Laser scribing trench opening control in wafer dicing using a hybrid laser scribing and plasma etching approach
The hybrid laser scribing and plasma etching method addresses the inefficiencies of traditional dicing methods by minimizing kerf widths and improving die density, resulting in higher wafer yield and reduced manufacturing costs.
Patent Information
- Application Number
- JP2022578613
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-22
- Filing Date
- 2021-05-21
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-05-21
AI Technical Summary
Current methods for dicing semiconductor wafers, such as scribing and sawing, result in chipping and cracking of integrated circuits, leading to waste of wafer area and increased manufacturing costs, while plasma dicing faces challenges with high implementation costs and throughput limitations.
A hybrid method involving dual laser scribing processes followed by plasma etching, where a first laser process sets the kerf width and a second laser process widens the trench without increasing the kerf width, followed by plasma etching to singulate the integrated circuits.
This approach reduces kerf widths, increases die density, and improves wafer yield by minimizing chipping and cracking, allowing for more efficient use of wafer space and reducing manufacturing costs.
Smart Images

Figure 0007576107000001 
Figure 0007576107000002 
Figure 0007576107000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Patent Application No. 16 / 908,542, filed June 22, 2020, the entire contents of which are incorporated herein by reference.
[0002] FIELD OF THE DISCLOSURE Embodiments of the present disclosure relate to the field of semiconductor processing, and more particularly to a method for dicing semiconductor wafers, each wafer having multiple integrated circuits thereon. [Background technology]
[0003] In semiconductor wafer processing, integrated circuits are formed on wafers (also called substrates) composed of silicon or other semiconductor materials. Typically, layers of various materials that are either semiconductive, conductive, or insulating are utilized to form the integrated circuits. These materials are doped, deposited, and etched using various well-known processes to form the integrated circuits. Each wafer is processed to form a number of individual areas that contain the integrated circuits, known as dies.
[0004] Following the integrated circuit formation process, the wafer is "diced" to separate the dies into separate dies for packaging or for use in unpackaged form in a larger circuit. The two main techniques used to dice wafers are scribing and sawing. In scribing, a diamond-tipped scriber is moved across the wafer surface along pre-formed scribe lines. These scribe lines extend along the spaces between the dies. These spaces are commonly referred to as "streets." The diamond scriber creates shallow scratches in the wafer surface along the streets. When pressure is applied, such as with a roller, the wafer separates along the scribe lines. The cracks in the wafer are aligned with the crystal lattice structure of the wafer substrate. Scribing can be used for wafers up to about 10 mils (thousandths of an inch) thick. For dicing thicker wafers, sawing is currently the preferred method.
[0005] In sawing, a diamond tipped saw rotating at high revolutions per minute contacts the wafer surface and cuts the wafer along the streets. The wafer is mounted on a support, such as an adhesive film stretched across a film frame, and the saw repeatedly strikes both the vertical and horizontal streets. A problem with both scribing and sawing is that chips and grooves can form along the cut edge of the die. In addition, cracks can form and propagate from the edge of the die into the substrate, rendering the integrated circuit inoperable. The crystal structure of the wafer is affected by the lattice constants, which can cause chips and grooves to form along the cut edge of the die. <110> In the 100 mm orientation, chipping and crack formation are particularly problematic with scribing because only one side of a square or rectangular die can be scribed. As a result, cleaving the other side of the die results in a jagged separation line. Chipping and crack formation require greater die spacing on the wafer (e.g., chips and cracks are kept a certain distance from the actual integrated circuit) to prevent damage to the integrated circuits. This spacing requirement results in fewer die being formed on a standard size wafer, wasting wafer real estate that could be used for circuits. The waste of semiconductor wafer real estate is exacerbated by the use of saws. The blade of a saw is approximately 15 microns thick. Thus, the circuits on each die must often be spaced 300 to 500 microns apart to prevent the integrated circuits from being adversely affected by cracks or other damage around the cuts made by the saw. Additionally, after sawing, each die must be thoroughly cleaned to remove particles and other contaminants from the sawing process.
[0006] Plasma dicing has also been used, but it can have limitations. For example, one limitation that can prevent the implementation of plasma dicing can be cost. Standard lithography steps for patterning resist can make the implementation cost prohibitive. Another limitation that can prevent the implementation of plasma dicing is that plasma processing of common metals (such as copper) for dicing along the streets can cause manufacturing issues or throughput limitations. Summary of the Invention
[0007] An embodiment disclosed herein includes a method of dicing a wafer comprising a plurality of integrated circuits. In an embodiment, the method includes forming a mask over a semiconductor wafer and patterning the mask and the semiconductor wafer with a first laser process. The method may further include patterning the mask and the semiconductor wafer with a second laser process, where the second laser process is different from the first laser process. In an embodiment, the method may further include etching the semiconductor wafer with a plasma etching process to singulate the integrated circuits.
[0008] According to further embodiments disclosed herein, there is provided a method of dicing a semiconductor wafer comprising a plurality of integrated circuits. In one embodiment, the method includes forming a mask over the semiconductor wafer and performing a first laser process to form openings through the mask in a device layer of the semiconductor wafer. In one embodiment, the method further includes performing a second laser process to singulate the plurality of integrated circuits.
