Polyamide resin composition and polyamide molded article
A polyamide resin composition with specific dicarboxylic acid and diamine units, combined with flame retardants, addresses the issue of electrical resistance loss at high temperatures, maintaining mechanical and electrical integrity in electrical equipment.
Patent Information
- Application Number
- JP2023510975
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-30
- Filing Date
- 2022-03-18
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2042-03-18
AI Technical Summary
Polyamide resin compositions used in electrical equipment face a decrease in electrical resistance when a flame retardant is added, especially at high temperatures, which is problematic for miniaturized and high-output electrical equipment.
A polyamide resin composition is formulated with specific dicarboxylic acid and diamine units, including aromatic or alicyclic dicarboxylic acid and alkylene diamines, along with flame retardants like polybrominated styrene and phosphinate compounds, to maintain high electrical resistance and heat resistance in high temperature ranges.
The composition achieves high electrical resistance and heat resistance in a high temperature range, preventing a decrease in mechanical strength and ensuring the integrity of electrical equipment performance.
Smart Images

Figure 0007576159000013 
Figure 0007576159000001 
Figure 0007576159000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a polyamide resin composition and a polyamide molded article. [Background technology]
[0002] Polyamide resin compositions have been widely used as materials for various parts for clothing, industrial materials, automobiles, electrical and electronic products, industrial applications, etc. because of their excellent moldability, mechanical properties, and chemical resistance.
[0003] Various additives are added to the polyamide resin compositions used for these applications in order to develop properties suited to each application.
[0004] For example, Patent Document 1 describes a polyamide composition for sealing electric / electronic parts, which comprises 100 parts by weight of semi-aromatic polyamide (A) consisting of dicarboxylic acid units (a) containing 50 to 100 mol % of terephthalic acid units and diamine units (b) containing 50 to 100 mol % of aliphatic alkylenediamine units having 6 to 18 carbon atoms, 50 to 700 parts by weight of inorganic filler (B), and 10 to 200 parts by weight of flame retardant (C). Patent Document 1 describes that this polyamide resin composition has excellent heat resistance and mechanical properties.
[0005] Also, attempts have been made to change the physical properties of polyamide resins by changing the raw materials of the polyamide resins. For example, Patent Document 2 and Patent Document 3 describe polyamide resins using 1,3-bis(aminomethyl)cyclohexane as a diamine component used in the production of polyamides by polycondensing a diamine component and a dicarboxylic acid component. Patent Document 2 describes that the polyamide resin described in said document has high transparency, and Patent Document 3 describes that the polyamide resin described in said document has a high glass transition point and improved crystallization ability. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2003-176408 A [Patent Document 2] Japanese Patent Application Publication No. 49-55796 [Patent Document 3] JP 2017-75303 A Summary of the Invention [Problem to be solved by the invention]
[0007] As described in Patent Document 1, a polyamide resin composition to which a flame retardant is added in order to enhance heat resistance is known.
[0008] When polyamide resins are used as parts of electrical devices, they are required to have higher electrical resistance in order to accommodate the recent trend toward smaller electrical devices. In addition, they are required to have high electrical resistance in the high temperature range (around 130°C) in order to accommodate the high output of electrical devices. However, according to the findings of the present inventors, the addition of a flame retardant to a polyamide resin composition can result in a decrease in electrical resistance at high temperatures.
[0009] In view of these circumstances, an object of the present disclosure is to provide a polyamide resin composition that has high heat resistance while suppressing a decrease in electrical resistance in a high temperature range (around 130°C) or capable of further increasing electrical resistance, and a polyamide molded article containing the polyamide resin composition. [Means for solving the problem]
[0010] [1] A polyamide resin comprising a component unit (a) derived from a dicarboxylic acid and a component unit (b) derived from a diamine, The dicarboxylic acid-derived component unit (a) includes an aromatic dicarboxylic acid or an alicyclic dicarboxylic acid-derived component unit, The diamine-derived component unit (b) is a component unit (b1) derived from an alkylene diamine having 4 to 18 carbon atoms, the component unit (b1) being more than 50 mol % and not more than 90 mol % of the total number of moles of the component unit (b) derived from the diamine; A component unit (b2) derived from a diamine represented by the following formula (1) in an amount of 10 mol % or more and less than 50 mol % based on the total number of moles of the component unit (b) derived from the diamine: A polyamide resin in an amount of 20% by mass or more and 80% by mass or less based on the total mass of the polyamide resin composition, [ka] (In formula (1), n and two m's each independently represent 0 or 1; -X- is a single bond or a divalent group selected from the group consisting of -O-, -S-, -SO2-, -CO- and -CH2-. A flame retardant, The flame retardant is At least one flame retardant (X) selected from the group consisting of polybrominated styrene, brominated polystyrene, and brominated polyphenylene, in an amount of 1% by mass or more and 40% by mass or less based on the total mass of the polyamide resin composition; or a flame retardant (Y) containing a phosphinate compound represented by formula (I) or a bisphosphinate compound represented by formula (II), or a polymer thereof, in an amount of 3 mass% or more and 20 mass% or less relative to the total mass of the polyamide resin composition; [ka] [In the formula, R 1 and R 2 are independently a linear or branched alkyl or aryl group having from 1 to 6 carbon atoms, R 3 each independently represents a linear or branched alkylene group having from 1 to 10 carbon atoms, an arylene group having from 6 to 10 carbon atoms, an alkylarylene group having from 6 to 10 carbon atoms, or an arylalkylene group having from 6 to 10 carbon atoms, M is an atom or an atomic group selected from the group consisting of Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K, and protonated nitrogen bases; m represents an integer of 1 to 4, n represents an integer of 1 to 4, and x represents an integer of 1 to 4. [2] The polyamide resin composition according to [1], wherein the polyamide resin contains component units (b2) derived from the diamine represented by formula (1) in an amount of 15 mol % or more and less than 45 mol % based on the total number of moles of the component units (b) derived from the diamine. [3] The component unit (b1) derived from an alkylenediamine having 4 to 18 carbon atoms includes a component unit derived from a linear alkylenediamine or a branched alkylenediamine. The polyamide resin composition according to [1] or [2]. [4] The linear or branched alkylenediamine is a diamine selected from the group consisting of 1,4-diaminobutane, 1,6-diaminohexane, 1,9-nonanediamine, 1,10-decanediamine, 2-methyl-1,5-pentanediamine, and 2-methyl-1,8-octanediamine; The polyamide resin composition according to [3]. [5] The aromatic dicarboxylic acid or alicyclic dicarboxylic acid is terephthalic acid, naphthalenedicarboxylic acid or cyclohexanedicarboxylic acid; The polyamide resin composition according to any one of [1] to [4]. [6] The flame retardant is a flame retardant (Y) containing a phosphinate compound represented by formula (I) or a bisphosphinate compound represented by formula (II), or a polymer thereof; The polyamide resin composition according to any one of [1] to [5]. [7] The flame retardant is at least one flame retardant (X) selected from the group consisting of polybrominated styrene, brominated polystyrene, and brominated polyphenylene; The polyamide resin composition according to any one of [1] to [5]. [8] The polyamide resin composition according to [7], further comprising 0.01% by mass or more and 5% by mass or less of an antimony compound, based on the total mass of the polyamide resin composition. [9] The polyamide resin composition according to [8], further comprising 0.5 mass % or more and 10 mass % or less of a zinc salt or a calcium salt, based on the total mass of the polyamide resin composition.
[10] A resin composition for use as an insulating material, comprising the polyamide resin composition according to any one of [1] to [9].
[11] The polyamide resin composition according to any one of [1] to
[10] , Polyamide molding.
[12] A component of an electrical device.
[11] The polyamide molding according to claim 1. Effect of the Invention
[0011] According to the present disclosure, it is possible to provide a polyamide resin composition that has high heat resistance and can exhibit high electrical resistance in the high temperature range (around 130°C), and a polyamide molded article containing the polyamide resin composition. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a diagram showing the relationship between the temperature and time of the reflow process in the reflow heat resistance test carried out in the examples and comparative examples of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] In the present disclosure, a numerical range indicated using "~" means a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively.
[0014] In the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in the present disclosure. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.
[0015] 1. First embodiment A first embodiment of the present disclosure relates to a polyamide resin composition.
[0016] The polyamide resin composition is a resin composition in which the main component of the resin components is a polyamide resin. The main component means that the proportion of the polyamide resin in the resin components is 50% by mass or more. The proportion of the polyamide resin in the resin components is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more. The upper limit of the proportion of the polyamide resin in the resin components is not particularly limited, but can be 100% by mass or less, may be 90% by mass or less, or may be 80% by mass or less.
[0017] The proportion of the polyamide resin contained in the polyamide resin composition is preferably 20% by mass or more and 80% by mass based on the total mass of the polyamide resin composition.
[0018] 1-1.Polyamide resin The polyamide resin may be a polyamide resin containing a component unit (a) derived from a dicarboxylic acid and a component unit (b) derived from a diamine. In this case, in order to set the melting point (Tm) and glass transition temperature (Tg) of the polyamide resin within the above range, the component unit (a) derived from a dicarboxylic acid preferably contains a component unit derived from an aromatic dicarboxylic acid or an alicyclic dicarboxylic acid, and the component unit (b) derived from a diamine preferably contains a component unit (b1) derived from an alkylene diamine having 4 to 18 carbon atoms, which is more than 50 mol% and not more than 90 mol% of the total number of moles of the component unit (b) derived from the diamine, and a component unit (b2) derived from a diamine represented by formula (1), which is 10 mol% or more and less than 50 mol% of the total number of moles of the component unit (b) derived from the diamine.
[0019] [Component unit (a) derived from dicarboxylic acid] When the polyamide resin contains a component unit derived from an aromatic dicarboxylic acid or an alicyclic dicarboxylic acid as the component unit (a) derived from a dicarboxylic acid, the melting point (Tm) and crystallinity can be sufficiently increased.
[0020] Examples of aromatic dicarboxylic acids include terephthalic acid, naphthalenedicarboxylic acid, and their esters. Examples of alicyclic dicarboxylic acids include cyclohexanedicarboxylic acid and its esters. Among them, from the viewpoint of obtaining a polyamide resin having high crystallinity and high heat resistance, the component unit (a) derived from a dicarboxylic acid preferably includes a component unit derived from an aromatic dicarboxylic acid, and more preferably includes a component unit derived from terephthalic acid.
[0021] The content of the component unit derived from an aromatic dicarboxylic acid or an alicyclic dicarboxylic acid (preferably a component unit derived from an aromatic dicarboxylic acid, more preferably a component unit derived from terephthalic acid) is not particularly limited, but is preferably 50 mol% or more and 100 mol% or less based on the total number of moles of the component unit (a) derived from a dicarboxylic acid. If the content of the component unit is 50 mol% or more, the crystallinity of the polyamide resin is easily increased. From the same viewpoint, the content of the component unit is more preferably 70 mol% or more and 100 mol% or less.
