Coating roll
A silicon carbide layer on the coating roll base material addresses wear and scratch issues by enhancing hardness, providing effective protection against hard particles and ensuring durability.
Patent Information
- Application Number
- JP2020060963
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-03-30
AI Technical Summary
Coating rolls used in applying functional films to substrates face significant wear and scratch issues due to the presence of hard particles like SiO2 and ZrO2, leading to plastic deformation and damage of the soft base material, despite surface hardening methods like HCr plating and DLC films not providing sufficient protection.
A silicon carbide (SiC) layer is applied to the surface or inside of the roll base material, enhancing its hardness to 250 HV or more, with optional DLC film on top for additional properties, using carbon steel, stainless steel, or aluminum alloy as the base material.
The SiC layer significantly increases the roll's wear resistance and fracture toughness, preventing scratch marks and plastic deformation even with hard particles, ensuring durability and longevity.
Smart Images

Figure 0007576922000001 
Figure 0007576922000002 
Figure 0007576922000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating roll used for applying a coating liquid to a substrate such as a film. [Background technology]
[0002] Optical devices such as smartphones and organic electroluminescence (EL) displays use functional films (hereinafter referred to as "films") with various functions.
[0003] These films are produced by coating a base PET film or TAC film with a coating liquid containing resin-based or metal-based fine particles (fillers) with functions according to the purpose. A coating roll (for example, Patent Document 1) is used to apply the coating liquid to the film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-344759 A Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, a coating roll is required to have high hardness, abrasion resistance, solvent resistance, and high fracture toughness because it is constantly in contact with the filler, the opposing film, and a metal blade that scrapes off excess coating liquid from the roll surface.
[0006] In recent years, in order to meet the demands of high quality and high functionality of the films produced, hard particles such as silicon dioxide (SiO2) and zirconia (ZrO2) have come to be used as fillers in the coating solution. This causes significant wear to the roll surface, so it is essential that the coating roll has high wear resistance and fracture toughness.
[0007] Furthermore, the fine particles tend to aggregate and become coarse. If these coarse hard fine particles become interposed between the blade and the coating roll, the hard fine particles may cause localized scratch marks on the surface of the coating roll, as shown in Figure 8.
[0008] As a countermeasure against these problems, the roll surface is treated with a coating having a hardness of 900HV or more, such as hard chrome plating (HCr plating) or DLC (diamond-like carbon) film. However, since the hardness of these coatings is largely dependent on the hardness of the base material, it is difficult to say that sufficient effects are obtained.
[0009] In particular, DLC films have a thickness of only a few micrometers, so their hardness is highly dependent on the hardness of the substrate. Carbon steels such as STKM13A and stainless steels such as SUS304 and SUS440C are used as substrate materials for rolls, but the hardness of these materials is 200HV or less, which is one-fifth that of SiO2 and ZrO2, which have a hardness of 1100HV or more, and they are extremely soft.
[0010] Even if a hard coating is formed on the surface of such a soft substrate, the substrate X, which serves as the base, will be plastically deformed and the coating Y will be damaged, as shown in Figures 9(a) and (b). In order to eliminate this inconvenience, it is essential to increase the hardness of the surface of the substrate X.
