Multilayer Ceramic Capacitors

The multilayer ceramic capacitor addresses cracking and chipping issues by employing a specific layer arrangement and varying dielectric ceramic compositions, enhancing reliability through stress reduction.

JP7575913B2Active Publication Date: 2024-10-30MURATA MFG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020186019
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-11-06
Publication Date
2024-10-30
Estimated Expiration
2040-11-06

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors face issues with cracking or chipping of dielectric ceramic layers due to stress during firing, particularly when optimizing the composition of dielectric laminate sheets and ceramic pastes for eliminating step differences.

Method used

The multilayer ceramic capacitor design includes a specific arrangement of dielectric ceramic layers and internal electrode layers, with alternating layers and external electrodes connected to internal electrode layers, and the use of different compositions for dielectric ceramic layers to enhance reliability and reduce stress-induced cracking.

Benefits of technology

This design effectively suppresses cracking and chipping of dielectric ceramic layers, improving the reliability and performance of the multilayer ceramic capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575913000006
    Figure 0007575913000006
  • Figure 0007575913000007
    Figure 0007575913000007
  • Figure 0007575913000008
    Figure 0007575913000008
Patent Text Reader

Abstract

To provide a multilayer ceramic capacitor which can suppress a dielectric ceramic layer arranged for the purpose of eliminating a step from being cracked or chipped by at least a stress to be produced in sintering.SOLUTION: The multilayer ceramic capacitor has a defective part in at least one of a region between an end of a first internal electrode layer which is not connected to a second external electrode and the second external electrode in a length direction, and a region between an end of a second internal electrode layer which is not connected to a first external electrode and the first external electrode; in a plane involving a lamination direction and a width direction, the location of the defective part is between first dielectric ceramic layers in the lamination direction, and the location is between a second dielectric ceramic layer and a third dielectric ceramic layer in the width direction.SELECTED DRAWING: Figure 28
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer ceramic capacitor. [Background technology]

[0002] In recent years, efforts have been made to reduce the size and increase the capacity of multilayer ceramic electronic components such as multilayer ceramic capacitors. In order to achieve a reduction in size and an increase in capacity of a multilayer ceramic capacitor, it is effective to increase the areas of the mutually opposing internal electrode layers by thinning the side margins on each side of a laminate in which a plurality of dielectric ceramic layers and a plurality of internal electrode layers are laminated.

[0003] Patent Document 1 discloses a method for manufacturing an electronic component, comprising the steps of preparing a chip including a plurality of laminated dielectric ceramic layers and a plurality of internal electrode layers, with the plurality of internal electrode layers exposed on the side surfaces, bonding a plurality of covering dielectric sheets together to form a dielectric laminate sheet, and attaching the dielectric laminate sheet to the side surfaces of the chip.

[0004] Furthermore, Patent Document 2 discloses that when a multilayer ceramic capacitor is manufactured by stacking a plurality of ceramic green sheets on which internal electrodes are printed, pressing and firing the sheets, a step-eliminating ceramic slurry can be applied to areas on which the internal electrodes are not printed, thereby preventing steps from occurring between areas where the internal electrodes overlap and areas where they do not overlap. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-147358 A [Patent Document 2] JP 2003-209025 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, there is no particular mention in Cited Document 1 of the composition of the ceramic dielectric sheets to be attached to the side surfaces of the laminate. There is also no particular mention of the composition of the ceramic paste for elimination of steps used in Cited Document 2. Therefore, Cited Documents 1 and 2 leave room for improving the reliability of the multilayer ceramic capacitor by optimizing the compositions of the dielectric laminate sheets and the ceramic paste for elimination of steps. Furthermore, when a dielectric ceramic layer is provided between the stacked internal electrode layers, such as the dielectric ceramic layer made of the step-eliminating ceramic slurry described in Reference 2, the dielectric ceramic layer may crack or chip due to stress generated during firing.

[0007] An object of the present invention is to provide a multilayer ceramic capacitor capable of suppressing the occurrence of cracks or chips in the dielectric ceramic layers for eliminating steps due to stress at least during firing. [Means for solving the problem]

[0008] The multilayer ceramic capacitor of the present invention is a multilayer ceramic capacitor comprising a laminate including dielectric ceramic layers and internal electrode layers laminated in a lamination direction, and external electrodes connected to the internal electrode layers, the laminate having a first main surface and a second main surface opposing each other in the lamination direction, a first side surface and a second side surface opposing each other in a width direction perpendicular to the lamination direction, and a first end surface and a second end surface opposing each other in a length direction perpendicular to the lamination direction and the width direction, and the internal electrode layers have a first inner conductor extending to the first end surface. and a second internal electrode layer extending to the second end face so as to face the first internal electrode layer via the dielectric ceramic layer, the external electrode including a first external electrode disposed on the first end face and connected to the first internal electrode layer, and a second external electrode disposed on the second end face and connected to the second internal electrode layer, the dielectric ceramic layer being made of a first dielectric ceramic layer and a second dielectric ceramic layer, the first dielectric ceramic layer being made of a first internal electrode layer and a second internal the second dielectric ceramic layer is disposed between the first dielectric ceramic layers, the second dielectric ceramic layer including a region between the first dielectric ceramic layers opposed to each other via the internal electrode layer where the internal electrode layer is not disposed, and a part of the second dielectric ceramic layer is disposed so as to overlap the first dielectric ceramic layer in the stacking direction; the laminate has an inner layer portion in which the first internal electrode layers and the second internal electrode layers are alternately stacked via the dielectric ceramic layers, an outer layer portion which is disposed so as to sandwich the inner layer portion in the stacking direction and is made of a ceramic material, and a third dielectric ceramic layer which is disposed so as to sandwich the inner layer portion and the outer layer portion in the width direction and is made of a dielectric ceramic material, and in the length direction, in at least one region between an end portion of the first internal electrode layer not connected to the second external electrode and the second external electrode, and between an end portion of the second internal electrode layer not connected to the first external electrode and the first external electrode, a position in the stacking direction is between the first dielectric ceramic layers in a plane including the stacking direction and the width direction,At the position in the width direction, there is a missing portion between the second dielectric ceramic layer and the third dielectric ceramic layer. Effect of the Invention

[0009] According to the present invention, it is possible to provide a multilayer ceramic capacitor capable of suppressing the occurrence of cracks or chips in the dielectric ceramic layers for elimination of steps due to stress during firing. [Brief description of the drawings]

[0010] [Figure 1] 1 is a perspective view illustrating an example of a multilayer ceramic capacitor according to the present invention. [Diagram 2] 2 is a perspective view showing a schematic diagram of an example of a laminate constituting the multilayer ceramic capacitor shown in FIG. 1. [Diagram 3] 2 is a cross-sectional view taken along line AA of the multilayer ceramic capacitor shown in FIG. [Figure 4] 2 is a cross-sectional view of the multilayer ceramic capacitor shown in FIG. 1 taken along line CC. [Diagram 5] 2 is a cross-sectional view of the multilayer ceramic capacitor shown in FIG. 1 along line BB. [Figure 6] FIG. 2 is a plan view illustrating an example of a ceramic green sheet. [Figure 7] FIG. 2 is a plan view illustrating an example of a ceramic green sheet. [Figure 8] FIG. 2 is a plan view illustrating an example of a ceramic green sheet. [Figure 9] FIG. 2 is an exploded perspective view illustrating an example of a mother block. [Figure 10] FIG. 2 is a perspective view showing a schematic diagram of an example of a green chip. [Figure 11] FIG. 2 is a diagram showing a part of an LT cross section of the multilayer ceramic capacitor of the present invention, and is a schematic diagram showing a first alloy portion and a second alloy portion. [Figure 12] FIG. 12 is a partially enlarged view of FIG. [Figure 13]1 is a diagram showing a part of an LT cross section of a multilayer ceramic capacitor of the present invention, and is a schematic diagram showing a first interspersed internal electrode, a second interspersed internal electrode, and a fourth alloy portion. [Figure 14] FIG. 2 is a diagram showing a part of a WT cross section of the multilayer ceramic capacitor of the present invention, which diagrammatically shows a first alloy portion and a third alloy portion. [Figure 15] FIG. 15 is a partially enlarged view of FIG. 14, showing a schematic diagram of a fifth alloy part. [Figure 16] 3 is a cross-sectional view showing a schematic configuration in which an end of a second dielectric ceramic layer overlaps an end of an internal electrode layer in the multilayer ceramic capacitor of the present invention. FIG. [Figure 17] 3 is a cross-sectional view showing a schematic configuration in which an end of a second dielectric ceramic layer overlaps an end of an internal electrode layer in the multilayer ceramic capacitor of the present invention. FIG. [Figure 18] FIG. 2 is a diagram for explaining a TEM analysis method for analyzing the amounts of metal elements contained in the internal electrode layers of the multilayer ceramic capacitor of the present invention. [Figure 19] FIG. 6 is a diagram showing a part of FIG. 5 and a vicinity of an intersection point of the present invention. [Figure 20] FIG. 4 is a diagram for explaining a method for measuring the average particle size of dielectric particles contained in the first dielectric ceramic layer and the third dielectric ceramic layer. [Figure 21] FIG. 4 is a diagram for explaining a method for measuring the average particle size of dielectric particles contained in the third dielectric ceramic layer. [Figure 22] FIG. 4 is a diagram for explaining a first step of a method for measuring the average particle size of dielectric particles contained in the second dielectric ceramic layer and the region in the vicinity of the intersection points. [Diagram 23] FIG. 11 is a diagram for explaining a second step of the method for measuring the average particle size of dielectric particles contained in the second dielectric ceramic layer and the regions in the vicinity of the intersections. [Figure 24] FIG. 13 is a diagram for explaining a method for measuring the average particle size of dielectric particles contained in the region near the intersection point. [Diagram 25]4A to 4C are diagrams each showing a schematic diagram of a step of removing a side surface of an unfired laminate in a method for producing a multilayer ceramic capacitor according to the present invention. [Figure 26] 3 is a diagram showing an end face of an unsintered laminate from which a side surface has been removed in a method for producing a multilayer ceramic capacitor according to the present invention. FIG. [Figure 27] 3 is a cross-sectional view showing a schematic configuration in which an end portion of a second dielectric ceramic layer is overlapped on an end portion of an internal electrode layer in a manufacturing method of a multilayer ceramic capacitor according to the present invention. FIG. [Figure 28] 3 is a diagram showing a part of a WT cross section of the multilayer ceramic capacitor of the present invention, and is a schematic diagram showing a defective portion of a second dielectric ceramic layer. FIG. [Figure 29] 29 is a cross-sectional view taken along line KK in FIG. 28. [Diagram 30] FIG. 2 is a diagram showing a part of an LT cross section of the multilayer ceramic capacitor of the present invention, and is a schematic diagram showing a first segregation. [Diagram 31] FIG. 31 is a partially enlarged view of FIG. 30. [Diagram 32] 4 is a diagram showing a part of a WT cross section of the multilayer ceramic capacitor of the present invention, and is a schematic diagram showing a second segregation. FIG. [Diagram 33] 13 is a diagram showing a part of an LW cross section of the multilayer ceramic capacitor of the present invention, illustrating a third segregation occurring in a first corner region and a second corner region. FIG. [Diagram 34] 4 is a cross-sectional view illustrating a mode in which an end portion of a second dielectric ceramic layer overlaps a third segregation in the multilayer ceramic capacitor of the present invention. FIG. [Diagram 35] 3 is a diagram showing the thickness of a first dielectric ceramic layer at the center in the length (L) direction of the multilayer ceramic capacitor of the present invention. FIG. [Diagram 36] FIG. 4 is a diagram showing the thickness of a second dielectric ceramic layer of the multilayer ceramic capacitor of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The multilayer ceramic capacitor of the present invention will now be described. However, the present invention is not limited to the following configurations, and can be modified as appropriate within the scope of the present invention. Note that the present invention also includes a combination of two or more of the individual desirable configurations described below.

[0012] [Multilayer ceramic capacitors] Fig. 1 is a perspective view showing an example of a multilayer ceramic capacitor of the present invention. Fig. 2 is a perspective view showing an example of a laminate constituting the multilayer ceramic capacitor shown in Fig. 1. Fig. 3 is a cross-sectional view taken along line AA of the multilayer ceramic capacitor shown in Fig. 1. Fig. 4 is a cross-sectional view taken along line CC of the multilayer ceramic capacitor shown in Fig. 1.

[0013] In this specification, the lamination direction, width direction, and length direction of the multilayer ceramic capacitor and laminate are defined as the directions indicated by arrows T, W, and L, respectively, in the multilayer ceramic capacitor 1 shown in Fig. 1 and the laminate 10 shown in Fig. 2. Here, the lamination (T) direction, width (W) direction, and length (L) direction are mutually perpendicular. The lamination (T) direction is the direction in which the multiple dielectric ceramic layers 20 and the multiple pairs of first internal electrode layers 21 and second internal electrode layers 22 are stacked.

[0014] The multilayer ceramic capacitor 1 shown in FIG. 1 includes a laminate 10, and a first external electrode 51 and a second external electrode 52 provided on both end faces of the laminate 10, respectively.

[0015] As shown in FIG. 2, the laminate 10 has a rectangular or approximately rectangular shape and has a first main surface 11 and a second main surface 12 facing each other in the stacking (T) direction, a first side surface 13 and a second side surface 14 facing each other in a width (W) direction perpendicular to the stacking (T) direction, and a first end surface 15 and a second end surface 16 facing each other in a length (L) direction perpendicular to the stacking (T) direction and the width (W) direction.

[0016] In this specification, a cross section of the multilayer ceramic capacitor 1 or the laminate 10 perpendicular to the first end face 15 and the second end face 16 and parallel to the lamination (T) direction is referred to as an LT cross section, which is a cross section in the length (L) direction and the lamination (T) direction. A cross section of the multilayer ceramic capacitor 1 or the laminate 10 perpendicular to the first side face 13 and the second side face 14 and parallel to the lamination (T) direction is referred to as a WT cross section, which is a cross section in the width (W) direction and the lamination (T) direction. A cross section of the multilayer ceramic capacitor 1 or the laminate 10 perpendicular to the first side face 13, the second side face 14, the first end face 15, and the second end face 16 and perpendicular to the lamination (T) direction is referred to as an LW cross section, which is a cross section in the length (L) direction and the width (W) direction. Therefore, FIG. 3 is an LT cross section of the multilayer ceramic capacitor 1, and FIG. 4 is a WT cross section of the multilayer ceramic capacitor 1.

[0017] It is preferable that the corners and ridges of the laminate 10 are rounded. A corner is a portion where three surfaces of the laminate intersect, and a ridge is a portion where two surfaces of the laminate intersect.

[0018] 2, 3 and 4, the laminate 10 has a laminated structure including a plurality of dielectric ceramic layers 20 laminated in a lamination (T) direction, and a plurality of pairs of first internal electrode layers 21 and second internal electrode layers 22 formed along the interfaces between the dielectric ceramic layers 20. The dielectric ceramic layers 20 extend in the width (W) and length (L) directions, and each of the first internal electrode layers 21 and second internal electrode layers 22 extends in a flat plate shape along the dielectric ceramic layers 20.

[0019] The first internal electrode layer 21 is extended to a first end face 15 of the laminate 10. On the other hand, the second internal electrode layer 22 is extended to a second end face 16 of the laminate 10.

[0020] The first internal electrode layer 21 and the second internal electrode layer 22 face each other in the stacking (T) direction via the dielectric ceramic layer 20. A capacitance is generated by the portion where the first internal electrode layer 21 and the second internal electrode layer 22 face each other via the dielectric ceramic layer 20.

