Insulated gate semiconductor device and method for manufacturing the same
By forming a silicon oxide film on silicon carbide and using carbon dioxide nitriding to stabilize the interface, the method addresses interface state density issues, reducing gate threshold voltage fluctuations and enhancing the reliability of SiC-based MOSFETs.
Patent Information
- Application Number
- JP2021083216
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-05-17
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2041-05-17
AI Technical Summary
Existing insulated gate semiconductor devices using silicon carbide (SiC) face issues with high interface state density leading to decreased channel mobility and fluctuations in gate threshold voltage due to negative bias temperature instability (NBTI) and positive bias temperature instability (PBTI), affecting the reliability of MOSFETs in power semiconductor devices.
A method involving the formation of a silicon oxide film on a silicon carbide channel, followed by nitriding the interface with carbon dioxide to create an intermediate nitride layer, and subsequent removal of excess nitrogen atoms using a gas treatment to form a nitrided termination layer, which stabilizes the gate threshold voltage.
This approach reduces fluctuations in gate threshold voltage and enhances the reliability of semiconductor devices by minimizing electron trap levels in the gate insulating film, thereby improving the operational stability of MOSFETs.
Smart Images

Figure 0007576274000001 
Figure 0007576274000002 
Figure 0007576274000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an insulated gate semiconductor device and a method for manufacturing an insulated gate semiconductor device, and more particularly to an insulated gate semiconductor device using silicon carbide (SiC) and a method for manufacturing an insulated gate semiconductor device. [Background technology]
[0002] In a MOS field effect transistor (FET) using SiC, a high density of interface states is formed when a gate insulating film is formed on a semiconductor layer. This causes a problem that the mobility of the channel is reduced, and the electrical characteristics such as the on-resistance of the MOSFET are deteriorated. It has been proposed to reduce the interface state density (Dit) at the gate insulating film interface and increase the mobility by performing a heat treatment in a gas containing nitrogen (N) after the gate insulating film is formed and forming a high concentration nitrided region at the interface between the silicon oxide (SiO2) film and the SiC. However, there is a problem that the operational reliability of the semiconductor device cannot be ensured depending on the driving conditions due to negative bias temperature instability (NBTI), which causes fluctuations in the gate threshold voltage, which is the on-off voltage of the device, in response to negative bias application stress. Non-Patent Document 1 points out the possibility that the NBTI problem is caused by the generation of hole traps due to nitrogen atoms that enter the SiO2 film, which is the gate insulating film, during the nitrided region formation process. Non-Patent Document 2 reports the effect of heat treatment with various gases including CO2 on the electrical characteristics of the SiC / SiO2 interface.
[0003] Patent Document 1 discloses a technique for improving NBTI by specifying the N concentration near the interface between a SiO2 film and SiC. Specifically, the interface is defined as the position where the oxygen (O) concentration is 90% of the O concentration in the SiO2 film, and the N concentration in the region ±5 nm from the interface is set to 5×10 13 cm -2 Higher, 1.6×10 14 cm -2However, in the technology of Patent Document 1, the amount of N atoms contributing to interface passivation is reduced, so the nitridation effect is insufficient and channel mobility is reduced. In addition, fluctuations in the gate threshold voltage due to positive bias temperature instability (PBTI) become an issue.
[0004] SiC-MOSFETs have been put to practical use as power semiconductor elements such as inverters. In inverters, MOSFETs are driven as switching elements by repeatedly turning on and off alternately. For example, when positive and negative gate voltages are repeatedly applied to the gate electrode of an n-type MOSFET, the gate threshold voltage fluctuates due to an increase in the density of electrons trapped in the gate oxide film, resulting in a problem of reduced reliability. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2011-82454 A [Non-patent literature]
[0006] [Non-Patent Document 1] J. Rozen et al., "Increase in oxide hole trap density associated with nitrogen incorporation at the SiO2 / SiC interface," J. Appl. Phys., Vol. 103, 2008, p. 124513 [Non-Patent Document 2] W. Wang et al., "Interface Properties of 4H-SiC / SiO2 with MOS Capacitors and FETs annealed in O2, N2O, NO and CO2," Materials Science Forum, Vol. 457-460, 2004, pp. 1309-1312 Summary of the Invention [Problem to be solved by the invention]
[0007] In view of the above problems, an object of the present invention is to provide an insulated gate semiconductor device and a method for manufacturing an insulated gate semiconductor device that can reduce fluctuations in gate threshold voltage and suppress deterioration of the reliability of the semiconductor device. [Means for solving the problem]
[0008] In order to achieve the above object, one aspect of the present invention is a method for manufacturing an insulated gate semiconductor device, comprising the steps of: (a) forming a gate insulating film made of a silicon oxide film on an upper surface of a channel formation region made of silicon carbide; (b) heat-treating the gate insulating film with a gas containing nitrogen atoms to nitride an interface between the gate insulating film and the silicon carbide to form an intermediate nitride layer at the interface between the channel formation region and the gate insulating film; (c) heat-treating the gate insulating film with a gas containing carbon dioxide to remove some of the nitrogen atoms in the gate insulating film and form a nitride termination layer at the interface; (d) heat-treating the gate insulating film with an inert gas after forming the nitride termination layer; and (e) forming a gate electrode on the gate insulating film to control a surface potential of the channel formation region.
