Method for manufacturing positive electrode for lithium ion secondary battery
By using a high-aspect-ratio conductive material without pressing, the method forms dense conductive paths and maintains porosity in the positive electrode composite layer, addressing the challenge of reduced output in lithium ion secondary batteries.
Patent Information
- Application Number
- JP2020141742
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-08-25
AI Technical Summary
The challenge in manufacturing lithium ion secondary batteries is to form sufficient conductive paths in the positive electrode composite material layer while maintaining high porosity, which is compromised by increasing density through pressing processes.
A method involving the use of a conductive material with an aspect ratio of 80 or more, applied without a pressing step after drying the positive electrode paste, to form a dense conductive network and increase porosity in the positive electrode composite layer.
This approach enhances conductive paths and porosity, reducing electronic resistance and improving the output of the lithium ion secondary battery while simplifying the manufacturing process.
Smart Images

Figure 0007576741000001 
Figure 0007576741000002 
Figure 0007576741000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a positive electrode for a lithium ion secondary battery, a positive electrode for a lithium ion secondary battery, and a lithium ion secondary battery. [Background technology]
[0002] Lithium ion secondary batteries are secondary batteries that can be charged and discharged by the movement of lithium ions in an electrolyte between a positive electrode and a negative electrode, which absorb and release lithium ions.
[0003] Patent Document 1 discloses a technique for a manufacturing method of an electrode for a lithium ion secondary battery that can omit or simplify the rolling process. The technique disclosed in Patent Document 1 makes it possible to omit or simplify the rolling process by using a negative electrode active material powder and a positive electrode conductive agent powder in which a polymer compound component is chemically covalently bonded to the particle surface. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-100360 A Summary of the Invention [Problem to be solved by the invention]
[0005] The positive electrode of the lithium ion secondary battery includes a positive electrode current collector and a positive electrode mixture layer formed on the positive electrode current collector. The positive electrode mixture layer contains a positive electrode active material and a conductive material, and a conductive path is formed in the positive electrode mixture layer by using the conductive material.
[0006] In order to form a sufficient conductive path in the positive electrode mixture layer, it is necessary to increase the density of the positive electrode mixture layer by a pressing process. However, when the density of the positive electrode mixture layer is increased by the pressing process, the porosity of the positive electrode mixture layer is reduced, resulting in a problem of a decrease in the output of the lithium-ion secondary battery.
[0007] In view of the above problems, an object of the present invention is to provide a method for manufacturing a positive electrode for a lithium ion secondary battery, a positive electrode for a lithium ion secondary battery, and a lithium ion secondary battery, which are capable of forming a sufficient conductive path in the positive electrode mixture layer and increasing the porosity of the positive electrode mixture layer. [Means for solving the problem]
[0008] A method for producing a positive electrode for a lithium ion secondary battery according to one aspect of the present invention is a method for producing a positive electrode for a lithium ion secondary battery comprising a positive electrode current collector and a positive electrode composite layer formed on the positive electrode current collector, the method comprising the steps of: preparing a positive electrode paste containing at least a positive electrode active material, a conductive material, and a solvent, applying the positive electrode paste onto the positive electrode current collector, and drying the applied positive electrode paste to form the positive electrode composite layer on the positive electrode current collector. The conductive material contained in the positive electrode paste has an aspect ratio of 80 or more, and the method does not include a pressing step after drying the positive electrode paste.
[0009] A positive electrode for a lithium-ion secondary battery according to one embodiment of the present invention includes a positive electrode current collector and a positive electrode composite layer formed on the positive electrode current collector, the positive electrode composite layer including at least a positive electrode active material and a conductive material, and the conductive material has an aspect ratio of 80 or more.
