Manufacturing method for MIS type semiconductor device

By forming MIS type semiconductor devices with hydrogen-terminated diamond surfaces in controlled atmospheres and using boron nitride insulators, the method enhances carrier mobility and reduces power consumption, ensuring safe and efficient high-speed operation.

JP7576352B2Active Publication Date: 2024-10-31NAT INST FOR MATERIALS SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023178336
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-10-16
Publication Date
2024-10-31
Estimated Expiration
2039-09-13

AI Technical Summary

Technical Problem

MIS type semiconductor devices using hydrogen-terminated diamond semiconductors face challenges with insufficient hole mobility, leading to high power consumption and unsuitable operation speed, as well as unwanted current flow without applied voltage, which compromises safety and efficiency.

Method used

The method involves forming a semiconductor layer with a hydrogen-terminated diamond surface, followed by an insulator layer in controlled atmospheres such as vacuum or inert gases, using boron nitride as the insulator, to reduce negative charge density and enhance carrier mobility, ensuring the device operates normally off and has low power consumption.

Benefits of technology

The method results in a semiconductor device with high hole mobility, low power consumption, and safe operation, suitable for high-speed applications by minimizing charge scattering and reducing leakage current.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576352000003
    Figure 0007576352000003
  • Figure 0007576352000004
    Figure 0007576352000004
  • Figure 0007576352000005
    Figure 0007576352000005
Patent Text Reader

Abstract

To provide a manufacturing method of an MIS type semiconductor device using a diamond semiconductor with high mobility.SOLUTION: A method includes forming a semiconductor layer whose first main surface is terminated with hydrogen, forming an insulator layer in contact with a hydrogen-terminated diamond layer, forming a conductive layer on at least a portion of the insulating layer, forming a hydrogen-terminated semiconductor layer, and forming an insulator layer, and the atmosphere between the two layers is vacuum, hydrogen gas, an inert gas, or hydrogen gas to which the inert gas is added.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an MIS type semiconductor device, and more particularly to a method for manufacturing an MIS type semiconductor device using a diamond semiconductor, which is safe, energy-saving, has high mobility, and is suitable for high-speed operation. [Background technology]

[0002] Semiconductor diamond has a wide band gap energy (5.47 eV), a low dielectric constant (5.7), a high dielectric breakdown field strength (10 MV / cm), and a high carrier saturation velocity (1.5–2.7 × 10 for electrons and holes, respectively). 7 cm / s and 0.85 to 1.2 × 10 7 cm / s), high thermal conductivity (22 W / cm K) and high carrier mobility (4500 cm for electrons and holes, respectively). 2 / V s and 3800 cm 2 / V s), where the above values ​​are at room temperature. For this reason, electronic devices using diamond as a semiconductor are expected to exhibit high-power operation, high-speed and high-frequency operation, high voltage resistance, and high thermal limit. In particular, MIS (Metal Insulator Semiconductor) type semiconductor devices that use diamond as a semiconductor have attracted attention as core elements for constructing high-performance inverters and high-output high-frequency amplifiers.

[0003] Diamond semiconductors have higher carrier mobility than silicon (Si) and silicon carbide (SiC), which are currently the mainstream materials used for power devices. Due to this high mobility, MIS-type semiconductor devices that use diamond as a semiconductor have the potential to lower the on-resistance, suppress losses, and shorten switching times, enabling elements to operate at high speeds.

[0004] In recent years, hydrogen-terminated diamond semiconductors have been actively investigated (see Non-Patent Document 1). One of the reasons for this is that in diamond semiconductors, the activation energy of dopants is large, making it difficult to achieve both high carrier density and mobility. Another factor that can be cited is that when diamond is produced by vapor phase synthesis, the surface of the diamond is automatically almost completely hydrogen-terminated due to hydrogen atoms, which are an essential process gas in the vapor phase synthesis process. Hydrogen-terminated diamond semiconductors have the advantage in terms of manufacturing, in that the number of processes can be reduced, and because hydrogen termination is almost complete, they also have the advantage of being easy to obtain high quality. When the surface of a diamond semiconductor is hydrogen-terminated, an electrically conductive region is formed near the surface of the diamond semiconductor, and the diamond semiconductor becomes a p-type semiconductor.

[0005] Recent research has suggested that the occurrence of electrical conductivity near the surface of a hydrogen-terminated diamond semiconductor is due to the contribution of negative charges adsorbed on the surface of the diamond semiconductor or present in the insulating film formed in contact with the diamond semiconductor. Sources of this negative charge include, for example, adsorbed gases such as nitrogen dioxide (NO2) and ozone (O3), and solids such as tungsten oxide (WO3), molybdenum oxide (MoO3), vanadium oxide (V2O5), niobium oxide (Nb2O3), and aluminum oxide (Al2O3) (Non-Patent Document 2). Non-Patent Document 3 discloses that unoccupied energy levels due to oxygen point defects and Al vacancies in an Al2O3 film formed on the surface of a diamond become negatively charged, inducing holes near the diamond surface and resulting in electrical conduction. Furthermore, Non-Patent Document 4 discloses an example in which a diamond is exposed to NO2 gas in order to accumulate a high concentration of holes near the surface of the diamond, and then sealed with an Al2O3 film to fabricate a FET (Field Effect Transistor). [Prior art documents] [Non-patent literature]

[0006] [Non-Patent Document 1] IEEE Electron Device Letters,39,1373(2018) [Non-Patent Document 2] Phys.Status Solidi A,1800681(2018) [Non-Patent Document 3] Scientific Reports,7,42368(2017) [Non-Patent Document 4] Jpn.J.Appl.Phys.,56,01AA01(2017) [Non-Patent Document 5] APL Materials,6,111105(2018) [Non-Patent Document 6] Phys.Status Solidi RRL,1700401(2018) Summary of the Invention [Problem to be solved by the invention]

[0007] As described above, diamond semiconductors have excellent material properties for use in MIS-type semiconductor devices, and hydrogen termination is helping to resolve issues regarding productivity and quality. However, when an MIS-type semiconductor device using a hydrogen-terminated diamond semiconductor layer was manufactured, the manufactured MIS-type semiconductor device had a problem that the mobility of holes was insufficient and did not contribute to low power consumption and high-speed operation. In addition, the flow of current when no voltage is applied is undesirable in terms of power consumption and safety, but the reduction of this current and the improvement of mobility could not be achieved at the same time.

[0008] The problem to be solved by the present invention is to provide a method for manufacturing an MIS type semiconductor device using a diamond semiconductor which is safe, energy-saving, has high mobility, and is suitable for high-speed operation. [Means for solving the problem]

[0009] The configuration of the present invention is shown below. (Configuration 1) forming a semiconductor layer having a first major surface comprised of hydrogen-terminated diamond; forming an insulator layer in contact with at least a portion of the hydrogen-terminated surface of the semiconductor layer; forming a conductive layer over at least a portion of the insulating layer; A method for manufacturing an MIS type semiconductor device, wherein the atmosphere during the period from immediately after forming the semiconductor layer to immediately before forming the insulator layer is any one selected from the group consisting of vacuum, hydrogen gas, an inert gas, and hydrogen gas with an inert gas added. (Configuration 2) preparing a member having a first main surface on which at least a portion of a semiconductor layer made of diamond is exposed; hydrogen treatment of at least a portion of the exposed portion of the semiconductor layer; forming an insulator layer in contact with at least a portion of the hydrogen-treated portion of the semiconductor layer; forming a conductive layer over at least a portion of the insulating layer; A method for manufacturing an MIS type semiconductor device, wherein the atmosphere during the period from immediately after the hydrogen treatment to immediately before the formation of the insulating layer is any one selected from the group consisting of vacuum, hydrogen gas, an inert gas, and hydrogen gas with an inert gas added. (Configuration 3) 3. The method for manufacturing an MIS type semiconductor device according to claim 1 or 2, wherein the atmosphere for forming the insulating layer is any one selected from the group consisting of vacuum, hydrogen gas, inert gas, and hydrogen gas with an inert gas added thereto. (Configuration 4) 4. The method for manufacturing an MIS type semiconductor device according to any one of claims 1 to 3, wherein the insulating layer is made of boron nitride. (Configuration 5) 5. The method for manufacturing an MIS type semiconductor device according to any one of claims 1 to 4, wherein the insulating layer is made of a single crystal of boron nitride. (Configuration 6) 6. The method for manufacturing an MIS type semiconductor device according to any one of configurations 1 to 5, wherein the insulating layer is made of hexagonal boron nitride (h-BN). (Configuration 7) The density of charged impurities at the interface between the semiconductor layer and the insulator layer is 0 cm -2 5×10 or more 11 cm -2 7. A method for manufacturing an MIS type semiconductor device according to any one of configurations 1 to 6, comprising: (Configuration 8) The density of charged impurities at the interface between the semiconductor layer and the insulator layer is 0 cm -2 More than 1×10 11 cm -2 7. A method for manufacturing an MIS type semiconductor device according to any one of configurations 1 to 6, comprising: (Configuration 9) 9. The method for manufacturing an MIS type semiconductor device according to any one of configurations 1 to 8, wherein the inert gas is argon gas. (Configuration 10) 3. The method for producing an MIS type semiconductor device according to configuration 1 or 2, wherein the pressure of the atmosphere is atmospheric pressure. Effect of the Invention