[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a high-strength coating roll having high abrasion resistance and fracture toughness capable of withstanding the presence of hard fine particles. [Means for solving the problem]
[0012] The coating roll of the present invention is a roll base having a hardness of 250HV or less, on the surface or from the inside to the surface of the roll base, on which a silicon carbide layer (SiC layer) is formed to harden (modify) the roll base. The roll base can be made of carbon steel, stainless steel or aluminum alloy. The roll base can have a diameter of 4mm or more. The SiC layer can have an implantation depth of 5nm to 5000nm. The coating roll of the present invention may have a DLC film on the surface of the SiC layer. Effect of the Invention
[0013] The coating roll of the present invention has a SiC layer provided (modified) on the surface of the roll substrate to harden the roll substrate, so that the roll substrate is less likely to be scratched even if coarse hard microparticles are interposed between the blade and the coating roll. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2( a ) is a front view showing an example of a coating roll of the present invention, and FIG. 2( b ) is a schematic explanatory view of the surface structure of the coating roll of (a). [Diagram 2] FIG. 2( a ) is a front view showing another example of a coating roll of the present invention, and FIG. 2( b ) is a schematic explanatory view of the surface structure of the coating roll of (a). [Diagram 3] An explanatory image of a sample after focused ion beam (FIB) processing and the areas analyzed using an EDS (dispersive X-ray spectrometry) system. [Figure 4] Line analysis image showing the distribution of SiC content. [Diagram 5] Analysis image taken with a Fourier transform infrared spectrophotometer (FTIR). [Figure 6] 2 is a flowchart showing an example of a method for producing a coating roll of the present invention. [Figure 7] 1 shows an example of a manufacturing apparatus for a coating roll of the present invention. [Figure 8] A photograph of a coating roll with scratches caused by hard microparticles. [Figure 9] (a) and (b) are diagrams illustrating how hard microparticles cause plastic deformation of the substrate, resulting in damage to the coating. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] (Embodiment) An example of an embodiment of a coating roll of the present invention will be described with reference to the drawings. As an example, the coating roll shown in Fig. 1(a)(b) is a roll for solvent coating, in which a SiC layer 2 is formed (injected) on the surface or from the inside of a roll substrate 1. Fig. 1(a) shows an example in which the roll substrate 1 is mounted on the outer periphery of a shaft 3, but the roll substrate 1 can also be mounted via a bearing attached to a flange.
[0016] The roll substrate 1 is a roll-shaped tubular member that serves as the base of a coating roll. The roll substrate 1 may be made of a material having a hardness of 250HV or less (for example, a hardness of 200HV or less) as measured by a Vickers hardness tester, specifically, carbon steel or stainless steel. The roll substrate 1 may be made of an aluminum alloy. Alternatively, the roll substrate 1 may be provided with a thermal spray coating formed by WC thermal spraying or Co thermal spraying. In any case, the roll substrate 1 preferably has a diameter of 4mm or more.
[0017] As the carbon steel, for example, carbon steels represented by S25C, S45C, S50C, etc., carbon steel pipes for machine structures represented by STKM13A, STKM17C, STK400, etc., machine structural materials such as SS400, etc. can be used.
[0018] Examples of the stainless steel that can be used include austenitic stainless steels such as SUS303, SUS304, and SUS316, as well as duplex stainless steels such as SUS329J1, martensitic stainless steels such as SUS420, SUS431, and SUS440C, ferritic stainless steels such as SUS430, precipitation hardening stainless steels such as SUS630 and SUS631, and super stainless steels such as SUS2507 and SUS2545MO.
[0019] Although not shown in the drawings, the surface of the roll substrate 1 has irregularities (cells) of various shapes, such as oblique lines, a lattice shape, or a pyramid shape. The depth and pitch of the cells are about several μm to several thousand μm. The shapes, depths, and pitches of the cells are merely examples, and other shapes may be used. The cells may be provided on the entire surface of the roll substrate 1, or on a part of it.
[0020] The SiC layer 2 is a layer for modifying and hardening the surface of the roll substrate 1. As shown in Fig. 1(b), the SiC layer 2 is implanted into the surface layer of the roll substrate 1. The SiC layer 2 may have an implantation depth of preferably about 5 nm to 5000 nm, more preferably about 10 nm to 1200 nm, and even more preferably about 10 nm to 1000 nm.
[0021] In the present application, the implantation depth means a depth D from the surface of the roll substrate 1, as shown in Fig. 1(b). When forming a SiC layer 2 on the roll substrate 1, in addition to a portion (implanted portion) 2a that is implanted on the surface of the roll substrate 1, a portion (exposed portion) 2b that protrudes outward from the surface of the roll substrate 1 exists, but the implantation depth in the present application does not include the thickness of the exposed portion 2b.