[0009] Another aspect of the present invention is a semiconductor device comprising: (a) a gate insulating film made of a silicon oxide film provided on an upper surface of a channel formation region made of silicon carbide; (b) a nitride termination layer made of silicon nitride provided at an interface between the channel formation region and the gate insulating film; and (c) a gate electrode provided on the gate insulating film for controlling a surface potential of the channel formation region, wherein the amount of injected charge injected into the gate insulating film by energizing the channel formation region and the gate insulating film is 5×10 15 cm -2 That's it, 1×10 16 cm -2 When electrons are injected with the following charge amount, the average density of electrons captured in the gate insulating film is 2×10 17 cm -3 The present invention relates to an insulated gate semiconductor device as described below. Effect of the Invention
[0010] According to the present invention, it is possible to provide an insulated gate semiconductor device capable of reducing fluctuations in gate threshold voltage and suppressing deterioration in the reliability of the semiconductor device, and a method for manufacturing the insulated gate semiconductor device. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view showing an example of an insulated gate semiconductor device according to an embodiment of the present invention. [Diagram 2] 5A to 5C are schematic cross-sectional views for explaining an example of a process for a method of manufacturing a MOS capacitor used for evaluating an insulated gate structure according to an embodiment. [Diagram 3] 3 is a schematic cross-sectional view for explaining an example of a step subsequent to that of FIG. 2 in a method for manufacturing a MOS capacitor used for evaluating an insulated gate structure according to an embodiment. FIG. [Figure 4] 4 is a schematic cross-sectional view for explaining an example of a step subsequent to that of FIG. 3 in a method for manufacturing a MOS capacitor used for evaluating an insulated gate structure according to an embodiment. FIG. [Diagram 5] 5 is a schematic cross-sectional view for explaining an example of a step subsequent to that of FIG. 4 in a method for manufacturing a MOS capacitor used for evaluating an insulated gate structure according to an embodiment. FIG. [Figure 6] 1 is a schematic cross-sectional view showing an example of a MOS capacitor according to Comparative Example 1 or 2. FIG. [Figure 7] FIG. 1 is a band diagram for explaining an outline of a current test of a gate insulating film of a MOS capacitor. [Figure 8] 1A and 1B are diagrams for explaining an evaluation method of a gate insulating film of a MOS capacitor by a current test. [Figure 9] 1 is a diagram showing an example of the relationship between the amount of injected electrons and the density of trapped electrons obtained in a current test of a gate insulating film according to an embodiment. [Figure 10] 1 is a table showing an example of evaluation results of a current test of a gate insulating film according to an embodiment. [Figure 11] 5A to 5C are schematic cross-sectional views for explaining an example of a process of a method for manufacturing an insulated gate semiconductor device according to an embodiment. [Figure 12] 12 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 11 in the method for manufacturing an insulated gate semiconductor device according to the embodiment. FIG. [Figure 13] 13 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 12 in the method for manufacturing an insulated gate semiconductor device according to the embodiment. FIG. [Figure 14] 14 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 13 in the method for manufacturing an insulated gate semiconductor device according to the embodiment. FIG. [Figure 15] 15 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 14 in the method for manufacturing an insulated gate semiconductor device according to the embodiment. FIG. [Figure 16] 16 is a schematic cross-sectional view for explaining an example of a step subsequent to FIG. 15 in the method for manufacturing an insulated gate semiconductor device according to the embodiment. FIG. [Figure 17] 1 is a schematic cross-sectional view showing an example of an insulated gate semiconductor device according to Comparative Example 3 or 4. FIG. [Figure 18] 1 is a diagram showing an example of the relationship between the shift amount of the gate threshold voltage and the gate voltage application time of the insulated gate semiconductor device according to the embodiment. FIG. [Figure 19]1 is a table showing an example of a result of evaluation of the amount of shift in gate threshold voltage of an insulated gate semiconductor device according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the description of the drawings, the same or similar parts are given the same or similar reference numerals, and duplicated explanations are omitted. However, the drawings are schematic, and the relationship between thickness and planar dimensions, the ratio of thickness of each layer, etc. may differ from the actual ones. In addition, parts with different dimensional relationships and ratios may be included between the drawings. In addition, the embodiments shown below are examples of devices and methods for embodying the technical idea of the present invention, and the technical idea of the present invention does not specify the materials, shapes, structures, arrangements, etc. of the components as described below.