[0009] According to further embodiments disclosed herein, a system for dicing a semiconductor wafer comprising a plurality of integrated circuits is provided. In one embodiment, the system comprises a factory interface and a laser scribe apparatus coupled to the factory interface. The laser scribe apparatus comprises a laser assembly configured to provide a first laser process and a second laser process. In one embodiment, the system further comprises a plasma etch chamber coupled to the factory interface. [Brief description of the drawings]
[0010] [Figure 1] 1 is a flow chart illustrating operations of a method for dicing a semiconductor wafer containing multiple integrated circuits according to one embodiment of the present disclosure. [Figure 2A] 1 illustrates a cross-sectional view of a semiconductor wafer including multiple integrated circuits during a method of dicing the semiconductor wafer, corresponding to operation 121 of the flowchart of FIG. 1, according to one embodiment of the present disclosure. [Figure 2B] 1 illustrates a cross-sectional view of a semiconductor wafer including multiple integrated circuits during a method of dicing the semiconductor wafer, corresponding to operation 122 of the flowchart of FIG. 1, according to one embodiment of the present disclosure. [Figure 2C] 1 illustrates a cross-sectional view of a semiconductor wafer including multiple integrated circuits during a method of dicing the semiconductor wafer, corresponding to operation 123 of the flowchart of FIG. 1, according to one embodiment of the present disclosure. [Figure 2D] 1 illustrates a cross-sectional view of a semiconductor wafer including multiple integrated circuits during a method of dicing the semiconductor wafer, corresponding to operation 125 of the flowchart of FIG. 1, according to one embodiment of the present disclosure. [Diagram 3] 1 illustrates a cross-sectional view of a stack of materials that may be used in the street area of a semiconductor wafer or substrate according to one embodiment of the present disclosure. [Figure 4A] 4A-4E illustrate cross-sectional views of various operations of a method for dicing a semiconductor wafer according to one embodiment of the present disclosure. [Figure 4B]4A-4E illustrate cross-sectional views of various operations of a method for dicing a semiconductor wafer according to one embodiment of the present disclosure. [Figure 4C] 4A-4E illustrate cross-sectional views of various operations of a method for dicing a semiconductor wafer according to one embodiment of the present disclosure. [Figure 4D] 4A-4E illustrate cross-sectional views of various operations of a method for dicing a semiconductor wafer according to one embodiment of the present disclosure. [Figure 4E] 4A-4E illustrate cross-sectional views of various operations of a method for dicing a semiconductor wafer according to one embodiment of the present disclosure. [Diagram 5] FIG. 1 illustrates a block diagram of a tool layout for laser and plasma dicing of a wafer or substrate according to one embodiment of the present disclosure. [Figure 6] FIG. 1 illustrates a block diagram of an exemplary computer system according to one embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] A method for dicing multiple semiconductor wafers, each having multiple integrated circuits (ICs) thereon, is described. In the following description, numerous specific details are described, such as dual laser scribing processes, plasma etching conditions, and material regimes, to provide a thorough understanding of the embodiments of the present disclosure. It will be apparent to one of ordinary skill in the art that the embodiments of the present disclosure may be practiced without these specific details. In other instances, well-known aspects, such as the fabrication of integrated circuits, have not been described in detail in order to not unnecessarily obscure the embodiments of the present disclosure. Furthermore, it should be understood that the various embodiments shown in the figures are illustrative representations and are not necessarily drawn to scale.
[0012] A hybrid wafer or substrate dicing process may be performed that includes first laser scribing followed by plasma etching to singulate the dies. The laser scribing process may be used to cleanly remove the mask layers, organic and inorganic dielectric layers, and device layers. The laser scribing process may then be terminated once the wafer or substrate is exposed or partially scribed. The plasma etching portion of the dicing process may then be used to etch through the bulk of the wafer or substrate, such as bulk single crystal silicon, to effect singulation or dicing of the dies or chips. More specifically, one or more embodiments are directed to performing a dual laser scribing process that includes a first laser process and a second laser process, for example for dicing applications.
[0013] A dual laser scribing process for a hybrid laser scribing and plasma etching approach is described. For example, the dual laser scribing process may be implemented by providing a first laser scribing process having a first laser condition and a second laser scribing process having a second laser condition. The first condition and the second condition may include parameters such as laser fluence, beam size, beam polarization, etc. The dual laser scribing process described herein may be implemented to provide improved kerf width control of the hybrid laser scribing and plasma etching process. The embodiments may also be implemented to provide improved kerf width control of the laser dicing process. In one embodiment, the first laser scribing process sets a kerf width in a device layer of a semiconductor wafer and the second laser scribing process widens the width of a trench that penetrates a mask layer above the device layer. In one embodiment, the second laser scribing process maintains a desired kerf width and also improves the quality of the surface in the device layer to prepare for a subsequent plasma etch. The second laser scribing process will not significantly change the kerf width set by the first laser scribing process.
[0014] To provide context, the use of lasers for laser scribing operations is currently performed with the laser penetrating a mask to form a trench in an underlying semiconductor wafer. The laser scribing provides a trench opening having a desired width through the mask in the device layer of the semiconductor wafer. The desired width (i.e., the kerf width) is selected such that the kerf width is equal to or less than the width of the streets between the dies on the semiconductor wafer. However, the small width through the mask creates difficulties in the subsequent plasma etch used to singulate the dies. Therefore, the kerf width needs to be increased to provide suitable conditions for the subsequent plasma etch.
[0015] To address that challenge, embodiments disclosed herein include a dual laser scribing process that allows for small kerf widths in the semiconductor wafer and wide trenches through the mask layer. In one embodiment, a first laser scribing operation may be performed at a first laser intensity to provide a first opening through the mask and into the device layer of the semiconductor wafer. A second laser scribing operation is then performed using a second (higher) laser intensity to widen the trench opening through the mask layer without significantly increasing the kerf width in the device layer. The higher intensity laser may also complete the formation of a trench through the device layer to expose the underlying bulk semiconductor substrate. The kerf width does not increase because the tail of the laser pulse is substantially blocked by the mask layer.
[0016] Advantages of implementing one or more embodiments described herein may include one or more of: (1) smaller kerf width, (2) increased die density on the wafer, and / or (3) higher wafer yield. The smaller kerf width may be obtained because the mask is subsequently etched to increase the width of the opening without the need to increase the kerf width. Thus, the width of the street may be reduced and the die density increased. Furthermore, the surface of the die edge through the device layer may be made smoother by the second laser scribing operation, which results in improved plasma etching. This may result in higher wafer yield.
[0017] According to one or more embodiments of the present disclosure, a dual laser scribing process is disclosed for improving the laser scribing operation in hybrid laser dicing. Thus, one aspect of the present disclosure can use a combination of a dual laser scribing process and a plasma etching process to dice a semiconductor wafer into singulated integrated circuits. FIG. 1 is a flowchart 120 illustrating operations of a method for dicing a semiconductor wafer including multiple integrated circuits according to one embodiment of the present disclosure. FIGS. 2A-2D show cross-sectional views of a semiconductor wafer including multiple integrated circuits during operations of the method for dicing a semiconductor wafer according to one embodiment of the present disclosure corresponding to the operations of the flowchart 120.
