Method for manufacturing welded molded body, welded molded body and pipe

The described method addresses the challenge of bonding liquid crystal polyester by heating and vibration welding protruding portions with specific width ratios and burr filling rates, ensuring strong and reliable welded molded bodies.

JP7576030B2Active Publication Date: 2024-10-30SUMITOMO CHEM CO LTD
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2021533097
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-17
Filing Date
2020-07-16
Publication Date
2024-10-30
Estimated Expiration
2040-07-16

AI Technical Summary

Technical Problem

Liquid crystal polyester has a fast solidification rate during melting, leading to interfacial flow and the creation of new interfaces during welding, making it difficult to bond and resulting in insufficient strength at the welded portions of molded bodies.

Method used

A method involving the use of liquid crystal polyester for producing a welded molded body by heating protruding portions to a temperature above its flow start temperature, vibration welding these portions while pressing them together, and ensuring the width ratio of the protruding surfaces is between 90% to 110%, with a filling rate of burrs in the holding space of 20% or more and less than 100%, to enhance bonding strength.

Benefits of technology

This method allows for the production of a welded molded body with guaranteed strength at the welded portion, resulting in a highly reliable pipe with improved bonding integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576030000005
    Figure 0007576030000005
  • Figure 0007576030000006
    Figure 0007576030000006
  • Figure 0007576030000007
    Figure 0007576030000007
Patent Text Reader

Abstract

This method is for manufacturing a welded molding formed by using liquid crystal polyester as a material, the method comprising: a step for heating a first projection of a first member formed by using a liquid crystal polyester as a material and a second projection of a second member formed by using a liquid crystal polyester as a material, to a temperature equal to or higher than the flowing start temperatures of the respective liquid crystal polyesters; and a step for bringing the first and second projections into contact with each other and vibrating and welding the first and second projections while pressing the projections in directions bringing the two toward each other relatively.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a welded molded article, a welded molded article, and a pipe. This application claims priority based on Japanese Patent Application No. 2019-131629, filed on July 17, 2019, the contents of which are incorporated herein by reference. [Background technology]

[0002] In general, resin molded bodies having complex shapes are manufactured by injection molding each of the components that make up the desired resin molded body, and then welding the components together (see, for example, Patent Documents 1 and 2). An example of a "resin molded body having a complex shape" is a pipe through which a fluid flows. Moreover, a thermoplastic resin is used as a material for forming such resin molded bodies. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-171712 A [Patent Document 2] JP 2007-169379 A Summary of the Invention [Problem to be solved by the invention]

[0004] Among thermoplastic resins, liquid crystal polyester has excellent melt flowability, heat resistance, strength, and rigidity, and is therefore used as an injection molding material for manufacturing electrical and electronic components. Taking advantage of these properties, liquid crystal polyester is adopted for electrical and electronic components, mechanical components, etc., and its applications are expanding.

[0005] However, liquid crystal polyester has a high solidification rate when melted, and solidifies while interfacial flow occurs at the bonding interface during welding. Therefore, a new interface is generated at the bonding surface, making bonding difficult. In other words, even if multiple molded bodies using liquid crystal polyester are welded together, the strength of the welded parts is likely to be insufficient, and an improvement has been required.

[0006] The present invention has been made in consideration of the above circumstances, and aims to provide a method for manufacturing a welded molded body that uses liquid crystal polyester as a forming material and can suitably manufacture a welded molded body. Another aim is to provide a welded molded body in which the strength of the welded part is guaranteed. Another aim is to provide a pipe that is a welded molded body using liquid crystal polyester as a forming material and has high reliability. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention includes the following aspects.

[0008] [1] A method for producing a welded molded product using liquid crystal polyester as a forming material, the method comprising the steps of: heating a first convex streak portion of a first member using liquid crystal polyester as a forming material and a second convex streak portion of a second member using liquid crystal polyester as a forming material, to a temperature equal to or higher than the flow start temperature of the liquid crystal polyester; and bringing the first convex streak portion and the second convex streak portion into contact with each other and vibration welding the first convex streak portion and the second convex streak portion while pressing them in a direction such that they approach each other relatively.

[0009] [2] The first member has a first base, the first convex streak protruding from the first base, and a pair of first ribs provided on both sides of the first convex streak along the extension direction of the first convex streak and protruding on the same side of the first base as the first convex streak; the second member has a second base, the second convex streak protruding from the second base, and a pair of second ribs provided on both sides of the second convex streak along the extension direction of the second convex streak and protruding on the same side of the second base as the second convex streak; and in the vibration welding process, the first member and the second member are brought closer together until the first ribs and the second ribs abut.

[0010] [3] The method for manufacturing a welded molded body described in [2], in which the vibration welding process is terminated before molten resin leaks out from the space surrounded by the first convex ridge portion, the second convex ridge portion, the first rib, and the second rib.

[0011] [4] A method for producing a welded molded body according to any one of [1] to [3], wherein the width of the top surface of the first convex rib portion is 90% or more and 110% or less of the width of the top surface of the second convex rib portion.

[0012] [5] A welded molded body comprising a first member and a second member, the first member and the second member each made of liquid crystal polyester, and a welded portion formed by thermally welding the first member and the second member, the welded portion having a welded main body portion formed by thermally welding the first member and the second member, and a pair of ribs provided on both sides of the welded main body portion, a cylindrical retaining space being formed between the welded main body portion and the rib, the retaining space being filled with burrs formed of the liquid crystal polyester, and a filling rate of the burrs in the retaining space at a cross section intersecting the welded main body portion and the pair of ribs is 20% or more and less than 100%.

[0013] [6] A welded molded body comprising a first member and a second member, the first member and the second member each being made of liquid crystal polyester, and the tensile strength of the welded portion where the first member and the second member are heat-welded is 13 MPa or more.

[0014] [7] A pipe which is a welded molded article according to [5] or [6]. Effect of the Invention

[0015] According to the present invention, a method for manufacturing a welded molded product using liquid crystal polyester as a forming material, which enables a welded molded product to be suitably manufactured, can be provided. Also, a welded molded product with guaranteed strength at the welded portion can be provided. Also, a pipe that is a welded molded product using liquid crystal polyester as a forming material and has high reliability can be provided. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic perspective view showing a welded molded body in an embodiment. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 3 is a cross-sectional view taken along line III-III in FIG. [Figure 4] FIG. 4 is a schematic diagram showing the method for producing the welded molded article of this embodiment. [Diagram 5] FIG. 5 is a schematic diagram showing a method for producing a welded molded article according to this embodiment. [Figure 6] FIG. 6 is a schematic diagram showing a commonly known vibration welding process. [Figure 7] FIG. 7 is a schematic diagram showing a test piece used in the examples. [Figure 8] FIG. 8 is a schematic diagram showing a test piece used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] [Welded molded body] Hereinafter, a description will be given of a welded molded body and a welded molded body according to an embodiment of the present invention with reference to the drawings. In addition, in all the following drawings, the dimensions and ratios of each component are appropriately changed in order to make the drawings easier to understand.