[0010] A lithium ion secondary battery according to one aspect of the present invention is a lithium ion secondary battery having the above-mentioned positive electrode for lithium ion secondary batteries. Effect of the Invention
[0011] The present invention can provide a method for producing a positive electrode for a lithium ion secondary battery, which is capable of forming a sufficient conductive path in the positive electrode mixture layer and increasing the porosity of the positive electrode mixture layer, a positive electrode for a lithium ion secondary battery, and a lithium ion secondary battery. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a cross-sectional view for explaining a configuration example of a positive electrode for a lithium ion secondary battery according to an embodiment. [Diagram 2] FIG. 2 is a schematic diagram for explaining details of a positive electrode mixture layer included in the positive electrode for a lithium ion secondary battery according to the embodiment. [Diagram 3] 2 is a flowchart for explaining a method for producing a positive electrode for a lithium ion secondary battery according to an embodiment. [Figure 4] FIG. 4 is a cross-sectional view for illustrating another configuration example of the positive electrode for a lithium ion secondary battery according to the embodiment. [Diagram 5] 1 is a graph showing the relationship between the porosity and resistance value of a positive electrode mixture layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a cross-sectional view for explaining a configuration example of a positive electrode for a lithium ion secondary battery according to the present embodiment. Fig. 2 is a schematic diagram for explaining details of a positive electrode mixture layer included in the positive electrode for a lithium ion secondary battery according to the present embodiment. As shown in Fig. 1, a positive electrode for a lithium ion secondary battery 1 according to the present embodiment includes a positive electrode current collector 10 and a positive electrode mixture layer 11 formed on the positive electrode current collector 10.
[0014] The positive electrode current collector 10 is made of a metal foil or a metal plate. For the positive electrode current collector 10, for example, aluminum or an alloy containing aluminum as a main component can be used.
[0015] As shown in FIG. 2, positive electrode mixture layer 11 contains at least positive electrode active material 15 and conductive material 16.
[0016] The positive electrode active material 15 is a material capable of absorbing and releasing lithium ions, and may be, for example, lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel oxide (LiNiO2), lithium aluminate (LiAlO2), or the like. For example, an NCA-based material in which lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), and lithium aluminate (LiAlO2) are mixed in any ratio may be used. As an example, LiNi 0.8 Co 0.15 Al 0.05 LiCoO2, LiMn2O4, and LiNiO2 may be mixed in any ratio. For example, lithium nickel cobalt manganese oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) may also be used.
[0017] The particle size of the positive electrode active material is, for example, 3 to 15 μm. In the present invention, the particle size of each material is the median diameter D50, which is a value measured using a laser diffraction / scattering method. The positive electrode active material is not limited to these materials, and may be any material that can absorb and release lithium ions.
[0018] Conductive material 16 is a material for forming a conductive path in positive electrode composite layer 11, and is adjusted so that the aspect ratio is 80 or more. In this embodiment, the aspect ratio of conductive material 16 is preferably 100 or more. An aspect ratio exceeding 1000 is also not preferable because the conductive material does not disperse when made into a paste. As shown in FIG. 2, in the positive electrode according to this embodiment, conductive material 16 covers a part of the surface of positive electrode active material 15. Note that the aspect ratio mentioned here is the aspect ratio after the positive electrode mixture layer has been coated and dried. There are cases in which the conductive material is cut when it is dispersed in the solvent using the positive electrode paste. In such cases, this should also be taken into consideration when selecting the conductive material.
[0019] Furthermore, the conductive material 16 may have a functional group on the surface thereof. The amount of the functional group contained in the conductive material 16 may be 0.1% by mass or more and 30% by mass or less, and preferably 1% by mass or more and 5% by mass or less, based on the mass of the conductive material 16.
[0020] When the conductive material 16 has a functional group on its surface, the functional groups on the surfaces of the conductive material 16 attract each other, and the conductive material 16 electrically connects to each other (see reference numeral 18 in FIG. 2). Thus, a conductive path can be efficiently formed in the positive electrode mixture layer 11. That is, when the conductive material 16 has a functional group on its surface, the conductive material 16 (or the conductive material 16 and the positive electrode active material 15) in the positive electrode paste contact each other through weak bonds such as hydrogen bonds in a fluid state immediately after coating in a coating step (see step S2 in FIG. 3) described later, and a dense conductive network (conductive path) is formed.