[0018] 2A, a mask 202 is formed over a semiconductor wafer or substrate 204. The mask 202 is comprised of a layer that covers and protects the integrated circuits 206 formed on the surface of the semiconductor wafer 204. The mask 202 also covers the intervening streets 207 formed between each integrated circuit 206.
[0019] According to one embodiment of the present disclosure, forming the mask 202 includes forming a layer, such as, but not limited to, a photoresist layer or an I-line patterning layer. For example, the polymer layer, such as a photoresist layer, may be composed of a material that would otherwise be suitable for use in a lithography process. In one embodiment, the photoresist layer is composed of a positive photoresist material, such as, but not limited to, a 248 nanometer (nm) resist, a 193 nm resist, a 157 nm resist, an extreme ultraviolet (EUV) resist, or a phenolic resin matrix with a diazonaphthoquinone sensitizer. In another embodiment, the photoresist layer is composed of a negative photoresist material, such as, but not limited to, polycis-isoprene or polyvinylcinnamate.
[0020] In another embodiment, forming the mask 202 includes forming a layer that is deposited in a plasma deposition process. For example, in one such embodiment, the mask 202 is a plasma deposited Teflon layer or a Teflon-like (polymeric CF 2 In one particular embodiment, the polymer CF 2 Layer is Gas C 4 F 8 The coating is deposited in a plasma deposition process comprising:
[0021] In another embodiment, forming the mask 202 includes forming a water-soluble mask layer. In one embodiment, the water-soluble mask layer is readily soluble in an aqueous medium. For example, in one embodiment, the water-soluble mask layer is comprised of a material that is soluble in one or more of an alkaline solution, an acidic solution, or deionized water. In one embodiment, the water-soluble mask layer maintains its water solubility even when exposed to a heating process (e.g., heated in the range of about 50-160 degrees Celsius). For example, in one embodiment, the water-soluble mask layer is soluble in an aqueous solution after exposure to chamber conditions used in a laser and plasma etch singulation process. In one embodiment, the water-soluble mask layer is comprised of a material such as, but not limited to, polyvinyl alcohol, polyacrylic acid, dextran, polymethacrylic acid, polyethyleneimine, or polyethylene oxide. In a particular embodiment, the water-soluble mask layer has an etch rate in an aqueous solution in the range of about 1-15 microns per minute, and in particular, about 1.3 microns per minute.
[0022] In another embodiment, forming the mask 202 includes forming a UV curable mask layer. In one embodiment, the mask layer has a sensitivity to UV light that reduces the adhesive properties of the UV curable layer by at least about 80%. In one such embodiment, the UV layer is composed of a polyvinyl chloride or acrylic material. In one embodiment, the UV curable layer is composed of a material or a stack of such materials whose adhesive properties weaken when exposed to UV light. In one embodiment, the UV curable adhesive film is sensitive to UV light at about 365 nm. In one such embodiment, this photosensitivity allows for the use of LED light to perform the cure.
[0023] In one embodiment, the semiconductor wafer or substrate 204 is made of a material suitable for withstanding the manufacturing process, upon which the semiconductor processing layers may be appropriately disposed. For example, in one embodiment, the semiconductor wafer or substrate 204 is made of a Group IV material, such as, but not limited to, crystalline silicon, germanium, or silicon / germanium. In one particular embodiment, providing the semiconductor wafer 204 includes providing a monocrystalline silicon substrate. In one particular embodiment, the monocrystalline silicon substrate is doped with impurity atoms. In another embodiment, the semiconductor wafer or substrate 204 is made of a III-V material, such as, for example, a III-V material substrate used in the fabrication of light emitting diodes (LEDs).
[0024] In one embodiment, a semiconductor wafer or substrate 204 has an array of semiconductor devices disposed thereon or within it as part of an integrated circuit 206. Examples of such semiconductor devices include, but are not limited to, memory devices or complementary metal oxide semiconductor (CMOS) transistors fabricated in a silicon substrate and encapsulated in a dielectric layer. Metal interconnects may be formed in the dielectric layer over and around the devices or transistors and may be used to electrically couple the devices or transistors to form the integrated circuit 206. The materials making up the streets 207 may be similar or identical to the materials used to form the integrated circuit 206. For example, the streets 207 may be composed of layers of dielectric materials, semiconductor materials, and metallization. In one embodiment, one or more of the streets 207 include test devices similar to the actual devices of the integrated circuit 206.
[0025] In one embodiment, the integrated circuit 206 and the streets 207 may have a first thickness and the mask 202 may have a second thickness. The second thickness may be greater than the first thickness. For example, the first thickness may be between 3 μm and 6 μm and the second thickness may be between 30 μm and 40 μm.
[0026] Referring to operation 122 of Flowchart 120 and corresponding FIG. 2B, mask 202 is patterned in a first laser scribing process to provide patterned mask 208 having trenches 210. The trenches 210 may extend through the patterned mask 208 and into the streets 207. In one embodiment, there is no (or substantially no) recession at the interface between the patterned mask 208 and the device layer (including the integrated circuit 206 and the streets 207). That is, the sidewalls of the trenches 210 through the patterned mask 208 may be substantially coplanar with the sidewalls of the trenches 210 in the streets 207. In some embodiments, the sidewalls of the trenches 210 may be tapered (i.e., not perpendicular to the top surface of the patterned mask 208). In one embodiment, the first laser scribing process includes using a Gaussian source laser beam. In one such embodiment, the first laser scribing process includes using a femtosecond source laser beam.
[0027] In one embodiment, a femtosecond-based laser is used as the light source for the first laser scribing process. For example, in one embodiment, a laser having a wavelength in the visible spectrum plus ultraviolet (UV) and infrared (IR) ranges (together a broadband optical spectrum) is used to provide the femtosecond-based laser pulses, and the femtosecond-based laser pulses are generated over a period of about 10 femtoseconds (100 s). -15 In one embodiment, the ablation is not wavelength dependent or essentially not wavelength dependent, and therefore suitable for composite films such as the films of the mask 202 and the streets 207.