[0018] The welded molded article of this embodiment is made of liquid crystal polyester.

[0019] [Liquid crystal polyester] The liquid crystal polyester used in this embodiment is one of thermotropic liquid crystal polymers, and is a polymer that can form a melt exhibiting optical anisotropy at a temperature of 450° C. or less.

[0020] The liquid crystal polyester of the present embodiment preferably has a repeating unit represented by the following general formula (1), and more preferably has a repeating unit (1), a repeating unit represented by the following general formula (2), and a repeating unit represented by the following general formula (3). Hereinafter, the repeating unit represented by the following general formula (1) may be referred to as "repeating unit (1)". The repeating unit represented by the following general formula (2) may be referred to as "repeating unit (2)". The repeating unit represented by the following general formula (3) may be referred to as "repeating unit (3)".

[0021] (1)-O-Ar 1 -CO- (2)-CO-Ar 2 -CO- (3)-X-Ar 3 -Y- (In the formula, Ar 1 represents a phenylene group, a naphthylene group or a biphenylylene group. 2 and Ar 3 each independently represents a phenylene group, a naphthylene group, a biphenylylene group, or a group represented by the following general formula (4). X and Y each independently represent an oxygen atom or an imino group (-NH-). Ar 1 , Ar 2 Or Ar 3 One or more hydrogen atoms in the group represented by the formula (I) may be independently substituted with a halogen atom, an alkyl group, or an aryl group.

[0022] (4)-Ar 4 -Z-Ar 5 - (In the formula, Ar4 and Ar 5 each independently represents a phenylene group or a naphthylene group. Z represents an oxygen atom, a sulfur atom, a carbonyl group, a sulfonyl group, or an alkylidene group.

[0023] Specific examples of the liquid crystal polyester used in the present embodiment include: (1) A polymer obtained by polymerizing a combination of an aromatic hydroxycarboxylic acid, an aromatic dicarboxylic acid, and an aromatic diol, (2) A polymer obtained by polymerizing a plurality of aromatic hydroxycarboxylic acids. (3) A polymer obtained by polymerizing a combination of an aromatic dicarboxylic acid and an aromatic diol. (4) Polymers obtained by reacting a crystalline polyester such as polyethylene terephthalate with an aromatic hydroxycarboxylic acid.

[0024] In the production of the liquid crystal polyester, a part or all of the aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid and aromatic diol used as raw material monomers may be converted into ester-forming derivatives in advance and then subjected to polymerization. The use of such ester-forming derivatives has the advantage of making it easier to produce the liquid crystal polyester.

[0025] Examples of the ester-forming derivatives include the following compounds:

[0026] Examples of ester-forming derivatives of aromatic hydroxycarboxylic acids and aromatic dicarboxylic acids having a carboxy group in the molecule include compounds in which the carboxy group is converted into a highly reactive group such as a haloformyl group (acid halide) or an acyloxycarbonyl group (acid anhydride), and compounds in which the carboxy group forms an ester with a monohydric alcohol, a polyhydric alcohol such as ethylene glycol, or a phenol, so as to produce a polyester by a transesterification reaction.

[0027] Examples of polymerizable derivatives of compounds having a phenolic hydroxyl group, such as aromatic hydroxycarboxylic acids and aromatic diols, include compounds in which the phenolic hydroxyl group forms an ester with a lower carboxylic acid so as to produce a polyester by transesterification.

[0028] Furthermore, the above-mentioned aromatic hydroxycarboxylic acids, aromatic dicarboxylic acids, and aromatic diols may have, as a substituent on an aromatic ring in the molecule, a halogen atom such as a chlorine atom or a fluorine atom; an alkyl group having 1 to 10 carbon atoms such as a methyl group, an ethyl group, or a butyl group; or an aryl group having 6 to 20 carbon atoms such as a phenyl group, so long as the ester forming ability is not inhibited.

[0029] Examples of aromatic hydroxycarboxylic acids include p-hydroxybenzoic acid, m-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 3-hydroxy-2-naphthoic acid, 5-hydroxy-1-naphthoic acid, and 4-hydroxy-4'-carboxydiphenyl ether. In addition, examples of aromatic hydroxycarboxylic acids include those in which a portion of the hydrogen atoms in the aromatic ring of the aromatic hydroxycarboxylic acid is substituted with one or more substituents selected from the group consisting of an alkyl group, an aryl group, and a halogen atom.

[0030] p-Hydroxybenzoic acid is an aromatic hydroxycarboxylic acid from which (A1) described below is derived.

[0031] 6-Hydroxy-2-naphthoic acid is an aromatic hydroxycarboxylic acid from which (A2) described below can be derived.

[0032] In producing the liquid crystal polyester, the aromatic hydroxycarboxylic acid may be used alone or in combination of two or more kinds.

[0033] The repeating unit (1) is a repeating unit derived from a specific aromatic hydroxycarboxylic acid. Examples of the repeating unit derived from an aromatic hydroxycarboxylic acid include the repeating units shown below. In addition, a part of the hydrogen atoms in the aromatic ring of the repeating unit derived from an aromatic hydroxycarboxylic acid may be substituted with one or more substituents selected from the group consisting of halogen atoms, alkyl groups, and aryl groups.

[0034] In this specification, the term "derived from" means that the chemical structure is changed due to the polymerization of the raw material monomer, and no other structural changes occur.

[0035] [ka]

[0036] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, biphenyl-4,4'-dicarboxylic acid, 2,6-naphthalenedicarboxylic acid, diphenylether-4,4'-dicarboxylic acid, and diphenylthioether-4,4'-dicarboxylic acid.Further examples include aromatic dicarboxylic acids in which some of the hydrogen atoms in the aromatic rings of these aromatic dicarboxylic acids are substituted with one or more substituents selected from the group consisting of alkyl groups, aryl groups, and halogen atoms.

[0037] Terephthalic acid is an aromatic dicarboxylic acid from which (B1) described below is derived.

[0038] Isophthalic acid is an aromatic dicarboxylic acid from which (B2) described below is derived.

[0039] 2,6-Naphthalenedicarboxylic acid is an aromatic dicarboxylic acid from which (B3) described below can be derived.

[0040] In producing the liquid crystal polyester, the aromatic dicarboxylic acid may be used alone or in combination of two or more kinds.

[0041] The repeating unit (2) is a repeating unit derived from a specific aromatic dicarboxylic acid. Examples of the repeating unit derived from an aromatic dicarboxylic acid include the repeating units shown below. In addition, a part of the hydrogen atoms in the aromatic ring of the repeating unit derived from an aromatic dicarboxylic acid may be substituted with one or more substituents selected from the group consisting of halogen atoms, alkyl groups, and aryl groups.