[0021] Each of the first internal electrode layer 21 and the second internal electrode layer 22 preferably contains a metal such as Ni, Cu, Ag, Pd, an Ag-Pd alloy, Au, etc. Each of the first internal electrode layer 21 and the second internal electrode layer 22 may contain the same dielectric ceramic material as the dielectric ceramic layer 20 in addition to the above metals.

[0022] The dielectric ceramic layer 20 includes a first dielectric ceramic layer 20a and a second dielectric ceramic layer 20b. The first dielectric ceramic layer 20 a is a dielectric ceramic layer disposed between the first internal electrode layer 21 and the second internal electrode layer 22 . The second dielectric ceramic layer 20b is a dielectric ceramic layer disposed between the first dielectric ceramic layers 20a opposing each other via the internal electrode layers (21, 22) in a region where the internal electrode layers (21, 22) are not disposed.

[0023] The first external electrode 51 is provided on a first end face 15 of the laminate 10, and in Fig. 1 has a portion that extends around each of the first main face 11, the second main face 12, the first side face 13, and the second side face 14. The first external electrode 51 is connected to the first internal electrode layer 21 at the first end face 15.

[0024] The second external electrode 52 is provided on the second end face 16 of the laminate 10, and in Fig. 1 has a portion that extends around each of the first main face 11, the second main face 12, the first side face 13, and the second side face 14. The second external electrode 52 is connected to the second internal electrode layer 22 at the second end face 16.

[0025] Each of the first external electrode 51 and the second external electrode 52 preferably includes a Ni layer containing Ni and a ceramic material. The Ni layer is a base electrode layer. Such a Ni layer can be formed by a so-called co-firing method in which the Ni layer is fired simultaneously with the first internal electrode layer 21 and the second internal electrode layer 22. The Ni layer is preferably disposed directly on the laminate 10.

[0026] The first external electrode 51 preferably includes, in order from the first end face 15 side of the laminate 10, a Ni layer, a first plating layer, and a second plating layer. Similarly, the second external electrode 52 preferably includes, in order from the second end face 16 side of the laminate 10, a Ni layer, a first plating layer, and a second plating layer. The first plating layer is preferably formed by Ni plating, and the second plating layer is preferably formed by Sn plating. The first external electrode 51 and the second external electrode 52 may each include a conductive resin layer containing conductive particles and resin between the Ni layer and the first plating layer. Examples of conductive particles in the conductive resin layer include metal particles such as Cu, Ag, and Ni.

[0027] The Ni layer may be formed by a so-called post-fire method in which a conductive paste is applied to the end face of the fired laminate and then baked. In this case, the Ni layer does not need to contain a ceramic material.

[0028] Alternatively, each of the first external electrode 51 and the second external electrode 52 may include an underlying electrode layer containing a metal such as Cu. The underlying electrode layer may be formed by a co-firing method or a post-firing method. The underlying electrode layer may be a multi-layer structure.

[0029] For example, the first external electrode 51 may have a four-layer structure including, in order from the first end face 15 side of the laminate 10, a Cu layer serving as a base electrode layer, a conductive resin layer containing conductive particles and resin, a first plating layer, and a second plating layer. Similarly, the second external electrode 52 may have a four-layer structure including, in order from the second end face 16 side of the laminate 10, a Cu layer serving as a base electrode layer, a conductive resin layer containing conductive particles and resin, a first plating layer, and a second plating layer.

[0030] As shown in FIGS. 3 and 4, the dielectric ceramic layer 20 includes a first dielectric ceramic layer 20a and a second dielectric ceramic layer 20b. The first dielectric ceramic layer 20 a is disposed between the first internal electrode layer 21 and the second internal electrode layer 22 . The second dielectric ceramic layer 20b is disposed between the first dielectric ceramic layers 20a facing each other with the internal electrode layer interposed therebetween, in a region where no internal electrode layer is disposed.

[0031] 2, 3 and 4, the laminate 10 includes an inner layer portion 30 in which a first internal electrode layer 21 and a second internal electrode layer 22 face each other via a dielectric ceramic layer 20, outer layer portions 31 and 32 arranged to sandwich the inner layer portion 30 in the stacking (T) direction, and third dielectric ceramic layers 41 and 42 arranged to sandwich the inner layer portion 30, the outer layer portion 31 and the outer layer portion 32 in the width (W) direction. The third dielectric ceramic layers 41 and 42 are also called side margin portions. 3 and 4, the inner layer portion 30 is a region sandwiched along the stacking (T) direction between the first internal electrode layer 21 closest to the first main surface 11 and the first internal electrode layer 21 closest to the second main surface 12. Although not shown, each of the outer layer portions 31 and 32 is preferably composed of a plurality of dielectric ceramic layers 20 stacked in the stacking (T) direction, and more preferably composed of a first dielectric ceramic layer 20a.

[0032] The thickness of each of the outer layer portions 31 and 32 is preferably 15 μm or more and 40 μm or less. Each of the outer layer portions 31 and 32 may have a single layer structure instead of a multilayer structure.

[0033] As shown in FIG. 4, each of the third dielectric ceramic layer 41 and the third dielectric ceramic layer 42 may be composed of a plurality of dielectric ceramic layers stacked in the width (W) direction. Among the multiple dielectric ceramic layers constituting the third dielectric ceramic layer, the innermost layer in the width direction is called the inner layer, and the outermost layer is called the outer layer. An interface exists between the inner layer and the outer layer. 4, the third dielectric ceramic layer 41 has a two-layer structure including, as the dielectric ceramic layer, an inner layer 41a arranged on the innermost side of the laminate 10 and an outer layer 41b arranged on the outermost side of the laminate 10. Similarly, the third dielectric ceramic layer 42 has a two-layer structure including, as the dielectric ceramic layer, an inner layer 42a arranged on the innermost side of the laminate 10 and an outer layer 42b arranged on the outermost side of the laminate 10. The third dielectric ceramic layer is not limited to a two-layer structure, and may be a three-layer or more structure. When the third dielectric ceramic layer includes three or more dielectric ceramic layers, the dielectric ceramic layer arranged on the innermost side in the width direction is defined as an inner layer, and the dielectric ceramic layer arranged on the outermost side in the width direction is defined as an outer layer. Furthermore, the number of third dielectric ceramic layers on the first side surface of the laminate may be different from the number of third dielectric ceramic layers on the second side surface of the laminate.

[0034] When the third dielectric ceramic layer has a two-layer structure including an inner layer and an outer layer, the difference in sinterability between the inner layer and the outer layer can be observed under a dark field optical microscope to confirm that the layer has a two-layer structure and the interface between the layers. The same applies when the third dielectric ceramic layer has a structure of three or more layers.

[0035] The first dielectric ceramic layer 20a, the second dielectric ceramic layer 20b and the third dielectric ceramic layers 41 and 42 are made of a dielectric ceramic material mainly composed of BaTiO3, etc. The dielectric ceramic layer 20 constituting the inner layer portion 30 may further contain a sintering aid element.

[0036] The dielectric ceramic layers constituting the first dielectric ceramic layer, the second dielectric ceramic layer and the third dielectric ceramic layer may include ceramic grains, the diameter of which will be described in detail later.

[0037] In the multilayer ceramic capacitor of the present invention, the composition of at least one of the first, second and third dielectric ceramic layers is different from the composition of the other dielectric ceramic layers. Since the first dielectric ceramic layer, the second dielectric ceramic layer, and the third dielectric ceramic layer all have different purposes for which they are placed and different properties required for their manufacturing methods, by making the composition of at least one of the first dielectric ceramic layer, the second dielectric ceramic layer, and the third dielectric ceramic layer different from the composition of the other dielectric ceramic layers, it is possible to achieve an optimal composition according to the location where the dielectric ceramic layer is placed, and thereby improve reliability.

[0038] In the multilayer ceramic capacitor of the present invention, the composition of the first dielectric ceramic layer may be different from the compositions of the second dielectric ceramic layer and the third dielectric ceramic layer, the composition of the second dielectric ceramic layer may be different from the compositions of the first dielectric ceramic layer and the third dielectric ceramic layer, the composition of the third dielectric ceramic layer may be different from the compositions of the first dielectric ceramic layer and the second dielectric ceramic layer, or the compositions of the first dielectric ceramic layer, the second dielectric ceramic layer and the third dielectric ceramic layer may be different from each other.

[0039] In the multilayer ceramic capacitor of the present invention, it is preferable that the composition of the second dielectric ceramic layer is different from the composition of the third dielectric ceramic layer, and it is more preferable that the compositions of the first dielectric ceramic layer, the second dielectric ceramic layer and the third dielectric ceramic layer are all different.

[0040] In addition, when the third dielectric ceramic layer is composed of a plurality of dielectric ceramic layers, the plurality of dielectric ceramic layers constituting the third dielectric ceramic layer may have the same composition or different compositions. When the composition of any one of the multiple dielectric ceramic layers constituting the third dielectric ceramic layer is different from that of the first dielectric ceramic layer, it can be said that the composition of the third dielectric ceramic layer is different from the composition of the first dielectric ceramic layer. Furthermore, when the composition of any one of the multiple dielectric ceramic layers constituting the third dielectric ceramic layer is different from that of the second dielectric ceramic layer, it can be said that the composition of the third dielectric ceramic layer is different from the composition of the second dielectric ceramic layer.

[0041] Of the first, second and third dielectric ceramic layers, the dielectric ceramic layers having different compositions preferably have a common main component but different types of additives. The main components include BaTiO3, CaTiO3, SrTiO3, and the like. Additives include elements such as Si, Mg, Mn, Sn, Cu, rare earths, Ni and Al. It is preferable. The first dielectric ceramic layer, the second dielectric ceramic layer and the third dielectric ceramic layer may contain two or more of the above elements.

[0042] Here, "the same composition" means that the types of elements contained in the dielectric ceramic that constitutes each dielectric ceramic layer are the same, and the contents (molar ratios) of other elements based on Ti are all within ±0.5%. It should be noted that differences in the diameter of the ceramic grains constituting each dielectric ceramic layer and differences in the porosity are not included in the differences in the composition of the dielectric ceramic layers.

[0043] The composition of each dielectric ceramic layer can be determined by cutting the multilayer ceramic capacitor to expose the dielectric ceramic layer and performing elemental analysis on the cut surface using wavelength dispersive X-ray analysis (WDX) or transmission electron microscope-energy dispersive X-ray analysis (TEM-EDX). At this time, the composition of each dielectric ceramic layer is measured at five points and the average value is calculated. For the second dielectric ceramic layer, the average value is obtained by measuring five locations on the second dielectric ceramic layer exposed on the first end face of the laminate and five locations on the second dielectric ceramic layer exposed on the second end face of the laminate. When the third dielectric ceramic layer has a multi-layer structure, the composition of each layer is measured at five locations, and the composition is multiplied by the proportion of the thickness of each layer in the third dielectric ceramic layer, and the total thickness is the sum of the results. If elemental segregation is observed near the interface with other dielectric ceramic layers or internal electrode layers, the location where elemental segregation is observed shall not be subject to WDX measurement.

[0044] The element added to the first dielectric ceramic layer is preferably Mg. The content of Mg in the first dielectric ceramic layer is preferably 0.05 mol % or more and 3.0 mol % or less with respect to 100 mol of Ti. More preferably, the Mg content in the first dielectric ceramic layer is lower than the Mg content in the second and third dielectric ceramic layers. When the Mg content in the first dielectric ceramic layers is low, the relative dielectric constant of the first dielectric ceramic layers is increased, and therefore the capacitance of the multilayer ceramic capacitor can be improved. In some cases, it is preferable that the Mg content in the first dielectric ceramic layers is as low as possible.

[0045] The element added to the second dielectric ceramic layer is preferably Sn. The content of Sn in the second dielectric ceramic layer is preferably 0.05 mol % or more and 3.0 mol % or less with respect to 100 mol of Ti. The Sn content in the second dielectric ceramic layer is preferably higher than the Sn content in the first dielectric ceramic layer and the third dielectric ceramic layer.

[0046] The element added to the third dielectric ceramic layer is preferably Si. The content of Si in the third dielectric ceramic layer is preferably 0.05 mol % or more and 5.0 mol % or less with respect to 100 mol of Ti. The Si content in the third dielectric ceramic layer is preferably higher than the Si content in the first and second dielectric ceramic layers. When the third dielectric ceramic layer has a high Si content, the sinterability of the dielectric ceramic layer is improved, thereby preventing moisture and the like from penetrating through the first and second side surfaces of the laminate and causing deterioration of the internal electrode layer.

[0047] The element added to the third dielectric ceramic layer is preferably Mg. The content of Mg in the third dielectric ceramic layer is preferably 0.05 mol % or more and 5.0 mol % or less with respect to 100 mol of Ti. The Mg content in the third dielectric ceramic layer is preferably higher than the Mg content in the first and second dielectric ceramic layers. When the third dielectric ceramic layer has a high Mg content, the grain growth of the ceramic grains contained in the third dielectric ceramic layer can be suppressed, making it difficult for short circuits to occur between the internal electrode layers.

[0048] The element added to the third dielectric ceramic layer is preferably Mn. The content of Mn in the third dielectric ceramic layer is preferably 0.01 mol % or more and 3.0 mol % or less with respect to 100 mol of Ti. The Mn content in the third dielectric ceramic layer is preferably higher than the Mn contents in the first and second dielectric ceramic layers. When the third dielectric ceramic layer has a high Mn content, the grain growth of the ceramic grains contained in the third dielectric ceramic layer can be suppressed, making it difficult for short circuits to occur between the internal electrode layers.

[0049] In the first, second and third dielectric ceramic layers, elements other than the main component contained in each of the dielectric ceramic layers are preferably diffused into the other dielectric ceramic layers. It is also preferable that a portion of the elements contained as additives in the first dielectric ceramic layer, the second dielectric ceramic layer and the third dielectric ceramic layer diffuse into the adjacent other dielectric ceramic layers and internal electrode layers.

[0050] FIG. 5 is a cross-sectional view of the multilayer ceramic capacitor shown in FIG. 1 taken along line BB. FIG. 5 is a LW cross section of the multilayer ceramic capacitor 1. 5, the second internal electrode layer 22 is exposed at the second end face 16 of the laminate 10, and the second dielectric ceramic layer 20b is exposed at the first end face 15 of the laminate 10. In addition, a third dielectric ceramic layer 41 and a third dielectric ceramic layer 42 are disposed on the first side face 13 and the second side face 14 of the laminate 10, respectively.

[0051] 5, an interface 2220b exists between the second internal electrode layer 22 and the second dielectric ceramic layer 20b. Furthermore, interfaces 2241 and 2242 exist between the second internal electrode layer 22 and the third dielectric ceramic layers 41 and 42. Furthermore, interfaces 20b41 and 20b42 exist between the second dielectric ceramic layer 20b and the third dielectric ceramic layers 41 and 42.

[0052] 5, the first dielectric ceramic layer 20a is disposed on both sides in the thickness direction of the second internal electrode layer 22 and the second dielectric ceramic layer 20b. Therefore, it can be said that the first dielectric ceramic layer 20a has interfaces in direct contact with the second dielectric ceramic layer 20b, the third dielectric ceramic layers 41, 42, and the internal electrode layers 21, 22.

[0053] Furthermore, like the second internal electrode layer 22 shown in FIG. 5, the first internal electrode layer 21 has interfaces with the first dielectric ceramic layer 20a, the second dielectric ceramic layer 20b, and the third dielectric ceramic layers 41, 42.

