Nd-Fe-B sintered laminate magnet and its manufacturing method

By laminating ultra-thin Nd-Fe-B magnets with oriented c-axis direction and grain boundary diffusion, the method addresses the challenges of high manufacturing costs and non-uniformity in Nd-Fe-B magnets, achieving efficient and cost-effective magnets for electric vehicles with reduced Dy and Tb usage.

JP7576862B2Active Publication Date: 2024-11-01NDFEB
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022578247
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-26
Filing Date
2022-01-17
Publication Date
2024-11-01
Estimated Expiration
2042-01-17

AI Technical Summary

Technical Problem

Current Nd-Fe-B sintered magnets used in electric vehicles and hybrid electric vehicles face challenges in reducing the use of expensive and rare Dy and Tb while maintaining high magnetic properties and uniform coercive force, as they are typically manufactured by cutting thick blocks, leading to high costs and non-uniformity due to insufficient grain boundary diffusion.

Method used

The method involves laminating ultra-thin Nd-Fe-B thin plate sintered magnets with a high electrical resistance layer, orienting the c-axis direction of the B tetragonal compound within the main plane, and applying grain boundary diffusion treatment to achieve uniform coercive force without machining, using the PLP or NPLP methods to produce magnets with a thickness of 3 mm or less and at least 4 layers.

Benefits of technology

This approach allows for the industrial production of magnetically uniform, high-performance laminated magnets with reduced eddy current loss and coercive force, eliminating the need for cutting processes and minimizing the use of Dy and Tb, thus lowering costs and ensuring consistent magnetic properties across the magnet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576862000006
    Figure 0007576862000006
  • Figure 0007576862000007
    Figure 0007576862000007
  • Figure 0007576862000008
    Figure 0007576862000008
Patent Text Reader

Abstract

The present invention provides: an Nd-Fe-B multilayer sintered magnet which is magnetically uniform, while having high magnetic characteristics; and a method for producing this Nd-Fe-B sintered magnet without carrying out a cutting step. This method comprises: a step for producing an Nd-Fe-B thin plate-like sintered magnet, which has a thickness of 3 mm or less and a high orientation degree of 90% or more, and wherein the c-axis direction of an Nd2Fe14B tetragonal compound is oriented within the main surface of the Nd-Fe-B thin plate-like sintered magnet, without carrying out a cutting step by supplying and filling a mold with an alloy powder, the mold having a structure that is divided by a plurality of partition plates which are arranged at regular intervals, subsequently having the alloy powder oriented by applying a magnetic field in a direction that is parallel to the main surface of a cavity that is divided by the partition plates, and then performing sintering; and a step for stacking a plurality of Nd-Fe-B thin plate-like sintered magnets that are obtained by the above-described step.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an Nd-Fe-B sintered laminated magnet, in particular an Nd-Fe-B sintered laminated magnet used in large motors such as main motors for electric vehicles and generators, and a method for producing the same. [Background technology]

[0002] The Nd-Fe-B sintered magnet was invented by the present inventors in 1982 (JP Patent Publication 61-3424). Not only does it far surpass the magnetic properties of previous permanent magnet materials, but it is also inexpensive because it is made mainly from abundant raw materials such as neodymium (Nd: a rare earth element), iron, and boron, and has steadily expanded its market as an ideal permanent magnet material. Its applications are diverse, including computer HDDs (hard disk drives), magnetic head drive motors (VCM: voice coil motors), high-end speakers, headphones, electrically assisted bicycles, golf carts, and permanent magnet magnetic resonance imaging (MRI). Furthermore, in recent years, it has been rapidly put into practical use in drive motors for hybrid cars and electric cars, energy-saving and low-noise large home appliances (air conditioners and refrigerators), elevators, and other industrial motors.

[0003] However, although Nd-Fe-B sintered magnets have high magnetic properties, they have the drawback of poor temperature characteristics, and the temperature characteristics of coercivity are particularly important. When used in home appliances or industrial motors, it is unavoidable to raise the temperature due to the coil current. In addition, because a reverse magnetic field acts from the motor armature, when the temperature rises and the coercivity decreases, irreversible demagnetization occurs in the permanent magnet. Therefore, the only way to prevent irreversible demagnetization is to increase the coercivity in advance.

[0004] After the discovery of Nd-Fe-B sintered magnets, the effects of adding elements (Patent No. 1606420, etc.), heat treatment (Patent No. 1818977, etc.), and controlling crystal grain size (Patent No. 1662257, etc.) to improve properties such as coercivity were revealed, but the most effective way to improve coercivity was to add heavy rare earth elements (Dy, Tb) (Patent No. 1802487). However, while using a large amount of heavy rare earth elements will definitely increase coercivity, it will also reduce saturation magnetization and the maximum energy product. In addition, Dy and Tb are scarce resources and expensive, so it will be difficult to meet the large demand expected for electric vehicles and industrial and household motors.

[0005] Later, a method was discovered that increases the coercivity without causing a significant decrease in saturation magnetization or maximum energy product by using a grain boundary diffusion (GBD) method, in which, rather than adding Dy / Tb, etc. to the alloy composition, a sintered body is prepared and metals or compounds such as Dy / Tb are diffused from the outside into the crystal grain boundaries inside the sintered body by heat treatment (Patent No. 4450239, etc.).

[0006] Meanwhile, as magnets for electric vehicles, Nd-Fe-B sintered magnets have been proposed in which the magnets are divided and laminated in order to reduce losses due to eddy currents during operation, suppress heat generation in the magnets, and reduce the temperature rise of the magnets. In one example of this proposal, a 5 mm thick Nd-Fe-B sintered magnet is coated with Dy fluoride powder and heated in Ar at 900°C for 1 hour to carry out grain boundary diffusion treatment, after which 18 of these divided magnets are stacked and inserted into the magnet insertion holes of the motor rotor and solidified with epoxy resin. An IPM motor equipped with a rotor manufactured in this way is proposed in JP 2011-78268 A.

[0007] Another important background technology is magnet powder molding orientation technology for manufacturing Nd-Fe-B sintered magnets. Magnet manufacturers around the world manufacture Nd-Fe-B sintered magnets using a magnetic die pressing method. In other words, magnet alloy powder is oriented in a die to which a magnetic field is applied, pressure-molded, and the oriented green compact is sintered to produce a sintered magnet. With this method, thin plate magnets, which are in high demand, are made by mechanically cutting a large block magnet after it has been made.

[0008] In response to this, the present inventors have developed and proposed the "PressLess Process (PLP)" (see Patent Document 1 below, etc.). In this method, instead of transporting a powder compression molded body made using a magnetic field die pressing method to a sintering furnace, magnetic field orientation is applied to magnet alloy fine powder packed at high density in a filling container (hereinafter referred to as a "mold"), and the mold is transported to the sintering furnace as is. Thin plate magnets are produced by filling a mold with a shallow, large-area dish-shaped cavity with magnet alloy powder, orienting it, and then sintering it, and the orientation direction of the thin plate magnet is perpendicular to the main surface of the thin plate. In the conventional pressing method, it is necessary to produce a powder compression molded body with sufficient strength for transportation to the next process, the sintering process, so it is difficult to produce a highly oriented thin plate compact by the pressing method.In contrast, with the PLP method, the powder oriented molded body is transported together with the mold, making it possible to directly manufacture thin plate magnets industrially.