[0028] To achieve a clean laser scribe cut, the selection of laser parameters such as beam profile will be important to develop a good laser scribing and dicing process that minimizes chipping, microcracks, and delamination. The cleaner the laser scribe cut, the smoother the etching process that may be performed for final die singulation. A semiconductor device wafer typically has multiple functional layers disposed thereon of different material types (e.g., conductors, insulators, semiconductors) and different thicknesses. Such materials may include, but are not limited to, organic materials such as polymers, metals, or inorganic dielectrics such as silicon dioxide and silicon nitride.
[0029] The streets between individual integrated circuits disposed on a wafer or substrate may include layers similar to or identical to the integrated circuits themselves. For example, Figure 3 shows a cross-sectional view of a stack of materials that may be used in the street regions of a semiconductor wafer or substrate according to one embodiment of the present disclosure.
[0030] 3, a street region 300 includes a top 302 of a silicon substrate, a first silicon dioxide layer 304, a first etch stop layer 306, a first low-k dielectric layer 308 (e.g., having a dielectric constant lower than the dielectric constant of silicon dioxide, 4.0), a second etch stop layer 310, a second low-k dielectric layer 312, a third etch stop layer 314, an undoped silica glass (USG) layer 316, a second silicon dioxide layer 318, and layers of photoresist 320, the relative thicknesses of which are depicted. Copper metallization 322 is disposed between the first etch stop layer 306 and the third etch stop 314 and through the second etch stop layer 310. In one particular embodiment, the first etch stop layer 306, the second etch stop layer 310, and the third etch stop layer 314 are composed of silicon nitride, while the low-k dielectric layers 308 and 312 are composed of a carbon-doped silicon oxide material.
[0031] When the laser beam is a femtosecond-based laser beam, in one embodiment, suitable femtosecond-based laser processes are typically characterized by high peak intensity (irradiance) that results in nonlinear interactions in various materials. In one such embodiment, the femtosecond laser source has a pulse width in the range of about 10 femtoseconds to 500 femtoseconds, but preferably in the range of 100 femtoseconds to 400 femtoseconds. In one embodiment, the laser beam may have a pulse width in the range of about 10 femtoseconds to 100 picoseconds. In one embodiment, the femtosecond laser source has a wavelength in the range of about 1570 nanometers to 200 nanometers, but preferably in the range of about 540 nanometers to 250 nanometers. In one embodiment, the laser and corresponding optical system provide a focal spot at the work surface in the range of about 3 microns to 15 microns, but preferably in the range of about 5 microns to 10 microns, or between 10-15 microns.
[0032] In one embodiment, a first laser scribing process is performed at first laser conditions 212. The laser conditions 212 may include a set of laser parameters used to provide a trench having a desired topography. For example, the laser conditions 212 may include parameters such as, but not limited to, pulse repetition rate, laser fluence, laser speed across the surface, and kerf width.
[0033] In one embodiment, the first laser conditions 212 include a pulse repetition rate in the range of about 200 kHz to 10 MHz, but preferably in the range of about 500 kHz to 5 MHz. In one embodiment, the laser conditions 212 deliver a pulse energy in the range of about 1 μJ to 3 μJ to the work surface. In one embodiment, the laser scribing process proceeds along the workpiece surface at a speed in the range of about 500 mm / sec to 5 m / sec, but preferably in the range of about 600 mm / sec to 2 m / sec.
[0034] The laser scribing process may be performed in only one pass or multiple passes, but in one embodiment is preferably performed in 1-2 passes. In one embodiment, the kerf width of the generated laser beam ranges from about 2 microns to 15 microns, but for scribing / dicing silicon wafers, preferably ranges from about 6 microns to 10 microns (measured at the device / silicon interface).
[0035] Referring to operation 123 of flowchart 120 and corresponding FIG. 2C, mask 208 is patterned in a second laser scribing process to provide a patterned mask 208′ having trenches 211. In one embodiment, the second laser scribing process is performed with second laser conditions 214. The second laser conditions of the second laser scribing process may be similar to the embodiments of the first laser conditions of the first laser scribing process described, except for the laser fluence. For example, the second laser conditions 214 include a laser fluence higher than the laser fluence of the first laser condition. For example, the laser conditions 214 provide a pulse energy in the range of about 6 μJ to 8 μJ to the work surface. In one embodiment, the ratio of the laser fluence between the second laser scribing process and the first laser scribing process may be about 3:1 or more.
[0036] In one embodiment, the second laser scribing process increases the width of the trenches 211 in the patterned mask 208'. However, the kerf width in the streets 207 does not increase substantially. Thus, embodiments may include a small amount of recession of the patterned mask 208' at the interface with the streets 207. For example, a portion of the top surface 217 of the streets 207 may be exposed during the second laser scribing process. In one embodiment, the low intensity tail of the pulse is blocked by the mask layer, so there is only a small amount of recession of the mask at the mask / device layer interface. In one embodiment, the minimum width of the trenches 211 through the patterned mask 208'' is greater than the maximum width of the trenches 211 through the streets 207.
[0037] In one embodiment, the second laser scribing process increases the depth of trench 211 through street 207. In some embodiments, trench 211 may extend into substrate 204 below street 207. The second laser scribing process may also clean the surface of trench 211 in some embodiments.
[0038] In one embodiment, the first and second laser scribing processes may be performed with a single laser source. For example, a single laser source may perform a first pass (or passes) at a first intensity and the single laser source may perform a second pass (or passes) at a second intensity. In other embodiments, a first laser source may perform the first laser scribing process and a second laser source may perform the second laser scribing process.
[0039] The laser parameters for the first and second laser processes may be selected to have benefits and advantages, such as providing a sufficiently high laser intensity to achieve ionization of the inorganic dielectric (e.g., silicon dioxide) and minimizing delamination and chipping caused by underlayer damage prior to direct ablation of the inorganic dielectric. The parameters may also be selected to precisely control the width (e.g., kerf width) and depth of the ablation to provide a process throughput that is meaningful for industrial applications. In one embodiment, the first and second laser scribing processes are suitable to provide such benefits.
