting a portion of the Fe sites contained in the raw material solution added to the reaction system, the raw material solution and the aqueous alkali solution containing 0.4 equivalents to 1.8 equivalents of alkali with respect to the sum of the amounts of acid radicals contained in the raw material solution are each continuously or intermittently added to the reaction system and mixed, to adjust the pH of the reaction system to 1.0 to 3.0. (7) In the first neutralization step of the above item (5), it is preferable to adjust the addition rates of the raw material solution and the aqueous alkali solution so that the cumulative amount of the aqueous alkali solution added relative to the total cumulative amount of acid radicals contained in the raw material solution is maintained in the range of 0.4 equivalents or more and 0.9 equivalents or less throughout the step. (8) In the first neutralization step of the above item (4), it is preferable to add the raw material solution and the alkaline aqueous solution over a period of 10 minutes or more. (9) The average particle size of the slurry containing iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element obtained in the second neutralization step in (4) above, as measured with a dynamic light scattering particle size distribution analyzer, is preferably 300 nm or less. (10) As a source of the trivalent iron ion contained in the raw material solution of the above item (4), it is preferable to use iron (III) chloride. (11) The cumulative amount of alkali added relative to the total cumulative amount of acid radicals added in the raw solution of (5) above is preferably 0.6 equivalents or more and 0.9 equivalents or less throughout the first neutralization step. (12) The cumulative amount of alkali added relative to the total cumulative amount of acid radicals added in the raw solution of (6) above is preferably 0.4 equivalents or more and 1.8 equivalents or less throughout the first neutralization step. Effect of the Invention

[0012] By using the manufacturing method of the present invention, it is possible to obtain an iron-based oxide magnetic powder in which the content of fine particles and coarse particles that do not contribute to improving magnetic recording characteristics is sufficiently reduced, and the particle shape is close to spherical, making it suitable for use in magnetic recording media. [Brief description of the drawings]

[0013] [Figure 1] 1 is a TEM photograph of the iron oxyhydroxide crystals containing a substitution element obtained in Example 2. [Diagram 2] 3 is a TEM photograph of the iron-based oxide magnetic powder obtained in Example 2. [Diagram 3] 3 is a TEM photograph of the iron-based oxide magnetic powder obtained in Example 3. [Figure 4] 4 is a TEM photograph of the iron-based oxide magnetic powder obtained in Example 4. [Diagram 5] 3 is a TEM photograph of the iron-based oxide magnetic powder obtained in Comparative Example 1. [Figure 6] 1 is a TEM photograph of iron oxyhydroxide crystals containing a substitution element obtained in Comparative Example 2. [Figure 7] 3 is a TEM photograph of the iron-based oxide magnetic powder obtained in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] [Iron-based oxide magnetic powder] The iron-based oxide magnetic powder obtained by the present invention is composed of ε-iron oxide particles, or ε-iron oxide particles in which part of the Fe site is substituted with other metal elements (hereinafter, may be referred to as substituted ε-iron oxide particles). The magnetic powder may contain a different phase (e.g., α-Fe2O3 in which part of the Fe site is substituted with other metal elements) that is unavoidable in the manufacturing process. It is possible to confirm that the magnetic powder is composed of ε-iron oxide particles in which part of the Fe site is substituted with other metal elements using X-ray diffraction (XRD), high-energy electron diffraction (HEED), etc.

[0015] Substituted ε-iron oxide particles that can be produced by the production method of the present invention include the following. General formula ε-C z Fe 2-z O3 (wherein C is one or more trivalent metallic elements selected from In, Ga, Al, Cr, Nd, Dy and Gd). General formula ε-A x B y Fe 2-x-y O3 (wherein A is one or more divalent metallic elements selected from Co, Ni, Mn, and Zn, and B is one or more tetravalent metallic elements selected from Ti and Sn). General formula ε-A x C z Fe 2-x-z O3 (wherein A is one or more divalent metallic elements selected from Co, Ni, Mn, and Zn, and C is one or more trivalent metallic elements selected from In, Ga, Al, Cr, Nd, Dy, and Gd). General formula ε-B y C z Fe 2-y-z O3 (wherein B is one or more tetravalent metallic elements selected from Ti and Sn, and C is one or more trivalent metallic elements selected from In, Ga, Al, Cr, Nd, Dy and Gd). General formula ε-A x B y C z Fe 2-x-y-zO3 (wherein A is one or more divalent metal elements selected from Co, Ni, Mn, and Zn, B is one or more tetravalent metal elements selected from Ti and Sn, and C is one or more trivalent metal elements selected from In, Ga, Al, Cr, Nd, Dy, and Gd). From the viewpoint of the balance between magnetic properties and thermal stability, the metal element substituting a part of the Fe site is preferably one or more of Ga, Co and Ti. In addition to Ga, Co and Ti, one or more of Ni, Mn, Cr, Nd, Dy and Gd can be used as the substituting element.

[0016] [Particle size] The ε iron oxide particles or substituted ε iron oxide particles constituting the iron-based oxide magnetic powder of the present invention preferably have an average particle diameter (hereinafter sometimes referred to as TEM average particle diameter) measured by a transmission electron microscope of 10 nm or more and 20 nm or less. If the TEM average particle diameter is 20 nm or less, the electromagnetic conversion characteristics can be improved when the iron-based oxide magnetic powder is used in a magnetic recording medium. The TEM average particle diameter is preferably 17 nm or less. If the TEM average particle diameter of the substituted ε iron oxide particles becomes small, the ratio of fine particles that do not contribute to improving the magnetic characteristics increases, and the magnetic characteristics per unit mass of the magnetic powder deteriorate, so the TEM average particle diameter is preferably 10 nm or more. In this specification, the particle diameter measured by a transmission electron microscope refers to the particle diameter of primary particles of ε iron oxide in which the Fe site is partially substituted.

[0017] The iron-based oxide magnetic powder of the present invention is characterized in that, for the ε-iron oxide particles or substituted ε-iron oxide particles, the proportion of particles having a particle diameter of 8 nm or less as measured by a transmission electron microscope (hereinafter sometimes referred to as TEM particle diameter) is 3% or less, and the proportion of particles having a TEM particle diameter of 20 nm or more is 25% or less. ε-iron oxide particles or substituted ε-iron oxide particles with a TEM particle diameter of 8 nm or less have a low coercive force and therefore do not contribute to magnetic recording even if present in a magnetic recording medium, and may instead lead to an increase in noise components in the electromagnetic conversion characteristics of the magnetic recording medium. Therefore, it is preferable that the number ratio of particles with a TEM particle diameter of 8 nm or less in the ε-iron oxide particles or substituted ε-iron oxide particles is as small as possible. Since the number ratio of particles with a TEM particle diameter of 8 nm or less in the iron-based oxide magnetic powder of the present invention is 3% or less, the amount of noise components in the electromagnetic conversion characteristics when the iron-based oxide magnetic powder is used in a magnetic recording medium can be reduced compared to when a conventional iron-based oxide magnetic powder is used. In addition, in the iron-based oxide magnetic powder consisting of ε-iron oxide particles or substituted ε-iron oxide particles having a TEM average particle size of 10 nm or more and 20 nm or less, ε-iron oxide particles or substituted ε-iron oxide particles having a TEM particle size of 20 nm or more have a larger coercive force than particles having an average particle size, so that even if they are present in a magnetic recording medium, magnetic recording cannot be written by a magnetic head, and they are particles that do not contribute to magnetic recording, so they may lead to a decrease in the magnetic recording density of the medium. Therefore, it is preferable that the number ratio of particles of 20 nm or more is small. Since the number ratio of particles having a TEM particle size of 20 nm or more in the iron-based oxide magnetic powder of the present invention is 25% or less, the magnetic recording density when the iron-based oxide magnetic powder is used in a magnetic recording medium can be improved compared to the case of using conventional iron-based oxide magnetic powder.

[0018] In the iron-based oxide magnetic powder of the present invention, the ε-iron oxide particles or substituted ε-iron oxide particles constituting the magnetic powder have a particle size variation coefficient of 19% or less. A particle size variation coefficient of 19% or less is advantageous for improving the electromagnetic conversion characteristics when the iron-based oxide magnetic powder is used in a magnetic recording medium.

[0019] [Average circularity] In the present invention, the particle shape of the ε iron oxide particles or substituted ε iron oxide particles is evaluated by the average circularity of the particles observed under a transmission electron microscope, as defined below. Circularity is a concept for evaluating how close the shape of a certain particle is to a perfect sphere, and refers to a value obtained by dividing the product of the projected area of ​​the particle and 4π by the square of the perimeter of the projected image of the particle, and takes a value of 0 to 1. In the case of a perfect circle, the circularity is 1. The method for measuring circularity will be described later, but for the substituted ε iron oxide particles, the number of particles for which the circularity is measured is increased and the average value is calculated, so that the deviation of the ε iron oxide particles or substituted ε iron oxide particles from a perfect sphere can be evaluated. The ε-iron oxide particles or substituted ε-iron oxide particles constituting the iron-based oxide magnetic powder of the present invention preferably have an average particle circularity of 0.955 or more as observed by a transmission electron microscope. If the average particle circularity is 0.955 or more, when a magnetic recording medium is manufactured by orienting the ε-iron oxide particles or substituted ε-iron oxide particles by an external magnetic field, the substituted ε-iron oxide particles are more likely to be oriented, which results in an improvement in the magnetic recording density of the magnetic recording medium. It is more preferable that the average particle circularity observed by a transmission electron microscope is 0.96 or more.

[0020] [Method of manufacturing iron-based oxide magnetic powder] In the method for producing the iron-based oxide magnetic powder of the present invention, the precursor particles, which are precursors of the ε iron oxide particles or substituted ε iron oxide particles, are characterized by having a larger particle size and better dispersibility than precursor particles obtained by conventional known production methods. The present inventors presume that in the precursor particle production process disclosed in Patent Document 4, very fine precursor particles with a particle size of 1 nm or less are produced, and the precursor particles are coated with a silicon compound in a state of agglomeration to the order of several tens of nm and then subjected to a firing process, resulting in the formation of iron-based oxide particles with an average particle size of about 10 to 30 nm. In the production method disclosed in Patent Document 4, it is difficult to arbitrarily control the degree of agglomeration of the precursor particles, and it is considered that only iron-based oxide magnetic powders with a wide particle size distribution were obtained as a result. In the production method of the present invention, precursor particles with a large particle size and good dispersibility are obtained by improving the production method of the precursor particles, and it is believed that by using such a precursor, the ratio of particles finer than the average particle size or coarse iron-based oxide particles produced can be reduced, and ε iron oxide particles or substituted ε iron oxide particles with a particle shape closer to a true sphere can be obtained. In addition, in the method for producing the iron-based oxide magnetic powder of the present invention, the content of fine particles can be further reduced by classifying the slurry containing the ε-iron oxide particles or substituted ε-iron oxide particles having a particle shape closer to a spherical shape.

[0021] [Starting materials] In the method for producing the iron-based oxide magnetic powder of the present invention, an acidic aqueous solution (raw material solution) containing trivalent iron ions or trivalent iron ions and metal ions of a metal element that will ultimately replace the Fe site of the ε-iron oxide particles is used as a starting material for the iron-based oxide magnetic particles. In the specification, acidic refers to a pH of 7 or less. As a supply source for these iron ions or metal ions of the replacement element, water-soluble inorganic acid salts such as nitrates, sulfates, and chlorides can be used in terms of ease of availability and cost. In order to ultimately obtain ε-iron oxide particles or substituted ε-iron oxide particles, it is preferable to use β-FeOOH as a precursor, and since halogen ions are necessary to obtain β-FeOOH as the crystal structure of the precursor, it is preferable to use iron(III) chloride among the iron salts exemplified. In the production method of the present invention, in the raw solution preparation step, the raw solution and an aqueous alkali solution to be used for neutralizing the raw solution in the first neutralization step described below are prepared in advance. The alkali for neutralizing the raw solution may be any of alkali metal or alkaline earth hydroxides, ammonia water, and ammonium salts such as ammonium hydrogen carbonate, but it is preferable to use ammonia water or ammonium hydrogen carbonate, which are unlikely to leave impurities when the raw solution is finally heat-treated to form ε-iron oxide particles or substituted ε-iron oxide particles.

[0022] [First neutralization step] The most important technical feature of the method for producing the iron-based oxide magnetic powder of the present invention is that in the first neutralization step, the raw material solution obtained in the previous step and an alkaline aqueous solution for neutralizing it are added to the reaction system, which will be described later. In the conventional method for producing iron-based oxide magnetic powders consisting of ε-iron oxide particles or substituted ε-iron oxide particles using an aqueous solution, an alkaline aqueous solution is normally added continuously to the entire amount of the raw material solution used in the reaction. In this case, a time lag occurs between the addition of the alkaline aqueous solution and the reaction system becoming homogeneously mixed, and metal ions and OH groups are generated in the reaction system. -It is presumed that local fluctuations in the composition ratio of ions locally caused local changes in the generation frequency and particle size of the aforementioned precursors generated by the neutralization reaction, making it difficult to control the degree of aggregation of the precursor particles. In contrast, in the first neutralization step in the production method of the present invention, the concentrations of the raw material solution and the alkaline aqueous solution to be added and the addition rates thereof to the reaction system can be changed arbitrarily, so that the metal ions and OH groups in the reaction system can be neutralized. - It becomes possible to more uniformly control the composition ratio of ions, and precursor particles having a large particle size and good dispersibility can be obtained, resulting in an iron-based oxide magnetic powder having a narrow particle size distribution.

[0023] In the first neutralization step of the production method of the present invention, the raw material solution and the alkaline aqueous solution obtained in the previous step are added to the reaction system continuously or intermittently and mixed, and the pH of the reaction system is adjusted to 1.0 to 3.0. Although the detailed crystal structure is unknown in the aqueous solution obtained by mixing the raw material solution and the alkaline aqueous solution, it is believed that extremely fine particles of oxyhydroxide of trivalent iron or a substituted metal element, hydroxide of trivalent iron or a substituted metal element, or a mixture thereof are generated to form a colloidal solution. In the production method of the present invention, the metal ions and OH in the reaction system are mixed. - Since the composition ratio of ions can be precisely controlled, it becomes possible to control the state in which the colloidal particles are generated to a desired state. In this specification, the reaction system refers to a reaction solution in which a raw material solution and an alkaline aqueous solution are mixed and a neutralization reaction occurs. In the first embodiment of the present invention, the first neutralization step is typically started by simultaneously adding the raw material solution and the alkaline aqueous solution to pure water, which is a reaction system that does not contain trivalent iron ions and ions of metal elements that substitute for a part of the Fe sites. In this case, the reaction system at the very beginning is pure water, and the reaction system after the start of the addition of the raw material solution and the alkaline aqueous solution becomes a reaction solution in which the pure water, the raw material solution, and the alkaline aqueous solution are mixed. In the first embodiment of this production method, the raw material solution and the alkaline aqueous solution may be added simultaneously directly to an empty reaction vessel for containing the reaction solution. In this case, the reaction system is a mixed solution of the raw material solution and the alkaline aqueous solution. In a second embodiment of the manufacturing method of the present invention, the initial reaction system is an acidic metal salt solution containing trivalent iron ions or trivalent iron ions and ions of a metal element that replaces a part of the Fe site, and the raw material solution and an alkali are added to this metal salt solution at the same time. Here, the type of metal salt contained in the metal salt solution may be the same as the form of the metal salt contained in the raw material solution described above. In this case, the amount of metal ions contained in the metal salt solution, which is the initial reaction system, is preferably 50 mol % or less of the total amount of metal ions contained in the metal salt solution and the amount of metal ions contained in the raw material solution added in the first neutralization step.

