SYSTEM AND METHOD FOR INTEGRATING DEVICES ON ENGINEERED SUBSTRATES - Patent application
By using a polycrystalline ceramic core encapsulated with adhesive and barrier layers, the integration of GaN semiconductor devices on a processed substrate addresses the uniformity issues in heteroepitaxial growth, enabling high-quality, thick epitaxial layers and reliable device integration.
Patent Information
- Application Number
- JP2023114791
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-03
- Filing Date
- 2023-07-12
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2038-12-04
AI Technical Summary
Heteroepitaxial growth of gallium nitride-based semiconductors on substrates like sapphire, silicon carbide, and silicon results in reduced uniformity and adverse effects on electronic/optical properties, necessitating improved methods and systems for epitaxial growth processes and substrate structures.
The integration of gallium nitride (GaN) semiconductor devices is achieved through a method involving a polycrystalline ceramic core encapsulated with adhesive and barrier layers, followed by the formation of a single crystal layer and epitaxial III-V layers, with planarization and interconnects to form monolithically integrated devices on a processed substrate.
This approach enables the growth of high-quality, thick epitaxial layers with low defect density, allowing for the integration of various GaN devices on a single substrate, enhancing thermal stability and reducing manufacturing costs while improving device reliability and performance.
Smart Images

Figure 0007576128000001 
Figure 0007576128000002 
Figure 0007576128000003
Abstract
Description
[Technical field]
[0001]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Patent Application No. 16 / 207,793, filed December 3, 2018, which claims the benefit of U.S. Provisional Patent Application No. 62 / 595,533, filed December 6, 2017, the disclosures of which are incorporated herein by reference in their entireties for all purposes.
[0002]
[0002] The present disclosure relates to methods and systems for integrating electronic devices onto engineered substrates. [Background technology]
[0003]
[0003] Heteroepitaxy of gallium nitride-based compound semiconductors on sapphire, silicon carbide, and silicon is currently used to fabricate devices such as light emitting diodes (LEDs), high power devices, and high speed radio frequency (RF) devices. Applications include lighting, computer monitors, displays, wide band gap communications, automotive, and industrial power supplies. The growth of gallium nitride-based devices on sapphire substrates is a heteroepitaxial growth process because the substrate and epitaxial layers are composed of different materials. Due to the heteroepitaxial growth process, the epitaxially grown material may exhibit various adverse effects, including reduced uniformity and reduced metrics related to the electronic / optical properties of the epitaxial layers. Thus, there is a need in the art for improved methods and systems related to the epitaxial growth process and substrate structures used to fabricate devices. Summary of the Invention [Means for solving the problem]
[0004]
[0004] The present invention relates generally to III-V semiconductor devices formed on engineered substrate structures. More specifically, the present invention relates to methods and systems suitable for fabricating integrated gallium nitride (GaN) semiconductor devices using epitaxial growth processes. As described herein, embodiments of the present invention are applied to methods and systems for monolithically integrating different types of GaN devices on the same engineered substrate structure.
[0005] According to one embodiment of the present invention, a method for forming a plurality of devices on a substrate is provided. The method includes forming a substrate by providing a polycrystalline ceramic core, encapsulating the polycrystalline ceramic core with a first adhesive shell, encapsulating the first adhesive shell with a barrier layer, forming a bonding layer on the barrier layer, and forming a substantially monocrystalline layer bonded to the bonding layer. The method further includes forming a buffer layer bonded to the substantially monocrystalline layer, forming one or more epitaxial III-V layers on the buffer layer according to requirements related to the plurality of devices, and forming the plurality of devices on the substrate by removing portions of the one or more epitaxial III-V layers disposed between the plurality of devices and removing portions of the buffer layer disposed between the plurality of devices. In some embodiments, the one or more epitaxial III-V layers may include GaN.
[0006]
[0006] In some embodiments, the method can include planarizing a plurality of devices on a substrate. Planarizing the plurality of devices can include forming a dielectric layer on the plurality of devices and smoothing the plurality of devices using chemical mechanical planarization. In some embodiments, the method can include fabricating one or more interconnects between a first device of the plurality of devices and a second device of the plurality of devices. In some cases, the method can include bonding a first surface of each of the plurality of devices to a temporary carrier, the first surface facing the substrate, removing the substrate to expose a second surface of each of the devices, forming a conductive layer on the second surface, and bonding the carrier wafer to the conductive layer. In some embodiments, the method can include removing one or more sections of the carrier wafer to form one or more backside contacts.
[0007] According to another embodiment of the present invention, a method for forming a plurality of devices on a substrate is provided. The method includes forming a substrate by providing a polycrystalline ceramic core, encapsulating the polycrystalline ceramic core with an adhesive shell, encapsulating the adhesive shell with a barrier layer, forming a bonding layer on the barrier layer, and forming a substantially monocrystalline layer bonded to the bonding layer. The method further includes forming a conductive layer bonded to the substantially monocrystalline layer, forming a buffer layer bonded to the conductive layer, and forming one or more epitaxial III-V layers on the buffer layer according to requirements for each of the plurality of devices. The method further includes forming the plurality of devices by removing portions of the one or more epitaxial III-V layers and portions of the buffer layer disposed between the plurality of devices to expose portions of the conductive layer, forming contacts bonded to portions of the exposed portions of the conductive layer, and removing remaining exposed portions of the conductive layer not bonded to the contacts. In some embodiments, the one or more epitaxial III-V layers may include GaN.
[0008]
[0008] In some embodiments, the method further includes planarizing the plurality of devices on the substrate. Planarizing the plurality of devices can include forming a dielectric layer on the plurality of devices and smoothing the plurality of devices using chemical mechanical planarization. In some embodiments, the method can include fabricating one or more interconnects between a first device of the plurality of devices and a second device of the plurality of devices. In some embodiments, the method can include bonding a first surface of each of the plurality of devices to a temporary carrier, the first surface facing the substrate, removing the substrate to expose a second surface of each of the devices, forming a conductive layer on the second surface, and bonding the carrier wafer to the conductive layer. In some embodiments, the method can include removing one or more sections of the carrier wafer to form one or more backside contacts.
[0009] According to a further embodiment, a method for forming a plurality of devices is provided. The method includes forming a substrate by providing a polycrystalline ceramic core, encapsulating the polycrystalline ceramic core with a first adhesive shell, encapsulating the first adhesive shell with a barrier layer, forming a bonding layer on the barrier layer, and forming a substantially monocrystalline layer bonded to the bonding layer. The method further includes forming a first mask having a first exposed portion of the substantially monocrystalline layer, forming a first buffer layer associated with a first device structure on the first exposed portion, removing the first mask, forming a second mask having a second exposed portion of the substantially monocrystalline layer, forming a second buffer layer associated with a second device structure on the second exposed portion, forming one or more epitaxial III-V layers on the first buffer layer and the second buffer layer, where the one or more epitaxial III-V layers are formed according to requirements associated with the plurality of devices, and etching between the plurality of devices.
[0010]
[0010] In some embodiments, the method further includes planarizing the plurality of devices on the substrate. Planarizing the plurality of devices can include forming a dielectric layer on the plurality of devices and smoothing the plurality of devices using chemical mechanical planarization. In some embodiments, the method can include fabricating one or more interconnects between a first device of the plurality of devices and a second device of the plurality of devices. In some embodiments, the method can include bonding a first surface of each of the plurality of devices to a temporary carrier, the first surface facing the substrate, removing the substrate to expose a second surface of each of the devices, forming a conductive layer on the second surface, and bonding the carrier wafer to the conductive layer. In some embodiments, the method can include removing one or more sections of the carrier wafer to form one or more backside contacts.
[0011] In some embodiments, the method further includes forming a conductive layer coupled to the substantially monocrystalline layer and at least one of the first buffer layer and the second buffer layer, exposing a portion of the conductive layer, and forming a contact on the exposed portion of the conductive layer. In some cases, etching between the plurality of devices can include etching into a polycrystalline ceramic core.
[0012]
[0012] According to some embodiments, a semiconductor device includes a substrate. The substrate may include a polycrystalline ceramic core, a first adhesive shell encapsulating the polycrystalline ceramic core, a barrier layer encapsulating the first adhesive shell, a bonding layer bonded to the barrier layer, and a substantially monocrystalline layer bonded to the bonding layer. The semiconductor device further includes a buffer layer bonded to the substantially monocrystalline layer, and one or more epitaxial III-V layers bonded to the buffer layer. The one or more epitaxial III-V layers define a trench dividing the one or more epitaxial III-V layers into a first section and a second section. The semiconductor device further includes a first semiconductor device formed in the first section of the one or more epitaxial III-V layers, and a second semiconductor device formed in the second section of the one or more epitaxial III-V layers.
[0013] In some embodiments, the first semiconductor device is a depletion mode high electron mobility transistor (HEMT) and the second semiconductor device is an enhancement mode HEMT. In some other embodiments, the first semiconductor device is a first depletion mode high electron mobility transistor (HEMT) and the second semiconductor device is a second depletion mode HEMT. In some further embodiments, the first semiconductor device is a first enhancement mode high electron mobility transistor (HEMT) and the second semiconductor device is a second enhancement mode HEMT. In some embodiments, the semiconductor device further includes a conductive layer disposed between the substantially single crystalline layer and the buffer layer. In some embodiments, the first semiconductor device is a high electron mobility transistor (HEMT) and the second semiconductor device is a vertical semiconductor device. In some embodiments, the vertical semiconductor device is a vertical PN diode or a vertical Schottky diode.
[0014] In some embodiments, the polycrystalline ceramic core may include aluminum nitride. The first adhesion layer may include a tetraethylorthosilicate (TEOS) oxide layer. The barrier layer may include silicon nitride. The bonding layer may include silicon oxide. The substantially monocrystalline layer may include silicon. The one or more epitaxial III-V layers may include a GaN layer and an AlGaN layer.
[0015]
[0015] These and other embodiments of the present invention, along with many of its advantages and features, are described in more detail in the following text and accompanying drawings. [Brief description of the drawings]
[0016] [Figure 1] 1 is a simplified schematic cross-sectional view illustrating an engineered substrate structure, according to one embodiment of the present invention. [Figure 2A] FIG. 2 is a SIMS profile showing species concentration as a function of depth for an engineered structure in accordance with one embodiment of the present invention. [Figure 2B] FIG. 13 is a SIMS profile showing species concentration as a function of depth for an annealed engineered structure in accordance with one embodiment of the present invention. [Figure 2C] FIG. 2 is a SIMS profile showing species concentration as a function of depth for a processed structure having a silicon nitride layer after annealing, in accordance with an embodiment of the present invention. [Diagram 3] 2 is a simplified schematic cross-sectional view illustrating an engineered substrate structure according to another embodiment of the present invention. [Figure 4] 1 is a simplified schematic cross-sectional view illustrating an engineered substrate structure according to yet another embodiment of the present invention. [Diagram 5] 4 is a simplified flow chart illustrating a method of manufacturing an engineered substrate, according to one embodiment of the present invention. [Figure 6] 4 is a simplified flow chart illustrating a method of manufacturing an engineered substrate according to another embodiment of the present invention. [Figure 7]FIG. 1 is a simplified schematic cross-sectional view of an epitaxial / engineered substrate structure for RF and power applications, according to one embodiment of the present invention. [Figure 8A] FIG. 2 is a simplified schematic diagram illustrating III-V epitaxial layers on an engineered substrate structure in accordance with one embodiment of the present invention. [Figure 8B] FIG. 2 is a simplified schematic plan view illustrating a via configuration for a semiconductor device formed on an engineered substrate in accordance with another embodiment of the present invention. [Figure 9] FIG. 2 is a simplified plan view of a number of devices formed on an engineered substrate in accordance with another embodiment of the present invention. [Figure 10A] 2 is a simplified schematic cross-sectional view illustrating a number of devices formed on an engineered substrate in accordance with another embodiment of the present invention. [Figure 10B] 2 is a simplified schematic cross-sectional view illustrating multiple epitaxial III-V layers formed on an engineered substrate according to another embodiment of the present invention. [Figure 10C] 2 is a simplified schematic cross-sectional view illustrating a number of devices formed on an engineered substrate in accordance with another embodiment of the present invention. [Figure 11] 4 is a simplified flow chart illustrating a method for fabricating multiple devices on an engineered substrate in accordance with another embodiment of the present invention. [Figure 12] 2 is a simplified schematic cross-sectional view illustrating a number of devices formed on an engineered substrate in accordance with another embodiment of the present invention. [Figure 13] 4 is a simplified flow chart illustrating a method for fabricating multiple devices on an engineered substrate, according to one embodiment of the present invention. [Figure 14A] 1 is a simplified schematic cross-sectional view illustrating multiple devices having different buffer layer epitaxial structures fabricated on a single substrate according to another embodiment of the present invention. [Figure 14B] 1 is a simplified schematic cross-sectional view illustrating multiple devices having different buffer layer epitaxial structures fabricated on a single substrate according to another embodiment of the present invention. [Figure 14C]1 is a simplified schematic cross-sectional view illustrating a number of devices having different buffer layer epitaxial structures fabricated on a single substrate in accordance with another embodiment of the present invention. [Figure 14D] 1 is a simplified schematic cross-sectional view illustrating a number of devices having different buffer layer epitaxial structures fabricated on a single substrate in accordance with another embodiment of the present invention. [Figure 15] 4 is a simplified flow chart illustrating a method for fabricating multiple devices having different buffer layer epitaxial structures on a single substrate in accordance with another embodiment of the present invention. [Figure 16A] FIG. 1 illustrates an embodiment of the present invention used to form backside connections on devices grown on an engineered substrate. [Figure 16B] FIG. 1 illustrates an embodiment of the present invention used to form backside connections on devices grown on an engineered substrate. [Figure 16C] FIG. 1 illustrates an embodiment of the present invention used to form backside connections on devices grown on an engineered substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017]
[0037] The present invention generally relates to the integration of semiconductor devices on engineered substrate structures. More specifically, the present invention relates to a method suitable for manufacturing various III-V semiconductor devices using an epitaxial growth process. By way of example only, the present invention is applied to a method and system for manufacturing various III-V semiconductor devices by epitaxial growth, where the substrate structure is characterized by a coefficient of thermal expansion (CTE) substantially matched to the epitaxial layers forming the power devices. The methods and techniques can be applied to various semiconductor processing operations.