[0022] In this embodiment, the component unit (a) derived from a dicarboxylic acid preferably includes a component unit (a1) derived from terephthalic acid, naphthalenedicarboxylic acid, or cyclohexanedicarboxylic acid. These component units (a1) can enhance the crystallinity of polyamide, unlike, for example, isophthalic acid. The content of these component units (a1) is set to more than 20 mol% and not more than 100 mol% based on the total number of moles of the component units (a) derived from dicarboxylic acid, from the viewpoint of ensuring the crystallinity of the polyamide resin. From the viewpoint of further enhancing the crystallinity of the polyamide resin, the content of these component units (a1) is preferably 45 mol% or more and 100 mol% or less based on the total number of moles of the component units (a) derived from dicarboxylic acid, more preferably 50 mol% or more and 99 mol% or less, even more preferably 80 mol% or more and 99 mol% or less, and particularly preferably 90 mol% or more and 99 mol% or less.
[0023] The dicarboxylic acid-derived component unit (a) may contain aromatic carboxylic acid component units (a2) other than the above component unit (a1) or aliphatic dicarboxylic acid component units (a3) having 4 to 20 carbon atoms, provided that the effects disclosed herein are not impaired. However, from the viewpoint of not impairing the crystallinity of the resin, the content of component units derived from isophthalic acid and component units derived from aliphatic dicarboxylic acids having 4 to 18 carbon atoms other than adipic acid is small, specifically, preferably 20 mol % or less, more preferably 10 mol % or less, based on the total number of moles of the dicarboxylic acid-derived component units (a).
[0024] Examples of aromatic dicarboxylic acid component units (a2) other than terephthalic acid include component units derived from isophthalic acid and 2-methylterephthalic acid. Among these, component units derived from isophthalic acid are preferred. From the viewpoint of ensuring the crystallinity of the polyamide resin, the content of these component units (a2) is preferably 1 mol% or more and 50 mol% or less, more preferably 1 mol% or more and 20 mol% or less, even more preferably 1 mol% or more and 10 mol% or less, and particularly preferably 1 mol% or more and 5 mol% or less, based on the total number of moles of component units (a) derived from dicarboxylic acid.
[0025] The component unit (a3) derived from an aliphatic dicarboxylic acid is a component unit derived from an aliphatic dicarboxylic acid having an alkylene group with 4 to 20 carbon atoms, and is preferably a constituent unit derived from an aliphatic dicarboxylic acid having an alkylene group with 6 to 12 carbon atoms. Examples of the aliphatic dicarboxylic acid include succinic acid, glutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, 2,2-dimethylglutaric acid, 3,3-diethylsuccinic acid, azelaic acid, sebacic acid, and suberic acid component units. Among these, adipic acid and sebacic acid are preferred. From the viewpoint of ensuring the crystallinity of the polyamide resin, the content of these component units (a3) is preferably 0 mol% to 40 mol%, more preferably 0 mol% to 20 mol%, even more preferably 1 mol% to 10 mol%, and particularly preferably 1 mol% to 5 mol% based on the total moles of the component units (a) derived from dicarboxylic acids.
[0026] The semi-aromatic polyamide resin (A) may further contain a small amount of a tribasic or higher polybasic carboxylic acid unit such as trimellitic acid or pyromellitic acid in addition to the above-mentioned component units (a1), (a2), and (a3). The content of such a polybasic carboxylic acid unit may be 0 mol% or more and 5 mol% or less based on the total number of moles of the component units (a) derived from dicarboxylic acids.
[0027] [Diamine-derived component unit (b)] When a polyamide resin contains, as the diamine-derived component unit (b), a component unit (b2) derived from an alkylenediamine having a specific cyclic structure (diamine represented by formula (1)) in addition to a component unit (b1) derived from an alkylenediamine having 4 to 18 carbon atoms, the glass transition temperature (Tg) can be sufficiently increased.
[0028] That is, the component unit (b2) derived from the diamine represented by formula (1) has a nonlinear structure, and therefore reduces the mobility of the molecular chain of the polyamide resin. Therefore, the component unit (b2) derived from the diamine represented by formula (1) can increase the glass transition temperature (Tg) of the polyamide resin having the component unit (b2) compared to the polyamide resin not having the component unit (b2). It is also believed that this allows the polyamide resin having the component unit (b2) to have high mechanical strength even at high temperatures and to maintain this high mechanical strength for a long period of time.
[0029] Furthermore, the component unit (b2) derived from the diamine represented by formula (1) can appropriately lower the melting point (Tm) of the polyamide resin having the component unit (b2) as compared with the polyamide resin not having the component unit (b2), thereby providing the polyamide resin having the component unit (b2) with high fluidity during injection molding and high moldability.
[0030] On the other hand, according to the findings of the present inventors, fully aromatic polymers such as polyethersulfone (PES), polyphenylene sulfide (PPS), and polyetheretherketone (PEEK) are prone to short circuiting (tracking) due to carbonization of aromatic rings, and tend to have low electrical resistance. In addition, if a resin composition containing these resins further contains a flame retardant, the aromatic rings are likely to be carbonized due to the movement of the resin molecules at the interface between the flame retardant and the resin and interacting with the flame retardant during heating, and tracking may cause a decrease in electrical resistance. When the addition of this flame retardant causes a decrease in electrical resistance at high temperatures, a similar tendency is observed in polyamide resins. In contrast, semi-aromatic polyamides and aliphatic polyamides, which have a smaller number of aromatic rings, are less prone to tracking and have high electrical resistance.
[0031] Therefore, in semi-aromatic polyamides or aliphatic polyamides having high electrical resistance, by reducing the molecular mobility in the high temperature range with the component unit (b2) derived from the diamine represented by formula (1), even if some aromatic rings are carbonized in the high temperature range, it is possible to make it difficult for the carbonized aromatic rings to move close to each other. This is believed to make it easier to ensure high electrical resistance of the polyamide resin in the high temperature range.
[0032] Furthermore, according to the present inventors' new findings, by incorporating the component unit (b2) derived from the diamine represented by formula (1) into a semi-aromatic polyamide or an aliphatic polyamide, it is possible to suppress the decrease in tensile strength of the polyamide resin composition at high temperatures when a flame retardant is added.
[0033] In addition, the polyamide resin has high fluidity and mechanical strength during injection molding because it has crystallinity due to the component unit (b1) derived from an alkylenediamine having from 4 to 18 carbon atoms. Furthermore, the polyamide resin has high mechanical strength and electrical resistance even at high temperatures because of its high glass transition temperature (Tg), and is considered to be able to easily maintain these high mechanical strength and electrical resistance.
[0034] The number of carbon atoms in the alkylenediamine having 4 to 18 carbon atoms, which is the raw material of the component unit (b1), is more preferably 4 to 10, from the viewpoint of preventing a decrease in the Tg of the resin.
[0035] The alkylenediamine having 4 to 18 carbon atoms may include a linear alkylenediamine or a branched alkylenediamine. From the viewpoint of enhancing the crystallinity of the resin, the alkylenediamine having 4 to 18 carbon atoms preferably includes a linear alkylenediamine. That is, the component unit derived from the alkylenediamine having 4 to 18 carbon atoms preferably includes a component unit derived from a linear alkylenediamine.
[0036] Examples of alkylenediamines having 4 to 18 carbon atoms include linear alkylenediamines including 1,4-diaminobutane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine, and branched alkylenediamines including 2-methyl-1,5-pentanediamine and 2-methyl-1,8-octanediamine. Among these, 1,4-diaminobutane, 1,6-diaminohexane, 1,9-nonanediamine, 1,10-decanediamine, 2-methyl-1,5-pentanediamine, and 2-methyl-1,8-octanediamine are preferred, and 1,6-diaminohexane and 1,10-decanediamine are preferred. These alkylenediamines may be one type or two or more types.
[0037] Regarding the component unit (b2) derived from an alkylenediamine having a specific cyclic structure: The alkylene diamine having a specific cyclic structure is a diamine represented by the following formula (1). [ka]
[0038] In formula (1), n and two m's are each independently 0 or 1, and -X- is a single bond or a divalent group selected from the group consisting of -O-, -S-, -SO2-, -CO- and -CH2-.
[0039] The diamine represented by formula (1) is preferably norbornanediamine (m=n=0) or bisaminomethylnorbornane (m=1, n=0), more preferably bisaminomethylnorbornane, and even more preferably 2,5-bisaminomethylnorbornane or 2,6-bisaminomethylnorbornane. The diamine represented by formula (1) may contain two or more kinds, for example, both 2,5-bisaminomethylnorbornane and 2,6-bisaminomethylnorbornane.
[0040] In particular, when one or both of the two m's are 1, the mechanical strength of the polyamide resin is increased and the high mechanical strength is likely to be maintained.
[0041] When the diamine represented by formula (1) has geometric isomers (such as trans and cis isomers), either isomer may be used, and the isomer ratio is not particularly limited.
[0042] The content of the component unit (b1) derived from an alkylene diamine having 4 to 18 carbon atoms is preferably more than 50 mol % and not more than 90 mol % based on the total number of moles of the component unit (b) derived from the diamine. When the content is more than 50 mol %, the crystallinity of the polyamide resin can be sufficiently increased, and the flowability and mechanical strength of the resin during injection molding can be further increased. When the content is not more than 90 mol %, the content of the component unit (b2) derived from the diamine represented by formula (1) can be increased. This increases the glass transition temperature (Tg) of the polyamide resin, thereby increasing the mechanical strength and electrical resistance in the high temperature range, and appropriately lowers the (Tm) of the polyamide resin, thereby improving the moldability.
[0043] On the other hand, the content of the component unit (b2) derived from the diamine represented by formula (1) is preferably 10 mol% or more and less than 50 mol% based on the total number of moles of the component unit (b) derived from the diamine. When the content is 10 mol% or less, the glass transition temperature (Tg) of the polyamide resin is increased, the mechanical strength and electrical resistance in the high temperature range are increased, and the (Tm) of the polyamide resin is appropriately decreased, thereby improving the moldability. When the content is less than 50 mol%, the content of the component unit (b1) derived from an alkylene diamine having 4 to 18 carbon atoms can be increased. This sufficiently increases the crystallinity of the polyamide resin, thereby further improving the flowability and mechanical strength during injection molding of the resin.