[0013] In this specification, the source region of a MOS transistor is "one main region (first main region)" that can be selected as the emitter region of an insulated gate bipolar transistor (IGBT). In addition, in a thyristor such as a MOS controlled static induction thyristor (SI thyristor), one main region can be selected as the cathode region. The drain region of a MOS transistor is "the other main region (second main region)" of a semiconductor device that can be selected as the collector region in an IGBT or as the anode region in a thyristor. In this specification, when the term "main region" is used simply, it means either the first main region or the second main region that is appropriate from the technical common sense of a person skilled in the art.
[0014] In addition, the definitions of the directions such as up and down in the following description are merely for the convenience of explanation and do not limit the technical idea of the present invention. For example, if an object is rotated 90 degrees and observed, up and down are converted to left and right and read, and if it is rotated 180 degrees and observed, up and down are read inverted. In the following description, the case where the first conductivity type is p-type and the opposite second conductivity type is n-type will be described as an example. However, the conductivity types may be selected in an inverse relationship, with the first conductivity type being n-type and the second conductivity type being p-type. In addition, + and - added to n and p mean that the semiconductor region has a relatively high or low impurity density, respectively, compared to a semiconductor region without + and -. However, even if the same n and n are added to the semiconductor region, it does not mean that the impurity density of each semiconductor region is strictly the same. In addition, in the notation of Miller indices in this specification, "-" means a bar attached to the index immediately after it, and adding "-" before the index represents a negative index.
[0015] The insulated gate semiconductor device according to the embodiment of the present invention is a lateral MOSFET using a silicon oxide (SiO2) film as a gate insulating film. As shown in FIG. 1, it has a channel formation region (base region) 3 of a first conductivity type (p-type), and an inversion channel is formed on the surface of the channel formation region 3. A high-impurity-density second conductivity type (n + In the semiconductor device, main regions of a gate type, such as a source region (first main region) 4a and a drain region (second main region) 4b, are selectively provided. An insulated gate electrode structure (5, 7) is provided on the upper surface of the channel formation region 3 across the source region 4a and the drain region 4b, with a nitride termination layer 6 terminated with nitrogen (N) interposed therebetween. The insulated gate electrode structure (5, 7) is composed of a gate insulating film 5 made of a SiO2 film and a gate electrode (control electrode) 7 on the gate insulating film 5. The gate electrode 7 electrostatically controls the surface potential of the channel formation region 3 via the gate insulating film 5, forming an inversion channel on the surface of the channel formation region 3.
[0016] The nitrided termination layer 6 is a nitrogen termination layer provided by nitriding the interface between the gate insulating film 5 and the channel formation region 3 and then heat-treating it with carbon dioxide (CO2) gas. As the silicon oxide film (SiO2 film) which is the gate insulating film 5 of the MOSFET, a thermal oxide film such as oxygen (O2) dry oxidation or wet oxidation, or a deposited oxide film such as sputtering, thermal chemical vapor deposition (CVD), or plasma CVD can be used. As the material for the gate electrode 7, a metal film such as aluminum (Al), a polysilicon layer (doped polysilicon layer) to which impurities such as phosphorus (P) and boron (B) are added at high concentrations, or the like can be used.
[0017] As shown in FIG. 1, the channel formation region 3 is epitaxially grown on a substrate 1 made of an n-type SiC semiconductor. A source electrode 8a and a drain electrode 8b are provided so as to be in physical contact with the source region 4a and the drain region 4b, respectively. The source electrode 8a and the drain electrode 8b are ohmic-connected to the source region 4a and the drain region 4b, respectively. The source electrode 8a and the drain electrode 8b are formed of, for example, a single layer film made of Al or nickel silicide (NiSi x A metal film in which a metal film including a titanium nitride (TiN) and an Al layer is laminated in this order can be used. Although not shown in the figure, a p + A contact region is disposed in the channel forming region 3 and is separated from the source region 4a.
[0018] There are crystal polymorphs in SiC crystals, the main ones being cubic 3C, and hexagonal 4H and 6H. The band gap at room temperature has been reported to be 2.23 eV for 3C-SiC, 3.26 eV for 4H-SiC, and 3.02 eV for 6H-SiC. The insulated gate type semiconductor device according to the embodiment of the present invention will be described using 4H-SiC. In the insulated gate type semiconductor device according to the embodiment, a semiconductor substrate (SiC substrate) made of SiC is used as the substrate 1. When a SiC substrate is used, a structure in which the channel formation region 3 is made of an epitaxial layer (SiC layer) made of SiC is exemplified. The surface orientation of the SiC substrate will be described using the (0001) surface (Si surface), but the (11-20) surface (a surface), (1-100) surface (m surface), and (000-1) surface (C surface) may also be used.