[0009] The inventors of the present application also proposed the "New-PLP Method = NPLP Method", which is an improvement over the above-mentioned "PLP Method" (see Patent Document 2 below, etc.). In this NPLP method, an oriented packed compact is made of magnet alloy fine powder filled in a mold at an appropriate density and oriented in a magnetic field, and then the outer wall member of the mold is removed, moved to a sintering plate, and carried into a sintering furnace. When manufacturing a thin plate magnet, the cavity in the mold is divided into narrow cavities by multiple partition plates, and magnet alloy powder is filled into the narrow cavities separated by the partition plates. The mold is then covered and a magnetic field is applied to orient the magnet alloy powder. The magnetic field is applied perpendicular to the main surface of the narrow cavity. The mold and the powder-molded oriented body are then transferred to a sintering plate, and the outer wall of the mold is removed, leaving only the powder-partition plate laminate consisting of the multi-layered powder and partition plates formed inside the mold on the sintering plate. The powder-partition plate laminate left on the sintering plate is then heated in a sintering furnace to produce multiple thin sintered bodies. The molds used in manufacturing sintered magnets are made from materials that require a certain degree of precision, but when they are repeatedly exposed to high sintering temperatures of over 1000°C, the molds wear out, which is a problem with the PLP method in that the molds are costly. However, with the NPLP method, the mold does not need to be placed in the sintering furnace, eliminating the problem of mold costs.

[0010] In this way, the PLP and NPLP methods described above have established the technology to directly manufacture thin plate sintered Nd-Fe-B magnets without machining. In these thin plate magnets, the orientation of the magnets, i.e., the magnetization direction, is perpendicular to the main surface of the plate. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent No. 4391897 [Patent Document 2] Patent No. 6280137 Summary of the Invention [Problem to be solved by the invention]

[0012] As the electrification of automobiles continues to progress in the future, it is desirable to reduce the cost of Nd-Fe-B sintered magnets used in main motors to the minimum possible extent while maintaining the best magnetic properties, and to reduce the amount of Dy and Tb contained in the magnets to the maximum extent permitted by resource availability.However, at present, the Nd-Fe-B magnets used in EVs (Electric Vehicles) and HEVs (Hybrid Electric Vehicles) contain a certain amount of Dy and Tb, and reduction in manufacturing costs has not been sufficient.

[0013] The reason why the above-mentioned Nd-Fe-B sintered magnets for EVs and HEVs do not have sufficient Dy and Tb reductions and manufacturing costs cannot be reduced is because laminated magnets made by stacking Nd-Fe-B thin plate magnets cannot be made cheaply. The only way to make thin plate magnets from Nd-Fe-B sintered magnets is to cut out thin magnets from block magnets using mechanical processing such as cutting wheels and wire saws. In this case, the plate magnet is cut out so that the easy magnetization direction is within the main plane of the plate. Cutting out such thin plate magnets from block magnets not only requires expensive processing costs, but also generates a large amount of cutting chips, resulting in a large loss of material.

[0014] Silicon steel sheets, which are the iron core material used in motors, are punched out to a specified shape with a thickness of 0.5 mm or less and laminated for use in order to reduce eddy current loss that occurs during motor operation. It would be desirable if Nd-Fe-B sintered magnets used in the same motor could also be punched out thinly to reduce eddy current loss to the utmost, but this is not possible. Therefore, Nd-Fe-B sintered magnets used in the main motors of electric vehicles are used as divided magnets with a thickness of about 5 mm, as in the above-mentioned known example (JP Patent Publication 2011-78268). Magnets with a thickness of 5 mm are cut out by machining from a large block magnet (called a block magnet), which incurs processing costs and costs due to reduced material yield. Furthermore, a laminate with a thickness of about 5 mm is insufficient in reducing eddy current loss. Each thin plate-shaped magnet that forms a laminated magnet is called a "unit magnet."

[0015] When unit magnets are made into laminated magnets with a thickness of 5 mm, eddy current loss is reduced more than when they are made from a non-laminated block magnet, but this is still not reduced enough. If the unit magnets were made thinner than 5 mm, for example processed to 3 mm or less and then laminated, it is expected that the eddy current loss generated in the motor would be greatly reduced, but making such thin unit magnets requires huge processing costs and the loss of material as cutting chips, i.e., a reduction in material yield, making it too expensive for practical use.

[0016] Another disadvantage of not being able to make Nd-Fe-B magnets thinner is that when grain boundary diffusion treatment is applied to thick magnets, Tb and Dy do not permeate the entire magnet, resulting in non-uniform coercive force within the magnet. As in the above-mentioned known example, even if a magnet is divided into 5mm thick magnets and grain boundary diffusion treatment is applied to the divided unit magnets, it is difficult to achieve a uniform grain boundary diffusion effect all the way to the inside of the magnet. If these are stacked and installed in a motor, non-uniformity in coercive force will exist within the magnet. This will remain as a weak point of the motor within the electric vehicle.

[0017] Because laminated magnets consisting of sufficiently thin unit magnets cannot be used for magnets in the main motors of EVs and HEVs, the temperature of the motor rises significantly while the vehicle is in operation. Furthermore, because the unit magnets are thick, the effect of improving the coercive force using the grain boundary diffusion method is insufficient and non-uniform. For these reasons, the Nd-Fe-B sintered magnets currently used in EV main motors are made of a material with 2-3% or more Tb or Dy contained in the base material, but Tb and Dy are only found in small amounts in rare earth ores. In the Nd-Fe-B magnets used in EVs and HEVs, it is strongly desired that the amount of Tb and Dy used be kept within the component limit contained in monazite and bastenasite, which are known to be abundant rare earth ores, and that limit is 0.5% of the Nd-Fe-B magnet weight.