[0040] It should be understood that if laser scribing is also used to pattern the mask as well as scribe completely through the wafer or substrate to singulate the dies, the dicing or singulation process may be stopped after the dual laser scribing process described above. Thus, in such a case, no further singulation processing would be required. However, if laser scribing alone is not performed for complete singulation, the following embodiment may be considered.
[0041] Referring now to optional operation 124 of flowchart 120, an intermediate post-mask opening cleaning operation is performed. In one embodiment, the mask opening cleaning operation is a plasma-based cleaning process. In a first example, as described below, the plasma-based cleaning process reacts with the areas of substrate 204 exposed by trenches 211. In the case of a reactive plasma-based cleaning process, the cleaning process itself may form or extend trenches 211 in substrate 204, since the reactive plasma-based cleaning operation is at least somewhat etchant for substrate 204. In a second, different example, also described below, the plasma-based cleaning process does not react with the areas of substrate 204 exposed by trenches 211.
[0042] According to a first embodiment, a plasma-based cleaning process reacts with the exposed areas of the substrate 204, which are partially etched in the cleaning process. In one such embodiment, Ar or another non-reactive gas (or mixtures thereof) is used in place of SF for the high bias plasma treatment to clean the scribed openings. 6 A mixed gas (Ar+SF) is injected under high bias power to bombard the mask opening area and achieve cleaning of the mask opening area. 6 In the reactive breakthrough process, plasma treatment is carried out using Ar and SF 6 Physical collisions and SF 6 Both the through-etching and chemical etching with F ions contribute to cleaning the mask open areas. This approach may be suitable for photoresist or plasma deposited Teflon masks 202. In that case, the through-etching process results in a fairly uniform reduction in mask thickness and a gentle Si etch. However, such through-etching processes may not be optimal for water-soluble mask materials.
[0043] According to a second embodiment, the plasma-based cleaning process does not react with the exposed areas of the substrate 204, and the exposed areas are not etched or are etched only negligibly during the cleaning process. In one such embodiment, only plasma cleaning of a non-reactive gas is used. For example, Ar or another non-reactive gas (or mixture) is used to perform a high-bias plasma treatment for both mask condensation and cleaning of the scribed openings. This approach may be suitable for water-soluble masks or thinner plasma-deposited Teflon 202. In another such embodiment, separate mask condensation and scribed trench cleaning operations are used. For example, a high-bias plasma treatment with Ar or a non-reactive gas (or mixture) for mask condensation is performed first, followed by Ar+SF 6Plasma cleaning of the laser scribed trenches is performed with Ar+SF. This embodiment may be suitable when the mask material is too thick and therefore Ar cleaning is insufficient for trench cleaning. A thinner mask improves cleaning efficiency but significantly reduces the mask etch rate and is little consumed in the subsequent deep silicon etch process. Yet another such embodiment includes (a) high bias plasma treatment with Ar or a non-reactive gas (or mixture) for mask condensation, (b) Ar+SF for the laser scribed trenches. 6 Three cleaning operations are performed: (a) high bias plasma cleaning with Ar and (b) high bias plasma treatment with Ar or a non-reactive gas (or mixtures thereof) for mask condensation. According to another embodiment of the present disclosure, the plasma cleaning operation includes first using a reactive plasma cleaning process as described above in the first aspect of operation 106. The reactive plasma cleaning process is then followed by a non-reactive plasma cleaning process as described in connection with the second aspect of operation 106.
[0044] With reference to operation 125 of Flowchart 120 and corresponding FIG. 2D , the semiconductor wafer 204 is etched through the gaps 211 of the patterned mask 208 to singulate the integrated circuits 206. According to one embodiment of the present disclosure, etching the semiconductor wafer 204 includes eventually etching completely through the semiconductor wafer 204 by etching the trenches 211 that were initially formed in a dual laser scribing process, as depicted in FIG. 2D .
[0045] In one embodiment, patterning the mask with a laser scribing process includes forming trenches in areas between the integrated circuits of the semiconductor wafer, and plasma etching the semiconductor wafer includes extending the trenches to form corresponding trench extensions, in one such embodiment, each of the trenches has a width and each of the corresponding trench extensions has the width.
[0046] According to an embodiment of the present disclosure, the roughness of the mask opening resulting from laser scribing can affect the quality of the die sidewall resulting from the formation of the subsequent plasma etched trench. Lithographically opened masks often have a smooth profile, leading to correspondingly smooth sidewalls of the plasma etched trench. In contrast, conventional laser opened masks can have a very rough profile along the scribing direction if inappropriate laser process parameters are selected (e.g., spot overlap leading to horizontal roughness of the plasma etched trench sidewall). Although the surface roughness can be smoothed by an additional plasma process, there are cost and throughput tradeoffs to overcome such challenges. Thus, embodiments described herein may be advantageous in providing a smoother scribing process and / or a more reliable trench formation process from the laser scribing portion of the singulation process.
[0047] In one embodiment, etching the semiconductor wafer 204 includes using a plasma etching process. In one embodiment, a through silicon via etching process is used. For example, in one particular embodiment, the etch rate of the semiconductor wafer 204 material exceeds 25 microns per minute. For the plasma etching portion of the die singulation process, an ultra-high density plasma source may be used. One example of a suitable processing chamber for performing such a plasma etching process is the Applied Centura® Silvia™ Etch system available from Applied Materials, Sunnyvale, Calif., USA. The Applied Centura® Silvia™ Etch system combines capacitive and inductive RF coupling. This allows for more independent control of ion density and ion energy than is possible with capacitive coupling alone, with even improvements from magnetic enhancement. This combination effectively decouples ion density from ion energy, allowing for relatively high density plasma to be achieved even at very low pressures, without the use of potentially damaging high DC bias levels. This results in an exceptionally wide processing window. However, any plasma etch chamber capable of etching silicon may be used. In one exemplary embodiment, a deep silicon etch is used to etch a single crystal silicon substrate or wafer 204 at an etch rate greater than about 40% of a conventional silicon etch rate while maintaining essentially precise profile control and essentially scallop-free sidewalls. In one particular embodiment, a through silicon via etch process is used. The etch process is generally based on a SF 6 , C 4 F 8 , CHF 3 , XeF 2The plasma etching process is based on a plasma generated from a reactive gas, which may be a fluorine-based gas such as fluorine-based gas, or some other reactive gas capable of etching silicon at a relatively fast etching rate. In one embodiment, the mask layer 208 is removed after the singulation process, as depicted in FIG. 2D. In another embodiment, the plasma etching operation described in connection with FIG. 2D employs a conventional Bosch-type deposition / etch / deposition process to etch through the substrate 204. Typically, the Bosch-type process is composed of three sub-operations: deposition, directional bombardment etching, and isotropic chemical etching, which are performed multiple times (cycles) until the silicon is etched through.
