Cement-based composition, method for producing cement-based composition, and method for recovering carbon dioxide
Incorporating alkali metal carbonates in cement compositions allows for controlled CO2 absorption and regeneration at 100-300°C, enhancing absorption capacity and preventing atmospheric release, addressing the limitations of conventional cement compositions.
Patent Information
- Application Number
- JP2022016650
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-02-04
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-02-04
AI Technical Summary
Conventional cement compositions absorb carbon dioxide up to a limit and then cease absorption, and regenerating their capacity involves high temperatures that degrade the cement, releasing CO2 back into the atmosphere, contradicting emission reduction goals.
Incorporating alkali metal carbonates like potassium carbonate and sodium ferrite as absorbents in cement compositions, which release CO2 at 100-300°C, allowing regeneration without strength loss, and encapsulating these materials to control absorption and release.
Enhances CO2 absorption capacity by 5-50% and maintains cement strength, prolongs reinforcing bar corrosion resistance, and prevents atmospheric CO2 release during regeneration.
Smart Images

Figure 0007576586000001 
Figure 0007576586000002 
Figure 0007576586000003
Abstract
Description
[Technical field]
[0001] The present invention relates to cement-based compositions, such as concrete, that have carbon dioxide absorption capacity. [Background technology]
[0002] It has long been known that cementitious compositions such as concrete have the ability to absorb carbon dioxide. Due to the growing awareness of environmental issues in recent years, there is a demand to further improve the carbon dioxide absorption capacity of cement-based compositions such as concrete, so that carbon dioxide can be absorbed by concrete, road surfaces, and other structures, thereby suppressing the carbon dioxide concentration in the atmosphere. However, most substances with carbon dioxide absorption capacity absorb carbon dioxide, and once the amount of carbon dioxide they can absorb reaches a limit, they are no longer able to absorb any more. The same is true for concrete with carbon dioxide absorption capacity; after it is poured and installed in a building, it has the problem of no longer absorbing carbon dioxide after a certain period of time has passed.
[0003] In recent years, with the rise in environmental awareness, carbon dioxide absorbents that repeatedly absorb and release carbon dioxide when some external force such as heat or pressure is applied have been attracting attention (for example, Patent Document 1). If a cement-based composition contains a carbon dioxide absorbent that releases carbon dioxide when heat is applied, it is expected that the ability to absorb carbon dioxide will be exerted again (regenerated, restored, or revived) by heating and releasing carbon dioxide. Conventional carbon dioxide absorbents need to be heated to around 600°C to regenerate (recover) their absorption capacity after absorbing carbon dioxide (CO2). For example, lithium silicate (Li4SiO4) absorbs carbon dioxide at temperatures between room temperature and 700°C, and releases carbon dioxide at temperatures above 700°C. However, the strength of cement-based compositions such as concrete drops significantly when the temperature exceeds 300°C. Therefore, it is inconvenient to use a material that releases absorbed carbon dioxide at a temperature exceeding 300°C in a cement-based composition having carbon dioxide absorption capacity. Furthermore, it is known that cement-based compositions such as concrete will explode, deteriorate, or discolor when heated to about 600°C. Therefore, a cement-based composition having carbon dioxide absorption capacity preferably has the property of releasing absorbed carbon dioxide at 100 to 300° C., but such a cement-based composition has not yet been proposed. In addition, if the carbon dioxide released during the process of releasing the absorbed carbon dioxide to restore the carbon dioxide absorption capacity (regenerating, recovering, or reviving the carbon dioxide absorption capacity) is dispersed into the atmosphere, this goes against the purpose of reducing carbon dioxide emissions. Similarly, when a cement-based composition such as concrete is reused, if it is heated to release carbon dioxide and dissipate it into the atmosphere, this does not reduce the amount of carbon dioxide emissions.
[0004] As another prior art, a technology has been proposed that significantly reduces carbon dioxide compared to the amount of carbon dioxide generated during the manufacturing process (see Patent Document 2). However, this technology (Patent Document 2), which aims to reduce the amount of carbon dioxide generated during the manufacturing process of cement-based compositions such as concrete, does not intend to improve the carbon dioxide absorption capacity of the cement-based composition itself in the natural environment, and does not take into consideration the regeneration (restoration) of the carbon dioxide absorption capacity or the carbon dioxide released when regenerating (restoring) the carbon dioxide absorption capacity. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6080122 [Patent Document 2] Patent No. 5504000 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been proposed in consideration of the above-mentioned problems of the conventional technology, and aims to provide a cement-based composition that improves the carbon dioxide absorption capacity of the cement-based composition itself in a natural environment and regenerates (recovers) the carbon dioxide absorption capacity of the cement-based composition itself. Another object of the present invention is to provide a technique capable of preventing carbon dioxide from being released into the atmosphere during production or during regeneration (restoration) of carbon dioxide absorption capacity. [Means for solving the problem]
[0007] The cementitious composition of the present invention contains a material that absorbs carbon dioxide (CO2), Carbon dioxide absorbing materials are characterized by the ability to absorb CO2 at room temperature and pressure, and release the absorbed CO2 when heated to 100 to 300°C. Alternatively, the cement-based composition of the present invention is characterized in that it absorbs CO2 at room temperature and pressure, and releases the absorbed CO2 when heated to 100 to 300°C, thereby regenerating the CO2 absorption capacity. The CO2 absorbing material includes alkali metal carbonates (potassium carbonate, sodium carbonate, etc.), cerium oxide, sodium ferrite, etc., and in the present invention, potassium carbonate and sodium ferrite are preferred.
[0008] In implementing the cementitious composition of the present invention, the CO2 absorbing material can be encapsulated in a water-soluble capsule so that the CO2 absorbing material does not absorb CO2 at room temperature and pressure. Alternatively, the CO2 absorbing material can be covered with asphalt, resin, etc.