[0018] Therefore, an object of the present invention is to provide a Nd-Fe-B sintered laminated magnet that is magnetically uniform and has high magnetic properties. Another object of the present invention is to provide a method for producing a laminated magnet consisting of extremely thin unit magnets (e.g., a thickness of 3 mm or less, preferably 2.5 mm or less) without a cutting process after sintering the Nd-Fe-B sintered magnet. [Means for solving the problem]

[0019] The present inventors have provided the following 1) to 7): 1) In order to minimize eddy current loss that occurs within the magnet, the thickness of the unit magnet of the laminated magnet should be 3 mm or less (preferably 2.5 mm or less), and the number of layers should be 4 or more, preferably 10 or more. 2) In order to reduce machining costs to the minimum, the PLP method or NPLP method is used to insert NdFe into the main surface of the Nd-Fe-B thin plate sintered magnet. 14 We directly manufacture Nd-Fe-B thin plate sintered magnets with the c-axis (easy magnetization direction) of the B tetragonal compound oriented without any machining. 3) Unit magnets with a thickness of 3 mm or less, which have been produced by repurposing the PLP or NPLP method, are bonded with an adhesive or compressed by a hot press method to produce a laminated magnet. 4) If necessary, the unit magnets are subjected to grain boundary diffusion treatment to increase their coercive force. The grain boundary diffusion treatment is carried out either before or after the unit magnets are stacked. 5) In order to reduce the cost of the laminated magnet and to improve its performance as a laminated magnet, the surface layer containing a large amount of Nd that was generated during the production of the unit magnets is not completely removed, but at least a part of it is left in place and then laminated or subjected to grain boundary diffusion treatment. 6) To ensure that the grain boundary diffusion effect is uniform and strong throughout the magnet, the thickness of the unit magnet is kept to 3 mm or less. 7) In order to increase the coercive force of the magnets produced, fine powders with an average particle size of 3 μm or thereabouts are used in the PLP or NPLP method. The present invention has been completed based on the finding that the above problems can be solved by the above method.

[0020] That is, the present invention has the following configuration. [1] A method for producing a Nd-Fe-B laminated sintered magnet in which Nd-Fe-B thin plate sintered magnets are laminated via a high electrical resistance layer, comprising the steps of: After alloy powder is fed and filled into a mold having a structure partitioned by a number of partition plates arranged at regular intervals, a magnetic field is applied in a direction parallel to the main surface of the cavity partitioned by the partition plates to orient the alloy powder, and then sintering is performed, thereby producing Nd2Fe 14 a step of producing a Nd—Fe—B sintered thin plate magnet in which the c-axis direction of the B tetragonal compound is oriented in the main surface of the Nd—Fe—B sintered thin plate magnet, the degree of orientation being high at 90% or more, and the thickness being 3 mm or less; A process for stacking a plurality of Nd-Fe-B thin plate sintered magnets obtained in the above process. 2. A method for producing a Nd—Fe—B sintered laminate magnet, comprising: [2] A method for producing a Nd-Fe-B laminated sintered magnet according to [1], characterized in that the Nd-Fe-B laminated sintered magnet is laminated on the surface of the Nd-Fe-B laminated sintered magnet while leaving at least a part of a surface layer containing a large amount of Nd produced during the sintering. [3] A method for producing a Nd-Fe-B sintered laminated magnet according to [1] or [2], characterized in that the Nd-Fe-B sintered laminated magnets are bonded to each other and laminated. [4] A method for producing a Nd-Fe-B sintered laminate magnet according to [1] or [2], characterized in that the Nd-Fe-B thin plate sintered magnets are compressed by hot pressing. [5] A method for producing a Nd-Fe-B laminated sintered magnet according to [1] or [2], characterized in that a compound powder or alloy powder containing Dy and / or Tb is applied to each of the Nd-Fe-B thin plate sintered magnets, a grain boundary diffusion treatment is performed, and then the Nd-Fe-B thin plate sintered magnets are bonded to each other. [6] A method for producing a Nd-Fe-B laminated sintered magnet according to [1] or [2], characterized in that the Nd-Fe-B thin plate sintered magnets are bonded or pressed together with a compound powder or alloy powder containing Dy and / or Tb interposed between the Nd-Fe-B thin plate sintered magnets, and then subjected to a grain boundary diffusion treatment. [7] A method for producing a Nd-Fe-B sintered laminated magnet according to [3], characterized in that the Nd-Fe-B thin plate sintered magnets are bonded to each other using an adhesive. [8] A method for producing a Nd-Fe-B laminated sintered magnet according to [3], characterized in that a plurality of the Nd-Fe-B thin plate sintered magnets are fixed in a stacked state in an injection molding die, and then resin is injected into the die to bond and mold the magnets. [9] The method for producing a Nd-Fe-B sintered laminate magnet according to any one of [1] to [8], characterized in that 10 or more layers of the Nd-Fe-B sintered laminate magnets are laminated.

[10] The Nd-Fe-B thin plate sintered magnet is A method in which alloy powder is fed and filled into a mold separated by a number of partition plates arranged at regular intervals, and then the powder is oriented in a magnetic field in a direction parallel to the main surface of the cavity separated by the partition plates, and then the mold is transported to a sintering furnace for sintering, or A method for producing a filled compact by feeding and filling an alloy powder into a mold having a side wall divided into two or more parts and a structure partitioned by a plurality of partition plates arranged at regular intervals, applying a magnetic field in a direction within the main surface of the filled compact to orient the alloy powder in the filled compact to produce an oriented filled compact, and then separating the side wall of the mold from the oriented filled compact to remove the oriented filled compact from the mold, and sintering the removed oriented filled compact. The method for producing a Nd-Fe-B sintered laminated magnet according to any one of [1] to [9] above, wherein the magnet is produced by using any one of the methods above.

[11] NdFe 14The c-axis direction of B tetragonal compound is oriented within the main surface of the Nd-Fe-B thin plate sintered magnet, the c-axis direction being oriented within the main surface of the Nd-Fe-B thin plate sintered magnet, and the c-axis direction is oriented within the main surface of the Nd-Fe-B thin plate sintered magnet. The c-axis direction of B tetragonal compound is oriented within the main surface of the Nd-Fe-B thin plate sintered magnet, and the c-axis direction of B tetragonal compound is oriented within the main surface of the Nd-Fe-B thin plate sintered magnet. The ...

[12] The Nd-Fe-B laminated sintered magnet according to

[11] , characterized in that the Nd-Fe-B thin plate sintered magnets have been subjected to grain boundary diffusion treatment, and the Nd-Fe-B thin plate sintered magnets are laminated by being bonded with an adhesive or pressure-bonded by hot pressing. Effect of the Invention

[0021] The effects of the present invention are as follows. (1) After sintering Nd-Fe-B sintered magnets, it is possible to manufacture laminated magnets consisting of extremely thin unit magnets without a cutting process. Therefore, laminated magnets consisting of extremely thin unit magnets can be industrially produced without generating a large amount of cutting waste due to the cutting process and without the need for an expensive cutting process. (2) Nd-Fe-B sintered laminated magnets, which are magnetically uniform and have high magnetic properties, can be produced industrially.