[0044] From the above viewpoints, the content of the component units (b1) derived from an alkylene diamine having from 4 to 18 carbon atoms is preferably more than 50 mol % and not more than 90 mol %, more preferably from 55 mol % to 85 mol %, and even more preferably from 60 mol % to 80 mol %, based on the total number of moles of the component units (b) derived from diamine.
[0045] From the above viewpoints, the content of the component unit (b2) derived from the diamine represented by formula (1) is preferably 10 mol % or more and less than 50 mol %, more preferably 15 mol % or more and less than 45 mol %, even more preferably 20 mol % or more and 40 mol % or less, and particularly preferably 25 mol % or more and 40 mol % or less, based on the total number of moles of the component unit (b) derived from the diamine.
[0046] The diamine-derived component unit (b) may further contain another diamine-derived component unit (b3) within the range not impairing the effects disclosed herein. Examples of the other diamine include aromatic diamines and alicyclic diamines. The content of the other diamine-derived component unit (b3) may be 50 mol % or less based on the total number of moles of the diamine-derived component unit (b).
[0047] In order to improve the thermal stability during compounding or molding and to further increase the mechanical strength, at least some of the molecular terminal groups of the polyamide resin may be blocked with a terminal blocking agent. When the molecular terminal is a carboxyl group, the terminal blocking agent is preferably a monoamine, and when the molecular terminal is an amino group, the terminal blocking agent is preferably a monocarboxylic acid.
[0048] Examples of monoamines include aliphatic monoamines including methylamine, ethylamine, propylamine, and butylamine, alicyclic monoamines including cyclohexylamine and dicyclohexylamine, and aromatic monoamines including aniline and toluidine. Examples of monocarboxylic acids include aliphatic monocarboxylic acids having 2 to 30 carbon atoms including acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecylic acid, myristic acid, palmitic acid, stearic acid, oleic acid, and linoleic acid, aromatic monocarboxylic acids including benzoic acid, toluic acid, naphthalenecarboxylic acid, methylnaphthalenecarboxylic acid, and phenylacetic acid, and alicyclic monocarboxylic acids including cyclohexanecarboxylic acid. The aromatic monocarboxylic acid and the alicyclic monocarboxylic acid may have a substituent on the ring structure portion.
[0049] [Physical Properties] The polyamide resin may have a melting point (Tm) measured by a differential scanning calorimeter (DSC) of 280° C. or more and 335° C. or less, and preferably has a glass transition temperature (Tg) measured by DSC of 135° C. or more and 180° C. or less. The melting point (Tm) and glass transition temperature (Tg) may be measured at a heating rate of 10° C. / min.
[0050] When the melting point (Tm) of the polyamide resin is 280°C or higher, the mechanical strength and heat resistance of the polyamide resin composition and the molded product in the high temperature range are not easily impaired. When the melting point (Tm) of the polyamide resin is 335°C or lower, the molding temperature does not need to be excessively high, so that the molding processability of the polyamide resin composition is likely to be good. When the molding temperature does not need to be excessively high, the flame retardant is not easily decomposed during molding, so that the amount of flame retardant added can be appropriately suppressed, and the decrease in mechanical strength due to the addition of the flame retardant can be suppressed. From the above viewpoint, the melting point (Tm) of the polyamide resin is more preferably 290°C or higher and 330°C or lower, and even more preferably 300°C or higher and 325°C or lower.
[0051] When the glass transition temperature (Tg) of the polyamide resin is 135°C or higher, the heat resistance of the polyamide resin composition and the molded article is not easily impaired, and at the same time, the mechanical strength and electrical resistance at high temperatures are increased, and further, the decrease in tensile strength at high temperatures caused by the addition of a flame retardant that is a phosphinate compound or a bisphosphinate compound can be more sufficiently suppressed. When the glass transition temperature (Tg) of the polyamide resin is 180°C or lower, the moldability of the polyamide resin composition is likely to be good. From the above viewpoint, the glass transition temperature (Tg) of the polyamide resin is more preferably 140°C or higher and 170°C or lower.
[0052] The heat of fusion (ΔH) of the crystalline polyamide resin is preferably 10 mJ / mg or more. When the heat of fusion (ΔH) of the crystalline polyamide resin is 10 mJ / mg or more, it has crystallinity, and therefore it is easy to improve the flowability and mechanical strength during injection molding. From the same viewpoint, the heat of fusion (ΔH) of the crystalline polyamide resin is more preferably 15 mJ / mg or more, and even more preferably 20 mJ / mg or more. The upper limit of the heat of fusion (ΔH) of the crystalline polyamide resin is not particularly limited, but it may be 90 mJ / mg from the viewpoint of not impairing the moldability.
[0053] The heat of fusion (ΔH), melting point (Tm) and glass transition temperature (Tg) of the polyamide resin can be measured using a differential scanning calorimeter (DSC220C, manufactured by Seiko Instruments Inc.).
[0054] Specifically, about 5 mg of polyamide resin is sealed in a measuring aluminum pan and heated from room temperature to 350°C at 10°C / min. In order to completely melt the resin, it is held at 360°C for 3 minutes and then cooled to 30°C at 10°C / min. After leaving it at 30°C for 5 minutes, it is heated a second time to 360°C at 10°C / min. The temperature (°C) of the endothermic peak in this second heating is the melting point (Tm) of the crystalline polyamide resin, and the transition point corresponding to the glass transition is the glass transition temperature (Tg). The heat of fusion (ΔH) is calculated from the area of the endothermic peak of crystallization during the first heating process in accordance with JIS K7122.
[0055] The melting point (Tm), glass transition temperature (Tg) and heat of fusion (ΔH) of the crystalline polyamide resin can be adjusted by the structure of the component unit (a) derived from dicarboxylic acid, the content of the component unit (b2) derived from the diamine represented by formula (1), the content ratio of the component unit (b1) derived from an alkylenediamine having 4 to 18 carbon atoms to the component unit (b2) derived from the diamine represented by formula (1), and the number of carbon atoms of the alkylenediamine having 4 to 18 carbon atoms.
[0056] Furthermore, when increasing the heat of fusion (ΔH) of the crystalline polyamide resin, it is preferable to reduce the content or ratio of the component unit (b2) (the ratio of the component unit (b2) to the total number of moles of the component unit (b) derived from the diamine). On the other hand, when increasing the glass transition temperature (Tg) and decreasing the melting point (Tm) of the crystalline polyamide resin, it is preferable to increase the content or ratio of the component unit (b2) (the ratio of the component unit (b2) to the total number of moles of the component unit (b) derived from the diamine), for example.
[0057] The intrinsic viscosity [η] of the crystalline polyamide resin measured in 96.5% sulfuric acid at a temperature of 25° C. is preferably 0.6 dl / g or more and 1.5 dl / g or less. When the intrinsic viscosity [η] of the crystalline polyamide resin is 0.6 dl / g or more, the mechanical strength (toughness, etc.) of the molded body is easily increased, and when it is 1.5 dl / g or less, the fluidity during molding of the resin composition is not easily impaired. From the same viewpoint, the intrinsic viscosity [η] of the crystalline polyamide resin is more preferably 0.8 dl / g or more and 1.2 dl / g or less. The intrinsic viscosity [η] can be adjusted by the amount of terminal blocking of the crystalline polyamide resin, etc.
[0058] The intrinsic viscosity of the crystalline polyamide resin can be measured in accordance with JIS K6810-1977. Specifically, 0.5 g of crystalline polyamide resin is dissolved in 50 ml of 96.5% sulfuric acid solution to prepare a sample solution. The number of seconds it takes for this sample solution to flow down is measured using an Ubbelohde viscometer under conditions of 25±0.05°C, and the obtained value can be applied to the following formula to calculate the viscosity. [η]=ηSP / [C(1+0.205ηSP)]
[0059] In the above formula, each algebra or variable represents the following: [η]: Intrinsic viscosity (dl / g) ηSP: Specific viscosity C: Sample concentration (g / dl)
[0060] ηSP is calculated by the following formula: ηSP=(t-t0) / t0 t: Time required for sample solution to flow (seconds) t0: Number of seconds that blank sulfuric acid flows (seconds)
[0061] [Manufacturing method] The polyamide resin can be produced, for example, by polycondensing the above-mentioned dicarboxylic acid and the above-mentioned diamine in a homogeneous solution. Specifically, the dicarboxylic acid and the diamine are heated in the presence of a catalyst as described in WO 03 / 085029 to obtain a low-order condensate, and then the melt of the low-order condensate is subjected to shear stress to polycondense the low-order condensate.
[0062] From the viewpoint of adjusting the intrinsic viscosity of the polyamide resin, the above-mentioned terminal blocking agent may be added to the reaction system. The intrinsic viscosity [η] (or molecular weight) of the polyamide resin can be adjusted by the amount of terminal blocking agent added.
[0063] The terminal blocking agent is added to the reaction system of the dicarboxylic acid and the diamine, and the amount added is preferably 0.07 mol or less, and more preferably 0.05 mol or less, per 1 mol of the total amount of the dicarboxylic acid.
[0064] 1-2.Flame retardants The polyamide resin composition preferably contains any one of the following flame retardants: The polyamide resin composition may contain both the flame retardant (X) and the flame retardant (Y). (X) Polybrominated styrene, brominated polystyrene, or brominated polyphenylene (Y) a phosphinate compound represented by formula (I) or a bisphosphinate compound represented by formula (II), or a polymer thereof
[0065] [ka]
[0066] In formula (I) and formula (II), R 1 and R 2 are independently a linear or branched alkyl or aryl group having from 1 to 6 carbon atoms, R 3each independently represents a linear or branched alkylene group having from 1 to 10 carbon atoms, an arylene group having from 6 to 10 carbon atoms, an alkylarylene group having from 6 to 10 carbon atoms, or an arylalkylene group having from 6 to 10 carbon atoms, M is an atom or an atomic group selected from the group consisting of Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K, and protonated nitrogen bases; m represents an integer of 1 to 4; n represents an integer of 1 to 4; and x represents an integer of 1 to 4.
[0067] These flame retardants are not as strongly basic as other flame retardants such as magnesium oxide and aluminum hydroxide, and therefore suppress the decomposition of the polyamide resin, making it easier to maintain the mechanical strength of the molded product.
[0068] 1-2-1.Flame retardants (X) The flame retardant (X) is polybrominated styrene, brominated polystyrene, or brominated polyphenylene.
[0069] The polybrominated styrene is a polymer containing a component unit derived from brominated styrene or brominated α-methylstyrene. Examples of the brominated styrene include dibromostyrene, tribromostyrene, and pentabromostyrene. Examples of the brominated α-methylstyrene include tribromoα-methylstyrene. The polybrominated styrene may be a copolymer of brominated styrene or brominated α-methylstyrene and a (meth)acrylic acid ester compound having an epoxy group. Furthermore, the polybrominated styrene may be a copolymer obtained by graft-copolymerizing the above-mentioned various polymers with an unsaturated carboxylic acid or its derivative.