[0042] [ka]

[0043] Examples of aromatic diols include 4,4'-dihydroxybiphenyl, hydroquinone, resorcin, 4,4'-dihydroxydiphenyl ketone, 4,4'-dihydroxydiphenyl ether, bis(4-hydroxyphenyl)methane, 1,2-bis(4-hydroxyphenyl)ethane, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl thioether, 2,6-dihydroxynaphthalene, and 1,5-dihydroxynaphthalene.Further examples include aromatic diols in which a portion of the hydrogen atoms in the aromatic ring of these aromatic diols is substituted with one or more substituents selected from the group consisting of alkyl groups, aryl groups, and halogen atoms.

[0044] 4,4'-Dihydroxybiphenyl is an aromatic diol from which (C1) described below is derived.

[0045] Hydroquinone is an aromatic diol which derives (C2) below.

[0046] Resorcinol is an aromatic diol that derives (C3) described below.

[0047] In producing the liquid crystal polyester, the aromatic diol may be used alone or in combination of two or more kinds.

[0048] The repeating unit (3) described above includes a repeating unit derived from a specific aromatic diol. Examples of the repeating unit derived from an aromatic diol include the repeating units shown below. In addition, a part of the hydrogen atoms in the aromatic ring of the repeating unit derived from an aromatic diol may be substituted with one or more substituents selected from the group consisting of halogen atoms, alkyl groups, and aryl groups.

[0049] [ka]

[0050] Examples of the substituent that may be optionally contained in the repeating unit derived from an aromatic hydroxycarboxylic acid, the repeating unit derived from an aromatic dicarboxylic acid, and the repeating unit derived from an aromatic diol include the following substituents. Examples of the halogen atom include a fluorine atom, a chlorine atom, and a bromine atom. Examples of the alkyl group include lower alkyl groups having about 1 to 4 carbon atoms, such as a methyl group, an ethyl group, and a butyl group. An example of an aryl group is a phenyl group.

[0051] A particularly preferred liquid crystal polyester will now be described. The repeating unit derived from an aromatic hydroxycarboxylic acid preferably contains a repeating unit ((A1)) derived from parahydroxybenzoic acid or a repeating unit ((A2)) derived from 2-hydroxy-6-naphthoic acid or both.

[0052] The repeating unit derived from an aromatic dicarboxylic acid is preferably a repeating unit selected from the group consisting of a repeating unit derived from terephthalic acid ((B1)), a repeating unit derived from isophthalic acid ((B2)) and a repeating unit derived from 2,6-naphthalenedicarboxylic acid ((B3)).

[0053] The repeating unit derived from an aromatic diol preferably includes a repeating unit derived from hydroquinone ((C2)) or a repeating unit derived from 4,4'-dihydroxybiphenyl or both ((C1)).

[0054] As the combinations thereof, the combinations represented by the following (a) to (h) are preferable: With the combinations of the repeating units (a) to (h), a liquid crystal polyester having good electrical insulation properties can be obtained.

[0055] (a): A combination of (A1), (B1) and (C1), or a combination of (A1), (B1), (B2) and (C1). (b): A combination of (A2), (B3) and (C2), or a combination of (A2), (B1), (B3) and (C2). (c): A combination of (A1) and (A2). (d): A combination of repeating units (a) in which part or all of (A1) is replaced with (A2). (e): In the combination of repeating units (a), a part or all of (B1) is replaced with (B3). (f): A combination of repeating units (a) in which part or all of (C1) is replaced with (C3). (g): In the combination of repeating units (b), a part or all of (A2) is replaced with (A1). (h): A combination of repeating units (c) plus (B1) and (C2).

[0056] Particularly preferred liquid crystal polyesters include those in which the total of repeating units derived from aromatic hydroxycarboxylic acids is 30 to 80 mol %, the total of repeating units derived from aromatic diols is 10 to 35 mol %, and the total of repeating units derived from aromatic dicarboxylic acids is 10 to 35 mol %, based on the total of all repeating units.

[0057] The liquid crystal polyester can be produced by known methods such as those described in JP-A-2002-146003. That is, the above-mentioned raw material monomers (aromatic hydroxycarboxylic acid, aromatic dicarboxylic acid, aromatic diol, or their ester-forming derivatives) are melt-polymerized (polycondensed) to obtain a relatively low molecular weight aromatic polyester (hereinafter abbreviated as "prepolymer"), and then the prepolymer is powdered and heated to perform solid-phase polymerization. By performing solid-phase polymerization in this manner, polymerization proceeds further, and a liquid crystal polyester with a higher molecular weight can be obtained.

[0058] In addition, methods for producing liquid crystal polyesters having the most basic structure of the combination of repeating units (a) and (b) are also described in JP-B-47-47870 and JP-B-63-3888.

[0059] The melt polymerization may be carried out in the presence of a catalyst. Examples of the catalyst used in the melt polymerization include metal compounds such as magnesium acetate, stannous acetate, tetrabutyl titanate, lead acetate, sodium acetate, potassium acetate, and antimony trioxide, and nitrogen-containing heterocyclic compounds such as 4-(dimethylamino)pyridine and 1-methylimidazole, and nitrogen-containing heterocyclic compounds are preferably used.

[0060] The liquid crystal polyester used in the welded molded article of this embodiment is preferably a liquid crystal polyester having a flow start temperature of 280°C or more as determined by the following method. As described above, when solid-phase polymerization is used in the production of the liquid crystal polyester, it is possible to increase the flow start temperature of the liquid crystal polyester to 280°C or more in a relatively short time. By using a liquid crystal polyester having such a flow start temperature, the obtained molded article has a high degree of heat resistance. On the other hand, from the viewpoint of molding the molded article in a practical temperature range, the flow start temperature of the liquid crystal polyester used in the welded molded article of this embodiment is preferably 420°C or less, more preferably 390°C or less.

[0061] Here, the flow initiation temperature is the temperature at which the material begins to flow, measured using a capillary rheometer equipped with a die having an inner diameter of 1 mm and a length of 10 mm, at a pressure of 9.8 MPa (100 kg / cm 2 The flow starting temperature is the temperature at which the liquid crystal polyester has a melt viscosity of 4800 Pa·s (48000 poise) when it is extruded from a nozzle at a heating rate of 4°C / min under a load of 1000 g / mol. The flow starting temperature is an index that indicates the molecular weight of liquid crystal polyester, which is well known in the art (see "Liquid Crystal Polymer Synthesis, Molding, and Application" edited by Koide Naoyuki, pp. 95-105, CMC, published June 5, 1987). As an apparatus for measuring the flow starting temperature, for example, a flow property evaluation apparatus "Flow Tester CFT-500D" manufactured by Shimadzu Corporation can be used.

[0062] [Filling material] The welded molded body of this embodiment may contain a filler. In this embodiment, the welded molded body contains a filler, which can impart sufficient strength to the welded molded body.

[0063] The filler used in this embodiment may be an inorganic filler or an organic filler. In addition, it may be a fibrous filler, a plate-like filler, or a granular filler.