[0022] The above effects allow all metallic magnetic materials in the main motors of EVs and HEVs to be laminated to reduce eddy current loss. In other words, lamination to reduce eddy current loss has been achieved in silicon steel sheets as iron core materials, but the technology of this invention makes it possible for the first time to industrially realize lamination required to reduce eddy current loss in Nd-Fe-B sintered magnets, which are the highest performance magnets, at low cost. In addition, it is possible to reduce eddy current loss by reducing the thickness of the thin plate-shaped unit magnets, in response to requests from motor designers. Furthermore, the uniform grain boundary diffusion effect makes it possible to industrially produce high coercive force laminated magnets with uniform coercive force for the entire laminated magnet, regardless of the size of the magnet as a whole. [Brief description of the drawings]

[0023] [Figure 1]FIG. 1 is a schematic diagram showing each step of the NPLP method (New-Press Less Process method) used in the production method of the present invention. [Diagram 2] FIG. 1 shows a preferred example of a mold (used in Example 1) used in the manufacturing method of the present invention, showing the state when alloy powder is filled into the mold. The upper figure is a plan view, and the lower figure shows the structure at the AA cross section in the upper figure, along with an arrow indicating the magnetic field direction during the orientation process. [Diagram 3] 1 is a photograph showing the appearance of unit magnets produced in Example 1 of the present invention and a laminate produced by stacking the unit magnets and hot pressing them. [Figure 4] FIG. 11 is a diagram showing a method for applying GBD (grain boundary diffusion) paste between unit magnets (machining-less sintered base materials), stacking them, and applying pressure in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The present invention is a method for producing a Nd-Fe-B sintered laminate magnet in which Nd-Fe-B thin sintered magnets are stacked via a high electrical resistance layer. FIG. 1 shows a schematic diagram of the NPLP method used in the production method of the present invention. In the first step of the manufacturing method of the present invention, a mold is constructed having a structure partitioned by a plurality of partition plates arranged at regular intervals, and alloy powder (magnet alloy powder) is fed and filled into the mold. After that, a magnetic field is applied to orient the alloy powder, and then sintering is performed, thereby producing a NdFe 14 The c-axis direction of the B tetragonal compound is oriented within the main surface of the Nd-Fe-B thin plate sintered magnet, and a high degree of orientation of 90% or more and a thickness of 3 mm or less are produced. In this step, a mold is prepared, as shown in Fig. 1 1, in which the cavity inside the mold is divided into narrow cavities by multiple partition plates arranged at regular intervals (preferably 1 mm to 5 mm, more preferably 1 mm to 3.5 mm), and alloy powder is filled into the multiple narrow cavities separated by the partition plates (mold assembly / powder filling). In this case, the filling density of the alloy powder is preferably 3.4 to 3.8 g / cc.

[0025] FIG. 2 shows an example of a mold used in the manufacturing method of the present invention, which has a side wall (outer wall member) divided into two or more parts and has a structure that allows the side wall of the mold to be removed after filling with alloy powder. However, the structure of the mold used in the present invention is not limited to this, and a mold having a structure in which the side wall cannot be removed may also be used. The mold shown in Fig. 2 is made up of four side plates 1 and a bottom plate 2, and has a plurality of partition plates 3 arranged at regular intervals inside to form a plurality of cavities 5. Magnetic poles 4 are arranged perpendicular to the partition plates 3 on the top and bottom sides of the mold. The magnetic poles 4 are made of a ferromagnetic or ferrimagnetic material and have the effect of homogenizing the magnetic field applied to the alloy powder and aligning its orientation. If they are made of a material that does not deform during sintering, such as iron or silicon steel, they do not need to be removed during sintering. The magnetic poles 4 are useful and desirable for aligning the orientation of the magnetic particles in the sintered body to improve the quality of the sintered body, but are not necessary if the disturbance in orientation can be ignored without the magnetic poles.

[0026] The mold is then covered as shown in Figure 1, part 2, and a magnetic field H is applied in the direction of the arrow (from top to bottom) to orient the alloy powder filled in the cavity of the mold, resulting in an oriented filled compact. In this case, the direction of the magnetic field application is within the main surface of the oriented filled compact (i.e., the vertical direction), and a pulsed magnetic field using an air-core coil can apply a stronger magnetic field than a static magnetic field using an electromagnet. Furthermore, applying a stronger magnetic field can align the crystal axes of the particles that make up the powder in one direction, which improves the magnetic properties after sintering. In the manufacturing method of the present invention, NdFe 14 The c-axis direction of the B tetragonal compound is oriented within the main surface of the Nd-Fe-B thin plate sintered magnet, and Nd-Fe-B thin plate sintered magnets are produced that have a high degree of orientation of 90% or more and a thickness of 3 mm or less. The desirable range of the strength of the applied magnetic field to produce such thin plate sintered magnets is 3 Tesla or more, and 3.5 Tesla or more is necessary to achieve a high orientation in which the ratio of residual magnetization to saturation magnetization is 93% or more, and 4 Tesla or more is necessary to achieve an even higher orientation of 95% or more. In the present invention, the electric charge stored in the capacitor bank is usually discharged in a short time, and a large current is passed through a normal conducting air-core coil to generate a high magnetic field, and the width of one pulse magnetic field is usually between 1 ms and 1 second. The waveform of the pulse current may be a DC (unidirectional) pulse waveform or an AC decay waveform. In the present invention, a pulse magnetic field having both a DC pulse waveform and an AC pulse waveform may be combined, or a high magnetic field may be generated by passing a large current through a high-temperature superconducting air-core coil. In this case, since it is difficult to change the current in such a short time in superconductivity, the magnetic field may be applied for 1 second or more. However, in consideration of the efficiency of the process, it is preferable that the magnetic field is applied for 10 seconds or less.

[0027] Then, when the mold and the oriented packed compact are transferred to the sintering plate as shown in 3 of Fig. 1, the outer wall of the mold is removed, and only the powder / partition plate laminate formed inside the mold is left on the sintering plate (mold disassembly), and is transported into the sintering furnace. In the present invention, when a mold with a structure in which the side walls cannot be removed is used, the mold is transported into the sintering furnace as it is. Then, as shown in FIG. 1, the powder-partition plate laminate on the sintering plate is placed in a sintering furnace and sintered, resulting in the formation of NdFeB magnets on the main surfaces of the Nd-Fe-B thin plate sintered magnets. 14 It is possible to directly manufacture multiple Nd—Fe—B sintered thin plate magnets in which the c-axis direction of the B tetragonal compound is aligned, without performing any machining. In the present invention, the sintering temperature and sintering time during the sintering step are appropriately determined based on the composition and particle size of the alloy powder. In the case of a Nd-Fe-B based sintered magnet, the sintering temperature is typically about 900 to 1100°C, and the sintering time, including the heating time, is typically about 10 to 40 hours.

[0028] Furthermore, the manufacturing method of the present invention includes a step of stacking a plurality of the Nd-Fe-B sintered thin plate magnets obtained above (preferably four or more layers). In this step, the Nd-Fe-B sintered thin plate magnets may be stacked by adhering them to each other with an adhesive, or may be stacked by pressing them together using a hot press. In this case, the following two types of modes can be mentioned as modes for carrying out pressure bonding by hot pressing. (1) A laminated magnet is produced by simply pressing at least four or more layers (e.g., 10 or more layers) of thin-layer unit magnets together at a high temperature of 700°C or higher using a hot press. (2) At least four layers (e.g., ten layers or more) of stacked thin-layer unit magnets are placed in a mold in a hot press device, and the stacked thin-plate magnets are compressed using upper and lower punches at a high temperature of 700°C or higher, deforming the thin-layer unit magnets in a direction perpendicular to the compression direction and pressing them against the inner surface of the mold, thereby adjusting the shape and dimensions of the laminate.