[0009] The cementitious composition of the present invention preferably contains 0.5 to 20% by volume of the CO2 absorbing material. In the present invention, in order to improve the strength and other physical properties, fibers, admixtures (for example, water reducing agents) and / or admixtures (for example, ground granulated blast furnace slag) can be added. In the present invention, part or all of the cement, which is the solidifying agent, can be replaced with ground granulated blast furnace slag or fly ash.
[0010] The method for producing a cement-based composition of the present invention is characterized by having a step of mixing a material (CO2 absorbent) that has the property of absorbing CO2 at room temperature and pressure and releasing the absorbed CO2 when heated to 100 to 300°C (in the process of producing a cement-based composition that has not yet hardened) with a solidification material and water (e.g., a solidification material, aggregate, water, admixture and / or admixture). In the manufacturing method of the present invention, the CO2 absorbent is preferably potassium carbonate or sodium ferrite.
[0011] In addition, the manufacturing method of the present invention preferably includes a step of heating a cementitious composition (e.g., dismantled concrete of the present invention) containing a CO2 absorbent that has lost its ability to absorb CO2 or has a reduced CO2 absorption capacity to regenerate (restore) the ability to absorb CO2, and a step of adding the cementitious composition (CO2 absorption performance regenerated material) containing a CO2 absorbent that has regenerated (restored) its ability to absorb CO2 to a mixture of a CO2 absorbing material that has not yet been used (a new CO2 absorbing material), a solidifying material, aggregate, water, admixtures and / or admixtures (e.g., a mixture of a new CO2 absorbing material, a solidifying material, aggregate, water, admixtures and / or admixtures). Here, the unused CO2 absorbing material (the novel CO2 absorbing material) can be mixed with the solidification material, aggregate, water, admixture and / or admixture at the manufacturing facility, or the unused CO2 absorbing material (the novel CO2 absorbing material) can be mixed at the construction site with the mixture of the solidification material, aggregate, water, admixture and / or admixture that has been transported to the construction site. In addition, in the process of heating a CO2-absorbing cementitious composition (e.g., demolished concrete of the present invention) that has lost or reduced its ability to absorb CO2, to regenerate (recover) its ability to absorb CO2, it is preferable to recover the released CO2.
[0012] The method for recovering carbon dioxide (CO2) of the present invention comprises: A regeneration step of heating a CO2 absorbing cementitious composition (e.g., a demolished concrete of the present invention) that has lost or reduced its ability to absorb CO2, to regenerate (recover) its ability to absorb CO2; The method is characterized by having a recovery process of recovering the CO2 released from the cementitious composition containing the CO2 absorbent when the CO2 absorption capacity is regenerated (recovered) in the regeneration process.
[0013] The method for recovering CO2 of the present invention further comprises the steps of: A heating step of heating an area where a CO2 absorbing cementitious composition having the ability to absorb CO2 has been applied (cast) to release CO2 from the applied (cast) CO2 absorbing cementitious composition; It is characterized by having a recovery process for recovering the CO2 released in the heating process. Effect of the Invention
[0014] The cement-based composition of the present invention having the above-mentioned configuration contains potassium carbonate, sodium ferrite, etc. as a CO2 absorbing material in a volume ratio of 0.5 to 20% relative to the cement-based composition. According to the inventor's experiments, the cement-based composition of the present invention absorbs about 5 to 50% more CO2 than a normal cement-based composition (a cement-based composition that does not contain a CO2 absorbing material such as potassium carbonate, sodium ferrite, etc.). Therefore, the object of the present invention, which is to improve the CO2 absorption capacity of the cement-based composition, can be achieved. The cementitious composition of the present invention contains a CO2 absorbing material, which absorbs CO2 at normal temperature and pressure, and therefore does not require any special operation for absorbing CO2. In addition, according to the CO2 absorbing cement composition of the present invention, the CO2 absorbing material absorbs CO2 from the atmosphere, so the rate at which concrete containing the CO2 absorbing material of the present invention (CO2 absorbing concrete) is neutralized (neutralization rate) is slower than that of concrete that does not contain the CO2 absorbing material. Therefore, for example, if the cement composition of the present invention is cast into reinforced concrete, it is expected that the time until the reinforcing steel corrodes after casting will be extended. Furthermore, the CO2 absorbing concrete, which is the CO2 absorbing cement-based composition of the present invention, has the same properties after hardening (strength characteristics such as compression and bending, shrinkage characteristics, abrasion resistance, skid resistance, etc.) as concrete that does not contain the CO2 absorbing material.