[0010] According to the present invention, it is possible to provide a method for manufacturing an MIS-type semiconductor device using a diamond semiconductor that is safe, energy-saving, has high mobility, and is suitable for high-speed operation. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing a structure of an MIS type semiconductor device according to the present invention. [Diagram 2] 1 is a bird's-eye view showing the crystal structures of a semiconductor layer and a gate insulator layer according to the present invention. [Diagram 3] 1A to 1C are cross-sectional views showing a manufacturing process of the MIS type semiconductor device of the present invention; [Figure 4] 1A to 1C are cross-sectional views showing a manufacturing process of the MIS type semiconductor device of the present invention; [Diagram 5] FIG. 2 is a flow chart illustrating the manufacturing process of the MIS type semiconductor device of the present invention. [Figure 6] FIG. 2 is a flow chart illustrating the manufacturing process of the MIS type semiconductor device of the present invention. [Figure 7] 1A is a cross-sectional view showing the structure of the MIS-type semiconductor device of Example 1, in which (a) is a plan view seen from above, (b) is a cross-sectional view taken along the line connecting A and A' in (a), and (c) is a cross-sectional view taken along the line connecting B and B' in (a). [Figure 8] 3A to 3C are cross-sectional views showing the manufacturing process of the MIS type semiconductor device according to the first embodiment. [Figure 9] 3A to 3C are cross-sectional views showing the manufacturing process of the MIS type semiconductor device according to the first embodiment. [Figure 10] 3A to 3C are cross-sectional views showing the manufacturing process of the MIS type semiconductor device according to the first embodiment. [Figure 11] 3A to 3C are cross-sectional views showing the manufacturing process of the MIS type semiconductor device according to the first embodiment. [Figure 12] 3A to 3C are cross-sectional views showing the manufacturing process of the MIS type semiconductor device according to the first embodiment. [Figure 13] 3A to 3C are cross-sectional views showing the manufacturing process of the MIS type semiconductor device according to the first embodiment. [Figure 14] FIG. 2 is a schematic diagram of the configuration of a processing apparatus used in Example 1. [Figure 15] FIG. 2 is a schematic diagram of the configuration of a processing apparatus used in Example 1. [Figure 16] 3 is a top view photograph of the MIS type semiconductor device fabricated in Example 1. [Figure 17] FIG. 3 is a characteristic diagram showing the electrical characteristics of the MIS type semiconductor device fabricated in Example 1. [Figure 18] FIG. 3 is a characteristic diagram showing the electrical characteristics of the MIS type semiconductor device fabricated in Example 1. [Figure 19] FIG. 3 is a characteristic diagram showing the electrical characteristics of the MIS type semiconductor device fabricated in Example 1. [Figure 20] FIG. 3 is a characteristic diagram showing the electrical characteristics of the MIS type semiconductor device fabricated in Example 1. [Figure 21] FIG. 3 is a characteristic diagram showing the electrical characteristics of the MIS type semiconductor device fabricated in Example 1. [Figure 22] FIG. 3 is a characteristic diagram showing the electrical characteristics of the MIS type semiconductor device fabricated in Example 1. [Figure 23]FIG. 3 is a characteristic diagram showing the electrical characteristics of the MIS type semiconductor device fabricated in Example 1. [Figure 24] FIG. 3 is a characteristic diagram showing the electrical characteristics of the MIS type semiconductor device fabricated in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] (Embodiment 1) Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0013] <Concept> As mentioned above, in the case of hydrogen-terminated diamond semiconductors, it has been thought that the electrical conduction near the hydrogen-terminated semiconductor surface requires negative charges attached to the surface of the diamond semiconductor or in the insulating film in contact with the diamond semiconductor. In response to this, the inventors have found that this negative charge is not necessarily required, but rather that the negative charge reduces the mobility of charge carriers through Coulomb scattering and also promotes normally-on operation (i.e., a positive threshold voltage V TH Therefore, by forming an insulating film in contact with the hydrogen-terminated diamond semiconductor without exposing it to the atmosphere after forming the hydrogen-terminated diamond surface, the negative charge density can be reduced, and high carrier mobility (hole mobility) and negative threshold voltage V TH It was found that both of these could be achieved. In the present invention, the threshold voltage V TH is the gate voltage V applied to the gate with respect to the source in an MIS semiconductor device. G Drain current I flowing between the source and drain D The square root of the absolute value of (|I D | 1 / 2 ) characteristic curve is approximated by a straight line, and I D = 0, the gate voltage V G This refers to the value of .

[0014] Here, the material of the gate insulating film is not limited, and examples thereof include a single layer film made of boron nitride, aluminum oxide, silicon oxide, silicon oxynitride, hafnium oxide, titanium oxide, tantalum oxide, yttrium oxide, zirconium oxide, lanthanum aluminum oxide, and calcium fluoride, or a composite film made of these films. Among these, the gate insulating film is preferably boron nitride, more preferably single crystal boron nitride, and even more preferably hexagonal boron nitride (h-BN).When the insulating film is a composite film, the film on the surface in contact with the hydrogen-terminated diamond layer is preferably a film made of boron nitride, more preferably a film made of single crystal boron nitride, and even more preferably a film made of hexagonal boron nitride (h-BN). When boron nitride, preferably single crystal boron nitride, more preferably hexagonal boron nitride (h-BN), is used as the gate insulating film, the hole mobility can be further increased, and the threshold voltage V TH Therefore, the negative voltage becomes larger and the controllability is improved.

[0015] As a result of detailed investigations using experiments and simulations, in the method of the present invention, the negative charges attached to the surface of the diamond semiconductor and in the insulating film in contact with the diamond semiconductor are small in the electrical conduction near the hydrogen-terminated semiconductor surface, the conduction of the diamond semiconductor layer near the hydrogen termination can be controlled by the voltage applied to the gate, and scattering due to negative charges can be suppressed. In addition, for example, when h-BN is used as the gate insulating film, the mobility is 5×10 2 cm 2 V -1 s -1 It was even more expensive than that.

[0016] Threshold voltage V TH In a p-type MIS semiconductor device where the gate voltage V G When is 0, the drain current I D does not necessarily become 0. Gate voltage V G Drain current I D Characteristics are V GIn the case where the change is tailing off near |I D | 1 / 2 The characteristic curve of I D If dissociation occurs near V = 0, G = 0 and the drain current I D Sometimes it flows.

[0017] However, in the configuration of the present invention, when hexagonal boron nitride (h-BN) is used as the gate insulating film, |I D | 1 / 2 The approximate line of |I D | 1 / 2 This agrees well with the actual measurements of V G = 0 and the drain current I D is 4 × 10 -4 mA mm -1 In other words, the MIS semiconductor device of the present invention has a characteristic suitable for energy saving, that is, a normally-off state, in which no current flows when no voltage is applied to the gate electrode. In a standby state in which no voltage is applied to the gate electrode, the drain current I D Since no current flows, it is also safe. In addition, as mentioned above, the high hole mobility reduces the on-resistance, which in turn reduces conduction loss, resulting in energy savings during operation.

[0018] The inventors also formed a gate insulating film in contact with the surface of the hydrogen-terminated diamond semiconductor layer, and TH It has been discovered that one method of making the voltage negative is to use any one of the following atmospheres between the hydrogen-terminated semiconductor layer forming step and the insulator layer forming step: vacuum, hydrogen gas, inert gas, and hydrogen gas with an inert gas added thereto. Note that examples of the steps between the hydrogen-terminated semiconductor layer forming step and the insulator layer forming step include a sample transport step and a sample temporary storage step. Here, as the insulating film, as described above, boron nitride is preferable, single crystal boron nitride is more preferable, and hexagonal boron nitride (h-BN) is even more preferable.

[0019] <Structure and Features> 1, the MIS type semiconductor device 101 of the present invention has a diamond substrate 21, a diamond semiconductor layer 22, a gate insulator layer (gate insulating film) 23, and a conductive layer (gate electrode) 24 as basic components, and also has a source electrode and its wiring 28, a drain electrode and its wiring 29, a gate electrode wiring 27, an insulating film 25, and a low resistance layer 26. At least a first main surface of the diamond semiconductor layer 22 is hydrogen-terminated as described later. Here, even if the substrate is other than diamond, a thin film made of diamond may be formed on the substrate, and this may be used as the diamond semiconductor layer 22. Also, the diamond substrate 21 may be used as the semiconductor layer, and the surface layer of the diamond substrate 21 may be used as the diamond semiconductor layer 22. What is essential is that the semiconductor layer made of diamond is in contact with the gate insulating film 23. Here, the semiconductor layer made of diamond (diamond semiconductor layer) 22 may contain a dopant.

[0020] The present invention relates to an MIS type semiconductor device having a semiconductor layer made of diamond, a material having excellent electrical properties. One of the characteristic features of the structure of the MIS type semiconductor device of the present invention that enhances its effectiveness is that the gate insulator layer 23 is made of boron nitride, more preferably made of single crystal boron nitride, and even more preferably made of hexagonal boron nitride (h-BN).

[0021] Known boron nitride structures include amorphous boron nitride (a-BN) with an amorphous structure, turbostratic boron nitride (t-BN) with a disordered stacking structure in the c-axis direction, cubic boron nitride (c-BN) with a cubic zinc-blende structure, hexagonal boron nitride (h-BN) with a hexagonal graphite structure, and wurtzite boron nitride (w-BN) with a hexagonal wurtzite structure. Of these boron nitrides (BN), hexagonal boron nitride (h-BN) is most preferable for the gate insulator layer 23 from the viewpoint of reducing charge traps in the gate insulator layer 23, and it is more preferable that h-BN is in the form of a single crystal.

[0022] In the MIS-type semiconductor devices (diamond field-effect transistors) using diamond semiconductors reported so far, the gate insulator layer (gate insulating film) is mostly an amorphous film, which is mainly formed by vapor deposition or atomic layer deposition (ALD). The gate insulator layer formed by these methods has a relatively high charge trap density due to atomic vacancies, and a relatively high interface state is formed at the interface with the diamond semiconductor layer. The charge captured in such traps (states) is a factor that reduces the carrier mobility.