[0029] In the above-mentioned stacking step in the manufacturing method of the present invention, when stacking a plurality of (at least four or more layers) Nd-Fe-B sintered thin plate magnets to produce an Nd-Fe-B laminated magnet, a method may be used in which an adhesive such as epoxy resin is simply applied to the Nd-Fe-B sintered thin plate magnets to adhere the unit magnets and laminate them, or a method using injection molding may be used in which a plurality of the Nd-Fe-B sintered thin plate magnets are fixed in a laminated state in a metal mold, and then resin is injected into the metal mold to adhere them.

[0030] In the method of laminating Nd-Fe-B sintered thin plate magnets by adhesive bonding, the adhesive acts to increase the electrical resistance between the layers. In addition, in the method of laminating Nd-Fe-B sintered thin plate magnets by hot pressing, it is effective to coat the thin plate magnets with neodymium oxide before hot pressing, in addition to the oxide film on the surface of the thin plate magnet. Furthermore, it has been confirmed that when the surface of a thin plate magnet is coated with Tb or Dy oxide or fluoride powder and then hot pressed, these powders not only work to promote grain boundary diffusion of the magnet, but also work to increase the electrical resistance between the thin plate magnets. It has also been confirmed that when silicon oil or silicon grease is applied to the thin plate magnet, the oxygen, carbon, and silicon contained in these resins react with the magnet components to create a high electrical resistance layer. In this specification, the "high electrical resistance layer" refers to an oxide film formed on the surface of a thin magnet plate, an adhesive applied thereto, or the above-mentioned compound, and further, when the magnet plate is bonded by hot pressing, the layer is made up of an oxide formed on the surface of the thin magnet plate, a fluoride or oxide of Tb or Dy, or a mixture or reaction product of a resin or silicon grease applied before hot pressing. These applied substances or reaction products formed during hot pressing act as the high electrical resistance layer. It is desirable that such a high electrical resistance layer be as thin as possible and have a high electrical resistivity. The thickness of the high electrical resistance layer is desirably 0.1 mm or less, and more desirably 0.05 mm or less. And, due to these high electrical resistance layers, the electrical resistance value measured by attaching electrodes to both end faces of the laminated magnet is preferably 5 times or more, more desirably 10 times or more, and most desirably 100 times or more, of the electrical resistance value measured by attaching electrodes to both end faces of a non-laminated lump of magnet of the same size.

[0031] In the present invention, when bonding the Nd-Fe-B thin plate sintered magnets to each other, it is preferable to coat each of the Nd-Fe-B thin plate sintered magnets with a compound powder or alloy powder containing Dy and / or Tb, perform a grain boundary diffusion treatment, and then bond the Nd-Fe-B thin plate sintered magnets to each other. In addition, in the present invention, it is preferable to bond or press the Nd-Fe-B sintered thin plate magnets together with a compound powder or alloy powder containing Dy and / or Tb interposed between the Nd-Fe-B sintered thin plate magnets, and then to perform grain boundary diffusion treatment. In this case, the compound powder or alloy powder containing Dy and / or Tb is suspended in an organic solvent such as ethyl alcohol and applied to the unit magnets. From the viewpoint of resources, it is preferable that the amount of the heavy rare earth metal component contained in the powder to be applied is 0.5% or less of the weight of the unit magnet. The grain boundary diffusion treatment is performed by stacking the unit magnets coated with the compound powder containing Dy and / or Tb and heating them in a vacuum or in an inert gas at 800-900°C for 5-20 hours, and then bonding the unit magnets together by adhesion or hot pressing to produce a laminated magnet. When manufacturing a laminated magnet by hot pressing unit magnets coated with compound powder containing Dy and / or Tb, it is preferable to heat the unit magnets for a long period of time, for example, 5 to 20 hours at 800 to 900°C after hot pressing in order to enhance the grain boundary diffusion effect. In the present invention, the above-mentioned compound powder or alloy powder containing Dy and / or Tb is preferably R2O3, R4O 7、 RF3 or a mixture of RF3 and LiF (lithium fluoride), etc. In addition, alloys of Dy and / or Tb with metal elements such as Fe, Ni, and Al are hydrogenated and crushed to produce hydride powder, or RH δ A preferred example is rare earth hydride powder represented by the formula: When these metal hydrides are heated to high temperatures of 800°C or higher, they become dehydrogenated metal or alloy powder. For laminated magnets, it is desirable for the bonding layer to have high electrical resistance, so metal powder or metal hydride powder is mixed with the rare earth oxide or rare earth fluoride powder described above and used to form the bonding layer.

[0032] The present inventors have confirmed that by using the above-mentioned method for producing a thin sintered Nd-Fe-B magnet plate, it is possible to produce an extremely thin sintered magnet with a thickness of 3 mm or less, preferably 2.5 mm or less, and even thinner, up to 0.8 mm. Furthermore, they have confirmed that by stacking the thin sintered magnet plates produced in this way, a laminated magnet can be produced without machining. With conventional technology, Nd-Fe-B magnets are made into thin plate magnets by machining, such as cutting and grinding with a grindstone. Cutting and grinding processes are very costly, and generate a large amount of cutting waste, which reduces material yield, which is a problem. With the manufacturing method of the present invention, unit magnets can be made without cutting or grinding, and the unit magnets made in this way can be stacked to make a laminated magnet.

[0033] A laminated sintered magnet obtained by laminating four or more layers of the Nd-Fe-B sintered thin magnet plates produced by the above-mentioned production method can be used, for example, in the main motor of an electric vehicle. The laminated sintered magnet of the present invention has a structure in which multiple homogeneous Nd-Fe-B sintered thin plate magnets are stacked together. In order to obtain the eddy current reduction effect targeted by the present invention, multiple Nd-Fe-B sintered thin plate magnets must be stacked together. However, for convenience when loading the magnet into a motor, it is preferable for the number of stacked layers to be four or more, and for the main motor of an electric vehicle, a number of stacked layers of ten or more is practical. At this time, in order to reduce eddy current loss while the motor is running, it is necessary to stack the thin sintered magnets together with a high electrical resistance layer between them. It is known that the electrical resistance value of the high electrical resistance layer does not need to be as high as that of electrical insulation.

[0034] In the manufacturing method of the present invention, when the Nd-Fe-B thin plate sintered magnet is manufactured, a) Pressless process (PLP method) in which alloy powder is fed and filled into a mold having a structure partitioned by a number of partition plates arranged at regular intervals, and then oriented in a magnetic field in a direction parallel to the main surface of the cavity partitioned by the partition plates, and then the mold is transported to a sintering furnace for sintering, or b) A new pressless process (NPLP method) in which an alloy powder is fed and filled into a mold having a structure with a side wall divided into two or more parts and partitioned by a plurality of partition plates arranged at regular intervals to produce a filled compact, a magnetic field is applied in a direction within the main surface of the filled compact to orient the alloy powder in the filled compact to produce an oriented filled compact, the side wall of the mold is then separated from the oriented filled compact to remove the oriented filled compact from the mold, and the removed oriented filled compact is sintered. Either method can be used.