[0015] The method for recovering CO2 of the present invention further comprises the steps of: The method includes a recovery process for recovering the CO2 released when a CO2-absorbing cementitious composition (e.g., demolished concrete of the present invention) that has lost its ability to absorb CO2 or whose CO2 absorption performance has decreased is heated to regenerate (restore) its ability to absorb CO2, or for recovering the CO2 released from the constructed (cast) CO2-absorbing cementitious composition by heating an area where a CO2-absorbing cementitious composition having CO2 absorption ability has been constructed (cast). This makes it possible to prevent the released CO2 from diffusing into the atmosphere and increasing CO2 emissions. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is an explanatory diagram showing a manufacturing facility for manufacturing a CO2 absorbing cement-based composition using only novel materials. [Diagram 2] FIG. 2 is an explanatory diagram showing a manufacturing facility for manufacturing a CO2 absorbing cement-based composition using only novel materials, which is different from FIG. 1. [Diagram 3] FIG. 1 is an explanatory diagram showing an equipment for producing a CO2-absorbing cement-based composition by reviving (restoring) the CO2 absorption performance of a CO2-absorbing cement-based composition whose CO2 absorption capacity has been lost or reduced, and reusing the composition, and at the same time, recovering the CO2 released when the CO2 absorption capacity is revitalized (recovered). [Figure 4]FIG. 4 is an explanatory diagram showing an embodiment different from that shown in FIG. 3 of an equipment for producing a CO2-absorbing cement-based composition by reviving (restoring) the CO2 absorption performance of a CO2-absorbing cement-based composition that has lost or decreased its CO2 absorption capacity and reusing the composition, and at the same time, recovering the CO2 released when reviving (restoring) the CO2 absorption performance. [Diagram 5] FIG. 1 is an explanatory diagram showing a mechanism in which a heater vehicle is used to release CO2 from a laid CO2 absorbent cement composition to restore (recover) the CO2 absorption performance, and the released CO2 is captured by a CO2 capture vehicle. [Figure 6] FIG. 2 is a diagram showing a formulation of a cement-based composition according to an embodiment in the form of a table. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described. Cementitious compositions (such as concrete and cement paste) according to embodiments of the present invention contain a material that absorbs carbon dioxide (CO2). A material that absorbs CO2 is a material that has the property of absorbing CO2 at room temperature and pressure and releasing the absorbed CO2 when heated to 100°C or higher (for example, 100 to 300°C). Examples of such materials include potassium carbonate and sodium ferrite. The cementitious composition according to the embodiment contains potassium carbonate, sodium ferrite, etc. in a volume ratio of 0.5 to 20% relative to the cementitious composition. According to the inventor's experiments, the cementitious composition according to the embodiment of the present invention absorbs about 5 to 50% more CO2 than a normal cementitious composition (a cementitious composition that does not contain a material that absorbs CO2, such as potassium carbonate, sodium ferrite, etc.). Therefore, it meets the object of the present invention to improve the CO2 absorption capacity of the cementitious composition. The cement used in the illustrated embodiment may be Portland cement (ordinary Portland cement, high-early-strength Portland cement, extra-high-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, sulfate-resistant Portland cement), blended cement (blast-furnace cement specified in JIS R 5211, silica cement specified in JIS R 5212, fly ash cement specified in JIS R 5213), or ecocement specified in JIS R 5214.
[0018] As described later, cementitious compositions such as concrete will explode, deteriorate, and discolor when heated to around 600°C. In addition, the strength of concrete will decrease significantly when heated above 300°C. Therefore, materials that release CO2 at temperatures above 300°C cannot be used as CO2 absorbers. In the case of the above-mentioned CO2 absorbents such as potassium carbonate and sodium ferrite, the temperature at which they release CO2 is 100 to 300°C, which is below 300°C. For example, potassium carbonate starts to release (desorb) CO2 at 110 to 140°C. Therefore, when heating to restore (recover) the ability to absorb CO2, it is possible to release the absorbed CO2 without reducing the strength, spalling, deterioration, or discoloration of the cement-based composition such as concrete, and it is also possible to restore (recover) the ability to absorb CO2.
[0019] In experiments conducted by the inventors, when the content of a CO2 absorbing material such as potassium carbonate or sodium ferrite is less than 0.5% by volume of the cementitious composition, the CO2 absorbing ability may not be significantly different from that of a normal cementitious composition (a cementitious composition that does not contain a CO2 absorbing material such as potassium carbonate or sodium ferrite). On the other hand, when the content is more than 20% by volume of the cementitious composition, the properties after hardening (strength characteristics such as compression and bending, shrinkage characteristics, abrasion resistance, slip resistance, etc.) are inferior to cementitious compositions such as concrete that do not contain a CO2 absorbing material. In contrast, when the content of CO2 absorbing materials such as potassium carbonate and sodium ferrite is 0.5 to 20% by volume relative to the cementitious composition, the ability to absorb CO2 is improved compared to ordinary cementitious compositions, and as the content of CO2 absorbing materials such as potassium carbonate and sodium ferrite increases, the ability to absorb CO2 is improved, and the properties after hardening are equivalent to those of cementitious compositions such as concrete that do not contain CO2 absorbing materials.
[0020] Concrete (CO2 absorbing concrete), which is a cementitious composition according to the embodiment, absorbs CO2 at room temperature and pressure, so no special operations are required to absorb CO2. According to experiments by the inventors, the neutralization rate of the CO2 absorbing concrete according to the embodiment was slower (the neutralization rate was reduced) than that of normal concrete that does not contain a CO2 absorbing material. This is thought to be due to the fact that materials that absorb CO2, such as potassium carbonate and sodium ferrite, absorb CO2 from the atmosphere. From these experimental results, it can be expected that the CO2 absorbing concrete according to the embodiment will prolong the period until rebar corrosion occurs.
[0021] In addition, in another experiment conducted by the inventors, it was confirmed that the CO2 absorbing concrete using the cementitious composition according to the embodiment had the same properties after hardening (strength characteristics such as compression and bending, shrinkage characteristics, abrasion resistance, slip resistance, etc.) as ordinary concrete that did not contain a CO2 absorbing material.
[0022] When manufacturing the cement-based composition according to the embodiment, there is a risk that the CO2 absorbing material (potassium carbonate, sodium ferrite, etc.) will absorb CO2 at room temperature and pressure before manufacturing. In response to this, the CO2 absorbing material (potassium carbonate, sodium ferrite, etc.) can be encapsulated in a water-soluble material (for example, in a microcapsule or oblate) to prevent the CO2 absorption until the CO2 absorbing material is mixed with water, and the CO2 absorption capacity after use can be extended. Similarly, by covering a CO2 absorbing material (potassium carbonate, sodium ferrite, etc.) with asphalt or resin, the CO2 absorbing material (potassium carbonate, sodium ferrite, etc.) can be prevented from absorbing CO2 before the cement-based composition according to the embodiment is produced. When covering a CO2 absorbing material (potassium carbonate, sodium ferrite, etc.) with asphalt, the CO2 absorbing material is heated when covered with asphalt, so that the CO2 absorbed before the production of the CO2 absorbing cement-based composition can be released and the CO2 absorption performance can be restored (recovered). In addition, sodium ferrite has the property of being decomposed by immersion in water, so that decomposition can be prevented by covering with asphalt.