[0019] 1, in the insulated gate semiconductor device according to the embodiment, a voltage is applied to the gate electrode 7 to form an inversion layer that becomes a channel at the interface between the gate insulating film 5 and the channel formation region 3. At this time, a voltage is applied between the source electrode 8a and the drain electrode 8b, so that carriers (electrons) are injected from the source region 4a into the channel. The injected carriers travel through the channel and flow into the drain region 4b.
[0020] Usually, when the SiO2 film used for the gate insulating film 5 is formed by a thermal oxidation method or the like, C atoms remain at the interface between the SiO2 film and the SiC semiconductor layer, forming a high-density interface state. When electrons are captured at the interface state, the electron mobility decreases due to Coulomb scattering or the like. A method has been proposed to reduce the interface state density by terminating the interface between the SiO2 film and the SiC semiconductor layer with N atoms. However, when a high-concentration nitrided region is formed at the interface between the SiO2 film and the SiC semiconductor layer, the gate threshold voltage of the semiconductor device fluctuates in response to the stress of applying a negative gate voltage.
[0021] In the insulated gate semiconductor device according to the embodiment, the intermediate nitride termination layer formed at the interface between the gate insulating film 5 and the channel formation region 3 by nitridation is heat-treated with carbon dioxide (CO2) gas to provide the nitride termination layer 6. The CO2 heat treatment breaks the Si-N bonds in the nitride termination layer 6 and the gate insulating film 5, and the excess N atoms can be eliminated, thereby removing the hole traps in the gate insulating film 5. Furthermore, after the CO2 heat treatment, the gate insulating film 5 is heat-treated with an inert gas such as nitrogen (N2) or argon (Ar) to reduce the electron trap level in the gate insulating film 5 that remains without being removed by the nitridation or CO2 heat treatment. As a result, it becomes possible to suppress the gate threshold voltage fluctuation of the semiconductor device.
[0022] The fluctuation of the gate threshold voltage of a semiconductor device is, for example, the flat band voltage (V FB ) shift. Therefore, a MOS capacitor corresponding to the insulated gate structure according to the embodiment was fabricated to evaluate the interface characteristics of the MOS capacitor. A manufacturing method of a MOS capacitor corresponding to the insulated gate structure according to the embodiment will be described with reference to the process diagrams shown in Figs. 2 to 5. Note that the manufacturing method of a MOS capacitor described below is one example, and it goes without saying that various other manufacturing methods, including modified examples thereof, can be used within the scope of the spirit of the claims.
[0023] First, an n-type SiC substrate (substrate) 2 doped with n-type impurities such as nitrogen (N) is prepared. The substrate 2 is a 4H-SiC substrate, and has a surface orientation of (0001) (Si surface). First, the substrate 2 is subjected to RCA cleaning, which involves adding an alkali or acid to hydrogen peroxide and heating to clean it, and then is treated with hydrogen fluoride (HF) and dried. As shown in FIG. 2, the top surface of the cleaned substrate 2 is heated in a 100% oxygen (O2) gas atmosphere at a temperature of 1100°C to 1300°C, for example, about 1200°C, for about 160 minutes to form an oxide film 5a made of SiO2 with a thickness of about 50 nm. Although a dry oxide film is exemplified as the oxide film 5a, a wet oxide film may also be used, and a deposited oxide film may also be used by sputtering, thermal CVD, plasma CVD, or the like. For example, the oxide film 5a may be deposited by reduced pressure thermal CVD using silane (SiH4) gas and O2 gas at a pressure of about 0.2 Pa and a temperature of about 600°C.
[0024] Next, in a gas atmosphere in which nitric oxide (NO) gas is added at 10% to nitrogen (N2) gas, the substrate is heated at a temperature of 1150°C to 1300°C, for example, at about 1250°C, for about 60 minutes to perform nitriding treatment. By this nitriding treatment, an intermediate nitride layer 6a is formed at the interface between the oxide film 5a and the substrate 2, as shown in Fig. 3. Nitrous oxide (N2O) gas may be used instead of NO for the nitriding treatment.
