Sealing material
A silicone rubber seal member with specific polydimethylsiloxane and silica particle composition addresses the issue of scratches in connector housings by balancing hardness and strength, ensuring durability and reliability in connector housings with multiple insertion holes.
Patent Information
- Application Number
- JP2021072577
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-22
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2041-04-22
AI Technical Summary
Conventional silicone rubber seals used in connector housings with multiple insertion holes are prone to damage and scratches due to the insertion of terminals with corners, leading to reduced sealing performance, especially as connector housings become smaller and the number of inserted wires increases, and existing materials fail to effectively balance hardness and scratch resistance.
A silicone rubber seal member composed of polydimethylsiloxane with an average degree of polymerization between 40 and 1,700, combined with silica particles, meeting specific conditions for elastic recovery rate, hardness, tensile strength, and surface friction to minimize scratches during insertion and removal of mating members.
The seal member achieves low hardness and high mechanical strength, reducing the likelihood of scratches and ensuring durability and reliability even with repeated use, maintaining effective sealing performance.
Smart Images

Figure 0007576507000003 
Figure 0007576507000004 
Figure 0007576507000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a silicone rubber-based sealing member having a plurality of insertion holes into which mating members are inserted. [Background technology]
[0002] A mat seal is known that is disposed at an electric wire pull-out portion of a connector housing and seals between the electric wire and the connector housing (see, for example, Patent Documents 1 and 2). The mat seal is made of an elastic material such as rubber and has a plurality of insertion holes penetrating in the thickness direction, and an electric wire is inserted into each of the insertion holes. A terminal is attached to the end of the electric wire. When an electric wire is inserted into the insertion hole of the mat seal, the terminal is first inserted into the insertion hole and passed through while pushing the insertion hole wider. The terminal that has passed through the insertion hole is inserted into the terminal receiving chamber, and the electric wire extending from the terminal is placed in the insertion hole. An annular lip portion is formed on the inner peripheral surface of the insertion hole, and the lip portion is in close contact with the outer periphery of the electric wire, thereby suppressing the intrusion of moisture into the connector housing. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-58138 A [Patent Document 2] JP 2018-159020 A [Patent Document 3] JP 2018-53237 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, connector housings have become smaller, and the number of wires inserted has increased. Accordingly, mat seals are also required to have an increased number of insertion holes and smaller hole diameters. Terminals attached to the ends of wires are often made of metal and have corners. For this reason, when the terminals pass through the insertion holes, they can damage the surface of the insertion holes, resulting in a decrease in sealing performance.
[0005] In this regard, Patent Document 1 describes silicone rubber containing polyrotaxane as a material for a sealing member used in mat seals and the like. However, polyrotaxane is relatively expensive, which increases costs. Patent Document 1 does not describe what type of damage is reduced, but according to paragraphs
[0009] and
[0053] , adding polyrotaxane allows silicone rubber molecules to slide against each other, making the rubber material more susceptible to elongation and deformation, thereby reducing the susceptibility of the sealing member to damage.
[0006] Conventionally, the problem of damage to sealing members was the "cracks" that developed from the incisions on the surface. For this reason, as a measure to suppress damage (cracks), studies have been made on increasing the tear strength taking into account the progress of the incisions. Patent Document 1 also lists tear strength as an evaluation item for characteristics (Tables 1 and 2). In response to this, the present inventors conducted extensive studies on damage to sealing members and found that in order to suppress a decrease in sealing performance, it is necessary to suppress the incisions themselves from being made, rather than the "cracks" that develop from the incisions. To achieve this, the problem cannot be solved by merely improving the tear strength, and conventional materials cannot sufficiently suppress the occurrence of incision damage.
[0007] Furthermore, Patent Document 2 describes, as a material for a sealing member for a waterproof connector, a thermosetting silicone rubber obtained by curing a composition containing a first silicone compound having at least two vinyl groups in the molecule, a second silicone compound having at least two hydrosilyl groups in the molecule, and an organic compound having at least two vinyl groups in the molecule. Paragraph
[0009] of Patent Document 2 states that by adding an organic compound, the modulus at break (tensile strength at break T defined in JIS K6251) can be increased. b It is described that since the elongation at break increases due to a decrease in the elongation at break, the stress when the terminal is inserted into the insertion hole is alleviated and tearing is suppressed.
[0008] As described above, as the housing becomes smaller and the number of wires inserted increases, the seal member is required to have a larger number of insertion holes and a smaller hole diameter. If the number of insertion holes increases and they are densely packed, interference between the insertion holes becomes a problem. For example, if the seal member is hard, a large stress is applied to the insertion hole when a mating member such as a terminal is inserted, and there is a risk that the adjacent insertion hole side is pressed and narrowed. If the insertion hole becomes narrow, cut scratches are likely to occur when the mating member is inserted. Therefore, it is necessary to reduce the hardness of the seal member from the viewpoint of suppressing interference between the insertion holes and making it difficult for cut scratches to occur.
[0009] In some cases, a reinforcing material such as silica is mixed into the sealing member for the purpose of adjusting the hardness and improving the mechanical strength. In this case, the hardness of the sealing member can be reduced by reducing the amount of the reinforcing material. However, if the hardness is reduced to a region where the type A durometer hardness is less than 15, for example, the strength of the rubber material is significantly reduced due to the reduction in the reinforcing material, and the rubber material itself becomes brittle, making it more likely to cause cuts. In this way, suppressing the occurrence of cuts in the sealing member and reducing the hardness are in a trade-off relationship, and it has been difficult to achieve both. Incidentally, in the above-mentioned Patent Documents 1 and 2, there is no consideration of reducing the hardness of the sealing member.