[0024] In the first neutralization step of the first embodiment of the production method of the present invention, an aqueous alkali solution containing 0.4 to 0.9 equivalents of alkali relative to the sum of the amounts of the raw solution and the acid radicals contained in the raw solution is added to adjust the pH of the reaction system to 1.0 to 3.0. In the case of chlorides, the acid radical is Cl. - , and NO3 in the case of nitrates. - , and SO4 in the case of sulfates. 2- Refers to... In this case, the equivalent [moles of alkali used for neutralization × alkali valence] / [(moles of acid radicals contained in raw solution × valence of acid radicals)] Here, the alkali valence is the number of OH atoms stoichiometrically generated from 1 mol of alkali. - The number of moles of an ion. For example, the alkali valences of NaOH, Ca(OH)2, and NH3 are 1, 2, and 1, respectively. The valence of an acid radical is the valence of an anion of the acid radical. For example, chloride Cl - , Nitrate NO3 - and sulfate SO4 2- The valences of the acid radicals are 1, 1, and 2, respectively. If the amount of alkali added is less than 0.4 equivalents, the amount of colloid generated by neutralization of the raw solution is reduced, and the effect of the present invention cannot be obtained, which is not preferable. If the amount of alkali added is more than 0.9 equivalents, the dispersibility of the resulting colloidal solution is deteriorated, and the effect of the present invention cannot be obtained, which is not preferable. If the pH after neutralization is less than 1.0, the amount of colloid generated by neutralization of the raw solution is reduced, and the effect of the present invention cannot be obtained, which is not preferable. If the pH after neutralization is more than 3.0, the dispersibility of the resulting colloidal solution is deteriorated, and the effect of the present invention cannot be obtained, which is also not preferable. The pH values ​​described in this specification were measured using a glass electrode based on JIS Z8802. The pH standard solution refers to a value measured using a pH meter calibrated with an appropriate buffer solution according to the pH range to be measured. The pH values ​​described in this specification are values ​​directly read from the pH meter compensated by a temperature compensation electrode under reaction temperature conditions.

[0025] The raw material solution and the alkaline aqueous solution may be added continuously or intermittently. The rate of addition of the raw material solution and the alkaline aqueous solution may be constant or may be changed during the process. The raw material solution and the alkaline aqueous solution are added at the same time, but the addition of either the raw material solution or the alkaline aqueous solution may be completed first, and there may be a time when only the other is added. In the first neutralization step of the production method of the present invention, the raw material solution and the aqueous alkali solution are added to the reaction system continuously or intermittently, so it is preferable to control the addition rate of each of them using the concept of "cumulative alkali addition equivalent", which is the cumulative addition amount equivalent number of alkali to 1 equivalent of the cumulative addition amount of acid radical contained in the raw material solution. [The cumulative amount of alkali moles used for neutralization × alkali valence] / [(The cumulative amount of acid radicals in moles contained in the raw solution × the valence of acid radicals)] It can be expressed as: Here, the term "integrated amount of alkali in moles" refers to the integrated amount of the number of moles of alkali added, and the term "integrated amount of acid radical in moles" refers to the integrated amount of moles of acid radical added. In the first neutralization step of the first embodiment of the production method of the present invention, it is preferable to adjust the addition rates of the raw material solution and the aqueous alkali solution so that the cumulative alkali addition equivalent is maintained in the range of 0.4 equivalents to 0.9 equivalents throughout the first neutralization step, and more preferably, the cumulative alkali addition equivalent is maintained in the range of 0.6 equivalents to 0.9 equivalents throughout the first neutralization step. Strictly speaking, if the timings at which the addition of the raw material solution and the aqueous alkaline solution is started are not exactly the same, the cumulative equivalent of the added alkali may not be 0.4 or more and 0.9 or less equivalents at the very beginning of the reaction. In such a case, the timings at which the addition of the raw material solution and the aqueous alkaline solution is started are deemed to be exactly the same.

[0026] By adjusting the cumulative alkali addition equivalent in the first neutralization step to 0.4 equivalents or more throughout the first neutralization step, it is possible to prevent the free trivalent iron ion concentration in the reaction system from increasing, and therefore the number of precursor core particles formed when an alkali is added to the reaction system can be reduced. As a result, the particle size of the colloid contained in the colloidal solution obtained in the first neutralization step can be made larger than that in Patent Document 4, and the particle size of the precursor particles of the ε iron oxide particles or substituted ε iron oxide particles obtained in the subsequent second neutralization step can be made larger. If the cumulative alkali addition equivalent is not maintained at 0.4 equivalents or more and there is a period when it becomes less than 0.4 equivalents, the particle size of the colloid contained in the colloidal solution obtained in the first neutralization step becomes small, and as a result, the effect of the present invention may not be obtained.

[0027] By adjusting the cumulative alkali addition equivalent in the first neutralization step to 0.9 equivalents or less throughout the first neutralization step, the pH of the reaction system can be prevented from exceeding 3.0, and the precursor particles can grow in a dispersed state in the reaction system. As a result, precursor particles with good dispersibility (i.e., little interparticle aggregation) and narrow particle size distribution can be obtained in the subsequent second neutralization step. If the cumulative alkali addition equivalent is not maintained at 0.9 equivalents or less and there is a period when it exceeds 0.9 equivalents, the dispersibility of the colloidal solution obtained in the first neutralization step will be poor (i.e., there will be a lot of interparticle aggregation), and as a result, the effects of the present invention may not be obtained.

[0028] In the first neutralization step of the second embodiment of the production method of the present invention, the raw material solution and an aqueous alkali solution containing 0.4 to 1.8 equivalents of alkali relative to the sum of the amounts of acid radicals contained in the raw material solution are added to adjust the pH of the reaction system to 1.0 to 3.0. In the first neutralization step of the second embodiment of the production method of the present invention, it is preferable to adjust the addition rates of the raw material solution and the aqueous alkali solution so that the cumulative alkali addition equivalent is maintained in the range of 0.4 to 1.8 equivalents and the pH of the reaction system is maintained in the range of 3.0 or less (preferably 0.0 or more) throughout the neutralization step, and the pH is adjusted to 1.0 to 3.0 at the end of the first neutralization step.

[0029] The total metal ion concentration in the raw solution is not particularly specified in the present invention, but it is preferable to adjust the total concentration after the addition of alkali in the second neutralization step to 0.01 mol / kg or more and 0.5 mol / kg or less. If it is less than 0.01 mol / kg, the amount of iron-based oxide magnetic powder obtained in one reaction is small, which is not economically preferable. If the total metal ion concentration exceeds 0.5 mol / kg, the reaction solution is likely to gel due to rapid hydroxide precipitation, which is not preferable. The alkali concentration of the alkaline aqueous solution, in other words, the pH of the alkaline aqueous solution, is also appropriately adjusted based on the same idea. In the first neutralization step of the production method of the present invention, the raw material solution and the alkaline aqueous solution are added to the reaction system over a period of 10 minutes or more and mixed. If the addition time is less than 10 minutes, the core particles of the precursor are generated all at once immediately after the addition, and the ions that would have been used for the core growth are consumed, resulting in a small size of the precursor, which is not preferable in terms of obtaining the effects of the present invention. Although the particle size of the colloid obtained in the first neutralization step can be controlled by extending the addition time, extending the time too much is not preferable because it reduces productivity. Therefore, the addition time is preferably 10 min to 480 min, more preferably 60 min to 300 min. In the production method of the present invention, the treatment temperature during the first neutralization treatment is not particularly limited, but is preferably 20°C or higher and 60°C or lower.

[0030] [Hydroxycarboxylic acid addition process] In the manufacturing method of the present invention, a hydroxycarboxylic acid is added to the colloidal solution obtained in the first neutralization step described above. The hydroxycarboxylic acid is a carboxylic acid having an OH group in the molecule, and acts as a complexing agent for iron ions. Here, the hydroxycarboxylic acid forms a complex with the trivalent iron ions dissolved in the reaction solution, and is considered to have the effect of delaying the reaction of forming iron hydroxide when the second neutralization treatment is performed in the next step, thereby narrowing the distribution of the average particle size of the precursor fine particles containing iron oxyhydroxide that are generated as a result. It is considered that the hydroxycarboxylic acid also forms a partial complex with the metal ion of the substitution element. The type and amount of the hydroxycarboxylic acid to be added may follow the known technology of Patent Document 4. There are many types of hydroxycarboxylic acids, including glycolic acid, lactic acid, various hydroxybutyric acids, glyceric acid, malic acid, tartaric acid, citric acid, and mevalonic acid. From the viewpoint of complexing ability, polyvalent aliphatic hydroxycarboxylic acids are preferred, and from the viewpoints of cost and availability, tartaric acid, citric acid, and malic acid are more preferred. The amount of hydroxycarboxylic acid added is preferably such that the molar ratio (D / (Fe+M)) of the amount of hydroxycarboxylic acid to the combined amount of trivalent iron ions and ions of the substituting metal element M is 0.125 or more and 1.0 or less. The hydroxycarboxylic acid may be added under mechanical stirring without changing the reaction temperature in the first neutralization step, which is the preceding step. It may be added to the reaction solution in the form of a solid, but it is preferable to add it in the form of an aqueous solution in order to ensure the uniformity of the reaction.

[0031] [Second neutralization process] In the production method of the present invention, an alkali is further added to the reaction solution after the addition of the hydroxycarboxylic acid, and the solution is neutralized until the pH is 7.0 or more and 10.0 or less. The alkali to be added can be the aqueous alkali solution used in the first neutralization step, but a solution with a different alkali concentration can also be used. In this step, the nuclei of the iron oxyhydroxide, which is the precursor of the substituted ε-iron oxide particles produced in the first neutralization step, grow to form the final precursor particles. In this step, by making the pH after neutralization 7.0 or more and 10.0 or less, when the trivalent iron and the replacing metal element are neutralized, it is possible to obtain an iron oxyhydroxide containing the replacing metal element as a solid without leaving the dissolved ions of the trivalent iron and the replacing metal element in the reaction solution. If the pH after neutralization is less than 7.0, the replacing metal element that was not completely neutralized in the first neutralization step, such as Co, remains as ions in the solution, causing a composition shift in the recovered solid, and the replacing metal element is wasted, which is not preferable from the viewpoint of production cost. In addition, if the pH after neutralization exceeds 10.0, the neutralization effect is saturated, and when an amphoteric metal such as Al is used as the replacing metal element, there are problems such as ions remaining in the solution, composition shift, and replacing metal element being wasted, as in the case of a pH of less than 7.0, which is not preferable. The iron oxyhydroxide particles or substituted metal element-containing iron oxyhydroxide particles (precursor particles) contained in the slurry obtained in this step preferably have an average diameter measured by a dynamic light scattering particle size distribution analyzer (hereinafter sometimes referred to as DLS average diameter) of 300 nm or less, more preferably 100 nm or less, and even more preferably 70 nm or less. Such a small DLS average diameter means that the precursor particles have good dispersibility and a low degree of aggregation, which is advantageous for reducing the proportion of coarse particles having a particle diameter of 20 nm or more for the ε iron oxide particles or substituted ε iron oxide particles that constitute the finally obtained iron-based oxide magnetic powder. There is no particular restriction on the lower limit of the DLS average diameter of the slurry containing the precursor particles, but the production method of the present invention can obtain particles of about 20 nm or more.

[0032] [Water washing process] In the manufacturing method of the present invention, the precursor iron oxyhydroxide produced in the above steps has a small DLS average diameter and high dispersibility. However, the ionic strength in the solution increases as the hydroxycarboxylic acid addition step and neutralization step are carried out in the previous steps. If the ionic strength remains high, it will become an aggregated system in the subsequent silicon oxide coating step, which is not preferable. Therefore, it is preferable to wash the slurry obtained in the above step with water to reduce the ionic strength in the solution and make it in a dispersed state. There is no particular restriction on the method of washing, but in consideration of the maintenance of particle dispersibility in this step, washing uniformity, connection with previous and subsequent steps, and handleability, a method of washing with water while the slurry is in a state of being in a slurry state is preferable. Considering these points, washing with water using an ultrafiltration membrane or an ion exchange membrane is preferable. In the case of washing with an ultrafiltration membrane, a membrane with a molecular weight cutoff that does not allow particles to pass through to the filtrate side is used, and it is preferable to end the washing until the electrical conductivity of the filtrate is 200 mS / m or less, more preferably 100 mS / m or less, and even more preferably 30 mS / m or less. If there are a large number of residual ions, the melting point of the silicon oxide will be locally decreased in the subsequent heating step, which will lead to a problem that sintering will occur when obtaining ε-iron oxide, resulting in the formation of coarse particles.

[0033] [Silicon oxide coating process] In the manufacturing method of the present invention, since the precursor particles generated in the above steps are unlikely to undergo a phase change to substituted ε-iron oxide particles even if they are subjected to a heat treatment in their original state, the precursor particles are coated with a silicon oxide prior to the heat treatment. As a method for coating with silicon oxide, it is preferable to apply a sol-gel method. Note that the silicon oxide here includes not only those with a stoichiometric composition, but also those with a non-stoichiometric composition such as silanol derivatives described later.

[0034] In the case of the sol-gel method, a silicon compound having a hydrolyzable group, for example, tetraethoxysilane (TEOS), tetramethoxysilane (TMOS), or a silane compound such as various silane coupling agents, is added to the aqueous solution of dispersed iron oxyhydroxide crystals or iron oxyhydroxide crystals containing a substitution element after the precursor reaction, and a hydrolysis reaction is caused under stirring, and the surface of the iron oxyhydroxide crystals is coated with the generated silanol derivative. An acid catalyst or an alkali catalyst may also be added. Considering the processing time, it is preferable to add them. A typical example of an acid catalyst is hydrochloric acid, and an alkali catalyst is ammonia. When an acid catalyst is used, it is necessary to add only an amount that does not dissolve the iron oxyhydroxide particles or the iron oxyhydroxide particles containing a substitution element. The specific method for coating with silicon oxide can be the same as that of the sol-gel method in the known process. For example, the reaction temperature for coating with silicon oxide by the sol-gel method is 20°C to 60°C, and the reaction time is about 1 hour to 20 hours. After the coating process with silicon oxide, solid-liquid separation and drying are performed to obtain a sample before the heating process. After the coating process, water washing may be performed before solid-liquid separation. In addition, a flocculant may be added during solid-liquid separation.

[0035] [Heating process] In the manufacturing method of the present invention, the precursor particles coated with silicon oxide are heat-treated to obtain ε-iron oxide particles or substituted ε-iron oxide particles. Before the heat treatment, a washing and drying step may be performed. The heat treatment is performed in an oxidizing atmosphere, which may be an air atmosphere. The heat treatment temperature varies depending on the amount of silicon oxide coating, so it is not a general rule, but the heating can be performed in the range of about 700°C to 1300°C. If the heating temperature is too low, different phases or compounds with insufficient phase transformation are likely to be mixed. If the lower limit of the heating temperature is set to 700°C or higher, the substituted ε-iron oxide particles, which are the object of the present invention, can be selectively and stably obtained, and the generation of different phases or compounds with insufficient phase transformation can be suppressed. If the heating temperature is high, α-Fe2O3 and partial substitution products of α-Fe2O3, which are thermodynamically stable phases, are likely to be generated, so the heat treatment is preferably performed at 900°C to 1200°C, more preferably 950°C to 1150°C. The heat treatment time can be adjusted within a range of about 0.5 to 10 hours, but good results are likely to be obtained within a range of 2 to 5 hours.