[0054] In the first dielectric ceramic layer 20a, elements derived from the second dielectric ceramic layer 20b may be segregated in the vicinity of the interface with the second dielectric ceramic layer 20b. In addition, in the first dielectric ceramic layer 20a, elements derived from the third dielectric ceramic layer 41 or 42 may be segregated in the vicinity of the interface with the third dielectric ceramic layer 41 or 42.

[0055] In the second dielectric ceramic layer 20b, elements derived from the first dielectric ceramic layer 20a may be segregated in the vicinity of the interface with the first dielectric ceramic layer 20a. In addition, in the second dielectric ceramic layer 20b, elements derived from the third dielectric ceramic layer 41 or 42 may be segregated in the vicinity of the interfaces 20b41, 20b42 with the third dielectric ceramic layer 41 or 42.

[0056] In the third dielectric ceramic layers 41 and 42, elements derived from the first dielectric ceramic layer 20a may be segregated near the interfaces with the first dielectric ceramic layer 20a. In addition, in the third dielectric ceramic layers 41 and 42, elements derived from the second dielectric ceramic layer 20b may be segregated near the interfaces 20b41 and 20b42 with the second dielectric ceramic layer 20b.

[0057] In the first internal electrode layer 21 and the second internal electrode layer 22, elements derived from the first dielectric ceramic layer 20a may be segregated near the interface with the first dielectric ceramic layer 20a. In addition, in the first internal electrode layer 21 and the second internal electrode layer 22, elements derived from the second dielectric ceramic layer 20b may be segregated near the interface 2220b with the second dielectric ceramic layer 20b. Furthermore, in the first internal electrode layer 21 and the second internal electrode layer 22, elements derived from the third dielectric ceramic layer 41, 42 may be segregated near the interfaces 2241, 2242 with the third dielectric ceramic layers 41, 42. In addition, in the vicinity of the portion where the interface 2220b between the second internal electrode layer 22 and the second dielectric ceramic layer 20b and the interface 2241 or 2242 between the second internal electrode layer 22 and the third dielectric ceramic layer 41 or 42 are in contact (the corner portion on the first end face 15 side of the second internal electrode layer 22), both elements derived from the second dielectric ceramic layer 20b and elements derived from the third dielectric ceramic layer 41 or 42 may be segregated.

[0058] The porosity of the first dielectric ceramic layer, the second dielectric ceramic layer and the third dielectric ceramic layer may be the same or different from each other. The multilayer ceramic capacitor is cut to expose each dielectric ceramic layer, and the cut surface is observed at 20,000x magnification using a scanning electron microscope (SEM). An area with a field of view size of 6.3 μm x 4.4 μm is photographed at five locations so that the areas do not overlap, and the ratio of the area occupied by voids to the entire field of view is calculated as the porosity using image analysis of each obtained SEM image, and the average value for the five fields of view is calculated. However, if the third dielectric ceramic layer is composed of multiple layers, the porosity of each layer is calculated individually, and then the thickness of the layer is divided by the thickness of the third dielectric ceramic layer, and the sum of the product of the porosity of each layer is determined as the porosity of the third dielectric ceramic layer.

[0059] The first dielectric ceramic layer, the second dielectric ceramic layer and the third dielectric ceramic layer preferably include ceramic grains. When the dielectric ceramic layer contains ceramic grains, an interface resistance occurs at the interface between the ceramic grains, which increases the insulation resistance between the internal electrode layers and makes it possible to prevent the occurrence of short circuits.

[0060] It is preferred that rare earths are present at the interfaces of the ceramic grains. The presence of rare earth elements at the interface of ceramic grains can be confirmed by elemental analysis using TEM-EDX. Examples of rare earth elements include La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Y, etc. The presence of rare earth elements at the interface between ceramic grains can further increase the interface resistance of the dielectric ceramic layer, thereby improving the reliability of the multilayer ceramic capacitor. Mg, Mn, Si, etc. may also be present.

[0061] The rare earth is preferably present in an amount of 0.2 mol % or more and 5 mol % or less based on 100 mol of Ti. The term Ti100 moles here refers to the amount of rare earth present relative to Ti100 moles, based on the premise that the dielectric ceramic material constituting the dielectric ceramic layer is primarily composed of a compound having a perovskite structure (structure represented by ABO3, B=Ti). The abundance of rare earth elements can be confirmed by TEM-EDX.

[0062] In the multilayer ceramic capacitor, the thickness of each of the first internal electrode layer and the second internal electrode layer is preferably 0.4 μm or less. Moreover, it is preferable that the thickness of each of the first internal electrode layers and the second internal electrode layers is 0.38 μm or less. Moreover, it is preferable that the thickness of each of the first internal electrode layers and the second internal electrode layers is 0.25 μm or more.

[0063] The first dielectric ceramic layer preferably has a thickness of 0.55 μm or less. Moreover, the thickness of each of the first dielectric ceramic layers is preferably 0.4 μm or more.

[0064] The thickness of the second dielectric ceramic layer is preferably the same as that of the internal electrode layer.

[0065] The thickness of each of the third dielectric ceramic layers 41 and 42 is preferably 5 μm or more and 40 μm or less, and more preferably 5 μm or more and 20 μm or less. The thicknesses of the third dielectric ceramic layers 41 and 42 are preferably the same as each other. However, it is preferable that the outer layer 41b is thicker than the inner layer 41a while the inner layer 41a and the outer layer 41b satisfy the above range. Similarly, it is preferable that the outer layer 42b is thicker than the inner layer 42a while the inner layer 42a and the outer layer 42b satisfy the above range.

[0066] The inner layer 41a is preferably thinner than the outer layer 41b in order to maintain the shape and performance of the multilayer ceramic capacitor 1. Similarly, the inner layer 42a is preferably thinner than the outer layer 42b.

[0067] The thickness of each of the inner layers 41a and 42a is preferably 0.1 μm or more and 20 μm or less. The thickness of the inner layers 41a and 42a is preferably the same as each other.

[0068] The thickness of each of the outer layers 41b and 42b is preferably not less than 5 μm and not more than 20 μm. The thickness of the outer layers 41b and 42b is preferably the same as each other.

[0069] The thickness of each ceramic layer in the side margin portion means the average value when the thickness of the third dielectric ceramic layer is measured at multiple points along the stacking (T) direction.

[0070] [Manufacturing method of multilayer ceramic capacitors] A method for producing a multilayer ceramic capacitor according to the present invention preferably includes the steps of: preparing a green chip having a laminated structure constituted of a plurality of first dielectric ceramic layers and a plurality of second dielectric ceramic layers in an unfired state, and a plurality of pairs of first internal electrode layers and second internal electrode layers, the first internal electrode layers and the second internal electrode layers being exposed on a first side surface and a second side surface facing each other in a width direction perpendicular to a lamination direction; forming an unfired third dielectric ceramic layer on the first side surface and the second side surface of the green chip to produce an unfired laminate; and firing the unfired laminate, In the step of preparing the unsintered laminate, an unsintered first internal electrode layer or a second internal electrode layer is formed on a surface of an unsintered first dielectric ceramic layer, and an unsintered second dielectric ceramic layer is formed in an area where the first internal electrode layer and the second internal electrode layer are not provided, and the obtained ceramic green sheets are laminated. In the step of preparing the unsintered laminate, an unsintered inner layer is formed on the first side surface and the second side surface, and an unsintered outer layer is formed on the outermost side, thereby forming the unsintered side margin portion, and at least one of the dielectric ceramic layers among the first dielectric ceramic layer, the second dielectric ceramic layer, and the third dielectric ceramic layer has a different composition.

[0071] An example of a method for manufacturing the multilayer ceramic capacitor 1 shown in FIG. 1 will now be described.

[0072] First, ceramic green sheets to become the first dielectric ceramic layer 20a, the second dielectric ceramic layer 20b, and the third dielectric ceramic layer 41, 42 are prepared. The ceramic green sheets contain ceramic raw materials containing the above-mentioned dielectric ceramic material, as well as binders and solvents. In addition, additives containing rare earths may be added to the ceramic raw materials. By changing the elements contained in the additives, the compositions of the first dielectric ceramic layer, the second dielectric ceramic layer, and the third dielectric ceramic layer can be changed. It is preferable that the ceramic raw materials, which are the main components, are the same. The ceramic green sheet is formed, for example, on a carrier film using a die coater, a gravure coater, a microgravure coater, or the like.

[0073] Figures 6, 7 and 8 are plan views showing examples of ceramic green sheets, each of which shows a first ceramic green sheet 101 for forming the inner layer portion 30, a second ceramic green sheet 102 for forming the inner layer portion 30, and a third ceramic green sheet 103 for forming the outer layer portion 31 or 32, respectively.

[0074] 6, 7, and 8, the first ceramic green sheet 101, the second ceramic green sheet 102, and the third ceramic green sheet 103 are not cut into individual multilayer ceramic capacitors 1. Fig. 6, 7, and 8 show cutting lines X and Y for cutting into individual multilayer ceramic capacitors 1. The cutting line X is parallel to the length (L) direction, and the cutting line Y is parallel to the width (W) direction.

[0075] 6, in the first ceramic green sheet 101, an unfired first internal electrode layer 121 corresponding to the first internal electrode layer 21 is formed on an unfired first dielectric ceramic layer 120a corresponding to the first dielectric ceramic layer 20a. Also, an unfired second dielectric ceramic layer 120b corresponding to the second dielectric ceramic layer 20b is formed in an area where the unfired first internal electrode layer 121 is not formed. The unsintered first dielectric ceramic layer 120 a and the unsintered second dielectric ceramic layer 120 b are also unsintered dielectric ceramic layers 120 that correspond to the dielectric ceramic layer 20 .

[0076] 7, in the second ceramic green sheet 102, an unsintered second internal electrode layer 122 corresponding to the second internal electrode layer 22 is formed on an unsintered first dielectric ceramic layer 120a corresponding to the first dielectric ceramic layer 20a. Also, an unsintered second dielectric ceramic layer 120b corresponding to the second dielectric ceramic layer 20b is formed in an area where the unsintered second internal electrode layer 122 is not formed. The unsintered first dielectric ceramic layer 120 a and the unsintered second dielectric ceramic layer 120 b are also unsintered dielectric ceramic layers 120 that correspond to the dielectric ceramic layer 20 .

[0077] The method for producing the first ceramic green sheet 101 shown in FIG. 6 and the second ceramic green sheet shown in FIG. 7 is not particularly limited, but may be a method in which a dielectric paste, which is a mixture of a dielectric ceramic and a solvent that will become the second dielectric ceramic layer 20b when fired, and a conductive paste that will become the internal electrode layer 21 or 22 when fired, are applied to predetermined areas on the surface of the unsintered first dielectric ceramic layer 120a. The order in which the dielectric paste and the conductive paste are applied is not particularly limited, and the dielectric paste may be applied first and then the conductive paste, or the conductive paste may be applied first and then the dielectric paste. The dielectric paste and conductive paste may be applied so that the later applied paste partially covers part of the surface of the previously applied paste.

[0078] As shown in FIG. 8, the third ceramic green sheet 103 corresponding to the outer layer portion 31 or 32 consists of an unsintered first dielectric ceramic layer 120a corresponding to the first dielectric ceramic layer, and does not include an unsintered internal electrode layer 121 or 122 or an unsintered second dielectric ceramic layer 120b.

[0079] The first internal electrode layer 121 and the second internal electrode layer 122 can be formed using any conductive paste. For example, a screen printing method, a gravure printing method, or the like can be used to form the first internal electrode layer 121 and the second internal electrode layer 122 using a conductive paste.

[0080] The first internal electrode layer 121 and the second internal electrode layer 122 are disposed across two adjacent regions in the length (L) direction separated by a cutting line Y, and extend in a strip shape in the width (W) direction. The regions separated by the cutting line Y in the first internal electrode layer 121 and the second internal electrode layer 122 are shifted by one row in the length (L) direction. That is, the cutting line Y passing through the center of the first internal electrode layer 121 passes through the region between the second internal electrode layers 122 (i.e., the center of the second dielectric ceramic layer 120b), and the cutting line Y passing through the center of the second internal electrode layer 122 passes through the region between the first internal electrode layers 121 (i.e., the center of the second dielectric ceramic layer 120b).

[0081] Thereafter, the first ceramic green sheet 101, the second ceramic green sheet 102 and the third ceramic green sheet 103 are laminated to prepare a mother block.

[0082] FIG. 9 is an exploded perspective view illustrating an example of a mother block. 9, for convenience of explanation, the first ceramic green sheet 101, the second ceramic green sheet 102, and the third ceramic green sheet 103 are shown in an exploded view. In the actual mother block 104, the first ceramic green sheet 101, the second ceramic green sheet 102, and the third ceramic green sheet 103 are integrated by being pressed together by a means such as a hydrostatic press.

[0083] In the mother block 104 shown in Fig. 9, first ceramic green sheets 101 and second ceramic green sheets 102 corresponding to the inner layer portion 30 are alternately laminated in the lamination (T) direction. Furthermore, third ceramic green sheets 103 corresponding to the outer layer portions 31 and 32 are laminated on the upper and lower surfaces in the lamination (T) direction of the alternately laminated first ceramic green sheets 101 and second ceramic green sheets 102. Note that, although three each of the third ceramic green sheets 103 are laminated in Fig. 9, the number of third ceramic green sheets 103 can be changed as appropriate.

[0084] The mother block 104 thus obtained is cut along cutting lines X and Y (see FIGS. 6, 7, and 8) to produce a plurality of green chips. For this cutting, a method such as dicing, press cutting, or laser cutting is applied.

[0085] FIG. 10 is a perspective view illustrating an example of a green chip. The green chip 110 shown in FIG. 10 has a laminated structure including a plurality of first dielectric ceramic layers 120a and second dielectric ceramic layers 120b in an unfired state and a plurality of pairs of first internal electrode layers 121 and second internal electrode layers 122. The first side surface 113 and the second side surface 114 of the green chip 110 are surfaces that appear by cutting along a cutting line X, and the first end surface 115 and the second end surface 116 are surfaces that appear by cutting along a cutting line Y. The first side surface 113 and the second side surface 114 expose the first internal electrode layer 121 and the second internal electrode layer 122. Also, only the first internal electrode layer 121 and the second dielectric ceramic layer 120b are exposed on the first end surface 115, and only the second internal electrode layer 122 and the second dielectric ceramic layer 120b are exposed on the second end surface 116. The first dielectric ceramic layer 120a is exposed on a first side surface 113, a second side surface 114, a first end surface 115 and a second end surface 116, but the second dielectric ceramic layer is exposed at a different location in the region in which it is disposed. That is, the second dielectric ceramic layer 120b arranged on the first end face 115 side is not exposed to the second end face 116, and the second dielectric ceramic layer 120b arranged on the second end face 116 side is not exposed to the first end face 115.

[0086] An unsintered third dielectric ceramic layer is formed on the first side surface 113 and the second side surface 114 of the obtained green chip 110 to produce an unsintered laminate. The unsintered third dielectric ceramic layer is formed, for example, by attaching ceramic green sheets made of dielectric ceramic to the first side surface 113 and the second side surface of the green chip.

[0087] For example, when the third dielectric ceramic layer is composed of two layers, an inner layer and an outer layer, first, a ceramic slurry containing a ceramic raw material containing a dielectric ceramic material mainly composed of BaTiO3, etc., as well as a binder and a solvent, etc. is prepared to prepare a ceramic green sheet for the inner layer. The ceramic slurry for the inner layer may contain Si as a sintering aid. The inner layer serves to adhere to the green chip 110. In addition, liquid-phase metals may be added to the ceramic slurry for the inner layer, and rare earth elements, Mg, and Mn may be added to the ceramic slurry for the inner layer in amounts larger than those of the ceramic green sheets for forming the inner layer portion. By doing so, it is possible to suppress the grain growth of the ceramic grains contained in the dielectric ceramic layer sandwiched between the widthwise ends of the internal electrode layers.