[0035] In the present invention, Nd-Fe-B sintered thin plate magnets are produced using the PLP method or NPLP method, so unlike the conventional method of producing a block-shaped sintered magnet and then cutting it to a certain thickness, a thin plate magnet can be obtained directly without going through a cutting process. Therefore, in the case of Nd-Fe-B sintered thin plate magnets produced using the production method of the present invention, there is no deterioration in magnetic properties due to mechanical processing, which is well known in the past.

[0036] The PLP method described in this invention is as shown in Japanese Patent No. 4391897 and the NPLP method is as shown in Japanese Patent No. 6280137, but in this process the magnetization direction is perpendicular to the main surface (plate surface) of the magnet, that is, in the thickness direction of the magnet. In this invention, the manufacturing process of thin plate magnets as unit magnets that make up the laminated magnet is mostly the same for the above-mentioned PLP method and NPLP method, but in the manufacturing method of thin plate magnets to be used in the laminated magnet of this invention, the magnetization direction in this process is in the main surface of the magnet (parallel to the main surface).

[0037] In this invention, an oxide film is formed on the surface of the thin plate magnet made by the PLP method or the NPLP method, and it has been confirmed that this naturally formed oxide film is effective in increasing the electrical resistance between the thin plate magnets. Furthermore, the inventors have found that this Nd-rich surface layer has the effect of suppressing the deterioration of the magnetic properties of the thin plate magnet, and have confirmed that removing this surface layer reduces the coercive force of the magnet. For this reason, in the present invention, it is preferable to effectively utilize the Nd-rich surface layer formed during the sintering process without completely removing it, and to stack Nd-Fe-B sintered thin plate magnets on the surface of the Nd-Fe-B sintered thin plate magnets while leaving at least a portion of the Nd-rich surface layer formed during the sintering process.

[0038] Here, "during the sintering process" includes the processes of heating, maintaining the sintering temperature, and cooling in the sintering furnace. It is presumed that the Nd-rich surface layer formed on the surface of the unit magnet is generated during this sintering process. In conventional methods, a relatively large block sintered magnet body is produced to manufacture a thin plate, and then the thin plate magnet is obtained mainly by cutting, but the manufacturing method of the present invention does not require a cutting process. In this specification, the expression "without a cutting process" means that the block sintered body is not cut, but rather the thin plate sintered magnet is directly obtained.

[0039] The Nd-Fe-B sintered magnet of the present invention adopts the well-known notation "Nd-Fe-B", but does not only contain Nd, Fe, and B elements. Nd represents rare earth elements including Y and Sc, specifically Y, Sc, La, Ce, Pr, Nd, Eu, Gd, Tb, Dy, Ho, Yb, and Lu, and represents one or more of them. Preferably, Nd, Pr, Dy, and Tb are the main elements. These rare earth elements including Y and Sc are preferably 10 to 15 atomic %, particularly 12 to 15 atomic %, of the entire alloy. B is preferably contained in an amount of 3 to 15 atomic %, particularly 4 to 8 atomic %. In addition, one or more selected from Al, Cu, Zn, In, Si, P, S, Ti, V, Cr, Mn, Ni, Ga, Ge, Zr, Nb, Mo, Pd, Ag, Cd, Sn, Sb, Hf, Ta, and W may be contained in an amount of 0 to 11 atomic %, particularly 0.1 to 5 atomic %. The remainder is inevitable impurities such as Fe and C, N, and O, and it is preferable that Fe is contained in an amount of 50 atomic % or more, particularly 65 atomic % or more. In addition, a part of Fe, for example, 0 to 40 atomic %, particularly 0 to 15 atomic % of Fe may be replaced with Co.

[0040] The Nd-Fe-B laminated sintered magnet of the present invention is formed by laminating Nd-Fe-B thin plate sintered magnets produced by the PLP method or NPLP method by bonding or hot pressing (welding). 14 The magnet is characterized in that the c-axis direction of the B tetragonal compound is oriented within the main surface of the Nd-Fe-B thin plate sintered magnet, the magnet has a high degree of orientation (evaluated by the value obtained by dividing the residual magnetic flux density Br by the saturation magnetization Js) of 90% or more, and is a laminate comprising a plurality of Nd-Fe-B thin plate sintered magnets, preferably 4 or more, and particularly preferably 10 or more, each of which has a thickness of 3 mm or less.

[0041] In the present invention, it is preferable that the Nd-Fe-B sintered thin plate magnets are subjected to grain boundary diffusion treatment, and the Nd-Fe-B sintered thin plate magnets are laminated by being bonded with an adhesive. In the present invention, it is also preferable that an adhesive layer is present between the Nd-Fe-B thin plate sintered magnets, the adhesive layer being formed by hot pressing a compound (e.g., an oxide) powder or alloy powder containing Dy and / or Tb, and the Nd-Fe-B thin plate sintered magnets are adhered to each other and stacked by this adhesive layer, and such an adhesive layer functions as a high electrical resistance layer.

[0042] From the viewpoint of resources, it is preferable to minimize the content of Dy and Tb in Nd-Fe-B thin plate sintered magnets (unit magnets).The above-mentioned high electrical resistance layers can be the gaps between the thin plate magnets, adhesive layers, oxide films or oxygen-rich films formed during the manufacture of the unit magnets, or layers made of oxides or fluorides of Dy or Tb or altered substances thereof applied for grain boundary diffusion treatment.

[0043] By using the manufacturing method of the present invention, it is possible to produce Nd-Fe-B sintered laminated magnets consisting of extremely thin unit magnets without a cutting process. These sintered laminated magnets are magnetically uniform and have high magnetic properties, making them useful not only as magnets for electric vehicles, but also as magnets for various industrial and domestic motors. EXAMPLES

[0044] Example 1 We created the mold shown in Figure 2. The material of this mold is stainless steel (SUS304), and in Figure 2, reference numeral 1 denotes a side plate, 2 denotes a bottom plate, 3 denotes a partition plate, 4 denotes a magnetic pole, 5 denotes a cavity, and 6 denotes a lid. Then, an alloy powder having the composition shown in Table 1 below was prepared as a starting alloy (strip cast alloy = SC alloy) for producing a Nd-Fe-B sintered magnet.

[0045] [Table 1]

[0046] The SC alloy having the above composition was hydrogen-disintegrated and pulverized to an average particle size D50 of 3 μm using a nitrogen jet mill. The jet-milled powder was then placed in a mold shown in FIG. 2 at a packing density of 3.5 g / cm. 3 Next, the mold was inserted into an orientation coil, and a pulsed magnetic field of 4 Tesla was applied in the direction of the arrow in Figure 2 to orient the alloy powder. The mold used this time has 28 cavities, each with a width (called a) of 18.2 mm, a height (called b) of 10.8 mm, and a gap width (called c) of 2.35 mm. Each cavity is separated by a partition plate, which is made of stainless steel and has a thickness of 0.5 mm. When the alloy powder was fed, the alloy powder was weighed for each cavity so that the weight of the alloy powder fed to each cavity would be uniform.