[0064] Examples of fibrous fillers include glass fibers, carbon fibers such as bread-based carbon fibers and pitch-based carbon fibers, ceramic fibers such as silica fibers, alumina fibers, and silica-alumina fibers, and metal fibers such as stainless steel fibers.Furthermore, whiskers such as potassium titanate whiskers, barium titanate whiskers, wollastonite whiskers, aluminum borate whiskers, silicon nitride whiskers, and silicon carbide whiskers can also be mentioned.

[0065] Examples of plate-like fillers include talc, mica, graphite, wollastonite, barium sulfate, calcium carbonate, etc. The mica may be muscovite, phlogopite, fluorophlogopite, or tetrasilicic mica.

[0066] Examples of particulate fillers include silica, alumina, titanium oxide, boron nitride, silicon carbide, and calcium carbonate.

[0067] [Other ingredients] The welded molded article according to this embodiment may contain other components that do not fall under either the liquid crystal polyester or the filler, as long as the effects of the present invention are not impaired.

[0068] Examples of the other components include additives that are commonly used in resin molded bodies, such as release improvers such as fluororesins and metal soaps; colorants such as dyes and pigments; antioxidants; heat stabilizers; ultraviolet absorbers; antistatic agents; and surfactants.

[0069] Examples of the other components include compounds having an external lubricant effect, such as higher fatty acids, higher fatty acid esters, higher fatty acid metal salts, and fluorocarbon surfactants.

[0070] Further, examples of the other components include thermosetting resins such as phenol resins, epoxy resins, and polyimide resins.

[0071] In this embodiment, the liquid crystal polyester, the filler, and other components used as necessary are mixed together or in a suitable order.

[0072] In the present embodiment, it is preferable that the liquid crystal polyester, the filler, and other components used as necessary are melt-kneaded using an extruder, and then pelletized.

[0073] Fig. 1 is a schematic perspective view showing a welded molded body in this embodiment, Fig. 2 is a cross-sectional view taken along line II-II in Fig. 1, and Fig. 3 is a cross-sectional view taken along line III-III in Fig. 1.

[0074] 1 to 3, the welded molded article 100 is a pipe. In the following description, the welded molded article 100 will be referred to as the pipe 100.

[0075] The pipe 100 has a first pipe 101 with one end closed, and a second pipe 102 connected to a through hole 110x provided in the wall surface of the first pipe 101. The first pipe 101 and the second pipe 102 communicate with each other at the through hole 110x.

[0076] The first pipe 101 has a cylindrical internal space 110a formed by combining a first member 1 and a second member 2. The internal space 110a is a space through which liquid or gas flows depending on the use of the pipe 100, for example.

[0077] In the following description, an xyz Cartesian coordinate system is set, and the positional relationship of each component is described with reference to this xyz Cartesian coordinate system. Here, the extension direction of the first pipe 101 is defined as the x-axis direction, the direction perpendicular to the x-axis direction in a horizontal plane is defined as the y-axis direction, and the direction perpendicular to both the x-axis direction and the y-axis direction, i.e., the vertical direction, is defined as the z-axis direction.

[0078] Hereinafter, the +z-axis direction may be referred to as the "upward direction" and the -z-axis direction as the "downward direction." Additionally, the +z-axis side of a certain component or structure may be referred to as the "upper" and the -z-axis side of a certain component or structure as the "lower."

[0079] The first pipe 101 has a pipe main body 110 and a welded portion 130 provided on the outer periphery of the pipe main body 110. The welded portion 130 is a convex portion that protrudes in a band shape along the outer surface of the first pipe 101 that overlaps with the xy plane.

[0080] 1 to 3, it is generally difficult to integrally form the pipe 100 by injection molding. Such molded articles that are difficult to integrally form by injection molding are usually manufactured by injection molding a plurality of separate members and combining the molded members.

[0081] 3, the pipe 100 of this embodiment is a welded molded body in which a first member 1, which is an injection-molded body of liquid crystal polyester, and a second member 2, which is an injection-molded body of liquid crystal polyester, are welded together. The first member 1 and the second member 2 are welded together at a welded portion 130.

[0082] The first member 1 is a substantially semi-cylindrical member having a first pipe upper portion 111 constituting the upper half of the pipe main body 110, and a first welded portion 140 constituting the upper half of the welded portion 130. The first welded portion 140 is provided on both sides of the first pipe upper portion 111. The end portion in the +x-axis direction of the first pipe upper portion 111 is rounded so as to close the end portion of the first pipe 101 formed by combining with the second member 2.

[0083] The second member 2 is a member having a first pipe lower portion 112 constituting the lower half of the pipe main body 110, a second welded portion 150 constituting the lower half of the welded portion 130, and a second pipe 102 connected to the first pipe lower portion 112. The second welded portions 160 are provided on both sides of the first pipe lower portion 112. The end portion in the +x-axis direction of the first pipe lower portion 112 is rounded so as to close the end portion of the first pipe 101 formed by combining with the first member 1.

[0084] The welded part 130 has a welded main body 131 and a pair of ribs 132, 133 provided on both sides of the welded main body 131 in the field of view of Fig. 3. The ribs 132, 133 correspond to the "pair of ribs" in this invention. The cross section in the field of view of Fig. 3 corresponds to the "cross section intersecting the welded main body and the pair of ribs" in this invention.

[0085] On the side surface of the welded portion 130, a joining line 130x appears, which is formed at the position where the first welded portion 140 and the second welded portion 150 come into contact with each other.

[0086] Welded main body 131 is a convex stripe portion formed in a band shape along the outer surface of first pipe 101 inside welded portion 130. Welded main body 131 is a portion where first member 1 and second member 2 are thermally welded by a method described later.

[0087] In the portion indicated by the symbol X in the welded main body 131, the liquid crystalline polyester constituting the first member 1 and the liquid crystalline polyester constituting the second member are melted and mixed together.

[0088] The pair of ribs 132, 133 are convex stripes formed along both sides of the welded main body 131 inside the welded portion 130. In the drawing, the rib on the piping main body 110 side of the welded main body 131 is rib 132, and the rib on the opposite side of the welded main body 131 from the piping main body 110 is rib 133.

[0089] Between the welded main body 131 and the rib 132, and between the welded main body 131 and the rib 133, cylindrical holding spaces 130a are formed along both sides of the welded main body 131. The inside of the holding spaces 130a is filled with flash 139.

[0090] The burrs 139 are portions where molten resin solidifies during a manufacturing method described below, and are formed from resin in which the materials forming the first member 1 and the materials forming the second member 2 are melted and mixed together.

[0091] In the pipe 100 of this embodiment, the filling rate of the burrs 139 in the retention space 130a is 20% or more and less than 100%. The filling rate is preferably 25% or more, more preferably 30% or more, and even more preferably 50% or more. That is, the filling rate of the burrs 139 in the retention space 130a is preferably 25% or more and less than 100%, more preferably 30% or more and less than 100%, even more preferably 50% or more and less than 100%, and even more preferably 65% ​​or more and less than 100%.

[0092] The filling rate of the burrs in the holding space can be measured by image analysis using cross-sectional images. Specifically, image processing software (WinROOF2018, Mitani Shoji Co., Ltd.) is used.