[0010] For example, Patent Document 3 describes a silicone rubber that contains a vinyl-group-containing organopolysiloxane and silica particles, and has low hardness, high tear strength, and small tensile permanent set. However, the silicone rubber described in Patent Document 3 is used in medical molded products such as medical tubes (paragraph
[0126] ). For this reason, the type A durometer hardness of the silicone rubber is 23.4 to 39.0 (Table 1), which is not appropriate for the hardness required for a seal member having multiple insertion holes through which a mating member is inserted and removed. As mentioned above, the occurrence of cut marks cannot be suppressed by improving the tear strength alone. Patent Document 3 describes the reduction of tensile permanent set as a problem focused on the use of medical molded products. Tensile permanent set is a characteristic that indicates that the elongation does not return to the original state after stretching (tensile residual set), and is recognized as a different characteristic from compression permanent set, which is a distortion that remains when compressed (paragraph
[0126] ).
[0011] In Patent Document 3, damage caused by inserting and removing a mating member such as a terminal is not considered.
[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a silicone rubber-based sealing member that has low hardness and is less likely to cause cuts in the insertion hole when a mating member is inserted or removed. [Means for solving the problem]
[0012] In order to solve the above problems, the sealing member of the present invention is a sealing member having a plurality of insertion holes into which a mating member is inserted, which is a cured product of a silicone rubber composition containing polydimethylsiloxane having an average degree of polymerization of 40 or more and 1,700 or less, and silica particles, and is characterized in that it satisfies the following conditions (a) to (d): (a) When the content of the silica particles relative to 100 parts by mass of the polydimethylsiloxane is X parts by mass, elastic recovery rate (%) / X (parts by mass)=5.7 to 19. (b) Type A durometer hardness is greater than or equal to 10 and less than 15. (c) The tensile strength at break is 2.1 MPa or more. (d) the coefficient of kinetic friction of the surface of the insertion hole is 2.5 or less. Effect of the Invention
[0013] The sealing member of the present invention is a cured product of a silicone rubber composition having polydimethylsiloxane with an average degree of polymerization of 40 or more and 1,700 or less, and silica particles. The sealing member of the present invention contains silica particles. This makes it easy to adjust the hardness of the sealing member, and it is easy to improve mechanical strength such as tensile strength. In addition, the sealing member of the present invention uses polydimethylsiloxane with an average degree of polymerization within a specific range as a base polymer. By limiting the average degree of polymerization to 40 or more and 1,700 or less, it is possible to optimize the crosslinked structure and achieve the desired mechanical strength. Therefore, even if the amount of silica particles is reduced to reduce the hardness, the resulting decrease in mechanical strength can be compensated for. Furthermore, the sealing member of the present invention satisfies the above conditions (a) to (d). These four conditions are conditions specified to achieve both low hardness and the suppression of the occurrence of cuts discovered by the present inventor.
[0014] As defined by the condition (a), in the sealing member of the present invention, the ratio of the elastic recovery to the content of the silica particles is 5.7 to 19. The elastic recovery is determined by the elastic deformation power η IT(%), and the closer to 100%, the easier it is to elastically deform, in other words, the easier it is to return to its original state even after deformation. The present inventor has found that both the elastic recovery rate of the sealing member and the content of silica particles have a large effect on the cut scratches that occur when inserting and removing a mating member into and from the insertion hole of the sealing member, and has specified a range that is effective for suppressing cut scratches in the ratio of the two. For example, if only the elastic recovery rate is focused on and its value is large, the recovery force against repeated deformation is large, so it seems to be an indicator of cut scratch suppression. However, even if the elastic recovery rate is large, if the content of silica particles is too small, the rubber material itself becomes brittle, so cut scratches are likely to occur. In this way, the occurrence of cut scratches cannot be suppressed by only specifying either the elastic recovery rate or the content of silica particles. By satisfying condition (a), it is possible to achieve both the elastic recovery rate and mechanical strength of the rubber material (sealing member). As a result, the residual strain due to compression and tension accompanying the insertion and removal of the mating member is reduced, and the sealing member is less likely to be fatigue-destroyed even when insertion and removal are repeated.
[0015] As defined by condition (b), the type A durometer hardness of the seal member of the present invention is equal to or greater than 10 and less than 15. By satisfying condition (b), a low hardness of the seal member is achieved.
[0016] As stipulated in condition (c), the tensile strength at break of the sealing member of the present invention is 2.1 MPa or more. When condition (c) is satisfied, the intermolecular bonds of the rubber are strong, so that the rubber molecules are less likely to be broken by the mechanical and thermal loads applied when the mating member is inserted or removed. As a result, the mechanical strength of the rubber material (sealing member) is ensured, and the occurrence of cut scratches can be suppressed.
[0017] As stipulated in condition (d), the dynamic friction coefficient of the surface of the insertion hole of the seal member of the present invention is 2.5 or less. By satisfying condition (d), the friction of the surface of the insertion hole (the sliding surface with the mating member) is reduced. This reduces the mechanical and thermal loads applied when the mating member is inserted or removed, making it difficult for the rubber molecules to be cut. As a result, the occurrence of cut marks can be suppressed.