[0036] [Silicon oxide coating removal process] By the above steps, ε-iron oxide particles or substituted ε-iron oxide particles coated with silicon oxide can be obtained. In the production method of the present invention, the silicon oxide coating is dissolved and removed prior to the classification treatment described below. Specifically, since silicon oxide is soluble in an alkaline aqueous solution, the ε-iron oxide particles or substituted ε-iron oxide particles coated with silicon oxide after heat treatment can be dissolved and removed by immersing them in an aqueous solution containing a strong alkali such as NaOH or KOH and stirring the solution. To accelerate the dissolution rate, it is advisable to heat the aqueous alkaline solution. Typically, silicon oxide can be dissolved well by adding an alkali such as NaOH in an amount three times the molar amount of silicon oxide or more and stirring the slurry containing the powder at an aqueous solution temperature of 60°C to 70°C.

[0037] [Slurry containing iron oxide particles] In the manufacturing method of the present invention, the ε-iron oxide particles or substituted ε-iron oxide particles obtained by the silicon oxide coating removal step are dispersed in water to form a slurry. In this case, from the viewpoint of suppressing the aggregation of the iron oxide particles and reducing impurities, it is preferable to wash the slurry with pure water until the conductivity of the solvent is ≦15 mS / m. Thereafter, a quaternary ammonium salt is added to the slurry to adjust the pH of the slurry to 11.0 to 14.0. By adding a quaternary ammonium salt to the slurry to adjust the pH of the slurry to 11.0 to 14.0, excellent dispersibility of the substituted ε-iron oxide particles in the slurry is ensured. If the pH of the slurry is less than 11.0, the dispersibility of the ε-iron oxide particles or substituted ε-iron oxide particles decreases, and if the pH of the slurry is more than 14.0, the effect of improving the dispersibility is saturated and the cost of the alkaline chemicals increases, which are both undesirable. As will be described later, if a hydroxide of a tetraalkylammonium salt is used as the quaternary ammonium salt, the pH of the slurry will be in the above range even without adding another alkali.

[0038] [Quaternary ammonium ion] Quaternary ammonium ions are ammonium ions (NH4 + ) are cations in which all four hydrogen atoms have been substituted with organic groups, and the substituents are usually alkyl groups or aryl groups. In the production method of the present invention, a quaternary ammonium ion is used as a surface modifier for the ε-iron oxide particles or substituted ε-iron oxide particles, and is stable in a strong alkaline range, providing good dispersibility for the iron oxide particles. Among the quaternary ammonium ions, it is preferable to use tetraalkylammonium ions, which are easily available industrially. Tetraalkylammonium ions are quaternary ammonium cations with the molecular formula NR4 +(R is any alkyl group). Tetraalkylammonium salts are completely dissociated salts, and tetraalkylammonium ions exist as stable ions in an alkaline aqueous solution, so in the production method of the present invention, they are used as a surface modifier for improving the dispersibility of substituted ε-iron oxide particles in a slurry. Sources of tetraalkylammonium ions include hydroxides, chlorides, bromides, etc., but since the hydroxides of tetraalkylammonium ions are themselves strong alkalis, when they are added to a slurry, the pH of the slurry falls within the above-mentioned preferred pH range without the need to add other alkalis, so it is more preferable to use tetraalkylammonium hydroxide as a surface modifier. It is also possible to use chlorides or bromides of tetraalkylammonium ions as a supply source of tetraalkylammonium ions. In this case, however, when such salts are added to a slurry, an increase in pH is suppressed, and an extra alkali is required for pH adjustment, which increases the ionic strength of the system, so that the dispersibility of the substituted ε-iron oxide particles is somewhat inferior to that in the case where hydroxides are used. The tetraalkylammonium salts include quaternary ammonium salts having the same alkyl group, such as tetramethylammonium salts, tetrapropylammonium salts, and tetrabutylammonium salts, as well as quaternary ammonium salts having different alkyl groups. Any of these can be used, but it is preferable to use hydroxides such as tetramethylammonium hydroxide (tetramethylammonium hydroxide), tetrapropylammonium hydroxide (tetrapropylammonium hydroxide), and tetrabutylammonium hydroxide (tetrabutylammonium hydroxide). The concentration of tetraalkylammonium ions is set to 0.009 mol / kg or more and 1.0 mol / kg or less in order to modify the surface of the ε iron oxide particles or substituted ε iron oxide particles in the slurry and to improve dispersibility. If the concentration is either less than 0.009 mol% or more than 1.0 mol / kg, the effect of improving dispersibility is insufficient, and it is not possible to obtain a CV value of 19% or less after classification.

[0039] [Distributed processing] In the manufacturing method of the present invention, the surface modifier-containing slurry to which the surface modifier has been added is subjected to a dispersion treatment to obtain an iron oxide particle dispersion slurry. Here, the dispersion treatment is a treatment for loosening the agglomerates of the ε-iron oxide particles or substituted ε-iron oxide particles contained in the surface modifier-containing slurry. As the dispersion treatment method, known methods such as dispersion using an ultrasonic disperser, grinding using media such as a bead mill, and stirring using a stirring blade, a shaker, or a shaker can be used. The dispersion treatment of the surface modifier-containing slurry is preferably carried out until the average secondary particle size (DLS particle size) of the iron oxide particles measured by a dynamic light scattering particle size distribution analyzer becomes 65 nm or less. If the DLS particle size exceeds 65 nm, it is not preferable because it is not possible to obtain a CV value of 19% or less when the particle size is small, such as a TEM average particle size of 20 nm or less.

[0040] [Classification operation] In the manufacturing method of the present invention, a surface modifier-containing slurry to which a surface modifier has been added is subjected to a dispersion treatment, and the above-mentioned ε iron oxide particle or substituted ε iron oxide particle dispersion slurry is subjected to a classification operation. As the classification operation, a known wet classification means such as a centrifugation method can be adopted. Fine particles can be removed by removing the supernatant after centrifugation, and coarse particles can be removed by removing the precipitate after centrifugation. The gravitational acceleration during centrifugation is preferably 40,000 G or more. In addition, the classification operation is preferably repeated three or more times. After the classification operation, a magnetic powder consisting of ε iron oxide particles or substituted ε iron oxide particles is recovered using a known solid-liquid separation means, and is washed with water as necessary and then dried.

[0041] [Transmission electron microscope (TEM) observation] TEM observation of the magnetic powder made of substituted ε-iron oxide obtained by the production method of the present invention was carried out under the following conditions. JEM-1011 manufactured by JEOL Ltd. was used for TEM observation. For particle observation, TEM photographs taken at magnifications of 10,000x and 100,000x were used (those after removing the silicon oxide coating). -Measurement of average particle size, particle size distribution, and circularity- Digitizing was used to evaluate the TEM average particle size, particle size distribution, and circularity. Mac-View Ver. 4.0 was used as the image processing software. When using this image processing software, the particle size of a particle is calculated as the length of the long side of the rectangle that circumscribes the particle and has the smallest area. The circularity of a particle is calculated as the product of the particle's area and 4π divided by the square of the particle's perimeter. More than 200 particles were measured. Among the particles shown on the transmission electron microscope photograph, the selection criteria for particles to be measured were as follows: [1] Particles with any part lying outside the field of view of the photograph will not be measured. [2] Particles that are clearly defined and isolated are measured. [3] Particles that are independent and can be measured as single particles will be measured, even if they deviate from the average particle shape. [4] When particles overlap but have a clear boundary between them and the overall shape of the particle can be determined, each particle is measured as a single particle. [5] Particles that overlap, have unclear boundaries, and whose overall shape cannot be determined are not measured as their shape cannot be determined. The number average value of the particle diameters of the particles selected based on the above criteria was calculated, and this was taken as the average particle diameter of the iron oxide magnetic powder as observed by TEM. In addition, the "standard deviation of the particle diameters of the selected particles" was divided by the "number average value of the particle diameters of the selected particles (=average particle diameter)" to calculate the coefficient of variation of the particle diameters as observed by TEM. In addition, the number average value of the circularity of the selected particles was calculated, and this was taken as the average circularity of the iron oxide magnetic powder as observed by TEM.

[0042] [DLS average diameter] The DLS particle sizes of the slurries containing iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element obtained by the production method of the present invention, and the iron oxide particle dispersion slurries after dispersion treatment, were measured by dynamic light scattering particle size distribution measurement method under the following conditions. The dynamic light scattering particle size distribution analyzer used was manufactured by Otsuka Electronics Co., Ltd. (FPAR-1000K high sensitivity model), and the fiber probe used was a dilute system probe. The measurement conditions were a measurement time of 180 seconds, a repetition rate of 1, and a solvent setting of Water. The analysis mode was the cumulant method.

[0043] [Composition analysis by inductively coupled plasma emission spectrometry (ICP)] The composition of the magnetic powder made of the obtained substituted ε-iron oxide particles was analyzed. The composition analysis was performed using an Agilent Technologies ICP-720ES, with measurement wavelengths (nm) of Fe: 259.940 nm, Ga: 294.363 nm, Co: 230.786 nm, Ti: 336.122 nm, Ni: 231.604 nm, and Cr: 267.716 nm. The measurement wavelength for each metal element was selected according to the composition of the iron-based oxide magnetic powder to be analyzed, so that there was no interference from the spectra of other elements and the linearity of the calibration curve could be obtained.

[0044] [Magnetic hysteresis curve (BH curve) measurement] The magnetic properties of the obtained magnetic powder made of substituted ε iron oxide particles were measured under the following conditions. In the case of iron-based oxide magnetic powder consisting of substituted ε-iron oxide particles, a vibrating sample magnetometer (VSM) (VSM-5 manufactured by Toei Industry Co., Ltd.) was used as the magnetic property measurement device, and the applied magnetic field was 1035 kA / m (13 kOe) and the M measurement range was 0.005 A m 2 The magnetic properties were measured at a magnetic field intensity of 5 emu, a rate of change in applied magnetic field of 15 (kA / m s), a time constant of 0.03 sec, and a wait time of 0.1 sec. The coercive force Hc, saturation magnetization σs, SFD, and squareness ratio SQ were evaluated using the BH curve, and the low Hc components that do not contribute to magnetic recording were evaluated using the differential BH curve. In this case, the intercept of the vertical axis of the differential BH curve at a magnetic field of 0 was taken as I L , the peak height on the high Hc side is I HThe SFD is the value obtained by dividing the half-width of the peak on the high Hc side by the coercive force Hc. The attached software (Ver. 2.1) made by Toei Kogyo Co., Ltd. was used for this measurement and evaluation. The squareness ratio SQ is for the entire BH curve. The value at the maximum magnetic field of the differential BH curve is I Hmax Then, I Hmax / I H If is less than 0.2, the above measurement results are used. Hmax / I H If the error was greater than 0.2, the measurement was repeated using the following procedure. The measurement was performed with an applied magnetic field of 1035 kA / m (13 kOe). Hmax / I H When the value exceeds 0.2, a high-temperature superconducting VSM (VSM-5HSC manufactured by Toei Kogyo Co., Ltd.) is used, and the applied magnetic field Hmax is 2387 kA / m (30 kOe) and the M measurement range is 0.005 A m 2 The magnetic properties were measured at a magnetic field change rate of 30 kA / (m s), a time constant of 0.03 seconds, and a wait time of 0.1 seconds. Hmax / I H If is 0.2 or less, use the above measurement results and Hmax / I H If the value exceeded 0.2, the measurement was repeated again using the following procedure. Measurements were performed at applied magnetic fields of 1035 kA / m (13 kOe) and 2387 kA / m (30 kOe). Hmax / I H When the value exceeds 0.2, a high-temperature superconducting VSM (VSM-5HSC manufactured by Toei Kogyo Co., Ltd.) is used, and the applied magnetic field Hmax is 3979 kA / m (50 kOe) and the M measurement range is 0.005 A m 2 The magnetic properties were measured at a magnetic field change rate of 30 kA / (m s), a time constant of 0.03 seconds, and a wait time of 0.1 seconds. Hmax / I H was confirmed to be 0.2 or less, and this measurement result was used. EXAMPLES

[0045] [Example 1] A raw material aqueous solution was prepared by mixing 349.8g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 84.1g of Ga(III) nitrate solution with a Ga concentration of 10.9% by mass and a nitric acid concentration of 33% by mass as raw materials of substitution elements, 15.8g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 10.9g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 468.9g of pure water. The molar ratio of metal ions in this raw material aqueous solution is Fe:Ga:Co:Ti=1.705:0.175:0.070:0.050. Next, 1500g of pure water was placed in a 5L reaction tank, and the liquid temperature was adjusted to 40°C while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material aqueous solution and 6.2% ammonia aqueous solution (as alkali) were added simultaneously to this pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 3.87 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at an addition rate of 3.87 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.75 equivalents. The pH of the obtained colloidal solution was 1.68. Next, 288.8 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 186.6 g of 22.14% ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 186.6 g of the ammonia solution all at once was 8.5.

[0046] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 36.2 nm. Next, 935.7 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1100 g. The temperature was adjusted to 40°C while stirring, 1288.4 g of ethanol was added and stirred for 5 minutes, after which 283.6 g of 22.14 mass% ammonia aqueous solution was added. Furthermore, 1130.3 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the mixture was coated with the hydrolysis product of the silicon compound. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0047] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0048] Next, a 25% by mass aqueous solution of tetramethylammonium hydroxide (hereinafter referred to as TMAOH) was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 4.1%. The amount of the aqueous TMAOH solution added was set so that the TMAOH concentration in the slurry containing the surface modifier was 0.065 mol / kg. In this case, the pH of the slurry was 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 14000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 24000 G. The operation of adding 30 g of 0.065 mol / kg TMAOH aqueous solution to the slurry on the precipitate side, ultrasonic dispersion, centrifuging for 30 minutes at 14000 rpm and 24000 G, and collecting 30 g of the supernatant slurry was repeated 9 more times to collect a total of 300 g of the supernatant slurry. The collected 300 g of the supernatant slurry was mixed and 40 g was separated. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was further subjected to 9 times of addition of 30 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry, to obtain a precipitate-side slurry. The precipitate-side slurry was then added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was recovered and then dried to obtain an iron-based oxide magnetic powder according to Example 1.

[0049] The coercive force of the obtained iron oxide magnetic powder is 314 (kA / m) and the saturation magnetization is 16.6 (Am 2 / kg), squareness ratio is 0.637, SFD is 0.71, I L / I HThe value of was 0.14. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid to adhere to it, and after natural drying, carbon deposition was performed and subjected to TEM observation. As a result of measuring 200 particles by TEM observation, the TEM average particle size was 16.0 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.0%, the number ratio of particles with a particle diameter of 20 nm or more was 1.3%, the coefficient of variation (CV value) was 12%, and the average circularity of the particles was 0.974. In addition, the composition analysis was evaluated, and the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles was calculated. The above manufacturing conditions are shown in Tables 1 and 2, and the measurement results of the obtained iron oxide magnetic powder are shown in Tables 3 and 4 (the same applies to the following Examples and Comparative Examples).