[0021] The functional group is preferably a functional group containing oxygen, such as OC=O, O=CN, or OH. Since oxygen has a high electronegativity, it easily forms hydrogen bonds with the functional group of the conductive material. Therefore, the conductive material 16 (or the conductive material 16 and the positive electrode active material 15) are bonded to each other by hydrogen bonds.
[0022] For example, carbon nanotubes can be used for the conductive material 13. When forming functional groups on the surface of the conductive material 16, an acid treatment, a base treatment, or the like may be performed.
[0023] In this embodiment, the amount of conductive material 16 relative to positive electrode active material 15 can be set to 0.1 mass % or more and 10 mass % or less, and preferably 0.1 mass % or more and 2 mass % or less.
[0024] Positive electrode mixture layer 11 may further contain a dispersant and a binder.
[0025] Examples of the dispersant include polyvinyl alcohol (PVA), polyvinyl butyral (PVB), polyvinylpyrrolidone (PVP), polyacrylate, polymethacrylate, polyoxyethylene alkyl ether, polyalkylene polyamine, and benzimidazole.
[0026] For the binder 14, for example, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyacrylic acid, polyacrylate, or the like can be used.
[0027] In this embodiment, the density of positive electrode mixture layer 11 is 1.2 to 2.4 g / cm 3 It is preferable that the porosity of positive electrode mixture layer 11 is 50% or more and 70% or less. It is preferable that the thickness of positive electrode mixture layer 11 is 20 to 150 μm.
[0028] Next, a method for producing a positive electrode for a lithium ion secondary battery according to this embodiment will be described. Fig. 3 is a flow chart for explaining the method for producing a positive electrode for a lithium ion secondary battery according to this embodiment.
[0029] When manufacturing a positive electrode for a lithium ion secondary battery, a positive electrode paste is first prepared (step S1). Specifically, a positive electrode paste containing at least a positive electrode active material, a conductive material, and a solvent is prepared. The above-mentioned materials can be used for the positive electrode active material and the conductive material. For example, isopropyl alcohol, N-methylpyrrolidone, water, etc. can be used for the solvent. The positive electrode paste may further contain a dispersant and a binder. The above-mentioned materials can be used for the dispersant and the binder. In this embodiment, the aspect ratio of the conductive material contained in the positive electrode paste is set to 80 or more.
[0030] Next, the positive electrode paste prepared in step S1 is applied onto the positive electrode current collector 10 (step S2). The above-mentioned materials can be used for the positive electrode current collector 10. The viscosity of the positive electrode paste is preferably 500 to 30,000 mps. If the viscosity of the positive electrode paste is too low, it becomes difficult to apply the positive electrode paste onto the positive electrode current collector 10. If the viscosity of the positive electrode paste is too high, the fluidity of the conductive material in the positive electrode paste becomes poor when the positive electrode paste is applied onto the positive electrode current collector 10, and the formation of a conductive path is hindered.
[0031] Thereafter, the positive electrode paste applied on the positive electrode current collector 10 is dried to form a positive electrode mixture layer 11 on the positive electrode current collector 10 (step S3). The drying temperature at this time is 100°C to 200°C. Through these steps, a positive electrode 1 for a lithium ion secondary battery as shown in FIG. 1 can be manufactured. In this embodiment, it is preferable that the porosity of the positive electrode mixture layer of the manufactured positive electrode is 50% or more and 70% or less. The porosity of the positive electrode mixture layer 11 can be adjusted by changing the material used for the positive electrode paste, the drying speed when drying the positive electrode paste in step S3, and the like.