[0047] Specifically, the total amount of alloy powder was 45.27 g, and 1.616 g was precisely weighed and fed into each cavity. After that, the magnetic pole, lid, and side plate were removed from the mold in that order, and the alloy powder compact including the partition plate was transferred to a carbon plate and then loaded into a vacuum sintering furnace. In this way, an in-plane oriented thin plate magnet was produced, which will become the unit that constitutes the laminated magnet.

[0048] The sintering conditions were as follows: 1×10 -3 After evacuating to a pressure of less than 1 Pa, the material was heated in a vacuum at a rate of 1°C / min to 400°C and then held at 400°C for 9 hours. The material was then heated at a rate of 2°C / min to 1000°C and held at 1000°C for 3 hours, after which it was cooled in the furnace to obtain a Nd-Fe-B thin plate sintered magnet. The dimensions of the sintered magnet after sintering were approximately a = 15.5 mm, b = 7 mm, and c (thickness) = 2 mm. This sintered magnet is hereinafter referred to as the "unit magnet". The degree of orientation (Br / Js) of the unit magnet obtained by the above sintering was 95% or more, confirming that it had a high degree of orientation.

[0049] Immediately after sintering, Tb2O3 powder with an average particle size of 5μm was applied to the top and bottom surfaces of the unit magnet. The amount of powder applied was 0.5% of the weight of the unit magnet. The powder was suspended in liquid paraffin and the suspension was applied to the unit magnet. 15 unit magnets coated with Tb2O3 powder in this way were stacked and hot pressed to create a laminated magnet. Fifteen of these unit magnets were stacked and loaded into a graphite split mold, and hot pressed to produce the Nd-Fe-B sintered laminate magnet of the present invention. The inner dimensions of the split mold were a=16.0mm and b=7.2mm, assuming the product dimensions. The hot pressing conditions were: in a vacuum, 750°C, and a pressure of 40MPa, held for 10 minutes.

[0050] When the strength of the Nd-Fe-B sintered laminated magnet produced in this manner was evaluated, it was confirmed that it had a strength comparable to that of a sintered magnet. Next, the dimensions of this laminated magnet were evaluated, finding a = 16.0 mm, b = 7.2 mm, c' (lamination thickness) = 28.1 mm. As the dimensions a and b are the same as the inner dimensions of the split mold, it is believed that the laminated unit magnets deformed toward the inner wall of the mold as soon as they were joined during the hot press, and that the deformation stopped after they reached the inner wall. It was found that it was possible to realize an integrated laminated magnet with the designed dimensions without any additional processing. FIG. 3 shows a photograph showing the appearance of the unit magnets produced in Example 1 and the laminate produced by stacking these and hot pressing. The hot-pressed laminate thus produced was heat-treated for 1 hour at 800° C. and then for 1 hour at 500° C., after which a 7 mm cube was cut out and subjected to magnetic measurement. The results are shown in Table 2.

[0051] [Table 2]

[0052] SEM observation of the cross section of the hot-pressed laminate confirmed that a high electrical resistance layer consisting of a mixture of Tb oxide, Nd oxide, and Nd-Fe-B alloy was formed on the cross section of the laminate.

[0053] Example 2 Five unit magnets were prepared using the method of Example 1, and TbF3 powder (GBD paste) was applied between the unit magnets (machining-free sintered base material) on the top and bottom surfaces of the unit magnets so that the Tb weight was 0.3% of the total weight of the five unit magnets, as shown in Figure 4. A stainless steel block weighing 5 kg was placed on top of this stack of five magnets and placed in a vacuum furnace, and the stack was heat-treated in a vacuum at 900°C for 10 hours. Then, heat treatment was performed at 500°C for 1 hour. A 7 mm square thin plate was cut from one of the unit magnets that had undergone the above heat treatment, and its magnetic properties were measured. The results are shown in Table 3.

[0054] [Table 3]

[0055] The results in Table 3 above show that high coercivity can be obtained even when TbF3 powder is placed between unit magnets and a weight is placed on them while the unit magnets are in a simple laminated state and the grain boundary diffusion treatment is performed. It was also confirmed that a high-performance Nd-Fe-B laminated magnet with high interlayer insulation and magnetic properties shown in Table 3 can be obtained by laminating five unit magnets that have been subjected to the grain boundary diffusion treatment and bonding them with an adhesive.

[0056] Example 3 Five unit magnets made in Example 1 were prepared, and after chamfering to remove burrs, a long-curing two-part epoxy resin was evenly applied to both sides of each unit magnet with a spatula, and the five magnets were stacked together and cured under a weight of about 500 g. In order to shorten the curing time, the magnets were placed in a 90°C oven for one hour and then removed, producing the Nd-Fe-B sintered laminated magnet of the present invention.

[0057] Measurements of the resistivity at both ends of the laminated magnet produced in this manner revealed that it was greater than 6.5 MΩ·cm. The eddy current loss of the laminated magnet produced above was also measured. For comparison, an integrated magnet (block-shaped magnet) of the same size as the laminated magnet was also produced and similarly subjected to measurement. Furthermore, the test magnet was placed in the center of the air-core coil, and the AC resistance Rs of the coil was measured when an AC magnetic field of 20 mA was applied in the frequency range of 100 to 50 kHz. The AC resistance Rs of the coil of an integrated magnet of the same size was also measured under the same conditions, and the two were compared. As a result, it was found that the coil AC resistance Rs of the fabricated laminated magnet was 24.7% of that of the monolithic magnet, demonstrating a significant eddy current reduction effect.

[0058] Example 4 Unit magnets were produced using the same alloy and powder as in Example 1, and in the same manner. Part of these unit magnets was polished by 0.1 mm on all sides with sandpaper. All magnets were then heat-treated by holding them at 800°C for one hour, then quenching, and then holding them at 500°C for another hour, then quenching. These two types of unit magnets (polished and unpolished) were used to produce laminated magnets by stacking five of each type, and bonding them with epoxy resin.

[0059] Three 7 mm cube samples were cut from each of the two types of laminated magnets thus produced, and the magnetic properties were measured using a BH tracer. As a result, the average magnetic properties of the laminated magnet (comparison product) obtained by stacking unit magnets that had been fully polished were a residual magnetic flux density Br of 14.1 kG and a coercive force Hcj of 14.8 kOe. On the other hand, the laminated magnet (product of the present invention) obtained by stacking unit magnets that had not been machined had Br of 14.4 kG and Hcj of 16.1 kOe. There was not much difference in Br between the two laminated magnets, but it was found that the coercive force Hcj of the laminated magnet (product of the present invention) made from unit magnets that had not been machined was more than 1 kOe greater than that of the laminated magnet (comparison product) made from unit magnets that had been fully polished.