[0025] Next, in a CO2 gas atmosphere, heat treatment (CO2 heat treatment) is performed at 900°C to 1400°C, preferably 950°C to 1300°C, for about 30 minutes. The temperature of the CO2 heat treatment is 950°C in Example 1, and 1100°C in Examples 2 and 3. Furthermore, in Example 3, heat treatment (N2 heat treatment) is performed at about 1100°C for about 30 minutes in an inert gas, for example, N2 gas, atmosphere. By the three types of heat treatment in Examples 1 to 3, as shown in FIG. 4, the N atom concentration in the oxide film 5a near the interface between the oxide film 5a and the substrate 2 is reduced, and the nitrided termination layer 6 in which some N atoms are removed from the intermediate nitrided layer 6a is generated in three different modes. In the CO2 heat treatment, 100% CO2 gas is used, but a mixed gas of CO2 gas and an inert gas such as N2 or Ar may be used.
[0026] As shown in Fig. 5, a circular pattern of a metal film with a diameter of about 200 µm is formed on the upper surface of the oxide film 5a by lift-off or normal photolithography. The metal film that is the premise of the circular pattern may be a metal film of Al or the like with a thickness of about 100 µm deposited on the upper surface of the oxide film 5a by sputtering, vacuum deposition, or the like. Subsequently, a metal film of Al or the like with a thickness of about 100 µm is deposited on the entire rear surface of the substrate 2 by sputtering, vacuum deposition, or the like. In this manner, the front electrode 10 and the rear electrode 11 are formed.
[0027] The three types of Examples 1 to 3 thus fabricated were repeatedly subjected to current tests and CV measurements to evaluate the average density of electrons captured in the trap levels in the oxide film 5a (trapped electron density). In addition, in order to compare with Examples 1 to 3, Comparative Example 1 was fabricated and evaluated in which the front electrode 10 and the back electrode 11 were formed without performing the CO2 heat treatment after the formation of the intermediate nitride layer 6a in FIG. 3, as shown in FIG. 6. Comparative Example 2 was also fabricated and evaluated in which, after the formation of the intermediate nitride layer 6a, N2 heat treatment was performed for about 30 minutes at about 1100°C instead of the CO2 heat treatment.
[0028] In the current test, as shown in FIG. 7, a positive voltage V G By applying a voltage of 100 V, a small current I flows from the n-type SiC semiconductor layer (substrate 2) to the Al metal film. G is passed for a certain period of time. During the passage of the current, electrons accumulated at the semiconductor interface between the SiC semiconductor layer and the SiO2 oxide film corresponding to the oxide film 5a are injected into the oxide film by crossing or tunneling over the barrier at the interface. G is a constant current in the range of 30 pA to 100 pA, for example, about 50 pA. The amount of electrons (charges) injected into the oxide film is G It can be calculated by dividing the product of the current flow time and the elementary charge.
[0029] The flat band voltage V obtained from CV measurements of a MOS capacitor FB The change in ΔV FB Using the above, the electron density n trapped in the oxide film is calculated. Tcan be calculated from equation (1). Note that the trapped electron density n T is a value obtained on the assumption that the trapped electrons are uniformly distributed in the oxide film, but it does not indicate that the electron trap sites are actually distributed uniformly in the oxide film. Rather, the value obtained on this assumption is used as an index of the number of electron traps present in the oxide film. n T =-(2Cox / d)ΔV FB (1) where Cox is the oxide capacitance per unit area and d is the oxide thickness. Figure 8 shows the relationship between the amount of electrons injected into the oxide and V FB The change in ΔV FB or trapped electron density n T As shown in FIG. 8, the change amount ΔV FB or trapped electron density n T The current flow rate tends to saturate as the amount of injected electrons accumulates with increasing current flow time. When the accumulated amount of injected electrons reaches a limit due to long-term current flow, dielectric breakdown of the oxide film occurs.
[0030] FIG. 9 shows the trap electron density n T 9 is a double logarithmic graph showing the relationship between the amount of injected electrons and the trapped electron density n T The trapped electron density n T is the amount of injected electrons is 10 15 cm -2 The following is the same as Comparative Example 1, but the amount of injected electrons is 10 15 cm -2 When the trapped electron density n T is the amount of injected electrons is 10 15 cm -2 In the following, the results are similar to those of Comparative Example 2 in which N2 heat treatment was performed instead of CO2 heat treatment, but the amount of injected electrons is 10 15 cm -2 When the amount of injected electrons exceeds 5×1015 cm -2 At about this level or higher, the trapped electron density n T The trapped electron density n T The reduction effect is 5×10 15 cm -2 above, 1×10 16 cm -2 In addition, in Example 3 in which the N2 heat treatment was performed after the CO2 heat treatment, the trapped electron density n T This indicates that the trap level of electrons remaining in the oxide film 5a without being removed by the nitriding treatment and the CO2 heat treatment is reduced by the N2 heat treatment, and the trapped electron density n T is estimated to be reduced.