[0093] First, the pipe is cut along a plane perpendicular to the extension direction of the holding space to obtain a cross section. For observation, the cross section and exposed gaps may be filled with a light-transmitting curable resin such as epoxy resin, cured, and then polished to make the cross section smooth.

[0094] In the image analysis, the cross section is photographed, the holding space where the burr exists is specified in the obtained cross section image, and the area occupied by the burr in the holding space and the area occupied by the gap are binarized and distinguished by a binarization command, which is a function of the image processing software. The binarization threshold is a value at which the boundary between the burr and the gap that can be determined from the cross section image coincides with the boundary between the burr and the gap in the binarized image. When executing the "binarization command", the worker adjusts the image processing software to set the threshold value of the above condition. However, the worker visually distinguishes the boundary between the burr and the welded main body that forms the holding space. Similarly, the worker visually distinguishes the boundary between the burr and the rib that forms the holding space, the boundary between the gap and the welded main body, and the boundary between the gap and the rib.

[0095] The burr filling rate is calculated by dividing the area of ​​the region occupied by the burrs in the retaining space in the cross-sectional image by the total area of ​​the retaining space, which is the sum of the area occupied by the burrs and the area occupied by the voids.

[0096] When the burr filling rate is to be calculated for a pipe with many bends, the burr filling rate is calculated for multiple cross sections in the pipe using the above method, and the arithmetic average of the obtained filling rates is used as the burr filling rate to be calculated. In this case, the burr filling rate is calculated for three or more cross sections. In addition, it is recommended that the burr filling rate be calculated for 10 or fewer cross sections, taking into account work efficiency.

[0097] In this embodiment, the "burr filling rate in the retaining space" refers to a value calculated as a ratio (%) of the total area of ​​the burrs 139 filled in the two retaining spaces 130a to the total area of ​​the two retaining spaces 130a exposed in the cross section of the welded part 130. When calculating the burr filling rate in the retaining space, the cross section of the welded part 130 including the target retaining space may be taken as a cross section in a virtual plane perpendicular to the extension direction of the retaining space. The filling rate of the burrs can be adjusted by controlling the manufacturing conditions (heating conditions, pressing conditions, vibration conditions) in the manufacturing method described below.

[0098] When the filling rate is 20% or more, the burrs 139 cover the side surfaces of the welded main body 131, effectively reinforcing the welded main body 131. Therefore, the welded molded body 100 having the filling rate of 20% or more has excellent weld strength of the welded part 130, and is a highly reliable molded body.

[0099] Furthermore, if the filling rate is 25% or more, for example, gas or liquid flowing through the internal space 110a of the pipe 100 is unlikely to infiltrate into the holding space 130a. Therefore, problems such as the gas or liquid flowing through the internal space 110a causing the welded main body 131 to swell and reducing the weld strength are unlikely to occur.

[0100] On the other hand, if the filling rate is less than 100%, the burrs 139 do not leak out of the retaining space 130a and remain in the retaining space 130a. Therefore, if the filling rate is less than 100%, the appearance defect of the welded part 130 caused by the burrs 139 does not occur.

[0101] Furthermore, when the filling rate is less than 100%, the burrs 139 remain in the holding space 130a without leaking into the internal space 110a of the pipe 100. Therefore, when the filling rate is less than 100%, the burrs 139 are less likely to be mixed into the gas or liquid flowing inside the pipe 100.

[0102] In this embodiment, the welding strength of the welded portion 130 where the first member 1 and the second member 2 are heat-welded is the tensile strength of the welded portion 130. The welding strength of the welded portion 130 where the first member 1 and the second member 2 are heat-welded is preferably 13 MPa or more, more preferably 15 MPa or more, and even more preferably 20 MPa or more. If the welding strength of the welded portion 130 is 13 MPa or more, the molded body is less likely to break and has high reliability. In addition, the welding strength of the heat-welded welded portion 130 is usually 100 MPa or less. That is, the welding strength of the welded portion 130 where the first member 1 and the second member 2 are heat-welded is preferably 13 MPa or more and 100 MPa or less, more preferably 15 MPa or more and 100 MPa or less, and even more preferably 20 MPa or more and 100 MPa or less.

[0103] The welding strength of the welded portion 130 can be measured by preparing a test piece by cutting out the welded portion 130 to a thickness of 10 mm in the extension direction of the welded portion 130, and performing a tensile test on the obtained test piece in which it is pulled in a direction perpendicular to the welded surface, and measuring the maximum stress until the test piece breaks at the welded surface of the test piece.

[0104] In addition, when the welded molded body has a pipe shape and has welded parts on both sides of the extension direction of the pipe as in this embodiment, the welded molded body may be cut into 10 mm thick slices to prepare test pieces, and the above-mentioned tensile test may be performed on the obtained test pieces. In this case, the test piece has two welded parts, and the maximum stress until the test piece breaks at the welded surface of one of the welded parts is measured. Therefore, the technical meaning of the measured value is different from the case where a tensile test is performed on only one welded part. Even in this case, the weld strength of the welded part can be evaluated by comparing the measured values ​​of test pieces of the same shape.

[0105] The tensile test is carried out using a universal testing machine (Tensilon RTG-1250, manufactured by A&D Co., Ltd.). The measurement conditions for the tensile test are a span distance of 20 mm and a test speed of 5 mm / min. The number of tests for the tensile test is preferably, for example, 3 to 10 times. The tensile test is carried out on multiple test pieces, and the arithmetic average value of the obtained multiple weld strengths is taken as the weld strength.

[0106] [Method of manufacturing welded molded body] 4 and 5 are schematic diagrams showing the manufacturing method of the welded molded body of this embodiment. As described above, the welded molded body 100 of this embodiment is made of liquid crystal polyester as a forming material.

[0107] 4, the method for producing a welded molded article of this embodiment uses a first member 1 and a second member 2. The first member 1 and the second member 2 are each an injection molded article made of liquid crystalline polyester.

[0108] The first member 1 has a first piping upper portion 111 and a first welded portion 140. The first welded portion 140 has a first base portion 141, a first convex strip portion 142, a pair of first ribs 143, 144, and a rib 145.

[0109] The first base portion 141 protrudes from a side surface of the first piping upper portion 111 in the xy plane direction.

[0110] The first convex portion 142 protrudes downward (in the -z-axis direction) from the first base portion 141. The first convex portion 142 has a substantially rectangular structure in which a top surface 142a is perpendicular to the protruding direction of the first convex portion 142 in a cross-sectional view.

[0111] The first ribs 143, 144 are provided on both sides of the first convex stripe portion 142 along the extension direction of the first convex stripe portion 142, and protrude from the first base portion 141 on the same side as the first convex stripe portion 142. In the drawing, the rib on the first piping upper portion 111 side of the first convex stripe portion 142 is indicated by reference numeral 143, and the rib on the opposite side of the first piping upper portion 111 from the first convex stripe portion 142 is indicated by reference numeral 144.