[0018]
[0038] FIGURE 1 is a simplified schematic cross-sectional view illustrating an engineered substrate structure, according to one embodiment of the present invention. The engineered substrate 100 shown in FIGURE 1 is suitable for a variety of electronic and optical applications. Engineered substrate 100 includes a core 110 that can have a coefficient of thermal expansion (CTE) that is substantially matched to the CTE of an epitaxial material that is grown on engineered substrate 100. Epitaxial material 130 is shown as optional because it is not required as an element of engineered substrate 100, but would typically be grown on engineered substrate 100.
[0019]
[0039] In applications involving the growth of gallium nitride (GaN)-based materials (epitaxial layers including GaN-based layers), the core 110 can be a polycrystalline ceramic material, such as polycrystalline aluminum nitride (AlN), which can include a binder material such as yttrium oxide. Other materials can be utilized in the core 110, including polycrystalline gallium nitride (GaN), polycrystalline aluminum gallium nitride (AlGaN), polycrystalline silicon carbide (SiC), polycrystalline zinc oxide (ZnO), polycrystalline gallium trioxide (Ga2O3), and the like.
[0020]
[0040] The thickness of the core can be on the order of 100 μm to 1,500 μm, for example, 725 μm. The core 110 is encapsulated within an adhesion layer 112, which can be referred to as a shell or encapsulation shell. In one embodiment, the adhesion layer 112 comprises a tetraethylorthosilicate (TEOS) oxide layer on the order of 1,000 Å in thickness. In other embodiments, the thickness of the adhesion layer varies, for example, from 100 Å to 2000 Å. In some embodiments, TEOS oxide is utilized for the adhesion layer, although other materials that provide adhesion between a subsequently deposited layer and an underlying layer or material (e.g., ceramic, particularly polycrystalline ceramic) can be utilized in accordance with embodiments of the present invention. For example, SiO2 or other silicon oxides (Si x O y) adheres well to ceramic materials and provides a suitable surface for subsequent deposition of, for example, conductive materials. In some embodiments, adhesion layer 112 completely surrounds core 110 to form a fully encapsulated core. Adhesion layer 112 may be formed using a low pressure chemical vapor deposition (LPCVD) process. The adhesion layer provides a surface to which subsequent layers may adhere to form elements of the engineered substrate 100 structure.
[0021]
[0041] In addition to forming an encapsulating first adhesion layer using an LPCVD process, furnace-based process, or the like, other semiconductor processes, including CVD processes or similar deposition processes, can be utilized in accordance with embodiments of the present invention. As an example, a deposition process can be utilized to coat a portion of the core, the core can be turned over, and the deposition process repeated to coat an additional portion of the core. Thus, while in some embodiments, LPCVD techniques are utilized to achieve a fully encapsulated structure, other film formation techniques can be utilized depending on the particular application.
[0022]
[0042] A conductive layer 114 is formed surrounding the adhesion layer 112. In one embodiment, the conductive layer 114 is a shell of polysilicon (i.e., polycrystalline silicon) formed surrounding the first adhesion layer 112, since polysilicon may exhibit poor adhesion to ceramic materials. In embodiments in which the conductive layer 114 is polysilicon, the thickness of the polysilicon layer may be on the order of 500-5,000 Å, for example, 2,500 Å. In some embodiments, the polysilicon layer may be formed as a shell that completely surrounds the first adhesion layer 112 (e.g., a TEOS oxide layer), thereby forming a completely encapsulated first adhesion layer, which may be formed using an LPCVD process. In other embodiments, as described below, the conductive material may be formed on a portion of the adhesion layer, for example, on the bottom half of the substrate structure. In some embodiments, the conductive material may be formed as a completely encapsulating layer and then removed on one side of the substrate structure.
[0023]
[0043] In one embodiment, the conductive layer 114 may be a polysilicon layer that is doped to provide a highly conductive material, for example, doped with boron to provide a P-type polysilicon layer. In some embodiments, the doping with boron is at least 1×10 to provide high conductivity. 19 cm -3 ~1×10 20 cm -3 Other dopants at various dopant concentrations (e.g., 1×10 16 cm -3 ~5×10 18 cm -3 Dopant concentrations ranging from 0.1 to 100% may be used (eg, phosphorus, arsenic, bismuth, etc.). One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0024]
[0044] The presence of conductive layer 114 is useful during electrostatic chucking of processed substrate 100 to a semiconductor processing tool, for example, a tool having an electrostatic discharge (ESD) chuck. Conductive layer 114 allows for rapid dechucking after processing in the semiconductor processing tool. Thus, embodiments of the present invention provide a substrate structure that can be processed in the manner utilized for conventional silicon wafers. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0025]
[0045] A second adhesion layer 116 (e.g., a TEOS oxide layer on the order of 1,000 Å thick) is formed surrounding the conductive layer 114. In some embodiments, the second adhesion layer 116 completely surrounds the conductive layer 114 to form a fully encapsulated structure. The second adhesion layer 116 can be formed using an LPCVD process, a CVD process, or any other suitable deposition process, including deposition of a spin-on dielectric.
[0026]
[0046] A barrier layer 118, for example a silicon nitride layer, is formed surrounding the second adhesive layer 116. In one embodiment, the barrier layer 118 is a silicon nitride layer with a thickness on the order of 4000 Å to 5000 Å. The barrier layer 118 completely surrounds the second adhesive layer 116 to form a fully encapsulated structure in some embodiments and can be formed using an LPCVD process. In addition to silicon nitride layers, amorphous materials including SiCN, SiON, AlN, SiC, etc. can be utilized as the barrier layer. In some implementations, the barrier layer is composed of several sub-layers that are constructed to form the barrier layer. Thus, the term barrier layer does not mean a single layer or a single material, but rather encompasses one or more materials layered in a composite manner. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0027]
[0047] In some embodiments, the barrier layer, e.g., a silicon nitride layer, prevents diffusion and / or outgassing of elements present in the core 110 into the environment of a semiconductor processing chamber in which the engineered substrate 100 may reside, e.g., during a high temperature (e.g., 1,000° C.) epitaxial growth process. Elements present in the core 110 may include, e.g., yttrium oxide (i.e., yttria), oxygen, metallic impurities, other trace elements, and the like. Elements that diffuse from the core 110 may cause unintended doping of the engineered layers 120 / 122. Elements that outgas from the core 110 may migrate through the chamber and adsorb elsewhere on the wafer, causing impurities in the engineered layers 120 / 122 and epitaxial material 130. Utilizing the encapsulation layers described herein, ceramic materials including polycrystalline AlN designed for non-cleanroom environments may be utilized in semiconductor process flows and cleanroom environments.
[0028]
[0048] FIG. 2A is a secondary ion mass spectrometry (SIMS) profile showing species concentration as a function of depth for an engineered structure according to an embodiment of the present invention. The x-axis represents the depth 202 from the surface of the engineered layer 120 / 122 to the core 110. The line 208 represents the interface between the engineered layer 120 / 122 and the core 110. The first y-axis represents the species concentration 204 in atoms per cubic centimeter. The second y-axis represents the signal intensity 206 of the ions in counts per second. The engineered structure of FIG. 2A does not include a barrier layer 118. With reference to FIG. 2A, some species present in the ceramic core 110 (e.g., yttrium, calcium, and aluminum) are reduced to negligible concentrations in the engineered layer 120 / 122. The concentrations of calcium 210, yttrium 220, and aluminum 230 are reduced by three, four, and six orders of magnitude, respectively.
[0029]
[0049] 2B is a SIMS profile showing species concentration as a function of depth for a processed structure without a barrier layer after annealing according to an embodiment of the present invention. As described above, during semiconductor processing operations, the processed substrate structure provided by an embodiment of the present invention may be exposed to high temperatures (about 1,100° C.) for several hours, for example during epitaxial growth of GaN-based layers. For the profile shown in FIG. 2B, the processed substrate structure was annealed at 1,100° C. for 4 hours. As shown in FIG. 2B, calcium 210, yttrium 220, and aluminum 230, originally present in low concentrations in the processed layer 120 / 122, diffuse into the processed layer 120 / 122 and reach similar concentrations to the other elements.
[0030]
[0050] Thus, embodiments of the present invention incorporate a barrier layer (e.g., a silicon nitride layer) to the working layer 120 / 122 and optional epitaxial material 130, such as a GaN layer, to prevent out-diffusion of background elements from the polycrystalline ceramic material (e.g., AlN). The silicon nitride layer, which encapsulates the underlying layers and materials, performs the desired barrier layer 118 function.
[0031]
[0051] FIG. 2C is a SIMS profile showing species concentration as a function of depth for a processed structure having a barrier layer 118 represented by a dotted line 240 after annealing according to an embodiment of the present invention. The integration of a diffusion barrier layer 118 (e.g., a silicon nitride layer) into the processed substrate structure prevents diffusion of calcium, yttrium, and aluminum into the processed layer during the annealing process performed when the diffusion barrier layer was not present. As shown in FIG. 2C, calcium 210, yttrium 220, and aluminum 230 present in the ceramic core remain in low concentrations in the processed layer after annealing. Thus, the use of a barrier layer 118 (e.g., a silicon nitride layer) prevents these elements from diffusing through the diffusion barrier, thereby preventing them from being released into the environment surrounding the processed substrate. Similarly, any other impurities contained within the bulk ceramic material should be contained by the barrier layer.
[0032]
[0052] Typically, the ceramic material utilized to form the core 110 is fired at a temperature in the range of 1,800°C. This process is expected to drive off a significant amount of impurities present in the ceramic material. These impurities can include yttrium resulting from the use of yttria, calcium, and other elements and compounds as sintering agents. Subsequent diffusion of these impurities is expected to be insignificant during the epitaxial growth process, which is carried out at much lower temperatures in the range of 800°C to 1,100°C. However, contrary to conventional expectations, the inventors have determined that there was significant diffusion of elements through the layers of the engineered substrate even during the epitaxial growth process at temperatures much lower than the firing temperature of the ceramic material. Accordingly, embodiments of the present invention integrate a barrier layer 118 into the engineered substrate 100 to prevent this undesired diffusion.
[0033]
[0053] Referring again to FIG. 1, a bonding layer 120 (e.g., a silicon oxide layer) is deposited on a portion of the barrier layer 118, e.g., on top of the barrier layer, and is then used during bonding of the monocrystalline layer 122. The bonding layer 120 may be about 1.5 μm thick in some embodiments. The monocrystalline layer 122 may include, for example, Si, SiC, sapphire, GaN, AlN, SiGe, Ge, diamond, Ga2O3, AlGaN, InGaN, InN, and / or ZnO. In some embodiments, the monocrystalline layer may have a thickness of 0-0.5 μm. The monocrystalline layer 122 is suitable for use as a growth layer during an epitaxial growth process for the formation of the epitaxial material 130. The crystalline layer of the epitaxial material 130 is an extension of the underlying semiconductor lattice associated with the monocrystalline layer 122. The unique CTE matching properties of the engineered substrate 100 allow for the growth of a thicker epitaxial material 130 than existing techniques. In some embodiments, the epitaxial material 130 comprises a 2 μm to 10 μm thick layer of gallium nitride, which may be utilized as one of multiple layers utilized in optoelectronic devices, power devices, etc. In one embodiment, the bonding layer 120 comprises a single crystal silicon layer that is attached to the silicon oxide barrier layer 118 using a layer transfer process.