[0031] FIG. 10 shows the total amount of injected electrons obtained by current tests and CV measurements for Examples 1 to 3 and Comparative Examples 1 and 2. 15 cm -2 Trap electron density at about n T As shown in the table of FIG. 10, in Comparative Examples 1 and 2 in which the CO2 heat treatment was not performed, the trapped electron density n T are 3.5×10 17 cm -3 and 3.35 x 10 17 cm -3 On the other hand, in Examples 1 and 2 in which the CO2 heat treatment was performed, the trapped electron density n T are 1.95×10 17 cm -3 , and 0.66×10 17 cm -3 This gives us 2×10 17 cm -3 Furthermore, in Example 3 in which the N2 heat treatment was performed after the CO2 heat treatment, the trapped electron density n T is 0.26 x 10 17 cm -3 Thus, the CO2 heat treatment at high temperatures reduces the trapped electron density n TIn addition, when the N2 heat treatment is performed after the CO2 heat treatment, the trapped electron density n T can be reduced by an order of magnitude or more.
[0032] In the insulating gate structure according to the embodiment, after the nitridation of the oxide film 5a, a CO2 heat treatment is performed, and then an N2 heat treatment is performed. In the CO2 treatment, the Si-N bonds or Si-ON bonds in the oxide film 5a introduced by the nitridation are broken. Although heat treatment with O2 gas instead of CO2 gas has the effect of breaking the Si-N bonds and converting them to Si-O bonds, the SiC surface of the substrate 2 is also oxidized, and the N passivation at the interface formed by the nitridation is destroyed. On the other hand, CO2 gas is decomposed into CO as a reducing gas and O2 as an oxidizing gas at about 800°C to 1400°C. CO can break the Si-N bonds in the SiO2 film, but it is less likely to destroy the N passivation at the interface than O2. Therefore, the interface state density can be reduced. In addition, by performing an additional N2 heat treatment, the electron trap level in the oxide film 5a, which is difficult to repair by the nitridation or CO2 heat treatment, can be reduced. As a result, it is possible to suppress the gate threshold voltage fluctuation of the semiconductor device.
[0033] In the above description, a SiC substrate with a (0001) plane (Si plane) orientation is used as the substrate 2. The Si plane has a faster oxidation rate than the (11-20) plane (a plane), the (1-100) plane (m plane), and the (000-1) plane (C plane). Therefore, for the Si plane, the CO2 heat treatment temperature is preferably in the range of 1000°C to 1400°C, and more preferably in the range of 1100°C to 1300°C. For the a-plane, m-plane, and C-plane, the CO2 heat treatment temperature is preferably in the range of 800°C to 1200°C, and more preferably in the range of 1000°C to 1200°C.
[0034] (Method of Manufacturing Insulated Gate Semiconductor Device) Next, a method for manufacturing an insulated gate semiconductor device according to an embodiment will be described using a lateral MOSFET as an example, with reference to the process diagrams shown in Figures 11 to 16. Note that the method for manufacturing a MOSFET described below is only an example, and it goes without saying that various other manufacturing methods, including modifications thereof, can be used within the scope of the spirit of the claims.
[0035] First, an n-type SiC substrate (substrate) 1 doped with n-type impurities such as nitrogen (N) is prepared. The substrate 1 is a 4H-SiC substrate, and has a (0001) plane (Si plane) orientation. A p-type channel formation region (base region) 3 is epitaxially grown on the upper surface of the substrate 1. N-type impurities such as N are selectively implanted from the upper surface side of the channel formation region 3 by photolithography technology, ion implantation technology, or the like. The implanted n-type impurity ions are activated by heat treatment. As a result, n-type impurity ions are formed in the upper part of the channel formation region 3, as shown in FIG. + A source region (first main region) 4a and a drain region (second main region) 4b of the same type are selectively buried.
[0036] 12, an oxide film 5b made of SiO2 and about 50 nm thick is formed on the upper surface of the channel formation region 3 by heating in a 100% O2 gas atmosphere at a temperature of about 1200°C for about 160 minutes. Although a dry oxide film is exemplified as the oxide film 5b, a wet oxide film or a deposited oxide film by thermal CVD, plasma CVD, or the like may also be used. For example, the oxide film 5b may be deposited by low-pressure thermal CVD using silane (SiH4) gas and oxygen (O2) gas at a pressure of about 0.2 Pa and a temperature of about 600°C.
[0037] Next, the substrate is heated at about 1250°C for about 60 minutes in an atmosphere of N2 gas with 10% nitric oxide (NO) gas to perform nitridation. As a result of this nitridation, an intermediate nitride layer 6a is formed at the interfaces between the oxide film 5b and the channel formation region 3, the source region 4a, and the drain region 4b, as shown in Fig. 13. Note that NO gas may be used instead of NO for the nitridation.