[0050] [Example 2] A raw aqueous solution was prepared by mixing 350.8 g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 95.3 g of Ga(III) nitrate solution with a Ga concentration of 11.0% by mass and a nitric acid concentration of 33% by mass as raw materials of substitution elements, 10.1 g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 9.8 g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 474.5 g of pure water. The molar ratio of metal ions in this raw aqueous solution is Fe:Ga:Co:Ti=1.710:0.200:0.045:0.045. Next, 1500 g of pure water was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40° C. while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material aqueous solution and 6.5% ammonia aqueous solution (as alkali) were added simultaneously to the pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 3.92 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at an addition rate of 3.92 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.80 equivalents. The pH of the obtained colloidal solution was 1.85. Next, 288.8 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid (hydroxycarboxylic acid addition step), and then 189.8 g of 21.87% ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 189.8 g of the ammonia solution all at once was 8.62.

[0051] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The washed slurry obtained in step 3 was dropped onto a collodion film on a grid, allowed to adhere, and then naturally dried, followed by carbon deposition and TEM observation. Figure 1 shows a TEM photograph of the precursor particles (particles of iron oxyhydroxide containing substitution elements) obtained in this example. The length indicated by the white horizontal line shown in the lower right of the TEM photograph is 100 nm. In addition, the DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured, and the DLS average diameter was 48.4 nm. Next, 704.7 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 807 g. The temperature was adjusted to 40°C while stirring, 945.2 g of 2-propanol was added and stirred for 5 minutes, after which 207.0 g of 22.3 mass% aqueous ammonia was added. Furthermore, 829.2 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4). The cake obtained in step 4 (precursor coated with gel-like hydrolysis product) was dried, and then the dried powder was heat-treated in a furnace in an air atmosphere at 1050°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0052] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 5.9%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the slurry containing the surface modifier was 0.065 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 16000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 31000 G. The operation of adding 30 g of 0.065 mol / kg TMAOH aqueous solution to the slurry on the precipitate side, ultrasonic dispersion, centrifuging for 30 minutes at 16000 rpm and 31000 G, and collecting 30 g of the supernatant slurry was repeated 9 more times to collect a total of 300 g of the supernatant slurry. The collected 300 g of the supernatant slurry was mixed and 40 g was separated. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was further subjected to 9 times of addition of 30 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry. The precipitate-side slurry was then added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was recovered and then dried to obtain an iron-based oxide magnetic powder according to Example 2.

[0053] The coercive force of the obtained iron oxide magnetic powder is 317 (kA / m) and the saturation magnetization is 14.7 (Am 2 / kg), squareness ratio is 0.590, SFD is 1.43, I L / IH The value was 0.56. The obtained iron oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle size was 14.2 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.5%, the number ratio of particles with a particle diameter of 20 nm or more was 7.2%, the coefficient of variation (CV value) was 19%, and the average circularity of the particles was 0.960. FIG. 2 shows a TEM photograph of the iron oxide magnetic powder obtained in this example. The length indicated by the white horizontal line shown in the lower right of the TEM photograph is 100 nm. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0054] [Example 3] A raw aqueous solution was prepared by mixing 414.1 g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 39.7 g of Ga(III) nitrate solution with a Ga concentration of 10.9% by mass and a nitric acid concentration of 31% by mass as raw materials of substitution elements, 11.2 g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 10.8 g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 641.5 g of pure water. The molar ratio of metal ions in this raw aqueous solution is Fe:Ga:Co:Ti=1.835:0.075:0.045:0.045. Next, 1500 g of pure water was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40° C. while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material aqueous solution and 6.2% ammonia aqueous solution (as alkali) were added simultaneously to this pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 4.21 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at an addition rate of 4.21 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.75 equivalents. The pH of the obtained colloidal solution was 2.11. Next, 288.8 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 186.1 g of 22.14% ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 186.1 g of the ammonia solution all at once was 8.88.

[0055] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 35.5 nm. Next, 848.1 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1000 g. The temperature was adjusted to 40°C while stirring, 1171.3 g of ethanol was added and stirred for 5 minutes, and then 257.8 g of 22.14 mass% ammonia aqueous solution was added. Furthermore, 1027.5 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4). After drying the cake (precursor coated with gel-like hydrolysis product) obtained in step 4, the dried powder was heat-treated in a furnace in an air atmosphere at 1110°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0056] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 5.7%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the slurry containing the surface modifier was 0.065 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 16000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 31000 G. The operation of adding 30 g of 0.065 mol / kg TMAOH aqueous solution to the slurry on the precipitate side, ultrasonic dispersion, centrifuging for 30 minutes at 16000 rpm and 31000 G, and collecting 30 g of the supernatant slurry was repeated 9 more times to collect a total of 300 g of the supernatant slurry. The collected 300 g of the supernatant slurry was mixed and 40 g was separated. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The procedure of adding 30 g of 0.065 mol / kg TMAOH aqueous solution to the precipitate-side slurry, ultrasonic dispersion, centrifuging at 18,000 rpm and 39,000 G for 30 minutes, and removing 30 g of the supernatant slurry was repeated 9 times to obtain a precipitate-side slurry. The pH was adjusted to 6.5 by adding 1 mass % sulfuric acid aqueous solution to the precipitate-side slurry, and the substitutional ε iron oxide particles were agglomerated, and then the slurry was filtered with a membrane filter, and the solid content was collected and dried to obtain an iron-based oxide magnetic powder according to Example 3.

[0057] The coercive force of the obtained iron oxide magnetic powder was 441 (kA / m) and the saturation magnetization was 12.8 (Am 2 / kg), squareness ratio is 0.645, SFD is 1.08, I L / I H The value was 0.42. The obtained iron oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle size was 14.1 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.0%, the number ratio of particles with a particle diameter of 20 nm or more was 0.0%, the coefficient of variation (CV value) was 14%, and the average circularity of the particles was 0.972. FIG. 3 shows a TEM photograph of the iron oxide magnetic powder obtained in this example. The length indicated by the white horizontal line shown in the lower right of the TEM photograph is 100 nm. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0058] [Example 4] A raw aqueous solution was prepared by mixing 391.9 g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 10.1 g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass as a raw material of a substitution element, 9.8 g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 667.4 g of pure water. The molar ratio of metal ions in this raw aqueous solution is Fe:Co:Ti=1.910:0.045:0.045. Next, 1500 g of pure water was placed in a 5L reaction tank, and the liquid temperature was adjusted to 40°C while mechanically stirring with a stirring blade. Next, while continuing the stirring and maintaining the liquid temperature at 40°C, the raw aqueous solution and a 5.6% aqueous ammonia solution (as an alkali) were added simultaneously to this pure water, and then the liquid temperature was maintained at 40°C and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at a rate of 4.22 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at a rate of 4.22 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.75 equivalents. The pH of the resulting colloidal solution was 2.00. Next, 288.8 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 185.4 g of 22.14% ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after adding 185.4 g of the ammonia solution all at once was 8.90.

[0059] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 36.9 nm. Next, 848.8 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1000 g. The temperature was adjusted to 40°C while stirring, 1171.3 g of ethanol was added and stirred for 5 minutes, and then 257.8 g of 22.14 mass% ammonia aqueous solution was added. Furthermore, 1027.5 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4). After drying the cake (precursor coated with gel-like hydrolysis product) obtained in step 4, the dried powder was heat-treated in a furnace in an air atmosphere at 1110°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0060] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 5.7%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the slurry containing the surface modifier was 0.065 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 16000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 31000 G. The operation of adding 30 g of 0.065 mol / kg TMAOH aqueous solution to the slurry on the precipitate side, ultrasonic dispersion, centrifuging for 30 minutes at 16000 rpm and 31000 G, and collecting 30 g of the supernatant slurry was repeated 9 more times to collect a total of 300 g of the supernatant slurry. The collected 300 g of the supernatant slurry was mixed and 40 g was separated. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was further subjected to 9 times of addition of 30 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry, to obtain a precipitate-side slurry. The precipitate-side slurry was then added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was recovered and then dried to obtain an iron-based oxide magnetic powder according to Example 4.

[0061] The coercive force of the obtained iron oxide magnetic powder was 558 (kA / m) and the saturation magnetization was 11.4 (Am 2 / kg), squareness ratio is 0.673, SFD is 0.89, I L / I HThe value was 0.29. The obtained iron oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle size was 14.2 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.0%, the number ratio of particles with a particle diameter of 20 nm or more was 0.0%, the coefficient of variation (CV value) was 12%, and the average circularity of the particles was 0.972. FIG. 4 shows a TEM photograph of the iron oxide magnetic powder obtained in this example. The length indicated by the white horizontal line shown in the lower right of the TEM photograph is 100 nm. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0062] [Example 5] A raw aqueous solution was prepared by mixing 354.9 g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 72.1 g of Ga(III) nitrate solution with a Ga concentration of 10.9% by mass and a nitric acid concentration of 33% by mass as raw materials of substitution elements, 15.8 g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 10.9 g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 475.6 g of pure water. The molar ratio of metal ions in this raw aqueous solution is Fe:Ga:Co:Ti=1.730:0.150:0.070:0.050. Next, 1500 g of pure water was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40° C. while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material aqueous solution and 6.2% ammonia aqueous solution (as alkali) were added simultaneously to this pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 3.87 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at an addition rate of 3.87 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.75 equivalents. The pH of the obtained colloidal solution was 1.65. Next, 288.8 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 186.3 g of 22.14% ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). After adding 185.4 g of ammonia solution all at once, the pH was 8.43.

[0063] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 37.4 nm. Next, 997.6 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1100 g. The temperature was adjusted to 40°C while stirring, 1288.4 g of ethanol was added and stirred for 5 minutes, after which 283.6 g of 22.14 mass% aqueous ammonia was added. Furthermore, 1130.3 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4). After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0064] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 4.1%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the slurry containing the surface modifier was 0.065 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 14000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 24000 G. The operation of adding 30 g of 0.065 mol / kg TMAOH aqueous solution to the slurry on the precipitate side, ultrasonic dispersion, centrifuging for 30 minutes at 14000 rpm and 24000 G, and collecting 30 g of the supernatant slurry was repeated 9 more times to collect a total of 300 g of the supernatant slurry. The collected 300 g of the supernatant slurry was mixed and 40 g was separated. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate slurry was further subjected to 9 times of addition of 30 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry. The precipitate slurry was then added with 1 mass % sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was recovered and then dried to obtain an iron-based oxide magnetic powder according to Example 5.

[0065] The coercive force of the obtained iron oxide magnetic powder is 341 (kA / m) and the saturation magnetization is 16.2 (Am 2 / kg), squareness ratio is 0.641, SFD is 0.69, I L / I H The value of was 0.14. The obtained iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle size was 15.3 nm, the number ratio of particles with a particle size of 8 nm or less was 0.1%, the number ratio of particles with a particle size of 20 nm or more was 0.0%, the coefficient of variation (CV value) was 13%, and the average circularity of the particles was 0.973. In addition, composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0066] [Example 6] A raw aqueous solution was prepared by mixing 329.3 g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 132.2 g of Ga(III) nitrate solution with a Ga concentration of 10.9% by mass and a nitric acid concentration of 33% by mass as raw materials of substitution elements, 15.8 g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 10.9 g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 441.5 g of pure water. The molar ratio of metal ions in this raw aqueous solution is Fe:Ga:Co:Ti=1.650:0.275:0.070:0.050. Next, 1500 g of pure water was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40° C. while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material aqueous solution and 6.2% ammonia aqueous solution (as alkali) were added simultaneously to this pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 3.87 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at an addition rate of 3.87 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.75 equivalents. The pH of the obtained colloidal solution was 1.66. Next, 288.8 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid (hydroxycarboxylic acid addition step), and then 186.8 g of 22.25% ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). After adding 185.4 g of ammonia solution all at once, the pH was 8.51.

[0067] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 32.5 nm. Next, 971.0 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1100 g. The temperature was adjusted to 40°C while stirring, 1288.4 g of ethanol was added and stirred for 5 minutes, after which 283.6 g of 22.14 mass% aqueous ammonia was added. Furthermore, 1130.3 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4). After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0068] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 4.3%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the slurry containing the surface modifier was 0.065 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 14000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 24000 G. The operation of adding 30 g of 0.065 mol / kg TMAOH aqueous solution to the slurry on the precipitate side, ultrasonic dispersion, centrifuging for 30 minutes at 14000 rpm and 24000 G, and collecting 30 g of the supernatant slurry was repeated 9 more times to collect a total of 300 g of the supernatant slurry. The collected 300 g of the supernatant slurry was mixed and 40 g was separated. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was further subjected to 9 times of addition of 30 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry. The precipitate-side slurry was then added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was recovered and then dried to obtain an iron-based oxide magnetic powder according to Example 6.

[0069] The coercive force of the obtained iron oxide magnetic powder is 200 kA / m, and the saturation magnetization is 17.4 (Am 2 / kg), squareness ratio is 0.577, SFD is 1.02, I L / I HThe value of was 0.27. The obtained iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle size was 15.7 nm, the number ratio of particles with a particle size of 8 nm or less was 0.0%, the number ratio of particles with a particle size of 20 nm or more was 1.0%, the coefficient of variation (CV value) was 15%, and the average circularity of the particles was 0.970. In addition, composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0070] [Example 7] A raw aqueous solution was prepared by mixing 334.4g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 120.2g of Ga(III) nitrate solution with a Ga concentration of 10.9% by mass and a nitric acid concentration of 33% by mass as raw materials of substitution elements, 15.8g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 10.9g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 448.2g of pure water. The molar ratio of metal ions in this raw aqueous solution is Fe:Ga:Co:Ti=1.630:0.250:0.070:0.050. Next, 1500g of pure water was placed in a 5L reaction tank, and the liquid temperature was adjusted to 40°C while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material aqueous solution and 6.2% ammonia aqueous solution (as alkali) were added simultaneously to this pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 3.87 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at an addition rate of 3.87 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.75 equivalents. The pH of the obtained colloidal solution was 1.61. Next, 288.8 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid (hydroxycarboxylic acid addition step), and then 186.5 g of 22.25% ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after adding 186.5 g of the ammonia solution all at once was 8.43.

[0071] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 32.3 nm. Next, 923.2 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1100 g. The temperature was adjusted to 40°C while stirring, 1288.4 g of ethanol was added and stirred for 5 minutes, after which 283.6 g of 22.14 mass% ammonia aqueous solution was added. Furthermore, 1130.3 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4). After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0072] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 4.3%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the slurry containing the surface modifier was 0.065 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 14000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 24000 G. The operation of adding 30 g of 0.065 mol / kg TMAOH aqueous solution to the slurry on the precipitate side, ultrasonic dispersion, centrifuging for 30 minutes at 14000 rpm and 24000 G, and collecting 30 g of the supernatant slurry was repeated 9 more times to collect a total of 300 g of the supernatant slurry. The collected 300 g of the supernatant slurry was mixed and 40 g was separated. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was further subjected to 9 times of addition of 30 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry. The precipitate-side slurry was then added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was recovered and then dried to obtain an iron-based oxide magnetic powder according to Example 7.