[0032] This embodiment is characterized in that there is no pressing step after drying the positive electrode paste in step S3. In the present invention, the pressing step is a step of applying an external force to the positive electrode mixture layer to compress the positive electrode mixture layer, and is a step of reducing the porosity of the positive electrode mixture layer by 5% or more. In other words, even if an external force is applied to the positive electrode mixture layer, if the reduction in the porosity of the positive electrode mixture layer is less than 5%, it is not included in the pressing step of the present invention. For example, a step of applying an external force to the positive electrode mixture layer to adjust the shape of the positive electrode mixture layer after forming the positive electrode mixture layer (the reduction in the porosity of the positive electrode mixture layer is less than 5%) is not included in the pressing step.
[0033] As described above, in the present embodiment, conductive material 16 contained in positive electrode mixture layer 11 has an aspect ratio of 80 or more. When a conductive material with an aspect ratio of 80 or more is used in this manner, a dense conductive network (conductive path) can be formed in positive electrode mixture layer 11 (see FIG. 2).
[0034] On the other hand, the present inventors have found that such conductive paths are broken when an external force is applied to the positive electrode mixture layer by the pressing process when a conductive material with an aspect ratio of 80 or more is used, and the electronic resistance of the positive electrode mixture layer increases. This is thought to be because, in a fluid paste state, the contact state between the conductive materials and between the conductive material and the active material is good, and pressing destroys this good state. For this reason, in the invention according to this embodiment, the pressing process of pressing the positive electrode mixture layer after drying the positive electrode paste in step S3 is omitted. By omitting the pressing process in this way, it is possible to suppress the conductive network (conductive path) in the positive electrode mixture layer from being broken, and the conductive path in the positive electrode mixture layer can be made dense. Therefore, it is possible to improve the electronic conductivity in the positive electrode mixture layer. Therefore, it is possible to suppress an increase in the resistance of the positive electrode for a lithium ion secondary battery. In other words, it is possible to suppress an increase in the internal resistance of the lithium ion secondary battery.
[0035] In addition, the electronic resistance of the positive electrode mixture layer increases due to the separation of the contact points between the positive electrode active material and the conductive material after the pressing process, but if the positive electrode mixture layer is further pressed to increase the density of the positive electrode mixture layer, the contact points between the positive electrode active material and the conductive material gradually increase, and the electronic resistance of the positive electrode mixture layer decreases. However, even in this case, the electronic resistance of the positive electrode mixture layer is not as low as when the pressing process is omitted. In addition, when a conductive material with an aspect ratio shorter than 80 is used, the resistance when not pressed is higher than the resistance when pressed, so the above phenomenon is considered to be unique to conductive materials with an aspect ratio of 80 or more.
[0036] In addition, in the present embodiment, the pressing step of pressing the positive electrode mixture layer is omitted, so that the porosity of the positive electrode mixture layer can be increased, and therefore the output of the lithium ion secondary battery can be increased.
[0037] As described above, in the present embodiment, the conductive material contained in the positive electrode mixture layer has an aspect ratio of 80 or more, and the pressing step of pressing the positive electrode mixture layer is omitted. Therefore, a sufficient conductive path can be formed in the positive electrode mixture layer, and the porosity of the positive electrode mixture layer can be increased.
[0038] Furthermore, in the invention according to this embodiment, the pressing step of pressing the positive electrode mixture layer can be omitted, and therefore the manufacturing process of the positive electrode for a lithium ion secondary battery can be simplified.
[0039] Next, another example of the configuration of the positive electrode for a lithium ion secondary battery according to the present embodiment will be described. As described above, if the pressing step of pressing the positive electrode mixture layer 11 is omitted, the resistance between the positive electrode current collector 10 and the positive electrode mixture layer 11 may increase. In such a case, it is preferable to form a conductive path between the positive electrode current collector 10 and the positive electrode mixture layer 11 to reduce the resistance.