[0034]
[0054] FIG. 3 is a simplified schematic cross-sectional view illustrating an engineered substrate structure, according to one embodiment of the present invention. The engineered substrate 300 shown in FIG. 3 is suitable for a variety of electronic and optical applications. The engineered substrate 300 includes a core 110 that can have a coefficient of thermal expansion (CTE) that is substantially matched to the CTE of an epitaxial material that is grown on the engineered substrate 300. An epitaxial material 130 is shown as optional because it is not required as an element of the engineered substrate structure, but would typically be grown on the engineered substrate structure.
[0035]
[0055] For applications involving the growth of gallium nitride (GaN)-based materials (epitaxial layers including GaN-based layers), the core 110 may be a polycrystalline ceramic material, for example, polycrystalline aluminum nitride (AlN). The thickness of the core may be on the order of 100 μm to 1,500 μm, for example, 725 μm. The core 110 is encapsulated within an adhesion layer 112, which may be referred to as a shell or encapsulation shell. In this implementation, the adhesion layer 112 completely encapsulates the core, although this is not required by the present invention, as will be explained in more detail with respect to FIG. 4.
[0036]
[0056] In one embodiment, the adhesion layer 112 comprises a tetraethylorthosilicate (TEOS) oxide layer on the order of 1,000 Å thick. In other embodiments, the thickness of the adhesion layer varies, for example, from 100 Å to 2000 Å. In some embodiments, TEOS oxide is utilized for the adhesion layer, but other materials that provide adhesion between a subsequently deposited layer and an underlying layer or material can be utilized in accordance with embodiments of the present invention. For example, SiO2, SiON, etc., adhere well to ceramic materials and provide a suitable surface for subsequent deposition of, for example, conductive materials. The adhesion layer 112, in some embodiments, completely surrounds the core 110 to form a fully encapsulated core and can be formed using an LPCVD process. The adhesion layer 112 provides a surface to which subsequent layers adhere to form elements of the engineered substrate structure.
[0037]
[0057] In addition to forming the encapsulating adhesion layer 112 using an LPCVD process, a furnace-based process, or the like, other semiconductor processes may be utilized in accordance with embodiments of the present invention. As an example, a deposition process, e.g., CVD, PECVD, etc., may be utilized to coat a portion of the core 110, the core 110 may be turned over, and the deposition process may be repeated to coat an additional portion of the core 110.
[0038]
[0058] A conductive layer 314 is formed on at least a portion of adhesion layer 112. In one embodiment, conductive layer 314 comprises polysilicon (i.e., polycrystalline silicon) formed by a deposition process on a lower portion (e.g., bottom half or backside) of the structure formed by core 110 and adhesion layer 112. In embodiments in which conductive layer 314 is polysilicon, the thickness of the polysilicon layer may be on the order of several thousand angstroms, e.g., 3,000 Å. In some embodiments, the polysilicon layer may be formed using an LPCVD process.
[0039]
[0059] In one embodiment, the conductive layer 314 may be a polysilicon layer that is doped to achieve a highly conductive material, for example, the conductive layer 314 may be doped with boron to achieve a P-type polysilicon layer. In some embodiments, the doping with boron is about 1×10 to achieve high conductivity. 19 cm -3 From 1×10 20 cm -3 to levels ranging from 0.1 to 100 .mu.m. The presence of conductive layer 314 is useful during electrostatic chucking of a processed substrate to a semiconductor processing tool, for example, a tool having an electrostatic discharge (ESD) chuck. Conductive layer 314 allows for rapid dechucking after processing. Thus, embodiments of the present invention provide a substrate structure that can be processed in the manner utilized for conventional silicon wafers. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0040]
[0060] A second adhesion layer 316 (e.g., a second TEOS oxide layer) is formed surrounding the conductive layer 314 (e.g., a polysilicon layer). The second adhesion layer 316 is on the order of 1,000 Å in thickness. The second adhesion layer 316 completely surrounds the conductive layer 114 to form a fully encapsulated structure, in some embodiments, and may be formed using an LPCVD process.
[0041]
[0061] A barrier layer 118 (e.g., a silicon nitride layer) is formed surrounding the second adhesion layer 316. The barrier layer 118, in some embodiments, is on the order of 4,000 Å to 5,000 Å in thickness. The barrier layer 118, in some embodiments, completely surrounds the second adhesion layer 316 to form a fully encapsulated structure, and may be formed using an LPCVD process.
[0042]
[0062] In some embodiments, the barrier layer 118 comprising silicon nitride is used to prevent diffusion and / or outgassing of elements present in the core 110 into the environment of a semiconductor processing chamber in which a fabricated substrate may be present, for example, during a high temperature (e.g., 1,000° C.) epitaxial growth process. Elements present in the core include, for example, yttrium oxide (i.e., yttria), oxygen, metallic impurities, other trace elements, etc. Utilizing the encapsulation layers described herein, ceramic materials including polycrystalline AlN designed for non-cleanroom environments can be utilized in semiconductor process flows and cleanroom environments.
[0043]
[0063] In some embodiments, the engineered substrate 100 can be compliant with Semiconductor Equipment and Materials Association (SEMI) standard specifications. Because the engineered substrate 100 can be compliant with SEMI specifications, the engineered substrate 100 can be used with existing semiconductor manufacturing tools. For example, the engineered substrate wafer diameter can be 4 inches, 6 inches, or 8 inches. In some embodiments, an 8 inch engineered substrate wafer can be 725-750 μm thick. In contrast, current silicon substrates used in the manufacture of epitaxial gallium nitride layers are not SEMI specification compliant because the silicon substrate has a thickness of 1050-1500 μm. As a result of the non-compliance, silicon substrates of standard wafer diameters cannot be used in equipment compliant with SEMI specifications to grow GaN-based devices.
[0044]
[0064] FIG. 4 is a simplified schematic cross-sectional view illustrating an engineered substrate structure 400 according to another embodiment of the present invention. In the embodiment shown in FIG. 4, an adhesion layer 412 is formed over at least a portion of the core 110, but does not encapsulate the core 110. In this implementation, the adhesion layer 412 is formed on the underside of the core (the backside of the core) to enhance adhesion of a subsequently formed conductive layer 414, as described more fully below. Although the adhesion layer 412 is shown only on the underside of the core in FIG. 4, it will be appreciated that deposition of adhesion layer material on other portions of the core does not adversely affect the performance of the engineered substrate structure, and such material can be present in various embodiments. Those skilled in the art will recognize many variations, modifications, and alternatives.
[0045]
[0065] The conductive layer 414 is not formed as a shell as shown in FIG. 3, but does not encapsulate the adhesive layer 412 and the core 110, and is substantially aligned with the adhesive layer 412. Although the conductive layer 414 is shown as extending along the bottom or back side of the adhesive layer 412 and over a portion of the side, this is not required by the present invention. Thus, embodiments may utilize deposition on one side of the substrate structure, masking on one side of the substrate structure, and the like. The conductive layer 414 may be formed on a portion of one side of the adhesive layer 412, e.g., the bottom / back side. The conductive layer 414 provides electrical conduction on one side of the engineered substrate structure 400, which may be advantageous in RF and high power applications. The conductive layer 414 may include doped polysilicon, as described with respect to the conductive layer 114 of FIG. 1. In addition to semiconductor-based conductive layers, in other embodiments, the conductive layer 414 is a metal layer, such as, for example, 500 Å of titanium.
[0046]
[0066] A portion of the core 110, a portion of the adhesive layer 412, and the conductive layer 414 are covered with a second adhesive layer 416 to enhance adhesion of the barrier layer 418 to the underlying material. The barrier layer 418 forms an encapsulation structure to prevent diffusion from the underlying layers, as described above in connection with Figures 2A, 2B, and 2C.
[0047]
[0067] Referring again to FIG. 4, depending on the implementation, one or more layers may be removed. For example, the adhesive layer 412 and the conductive layer 414 may be removed, leaving only a single adhesive shell 416 and a barrier layer 418. In another embodiment, only the conductive layer 414 may be removed, leaving only a single adhesive layer 412 under the barrier layer 418. In this embodiment, the adhesive layer 412 may also balance the stress and wafer warpage induced by the bonding layer 120, which is deposited on top of the barrier layer 418. Building a substrate structure with an insulating layer on top of the core 110 (e.g., with only an insulating layer between the core 110 and the bonding layer 120) provides advantages for power / RF applications where a highly insulating substrate is desired.
[0048]
[0068] In another embodiment, the barrier layer 418 can directly encapsulate the core 110, followed by the conductive layer 414 and subsequent adhesive layer 416. In this embodiment, the bonding layer 120 can be deposited directly onto the adhesive layer 416 from the top surface. In yet another embodiment, the adhesive layer 416 can be deposited on the core 110, followed by the barrier layer 418, then the conductive layer 414 and another adhesive layer 412.
[0049]
[0069] Although some embodiments have been described with respect to layers, it should be understood that the term layer can include several sub-layers that are constructed to form the layer of interest. Thus, the term layer does not mean a single layer made of a single material, but encompasses one or more materials that are layered in a composite manner to form a desired structure. Those skilled in the art will recognize many variations, modifications, and alternatives.
[0050]
[0070] FIG. 5 is a simplified flow chart illustrating a method for fabricating an engineered substrate according to an embodiment of the present invention. The method can be utilized to fabricate a substrate with a CTE matched to one or more epitaxial layers grown on the substrate. The method 500 includes forming a support structure by providing a polycrystalline ceramic core (510), encapsulating the polycrystalline ceramic core in a first adhesion layer that forms a shell (e.g., a tetraethylorthosilicate (TEOS) oxide shell) (512), and encapsulating the first adhesion layer in a conductive shell (e.g., a polysilicon shell) (514). The first adhesion layer can be formed as a single layer of TEOS oxide. The conductive shell can be formed as a single layer of polysilicon.
[0051]
[0071] The method also includes encapsulating the conductive shell in a second adhesion layer (e.g., a second TEOS oxide shell) (516), and encapsulating the second adhesion layer in a barrier layer shell (518). The second adhesion layer can be formed as a single layer of TEOS oxide. The barrier layer shell can be formed as a single layer of silicon nitride.
[0052]
[0072] Once the support structure is formed by processes 510-518, the method further includes bonding a bonding layer (e.g., a silicon oxide layer) to the support structure (520), and bonding a substantially single crystalline layer, e.g., a single crystalline silicon layer, to the silicon oxide layer (522). Other substantially single crystalline layers, including SiC, sapphire, GaN, AlN, SiGe, Ge, diamond, Ga2O3, ZnO, etc., can be used in accordance with embodiments of the present invention. Bonding the bonding layer can include deposition of a bonding material followed by a planarization process, as described herein. In the embodiments described below, bonding the substantially single crystalline layer (e.g., a single crystalline silicon layer) to the bonding layer utilizes a layer transfer process, in which the layer is a single crystalline silicon layer transferred from a silicon wafer.
[0053]
[0073] With reference to FIG. 1, the bonding layer 120 can be formed by deposition of a thick (e.g., 4 μm thick) oxide layer followed by a chemical mechanical polishing (CMP) process that thins the oxide to a thickness of about 1.5 μm. The thick initial oxide serves to fill gaps and surface features present on the support structure that may be present after fabrication of the polycrystalline core and continue to be present when the encapsulation layer shown in FIG. 1 is formed. The oxide layer also serves as a dielectric layer for the device. The CMP process achieves a substantially flat surface free of gaps, particles, or other features that can then be used during a wafer transfer process to bond a monocrystalline layer 122 (e.g., a monocrystalline silicon layer) to the bonding layer 120. The bonding layer need not be characterized by an atomically flat surface, but should achieve a substantially flat surface that supports bonding of a monocrystalline layer (e.g., a monocrystalline silicon layer) with the desired reliability.