[0038] After the nitridation process, a CO2 heat treatment is performed in a CO2 gas atmosphere at two different temperatures for about 30 minutes each. The two temperatures are about 950°C for Example 4 and about 1100°C for Examples 5 and 6. For Example 3, after the CO2 heat treatment, a N2 heat treatment is further performed in a N2 gas atmosphere at about 1100°C for about 30 minutes. As shown in FIG. 14, the heat treatment in Examples 4 to 6 reduces the N atom concentration in the oxide film 5b near the interface between the oxide film 5b and the channel formation region 3, the source region 4a, and the drain region 4b in each mode. Also, in each mode, a nitride termination layer 6 in which some N atoms are removed from the intermediate nitride layer 6a is generated. In the CO2 heat treatment, 100% CO2 gas is used, but a mixed gas of CO2 gas and an inert gas such as N2 or Ar may be used.
[0039] A source contact hole and a drain contact hole are opened in the oxide film 5b by photolithography, dry etching, etc. As a result, as shown in FIG. 15, a pattern of the gate insulating film 5 selectively remains on the upper surface of the channel formation region 3 so as to straddle the source region 4a and the drain region 4b.
[0040] A metal film such as Al having a thickness of about 100 μm is deposited on the upper surfaces of the gate insulating film 5, the source contact hole, and the drain contact hole by sputtering, vacuum deposition, or the like. The metal film is separated by photolithography, dry etching, or the like to form patterns of the gate electrode 7, the source electrode 8a, and the drain electrode 8b. As a result, an insulated gate electrode structure (5, 7) is formed on the upper surface of the channel formation region 3 via the nitride termination layer 6 so as to straddle a part of the ends of the source region 4a and the drain region 4b. In this manner, the insulated gate semiconductor device according to the embodiment shown in FIG. 16 is completed.
[0041] For the three types of lateral MOSFETs fabricated in this way, Examples 4 to 6, the transistor characteristics were measured by a transistor drive test, and the gate threshold voltage (V TH ) shift amount ΔV THThe transistor drive test was performed by applying a square wave voltage of +20V / -10V as the gate voltage for 10,000 hours at room temperature with a switching frequency of 200 kHz. As shown in FIG. 17, in order to compare with Examples 4 to 6, Comparative Example 3 in which the gate insulating film 5, the gate electrode 7, the source electrode 8a, and the drain electrode 8b were formed without performing the CO2 heat treatment after the formation of the intermediate nitride layer 6a in FIG. 13 was also similarly evaluated. In addition, Comparative Example 4 in which, instead of the CO2 heat treatment, an N2 heat treatment at about 1100°C for about 30 minutes was performed after the formation of the intermediate nitride layer 6a was also produced and evaluated.
[0042] FIG. 18 shows the gate threshold voltage shift ΔV TH As shown in FIG. TH increases with increasing driving time. TH is similar to that of Comparative Example 3 when the driving time is less than 1000 hours, but is smaller than that of Comparative Example 3 when the driving time is 1000 hours or more. TH When the driving time is 100 hours or less, the shift amount ΔV in Example 5 is approximately the same as that in Comparative Example 4 in which N2 heat treatment was performed instead of CO2 heat treatment, but when the driving time exceeds 100 hours, the shift amount ΔV in Example 5 is smaller than that in Comparative Example 4. TH When the driving time exceeds 1000 hours, the shift amount ΔV TH Also, in Example 6, in which the N2 heat treatment was performed after the CO2 heat treatment, the shift amount ΔV TH The driving time and shift amount ΔV shown in Fig. 18 are small. TH The relationship between the injected electron amount and the trapped electron density n T In particular, the relationship between the trapped electron density n T Linear interpolation between the measured values of 5×10 15 cm -2 Trap electron density at about n T However, the shift amount ΔV after 1000 hours of operation TH It can be seen that this corresponds to the magnitude relationship of
[0043] FIG. 19 shows the shift in gate threshold voltage ΔV after 10,000 hours of operation. TH As shown in the table of FIG. 19, the shift amount ΔV of Example 4 and Example 5, which were subjected to CO2 heat treatment at 950° C. and 1100° C., TH are 0.30 V and 0.10 V, respectively. The shift amount ΔV in Example 6 in which the CO2 heat treatment and the N2 heat treatment were performed at 1100° C. T On the other hand, the shift amount ΔV in Comparative Example 3, which only uses the conventional nitriding treatment, is 0.06V. T The shift amount ΔV in Comparative Example 4, in which N2 heat treatment was performed instead of CO2 heat treatment, was 0.94V. T In this way, in Examples 4 to 6, the shift amount ΔV of the gate threshold voltage after 10,000 hours of operation TH A large improvement is seen in the shift amount ΔV in Examples 4 to 6. TH In this manner, in the insulated gate semiconductor device according to the embodiment, the gate threshold voltage shift can be suppressed, and deterioration of the reliability of the semiconductor device can be suppressed.