[0023] Diamond is made up of a crystal in which each carbon atom is covalently bonded to the four surrounding atoms. On the surface of diamond, there are extra bonds. These dangling bonds are unstable and act as surface states. The dangling bonds can be stabilized by bonding with hydrogen, a state called hydrogen termination. For example, the surface of diamond produced by chemical vapor deposition is hydrogen-terminated because it is exposed to hydrogen plasma during synthesis. Using such a hydrogen-terminated diamond surface can reduce the surface state density on the diamond side. On the other hand, the surface of h-BN has no dangling bonds due to its structure. Therefore, the interface state density at the junction interface between h-BN and hydrogen-terminated diamond is low. Furthermore, the trap density in the insulator layer (insulator film) made of single-crystal h-BN is small. These factors reduce carrier scattering due to charges captured in traps in the insulator layer and interface states.

[0024] In addition, h-BN has a large dielectric breakdown field (parallel to the c-axis) of approximately 12 MV / cm, which induces high-density carriers and results in low on-resistance. Furthermore, the lattice mismatch between h-BN and the hydrogen-terminated diamond (111) surface is approximately 0.7%, which is suitable for forming an interface with few lattice defects and distortion. This also contributes to improving the characteristics of MIS-type semiconductor devices. For reference, a bird's-eye view schematic diagram of the crystal structure of h-BN and hydrogen-terminated diamond crystal (111) is shown in Figure 2. In Figure 2, 11 represents carbon, 12 represents hydrogen, 13 represents boron, and 14 represents nitrogen atoms.

[0025] The gate insulator layer 23 preferably has a thickness of one atomic pair layer of boron and nitrogen or more and 300 nm or less, and more preferably has a thickness of 1 nm or more and 100 nm or less. A dense film with a thickness of one atomic pair or more suppresses leakage current and is more likely to function as a gate insulator layer. A thickness of 1 nm or more is preferable to suppress leakage current, including tunnel current. Furthermore, when the thickness of the gate insulating layer 23 is 300 nm or less, it becomes easier to obtain a sufficient capacitance as an MIS type semiconductor device.

[0026] The diamond semiconductor layer 22 is preferably a single crystal having a (100) or (111) crystal face.

[0027] The density of charged impurities present at the interface between the diamond semiconductor layer 22 and the gate insulator layer 23 (interface concentration) is 0 cm -2 5×10 or more 11 cm -2 Less than or equal to 0 cm, more preferably -2 More than 1×10 11 cm -2 When the density of the charged impurities is within this range, scattering of holes moving through the channel layer formed in the vicinity of the hydrogen-terminated surface of the diamond semiconductor layer 22 by the charged impurities is suppressed, and it is possible to provide the MIS type semiconductor device 101 having high mobility. Here, the MIS semiconductor device 101 induces holes in the channel layer by a negative potential applied to the gate electrode 24. On the other hand, when no voltage is applied to the gate electrode 24, the device is shut off and the MIS semiconductor device 101 operates normally off. When the density of the charged impurities is within the above range, the number of holes induced by the charged impurities is extremely small, and therefore the leakage current between the source and drain when no voltage is applied to the gate electrode 24 is very small.

[0028] The inventors have found that the density of charged impurities can be reduced to 0 cm by a relatively simple process of placing the sample in a vacuum or in an inert gas environment such as Ar gas after the hydrogen termination until the hydrogen-terminated surface is covered with the gate insulating layer 23.-2 5×10 or more 11 cm -2 It has been found that it is possible to keep the density of charged impurities within the above ranges without the need for washing, cleaning, heat treatments and surface treatments.

[0029] Both diamond and h-BN have wide bandgaps (5.47 eV and 5.97 eV), making them suitable for high-temperature operation. The high thermal conductivity of h-BN, 4 W / cm K at room temperature, which is comparable to that of copper, along with the high thermal conductivity of diamond (22 W / cm K at room temperature), contributes to excellent heat dissipation from the channel. In addition, h-BN is known to act as a coating material that prevents oxidation at high temperatures of 1000°C. Therefore, it also functions to protect the hydrogen termination on the diamond surface at high temperatures. On the other hand, the low dielectric constants of diamond and h-BN (5.7 and 5.1 (c-axis parallel)) are desirable properties for high-speed and high-frequency operation.

[0030] It is preferable that the gate insulator layer 23 is in direct contact with the surface of the terminated diamond semiconductor layer 22 without sandwiching a layer of water, hydrocarbon, resist residue, etc. This is because if such a layer is sandwiched, an interface state is likely to occur.

[0031] In a conventional structure using an amorphous film such as Al2O3 as the gate insulator layer 23, there is a tendency for many traps (charge traps) to be contained in the gate insulator layer 23 and at the interface between the gate insulator layer 23 and the diamond semiconductor layer 22. As a result, carrier conduction is scattered, resulting in low carrier mobility. On the other hand, in the structure of the present invention in which boron nitride, preferably single crystal boron nitride, more preferably h-BN, and even more preferably single crystal h-BN is used as the gate insulator layer (gate insulating film), there tends to be fewer charge traps in the gate insulator layer 23. Therefore, carrier conduction is less scattered, and high carrier mobility is obtained.

[0032] The diamond substrate 21 preferably has few crystal defects, high cleanliness, and a flat, smooth surface so that the diamond semiconductor layer 22 formed thereon will be a high-quality crystal with few defects. In addition, in order to reduce the effect of surface roughness scattering, it is preferable that the surface of the semiconductor layer is also flat and smooth.

[0033] The gate electrode 24 has a threshold voltage V TH The conductive material has a work function such that the potential at the surface of the conductive film is negative. Specific examples include conductive films of metals, graphite (C), and polysilicon to which a dopant is added. Metals include copper (Cu), tungsten (W), titanium (Ti), aluminum (Al), chromium (Cr), and tantalum (Ta). In addition, alloys such as AlCu, CuNiFe, and NiCr, silicides and polycides such as WSi and TiSi, WN, TiN, CrN, and Metal compounds such as TaN and the like can also be used. An appropriate material for the gate electrode 24 may be selected from these materials, taking into consideration the electrical conductivity, work function, processability, and the like. In addition, the threshold voltage V TH It depends on the material of the gate electrode 24, the material and thickness of the gate insulator layer 23, the material of the semiconductor channel layer, the impurities and their concentrations, etc. Furthermore, when the MIS semiconductor device of the present invention is used as an integrated circuit, various heat treatments are added as part of the integration, and the materials must be selected taking into consideration the diffusion of the materials in these heat treatments.

[0034] The source electrode and its wiring 28, the drain electrode and its wiring 29, and the gate electrode wiring 27 are made of a conductive film such as metal, graphite, or polysilicon with dopants added. Examples of metals include gold (Au), silver (Ag), Cu, platinum (Pt), palladium (Pd), W, Ti, Al, Cr, and Ta. In addition, alloys such as AlCu, CuNiFe, and NiCr, polycides using W or Ti, and metal compounds such as WN, TiN, CrN, and TaN can also be used. It is preferable that these conductive films can make ohmic contact at the portion in contact with the diamond semiconductor layer 22. For example, it is preferable to use a metal having a high work function such as gold (Au) or palladium (Pd) as the conductive film. These high work function metals have the characteristic that they can make ohmic contact by direct contact. Titanium (Ti) can also be used. Here, it is preferable to anneal Ti to react with diamond and form TiC. On the other hand, since Ti is easily oxidized, when making electrical contact with the diamond semiconductor layer 22, it is preferable to use a conductive film structure in which Ti is laminated from the diamond semiconductor layer 22 side, and a material such as Pt, Au or W is laminated thereon.

[0035] In order to reliably obtain ohmic contact with the source electrode 28 and the drain electrode 29 and to reduce the resistance of the diamond semiconductor layer 22 other than the channel portion, it is preferable to form a low resistance layer 26 at the interface between the diamond semiconductor layer 22 and the source electrode 28 or the drain electrode 29. For example, when the source electrode 28 and the drain electrode 29 are made of Ti, the low resistance layer may be TiC formed by annealing.

[0036] The insulating film 25 provides electrical insulation and prevents the diffusion of moisture and impurities, thereby playing a role in the stable operation of the MIS semiconductor device 101. Examples of materials for the insulating film 25 include a silicon oxide (SiO2) film, a silicon nitride (SiN) film, a silicon oxynitride (SiNO) film, a silicon carbide (SiC) film, a silicon carbonitride (SiCN) film, a silicon carbonitride oxide (SiCNO) film, an alumina (Al2O3) film, a boron nitride (BN) film, and an organic film such as polyimide.

[0037] <Manufacturing method> Next, a manufacturing method of this MIS type semiconductor device 101 will be described with reference to FIGS. 3 and 4 showing a cross-sectional structure and FIG. 5 showing a flow chart. 3(a), a diamond substrate 21 is prepared. As the diamond substrate, for example, one of type Ib or type IIa with a crystal plane of 100 or 111 can be preferably used. Here, the surface of the diamond substrate 21 is preferably flat (planar) and atomically smooth. For the electrical characteristics of a field effect transistor, the flatness and smoothness of the interface between the diamond semiconductor layer 22 and the gate insulator layer 23 are important, but in order to make the flatness and smoothness of the interface sufficiently high, it is necessary to sufficiently increase the flatness, smoothness and cleanliness of the diamond substrate 21 surface.

[0038] Thereafter, as shown in FIG. 3(b), a diamond semiconductor layer terminated with hydrogen is epitaxially grown on the diamond substrate 21 to form a hydrogen-terminated diamond semiconductor layer 22 (S1 in FIG. 5). The hydrogen-terminated diamond semiconductor layer 22 can be formed by, for example, microwave plasma CVD (Chemical Vapor Deposition) using CH4 gas and H2 gas. The thickness of the diamond semiconductor layer 22 is preferably 10 nm or more. If the thickness is 10 nm or more, it is possible to suppress the intrusion of impurities from the substrate, particularly in the case of an Ib substrate.