[0088] Next, in order to prepare the ceramic green sheets for the outer layer, a ceramic slurry is prepared that contains a ceramic raw material containing a dielectric ceramic material mainly composed of BaTiO3, etc., as well as a binder and a solvent. The ceramic slurry for the outer layer may contain Si as a sintering aid. The amount of Si contained in the ceramic green sheets for the inner layer is preferably greater than the amount of Si contained in the ceramic green sheets for the outer layer. The amount of Si contained in the ceramic green sheets for the inner layer is determined by imaging the cross section by WDX and judging the area of ​​the region where Si is detected.

[0089] The ceramic slurry for the outer layer is applied to the surface of the resin film and dried to form a ceramic green sheet for the outer layer. The ceramic slurry for the inner layer is applied to the surface of the ceramic green sheet for the outer layer on the resin film and dried to form a ceramic green sheet for the inner layer. As a result, a ceramic green sheet having a two-layer structure is obtained.

[0090] A ceramic green sheet having a two-layer structure can also be obtained by, for example, forming an outer layer ceramic green sheet and an inner layer ceramic green sheet in advance and then bonding them together. The ceramic green sheet is not limited to having two layers, and may have three or more layers.

[0091] Thereafter, the ceramic green sheet is peeled off from the resin film.

[0092] Next, the ceramic green sheet for the inner layer of the ceramic green sheet and the first side surface 113 of the green chip 110 are opposed to each other, and pressed together to form an unsintered side margin portion 41. Furthermore, the ceramic green sheet for the inner layer of the ceramic green sheet is opposed to the second side surface 114 of the green chip 110, and pressed together to form an unsintered side margin portion 42. At this time, it is preferable to apply an organic solvent to the side surface of the green chip in advance to serve as an adhesive. As a result of the above, an unsintered laminate is obtained.

[0093] The green laminate obtained by the above method is preferably subjected to barrel polishing, etc. By polishing the green laminate, the corners and ridges of the laminate 10 after firing are rounded.

[0094] Thereafter, in the unfired laminate, a conductive paste for external electrodes containing Ni and a ceramic material is applied onto each of first end face 115 and second end face 116 of green chip 110.

[0095] The conductive paste for external electrodes preferably contains, as a ceramic material, the same dielectric ceramic material as that of the first dielectric ceramic layer, the second dielectric ceramic layer, or the outer layer. The content of the ceramic material in the conductive paste for external electrodes is preferably 15% by weight or more. The content of the ceramic material in the conductive paste for external electrodes is preferably 25% by weight or less.

[0096] Next, the unfired laminate coated with the conductive paste for external electrodes is degreased under predetermined conditions, for example, in a nitrogen atmosphere, and then fired at a predetermined temperature in a nitrogen-hydrogen-water vapor mixed atmosphere. As a result, the unfired laminate and the conductive paste for external electrodes are fired simultaneously, and the laminate 10, the Ni layer connected to the first internal electrode layer 21, and the Ni layer connected to the second internal electrode layer 22 are simultaneously formed by the so-called co-firing method. After that, a first plating layer made of Ni plating and a second plating layer made of Sn plating are sequentially laminated on the surface of each Ni layer. As a result, the first external electrode 51 and the second external electrode 52 are formed.

[0097] The laminate 10, the first external electrode 51, and the second external electrode 52 may be formed at different times by a so-called post-fire method. Specifically, the unfired laminate is first degreased under predetermined conditions in a nitrogen atmosphere, and then fired at a predetermined temperature in a nitrogen-hydrogen-water vapor mixed atmosphere to form the laminate 10. Then, a conductive paste containing Cu powder is applied and baked on each end face of the first end face 15 and the second end face 16 of the laminate 10. As a result, a base electrode layer connected to the first internal electrode layer 21 and a base electrode layer connected to the second internal electrode layer 22 are formed. Then, a conductive resin layer containing conductive particles (e.g., metal particles such as Cu, Ag, Ni, etc.) and resin, a first plating layer formed by Ni plating, and a second plating layer formed by Sn plating are sequentially laminated on the surface of each base electrode layer. As a result, the first external electrode 51 and the second external electrode 52 are formed.

[0098] In this manner, the multilayer ceramic capacitor 1 is manufactured.

[0099] In the above-described embodiment, the mother block 104 is cut along the cutting lines X and Y to obtain a plurality of green chips, and then an unsintered third dielectric ceramic layer is formed on both side surfaces of the green chips. However, the following modification is also possible.

[0100] That is, the mother block may be cut only along the cutting line X to obtain a plurality of rod-shaped green block bodies with the first internal electrode layers and the second internal electrode layers exposed on the side surfaces that are revealed by cutting along the cutting line X, and then unsintered third dielectric ceramic layers may be formed on both side surfaces of the green block body, followed by cutting along the cutting line Y to obtain a plurality of unsintered laminates, and then firing the unsintered laminates. After firing, a multilayer ceramic capacitor can be manufactured by carrying out the same steps as in the above-mentioned embodiment.

[0101] The present invention further includes the following features [1] to [7].

[0102] [1] Alloyed parts between the dielectric ceramic layer and the internal electrode layer and external electrode 11, in the multilayer ceramic capacitor 1 of the present invention, a second alloy portion 320 is formed between the second dielectric ceramic layer 20b and the first internal electrode layer 21, and between the second dielectric ceramic layer 20b and the second internal electrode layer 22. In addition, in the multilayer ceramic capacitor 1 of the present invention, a first alloy portion 310 is formed between the first dielectric ceramic layer 20a and the first internal electrode layer 21, and between the first dielectric ceramic layer 20a and the second internal electrode layer 22.

[0103] As shown in FIG. 12, the metal element 321a is segregated at the interface 2220b between the second internal electrode layer 22 and the second dielectric ceramic layer 20b. The second alloy part 320 is formed by a segregation layer 321 which is a layer-like segregation of the metal element 321a. Similarly, the metal element 321a is segregated to form a segregation layer 321 at the interface 2220b between the first internal electrode layer 21 and the second dielectric ceramic layer 20b, and the second alloy part 320 is formed by the segregation layer 321. The second alloy part 320 is formed on the surface of the first internal electrode layer 21 and the second internal electrode layer 22 on the second dielectric ceramic layer 20b side. The second alloy part 320 is formed between the first internal electrode layer 21 and the second dielectric ceramic layer 20b and between the second internal electrode layer 22 and the second dielectric ceramic layer 20b.

[0104] As shown in FIG. 12, the metal element 311a is segregated at the interface 2220a between the second internal electrode layer 22 and the first dielectric ceramic layer 20a. The first alloy part 310 is formed by a segregation layer 311 which is a layer-like segregation of the metal element 311a. Similarly, the metal element 311a is segregated at the interface 2220a between the first internal electrode layer 21 and the first dielectric ceramic layer 20a to form a segregation layer 311, and the first alloy part 310 is formed by the segregation layer 311. The first alloy part 310 is formed on the surface of the first internal electrode layer 21 and the second internal electrode layer 22 on the first dielectric ceramic layer 20a side. The first alloy part 310 is formed between the first internal electrode layer 21 and the first dielectric ceramic layer 20a and between the second internal electrode layer 22 and the first dielectric ceramic layer 20a.

[0105] There are multiple types of segregated metal elements 321a forming the second alloy part 320. The multiple types of metal elements 321a forming the segregation layer 321 include the metal element that is most abundant among the metal elements forming the first internal electrode layer 21 and the second internal electrode layer 22, and an element derived from the second dielectric ceramic layer 20b. The same is true for the segregated metal element 311a forming the first alloy part 310. That is, the metal element 311a includes the metal element that is most abundant among the metal elements forming the first internal electrode layer 21 and the second internal electrode layer 22, and an element derived from the first dielectric ceramic layer 20a.

[0106] The metal element that is most abundant among the metal elements constituting the first internal electrode layer 21 and the second internal electrode layer 22 may be, for example, one of Ni, Cu, Ag, Pd, Au, or Pt. On the other hand, the elements derived from the second dielectric ceramic layer 20b and the first dielectric ceramic layer 20a may be, for example, metal elements as additives. Specifically, any one or more metal elements from the metal group of Sn, In, Ga, Zn, Bi, Pb, Cu, Ag, Pd, Pt, Ph, Ir, Ru, Os, Fe, V, Y, and Ge may be mentioned, and among these, Sn, Ga, and Ge are particularly preferred. Hereinafter, this metal group may be referred to as the metal group M.

[0107] The segregation of the metal element 321a occurs when the metal element contained in the second dielectric ceramic layer 20b migrates to the first internal electrode layer 21 and the second internal electrode layer 22 when the second dielectric ceramic layer 20b is fired. The segregation of the metal element 311a occurs when the metal element contained in the first dielectric ceramic layer 20a migrates to the first internal electrode layer 21 and the second internal electrode layer 22 when the first dielectric ceramic layer 20a is fired.

[0108] When the first dielectric ceramic layer 20a is mainly composed of BaTiO3, the second alloy part 320 has a higher molar ratio of the content of the metal elements contained in the second dielectric ceramic layer 20b, i.e., any one or more types of the above metal group M, to 100 moles of Ti, than the first alloy part 310.

[0109] FIG. 13 shows a surface including the center in the width (W) direction, the length (L) direction, and the stacking (T) direction of the laminate 10. In the multilayer ceramic capacitor 1 of the present invention, in the surface shown in FIG. 13, the first internal electrode layer 21 includes a plurality of first interspersed internal electrodes 210 that are discontinuously interspersed in the length (L) direction at an end in the length (L) direction that is not connected to the second external electrode 52. The second internal electrode layer 22 includes a plurality of second interspersed internal electrodes 220 that are discontinuously interspersed in the length (L) direction at an end in the length (L) direction that is not connected to the first external electrode 51. Each of the first interspersed internal electrodes 210 and the second interspersed internal electrodes 220 is formed inside the second dielectric ceramic layer 20b. The plurality of first interspersed internal electrodes 210 may be connected to the first internal electrode layer 21 while extending in the width (W) direction. Furthermore, the multiple second interspersed internal electrodes 220 may also be connected to the second internal electrode layer 22 while extending in the width (W) direction.

[0110] A fourth alloy portion 340 is formed around each of the first interspersed internal electrode 210 and the second interspersed internal electrode 220. The fourth alloy portion 340 is formed of a segregation layer 341 that is a layered segregation of a metal element 341a. The metal element 341a includes a metal element that is contained most abundantly among the metal elements that constitute the first internal electrode layer 21 and the second internal electrode layer 22, and one or more types of metal elements of the metal group M derived from the second dielectric ceramic layer 20b.

[0111] The segregation of the metal element 341a occurs when the metal element contained in the second dielectric ceramic layer 20b migrates to the first interspersed internal electrode 210 and the second interspersed internal electrode 220 during firing of the second dielectric ceramic layer 20b. The segregation of the metal element 341a occurs around one or more of the first interspersed internal electrodes 210 and the multiple second interspersed internal electrodes 220. Alternatively, the segregation may occur around the entire first interspersed internal electrode 210 and the entire second interspersed internal electrode 220.

[0112] As shown in FIG. 14, in the multilayer ceramic capacitor 1 of the present invention, a third alloy portion 330 is formed between the third dielectric ceramic layers 41 and 42 and the first internal electrode layer 21, and between the third dielectric ceramic layers 41 and 42 and the second internal electrode layer 22, respectively.

[0113] As shown in FIG. 14, the metal element 331a is segregated at the interface 2220c between the first internal electrode layer 21 and the third dielectric ceramic layers 41 and 42. The metal element 331a is also segregated at the interface 2220c between the second internal electrode layer 22 and the third dielectric ceramic layers 41 and 42. The third alloy part 330 is formed by layered segregation of the metal element 331a, that is, the segregation layer 331. The third alloy part 330 is formed on the surfaces of the first internal electrode layer 21 and the second internal electrode layer 22 on the third dielectric ceramic layer 41 side and the third dielectric ceramic layer 42 side, respectively. The third alloy part 330 is formed between the first internal electrode layer 21 and the third dielectric ceramic layers 41 and 42, and between the second internal electrode layer 22 and the third dielectric ceramic layers 41 and 42, respectively.

[0114] The metal element 331a includes the metal element that is contained most abundantly among the metal elements constituting the first internal electrode layer 21 and the second internal electrode layer 22, and one or more kinds of metal elements in the metal group M derived from the third dielectric ceramic layers 41 and 42. Examples of the elements derived from the third dielectric ceramic layers 41 and 42 include metal elements as additives. Specifically, one or more kinds of metal elements in the metal group M are included.

[0115] The segregation of the metal element 331a occurs when the metal element contained in the third dielectric ceramic layers 41 and 42 migrates to the first internal electrode layer 21 and the second internal electrode layer 22 when the third dielectric ceramic layers 41 and 42 are fired.

[0116] In the multilayer ceramic capacitor 1 of the present invention, when the first external electrode 51 and the second external electrode 52 each include a Ni layer as a base electrode layer and are formed by a co-firing method, a fifth alloy portion 350 is formed in the Ni layer, as shown in FIG. 15.

[0117] 15 shows a state where a fifth alloy part 350 is formed at the interface 51b between the first external electrode 51 and the second dielectric ceramic layer 20b. The fifth alloy part 350 is formed of a segregation layer 351 which is a layer-like segregation of a metal element 351a. Similarly, a fifth alloy part 350 is formed at the interface 51b between the second external electrode 52 and the second dielectric ceramic layer 20b by segregation of the metal element 351a. The segregation of the metal element 351a occurs when the metal element contained in the second dielectric ceramic layer 20b moves to the first external electrode 51 and the second external electrode 52 when the second dielectric ceramic layer 20b is fired.

[0118] In the laminate 10 of the multilayer ceramic capacitor 1 of the present invention, the mutually adjacent ends of the first internal electrode layer 21 and the second internal electrode layer 22 and the second dielectric ceramic layer 20b may overlap each other. For example, as shown in FIG. 16, the end of the second dielectric ceramic layer 20b may overlap the end of the second internal electrode layer 22. Also, as shown in FIG. 17, the end of the second dielectric ceramic layer 20b may overlap the end of the first internal electrode layer 21. In such an embodiment in which the ends overlap, the first internal electrode layer 21 and the second internal electrode layer 22 may each overlap the second dielectric ceramic layer 20b.

[0119] In the multilayer ceramic capacitor 1 of the present invention, a second alloy portion 320 containing one metal element that is most abundant among the metal elements constituting the internal electrode layer and one or more metal elements selected from a metal group M of Sn, In, Ga, Zn, Bi, Pb, Cu, Ag, Pd, Pt, Ph, Ir, Ru, Os, Fe, V, and Y is formed between the second dielectric ceramic layer 20b and the first internal electrode layer 21, and between the second dielectric ceramic layer 20b and the second internal electrode layer 22.

[0120] An electric field is likely to concentrate at the ends of the first internal electrode layer 21 and the second internal electrode layer 22 that are in contact with the second dielectric ceramic layer 20b, which may reduce the reliability of the multilayer ceramic capacitor. However, in the multilayer ceramic capacitor 1 of the present invention, the second alloy part 320 is formed between the second dielectric ceramic layer 20b and the first internal electrode layer 21 and the second internal electrode layer 22, thereby suppressing the electric field concentration and improving the reliability.