[0048] Thus, referring back to Flowchart 120 and Figures 2A-2D, wafer dicing may be performed by initial ablation using a dual laser scribing process to penetrate the mask layer, penetrate the wafer streets (including metallization), and partially ablate into the silicon substrate. Die singulation may then be completed by a subsequent deep through-silicon plasma etch. One particular example of a material stack for dicing, according to one embodiment of the present disclosure, is described below in conjunction with Figures 4A-4E.
[0049] Referring to FIG. 4A, a material stack for hybrid laser ablation and plasma etch dicing includes a mask layer 402, a device layer 404, and a substrate 406. The mask layer, device layer, and substrate are disposed on a die attach film 408 that is attached to a support tape 410. In one embodiment, the mask layer 402 is a water-soluble layer (such as the water-soluble layer described above in connection with mask 202). The device layer 404 includes an inorganic dielectric layer (such as a silicon dioxide layer) disposed on one or more metal layers (such as a copper layer) and one or more low-k dielectric layers (such as a carbon-doped oxide layer). The device layer 404 also includes streets disposed between integrated circuits, the streets including layers the same as or similar to the integrated circuits. The substrate 406 is a bulk single crystal silicon substrate.
[0050] In one embodiment, the bulk single crystal silicon substrate 406 is thinned from the backside prior to being attached to the die attach film 408. The thinning may be performed by a backside grinding process. In one embodiment, the bulk single crystal silicon substrate 406 is thinned to a thickness in the range of about 50-100 microns. It is important to note that in one embodiment, the thinning is performed prior to the dicing process of laser ablation and plasma etching. In one embodiment, the photoresist layer 402 has a thickness of about 30 microns to 40 microns, and the device layer 404 has a thickness in the range of about 2-6 microns. In one embodiment, the die attach film 408 (or any suitable alternative capable of bonding a thinned or thinned wafer or substrate to the support tape 410) has a thickness of about 20 microns.
[0051] 4B, the mask 402 and a portion of the device layer 404 are patterned with a first laser scribing process 412 to form a trench 410. In one embodiment, the first laser scribing process 412 has first laser conditions. In one particular embodiment, the first laser conditions deliver a pulse energy at the work surface in a range of about 2 μJ to 3 μJ. The trench 410 may have a tapered sidewall profile, and the sidewalls of the trench 410 in the device layer 404 may be substantially coplanar with the sidewalls of the trench in the mask layer 402.
[0052] 4C, a second laser scribing process 414 is performed to widen the trench 410 in the mask 402 and extend the trench 410 through the device layer 404. The modified trench 411 may also extend into the silicon substrate 406. In one embodiment, the second laser scribing process 414 is performed with a second laser condition. In one particular embodiment, the second laser condition provides a pulse energy at the work surface in a range of about 6 μJ to 8 μJ. In one embodiment, the ratio of the fluence of the second laser condition to the fluence of the first laser condition may be about 3:1 or greater.
[0053] In one embodiment, the second laser scribing process increases the width of the trench 411 in the patterned mask 402. However, the kerf width in the device layer 404 does not increase substantially. Thus, embodiments may include a small amount of recession of the patterned mask 402 at the interface with the device layer 404. For example, a portion of the top surface 417 of the device layer 404 may be exposed during the second laser scribing process. In one embodiment, the low intensity tail of the pulse is blocked by the mask layer, so there is only a small amount of recession of the mask at the mask / device layer interface. In one embodiment, the minimum width of the trench 411 through the mask 402 is greater than the maximum width of the trench 411 through the device layer 404.
[0054] 4D , a deep through-silicon plasma etch process 416 is used to extend trenches 413 down to the die attach film 408, exposing a top portion of the die attach film 408 and singulating the silicon substrate 406. During the deep through-silicon plasma etch process 416, the device layer 404 is protected by the mask layer 402.
[0055] 4E, the singulation process may further include patterning the die attach film 408, exposing a top portion of the support tape 410 to singulate the die attach film 408. In an embodiment, the die attach film is singulated by a laser process or by an etching process. Further embodiments may then include removing the singulated portion of the substrate 406 (e.g., as individual integrated circuits) from the support tape 410. In an embodiment, the singulated die attach film 408 is retained on the backside of the singulated portion of the substrate 406. Other embodiments may include removing the mask layer 402 from the device layer 404. In an alternative embodiment, if the substrate 406 is thinner than about 50 microns, a dual laser scribing process 412 / 414 is used to completely singulate the substrate 406 without the use of an additional plasma process.
[0056] A single process tool may be configured to perform many or all of the operations in a dual laser ablation and plasma etch singulation process. For example, Figure 5 shows a block diagram of a tool layout for laser and plasma dicing of a wafer or substrate according to one embodiment of the present disclosure.
[0057] 5, a process tool 500 includes a factory interface 502 (FI) to which a number of load locks 504 are coupled. Coupled to the factory interface 502 is a cluster tool 506. The cluster tool 506 includes one or more plasma etch chambers, such as a plasma etch chamber 508. A laser scribe apparatus 510 is also coupled to the factory interface 502. The overall footprint of the process tool 500, in one embodiment, may be about 3500 millimeters (3.5 meters) by about 3800 millimeters (3.8 meters), as shown in FIG.