[0018] As described above, the sealing member of the present invention uses polydimethylsiloxane having an average degree of polymerization of 40 to 1,700 and satisfies the conditions (a) to (d), so that the sealing member has low hardness and is less likely to develop cuts in the insertion hole even when the mating member is repeatedly inserted and removed. Therefore, the sealing member of the present invention has excellent durability and high reliability. [Brief description of the drawings]
[0019] [Figure 1] 1 is a front view of a mat seal which is an embodiment of a sealing member of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view taken along line II-II of FIG. [Diagram 3] FIG. 1 is an explanatory diagram of a method for evaluating the scratch resistance of a matte seal. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] First, an embodiment of the sealing member of the present invention will be described, in which the mat seal is used as a mat seal for a waterproof connector. Fig. 1 shows a front view of the mat seal of this embodiment. Fig. 2 shows a cross-sectional view taken along line II-II in Fig. 1. As shown in Figs. 1 and 2, the mat seal 1 has a main body 10 and five insertion holes 20.
[0021] The main body 10 has a rectangular plate shape and is a cured product of a silicone rubber composition having two types of vinyl-terminated polydimethylsiloxanes as base polymers, an organohydrogenpolysiloxane as a crosslinking agent, silica particles, and a phenyl-containing silicone oil. One of the two types of vinyl-terminated polydimethylsiloxanes is a low molecular weight polydimethylsiloxane with an average degree of polymerization of 40, and the other is a high molecular weight polydimethylsiloxane with an average degree of polymerization of 800. The blending ratio of the high molecular weight polydimethylsiloxane to the low molecular weight polydimethylsiloxane is 90:10. The content of the silica particles in the main body 10 is 5 parts by mass relative to a total of 100 parts by mass of the two types of polydimethylsiloxanes, and the value of "elastic recovery rate / silica particle content" under condition (a) is 19, the type A durometer hardness under condition (b) is 14, and the tensile strength at break under condition (c) is 2.7 MPa.
[0022] Each of the five insertion holes 20 is formed penetrating the main body 10 in the thickness direction. Each of the five insertion holes 20 has a circular opening when viewed from the front, and is arranged in a row in the left-right direction at equal intervals. The distance D between adjacent insertion holes 20 is 2.6 mm. Each of the five insertion holes 20 has a lip portion 21 protruding inward. The lip portion 21 has an annular shape, and two of them are arranged parallel to the thickness direction of the main body 10. An oil film (not shown) is arranged on the surface (inner peripheral surface) of the insertion hole 20. The oil film is formed by exuding phenyl group-containing silicone oil, which is a component of the silicone rubber composition, onto the surface of the insertion hole 20. The dynamic friction coefficient of the surface of the insertion hole 20 under condition (d) is 1.5. The shape, size, etc. of the five insertion holes 20 are all the same.
[0023] As shown in Fig. 2, an electric wire with terminal 8 is inserted into each of the five insertion holes 20 from the rear. The electric wire with terminal 8 has a terminal 80 and an electric wire 81. The terminal 80 is made of metal and has a rectangular parallelepiped shape with protrusions. The terminal 80 is attached to the tip (front end) of the electric wire 81. The electric wire with terminal 8 is included in the concept of a mating member in the present invention.
[0024] The waterproof connector is mainly composed of a mat seal 1, an outer housing (connector housing) and an inner housing (not shown). The outer housing is box-shaped with a rectangular cylindrical side wall and a rear wall that closes the rear end opening of the side wall, and the rear wall has five terminal insertion holes through which the terminal-attached electric wires 8 can pass. The mat seal 1 is disposed inside the rear wall of the outer housing, and the insertion holes 20 are disposed to correspond to the terminal insertion holes. The rear surface of the mat seal 1 is disposed in close contact with the rear wall of the outer housing. The inner housing is disposed in close contact with the front surface of the mat seal 1. The inner housing has a terminal accommodating portion that accommodates the terminals 80 that have passed through the insertion holes 20.
[0025] The electric wire 8 with terminal is inserted from the terminal insertion hole of the outer housing into the insertion hole 20 of the mat seal 20. The terminal 80 advances forward while pushing and widening the insertion hole 20, and after passing through the insertion hole 20, is accommodated in the terminal accommodating section of the inner housing. The lip portion 21 of the insertion hole 20 comes into close contact with the outer periphery of the electric wire 81 extending rearward from the terminal 80, thereby sealing the gap between the insertion hole 20 and the electric wire 81.
[0026] The mat seal 1 of this embodiment is a cured product of a silicone rubber composition containing polydimethylsiloxane with an average degree of polymerization of 40 or more and 1,700 or less, and silica particles, and satisfies four conditions (a) to (d). In particular, as can be seen from the type A durometer hardness of 14 in condition (b), the mat seal 1 has low hardness, and as can be seen from the tensile strength at break of 2.7 MPa in condition (c), the mat seal 1 has high mechanical strength. As a result, even if the terminal 80 is repeatedly inserted and removed, the insertion holes 20 in the mat seal 1 are unlikely to interfere with each other, and cut scratches are unlikely to occur in the insertion holes 20. Therefore, the mat seal 1 has excellent durability and high reliability.
[0027] While one embodiment of the sealing member of the present invention has been described above, the sealing member of the present invention is not limited to this embodiment, and can be embodied in various forms incorporating modifications and improvements that can be made by those skilled in the art, as long as they do not deviate from the gist of the present invention.