[0023] In order to improve various properties such as strength properties in the cement-based composition according to the embodiment, in addition to the material that absorbs CO2 (potassium carbonate, sodium ferrite, etc.), it is also possible to add fibers, admixtures and / or admixtures. In the inventor's experiments, it was found that fibers commonly used in concrete, such as PVA (vinylon) fibers, PP (polypropylene) fibers, steel fibers, etc., were applicable as fibers. In addition, it was found that water-reducing agents, superplasticizers, etc. were applicable as admixtures, and blast furnace slag powder, fly ash, etc. were applicable as admixtures. In addition, in another experiment conducted by the inventors, it was found possible to replace part or all of the cement, which is a solidification material, with other solidification materials such as ground granulated blast furnace slag or fly ash. FIG. 6 illustrates an example of the formulation of a cementitious composition according to an embodiment of the present invention. In each of Figs. 6(1) to (6), the values in the second row indicate a suitable blending example, and the values in the third row indicate the range of the composition (upper and lower limits). Here, in Figure 6, "W" stands for water, "C" stands for cement, "S" stands for fine aggregate, "G" stands for coarse aggregate, "G(4005)" stands for coarse aggregate with a particle size of 40 to 5 mm, "CO2" stands for CO2 absorbent, and "SF" stands for steel fiber. Furthermore, "cement paste" stands for something used as cement milk for semi-flexible pavement.
[0024] Here, if the water-cement ratio is too high, the strength may decrease, whereas if it is too low, workability may not be ensured. If the fine aggregate ratio and water are too high or too low, workability may not be ensured. To ensure appropriate consistency (workability), it is desirable to keep them within the range shown in Figure 6. Regarding cement, if there is too much, the risk of damage such as shrinkage and cracks after hardening increases and the economics become poor. On the other hand, if there is too little cement, there is a possibility that the strength cannot be secured. It was also found that too much CO2 absorbent may result in insufficient strength or ease of construction, while too little may result in insufficient CO2 absorption performance. Based on these findings, the mix example in Figure 6 was determined. The mix example in Figure 6 can be used as the cement milk for "semi-flexible pavement."
[0025] Next, the production of a cement-based composition according to an embodiment will be described with reference to FIGS. FIG. 1 shows a case where a CO2 absorbing cement-based composition is produced in a production facility (production plant) using only new materials (materials that are not recycled materials). In Fig. 1, a manufacturing plant generally indicated by reference numeral 10 has therein a CO2 absorbing material storage device 12 for storing a new CO2 absorbing material, an aggregate storage device 14 for storing a new aggregate, a cement storage device 16 for storing a new cement, a water storage device 18, an admixture and / or admixture storage device 19, and a mixer 20 (mixer). Here, the term "new" means that the material has not been used in the past as a material for a cement-based composition.
[0026] The CO2 absorbing material storage device 12 is supplied with a CO2 absorbing material (such as potassium carbonate or sodium ferrite) from a CO2 absorbing material supply system (not shown), and supplies the CO2 absorbing material to the mixer 20 via a path L1. The aggregate storage device 14 is supplied with aggregate (eg, sand) from an aggregate supply system (not shown), and supplies the aggregate to the mixer 20 via a path L2. Cement is supplied to the cement storage device 16 from a cement supply system (not shown), and the cement is supplied to the mixer 20 via a path L3. Water (for example, tap water) is supplied to the water storage device 18 from a water supply system (not shown), and the water is supplied to the mixer 20 via a path L4. The admixture and / or additive storage device 19 is supplied with admixtures (e.g., water reducing agents) and / or admixtures (e.g., ground granulated blast furnace slag) from an admixture and / or additive supply system (not shown), and supplies the admixtures and / or additives to the mixer 20 via path L7. The paths L1 to L4 and L7 can be configured with known supply equipment such as pipelines and conveyors.
[0027] In the mixer 20, the CO2 absorbing material, aggregate, cement, water, admixtures and / or admixtures are mixed, and the mixture, i.e., the pre-solidified CO2 absorbing cementitious composition, is fed into a hopper 24 of a vehicle 22 having a storage device 23 via a path L5. When the CO2 absorbing material is encapsulated in water-soluble capsules, the water-soluble capsules dissolve when mixed in the mixer 20, and the CO2 absorbing material comes into contact with and is mixed with the cement or the like. Here, it is preferable that the vehicle 22 be a so-called "agitator vehicle" so that the cementitious composition is prevented from solidifying and the storage device 23 is constantly rotating to keep the cementitious composition agitated. The vehicle 22 travels to a site where the cementitious composition is to be poured, and the cementitious composition is poured and installed at the site (arrow A1).
[0028] Here, if the CO2 absorbing material is added in the manufacturing plant 10, there is a risk that the CO2 absorbing material will absorb CO2 before being installed at the site, thereby reducing the amount of CO2 that can be absorbed at the installation site. In order to eliminate such inconveniences, the manufacturing plant 10A shown in FIG. 2 is provided with an aggregate storage device 14, a cement storage device 16, a water storage device 18, and an admixture and / or admixture storage device 19, but does not have any device equivalent to the CO2 absorbing material storage device 12 in FIG. 1. The aggregate stored in the aggregate storage device 14, the cement stored in the cement storage device 16, the water stored in the water storage device 18, and the admixture and / or admixture stored in the admixture and / or admixture storage device 19 are mixed in a mixer 20 and fed into a hopper 24 of a vehicle 22 (agitator vehicle). The agitator vehicle 22 travels to the construction site generally indicated by reference numeral 30 in FIG. 2 (arrow A2). Other configurations and functions and effects of the manufacturing plant 10A in FIG. 2 are similar to those of the manufacturing plant 10 in FIG. 1, and therefore description thereof will be omitted.