[0058] In one embodiment, the laser scribing apparatus 510 contains a laser assembly configured to provide a dual laser scribing process. In one such embodiment, the laser assembly is configured to provide a first laser scribing process having a first laser condition and a second laser scribing process having a second laser condition. The first laser condition sets a kerf width in a device layer of a semiconductor wafer, and the second laser condition increases the width of a trench through a mask layer above the device layer. The second laser condition will not significantly increase the kerf width in the device layer. In one embodiment, the laser assembly includes a Gaussian light source laser beam. In one embodiment, the laser assembly includes a femtosecond light source laser beam.
[0059] In one embodiment, the laser is suitable for performing the laser ablation portion of a hybrid laser and etch singulation process (such as the laser ablation process described above). In one embodiment, the laser scribe apparatus 510 also includes a moveable stage configured to move the wafer or substrate (or its carrier) relative to the laser. In one particular embodiment, the laser is also moveable. The overall footprint of the laser scribe apparatus 510 may be, in one embodiment, about 2240 millimeters by about 1270 millimeters, as depicted in FIG. 5.
[0060] In one embodiment, the one or more plasma etch chambers 508 are configured to etch the wafer or substrate through gaps in a patterned mask to singulate a plurality of integrated circuits. In one such embodiment, the one or more plasma etch chambers 508 are configured to perform a deep silicon etch process. In one particular embodiment, the one or more plasma etch chambers 508 are Applied Centura® Silvia™ Etch systems available from Applied Materials, Sunnyvale, Calif., USA. The etch chambers may be specifically designed for deep silicon etching used to create singulated integrated circuits contained on or in single crystal silicon substrates or wafers. In one embodiment, a high density plasma source is included in the plasma etch chamber 508 to increase the silicon etch rate. In one embodiment, two or more etch chambers are included in the cluster tool 506 portion of the process tool 500 to enable high manufacturing throughput of the singulation or dicing process.
[0061] The factory interface 502 may be an atmospheric port suitable for interfacing between an external manufacturing facility with a laser scribe apparatus 510 and the cluster tool 506. The factory interface 502 may include a robot with an arm or blade for transporting wafers (or their carriers) from a storage unit (such as a front-opening unified pod) into either the cluster tool 506 or the laser scribe apparatus 510, or both.
[0062] The cluster tool 506 may include other chambers suitable for performing functions in the singulation method. For example, in one embodiment, instead of the additional etch chamber, a deposition chamber 512 is included. The deposition chamber 512 may be configured to deposit a mask on or above the device layer of the wafer or substrate prior to laser scribing of the wafer or substrate. In one such embodiment, the deposition chamber 512 is suitable for depositing a photoresist layer. In another embodiment, instead of the additional etch chamber, a wet / dry station 514 is included. The wet / dry station may be suitable for cleaning residues and fragments or removing a mask after the substrate or wafer laser scribing and plasma etching singulation process. In yet another embodiment, instead of the additional deep silicon etch chamber, a plasma etch chamber is included, which is configured to perform a plasma-based cleaning process. In one embodiment, a metrology station is also included as a component of the process tool 500.
[0063] An embodiment of the present disclosure may be provided as a computer program product or software that may include a machine-readable medium having instructions stored thereon, which may be used to program a computer system (or other electronic device) to perform a process according to an embodiment of the present disclosure. In one embodiment, the computer system is coupled to a process tool 500, as described in connection with FIG. 5. A machine-readable medium includes any mechanism for storing or transmitting information in a form readable by a machine (e.g., a computer). For example, a machine-readable (e.g., computer-readable) medium includes a machine (e.g., computer) readable storage medium (e.g., read-only memory (ROM), random access memory (RAM), magnetic disk storage media, optical storage media, flash memory devices, etc.), a machine (e.g., computer) readable transmission medium (in electrical, optical, acoustic, or other form of propagated signal (e.g., infrared signal, digital signal, etc.)), etc.
[0064] 6 shows a schematic diagram of an exemplary form of a machine, a computer system 600, within which a set of instructions may be executed to cause the machine to perform any one or more of the methods described herein. In alternative embodiments, the machine may be connected (e.g., networked) to other machines in a local area network (LAN), an intranet, an extranet, or the Internet. The machine may function as a server or a client machine in a client-server network environment, or as a peer machine in a peer-to-peer (or distributed) network environment. The machine may be a personal computer (PC), a tablet PC, a set-top box (STB), a personal digital assistant (PDA), a mobile phone, a web appliance, a server, a network router, switch, or bridge, or any machine capable of executing a set of instructions (sequential or otherwise) that define operations to be performed by the machine. Additionally, although a single machine is illustrated, the term "machine" should also be interpreted to include any collection of machines (e.g., computers) that individually or jointly execute a set (or sets) of instructions to perform any one or more of the methodologies described herein.
[0065] The exemplary computer system 600 includes a processor 602, a main memory 604 (e.g., read only memory (ROM), flash memory, dynamic random access memory (DRAM) such as synchronous DRAM (SDRAM) or Rambus DRAM (RDRAM), etc.), a static memory 606 (e.g., flash memory, static random access memory (SRAM), MRAM, etc.), and a secondary memory 618 (e.g., a data storage device), which communicate with each other via a bus 630.
[0066] Processor 602 represents one or more general-purpose processing devices, such as a microprocessor, a central processing unit, or the like. In particular, processor 602 may be a complex instruction set computing (CISC) microprocessor, a reduced instruction set computing (RISC) microprocessor, a very long instruction word (VLIW) microprocessor, a processor implementing other instruction sets, or a processor implementing a combination of instruction sets. Processor 602 may also be one or more special-purpose processing devices, such as an application specific integrated circuit (ASIC), a field programmable gate array (FPGA), a digital signal processor (DSP), a network processor, or the like. Processor 602 is configured to execute processing logic 626 for performing the operations described herein.