[0121] In the multilayer ceramic capacitor 1 of the present invention, when the first dielectric ceramic layer 20a contains Ba and Ti, a first alloy part 310 containing the metal element contained most abundantly among the metal elements constituting the internal electrode layer and one or more metal elements of the metal group M is formed between the first dielectric ceramic layer 20a and the first internal electrode layer 21 and between the first dielectric ceramic layer 20a and the second internal electrode layer 22. The second alloy part 320 has a higher molar ratio of the content of the metal group M to 100 moles of Ti than the first alloy part 310.

[0122] As a result, electric field concentration is suppressed by the second alloy part 320 in the vicinity of the interface between the first internal electrode layer 21 and the second internal electrode layer 22 and the second dielectric ceramic layer 20b, and reliability can be improved. In addition, by making the molar ratio of the content of the metal group M to Ti100 moles higher in the second alloy part 320 formed at the end of the first internal electrode layer 21 and the second internal electrode layer 22 in contact with the second dielectric ceramic layer 20b where electric field concentration is likely to occur, than in the first alloy part 310 formed on the first dielectric ceramic layer 20a side, electric field concentration on the second dielectric ceramic layer 20b side can be effectively suppressed, and reliability can be further improved.

[0123] By controlling the amount of metal of the metal group M added to each of the first dielectric ceramic layer 20a and the second dielectric ceramic layer 20b, it is possible to control the thickness of the first alloy portion 310 and the second alloy portion 320 and the concentration of the metal group M contained therein. For example, when the concentration of the metal group M added to the second dielectric ceramic layer 20b is higher than that of the first dielectric ceramic layer 20a, as shown in Fig. 12, the thickness of the second alloy portion 320 increases or the concentration of the metal group M becomes higher toward the second dielectric ceramic layer 20b, and in some cases, both changes occur.

[0124] In the multilayer ceramic capacitor 1 of the present invention, in a surface of the laminate 10 including the center in the width (W) direction, the length (L) direction, and the stacking (T) direction, the first internal electrode layer 21 includes first interspersed internal electrodes 210 discontinuously scattered in the length (L) direction at an end in the length (L) direction that is not connected to the second external electrode 52, and the second internal electrode layer 22 includes second interspersed internal electrodes 220 discontinuously scattered in the length (L) direction at an end in the length (L) direction that is not connected to the first external electrode 51, and a fourth alloy part 340 containing the metal element that is most abundant among the metal elements constituting the internal electrode layer and any one or more types of metal elements from the above-mentioned metal group M is formed around each of the first interspersed internal electrodes 210 and the second interspersed internal electrodes 220.

[0125] When the first interspersed internal electrode 210 and the second interspersed internal electrode 220 extend in the width (W) direction and are connected to the first internal electrode layer 21 and the second internal electrode layer 22, respectively, if an electric field concentrates at the connection portion, there is a risk of dielectric breakdown occurring and reliability decreasing. However, in the multilayer ceramic capacitor 1 of the present invention, the fourth alloy portion 340 formed around each of the first interspersed internal electrode 210 and the second interspersed internal electrode 220 suppresses dielectric breakdown due to electric field concentration, thereby improving reliability.

[0126] In the multilayer ceramic capacitor 1 of the present invention, a third alloy portion 330 containing the metal element that is most abundant among the metal elements constituting the internal electrode layer and one or more types of metal elements selected from the metal group M is formed between the third dielectric ceramic layers 41 and 42 and the first internal electrode layer 21, and between the third dielectric ceramic layers 41 and 42 and the second internal electrode layer 22, respectively.

[0127] As a result, electric field concentration is suppressed by the third alloy part 330 in the vicinity of the interfaces between the first internal electrode layer 21 and the second internal electrode layer 22 and the third dielectric ceramic layers 41 and 42, thereby improving reliability.

[0128] In the multilayer ceramic capacitor 1 of the present invention, the first external electrode 51 and the second external electrode 52 contain Ni, and a fifth alloy portion 350 in which any one or more metal elements selected from the metal group M are segregated to Ni is formed between the second dielectric ceramic layer 20b and the first external electrode 51 and the second external electrode 52.

[0129] As a result, even when the gap between the first internal electrode layer 21 and the second external electrode 52, and between the second internal electrode layer 22 and the first external electrode 51, i.e., the distance in the length (L) direction of the second dielectric ceramic layer 20b, is narrow, for example, less than 15 μm, the presence of the fifth alloy part 350 makes it difficult for insulation breakdown due to electric field concentration to occur between the internal electrode layer and the external electrode, thereby improving reliability.

[0130] [Test Example 1] Next, a first test example will be described which examines the effects of the first alloy part 310, the second alloy part 320 and the third alloy part 330 in the multilayer ceramic capacitor 1 of the present invention.

[0131] About TEM analysis In the manufacturing method of the multilayer ceramic capacitor of the present invention described above, the first external electrode 51 and the second external electrode 52 are not co-fired, and the laminate 10 obtained by firing the green chip 110 is polished from the first side surface 13 side and the second side surface 14 side to obtain a polished body with the center portion in the width (W) direction remaining as shown in Figure 18 as a test specimen. The types and amounts of metal elements (metal concentrations) contained in the first alloy portion 310 were analyzed as follows. 18, a virtual line OL1 perpendicular to the length (L) direction is assumed at the center of the length (L) direction. Then, along the virtual line OL1, a region in which the first dielectric ceramic layer 20a, the first internal electrode layer 21, and the second internal electrode layer 22 related to obtaining the electrostatic capacitance of the polished body are laminated is divided into three equal regions in the lamination direction, that is, an upper region E1, a central region E2, and a lower region E3. The upper region E1, the central region E2 and the lower region E3 are cut out from the polished body, and each of the upper region E1, the central region E2 and the lower region E3 is thinned by Ar ion milling or the like to obtain three thin film samples from each region.

[0132] The three thin film samples of the upper region E1, the central region E2, and the lower region E3 of the specimen obtained as described above were subjected to TEM observation and elemental mapping by EDX attached to the TEM. As a result, since no significant difference was observed between the upper region E1 and the lower region E3 and the central region E2, the results obtained from the central region E2 are regarded as the microstructure of the dielectric ceramic layer and the internal electrode layer. As a result, the type and amount of metal (metal concentration) of the metal element contained in the first alloy part 310 can be known. The type and amount (metal concentration) of the metal element contained in the second alloy part 320 can be analyzed by obtaining a thin film sample in the same manner as described above at one end of the length (L) direction where the second alloy part 320 exists. That is, in the polished body shown in FIG. 18, a virtual line OL2 perpendicular to the length (L) direction is assumed at one end of the length (L) direction, and thin film samples are obtained in three regions, an upper region E4, a central region E5, and a lower region E6, which are divided into three equal parts in the stacking direction along the virtual line OL2. Then, the three thin film samples of the upper region E4, the central region E5, and the lower region E6 were observed by TEM and element mapping was performed by EDX attached to the TEM to examine the type and amount (metal concentration) of the metal element contained in the second alloy part 320.

[0133] The second alloy part and the first alloy part were examined for Sn concentration by analysis of EDX mapping images from TEM observation images. TEM measurement points were measured at intervals of approximately 5 nm to 10 nm. At the interface between the internal electrode layer and the dielectric ceramic layer, the area where the observed value was three times or more higher than other measurement points was determined as the alloy part, and the average value was determined as the metal concentration of the alloy part.

[0134] Eighteen multilayer ceramic capacitors were prepared for each of Test Examples 1-1 to 1-5 shown in Table 1. Test Example 1-2 was a multilayer ceramic capacitor of the present invention, in which the first internal electrode layer 21 and the second internal electrode layer 22 were made of Ni, and the same amount of Sn was added as an additive to the first dielectric ceramic layer 20a and the second dielectric ceramic layer 20b. Test Examples 1-3 to 1-5 were made such that the amount of Sn added to the second dielectric ceramic layer 20b was gradually increased compared to Test Example 1-2. Test Example 1-1 was a multilayer ceramic capacitor under the same conditions as Test Examples 1-2 to 1-5, except that Sn was not added to the second dielectric ceramic layer 20b.

[0135] For the multilayer ceramic capacitors of test examples 1-1 to 1-5, the resistance value (kΩ) was measured under a voltage of 6.3 V applied in an environment of room temperature 150°C, and the MTTF (mean time to failure) was examined and judged. The MTTF was the point at which the resistance value became 10 kΩ or less, and when the MTTF was 15.3 hours (hr) or less, it was judged as ×, when it was more than 15.3 hours (hr) to 30 hours, it was judged as ◯ (good), and when it was more than 30 hours, it was judged as ◎ (excellent). The results are also shown in Table 1. Note that when the coverage of the internal electrode layer was less than 80%, it was deemed impossible to measure because it was difficult to obtain the electrostatic capacitance.

[0136] [Table 1]

[0137] According to Table 1, the formation of the second alloy part results in a good MTTF exceeding the prescribed time of 15.3 hours, and the higher the Sn concentration, the better the MTTF is. On the other hand, in Test Example 1-1, where the second alloy part of Sn is not formed, the MTTF did not exceed the prescribed time. This confirmed that the second alloy part increases the reliability of the multilayer ceramic capacitor.

[0138] Next, in addition to Test Example 1-1, 18 pieces of each of the multilayer ceramic capacitors of Test Examples 1-6 to 1-9 shown in Table 2 were prepared. Test Example 1-6 further added Sn as an additive to the third dielectric ceramic layer in the same amount as that of the first and second dielectric ceramic layers in Test Example 1-2. Test Examples 1-7 to 1-9 added gradually more Sn to the third dielectric ceramic layer than Test Example 1-6. Test Example 1-1 did not add Sn to the third dielectric ceramic layer.

[0139] For Test Examples 1-1 and 1-6 to 1-9, MTTF determination was performed in the same manner as for Test Examples 1-1 to 1-5. The results are shown in Table 2.

[0140] [Table 2]

[0141] According to Table 2, by forming the third alloy part together with the second alloy part, the MTTF exceeded the prescribed time of 15.3 hours, which is good, and the higher the Sn concentration, the better the MTTF was. On the other hand, in Test Example 1-1, where neither the second alloy part nor the third alloy part made of Sn was formed, the MTTF did not exceed the prescribed time. This confirmed that the second alloy part and the third alloy part increase the reliability of the multilayer ceramic capacitor.

[0142] [2] Average particle size of dielectric particles contained in the area near the intersection 19 shows a surface including the length (L) direction and the width (W) direction of the multilayer ceramic capacitor 1 of the present invention, which includes the second dielectric ceramic layer 20b and the second internal electrode layer 22. As shown in FIG. 19, both sides in the width (W) direction of the end portion on the first end face 15 side of the multilayer ceramic capacitor 1 have an intersection point 400 of the interface surrounded by the second dielectric ceramic layer 20b, the second internal electrode layer 22, and the third dielectric ceramic layers 41 and 42. This intersection point 400 is an intersection point between the interface 2220b between the second dielectric ceramic layer 20b and the second internal electrode layer 22 and the inner surface 401 in the width (W) direction of the third dielectric ceramic layers 41 and 42. Similarly, both sides in the width (W) direction of the end portion on the second end face 16 side also have an intersection point 400 of the interface surrounded by the second dielectric ceramic layer 20b, the first internal electrode layer 21, and the third dielectric ceramic layers 41 and 42.

[0143] The region inside a circle 400r having a radius of 5 μm and centered on the intersection 400 is defined as a second intersection neighborhood region 420. The region inside a circle 400r having a radius of 5 μm and centered on the intersection 400 is defined as a third intersection neighborhood region 430. The region inside the circle 400r includes the line of the circle 400r. In the following description, the second intersection neighborhood region 420 on the second dielectric ceramic layer 20b side and the third intersection neighborhood region 430 on the third dielectric ceramic layers 41 and 42 side may be collectively referred to as an intersection neighborhood region 440. A part of the second dielectric ceramic layer 20b is included in the region inside the second intersection vicinity region 420. A part of the third dielectric ceramic layers 41 and 42 is included in the region inside the third intersection vicinity region 430.

[0144] In the multilayer ceramic capacitor 1 of the present invention, (A) The average particle size of the dielectric particles contained in each intersection vicinity region 440 is smaller than the average particle size of the dielectric particles contained in the first dielectric ceramic layer 20a, the average particle size of the dielectric particles contained in the second dielectric ceramic layer 20b, and the average particle size of the dielectric particles contained in the third dielectric ceramic layers 41 and 42.

[0145] (B) Furthermore, it is preferable that the ratio of smallness is 5% or more smaller.

[0146] In this case, the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b refers to the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b in the portions other than the second intersection neighborhood region 420, and the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42 refers to the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42 in the portions other than the third intersection neighborhood region 430.

[0147] The multilayer ceramic capacitor 1 of the present invention having the above configuration (A) or (B) preferably further has any one of the following configurations (C) to (I).

[0148] (C) The difference between the average particle size of the dielectric particles contained in the second dielectric ceramic layer 20b and the average particle size of the dielectric particles contained in the third dielectric ceramic layers 41 and 42 is within 5%, the average particle size of the dielectric particles contained in the first dielectric ceramic layer 20a is larger than both of the average particle size of the dielectric particles contained in the second dielectric ceramic layer 20b and the average particle size of the dielectric particles contained in the third dielectric ceramic layers 41 and 42, and the average particle size of the dielectric particles contained in the intersection vicinity region 440 is smaller than both of the average particle size of the dielectric particles contained in the second dielectric ceramic layer 20b and the average particle size of the dielectric particles contained in the third dielectric ceramic layers 41 and 42.

[0149] (D) The difference between the average particle size of the dielectric particles contained in the first dielectric ceramic layer 20a and the average particle size of the dielectric particles contained in the second dielectric ceramic layer 20b is within 5%, the average particle size of the dielectric particles contained in the third dielectric ceramic layers 41 and 42 is smaller than both the average particle size of the dielectric particles contained in the first dielectric ceramic layer 20a and the average particle size of the dielectric particles contained in the second dielectric ceramic layer 20b, and the average particle size of the dielectric particles contained in the intersection vicinity region 440 is smaller than the average particle size of the dielectric particles contained in the third dielectric ceramic layers 41 and 42.

[0150] (E) The difference between the average particle diameter of the dielectric particles contained in the first dielectric ceramic layer 20a and the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42 is within 5%, the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b is smaller than both the average particle diameter of the dielectric particles contained in the first dielectric ceramic layer 20a and the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42, and the average particle diameter of the dielectric particles contained in the intersection vicinity region 440 is smaller than the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b.

[0151] (F) The difference between the average particle size of the dielectric particles contained in the first dielectric ceramic layer 20a and the average particle size of the dielectric particles contained in the second dielectric ceramic layer 20b, the difference between the average particle size of the dielectric particles contained in the first dielectric ceramic layer 20a and the average particle size of the dielectric particles contained in the third dielectric ceramic layers 41 and 42, and the difference between the average particle size of the dielectric particles contained in the second dielectric ceramic layer 20b and the average particle size of the dielectric particles contained in the third dielectric ceramic layers 41 and 42 are all within 5%, and the average particle size of the dielectric particles contained in the intersection vicinity region 440 is smaller than any of the average particle size of the dielectric particles contained in the first dielectric ceramic layer 20a, the average particle size of the dielectric particles contained in the second dielectric ceramic layer 20b, and the average particle size of the dielectric particles contained in the third dielectric ceramic layers 41 and 42.

[0152] (G) The average particle diameter of the dielectric particles contained in the first dielectric ceramic layer 20a is smaller than the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b, the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42 is smaller than the average particle diameter of the dielectric particles contained in the first dielectric ceramic layer 20a, and the average particle diameter of the dielectric particles contained in the intersection vicinity region 440 is smaller than the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42.