[0070] In these polybrominated styrenes, bromine atoms exist in the (co)polymer by replacing hydrogen atoms bonded to carbon atoms forming an aromatic ring, and usually, hydrogen atoms forming an alkyl chain forming the main skeleton of the (co)polymer are not substantially replaced by bromine atoms.
[0071] The term "substantially not substituted with bromine atoms" means that the ratio of hydrogen atoms substituted with bromine atoms among hydrogen atoms bonded to carbon atoms constituting the alkyl chain constituting the main skeleton of the (co)polymer is 0.0% by mass or more and 0.5% by mass or less. In the polybrominated styrene, the ratio of hydrogen atoms substituted with bromine atoms is preferably 0.0% by mass or more and 0.2% by mass or less.
[0072] Brominated polystyrene is a (co)polymer obtained by brominating polystyrene or poly-α-methylstyrene. Like polybrominated styrene, brominated polystyrene contains bromine atoms replacing hydrogen atoms bonded to carbon atoms forming an aromatic ring, but also contains bromine atoms replacing hydrogen atoms forming an alkyl chain forming the main skeleton of the (co)polymer. Specifically, in brominated polystyrene, the ratio of hydrogen atoms replaced by bromine atoms among hydrogen atoms bonded to carbon atoms constituting the alkyl chain forming the main skeleton of the (co)polymer is more than 0.5 mass%.
[0073] Brominated polyphenylene is a (co)polymer obtained by brominating a polyphenylene ether resin. The brominated polyphenylene is preferably a compound represented by the following general formula (1).
[0074] [ka]
[0075] In general formula (1), X is Br, p is a number from 1 to 4, and q is a number of 1 or more. q is preferably 2 or more, and more preferably 5 or more. There is no particular limitation on the upper limit of q, but it is preferably 100 or less, more preferably 80 or less, even more preferably 60 or less, still more preferably 40 or less, still more preferably 20 or less, and particularly preferably 10 or less.
[0076] Examples of the brominated polyphenylene represented by the general formula (1) include polydibromo-p-phenylene oxide, polytribromo-p-phenylene oxide, polymonobromo-p-phenylene oxide, and polydibromo-o-phenylene oxide.
[0077] Among these flame retardants, polybrominated styrene and brominated polystyrene are preferred, and polybrominated styrene is more preferred, from the viewpoint of improving the electrical properties of the polyamide resin composition in the high temperature range. Note that polybrominated styrene is likely to increase the bending strength of the molded body, and brominated polystyrene is likely to increase the fluidity of the polyamide resin composition. Therefore, they may be used separately depending on the desired properties of the polyamide resin composition and the molded body.
[0078] The bromine atom content of these flame retardants is preferably 50% by mass or more and 80% by mass or less, and more preferably 60% by mass or more and 80% by mass or less.
[0079] Moreover, the weight average molecular weight (Mw) of these flame retardants is preferably from 1,000 to 400,000, more preferably from 2,000 to 100,000, and even more preferably from 2,000 to 60,000. The weight average molecular weight is a polystyrene-equivalent weight average molecular weight measured using GPC (gel permeation chromatography) with chloroform as the mobile phase, at a column temperature of 40° C., and using a differential refractometer detector.
[0080] The content of these flame retardants is preferably 1% by mass or more and 40% by mass or less with respect to the total mass of the polyamide resin composition. When the content of the flame retardants is 1% by mass or more, the flowability and electrical properties at high temperatures of the polyamide resin composition can be improved. When the content of the flame retardants is 40% by mass or less, the amount of polyamide resin in the resin composition can be increased, and various properties such as toughness of the polyamide resin composition can be improved. From the above viewpoint, the content of these flame retardants is more preferably 5% by mass or more and 30% by mass or less, and even more preferably 12% by mass or more and 25% by mass or less with respect to the total mass of the polyamide resin composition.
[0081] The content of these flame retardants is 10 parts by mass or more and 70 parts by mass or less relative to 100 parts by mass of the polyamide resin contained in the polyamide resin composition. When the content of the flame retardants is 10 parts by mass or more, the flowability and electrical properties at high temperatures of the polyamide resin composition can be improved. When the content of the flame retardants is 70 parts by mass or less, the amount of polyamide resin in the resin composition can be increased, and various properties such as toughness of the polyamide resin composition can be improved. From the above viewpoint, the content of these flame retardants is preferably 20 parts by mass or more and 60 parts by mass or less, more preferably 25 parts by mass or more and 55 parts by mass or less relative to 100 parts by mass of the polyamide resin contained in the polyamide resin composition.
[0082] 1-2-1-1.Flame retardant assistant The polyamide resin composition preferably contains an antimony compound in addition to the flame retardant (X), which acts as a flame retardant auxiliary to further enhance the effect of the flame retardant.
[0083] Examples of the antimony compound include antimony trioxide, antimony tetraoxide, antimony pentoxide, and sodium antimonate, etc. Among these, sodium antimonate is preferred.
[0084] The content of the antimony compound is preferably 0.01% by mass or more and 5% by mass or less with respect to the total mass of the polyamide resin composition. When the content of the flame retardant assistant is 0.01% by mass or more, the effect of improving the flowability and electrical properties at high temperatures due to the flame retardant is more effectively exhibited. When the content of the flame retardant assistant is 5% by mass or less, the amount of polyamide resin in the resin composition can be increased, and various properties such as toughness of the polyamide resin composition can be improved. From the above viewpoint, the content of the flame retardant assistant is more preferably 0.05% by mass or more and 3% by mass or less with respect to the total mass of the polyamide resin composition, further preferably 0.1% by mass or more and 1% by mass or less, and particularly preferably 0.15% by mass or more and 0.4% by mass or less.
[0085] The polyamide resin composition preferably further contains a zinc salt or a calcium salt in addition to the antimony compound, which, when used in combination with the antimony compound, can further efficiently enhance the action of the flame retardant.
[0086] Examples of the zinc salt include zinc borate, zinc stannate, and zinc phosphate. Examples of the calcium salt include calcium borate and calcium molybdate. Of these, zinc salts are preferred, and zinc borate is more preferred. Examples of the zinc borate include 2ZnO·3B2O3, 4ZnO·B2O3·H2O, and 2ZnO·3B2O3·3.5H2O. Of these, 2ZnO·3B2O3 and 4ZnO·B2O3·H2O are preferred, and anhydrous zinc borate (2ZnO·3B2O3) is more preferred.
[0087] The content of the zinc salt or calcium salt is preferably 0.5% by mass or more and 10% by mass or less with respect to the total mass of the polyamide resin composition. When the content of the zinc salt or calcium salt is 0.5% by mass or more, the effect of improving the flowability and electrical properties at high temperatures by the flame retardant described above is more effectively exhibited. When the content of the zinc salt or calcium salt is 10% by mass or less, the amount of polyamide resin in the resin composition can be increased, and various properties such as toughness of the polyamide resin composition can be improved. From the above viewpoint, the content of the zinc salt or calcium salt is more preferably 1% by mass or more and 5% by mass or less with respect to the total mass of the polyamide resin composition, and further preferably 1% by mass or more and 3% by mass or less.
[0088] The ratio of the content (α) of the antimony compound to the content (β) of the zinc salt or calcium salt is not particularly limited, and α / β can be selected within the range of 99 / 1 to 1 / 99. From the viewpoint of more suitably exerting the effect of the zinc salt or calcium salt, it is preferable that the content (β) of the zinc salt or calcium salt is greater than the content (α) of the antimony compound, and α / β is more preferably 30 / 70 to 1 / 99, and even more preferably 20 / 80 to 1 / 99.
[0089] 1-2-2. Flame retardant (Y) The flame retardant (Y) is a phosphinate compound represented by formula (I) or a bisphosphinate compound represented by formula (II), or a polymer thereof.
[0090] [ka]
[0091] In formula (I) and formula (II), R 1 and R 2 are independently a linear or branched alkyl or aryl group having from 1 to 6 carbon atoms, R 3each independently represents a linear or branched alkylene group having from 1 to 10 carbon atoms, an arylene group having from 6 to 10 carbon atoms, an alkylarylene group having from 6 to 10 carbon atoms, or an arylalkylene group having from 6 to 10 carbon atoms, M is an atom or an atomic group selected from the group consisting of Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K, and protonated nitrogen bases; m represents an integer of 1 to 4; n represents an integer of 1 to 4; and x represents an integer of 1 to 4.
[0092] Examples of the phosphinate compound represented by formula (I) and the bisphosphinate compound represented by formula (II) include calcium dimethylphosphinate, magnesium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, magnesium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, magnesium diethylphosphinate, aluminum diethylphosphinate, zinc diethylphosphinate, calcium methyl-n-propylphosphinate, magnesium methyl-n-propylphosphinate, aluminum methyl-n-propylphosphinate, zinc methyl-n-propylphosphinate, methane di(methyl)phosphinate, methane di(methylphosphinate) calcium, methane di(methylphosphinate) magnesium, methane di(methylphosphinate) aluminum, methane di(methylphosphinate) zinc, benzene-1,4-(dimethylphosphinate) calcium, benzene-1,4-(dimethylphosphinate) magnesium, benzene-1,4-(dimethylphosphinate) aluminum, benzene-1,4-(dimethylphosphinate) zinc, methylphenylphosphinate calcium, methylphenylphosphinate magnesium, methylphenylphosphinate aluminum, methylphenylphosphinate zinc, diphenylphosphinate calcium, diphenylphosphinate magnesium, diphenylphosphinate aluminum, and diphenylphosphinate zinc.
[0093] Among these, calcium dimethylphosphinate, aluminum dimethylphosphinate, zinc dimethylphosphinate, calcium ethylmethylphosphinate, aluminum ethylmethylphosphinate, zinc ethylmethylphosphinate, calcium diethylphosphinate, aluminum diethylphosphinate, and zinc diethylphosphinate are preferred; aluminum diethylphosphinate is more preferred.
[0094] Commercially available examples of the phosphinate compound represented by formula (I) and the bisphosphinate compound represented by formula (II) include EXOLIT OP1230 ("EXOLIT" is a registered trademark of the company), OP1311, OP1312, OP930, and OP935 manufactured by Clariant.
[0095] In addition, according to the findings of the present inventors, these flame retardants can improve the electrical properties of the polyamide resin composition at high temperatures. Although the reason for this is unclear, it is believed that the glass transition temperature is improved and the molecular mobility of the amorphous part at high temperatures is reduced. In addition, since the flame retardant (Y) has a high ability to suppress the decomposition of the polyamide resin, higher flame retardancy can be achieved even with the same content. Therefore, when the flame retardant (Y) is used, the effect of suppressing the decrease in mechanical strength caused by reducing the amount of the flame retardant added is remarkable.