[0067] Computer system 600 may further include a network interface device 608. Computer system 600 may also include a video display unit 610 (e.g., a liquid crystal display (LCD), a light emitting diode display (LED), or a cathode ray tube (CRT)), an alphanumeric input device 612 (e.g., a keyboard), a cursor control device 614 (e.g., a mouse), and a signal generating device 616 (e.g., a speaker).
[0068] The secondary memory 618 may include a machine-accessible storage medium (or specifically a computer-readable storage medium) 632 having stored thereon one or more sets of instructions (e.g., software 622) that embody any one or more of the methods or functions described herein. The software 622 may reside, completely or at least partially, within the main memory 604 and / or the processor 602 during execution by the computer system 600. The main memory 604 and the processor 602 also constitute machine-readable storage media. The software 622 may further be transmitted or received over the network 620 via the network interface device 608.
[0069] While in an exemplary embodiment, the machine-accessible storage medium 632 is depicted as a single medium, the term "machine-readable storage medium" should be interpreted to include a single medium or multiple media (e.g., a centralized or distributed database, and / or associated caches and servers) that store one or more sets of instructions. The term "machine-readable storage medium" should also be interpreted to include any medium capable of storing or encoding a set of instructions for execution by a machine that cause the machine to perform any one or more of the methods of the present disclosure. Thus, the term "machine-readable storage medium" should be interpreted to include, but is not limited to, solid-state memories, optical media, and magnetic media.
[0070] In accordance with one embodiment of the present invention, a machine accessible storage medium has stored thereon instructions for causing a data processing system to perform a method for dicing a semiconductor wafer having a plurality of integrated circuits. The method includes forming a mask on the semiconductor wafer, the mask being comprised of a layer that covers and protects the integrated circuits. The mask is then patterned using a dual laser scribing process to provide a patterned mask having gaps, exposing areas of the semiconductor wafer between the integrated circuits. The semiconductor wafer is then plasma etched through the gaps in the patterned mask to singulate the integrated circuits.
[0071] Thus, a hybrid wafer dicing approach using a dual laser scribing process and a plasma etching process has been disclosed.
Claims
1. 1. A method for dicing a semiconductor wafer having a plurality of integrated circuits, comprising: forming a mask over the semiconductor wafer; patterning the mask and the semiconductor wafer with a first laser process; patterning the mask and the semiconductor wafer with a second laser process different from the first laser process; and etching the semiconductor wafer with a plasma etch process to singulate the plurality of integrated circuits; the first laser process forms trenches through the mask in a device layer of the semiconductor wafer having a tapered sidewall profile; the second laser process increases a depth of the trench through the device layer, the second laser process increases a width of the trench in the mask while keeping a width of the trench in the device layer unincreased; a minimum width of the trench through the mask is greater than a maximum width of the trench through the device layer; method.
2. The method of claim 1 , wherein the first laser process has a first intensity and the second laser process has a second intensity, the second intensity being greater than the first intensity.
3. The method of claim 2 , wherein a ratio of the second intensity to the first intensity is 3:1 or greater.
4. The method of claim 2 , wherein the second intensity is greater than or equal to 6 μJ and the first intensity is less than or equal to 3 μJ.
5. The method of claim 1 , wherein after the first laser process, there is substantially no recession at the interface between the mask and the semiconductor wafer.
6. The method of claim 1 , further comprising a plasma cleaning operation between the second laser process and the plasma etching process.
7. The first laser process is performed using a femtosecond light source laser beam; The method of claim 1 , wherein the femtosecond source laser beam has a pulse width between 10 femtoseconds and 100 picoseconds.
8. 1. A method for dicing a semiconductor wafer having a plurality of integrated circuits, comprising: forming a mask over the semiconductor wafer; performing a first laser process to form an opening through the mask in a device layer of the semiconductor wafer having a tapered sidewall profile; and performing a second laser process to singulate the plurality of integrated circuits; the second laser process increases a depth of the opening through the device layer and increases a width of the opening in the mask while keeping a width of the opening in the device layer unchanged, the minimum width of the opening through the mask being greater than a maximum width of the opening through the device layer.
9. 9. The method of claim 8, wherein the first laser process has a first intensity and the second laser process has a second intensity, the second intensity being greater than the first intensity.
10. 10. The method of claim 9, wherein a ratio of the second intensity to the first intensity is 3:1 or greater.
11. 10. The method of claim 9, wherein the second intensity is greater than or equal to 6 μJ and the first intensity is less than or equal to 3 μJ.
12. 10. The method of claim 9, wherein after the first laser process, there is substantially no recession of the mask at an interface between the mask and the semiconductor wafer.
13. The method of claim 12 , wherein after the second laser process, there is a recession of the mask at the interface between the mask and the semiconductor wafer.
14. 14. The method of claim 13, wherein a maximum width of an opening through the semiconductor wafer is less than a minimum width of an opening through the mask.
15. 1. A system for dicing a semiconductor wafer having a plurality of integrated circuits, comprising: Factory interfaces, a laser scribing apparatus comprising a laser assembly coupled to the factory interface and configured to provide a first laser process and a second laser process; a plasma etch chamber coupled to the factory interface; The laser assembly includes: patterning a mask formed on the semiconductor wafer and the semiconductor wafer with the first laser process; patterning the mask and the semiconductor wafer with the second laser process different from the first laser process; and etching the semiconductor wafer with a plasma etch process to singulate the plurality of integrated circuits; the first laser process forms a trench through the mask in a device layer of the semiconductor wafer having a tapered sidewall profile; the second laser process increases a depth of the trench through the device layer, the second laser process increases a width of the trench in the mask while keeping a width of the trench in the device layer unincreased, and a minimum width of the trench through the mask is greater than a maximum width of the trench through the device layer.
16. 16. The system of claim 15, wherein the first laser process has a first intensity and the second laser process has a second intensity, the second intensity being greater than the first intensity.
Citation Information
Patent Citations
Wafer processing method
JP2014107283A
Water-soluble mask for dicing substrates by laser / plasma etching
JP2014523112A
Multi-step, asymmetrical laser beam scribing
JP2014523113A
Maskless hybrid laser scribing and plasma etching wafer dicing process
JP2016539497A
Dividing method for wafer
JP2017092363A