[0039] The diamond semiconductor layer 22 may be doped with a dopant. An example of a hole-based dopant is boron (B), and an example of an electron-based dopant is phosphorus (P). The amount of dopant added is 10 16 / cm 3 Over 10 19 / cm 3 The following is preferred: 10 16 / cm 3 The effect of doping is small below 10 19 / cm 3 If it exceeds this value, it will cause carrier scattering, resulting in a decrease in performance such as mobility.

[0040] Next, immediately after the surface (at least the first main surface) of the diamond semiconductor layer 22 is hydrogen-terminated, evacuation and / or inert gas replacement is performed so that the environment in which the sample is placed becomes any one selected from the group consisting of vacuum, hydrogen gas, inert gas, and hydrogen gas with an inert gas added thereto (S2 in FIG. 5). Examples of inert gas include noble gases such as Ar gas, Kr gas, and Xe gas, and N2 gas. Here, any one environment selected from the group consisting of vacuum, hydrogen gas, inert gas, and hydrogen gas with an inert gas added thereto is maintained at least until just before the insulating film 23a described below is formed. In this way, the charged impurities at the interface between the diamond semiconductor layer 22 and the insulating film 23a are reduced, and high hole mobility can be obtained.

[0041] In the case where the insulating film 23a is formed in the next process by a process such as CVD, which is performed in a vacuum environment, it is efficient and preferable to keep the sample environment in a vacuum, and in the case where the insulating film 23a is formed by bonding, it is preferable to keep the sample in an inert gas environment from the viewpoint of work efficiency. In addition, Ar gas is the most preferable inert gas, taking into consideration the inertness, the assurance of purity, and the cost.

[0042] When placed in a vacuum, the degree of vacuum is set to 1 x 10, taking into account the effect and the burden on the equipment. -5 A level of Pa is preferred. When an inert gas is used, atmospheric pressure is preferable because of ease of handling. Here, atmospheric pressure refers to pressure in an atmospheric environment including low pressure, high pressure, and high altitude, as well as pressure in a glove box or the like that is pressurized to prevent the inclusion of outside air. In addition, it is preferable that the concentration of oxygen gas (O2 gas) in the environment is 0.5 ppm or less, and the dew point is -80°C or less. The surface of hydrogen-terminated diamond is chemically stable, and in this level of environment, it is possible to obtain a surface state that serves as a semiconductor layer suitable for obtaining high hole mobility with few charged impurities and little scattering of charged impurities.

[0043] After that, as shown in Fig. 3(c), an insulating film 23a is formed on the diamond semiconductor layer 22 terminated with hydrogen or the like (S3 in Fig. 5). Here, as the insulating film 23a, boron nitride is preferable, a single crystal of boron nitride is particularly preferable, h-BN is more preferable, and a single crystal of h-BN is even more preferable. Below, an example in which the insulating film is made of boron nitride, which is highly effective, will be described. The insulating film 23a can be formed by laminating a boron nitride thin film obtained by cleavage, a chemical vapor deposition method such as thermal CVD or plasma CVD, a physical vapor deposition method such as sputtering, a physical chemical vapor deposition method, etc. Specific examples include metal-organic chemical vapor deposition (MOCVD) using triethylborane (TEB) and ammonia (NH3) as source gases and hydrogen (H2) as carrier gas, and molecular beam epitaxy (MBE) using activated nitrogen produced by RF plasma and boron heated and supplied by an electron gun. When the insulating film 23a is formed by bonding a boron nitride thin film obtained by cleavage, the bonding environment is preferably any one selected from the group consisting of vacuum, hydrogen gas, inert gas, and hydrogen gas with inert gas added thereto. That is, the environment for the formation process of the insulating film 23a is preferably any one selected from the group consisting of vacuum, hydrogen gas, inert gas, and hydrogen gas with inert gas added thereto.

[0044] In order to remove adsorbents at the interface between the diamond semiconductor layer 22 and the insulating film 23a and to clean the surface of the insulating film 23a, it is preferable to perform annealing using a mixed gas of an inert gas and hydrogen (H2) gas after forming the insulating film 23a. Here, the inert gas may be, for example, argon (Ar).

[0045] Thereafter, the gate electrode 24 is formed as shown in FIG. 3(d) (S4 in FIG. 5). The gate electrode 24 can be formed by depositing a conductive material constituting the gate electrode 24 on the insulating film 23a by sputtering, vapor deposition, CVD, lamination, or the like, forming a resist pattern by lithography, and then etching the gate electrode 24. Dry etching is preferably used as the etching method from the viewpoint of fine processing, but wet etching can also be used. Wet etching has the advantage that it is easy to suppress damage to the MIS semiconductor device 101 to be fabricated. Alternatively, a resist pattern for lift-off may be formed on the insulating film 23a, and then a conductive material for forming the gate electrode 24 may be deposited by sputtering, evaporation, CVD, or the like, followed by lift-off.

[0046] Here, examples of the sputtering method include DC sputtering and RF sputtering, with RF sputtering being more preferred from the viewpoint of throughput. Examples of the deposition method include thermal deposition and electron beam deposition. When polysilicon is used as the material for the gate electrode 24, the CVD method is preferably used as a method for forming the polysilicon film. At this time, it is preferable to add a dopant such as phosphorus (P) to reduce the resistance.

[0047] Thereafter, an insulating film 25a is formed by a sputtering method, an ALD method, a CVD method, a bonding method, or a coating method such as SOG (Spin on Glass) (FIG. 4(a)). Here, since the formed insulating film 25a often contains voids and undesired water that hinder the stabilization of electrical characteristics, it is preferable to perform annealing.

[0048] Subsequently, desired openings are formed in the insulating film 25a and the gate insulating film 23a by lithography and etching to form the insulating film 25 and the gate insulating layer (gate insulating film) 23, respectively (FIG. 4(b)).

[0049] Thereafter, a low-resistance layer 26 is formed on the exposed surface of the diamond semiconductor layer 22 at the opening, which provides ohmic contact between the electrode and the semiconductor layer and also provides low resistance (FIG. 4(c)). The low-resistance layer 26 can be obtained by depositing a metal that forms a carbide with diamond, such as Ti or Mo, and then forming a metal carbide by annealing. For the hydrogen-terminated semiconductor layer, deposited high-work function metals, such as Au, Pd, and Pt, can be used as the low-resistance layer.

[0050] Thereafter, a conductive film is deposited, and lithography and etching are performed to form a gate electrode wiring 27, a source electrode and its wiring 28, and a drain electrode and its wiring 29 (FIG. 4(d)). The aforementioned low resistance layer 26 may be formed by, for example, annealing the electrodes and / or wiring after they are formed. By the above steps, an MIS type semiconductor device 101 having a diamond semiconductor layer 22 and a gate insulator layer 23 made of h-BN is fabricated.

[0051] The MIS semiconductor device 101 of the present invention has high carrier mobility (hole mobility), consumes little power when off (standby) due to normally-off operation, and has a mutual conductance g m Since the on-resistance is low and the power consumption is low, the semiconductor device is suitable for energy saving. Since the device is not energized during standby, it is also suitable for security. Therefore, the present invention provides a high-performance MIS type semiconductor device that combines high levels of both mobility and carrier density.

[0052] Although the above describes a method for fabricating a single MIS type semiconductor device 101, it is also possible to fabricate an integrated MIS type semiconductor device by mounting a plurality of MIS type semiconductor devices 101 in the same manner. In this case, an insulating layer is provided between each MIS type semiconductor device 101, and element isolation is performed as necessary.

[0053] (Embodiment 2) In the first embodiment, a method for manufacturing the MIS type semiconductor device 101 via the hydrogen-terminated diamond semiconductor layer formation step S1, that is, the step of forming the diamond semiconductor layer 22 terminated with hydrogen on the diamond substrate 21, has been described. In the second embodiment, instead of the hydrogen-terminated diamond semiconductor layer formation step S1, a diamond semiconductor exposed member preparation step S11 and a hydrogen termination treatment step S12 are performed as shown in FIG. 6, and the other steps are performed in the same manner as in the first embodiment to provide an MIS type semiconductor device.

[0054] In the second embodiment, first, a member with exposed diamond semiconductor is prepared (step S11). The member with exposed diamond semiconductor can be a diamond semiconductor substrate, or a member with a part of the first main surface of the diamond semiconductor exposed and a conductive layer or / and an insulating layer for element isolation or the like formed on a part of the first main surface. Thereafter, at least a portion of the exposed diamond semiconductor is hydrogen-terminated (step S12). Hydrogen termination can be performed using plasma or heat treatment under hydrogen gas. For example, a plasma treatment can be performed for 10 minutes using an MP-CVD device under the following conditions: H2 flow rate 500sccm, pressure 4KPa, heater temperature setting 600℃, microwave output 300W. Hereinafter, the vacuum or inert gas environment treatment (S13) may be the same as the vacuum or inert gas environment treatment (S2) in embodiment 1, the boron nitride insulator layer formation process (S14) may be the same as the boron nitride insulator layer formation process (S3) in embodiment 1, and the conductor layer formation process (S15) may be the same as the conductor layer formation process (S4) in embodiment 1. As a result, it is possible to provide an MIS type semiconductor device having the same characteristics as those of the first embodiment. EXAMPLES

[0055] The present invention will be described in more detail below with reference to examples. However, these examples are provided merely to aid in the understanding of the present invention and are not intended to limit the present invention thereto.