[0073] The coercive force of the obtained iron oxide magnetic powder is 223 (kA / m) and the saturation magnetization is 17.4 (Am 2 / kg), squareness ratio is 0.595, SFD is 0.91, I L / I H The value of was 0.21. The obtained iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle size was 15.5 nm, the number ratio of particles with a particle size of 8 nm or less was 0.0%, the number ratio of particles with a particle size of 20 nm or more was 0.5%, the coefficient of variation (CV value) was 14%, and the average circularity of the particles was 0.972. In addition, composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0074] [Example 8] A raw aqueous solution was prepared by mixing 627.8 g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 333.4 g of Ga(III) nitrate solution with a Ga concentration of 11.0% by mass and a nitric acid concentration of 33% by mass as raw materials of substitution elements, 31.6 g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 21.8 g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 814.3 g of pure water. The molar ratio of metal ions in this raw aqueous solution is Fe:Ga:Co:Ti=1.530:0.350:0.070:0.050. Next, 3000 g of pure water was placed in a 10 L reaction tank, and the liquid temperature was adjusted to 40° C. while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material aqueous solution and 6.8% ammonia aqueous solution (as alkali) were added simultaneously to this pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 7.62 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at an addition rate of 7.62 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.80 equivalents. The pH of the obtained colloidal solution was 1.86. Next, 577.5 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid (hydroxycarboxylic acid addition step), and then 376.6 g of 22.13% ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 376.6 g of the ammonia solution all at once was 8.6.

[0075] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 50.8 nm. Next, 1975.5 g of the washed slurry obtained in step 4 was taken, and pure water was added to make the total volume 2500 g. The temperature was adjusted to 40°C while stirring, 2928.2 g of ethanol was added and stirred for 5 minutes, and then 702.0 g of 21.87 mass% ammonia aqueous solution was added. Furthermore, 2763.9 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 5). The cake obtained in step 5 (the precursor coated with the gel-like hydrolysis product) was dried, and then the dried powder was heat-treated in a furnace in an air atmosphere at 1116°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 6). The iron oxide powder containing the substituted metal elements coated with silicon oxide obtained in step 6 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites have been substituted with other metal elements (step 7). The slurry from step 7 was washed until the conductivity was ≦15 mS / m.

[0076] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 35%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the slurry containing the surface modifier was 0.065 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (550 g) was subjected to ultrasonic dispersion treatment in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.) for 1 hour, and then centrifuged at 8800 rpm for 130 minutes in an R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to remove 250 g of the supernatant slurry. The gravitational acceleration in the centrifugation treatment was 15000 G. The slurry on the precipitate side was subjected to the addition of 250 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation treatment at 8800 rpm and 15000 G for 130 minutes, and the removal of 250 g of the supernatant slurry, which were repeated 12 more times, to obtain a slurry on the precipitate side (step 8). Next, 250 g of 0.065 mol / kg TMAOH aqueous solution was added to 300 g of the precipitated slurry obtained in step 8, and then ultrasonic dispersion treatment was performed for 1 hour using an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifugal separation treatment was performed for 59 minutes at a rotation speed of 8800 rpm using the R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to recover 250 g of supernatant slurry. The gravitational acceleration in the centrifugation treatment was 15000 G. The operation of adding 250 g of 0.065 mol / kg TMAOH aqueous solution to the precipitated slurry, ultrasonic dispersion, centrifugal separation treatment for 59 minutes at 8800 rpm and 15000 G, and recovering 250 g of supernatant slurry was repeated 12 times to recover a total of 3250 g of supernatant slurry. After mixing 3250 g of the recovered supernatant slurry, a 1 mass % aqueous sulfuric acid solution was added to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then the mixture was filtered through a membrane filter. The solid content was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 8.

[0077] The coercive force of the obtained iron oxide magnetic powder was 183 (kA / m) and the saturation magnetization was 17.7 (Am 2 / kg), squareness ratio is 0.558, SFD is 1.19, I L / I HThe value of was 0.32. The obtained iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle size was 15.0 nm, the number ratio of particles with a particle size of 8 nm or less was 0.3%, the number ratio of particles with a particle size of 20 nm or more was 1.0%, the coefficient of variation (CV value) was 14%, and the average circularity of the particles was 0.974. In addition, composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0078] [Example 9] A raw aqueous solution was prepared by mixing 342.6 g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 114.3 g of Ga(III) nitrate solution with a Ga concentration of 11.0% by mass and a nitric acid concentration of 33% by mass as raw materials of substitution elements, 10.1 g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 9.8 g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 464.0 g of pure water. The molar ratio of metal ions in this raw aqueous solution is Fe:Ga:Co:Ti=1.670:0.240:0.045:0.045. Next, 1500 g of pure water was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40° C. while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material aqueous solution and 6.5% ammonia aqueous solution (as alkali) were added simultaneously to this pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 3.92 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at an addition rate of 3.92 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.79 equivalents. The pH of the obtained colloidal solution was 1.81. Next, 288.8 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid (hydroxycarboxylic acid addition step), and then 190.2 g of 21.87% ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 190.2 g of ammonia solution all at once was 8.67.

[0079] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 58.1 nm. Next, 695.5 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 807 g. The temperature was adjusted to 40°C while stirring, 945.2 g of ethanol was added, and the mixture was stirred for 5 minutes, after which 207.02 g of 22.25 mass% aqueous ammonia was added. Furthermore, 829.2 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the mixture was stirred for 1 hour while maintaining the liquid temperature at 40°C, and coated with the hydrolysis product of the silicon compound. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4). The cake obtained in step 4 (precursor coated with gel-like hydrolysis product) was dried, and then the dried powder was heat-treated in a furnace in an air atmosphere at 1050°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0080] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 4.1%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the slurry containing the surface modifier was 0.065 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at 20,000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to remove 30 g of the supernatant slurry. The gravitational acceleration in the centrifugation treatment was 48,000 G. The slurry on the precipitate side was subjected to the addition of 30 g of a 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 30 minutes at 20,000 rpm and 48,000 G, and the removal of 30 g of the supernatant slurry, which were repeated 9 more times to obtain a slurry on the precipitate side (step 7).

[0081] 30 g of 0.065 mol / kg TMAOH aqueous solution was added to 10 g of the slurry on the precipitate side obtained in step 7, and then ultrasonic dispersion treatment was performed for 1 hour using an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifugal separation treatment was performed for 30 minutes at a rotation speed of 19000 rpm using the R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was removed. The gravitational acceleration during the centrifugation treatment was 43000 G. The slurry on the precipitate side was subjected to the addition of 250 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 30 minutes at 19000 rpm and 43000 G, and the removal of 30 g of the supernatant slurry, which were repeated nine times, to obtain a slurry on the precipitate side (step 8). 30 g of 0.065 mol / kg TMAOH aqueous solution was added to 10 g of the precipitated slurry obtained in step 8, and then ultrasonic dispersion was performed for 1 hour using an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), followed by 30 minutes of centrifugation at 18,000 rpm using the R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was collected. The gravitational acceleration during the centrifugation was 39,000 G. The procedure of adding 30 g of 0.065 mol / kg TMAOH aqueous solution to the precipitated slurry, ultrasonic dispersion, 30 minutes of centrifugation at 18,000 rpm and 39,000 G, and collecting 30 g of the supernatant slurry was repeated 9 more times to collect a total of 300 g of the supernatant slurry. 300 g of the collected supernatant slurry was mixed and then 1 mass % of sulfuric acid aqueous solution was added to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, followed by filtration through a membrane filter. The solid content was collected and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 9.

[0082] The coercive force of the obtained iron oxide magnetic powder was 272 (kA / m) and the saturation magnetization was 15.0 (Am 2 / kg), squareness ratio is 0.606, SFD is 1.16, I L / I HThe value of was 0.34. The obtained iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle size was 14.0 nm, the number ratio of particles with a particle size of 8 nm or less was 0.3%, the number ratio of particles with a particle size of 20 nm or more was 0.6%, the coefficient of variation (CV value) was 14%, and the average circularity of the particles was 0.966. In addition, composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0083] [Comparative Example 1] A raw material solution was prepared by mixing 313.9 g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 195.1 g of gallium (III) nitrate solution with a Ga concentration of 9.4% by mass and a nitric acid concentration of 24% as raw materials of substitution elements, 15.8 g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 10.9 g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 398.0 g of pure water. The molar ratio of metal ions in this raw material solution is Fe:Ga:Co:Ti=1.530:0.350:0.070:0.050. Next, 1500 g of pure water was added to a 5L reaction tank, and the liquid temperature was adjusted to 40°C while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material aqueous solution and 6.4 mass% aqueous ammonia solution as an aqueous alkali solution were added simultaneously to the pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 3.9 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 3.9 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the cumulative amount of alkali added relative to the total cumulative amount of acid radicals contained in the raw material solution was 0.80. The pH of the obtained colloidal solution was 1.8. Next, 288.75 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 152.86 g of 22.4% by mass aqueous ammonia solution was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a slurry of precursor particles, which is an intermediate product (step 2, second neutralization step). After adding 152.86 g of the ammonia solution all at once, the pH was 8.6. The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 506.1 g of the washed slurry obtained in step 3 was taken, the temperature was adjusted to 40°C while stirring, 138.8 g of 22.1 mass% ammonia aqueous solution and 1171.3 g of 2-propanol were added and stirred for 5 minutes, and 552.8 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 7 hours, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4). After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal elements coated with silicon oxide obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 1. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and the slurry was then filtered through a membrane filter. The solid content was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 1. The coercive force of this iron-based oxide magnetic powder was 177 kA / m and the saturation magnetization was 17.9 Am. 2 / kg, SFD is 1.00, I L / I H The value was 0.41. The obtained iron-based oxide magnetic powder according to Comparative Example 1 was subjected to TEM observation in the same manner as in Example 1. As a result, the TEM average particle size was 16.6 nm, the number ratio of particles with a particle size of 8 nm or less was 0.0%, the number ratio of particles with a particle size of 20 nm or more was 14.9%, the coefficient of variation (CV value) was 20%, and the average circularity of the particles was 0.972. FIG. 5 shows a TEM photograph of the iron-based oxide magnetic powder obtained in this comparative example. The length indicated by the white horizontal line shown in the lower right of the TEM photograph is 100 nm. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles. The above manufacturing conditions are shown in Tables 1 and 2, and the measurement results of the obtained iron-based oxide magnetic powder are shown in Tables 3 and 4.

[0084] [Comparative Example 2] In a 5L reaction tank, 291.32g of ferric nitrate (III) nonahydrate with a purity of 99.4%, 80.18g of Ga(III) nitrate solution with a Ga concentration of 10.1%, 6.58g of cobalt(II) nitrate hexahydrate with a purity of 97%, and 7.14g of titanium(IV) sulfate n-hydrate with a Ti concentration of 14.7% are dissolved in 3214.78g of pure water while mechanically stirring with a stirring blade under the conditions of 40°C in an air atmosphere. The molar ratio of metal ions in this charged solution is Fe:Ga:Co:Ti=1.635:0.265:0.050:0.050. The numbers in parentheses after the names of the reagents indicate the valence of the metal elements. In an air atmosphere at 40°C, 166.29 g of 21.2% ammonia solution was added all at once while mechanically stirring with a stirring blade so that the pH after neutralization was between 1.0 and 3.0, and stirring was continued for 2 hours. At the beginning of the addition, the liquid was brown and cloudy, but after 2 hours it became a transparent brown reaction liquid with a pH of 1.96. Next, 252.66 g of citric acid solution with a citric acid concentration of 10 mass% was added continuously over 1 hour under the condition of 40 ° C., and then 200 g of 10 mass% ammonia solution was added all at once so that the pH was 7.0 to 10.0. After the pH was adjusted to 8.47, the mixture was kept under stirring at a temperature of 40 ° C. for 1 hour to generate crystals of iron oxyhydroxide containing the substitution element of the precursor, which is an intermediate product (step 1). In this example, the molar ratio O / (Fe+M) of the total amount of trivalent iron ions and the metal ions M that partially substitute the Fe site was 0.15. The slurry containing the iron oxyhydroxide crystals obtained in step 1 was dropped and attached to a collodion film on a grid, naturally dried, and then carbon deposition was performed, and the slurry was subjected to TEM observation. Figure 6 shows a TEM photograph of the precursor particles (particles of iron oxyhydroxide containing substitution elements) obtained in this comparative example. The length indicated by the white horizontal line shown in the lower right of the TEM photograph is 100 nm. In addition, when the slurry obtained in step 1 was subjected to measurement of the DLS average diameter of the precursor particles, the result was outside the allowable measurement range (up to 500 nm), and the DLS average diameter could not be measured. Then, in an air atmosphere at 30°C, 488.13 g of tetraethoxysilane is added to the precursor slurry obtained in step 1 over 35 minutes while stirring. The temperature is maintained at 30°C and stirring is continued for about a day to coat the precursor with the silanol derivative generated by hydrolysis. Then, a solution of 194.7 g of ammonium sulfate dissolved in 300 g of pure water is added, and the resulting solution is washed and separated into solid and liquid, and collected as a cake (step 2). After drying the precipitate (gel-like SiO2-coated precursor) obtained in step 2, the dried powder was heat-treated in a furnace in an air atmosphere at 1070°C for 4 hours to obtain iron-based oxide magnetic particle powder coated with silicon oxide. Note that the silanol derivative is converted to an oxide when heat-treated in an air atmosphere (step 3). The heat-treated powder obtained in step 3 was stirred in a 20 mass% NaOH aqueous solution at about 70°C for 24 hours to remove silicon oxide from the particle surface. It was then washed until the conductivity of the washing slurry became ≦15mS / m, and after drying, it was subjected to chemical analysis of the composition, XRD measurement, TEM observation, and measurement of magnetic properties. The chemical composition of the obtained iron-based oxide magnetic particles was slightly high in Fe and slightly low in Ga, but was almost the same as the composition at the time of charging. The iron-based oxide magnetic particles obtained in this comparative example were subjected to TEM observation in the same manner as in Example 1, and the average particle size was 16.6 nm and the coefficient of variation (CV value) was 40.2%. Figure 7 shows a TEM photograph of the iron-based oxide magnetic particles obtained in this comparative example. Two peaks were clearly observed in the differential BH curve, and the SFD calculated from the half-width of the peak of the high Hc component was 0.89, and the ratio I of the low Hc component was 0. L / I H was 0.50.