[0028] [Sealing material composition] The sealing member of the present invention has a plurality of insertion holes into which mating members are inserted. The type, material, shape, size, etc. of the mating members are not particularly limited. For example, when the mating member is made of metal and has corners, such as the terminal of the above embodiment, notches are likely to occur. Therefore, the sealing member of the present invention, which has a high effect of suppressing the occurrence of notches, is suitable for such mating members.
[0029] The number of insertion holes is not particularly limited as long as it is two or more. The number of insertion holes, the arrangement form, the shape of the opening, the diameter of the opening, etc. may be appropriately determined according to the use of the seal member, the number of mating members, the material, the shape, the size, etc. of the mating members. The insertion holes may or may not penetrate the seal member in the thickness direction. For example, when the seal member has a flat body portion and the body portion has multiple insertion holes, if the distance between the insertion holes becomes close, the insertion holes are likely to interfere with each other when the mating member is inserted and removed. That is, when the mating member is inserted into any insertion hole, the adjacent insertion hole is likely to be pressed and narrowed. In this case, when the mating member is inserted into the adjacent insertion hole, a cut is likely to occur. In this way, it is expected that the more dense the number of insertion holes, the more likely the cut is to occur. From the viewpoint of reducing interference between the insertion holes, when the body portion in which the insertion holes are formed is viewed from the insertion direction of the mating member, the distance between adjacent insertion holes is desirably 1.3 mm or more and 8.8 mm or less. Here, the distance between adjacent insertion holes means the distance between the central axes of adjacent insertion holes.
[0030] From the viewpoint of reducing the dynamic friction coefficient of the surface of the insertion hole, it is desirable to arrange an oil film on at least a part of the surface of the insertion hole. The oil film may be formed by the oil contained in the silicone rubber composition seeping (bleeding) onto the surface of the insertion hole, or may be formed by applying oil to the surface of the insertion hole, or both. The oil that forms the oil film will be described later.
[0031] [Sealing material components and characteristics] The sealing member of the present invention is a cured product of a silicone rubber composition having polydimethylsiloxane with an average degree of polymerization of 40 to 1,700, and silica particles. The polydimethylsiloxane as the base polymer may be liquid rubber or solid (millable) rubber. Liquid rubber is preferable because it can be molded with good dimensional accuracy, including the lip portion. In this specification, the average degree of polymerization is the weight average degree of polymerization in terms of polystyrene, measured by GPC (gel permeation chromatography) method (solvent: toluene).
[0032] When the average degree of polymerization of polydimethylsiloxane is less than 40, the polymer molecules become shorter, so that the crosslinking points increase and tend to be dense. When the crosslinking points are dense, the rubber itself becomes hard. In addition, the CC bonds at the crosslinking points are weaker and more easily cut than the Si-O bonds of the polymer molecules. Therefore, when the crosslinking points are dense, stress is concentrated in that area, leading to a decrease in mechanical strength. On the other hand, when the average degree of polymerization is greater than 1,700, the polymer molecules become longer. For this reason, for example, when a reactive group (such as an alkenyl group) that contributes to crosslinking is located at the end of the polymer molecule, it becomes difficult for a crosslinking reaction to occur between polymer molecules via the reactive group. As a result, the crosslinking does not proceed sufficiently, the crosslinking density becomes small, and the elastic recovery rate and mechanical strength are reduced. Considering the hardness and mechanical strength of the sealing member, a form having polydimethylsiloxane with an average degree of polymerization of 600 to 1,700 is more preferable.
[0033] From the viewpoint of further increasing the mechanical strength, it is desirable to use multiple polydimethylsiloxanes with different average polymerization degrees in combination. For example, a high molecular weight polydimethylsiloxane with an average polymerization degree of 800 to 1,700 and a low molecular weight polydimethylsiloxane with an average polymerization degree of 40 to 110 can be used in combination. For example, when one type of polydimethylsiloxane is used, crosslinking points are formed in the rubber and dispersed almost uniformly. In this case, stress is applied evenly to the crosslinking points, so it is difficult to release the stress. In contrast, when multiple polydimethylsiloxanes with different average polymerization degrees are used, crosslinking points are densely distributed in the rubber. That is, crosslinking points formed from a polymer with a low molecular weight are close to each other because the polymer molecules are short, resulting in a "dense" state. Although the CC bonds at the crosslinking points are relatively weak, the strength can be ensured by being densely packed. Crosslinking points formed from a polymer with a high molecular weight are far from each other because the polymer molecules are long, resulting in a "sparse" state. The part with long polymer molecules is relatively easy to stretch, so it is possible to disperse and attenuate the applied stress. In this way, by using multiple polydimethylsiloxanes with different average degrees of polymerization to create a distribution of cross-linking points with different densities, it is possible to attenuate stress in the "sparse" areas while ensuring the strength to withstand stress in the "dense" areas, thereby increasing the mechanical strength of the sealing member overall.
[0034] When a high molecular weight polydimethylsiloxane having an average degree of polymerization of 800 or more and 1,700 or less is used in combination with a low molecular weight polydimethylsiloxane having an average degree of polymerization of 40 or more and 110 or less, the blending ratio of the high molecular weight polydimethylsiloxane to the low molecular weight polydimethylsiloxane is preferably high molecular weight: low molecular weight = 90: 10 to 60: 40, with the total mass of both being 100 parts by mass. If the blending ratio of the low molecular weight polydimethylsiloxane is small, the mechanical strength of the sealing member tends to be low, and conversely, if the blending ratio is large, the sealing member tends to be hard.