[0029] A CO2 absorbing material storage device 12A is provided at the construction site 30, and the CO2 absorbing material storage device 12A receives new CO2 absorbing material from a CO2 absorbing material supply system (not shown), and feeds the new CO2 absorbing material into the hopper 24 of the agitator vehicle 22 via path L1A. When the agitator vehicle 22 arrives at the construction site 30, the storage device 23 of the agitator vehicle 22 is already charged with a mixture of aggregate, cement, water, admixtures and / or admixtures (cementitious composition), and the CO2 absorbing material is added and mixed with the cementitious composition and stirred, so that the contents of the storage device 23 become a CO2 absorbing cementitious composition. The stirred CO2 absorbing cementitious composition is immediately poured and constructed at the construction site 30 (arrow A2). Here, since the CO2 absorbing material is loaded into the agitator vehicle 22 at the construction site 30, the time from loading the CO2 absorbing material to pouring and construction of the CO2 absorbing cement composition is shortened at least by the time it takes the agitator vehicle 22 to travel from the manufacturing plant 10A to the construction site 30, as compared with the case shown in Fig. 1, and the time that the CO2 absorbing material that has not been installed or poured absorbs CO2 is also shortened. Therefore, according to the manufacturing embodiment shown in Fig. 2, the possibility of a decrease in the amount of CO2 that can be absorbed at the construction site is reduced, as compared with the embodiment in Fig. 1.
[0030] In the embodiment shown in Fig. 1 and Fig. 2, only new materials (materials not used in cementitious compositions in the past) are used. However, it is also possible to reuse existing CO2-absorbing cementitious compositions that have been applied in the past and have lost or decreased their CO2-absorbing performance. In other words, when manufacturing a CO2-absorbing cementitious composition using the cementitious composition according to the embodiment, it is possible to reuse CO2-absorbing cementitious compositions that have been applied and cast in the past. An embodiment of producing a CO2-absorbing cementitious composition by reusing a CO2-absorbing cementitious composition that has been applied or cast in the past is shown in Figs. 3 and 4.
[0031] The embodiment shown in FIG. 3, like FIG. 1, shows an embodiment in which the production of a CO2 absorbing cementitious composition by reusing a CO2 absorbing cementitious composition is carried out in a production facility (production plant). In order to implement the embodiment of Fig. 3, a storage facility 40, a regeneration facility 50, a CO2 absorbing performance regenerator storage device 60, and a manufacturing facility 10C (manufacturing plant) are provided. In Fig. 3, reference numeral 22 denotes a transport vehicle, which is preferably an agitator vehicle. The storage facility 40 is a facility for storing, as waste material, the CO2 absorbing cementitious composition that has absorbed CO2 and lost or reduced its CO2 absorption capacity, and has a second storage device 42 for storing the cementitious composition that has lost or reduced its CO2 absorption capacity. The CO2 absorbing cementitious composition stored in the second storage device 42, which has lost or reduced CO2 absorption capacity, is supplied to the crushing device 52 of the regeneration facility 50 via a path L11.
[0032] The regeneration facility 50 is equipped with a crushing device 52, a heating device 54, and a CO2 capture device 56. The crushing device 52 crushes the CO2 absorbing cementitious composition (a CO2 absorbing cementitious composition that has lost its CO2 absorption capacity or has reduced CO2 absorption performance) transported from the storage facility 40 (second storage device 42) via path L11, and supplies the crushed CO2 absorbing cementitious composition to the heating device 54 via path L12. The heating device 54 heats the CO2 absorbing cement-based composition that has lost its CO2 absorbing capacity or has reduced CO2 absorbing performance, which has been crushed by the crushing device 52. By heating with the heating device 54, the CO2 absorbed by the CO2 absorbing material is released, and the CO2 absorbing performance of the CO2 absorbing material or the CO2 absorbing cement-based composition is restored (regenerated). Then, the CO2 absorbing performance regenerated material (crushed and heated CO2 absorbing cement-based composition) whose CO2 absorbing performance has been restored (regenerated) is supplied to the CO2 absorbing performance regenerated material storage device 60 via the path L13. The CO2 released during heating in the heating device 54 is captured in the CO2 capture device 56.
[0033] Here, the CO2 absorption performance regenerated material, whose CO2 absorption performance has been restored (recovered) by the heating device 54, is heated to 100 to 300°C. As described above, the CO2 absorption material used in the embodiment releases (regenerates) the absorbed CO2 when heated to 100 to 300°C, so there is no need to heat it above 300°C, at which the strength of the cement-based composition is significantly reduced. Therefore, the strength, etc. of the regenerated CO2 absorption performance regenerated material does not decrease. In addition, since the temperature required for regeneration is 100 to 300°C, the energy or fuel required for heating is not consumed in large quantities, as compared with a cement-based composition that uses lithium silicate as a CO2 absorbent.
[0034] As described above, by heating the CO2 absorbing cement composition at 100 to 300°C in the heating device 54, CO2 is released from the CO2 absorbing cement composition which has lost or reduced its CO2 absorbing capacity, and the released CO2 is captured by the CO2 capture device 56 via the path L14. The CO2 capture device 56 may be any device according to any known technology. The CO2 capture device 56 supplies the captured CO2 to a known CO2 utilization device via a route not shown in the figure without discharging it into the atmosphere. This makes it possible to effectively utilize the CO2 generated when the CO2 absorption performance of the CO2 absorption cement composition is restored without being released into the atmosphere.