[0085] [Comparative Example 3] In a 5L reaction tank, 465.93g of 99.7% purity ferric nitrate (III) nonahydrate, 152.80g of Ga(III) nitrate solution with a Ga concentration of 12.0 mass%, 15.78g of 97% purity cobalt (II) nitrate hexahydrate, and 11.91g of titanium (IV) sulfate solution with a Ti concentration of 15.1 mass% were dissolved in 2453.58g of pure water while mechanically stirring with a stirring blade under the conditions of 40°C in an air atmosphere. The molar ratio of metal ions in this charged solution was Fe:Ga:Co:Ti=1.530:0.350:0.070:0.050. In an air atmosphere at 40°C, 268.52 g of 22.4% aqueous ammonia solution was added all at once while mechanically stirring with a stirring blade, and stirring was continued for 2 hours (first neutralization step). At the beginning of the addition, the liquid was brown and cloudy, but after 2 hours it became a transparent brown reaction liquid with a pH of 1.9. Next, 288.75 g of citric acid solution with a citric acid concentration of 20% by mass as hydroxycarboxylic acid was added continuously over 1 hour at 40° C. (hydroxycarboxylic acid addition step), and then 152.86 g of 22.4% ammonia solution was added all at once, and the mixture was kept at 40° C. with stirring for 1 hour to produce iron oxyhydroxide crystals containing the substitution element of the precursor, which is the intermediate product (step 1, second neutralization step). After adding 152.86 g of the ammonia solution all at once, the pH was 8.6. Then, 416.89 g of tetraethoxysilane (TEOS) is added to the precursor slurry obtained in step 1 over 35 minutes while stirring at 40°C in an air atmosphere. Stirring is continued for about a day, and the mixture is coated with the hydrolysis product of the silane compound produced by hydrolysis. The resulting solution is then washed and separated into solid and liquid, and collected as a cake (step 2). After drying the precipitate (gel-like SiO2-coated precursor) obtained in step 2, the dried powder was heat-treated in a furnace in an air atmosphere at 971°C for 4 hours to obtain a powder of substituted ε-iron oxide coated with silicon oxide. Note that the hydrolysis product of the silane compound is converted to an oxide when heat-treated in an air atmosphere (step 3). The powder of substituted ε-iron oxide coated with silicon oxide obtained in step 3 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing iron-based oxide particles (step 4). When the slurry obtained in step 4 was observed with a transmission electron microscope, the TEM average particle size was 17.8 nm and the coefficient of variation (CV value) was 39%. The slurry obtained in step 4 was washed until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 1. A 1% by mass aqueous sulfuric acid solution was added to the obtained washed slurry to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then the slurry was filtered through a membrane filter. The solid content was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder before classification. The coercive force of this iron-based oxide magnetic powder before classification was 171 (kA / m), and the saturation magnetization was 15.7 (Am 2 / kg), squareness ratio is 0.433, SFD is 1.40, IL / I H The value of β-methyl-2-pyridine was 0.82 and the BET specific surface area was 85.5 m2 / g. Next, a 25% by mass aqueous solution of tetramethylammonium hydroxide (hereinafter referred to as TMAOH) was added as a surface modifier to the washed slurry to obtain a surface modifier-containing slurry according to Comparative Example 3. The amount of the TMAOH aqueous solution added was set so that the TMAOH concentration in the surface modifier-containing slurry was 0.065 mol / kg. In this case, the pH of the slurry was 13. 40 g of the obtained surface modifier-containing slurry was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 15 minutes at 20,000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 33 g of the supernatant containing fine particles was removed to obtain a precipitate. The gravitational acceleration in the centrifugation treatment was 48,000 G. In addition, the average secondary particle diameter (DLS particle diameter) of the iron-based oxide in the surface modifier-containing slurry after the ultrasonic treatment was measured and found to be 29 nm. Then, 33 g of a 0.065 mol / kg TMAOH aqueous solution was added to the obtained precipitate, and the above-mentioned ultrasonic dispersion treatment, the above-mentioned centrifugation treatment, and the removal of 33 g of the supernatant were repeated nine times to obtain a slurry of iron-based oxide magnetic powder of Comparative Example 3. The obtained slurry of the iron-based oxide magnetic powder according to Comparative Example 3 was observed by TEM, and the TEM average particle size was 18.8 nm and the coefficient of variation (CV value) was 29%. The TEM observation of the slurry refers to dropping the slurry onto a collodion film on a grid, allowing it to adhere, allowing it to dry naturally, and then subjecting it to carbon deposition for TEM observation. Figure 1 shows a TEM photograph of the iron-based oxide magnetic powder obtained in this example. The length of the white vertical line shown in the center left of the TEM photograph is 50 nm. 33 g of pure water was added to the obtained slurry of iron-based oxide magnetic powder of Comparative Example 3, and a 1 mass% aqueous sulfuric acid solution was added to adjust the pH to 6.5. The mixture was then filtered through a membrane, and the cake was recovered and dried to obtain iron-based oxide magnetic powder of Comparative Example 3. The chemical composition of the obtained iron-based oxide magnetic powder was calculated so that the total molar ratio of Fe, Ga, Co, and Ti was 2.0, and the results are shown in Table 2. L / I H The value was 0.25.

[0086] [Example 10] As the raw material solution, 1013 g of an aqueous solution with a Fe(III) concentration of 1.112 mol / kg and a chloride ion concentration of 3.337 mol / kg was prepared. Next, 1603 g of an aqueous solution with a Fe(III) concentration of 0.234 mol / kg and a chloride ion concentration of 0.703 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 30 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and a 3.337 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 30 ° C. and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 4.2 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 4.2 g / min over 240 minutes. During the addition of the raw solution and the ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw solution was 1.0 equivalent. The pH of the resulting colloidal solution was 2.3. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 over a period of 60 minutes at 30° C. (hydroxycarboxylic acid addition step), and then 189 g of ammonia solution with a concentration of 12.864 mol / kg was added all at once. The mixture was then kept at 30° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 189 g of ammonia solution all at once was 9.2.

[0087] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 127.8 nm. Next, 857 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 950 g. The temperature was adjusted to 40°C while stirring, 1171 g of ethanol was added and stirred for 5 minutes, after which 260 g of 21.92 mass% aqueous ammonia was added. Furthermore, 1028 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0088] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass % NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0089] Next, 35% by mass of TEAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 5.0%. The amount of the TEAOH aqueous solution added was set so that the TEAOH concentration in the slurry containing the surface modifier was 0.099 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 60 minutes at 20,000 rpm in the R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry containing fine particles was removed to obtain a slurry on the precipitate side. The gravitational acceleration in the centrifugation treatment was 48,000 G. The slurry on the precipitate side was further subjected to the addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 60 minutes at 20,000 rpm and 48,000 G, and the removal of 30 g of the supernatant slurry, nine times to obtain a slurry on the precipitate side. 30 g of 0.099 mol / kg TEAOH aqueous solution was added to 10 g of the obtained precipitate side slurry, and then ultrasonic dispersion treatment was performed for 1 hour using an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), followed by centrifugation treatment for 50 minutes at 20,000 rpm using the R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate side slurry. The gravitational acceleration in the centrifugation treatment was 48,000 G. The slurry on the precipitate side was further subjected to the following operations: addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 50 minutes at 20,000 rpm and 48,000 G, and removal of 30 g of the supernatant slurry, nine times to obtain a precipitate side slurry. 30 g of 0.099 mol / kg TEAOH aqueous solution was added to 10 g of the obtained precipitate side slurry, and then ultrasonic dispersion treatment was performed for 1 hour using an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), followed by centrifugation treatment for 40 minutes at a rotation speed of 20,000 rpm using the R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 30 g of the supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 48,000 G. The operation of adding 30 g of 0.099 mol / kg TEAOH aqueous solution to the obtained precipitate side slurry, ultrasonic dispersion, centrifugation treatment for 40 minutes at 20,000 rpm and 48,000 G, and collecting 30 g of the supernatant slurry was repeated 9 more times to collect a total of 300 g of the supernatant slurry. A 1% by mass aqueous sulfuric acid solution was added to the recovered supernatant slurry to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then the mixture was filtered through a membrane filter. The solid content was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 10.

[0090] The coercive force of the obtained iron oxide magnetic powder was 560 (kA / m) and the saturation magnetization was 12.8 (Am 2 / kg), squareness ratio is 0.544, SFD is 1.99, I L / I H The value of was 0.47. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 10.3 nm, the number ratio of particles with a particle diameter of 8 nm or less was 1.2%, the number ratio of particles with a particle diameter of 20 nm or more was 0.0%, the coefficient of variation (CV value) was 9%, and the average circularity of the particles was 0.970. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0091] [Example 11] As the raw material solution, 1019 g of an aqueous solution with a Fe(III) concentration of 1.056 mol / kg, a Co(II) concentration of 0.066 mol / kg, a chloride ion concentration of 3.167 mol / kg, and a nitrate ion concentration of 0.133 mol / kg was prepared. Next, 1598 g of an aqueous solution with a Fe(III) concentration of 0.225 mol / kg and a chloride ion concentration of 0.674 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and a 3.267 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. while stirring for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 4.2 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 4.2 g / min over 240 minutes. During the addition of the raw solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw solution was 0.99 equivalents. The pH of the resulting colloidal solution was 2.1. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 194 g of ammonia solution with a concentration of 12.347 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 194 g of ammonia solution all at once was 9.2.

[0092] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 147.1 nm. Next, 894 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 950 g. The temperature was adjusted to 40°C while stirring, 1171 g of ethanol was added and stirred for 5 minutes, after which 271 g of 21.04 mass% aqueous ammonia was added. Furthermore, 1028 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0093] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0094] Next, 35% by mass of TEAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 3.1%. The amount of the TEAOH aqueous solution added was set so that the TEAOH concentration in the slurry containing the surface modifier was 0.099 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 20,000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation treatment was 48,000 G. The obtained precipitated side slurry was subjected to the addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 30 minutes at 20,000 rpm and 48,000 G, and the recovery of 30 g of supernatant slurry, which were repeated 9 more times, to recover a total of 300 g of supernatant slurry. The recovered 300 g of supernatant slurry was mixed and then 40 g was separated. The collected 40 g of supernatant slurry was centrifuged for 30 minutes at 16,000 rpm in the R20A2 rotor of a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation was 31,000 G. The procedure of adding 30 g of 0.099 mol / kg TEAOH aqueous solution to the obtained precipitated slurry, ultrasonic dispersion, centrifuging for 30 minutes at 16,000 rpm and 31,000 G, and recovering 30 g of supernatant slurry was repeated 9 more times to recover a total of 300 g of supernatant slurry. The collected 300 g of supernatant slurry was mixed and then 40 g was collected. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was subjected to the following operations: addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry, which were repeated nine times to obtain a precipitate-side slurry. The precipitate-side slurry was added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was collected and then dried to obtain an iron-based oxide magnetic powder according to Example 11.

[0095] The coercive force of the obtained iron oxide magnetic powder was 875 (kA / m) and the saturation magnetization was 20.6 (Am 2 / kg), squareness ratio is 0.502, SFD is 1.66, I L / I H The value of was 0.50. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 16.5 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.5%, the number ratio of particles with a particle diameter of 20 nm or more was 3.0%, the coefficient of variation (CV value) was 12%, and the average circularity of the particles was 0.966. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0096] [Example 12] As the raw material solution, 1021 g of an aqueous solution with a Fe(III) concentration of 1.055 mol / kg, a Ti(IV) concentration of 0.066 mol / kg, and a chloride ion concentration of 3.332 mol / kg was prepared. Next, 1598 g of an aqueous solution with a Fe(III) concentration of 0.225 mol / kg and a chloride ion concentration of 0.674 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and a 3.290 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 4.3 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 4.3 g / min over 240 minutes. During the addition of the raw solution and the ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw solution was 0.99 equivalents. The pH of the resulting colloidal solution was 1.8. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.347 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). After adding 194 g of ammonia solution all at once, the pH was 9.1.

[0097] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 36.1 nm. Next, 882 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 950 g. The temperature was adjusted to 40°C while stirring, 1171 g of ethanol was added and stirred for 5 minutes, after which 271 g of 21.04 mass% aqueous ammonia was added. Furthermore, 1028 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0098] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal elements coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 15 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites have been substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0099] Next, 35% by mass of TEAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 3.1%. The amount of the TEAOH aqueous solution added was set so that the TEAOH concentration in the slurry containing the surface modifier was 0.099 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 20,000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation treatment was 48,000 G. The obtained precipitated side slurry was subjected to the addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 30 minutes at 20,000 rpm and 48,000 G, and the recovery of 30 g of supernatant slurry, which were repeated 9 more times, to recover a total of 300 g of supernatant slurry. The recovered 300 g of supernatant slurry was mixed and then 40 g was separated. The collected 40 g of supernatant slurry was centrifuged for 30 minutes at 16,000 rpm in the R20A2 rotor of a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation was 31,000 G. The procedure of adding 30 g of 0.099 mol / kg TEAOH aqueous solution to the obtained precipitated slurry, ultrasonic dispersion, centrifuging for 30 minutes at 16,000 rpm and 31,000 G, and recovering 30 g of supernatant slurry was repeated 9 more times to recover a total of 300 g of supernatant slurry. The collected 300 g of supernatant slurry was mixed and then 40 g was collected. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was subjected to the following operations: addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry, which were repeated nine times to obtain a precipitate-side slurry. The precipitate-side slurry was added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was collected and then dried to obtain an iron-based oxide magnetic powder according to Example 12.

[0100] The coercive force of the obtained iron oxide magnetic powder was 1267 (kA / m) and the saturation magnetization was 16.0 (Am 2 / kg), squareness ratio is 0.546, SFD is 0.50, I L / I H The value of was 0.12. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 15.9 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.0%, the number ratio of particles with a particle diameter of 20 nm or more was 1.6%, the coefficient of variation (CV value) was 12%, and the average circularity of the particles was 0.974. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0101] [Example 13] As the raw material solution, 1018 g of an aqueous solution with Fe(III) concentration of 1.045 mol / kg, Co(II) concentration of 0.050 mol / kg, Ti(IV) concentration of 0.033 mol / kg, chloride ion concentration of 3.219 mol / kg, and nitrate ion concentration of 0.100 mol / kg was prepared. Next, 1597 g of an aqueous solution with Fe(III) concentration of 0.222 mol / kg and chloride ion concentration of 0.666 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.272 mol / kg ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at a rate of 4.2 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at a rate of 4.2 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.99 equivalents. The pH of the resulting colloidal solution was 1.6. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.512 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 192 g of ammonia solution all at once was 8.8.

[0102] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 38.7 nm. Next, 852 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 950 g. The temperature was adjusted to 40°C while stirring, 1171 g of ethanol was added and stirred for 5 minutes, after which 268 g of 21.32 mass% aqueous ammonia was added. Furthermore, 1028 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0103] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0104] Next, 35% by mass of TEAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 5.7%. The amount of the TEAOH aqueous solution added was set so that the TEAOH concentration in the slurry containing the surface modifier was 0.099 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 16000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation treatment was 31000 G. The obtained precipitated side slurry was subjected to the addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 30 minutes at 16000 rpm and 31000 G, and the recovery of 30 g of supernatant slurry, which were repeated 9 more times, to recover a total of 300 g of supernatant slurry. The recovered 300 g of supernatant slurry was mixed and then 40 g was separated. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was subjected to the addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry, which were repeated nine times to obtain a precipitate-side slurry. The precipitate-side slurry was added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was collected and then dried to obtain an iron-based oxide magnetic powder according to Example 13.

[0105] The coercive force of the obtained iron oxide magnetic powder is 499 (kA / m) and the saturation magnetization is 14.8 (Am 2 / kg), squareness ratio is 0.529, SFD is 1.78, I L / I HThe value of was 0.46. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 13.3 nm, the number ratio of particles with a particle diameter of 8 nm or less was 1.4%, the number ratio of particles with a particle diameter of 20 nm or more was 0.5%, the coefficient of variation (CV value) was 17%, and the average circularity of the particles was 0.970. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0106] [Example 14] As the raw material solution, 936 g of an aqueous solution with Fe(III) concentration of 0.921 mol / kg, Ga(III) concentration of 0.321 mol / kg, Co(II) concentration of 0.056 mol / kg, chloride ion concentration of 1.288 mol / kg, and nitrate ion concentration of 2.659 mol / kg was prepared. Next, 1578 g of an aqueous solution with Fe(III) concentration of 0.182 mol / kg and chloride ion concentration of 0.546 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.651 mol / kg ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at a rate of 3.9 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at a rate of 3.9 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.93 equivalents. The pH of the resulting colloidal solution was 2.0. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.553 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). After adding 192 g of ammonia solution all at once, the pH was 8.6.