[0054]
[0074] A layer transfer process is used to bond the monocrystalline layer 122 (e.g., monocrystalline silicon layer) to the bonding layer 120. In some embodiments, a silicon wafer including a substantially monocrystalline layer 122 (e.g., monocrystalline silicon layer) is embedded to form a cleavage plane. In this embodiment, after wafer bonding, the silicon substrate can be removed along with a portion of the monocrystalline silicon layer below the cleavage plane, resulting in a delaminated monocrystalline silicon layer. The thickness of the monocrystalline layer 122 can be varied to meet various application specifications. Moreover, the crystal orientation of the monocrystalline layer 122 can be varied to meet application specifications. Furthermore, the doping level and profile within the monocrystalline layer can be varied to meet specific application specifications. In some embodiments, the embedment depth can be adjusted to be greater than the desired final thickness of the monocrystalline layer 122. Further thickening allows removal of a thin portion of the transferred substantially monocrystalline layer that is damaged, leaving behind an undamaged portion of the desired final thickness. In some embodiments, the surface roughness can be modified for high quality epitaxial growth. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0055]
[0075] In some embodiments, the monocrystalline layer 122 may be thick enough to provide a high quality lattice template for the subsequent growth of one or more epitaxial layers, but thin enough to be highly conformal. The monocrystalline layer 122 may be said to be "conformal" when it is relatively thin so that its physical properties are less constrained, less prone to crystalline defects, and can mimic the properties of the material that surrounds it. The conformance of the monocrystalline layer 122 may be inversely proportional to the thickness of the monocrystalline layer 122. The higher the conformance, the lower the defect density of the epitaxial layer grown on the template, allowing for the growth of a thicker epitaxial layer. In some embodiments, the thickness of the monocrystalline layer 122 may be increased by epitaxial growth of silicon on the exfoliated silicon layer.
[0056]
[0076] In some embodiments, tuning the final thickness of the monocrystalline layer 122 may be achieved by thermal oxidation of the top of the exfoliated silicon layer followed by an oxide layer strip with hydrofluoric (HF) acid. For example, a exfoliated silicon layer with an initial thickness of 0.5 μm may be thermally oxidized to create a silicon dioxide layer with a thickness of about 420 nm. After removing the grown thermal oxide, the remaining silicon thickness of the transferred layer may be about 53 nm. During thermal oxidation, embedded hydrogen may migrate towards the surface. Thus, the subsequent oxide layer strip may remove some damage. Also, thermal oxidation is usually performed at temperatures of 1000° C. or higher. The increase in temperature may also repair lattice damage.
[0057]
[0077] The silicon oxide layer formed on top of the single crystal layer during thermal oxidation can be stripped using HF acid etching. The etch selectivity between silicon oxide and silicon (SiO2:Si) by HF acid may be adjusted by adjusting the temperature and concentration of the HF solution as well as the stoichiometric ratio and density of silicon oxide. Etch selectivity refers to the etch rate of one material over another. For (SiO2:Si), the selectivity of the HF solution may range from about 10:1 to about 100:1. High etch selectivity may reduce the surface roughness by a similar factor from the initial surface roughness. However, the surface roughness of the resulting single crystal layer 122 may still be greater than desired. For example, the surface of bulk Si(111) may have a root mean square (RMS) surface roughness of less than 0.1 nm as measured by an atomic force microscope (AFM) scan of 2 μm×2 μm before further processing. In some embodiments, a desirable surface roughness for epitaxial growth of gallium nitride materials on Si(111) may be, for example, less than 1 nm, less than 0.5 nm, or less than 0.2 nm over a 30 μm×30 μm AFM scan area.
[0058]
[0078] If the surface roughness of the single crystal layer 122 after thermal oxidation and oxide layer strip exceeds the desired surface roughness, further surface smoothing may be performed. There are several methods for smoothing the silicon surface. These methods may include hydrogen annealing, laser trimming, plasma smoothing, and touch polishing (e.g., CMP). These methods may include peripheral attack of high aspect ratio surface peaks. Thus, high aspect ratio features on the surface may be removed more quickly than low aspect ratio features, resulting in a smoother surface.
[0059]
[0079] It should be appreciated that the specific steps illustrated in FIG. 5 provide a particular method of manufacturing an engineered substrate in accordance with one embodiment of the present invention. Other sequences of steps may be performed according to alternative embodiments. For example, alternative embodiments of the present invention may perform the steps outlined above in a different order. Moreover, each step illustrated in FIG. 5 may include multiple sub-steps that may be performed in various orders as appropriate for the individual step. Furthermore, additional steps may be added or removed depending on the particular application. Those skilled in the art will recognize many variations, modifications, and alternatives.
[0060]
[0080] 6 is a simplified flow chart illustrating a method of manufacturing an engineered substrate according to another embodiment of the present invention. The method includes forming a support structure by providing a polycrystalline ceramic core (610) and forming an adhesion layer bonded to at least a portion of the polycrystalline ceramic core (612). The first adhesion layer can include a tetraethylorthosilicate (TEOS) oxide layer. The first adhesion layer can be formed as a single layer of TEOS oxide. The method also includes forming a conductive layer bonded to the first adhesion layer (614). The conductive layer can be a polysilicon layer. The conductive layer can be formed as a single layer of polysilicon.
[0061]
[0081] The method also includes forming a second adhesion layer bonded to at least a portion of the first adhesion layer (616), and forming a barrier shell (618). The second adhesion layer can be formed as a single layer of TEOS oxide. The barrier shell can be formed as a single layer or a series of sublayers of silicon nitride that form the barrier shell.
[0062]
[0082] Once the support structure is formed by processes 610-618, the method further includes bonding a bonding layer (e.g., a silicon oxide layer) to the support structure (620), and bonding a monocrystalline silicon layer or a substantially monocrystalline layer to the silicon oxide layer (622). Bonding the bonding layer can include deposition of a bonding material followed by a planarization process, as described herein. In the embodiments described below, bonding the monocrystalline layer (e.g., a monocrystalline silicon layer) to the bonding layer utilizes a layer transfer process in which the monocrystalline silicon layer is transferred from a silicon wafer.
[0063]
[0083] It should be appreciated that the specific steps illustrated in FIG. 6 provide a particular method of manufacturing a processed substrate according to another embodiment of the present invention. Other sequences of steps may be performed according to alternative embodiments. For example, alternative embodiments of the present invention may perform the steps outlined above in a different order. Moreover, each step illustrated in FIG. 6 may include multiple sub-steps that may be performed in various orders appropriate to the individual step. Furthermore, additional steps may be added or removed depending on the particular application. Those skilled in the art will recognize many variations, modifications, and alternatives.
[0064]
[0084] 7 is a simplified schematic cross-sectional view of an epitaxial / engineered substrate structure 700 for RF and power applications, according to one embodiment of the present invention. In some LED applications, the engineered substrate structure provides a growth substrate that enables the growth of high quality GaN layers, and the engineered substrate structure is then removed. However, in RF and power device applications, the engineered substrate structure forms part of the completed device, and as a result, the electrical, thermal, and other properties of the engineered substrate structure, or elements of the engineered substrate structure, are important for the particular application.
[0065]
[0085] Referring to FIG. 1, the monocrystalline layer 122 may be an exfoliated monocrystalline silicon layer that has been split from a silicon donor wafer using an implant and exfoliation technique. Typical implant agents are hydrogen and boron. In power and RF device applications, the electrical properties of the layers and materials of the engineered substrate structure are important. For example, some device architectures utilize highly insulating silicon layers with resistivities greater than 103 ohm cm to reduce or eliminate leakage through substrate and interface layers. Other applications utilize designs that include a conductive silicon layer of a predetermined thickness (e.g., 1 μm) to connect the source of the device to other elements. Therefore, control of the dimensions and properties of the monocrystalline silicon layer is desirable in these applications. In designs where an implant and exfoliation technique is used during layer transfer, residual implant atoms, e.g., hydrogen or boron, are present in the silicon layer, thereby changing the electrical properties. Additionally, it may be difficult to control the thickness, conductivity, and other properties of the thin silicon layer, e.g., using adjustments to the implant dose, which may affect the conductivity, and the implant depth, which may affect the thickness of the layer.
[0066]
[0086] According to an embodiment of the present invention, silicon epitaxy on an engineered substrate structure is utilized to achieve desired properties for a single crystal silicon layer appropriate for a particular device design.
[0067]
[0087] Referring to FIG. 7, an epitaxial / engineered substrate structure 700 includes an engineered substrate structure 710 and an epitaxial single crystal layer 720 formed thereon. In some embodiments, the epitaxial single crystal layer 720 can be a single crystal silicon layer. The engineered substrate structure 710 can be similar to the engineered substrate structures shown in FIGS. 1, 3, and 4. Typically, the single crystal layer 122 (e.g., a single crystal silicon layer) is on the order of 0.5 μm after layer transfer. In some processes, a surface conditioning process can be utilized to reduce the thickness of the single crystal layer 122 to about 0.3 μm. An epitaxial process is used, for example, to grow an epitaxial single crystal layer 720 on the single crystal layer 122 formed by the layer transfer process to increase the thickness of the single crystal layer 122 to about 1 μm for use in making reliable ohmic contacts. A variety of epitaxial growth processes can be used to grow the epitaxial monocrystalline layer 720, including atomic layer deposition (ALD), CVD, LPCVD, MBE, etc. The epitaxial monocrystalline layer 720 can include, for example, Si, SiC, sapphire, GaN, AlN, SiGe, Ge, diamond, Ga2O3, and / or ZnO. The thickness of the epitaxial monocrystalline layer 720 can range from about 0.1 μm to about 20 μm, for example, between 0.1 μm and 10 μm.
[0068]
[0088] FIG. 8A is a simplified schematic cross-sectional view showing a III-V epitaxial layer on an engineered substrate structure according to an embodiment of the present invention. The structure shown in FIG. 8A can be referred to as a dual epitaxial structure 800, as described below. As shown in FIG. 8A, an engineered substrate structure 810 including an epitaxial monocrystalline layer 720 has a III-V epitaxial layer 820 formed thereon. In one embodiment, the III-V epitaxial layer includes gallium nitride (GaN). To achieve electrical conductivity between portions of the III-V epitaxial layer, which may include multiple sublayers, in this example, a series of vias 824 are formed from a top surface 801 of the III-V epitaxial layer 820 through the epitaxial monocrystalline layer 720. FIG. 8A shows the vias 824 extending through the epitaxial layer 820 to the epitaxial monocrystalline layer 720. As an example, these vias can be used to connect electrodes of a diode or transistor to underlying layers by providing an ohmic contact through the vias 824, thereby mitigating charge build-up in the device. In some embodiments, one or more of the vias 824 may be insulated on their sidewalls such that they are not electrically connected to the III-V epitaxial layer 820. The electrical contacts can facilitate removal of parasitic charges, thereby enabling faster switching of the power device.
[0069]
[0089] In some embodiments, the via 826 can extend to the single crystal layer 122. To address the difficulty of fabricating the via 826 to contact the single crystal layer 122, an additional conductive epitaxial layer 822 can be grown on the single crystal layer 122 and the single crystal layer 720 to increase the size of the target conductive layer for the via 826, i.e., the thickness of the layer where the via terminates. The epitaxial single crystal layer 720 and the epitaxial III-V layer 820 can be formed thicker than conventional substrates due to the unique CTE and diffusion characteristics of the engineered substrate structure 810. Thus, existing substrate technology cannot support the growth of epitaxial layers that are defect-free enough to include the conductive epitaxial layer 822 in a device. In some embodiments, the conductive epitaxial layer 822 can be AlN, AlGaN, GaN, or a sufficiently doped semiconductor material. In certain embodiments, the conductive epitaxial layer 822 can have a thickness of 0.1 to 10 μm. In other embodiments, the thickness of the conductive epitaxial layer 822 can vary depending on the requirements of the semiconductor device. In some embodiments, the engineered substrate structure and the single crystal layer 122 can be removed to expose the epitaxial single crystal layer 720 and / or the conductive epitaxial layer 822. After removing the substrate, contacts can be formed on the exposed epitaxial layer. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0070]
[0090] In some embodiments, III-V epitaxial layers can be grown on the monocrystalline layer 122. Ohmic contacts using vias to terminate in the monocrystalline layer 122 can be made with 0.3 μm of monocrystalline layer across the wafer. Using embodiments of the present invention, monocrystalline layers with thicknesses of several microns can be achieved. Achieving thicknesses of several microns using implant and lift-off processes is difficult because large implant depths require high implant energies. The thick epitaxial monocrystalline layers described herein then enable applications such as the vias shown, enabling a variety of device designs.
[0071]
[0091] In addition to increasing the thickness of the "layer" by epitaxially growing epitaxial single crystal layer 720 on single crystal layer 122, other adjustments can be made to the original properties of single crystal layer 122, including modifying electrical conductivity, crystallinity, etc. For example, if a silicon layer on the order of 10 μm is desired prior to further epitaxial growth of III-V layers or other materials, such a thick layer can be grown according to embodiments of the present invention.
[0072]
[0092] The embedding process may affect the properties of the monocrystalline layer 122, for example, residual boron / hydrogen atoms may cause defects that affect the electrical properties of the silicon crystal layer. In some embodiments of the invention, a portion of the monocrystalline layer 122 may be removed prior to epitaxial growth of the epitaxial monocrystalline layer 720. For example, the monocrystalline silicon layer may be thinned to form a layer having a thickness of 0.1 μm or less, removing most or all of the residual boron / hydrogen atoms. Subsequent growth of a monocrystalline silicon layer is then used to achieve a monocrystalline material having electrical and / or other properties substantially independent of the corresponding properties of a layer formed using a layer transfer process.