[0035] 1, the manufacturing plant 10C includes a storage device 12 for storing new CO2 absorbing material, a storage device 14 for storing new aggregate, a device 16 for storing new cement, a water storage device 18, and an admixture and / or admixture storage device 19. Also, the manufacturing plant 10C includes a mixer 20C as a mixing device. As in the manufacturing plant 10 of FIG. 1, in the manufacturing plant 10C of FIG. 3, new CO2 absorbing material, new aggregate, new cement, water, admixture and / or admixture are fed into the mixer 20C and kneaded. In addition, in the manufacturing plant 10C of FIG. 3, the CO2 absorbing performance regenerated material (crushed and heated CO2 absorbing cement composition) whose CO2 absorbing performance has been restored (recovered) and stored in the CO2 absorbing performance regenerated material storage device 60 is fed into the mixer 20C via the path L15. Therefore, when the content of the CO2 absorbing material in the regenerated CO2 absorbing cement composition is insufficient, the new CO2 absorbing material may be supplied to the mixer 20C only in the amount of the deficiency (the amount of the deficiency relative to the required amount). A new CO2 absorbing material, a new aggregate, a new cement, a CO2 absorbing recycled material, water, and admixtures and / or admixtures are charged into the mixer 20C and mixed together to produce a CO2 absorbing cement-based composition using the CO2 absorbing recycled material (a CO2 absorbing cement-based composition using recycled material).
[0036] The CO2 absorbing cementitious composition using the CO2 absorbing performance recycled material kneaded in the mixer 20C is loaded into the hopper 24 of the transport vehicle 22 (preferably an agitator vehicle) via the route L5C, transported to the construction site, and constructed and poured (arrow A3). Other configurations and effects of the plant 10C in FIG. 3 are similar to those of the manufacturing plant 10 in FIG.
[0037] In the embodiment of Fig. 3, since the recycled CO2 absorbing recycled material is used, the consumption of new cement, new aggregate, and new CO2 absorbing material can be reduced. The recycled CO2 absorbing cement-based composition using recycled materials including the recycled CO2 absorbing recycled material can be reused as, for example, a roadbed that absorbs CO2 or a CO2 absorbing cement-based composition. According to separate experiments conducted by the inventors, the CO2 absorbing material can be regenerated and reused multiple times. Furthermore, the CO2 absorbed in the used CO2 absorbing cementitious composition (CO2 absorbing cementitious composition that has lost or reduced its CO2 absorbing capacity) can be recovered and reused by known techniques. As a result, the amount of CO2 emitted into the atmosphere can be reduced.
[0038] As explained with reference to FIG. 2, even in the case of FIG. 3 in which a regenerated CO2 absorption performance regenerated material is used, new CO2 absorbing material is added in the manufacturing plant 10C. Thereafter, the new CO2 absorbing material may absorb CO2 before being installed at the site, and the amount of CO2 that the new CO2 absorbing material can absorb at the installation site may decrease. In order to eliminate such inconveniences, as shown in Figure 4, a novel CO2 absorbing material can be added to a recycled CO2 absorbing cement-based composition consisting of aggregate, cement, water, admixture and / or admixture, and a CO2 absorbing performance recycled material at the construction site.
[0039] In FIG. 4, the storage facility 40, the regeneration facility 50, and the CO2 absorbent regenerated material storage device 60 are similar to those described with reference to FIG. 3, and therefore detailed description thereof will be omitted. The manufacturing facility 10D (manufacturing plant) in FIG. 4 is similar to the manufacturing plant 10A shown in FIG. 2, and is provided with an aggregate storage device 14, a cement storage device 16, and a water storage device 18, but does not include a device corresponding to the storage device 12 for the novel CO2 absorbing material in FIG. 3. In Fig. 4, new aggregate stored in aggregate storage device 14, new cement stored in cement storage device 16, water stored in water storage device 18, and admixture and / or additive stored in admixture and / or additive storage device 19 are kneaded in mixer 20D. In addition, in the manufacturing plant 10D in Fig. 4, the CO2 absorbing performance regenerated material (crushed and heated CO2 absorbing cementitious composition) whose CO2 absorbing performance has been restored (recovered) and stored in CO2 absorbing performance regenerated material storage device 60 is fed into mixer 20D via path L15D. The recycled CO2 absorbing recycled material, new aggregate, new cement, water, and admixtures and / or admixtures are fed into the mixer 20D and mixed together to produce a CO2 absorbing cement-based composition using the CO2 absorbing recycled material (a CO2 absorbing cement-based composition using recycled material).
[0040] The CO2 absorbing cementitious composition using the recycled materials kneaded in the mixer 20D is put into the hopper 24 of the transport vehicle 22 (agitator vehicle) via the route L5D, and is transported to the construction site 30D (arrow A5). Other configurations and functions and effects of the production plant 10D in FIG. 4 are similar to those of the production plant 10 in FIG. 1 or the production plant 10A in FIG. 2, and therefore description thereof will be omitted.
[0041] A CO2 absorbing material storage device 12D storing new CO2 absorbing material is provided at the construction site 30D, and new CO2 absorbing material is supplied to the CO2 absorbing material storage device 12D from a CO2 absorbing material supply system not shown, and the new CO2 absorbing material is fed into the hopper 24 of the agitator vehicle 22 via a path L1D. The storage device 23 of the agitator vehicle 22 that has arrived at the construction site 30D has already been charged with the regenerated CO2 absorbing cementitious composition. When the content of the CO2 absorbing material in the regenerated CO2 absorbing cementitious composition is insufficient, the new CO2 absorbing material charged via the path L1D is supplied to the agitator vehicle 22 only in the amount corresponding to the shortage (the amount relative to the required amount).