[0107] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 150 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 195.5 nm. Next, 852 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 950 g. The temperature was adjusted to 40°C while stirring, 1171 g of ethanol was added and stirred for 5 minutes, after which 268 g of 21.32 mass% aqueous ammonia was added. Furthermore, 1028 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0108] The cake obtained in step 4 (the precursor coated with the gel-like hydrolysis product) was dried, and then the dried powder was heat-treated in a furnace in an air atmosphere at 1060°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 14 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites have been substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0109] Next, 35% by mass of TEAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 3.1%. The amount of the TEAOH aqueous solution added was set so that the TEAOH concentration in the slurry containing the surface modifier was 0.099 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 20,000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation treatment was 48,000 G. The obtained precipitated side slurry was subjected to the addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 30 minutes at 20,000 rpm and 48,000 G, and the recovery of 30 g of supernatant slurry, which were repeated 9 more times, to recover a total of 300 g of supernatant slurry. The recovered 300 g of supernatant slurry was mixed and then 40 g was separated. The collected 40 g of supernatant slurry was centrifuged for 30 minutes at 16,000 rpm in the R20A2 rotor of a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation was 31,000 G. The procedure of adding 30 g of 0.099 mol / kg TEAOH aqueous solution to the obtained precipitated slurry, ultrasonic dispersion, centrifuging for 30 minutes at 16,000 rpm and 31,000 G, and recovering 30 g of supernatant slurry was repeated 9 more times to recover a total of 300 g of supernatant slurry. The collected 300 g of supernatant slurry was mixed and then 40 g was collected. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was subjected to the following operations: addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry, which were repeated nine times to obtain a precipitate-side slurry. The precipitate-side slurry was added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was collected and then dried to obtain an iron-based oxide magnetic powder according to Example 14.

[0110] The coercive force of the obtained iron oxide magnetic powder is 324 (kA / m) and the saturation magnetization is 16.9 (Am 2 / kg), squareness ratio is 0.626, SFD is 0.77, I L / I HThe value of was 0.20. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 16.4 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.0%, the number ratio of particles with a particle diameter of 20 nm or more was 2.4%, the coefficient of variation (CV value) was 12%, and the average circularity of the particles was 0.975. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0111] [Example 15] As the raw material solution, 893 g of an aqueous solution with Fe(III) concentration of 0.993 mol / kg, Ga(III) concentration of 0.235 mol / kg, Co(II) concentration of 0.038 mol / kg, Ni(II) concentration of 0.084 mol / kg, chloride ion concentration of 2.980 mol / kg, and nitrate ion concentration of 1.005 mol / kg was prepared. Next, 1581 g of an aqueous solution with Fe(III) concentration of 0.187 mol / kg and chloride ion concentration of 0.561 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and maintaining the liquid temperature at 40 ° C., the raw material solution and 3.734 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at a rate of 3.7 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at a rate of 3.7 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.94 equivalents. The pH of the resulting colloidal solution was 2.1. Next, 274.3 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 193 g of ammonia solution with a concentration of 12.465 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 193 g of ammonia solution all at once was 8.8.

[0112] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 39.9 nm. Next, 1057 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150 g. The temperature was adjusted to 40°C while stirring, 1406 g of ethanol was added, and the mixture was stirred for 5 minutes, after which 347 g of 21.24 mass% aqueous ammonia was added. Furthermore, 1327 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the mixture was stirred for 1 hour while maintaining the liquid temperature at 40°C, and coated with the hydrolysis product of the silicon compound. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0113] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal elements coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 14 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0114] Next, 35% by mass of TEAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a slurry containing the surface modifier with a solid content of 3.1%. The amount of the TEAOH aqueous solution added was set so that the TEAOH concentration in the slurry containing the surface modifier was 0.099 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 20,000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation treatment was 48,000 G. The obtained precipitated side slurry was subjected to the addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 30 minutes at 20,000 rpm and 48,000 G, and the recovery of 30 g of supernatant slurry, which were repeated 9 more times, to recover a total of 300 g of supernatant slurry. The recovered 300 g of supernatant slurry was mixed and then 40 g was separated. The collected 40 g of supernatant slurry was centrifuged for 30 minutes at 16,000 rpm in the R20A2 rotor of a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation was 31,000 G. The procedure of adding 30 g of 0.099 mol / kg TEAOH aqueous solution to the obtained precipitated slurry, ultrasonic dispersion, centrifuging for 30 minutes at 16,000 rpm and 31,000 G, and recovering 30 g of supernatant slurry was repeated 9 more times to recover a total of 300 g of supernatant slurry. The collected 300 g of supernatant slurry was mixed and then 40 g was collected. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was subjected to the following operations: addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry, which were repeated nine times to obtain a precipitate-side slurry. The precipitate-side slurry was added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was collected and then dried to obtain an iron-based oxide magnetic powder according to Example 15.

[0115] The coercive force of the obtained iron oxide magnetic powder was 505 (kA / m) and the saturation magnetization was 22.4 (Am 2 / kg), squareness ratio is 0.494, SFD is 0.72, I L / I HThe value of was 0.59. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid to adhere to it, and after natural drying, carbon deposition was performed and the particles were subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 15.8 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.6%, the number ratio of particles with a particle diameter of 20 nm or more was 1.8%, the coefficient of variation (CV value) was 12%, and the average circularity of the particles was 0.973. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0116] [Example 16] As the raw material solution, 895 g of an aqueous solution with Fe(III) concentration of 0.991 mol / kg, Ga(III) concentration of 0.235 mol / kg, Co(II) concentration of 0.038 mol / kg, Cr(III) concentration of 0.084 mol / kg, chloride ion concentration of 2.974 mol / kg, and nitrate ion concentration of 1.087 mol / kg was prepared. Next, 1581 g of an aqueous solution with Fe(III) concentration of 0.187 mol / kg and chloride ion concentration of 0.561 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.808 mol / kg of ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at a rate of 3.7 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at a rate of 3.7 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.94 equivalents. The pH of the resulting colloidal solution was 2.0. Next, 288.8 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.553 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 196 g of ammonia solution all at once was 8.5.

[0117] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 354.1 nm. Next, 1084 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150 g. The temperature was adjusted to 40°C while stirring, 1406 g of ethanol was added, and the mixture was stirred for 5 minutes, after which 345 g of 21.39 mass% aqueous ammonia was added. Furthermore, 1327 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the mixture was stirred for 1 hour while maintaining the liquid temperature at 40°C, and coated with the hydrolysis product of the silicon compound. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0118] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1130°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal elements coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 60°C and stirred for 14 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites were substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦15 mS / m.

[0119] Next, 35% by mass of TEAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a surface modifier-containing slurry with a solid content of 3.2%. The amount of TEAOH aqueous solution added was set so that the TEAOH concentration in the surface modifier-containing slurry was 0.099 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (40 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 30 minutes at a rotation speed of 20,000 rpm in an R20A2 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation treatment was 48,000 G. The obtained precipitated side slurry was subjected to the addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 30 minutes at 20,000 rpm and 48,000 G, and the recovery of 30 g of supernatant slurry, which were repeated 9 more times, to recover a total of 300 g of supernatant slurry. The recovered 300 g of supernatant slurry was mixed and then 40 g was separated. The collected 40 g of supernatant slurry was centrifuged for 30 minutes at 16,000 rpm in the R20A2 rotor of a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) to recover 30 g of supernatant slurry. The gravitational acceleration in the centrifugation was 31,000 G. The procedure of adding 30 g of 0.099 mol / kg TEAOH aqueous solution to the obtained precipitated slurry, ultrasonic dispersion, centrifuging for 30 minutes at 16,000 rpm and 31,000 G, and recovering 30 g of supernatant slurry was repeated 9 more times to recover a total of 300 g of supernatant slurry. The collected 300 g of supernatant slurry was mixed and then 40 g was collected. The collected supernatant slurry (40 g) was centrifuged for 30 minutes at 18,000 rpm in a centrifuge (Hitachi Koki Co., Ltd., himac CR21GII) with an R20A2 rotor, and 30 g of the supernatant slurry containing fine particles was removed to obtain a precipitate-side slurry. The gravitational acceleration in the centrifugation was 39,000 G. The precipitate-side slurry was subjected to the following operations: addition of 30 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation at 18,000 rpm and 39,000 G for 30 minutes, and removal of 30 g of the supernatant slurry, which were repeated nine times to obtain a precipitate-side slurry. The precipitate-side slurry was added with a 1% by mass sulfuric acid aqueous solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered with a membrane filter. The solid content was collected and then dried to obtain an iron-based oxide magnetic powder according to Example 16.

[0120] The coercive force of the obtained iron oxide magnetic powder was 471 (kA / m) and the saturation magnetization was 16.1 (Am 2 / kg), squareness ratio is 0.542, SFD is 0.78, I L / I HThe value of was 0.18. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 15.8 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.0%, the number ratio of particles with a particle diameter of 20 nm or more was 2.0%, the coefficient of variation (CV value) was 13%, and the average circularity of the particles was 0.975. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0121] [Example 17] As the raw material solution, 1829 g of an aqueous solution was prepared with Fe(III) concentration of 1.257 mol / kg, Ga(III) concentration of 0.288 mol / kg, Co(II) concentration of 0.058 mol / kg, Ti(IV) concentration of 0.041 mol / kg, chloride ion concentration of 3.876 mol / kg, and nitrate ion concentration of 1.075 mol / kg. Next, 3000 g of pure water was placed in a 10 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.961 mol / kg aqueous ammonia solution were added simultaneously to the pure water, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at an addition rate of 7.6 g / min for 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 7.6 g / min for 240 minutes. During the addition of the raw solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw solution was 0.80 equivalents. The pH of the resulting colloidal solution was 1.8. Next, 578 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 377 g of ammonia solution with a concentration of 12.987 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 377 g of ammonia solution all at once was 8.8.

[0122] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 1 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 46.2 nm. Next, 1294 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 2400 g. The temperature was adjusted to 40°C while stirring, 2928 g of ethanol was added, and the mixture was stirred for 5 minutes, after which 694 g of 22.13 mass% aqueous ammonia solution was added. Furthermore, 2764 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the mixture was stirred for 1 hour while maintaining the liquid temperature at 40°C, and coated with the hydrolysis product of the silicon compound. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0123] After drying the cake (precursor coated with gel-like hydrolysis product) obtained in step 4, the dried powder was heat-treated in a furnace in an air atmosphere at 1116°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 80°C and stirred for 20 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites have been substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦1 mS / m.

[0124] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a surface modifier-containing slurry with a solid content of 36.0%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the surface modifier-containing slurry was 0.065 mol / kg. In this case, the pH of the slurry became 13. The obtained slurry containing the surface modifier (460 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 130 minutes at 8800 rpm in the R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 250 g of the supernatant slurry containing fine particles was removed to obtain a slurry on the precipitate side. The gravitational acceleration in the centrifugation treatment was 15000 G. The slurry on the precipitate side was subjected to the addition of 250 g of a 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 130 minutes at 8800 rpm and 15000 G, and the removal of 250 g of the supernatant slurry, which were repeated 9 times to obtain a slurry on the precipitate side. 250 g of 0.065 mol / kg TMAOH aqueous solution was added to 210 g of the obtained precipitate side slurry, and then ultrasonic dispersion treatment was performed for 1 hour using an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), followed by centrifugation treatment for 70 minutes at a rotation speed of 8800 rpm using the R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 250 g of supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 15000 G. The operation of adding 250 g of 0.065 mol / kg TMAOH aqueous solution to the obtained precipitate side slurry, ultrasonic dispersion, centrifugation treatment for 70 minutes at 8800 rpm and 15000 G, and collecting 250 g of supernatant slurry was repeated 15 times to collect a total of 4000 g of supernatant slurry. A 1% by mass aqueous sulfuric acid solution was added to the recovered supernatant slurry to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then the mixture was filtered through a membrane filter. The solid content was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 17.

[0125] The coercive force of the obtained iron oxide magnetic powder was 171 (kA / m) and the saturation magnetization was 16.6 (Am 2 / kg), squareness ratio is 0.556, SFD is 1.21, I L / I H The value of was 0.33. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 15.3 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.3%, the number ratio of particles with a particle diameter of 20 nm or more was 2.1%, the coefficient of variation (CV value) was 14%, and the average circularity of the particles was 0.973. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0126] [Example 18] As the raw material solution, 2687 g of an aqueous solution with Fe(III) concentration of 1.430 mol / kg, Ga(III) concentration of 0.147 mol / kg, Co(II) concentration of 0.059 mol / kg, Ti(IV) concentration of 0.042 mol / kg, chloride ion concentration of 4.398 mol / kg, and nitrate ion concentration of 0.592 mol / kg was prepared. Next, 4500 g of pure water was placed in a 10 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.742 mol / kg of ammonia aqueous solution were added simultaneously to the pure water, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at a rate of 11.2 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at a rate of 11.2 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.75 equivalents. The pH of the resulting colloidal solution was 1.7. Next, 866 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously as hydroxycarboxylic acid to the colloidal solution obtained in step 1 over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 557 g of ammonia solution with a concentration of 12.993 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 557 g of ammonia solution all at once was 8.5.

[0127] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 37.8 nm. Next, 710 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1650 g. The temperature was adjusted to 40°C while stirring, 2050 g of ethanol was added and stirred for 5 minutes, after which 971 g of 22.14 mass% aqueous ammonia was added. Furthermore, 3870 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0128] After drying the cake (precursor coated with gel-like hydrolysis product) obtained in step 4, the dried powder was heat-treated at 1115°C for 4 hours in a furnace in an air atmosphere to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 80°C and stirred for 20 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites have been substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦1 mS / m.

[0129] Next, 25% by mass of TMAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a surface modifier-containing slurry with a solid content of 40.0%. The amount of TMAOH aqueous solution added was set so that the TMAOH concentration in the surface modifier-containing slurry was 0.065 mol / kg. In this case, the pH of the slurry was 13. The obtained surface modifier-containing slurry (460 g) was subjected to ultrasonic dispersion treatment in an ultrasonic cleaner (Yamato5510, manufactured by Branson (Yamato Scientific) Co., Ltd.) for 1 hour, and then centrifuged for 60 minutes at a rotation speed of 8800 rpm in an R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.) to recover 250 g of supernatant slurry. The gravitational acceleration in the centrifugation treatment was 15000 G. The obtained slurry on the precipitate side was subjected to the addition of 250 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 70 minutes at 8800 rpm and 15000 G, and the recovery of 250 g of supernatant slurry, which were repeated 12 times, to recover a total of 3250 g of supernatant slurry. The recovered 3250 g of supernatant slurry was mixed and then 460 g was collected. The collected supernatant slurry (460 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 130 minutes at 8800 rpm in an R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 250 g of the supernatant slurry containing fine particles was removed to obtain a precipitated slurry. The gravitational acceleration in the centrifugation treatment was 15000 G. The slurry on the precipitated side was subjected to the addition of 250 g of 0.065 mol / kg TMAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 130 minutes at 8800 rpm and 15000 G, and the removal of 250 g of the supernatant slurry, which were repeated 8 more times to obtain a precipitated slurry. 250 g of 0.065 mol / kg TMAOH aqueous solution was added to 210 g of the obtained precipitate side slurry, and then ultrasonic dispersion treatment was performed for 1 hour using an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), followed by centrifugation treatment for 70 minutes at a rotation speed of 8800 rpm using the R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 250 g of supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 15000 G. The operation of adding 250 g of 0.065 mol / kg TMAOH aqueous solution to the obtained precipitate side slurry, ultrasonic dispersion, centrifugation treatment for 70 minutes at 8800 rpm and 15000 G, and collecting 250 g of supernatant slurry was repeated 12 times to collect a total of 3250 g of supernatant slurry. A 1% by mass aqueous sulfuric acid solution was added to the recovered supernatant slurry to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then the mixture was filtered through a membrane filter. The solid content was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 18.