[0073]
[0093] In addition to increasing the thickness of the single crystal silicon material bonded to the engineered substrate structure, the electrical properties, including electrical conductivity, of the epitaxial single crystal layer 720 may differ from those of the single crystal layer 122. Doping of the epitaxial single crystal layer 720 during growth can produce P-type silicon by doping with boron and N-type silicon by doping with phosphorus. Undoped silicon can be grown to achieve high resistivity silicon for use in devices with insulating regions. Insulating layers can be used, among other things, in RF devices.
[0074]
[0094] The lattice constant of the epitaxial single crystal layer 720 can be tailored during growth to be different from the lattice constant of the single crystal layer 122 to produce a strained epitaxial material. In addition to silicon, other elements can be epitaxially grown to achieve layers including strained layers including silicon germanium and the like. Additionally, the crystal orientation of the crystal planes can be utilized to introduce strain, for example, growth of (111) silicon on (100) silicon. For example, buffer layers can be grown on the single crystal layer 122, on the epitaxial single crystal layer 720, or between layers to enhance subsequent epitaxial growth. These buffer layers can include III-V semiconductor material layers such as aluminum gallium nitride, indium gallium nitride, and indium aluminum gallium nitride, silicon germanium strained layers, and the like. The strain of the III-V semiconductor material layers can be tailored to the desired material properties. Additionally, the buffer layers and other epitaxial layers can be graded by mole fraction, dopant, polarity, and the like. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0075]
[0095] In some embodiments, strain present in the single crystal layer 122 or the epitaxial single crystal layer 720 may be relieved during growth of subsequent epitaxial layers, including epitaxial III-V layers.
[0076]
[0096] FIG. 8B is a simplified schematic plan view showing four dual epitaxial structures according to an embodiment of the present invention. The dual epitaxial structures shown in FIG. 8B each include a set of vias 824. The first dual epitaxial structure 830 shows a packed via configuration. The second dual epitaxial structure 840 shows a distributed via configuration. The distributed via configuration increases the likelihood of encountering charge build-up using the vias 824 within the active area of the device. The third dual epitaxial structure 850 shows a patterned via configuration. The patterned via configuration can space the vias 824 at equal distances across the dual epitaxial structure 850. The fourth dual epitaxial structure 860 shows a lateral via 828. The lateral via 828 can be fabricated to run substantially parallel to the epitaxial layers of the dual epitaxial structure 860 and contact the single crystal layer 122 at, for example, an edge 862. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0077]
[0097] The engineered substrates described above can provide epitaxial growth thereon of gallium nitride device layers that are substantially lattice matched to the engineered substrate and feature a coefficient of thermal expansion (CTE) that is substantially matched to the engineered substrate. Thus, the engineered substrate can provide excellent thermal stability and shape control. The engineered substrate can also enable wafer diameter scaling with reuse capabilities. Relatively thick (e.g., greater than 20 μm), high-quality epitaxial gallium nitride layers can be formed on crack-free engineered substrates, and feature low defect density, low post-epitaxial warpage and stress. Multiple applications, such as power devices, radio frequency (RF) devices, monolithic microwave integrated circuits (MMICs), displays, light emitting diodes (LEDs), etc., can be implemented on a single platform. Such engineered substrates may also be suitable for various device architectures, such as lateral devices, vertical devices, and chip-scale package (CSP) devices.
[0078]
[0098] Gallium nitride (GaN) and similar wide bandgap semiconductor materials offer superior physical properties over silicon, enabling power semiconductor devices based on them to withstand high voltages and temperatures. These properties also enable higher frequency response, greater current density, and faster switching. Continuously driving higher power densities at the device and package levels results in higher temperatures and thermal gradients across the package. The use of engineered substrates for forming CTE-matched epitaxial device layers can mitigate many of the heat-related failure mechanisms common to wide bandgap devices, as described below.
[0079]
[0099] Compound semiconductor devices such as gallium nitride (GaN)-based high electron mobility transistors (HEMTs) can go into deep saturation while being exposed to high electric fields and high currents (e.g., large signal RF). Contact degradation, inverse piezoelectric effect, hot electron effect, and self-heating are among some of the common issues. For example, Schottky and ohmic contacts may show increased contact resistance and passivation cracking at temperatures above about 300°C. Interdiffusion within the gate metal stack and outdiffusion of gallium into the metal layers can occur. Hot electron effects can occur when electrons accelerated in large electric fields gain very high kinetic energy. Hot electron effects can lead to trap formation in aluminum gallium nitride (AlGaN) layers, AlGaN / GaN interfaces, passivation layer / GaN cap layer interfaces, and buffer layers.
[0080]
[0100] Trap formation can then cause current collapse and gate lag, thereby resulting in reversible degradation of the transconductance and the saturated drain current. Slow current transients are observed even when the drain or gate voltages are changed abruptly. The slow transient response of the drain current when the drain-source voltage is pulsed is called drain lag, or gate lag in the case of gate-source voltage. When the voltage in the pulse is higher than the quiescent bias point, the buffer traps capture free charges. This phenomenon is very fast compared to the pulse length. When the voltage in the pulse is lower than the quiescent bias point, the traps release their charge. This process can be very slow, even several seconds in some cases. Because the free carriers are captured and released, they do not contribute instantaneously to the output current. This phenomenon is the cause of the current transients.
[0081]
[0101] The combined effects of drain lag and gate lag lead to current collapse (a decrease in two-dimensional electron gas [2-DEG] density). Gate lag due to buffer traps is prominent when the deep acceptor density in the buffer layer is high. The inverse piezoelectric effect can occur when a high reverse bias on the gate leads to the creation of crystallographic defects. Beyond a certain critical voltage, irreversible damage to the device can occur, which can result in leakage paths through the defects. Self-heating can occur under high power stress, resulting in thermal stress distortion. Compound semiconductor devices can also suffer from field-induced degradation, such as gate hardening, and degradation at contacts, surfaces, and interfaces. Gate degradation can lead to increased leakage currents and dielectric breakdown.
[0082]
[0102] High temperature reverse bias (HTRB) testing is one of the most common reliability tests for power devices. HTRB testing evaluates long-term stability under high drain-source bias. HTRB testing aims to accelerate thermally activated failure mechanisms using biased operating conditions. During HTRB testing, device samples are stressed to or slightly below their maximum rated reverse breakdown voltage at an ambient temperature close to their maximum rated junction temperature for an extended period of time (e.g., 1,000 hours). This tests that high temperature accelerates failure mechanisms according to the Arrhenius equation, which describes the temperature dependence of reaction rates. Delamination, popping, device blow-up, and other mechanical problems can occur during HTRB testing.
[0083]
[0103] A failure mechanism similar to time-dependent dielectric breakdown (TDDB), a common failure mechanism in MOSFETs, is also observed in the gate dielectric of wide bandgap semiconductor devices such as GaN power devices. TDDB occurs when the gate dielectric breaks down due to the application of a relatively low electric field for a long period of time (as opposed to the immediate breakdown caused by a strong electric field). In addition, failures during temperature cycling (TMCL) can be related to package stress, bond pad hardening, mold compound, moisture sensitivity, and other package-level issues.
[0084]
[0104] As discussed above, the engineered substrate can have a CTE that matches the CTE of one or more epitaxial GaN device layers grown thereon. The epitaxial GaN device layers may be lattice matched to the engineered substrate. Thus, the epitaxial GaN device layers can have a lower defect density and higher quality. A relatively thick drift region may be formed by epitaxial growth. Also, large diameter wafers may be created from the engineered substrate, thereby lowering manufacturing costs. The engineered substrate can improve device reliability. For example, matching the CTE with the CTE of the epitaxial GaN device can help alleviate thermal stress, which is a key factor in device reliability. Device failures related to thermal stress include thermally activated drain-source breakdown, punch-through effects, breakdown along the channel, and breakdown through the buffer layer. Self-heating may also be reduced. In addition, high quality epitaxial GaN layers with low defect density can help improve device reliability, since some defects can be activated with voltage stress and contribute to lateral and vertical leakage. High-quality epitaxial GaN layers can also address issues such as localized non-stoichiometric regions that can affect the electric field distribution and dislocation density.
[0085]
[0105] Conventional silicon-based MOSFET technology is approaching its physical limits in performance and switching speed. Lateral GaN-based high electron mobility transistors (HEMTs) offer opportunities beyond the silicon-based MOSFET realm in medium to low power systems such as solar inverters, power factor correction (PFC), switch mode power supplies (SMPS), motor drives, RF power amplifiers, solid-state lighting (SSL), smart grids, and automotive motor drive systems. Lateral GaN-based HEMTs can offer high efficiency, high frequency operation, and low switching and conduction losses, among many other advantages.
[0086]
[0106] Some embodiments of the present invention use the mechanical and electrical properties realized by engineered substrates to integrate various device types, such as lateral GaN-based power devices and optoelectronics, onto a single substrate. FIG. 9 is a simplified plan view of multiple devices fabricated on engineered substrate 900. The unique properties of engineered substrates described above facilitate the integration of devices that cannot be combined on other substrates. Engineered substrates provide an insulating substrate with excellent thermal conductivity on which high quality thick GaN can be grown. For example, engineered substrate 900 can include an integrated circuit having multiple devices, each device being a different type of device. A first device 902 can be a lateral enhancement mode (normally off) high electron mobility transistor (HEMT). A second device 904 can be a lateral depletion mode (normally on) HEMT. A third device 906 can be a vertical enhancement mode HEMT, and a fourth device 908 can be a vertical depletion mode HEMT.
[0087]
[0107] The device types are not limited to the examples provided herein. Any combination of enhancement mode (EM) and depletion mode (DM) devices can be formed on the engineered substrate 900. Although lateral devices are preferred for most integrated circuits, the embodiments described herein using engineered substrate 900 can combine EM or DM lateral devices with EM or DM vertical devices. In addition to differences in lateral dimensions, adjacent devices on substrate 900 can differ in semiconductor structure and construction. The structure and construction can be used to control differences in operating voltages and currents of individual devices. In addition to individual device characteristics, the processes described herein can provide electrical isolation between individual devices. Thus, engineered substrate 900 provides a surface that can isolate devices. In some embodiments, multiple devices can be fabricated on the engineered substrate such that there is no electrical conduction between the multiple devices through the substrate. One skilled in the art would recognize many variations, modifications, and alternatives.
[0088]
[0108] FIG. 10A is a simplified schematic cross-sectional view illustrating a plurality of devices formed on an engineered substrate 1010 according to another embodiment of the present invention. The plurality of devices includes a first device 1004 fabricated according to a process flow that causes the device to function as a depletion mode (normally on) HEMT, and a second device 1006 fabricated according to a process flow that includes a recess 1042 in a second channel region 1044. The recess 1042 in the second channel region 1044 causes the second device 1006 to function as an enhancement mode (normally off) HEMT. The plurality of devices can be formed on the engineered substrate 1010 according to a unique set of device requirements for each of the plurality of devices. In some embodiments, the engineered substrate 1010 may include a polycrystalline ceramic core 1008, a first adhesion layer bonded to the polycrystalline ceramic core 1008, a barrier layer bonded to the first adhesion layer, a bonding layer bonded to the barrier layer, and a substantially single crystalline layer bonded to the bonding layer, as described above with reference to FIGS. 1, 3, and 4. In some embodiments, the adhesion, bonding, and barrier layers may be formed as shells surrounding the polycrystalline ceramic core 1008 .
[0089]
[0109] Although FIG. 10A illustrates the first device 1004 as a depletion mode (normally on) HEMT and the second device 1006 as an enhancement mode (normally off) HEMT, the first device 1004 and the second device 1006 may both be depletion mode (normally on) HEMTs or both enhancement mode (normally off) HEMTs, according to various embodiments.
[0090]
[0110] According to one embodiment, the engineered substrate 1010 may further include a substantially single crystalline layer 1012 bonded to the bonding layer. For example, the substantially single crystalline layer 1012 may comprise a substantially single layer of crystalline silicon. In some embodiments, the engineered substrate 1010 may further include a nucleation layer 1014 bonded to the substantially single crystalline layer 1012 to facilitate the formation of an epitaxial device layer comprising a substantially single crystalline GaN-based material. In some embodiments, the nucleation layer 1014 may be doped at a level equal to, less than, or greater than the surrounding layers. In other embodiments, the composition of the nucleation layer may be designed and implemented with a predetermined composition.