[0056] Example 1 <Element structure> The element structure of the MIS type semiconductor device 201 of the first embodiment will be described with reference to Fig. 7, which is a cross-sectional view of the essential parts. Fig. 7(a) is a plan view seen from above, and Fig. 7(b) and Fig. 7(c) are cross-sectional views taken along the lines connecting A and A' and B and B' in Fig. 7(a), respectively. In Fig. 7, the components are simplified by using rectangles, etc., in order to make the configuration easier to understand. This MIS type semiconductor device 201 includes a diamond substrate 31, a hydrogen-terminated layer 32, a gate insulating film 33, and a gate electrode 34. G , source electrode 37 S and drain electrode 37 D , gate electrode wiring 62 G , source electrode wiring 62 S , drain electrode wiring 62 D and insulating film 61. Here, the source electrode 37 S and drain electrode 37 D It is composed of, from the top down, a conductive film 36 made of platinum (Pt) and having a thickness of 5 nm, a conductive film 35 made of Ti and having a thickness of 5 nm, and a low resistance layer 42 made of titanium carbide (TiC) generated at the interface between the diamond substrate 31 and the Ti of the conductive film 35. The gate insulating film 33 is made of hexagonal boron nitride (h-BN) and has a thickness of 23 nm.

[0057] The diamond substrate 31 is formed with a hydrogen termination layer 32 in the channel portion located directly below the gate insulating film 33, a low resistance layer 42 made of TiC located directly below the conductive film 35, and an oxygen termination layer 43 in the remaining surface layer portion.

[0058] Gate electrode 34 G The gate electrode 34 is made of graphite having a thickness of 20 nm. G A gate electrode wiring (bonding pad wiring) 62 in which 10 nm thick Ti and 100 nm thick Au are laminated in sequence on the G is formed.

[0059] The source is a conductive film for ohmic contact made of Ti with a thickness of 5 nm and platinum (Pt) with a thickness of 5 nm (respectively 35 and 36 in FIG. 7) and a source electrode wiring (bonding pad wiring) 62 S Here, the source electrode wiring 62 S The conductive film 35 has a structure in which Ti with a thickness of 5 nm, Pt with a thickness of 5 nm, Ti with a thickness of 10 nm, and Au with a thickness of 100 nm are laminated in that order. In addition, a low resistance layer 42 made of TiC is formed in the boundary region between the conductive film 35 and the diamond substrate 31. Similarly, the drain is formed by a conductive film for ohmic contact made of Ti with a thickness of 5 nm and Pt with a thickness of 5 nm (respectively 35 and 36 in FIG. 7) and a drain electrode wiring (bonding pad wiring) 62 D Here, the drain electrode wiring 62 D The conductive film 35 has a structure in which 5 nm thick Ti, 5 nm thick Pt, 10 nm thick Ti, and 100 nm thick Au are sequentially laminated, and a low resistance layer 42 made of TiC is formed in the boundary region between the conductive film 35 and the diamond substrate 31.

[0060] In addition, the channel layer 32 is connected to the gate electrode wiring (bonding pad wiring) 62 G The gate electrode wiring 62 is sufficiently insulated from the G An insulating film 61 for element isolation is formed so as to cover an edge portion (the boundary between the oxygen-terminated and hydrogen-terminated regions) 71 of the gate insulating film 33 where the oxide is formed. The insulating film 61 is also made of hexagonal boron nitride (h-BN) and has a thickness of 63 nm.

[0061] <Production method> The device fabrication process will be described below with reference to the cross-sectional views of Figures 8 to 13. Figures 8-10 are cross-sectional views taken along the line connecting A and A' in Figure 7(a), and Figures 11-13 are cross-sectional views taken along the line connecting B and B' in Figure 7(a).

[0062] 1. Substrate Preparation A high-temperature, high-pressure synthesis IIa (111) diamond single crystal substrate manufactured by the TISNCM Institute in Russia was prepared as the diamond substrate 31, and the substrate was cleaned by a conventional method using hot mixed acid and organic cleaning. The size of the diamond substrate 31 used here was 2.5 mm × 2.5 mm × 0.3 mm.

[0063] 2. Creation of alignment marks An alignment mark (not shown) was formed on the diamond substrate 31 by laser lithography. The process of forming the alignment marks will now be described. First, the surface of the diamond substrate 31 was spin-coated with a lower layer resist PMGI-SF6S (manufactured by Microchem) and baked at 180° C. for 5 minutes. Then, a photoresist AZ-5214E ​​(manufactured by Merck Performance Materials) was spin-coated and baked at 110° C. for 2 minutes. Next, an alignment mark pattern was written using a high-speed maskless exposure device (DL-1000 / NC2P, manufactured by Nano System Solutions). After developing with 2.38% TMAH (tetramethylammonium hydroxide) for a total of 150 seconds, the substrate was washed with pure water for a total of 120 seconds, and then nitrogen was blown.

[0064] Thereafter, Ti to a thickness of 10 nm, Pt to a thickness of 15 nm, Au to a thickness of 60 nm, and Pt to a thickness of 25 nm were successively deposited by an electron gun type deposition apparatus. Thereafter, the sample was immersed in NMP heated in a water bath set to 80°C, and lift-off was performed. Finally, the diamond substrate 31 was rinsed with acetone and IPA, and then nitrogen was blown to form alignment marks at predetermined positions on the diamond substrate 31.

[0065] 3. Ohmic Electrode Fabrication An electron beam resist gL-2000DR2.0 (manufactured by Gluon Lab) was spin-coated on the diamond substrate 31 and baked at 180° C. for 5 minutes. Then, Espacer 300Z (Showa Denko) was spin-coated, and a pattern of an ohmic electrode was drawn using a 100 kV electron beam lithography system (Elionix, ELS-7000). After drawing, the substrate was washed with pure water for 60 seconds to remove the Espacer, and then nitrogen was blown. Then, the substrate was developed with xylene for 60 seconds, washed with IPA for 60 seconds, and nitrogen was blown to form a resist pattern 51 on the diamond substrate 31 (Fig. 8(a), Fig. 11(a)).

[0066] Next, a conductive film 35a made of Ti and having a thickness of 5 nm and a conductive film 36a made of Pt and having a thickness of 5 nm were sequentially deposited by an electron gun type deposition apparatus (FIGS. 8(b) and 11(b)). After that, the sample was immersed in NMP heated in a water bath set to 80°C and lifted off. After rinsing with acetone and IPA, nitrogen was blown. Thereafter, annealing was performed for 35 minutes in an H2 atmosphere (H2 flow rate 500sccm, pressure 80Torr) in an MPCVD apparatus (Seki Technotron, AX5200-S), forming a low resistance layer 42 made of TiC at the interface between the diamond and Ti (Fig. 8(c), Fig. 11(c)). The set temperature during annealing was raised to 650°C in approximately 31 minutes, and held at 650°C for 35 minutes.

[0067] 4. Hydrogen termination of diamond surface and removal of resist residue Following the formation of the ohmic electrodes, the diamond was exposed to hydrogen plasma for 10 minutes in an MPCVD apparatus (AX5200-S, manufactured by Seki Technotron) to hydrogen-terminate the surface and remove the resist residue, thereby forming a hydrogen-terminated layer 32 on the exposed surface of the diamond substrate 31 (FIG. 8(d), FIG. 11(d)). The hydrogen plasma conditions were: H2 flow rate 500 sccm, pressure 30 Torr, heater set temperature 600°C, and microwave output 300W. Furthermore, annealing was performed for 35 minutes in a H2 atmosphere (H2 flow rate 500sccm, pressure 80Torr) in another MPCVD device (Seki Technotron, AX5000) that can be connected to a vacuum transfer chamber. The set temperature during annealing was raised to 710°C in approximately 34 minutes and held at 710°C for 35 minutes. The diamond was exposed to hydrogen plasma for 10 minutes in an MPCVD apparatus (Seki Technotron, AX5000) to remove the surface adsorbates. The hydrogen plasma conditions were H2 flow rate 500sccm, pressure 30Torr, heater temperature setting 670℃, and microwave output 300W.

[0068] Subsequently, the diamond substrate 31 that had been subjected to the hydrogen plasma treatment was transferred to a glove box with an argon gas atmosphere through a sample transfer path that was kept in vacuum, without being exposed to the atmosphere. The details will be explained below with reference to Figures 14 and 15, which are cross-sectional diagrams of the apparatus configuration.

[0069] FIG. 14 is a cross-sectional view showing an outline of a processing apparatus 1001 for performing hydrogen plasma processing. The main components of the processing apparatus 1001 are a hydrogen termination treatment chamber 1011 and a sample transfer and temporary storage chamber 1025. The processing apparatus 1001 is broadly divided into a hydrogen termination processing section E1 mainly composed of the hydrogen termination treatment chamber 1011, and a sample transfer section E2 mainly composed of the sample transfer and temporary storage chamber 1025, and the sections E1 and E2 can be separated beyond a gate valve 1024 (the connection between the gate valve 1024 and the transfer intermediate chamber 1027).

[0070] The hydrogen termination treatment chamber 1011 is connected to a sample transfer / temporary storage chamber 1025 via two gate valves 1024 and 1026 and a transfer intermediate chamber 1027, and a sample rod 1029 allows the sample to be transferred from the hydrogen termination treatment chamber 1011 to the sample transfer / temporary storage chamber 1025. Here, the transfer intermediate chamber 1027 is provided with a flange 1028 for connecting a vacuum exhaust system, and is closed by the flange (blank flange) 1028 when the vacuum exhaust system is not connected. Also, a turbo exhaust set 1075 is connected to the sample transfer / temporary storage chamber 1025 via a pipe 1071, a valve 1072, a flange 1073, and a bellows pipe 1074. Here, the turbo exhaust set 1075 is a T-Station 75D (manufactured by Edwards) consisting of a turbo molecular pump and a diaphragm pump.

[0071] The hydrogen termination treatment chamber 1011 is a treatment chamber for hydrogen-terminating the exposed surface of the first main surface (diamond semiconductor layer) of the diamond substrate 31 by hydrogen plasma, and specifically is the treatment chamber of the above-mentioned MPCVD apparatus (AX5000, manufactured by Seki Technotron). The hydrogen termination treatment chamber 1011 is connected to a turbo pump (STP-iX455, manufactured by Edwards) 1013 via a gate valve 1012, and the turbo pump 1013 is connected to a scroll pump (nXDS15i, manufactured by Edwards) 1016 via a valve 1014 and piping 1015. This results in a so-called oil-free vacuum pump configuration. The degree of vacuum in 1011 can be read by a vacuum gauge 1063 (ionization vacuum gauge TG200, manufactured by Ampere).