[0035] Polydimethylsiloxane has a predetermined reactive group according to its crosslinking mechanism (curing mechanism). Examples of the reactive group include an alkenyl group (vinyl group, allyl group, butenyl group, pentenyl group, hexenyl group, etc.) and a silanol group. The former polydimethylsiloxane having an alkenyl group is crosslinked by a peroxide crosslinking reaction using an organic peroxide as a crosslinking agent, or an addition reaction using an organopolysiloxane (organohydrogenpolysiloxane) having a hydrosilyl group (SiH group) as a crosslinking agent. A hydrosilylation catalyst such as a platinum catalyst can be used in combination for the addition reaction. The latter polydimethylsiloxane having a silanol group is crosslinked by a condensation reaction. A condensation crosslinking agent can be used in combination for the condensation reaction. From the viewpoint of obtaining a cured product having good elasticity, it is preferable that the polydimethylsiloxane has at least two alkenyl groups in one molecule and that an organohydrogenpolysiloxane is used as a crosslinking agent.
[0036] The number of hydrosilyl groups in the organohydrogenpolysiloxane of the crosslinking agent is not particularly limited, but is preferably 2 to 50 in terms of high curing speed and excellent stability. In this case, it is preferable that the hydrogen of the hydrosilyl group is bonded to different Si. The organohydrogenpolysiloxane may be either linear or cyclic. Examples of the organohydrogenpolysiloxane include methylhydrogenpolysiloxane capped with trimethylsiloxy groups at both ends and dimethylsiloxane-methylhydrogensiloxane copolymer capped with trimethylsiloxy groups at both ends. The amount of the crosslinking agent to be blended is preferably 0.1 to 40 parts by mass per 100 parts by mass of polydimethylsiloxane having at least two alkenyl groups in one molecule.
[0037] In order to promote the crosslinking reaction of polydimethylsiloxane, a catalyst may be appropriately added. The above-mentioned hydrosilylation catalyst may include platinum catalyst, ruthenium catalyst, ruthenium catalyst, etc. The platinum catalyst may include fine particle platinum, platinum black, platinum-supported activated carbon, platinum-supported silica, chloroplatinic acid, alcohol solution of chloroplatinic acid, platinum olefin complex, platinum alkenylsiloxane complex, etc. These may be used alone or in combination of two or more.
[0038] As the silica particles, fumed silica, calcined silica, precipitated silica, etc. may be used. The silica particles may be surface-treated. For example, those that have been hydrophobized are preferable because they have excellent dispersibility in silicone rubber and can easily secure sufficient mechanical strength. The amount of silica particles may be appropriately adjusted to satisfy conditions (a) to (c). For example, it is preferable to use 5 parts by mass or more and 15 parts by mass or less per 100 parts by mass of polydimethylsiloxane. When the amount of silica particles is increased, the cured product (sealing member) becomes hard and the elastic recovery rate becomes small. Conversely, when the amount of silica particles is decreased, the cured product becomes soft and the elastic recovery rate becomes large. However, when the amount of silica particles is too small, the mechanical strength of the cured product decreases.
[0039] As described above, from the viewpoint of reducing the dynamic friction coefficient of the surface of the insertion hole, it is desirable to arrange an oil film on at least a part of the surface of the insertion hole. The oil film may be formed by exuding oil as a component of the silicone rubber composition onto the surface of the insertion hole, or may be formed by separately applying oil to the surface of the insertion hole. In the former case, it is desirable for the silicone rubber composition to have an oil that is poorly compatible with the polydimethylsiloxane of the base polymer. Examples of oils that are poorly compatible with polydimethylsiloxane and tend to bleed include phenyl group-containing oils, ether-modified oils, and liquid paraffin oils. One or more of these may be used in combination. Among them, phenyl group-containing oils are preferable from the viewpoint of easily controlling the timing of bleeding from polydimethylsiloxane and ensuring good moldability. The amount of oil to be blended may be appropriately adjusted to satisfy condition (d). For example, it is preferable to set the amount of oil to 0.5 parts by mass or more and 15 parts by mass or less with respect to 100 parts by mass of polydimethylsiloxane. It is more preferable to set the amount of oil to 4 parts by mass or more and 10 parts by mass or less. In the latter case (when applying oil to the surface of the insertion hole), the type of oil is not particularly limited, but it is preferable that the applied oil does not easily soak into the sealing member (cured product of the silicone rubber composition) and remains on the surface. From this viewpoint, as in the former case, it is preferable to use an oil that is poorly compatible with polydimethylsiloxane.
[0040] The silicone rubber composition may contain additives other than the above-mentioned materials so long as it satisfies the conditions (a) to (d). Examples of additives include crosslinking accelerators, crosslinking retarders, crosslinking assistants, reinforcing materials, antioxidants, softeners, plasticizers, lubricants, heat stabilizers, flame retardants, flame retardant assistants, ultraviolet absorbers, rust inhibitors, pigments, etc.
[0041] The sealing member of the present invention satisfies the following four conditions (a) to (d).