[0091]
[0111] In another embodiment, the polycrystalline ceramic core 1008 of the engineered substrate 1010 comprises aluminum nitride. In some embodiments, the engineered substrate 1010 may further comprise a conductive layer coupled to the first adhesive layer and a second adhesive layer coupled to the conductive layer, the conductive layer and the second adhesive layer being disposed between the first adhesive layer and the barrier layer, as described above with reference to FIG. 1. In some embodiments, the first adhesive layer may comprise a first tetraethylorthosilicate (TEOS) oxide layer and the second adhesive layer may comprise a second TEOS oxide layer. The barrier layer may comprise a silicon nitride layer. The conductive layer may comprise a polysilicon layer.
[0092]
[0112] According to one embodiment, devices 1000 further include a buffer layer 1020 (e.g., a gallium nitride (GaN) buffer layer) coupled to nucleation layer 1014 and substantially single crystalline layer 1012. Buffer layer 1020 may be formed by epitaxial growth on either nucleation layer 1014 or substantially single crystalline layer 1012. According to one embodiment, buffer layer 1020 may have a thickness greater than about 20 μm. In some embodiments, buffer layer 1020 may be formed of aluminum gallium nitride (i.e., Al x Ga 1-xGaN) buffer layers, or may be a combination of GaN and AlGaN layers, e.g., multiple layers of a single material or multiple layers of different materials. In some embodiments, the layers described as GaN layers may be Al x Ga 1-x Note that the buffer layer 1020 may be replaced with an N layer. As an example, the buffer layer 1020 may be made of a first set of mole fractions of Al x Ga 1-x N, and the barrier layer 1032 has a second set of mole fractions of Al x Ga 1-x N. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0093]
[0113] Al x Ga 1-x A power device using an N buffer layer has a first predetermined mole fraction (x) of AlN that extends from the engineered substrate and a second predetermined mole fraction (x) proximate the source, gate, and drain contacts. x Ga 1-x The channel region 1030 can be introduced by fabricating a N buffer layer. The first predetermined mole fraction (x) can be low, for example, less than 10%, to achieve the desired carrier confinement. In other embodiments, the aluminum mole fraction (x) is in the range of 10% to 30%. x Ga 1-x The N epitaxial layer may be doped with iron or carbon to further increase the resistivity of the epitaxial layer, which acts as an insulating or blocking layer. Further description regarding epitaxial buffer layers and materials used in the fabrication of epitaxial buffer layers is provided in U.S. Provisional Patent Application No. 62 / 447,857, the disclosure of which is incorporated herein by reference in its entirety for all purposes.
[0094]
[0114] A thicker buffer layer 1020 can provide lower leakage currents and higher breakdown voltages to the devices 1000. In some embodiments, the buffer layer 1020 can include multiple layers. For example, the buffer layer 1020 can include an aluminum nitride layer, an aluminum gallium nitride layer, and a gallium nitride layer. In some embodiments, the buffer layer 1020 can include as many as 150 layers of a superlattice, with each layer having a thickness of about 2-3 nm. A superlattice is an artificial lattice fabricated by periodic epitaxial growth. A periodic superlattice is realized by growing alternating layers of two semiconductors on top of each other, with each semiconductor grown to the same thickness and mole fraction each time. According to some embodiments of the present invention, an advantage of using a superlattice instead of other buffer layer designs is that the superlattice can reduce sheet resistance, for example by growing an AlGaN / GaN superlattice layer over the channel region, and can reduce potential barrier heights at heterointerfaces. In other embodiments, the superlattice does not reduce potential barrier heights at heterointerfaces. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0095]
[0115] According to an embodiment, the plurality of devices 1000 further includes a channel region for each device. The channel region for each device can be fabricated by forming one or more epitaxial III-V layers on the buffer layer 1020. The first device 1004 includes a first channel region 1030 corresponding to a region near an interface of the one or more epitaxial III-V layers associated with the first device 1004 and the buffer layer 1020. The first channel region 1030 has a first end 1024, a second end 1026, and a central portion 1028 disposed between the first end 1024 and the second end 1026. The central portion of the first channel region 1030 may include a channel region barrier layer. In some embodiments, the channel region barrier layer is a barrier layer 1032 (e.g., aluminum gallium nitride (Al GaN)) coupled to the buffer layer 1020. x Ga 1-xThe barrier layer 1032 may be a GaN (gallium nitride) cap layer, and a cap layer 1034 (e.g., a gallium nitride cap layer) coupled to the barrier layer 1032. The cap layer 1034 helps to reduce reverse leakage through the Schottky contact and reduces the peak electric field. The cap layer 1034 also protects the barrier layer 1032 during processing and prevents nitrogen outgassing. In addition, the cap layer 1034 also positively impacts device performance such as increased gain, increased power added efficiency, and improved DC stability.
[0096]
[0116] The first device 1004 further includes a source contact 1040 disposed at a first end of the first channel region 1030, a drain contact 1050 disposed at a second end of the first channel region 1030, and a gate contact 1060 coupled to the cap layer 1034 and disposed at a central portion of the channel region 1030. In some embodiments, the via 1002 can connect the source contact 1040 to the single crystal layer 1012 or a conductive layer to remove parasitic charges in the power device. In contrast to GaN on silicon, which can utilize a backside contact through a conductive silicon substrate, embodiments of the invention utilizing insulating engineered substrates can utilize vias such as the via 1002 to achieve electrical connection to the single crystal layer 1012. According to embodiments of the invention, the barrier layer 1032 and the cap layer 1034 are formed by epitaxial growth. As shown in FIG. 10A, during operation, a thin two-dimensional electron gas (2DEG) layer 1036 can be formed in the buffer layer 1020 at the interface between the buffer layer 1020 and the barrier layer 1032. The electrons in this thin 2DEG layer 1036 can move quickly without colliding with any impurities because the buffer layer 1020 is undoped, which can give the channel 1038 a very low resistivity, which in turn gives a very high electron mobility.
[0097]
[0117] In some embodiments, the first device 1004 may further include a passivation layer 1070 covering the cap layer 1034. The passivation layer 1070 may include silicon nitride or other insulating material. The first device 1004 may also include a first field plate metal 1080 electrically connecting to the source contact 1040 forming the source electrode, and a second metal 1090 disposed on the drain contact 1050 forming the drain electrode.
[0098]
[0118] The plurality of devices 1000 further includes a second device 1006. The second device may share one or more epitaxial III-V layers with the first device 1004, such as the barrier layer 1032. The second device may function as an enhancement mode (normally off) HEMT using a recess 1042 in a second channel region 1044. The second device 1006 may be formed on the same engineered substrate 1010 as the first device 1004. According to one embodiment, the second device 1006 may be formed on the same buffer layer 1020 as the first device 1004.
[0099]
[0119] The second device 1006 includes a second channel 1044 corresponding to a region near the interface of one or more epitaxial III-V layers associated with the second device 1006 and the buffer layer 1020. The channel region 1044 has a first end 1046, a second end 1048, and a central portion 1052 disposed between the first end 1046 and the second end 1048. The central portion 1052 of the channel region 1044 may include an epitaxial channel region barrier layer. In some embodiments, the epitaxial channel region barrier layer is a barrier layer 1032 (e.g., aluminum gallium nitride (Al GaN)) coupled to the buffer layer 1020. x Ga 1-xThe second device 1006 may be a first (N) barrier layer). According to an embodiment of the present invention, the barrier layer 1032 is formed by epitaxial growth. The barrier layer 1032 includes a recess 1042 in a central portion of the channel region 1052. The recess may be formed by removing a portion of the barrier layer 1032 using etching or other suitable techniques. The second device 1006 further includes an insulating layer 1062 disposed in the recess and coupled to the barrier layer 1032.
[0100]
[0120] The second device 1006 further includes a source contact 1054 disposed at a first end of the channel region 1044, a drain contact 1056 disposed at a second end of the channel region 1044, and a gate contact 1058 coupled to the insulating layer 1062 and disposed in a central portion of the channel region 1044. In various embodiments, the gate contact 1058 can be coupled to a multi-layer epitaxial gate structure. The epitaxial gate structure can be formed on the barrier layer instead of removing a portion of the barrier layer to form a normally-off HEMT. In some embodiments, a via 1064 can be used to connect the source contact 1054 to the single crystal layer 1012 to remove parasitic charges in the second device 1006.
[0101]
[0121] As shown in FIG. 10A, a thin 2DEG layer 1066 may be formed in the buffer layer 1020 adjacent to the barrier layer 1032 associated with the second device 1006. Electrons in this thin 2DEG layer 1066 can move quickly without colliding with any impurities because the buffer layer 1020 is undoped. This can give the second channel region 1044 a very low resistivity, or in other words, a very high electron mobility. In depletion mode (normally off), when the gate voltage is zero, the recess 1042 and the insulating layer 1062 block a portion of the 2DEG layer. Further description of the materials and fabrication of epitaxial buffer layers and epitaxial gate structures is provided in U.S. Patent Application Serial No. 15 / 684,724, the disclosure of which is incorporated herein by reference in its entirety for all purposes.
[0102]
[0122] The plurality of devices 1000 may be isolated by a non-conductive buffer layer. In some embodiments, the plurality of devices 1000 may be further isolated by forming a recess 1068 in a portion of the buffer layer 1020. The recess 1068 may be formed by removing a portion of the buffer layer 1020 disposed between the devices. The recess may be formed by removing a portion of the buffer layer 1020 using etching or other suitable techniques. One of ordinary skill in the art would recognize many variations, modifications, and alternatives.
[0103]
[0123] 10B is a simplified schematic cross-sectional view illustrating multiple epitaxial III-V layers that can be formed on an engineered substrate according to another embodiment of the present invention. In some embodiments, multiple epitaxial III-V layers can be formed on an engineered substrate 1010. For example, a back contact layer 1015 can be formed on the engineered substrate 1010. A buffer layer 1020 can be formed on the back contact layer 1015. A channel layer 1021 can be formed on the buffer layer 1020. The channel layer 1021 can be, for example, an AlN layer having a first predetermined mole fraction (x) and a second predetermined mole fraction (x) extending from the engineered substrate 1010 and / or the back contact layer 1015 to form the channel layer 1021. x Ga 1-x A first buffer layer 1020 may be formed by fabricating a first N buffer layer 1020. A p-type GaN layer or p-GaN layer 1023 may then be formed on the channel layer 1021. A second buffer layer 1025 may be formed on the p-GaN layer 1023. A second channel layer 1027 may be formed on the second buffer layer 1025. The thicknesses of the first buffer layer 1020 and the second buffer layer 1025 may be based on or related to the voltage rating of one or more devices formed by the epitaxial III-V layers. In some embodiments, the thickness may range from 1 μm to 15 μm. In some embodiments, an AlGaN gate layer 1029 may be formed on the second channel layer 1027.
[0104]
[0124] FIG. 10C is a simplified schematic cross-sectional view showing a plurality of devices formed on a processed substrate according to another embodiment of the present invention. In some embodiments, a portion of the epitaxial III-V layers shown in FIG. 10B can be selectively removed using one or more CMOS compatible processing techniques to form a plurality of devices on the processed substrate, e.g., HEMT devices and lateral junction gate field effect transistors (LJFETs). For example, a portion of the AlGaN gate layer 1029 can be removed to expose a portion of the second channel layer 1027 and form a first gate 1047 for the HEMT device. A first HEMT gate contact 1033 can be formed on the first gate 1047. A first HEMT drain contact 1035 and a first HEMT source contact 1031 can be formed on the exposed portion of the second channel layer 1027.
[0105]
[0125] In some embodiments, one or more portions of the second buffer layer 1025 can be removed to expose the p-GaN layer 1023. A HEMT back contact 1037 can be formed on a first exposed portion of the p-GaN layer 1023, and a second LJFET gate contact 1041 can be formed on a second exposed portion of the p-GaN layer 1023. One or more portions of the p-GaN layer 1023 can be removed to form one or more exposed portions of the channel layer 1021. A second LJFET source contact 1039 and a first LJFET drain contact 1043 can be formed on one or more exposed portions of the channel layer 1021. One or more portions of the channel layer 1021 and the buffer layer 1020 can be removed to expose one or more portions of the back contact layer 1015. A HEMT back contact 1045 can be formed on one or more exposed portions of the back contact layer 1015. It should be appreciated that the specific layers and devices shown in Figures 10B and 10C provide a particular arrangement of integrated devices formed on an engineered substrate according to an embodiment of the present invention. Other layers, devices, or contacts may be formed thereon according to alternative embodiments. Additionally, the individual devices, layers, and components shown in Figures 10B and 10C may include multiple sublayers that may be fabricated in various arrangements as appropriate for the individual devices. Additionally, additional devices, layers, or components may be added, or existing layers or components may be removed, depending on the particular application. Those skilled in the art will recognize many variations, modifications, and alternatives.