[0153] (H) The average particle diameter of the dielectric particles contained in the first dielectric ceramic layer 20a is smaller than the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42, the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b is smaller than the average particle diameter of the dielectric particles contained in the first dielectric ceramic layer 20a, and the average particle diameter of the dielectric particles contained in the intersection vicinity region 440 is smaller than the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b.

[0154] (I) The average particle diameter of the dielectric particles contained in the intersection vicinity region 440 is smaller than the average particle diameter of the dielectric particles contained in the first dielectric ceramic layer 20a, and the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42 or the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b is smaller than the average particle diameter of the dielectric particles contained in the intersection vicinity region 440.

[0155] The average particle size of the dielectric particles contained in the first dielectric ceramic layer 20a, the second dielectric ceramic layer 20b, and the third dielectric ceramic layers 41 and 42 can be controlled by adjusting the amount of sintering aids, such as Si and Mn, contained in the dielectric ceramic slurry forming each dielectric ceramic layer, and further by adjusting the firing temperature.

[0156] As described above, in the multilayer ceramic capacitor 1 of the present invention, the average particle diameter of the dielectric particles contained in the intersection vicinity region 440 is smaller than the average particle diameter of the dielectric particles contained in the first dielectric ceramic layer 20a around the intersection vicinity region 440, the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b, and the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42.

[0157] An electric field is likely to concentrate in the intersection vicinity region 440, and if electric field concentration occurs, there is a risk of reducing the reliability of the multilayer ceramic capacitor. However, in the multilayer ceramic capacitor 1 of the present invention, the average particle size of the dielectric particles contained in the intersection vicinity region 440 is smaller than the average particle size of the dielectric particles contained in the surrounding first dielectric ceramic layer 20a, second dielectric ceramic layer 20b, and third dielectric ceramic layers 41 and 42. Such a small average particle size results in the presence of many grain boundaries, suppressing electric field concentration. As a result, the reliability of the multilayer ceramic capacitor can be improved.

[0158] [Test Example 2] Next, a description will be given of Test Example 2, which verifies the advantage that, in the multilayer ceramic capacitor 1 of the present invention, the average particle size of the dielectric particles contained in the intersection vicinity region 440 is smaller than the average particle sizes of the dielectric particles contained in the surrounding first dielectric ceramic layer 20a and third dielectric ceramic layers 41 and 42.

[0159] The average particle size of the dielectric particles contained in each of the first dielectric ceramic layer, the second dielectric ceramic layer, and the third dielectric ceramic layer is measured as follows.

[0160] (Average particle size of dielectric particles contained in the first dielectric ceramic layer) In the manufacturing method of the multilayer ceramic capacitor of the present invention described above, the first external electrode 51 and the second external electrode 52 are not cofired, and the laminate 10 obtained by firing the green chip 110 is polished from the first end face 15 side or the second end face 16 side to obtain a polished body with the center portion in the length (L) direction remaining as shown in Figure 20 as a test specimen. As shown in FIG. 20, a virtual line OS1 perpendicular to the width (W) direction was assumed at the center of the width (W) direction. Then, along the virtual line OS1, the region in which the first dielectric ceramic layer 20a, the first internal electrode layer 21, and the second internal electrode layer 22 related to the acquisition of the electrostatic capacitance of the polished body were laminated was divided into three equal parts in the lamination direction, that is, an upper region F1, a central region F2, and a lower region F3. The first dielectric ceramic layer 20a was imaged in each of the regions F1, F2, and F3 with a field of view size of 4.3 μm×3.2 μm, and the area of ​​20 dielectric particles was measured by image processing for each of the regions F1, F2, and F3. Then, the circle equivalent diameter was calculated from the measured areas, and the average was taken to obtain the average particle diameter. The average grain size was measured in each of the upper region F1, the central region F2, and the lower region F3, and since no significant difference was found between the measured values, the average grain size in the central region F2 was regarded as the average grain size of the first dielectric ceramic layer.

[0161] (Average particle size of dielectric particles contained in the third dielectric ceramic layer) In the test specimen shown in FIG. 20, a virtual line is assumed that connects the ends of the first side surface 13 side or the second side surface 14 side of the plurality of first internal electrode layers 21 and the plurality of second internal electrode layers 22 in the stacking (T) direction. In FIG. 20, a virtual line OS3 is shown that connects the ends of the second side surface 14 side of the plurality of first internal electrode layers 21 and the plurality of second internal electrode layers 22 in the stacking (T) direction. As shown in FIG. 21, the third dielectric ceramic layer 42 was imaged from the virtual line OS3 with a field of view size of 4.3 μm×3.2 μm in a range of 5 μm on the third dielectric ceramic layer 42 side, and the area of ​​20 dielectric particles was measured by image processing for each of the regions F1, F2, and F3. The reference symbol 42F in FIG. 21 indicates the imaged region. Then, the circle equivalent diameter was calculated from the measured area and the average was taken to obtain the average particle diameter. The average grain size was measured in each of the upper region F1, the central region F2, and the lower region F3, and since no significant difference was found between the measured values, the average grain size in the central region F2 was regarded as the average grain size of the third dielectric ceramic layer.

[0162] (Average particle size of dielectric particles contained in the second dielectric ceramic layer) The laminate 10 is polished from the first end face 15 side or the second end face 16 side until at least one of the internal electrode layers appears. For example, as shown in FIG. 22, the laminate is polished from the second end face 16 side to a surface J immediately before the second internal electrode layer 22 appears. As shown in FIG. 23, a virtual line OS2 perpendicular to the width (W) direction is assumed at the center in the width (W) direction. Then, along the virtual line OS2, the second dielectric ceramic layer 20b is divided into three equal parts in the lamination direction, that is, an upper region G1, a central region G2, and a lower region G3. The second dielectric ceramic layer is imaged in each of the regions G1, G2, and G3 with a field of view size of 4.3 μm×3.2 μm, and the area of ​​20 dielectric particles is measured for each of the regions G1, G2, and G3 by image processing. Then, the circle equivalent diameter is calculated from the measured area and the average is taken to obtain the average particle diameter. The average grain size was measured in each of the upper region G1, the central region G2 and the lower region G3, and since no significant difference was found between the measured values, the average grain size in the central region G2 was regarded as the average grain size of the second dielectric ceramic layer.

[0163] (Average particle size of dielectric particles contained in the area near the intersection) In the test specimen shown in FIG. 23, a virtual line OS4 is assumed that connects the ends of the multiple first internal electrode layers 21 and the multiple second internal electrode layers 22 on the second side surface 14 side in the stacking (T) direction. Then, along the virtual line OS4, the regions on both sides of the width (W) direction of the virtual line OS4 including the intersection neighborhood region 440 are divided into three equal parts in the stacking direction, and are divided into three regions: an upper region H1, a central region H2, and a lower region H3. As shown in FIG. 24, the second dielectric ceramic layer 20b and the third dielectric ceramic layer 42 are imaged with a field of view size of 4.3 μm×3.2 μm in a range of 5 μm on both sides of the width (W) direction of the virtual line OS4, and the areas of 20 dielectric particles are measured by image processing for each of the regions F1, F2, and F3. The reference symbol 42H in FIG. 24 indicates the imaged region. Then, the circle equivalent diameter is calculated from the measured area and the average is taken to obtain the average particle diameter. The average particle diameter was measured in each of the upper region H1, the central region H2, and the lower region H3, and since no significant difference was found between the measured values, the average particle diameter in the central region H2 is regarded as the average particle diameter in the region 440 near the intersection.

[0164] Test Examples 2-1 to 2-24 shown in Table 3 were prepared as multilayer ceramic capacitors corresponding to the above-mentioned (C) to (I). In addition, in Test Examples 2-25 to 2-27, the average particle diameter of the dielectric particles contained in the intersection neighborhood region 440 was larger than the average particle diameter of the dielectric particles contained in the first dielectric ceramic layer 20a, the average particle diameter of the dielectric particles contained in the second dielectric ceramic layer 20b, and the average particle diameter of the dielectric particles contained in the third dielectric ceramic layers 41 and 42. For these Test Examples 2-1 to 2-27, the average particle diameters were examined by the above-mentioned measurement method.

[0165] In Table 3, in the section comparing average particle sizes, "first" is the average particle size of the dielectric particles contained in the first dielectric ceramic layer, "second" is the average particle size of the dielectric particles contained in the second dielectric ceramic layer, "third" is the average particle size of the dielectric particles contained in the third dielectric ceramic layer, and "intersection" is the average particle size of the dielectric particles contained in the region near the intersection.

[0166] On the other hand, for the multilayer ceramic capacitors of test examples 2-25 to 2-27, the resistance value (kΩ) was measured in a state where a voltage of 6.3 V was applied in an environment of room temperature 150°C, and the MTTF (mean time to failure) was examined and judged. The MTTF was the point at which the resistance value became 10 kΩ or less, and when the MTTF was 15.3 hours (hr) or less, it was judged as ×, when it was more than 15.3 hours (hr) to 30 hours, it was judged as ◯ (good), and when it was more than 30 hours, it was judged as ◎ (excellent). The results are also shown in Table 3. Note that when the coverage of the internal electrode layer was less than 80%, it was deemed impossible to measure because it was difficult to obtain the electrostatic capacitance.

[0167] [Table 3]

[0168] According to Table 3, it was confirmed that when the average particle size of the dielectric particles contained in the region near the intersection is smaller than the average particle size of the dielectric particles contained in each of the first dielectric ceramic layer, the second dielectric ceramic layer, and the third dielectric ceramic layer, the MTTF becomes larger and the reliability of the multilayer ceramic capacitor is improved.

[0169] [3] Manufacturing method including an additional step of removing the side surface of the laminate In the above-described method for manufacturing the multilayer ceramic capacitor 1 of the present invention, in order to obtain the green chip 110 which is the unsintered laminate 10, the following steps are performed: printing the unsintered first internal electrode layer 121 and the second internal electrode layer 122 on the unsintered first dielectric ceramic layer 120a; forming the unsintered second dielectric ceramic layer 120b in the area of ​​the first dielectric ceramic layer 120a other than the area where the first internal electrode layer 121 and the second internal electrode layer 122 are printed; and stacking a plurality of the first dielectric ceramic layers 120a to form a green chip. The method includes the steps of forming a lean chip 110, exposing the first internal electrode layer 121 and the second internal electrode layer 122, the first dielectric ceramic layer 120a, and the second dielectric ceramic layer 120b from the first side 113 and the second side 114 of each green chip 110 by cutting the mother block 104, and bonding an unsintered third dielectric ceramic layer (side margin portions 41 and 42) to the first side 113 and the second side 114 of each green chip 110. Here, the green chip 110 is an example of a laminate. The first dielectric ceramic layer 120a is an example of a dielectric layer. The first internal electrode layer 121 and the second internal electrode layer 122 are an example of an internal electrode pattern. The second dielectric ceramic layer 120b is an example of a dielectric pattern. The first side surface 113 and the second side surface 114 are an example of a side surface. The side margin portions 41 and 42, which are the unsintered third dielectric ceramic layer, are an example of a dielectric gap layer.

[0170] In this manufacturing method, after the step of exposing the first internal electrode layer 121 and the second internal electrode layer 122, the first dielectric ceramic layer 120a, and the second dielectric ceramic layer 120b from the first side surface 113 and the second side surface 114 of the green chip 110 by cutting the mother block 104, and before the step of forming a third dielectric ceramic layer by bonding it to the first side surface 113 and the second side surface 114 of the green chip 110, a removal step of removing a certain degree of thickness from the first side surface 113 and the second side surface 114 can be added. As a result, the side surfaces of the first dielectric ceramic layer 120a, the second dielectric ceramic layer 120b, the first internal electrode layer 121, and the second internal electrode layer 122 exposed to the first side surface 113 and the second side surface 114 are removed.

[0171] FIG. 25 shows a state in which the first side 113 and the second side 114 of the green chip 110 are removed by a certain thickness (for example, 1 μm or less) and flattened. In FIG. 25, the left side shows the state before the removing process, and the right side shows the state after the removing process. When the mother block 104 is cut to obtain a plurality of green chips 110, the first side 113 and the second side 114 of the green chip 110 may flow slightly downward and be plastically deformed as shown in FIG. 25 due to stress applied to the lower side in the figure, which is the cutting direction. In addition, the cut surface may not be sufficiently smooth, or foreign matter may be present on the cut surface. Therefore, a thickness is removed to the extent that the deformed portion is eliminated. The means for removing the first side 113 and the second side 114 in this way is not limited, but for example, polishing by an appropriate polishing means is preferable.

[0172] 26, the first side surface 113 and the second side surface 114 after the above-mentioned removing step are formed into smooth surfaces from which foreign matter has been removed. A third dielectric ceramic layer (side margin portions 41 and 42) is formed by bonding to the first side surface 113 and the second side surface 114 after the removing step.

[0173] In the present invention, each of the second dielectric ceramic layer 20b, the first internal electrode layer 21, and the second internal electrode layer 22 may contain a resin. The resin can be contained by adding it to the materials used during production. That is, the resin is contained in the dielectric paste of the second dielectric ceramic layer 20b, and the resin is contained in the conductive paste of the first internal electrode layer 21 and the second internal electrode layer 22.

[0174] Resins contained in the dielectric paste and conductive paste are added for the purpose of functioning as a binder, improving the viscosity of the material, etc. Examples of such resins include, but are not limited to, polyvinyl acetal resins such as polyvinyl butyral and polyvinyl acetoacetal, polyvinyl alcohol-based resins such as polyvinyl alcohol, cellulose-based resins such as methyl cellulose, ethyl cellulose, and cellulose acetate phthalate, (meth)acrylic resins such as (meth)acrylic acid esters, imide-based resins such as polyamide-imide and polyimide, ethylene-based resins such as polyethylene oxide, nitrile-based resins such as polyacrylonitrile and polymethallonitrile, urethane-based resins such as polyurethane, vinyl-based resins such as polyethylene, polypropylene, and vinyl acetate, and rubber-based resins such as styrene butadiene rubber.

[0175] In addition, the resin content in the second dielectric ceramic layer 20b is preferably different from the resin content in the first dielectric ceramic layer 20a. The resin content in the first dielectric ceramic layer 20a and the second dielectric ceramic layer 20b is preferably, for example, 30 wt% to 50 wt%. It is preferable that the resin contents of the first dielectric ceramic layer and the second dielectric ceramic layer 20b are different from each other within this range.

[0176] In the method for manufacturing a multilayer ceramic capacitor of the present invention, the thickness of the first dielectric ceramic layer 120a is preferably 0.4 μm or more and 0.8 μm or less. In the method for manufacturing a multilayer ceramic capacitor of the present invention, the thickness of the first internal electrode layer 121 and the second internal electrode layer 122 is preferably 0.4 μm or more and 0.8 μm or less.

[0177] In addition, when forming the green chip 110, a part of the second internal electrode layer 122 may overlap a part of the first internal electrode layer 121 and the second internal electrode layer 122. Specifically, the end portions of the second dielectric ceramic layer 120b, the first internal electrode layer 121, and the second internal electrode layer 122 adjacent to each other in the length (L) direction may overlap each other. For example, as shown in FIG. 27, the end portion of the second dielectric ceramic layer 120b may overlap the end portion of the first internal electrode layer 121 in the length (L) direction. Similarly, the end portion of the second dielectric ceramic layer 120b may overlap the end portion of the second internal electrode layer 122. In such an embodiment in which the end portions in the length (L) direction overlap, the end portion of the first internal electrode layer 121 and the end portion of the second dielectric ceramic layer 120b may overlap the end portion of the second dielectric ceramic layer 120b.