[0042] (a) Elastic recovery rate (%) / X (parts by mass) = 5.7 to 19 The elastic recovery rate is the elastic deformation power measured by the indentation test method. Elastic deformation power η IT The amount of plastic deformation work (W plast ) and elastic deformation work (W elast ) and calculate the total mechanical work as W total (=W plast +W elast ) is calculated using the following formula (i). η IT =W elast / W total ×100 (i) In this specification, the calculated elastic deformation power η IT The elastic recovery (%) is referred to as the elastic recovery, and the elastic recovery value is divided by the content (X parts by mass) of silica particles relative to 100 parts by mass of polydimethylsiloxane to determine the "elastic recovery (%) / X (parts by mass)" under condition (a).
[0043] If the ratio of elastic recovery to the silica particle content is less than 5.7, the sealing material becomes hard and is difficult to return to its original state after deformation, making it more susceptible to cuts. If it exceeds 19, the sealing material becomes brittle, reducing its mechanical strength and making it more susceptible to cuts.
[0044] (b) Type A durometer hardness: 10 or more and less than 15 The type A durometer hardness may be measured by a method conforming to JIS K 6253-3:2012. If the type A durometer hardness is less than 10, the seal member becomes soft and its mechanical strength decreases, making it more likely to develop cut marks. If it is 15 or more, the seal member becomes hard, making it difficult to insert and remove the mating member, and there is a risk that the adjacent insertion hole may be narrowed when the mating member is inserted, making it more likely to develop cut marks.
[0045] (c) Tensile strength at break: 2.1 MPa or more The tensile strength at break may be measured according to a method in accordance with JIS K 6251:2017. Dumbbell No. 3 specimens are used. If the tensile strength at break is less than 2.1 MPa, the mechanical strength of the sealing material decreases, making it more likely to develop cuts.
[0046] (d) Coefficient of dynamic friction on the surface of the insertion hole: 2.5 or less In this specification, the dynamic friction coefficient is a value measured using an automatic friction and wear analyzer (a surface contactor, "Triboster 500" manufactured by Kyowa Interface Science Co., Ltd.). The measurement conditions are a load of 100 gf (0.98 N) and a tensile speed of 500 mm / min. If the dynamic friction coefficient exceeds 2.5, friction on the surface of the insertion hole (the sliding surface with the mating member) increases, making it more likely that cuts will occur. It is more preferable that the dynamic friction coefficient of the surface of the insertion hole is 2.0 or less.
[0047] [Method of manufacturing sealing material] The sealing member of the present invention may be produced by curing a silicone rubber composition containing polydimethylsiloxane having an average degree of polymerization within a specific range and silica particles. For example, the silicone rubber composition may be injected into a mold using an injection molding machine and heated to cure. The heating temperature may be about 140 to 170°C, and the curing time may be about 5 to 10 minutes. EXAMPLES
[0048] Next, the present invention will be described more specifically with reference to examples.
[0049] (1) Characteristics of sealing materials <Production of test pieces> First, various silicone rubber compositions were prepared by blending the prescribed raw materials in the amounts shown in Tables 1 and 2 below and mixing them using a planetary mixer. Next, the prepared silicone rubber compositions were hardened by press molding at a temperature of 170°C for 10 minutes to produce test pieces according to the measurement methods for the properties described below. The test pieces of Examples 1 to 15 shown in Table 1 are included in the concept of the "cured product of the silicone rubber composition" that constitutes the sealing member of the present invention. Details of the raw materials used are as follows.
[0050] [Base polymer] [Ultra-low molecular weight polydimethylsiloxane] Vinyl-terminated polydimethylsiloxane A: "DMS-V05" manufactured by Gelest, average degree of polymerization 9. [Low molecular weight polydimethylsiloxane] Vinyl-terminated polydimethylsiloxane B: "Polymer VS50" manufactured by EVONIK, average degree of polymerization 40. Vinyl-terminated polydimethylsiloxane C: "Polymer VS100" manufactured by EVONIK, average degree of polymerization 65. Vinyl-terminated polydimethylsiloxane D: "Polymer VS200" manufactured by EVONIK, average degree of polymerization 110. [High molecular weight polydimethylsiloxane] Vinyl-terminated polydimethylsiloxane E: "Polymer VS65000" manufactured by EVONIK, average degree of polymerization 800. Vinyl-terminated polydimethylsiloxane F: EVONIK "Polymer VS100000", average degree of polymerization 1,700. [Ultra-high molecular weight polydimethylsiloxane] Vinyl-terminated polydimethylsiloxane G: EVONIK "Polymer VS165000", average degree of polymerization 1,800.
[0051] [Crosslinking agent] Organohydrogenpolysiloxane: "KF-9901" manufactured by Shin-Etsu Chemical Co., Ltd.
[0052] [Silica particles] Silica particles: hydrophobic fumed silica surface-treated with hexamethyldisilazane, "AEROSIL (registered trademark) RX200" manufactured by Nippon Aerosil Co., Ltd.
[0053] [oil] Phenyl group-containing silicone oil: "KF-53" manufactured by Shin-Etsu Chemical Co., Ltd. Ether-modified silicone oil: "KF-354L" manufactured by Shin-Etsu Chemical Co., Ltd. Liquid paraffin oil: "Liquid paraffin" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0054] [catalyst] Hydrosilylation platinum catalyst: "Pt-VTSC-3.0X" manufactured by Umicore Japan Co., Ltd.
[0055] <Method of measuring characteristics> The elastic recovery rate, type A durometer hardness, tensile strength at break, and dynamic friction coefficient of the cured silicone rubber composition were measured using the test pieces thus produced. Each measurement method is explained below.