[0112] Between the first protruding stripe 142 and the first rib 143, and between the first protruding stripe 142 and the first rib 144, recesses 149 are formed respectively.

[0113] In addition, the first ribs 143, 144 shown in the figure protrude in the -z axis direction parallel to the first convex portion 142, but this is not limited to this, and the first ribs 143, 144 may be inclined with respect to the first convex portion 142.

[0114] The first welded portion 140 has a rib 145 that protrudes from the first base portion 141 on the side opposite the first ridge portion 142 to the first piping upper portion 111 .

[0115] The second member 2 has the first piping lower portion 112 and a second welded portion 150. The second welded portion 150 has a second base portion 151, a second convex strip portion 152, a pair of second ribs 153, 154, and a rib 155.

[0116] The second base portion 151 protrudes from a side surface of the first piping lower portion 112 in the xy plane direction.

[0117] The second convex portion 152 protrudes upward (in the +z-axis direction) from the second base portion 151. The second convex portion 152 has a substantially rectangular structure in a cross-sectional view in which a top surface 152a is provided perpendicular to the direction in which the second convex portion 152 protrudes.

[0118] The second ribs 153, 154 are provided on both sides of the second convex stripe portion 152 along the extension direction of the second convex stripe portion 152, and protrude from the second base portion 151 on the same side as the second convex stripe portion 152. In the drawing, the rib on the first piping lower portion 112 side of the second convex stripe portion 152 is indicated by reference numeral 153, and the rib on the opposite side of the second convex stripe portion 152 to the first piping lower portion 112 is indicated by reference numeral 154.

[0119] Between the second protruding portion 152 and the second rib 153, and between the second protruding portion 152 and the second rib 154, a recess 159 is formed.

[0120] In addition, the second ribs 153, 154 shown in the figure protrude in the +z axis direction parallel to the second convex portion 152, but this is not limited to this, and the second ribs 153, 154 may be inclined with respect to the second convex portion 152.

[0121] The second welded portion 150 has a rib 155 that protrudes from the second base portion 151 on the opposite side to the second convex portion 152 and from the first piping lower portion 112 .

[0122] In the manufacturing method of the welded molded product of this embodiment, first, the first convex streak portion 142 of the first member 1 and the second convex streak portion 152 of the second member 2 are heated to a temperature equal to or higher than the flow start temperature of the liquid crystal polyester that is the material for forming each member. For example, the first convex streak portion 142 and the second convex streak portion 152 are each irradiated with infrared light IR to heat the first convex streak portion 142 and the second convex streak portion 152.

[0123] The first convex stripe 142 and the second convex stripe 152 can be heated by any commonly known method as long as the method heats the liquid crystal polyester to a temperature equal to or higher than the flow starting temperature. For example, in addition to infrared irradiation, the first convex stripe 142 and the second convex stripe 152 may be directly heated by contacting a heat source with the first convex stripe 142 and the second convex stripe 152.

[0124] Next, as shown in FIG. 5, the first convex streak portion 142 and the second convex streak portion 152 are brought into contact with each other, and vibration welding is performed while applying a force F in a direction in which the first convex streak portion 142 and the second convex streak portion 152 approach each other relatively.

[0125] When vibration welding is performed, the first convex streak portion 142 and the second convex streak portion 152 are preheated to a temperature equal to or higher than the flow start temperature of the liquid crystal polyester that is the material for forming each member. Therefore, when the first convex streak portion 142 and the second convex streak portion 152 are vibration welded together, the liquid crystal polyester is easily melted and is welded while being mixed with each other.

[0126] Therefore, according to the manufacturing method of the welded molded body of this embodiment, it is possible to easily vibration weld molded bodies of liquid crystal polyester, which are known according to common knowledge to be unsuitable for welding due to their fast solidification rate and the occurrence of interfacial flow.

[0127] As vibration welding progresses, the first member 1 and the second member 2 approach each other while the first convex streak portion 142 and the second convex streak portion 152 melt. At that time, it is preferable that the vibration welding brings the first member 1 and the second member 2 closer to each other until the first rib 143 and the second rib 153, and the first rib 144 and the second rib 154 come into contact with each other.

[0128] When the first rib 143 and the second rib 153 come into contact with each other, the recess 149 and the recess 159 are connected to each other, and the above-mentioned holding space 130a is formed, which is surrounded by the first rib 143, the second rib 153, the first convex rib portion 142, and the second convex rib portion 152. Furthermore, when the first rib 144 and the second rib 154 come into contact with each other, the recess 149 and the recess 159 are connected to each other, and the above-mentioned holding space 130a is formed, which is surrounded by the first rib 144, the second rib 154, the first convex rib portion 142, and the second convex rib portion 152.

[0129] During vibration welding, molten resin MR is discharged from the welded portion between the first convex streak portion 142 and the second convex streak portion 152. The discharged molten resin flows into and is held in the holding space described above. The molten resin MR becomes the flash 139 described above by solidifying.

[0130] It is preferable to terminate the vibration welding process described above before the molten resin MR leaks out from the space (retaining space 130a) surrounded by the first ridge portion 142, the second ridge portion 152, the first rib 143, and the second rib 153, or the space (retaining space 130a) surrounded by the first ridge portion 142, the second ridge portion 152, the first rib 144, and the second rib 154.

[0131] In carrying out the vibration welding described above, it is preferable that the width W1 of the top surface 142a of the first convex stripe 142 shown in Fig. 5 is 90% to 110% of the width W2 of the top surface 152a of the second convex stripe 152. If the sizes of the first convex stripe 142 and the second convex stripe 152 are in the above-mentioned relationship, the welding strength tends to be high, which is preferable. In the first member 1 and the second member 2 shown in the figures, the width W1 of the top surface 142a of the first convex stripe 142 and the width W2 of the top surface 152a of the second convex stripe 152 are the same (100%).

[0132] FIG. 6 is a schematic diagram showing a commonly known vibration welding process.

[0133] Based on knowledge of normal welding vibration, the width Wa of the top surface of one convex rib portion 142X is set to, for example, about 70% of the width Wb of the top surface of the other convex rib portion 152X. This is based on the idea that when the convex rib portion 142X and the convex rib portion 152X are vibrated relatively in the width direction of the convex rib portion 142X as shown in Fig. 6, the top surfaces of the convex rib portion 142X and the convex rib portion 152X are always vibrated in a state of contact with each other.

[0134] By setting the size of the top surface of the ridge portion 142X and the top surface of the ridge portion 152X in this relationship, the top surface of the ridge portion 152X is always in contact with the top surface of the ridge portion 142X, which prevents the ridge portion 152X from cooling, which is considered to be advantageous for vibration welding.

[0135] In contrast, in the manufacturing method of the welded molded body of this embodiment, it has been found that a higher weld strength can be obtained by setting the width W1 of the top surface 142a of the first ridge portion 142 to be between 90% and 110% of the width W2 of the top surface 152a of the second ridge portion 152, a size that is considered disadvantageous based on commonly known knowledge.