[0072] The hydrogen termination chamber 1011 is also provided with an exhaust path connected to a scroll pump 1016 via a valve 1017 and a pipe 1018 for the purpose of rough vacuum evacuation. For hydrogen termination control, valves 1019 and 1061 and a pipe 1062 are provided, through which the hydrogen termination chamber 1011 and the scroll pump 1016 are connected. The hydrogen termination treatment chamber 1011 is designed so that a process gas (H 2 gas) 1023 can be introduced through a valve 1022. The hydrogen termination chamber 1011 is also equipped with a Baratron vacuum gauge 1020 for monitoring the pressure inside the chamber 1011 when hydrogen termination is being performed.

[0073] FIG. 15 is a cross-sectional view showing an outline of a processing apparatus 1002 used in attaching an insulating film 33a made of h-BN to a sample. The processing apparatus 1002 mainly comprises a bonding processing chamber (glove box) 1031 and a sample transfer / temporary storage chamber 1025. The sample transfer section E2, which mainly comprises the sample transfer / temporary storage chamber 1025, is connected to a bonding processing section E3 via a gate valve 1043, so that the sample can be transferred to the bonding processing chamber (glove box) 1031 without being exposed to the atmosphere.

[0074] Here, a vacuum exhaust system E4 is connected via a flange 1028 so that the sample is not exposed to the atmosphere in the transfer intermediate chamber 1027 when the sample is transferred from the sample transfer / temporary storage chamber 1025 to the bonding processing chamber (glove box) 1031. The vacuum exhaust system E4 includes a chamber 1101 equipped with bellows piping 1109, 1111, a valve 1110, and a vacuum gauge (crystal / cold cathode combination gauge CC-10, manufactured by Tokyo Denshi) 1112, an angle valve 1102, a turbo pump (nEXT300D, manufactured by Edwards) 1103, a valve 1104, piping 1107, and a scroll pump (nXDS15i, manufactured by Edwards) 1105, and further includes piping 1107 and a valve 1106 for roughing the chamber 1101 with the scroll pump 1105.

[0075] The bonding process chamber 1031 is a process chamber in which an h-BN insulating film that becomes the insulating film 33a is bonded to the sample, and is connected to a pass box 1034 via a partition door 1032, and the pass box 1034 is connected to a scroll pump (nXDS15i, manufactured by Edwards) 1037 via a valve 1035 and a pipe 1036. The bonding process chamber 1031 is provided with a pipe and a valve 1038 for enabling direct evacuation by the scroll pump 1037, and the pass box 1034 is provided with a pressure gauge 1039.

[0076] The bonding process chamber 1031 is filled with an inert gas (Ar gas) at atmospheric pressure. Ar gas is supplied from an Ar gas cylinder 1052 to the bonding processing chamber 1031 and the pass box 1034 through a pipe 1053. Here, the pipe 1053 leading to the bonding processing chamber 1031 and the pass box 1034 is provided with valves 1054 and 1055, respectively. This Ar gas is constantly purified by an inert gas circulation refiner 1040 connected to the bonding processing chamber 1031 via pipes 1042, 1045 and valves 1041, 1044, and is kept at an oxygen concentration of 0.5 ppm or less and a dew point of −79° C. or less. This purified Ar gas can be introduced into the sample transport part E2 via a vacuum exhaust system E4 connected via a valve 1108. The bonding processing chamber 1031 is a so-called glove box, and is provided with butyl rubber gloves for performing bonding work while isolating the atmosphere from the outside. The bonding processing chamber 1031 is also connected to an Ar gas cylinder 1052 via a valve 1054, and to a scroll pump 1037 via a valve 1038, so that the pressure inside the bonding processing chamber 1031 can be adjusted when the hand is put in the glove. Furthermore, a microscope (not shown) is provided, and bonding work on the order of microns can be performed in an environment that is isolated from the outside in terms of atmosphere (gas). The image of the microscope can be observed on a monitor outside the bonding processing chamber 1031 without damaging the inert gas environment. The outer wall of the bonding processing chamber 1031 is made of stainless steel and glass, and the internal volume of the bonding processing chamber 1031 is about 310 liters.

[0077] The steps after hydrogen termination and before h-BN bonding are shown below. First, in a pre-processing step, the gate valves 1012, 1024, 1026 and the valve 1014 are opened, and the hydrogen termination treatment chamber 1011, the intermediate transfer chamber 1027 and the sample transfer / temporary storage chamber 1025 are evacuated using the turbo pump 1013 and the scroll pump 1016. The vacuum at this time is 3×10 as measured by the vacuum gauge 1063. -5 Pa or less. Thereafter, the gate valves 1012, 1024, 1026 and the valve 1014 were closed, and the valves 1022, 1019, 1061 were opened to perform the above-mentioned hydrogen termination treatment. During this treatment, the valves 1072 and 1026 were opened, and the sample transfer / temporary storage chamber 1025 and the transfer intermediate chamber 1027 were evacuated to a vacuum using the turbo exhaust set 1075.

[0078] After the hydrogen termination treatment was completed, the valves 1022 and 1019 were closed, the gate valve 1012 and the valve 1014 were opened, and the hydrogen termination treatment chamber 1011 was evacuated to a vacuum using the turbo pump 1013 and the scroll pump 1016 . After that, the valve 1072 was closed, and the turbo exhaust set 1075 was shut down. Also, the bellows piping 1074 was removed. The gate valves 1024 and 1026 were opened, and the sample was moved to the sample transfer / temporary storage chamber 1025 using the sample transfer rod 1029. Then, when the transfer was completed, the gate valve 1026 was closed. Thereafter, the gate valve 1012 was closed, and the valve 1022 was opened to introduce Ar gas to set the pressure in the hydrogen termination treatment chamber 1011 and the intermediate transfer chamber 1027 to atmospheric pressure, and then the valve 1024 was closed.

[0079] Thereafter, the sample transfer unit E2 was separated from the hydrogen termination unit E1 at the connection between the gate valve 1024 and the transfer intermediate chamber 1027, and the sample transfer unit E2 was connected to the bonding unit E3 at the gate valve 1043. The vacuum exhaust system E4 was connected to the sample transport section E2 at the flange 1028, and the transport intermediate chamber 1027 was evacuated by the turbo pump 1103 and the scroll pump 1105. The vacuum was 1×10 -3When the pressure dropped to below 1 Pa, the gate valve 1026 was opened. After the angle valve 1102 was closed, Ar gas was introduced into the transfer intermediate chamber 1027 and the sample transfer / temporary storage chamber 1025 via the bellows piping 1111, the valves 1108 and 1110, the chamber 1101, and the bellows piping 1109. Here, the bonding processing chamber (glove box) 1031 to which the bellows piping 1111 is connected is filled with Ar gas in a purified state at atmospheric pressure by the Ar gas cylinder 1052 and the inert gas circulation refiner (Ar gas circulation refiner) 1040.

[0080] Thereafter, the gate valve 1043 was opened, and the sample transport rod 1029 was operated to transport the sample to the bonding processing chamber 1031. Then, the gate valve 1043 was closed. After this, the h-BN was attached as shown below.

[0081] 5. Attachment of h-BN (hexagonal boron nitride) The sample, whose exposed first main surface of the diamond substrate 31 was hydrogen-terminated in the hydrogen termination chamber 1011 as described above, was transferred to the glove box 1031 filled with Ar gas via the sample transfer / temporary storage chamber 1025 maintained in vacuum. In this state, the oxygen concentration in the glove box 1031 was 0.6 ppm or less, and the dew point was -79°C or less.

[0082] Single crystal h-BN (synthesized at the National Institute for Materials Science) was cleaved by the Scotch tape method in a glove box 1031. The cleaved h-BN was transferred onto PDMS (Polydimethylsiloxane) attached to an acrylic substrate. The h-BN on the PDMS film was aligned with the diamond channel region using an optical microscope, and then the h-BN and diamond were bonded together to form an insulating film 33a (Figures 9(a) and 12(a)). Here, it took about 2 hours from the time the sample was transported to the glove box 1031 until the bonding of the h-BN was completed. Then, annealing was performed in a glove box using the following sequence: heating from 20°C to 100°C in 16 minutes, holding at 100°C for 30 minutes, heating to 200°C in 20 minutes, holding at 200°C for 30 minutes, and heating to 300°C in 20 minutes, holding at 300°C for 3 hours.

[0083] 6. Graphite Paste Graphite (Kish graphite, CoorsTek) was cleaved by the Scotch tape method in a glove box 1031. The cleaved graphite was transferred onto the PDMS attached to an acrylic substrate. The graphite on the PDMS film was aligned with the channel region of the diamond using an optical microscope, and the graphite was attached onto the h-BN / diamond. Then, annealing was performed in a glove box 1031. In this case, the following sequence was used: heating from 20° C. to 100° C. in 16 minutes, holding at 100° C. for 30 minutes, heating to 200° C. in 20 minutes, holding at 200° C. for 30 minutes, and heating to 300° C. in 20 minutes, holding at 300° C. for 1 hour.

[0084] 7. Formation of gate electrode After removing the sample from the glove box 1031, a Hall bar pattern was written by the above-mentioned electron beam lithography method. Here, PMMA-A6 (Microchem) was used as the resist, a 125 kV electron beam lithography system (Elionix, ELS-F125) was used for writing, and a mixture of MIBK (methyl isobutyl ketone):IPA = 1:3 was used as the developer. After that, the graphite was dry etched for 3 minutes using a CCP-RIE device, except for the area that was to become the gate electrode. The plasma conditions were N2 flow rate 96sccm, CHF3 flow rate 2sccm, O2 flow rate 2sccm, pressure 10Pa, and RF output 35W. During this etching, the h-BN was etched partway in the thickness direction. Thereafter, the sample was placed in acetone to remove the resist used as an etching mask. After cleaning with IPA, nitrogen was blown onto the sample to remove the gate electrode 34 made of graphite. GDuring this etching, the exposed region of the first main surface of the diamond substrate 31 is oxidized to form an oxygen-terminated layer 43a (FIG. 9(b), FIG. 12(b)).