[0056] [Elastic recovery rate] Using a microhardness tester based on the indentation test method (Fischer Instruments, Inc., "FISCHERSCOPE (registered trademark) H100C"), an indenter was pressed into the surface of a square sheet-shaped test piece under the following measurement conditions to create a load-displacement curve. The size of the test piece was 30 mm on one side and 2 mm thick. From the load-displacement curve obtained, the plastic deformation work (W plast ) and elastic deformation work (W elast ) and calculate the total mechanical work as W total (=W plast +W elast ) and from the previous equation (i), the elastic deformation power η IT (%) was calculated. The calculated elastic deformation power η IT The elastic recovery rate (%) was defined as the elastic recovery rate, and this value was divided by the content (X parts by mass) of silica particles per 100 parts by mass of the base polymer polydimethylsiloxane to obtain the "elastic recovery rate (%) / X (parts by mass)" for condition (a). Measurement conditions Indenter: Square vertical diamond indenter with an opposing angle of 136°. Initial load: 0mN. Maximum pressing load: 10mN (constant load). Time to reach maximum load: 3sec. Maximum load holding time: 5sec. Unloading time: 3sec. Measurement temperature: 25℃.
[0057] [Type A durometer hardness] The type A durometer hardness of the 12 mm thick test piece was measured using a method in accordance with JIS K 6253-3:2012.
[0058] [Tensile strength at break] The tensile strength at break T of a dumbbell No. 3 test piece (thickness 2 mm) was measured according to the method in accordance with JIS K 6251:2017. b (MPa) was measured.
[0059] [Kinematic friction coefficient] The dynamic friction coefficient of the surface of a square sheet-like test piece 2 mm thick and 30 mm square was measured using an automatic friction and wear analyzer (Kyowa Interface Science Co., Ltd., "Triboster 500", surface contact). The measurement conditions were a load of 100 gf (0.98 N) and a tensile speed of 500 mm / min. For the test pieces of Examples 12 to 14, which are indicated as "coated" in the oil column in Table 1, oil was applied to the surface of the test piece before measurement.
[0060] <Characteristics measurement results> Tables 1 and 2 show the raw materials used in the manufacture of the test specimens and the measurement results of their properties. [Table 1] [Table 2]
[0061] As shown in Table 1, the cured products of Examples 1 to 15 satisfied all of the four conditions (a) to (d). On the other hand, as shown in Table 2, the cured products of Comparative Examples 1 to 20, which differ from Examples 1 to 15 in the average degree of polymerization of the base polymer, the blending ratio, the amount of silica particles blended, the presence or absence of oil, etc., did not satisfy some of the four conditions (a) to (d).
[0062] First, comparing Example 5, which uses one type of polydimethylsiloxane as the base polymer, with Comparative Examples 3 to 5, the only difference between the two is the amount of silica particles. For example, the cured products of Comparative Examples 4 and 5, which have a smaller amount of silica particles than the cured product of Example 5, have a smaller tensile strength at break. In particular, the cured product of Comparative Example 5, which has a smaller amount of silica particles, also has a smaller type A durometer hardness. Conversely, the cured product of Comparative Example 3, which has a larger amount of silica particles than the cured product of Example 5, has a smaller ratio of elastic recovery to the content of silica particles and a larger type A durometer hardness.
[0063] In the cured product of Comparative Example 19, only polydimethylsiloxane with an average degree of polymerization of less than 40 was used. In this case, the type A durometer hardness was high and the tensile strength at break was low. In contrast, in the cured product of Comparative Example 20, only polydimethylsiloxane with an average degree of polymerization of more than 1,700 was used. In this case, the tensile strength at break was low and the dynamic friction coefficient was high.
[0064] Next, among the examples using two types of polydimethylsiloxanes with different average polymerization degrees as the base polymer, Examples 1 to 4 and Comparative Examples 6 to 11, in which the high molecular weight polydimethylsiloxane is the same "E", are compared. In this case, when the blending ratio of low molecular weight polydimethylsiloxane is small, the tensile strength at break is small (Comparative Examples 6, 8, and 10), and when the blending ratio is large, the type A durometer hardness is large (Comparative Examples 7, 9, and 11). The same results were obtained when Examples 6 to 9, 11, and 15, in which the high molecular weight polydimethylsiloxane is the same "F", were compared with Comparative Examples 12 to 17.
[0065] Next, Example 11 and Examples 12 to 14, which differ in the presence or absence of oil in the silicone rubber composition, are compared. In this case, the cured products of Examples 12 to 14, which were not blended with oil and were applied later, had a larger amount of oil on the surface than the cured product of Example 11, which was blended with oil, and therefore had a smaller dynamic friction coefficient. In contrast, the cured product of Comparative Example 18 was not blended with oil and was not applied later. Therefore, there was no oil film on the surface, and the dynamic friction coefficient was large.
[0066] (2) Evaluation of the scratch resistance of sealing materials In the same manner as in the manufacture of the above-mentioned test specimens, various silicone rubber compositions were prepared according to the formulations shown in Tables 1 and 2, and the compositions were press-molded to manufacture the mat seal 1 of the above-mentioned embodiment (see Figs. 1 and 2 above). For the mat seals of Examples 12 to 14, which are indicated as "coated" in the oil column in Table 1, oil was applied to the surface (inner circumferential surface) of the insertion hole of the manufactured mat seal. The mat seals of Examples 1 to 15 shown in Table 1 are included in the concept of the sealing member of the present invention. The manufactured mat seal was set in a housing, and the terminal was inserted and removed to evaluate the resistance to cut scratches (scratch resistance). The evaluation method is as follows. Fig. 3 shows an explanatory diagram of the evaluation method for the scratch resistance of the mat seal. Fig. 3 corresponds to Fig. 1 above.