[0106]
[0126] 11 is a simplified flow chart illustrating a method 1100 of fabricating multiple devices on an engineered substrate according to one embodiment of the present invention. According to one embodiment, the method 1100 includes, at 1110, providing a polycrystalline ceramic core, encapsulating the polycrystalline ceramic core with a first adhesive shell, encapsulating the first adhesive shell with a barrier layer, forming a bonding layer on the barrier layer, and bonding a substantially single crystalline layer to the bonding layer to form a substrate.
[0107]
[0127] The method 1100 further includes, at 1112, forming a buffer layer (e.g., a GaN buffer layer) on the substrate, and, at 1114, forming one or more epitaxial III-V layers on the buffer layer according to device-related requirements. In some embodiments, forming the one or more epitaxial III-V layers includes forming an epitaxial III-V barrier layer (e.g., Al SiO 2 ) on the buffer layer. x Ga 1-x The method can include forming a channel region on the buffer layer by forming an epitaxial cap layer (e.g., a gallium nitride cap layer) on the barrier layer, and forming an epitaxial cap layer (e.g., a gallium nitride cap layer) on the barrier layer. The channel region has a first end and a second end and a central portion between the first end and the second end.
[0108]
[0128] The method 1100 further includes, at 1116, forming a plurality of devices on the substrate by removing a portion of the one or more epitaxial III-V layers disposed between the plurality of devices and removing a portion of the buffer layer disposed between the plurality of devices. The one or more epitaxial III-V layers may include an active layer. The active layer and the buffer layer may be etched using techniques such as chemical etching or plasma etching. The active layer and the buffer layer may be removed to a certain depth. In some embodiments, the depth depends on the device requirements.
[0109]
[0129] In some embodiments, forming the plurality of devices can include forming a plurality of source contacts, each source contact at a first end of a channel region associated with one or more of the plurality of devices, forming a plurality of drain contacts, each drain contact at a second end of a channel region associated with one or more of the plurality of devices, and forming a gate contact central portion of the channel region, each gate contact associated with one or more of the plurality of devices. In some embodiments, the gate contacts can be formed on the cap layer and / or the epitaxial gate structure.
[0110]
[0130] In some embodiments, forming the plurality of devices on the substrate can further include planarizing the plurality of devices by various methods. Methods include, for example, depositing a dielectric material and performing chemical mechanical planarization (CMP). In various embodiments, the various device types can be monolithically integrated on the same engineered substrate with device interconnects. In some embodiments, street etching can be used to further isolate a first set of integrated devices from a second set of integrated devices. Following integration of the various device types, conductive pads can be formed on the integrated devices, and the integrated devices can be packaged for use as integrated circuits.
[0111]
[0131] It should be appreciated that the specific steps illustrated in FIG. 11 provide a particular method of fabricating multiple devices on an engineered substrate according to another embodiment of the present invention. Other sequences of steps may be performed according to alternative embodiments. For example, alternative embodiments of the present invention may perform the steps outlined above in a different order. Moreover, each step illustrated in FIG. 11 may include multiple sub-steps that may be performed in various orders as appropriate for the individual step. Furthermore, additional steps may be added or removed depending on the particular application. Those skilled in the art will recognize many variations, modifications, and alternatives.
[0112]
[0132] 12 is a simplified schematic cross-sectional view showing a plurality of devices 1200 formed on an engineered substrate 1210 according to another embodiment of the invention. The plurality of devices includes a first device 1204 fabricated on an engineered substrate 1210, a conductive layer 1248, and a buffer layer 1220. In some embodiments, the conductive layer 1248 is bonded to the engineered substrate 1210 and the buffer layer 1220. The first device 1204 is similar to the first device 1004 shown in FIG. 10A. In some embodiments, the second device 1206 can be fabricated using the same engineered substrate 1210, conductive layer 1248, and buffer layer 1220 as the first device 1204.
[0113]
[0133] In some embodiments, as described above with reference to Figures 1, 3, and 4, the engineered substrate 1210 may include a polycrystalline ceramic core 1208, a first adhesion layer bonded to the polycrystalline ceramic core 1208, a barrier layer bonded to the first adhesion layer, a bonding layer bonded to the barrier layer, and a substantially single crystalline layer bonded to the bonding layer. According to one embodiment, the engineered substrate 1210 may further include a substantially single crystalline layer 1212 bonded to the bonding layer. For example, the substantially single crystalline layer 1212 may comprise substantially single crystalline silicon. In some embodiments, the engineered substrate 1210 may further include a nucleation layer (not shown) bonded to the substantially single crystalline layer 1212 to facilitate formation of an epitaxial device layer. In various embodiments, the polycrystalline ceramic core 1208 is comprised of the materials described above with reference to Figures 1, 3, 4, and 10.
[0114]
[0134] According to one embodiment, the second device 1206 can be fabricated using a buffer layer 1220 bonded to a conductive layer 1248. The conductive layer 1248 is further bonded to the substantially single crystalline layer 1212. In some embodiments, the buffer layer 1220 can be a superlattice including multiple layers. For example, the buffer layer 1220 can include an aluminum nitride layer bonded to a single crystalline silicon layer, an aluminum gallium nitride layer bonded to the aluminum nitride layer, and a gallium nitride layer bonded to the aluminum gallium nitride layer. The second device 1206 can include a semi-insulating layer (not shown) bonded to the buffer layer 1220. In one embodiment, the semi-insulating layer includes gallium nitride.
[0115]
[0135] According to some embodiments, the buffer layer 1220 may be conductive. In various embodiments, the buffer layer 1220 may be doped to a predetermined concentration. The second device 1206 includes the buffer layer 1220 as a first N-type gallium nitride layer bonded to a conductive layer 1248, a second N-type gallium nitride layer 1244 bonded to the first N-type gallium nitride layer (buffer layer 1220), and a P-type gallium nitride layer 1246 bonded to the second N-type gallium nitride layer 1244. The buffer layer 1220 may function as an N region of a PN diode and may have a relatively high N-type doping concentration. The second N-type gallium nitride layer 1244 may function as a drift region and may have a relatively low doping concentration compared to the doping concentration of the first N-type gallium nitride layer (buffer layer 1220). The P-type gallium nitride layer 1246 may function as a P region of a PN diode and may have a relatively high P-type doping concentration.
[0116]
[0136] In one embodiment, a portion of the second N-type gallium nitride layer 1244, a portion of the P-type gallium nitride layer 1246, and the first N-type gallium nitride layer (buffer layer 1220) are removed to expose a portion of the conductive layer 1248 so that a cathode contact 1270 may be formed thereon. In other embodiments, a cathode contact may be formed on the first N-type gallium nitride layer (buffer layer 1220). In some embodiments, the cathode contact 1270 may comprise a titanium aluminum (Ti / Al) alloy or other suitable metallic material. A portion of the first N-type gallium nitride layer (buffer layer 1220), a portion of the second N-type gallium nitride layer 1244, and a portion of the P-type gallium nitride layer 1246 may be removed by etching or other suitable techniques. An anode contact 1260 is formed on the remaining portion of the conductive layer 1248. In some embodiments, the anode 1260 may comprise a nickel platinum (Ni / Pt) alloy, a nickel gold (Ni / Au) alloy, or the like. The second device 1206 may further include a first field plate 1282 coupled to the anode contact 1260 and a second field plate 1284 coupled to the cathode contact 1270. In some embodiments, the second device 1206 may further include a passivation layer 1070 covering the P-type gallium nitride layer 1246 and the exposed surfaces of the first N-type gallium nitride layer (buffer layer 1220), as well as the second N-type gallium nitride layer 1244. The passivation layer 1070 may include silicon nitride or other insulating material. In some other embodiments, the second device 1206 may be formed as a Schottky diode.
[0117]
[0137] In some embodiments, the second N-type gallium nitride layer 1244 can have a thickness of greater than about 20 μm. The unique CTE matching properties of the engineered substrate 1210 provide a substrate that can be used to deposit a relatively thick drift region with low dislocation density. These properties can provide the second device 1206 with low leakage currents and much higher breakdown voltages, as well as many other advantages.
[0118]
[0138] The first device 1204 is electrically isolated from the second device 1206 by a deep etch. The deep etch of one or more layers 1268 can remove the buffer layer 1220, the conductive layer 1248, and the substantially single crystalline layer 1212 to expose the polycrystalline ceramic core 1208 of the engineered substrate 1210. The individual device requirements or the specific application of the integrated circuit can determine whether the recess 1068 shown in FIG. 10A or the deep etch of one or more layers 1268 shown in FIG. 12 is fabricated. The deep etch of one or more etched layers 1268 can facilitate fabrication of lateral device structures, such as a cathode contact 1270 adjacent to the buffer layer 1220. Additionally, the removal of one or more etched layers 1268 can facilitate fabrication of a connection to the backside of the device, if desired. One skilled in the art would recognize many variations, modifications, and alternatives.
[0119]
[0139] 13 is a simplified flow chart illustrating a method 1300 of fabricating multiple devices on an engineered substrate in accordance with one embodiment of the present invention. The method 1300 includes forming a substrate at 1310 by providing a polycrystalline ceramic core, encapsulating the polycrystalline ceramic core with an adhesive shell, encapsulating the adhesive shell with a barrier layer, forming a bonding layer on the barrier layer, and forming a substantially single crystalline layer bonded to the bonding layer.
[0120]
[0140] The method 1300 further includes forming a conductive layer on the monocrystalline silicon layer at 1312 and forming a buffer layer on the conductive layer at 1314. In some embodiments, the buffer layer may be conductive and the conductive layer may be a properly doped epitaxial layer subset of a thicker buffer layer that includes multiple epitaxial layers. The method 1300 further includes forming one or more epitaxial III-V layers on the buffer layer according to requirements for multiple devices at 1316.
[0121]
[0141] According to some embodiments, the method 1300 further includes forming the plurality of devices at 1318 using the following steps: removing a portion of one or more epitaxial III-V layers and a portion of the buffer layer disposed between the plurality of devices to expose a portion of the conductive layer at 1320, forming a contact coupled to a portion of the exposed portion of the conductive layer at 1322, forming an anode contact on a remaining portion of the epitaxial P-type gallium nitride layer at 1324, and removing the remaining exposed portion of the conductive layer not coupled to the contact at 1326. The portions of the epitaxial III-V layers, the buffer layer, and the conductive layer can be removed using techniques such as etching and CMP. In some embodiments, the layers of the substrate described in FIG. 1 can be removed to a depth that reaches the polycrystalline ceramic core.
[0122]
[0142] In some embodiments, a portion of the substrate can be removed to form one or more backside contacts to one or more of the plurality of devices. The plurality of devices can be planarized by various methods, including using an epoxy or a photocurable polymer to fill the gaps. After forming the backside contacts and planarization, interconnects between the various types of devices can be fabricated. In various embodiments, the various device types can be monolithically integrated on the same engineered substrate using device interconnects. In some embodiments, street etching can be used to further isolate a first set of integrated devices from a second set of integrated devices. Following integration of the various device types, conductive pads can be formed on the integrated devices, and the integrated devices can be packaged for use as integrated circuits.
[0123]
[0143] It should be appreciated that the specific steps illustrated in FIG. 13 provide a particular method of fabricating multiple devices on an engineered substrate according to another embodiment of the present invention. Other sequences of steps may be performed according to alternative embodiments. For example, alternative embodiments of the present invention may perform the steps outlined above in a different order. Moreover, each step illustrated in FIG. 13 may include multiple sub-steps that may be performed in various orders as appropriate for the individual step. Furthermore, additional steps may be added or removed depending on the particular application. Those skilled in the art will recognize many variations, modifications, and alternatives.
[0124]
[0144] FIG. 14A is a simplified schematic cross-sectional view showing a substrate configured to fabricate a plurality of devices having various buffer layer epitaxial structures according to another embodiment of the present invention. FIG. 14A shows an engineered substrate 1402 having a mask 1404 configured to grow a first buffer layer 1406 and a first device structure 1408. FIG. 14B shows the engineered substrate 1402 after forming the first buffer layer 1406, the first device structure 1408, and a second mask 1420. The second mask 1420 formed on the engineered substrate 1402 covers the first buffer layer 1406 and the first device structure 1408. The second mask 1420 includes a window for growing a second buffer layer 1410 and a second device structure 1412. In some embodiments, the second buffer layer 1410 and the second device structure 1412 can include different epitaxial layers and different structures than the first buffer layer 1406 and the first device structure 1408. FIG. 14C shows the engineered substrate 1402 after forming the second buffer layer 1410, the second device structure 1412, and the third mask 1424. The third mask 1424 includes a larger window through which the third buffer layer 1414 and the third device structure 1416 are grown. In some embodiments, the window may be larger to facilitate forming electrical contact with the conductive layer at the base of the third buffer layer 1414. FIG. 14D shows the engineered substrate 1402 after forming the third buffer layer 1414 and the third device structure 1416. Any number of buffer layers and device types can be formed on the engineered substrate 1402 based on the requirements of a particular integrated circuit.