[0085] 8. Shaping h-BN Gate electrode 34 G After forming the resist pattern 52, a resist pattern 52 was formed by the above-mentioned laser lithography (FIG. 9(c), FIG. 12(c)). The resist was a single layer of AZ-5214E. Then, the h-BN was dry etched for 3 minutes using a CCP-RIE device. The plasma conditions were N2 flow rate 96 sccm, CHF3 flow rate 2 sccm, O2 flow rate 2 sccm, pressure 10 Pa, and RF power 35 W. The sample was then placed in acetone to remove the resist used as an etching mask. During this etching, the oxygen termination layer 43a was further oxidized, and the oxygen termination layer 43a was changed into a densely oxidized oxygen termination layer 43 (Figures 9(d) and 12(d)).

[0086] 9. Attachment of h-BN for element isolation The gate electrode 34 is formed by the above-mentioned bonding method. G Gate electrode wiring 62 from G The gate electrode wiring 62 is disposed so as not to come into electrical contact with the hydrogen-terminated channel portion 32. G The h-BN (61) for coating was attached to the boundary 71 between the oxygen-terminated and hydrogen-terminated regions to prevent contact (Figures 10(a) and 13(a)).

[0087] 10. Wiring Preparation Using the above-mentioned laser lithography, the gate electrode wiring (62 G ), source electrode wiring (62 S ), drain electrode wiring (62 D ) and a resist pattern 53 for forming each of the bonding pads. The resist is a single layer of AZ-5214E. Thereafter, Ti with a thickness of 10 nm and Au with a thickness of 100 nm were sequentially evaporated using an electron gun type evaporation device, and a conductive film 62a made of Ti and Au was deposited (FIG. 10(b), FIG. 13(b)). Thereafter, the sample is immersed in acetone to perform lift-off, rinsed with IPA, and then dried by nitrogen blowing to form a gate electrode wiring 62 having a bonding pad. G , source electrode wiring 62 S and drain electrode wiring 62 D Thus, an MIS type semiconductor device 201 having the above-mentioned structure was fabricated (FIG. 10(c), FIG. 13(c)). For reference, FIG. 16 shows an optical microscope photograph of the fabricated MIS type semiconductor device 201 taken from above.

[0088] <Electrical characteristics> The electrical characteristics of the FET (field effect transistor) of the MIS type semiconductor device 201 fabricated by the above-mentioned method were investigated. Here, the measuring instruments used were a source measure unit B2901A (manufactured by Keysight Technologies), a function generator 33220A (manufactured by Agilent Technologies), amplifiers 1201 and 1211 (manufactured by DL Instruments), and a digital voltmeter 34401A (manufactured by Agilent Technologies). In addition, Hall effect measurements were performed using a cryogen-free cooling device (manufactured by Niki Kogei) equipped with a superconducting magnet and the above-mentioned measuring instruments.

[0089] The measurement data of the gate voltage and Hall mobility are shown in Figure 17, and the measurement data of the gate voltage and Hall sheet carrier density are shown in Figure 18. Here, the thickness of the gate insulating film made of h-BN is 23 nm, and the measurement temperature is 300K. From Figure 17, 600 cm 2 V -1 s -1 It was confirmed that a high Hall mobility exceeding Also, from FIG. 18, the gate electrode 34 G As a negative voltage is applied to the gate electrode 34, the Hall sheet carrier density increases linearly.G When the voltage applied to is -10V, it is 6×10 12 cm -2 It has been demonstrated that a high Hall sheet carrier density exceeding

[0090] Based on the data in Figures 17 and 18, the relationship between the Hall density and the Hall mobility is plotted in Figure 19. The figure also shows the case where the environment is air after the hydrogen termination of the exposed surface of the diamond substrate 31 until the insulating film 33a (h-BN) is bonded, as well as the data disclosed in Non-Patent Document 5 (not necessarily data obtained from Hall effect measurement). In addition, the figure also shows a theoretical curve of the Hall density dependence of the Hall mobility due to the effects of acoustic phonons, surface roughness, surface charge impurities, and the sum of them. Here, the details of the method of calculating the theoretical curve are described below.

[0091] From the following equations (A1)-(A3), the relaxation time τ due to scattering due to negative charges on the surface, acoustic phonon scattering, and surface roughness scattering is imp , τ ac , τ r The relaxation time τ due to all of these scatterings was calculated using the following formula (A4). Here, formulas (A1)-(A4) are based on formulas (1), (2), (4) and (5) in Non-Patent Document 6, respectively. However, unlike Non-Patent Document 6, calculations were performed for the heavy hole band, the light hole band and the spin-orbit split-off band. In addition, a distinction was made between the effective mass being parallel to the surface and being perpendicular to the surface. As with the sample we prepared, the surface of the diamond is considered to be (111). The mobility of each is given by μ HH =eτ HH / m c HH* , μ LH =eτ LH / m c LH* , μ SO =eτ SO / m c SO* More calculated.

[0092]

number

[0093] where is the reduced Planck constant, n imp (2D) is the surface charge impurity concentration, m c * is the effective mass parallel to the surface, m z * is the effective mass perpendicular to the surface, e is the elementary charge, k F is the Fermi wave vector, ε0 is the vacuum dielectric constant, ε S is the relative dielectric constant of diamond, q is the two-dimensional wave vector, d is the distance from the surface where the surface charged impurity exists, and q TF is the Thomas-Fermi wave number, p s2D is the two-dimensional hole gas sheet density, k B is the Boltzmann constant, ρ is the crystal mass density, u l is the longitudinal acoustic phonon velocity, T is the temperature, Δ is the root mean square surface roughness, L is the transverse relaxation length of the surface roughness, and D ac is the acoustic deformation potential.

[0094] The theoretical curves of the mobility μ and carrier density n shown in Fig. 19 were obtained from the following equations (A5) and (A6). Considering that the mobility and carrier density were obtained from the Hall effect in a low magnetic field in the experiment, the following equations for the mobility and carrier density in a low magnetic field were used. μ =(n HH μ HH 2 +n LH μ LH 2 +n SO μ SO 2 ) / (n HH μ HH +n LH μ LH +n SO μ SO ) (A5) n = (n HH μ HH +n LH μLH +n SO μ SO ) 2 / (n HH μ HH 2 +n LH μ LH 2 +n SO μ SO 2 ) (A6) where n HH , n LH , n SO are the areal carrier densities of holes belonging to the heavy hole band, the light hole band, and the spin-orbit split-off band, respectively. For a certain total carrier density, n HH , n LH , n SO The distribution of the electrons in the electron beam was calculated by simultaneously solving the Schrödinger equation and the Poisson equation using the following equations (A7)-(A10).

[0095]

number

[0096] Here, i represents any of the states in the heavy hole band HH, the light hole band LH, or the spin-orbit split-off band SO. m z i is the effective mass in the direction normal to the surface (m z HH* , m z LH* , m z SO* ), m / / i is the effective mass parallel to the surface (m c HH* , m c LH* , m c SO* ), eφ(z) is the potential energy, E n i is the eigenenergy (i=HH, LH, SO, the highest energy of the nth subband), Ψn i is the specific energy E n i The wave function normal to the surface, E F is the Fermi level, n n i is the surface carrier density of holes filling the nth subband of i=HH, LH, SO, and n 2D is the total hole carrier density.

[0097] The parameters used in the calculation are as follows: Temperature T=300K Dielectric constant of diamond ε S =5.7 Density ρ=3515 kgm -3 Longitudinal acoustic phonon velocity u l =17536ms -1 Deformation potential D ac =8eV Root mean square (RMS) surface roughness Δ=0.25nm Lateral relaxation length of surface roughness L=2nm Distance from surface of negative charge d=0 Effective mass m parallel to the surface c * Heavy hole band m c HH* =0.299m0 Light hole band m c LH* =0.503m0 Spin-orbit split-off band m c SO* =0.375m0 (m0 is the rest mass) Effective mass normal to the surface m z * Heavy hole band m z HH* =0.763m0 Light hole band m z LH* =0.248m0 Spin-orbit split-off band m z SO* =0.375m0 Spin-orbit gap energy Δ SO =6 meV Donor density N D =1.76×10 16 cm -3 (0.1 ppm)

[0098] As shown in FIG. 19, a FET (MIS-type semiconductor device) fabricated using hydrogen-terminated diamond as the semiconductor layer and h-BN as the gate insulating film 33, with the environment from the formation of the hydrogen-terminated layer to bonding the h-BN under vacuum and atmospheric Ar gas pressure, had a 2×10 11 cm -2 From 6×10 12 cm -2 In the Hall density region, 5×10 2 cm 2 V -1 s -1 It can be seen that a high Hall mobility of 1000 nm or more can be obtained. This Hall mobility is about twice as high as that of an FET fabricated under atmospheric conditions from the formation of the hydrogen-terminated layer to the bonding of h-BN with the same structure. In addition, it is significantly higher than the mobility of diamond FETs reported so far (disclosed in Non-Patent Document 5 (shown in FIG. 19)) and the mobility of surface conduction of hydrogen-terminated diamond exposed to the atmosphere. In addition, when comparing the simulation results calculated by taking into account the effects of acoustic phonons, surface roughness, and surface charge impurities with the experimental results, the experimental results for the FET of the present invention show that the surface charge impurities are 5×10 11 cm -2 This shows that the surface charge impurities of the FET in Example 1, which was fabricated using hydrogen-terminated diamond as the semiconductor layer of the present invention, h-BN as the gate insulating film 33, and was fabricated under the conditions of vacuum and atmospheric Ar gas from the formation of the hydrogen-terminated layer until bonding of the h-BN, was approximately 5×10 11 cm -2It is considered that the surface charge impurity is 1×10 11 cm -2 If the above is reduced to 2 x 10 11 cm -2 From 6×10 12 cm -2 In the carrier density region of 1×10 3 cm 2 V -1 s -1 It has been theoretically calculated that a high mobility of at least 100 nm can be obtained. The FET of Example 1 has a carrier density of 10 12 ~10 13 cm -2 In this region, the mobility is less suppressed by the surface charges present at the interface between the diamond semiconductor layer 22 and the gate insulator layer 23, and the high mobility characteristic of the diamond semiconductor material can be fully utilized, resulting in high mobility.