[0067] As shown in Fig. 3, the five insertion holes 20 formed in the mat seal 1 were numbered No. 1 to No. 5 from the left. First, the terminals of the electric wires with terminals were inserted in the order of No. 1 to No. 5, and then the electric wires were pulled out in the order of No. 5 to No. 1. After repeating this operation three times, the mat seal 1 was cut in the left-right direction around the insertion holes 20 as shown by the dashed line C in Fig. 3, and the number of cuts on the surfaces (inner peripheral surfaces) of the five insertion holes 20 was counted.
[0068] The results are summarized in Tables 1 and 2. As shown in Table 1, the number of cuts in the mat seals of Examples 1 to 15, which satisfied all four conditions (a) to (d), was 20 or less, whereas the number of cuts in the mat seals of Comparative Examples 1 to 20, which did not satisfy any one of the conditions (a) to (d), exceeded 20. As is clear from the results of Comparative Examples 1 to 20, when the mechanical strength indicated by the tensile strength at break was low, or when the hardness indicated by the type A durometer hardness was not within a predetermined range, the occurrence of cuts could not be suppressed. In addition, when the average degree of polymerization of the polydimethylsiloxane used was less than 40 or more than 1,700, or when the dynamic friction coefficient of the surface of the insertion hole was large, the occurrence of cuts could not be suppressed. From the above, it was confirmed that in the seal member of the present invention, even if the hardness was low, cuts were unlikely to occur in the insertion hole due to insertion and removal of the mating member. It was also confirmed that using two types of polydimethylsiloxane with different average degrees of polymerization as the base polymer makes it easier to satisfy the conditions (a) to (d) necessary for suppressing the occurrence of cuts compared to using one type of polydimethylsiloxane. [Industrial Applicability]
[0069] The sealing member of the present invention can be applied to various parts in the fields of automobiles, industrial equipment, information and communication equipment, etc. In particular, it is suitable for multi-pole rubber plugs, multi-hole rubber bushings, multi-hole grommets, etc. for waterproof connectors, etc. [Explanation of symbols]
[0070] 1: mat seal, 10: main body, 20: insertion hole, 21: lip, 8: electric wire with terminal, 80: terminal, 81: electric wire.
Claims
1. A seal member having a plurality of insertion holes into which mating members are inserted, A sealing member which is a cured product of a silicone rubber composition containing polydimethylsiloxane having an average degree of polymerization of 40 or more and 1,700 or less, and silica particles, and which satisfies the following conditions (a) to (d): (a) When the content of the silica particles per 100 parts by mass of the polydimethylsiloxane is X parts by mass, elastic recovery rate (%) / X (parts by mass)=5.7 to 19. (b) Type A durometer hardness is 10 or more and less than 15. (c) The tensile strength at break is 2.1 MPa or more. (d) the coefficient of dynamic friction of the surface of the insertion hole is 2.5 or less.
2. 2. The sealing member according to claim 1, wherein the polydimethylsiloxane has an average degree of polymerization of 600 or more and 1,700 or less.
3. 2. The sealing member according to claim 1, wherein the polydimethylsiloxane comprises a high molecular weight polydimethylsiloxane having an average degree of polymerization of 800 or more and 1,700 or less, and a low molecular weight polydimethylsiloxane having an average degree of polymerization of 40 or more and 110 or less.
4. 4. The sealing member according to claim 3, wherein a compounding ratio of the high molecular weight polydimethylsiloxane to the low molecular weight polydimethylsiloxane is 90:10 to 60:40, where the total mass of the two is 100 parts by mass.
5. The polydimethylsiloxane has at least two alkenyl groups in one molecule, 5. The sealing member according to claim 1, wherein the silicone rubber composition contains a crosslinking agent having a hydrosilyl group (SiH group).
6. 6. The sealing member according to claim 1, wherein the content of the silica particles is 5 parts by mass or more and 15 parts by mass or less with respect to 100 parts by mass of the polydimethylsiloxane.
7. 7. The seal member according to claim 1, further comprising an oil film disposed on at least a portion of a surface of the insertion hole.
8. The silicone rubber composition contains an oil, The seal member according to claim 7 , wherein the oil film is formed by the oil seeping out onto the surface of the insertion hole.
9. 9. The seal member according to claim 7, wherein the oil film is formed by applying oil to the surface of the insertion hole.
10. 10. The sealing member according to claim 8, wherein the oil is at least one oil selected from the group consisting of phenyl group-containing oil, ether-modified oil, and liquid paraffin oil.
11. 11. The seal member according to claim 1, further comprising a flat body portion, and each of the plurality of insertion holes is formed penetrating the body portion in a thickness direction.
12. 12. The seal member according to claim 1, wherein the mating member is made of metal and has a corner.
Citation Information
Patent Citations
A composition used to prepare silicone elastomer and the synthesis and use of a silicone elastomer
EP2192157A1
Curable liquid silicone rubber composition for forming sealing member and sealing member
JP2011153305A
Seal member
JP2016058138A
Silicone rubber-based curable composition and molded body
JP2018053237A
Seal member and waterproof connector
JP2018159020A