[0096] The content of these flame retardants is preferably 3% by mass or more and 20% by mass or less with respect to the total mass of the polyamide resin composition. When the content of the flame retardants is 3% by mass or more, the flowability and electrical properties at high temperatures of the polyamide resin composition can be improved. When the content of the flame retardants is 20% by mass or less, the amount of polyamide resin in the resin composition can be increased, and various properties such as toughness of the polyamide resin composition can be improved, and the decrease in toughness due to the addition of the flame retardant can be easily suppressed. From the above viewpoint, the content of these flame retardants is more preferably 5% by mass or more and 18% by mass or less with respect to the total mass of the polyamide resin composition, and further preferably 10% by mass or more and 15% by mass or less.
[0097] The content of these flame retardants is 3 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of the polyamide resin contained in the polyamide resin composition. When the content of the flame retardant is 3 parts by mass or more, the flowability and electrical properties at high temperatures of the polyamide resin composition can be improved. When the content of the flame retardant is 50 parts by mass or less, the amount of polyamide resin in the resin composition can be increased, and various properties such as toughness of the polyamide resin composition can be improved, and the decrease in toughness due to the addition of the flame retardant can be easily suppressed. From the above viewpoint, the content of these flame retardants is preferably 5 parts by mass or more and 40 parts by mass or less, more preferably 10 parts by mass or more and 35 parts by mass or less with respect to 100 parts by mass of the polyamide resin contained in the polyamide resin composition.
[0098] 1-2-2-1.Flame retardant assistant The polyamide resin composition may contain a known flame retardant auxiliary in addition to the flame retardant described above. Examples of the flame retardant auxiliary include antimony compounds, zinc salts or calcium salts, calcium oxide, barium oxide, aluminum oxide, tin oxide, magnesium oxide, aluminum phosphate, boehmite, phosphazene compounds, and salts of one or more phosphorus compounds selected from phosphoric acid, pyrophosphoric acid, and polyphosphoric acid and one or more compounds selected from melamine, melam, and melem.
[0099] Examples of the antimony compound include antimony trioxide, antimony tetraoxide, antimony pentoxide, and sodium antimonate, etc. Among these, sodium antimonate is preferred.
[0100] The content of the antimony compound is preferably 0.01% by mass or more and 5% by mass or less with respect to the total mass of the polyamide resin composition. When the content of the flame retardant assistant is 0.01% by mass or more, the effect of improving the flowability and electrical properties in the high temperature range by the flame retardant is more effectively exhibited. When the content of the flame retardant assistant is 5% by mass or less, the amount of polyamide resin in the resin composition can be increased, and various properties such as toughness of the polyamide resin composition can be improved. From the above viewpoint, the content of the flame retardant assistant is more preferably 0.05% by mass or more and 3% by mass or less with respect to the total mass of the polyamide resin composition, further preferably 0.1% by mass or more and 1% by mass or less, and particularly preferably 0.15% by mass or more and 0.4% by mass or less.
[0101] Examples of the zinc salt include zinc borate, zinc stannate, and zinc phosphate. Examples of the calcium salt include calcium borate and calcium molybdate. Of these, zinc salts are preferred, and zinc borate is more preferred. Examples of the zinc borate include 2ZnO·3B2O3, 4ZnO·B2O3·H2O, and 2ZnO·3B2O3·3.5H2O. Of these, 2ZnO·3B2O3 and 4ZnO·B2O3·H2O are preferred, and anhydrous zinc borate (2ZnO·3B2O3) is more preferred.
[0102] The content of the zinc salt or calcium salt is preferably 0.5% by mass or more and 10% by mass or less with respect to the total mass of the polyamide resin composition. When the content of the zinc salt or calcium salt is 0.5% by mass or more, the effect of improving the flowability and electrical properties at high temperatures by the flame retardant described above is more effectively exhibited. When the content of the zinc salt or calcium salt is 10% by mass or less, the amount of polyamide resin in the resin composition can be increased, and various properties such as toughness of the polyamide resin composition can be improved. From the above viewpoint, the content of the zinc salt or calcium salt is more preferably 1% by mass or more and 5% by mass or less with respect to the total mass of the polyamide resin composition, and further preferably 1% by mass or more and 3% by mass or less.
[0103] 1-3.Other ingredients The polyamide resin composition may contain other known components. The content of the other components is preferably 0% by mass or more and 20% by mass or less, more preferably 0% by mass or more and 10% by mass or less, and even more preferably 0.5% by mass or more and 10% by mass or less, based on the total mass of the polyamide resin composition.
[0104] Examples of other components include reinforcing materials, crystal nucleating agents, flow improvers, corrosion resistance improvers, drip prevention agents, ion scavengers, elastomers (rubbers), antistatic agents, mold release agents, antioxidants (phenols, amines, sulfurs, phosphorus compounds, etc.), heat stabilizers (lactone compounds, vitamin E compounds, hydroquinones, copper halides, iodine compounds, etc.), light stabilizers (benzotriazoles, triazines, benzophenones, benzoates, hindered amines, oxanilides, etc.), other polymers (polyolefins, olefin copolymers such as ethylene-propylene copolymers, ethylene-1-butene copolymers, olefin copolymers such as propylene-1-butene copolymers, polystyrene, polyamides, polycarbonates, polyacetals, polysulfones, polyphenylene oxides, fluororesins, silicone resins, and LCPs). Among these, the resin composition of the present disclosure preferably further contains a reinforcing material from the viewpoint of increasing the mechanical strength of the molded body.
[0105] The reinforcing material can impart high mechanical strength to the resin composition. Examples of the reinforcing material include fibrous reinforcing materials such as glass fiber, wollastonite, potassium titanate whiskers, calcium carbonate whiskers, aluminum borate whiskers, magnesium sulfate whiskers, zinc oxide whiskers, milled fiber, and cut fiber, as well as granular reinforcing materials. Of these, one type may be used alone, or two or more types may be used in combination. Among these, wollastonite, glass fiber, and potassium titanate whiskers are preferred, and wollastonite or glass fiber is more preferred, because they are easy to increase the mechanical strength of the molded body.
[0106] The average fiber length of the fibrous reinforcing material may be, for example, from 1 μm to 20 mm, preferably from 5 μm to 10 mm, from the viewpoint of moldability of the resin composition and mechanical strength and heat resistance of the resulting molded product. The aspect ratio of the fibrous reinforcing material may be, for example, from 5 to 2000, preferably from 30 to 600.
[0107] The average fiber length and average fiber diameter of the fibrous reinforcing material can be measured by the following method. 1) The resin composition is dissolved in a hexafluoroisopropanol / chloroform solution (0.1 / 0.9% by volume), and then filtered to obtain a filtrate. 2) Disperse the filtrate obtained in 1) in water, and measure the fiber length (Li) and fiber diameter (di) of each of 300 randomly selected fibers using an optical microscope (magnification: 50x). The number of fibers with fiber length Li is designated as qi, and the weight average length (Lw) is calculated based on the following formula, which is the average fiber length of the fibrous reinforcing material. Weight average length (Lw) = (Σqi × Li 2 ) / (Σqi×Li) Similarly, the number of fibers having a fiber diameter Di is taken as ri, and the weight average diameter (Dw) is calculated based on the following formula, and this is taken as the average fiber diameter of the fibrous reinforcing material. Weight average diameter (Dw)=(Σri×Di 2 ) / (Σri×Di)
[0108] The content of the fibrous reinforcing material is not particularly limited, but can be, for example, from 15% by mass to 70% by mass with respect to the total mass of the polyamide resin composition.
[0109] The crystal nucleating agent can increase the crystallinity of the molded body. Examples of the crystal nucleating agent include metal salt-based compounds including sodium 2,2-methylenebis(4,6-di-t-butylphenyl)phosphate, aluminum tris(pt-butylbenzoate), and stearates, sorbitol-based compounds including bis(p-methylbenzylidene)sorbitol and bis(4-ethylbenzylidene)sorbitol, and inorganic substances including talc, calcium carbonate, and hydrotalcite. Among these, talc is preferred from the viewpoint of further increasing the crystallinity of the molded body. These crystal nucleating agents may be used alone or in combination of two or more.
[0110] The content of the crystal nucleating agent is preferably 0.1 parts by mass or more and 5 parts by mass or less, and more preferably 0.1 parts by mass or more and 3 parts by mass or less, based on the total mass of the polyamide resin composition. When the content of the crystal nucleating agent is within the above range, the crystallinity of the molded product is easily increased sufficiently, and sufficient mechanical strength is easily obtained.
[0111] The corrosion resistance improver may be a metal oxide or metal hydroxide. These compounds can suppress the corrosion wear of steel materials (such as screws, cylinders, dies, and nozzles used in molding machines) at high temperatures caused by the polyamide resin composition.
[0112] These metal oxides or hydroxides are preferably oxides or hydroxides of metals in Groups 1 to 12 of the Periodic Table, and more preferably oxides or hydroxides of metals in Groups 2 to 12 of the Periodic Table. In particular, the metal oxides are preferably oxides of metals in Groups 4 to 12 of the Periodic Table, and more preferably oxides of metals in Groups 7 to 12 of the Periodic Table.
[0113] In particular, these metal oxides or metal hydroxides are preferably oxides or hydroxides of iron, magnesium, or zinc, and more preferably oxides or hydroxides of magnesium or zinc. These metal oxides or metal hydroxides may also be composite oxides of metals such as zinc stannate and zinc hydroxystannate. Among these, magnesium hydroxide, magnesium oxide, and zinc oxide are preferred, and zinc oxide is more preferred. In particular, when a phosphinate compound represented by formula (I) or a bisphosphinate compound represented by formula (II), or a polymer thereof, is used as the flame retardant (Y), the use of zinc oxide in combination significantly inhibits corrosion and wear of the molding machine.
[0114] These metal oxides or metal hydroxides are preferably in the form of particles.
[0115] The content of the corrosion resistance improver is preferably 0.05 mass% or more and 2 mass% or less, more preferably 0.1 mass% or more and 1 mass% or less, and even more preferably 0.1 mass% or more and 0.5 mass% or less, relative to the total mass of the polyamide resin composition.
[0116] The flow improver enhances the injection flowability of the polyamide resin composition and improves the appearance of the resulting molded article. The flow improver can be a metal salt of a fatty acid, such as a metal salt of an oxycarboxylic acid or a metal salt of a higher fatty acid.