[0136] In FIG. 4, the top surface 142a of the first convex streak portion 142 is perpendicular to the protruding direction of the first convex streak portion 142 in a cross-sectional view, but this is not limited thereto.

[0137] It is preferable that the top surface 142a of the first convex streak portion 142 is inclined toward the recess 149. In the case of such a shape, the excess molten resin MR generated during welding can be efficiently discharged into the holding space 130a. In addition, in the case of such a shape, the molten resin MR generated in the first convex streak portion 142 is easily pushed toward the molten resin MR generated in the second convex streak portion 152, and the molten resins are easily mixed with each other, which makes it easy to improve the welding strength.

[0138] The shape of the top surface 142a may be inclined toward the recesses 149 on both sides of the center of the top surface 142a, that is, the top surface 142a may be convex toward the second convex stripe portion 152.

[0139] For the same reasons as for the preferred shape of the first convex stripe 142 described above, it is preferable that the top surface 152a of the second convex stripe 152 is inclined toward the recess 159. When the top surface 142a of the first convex stripe 142 and the top surface 152a of the second convex stripe 152 are both inclined, it is preferable that the inclination directions are different from each other. The first convex stripe 142 and the second convex stripe 152 are preferably welded to each other while facing each other so that the top surface 142a and the top surface 152a are approximately parallel.

[0140] According to the manufacturing method of the welded molded article having the above-mentioned configuration, it is possible to provide a manufacturing method of the welded molded article that enables the welded molded article to be suitably manufactured.

[0141] Furthermore, a pipe having the above-described configuration is a highly reliable pipe in which the strength of the welded portions is guaranteed.

[0142] In the present embodiment, the welded molded body 100 is described as a pipe, but is not limited thereto. A welded molded body having a welded part with the same configuration as the welded part 130 of the pipe 100 described above and a burr filling rate in the retention space of the welded part of 20% or more and less than 100% is a welded molded body with guaranteed strength at the welded part.

[0143] Although the preferred embodiment of the present invention has been described above with reference to the attached drawings, it goes without saying that the present invention is not limited to the above embodiment. The shapes and combinations of the components shown in the above embodiment are merely examples, and various modifications can be made based on design requirements, etc., without departing from the spirit of the present invention. EXAMPLES

[0144] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.

[0145] 7 and 8 are schematic diagrams showing a test piece used in the examples. In the examples, a test piece A as shown in Fig. 7 was injection molded using liquid crystal polyester as a forming material.

[0146] The test piece A has a flat main body A0, a base A1 arranged at one end side of the main body A0 so as to intersect with the main body A0, a convex rib portion A2 arranged so as to protrude from the base A1 on the opposite side of the main body A0, and a pair of ribs A3 arranged on both sides of the convex rib portion A2 along the extension direction of the convex rib portion A2 and protruding on the same side of the base A1 as the convex rib portion A2.

[0147] Test piece A is a model of first welded portion 140 of first member 1 and second welded portion 150 of second member 2 shown in the manufacturing method of the above embodiment.

[0148] The material and molding conditions for test piece A are as follows.

[0149] (Production of Liquid Crystalline Polyester) Into a reactor equipped with a stirrer, a torque meter, a nitrogen gas inlet tube, a thermometer, and a reflux condenser, 994.5 g (7.2 mol) of parahydroxybenzoic acid, 446.9 g (2.4 mol) of 4,4'-dihydroxybiphenyl, 299.0 g (1.8 mol) of terephthalic acid, 99.7 g (0.6 mol) of isophthalic acid, and 1347.6 g (13.2 mol) of acetic anhydride were placed.

[0150] After the inside of the reactor was replaced with nitrogen gas, 0.18 g of 1-methylimidazole was added under a nitrogen gas flow, and the temperature was raised to 150° C. over 30 minutes, and the mixture was refluxed for 30 minutes while maintaining the temperature.

[0151] Next, 2.4 g of 1-methylimidazole was added, and the mixture in the reactor was heated to 320°C over 2 hours and 50 minutes while distilling off the by-product acetic acid and unreacted acetic anhydride. The reaction was deemed to have ended when an increase in torque was observed, and the contents were removed.

[0152] The obtained solid was cooled to room temperature and crushed in a coarse crusher. The crushed solid was then heated from room temperature to 250°C over 1 hour in a nitrogen atmosphere, and then heated from 250°C to 295°C over 5 hours, and then held at 295°C for 3 hours to proceed with solid-phase polymerization. The reaction product was then cooled to obtain a liquid crystal polyester.

[0153] (Production of Liquid Crystal Polyester Resin Composition) 70 parts by mass of liquid crystal polyester powder and 30 parts by mass of chopped glass fiber (model number: CS03JAPX-1, manufactured by Owens Corning) were mixed, and the resulting mixture was melt-kneaded using a twin-screw extruder (model number: PCM-30, manufactured by Ikegai Corporation) to produce pellets of a liquid crystal polyester resin composition.

[0154] The melt kneading conditions were a cylinder temperature setting of 340° C. and a screw rotation speed of 150 rpm for the twin-screw extruder. The "cylinder temperature setting" refers to the arithmetic average value of the temperature settings of the heating device (cylinder heater) installed from the downstream side of the cylinder to approximately 2 / 3 of the cylinder length.

[0155] (Molding of test pieces) The obtained pellets were molded at 340°C using an injection molding machine (model number: PS40E5ASE, manufactured by Nissei Plastic Industrial Co., Ltd.) to mold a plurality of test pieces A having different shapes of the convex rib portion A2. The dimensions of the test piece A shown in Fig. 7 were L 100 mm × W 55 mm × H 5 mm.

[0156] Under the above molding conditions, a number of test pieces A were produced with different shapes of the ridges A2. The test pieces A had the same configuration except for the size and shape of the ridges A2. Therefore, the overall length of the test pieces A (the size of the symbol L in FIG. 7) differed depending on the shape of the ridges A2.

[0157] The test pieces thus prepared were paired with each other, each having a convex rib portion A2 as shown in Fig. 8. The numerical values ​​in Fig. 8 indicate the dimensions of the convex rib portion A2 and the rib A3. The unit of dimensions is mm.

[0158] (Examples 1 to 6) As shown in Fig. 8, each set of test pieces shown in Fig. 8 was designated as Examples 1 to 6. For each set of test pieces, the convex rib portions A2 were irradiated with infrared rays IR under the conditions described below to heat them, and then the convex rib portions A2 were vibration-welded to each other under the conditions described below to produce a welded molded body.

[0159] (Infrared heating conditions) Heating wire output: 7.5A Distance between test piece and heating wire: 2.0 mm Heating time: 40 seconds

[0160] (Vibration welding conditions) Amplitude: 1.0mm Vibration frequency: 220Hz Vibration time: 1.0 seconds Pressing load: 3MPa

[0161] Comparative Example 1 A welded molded article of Comparative Example 1 was produced in the same manner as in Example 2, except that the test pieces were not vibrated after being brought into contact with each other.