[0060] From these experimental results, it is presumed that Nd-Fe-B thin plate magnets produced by the NPLP method have a Nd-rich surface layer, which suppresses magnetic deterioration of the crystal grains near the magnet surface. In other words, in the normal manufacturing method for Nd-Fe-B sintered magnets, thin plate magnets are produced by cutting them from a large block magnet, so there is no Nd-rich surface layer on the surface of this thin plate magnet, and therefore it is thought that the coercive force of a laminated magnet produced from a thin plate magnet obtained by cutting a block magnet is about 1 kOe lower. This Example 4 demonstrates that the Nd-Fe-B laminated magnet produced by the manufacturing method of the present invention is more advantageous in terms of magnetic properties than laminated magnets produced by conventional methods.

[0061] Example 5 Using the same Nd-Fe-B alloy powder as in Example 1, unit magnets were produced in three thicknesses after sintering, 2 mm, 3 mm, and 5 mm, using the mold in Figure 2 with the same width a and height b as in Example 1 and only the gap width c changed. Using these unit magnets, a hot-press laminate was produced by stacking five unit magnets under the same conditions as in Example 1. Furthermore, the same unit magnets were subjected to grain boundary diffusion treatment with TbF3 under the same conditions as in Example 2 to produce unit magnets, and five of these were bonded together with resin to produce a laminated magnet. The AC resistance values ​​of these hot-pressed laminated magnets and resin-bonded laminated magnets were measured, and the results are shown in Table 4. The AC resistance was measured by winding a coil 50 turns around each magnet and changing the frequency of the AC magnetic field using a HIOKI IM3536LCR meter. The results at a measurement current of 1 mA and a frequency of 30 kHz are shown in Table 4.

[0062] [Table 4]

[0063] Table 4 shows that when the thickness of the unit magnet is 3 mm or less, there is a significant reduction in AC resistance, and the magnet squareness is 90% or more, which is desirable for EV magnets.

[0064] Example 6 A unit magnet was produced by the method of Example 1 from an SC alloy having the composition shown in Table 5. An oxide film (high electrical resistance layer) was formed on the surface of this unit magnet by sintering, and this unit magnet was used to produce a laminated magnet by stacking 24 unit magnets by the method of Example 1. However, in this case, the laminated magnet was produced by hot pressing 24 layers of the laminate with nothing sandwiched between the unit magnets. The hot pressing conditions were a maximum temperature of 850°C, a maximum pressure of 65 MPa, and a holding time of 20 minutes. The obtained laminated magnet was subjected to aging treatment in a vacuum at 800°C for 30 minutes, followed by aging treatment at 520°C for 1 hour.

[0065] [Table 5]

[0066] The magnetic properties of the obtained laminated magnet were Br=13890G, Hcj=20210Oe, (BH)max=47.0MGOe, and the mechanical strength toughness test was passed without any problems. Therefore, laminated magnets made without sandwiching anything between the layers can be used for applications with lower heat resistance temperatures. [Explanation of symbols]

[0067] 1 Side Panel 2 Bottom plate 3 Partition 4 magnetic poles 5 Cavity 6 Lid

Claims

1. A method for producing a Nd—Fe—B laminated sintered magnet in which Nd—Fe—B thin sintered magnets are laminated via a high electrical resistance layer, comprising the steps of: The alloy powder is fed and filled into a mold having a structure partitioned by a plurality of partition plates arranged at regular intervals, and then the mold is covered. After that, a magnetic field is applied in a direction parallel to the main surface of the cavity partitioned by the partition plates to orient the alloy powder, and then sintering is performed at 900 to 1100°C. This allows the production of Nd without a cutting process. 2 Fe 14 a step of producing a Nd—Fe—B sintered thin plate magnet in which the c-axis direction of the B tetragonal compound is oriented in the main surface of the Nd—Fe—B sintered thin plate magnet, the degree of orientation being high at 90% or more, and the thickness being 3 mm or less; The method includes a step of stacking a plurality of the Nd—Fe—B thin plate sintered magnets obtained in the above step, A method for producing a Nd-Fe-B laminated sintered magnet, comprising stacking the Nd-Fe-B thin plate sintered magnet on the surface of the Nd-Fe-B thin plate sintered magnet while leaving at least a portion of a surface layer containing a large amount of Nd produced during the sintering.

2. 2. The method for producing a Nd-Fe-B sintered laminated magnet according to claim 1, wherein the Nd-Fe-B sintered magnet sheets are laminated by bonding them to each other.

3. 2. The method for producing a Nd-Fe-B sintered laminate magnet according to claim 1, wherein the Nd-Fe-B sintered magnet sheets are pressure-bonded by hot pressing.

4. 2. The method for producing a Nd—Fe—B laminated sintered magnet according to claim 1, characterized in that each of the Nd—Fe—B thin plate sintered magnets is coated with a compound powder or alloy powder containing Dy and / or Tb, subjected to a grain boundary diffusion treatment, and then the Nd—Fe—B thin plate sintered magnets are bonded to each other.

5. 2. The method for producing a Nd—Fe—B laminated sintered magnet according to claim 1, characterized in that the Nd—Fe—B plate-shaped sintered magnets are bonded or pressed together with a compound powder or alloy powder containing Dy and / or Tb interposed between the Nd—Fe—B plate-shaped sintered magnets, and then subjected to grain boundary diffusion treatment.

6. 3. The method for producing a Nd-Fe-B sintered laminated magnet according to claim 2, wherein the Nd-Fe-B sintered magnet sheets are bonded to one another using an adhesive.

7. The method for producing a Nd-Fe-B laminated sintered magnet according to claim 2, characterized in that a plurality of the Nd-Fe-B thin plate sintered magnets are fixed in a stacked state in an injection molding die, and then resin is injected into the die to bond and mold the magnets.

8. 8. The method for producing a Nd-Fe-B sintered laminate magnet according to claim 1, wherein ten or more of the Nd-Fe-B sintered laminate magnets are laminated.

9. The Nd—Fe—B thin plate sintered magnet is a) A method in which alloy powder is fed and filled into a mold separated by a plurality of partition plates arranged at regular intervals, a lid is placed on the mold, and the powder is oriented in a magnetic field in a direction parallel to the main surface of the cavity separated by the partition plates, and then the mold is transported to a sintering furnace and sintered at 900 to 1100°C; or b) feeding and filling an alloy powder into a mold having a side wall divided into two or more parts and a structure partitioned by a plurality of partition plates arranged at a regular interval, closing a lid to produce a filled compact, applying a magnetic field in a direction within the main surface of the filled compact to orient the alloy powder in the filled compact to produce an oriented filled compact, and then separating the side wall of the mold from the oriented filled compact to remove the oriented filled compact from the mold, and sintering the removed oriented filled compact at 900 to 1100°C.

Citation Information

Patent Citations

  • Seat control device for vehicle

    JP1987080137A

  • Permanent magnet rotor

    JP1992079741A

  • Method for manufacturing r-t-b system sintered magnet

    JP2006303197A

  • Method and apparatus for manufacturing magnetically anisotropic rare earth sintered magnet

    JP2007134353A

  • Method of assembling rotor for IPM-type permanent magnet rotary machine

    JP2011078268A