[0099] FIG. 20 shows the drain voltage dependence of the drain current density of the fabricated MIS type semiconductor device 201. G is 8μm, gate width L W The thickness of the gate insulating film 33 made of h-BN is 23 nm. The measurement temperature is 300 K, and the gate voltage V G was set to -10 V. Although slight hysteresis was observed, good FET operation was obtained for the p-type.

[0100] Figure 21 shows the source-drain voltage V DS Drain current density at -10V gate voltage V G The dependence of gate length L G , gate width L W The thickness of the gate insulating film 33 and the measurement temperature are the same as those in FIG. 20. From this result, a high ON / OFF ratio of six orders of magnitude or more is obtained, and the gate voltage V G When the voltage is 0V, the drain current density is 4×10 -4 mA mm -1 It was confirmed that the fabricated MIS type semiconductor device 201 was a FET with low power consumption.

[0101] Figure 22 shows the mutual conductance g m Gate voltage V G In this case, the gate length L G , gate width L W , the thickness of the gate insulating film 33, and the source-drain voltage V DS The measurement temperature is the same as that in FIG. 21. The fabricated MIS semiconductor device 201 has a good transconductance g m It can be seen that the above characteristics are obtained.

[0102] Figure 23 shows the gate voltage V G and the drain current I D Based on the measured data, the square root of the drain current |I D | 1 / 2 Gate voltage V G The plot of the dependence is shown in FIG. 24. Here, the gate length L G is 8μm, gate width L W The thickness of the gate insulating film 33 made of h-BN is 23 nm. The measurement temperature is 300 K, and the drain voltage V D was set to -10V. From this result, the threshold voltage V TH was calculated to be −0.792 V, proving that the MIS type semiconductor device 201 fabricated in Example 1 performs a normally-off operation. [Industrial Applicability]

[0103] The present invention makes it possible to provide a method for manufacturing an MIS-type semiconductor device that has high carrier mobility (hole mobility) and low power consumption in standby mode, thereby contributing to energy conservation, by using a diamond semiconductor that has excellent material properties such as pressure resistance and heat resistance. Therefore, the present invention paves the way for semiconductor devices capable of handling high power, high frequency, and high temperatures, such as logic circuits that can be used in high temperature environments, and power devices such as inverters that can be used in high temperature environments, and is expected to be widely used in industry. [Explanation of symbols]

[0104] 11: Carbon 12: Hydrogen 13: Boron 14: Nitrogen 21: Diamond substrate 22: Diamond semiconductor layer 23: Gate insulator layer (gate insulating film) 23a: insulating film 24: Conductive layer (gate electrode) 25: Insulating film 25a: Insulating film 26: Low resistance layer 27: Gate electrode wiring 28: Source electrode and its electrode wiring 29: Drain electrode and its electrode wiring 31: Diamond substrate 32: Hydrogen-terminated layer 33: Gate insulating film (gate insulator h-BN) 33a: insulating film 34 G : Gate electrode (graphite) 35: Conductive film 35a: Conductive film 36: Conductive film 36a: Conductive film 37 S : Source electrode 37 D :Drain electrode 42: Low resistance layer 43: Oxygen-terminated layer 43a: Oxygen-terminated layer 51, 52, 53: Resist pattern 61: Insulating film (h-BN for element isolation) 62: Conductive film (electrode wiring) 62a: Conductive film 62 G : Gate electrode wiring (bonding pad wiring) 62 S : Source electrode wiring (bonding pad wiring) 62 D :Drain electrode wiring (bonding pad wiring) 71: Boundary between oxygen-terminated and hydrogen-terminated regions 101: MIS type semiconductor device 201: MIS type semiconductor device 1001: Processing device 1002: Processing device 1011: Hydrogen termination chamber 1012: Gate valve 1013: Turbo pump 1014: Valve 1015:Plumbing 1016:Scroll pump 1017: Valve 1018:Plumbing 1019: Valve 1020: Baratron vacuum gauge 1022: Valve 1023: Process gas 1024: Gate valve 1025: Sample transport and temporary storage room 1026: Gate valve 1027: Transport intermediate room 1028: Flange 1029: Sample transport rod 1031: Bonding processing room (glove box) 1032: Partition door 1034: Pass box 1035: Valve 1036:Plumbing 1037:Scroll pump 1038: Valve 1039: Pressure gauge 1040: Inert gas circulation refiner (Ar gas circulation refiner) 1041: Valve 1042:Plumbing 1043: Gate valve 1044: Valve 1045:Plumbing 1052: Ar gas cylinder 1053:Plumbing 1054: Valve 1055: Valve 1061: Displacement control valve 1062:Plumbing 1063: Vacuum gauge 1071:Plumbing 1072: Valve 1073: Flange 1074: Bellows piping 1075: Turbo exhaust set 1101: Chamber 1102: Angle valve 1103: Turbo pump 1104: Valve 1105:Scroll pump 1106: Valve 1107:Plumbing 1108: Valve 1109: Bellows piping 1110: Valve 1111: Bellows piping 1112: Vacuum gauge E1: Hydrogen termination treatment area E2: Sample transport section E3: Lamination processing section E4: Vacuum exhaust system

Claims

1. forming a semiconductor layer having a first major surface comprised of hydrogen-terminated diamond; forming an insulator layer in contact with at least a portion of the hydrogen-terminated surface of the semiconductor layer; forming a conductive layer over at least a portion of the insulating layer; an atmosphere during the period from immediately after forming the semiconductor layer to immediately before forming the insulator layer is any one selected from the group consisting of a vacuum, hydrogen gas, an inert gas, and hydrogen gas to which an inert gas has been added; A method for manufacturing a MIS type semiconductor device, wherein a density of charged impurities present at the interface between the semiconductor layer and the insulator layer is 0 cm -2 or more and 5 x 10 11 cm -2 or less.

2. forming a semiconductor layer having a first major surface comprised of hydrogen-terminated diamond; forming an insulator layer in contact with at least a portion of the hydrogen-terminated surface of the semiconductor layer; forming a conductive layer over at least a portion of the insulating layer; an atmosphere during the period from immediately after forming the semiconductor layer to immediately before forming the insulator layer is any one selected from the group consisting of hydrogen gas, an inert gas, and hydrogen gas to which an inert gas has been added; The pressure of the atmosphere is atmospheric pressure.

3. preparing a member having a first main surface on which at least a portion of a semiconductor layer made of diamond is exposed, and at least a portion of the semiconductor layer is hydrogen-terminated; forming an insulator layer in contact with at least a portion of the hydrogen-treated portion of the semiconductor layer; forming a conductive layer over at least a portion of the insulating layer; the hydrogen-terminated semiconductor layer is placed in an atmosphere selected from the group consisting of vacuum, hydrogen gas, inert gas, and hydrogen gas with an inert gas added thereto, from immediately after the hydrogen-terminated semiconductor layer is formed until immediately before the insulator layer is formed; A method for manufacturing a MIS type semiconductor device, wherein a density of charged impurities present at the interface between the semiconductor layer and the insulator layer is 0 cm -2 or more and 5 x 10 11 cm -2 or less.

4. preparing a member having a first main surface on which at least a portion of a semiconductor layer made of diamond is exposed, and at least a portion of the semiconductor layer is hydrogen-terminated; forming an insulator layer in contact with at least a portion of the hydrogen-treated portion of the semiconductor layer; forming a conductive layer over at least a portion of the insulating layer; the hydrogen-terminated semiconductor layer is placed in an atmosphere selected from the group consisting of hydrogen gas, an inert gas, and hydrogen gas to which an inert gas has been added, during the period from immediately after the hydrogen-terminated semiconductor layer is formed to immediately before the insulator layer is formed; The pressure of the atmosphere is atmospheric pressure.

5. 5. The method for manufacturing a MIS type semiconductor device according to claim 1, wherein the atmosphere in which the insulator layer is formed is any one selected from the group consisting of vacuum, hydrogen gas, inert gas, and hydrogen gas with an inert gas added thereto.

6. 6. The method for manufacturing a MIS type semiconductor device according to claim 1, wherein said insulating layer is made of boron nitride.

7. 7. The method for manufacturing a MIS type semiconductor device according to claim 1, wherein said insulating layer is made of a single crystal of boron nitride.

8. 8. The method for manufacturing a MIS type semiconductor device according to claim 1, wherein said insulating layer is made of hexagonal boron nitride (h-BN).

9. The density of charged impurities present at the interface between the semiconductor layer and the insulator layer is 0 cm -2 Above 1 x 10 11 cm -2 9. The method for manufacturing a MIS type semiconductor device according to claim 1, wherein:

10. 10. The method for manufacturing a MIS type semiconductor device according to claim 1, wherein said inert gas is argon gas.

Citation Information

Patent Citations

  • Manufacturing method of thin-film transistor

    JP2002237600A

  • Semiconductor device and manufacturing method therefor

    JP2003077844A

  • Power element

    JP2016157932A

  • MIS-type semiconductor device and method of manufacturing the same

    JP2019125771A