[0117] The oxycarboxylic acid constituting the oxycarboxylic acid metal salt may be an aliphatic oxycarboxylic acid or an aromatic oxycarboxylic acid. Examples of the aliphatic oxycarboxylic acid include aliphatic oxycarboxylic acids having 10 to 30 carbon atoms, such as α-hydroxymyristic acid, α-hydroxypalmitic acid, α-hydroxystearic acid, α-hydroxyeicosanoic acid, α-hydroxydocosanoic acid, α-hydroxytetraeicosanoic acid, α-hydroxyhexaeicosanoic acid, α-hydroxyoctaeicosanoic acid, α-hydroxytriacontanoic acid, β-hydroxymyristic acid, 10-hydroxydecanoic acid, 15-hydroxypentadecanoic acid, 16-hydroxyhexadecanoic acid, 12-hydroxystearic acid, and ricinoleic acid. Examples of the aromatic oxycarboxylic acid include salicylic acid, m-oxybenzoic acid, p-oxybenzoic acid, gallic acid, mandelic acid, and trovaic acid.
[0118] Examples of the metal constituting the metal oxycarboxylate include alkali metals such as lithium, and alkaline earth metals such as magnesium, calcium and barium.
[0119] Of these, the metal oxycarboxylate is preferably a metal salt of 12-hydroxystearic acid, and more preferably magnesium 12-hydroxystearate and calcium 12-hydroxystearate.
[0120] Examples of the higher fatty acid constituting the higher fatty acid metal salt include higher fatty acids having 15 to 30 carbon atoms, such as stearic acid, oleic acid, behenic acid, behenic acid, and montanic acid.
[0121] Examples of the metals constituting the above higher fatty acid metal salts include calcium, magnesium, barium, lithium, aluminum, zinc, sodium, and potassium.
[0122] Among these, the higher fatty acid metal salt is preferably calcium stearate, magnesium stearate, barium stearate, calcium behenate, sodium montanate, calcium montanate, etc. In particular, when the flame retardant (Y) is a phosphinate compound represented by formula (I) or a bisphosphinate compound represented by formula (II), or a polymer thereof, the use of barium stearate, preferably 12-hydroxy-barium stearate, in combination increases the injection flowability of the polyamide resin composition and significantly improves the appearance of the resulting molded article.
[0123] The content of the flowability improver is preferably 0.01% by mass or more and 1.3% by mass or less based on the total mass of the polyamide resin composition. When the content of the flowability improver is 0.01% by mass or more, the flowability during molding is likely to be increased, and the appearance of the obtained molded product is likely to be improved. When the content of the flowability improver is 1.3% by mass or less, gas due to decomposition of the flowability improver is unlikely to be generated during molding, and the appearance of the product is likely to be good.
[0124] The anti-drip agent prevents the resin from dripping when melted and liquefied by the heat of combustion. Examples of the anti-drip agent include fluororesins and modified polyolefins having carboxyl groups, acid anhydride groups, and amino groups in the molecule. Examples of the fluororesins include polytetrafluoroethylene (PTFE). Examples of the modified polyolefins include modified products such as aromatic vinyl compound-conjugated diene copolymers such as polyethylene and SEBS or hydrogenated products thereof, and polyolefin elastomers such as ethylene-propylene copolymers. Of these, modified polyolefins are preferred, and maleic acid modified SEBS is more preferred.
[0125] The content of the anti-drip agent is preferably 0.1 parts by mass or more and 5 parts by mass or less, more preferably 0.5 parts by mass or more and 5 parts by mass or less, based on the total mass of the polyamide resin composition. When the content of the anti-drip agent is within the above range, dripping of the resin during combustion can be sufficiently suppressed.
[0126] The ion scavenger traps hydrogen chloride (chlorine ions) and the like in the polyamide resin composition to suppress deterioration of the polyamide resin composition. Examples of the ion scavenger include hydrotalcite and zeolite. These ion scavenger are layered compounds, and probably have the effect of increasing the flame retardancy of the polyamide resin composition and the molded article by dehydrating interlayer water.
[0127] The content of the ion scavenger is preferably 0.01 parts by mass or more and 3 parts by mass or less, and more preferably 0.1 parts by mass or more and 1 part by mass or less, based on the total mass of the polyamide resin composition. When the content of the ion scavenger is within the above range, the stability and flame retardancy of the polyamide resin composition and the molded article can be more sufficiently improved.
[0128] 1-4. Manufacturing method The polyamide resin composition can be produced by a known resin kneading method, for example, by mixing the above-mentioned polyamide resin and, if necessary, other components with a Henschel mixer, V blender, ribbon blender, or tumbler blender, or by mixing and then melt-kneading the mixture with a single-screw extruder, a multi-screw extruder, a kneader, or a Banbury mixer, followed by granulation or pulverization.
[0129] 2. Second embodiment A second embodiment of the present disclosure relates to a polyamide resin composition having the following properties:
[0130] It should be noted that the polyamide resin composition according to the first embodiment described above can realize a polyamide resin composition having the following properties. However, the polyamide resin composition according to this embodiment is not limited to the polyamide resin composition according to the first embodiment, and the composition of the polyamide resin and the types and amounts of various additives are not limited to the polyamide resin composition according to the first embodiment as long as the following properties can be realized.
[0131] The polyamide resin has a melting point (Tm) of 280° C. or more and 330° C. or less, as measured by a differential scanning calorimeter (DSC), and a glass transition temperature (Tg) of 135° C. or more and 180° C. or less, as measured by DSC.
[0132] When the melting point (Tm) of the polyamide resin is 280° C. or higher, the mechanical strength and heat resistance of the polyamide resin composition and molded article in the high temperature range are not easily impaired, and when it is 330° C. or lower, the molding temperature does not need to be excessively high, so that the molding processability of the polyamide resin composition is likely to be good. From the above viewpoint, the melting point (Tm) of the polyamide resin is more preferably 290° C. or higher and 330° C. or lower, and further preferably 300° C. or higher and 330° C. or lower.
[0133] When the glass transition temperature (Tg) of the polyamide resin is 135°C or higher, the heat resistance of the polyamide resin composition and the molded article is not easily impaired, and at the same time, the mechanical strength and electrical resistance at high temperatures can be increased. When the glass transition temperature (Tg) of the polyamide resin is 180°C or lower, the moldability of the polyamide resin composition is likely to be good. From the above viewpoint, the glass transition temperature (Tg) of the polyamide resin is more preferably 140°C or higher and 170°C or lower.
[0134] The polyamide resin composition was injected into a barflow mold having a width of 10 mm and a thickness of 0.5 mm at an injection pressure of 2000 kg / cm 2 When the resin composition is injected with the cylinder temperature set to 10°C higher than the melting point of the polyamide resin and the mold temperature set to 120°C, the flow length of the resin composition in the mold (hereinafter simply referred to as "flow length") is 20 mm or more and 100 mm or less.
[0135] When the flow length is 20 mm or more, the moldability of the polyamide resin composition can be further improved. When the flow length is 100 mm or less, the generation of burrs at the edge of the molded article due to overfilling can be suppressed, and the appearance of the molded article can be improved. From the above viewpoint, the flow length is preferably 20 mm or more and 100 mm or less, more preferably 25 mm or more and 80 mm or less, and even more preferably 30 mm or more and 70 mm or less.
[0136] The polyamide resin composition was injected at a pressure of 2000 kg / cm 2 Test piece A, which is 64 mm long, 6 mm wide and 0.8 mm thick, was obtained by injection molding with a cylinder temperature 10°C higher than the melting point of the polyamide resin and a mold temperature of 120°C, and satisfies the following requirements I and II. Requirement I: The temperature at which the test piece does not melt or blister on the surface when heated with a reflow soldering device (hereinafter simply referred to as the "reflow heat resistance temperature") is 240°C or higher and 290°C or lower. Requirement II: When a bending test is performed at a bending speed of 5 mm / min in an atmosphere of 23°C and 50% relative humidity, the energy required to break the test piece (hereinafter also referred to simply as "thin-wall bending energy") is 30 mJ or more and 90 mJ or less.
[0137] When the reflow heat resistance temperature is 240° C. or more, sufficient resistance to lead-free reflow soldering is obtained. When the reflow heat resistance temperature is 290° C. or less, there is no need to excessively increase the melting point of the polyamide resin or to reduce the fluidity of the polyamide resin composition, so that the moldability of the polyamide resin composition is good. From the above viewpoint, the reflow heat resistance temperature is preferably 240° C. or more and 280° C. or less, and more preferably 250° C. or more and 275° C. or less.
[0138] When the thin-wall bending energy is 30 mJ or more, the strength of the molded body obtained from the polyamide resin composition is sufficiently high, so that the molded body can have sufficient stress resistance even when it is used as a part of an electronic device to which vibration is applied, or a part of various devices such as an automobile to which stress is applied. In particular, the strength of the molded body is sufficiently increased even when it is made into a thin-walled molded body, so that sufficient stress resistance can be obtained even when it is molded into a fine part for the purpose of responding to the miniaturization of electronic devices. When the thin-wall bending energy is 90 mJ or more, the stress relaxation property of the molded body is sufficient, and when it is subjected to an impact, it is difficult to transmit the impact to other parts, and it is difficult to cause the destruction of the other parts. From the above viewpoint, the thin-wall bending energy is preferably 30 mJ or more and 80 mJ or less, more preferably 33 mJ or more and 75 mJ or less, and even more preferably 35 mJ or more and 70 mJ or less.
[0139] The polyamide resin composition was injection molded at an injection pressure of 100 MPa, a cylinder temperature 10°C higher than the melting point of the polyamide resin, and a mold temperature of 120°C. The volume resistivity of a square plate test piece B having a size of 100 mm square and a thickness of 2 mm at 130°C (hereinafter, also referred to simply as "high temperature resistivity") was 10 13 Ω cm or more 10 18 Ω·cm or less.
[0140] The high temperature resistivity above is 10 13 If the resistivity is Ω·cm or more, the insulating properties of the molded product can be further improved. In particular, sufficient insulating properties can be obtained even when molded into fine parts for the purpose of responding to miniaturization of electronic devices, and insulating properties sufficient to respond to the increase in the output of electronic devices can be obtained. 18 If the resistivity is Ω·cm or less, static electricity is less likely to accumulate in the molded body, so that dust adhesion can be prevented, and deterioration of the long-term reliability of electronic devices caused by dust getting inside the electronic devices can be suppressed. 14 Ω cm or more 10 18 It is preferable that the resistance is less than 10 Ω·cm. 13 Ω cm or more 10 17It is more preferable that the resistance is 10 Ω·cm or less. 13 Ω cm or more 10 16 More preferably, it is 10 Ω·cm or less. 14 Ω cm or more 10 16 It is particularly preferable that the resistivity is Ω·cm or less.