[0022] In this embodiment, the SiC layer 2 is a layer made of carbon (C) and silicon (Si). However, the SiC layer 2 may contain a third element such as hydrogen (H) in addition to the main components C and Si.
[0023] A Si-based gas, for example, an organic silane such as tetramethylsilane (TMS) or hexamethyldisilazane (HMDS) can be used as a source gas for the SiC layer 2. The SiC layer 2 can be formed by using, for example, a plasma process.
[0024] The surface hardness of the SiC layer 2 is 1000HV or more, preferably 1100HV or more, and more preferably 1200HV or more, as measured by a Vickers hardness tester (using a test load of 300mgf in a nanoindentation test). If the surface hardness of the SiC layer 2 is lower than 1000HV, the roll base 1 itself may be plastically deformed. On the other hand, if the surface hardness of the SiC layer 2 is higher than 1000HV, the roll base 1 itself is unlikely to be plastically deformed.
[0025] As shown in Figures 2(a) and 2(b), the coating roll of the present invention may also have a DLC film 4 on the surface of the SiC layer 2. DLC is an amorphous material with an intermediate crystal structure between diamond and graphite, and has properties such as high hardness, low friction coefficient, abrasion resistance, electrical insulation, chemical resistance, antibacterial properties, hydrophilicity, water repellency, UV resistance, and gas barrier properties. When the DLC film 4 is formed, a Si gradient layer 2c is formed in the overlapping portion of the SiC layer 2 and the DLC film 4 as shown in Figure 2(b). The Si gradient layer 2c refers to the area where the exposed portion 2b and the DLC film 4 are in close contact with each other.
[0026] The DLC film 4 can be formed by various methods such as a plasma CVD method or a PVD method. When the plasma CVD method is used, the DLC film 4 can be formed by the same method as the SiC layer 2. The DLC film 4 may contain up to about 30 atm % of Si.
[0027] The applicant analyzed the implantation depth of the SiC layer 2 using a sample (substrate). Specifically, a focused ion beam (FIB) was used to process the cross section of the sample surface (preparation for analysis), and the obtained cross section was analyzed (line analysis of elements) by an energy dispersive X-ray analyzer (EDS). Figure 3 shows an explanatory image of the sample whose cross section was processed by FIB and the analysis points by EDS, and Figure 4 shows a line analysis image showing the distribution of the SiC content. In Figure 3, the part surrounded by a circle is the analysis point. It can be seen from Figure 4 that the implantation depth of Si is about 0.6 μm (600 nm) from the sample surface.
[0028] After the formation of the SiC layer 2, the applicant of the present invention performed an analysis using a Fourier transform infrared spectrophotometer (FTIR). The analysis results are shown in FIG. 5. As shown in FIG. 5, -1 Since a peak for Si-C bonds can be seen near this point, it is clear that a SiC structure is formed from the surface to the interior of the substrate.
[0029] (Manufacturing method of coating roll) Next, a method for manufacturing a coating roll will be described using a plasma process as an example. When using a plasma process, the coating roll can be manufactured through a cleaning process S1 and a SiC layer forming process S2, for example, as shown in Fig. 6. These manufacturing processes can be performed using an apparatus as shown in Fig. 7.
[0030] 7, 5 is a vacuum chamber, 6 is an RF high-frequency power supply, 7 is an RF electrode, 8 is a high-voltage pulse power supply, and 9 is a gas inlet. Instead of the RF high-frequency power supply 6 and the RF electrode 7, an ICP plasma source (ICP power supply) can also be used.
[0031] The cleaning step S1 is a step performed for the purpose of cleaning the roll substrate 1 and improving its adhesive strength. In this step, the roll substrate 1 is set in the RF electrode 7 of the vacuum chamber 5, and the inside of the vacuum chamber 5 is made into a vacuum state. In this state, the surface of the roll substrate 1 is cleaned by etching with argon (Ar). The etching process can be performed in the same manner as in the past. The cleaning step S1 may be performed as necessary, and can be omitted when not required. In the cleaning step S1, the oxide layer on the substrate surface may be reduced by using H ions in addition to Ar.