[0040] An example of a method for forming a conductive path between the positive electrode current collector 10 and the positive electrode mixture layer 11 is to form irregularities on the surface of the positive electrode current collector 10 on the side of the positive electrode mixture layer 11. When irregularities are formed on the surface of the positive electrode current collector 10 in this manner, the contact area between the positive electrode current collector 10 and the positive electrode mixture layer 11 increases, so that the resistance between the positive electrode current collector 10 and the positive electrode mixture layer 11 can be reduced. Specifically, the surface roughness of the positive electrode current collector 10 is preferably 100 nm or more. The unevenness on the surface can be formed by physically roughening the surface with sandpaper or the like, or by increasing the surface roughness of the press roll during rolling.
[0041] Also, as in the positive electrode 2 for lithium ion secondary battery shown in FIG. 4, the positive electrode mixture layer 20 may have a two-layer structure of a first positive electrode mixture layer 11 (corresponding to the positive electrode mixture layer 11 in FIG. 1) and a second positive electrode mixture layer 21. That is, the second positive electrode mixture layer 21 may be formed between the positive electrode current collector 10 and the first positive electrode mixture layer 11. In this case, the amount of conductive material contained in the second positive electrode mixture layer 21 may be greater than the amount of conductive material contained in the first positive electrode mixture layer 11. In this way, when the amount of conductive material of the second positive electrode mixture layer 21 on the side in contact with the positive electrode current collector 10 is increased, the resistance between the second positive electrode mixture layer 21 and the positive electrode current collector 10 can be reduced, and as a result, the resistance between the positive electrode current collector 10 and the positive electrode mixture layer 20 can be reduced. As one example, the proportion of the conductive material in second positive electrode mixture layer 21 may be 10% or more, and the proportion of the conductive material in first positive electrode mixture layer 11 may be less than 10%.
[0042] The conductive material of second positive electrode mixture layer 21 may be a material different from the conductive material of first positive electrode mixture layer 11. For example, the conductive material of second positive electrode mixture layer 21 may be acetylene black (AB) or a graphite-based material.
[0043] In addition, when manufacturing the positive electrode 2 for a lithium ion secondary battery shown in FIG. 4, the positive electrode paste may be applied onto the positive electrode collector 10, dried to form the second positive electrode mixture layer 21, and then the second positive electrode mixture layer 21 may be pressed. By pressing the second positive electrode mixture layer 21 in this manner, the density of the second positive electrode mixture layer 21 can be increased, and the conductivity can be improved. In addition, the resistance between the positive electrode collector 10 and the second positive electrode mixture layer 21 can be reduced. Thereafter, the first positive electrode mixture layer 11 is formed on the second positive electrode mixture layer 21 by using the above method (without the pressing process). That is, when manufacturing the positive electrode 2 for a lithium ion secondary battery shown in FIG. 4, only the second positive electrode mixture layer 21 may be pressed, and the first positive electrode mixture layer 11 may not be pressed.
[0044] Next, the lithium ion secondary battery according to this embodiment will be described. As an example, a lithium ion secondary battery including a wound electrode body will be described below. The wound electrode body is formed by stacking a long positive electrode sheet (positive electrode) and a long negative electrode sheet (negative electrode) with a long separator between them, winding this stack, and laterally crushing the resulting wound body. The above-mentioned positive electrode for lithium ion secondary batteries can be used for the positive electrode sheet. As with the positive electrode sheet, the negative electrode sheet can also be a negative electrode in which a negative electrode mixture layer containing a negative electrode active material is formed on both sides of a foil-shaped negative electrode current collector.
[0045] The container of the lithium ion secondary battery includes a flat rectangular container body with an open upper end and a lid that closes the opening. The material constituting the container is preferably a metal material such as aluminum or steel. Alternatively, the container may be made of a resin material such as polyphenylene sulfide resin (PPS) or polyimide resin. A positive electrode terminal that is electrically connected to the positive electrode of the wound electrode body and a negative electrode terminal that is electrically connected to the negative electrode of the wound electrode body are provided on the upper surface of the container (i.e., the lid).