[0141] 3. Uses of resin composition The resin composition of the present disclosure can be molded into various molded articles by known molding methods such as compression molding, injection molding, and extrusion molding.
[0142] The molded article of the resin composition of the present disclosure can be used for various applications. Examples of such applications include automotive exterior parts such as radiator grilles, rear spoilers, wheel covers, wheel caps, cowl vent grilles, air outlet louvers, air scoops, hood bulges, sunroofs, sunroof rails, fenders and back doors, cylinder head covers, engine mounts, air intake manifolds, throttle bodies, air intake pipes, radiator tanks, radiator supports, water pumps, water pump inlets, water pump outlets, thermostat housings, cooling fans, fan shrouds, oil pans, oil filter housings, oil filler caps, oil level gauges, oil pumps, timing belts, timing belt covers and engine covers, automotive engine room parts such as fuel caps, fuel filler tubes, automotive fuel tanks, fuel sender modules, fuel cut-off valves, quick connectors, canisters, fuel delivery pipes and fuel automotive fuel system parts such as fuel filler necks, automotive drive system parts such as shift lever housings and propeller shafts, automotive chassis parts such as stabilizer bars, linkage rods, engine mount brackets, automotive functional parts such as window regulators, door locks, door handles, outside door mirror stays, wipers and their parts, accelerator pedals, pedal modules, joints, plastic screws, nuts, bushings, seal rings, bearings, bearing retainers, gears and actuators, automotive electronics parts such as wire harnesses and connectors, relay blocks, sensor housings, fuse parts, encapsulations, ignition coils and distributor caps, general-purpose equipment fuel system parts such as fuel tanks for general-purpose equipment (brush cutters, lawn mowers and chainsaws), electrical and electronic parts such as connectors, bus bars and LED reflectors, building material parts, industrial equipment parts, as well as various housings or exterior parts such as small housings (including housings for personal computers and mobile phones) and exterior molded products.
[0143] In particular, since the resin composition of the present disclosure has high mechanical strength and electrical resistance at high temperatures, it can be suitably used as an insulating material in various applications, and can also be suitably used for parts of electrical equipment such as automotive electronics parts, electric and electronic parts, industrial equipment parts, and housings or exterior parts of electrical equipment. EXAMPLES
[0144] The present invention will be described in more detail below with reference to examples, which should not be construed as limiting the scope of the present disclosure.
[0145] In the following experiments, the melting point (Tm) and glass transition temperature (Tg) of the polyamide resin were measured by the following methods.
[0146] (Melting point (Tm), glass transition temperature (Tg)) The heat of fusion (ΔH), melting point (Tm) and glass transition temperature (Tg) of the polyamide resin were measured using a differential scanning calorimeter (DSC220C, manufactured by Seiko Instruments Inc.).
[0147] Specifically, about 5 mg of polyamide resin was sealed in a measuring aluminum pan and heated from room temperature to 350°C at 10°C / min. In order to completely melt the resin, it was held at 360°C for 3 minutes and then cooled to 30°C at 10°C / min. After leaving it at 30°C for 5 minutes, it was heated a second time to 360°C at 10°C / min. The temperature (°C) of the endothermic peak in this second heating was taken as the melting point (Tm) of the crystalline polyamide resin, and the transition point corresponding to the glass transition was taken as the glass transition temperature (Tg). The heat of fusion (ΔH) was calculated from the area of the endothermic peak of crystallization during the first heating process in accordance with JIS K7122.
[0148] (Intrinsic viscosity [η]) The intrinsic viscosity [η] of the polyamide resin was determined by dissolving 0.5 g of the polyamide resin in 50 ml of a 96.5% sulfuric acid solution, measuring the flow time of the resulting solution at 25°C ± 0.05°C using an Ubbelohde viscometer, and calculating the intrinsic viscosity [η] = ηSP / (C(1 + 0.205ηSP)) based on the formula. [η]: Intrinsic viscosity (dl / g) ηSP: Specific viscosity C: Sample concentration (g / dl) t: Time required for sample solution to flow (seconds) t0: Number of seconds that blank sulfuric acid flows (seconds) ηSP=(t-t0) / t0
[0149] (Heat of fusion (ΔH)) The heat of fusion (ΔH) of the polyamide resin was calculated from the area of the exothermic peak of crystallization during the first heating process in accordance with JIS K 7122 (2012).
[0150] 1. Synthesis / preparation of materials 1-1. Synthesis of polyamide resin (Synthesis Example 1) 259.5g (1561.7mmol) of terephthalic acid, 118.9g (1023.1mmol) of 1,6-diaminohexane, 85.0g (551.1mmol) of bisaminomethylnorbornane (manufactured by Mitsui Chemicals Fine Co., Ltd.), 0.37g of sodium hypophosphite monohydrate and 81.8g of distilled water were placed in an autoclave with a capacity of 1L and substituted with nitrogen. Stirring was started at 190°C, and the internal temperature was raised to 250°C over 3 hours. At this time, the internal pressure of the autoclave was raised to 3.0MPa. After the reaction was continued for 1 hour, the mixture was released into the atmosphere from a spray nozzle installed at the bottom of the autoclave, and the low-order condensation product was extracted. After that, the low-order condensation product was cooled to room temperature, pulverized to a particle size of 1.5mm or less with a pulverizer, and dried at 110°C for 24 hours.
[0151] Next, this low-order condensate was placed in a tray-type solid-phase polymerization apparatus, and after replacing with nitrogen, the temperature was raised to 215° C. over about 1 hour and 30 minutes, after which the reaction was continued for 1 hour and 30 minutes, and the temperature was lowered to room temperature.
[0152] The obtained prepolymer was then melt-polymerized in a twin-screw extruder with a screw diameter of 30 mm and L / D=36 at a barrel set temperature of 330° C., a screw rotation speed of 200 rpm, and a resin supply rate of 6 kg / h to obtain Polyamide Resin 1.
[0153] The resulting polyamide resin 1 had an intrinsic viscosity [η] of 0.97 dl / g, a melting point (Tm) of 312° C., a glass transition temperature (Tg) of 167° C., and a heat of fusion (ΔH) of 44 mJ / mg.
[0154] (Synthesis Example 2) The amount of terephthalic acid added to the autoclave was 162.2 g (976.1 mmol), 85.6 g (585.7 mmol) of adipic acid was added, the amount of 1,6-diaminohexane was 182.9 g (1574.2 mmol), and bisaminomethylnorbornane (manufactured by Mitsui Fine Chemicals, Inc.) was not added, and the procedure was the same as in Synthesis Example 1 to obtain polyamide resin 2. The intrinsic viscosity [η] of polyamide resin 2 was 0.8 dl / g, the melting point (Tm) was 320° C., the glass transition temperature (Tg) was 95° C., and the heat of fusion (ΔH) was 48 mJ / mg.
[0155] 1-2.Flame retardants The following flame retardants were used: Flame Retardant (X) Polybrominated styrene (Chemtura, Great Lakes PBS-64HW: homopolymer of dibromostyrene, bromine content 64% by mass) Brominated polystyrene (manufactured by Albemarle Corporation, SAYTEX HP-7010 ("SAYTEX" is a registered trademark of the company): brominated polystyrene, bromine content 68.5% by mass Flame retardant (Y) Aluminum phosphinate (Clariant, EXOLIT OP1230), aluminum salt of diethylphosphinic acid, CAS No. 225789-38-8
[0156] 1-3.Flame retardant synergists Antimony compounds (Nihon Seiko Co., Ltd., SA-A: sodium antimonate) Boric acid salts (Borax, Firebrake 500: 2ZnO 3B2O3)
[0157] 1-4. Reinforcement material Glass fiber (Central Glass Co., Ltd., ECS03-615)
[0158] 1-5. Ion trapping agents Hydrotalcite 1 (manufactured by Kyowa Chemical Industry Co., Ltd., DHT-4C ("DHT" is a registered trademark of the company)) Hydrotalcite 2 (Toda Kogyo Co., Ltd., NAOX-33)
[0159] 1-6. Nucleating agents ·talc
[0160] 1-7. Anti-drip agent Maleated SEBS (Tuftec M1913, manufactured by Asahi Kasei Corporation ("Tuftec" is a registered trademark of the company))
[0161] 1-8.Corrosion resistance improver Zinc oxide
[0162] 1-9. Fluidity improver Calcium montanate (manufactured by Clariant, LICOMONT CAV102 "LICOMONT" is a registered trademark of the company) 12-hydroxybarium stearate (BS-6, manufactured by Nitto Kasei Kogyo Co., Ltd.)
[0163] 2. Preparation of polyamide resin composition The above materials were mixed in a tumbler blender in the composition ratio (unit: parts by mass) shown in Table 1, and melt-kneaded using a 30 mmφ vented twin-screw extruder at a cylinder temperature of 300 to 335°C. The kneaded product was then extruded in the form of strands and cooled in a water tank. The strands were then taken up and cut by a pelletizer to obtain a pelletized polyamide resin composition.
[0164] 3. Evaluation The obtained polyamide resin compositions were evaluated according to the following criteria.
[0165] 3-1.Flow length Each polyamide resin composition was injected into a barflow mold having a width of 10 mm and a thickness of 0.5 mm under the following conditions, and the flow length (mm) of the polyamide resin composition in the mold was measured. Note that a longer flow length indicates better injection flowability. Molding machine: Toshiba Machine Co., Ltd., EC75N-2A Injection pressure setting: 2000kg / cm 2 Molding machine cylinder temperature: Polyamide resin melting point + 10℃ Mold temperature: 120℃
[0166] 3-2.Flame retardancy Each polyamide resin composition was injection molded under the following conditions to prepare test pieces of 1 / 32 inch x 1 / 2 x 5 inch. Using the prepared test pieces, a vertical flame test was carried out in accordance with the UL94 standard (UL Test No. UL94 dated June 18, 1991) to evaluate the flame retardancy. Molding machine: Sodick Plastic Co., Ltd., Tupearl TR40S3A Injection pressure setting: 2000kg / cm 2 Molding machine cylinder temperature: Polyamide resin melting point + 10℃ Mold temperature: 120℃
[0167] 3-3. Reflow heat resistance temperature Each polyamide resin composition was injection molded under the following conditions to prepare a test piece A having a length of 64 mm, a width of 6 mm and a thickness of 0.8 mm. The prepared test piece A was conditioned at a temperature of 40° C. and a relative humidity of 95% for 96 hours. Molding machine: Toshiba Machine Co., Ltd., EC75N-2A Injection pressure setting: 2000kg / cm 2 Molding machine cylinder temperature: Polyamide resin melting point + 10℃ Mold temperature: 120℃
[0168] The test piece A subjected to the above humidity conditioning treatment was placed on a glass epoxy board with a thickness of 1 mm. A temperature sensor was installed on this board. The glass epoxy board on which the test piece A was placed was set in an air reflow soldering device (AIS-20-82-C, manufactured by Atec Techtron Co., Ltd.), and a reflow process was performed with the temperature profile shown in FIG. 1. As shown in FIG. 1, the temperature was raised to 230°C at a predetermined speed, and then heated to a predetermined set temperature (a is 270°C, b is 265°C, c is 260°C, d is 255°C, and e is 235°C) in 20 seconds, and then cooled to 230°C. At this time, the maximum set temperature at which the test piece A did not melt and blisters did not occur on the surface was obtained, and this maximum set temperature was taken as the reflow heat resistance temperature.