[0042] The CO2 absorbing cement composition, which is mixed and stirred with the new CO2 absorbing material, is immediately cast and applied at the construction site 30D (arrow A5). Here, the new CO2 absorbing material is fed into the agitator vehicle 22 at the construction site 30D, so the time from the feeding of the new CO2 absorbing material to the casting and application of the recycled material-using CO2 absorbing cement composition is shortened at least by the time the agitator vehicle 22 travels from the manufacturing plant 10D to the construction site 30D (only the reference number and the lead line are shown in FIG. 3) compared to the case shown in FIG. 3. Therefore, the time that the CO2 absorbing material that has not been applied or cast absorbs CO2 is also shortened, and the manufacturing embodiment shown in FIG. 4 reduces the possibility of a decrease in the amount of CO2 that can be absorbed at the construction site compared to the embodiment in FIG. 3. In FIG. 4, since the CO2 absorbing cement composition using the CO2 absorbing performance recycled material is loaded into the vehicle 22 in the manufacturing plant 10D, it is preferable to use an agitator vehicle as the transport vehicle 22 in order to prevent the composition from solidifying.
[0043] In Figures 3 and 4, CO2 released from a CO2 absorbing cementitious composition (a CO2 absorbing cementitious composition that has lost or reduced CO2 absorption capacity) is recovered in a CO2 absorbing cementitious composition regeneration facility. However, the mechanism for releasing and capturing CO2 from CO2 absorbing cementitious compositions that have lost their CO2 absorption capacity is not only provided in regeneration facilities. For example, as shown in Figure 5, it is possible to release and capture CO2 from an installed CO2 absorbing cementitious composition.
[0044] In Fig. 5, the CO2 absorbing cement composition laid on the road surface has lost its CO2 absorbing capacity or has a reduced CO2 absorbing capacity, and a road surface CO2 absorbing cement composition regenerating vehicle, generally designated by reference numeral 70, is running on the CO2 absorbing cement composition RC. In Fig. 5, reference numeral F indicates the traveling direction of the road surface CO2 absorbing cement composition regenerating vehicle 70. Here, the CO2-absorbing cementitious composition RC is a CO2-absorbing cementitious composition according to an embodiment of the present invention. The road surface CO 2 absorption cement-based composition regeneration vehicle 70 has a hot air circulation heater vehicle 72 and a CO 2 recovery vehicle 74 .
[0045] The hot air circulation heater vehicle 72 has a function of blowing hot air (arrow 70A) onto the surface (road surface) of the laid CO2 absorbing cementitious composition RC so that the surface temperature (road surface temperature) becomes 100 to 300° C. A conventionally known structure is used for blowing hot air to heat the road surface to 100 to 300° C. As described above, the CO2 absorbing concrete according to the embodiment of the present invention releases the absorbed CO2 when heated to 100 to 300° C. Therefore, by blowing hot air 70A onto the road surface, the CO2 is released.
[0046] Following the hot air circulation heater vehicle 72, a CO2 capture vehicle 74 runs on the road surface onto which hot air 70A is blown. Although not clearly shown, the CO2 capture vehicle 74 has a built-in mechanism for sucking in and capturing CO2 released from the road surface and storing the captured CO2. The CO2 released from the road surface of the CO2 absorbing cementitious composition RC by blowing hot air 70A from a hot air circulation heater vehicle 72 is sucked in by a mechanism (not shown) in a CO2 capture vehicle 74 as shown by arrow 70B and stored. Furthermore, the CO2 in the gas discharged from a heater (not shown) of the hot air circulation heater vehicle 72 can also be captured in the CO2 capture vehicle 74.
[0047] The CO2 absorbing cementitious composition RC that has released CO2 by being blown with hot air 70A from the hot air circulation heater vehicle 72 recovers (restores) its CO2 absorbing ability (regenerates). The CO2 released from the CO2 absorbing cementitious composition RC is stored by a mechanism (not shown) in the CO2 capture vehicle 74, and is not discharged into the atmosphere. The CO2 stored by a mechanism (not shown) in the CO2 capture vehicle 74 can be reused by a known technology (not shown).
[0048] It should be noted that the illustrated embodiment is merely an example and is not intended to limit the technical scope of the present invention. [Explanation of symbols]
[0049] 10, 10A, 10C, 10D... Manufacturing plant 12, 12A: Novel CO2 absorption material storage device 12 14. Aggregate storage device 16. Cement storage device 18. Water storage device 19. Admixtures and / or admixture storage equipment 20, 20C, 20D...Mixing device (mixer) 22. Vehicle 23 Storage device 24 Hopper 30, 30D...Construction site 40 Storage facilities 42...Second storage device 50...Reproduction equipment 50 52 Crushing device 54...Heating device 56...CO2 capture equipment 60···CO2 absorption capacity recycled material storage device RC: CO2 absorbing cement-based composition laid on road surfaces, etc. 70... Road surface cement-based composition recycled vehicle 70A...Hot air 72 Hot air circulation heater vehicle 74 CO2 Capture Vehicle
Claims
1. To prepare paving concrete, which is a cement-based composition, the water-cement ratio is 37-44%, and the fine aggregate ratio is 35-44%, and the paving concrete is mixed with 130-150 kg of water, 295-405 kg of cement, and 50-100 kg of a material that absorbs carbon dioxide per square meter, The carbon dioxide absorbing material absorbs carbon dioxide at normal temperature and pressure, and releases the absorbed carbon dioxide when heated to 100 to 300°C. 2 It has the property of regenerating absorption performance, The carbon dioxide absorbing material is encapsulated in a water-soluble capsule to prevent the carbon dioxide absorbing material from absorbing carbon dioxide until it is mixed with water; The method for producing a cement-based composition, wherein the carbon dioxide absorbing material is sodium ferrite.