[0046] Then, a positive electrode lead terminal and a negative electrode lead terminal are provided on the exposed portions of the positive electrode sheet and the negative electrode sheet at both ends of the wound electrode body (portions without the positive electrode composite layer and the negative electrode composite layer), and are electrically connected to the positive electrode terminal and the negative electrode terminal, respectively. The wound electrode body thus produced is housed in a container body, and the opening of the container body is sealed with a lid. Thereafter, an electrolyte is poured through a liquid injection hole provided in the lid, and the liquid injection hole is closed with a sealing cap, thereby producing a lithium ion secondary battery. EXAMPLES
[0047] Next, an embodiment of the present invention will be described. Samples according to the examples and comparative examples were prepared using the following method.
[0048] <Example> A sample according to the embodiment was produced using the flow shown in FIG. 3. First, LiNi 1 / 3 Co1 / 3 Mn 1 / 3 O2 was prepared as a conductive material, carbon nanotubes as a conductive material, PVdF as a binder, and NMP as a solvent. The particle size (D50) of the positive electrode active material used was 5 to 10 μm. The conductive material (carbon nanotubes) used had an average outer diameter of 10 to 20 nm and an aspect ratio of 100 to 200 in a paste state. The conductive material had 1 to 2% functional groups (the sum of OC=O, O=CN, and OH) on its surface.
[0049] These raw materials were mixed to prepare a positive electrode paste. The mixture ratio was 55-60% by mass of the positive electrode active material, 0.1-3% by mass of the conductive material, 0.01-1% by mass of the dispersant, 0.3-2% by mass of the binder, and 30-45% by mass of the solvent. The viscosity of the positive electrode paste was adjusted to be between 5000 and 10000 mps. The viscosity of the positive electrode paste was measured using a rheometer (MCR-302, cone plate CP-50-1 manufactured by Anton Paar) at 25°C and a shear rate of 10 -2 s -1 ~10 3 s -1 The measurements were performed under the following conditions.
[0050] The prepared positive electrode paste was then applied to an aluminum foil positive electrode current collector. The positive electrode paste was then dried for 2 minutes at a drying temperature of 120° C. to form a positive electrode composite layer on the positive electrode current collector. The thickness of the positive electrode composite layer at this time was 35 to 40 μm.
[0051] <Comparative Example> As in the above-mentioned examples, a positive electrode composite layer was formed on a positive electrode current collector using the flow shown in Fig. 3, and the positive electrode composite layer was then pressed to produce samples according to Comparative Examples 1 to 4. The pressing conditions for the samples according to Comparative Examples 1 to 4 were 1.8, 2.0, 2.4, and 2.8 g / cc, respectively.
[0052] <Sample evaluation> The porosity of the positive electrode mixture layer of each sample was measured. Specifically, the volume of the material itself was calculated from the specific gravity and composition ratio of each material, and the volume of the voids was calculated by subtracting it from the volume of the actual positive electrode mixture layer. The porosity was then calculated by dividing the volume of the voids by the volume of the actual positive electrode mixture layer.
[0053] In addition, the electrical resistivity (Ω·cm) (hereinafter referred to as resistance value) of the positive electrode mixture layer of each sample was measured using MCP-T610 manufactured by Nitto Seiko Analytech Co., Ltd. (formerly Mitsubishi Chemical Analytech).
[0054] The relationship between the porosity and resistance value of the positive electrode mixture layer measured as described above is shown in FIG. 5. As shown in FIG. 5, the sample according to the embodiment was not subjected to press processing, and therefore showed the highest porosity value (64%). In addition, as described above, carbon nanotubes with an aspect ratio of 100 to 200 were used as the conductive material, so that the resistance value of the positive electrode mixture layer could be reduced even without press processing. Therefore, in the sample according to the embodiment, a sufficient conductive path could be formed in the positive electrode mixture layer, and the porosity of the positive electrode mixture layer could be increased.