[0162] Comparative Example 2 A welded molded article of Comparative Example 2 was produced in the same manner as in Example 1, except that the test piece was vibration-welded without being heated by infrared rays. However, the convex ridges were not welded to each other, and no welded molded article was obtained.

[0163] Comparative Example 3 A welded molded article of Comparative Example 3 was produced in the same manner as in Example 2, except that the test piece was vibration-welded without being heated by infrared rays. However, the convex ridges were not welded to each other, and no welded molded article was obtained.

[0164] Comparative Example 4 A welded molded article of Comparative Example 4 was produced in the same manner as in Comparative Example 1, except that the heating time by infrared radiation was changed to 7 seconds.

[0165] (burr filling rate) The burr filling rate was calculated according to the method described below. First, the prepared welded molded body was cut on a plane (cross section) perpendicular to the extension direction of the cylindrical holding space where the burrs were to be filled. An image of the cut cross section was captured, and the obtained cross section image was analyzed using image processing software (WinROOF2018, Mitani Corporation).

[0166] In the image analysis, the cross section was photographed, the retention space in which the burr was present was specified in the obtained cross section image, and the area occupied by the burr in the retention space and the area occupied by the gap were binarized and distinguished by a binarization command, which is a function of the image processing software. The binarization threshold was set to a value at which the boundary between the burr and the gap that can be determined from the cross section image coincided with the boundary between the burr and the gap in the binarized image. When executing the "binarization command," the worker adjusted the image processing software to set the threshold value of the above condition. The worker visually distinguished the boundary between the burr and the welded main body that forms the retention space, the boundary between the burr and the rib that forms the retention space, the boundary between the gap and the welded main body, and the boundary between the gap and the rib.

[0167] The burr filling rate was calculated by dividing the area of ​​the region occupied by the burrs in the retained space in the cross-sectional image by the total area of ​​the retained space, which is the sum of the area occupied by the burrs and the area occupied by the voids.

[0168] The filling rate of burrs was calculated using the total area of ​​the retaining spaces on both sides of the welded ridges and the total area of ​​the regions occupied by burrs in the retaining spaces on both sides of the ridges.

[0169] (Welding strength) The weld strength of the welded molded test piece was determined by measuring the tensile strength in a tensile test. The tensile strength measured by the following method was regarded as the weld strength of the welded molded test piece. Specifically, for the welded molded test pieces obtained in Examples 1 to 6 and Comparative Examples 1 to 4, the other end side of the main body A0 (the side opposite to the convex ridge portion A2) was gripped and a tensile test was performed to confirm the weld strength. The weld strength was measured three times using three welded molded bodies. The arithmetic mean value of the obtained weld strengths was determined as the desired weld strength value.

[0170] The tensile test was performed using a universal testing machine (Tensilon RTG-1250, manufactured by A&D Co., Ltd.) with a span distance of 20 mm and a test speed of 5 mm / min. The maximum stress in the tensile test was used as the measurement value of the weld strength.

[0171] The evaluation results are shown in Table 1.

[0172] [Table 1]

[0173] As a result of the evaluation, Examples 1 to 6 all showed higher welding strength than infrared irradiation alone (Comparative Examples 1 and 4) and vibration welding alone (Comparative Examples 2 and 3). Furthermore, the burr filling rate in the holding space of Examples 1 and 2 was high, at 73% and 61%, respectively. The burr filling rate in the holding space of Comparative Example 4 was 17%. Although the filling rate of burrs in the retaining space in Examples 3 to 6 was not actually measured, it was clearly greater than that in Comparative Example 4 by visual inspection, and it was strongly suggested that the filling rate was 20% or more.

[0174] From the above results, it was found that the present invention is useful. [Explanation of symbols]

[0175] 1...first member, 2...second member, 100...welded formed body (pipe), 130...welded portion, 130a...retaining space, 131...welded main body portion, 132, 133...rib, 139...burr, 141...first base portion, 142...first convex portion, 142a, 152a...top surface, 143, 144...first rib, 151...second base portion, 152...second convex portion, 153, 154...second rib, W1...width of top surface of first convex portion, W2...width of top surface of second convex portion

Claims

1. A method for producing a welded molded article using a liquid crystal polyester as a forming material, comprising the steps of: a step of heating a first convex portion of a first member formed of the liquid crystal polyester and a second convex portion of a second member formed of the liquid crystal polyester to a flow starting temperature of the liquid crystal polyester or higher; a step of bringing the first convex ridge portion and the second convex ridge portion into contact with each other, and vibration welding the first convex ridge portion and the second convex ridge portion while pressing them in a direction in which they approach each other relatively; A method for manufacturing a welded molded body, comprising heating only the first convex ridge portion in the first member, and heating only the second convex ridge portion in the second member.

2. The first member includes a first base portion and The first protruding portion protruding from the first base portion; a pair of first ribs provided on both sides of the first convex rib along an extension direction of the first convex rib and protruding from the first base portion on the same side as the first convex rib; The second member includes a second base portion and The second protruding portion protruding from the second base portion; a pair of second ribs provided on both sides of the second convex rib along an extension direction of the second convex rib and protruding on the same side as the second convex rib with respect to the second base portion; The method for manufacturing a welded molded product according to claim 1 , wherein in the vibration welding step, the first member and the second member are brought close to each other until the first rib and the second rib come into contact with each other.

3. The method for manufacturing a welded molded body according to claim 2 , wherein the vibration welding process is terminated before molten resin leaks out from the space surrounded by the first convex portion, the second convex portion, the first rib, and the second rib.

4. The method for producing a welded molded article according to any one of claims 1 to 3, wherein a width of a top surface of the first convex ridge portion is 90% or more and 110% or less of a width of a top surface of the second convex ridge portion.

5. A first member and a second member, The first member and the second member are each made of a liquid crystal polyester, a welded portion formed by thermally welding the first member and the second member, The welded portion has a welded main body portion formed by thermally welding the first member and the second member, and a pair of ribs provided on both sides of the welded main body portion, A cylindrical holding space is formed between the welding main body and the rib, The holding space is filled with a burr formed of the liquid crystal polyester, A welded molded body, in which the filling rate of the burrs in the retention space at a cross section intersecting the welded main body and the pair of ribs is 65% or more and less than 100%.

6. A welded molded body as described in claim 5, wherein the tensile strength of the welded portion is 13 MPa or more.

7. A pipe which is the welded formed article according to claim 5 or 6.

Citation Information

Patent Citations

  • Ultrasonic wave fusion-bonding method of high-melting resin

    JP1991184830A

  • Manufacture of welded resin molding and welded resin molding

    JP1999240073A

  • Joining method of liquid crystal polyester resin composition and joined product of liquid crystal resin composition

    JP2005320478A

  • Wholly aromatic liquid crystal polyester and composition thereof

    JP2007169379A

  • Polyester resin composition for laser welding and molded product using the same

    JP2009019135A