[0169] 3-4. Thin-wall bending energy Each of the obtained polyamide resin compositions was injection molded under the following conditions to prepare a test piece A having a length of 64 mm, a width of 6 mm and a thickness of 0.8 mm. Molding machine: Toshiba Machine Co., Ltd., EC75N-2A Injection pressure setting: 2000kg / cm 2 Molding machine cylinder temperature: Polyamide resin melting point + 10℃ Mold temperature: 120℃
[0170] The prepared test piece A was left for 24 hours in a nitrogen atmosphere at 23°C. Then, a bending test was performed in an atmosphere of 23°C and 50% relative humidity using a bending tester (NTESCO AB5), with a span of 26 mm and a bending speed of 5 mm / min. The energy required to break the test piece A (toughness) was calculated from the bending strength, strain and elastic modulus.
[0171] 3-5. High temperature resistivity Using the injection molding machine described below, square plate test pieces B of 100 mm square and 2 mm thick were molded under the molding conditions described below. Molding machine: Toshiba Machine Co., Ltd., EC75N-2A Injection pressure setting: 2000kg / cm 2 Molding machine cylinder temperature: Polyamide resin melting point + 10℃ Mold temperature: 120℃
[0172] This square plate-shaped test piece B was left for 24 hours in an atmosphere with a temperature of 23°C and a relative humidity of 50%. Thereafter, in accordance with ASTM D257:2007, the volume resistivity of the test piece B was measured at a chamber temperature of 130°C using a model 8340A manufactured by ADC Corporation, and was taken as high-temperature resistivity X1. For each resin composition, a resin composition having the same composition except that it did not contain a flame retardant or a flame retardant assistant was prepared, and the volume resistivity of the test piece B was measured in the same manner and was taken as high-temperature resistivity X2.
[0173] In addition, in order to confirm the extent to which the volume resistivity at high temperatures changed due to the addition of the flame retardant and the flame retardant assistant, the ratio (X1 / X2) and the difference (Δ(X2-X1) or Δ(X1-X2)) between the high temperature resistivity X1 and the high temperature resistivity X2 were calculated.
[0174] 3-6.High temperature tensile strength Each of the obtained polyamide resin compositions was injection molded under the following conditions to obtain (A) STM dumbbell-shaped test specimen Type I having a thickness of 3.2 mm.
[0175] Molding machine: Sumitomo Heavy Industries, SG50M3 Injection pressure setting: 2000kg / cm 2 Molding machine cylinder temperature: Polyamide resin melting point + 10℃ Mold temperature: 120℃ Injection setting speed: 60mm / sec The obtained test pieces were left at 23°C in a nitrogen atmosphere for 24 hours. Then, a tensile test was performed in an atmosphere of 130°C and 50% relative humidity, with the conditions other than temperature being in accordance with ASTM D638, and the obtained tensile strength was designated as high-temperature tensile strength Y1. For each resin composition, a resin composition of the same composition except that it did not contain a flame retardant or flame retardant assistant was prepared, and the tensile strength of a dumbbell-shaped test piece was measured in the same manner, and designated as high-temperature tensile strength Y2.
[0176] In addition, in order to confirm the extent to which the tensile strength at high temperatures changed due to the addition of the flame retardant and the flame retardant assistant, the ratio (Y1 / Y2) of the high temperature tensile strength Y1 to the high temperature tensile strength Y2 was calculated.
[0177] Tables 1 to 4 show the composition, flow length, flame retardancy, reflow heat resistance temperature, thin-wall bending energy, high-temperature resistivity, and high-temperature tensile strength of the prepared polyamide resin compositions.
[0178] [Table 1]
[0179] [Table 2]
[0180] [Table 3]
[0181] [Table 4]
[0182] As is clear from Tables 1 to 4, when a flame retardant (X) or flame retardant (Y) is used in combination with a polyamide resin having a diamine-derived component unit (b2) represented by formula (1) as the diamine-derived component unit (b), the decrease in electrical resistivity at high temperatures can be suppressed or the electrical resistivity at high temperatures can be further increased. In addition, when a flame retardant (X) or flame retardant (Y) is used in combination with a polyamide resin having a diamine-derived component unit (b2) represented by formula (1) as the diamine-derived component unit (b), the decrease in high-temperature tensile strength can be suppressed.
[0183] This application claims priority to Japanese Application No. 2021-057551 filed on March 30, 2021, and Japanese Application No. 2021-057558 filed on March 30, 2021, and the contents of the claims and specifications of such applications are incorporated by reference into this application. [Industrial Applicability]
[0184] The polyamide resin composition of the present disclosure has high electrical resistance at high temperatures, and is therefore expected to broaden the applicability of polyamide resins to parts of electrical devices that are expected to have high output or that require miniaturization, thereby contributing to the further popularization of polyamide resins.
Claims
1. A polyamide resin comprising a component unit (a) derived from a dicarboxylic acid and a component unit (b) derived from a diamine, The dicarboxylic acid-derived component unit (a) includes an aromatic dicarboxylic acid or an alicyclic dicarboxylic acid-derived component unit, The diamine-derived component unit (b) is a component unit (b1) derived from an alkylene diamine having from 4 to 18 carbon atoms, the component unit (b1) being from more than 50 mol % to 90 mol % of the total number of moles of the component unit (b) derived from the diamine; A component unit (b2) derived from a diamine represented by the following formula (1), which is 10 mol % or more and less than 50 mol % based on the total number of moles of the component unit (b) derived from the diamine: A polyamide resin in an amount of 20% by mass or more and 80% by mass or less based on the total mass of the polyamide resin composition, [Formula 1] (In formula (1), n and two m's each independently represent 0 or 1; -X- is a single bond, or -O-, -S-, or -SO 2 -, -CO- and -CH 2 - is a divalent group selected from the group consisting of A flame retardant, The flame retardant is At least one flame retardant (X) selected from the group consisting of polybrominated styrene, brominated polystyrene, and brominated polyphenylene, in an amount of 1 mass% or more and 40 mass% or less relative to the total mass of the polyamide resin composition; or a flame retardant (Y) containing a phosphinate compound represented by formula (I) or a bisphosphinate compound represented by formula (II), or a polymer thereof, in an amount of 3 mass% or more and 20 mass% or less relative to the total mass of the polyamide resin composition; [Case 2] [In the formula, R 1 and R 2are independently a linear or branched alkyl or aryl group having from 1 to 6 carbon atoms, R 3 each independently represents a linear or branched alkylene group having from 1 to 10 carbon atoms, an arylene group having from 6 to 10 carbon atoms, an alkylarylene group having from 6 to 10 carbon atoms, or an arylalkylene group having from 6 to 10 carbon atoms, M is an atom or an atomic group selected from the group consisting of Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K, and protonated nitrogen bases; m represents an integer of 1 to 4, n represents an integer of 1 to 4, and x represents an integer of 1 to 4. Polyamide resin composition.
2. The polyamide resin comprises 15 mol % or more and less than 45 mol % of the diamine-derived component unit (b2) represented by the formula (1) relative to the total number of moles of the diamine-derived component unit (b). The polyamide resin composition according to claim 1.
3. The component unit (b1) derived from an alkylenediamine having 4 to 18 carbon atoms includes a component unit derived from a linear alkylenediamine or a branched alkylenediamine. The polyamide resin composition according to claim 1 or 2.
4. The linear or branched alkylenediamine is a diamine selected from the group consisting of 1,4-diaminobutane, 1,6-diaminohexane, 1,9-nonanediamine, 1,10-decanediamine, 2-methyl-1,5-pentanediamine and 2-methyl-1,8-octanediamine; The polyamide resin composition according to claim 3.
5. The aromatic or cycloaliphatic dicarboxylic acid is terephthalic acid, naphthalenedicarboxylic acid or cyclohexanedicarboxylic acid; The polyamide resin composition according to any one of claims 1 to 4.
6. The polyamide resin contains component units (a1) derived from terephthalic acid, naphthalenedicarboxylic acid or cyclohexanedicarboxylic acid in an amount of more than 20 mol% and not more than 100 mol% based on the total mole number of component units (a) derived from the dicarboxylic acid. The polyamide resin composition according to claim 5. (However, this does not include polyamide resins in which the content of terephthalic acid is 0% by weight or more and 80% by weight or less based on the total weight of dicarboxylic acids.)
7. The polyamide resin has crystallinity. The polyamide resin composition according to any one of claims 1 to 6.
8. The melting point (Tm) of the polyamide resin measured by a differential scanning calorimeter (DSC) is 280°C or higher and 335°C or lower. The polyamide resin composition according to any one of claims 1 to 7.
9. The heat of fusion (ΔH) of the polyamide resin measured by a differential scanning calorimeter (DSC) is 10 mJ / mg or more. The polyamide resin composition according to any one of claims 1 to 8.
10. The flame retardant is a flame retardant (Y) containing a phosphinate compound represented by formula (I) or a bisphosphinate compound represented by formula (II), or a polymer thereof. The polyamide resin composition according to any one of claims 1 to 9.
11. The flame retardant is at least one flame retardant (X) selected from the group consisting of polybrominated styrene, brominated polystyrene, and brominated polyphenylene; The polyamide resin composition according to any one of claims 1 to 10.
12. The polyamide resin composition according to claim 11, further comprising 0.01% by mass or more and 5% by mass or less of an antimony compound, based on the total mass of the polyamide resin composition.
13. The polyamide resin composition according to claim 12, further comprising from 0.5% by mass to 10% by mass of a zinc salt or a calcium salt, based on the total mass of the polyamide resin composition.
14. The polyamide resin composition according to any one of claims 1 to 13, which is a resin composition for use as an insulating material.
15. The polyamide resin composition according to any one of claims 1 to 14, Polyamide molding.
16. It is a part of electrical equipment. The polyamide molding according to claim 15.
Citation Information
Patent Citations
JP1974055796A
Transparent copolyamide
JP1978125497A
Production of polyamide
JP1988154739A
Polyamide composition for sealing electric and electronic parts
JP2003176408A
Polyamide resin composition