2. To prepare structural concrete, which is a cement-based composition, the structural concrete has a water-cement ratio of 45-60% and a fine aggregate ratio of 40-50%, and the structural concrete is made by mixing 150-170 kg of water, 250-378 kg of cement, and 50-100 kg of a material that absorbs carbon dioxide per square meter, The carbon dioxide absorbing material absorbs carbon dioxide at normal temperature and pressure, and releases the absorbed carbon dioxide when heated to 100 to 300°C. 2 It has the property of regenerating its absorption capacity. The carbon dioxide absorbing material is encapsulated in a water-soluble capsule to prevent the carbon dioxide absorbing material from absorbing carbon dioxide until it is mixed with water; The method for producing a cement-based composition, wherein the carbon dioxide absorbing material is sodium ferrite.
3. To construct steel fiber reinforced concrete, which is a cement-based composition, the water-cement ratio of the steel fiber reinforced concrete is 35-45%, and the fine aggregate ratio is 40-55%, and the steel fiber reinforced concrete is mixed with 160-200 kg of water, 356-571 kg of cement, and 50-100 kg of a material that absorbs carbon dioxide per square meter, The carbon dioxide absorbing material absorbs carbon dioxide at normal temperature and pressure, and releases the absorbed carbon dioxide when heated to 100 to 300°C. 2 It has the property of regenerating its absorption capacity. The carbon dioxide absorbing material is encapsulated in a water-soluble capsule to prevent the carbon dioxide absorbing material from absorbing carbon dioxide until it is mixed with water; The method for producing a cement-based composition, wherein the carbon dioxide absorbing material is sodium ferrite.
4. To prepare early traffic open type concrete, which is a cement-based composition, the water-cement ratio of the early traffic open type concrete is 30-41%, and the fine aggregate ratio is 32-47%, and the early traffic open type concrete is mixed with 145-170 kg of water, 354-567 kg of cement, and 50-100 kg of a material that absorbs carbon dioxide per square meter, The carbon dioxide absorbing material absorbs carbon dioxide at normal temperature and pressure, and releases the absorbed carbon dioxide when heated to 100 to 300°C. 2 It has the property of regenerating its absorption capacity. The carbon dioxide absorbing material is encapsulated in a water-soluble capsule to prevent the carbon dioxide absorbing material from absorbing carbon dioxide until it is mixed with water; The method for producing a cement-based composition, wherein the carbon dioxide absorbing material is sodium ferrite.
5. To compose cement mortar, which is a cement-based composition, the water-cement ratio of the cement mortar is 45-55%, and the cement mortar contains 244-261 kg of water, 435-610 kg of cement, and 50-100 kg of a material that absorbs carbon dioxide per square meter; The carbon dioxide absorbing material absorbs carbon dioxide at normal temperature and pressure, and releases the absorbed carbon dioxide when heated to 100 to 300°C. 2 It has the property of regenerating its absorption capacity. The carbon dioxide absorbing material is encapsulated in a water-soluble capsule to prevent the carbon dioxide absorbing material from absorbing carbon dioxide until it is mixed with water; The method for producing a cement-based composition, wherein the carbon dioxide absorbing material is sodium ferrite.
6. To form a cement paste, which is a cement-based composition, the cement paste has a water-cement ratio of 40 to 60%, and contains 553 to 648 kg of water, 1,080 to 1,382 kg of cement, and 50 to 100 kg of a material that absorbs carbon dioxide per square meter; The carbon dioxide absorbing material absorbs carbon dioxide at normal temperature and pressure, and releases the absorbed carbon dioxide when heated to 100 to 300°C. 2 It has the property of regenerating its absorption capacity. The carbon dioxide absorbing material is encapsulated in a water-soluble capsule to prevent the carbon dioxide absorbing material from absorbing carbon dioxide until it is mixed with water; The method for producing a cement-based composition, wherein the carbon dioxide absorbing material is sodium ferrite.
7. A material that absorbs carbon dioxide at room temperature and pressure, releases the absorbed carbon dioxide when heated to 100 to 300°C, and has the property of regenerating carbon dioxide absorption performance, is sodium ferrite, The manufacturing method according to any one of claims 1 to 6, wherein sodium ferrite, which is a new material that has not been used in cement-based composition materials in the past, is mixed with a solidification material, an aggregate, water, an admixture and / or an admixture in a manufacturing facility or at a construction site.
8. A regeneration process for heating a cement-based composition containing sodium ferrite as a material for absorbing carbon dioxide and in which the sodium ferrite has lost or reduced ability to absorb carbon dioxide, thereby regenerating the ability of the sodium ferrite to absorb carbon dioxide; The manufacturing method according to claim 7, further comprising a step of adding the cementitious composition material whose ability to absorb carbon dioxide has been regenerated in the regeneration step to a mixture of the sodium ferrite, which is a new material that has not been used in cementitious composition materials in the past, a solidification material, an aggregate, water, and an admixture and / or an admixture.
9. A regeneration step of heating the cementitious composition produced by the method according to any one of claims 1 to 6, which has lost or reduced its ability to absorb carbon dioxide, to release carbon dioxide from the cementitious composition and regenerate its ability to absorb carbon dioxide; A method for regenerating a carbon dioxide absorption capacity and recovering released carbon dioxide, comprising a recovery step of recovering the carbon dioxide released when the carbon dioxide absorption capacity is regenerated in the regeneration step.
10. A heating step of heating an area where the cementitious composition produced by the method according to any one of claims 1 to 6 is applied, thereby releasing carbon dioxide from the applied cementitious composition and regenerating the ability to absorb carbon dioxide; A method for regenerating carbon dioxide absorption capacity and recovering released carbon dioxide, comprising a recovery step of recovering the carbon dioxide released in the heating step.
Citation Information
Patent Citations
Microcapsule and preparation method thereof as well as microcapsule reinforced concrete and preparation method thereof
CN108609880A
Device of forming at least two color images to cylindrical or head cut type article
JP1980004000A
Magnetic recording medium
JP1985080122A
Method for reusing waste concrete
JP2000239670A
Neutralization preventing concrete
JP2002012466A