[0178] The method for manufacturing a multilayer ceramic capacitor of the present invention involves removing a certain thickness from the first side 113 and the second side 114 of the green chip 110, which is the unsintered laminate 10, and then attaching an unsintered third dielectric ceramic layer to the first side 113 and the second side 114. This allows the unsintered third dielectric ceramic layer to be formed in a smooth and clean state on the first side 113 and the second side 114.

[0179] In the manufacturing method of the multilayer ceramic capacitor of the present invention, by removing first side 113 and second side 114 by polishing, first side 113 and second side 114 can be easily and accurately removed by a predetermined thickness.

[0180] In the method for manufacturing a multilayer ceramic capacitor of the present invention, the second dielectric ceramic layer 120b contains a resin, and the amount of the resin is preferably greater than the amount of resin contained in the first internal electrode layer 121 and the second internal electrode layer 122. This makes it possible to relatively increase the viscosity of the second dielectric ceramic layer 120b, and to suppress the occurrence of defects such as cracks and chips on the cut surface of the second dielectric ceramic layer 20b when the mother block 104 is cut.

[0181] In the method for manufacturing a multilayer ceramic capacitor of the present invention, the thickness of the first dielectric ceramic layer 120a is preferably 0.4 μm or more and 0.8 μm or less. In the method for manufacturing a multilayer ceramic capacitor of the present invention, the thickness of the first internal electrode layer 121 and the second internal electrode layer 122 is preferably 0.4 μm or more and 0.8 μm or less. By having the unfired dielectric layers and internal electrode layers have such thicknesses, the first dielectric ceramic layer 20a, the first internal electrode layer 21 and the second internal electrode layer 22 after firing can be formed to appropriate thicknesses.

[0182] In the method for manufacturing a multilayer ceramic capacitor of the present invention, a part of the second internal electrode layer 122 may overlap the first internal electrode layer 121 and the second internal electrode layer 122. This allows the second dielectric ceramic layer 20b to be arranged with a sufficient thickness without any gaps after firing.

[0183] [4] Defective portion of the second dielectric ceramic layer 28 and 29, in the multilayer ceramic capacitor 1 of the present invention, a missing portion 520, where a part of the second dielectric ceramic layer 20b is missing, is provided between at least one second dielectric ceramic layer 20b and one of the third dielectric ceramic layers 42. Similarly, a missing portion 520, where a part of the second dielectric ceramic layer 20b is missing, is provided between at least one second dielectric ceramic layer 20b and the other third dielectric ceramic layer 41.

[0184] The missing portion 520 is formed in at least one of the regions in which the second dielectric ceramic layer 20b is arranged, i.e., in the length (L) direction of the laminate 10, between an end of the first internal electrode layer 21 that is not connected to the second external electrode 52 and the second external electrode 52, and between an end of the second internal electrode layer 22 that is not connected to the first external electrode 51 and the first external electrode 51, between the first dielectric ceramic layers 20a in the stacking (T) direction in a plane including the stacking (T) direction and the width (W) direction, and between the second dielectric ceramic layer 20b and the third dielectric ceramic layer 41 or 42 in the width (W) direction.

[0185] When producing the green chip 110, which is the unsintered laminate 10, the side surface of the unsintered second dielectric ceramic layer 120b is processed and then fired to obtain the laminate 10 having a defect 520 on the side surface of the second dielectric ceramic layer 20b. Any processing method can be used to obtain the defect 520, and it can be formed, for example, by drilling with an appropriate tool.

[0186] Furthermore, in the above-mentioned "manufacturing method adding a step of removing the side surface of the laminate", when the first side surface 113 or the second side surface 114 of the unsintered green chip 110 is removed by means of polishing or the like, a part of the side surface of the second dielectric ceramic layer 20b may be chipped off, resulting in a minute hole. When such a hole is generated, the hole can be made into a missing portion 520. The missing portion 520 does not have to be formed on all the side surfaces of the second internal electrode layer 22, and it is sufficient that at least one missing portion 520 is formed on each of the first side surface 13 side and the second side surface 14 side at both ends in the length (L) direction.

[0187] 28 and 29, a segregation of Si 530 may be arranged in the defect portion 520. The segregation of Si 530 is a segregation of Si added as an additive to the second dielectric ceramic layer 20b.

[0188] The size of the Si segregation 530, in terms of the diameter of an equivalent circle, is preferably larger than ⅓ of the thickness of the second dielectric ceramic layer 20b, and may be 100 nm or more and 600 nm or less.

[0189] The missing portion 520 is preferably disposed adjacent to the first internal electrode layer 21 or the second internal electrode layer 22. In Fig. 29, the missing portion 520 is disposed adjacent to an end portion in the length (L) direction of the second internal electrode layer 22. Similarly, it is preferable that the missing portion 520 is disposed adjacent to an end portion in the length (L) direction of the first internal electrode layer 21.

[0190] The size of the Si segregation 530 in the width (W) direction is preferably 0.1% to 5% of the size of the third dielectric ceramic layers 41 and .

[0191] The multilayer ceramic capacitor 1 of the present invention has a missing portion 520 in a plane including the stacking (T) direction and the width (W) direction, in a region where the second dielectric ceramic layer 20b is arranged, i.e., in at least one of regions between an end of the first internal electrode layer 21 and the second external electrode 52, and between an end of the second internal electrode layer 22 not connected to the first external electrode 51 and the first external electrode 51, between the first dielectric ceramic layers 20a in the stacking (T) direction, and between the second dielectric ceramic layer 20b and the third dielectric ceramic layers 41 and 42 in the width (W) direction.

[0192] This makes it possible to alleviate stress generated in the second dielectric ceramic layer 20b during firing by the missing portion 520. As a result, it is possible to prevent cracks or chips from occurring in the second dielectric ceramic layer 20b.

[0193] In the multilayer ceramic capacitor 1 of the present invention, a Si segregation 530 may be disposed in the defect 520. When the segregation 530 is present in the defect 520, the segregation 530 suppresses the intrusion of moisture. The presence of the segregation 530 in the defect 520 improves the moisture resistance of the multilayer ceramic capacitor 1. The segregation 530 may be present in the entire defect 520, or may be present in a part of the defect 520. The defect 520 in which the segregation 530 is present can suppress the occurrence of cracks or chips in the second dielectric ceramic layer 20b, and can also improve the moisture resistance of the multilayer ceramic capacitor 1.

[0194] In the multilayer ceramic capacitor 1 of the present invention, the Si segregation 530 is equal to or greater than (or less than) ⅓ of the thickness of the second dielectric ceramic layer 20b.

[0195] In the multilayer ceramic capacitor 1 of the present invention, the missing portion 520 is disposed adjacent to the first internal electrode layer 21 and the second internal electrode layer 22. The regions adjacent to the first internal electrode layer 21 and the second internal electrode layer 22 are subjected to a relatively large stress during firing, but the stress is mitigated by the missing portion 520, so that the occurrence of cracks and chips can be effectively suppressed.

[0196] In the multilayer ceramic capacitor 1 of the present invention, the dimension of the Si segregation 530 in the width direction is preferably 0.1% to 5% of the dimension of the third dielectric ceramic layers 41 and 42. When the Si segregation 530 is present in the defect portion 520, the occurrence of cracks and chips can be effectively suppressed, and the moisture resistance of the multilayer ceramic capacitor 1 can also be improved.

[0197] [5] Segregation formed at the end of the second dielectric ceramic layer on the internal electrode layer side 30, in the multilayer ceramic capacitor 1 of the present invention, a first segregation 610 may be present at an end portion in the length (L) direction of the first internal electrode layer 21 that is not connected to the second external electrode 52. Also, a first segregation 610 may be present at an end portion in the length (L) direction of the second internal electrode layer 22 that is not connected to the first external electrode 51.

[0198] As shown in Fig. 31, the first segregation 610 is generated by the segregation of metal elements 610a originating from the second dielectric ceramic layer 20b in a layered manner. The metal elements 610a include, for example, at least one of Mg, Mn, and Si. The segregation 610 due to the metal elements 610a is generated when the metal elements contained in the second dielectric ceramic layer 20b move to the first internal electrode layer 21 and the second internal electrode layer 22 during firing of the second dielectric ceramic layer 20b.

[0199] 32, a second segregation 620 may be present at an end portion in the width (W) direction of the first internal electrode layer 21. Also, a second segregation 620 may be present at an end portion in the width (W) direction of the second internal electrode layer 22.

[0200] The second segregation 620 is generated by the segregation of metal elements 620a originating from the third dielectric ceramic layers 41 and 42 in contact with the first internal electrode layer 21 and the second internal electrode layer 22 in a layered manner. The metal elements 620a are, for example, at least one of Mg, Mn, and Si, similar to the first segregation 610. The segregation 620 due to the metal elements 620a is generated by the migration of the metal elements contained in the third dielectric ceramic layers 41 and 42 to the first internal electrode layer 21 and the second internal electrode layer 22 during firing of the third dielectric ceramic layers 41 and 42.

[0201] In the multilayer ceramic capacitor 1 of the present invention, it is preferable that the metal element contained in at least one set of segregations among the first segregation 610 segregated in the first internal electrode layer 21, the first segregation 610 segregated in the second internal electrode layer 22, the second segregation 620 segregated in the first internal electrode layer 21, and the second segregation 620 segregated in the second internal electrode layer 22 is different from the metal elements contained in the other segregations.

[0202] When the first dielectric ceramic layer 20a is mainly composed of BaTiO3, the content of the metal element contained in the first segregation 610 in the first internal electrode layer 21 and the second internal electrode layer 22 is 0.3 mol % or more relative to 100 mol of Ti. Similarly, the content of the metal element contained in the second segregation 620 in the first internal electrode layer 21 and the second internal electrode layer 22 is 0.3 mol % or more relative to 100 mol of Ti.

[0203] In the present invention, the region in which the first segregation 610 exists in the first internal electrode layer 21 preferably has a length of 0.1 μm or more along its length (L). Also, the region in which the first segregation 610 exists in the second internal electrode layer 22 preferably has a length of 0.1 μm or more along its length (L). Also, the region in which the second segregation 620 exists in the first internal electrode layer 21 preferably has a length of 0.1 μm or more along its width (W). Also, the region in which the second segregation 620 exists in the second internal electrode layer 22 preferably has a length of 0.1 μm or more along its width (W). By having these lengths, the effect of suppressing electric field concentration by segregation and improving reliability can be reliably obtained.

[0204] Regarding the length of the first segregation 610 and the second segregation 620, if it is shorter than the above length, it becomes difficult to suppress the electric field concentration. Furthermore, if the length of the first segregation 610 exceeds 0.5% in the length (L) direction, or if the length of the second segregation 620 exceeds 1.0% in the width (W) direction, the amount of segregated metal elements (at least one of Mg, Mn, and Si) becomes excessive, and the function of storing electric charge in the internal electrode layer decreases.

[0205] The length in the length (L) direction of the first segregation 610 can be controlled by adjusting the content of the metal element 610a that is contained in the second dielectric ceramic layer 20b and migrates to and segregates in the first internal electrode layer 21 and the second internal electrode layer 22. The length in the width (W) direction of the second segregation 620 can be controlled by adjusting the content of the metal element 620a that is contained in the third dielectric ceramic layers 41 and 42 and migrates to and segregates in the first internal electrode layer 21 and the second internal electrode layer 22.

[0206] In the multilayer ceramic capacitor 1 of the present invention, a first segregation 610 of at least one metal element selected from Mg, Mn, and Si is present at each of the ends of the first internal electrode layer 21 in the length (L) direction that is not connected to the second external electrode 52 and the ends of the second internal electrode layer 22 in the length (L) direction that is not connected to the first external electrode 51.

[0207] An electric field is likely to concentrate at the ends in the length (L) direction of each of the first internal electrode layer 21 and the second internal electrode layer 22 that are in contact with the second dielectric ceramic layer 20b, and if electric field concentration occurs, there is a risk of reducing the reliability of the multilayer ceramic capacitor. However, in the multilayer ceramic capacitor 1 of the present invention, the first segregation 610 suppresses electric field concentration, and the reliability can be improved.

[0208] In the multilayer ceramic capacitor 1 of the present invention, a second segregation 620 of at least one metal element selected from Mg, Mn, and Si is present at each of the ends in the width (W) direction of the first internal electrode layer 21 and the ends in the width (W) direction of the second internal electrode layer 22.

[0209] An electric field is likely to concentrate at the ends in the width (W) direction of each of the first internal electrode layer 21 and the second internal electrode layer 22 in contact with the third dielectric ceramic layers 41 and 42, and the occurrence of electric field concentration may reduce the reliability of the multilayer ceramic capacitor. However, in the multilayer ceramic capacitor 1 of the present invention, the electric field concentration is suppressed by the second segregation 620, and therefore the reliability can be improved.

[0210] In the multilayer ceramic capacitor 1 of the present invention, the metal elements contained in at least one set of segregations among the first segregation 610 segregated in the first internal electrode layer 21, the first segregation 610 segregated in the second internal electrode layer 22, the second segregation 620 segregated in the first internal electrode layer 21, and the second segregation 620 segregated in the second internal electrode layer 22 are different from the metal elements contained in the other segregations.

[0211] This allows optimal metal elements to be arranged in accordance with the locations where the first segregation region 610 and the second segregation region 620 are arranged, thereby improving reliability.

[0212] In the multilayer ceramic capacitor 1 of the present invention, the first dielectric ceramic layer 20a contains Ba and Ti, and the content of the metal element 610a contained in the first segregation 610 and the metal element 620a contained in the second segregation 620 in the internal electrode layer is 0.3 mol % or more relative to 100 mol of Ti.

[0213] This makes it possible to effectively suppress the electric field concentration described above, and further improve reliability.

[0214] In the multilayer ceramic capacitor 1 of the present invention, the region in the first internal electrode layer 21 where the first segregation 610 exists is preferably 0.3 μm or more in the length (L) direction, the region in the second internal electrode layer 22 where the first segregation 610 exists is preferably 0.3 μm or more in the length (L) direction, the region in the first segregation 610 where the second segregation 620 exists is preferably 0.3 μm or more in the width (W) direction, and the region in the second segregation 620 where the second segregation 620 exists is preferably 0.3 μm or more in the width (W) direction.

[0215] This reliably achieves the effect of suppressing electric field concentration through segregation and improving reliability.

[0216] [Test Example 3] Next, a third test example will be described, which examines the effects of the first segregation 610 and the second segregation 620 in the multilayer ceramic capacitor 1 of the present invention.

[0217] As shown in Table 4, test examples 3-1 to 3-18 of multilayer ceramic capacitors having the second dielectric ceramic layer 20b and the third dielectric ceramic layers 41 and 42 containing any one of Mg, Mn, and Si elements were prepared. Then, for each test example, the element concentration of the first segregation generated at the end in the length (L) direction of the first internal electrode layer 21 and the second internal electrode layer 22, the length in the length (L) direction, and the length in the width (W) direction were examined. The metal element concentrations of the first segregation and the second segregation were examined using the same method as the concentration of the second alloy part and the concentration of the third alloy part in the above-mentioned "Test Example 1". In addition, the respective lengths of the first segregation and the second segregation were measured by EDX analysis.