[0125]
[0145] Once the buffer layer and devices are formed, the devices can be planarized by various methods, such as using an epoxy or photocurable polymer to fill the gaps between the devices and performing CMP as necessary. After planarization, device interconnects can be fabricated and street etching can further isolate the integrated circuits on the engineered substrate 1402. After the device interconnects are fabricated, conductive pads can be formed and packaging can be completed. It should be appreciated that the specific steps illustrated in FIGS. 14A-14D provide a particular method of fabricating multiple islands on the same substrate with various epitaxial structures according to an embodiment of the present invention. Other sequences of steps may also be performed according to alternative embodiments. Moreover, the individual steps illustrated in FIGS. 14A-14D may include multiple sub-steps that may be performed in various orders appropriate to the individual steps. Furthermore, additional steps may be added or existing steps may be removed depending on the particular application. One skilled in the art would recognize many variations, modifications, and alternatives.
[0126]
[0146] 15 is a simplified flow chart illustrating a method 1500 of fabricating multiple devices having various buffer layer epitaxial structures on a single substrate according to another embodiment of the invention. The method 1500 includes forming a substrate at 1510 by providing a polycrystalline ceramic core, encapsulating the polycrystalline ceramic core with a first adhesive shell, encapsulating the first adhesive shell with a barrier layer, forming a bonding layer on the barrier layer, and forming a substantially single crystalline layer bonded to the bonding layer.
[0127]
[0147] The method 1500 further includes forming a first mask having a first exposed portion of the substantially monocrystalline layer at 1512, and forming a first buffer layer associated with the first device structure on the first exposed portion at 1514. The method 1500 further includes removing the first mask at 1516, forming a second mask having a second exposed portion of the substantially monocrystalline layer at 1518, and forming a second buffer layer associated with the second device structure on the second exposed portion at 1520. According to some embodiments, the first buffer layer can be an N-type gallium nitride layer having a first doping concentration. The second buffer layer can be a second epitaxial N-type gallium nitride layer having a second doping concentration different from the first doping concentration depending on the device requirements.
[0128]
[0148] According to some embodiments, the method 1500 further includes forming one or more epitaxial III-V layers on the first and second buffer layers at 1522, where the one or more epitaxial III-V layers are formed according to the requirements of the devices. The method further includes etching between the devices at 1524. Once the buffer layers and devices are formed, the devices can be planarized by various methods, such as using an epoxy or photocurable polymer to fill the gaps between the devices and performing CMP as needed. After planarization, device interconnects can be fabricated and street etching can further isolate the integrated circuits on the engineered substrate 1402. After the device interconnects are fabricated, conductive pads can be formed and packaging can be completed.
[0129]
[0149] It should be appreciated that the specific steps illustrated in FIG. 15 provide a particular method of fabricating a number of devices having various buffer layer epitaxial structures on an engineered substrate according to another embodiment of the present invention. Other sequences of steps may be performed according to alternative embodiments. For example, alternative embodiments of the present invention may perform the steps outlined above in a different order. Moreover, each step illustrated in FIG. 15 may include multiple sub-steps that may be performed in various orders appropriate to the individual step. Furthermore, additional steps may be added or removed depending on the particular application. Those skilled in the art will recognize many variations, modifications, and alternatives.
[0130]
[0150] Epitaxial growth and selective etching of the substrate can be used to form a particular integrated circuit and the devices it contains. In some embodiments, the device specialization scheme includes a pair of enhancement mode and depletion mode devices. If an epitaxial layer of a buffer layer is grown to fabricate an enhancement mode device, an additive or subtractive process can be used to form a depletion mode device using the same substrate and buffer layer. If an additive process is selected, a depletion mode device can be fabricated by depositing an epitaxial material, e.g., AlN, on the buffer layer using selective epitaxy. If a subtractive process is selected, a p-GaN etch can be used to form a depletion mode device.
[0131]
[0151] In other embodiments, an epitaxial layer of the buffer layer is grown to fabricate a depletion mode device. In these embodiments, the enhancement mode device can be fabricated using additive or subtractive processes. Enhancement mode devices can be fabricated by subtractive gate recess etching or additive atomic layer deposition (ALD) of p-GaN, e.g., p-GaN gates.
[0132]
[0152] In some embodiments, a variety of vertical devices can be fabricated using the engineered substrate. FIG. 16A shows three devices fabricated on engineered substrate 1602. A first surface 1650 of each of the multiple devices can be bonded to a front surface 1652 of a temporary carrier 1654. The first or front surface 1650 of each device faces the surface connected to the engineered substrate 1602. Once the devices are bonded to the temporary carrier 1654, the engineered substrate 1602 can be removed to expose a second surface 1656 on each device. FIG. 16B shows this particular embodiment. In some embodiments, after the engineered substrate 1602 is removed, further layers, such as a single crystal layer and further epitaxial layers, can be removed from the second surface 1656 depending on the device requirements. After the engineered substrate 1602 and any further layers are removed, a conductive layer 1658 can be formed on the exposed second surface 1656. In some embodiments, copper can be electroplated on the second surface 1656. The conductive layer 1658 can be bonded to a carrier wafer 1660 and the temporary carrier can be removed.
[0133]
[0153] FIG. 16C shows the device with the newly formed conductive layer 1658 bonded to a carrier wafer 1660. In some embodiments, after being bonded to the carrier wafer, the device can be isolated by etching into the carrier wafer. In some embodiments, backside contacts of one or more devices can be fabricated. In some embodiments, forming the plurality of devices on the substrate can further include planarizing the plurality of devices by various methods. Methods include, for example, depositing a dielectric material and performing chemical mechanical planarization. In various embodiments, the various device types can be monolithically integrated on the same processed substrate with device interconnects. In some embodiments, street etching can be used to further isolate a first set of integrated devices from a second set of integrated devices. Following integration of the various device types, conductive pads can be formed on the integrated devices, and the integrated devices can be packaged for use as integrated circuits.
[0134]
[0154] Several techniques can be used to remove the engineered substrate 1602 and further layers. For example, a chemical such as hydrofluoric acid (HF) can be implanted on the side of the wafer holding the vertical semiconductor diode to etch one or more of the buffer layer and semi-insulating layer, but leave the ceramic core and vertical semiconductor diode epitaxial stack intact. Etching one or more of the buffer layer and semi-insulating layer separates the vertical semiconductor diode epitaxial stack from the remainder of the engineered substrate while retaining the ceramic core for reuse. This chemical lift-off process also reduces the overall stress on the vertical semiconductor diode epitaxial stack by eliminating the polishing process. If a gallium nitride substrate was used, the substrate cannot be selectively removed. Furthermore, gallium nitride substrates contain defects such as face flipping, residual stress, brittleness, and miscut faces that affect the quality of the epitaxial layers grown thereon. In some embodiments using gallium nitride substrates, 75% of the resistance can be attributed to defects in the substrate. Embodiments of the present invention that remove the substrate to expose the epitaxial layers for contact formation can thereby reduce electrical and thermal resistance.
[0135]
[0155] In some embodiments, a sacrificial layer can be used for the chemical lift-off process. The sacrificial layer can be a metal such as titanium (Ti) that is highly likely to dissolve when exposed to HF. In some embodiments, the sacrificial layer can include one of titanium (Ti), vanadium (V), chromium (Cr), tantalum (Ta), tungsten (W), rhenium (Re), silicon oxide, silicon nitride, silicon oxynitride, or combinations thereof. In addition to the sacrificial layer, a protective layer can be used. The protective layer can prevent diffusion of material from the sacrificial layer 200, such as Ti, into the epitaxial GaN layer during epitaxial GaN growth. Further description related to the removal of the substrate, buffer layer, and semi-insulating layer is provided in U.S. Patent Application No. 15 / 288,506, the disclosure of which is incorporated herein by reference in its entirety for all purposes. The substrate removal process described in connection with the vertical semiconductor diode can be used with any of the devices described herein. One skilled in the art would recognize many variations, modifications, and alternatives.
[0136]
[0156] It should also be understood that the examples and embodiments described herein are for illustrative purposes only, and various modifications or changes may be suggested to one skilled in the art in light thereof, and should be included within the spirit and scope of this application and the scope of the appended claims.
Claims
1. A polycrystalline ceramic core; a first adhesive shell encapsulating the polycrystalline ceramic core; a barrier layer encapsulating the first adhesive shell; and a bonding layer coupled to the barrier layer; a single crystal layer bonded to the bonding layer; A substrate; a buffer layer bonded to the single crystal layer; one or more epitaxial layers coupled to the buffer layer, the one or more epitaxial layers defining a trench dividing the one or more epitaxial layers into a first section and a second section; a first semiconductor device formed in the first section of the one or more epitaxial layers; and a second semiconductor device formed in the second section of the one or more epitaxial layers; and Equipped with a portion of the buffer layer disposed between the first section and the second section is removed to expose a portion of the polycrystalline ceramic core of the substrate.
2. 2. The semiconductor device of claim 1, wherein the first semiconductor device comprises a depletion mode high electron mobility transistor (HEMT) and the second semiconductor device comprises an enhancement mode HEMT.
3. 2. The semiconductor device of claim 1, wherein the first semiconductor device comprises a first depletion mode high electron mobility transistor (HEMT) and the second semiconductor device comprises a second depletion mode HEMT.
4. 2. The semiconductor device of claim 1, wherein the first semiconductor device comprises a first enhancement mode high electron mobility transistor (HEMT) and the second semiconductor device comprises a second enhancement mode HEMT.
5. The semiconductor device of claim 1 , further comprising a conductive layer disposed between said single crystal layer and said buffer layer.
6. The semiconductor device of claim 5 , wherein the first semiconductor device comprises a high electron mobility transistor (HEMT) and the second semiconductor device comprises a vertical semiconductor device.
7. 7. The semiconductor device of claim 6, wherein the vertical semiconductor device comprises a vertical PN diode or a vertical Schottky diode.
8. The semiconductor device of claim 1 , wherein the polycrystalline ceramic core comprises aluminum nitride.
9. the first adhesion shell comprises a tetraethylorthosilicate (TEOS) oxide layer; the barrier layer comprises silicon nitride; the bonding layer comprises silicon oxide; The semiconductor device of claim 1 , wherein the single crystal layer comprises silicon.
10. The semiconductor device of claim 1 , wherein the one or more epitaxial layers comprise one or more epitaxial III-V layers.
11. 1. A method of forming a plurality of devices, comprising: providing a polycrystalline ceramic core; encapsulating the polycrystalline ceramic core with a first adhesive shell; encapsulating the first adhesive shell with a barrier layer; forming a bonding layer on the barrier layer; and forming a monocrystalline layer bonded to the bonding layer. forming a substrate by forming a first mask having a first exposed portion of the monocrystalline layer; forming a first buffer layer associated with a first device structure on the first exposed portion; removing the first mask; forming a second mask having a second exposed portion of the monocrystalline layer; forming a second buffer layer associated with a second device structure on the second exposed portion; forming one or more epitaxial layers on the first buffer layer and the second buffer layer, the one or more epitaxial layers being formed according to requirements associated with the plurality of devices; Etching between the devices. A method comprising:
12. The method of claim 11 , further comprising planarizing the plurality of devices on the substrate.
13. The planarizing step further comprises: forming a dielectric layer over the plurality of devices; planarizing the plurality of devices using chemical mechanical planarization; The method of claim 12 further comprising:
14. The method of claim 11 , further comprising fabricating one or more interconnects between a first device of the plurality of devices and a second device of the plurality of devices.
15. bonding a first surface of each of the plurality of devices to a temporary carrier, the first surface being opposite the substrate; removing the substrate to expose a second surface of each of the devices; forming a conductive layer on the second surface; bonding a carrier wafer to the conductive layer; The method of claim 11 further comprising:
16. The method of claim 15, further comprising forming one or more back surface contacts after the step of removing the substrate.
17. forming a conductive layer coupled to the single crystal layer and to at least one of the first buffer layer and the second buffer layer; exposing a portion of the conductive layer; forming a contact on the exposed portion of the conductive layer; The method of claim 11 further comprising:
18. The method of claim 11 , wherein etching between the devices further comprises etching into the polycrystalline ceramic core.
Citation Information
Patent Citations
Semiconductor device and its manufacture
JP2000208722A
Power semiconductor device comprising a mesa structure and a buffer layer including mesa steps.
JP2011503871A
Semiconductor device and method of manufacturing the semiconductor device
JP2012043965A
Epitaxial wafer for infrared LED, and infrared LED
JP2012146866A
Complementary gallium nitride integrated circuit and method of fabricating the same