[0032] The cleaning of the roll substrate 1 can be carried out, for example, under the following conditions. Gas used: Ar, H2 Negative pulse voltage: -0.5~-15kV RF output: 50~1500W
[0033] The SiC layer forming step S2 is a step of forming a SiC layer 2 using C and Si as main raw materials on the surface of the roll substrate 1. In this step, the inside of the vacuum chamber 5 in which the roll substrate 1 is set is kept at room temperature (preferably about 20°C to 50°C) and in a vacuum state. However, the SiC layer 2 can be formed not only at room temperature but also at a temperature of 400°C or lower, for example, about 200°C.
[0034] In this state, a high-frequency voltage is applied by the RF high-frequency power supply 6 to generate plasma around the roll substrate 1 (specifically, around the RF electrode 7 in the vacuum chamber 5), and a negative high-voltage pulse is applied to the roll substrate 1 by the high-voltage pulse power supply 8.
[0035] Thereafter, a source gas (e.g., C and Si) is injected into the vacuum chamber 5 from the gas injection port 9, and the source gas is reacted in the vacuum chamber 5 to deposit SiC on the surface of the roll substrate 1, thereby forming a SiC layer 2 on the roll substrate 1. The SiC layer 2 is formed by being injected into the roll substrate 1 and being deposited thereon.
[0036] The SiC layer 2 may contain a third element such as H in addition to C and Si. The source gas for the SiC layer 2 may be an organic silane such as TMS or HMDS.
[0037] In addition, when manufacturing a coating roll having a DLC film 4 on the surface of the SiC layer 2 as shown in Figures 2(a) and (b), a DLC film formation step S3 may be added after the formation of the SiC layer 2. The DLC film 4 can be formed in the same manner as the SiC layer 2. As a source gas for the DLC film 4, a hydrocarbon gas such as CH4 (methane), toluene (C7H8), acetylene (C2H2), or C6H6 (benzene) can be used. A third element such as Si, oxygen (O2), boron (B), nitrogen (N2), chromium (Cr), or titanium (Ti) may be contained to relieve internal stress.
[0038] The SiC layer 2 can be formed, for example, under the following conditions. Gases used: TMS, HMDS, H, C2H2 Negative pulse voltage: -1~-20kV RF output: 50~2500W [Industrial Applicability]
[0039] The coating roll of the present invention can be particularly suitably used when applying a coating liquid to a substrate, more specifically, when applying a coating liquid containing resin-based or metal-based fine particles (filler) having a function according to the purpose to a film such as a PET film or a TAC film. [Explanation of symbols]
[0040] 1 Roll substrate 2 SiC layer 2a Injection part 2b Exposed part 2c Si graded layer 3-axis 4 DLC film 5. Vacuum Chamber 6 RF high frequency power supply 7 RF electrode 8 High voltage pulse power supply 9 Gas inlet X Base material Y membrane
Claims
1. In a coating roll used for applying a coating liquid to a substrate, A SiC layer for hardening the roll base is injected into a surface layer including an inner side of the surface of the roll base having a hardness of 250 HV or less. A coating roll characterized by:
2. The coating roll according to claim 1, The implantation depth of the SiC layer is 5 nm to 5000 nm; A coating roll characterized by:
3. The coating roll according to claim 1 or 2, The roll base material is carbon steel, stainless steel or aluminum alloy. A coating roll characterized by:
4. The coating roll according to any one of claims 1 to 3, The roll substrate has a diameter of 4 mm or more. A coating roll characterized by:
5. The coating roll according to any one of claims 1 to 4, A DLC film is provided on the surface of the SiC layer. A coating roll characterized by:
Citation Information
Patent Citations
Roller coated with hydrophilic ceramics
JP1994199068A
Coating rod
JP2004344759A
Intaglio and method for manufacturing it
JP2008254331A
Suction member and device, and sucking method
JP2011199303A
Vacuum suction member
JP2015165528A