[0130] The coercive force of the obtained iron oxide magnetic powder is 349 (kA / m) and the saturation magnetization is 15.3 (Am 2 / kg), squareness ratio is 0.643, SFD is 0.71, I L / I H The value of was 0.15. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 15.8 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.0%, the number ratio of particles with a particle diameter of 20 nm or more was 1.4%, the coefficient of variation (CV value) was 12%, and the average circularity of the particles was 0.975. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0131] [Example 19] As the raw material solution, 2586 g of an aqueous solution with Fe(III) concentration of 1.000 mol / kg, Ga(III) concentration of 0.349 mol / kg, Co(II) concentration of 0.061 mol / kg, chloride ion concentration of 3.001 mol / kg, and nitrate ion concentration of 1.199 mol / kg was prepared. Next, 4735 g of an aqueous solution with Fe(III) concentration of 0.182 mol / kg and chloride ion concentration of 0.546 mol / kg was placed in a 10 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.894 mol / kg ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at a rate of 10.8 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at a rate of 10.8 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.93 equivalents. The pH of the resulting colloidal solution was 2.1. Next, 866 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 582 g of ammonia solution with a concentration of 12.465 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 582 g of ammonia solution all at once was 8.6.

[0132] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 150 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 30.2 nm. Next, 1299 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1680 g. The temperature was adjusted to 40°C while stirring, 2085 g of 2-propanol was added and stirred for 5 minutes, after which 1029 g of 21.24 mass% aqueous ammonia was added. Furthermore, 3936 g of tetraethoxysilane (TEOS) was added over 35 minutes as a silicon compound having a hydrolyzable group. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0133] The cake obtained in step 4 (the precursor coated with the gel-like hydrolysis product) was dried, and then the dried powder was heat-treated in a furnace in an air atmosphere at 1060°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 80°C and stirred for 20 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites have been substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦1 mS / m.

[0134] Next, 35% by mass of TEAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a surface modifier-containing slurry with a solid content of 35.0%. The amount of TEAOH aqueous solution added was set so that the TEAOH concentration in the surface modifier-containing slurry was 0.099 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (460 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 130 minutes at 8800 rpm in the R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 250 g of the supernatant slurry containing fine particles was removed to obtain a slurry on the precipitate side. The gravitational acceleration in the centrifugation treatment was 15000 G. The slurry on the precipitate side was further subjected to the addition of 250 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 130 minutes at 8800 rpm and 15000 G, and the removal of 250 g of the supernatant slurry, which were then repeated 15 times to obtain a slurry on the precipitate side. 250 g of 0.099 mol / kg TEAOH aqueous solution was added to 210 g of the obtained precipitate side slurry, and then ultrasonic dispersion treatment was performed for 1 hour using an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifugal separation treatment was performed for 60 minutes at a rotation speed of 8800 rpm using the R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 250 g of supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 15000 G. The operation of adding 250 g of 0.099 mol / kg TEAOH aqueous solution to the obtained precipitate side slurry, ultrasonic dispersion, centrifugal separation treatment for 60 minutes at 8800 rpm and 15000 G, and collecting 250 g of supernatant slurry was repeated 12 times to collect a total of 3250 g of supernatant slurry. The recovered supernatant slurry was added with 1 mass % aqueous sulfuric acid solution to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then filtered through a membrane filter. The solid content was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 19.

[0135] The coercive force of the obtained iron oxide magnetic powder is 353 (kA / m) and the saturation magnetization is 15.8 (Am 2 / kg), squareness ratio is 0.620, SFD is 0.84, I L / I HThe value of was 0.33. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 16.7 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.0%, the number ratio of particles with a particle diameter of 20 nm or more was 5.9%, the coefficient of variation (CV value) was 12%, and the average circularity of the particles was 0.970. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles.

[0136] [Example 20] As the raw material solution, 2586 g of an aqueous solution with Fe(III) concentration of 1.099 mol / kg, Ga(III) concentration of 0.184 mol / kg, Co(II) concentration of 0.061 mol / kg, Ti(IV) concentration of 0.044 mol / kg, chloride ion concentration of 3.408 mol / kg, and nitrate ion concentration of 0.673 mol / kg was prepared. Next, 4757 g of an aqueous solution with Fe(III) concentration of 0.198 mol / kg and chloride ion concentration of 0.594 mol / kg was placed in a 10 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.885 mol / kg ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material aqueous solution was added continuously at a rate of 10.7 g / min over 240 minutes, and the ammonia aqueous solution was added continuously at a rate of 10.7 g / min over 240 minutes. During the addition of the raw material aqueous solution and the ammonia aqueous solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.95 equivalents. The pH of the resulting colloidal solution was 1.9. Next, 866 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 573 g of ammonia solution with a concentration of 12.553 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 573 g of ammonia solution all at once was 8.6.

[0137] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 150 mS / m or less (step 3). The DLS average diameter of the precursor particles contained in the washed slurry obtained in step 3 was measured and found to be 30.8 nm. Next, 1220 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1680 g. The temperature was adjusted to 40°C while stirring, 2085 g of 2-propanol was added and stirred for 5 minutes, after which 1022 g of 21.39 mass% aqueous ammonia was added. Furthermore, 3936 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0138] The cake obtained in step 4 (precursor coated with gel-like hydrolysis product) was dried, and then the dried powder was heat-treated in an air furnace at 1062°C for 4 hours to obtain iron oxide powder containing a substituted metal element coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The iron oxide powder containing the substituted metal element coated with silicon oxide obtained in step 5 was placed in a 20 mass% NaOH aqueous solution at 80°C and stirred for 20 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which some of the Fe sites have been substituted with other metal elements (step 6). The slurry obtained in step 6 was washed until the conductivity was ≦1 mS / m.

[0139] Next, 35% by mass of TEAOH aqueous solution was added as a surface modifier to the washed slurry to obtain a surface modifier-containing slurry with a solid content of 40.0%. The amount of TEAOH aqueous solution added was set so that the TEAOH concentration in the surface modifier-containing slurry was 0.099 mol / kg. In this case, the pH of the slurry became 13. The obtained surface modifier-containing slurry (460 g) was subjected to ultrasonic dispersion treatment for 1 hour in an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifuged for 130 minutes at 8800 rpm in the R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 250 g of the supernatant slurry containing fine particles was removed to obtain a slurry on the precipitate side. The gravitational acceleration in the centrifugation treatment was 15000 G. The slurry on the precipitate side was subjected to the addition of 250 g of 0.099 mol / kg TEAOH aqueous solution, ultrasonic dispersion, centrifugation treatment for 130 minutes at 8800 rpm and 15000 G, and the removal of 250 g of the supernatant slurry, which were repeated 9 more times, to obtain a slurry on the precipitate side. 250 g of 0.099 mol / kg TEAOH aqueous solution was added to 210 g of the obtained precipitate side slurry, and then ultrasonic dispersion treatment was performed for 1 hour using an ultrasonic cleaner (Yamato 5510, manufactured by Branson (Yamato Scientific) Co., Ltd.), and then centrifugal separation treatment was performed for 60 minutes at a rotation speed of 8800 rpm using the R10A3 rotor of a centrifuge (himac CR21GII, manufactured by Hitachi Koki Co., Ltd.), and 250 g of supernatant slurry was collected. The gravitational acceleration in the centrifugation treatment was 15000 G. The operation of adding 250 g of 0.099 mol / kg TEAOH aqueous solution to the obtained precipitate side slurry, ultrasonic dispersion, centrifugal separation treatment for 60 minutes at 8800 rpm and 15000 G, and collecting 250 g of supernatant slurry was repeated 12 times to collect a total of 3250 g of supernatant slurry. A 1% by mass aqueous sulfuric acid solution was added to the recovered supernatant slurry to adjust the pH to 6.5 to aggregate the substituted ε iron oxide particles, and then the mixture was filtered through a membrane filter. The solid content was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 20.

[0140] The coercive force of the obtained iron oxide magnetic powder is 327 (kA / m) and the saturation magnetization is 15.4 (Am 2 / kg), squareness ratio is 0.628, SFD is 0.97, I L / I H The value of was 0.25. The obtained iron oxide magnetic powder was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped onto a collodion film on a grid and allowed to adhere, then naturally dried, carbon deposition was performed, and the result was subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 17.3 nm, the number ratio of particles with a particle diameter of 8 nm or less was 0.0%, the number ratio of particles with a particle diameter of 20 nm or more was 12.9%, the coefficient of variation (CV value) was 14%, and the average circularity of the particles was 0.969. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles. The above measurement results are shown in Tables 3 and 4.

[0141] [Table 1]

[0142]

Table 2

[0143]

Table 3

[0144]

Table 4

Claims

1. An iron-based oxide magnetic powder consisting of particles of ε-iron oxide or ε-iron oxide in which part of the Fe sites has been substituted with other metal elements, the particles having an average particle diameter of 10 nm or more and 20 nm or less as measured by a transmission electron microscope, the number ratio of particles having a particle diameter of 8 nm or less being 3% or less and the number ratio of particles having a particle diameter of 20 nm or more being 25% or less, the average circularity of the particles being 0.955 or more as measured by a transmission electron microscope, and the coefficient of variation of the particle diameters as measured by a transmission electron microscope being 19% or less.

2. 2. The iron-based oxide magnetic powder according to claim 1, wherein the metal element substituting a portion of the Fe sites is one or more of Ga, Co and Ti.

3. 2. The iron-based oxide magnetic powder according to claim 1, wherein the metal element substituting a portion of the Fe sites is one or more of Ga, Co, Ti, Ni, Mn, Cr, Nd, Dy and Gd.

4. A method for producing an iron-based oxide magnetic powder comprising particles of ε-iron oxide or ε-iron oxide in which a portion of the Fe site is substituted with another metal element, comprising the steps of: a raw material solution preparation step of preparing a raw material solution containing trivalent iron ions, or trivalent iron ions and ions of a metal element that partially substitutes the Fe site, and an alkaline aqueous solution for neutralizing the raw material solution; a first neutralization step of continuously or intermittently adding and mixing the raw material solution and the aqueous alkaline solution to a reaction system to adjust the pH of the reaction system to 1.0 or more and 3.0 or less; adding a hydroxycarboxylic acid to the aqueous solution after the first neutralization step; a second neutralization step of adding an alkali to the aqueous solution containing the hydroxycarboxylic acid to neutralize the pH to 7.0 or more and 10.0 or less to obtain a slurry containing a precipitate of iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element; a step of adding a silicon compound having a hydrolyzable group to a slurry containing the iron oxyhydroxide or the iron oxyhydroxide containing a substitution metal element, and coating the iron oxyhydroxide or the iron oxyhydroxide containing a substitution metal element with a hydrolysis product of the silicon compound; a step of heating the iron oxyhydroxide containing a substituted metal element and coated with the hydrolysis product of the silicon compound to obtain epsilon iron oxide coated with silicon oxide or epsilon iron oxide in which a part of the Fe site is substituted with another metal element; removing silicon oxide from the silicon oxide-coated ε-iron oxide or ε-iron oxide having a portion of the Fe sites substituted with another metal element to obtain a slurry containing ε-iron oxide or ε-iron oxide having a portion of the Fe sites substituted with another metal element; a step of adding a quaternary ammonium salt having a concentration of 0.009 mol / kg or more and 1.0 mol / kg or less as a surface modifier to a slurry containing the ε-iron oxide or the ε-iron oxide in which a part of the Fe sites is substituted with another metal element, and adjusting the pH to 11.0 or more and 14.0 or less; a step of subjecting the slurry containing the surface modifier to a dispersion treatment to obtain a dispersion slurry of ε-iron oxide particles or ε-iron oxide particles in which a part of the Fe sites is substituted with another metal element; a step of classifying a slurry of dispersed particles of the ε-iron oxide or the ε-iron oxide having a part of the Fe sites substituted with another metal element; The method for producing the iron-based oxide magnetic powder according to claim 1, comprising:

5. 5. The method for producing an iron-based oxide magnetic powder according to claim 4, wherein the first neutralization step comprises continuously or intermittently adding and mixing the raw material solution and the aqueous alkaline solution containing 0.4 equivalents or more and 0.9 equivalents or less of alkali relative to the sum of the amounts of acid radicals contained in the raw material solution to a reaction system not containing trivalent iron ions and ions of metal elements substituting a portion of the Fe sites, to adjust the pH of the reaction system to 1.0 or more and 3.0 or less.

6. 5. The method for producing an iron-based oxide magnetic powder according to claim 4, wherein the first neutralization step comprises continuously or intermittently adding the raw material solution and the alkaline aqueous solution to a reaction system already containing trivalent iron ions, or trivalent iron ions and ions of a metal element substituting a portion of the Fe sites, such that the amount of trivalent iron ions and ions of a metal element already contained in the reaction system is 50 mol % or less of the sum of the amount of the trivalent iron ions and ions of a metal element substituting a portion of the Fe sites and the amount of the trivalent iron ions and ions of a metal element substituting a portion of the Fe sites contained in the raw material solution added to the reaction system, and continuously or intermittently adding and mixing the raw material solution and the alkaline aqueous solution containing 0.4 equivalents to 1.8 equivalents of alkali with respect to the sum of the amounts of acid radicals contained in the raw material solution to the reaction system, and adjusting the pH of the reaction system to 1.0 to 3.

0.

7. 6. The method for producing an iron-based oxide magnetic powder according to claim 5, wherein in the first neutralization step, the addition rates of the raw material solution and the aqueous alkaline solution are adjusted to maintain the cumulative addition amount of the alkali relative to the total cumulative addition amount of the acid radicals contained in the raw material solution in the range of 0.4 equivalents or more and 0.9 equivalents or less throughout the step.

8. 5. The method for producing an iron-based oxide magnetic powder according to claim 4, wherein in the first neutralization step, the raw material solution and the alkaline aqueous solution are added over a period of 10 minutes or more.

9. 5. The method for producing an iron-based oxide magnetic powder according to claim 4, wherein the slurry containing the iron oxyhydroxide or the iron oxyhydroxide containing a substituted metal element obtained in the second neutralization step has an average particle size of 300 nm or less as measured by a dynamic light scattering particle size distribution analyzer.

10. 5. The method for producing an iron-based oxide magnetic powder according to claim 4, wherein iron (III) chloride is used as a source of the trivalent iron ions contained in the raw material solution.

11. 6. The method for producing an iron-based oxide magnetic powder according to claim 5, wherein the cumulative amount of alkali added relative to the total cumulative amount of acid radicals added contained in the raw material solution is 0.6 equivalents or more and 0.9 equivalents or less through the first neutralization step.

12. 7. The method for producing an iron-based oxide magnetic powder according to claim 6, wherein the cumulative amount of alkali added relative to the total cumulative amount of acid radicals added contained in the raw material solution is 0.4 equivalents or more and 1.8 equivalents or less through the first neutralization step.

Citation Information

Patent Citations

  • epsi-IRON OXIDE POWDER HAVING IMPROVED MAGNETIC PROPERTY

    JP2008063201A

  • METHOD FOR PRODUCING epsilon-Fe2O3 CRYSTAL

    JP2008174405A

  • Ferrous oxide magnetic particle powder, method for manufacturing the same, coating material, and magnetic recording medium

    JP2016130208A

  • Manufacturing method of iron-based oxide magnetic particle powder

    JP2017024981A

  • Core shell particle, baked product of core shell particle, method of producing core shell particle, epsilon type iron oxide compound particle, method of producing epsilon type iron oxide compound particle, magnetic recording medium, and method of producing magnetic recording medium

    JP2019001663A