[0218] The multilayer ceramic capacitors of Test Examples 3-1 to 3-18 were heated for 1 hour in an environment at 150°C and then cooled to room temperature, and the resistance value (kΩ) was measured and the MTTF (mean time to failure) was examined while applying a voltage of 6.3 V. In addition, the presence or absence of a decrease in capacitance was examined using an LCR meter (Keysight: E4980). A capacitance drop of 3% or more or an MTTF of 15.3 hours or less was rated as ×, a capacitance drop of less than 3% and an MTTF of more than 15.3 hours but less than 30 hours was rated as ◯ (good), and a capacitance drop of less than 3% and an MTTF of more than 30 hours was rated as ◎ (excellent). The results are shown in Table 4.

[0219] [Table 4]

[0220] By including Mg, Mn, and Si in the second dielectric layer, segregation is created at the length and width ends of the internal electrodes, eliminating the cause of reduced reliability that tends to occur at the ends. However, if the content is too high, the area that functions as a metal in the internal electrodes narrows, resulting in a decrease in capacitance.

[0221] [6] Segregation formed in the corner region of the second dielectric ceramic layer on the internal electrode layer side In the case where the above-described first segregation 610 and second segregation 620 are present, it is preferable that a third segregation 630 is further present as shown in Fig. 33. The third segregation 630 is present in each of the first corner region 710 and the second corner region 720.

[0222] The first corner region 710 is a region in the first internal electrode layer 21 where the length (L) direction in which the first segregation 610 exists overlaps with the width (W) direction of the second segregation 620. The second corner region 720 is a region in the second internal electrode layer 22 where the length (L) direction in which the first segregation 610 exists overlaps with the width (W) direction of the second segregation 620. The third segregation 630 is generated by segregation of the metal element 610a of the first segregation 610 and the metal element 620a of the second segregation 620.

[0223] In the present invention, it is preferable that the metal element 610a contained in the first segregation 610 and the metal element 620a contained in the second segregation 620 are different from each other, and the metal element 630a of the third segregation 630 contains both the metal element 610a contained in the first segregation 610 and the metal element 620a contained in the second segregation 620.

[0224] In the present invention, the region in which the first segregation 610 exists is It is preferable that the region where the second segregation 620 exists is 0.1 μm or more in the width (W) direction.

[0225] 33 shows a plane including the length (L) direction and the width (W) direction in the multilayer ceramic capacitor 1 of the present invention. In the plane including the length (L) direction and the width (W) direction, the third segregation 630 is preferably segregated in a substantially right-angled triangular shape so that the area of ​​the third segregation 630 becomes larger toward the end in the length (L) direction. A part or the whole of the third segregation 630 is included in the intersection neighborhood region 440 in FIG. 19.

[0226] In the multilayer ceramic capacitor 1 of the present invention, the second dielectric ceramic layer 20b is preferably disposed so that a part of the second dielectric ceramic layer 20b overlaps with the region where the third segregation 630 exists in the stacking (T) direction with respect to the first internal electrode layer 21 and the second internal electrode layer 22. Specifically, as shown in FIG. 34, an embodiment in which an end of the second dielectric ceramic layer 120b overlaps with an end of the second internal electrode layer 22 in the region including the third segregation 630 in the length (L) direction may be mentioned. Similarly, the end of the second dielectric ceramic layer 20b may overlap with an end of the first internal electrode layer 21. In such an embodiment in which the end portions in the length (L) direction overlap, the end of the first internal electrode layer 121 or the end of the second dielectric ceramic layer 120b may overlap with the end of the second dielectric ceramic layer 20b.

[0227] In the multilayer ceramic capacitor 1 of the present invention, a first segregation 610 of at least one metal element selected from Mg, Mn, and Si is present at each of the ends in the length (L) direction of the first internal electrode layer 21 that are not connected to the second external electrode 52 and the ends in the length (L) direction of the second internal electrode layer 22 that are not connected to the first external electrode 51, and at each of the ends in the width (W) direction of the first internal electrode layer 21 and the ends in the width (W) direction of the second internal electrode layer 22, at least one metal element selected from Mg, Mn, and Si is present. A second segregation 620 caused by one type of metal element is present, and a third segregation 630 caused by each of the metal elements of the first segregation 610 and the second segregation 620 is present in each of a first corner region 710 in the first internal electrode layer 21 where an end portion in the length (L) direction in which the first segregation 610 is present overlaps with a width (W) direction in which the second segregation 620 is present, and a second corner region 720 in the second internal electrode layer 22 where an end portion in the length (L) direction in which the first segregation 610 is present overlaps with a width (W) direction in which the second segregation 620 is present.

[0228] An electric field is likely to concentrate in the first corner region 710 and the second corner region 720, and if electric field concentration occurs, there is a risk of reducing the reliability of the multilayer ceramic capacitor. However, in the multilayer ceramic capacitor 1 of the present invention, the third segregation 630 suppresses the electric field concentration in the first corner region 710 and the second corner region 720, and therefore the reliability can be improved.

[0229] In the multilayer ceramic capacitor 1 of the present invention, the metal element 610a contained in the first segregation 610 and the metal element 620a contained in the second segregation 620 are different from each other, and the metal element contained in the third segregation 630 includes both the metal element 610a contained in the first segregation 610 and the metal element 620a contained in the second segregation 620.

[0230] As a result, the third segregation 630 suppresses electric field concentration in the first corner region 710 and the second corner region 720, thereby improving reliability.

[0231] In the third segregation 630, the metal element disposed on the side adjacent to the third dielectric ceramic layers 41 and 42 is preferably Mg. On the other hand, in the third segregation 630, the metal element disposed on the side adjacent to the second dielectric ceramic layer 20b is preferably Si from the viewpoint of the possibility of improving moisture resistance. Therefore, it is preferable that both Mg and Si are segregated in the first corner region 710 and the second corner region 720. In addition, the first segregation 610 at the end of the first internal electrode layer 21 and the second internal electrode layer 22 in the width (W) direction may cause short circuit recovery. In addition, it is more preferable that Sn is solid-solved in the first internal electrode layer 21 and the second internal electrode layer 22.

[0232] In the multilayer ceramic capacitor 1 of the present invention, the region where the first segregation 610 exists is 0.1 μm or more in the length (L) direction, and the region where the second segregation 620 exists is 0.1 μm or more in the width (W) direction. This reliably achieves the effect of suppressing electric field concentration by the segregation, thereby improving reliability.

[0233] In the multilayer ceramic capacitor 1 of the present invention, the third segregation 630 has an area in which it exists that becomes larger toward the end in the length (L) direction in a plane including the length (L) direction and the width (W) direction.

[0234] This increases the area of ​​the third segregation 630 at the end portion in the length (L) direction of the second dielectric ceramic layer 20b where electric field concentration is likely to occur, thereby more effectively suppressing the electric field concentration caused by the third segregation 630 and further improving reliability.

[0235] In the multilayer ceramic capacitor 1 of the present invention, the second dielectric ceramic layer 20b is arranged relative to the first internal electrode layer 21 and the second internal electrode layer 22 so that a portion of the second dielectric ceramic layer 20b overlaps with the region in which the third segregation 630 exists in the stacking (T) direction.

[0236] This makes it easier to form the third segregation 630 so that its presence area becomes larger toward the end in the length (L) direction in a plane including the length (L) direction and the width (W) direction.

[0237] [Test Example 4] Next, a fourth test example for verifying the effect of the third segregation 630 in the multilayer ceramic capacitor 1 of the present invention will be described.

[0238] As shown in Table 5, test examples 4-1 to 4-18 of multilayer ceramic capacitors having a second dielectric ceramic layer containing any one of the metal elements Mg, Mn, and Si, and a third dielectric ceramic layer containing any one of the metal elements Mg, Mn, and Si, were prepared. Then, the concentration of the metal element contained in the third segregation generated in the first corner region and the second corner region of each multilayer ceramic capacitor, the length in the length (L) direction, and the length in the width (W) direction were examined. The concentration of the metal element in the third segregation was examined using the same method as the concentration of the second alloy part and the concentration of the third alloy part in the above-mentioned "Test Example 1". In addition, the length of each of the third segregations was measured by EDX analysis.

[0239] For the multilayer ceramic capacitors of test examples 4-1 to 4-14, the resistance value (kΩ) was measured under a condition of applying a voltage of 6.3 V in an environment of room temperature 150°C, and the MTTF (mean time to failure) was examined and judged. The MTTF was the point at which the resistance value became 10 kΩ or less, and when the MTTF was 15.3 hours (hr) or less, it was judged as ×, when it was more than 15.3 hours (hr) to 30 hours, it was judged as ◯ (good), and when it was more than 30 hours, it was judged as ◎ (excellent). The results are also shown in Table 5. In addition, the presence or absence of a decrease in capacitance was checked using an LCR meter (Keysight: E4980), and when a capacitance decrease of 3% or more was shown, it was judged as ×. Note that when the coverage of the internal electrode layer was less than 80%, it was difficult to obtain the capacitance, so it was not possible to measure it.

[0240] [Table 5]

[0241] By including Si, Mg, and Mn in the second and third ceramic dielectric layers, it is possible to create many segregation regions at the corners. Electric field concentration occurs particularly at the corners, which tends to reduce reliability, but by creating segregation regions, reliability can be improved. However, if the content is too high, the area that functions as a metal in the internal electrodes will become narrower, resulting in a decrease in capacitance.

[0242] [7] Thickness of the second dielectric ceramic layer FIG. 35 shows a schematic WT cross section of the laminate 10 in the multilayer ceramic capacitor 1 of the present invention at the center in the length (L) direction, with the thickness of the first dielectric ceramic layer 20a in this cross section shown as T1 and the thickness of the end in the width (W) direction shown as T2.

[0243] 36 shows a part of the LT cross section of the multilayer ceramic capacitor 1 of the present invention, where T3 is the thickness of the second dielectric ceramic layer 20b. Although FIG. 36 shows the second dielectric ceramic layer 20b in contact with the second internal electrode layer 22, the thickness of the second dielectric ceramic layer 20b in contact with the first internal electrode layer 21 is also considered to be T3. In other words, the thickness T3 of the second dielectric ceramic layer 20b is the thickness between the end of the first internal electrode layer 21 in the length (L) direction that is not connected to the second external electrode 52 and the second external electrode 52, and between the end of the second internal electrode layer 22 in the length (L) direction that is not connected to the first external electrode 51 and the second external electrode 52.

[0244] In the present invention, the difference in thickness between T1 and T2 is relatively small, within 10% of T1. In contrast, the thickness of T3 is larger than T1 and T2, and the difference therebetween is preferably 10% or more of T1 and T2.

[0245] There is no limitation on the means for making the thickness T3 of the second dielectric ceramic layer 20b thicker than the thicknesses T1 and T2 of the first dielectric ceramic layer 20a as described above, but for example, when producing the green chip 110 before sintering, it is possible to overlap the end in the length (L) direction of the unsintered second dielectric ceramic layer 120b with the end in the length (L) direction of the unsintered first internal electrode layer 121 and second internal electrode layer 122, and then sinter the green chip 110.

[0246] Of T1, T2 and T3, the thickness T1 of the central portion of the first dielectric ceramic layer 20a is preferably 0.7 μm or less, and the thickness T3 of the second dielectric ceramic layer 20b is preferably 0.4 μm or more.

[0247] In the multilayer ceramic capacitor 1 of the present invention, if the thickness of the first dielectric ceramic layer 20a at the center in the length (L) direction and at the center in the stacking (T) direction on a plane including the stacking (T) direction and the width (W) direction is T1, the thickness of the end portion of the first dielectric ceramic layer 20a in the width (W) direction is T2, and the thickness between the end portion in the length (L) direction of the first internal electrode layer 21 that is not connected to the second external electrode 52 and the second external electrode 52, and the thickness between the end portion in the length (L) direction of the second internal electrode layer 22 that is not connected to the first external electrode 51 and the first external electrode 51 are T3, the difference in thickness between T1 and T2 is within 10% of T1, and the thickness of T3 is larger than T1 and T2, and the difference between them is 10% or more of T1 and T2.

[0248] As a result, the element thickness of the second dielectric ceramic layer 20b arranged between the first dielectric ceramic layers 20a sandwiching the first internal electrode layer 21 and the second internal electrode layer 22 for eliminating the step has a sufficient thickness, thereby improving reliability. [Explanation of symbols]

[0249] 1. Multilayer ceramic capacitors 10 Laminate 11 First main surface of laminate 12 Second main surface of laminate 13 First side (side) of laminate 14 Second side (side) of laminate 15 First end surface of laminate 16 Second end surface of laminate 20 Dielectric ceramic layer 20a: first dielectric ceramic layer 20b Second dielectric ceramic layer 21 First internal electrode layer 22 Second internal electrode layer 30 Inner Layer 31, 32 outer layer 41, 42 Third dielectric ceramic layer 51 First external electrode 52 Second external electrode 520 Missing part 530 Segregation

Claims

1. a laminate including dielectric ceramic layers and internal electrode layers laminated in a lamination direction; and an external electrode connected to the internal electrode layer, The laminate has a first main surface and a second main surface opposed to each other in the stacking direction, a first side surface and a second side surface opposed to each other in a width direction perpendicular to the stacking direction, and a first end surface and a second end surface opposed to each other in a length direction perpendicular to the stacking direction and the width direction, the internal electrode layers include a first internal electrode layer extended to the first end surface, and a second internal electrode layer extended to the second end surface so as to face the first internal electrode layer via the dielectric ceramic layer, the external electrodes include a first external electrode disposed on the first end surface and connected to the first internal electrode layer, and a second external electrode disposed on the second end surface and connected to the second internal electrode layer, the dielectric ceramic layer comprises a first dielectric ceramic layer and a second dielectric ceramic layer; the first dielectric ceramic layer is disposed between the first internal electrode layer and the second internal electrode layer, the second dielectric ceramic layer is disposed so as to overlap the first dielectric ceramic layer in the stacking direction, including a region between the first dielectric ceramic layers opposed to each other via the internal electrode layer, in which the internal electrode layer is not disposed, and a part of the region overlaps the first dielectric ceramic layer; the laminate has an inner layer portion in which the first internal electrode layers and the second internal electrode layers are alternately laminated with the dielectric ceramic layers interposed therebetween, outer layer portions arranged to sandwich the inner layer portion in the lamination direction and made of a ceramic material, and a third dielectric ceramic layer arranged to sandwich the inner layer portion and the outer layer portion in the width direction and made of a dielectric ceramic material, In the longitudinal direction, in at least one of a region between an end portion of the first internal electrode layer that is not connected to the second external electrode and the second external electrode, and a region between an end portion of the second internal electrode layer that is not connected to the first external electrode and the first external electrode, a missing portion in which a part of the second dielectric ceramic layer is missing, the missing portion being located between the first dielectric ceramic layers in the stacking direction and between the second dielectric ceramic layer and the third dielectric ceramic layer in the width direction.

2. The multilayer ceramic capacitor according to claim 1 , wherein a segregation of Si is arranged in the defect portion.

3. 3. The multilayer ceramic capacitor according to claim 2, wherein the segregation of Si is equal to or greater than ⅓ of a thickness of the second dielectric ceramic layer.

4. 4. The multilayer ceramic capacitor according to claim 1, wherein the recess is disposed adjacent to the internal electrode layer.

5. 5. The multilayer ceramic capacitor according to claim 1, wherein a dimension of the Si segregation in the width direction is 0.1% to 5% of a dimension of the third dielectric ceramic layer.

Citation Information

Patent Citations

  • Method for manufacturing stacked ceramic electronic component

    JP2003209025A

  • Multilayer ceramic capacitor

    JP2017028013A

  • Method of manufacturing electronic component

    JP2017147358A

  • Multilayer ceramic capacitor

    JP2019009442A

  • Multilayer ceramic electronic component and manufacturing method of the same

    JP2019102578A