[0044] (Other embodiments) As described above, the insulated gate semiconductor device according to the embodiment of the present invention has been described, but the description and drawings forming a part of this disclosure should not be understood as limiting the present invention. Various alternative embodiments, examples, and operating techniques will be apparent to those skilled in the art from this disclosure.
[0045] As described above, in the insulated gate semiconductor device according to the embodiment, a lateral MOSFET using 4H-SiC is exemplified, but the present invention can also be applied to semiconductor devices using 6H-SiC and 3C-SiC. Furthermore, the present invention can also be applied to a planar gate vertical MOSFET and a trench gate vertical MOSFET.
[0046] Thus, the present invention naturally includes various embodiments not described here, such as configurations obtained by arbitrarily applying the configurations described in the above embodiments and modifications. Therefore, the technical scope of the present invention is determined only by the invention-specifying matters according to the scope of the claims that are appropriate from the above description. [Explanation of symbols]
[0047] 1, 2...Substrate (SiC substrate) 3...Channel formation region (base region) 4a...Source area (first main area) 4b...Drain region (second main region) 5...Gate insulating film 5a, 5b...Oxide film 6...Nitride termination layer 6a: Intermediate nitride layer 7...Gate electrode (control electrode) 8a…Source electrode 8b...Drain electrode 10…Surface electrode 11…Back electrode
Claims
1. forming a gate insulating film made of a silicon oxide film on an upper surface of a channel formation region made of silicon carbide; a step of nitriding an interface between the gate insulating film and silicon carbide by heat-treating the gate insulating film with a gas containing nitrogen atoms, thereby forming an intermediate nitride layer at the interface between the channel formation region and the gate insulating film; a step of heat-treating the gate insulating film with a gas containing carbon dioxide to remove some of the nitrogen atoms in the gate insulating film and form a nitride termination layer at the interface; after forming the nitride termination layer, heat treating the gate insulating film with an inert gas; forming a gate electrode on the gate insulating film to control a surface potential of the channel formation region; 2. A method for manufacturing an insulated gate semiconductor device comprising:
2. The gate insulating film is formed by applying a current between the channel forming region and the gate electrode. 15 cm -2 That's it, 1 x 10 16 cm -2 When electrons are injected with the following injection charge amount, the average density of the electrons captured in the gate insulating film is 2×10 17 cm -3 2. The method for manufacturing an insulated gate semiconductor device according to claim 1, wherein:
3. 3. The method for manufacturing an insulated gate semiconductor device according to claim 1, wherein the heat treatment after the formation of the nitride termination layer is carried out in the inert gas at a temperature in the range of 900° C. or more and 1200° C. or less for a time period in the range of 30 minutes or more and 60 minutes or less.
4. 4. The method for manufacturing an insulated gate semiconductor device according to claim 1, wherein the nitride termination layer is formed in the gas containing carbon dioxide at a heat treatment temperature in the range of 900° C. or more and 1400° C. or less for a time period of 30 minutes or more and 120 minutes or less.
5. 5. The method for manufacturing an insulated gate semiconductor device according to claim 1, wherein the surface orientation of the upper surface of the channel formation region is a (0001) surface, and the nitride termination layer is formed at a heat treatment temperature of 1100° C. or more and 1300° C. or less.
6. 5. The method for manufacturing an insulated gate semiconductor device according to claim 1, wherein the surface orientation of the upper surface of the channel formation region is any one of a (000-1) surface, a (11-20) surface, and a (1-100) surface, and the nitride termination layer is formed at a heat treatment temperature of 1000° C. or more and 1200° C. or less.
7. a gate insulating film made of a silicon oxide film provided on an upper surface of a channel formation region made of silicon carbide; a nitride termination layer made of silicon nitride provided at an interface between the channel formation region and the gate insulating film; a gate electrode provided on the gate insulating film for controlling a surface potential of the channel formation region; Equipped with The gate insulating film is formed by applying a current between the channel forming region and the gate electrode. 15 cm -2 That's it, 1 x 10 16 cm -2 When electrons are injected with the following injection charge amount, the average density of the electrons captured in the gate insulating film is 2×10 17 cm -3 1. An insulated gate semiconductor device comprising:
Citation Information
Patent Citations
Silicon carbide semiconductor device and its manufacturing method
JP2006156478A
JP2011‐82454A
Silicon carbide semiconductor device and manufacturing method thereof
JP2020061475A
Method of manufacturing semiconductor device
JP2021048198A