[0055] On the other hand, the samples according to Comparative Examples 1 to 4 had a lower porosity than the examples. Also, the higher the pressing pressure, the lower the porosity. In the sample according to Comparative Example 1, the resistance value of the positive electrode mixture layer was the highest. This is because the pressing of the positive electrode mixture layer cut the conductive path in the positive electrode mixture layer, and as a result, the electronic resistance of the positive electrode mixture layer increased. On the other hand, as shown in Comparative Examples 2 to 4, when the pressing pressure was gradually increased, the resistance value of the positive electrode mixture layer tended to decrease. This is because, when the dried positive electrode mixture layer was pressed, the contact points between the positive electrode active material and the conductive material were separated, and the electronic resistance of the positive electrode mixture layer increased (Comparative Example 1), but when the density of the positive electrode mixture layer was increased by further pressing, the contact points between the positive electrode active material and the conductive material gradually increased, and the electronic resistance of the positive electrode mixture layer decreased (Comparative Examples 2 to 4). However, even Comparative Example 4, which had the lowest resistance value of the positive electrode mixture layer among the samples subjected to press working, had a higher resistance value of the positive electrode mixture layer than the samples according to the examples in which the press step was omitted.
[0056] While the present invention has been described above with reference to the above-described embodiment, the present invention is not limited to the configuration of the above-described embodiment, and naturally includes various modifications, alterations, and combinations that may be made by a person skilled in the art within the scope of the invention as defined in the claims of the present application. [Explanation of symbols]
[0057] 1 positive electrode 10 Positive electrode current collector 11 Positive electrode mixture layer (first positive electrode mixture layer) 15 Cathode active material 16 Conductive materials 20 Positive electrode mixture layer 21 Second positive electrode mixture layer
Claims
1. A method for producing a positive electrode for a lithium ion secondary battery, the method comprising: preparing a positive electrode paste containing at least a positive electrode active material, a conductive material, and a solvent; applying the positive electrode paste onto the positive electrode current collector; and drying the applied positive electrode paste to form the positive electrode mixture layer on the positive electrode current collector. the conductive material contained in the positive electrode paste is a carbon nanotube having an aspect ratio of 100 or more and 200 or less, The conductive material has a functional group on a surface thereof, the amount of the functional group contained in the conductive material is 1% by mass or more and 5% by mass or less, The viscosity of the positive electrode paste is 5000 to 10000 mPa s, The positive electrode paste is dried, and there is no pressing process. A method for producing a positive electrode for a lithium-ion secondary battery.
2. The method for producing a positive electrode for a lithium ion secondary battery according to claim 1 , wherein the conductive materials are bonded to each other by hydrogen bonds.
3. The method for producing a positive electrode for a lithium ion secondary battery according to claim 1 or 2, wherein the positive electrode mixture layer has a porosity of 50% or more and 70% or less.
4. The method for producing a positive electrode for a lithium ion secondary battery according to any one of claims 1 to 3, wherein unevenness is formed on a surface of the positive electrode current collector on the side of the positive electrode mixture layer.
5. The method further includes forming a second positive electrode mixture layer between the positive electrode current collector and the positive electrode mixture layer, the amount of conductive material contained in the second positive electrode mixture layer is greater than the amount of conductive material contained in the positive electrode mixture layer; The method for producing a positive electrode for a lithium ion secondary battery according to any one of claims 1 to 4.
Citation Information
Patent Citations
Lithium ion battery negative electrode active material fine particle, lithium ion battery negative electrode board and its manufacturing method, electric conductive agent fine particle for lithium ion battery positive electrode mixture, and lithium ion battery positive electrode board and its manufacturing method
JP2002100360A
Electrode for battery
JP2007280687A
Cathode material for lithium ion secondary battery and method of manufacturing the same
JP2011108522A
Lithium secondary battery
JP2012209161A
Sheet for positive pole of lithium ion secondary battery and positive pole using the same
JP2013077476A